Electrolytes, sodium secondary batteries, and power consumption devices
The electrolyte with cyclic ester, difluoro(oxalato)borate, and fluorocyclic carbonate compounds forms a stable SEI film, addressing gas generation issues in sodium secondary batteries, improving performance and stability.
Patent Information
- Application Number
- JP2026527383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-09
- Filing Date
- 2024-09-20
- Publication Date
- 2026-11-20
AI Technical Summary
Sodium-based secondary batteries suffer from gas generation issues that impair their electrical performance, preventing them from meeting the requirements of next-generation electrochemical systems.
An electrolyte comprising a cyclic ester compound with sulfate or sulfite groups, difluoro(oxalato)borate, and a fluorocyclic carbonate compound is used to form a stable Solid Electrolyte Interphase (SEI) film, reducing solubility and gas generation, and enhancing the performance of sodium secondary batteries.
The SEI film significantly reduces gas generation, lowers direct current impedance, improves storage and rapid charging performance, and enhances cycling performance of sodium secondary batteries.
Smart Images

Figure 2026539211000001_ABST
Abstract
Description
[Technical Field]
[0001] Cross-reference of related applications This application incorporates, by reference to, Chinese patent application No. 202311487395.8, filed on November 9, 2023, entitled “Electrolyte, Sodium Secondary Battery, and Power Consumption Device,” and all provisions of that application are incorporated therein.
[0002] This application relates to the field of sodium battery technology, and more particularly to electrolytes, sodium secondary batteries, and power consumption devices. [Background technology]
[0003] In recent years, secondary batteries have been widely applied in various fields, including energy storage and power systems such as hydroelectric, thermal, wind, and solar power plants, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, and aerospace.
[0004] Compared to lithium-ion batteries, sodium-based batteries have a greater competitive advantage due to their abundant and widely distributed sodium resources. However, sodium-based batteries suffer from a gas generation problem, which seriously impacts their electrical performance and prevents them from meeting the application requirements of next-generation electrochemical systems. [Overview of the project]
[0005] This application has been made in view of the above-mentioned problems, and its purpose is to provide an electrolyte that effectively enhances the stability of the SEI film, significantly reduces the amount of gas generated during the cycling and storage of sodium secondary batteries, and further enhances the storage performance, rapid charging performance, and cycling performance of sodium secondary batteries.
[0006] A first aspect of this application provides an electrolyte for a sodium secondary battery, the electrolyte comprising a first additive, a second additive, and a third additive, wherein the first additive comprises a cyclic ester compound containing a sulfate group and / or a sulfite group, the second additive comprises a difluoro(oxalato)borate, and the third additive comprises a fluorocyclic carbonate compound, the cyclic ester compound containing a sulfate group and / or a sulfite group comprises at least one of a compound having the structure shown in formula I-1 and a compound having the structure shown in formula I-2. [ka] In equation I-1, R1 is [ka] R2 and R3 are independent of each other, [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each include at least one of the following, [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group. In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R 14 It includes at least one of a single bond, a C1-C6 alkyl group, a C1-C6 ether group, and a C1-C3 alkoxy group, R 10 , R 11 , R 12 , R 13 Each of these independently contains at least one of the following: a single bond or a C1-C3 olefin group.
[0007] A first additive containing a cyclic ester compound with sulfate and / or sulfite groups, and a second additive containing difluoro(oxalato)borate, are preferentially reduced at the negative electrode over the solvent to form a film, generating components containing sulfate and / or sulfite groups, and other components containing borate in the SEI film. The cooperative use of both additives not only enhances the overall stability of the interfacial SEI film but also reduces to some extent the degree of solubility of the entire interfacial SEI film in the electrolyte. Simultaneously, by introducing a third additive containing a fluorocyclic carbonate compound into the electrolyte, the fluorocarbon compound forms a poorly soluble fluoride, such as poorly soluble NaF, at the interface of the negative electrode plate. This compensates for the defect in which the SEI film formed by a cyclic ester compound containing sulfate and / or sulfite groups and difluoro(oxalato)borate still retains a certain degree of solubility in the electrolyte, further reducing the degree of solubility of the entire interface SEI film in the electrolyte. This significantly reduces gas generation, lowers the DC impedance of the sodium secondary battery, improves the storage performance and rapid charging performance of the sodium secondary battery, and comprehensively improves the cycle performance of the sodium secondary battery.
[0008] The cyclic ester compound containing a sulfate group and / or a sulfite group can generate a component containing a sulfate group and / or a sulfite group in the SEI film, and the SEI film containing this component covers the surface of the negative electrode plate to reduce the extent to which the negative electrode plate is exposed to the electrolyte, reduce side reactions and gas generation, and improve the performance of the sodium secondary battery.
[0009] In any of the embodiments, the difluoro(oxalato)borate comprises the compound represented by Formula II, (F2C2O4B) y M y+ Formula II In Formula II, M y+ is Li + , Na + , K + , Rb + , Cs + , Mg 2+ , Ca 2+ , Ba 2+ , Fe 2+ , Ni 2+ , Al 3+ , Fe 3+ , Ni 3+ includes one or more of them, and y is 1, 2 or 3.
[0010] All of the above difluoro(oxalato)borates can generate other components containing borate in the SEI film, and these other components improve the stability of the entire SEI film on the surface of the negative electrode plate, reduce the degree of oxidative decomposition of the entire SEI film, and reduce the solubility of the entire SEI film in the electrolyte solvent to a certain extent, thereby improving the storage performance of the sodium secondary battery.
[0011] In any of the embodiments, the fluorocyclic carbonate-based compound includes a compound having the structure represented by Formula III, [Chemical Formula] In Formula III, R 15 , R 16 , R 17 , R 18Each independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an isocyanate group, an ester group, a cyano group, or a sulfonic acid group, and R 15 , R 16 , R 17 , R 18 At least one of them contains a fluorine atom.
[0012] The above-mentioned fluorocyclic carbonate compounds can all form sparingly soluble fluorides, such as sparingly soluble NaF, as a component of the SEI film during the charging process of sodium secondary batteries. This effectively reduces the solubility of the entire SEI film in the electrolyte solvent, significantly reducing the probability of the negative electrode plate being exposed to the electrolyte solvent, decreasing gas generation, and improving the storage and cycle performance of sodium secondary batteries.
[0013] In either embodiment, in formula I-1, R1 is [ka] R2 and R3 are independent of each other, [ka] It contains at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each independently contain at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and / or In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R 14 It contains at least one of a single bond, a C1-C6 alkyl group, or a C1-C6 ether group, R 10 , R 11 , R 12 , R 13 Each of these independently contains at least one of the following: a single bond or a C1-C3 olefin group.
[0014] In any embodiment, the cyclic ester compound containing a sulfate group and / or a sulfite group is [ka] [ka] It includes at least one of the following, and optionally, [ka] It includes at least one of the following.
[0015] The above substances are all soluble in the electrolyte as primary additives. The SEI film formed during the charging process covers the surface of the negative electrode plate, reducing the degree to which the negative electrode plate is exposed to the electrolyte, thereby reducing side reactions and gas generation, and improving the performance of the sodium secondary battery. [ka] Compared to the compound with the structure shown, the other compounds have a more stable structure, resulting in superior cycle performance for sodium secondary batteries.
[0016] In any embodiment, in formula II, M y+ Li + na + It includes at least one of the following.
[0017] Li + or Na + Because it has a smaller ionic radius, it provides higher solubility to sodium difluoro(oxalato)borate or lithium difluoro(oxalato)borate, and further reduces the effect of the introduction of the second additive on the electrolyte conductivity.
[0018] In either embodiment, in formula III, R 15 , R 16 , R 17 , R 18 Each independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, or an isocyanate group, and R 15 , R 16 , R 17 , R 18 At least one of them contains a fluorine atom.
[0019] In any of the embodiments, the structure shown in Equation III is [ka] It includes at least one of the following, and optionally, [ka] It includes at least one of the following.
[0020] The compounds with the structure shown in Formula III above all exhibit excellent solubility in electrolytes and can dissolve in the electrolyte to form an SEI film during the charge-discharge process.
[0021] In any embodiment, the mass ratio of the cyclic ester compound containing a sulfate group and / or a sulfite group to the difluoro(oxalato)borate is 0.01 to 500, and selectively 0.2 to 100 or 1 to 100.
[0022] By controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate within an appropriate range, it is possible to reduce the degree of intensified gas generation due to the intensified oxidative decomposition of the entire SEI film. Furthermore, it is possible to reduce the damage to the SEI film during the cycling process, which is caused by the relatively poor toughness of the entire SEI film and can further seriously affect the cycling performance. An appropriate ratio range allows for a balance between the storage performance and cycling performance of sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries. Moreover, controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate to 0.2 to 100 or 1 to 100 is advantageous for further balancing the storage performance and cycling performance of sodium secondary batteries.
[0023] In any embodiment, the mass ratio of the cyclic ester compound containing a sulfate group and / or a sulfite group to the fluorocyclic carbonate compound is 0.01 to 100, and selectively 0.1 to 50 or 1 to 50.
[0024] By controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to fluorocyclic carbonate compounds within an appropriate range, both storage performance and rapid charging performance of sodium secondary batteries can be achieved.
[0025] In any embodiment, the mass ratio of difluoro(oxalato)borate to the fluorocyclic carbonate compound is 0.01 to 100, and selectively 0.1 to 50 or 1 to 50.
[0026] By controlling the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compounds within an appropriate range, it is possible to reduce the impact on cycle performance due to the improvement of the limited solubility of the entire SEI film, as well as reduce the risk of sodium deposition caused by an excessively high proportion of fluorocyclic carbonate compounds, thereby comprehensively improving the performance of sodium secondary batteries. Furthermore, controlling the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compounds to 0.1-50 or 1-50 is advantageous for further enhancing the cycle performance of sodium secondary batteries.
[0027] In any embodiment, the ratio between the mass content A of cyclic ester compounds containing sulfate and / or sulfite groups, the mass content B of difluoro(oxalato)borate, and the mass content C of fluorocyclic carbonate compounds, based on the total mass of the electrolyte, is 0.01 ≤ (A × B) / C 2 The condition satisfies ≤500, and selectively, 0.05 ≤ (A × B) / C 2 The value is ≤ 100.
[0028] By simultaneously controlling the three components—cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borate, and fluorocyclic carbonate compounds—to satisfy the above relationship, it is possible to reduce the impact on cycle performance due to the improvement of the limited solubility of the entire SEI film caused by excessively high proportions of cyclic ester compounds containing sulfate and / or sulfite groups and difluoro(oxalato)borate. Furthermore, it is possible to reduce the risk of sodium deposition caused by excessively high proportions of fluorocyclic carbonate compounds, thereby comprehensively improving the performance of sodium secondary batteries.
[0029] In any of the embodiments, the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups is 0.01% to 5%, and selectively 0.1% to 2%, based on the total mass of the electrolyte.
[0030] By controlling the mass content of cyclic ester compounds containing sulfate and / or sulfite groups within an appropriate range, a component containing sulfate and / or sulfite groups is formed in the SEI film, reducing the degree of overall SEI film rupture due to the expansion of the sodium secondary battery during the cycle use process, further enhancing the overall protective capacity of the SEI film, and thus improving the storage performance of the sodium secondary battery. Furthermore, it is possible to reduce the degree to which excessive cyclic ester compounds are oxidized and decomposed on the positive electrode plate, intensifying gas generation, and the degree to which the oxidative decomposition products accumulate on the surface of the positive electrode plate, increasing the interfacial resistance of the positive electrode plate and intensifying the deterioration of the sodium secondary battery's performance. Moreover, by controlling the mass content of cyclic ester compounds to 0.1% to 2%, it is advantageous to achieve both storage performance and rapid charging performance of the sodium secondary battery, thereby comprehensively improving the performance of the sodium secondary battery.
[0031] In any of the embodiments, the mass content B of difluoro(oxalato)borate is 0.01% to 5%, and selectively 0.1% to 2%, based on the total mass of the electrolyte.
[0032] By controlling the mass content of difluoro(oxalato)borate within an appropriate range, other borate-containing components can be formed in the SEI film, effectively enhancing the overall stability of the interfacial SEI film, reducing the degree of gas generation, and improving the cycle performance and storage performance of sodium secondary batteries. Furthermore, excessive difluoro(oxalato)borate can be oxidized and decomposed on the positive electrode plate, intensifying gas generation and impacting storage performance. This can be mitigated, thus achieving a balance between cycle performance and storage performance in sodium secondary batteries. Moreover, controlling the mass content of difluoro(oxalato)borate to 0.1% to 2% is advantageous in achieving a balance between storage performance and rapid charging performance in sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries.
[0033] In any of the embodiments, the mass content C of the fluorocyclic carbonate compound is 0.01% to 5% of the total mass of the electrolyte, and selectively 0.1% to 2%.
[0034] By controlling the mass content of fluorocyclic carbonate compounds within an appropriate range, sufficient sparingly soluble NaF can be formed, effectively reducing the solubility of the entire interfacial SEI film in the electrolyte, thereby reducing the degree of gas generation. This is advantageous not only for improving the cycle performance and storage performance of sodium secondary batteries, but also for reducing the impact on cycle performance caused by the increased risk of sodium deposition due to excessively high mass content of fluorocyclic carbonate compounds, thus achieving a balance between cycle performance and storage performance. Furthermore, by controlling the mass content of fluorocyclic carbonate compounds to 0.1% to 2%, it is advantageous for achieving a balance between storage performance and rapid charging performance of sodium secondary batteries, thereby improving the overall performance of sodium secondary batteries.
[0035] A second aspect of this application provides a sodium secondary battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte according to the first aspect of this application.
[0036] In any embodiment, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer located on at least one side of the positive electrode current collector, the positive electrode material layer includes a positive electrode active material, the positive electrode active material includes at least one of a layered transition metal oxide, a Prussian blue compound, and a polyanionic compound.
[0037] In any embodiment, the general formula of the layered transition metal oxide is Na x Mn a Fe b Ni c M d N e O 2-δ Q fHere, M contains at least one of Ti, Li, V, Cr, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, Mg, Al, N contains at least one of Si, P, B, S, Se, and Q contains at least one of F, Cl, N, and 0.66 ≤ x ≤ 1, 0 <a≦0.7、0<b≦0.7、0≦c≦0.23、0≦d<0.3、0≦e≦0.3、0≦f≦0.3、0≦δ≦0.3、a+b+c+d+e=1、0<e+f≦0.3、0<(e+f) / a≦0.3、0.2≦d+e+f≦0.3、(b+c) / a≦1.5である。
[0038] In any embodiment, the positive electrode active material includes a layered transition metal oxide containing Cu element, The ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of Cu element in the positive electrode active material is 0.002 or higher, and the mass content of Cu element is based on the total mass of the positive electrode active material.
[0039] Introducing Cu into the positive electrode material layer is advantageous for the stability of the positive electrode active material structure. Furthermore, the Cu in the positive electrode material layer can oxidize at the interface between the positive electrode plate and cyclic ester compounds containing sulfate and / or sulfite groups, forming sparingly soluble Cu salts. This is advantageous in reducing the degree to which gas generation intensifies due to oxidative decomposition of the electrolyte of the positive electrode plate. By controlling the ratio of the mass content of cyclic ester compounds in the electrolyte to the mass content of Cu in the positive electrode active material within an appropriate range, the degree to which gas generation intensifies due to oxidative decomposition of the electrolyte of the positive electrode plate can be effectively reduced.
[0040] In any of the embodiments, the mass content of Cu element in the positive electrode active material is 23% or less, and selectively 5% to 20%, based on the total mass of the positive electrode active material.
[0041] By controlling the mass content of Cu in the positive electrode active material within an appropriate range, it is advantageous not only to provide sufficient Cu and increase the stability of the positive electrode active material structure, but also to reduce the extent to which excessively high Cu mass content in the positive electrode material layer participates in the oxidative decomposition of the electrolyte, causing performance degradation of the sodium secondary battery. Furthermore, controlling the mass content of Cu in the positive electrode active material to 5% to 20% is advantageous for further balancing the storage performance and rapid charging performance of the sodium secondary battery.
[0042] In any embodiment, the negative electrode plate includes a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, the negative electrode material layer includes the element Ca, The ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of element Ca in the negative electrode material layer is 1 or greater, and the mass content of element Ca is based on the total mass of the negative electrode material layer.
[0043] Introducing Ca element into the negative electrode active material is advantageous in reducing the degree of sodium dendrite formation, and also advantageous in forming an SEI film containing organocalcium salt components between the negative electrode active material and cyclic ester compounds containing sulfate and / or sulfite groups, further advantageous in increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. By controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Ca element in the negative electrode material layer within an appropriate range, both the storage performance and rapid charging performance of the sodium secondary battery can be achieved.
[0044] In any of the embodiments, the mass content of element Ca in the negative electrode material layer is 1 ppm to 3000 ppm, and selectively 50 ppm to 1000 ppm or 100 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.
[0045] By controlling the mass content of Ca element in the negative electrode material layer to an appropriate range, it is possible to form an SEI film that sufficiently contains organic calcium salt components, thereby increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. Furthermore, it is possible to reduce the risk of manufacturing failure of the negative electrode plate due to the gelation phenomenon of the slurry during the manufacturing process caused by an excessively high mass content of Ca element in the negative electrode material layer, the degree of reduction in the initial Coulomb efficiency and the degree of intensification of gas generation due to the formation of Ca(OH)2 during the manufacturing process, and the degree of deterioration of the sodium secondary battery's performance due to the increase in the DC impedance of the sodium secondary battery, thereby achieving both the storage performance and rapid charging performance of the sodium secondary battery. Moreover, controlling the mass content of Ca element in the negative electrode material layer to 10 ppm to 1000 ppm or 100 ppm to 1000 ppm is advantageous for further comprehensively improving the storage performance and rapid charging performance of the sodium secondary battery.
[0046] In any embodiment, the negative electrode material layer further comprises a negative electrode active material, the negative electrode active material comprising one or more of hard carbon, tin alloy, and metal oxide.
[0047] A third aspect of this application provides a power consumption device including a sodium secondary battery according to the second aspect of this application. [Brief explanation of the drawing]
[0048] To more clearly illustrate the technical concept of the embodiments of this application, the following is a brief introduction to the drawings that may be used in the embodiments of this application. It is obvious that the drawings described below represent only a few embodiments of this application, and those skilled in the art can obtain other drawings based on these drawings without expending any creative effort. [Figure 1] This is a schematic diagram of a sodium secondary battery according to one embodiment of the present application. [Figure 2] Figure 1 is an exploded view of a sodium secondary battery according to one embodiment of this application. [Figure 3] This is a schematic diagram of a battery module according to one embodiment of the present application. [Figure 4] This is a schematic diagram of a battery pack according to one embodiment of the present application. [Figure 5] Figure 4 is an exploded view of a battery pack according to one embodiment of this application. [Figure 6] This is a schematic diagram of a power consumption device that uses a sodium secondary battery as a power source according to one embodiment of this application. [Modes for carrying out the invention]
[0049] The following describes in detail embodiments of the electrolyte, sodium secondary battery, and power consumption device of this application, with appropriate reference to the drawings. However, unnecessary detailed explanations may be omitted. For example, detailed explanations of well-known matters and redundant explanations of structures that are actually the same may be omitted. This is to avoid making the following explanation unnecessarily long and to make it easily understandable to those skilled in the art. The drawings and the following explanation are provided to enable those skilled in the art to fully understand this application and do not limit the topics described in the claims.
[0050] The “range” disclosed in this application is limited in the form of a lower limit and an upper limit, and a given range is limited by selecting one lower limit and one upper limit, which define the boundary of a particular range. The range thus limited may or may not include the endpoints, and any combination is possible, that is, any lower limit can be combined with any upper limit to form a range. For example, if the ranges 60-120 and 80-110 are listed for a particular parameter, it is understood that the ranges 60-110 and 80-120 can also be assumed. Furthermore, if the minimum range values are listed as 1 and 2, and the maximum range values are listed as 3, 4 and 5, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 can all be assumed. In this application, unless otherwise specified, the numerical range “a-b” represents an abbreviated expression for any combination of real numbers a-b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 to 5" have already been listed in this specification, and "0 to 5" is simply an abbreviated representation of combinations of these numbers. Also, when a parameter is described as an integer ≥ 2, it is equivalent to disclosing that this parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0051] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical inventions.
[0052] Unless otherwise specified, all technical features and optional technical features of this application can be combined to form new technical concepts.
[0053] Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, the fact that the method includes steps (a) and (b) means that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, the fact that the method referred to above may further include step (c) means that step (c) may be added to the method in any order, for example the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), and so on.
[0054] Unless otherwise specified, the terms “includes” and “inclusion” as used in this application may be open or closed. For example, “includes” and “inclusion” may mean that other components not listed may be included or inclusion, or that only the listed components may be included or inclusion.
[0055] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the conditions A is true (or exists) and B is false (or does not exist), the condition A is false (or does not exist) but B is true (or exists), and the condition both A and B are true (or exist) all satisfy "A or B."
[0056] Gas generation in sodium-ion batteries has a serious impact on their electrical performance, particularly at low voltages, where gas generation from the negative electrode plate is a significant problem. Generally, by introducing film-forming additives into the electrolyte, a Solid Electrolyte Interphase (SEI) film is formed on the surface of the negative electrode plate. The formation of the SEI film prevents further decomposition of the electrolyte and gas generation to some extent, further improving the performance of sodium-ion batteries. However, gas generation problems still exist in sodium-ion batteries during cycle use and storage. Therefore, it is necessary to design electrolytes that meet the application requirements of next-generation electrochemical systems.
[0057] [Electrolyte] Based on this, this application proposes an electrolyte for a sodium secondary battery, the electrolyte comprising a first additive, a second additive, and a third additive, wherein the first additive comprises a cyclic ester compound containing a sulfate group and / or a sulfite group, the second additive comprises a difluoro(oxalato)borate, and the third additive comprises a fluorocyclic carbonate compound.
[0058] In this specification, "difluoro(oxalato)borate" means an anion [ka] The cation is Li + na + , K + , Rb + , Cs + Mg 2+ Ca 2+ Ba 2+ Fe 2+ Ni 2+ , Al 3+ Fe 3+ Ni 3+ A compound that contains one or more of the following, but is not limited to them.
[0059] In some embodiments, the cyclic ester compound containing a sulfate group and / or a sulfite group comprises at least one of a compound having the structure shown in formula I-1 and a compound having the structure shown in formula I-2. [ka] In equation I-1, R1 is [ka] R2 and R3 are independent of each other, [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each include at least one of the following, [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group. In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R 14 It includes at least one of a single bond, a C1-C6 alkyl group, a C1-C6 ether group, and a C1-C3 alkoxy group, R 10 , R 11 , R 12 , R 13 Each of these independently contains at least one of the following: a single bond or a C1-C3 olefin group.
[0060] In this application, the term "single bond" refers to a covalent bond formed by the sharing of a pair of electrons between two atoms, specifically, R 14 If it contains a single bond, R 14 This refers to a covalent bond that does not contain atoms, R 10 , R 11 , R 12 , R 13 If each of them independently contains a single bond, R 10 , R 11 , R 12 , R 13 This refers to the fact that each bond is a covalent bond that does not contain atoms.
[0061] Studies have shown that at low pressure, sodium secondary batteries still generate significant gas during cycle use and storage for two reasons. Firstly, the negative electrode potential of sodium secondary batteries is 0.3V higher than that of lithium secondary batteries. A higher potential drives film-forming additives to form an unstable SEI film mainly composed of several components. Such an unstable SEI film begins oxidative decomposition at 0.5V, generating a large amount of gas. Secondly, the solubility of the SEI film in the electrolyte of sodium secondary batteries is higher than that of the SEI film in lithium secondary batteries. The dissolution of the SEI film exposes the negative electrode plate to the electrolyte, causing side reactions between the negative electrode plate and the electrolyte, generating a large amount of gas.
[0062] For clarity, the first additive containing a cyclic ester compound having a sulfate group and / or a sulfite group, and the second additive comprising difluoro(oxalato)borate, are preferentially reduced at the negative electrode to form an SEI film rather than being reduced by the solvent, so as to generate a component containing a sulfate group and / or a sulfite group and another component containing a borate in the SEI film. The synergistic effect of the two additives not only improves the overall stability of the interfacial SEI film, but also reduces the dissolution degree of the entire interfacial SEI film in the electrolyte to a certain extent. Moreover, by further introducing a third additive comprising a fluorocyclic carbonate compound into the electrolyte, the fluorocarbonate compound forms a sparingly soluble fluoride, such as the sparingly soluble substance NaF, at the interface of the negative electrode plate, which compensates for the defect that the SEI film formed by the cyclic ester compound containing a sulfate group and / or a sulfite group and difluoro(oxalato)borate still has a certain solubility in the electrolyte. By further reducing the dissolution degree of the entire interfacial SEI film in the electrolyte, the degree of gas generation is greatly reduced, the direct current impedance of the sodium secondary battery is lowered, the storage performance and fast charging performance of the sodium secondary battery are improved, and the cycle performance of the sodium secondary battery is comprehensively enhanced.
[0063] In some embodiments, the difluoro(oxalato)borate includes the compound represented by Formula II, (F2C2O4B) y M y+ Formula II In Formula II, M y+ is one + , Na + , K + , Rb + , Cs + , Mg 2+ , Ca 2+ , Ba 2+ , Fe 2+ , Ni 2+ , Al 3+ , Fe 3+ , Ni 3+ or a plurality of the above, and y is 1, 2 or 3.
[0064] In some embodiments, difluoro(oxalato)borate comprises one or more of sodium difluoro(oxalato)borate, lithium difluoro(oxalato)borate, potassium difluoro(oxalato)borate, magnesium difluoro(oxalato)borate, and iron difluoro(oxalato)borate. In some embodiments, difluoro(oxalato)borate comprises sodium difluoro(oxalato)borate. In some embodiments, difluoro(oxalato)borate comprises lithium difluoro(oxalato)borate.
[0065] The above-mentioned difluoro(oxalato)borates can all generate other borate-containing components in the SEI film. These other components improve the overall stability of the surface SEI film on the negative electrode plate, reduce the degree of oxidative decomposition of the entire SEI film, and reduce the solubility of the entire SEI film in the electrolyte solvent to some extent, thereby improving the storage performance of the sodium secondary battery.
[0066] In some embodiments, in formula I-1, R1 is [ka] R2 and R3 are independent of each other, [ka] It contains at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each independently contain at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and / or In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R 14 It contains at least one of a single bond, a C1-C6 alkyl group, or a C1-C6 ether group, R 10 , R 11 , R 12 , R 13 Each of these independently contains at least one of the following: a single bond or a C1-C3 olefin group.
[0067] In some embodiments, cyclic ester compounds containing sulfate and / or sulfite groups are [ka] [ka] It includes at least one of the following.
[0068] In this specification, [ka] In R 10 , R 11 , R 12 , R 13 It is a single bond, and R9 is a CC. [ka] In R 10 , R 11 is a methylene group, R 12 , R 13 It is a single bond, and R9 is C. [ka] In R 10 , R 11 It is a single bond, R 12 , R 13 R9 is a methylene group, and R9 is CCOCC. [ka] In R 10 , R 11 It is a single bond, R 12 , R 13 R9 is a methylene group, and R9 is CC.
[0069] The above substances are all soluble in the electrolyte as primary additives. The SEI film formed during the charging process covers the surface of the negative electrode plate, reducing the degree to which the negative electrode plate is exposed to the electrolyte, thereby reducing side reactions and gas generation, and improving the performance of the sodium secondary battery. Compared to the compound with the structure shown in formula I-013, the other compounds have a more stable structure, resulting in superior cycle performance for the sodium secondary battery.
[0070] In some embodiments, in formula II, M y+ Li + na + It includes at least one of the following. In some embodiments, in formula II, M y+ Li + This includes. In some embodiments, in formula II, M y+ is, Na + Includes.
[0071] Li + or Na + Because it has a smaller ionic radius, it provides higher solubility to sodium difluoro(oxalato)borate or lithium difluoro(oxalato)borate, and further reduces the effect of the introduction of the second additive on the electrolyte conductivity.
[0072] In some embodiments, in Equation III, R 15, R 16 , R 17 , R 18 Each independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, or an isocyanate group, and R 15 , R 16 , R 17 , R 18 At least one of them contains a fluorine atom.
[0073] In some embodiments, the structure shown in Equation III is, [ka] It includes at least one of the following.
[0074] The compounds with the structure shown in Formula III above all exhibit excellent solubility in electrolytes and can dissolve in the electrolyte to form an SEI film during the charge-discharge process.
[0075] In some embodiments, the mass ratio of the cyclic ester compound containing a sulfate group and / or a sulfite group to the difluoro(oxalato)borate is 0.01 to 500, for example, 0.2 to 100 or 1 to 100. In some embodiments, the mass ratio of the cyclic ester compound containing a sulfate group and / or a sulfite group to the difluoro(oxalato)borate is selectively a value within the range of 0.01, 0.05, 0.1, 0.2, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 200, 300, 400, 500, or any two of the above.
[0076] By controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate within an appropriate range, it is possible to achieve both storage performance and cycle performance of sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries. When the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate is lower than 0.01, the entire SEI film tends to have a point-like distribution, the overall brittleness of the SEI is relatively high, and fracture is likely to occur due to volume expansion and contraction during the sodium secondary battery cycle, affecting the cycle performance of the sodium secondary battery. When the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate is higher than 500, the overall stability of the SEI film deteriorates. Furthermore, controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate to 0.2-100 or 1-100 is advantageous for further improving both the storage performance and cycle performance of sodium secondary batteries.
[0077] In some embodiments, the mass ratio of the cyclic ester compound containing sulfate and / or sulfite groups to the fluorocyclic carbonate compound is 0.01 to 100, for example, 0.1 to 50 or 1 to 50. In some embodiments, the mass ratio of the cyclic ester compound containing sulfate and / or sulfite groups to the fluorocyclic carbonate compound is selectively a value within the range of 0.01, 0.05, 0.1, 0.2, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, or any two of the above.
[0078] Research has shown that fluorocyclic carbonate compounds are unstable and readily generate acidic substances, such as HF, at high temperatures. These acidic substances destroy the interface of the positive electrode plate, making the positive electrode plate of a sodium secondary battery more susceptible to oxidation of the electrolyte and gas generation at high temperatures, thus affecting the performance of the sodium secondary battery. However, cyclic ester compounds containing sulfate and / or sulfite groups can not only form an SEI film on the negative electrode plate but also a CEI film on the interface of the positive electrode plate. The formation of a CEI film is advantageous in protecting the interface of the positive electrode plate from destruction by acidic substances. By controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to fluorocyclic carbonate compounds within an appropriate range, it is possible to achieve both storage performance and rapid charging performance in sodium secondary batteries. If the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to fluorocyclic carbonate compounds is less than 0.01, too much fluorocyclic carbonate compound exacerbates gas generation in sodium secondary batteries at high temperatures. If the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to fluorocyclic carbonate compounds is higher than 100, too much cyclic ester compound containing sulfate and / or sulfite groups tends to form an excessively thick CEI film on the positive electrode plate, increasing the DC impedance of the sodium secondary battery and affecting its rapid charging performance.
[0079] In some embodiments, the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compound is 0.01 to 100, for example, 0.1 to 50 or 1 to 50. In some embodiments, the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compound is selectively a value within the range of 0.01, 0.05, 0.1, 0.2, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, or any two of the above.
[0080] By controlling the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compounds within an appropriate range, the performance of sodium secondary batteries can be comprehensively improved. When the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compounds is lower than 0.01, sodium deposition intensifies, and when the mass ratio is higher than 100, there are limits to the reduction in gas generation. Furthermore, controlling the mass ratio of difluoro(oxalato)borate to fluorocyclic carbonate compounds to 0.1-50 or 1-50 is advantageous for further improving the cycle performance of sodium secondary batteries.
[0081] In some embodiments, the ratio between the mass content A of cyclic ester compounds containing sulfate and / or sulfite groups, the mass content B of difluoro(oxalato)borate, and the mass content C of fluorocyclic carbonate compounds, based on the total mass of the electrolyte, is 0.01 ≤ (A × B) / C 2 The condition satisfies ≤500, and in some embodiments, 0.05 ≤ (A × B) / C 2 The value is ≤100. In some embodiments, the relationship between the mass content A of cyclic ester compounds containing sulfate and / or sulfite groups, the mass content B of difluoro(oxalato)borate, and the mass content C of fluorocyclic carbonate compounds is expressed as (A × B) / C, based on the total mass of the electrolyte. 2 Selectively, this is a numerical value within the range of 0.01, 0.05, 0.1, 0.2, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 200, 300, 400, 500, or any two of the above.
[0082] SEI films containing sulfate esters, formed on the negative electrode plate using cyclic ester compounds containing sulfate and / or sulfite groups, and SEI films containing borates, formed on the negative electrode plate using difluoro(oxalato)borate, both have a certain solubility in the electrolyte solvent. SEI films containing fluorides, formed on the negative electrode plate using fluorocyclic carbonate compounds, can reduce the overall solubility of the SEI film, but they worsen the overall sodium conductivity of the SEI film. By simultaneously controlling the three components—cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borate, and fluorocyclic carbonate compounds—to satisfy the above relationship, it is possible to reduce the impact on cycle performance due to the improvement of the limited solubility of the SEI film as a whole, reduce the risk of sodium deposition, and comprehensively improve the performance of sodium secondary batteries. When the relationship between the three components—cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borate, and fluorocyclic carbonate compounds—is lower than 0.01, the degree of sodium precipitation is intensified. When the relationship between the three components—cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borate, and fluorocyclic carbonate compounds—is higher than 500, there is a limit to the reduction in the degree of gas generation.
[0083] In some embodiments, the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups is 0.01% to 5%, for example, 0.1% to 2%, based on the total mass of the electrolyte. In some embodiments, the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups is selectively a value within the range of 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, or any two of the above.
[0084] By controlling the mass content of cyclic ester compounds containing sulfate and / or sulfite groups within an appropriate range, components containing sulfate and / or sulfite groups are generated in the SEI film, reducing the degree of overall SEI film rupture due to expansion of the sodium secondary battery during the cycle use process, further enhancing the overall protective capacity of the SEI film, and thus improving the storage performance of the sodium secondary battery. Furthermore, it is possible to reduce the degree to which excessive cyclic ester compounds are oxidized and decomposed on the positive electrode plate, intensifying gas generation, and the degree to which the oxidative decomposition products accumulate on the surface of the positive electrode plate, increasing the interfacial resistance of the positive electrode plate and intensifying the deterioration of the sodium secondary battery's performance. Moreover, by controlling the mass content of cyclic ester compounds to 0.1% to 2%, it is advantageous to balance the storage performance and rapid charging performance of the sodium secondary battery, thereby comprehensively improving the performance of the sodium secondary battery.
[0085] In some embodiments, the mass content B of difluoro(oxalato)borate is 0.01% to 5% based on the total mass of the electrolyte, for example, 0.1% to 2%. In some embodiments, the mass content B of difluoro(oxalato)borate is selectively a value within the range of 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, or any two of the above.
[0086] By controlling the mass content of difluoro(oxalato)borate within an appropriate range, other borate-containing components are formed in the SEI film, effectively enhancing the overall stability of the interfacial SEI film, reducing the degree of gas generation, and thus improving the cycle performance and storage performance of sodium secondary batteries. Furthermore, excessively high mass content of difluoro(oxalato)borate can lead to oxidative decomposition of the difluoro(oxalato)borate on the positive electrode plate, intensifying gas generation and impacting storage performance. This is achieved by balancing the cycle performance and storage performance of sodium secondary batteries. Moreover, by controlling the mass content of difluoro(oxalato)borate to 0.1% to 2%, it is possible to balance the storage performance and rapid charging performance of sodium secondary batteries, which is advantageous in overall improving the performance of sodium secondary batteries.
[0087] In some embodiments, the mass content C of the fluorocyclic carbonate compound is 0.01% to 5% based on the total mass of the electrolyte, for example, 0.1% to 2%. In some embodiments, the mass content C of the fluorocyclic carbonate compound is selectively a value within the range of 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, or any two of the above.
[0088] By controlling the mass content of fluorocyclic carbonate compounds within an appropriate range, sufficient sparingly soluble NaF can be formed, effectively reducing the solubility of the entire interfacial SEI film in the electrolyte, thereby reducing the degree of gas generation. This is advantageous not only for improving the cycle performance and storage performance of sodium secondary batteries, but also for reducing the impact on cycle performance caused by the increased risk of sodium deposition due to excessively high mass content of fluorocyclic carbonate compounds, thus achieving a balance between cycle performance and storage performance. Furthermore, by controlling the mass content of fluorocyclic carbonate compounds to 0.1% to 2%, it is advantageous for achieving a balance between storage performance and rapid charging performance of sodium secondary batteries, thereby improving the overall performance of sodium secondary batteries.
[0089] In some embodiments, the electrolyte contains a sodium salt, which includes one or more of NaPF6, NaFSI, NaBF4, NaN(SO2F)2, NaClO4, NaAsF6, NaB(C2O4)2, and NaBF2(C2O4)2.
[0090] In some embodiments, the sodium salt comprises NaPF6. In some embodiments, the sodium salt comprises NaBF4. In some embodiments, the sodium salt comprises NaFSI. In some embodiments, the sodium salt comprises NaPF6 and NaFSI. In some embodiments, the sodium salt comprises NaPF6 and NaClO4.
[0091] In some embodiments, the electrolyte includes a solvent, the solvent being one or more of a linear carbonate solvent, a linear carboxylic acid ester solvent, a cyclic carbonate solvent, or an ether-based solvent.
[0092] In some embodiments, the linear carbonate solvent includes one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, dipropyl carbonate, and dibutyl carbonate. The chain-like carboxylic acid ester solvent includes one or more of methyl formate, ethyl formate, methyl propionate, ethyl propionate, propyl propionate, ethyl butyrate, methyl acetate, ethyl acetate, and propyl acetate. Cyclic carbonates include one or more of ethylene carbonate, propylene carbonate, butene carbonate, vinylene carbonate, fluoroethylene carbonate, ethylene sulfite, propylene sulfite, vinylethylene carbonate, 4-ethynyl-1,3-dioxolan-2-one, cis-4,5-difluoro-1,3-dioxolan-2-one, and trans-4,5-difluoro-1,3-dioxolan-2-one. The ether-based solvents include one or more of the following: dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, 1,2-diethoxyethane, and 1,2-dibutoxyethane.
[0093] [Positive electrode plate] The positive electrode plate includes a positive electrode current collector and a positive electrode material layer located on at least one side of the positive electrode current collector.
[0094] For example, a positive electrode current collector has two opposing surfaces in its own thickness direction, and the positive electrode material layer is placed on one or both of the two opposing surfaces of the positive electrode current collector.
[0095] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, aluminum foil may be used as the metal foil sheet. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer material substrate (for example, a substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), or polyethylene (PE)).
[0096] In some embodiments, the positive electrode material layer includes a positive electrode active material, which may be a positive electrode active material known in the art for batteries. For example, the positive electrode active material may include at least one of the following materials: a layered transition metal oxide, a polyanionic compound, or a Prussian blue compound. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may be used. These positive electrode active materials may be used individually or in combination of two or more. Here, the Prussian blue compound is Na x P[R(CN)6] δ·zH2O, wherein P and R are each independently selected from at least one of transition metal elements, 0<x≦2, 0<δ≦1 and 0≦z≦10, and the polyanionic compound comprises Na b Me c (PO4) d , wherein Me comprises one or more of Ti, Cr, Mn, Fe, Co, Ni, V, Cu and Zn, and 0<b≦4, 0<c≦2, 1≦d≦3.
[0097] In some embodiments, the general formula of the layered transition metal oxide is Na x Mn a Fe b Ni c M d N e O 2-δ Q f , wherein M comprises at least one of Ti, Li, V, Cr, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, Mg and Al, N comprises at least one of Si, P, B, S and Se, Q comprises at least one of F, Cl and N, 0.66≦x≦1, 0<a≦0.7, 0<b≦0.7, 0≦c≦0.23, 0≦d<0.3, 0≦e≦0.3, 0≦f≦0.3, 0≦δ≦0.3, a+b+c+d+e=1, 0<e+f≦0.3, 0<(e+f) / a≦0.3, 0.2≦d+e+f≦0.3, and (b+c) / a≦1.5.
[0098] The layered transition metal oxide positive electrode active material has the advantage of high voltage, but the transition metal therein catalyzes the oxidation of the solvent in the electrolyte to form RH + , and since RH + is not resistant to reduction, when the negative electrode plate is exposed, RH that has migrated to the surface of the negative electrode plate +The reduction of these components can form oxidation-resistant components, which can intensify gas generation at the negative electrode plate. Using a combination of the first and second additives is advantageous in improving the overall stability of the interfacial SEI film, and also reduces the degree of dissolution of the interfacial SEI film in the electrolyte, thereby reducing the degree of exposure of the negative electrode plate and significantly reducing gas generation, thereby comprehensively improving the cycle performance and storage performance of sodium secondary batteries.
[0099] In some embodiments, the positive electrode active material is Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 ]O2, Na 7 / 9 [Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 Contains at least one of the following: ]O2.
[0100] In some embodiments, the positive electrode active material includes a layered transition metal oxide containing Cu, and the ratio of the mass content of the cyclic ester compound in the electrolyte to the mass content of Cu in the positive electrode active material is 0.004 or greater, with the mass content of Cu being based on the total mass of the positive electrode active material. In some embodiments, the ratio of the mass content of the first additive in the electrolyte to the mass content of Cu in the positive electrode active material is selectively a value within the range of 0.004, 0.005, 0.01, 0.05, 0.1, 0.5, 1, 2, 3, 4, 5, 10, 50, 100, 500, 1000, 2000, 5000, or any two of the above, with the mass content of Cu being based on the total mass of the positive electrode active material.
[0101] To understand this, introducing the element Cu into the positive electrode active material is advantageous for the stability of the positive electrode active material structure and improves the cycle performance of sodium secondary batteries. However, at the same time, the Cu element in the positive electrode material layer undergoes a change in valence at high voltage, and Cu 3+ Generates Cu 3+These compounds have relatively high oxidative activity, which can accelerate the decomposition of the electrolyte and further degrade the performance of sodium secondary batteries. On the other hand, cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte can oxidize at the interface between the Cu element in the positive electrode material layer and the positive electrode plate to form sparingly soluble Cu salts, which is advantageous in reducing the degree to which gas generation is intensified by the decomposition of the electrolyte at the positive electrode plate. By controlling the ratio of the mass content of cyclic ester compounds in the electrolyte to the mass content of Cu element in the positive electrode active material to an appropriate range, the degree to which gas generation is intensified by the decomposition of the electrolyte at the positive electrode plate can be effectively reduced.
[0102] In some embodiments, the mass content of Cu in the positive electrode active material is 23% or less, based on the total mass of the positive electrode active material. In some embodiments, the mass content of Cu in the positive electrode active material is selectively a value within the range of 0.01%, 0.1%, 0.5%, 1%, 2%, 5%, 7%, 10%, 12%, 15%, 18%, 20%, 23%, or any two of the above.
[0103] By controlling the mass content of Cu in the positive electrode active material within an appropriate range, it is advantageous not only to provide sufficient Cu to increase the stability of the positive electrode active material structure, but also to reduce the extent to which excessively high Cu mass content in the positive electrode material layer can participate in the oxidative decomposition of the electrolyte and cause deterioration of the performance of sodium secondary batteries.
[0104] In some embodiments, the mass content of Cu element in the positive electrode active material is 5% to 20% based on the total mass of the positive electrode active material.
[0105] Furthermore, controlling the mass content of Cu element in the positive electrode active material layer to 5% to 20% is advantageous in further improving both the storage performance and rapid charging performance of sodium secondary batteries.
[0106] In some embodiments, the positive electrode active material does not need to contain the element Cu.
[0107] In some embodiments, the positive electrode material layer further selectively includes an adhesive. For example, the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0108] In some embodiments, the positive electrode material layer further selectively includes a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0109] In some embodiments, a positive electrode plate can be manufactured by the following method. Components for manufacturing the positive electrode plate, such as a positive electrode active material, a conductive agent, an adhesive, and any other component, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry. The positive electrode slurry is then coated onto a positive electrode current collector, and after processes such as drying and cold pressing, a positive electrode plate is obtained.
[0110] [Negative electrode plate] The negative electrode plate includes a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector.
[0111] For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode material layer is placed on one or both of the two opposing surfaces of the negative electrode current collector.
[0112] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, copper foil may be used as the metal foil sheet. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys) on a polymer material substrate (for example, a substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), or polyethylene (PE)).
[0113] The negative electrode material layer further comprises a negative electrode active material, the negative electrode active material comprising one or more of hard carbon, metallic sodium, sodium-tin alloy, and metal oxide.
[0114] All of the above-mentioned negative electrode active materials possess excellent sodium storage capacity, enabling sodium secondary batteries to have a high energy density.
[0115] In some embodiments, the negative electrode material layer further contains Ca element, and the ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is 1 or more, and the mass content of Ca element is based on the total mass of the negative electrode material layer. In some embodiments, the ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is selectively a numerical value within the range of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, or any two of the above, and the mass content of Ca element is based on the total mass of the negative electrode material layer.
[0116] Introducing Ca element into the negative electrode active material is advantageous in reducing the degree of sodium dendrite formation, and also advantageous in forming an SEI film containing an organic Ca salt component between the negative electrode active material and a cyclic ester compound containing sulfate and / or sulfite groups. Furthermore, it is advantageous in increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. By controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Ca element in the negative electrode material layer within an appropriate range, both the storage performance and rapid charging performance of the sodium secondary battery can be achieved.
[0117] In some embodiments, the mass content of Ca element in the negative electrode material layer is 1 ppm to 3000 ppm, based on the total mass of the negative electrode material layer. In some embodiments, the mass content of Ca element in the negative electrode material layer is selectively a value within the range of 1 ppm, 5 ppm, 10 ppm, 50 ppm, 100 ppm, 200 ppm, 400 ppm, 500 ppm, 600 ppm, 800 ppm, 1000 ppm, 1500 ppm, 2000 ppm, 2500 ppm, 3000 ppm, or any two of the above.
[0118] In some embodiments, the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte is 0.01% to 5%, and the mass content of Ca element in the negative electrode material layer is 0.1 ppm to 3000 ppm. For example, the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte is 0.1%, and the mass content of Ca element in the negative electrode material layer is 10 ppm. The ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is 0.1% / 10 ppm = 100, where 1% = 10000 ppm.
[0119] To make it understandable, the Ca element in the negative electrode material layer is involved in the formation of the SEI film, and by consuming some of the Ca element, the mass content of the Ca element in the negative electrode material layer can be reduced. For example, the mass content of the Ca element in the negative electrode material layer can be reduced to 1 ppm. Therefore, based on the total mass of the negative electrode material layer, the mass content of the Ca element is between 1 ppm and 3000 ppm, all of which are within the range protected in the embodiments of this application.
[0120] By controlling the mass content of Ca element in the negative electrode material layer to an appropriate range, it is possible to form an SEI film that sufficiently contains organic calcium salt components, thereby increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. Furthermore, it is possible to reduce the risk of manufacturing failure of the negative electrode plate due to the gelation phenomenon of the slurry during the manufacturing process caused by an excessively high mass content of Ca element in the negative electrode material layer, the degree of reduction in the initial Coulomb efficiency and the degree of intensification of gas generation due to the formation of Ca(OH)2 during the manufacturing process, and the degree of deterioration of the performance of the sodium secondary battery due to the increase in the DC impedance of the sodium secondary battery, thereby achieving both the storage performance and rapid charging performance of the sodium secondary battery.
[0121] In some embodiments, the mass content of Ca element in the negative electrode material layer is 50 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.
[0122] In some embodiments, the mass content of Ca element in the negative electrode material layer is 100 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.
[0123] Furthermore, controlling the mass content of Ca element in the negative electrode material layer to 50 ppm to 1000 ppm or 100 ppm to 1000 ppm is advantageous in further improving the overall storage performance and rapid charging performance of sodium secondary batteries.
[0124] In some embodiments, the negative electrode material layer further selectively includes an adhesive. The adhesive may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0125] In some embodiments, the negative electrode material layer further selectively includes a conductive agent. The conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0126] In some embodiments, the negative electrode material layer further selectively includes other additives, such as thickeners (e.g., sodium carboxymethylcellulose (CMC-Na)).
[0127] In some embodiments, the negative electrode plate can be manufactured by the following method. Components for manufacturing the negative electrode plate, such as a negative electrode active material, a conductive agent, an adhesive, and any other component, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry. The negative electrode slurry is then coated onto a negative electrode current collector, and after processes such as drying and cold pressing, the negative electrode plate is obtained.
[0128] [Separator] In some embodiments, the sodium secondary battery further includes a separator. Any known porous separator with good chemical and mechanical stability may be selected.
[0129] In some embodiments, the material of the separator may be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multilayer composite film. If the separator is a multilayer composite film, the materials of each layer may be the same or different.
[0130] [Sodium secondary battery] In some embodiments, the positive electrode plate, negative electrode plate, and separator can be manufactured into an electrode assembly by a winding process or a lamination process.
[0131] In some embodiments, the sodium secondary battery may include an outer casing. This casing may be used to package the electrode assembly and the electrolyte.
[0132] In some embodiments, the casing of the sodium secondary battery may be a rigid case, such as a rigid plastic case, an aluminum case, or a steel case. The casing of the sodium secondary battery may also be a pouch, such as a bag-shaped pouch. The material of the pouch may be plastic, and examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0133] In this application, the shape of the sodium secondary battery may be cylindrical, rectangular, or any other shape. For example, Figure 1 shows a rectangular sodium secondary battery 5 as an example.
[0134] In some embodiments, referring to Figure 2, the exterior body may include a case 51 and a cover plate 53. Here, the case 51 may include a bottom plate and side plates connected to the bottom plate, and the bottom plate and the side plates enclose to form a housing cavity. The case 51 has an opening communicating with the housing cavity, and the cover plate 53 can cover the opening so as to seal the housing cavity. The positive electrode plate, the negative electrode plate and the separator can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is packaged in the housing cavity. The electrolyte is infiltrated into the electrode assembly 52. The number of the electrode assemblies 52 included in the sodium secondary battery 5 may be one or more, and those skilled in the art can specifically select according to actual demands.
[0135] In some embodiments, the sodium secondary battery may be assembled into a battery module, the number of sodium secondary batteries included in the battery module may be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0136] Figure 3 shows a battery module 4 as an example. Referring to Figure 3, in the battery module 4, a plurality of sodium secondary batteries 5 may be arranged and installed in sequence along the longitudinal direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of these sodium secondary batteries 5 may be fixed by fasteners.
[0137] Alternatively, the battery module 4 may further include a housing having an accommodation space, and the plurality of sodium secondary batteries 5 are accommodated in this accommodation space.
[0138] In some embodiments, the above battery module may be further assembled into a battery pack, the number of battery modules included in the battery pack may be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0139] Figures 4 and 5 show an example of a battery pack 1. Referring to Figures 4 and 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 can be covered by the lower housing 3 to form a sealed space for housing the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.
[0140] Furthermore, this application provides a power consumption device comprising at least one of a sodium secondary battery, a battery module, or a battery pack according to this application. The sodium secondary battery, battery module, or battery pack may be used as a power source for the power consumption device or as an energy storage unit for the power consumption device. The power consumption device may include, but is not limited to, mobile devices (e.g., mobile phones, laptop computers, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0141] As the power consumption device, a sodium secondary battery, a battery module, or a battery pack can be selected according to the usage demand.
[0142] Figure 6 shows an example of a power consumption device. This power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the demand for high power output and high energy density of sodium secondary batteries in this power consumption device, a battery pack or battery module can be used.
[0143] Other examples of such devices may include mobile phones, tablet computers, and laptop computers. These devices generally require a thin profile and can use sodium-ion batteries as a power source.
[0144] Examples Examples of the present application are described below. The examples described below are illustrative and for interpretive purposes only, and should not be construed as limitations thereon. Where no specific technical or condition is described in the examples, the procedures are carried out in accordance with the technical or condition or product specifications described in the literature in the art. Where the manufacturer of the reagents or equipment used is not specified, they are all commonly available commercial products.
[0145] 1. Manufacturing method Example 1 1) Electrolyte In an argon gas-atmosphered glove box (H2O content < 10 ppm, O2 content < 1 ppm), propylene carbonate (PC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 30 / 70, 1 M NaPF6 sodium salt was dissolved, and the first additive was... [ka] , the second additive sodium difluoro(oxalato)borate and the third additive [ka] The following were added and the mixture was uniformly stirred to prepare the electrolyte. Based on the total mass of the electrolyte, the mass content of the compound with the structure described in formula I-19 of the first additive was 1%, the mass content of sodium difluoro(oxalato)borate of the second additive was 1%, and the mass content of the compound with the structure shown in formula III-1 of the third additive was 1%.
[0146] 2) Manufacturing of positive electrode plates Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3Production of O2 (13% Cu): 0.39M Na2CO3, 0.22M CuO, 0.06M Fe2O3, and a 0.67M MnO2 precursor are ball-milled for 12 hours using ethanol as a dispersant. After drying, the uniformly mixed powder is pressed into tablets at 20 MPa and sintered at 900°C for 12 hours. The sintered powder must be quickly transferred to a glove box for storage. The above positive electrode active material Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The material was uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, dried at room temperature, then transferred to a 120°C oven for 1 hour of drying, followed by cold pressing and slitting to obtain the positive electrode plate.
[0147] 3) Manufacturing of negative electrode plates Manufacturing of negative electrode materials: Negative electrode active material: Biomass material is calcined at 800°C for 2 hours in a tubular furnace containing an argon gas atmosphere, then washed with hydrochloric acid and deionized water and dried, polished, and then calcined at 1550°C for 4 hours in a tubular furnace with an argon gas atmosphere to obtain hard carbon. Manufacturing of the negative electrode plate: The hard carbon negative electrode active material, acetylene black conductive agent, styrene-butadiene rubber (SBR) adhesive, sodium carboxymethylcellulose (CMC-Na) thickener, and CaO are thoroughly stirred and uniformly mixed in a deionized water solvent system in a weight ratio of 90:4:4:2:0.014 to obtain a negative electrode slurry. CaO is added to the negative electrode slurry to adjust the Ca content at different gradients in the negative electrode plate, and the negative electrode slurry is prepared at 0.14 g (dry weight) / 1540.25 mm 2The copper foil, a negative electrode current collector with a thickness of 8 μm, was uniformly coated with the above amount, the copper foil was dried at room temperature, then transferred to an oven at 120°C and dried for 1 h, and a negative electrode plate was obtained through cold pressing and slitting.
[0148] 4) Separator A 9 μm polyethylene (PE) porous polymer film was used as the separator.
[0149] 5) Battery fabrication The positive electrode plate, the separator and the negative electrode plate were stacked in sequence, such that the separator was located between the positive and negative electrode plates to isolate the positive and negative electrode plates, followed by winding to obtain a bare cell, welding the tabs, placing the bare cell in an outer package, injecting the electrolyte prepared above into the dried battery core, and going through the processes of packaging, standing, formation, shaping, capacity test and the like, to obtain the sodium secondary battery product of Example 1.
[0150] The secondary batteries of Examples 2 to 33 and the secondary batteries of Comparative Examples 1 to 9 were similar to the manufacturing method of the sodium secondary battery of Example 1, except that the composition of the battery electrode plates and the product parameters were adjusted, and the details of the different product parameters are as shown in Table 1, Here, in Examples 2 to 14, the mass contents of the first additive, the second additive and the third additive can be adjusted by adjusting the content of the solvent in the electrolyte, The first additive in Example 15 is, [Chemical Formula] , The first additive in Example 16 is, [Chemical Formula] , The first additive in Example 17 is, [Chemical Formula] , The third additive in Example 21 is, [Chemical Formula] And, The third additive in Example 22 is [ka] And, The third additive in Example 23 is [ka] And, The negative electrode material layers containing different mass content of Ca element in Examples 24-28 can be adjusted by adding CaO with different mass content during the manufacturing process of the negative electrode plate. The positive electrode active materials containing different mass content of Cu in Examples 29-33 were obtained by adjusting the stoichiometric ratios of the precursor Fe2O3, CuO, MnO2, and Na2CO3 during the sintering process and the formulation of the positive electrode material with different Cu content during the manufacturing process of the positive electrode plate. Specifically, these are as follows: Na 1 / 2 Fe 1 / 2 Mn 1 / 2 Production of O2 (0% Cu): 0.25M Na2CO3, 0.25M Fe2O3, and 0.5M MnO2 precursor are ball-milled for 12 hours using ethanol as a dispersant. After drying, the uniformly mixed powder is pressed into tablets at 20 MPa and sintered at 900°C for 12 hours. The sintered powder must be quickly transferred to a glove box for storage. Na 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 Production of O2 (23% Cu): 0.45M Na2CO3, 0.4M CuO, 0.05M Fe2O3, and a 0.5M MnO2 precursor are ball-milled for 12 hours using ethanol as a dispersant. After drying, the uniformly mixed powder is pressed into tablets at 20 MPa and sintered at 900°C for 12 hours. The sintered powder must be quickly transferred to a glove box for storage. Example 29: Na of the positive electrode active material 1 / 2 Fe1 / 2 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 30: 50% Na of the positive electrode active material 1 / 2 Fe 1 / 2 Mn 1 / 2 O2, 50% Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 31: 50% Na of the positive electrode active material 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, 50% Na 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 32: Na of the positive electrode active material 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 33: Na of the positive electrode active material 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The material was uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, dried at room temperature, then transferred to a 120°C oven for 1 hour of drying, followed by cold pressing and slitting to obtain the positive electrode plate.
[0151] The first additive in Comparative Example 8 is vinyl sulfate. [ka] And, The third additive in Comparative Example 9 is a cyclic carbonate compound that does not contain fluorine atoms. [ka] That is the case.
[0152] 2. Performance Test 1, Electrolyte 1) Mass content test of the first additive, the second additive, and the third additive. The content of the first, second, and third additives in the electrolyte of sodium secondary batteries could be qualitatively and quantitatively tested using ion chromatography (JY / T 020~1996, published January 23, 1997, performed April 1, 1997) and gas chromatography (GB / T 6041-2002 and GB / T 9722-2006).
[0153] 2, negative electrode plate / positive electrode plate 1) Measurement of the Ca element content in the negative electrode material layer Referring to EPA 6010D-2014, the calcium content in the negative electrode material layer was tested using inductively coupled plasma atomic emission spectroscopy.
[0154] 2) Measurement of the dissolution rate of the SEI film in the negative electrode material layer. At room temperature, a sodium secondary battery was charged to 4.0V with a constant current of 1C, then charged again with a constant voltage of 4.0V until the current fell below 0.05C, and finally discharged to 1.5V at 0.33C. After full discharge, the sodium-ion battery was disassembled and the negative electrode plate was removed. The negative electrode plate was first washed three times with ethyl methyl carbonate solvent to remove a large amount of residual electrolyte, then immersed in ethyl methyl carbonate solvent for 1 hour to remove residual electrolyte, and finally, the cleaned negative electrode plate was obtained. 10g of the cleaned negative electrode plate was taken and immersed in 10g of ethyl methyl carbonate solvent for 24 hours, then filtered, and the supernatant was taken and tested for the sodium element content. Referring to EPA 6010D-2014, the sodium element content in the supernatant could be tested using inductively coupled plasma atomic emission spectroscopy. The amount of sodium in the solvent after 24 hours of immersion was used to represent the dissolution rate of SEI, and it was shown that a higher sodium content resulted in a faster dissolution rate of SEI.
[0155] 3) Measurement of the Cu element content in the positive electrode active material Referring to EPA 6010D-2014, the Cu content in the positive electrode material layer was tested using inductively coupled plasma atomic emission spectroscopy, i.e., the Cu content in the positive electrode active material = Cu content in the positive electrode material layer / mass content of the positive electrode active material in the positive electrode material layer.
[0156] 3, battery 1) Rate of change in storage volume at low pressure At 25°C, fresh sodium secondary batteries produced in the examples and comparative examples were left for 5 minutes, then charged with a constant current at a 1C multiplier up to 4.0V, charged with a constant voltage until the current was 0.05C or less, then left for 5 minutes, discharged with a constant current at a 1C multiplier up to 1.5V, the battery volume V1 was tested using the drainage method, and the batteries were placed in a 55°C oven and stored for 3 months. After removing the batteries, the test volume was taken to V2, and the rate of change in battery volume was calculated as (V2-V1) / V1 × 100%.
[0157] 2) Charging performance at 0℃ Fabrication of a three-electrode battery: First, a vanadium sodium phosphate reference electrode is manufactured. The active material, vanadium sodium phosphate, the conductive agent, acetylene black, and the adhesive, polyvinylidene fluoride (PVDF), are thoroughly stirred and uniformly mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to prepare a slurry. The slurry is uniformly applied to a 10 cm long aluminum wire (where the applied area occupies 1 cm), and after drying at 100°C, the target reference electrode is obtained. In the manufacturing process of a sodium secondary battery, when this reference electrode is placed between the negative electrode plate and the separator, a three-electrode battery is obtained. 0°C Rapid Charging Capacity Test: A three-electrode battery including the above reference electrode was charged at 25°C with a constant current of 1C until the voltage reached 4.0V, then charged with a constant voltage until the current was 0.05C or less, left for 5 minutes, discharged with a constant current at a multiplier of 1C until it reached 1.5V, and the discharge capacity was recorded as C1. Then, this battery was placed in a 0°C environment and left idle for 2 hours, and charged with a constant current of 0.33C until the voltage reached 4.0V, and the charge capacity relative to the negative electrode potential before the reference potential reached -3.377V was obtained as C2. The battery's charge performance at 0°C = C2 / C1 × 100%.
[0158] 3) DC impedance At 25°C, the cell's charge state was adjusted to 50% SOC and left standing for 30 minutes. The battery voltage at this time was recorded as U1 (V). The cell was then discharged for 10 seconds using 4C, and the battery voltage at this time was recorded as U2 (V). The corresponding discharge current I (mA) of the battery is 4 × the battery's design capacity (mAh). The DC impedance DCR = (U1 - U2) / I, and the unit is mΩ.
[0159] 4) Cycle performance At 25°C, the manufactured battery is charged to 4.0V with a constant current of 0.33C, then charged again with a constant voltage of 4.0V until the current drops to 0.05C, left to stand for 10 minutes, and then discharged to 1.5V with a constant current of 0.33C. This is considered the battery's first charge / discharge cycle, and the discharge capacity from this cycle is denoted as the battery's first cycle discharge capacity (C0). The above steps are repeated for the same battery, and the discharge capacity after 500 cycles (C1) and the capacity retention rate after 500 cycles are calculated as C1 / C0 × 100%. The test process for comparative examples and other examples is the same as above.
[0160] III. Analysis of Test Results for Each Example and Comparative Example Batteries for each example and comparative example were manufactured according to the method described above. The battery parameter tables are shown in Tables 1 and 2 below, and each performance parameter was measured. The results are shown in Table 3 below.
[0161] [Table 1-1] [Table 1-2] [Table 1-3] [Table 1-4] [Table 1-5] [Table 1-6]
[0162] [Table 2-1] [Table 2-2]
[0163] [Table 3-1] [Table 3-2]
[0164] The electrolytes in Examples 1 to 33 all contained a first additive, a second additive, and a third additive. The first additive contained a compound with the structure shown in formula I-013, a compound with the structure shown in formula I-014, a compound with the structure shown in formula I-019, or a compound with the structure shown in formula I-022. The second additive contained sodium difluoro(oxalato)borate, lithium difluoro(oxalato)borate, magnesium difluoro(oxalato)borate, or aluminum difluoro(oxalato)borate. The third additive contained a compound with the structure shown in formula III-1, a compound with the structure shown in formula III-2, a compound with the structure shown in formula III-3, or a compound with the structure shown in formula III-9. The sodium secondary batteries containing this electrolyte all exhibited excellent storage performance, cycle performance, and rapid charging performance, as well as a relatively low SEI film dissolution rate.
[0165] As can be seen from the comparison between Examples 1 to 23 and Comparative Example 1, the electrolyte containing the first additive, the second additive, and the third additive is advantageous in reducing the volume expansion rate of the sodium secondary battery after high-temperature storage, the DC impedance of the sodium secondary battery, and the dissolution rate of the SEI film, thereby improving the charging performance and cycle capacity maintenance rate of the sodium secondary battery.
[0166] As can be seen from the comparison between Examples 1, 7-14 and Comparative Example 2, Examples 1-5, 11-14 and Comparative Example 3, and Examples 1-10 and Comparative Example 4, compared to electrolytes containing a first additive, a second additive, or a third additive, the electrolyte in this application contains a first additive, a second additive, and a third additive simultaneously, which is advantageous in reducing the volume expansion rate of the sodium secondary battery after high-temperature storage, the DC impedance of the sodium secondary battery, and the dissolution rate of the SEI film, thereby improving the charging performance and cycle capacity maintenance rate of the sodium secondary battery.
[0167] As can be seen from the comparison between Examples 1, 11-14 and Comparative Example 5, Examples 1, 7-10 and Comparative Example 6, and Examples 1-5 and Comparative Example 7, while the electrolyte in the present application contains at least two of the first, second, and third additives, the electrolyte in the present application contains the first, second, and third additives simultaneously, enabling a balance between the charging performance and cycling performance of the sodium secondary battery.
[0168] As can be seen from the comparison between Examples 1, 15-23 and Comparative Examples 8-9, this application simultaneously contains a compound with the structure shown in formula I-1 or formula I-2 as a first additive, a difluoro(oxalato)borate as a second additive, and a fluorocarbonate compound as a third additive, which is advantageous in reducing the volume expansion rate of sodium secondary batteries after high-temperature storage, the DC impedance of sodium secondary batteries, and the dissolution rate of the SEI film, thereby improving the charging performance and cycle capacity maintenance rate of the sodium secondary batteries.
[0169] As can be seen from Examples 1 to 10, by controlling the mass ratio of the first additive to the second additive to 0.01 to 500, the sodium secondary battery was given a relatively low volume expansion rate after high-temperature storage, DC impedance and SEI film dissolution rate, and excellent charging and cycling performance. As can be seen from a comparison of Examples 1, 3 to 5, 7 to 10 with Examples 2 and 6, further controlling the mass ratio of the first additive to the second additive to 0.1 to 100 is advantageous for further reducing the volume expansion rate of the sodium secondary battery after high-temperature storage.
[0170] As can be seen from Examples 1 to 5, by controlling the mass content of the compound with the structure shown in formula I-019 of the first additive to 0.01% to 5% based on the total mass of the electrolyte, the sodium secondary battery was given a relatively low volume expansion coefficient after high-temperature storage, DC impedance and SEI film solvent rate, and excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 3 to 4 and Examples 2 and 5, by further controlling the mass content of the compound with the structure shown in formula I-019 of the first additive to 0.1% to 2% based on the total mass of the electrolyte, the DC impedance of the sodium secondary battery can be further reduced, which is advantageous in improving the charging performance of the sodium secondary battery.
[0171] As can be seen from Examples 1, 7-10, by controlling the mass content of the second additive, sodium difluoro(oxalato)borate, to 0.01%-5% based on the total mass of the electrolyte, the sodium secondary battery was given a relatively low volume expansion rate after high-temperature storage, DC impedance, SEI film dissolution rate, and excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 7-8 and Examples 9-10, by further controlling the mass content of the second additive, sodium difluoro(oxalato)borate, to 0.1%-2% based on the total mass of the electrolyte, the DC impedance of the sodium secondary battery is further reduced, which is advantageous in improving the charging performance of the sodium secondary battery.
[0172] As can be seen from Examples 1, 11-14, by controlling the mass content of the compound with the structure shown in formula III-1 of the third additive to 0.01%-5% based on the total mass of the electrolyte, the sodium secondary battery was given a relatively low volume expansion coefficient after high-temperature storage, DC impedance and SEI film solvent rate, and excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 12-13 and Examples 11 and 14, further controlling the mass content of the compound with the structure shown in formula III-1 of the third additive to 0.1%-2% based on the total mass of the electrolyte is advantageous in further reducing the DC impedance of the sodium secondary battery and improving its charging performance.
[0173] As can be seen from Examples 1, 15-23, the first additive includes a compound with the structure shown in formula I-013, a compound with the structure shown in formula I-014, a compound with the structure shown in formula I-019, or a compound with the structure shown in formula I-022; the second additive includes sodium difluoro(oxalato)borate, lithium difluoro(oxalato)borate, magnesium difluoro(oxalato)borate, or aluminum difluoro(oxalato)borate; and the third additive includes a compound with the structure shown in formula III-1, a compound with the structure shown in formula III-2, a compound with the structure shown in formula III-3, or a compound with the structure shown in formula III-9. All of these were able to give the sodium secondary battery a relatively low volume expansion coefficient and DC impedance after high-temperature storage, as well as excellent charging and cycling performance.
[0174] As can be seen from a comparison between Examples 1, 24-27 and Example 28, controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Ca element in the negative electrode material layer to 1 or more is advantageous in reducing the volume expansion rate and the dissolution rate of the SEI film of the sodium secondary battery after high-temperature storage, thereby improving the cycle capacity maintenance rate of the sodium secondary battery.
[0175] As can be seen from Examples 1, 24-27, by controlling the mass content of Ca element in the negative electrode material layer to 50 ppm to 3000 ppm, the sodium secondary battery was given a relatively low volume expansion rate after high-temperature storage, DC impedance and SEI film dissolution rate, and excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 24-25 and Example 26, further controlling the mass content of Ca element in the negative electrode material layer to 50 ppm to 1000 ppm is advantageous in further reducing the volume expansion rate, DC impedance and SEI film dissolution rate of the sodium secondary battery after high-temperature storage, thereby improving the charging performance and cycle capacity maintenance rate of the sodium secondary battery.
[0176] As can be seen from the comparison between Examples 1, 30-33 and Example 29, introducing Cu elements into the positive electrode active material is advantageous for improving the cycle performance of sodium secondary batteries.
[0177] As can be seen from Examples 1, 30-33, by controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Cu element in the positive electrode active material to 0.004 or higher, the sodium secondary battery was given a relatively low volume expansion coefficient after high-temperature storage, DC impedance and SEI film dissolution rate, and excellent charging and cycling performance.
[0178] As can be seen from Examples 3, 30-33, by controlling the mass content of Cu element in the positive electrode active material to 23% or less, the sodium secondary battery was given a relatively low volume expansion rate after high-temperature storage, DC impedance and SEI film dissolution rate, and excellent charging and cycling performance. As can be seen from the comparison between Examples 1, 30-31 and Example 32, further controlling the mass content of Cu element in the positive electrode active material to 6.5%-18% is advantageous in further reducing the volume expansion rate, DC impedance and SEI film dissolution rate of the sodium secondary battery after high-temperature storage, thereby improving the charging performance of the sodium secondary battery.
[0179] It should be noted that this application is not limited to the embodiments described above. The embodiments described above are merely illustrative, and any embodiments that have substantially the same configuration as the technical idea and produce the same effects within the scope of the technical proposal of this application are included within the scope of the technical proposal. Furthermore, other methods that are constructed by adding various modifications to the embodiments that a person skilled in the art could conceive of, and by combining some of the components of the embodiments, are also included within the scope of this application, without departing from the spirit of this application. [Explanation of Symbols]
[0180] 1. Battery pack, 2. Upper casing, 3. Lower casing, 4. Battery module, 5. Sodium secondary battery, 5. Case, 5. Electrode assembly, 5. Cover plate.
Claims
1. An electrolyte for a sodium secondary battery, comprising a first additive, a second additive, and a third additive, wherein the first additive comprises a cyclic ester compound containing a sulfate group and / or a sulfite group, the second additive comprises a difluoro(oxalato)borate, and the third additive comprises a fluorocyclic carbonate compound, and the cyclic ester compound containing a sulfate group and / or a sulfite group comprises at least one of a compound having the structure shown in formula I-1 and a compound having the structure shown in formula I-2. 【Chemistry 1】 In Equation I-1, R 1 teeth, 【Chemistry 2】 Includes R 2 , R 3 Each of them operates independently. 【Transformation 3】 , comprising at least one of a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group, and R 2 , R 3 At least one of them is 【Chemistry 4】 Includes R 4 teeth, 【Transformation 5】 It includes at least one of the following, R 5 , R 6 Each of them operates independently. 【Transformation 6】 It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group. In Formula I-2, R 7 is 【Transformation 7】 Includes R 8 teeth, 【Transformation 8】 It includes at least one of the following, R 9 C, 【Chemistry 9】 It includes at least one of the following, R 14 It comprises at least one of a single bond, a C1-C6 alkyl group, a C1-C6 ether group, and a C1-C3 alkoxy group, R 10 , R 11 , R 12 , R 13 Each of these is an electrolyte for a sodium secondary battery, each independently containing at least one of a single bond or a C1-C3 olefin group.
2. The aforementioned difluoro(oxalato)borate contains the compound shown in formula II, (F) 2 C 2 O 4 B) y M y+ Formula II In Equation II, M y+ Li + Na + _K + , Rb + , Cs + Mg 2+ Ca 2+ Ba 2+ Fe 2+ Ni 2+ Al 3+ Fe 3+ Ni 3+ It includes one or more of the following, where y = 1, 2, or 3, and / or The fluorocyclic carbonate compound includes a compound having the structure shown in formula III. 【Chemistry 10】 In Equation III, R 15 , R 16 , R 17 , R 18 Each independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an isocyanate group, an ester group, a cyano group, or a sulfonic acid group, and R 15 , R 16 , R 17 , R 18 The electrolyte according to claim 1, wherein at least one of the atoms contains an F atom.
3. In Equation I-1, R 1 teeth, 【Chemistry 11】 Includes R 2 , R 3 Each of them operates independently. 【Chemistry 12】 , containing at least one of a hydrogen atom, a C1-C6 alkyl group, and a halogen atom, and R 2 , R 3 At least one of them is 【Chemistry 13】 Includes R 4 teeth, 【Chemistry 14】 It includes at least one of the following, R 5 , R 6 Each independently comprises at least one of a hydrogen atom, a C1-C6 alkyl group, and / or a halogen atom. In Equation I-2, R 7 teeth, 【Chemistry 15】 Includes R 8 teeth, 【Chemistry 16】 It includes at least one of the following, R 9 C, 【Chemistry 17】 It includes at least one of the following, R 14 It contains at least one of a single bond, a C1-C6 alkyl group, or a C1-C6 ether group, R 10 , R 11 , R 12 , R 13 The electrolyte according to claim 1, wherein each independently comprises at least one of a single bond and a C1-C3 olefin group.
4. The cyclic ester compounds containing the aforementioned sulfate group and / or sulfite group are, [Chemistry 18] 【Chemistry 19】 The electrolyte according to claim 1, comprising at least one of the following.
5. The cyclic ester compounds containing the aforementioned sulfate group and / or sulfite group are, 【Chemistry 20】 The electrolyte according to claim 1, comprising at least one of the following.
6. In Equation II, M y+ Li + Na + The electrolyte according to claim 2, comprising at least one of the following.
7. In Equation III, R 15 , R 16 , R 17 , R 18 Each independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, or an isocyanate group, and R 15 , R 16 , R 17 , R 18 The electrolyte according to claim 2, wherein at least one of the atoms contains an F atom.
8. The structure shown in formula III above is, 【Chemistry 21】 The electrolyte according to claim 2, comprising at least one of the following.
9. The structure shown in formula III above is, 【Chemistry 22】 、 、 The electrolyte according to claim 2, comprising at least one of the following.
10. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the difluoro(oxalato)borate is 0.01 to 500.
11. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the difluoro(oxalato)borate is 0.1 to 100 or 1 to 100.
12. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the fluorocyclic carbonate compound is 0.01 to 100.
13. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the fluorocyclic carbonate compound is 0.1 to 50 or 1 to 50.
14. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the difluoro(oxalato)borate to the fluorocyclic carbonate compound is 0.01 to 100.
15. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the difluoro(oxalato)borate to the fluorocyclic carbonate compound is 0.1 to 50 or 1 to 50.
16. Based on the total mass of the electrolyte, the ratio between the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups, the mass content B of the difluoro(oxalato)borate, and the mass content C of the fluorocyclic carbonate compound is 0.01 ≤ (A × B) / C 2 The electrolyte according to any one of claims 1 to 9, satisfying ≤ 10000.
17. Based on the total mass of the electrolyte, the ratio between the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups, the mass content B of the difluoro(oxalato)borate, and the mass content C of the fluorocyclic carbonate compound is 0.05 ≤ (A × B) / C 2 The electrolyte according to any one of claims 1 to 9, satisfying ≤ 100.
18. The electrolyte according to any one of claims 1 to 9, wherein the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups is 0.01% to 5% based on the total mass of the electrolyte.
19. The electrolyte according to any one of claims 1 to 9, wherein the mass content A of the cyclic ester compound containing sulfate and / or sulfite groups is 0.1% to 2% based on the total mass of the electrolyte.
20. The electrolyte according to any one of claims 1 to 9, wherein the mass content B of the difluoro(oxalato)borate is 0.01% to 5% based on the total mass of the electrolyte.
21. The electrolyte according to any one of claims 1 to 9, wherein the mass content B of the difluoro(oxalato)borate is 0.1% to 2% based on the total mass of the electrolyte.
22. The electrolyte according to any one of claims 1 to 9, wherein the mass content C of the fluorocyclic carbonate compound is 0.01% to 5% based on the total mass of the electrolyte.
23. The electrolyte according to any one of claims 1 to 9, wherein the mass content C of the fluorocyclic carbonate compound is 0.1% to 2% based on the total mass of the electrolyte.
24. A sodium secondary battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte according to any one of claims 1 to 23.
25. The sodium secondary battery according to claim 24, wherein the positive electrode plate includes a positive electrode current collector and a positive electrode material layer located on at least one side of the positive electrode current collector, the positive electrode material layer includes a positive electrode active material, and the positive electrode active material includes at least one of a layered transition metal oxide, a Prussian blue compound, and a polyanion compound.
26. The general formula for the aforementioned layered transition metal oxide is Na x Mn a Fe b Ni c M d N e O 2-δ Q f The sodium secondary battery according to claim 25, wherein M includes at least one of Ti, Li, V, Cr, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, Mg, Al, N includes at least one of Si, P, B, S, Se, Q includes at least one of F, Cl, N, and 0.66 ≤ x ≤ 1, 0 < a ≤ 0.7, 0 < b ≤ 0.7, 0 ≤ c ≤ 0.23, 0 ≤ d < 0.3, 0 ≤ e ≤ 0.3, 0 ≤ f ≤ 0.3, 0 ≤ δ ≤ 0.3, a + b + c + d + e = 1, 0 < e + f ≤ 0.3, 0 < (e + f) / a ≤ 0.3, 0.2 ≤ d + e + f ≤ 0.3, (b + c) / a ≤ 1.
5.
27. The positive electrode active material includes a layered transition metal oxide containing Cu element, The sodium secondary battery according to claim 25 or 26, wherein the ratio of the mass content of the cyclic ester compound containing sulfate and / or sulfite groups in the electrolyte to the mass content of Cu element in the positive electrode active material is 0.002 or more, and the mass content of Cu element is based on the total mass of the positive electrode active material.
28. The sodium secondary battery according to claim 27, wherein the mass content of Cu element in the positive electrode active material is 23% or less, based on the total mass of the positive electrode active material.
29. The sodium secondary battery according to claim 27, wherein the mass content of Cu element in the positive electrode active material is 5% to 20% based on the total mass of the positive electrode active material.
30. The negative electrode plate includes a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, and the negative electrode material layer includes the element Ca. The sodium secondary battery according to any one of claims 24 to 26, 28 to 29, wherein the ratio of the mass content of the cyclic ester compound containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is 1 or more, and the mass content of Ca element is based on the total mass of the negative electrode material layer.
31. The sodium secondary battery according to claim 30, wherein the mass content of Ca element in the negative electrode material layer is 1 ppm to 3000 ppm, based on the total mass of the negative electrode material layer.
32. The sodium secondary battery according to claim 30, wherein the mass content of element Ca in the negative electrode material layer is 50 ppm to 1000 ppm or 100 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.
33. The sodium secondary battery according to claim 30, wherein the negative electrode material layer further comprises a negative electrode active material, and the negative electrode active material comprises one or more of hard carbon, tin alloy, and metal oxide.
34. A power consumption device comprising a sodium secondary battery according to any one of claims 24 to 33.