Electrolytes, sodium secondary batteries, and power consumption devices

The electrolyte with specific additives forms stable films in sodium secondary batteries, addressing gas generation issues and improving performance by reducing gas production and enhancing storage and cycling capabilities.

JP2026539214APending Publication Date: 2026-11-20CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026527395
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-09
Filing Date
2024-09-19
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Sodium-based secondary batteries suffer from gas generation issues that affect their electrical performance, preventing them from meeting the requirements of next-generation electrochemical systems.

Method used

An electrolyte comprising a cyclic ester compound with sulfate or sulfite groups, difluoro(oxalato)borate, and a sultone compound with a carbon-carbon double bond is introduced to form stable SEI and CEI films, reducing gas generation and enhancing the performance of sodium secondary batteries.

Benefits of technology

The electrolyte significantly reduces gas generation and improves storage, rapid charging, and cycling performance by stabilizing the SEI and CEI films, thereby enhancing the overall performance of sodium secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539214000001_ABST
    Figure 2026539214000001_ABST
Patent Text Reader

Abstract

This invention relates to an electrolyte, a sodium secondary battery, and a power consumption device. The electrolyte contains a first additive, a second additive, and a third additive. The first additive contains a cyclic ester compound containing a sulfate group and / or a sulfite group. The second additive contains difluoro(oxalato)borate. The third additive contains a sultone compound containing a carbon-carbon double bond. When the first, second, and third additives are used in combination, the stability of the SEI film can be effectively enhanced, a stable CEI film can be formed, the amount of gas generated during the cycling and storage of the sodium secondary battery can be significantly reduced, and the storage performance, rapid charging performance, and cycling performance of the sodium secondary battery can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Cross-reference of related applications This application claims priority to Chinese patent application No. 202311486877.1, filed on 9 November 2023, entitled “Electrolyte, Sodium Secondary Battery and Power Consumption Device,” all of which are incorporated herein by reference.

[0002] This application relates to the field of sodium battery technology, and more particularly to electrolytes, sodium secondary batteries, and power consumption devices. [Background technology]

[0003] In recent years, secondary batteries have been widely applied in various fields, including energy storage and power systems such as hydroelectric, thermal, wind, and solar power plants, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, and aerospace.

[0004] Compared to lithium-ion batteries, sodium-based batteries have a greater competitive advantage due to their abundant and widely distributed sodium resources. However, sodium-based batteries suffer from a gas generation problem, which seriously impacts their electrical performance and prevents them from meeting the application requirements of next-generation electrochemical systems. [Overview of the Initiative]

[0005] This application was made in view of the above-mentioned problems, and its purpose is to provide an electrolyte that effectively enhances the stability of the SEI film and the formation of the CEI film, significantly reduces the degree of gas generation during the cycling and storage of sodium secondary batteries, and further enhances the storage performance, rapid charging performance, and cycling performance of sodium secondary batteries.

[0006] A first aspect of this application provides an electrolyte for a sodium secondary battery, the electrolyte comprising a first additive, a second additive, and a third additive, wherein the first additive comprises a cyclic ester compound containing a sulfate group and / or a sulfite group, the second additive comprises a difluoro(oxalato)borate, and the third additive comprises a sultone compound containing a carbon-carbon double bond.

[0007] A first additive containing a cyclic ester compound containing sulfate and / or sulfite groups and a second additive containing difluoro(oxalato)borate are preferentially reduced at the negative electrode over the solvent to form a film, generating components containing sulfate and / or sulfite groups and other components containing borate in the SEI film. The cooperative use of both enhances the overall stability of the interfacial SEI film, reduces the degree of oxidation and gas generation during the discharge process of the SEI film, and also reduces the degree of dissolution of the entire interfacial SEI film in the electrolyte to some extent, preventing exposure of the negative electrode plate due to dissolution of the SEI film in the electrolyte. This also reduces the degree to which gas is generated by the reaction between the solvent and the negative electrode plate. Furthermore, by introducing a third additive containing a sultone compound containing a carbon-carbon double bond into the electrolyte, the sultone compound containing the carbon-carbon double bond preferentially undergoes an oxidative polymerization reaction on the surface of the positive electrode plate, forming a CEI film containing a sulfur-containing polymer that covers the surface of the positive electrode plate and inhibits direct contact between the positive electrode plate and the electrolyte. Thus, the degree to which gas is generated by side reactions between the solvent and the positive electrode plate in the electrolyte can be reduced, while RH generated by the catalytic oxidation of the transition metal in the layered transition metal oxide can be reduced. + This reduces the extent to which the material moves to the negative electrode side and accumulates on the negative electrode side, causing side reactions with the negative electrode, further reducing gas generation on the negative electrode side, and comprehensively improving the storage performance, rapid charging performance, and cycle performance of the sodium secondary battery.

[0008] In any embodiment, the cyclic ester compound containing the sulfate group and / or sulfite group comprises at least one of the compound having the structure shown in formula I-1 and the compound having the structure shown in formula I-2. [ka] In equation I-1, R1 is [ka] R2 and R3 are independent of each other. [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each include at least one of the following, [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group. In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R14 includes at least one of a single bond, a C1-C6 alkyl group, a C1-C6 ether group, and a C1-C3 alkoxy group, R 10 , R 11 , R 12 , R 13 each independently include at least one of a single bond and a C1-C3 alkylene group.

[0009] The cyclic ester compound containing a sulfate group and / or a sulfite group described above can generate a component containing a sulfate group and / or a sulfite group in the SEI film, and the SEI film containing this component covers the surface of the negative electrode plate, reduces the extent to which the negative electrode plate is exposed to the electrolyte, reduces side reactions and gas generation, and can improve the performance of the sodium secondary battery.

[0010] In any embodiment, the difluoro(oxalato)borate includes the compound represented by Formula II, (F2C2O4B) y M y+ Formula II, In Formula II, M y+ is Li + , Na + , K + , Rb + , Cs + , Mg 2+ , Ca 2+ , Ba 2+ , Fe 2+ , Ni 2+ , Al 3+ , Fe 3+ , Ni 3+ includes one or more of them, and y=1, 2 or 3.

[0011] All the above-mentioned difluoro(oxalato)borates can generate other borate-containing components in the SEI film, improve the stability of the entire SEI film on the surface of the negative electrode plate, reduce the degree of oxidative decomposition of the entire SEI film, and to a certain extent reduce the solubility of the entire SEI film in the electrolyte solvent, thereby improving the storage performance of the sodium secondary battery.

[0012] In any embodiment, the sultone compound containing the carbon-carbon double bond includes a compound having the structure shown in Formula III, [ka] In Equation III, R 15 It contains at least one of an alkylene group, an alkoxy group, a carbonyl group, or a haloalkylene group, R 16 , R 17 Each of these groups independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a phenyl group, an amino group, an amine group, a silyl group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group.

[0013] The above sultone compounds containing carbon-carbon double bonds all form a CEI film of sulfur-containing polymer on the positive electrode side, covering the surface of the positive electrode and inhibiting direct contact between the positive electrode and the electrolyte. This reduces the degree of gas generation due to side reactions between the solvent in the electrolyte and the positive electrode, while simultaneously reducing RH generated by the catalytic oxidation of the transition metal in layered transition metal oxides. + This reduces the extent to which the material moves to the negative electrode side and accumulates on the negative electrode side, causing side reactions with the negative electrode. It also reduces gas generation on both the positive and negative electrode sides, thereby comprehensively improving the storage and cycling performance of the sodium secondary battery.

[0014] In either embodiment, in formula I-1, R1 is [ka] R2 and R3 are independent of each other. [ka] It contains at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each independently contain at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and / or In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R 14 It contains at least one of a single bond, a C1-C6 alkyl group, or a C1-C6 ether group, R 10 , R 11 , R 12 , R 13 Each of these independently contains at least one of the following: a single bond or a C1-C3 alkylene group.

[0015] In any embodiment, the cyclic ester compound containing the sulfate group and / or sulfite group is [ka] [ka] It includes at least one of the following, and optionally, [ka] It includes at least one of the following.

[0016] The above substances, as primary additives, are all soluble in the electrolyte and form a dense SEI film during the charging process, covering the surface of the negative electrode plate and reducing the degree to which the negative electrode plate is exposed to the electrolyte, thereby reducing side reactions and gas generation, and improving the performance of the sodium secondary battery. [ka] Compared to the compound with the structure shown, the other compounds have a more stable structure, resulting in superior cycle performance for sodium secondary batteries.

[0017] In any embodiment, in formula II, M y+ Li + kaNa + It includes at least one of the following.

[0018] Li + or Na + Because it has a smaller ionic radius, it can provide higher solubility to sodium difluoro(oxalato)borate or lithium difluoro(oxalato)borate, and further reduce the impact of the introduction of the second additive on the electrolyte conductivity.

[0019] In either embodiment, in formula III, R 15 It contains at least one of an alkylene group, a carbonyl group, or a haloalkylene group, R 16 , R 17 Each of these groups independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 alkoxy group, a phenyl group, an amino group, or a silyl group.

[0020] In any of the embodiments, the structure shown in formula III is [ka] It includes at least one of the following.

[0021] The above-mentioned sultone compounds containing carbon-carbon double bonds are all soluble in the electrolyte, and their introduction as additives reduces the effect on the ionic conductivity of the electrolyte.

[0022] In any embodiment, the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the difluoro(oxalato)borate is 0.2 to 500, and selectively 1 to 100.

[0023] By controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate within an appropriate range, it is possible to reduce the degree of intensified gas generation due to the intensified oxidative decomposition of the entire SEI film. Furthermore, it is possible to reduce the damage to the SEI film during the cycling process, which is caused by the relatively poor toughness of the entire SEI film and can further seriously affect the cycling performance. An appropriate ratio range allows for a balance between the storage performance and cycling performance of sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries. Moreover, controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate to 0.2 to 100 or 1 to 100 is advantageous for further balancing the storage performance and cycling performance of sodium secondary batteries.

[0024] In any embodiment, the sum of the mass content of the cyclic ester compound containing sulfate groups and / or sulfite groups and the sultone compound containing carbon-carbon double bonds, based on the total mass of the electrolyte, is 0.1% to 6%, and selectively 0.5% to 5%.

[0025] By controlling the sum of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups and sultone compounds containing carbon-carbon double bonds within an appropriate range, both storage performance and rapid charging performance of sodium secondary batteries can be achieved.

[0026] In any embodiment, the mass ratio of the difluoro(oxalato)borate to the sultone compound containing the carbon-carbon double bond is 0.01 to 100, and selectively 1 to 50.

[0027] By controlling the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond within an appropriate range, it is possible to reduce the impact on cycle performance due to the improvement of the limited solubility of the entire SEI film, as well as reduce the risk of sodium deposition caused by an excessively high proportion of the sultone compound containing a carbon-carbon double bond, thereby comprehensively improving the performance of the sodium secondary battery. Furthermore, controlling the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond to 0.1-50 or 1-50 is advantageous for further enhancing the cycle performance of the sodium secondary battery.

[0028] In any embodiment, the product of the mass content of the cyclic ester compound containing sulfate and / or sulfite groups, the difluoro(oxalato)borate, and the sultone compound containing a carbon-carbon double bond, based on the total mass of the electrolyte, is 0.005 × 10⁻⁶ ―6 ~10×10 ―6 Therefore, selectively, 0.01 × 10 ―6 ~5×10 ―6 That is the case.

[0029] By simultaneously controlling the product of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borate, and sultone compounds containing carbon-carbon double bonds within an appropriate range, it is possible to reduce the impact on the degree of gas generation caused by having too low a mass content of any one of the three additives, as well as reduce the impact on the DC impedance and rapid charging performance of the sodium secondary battery caused by having too high a mass content of any one of the three additives, thereby comprehensively improving the performance of the sodium secondary battery.

[0030] In any of the embodiments, the mass content of the cyclic ester compound containing sulfate and / or sulfite groups is 0.01% to 5%, and selectively 0.1% to 3%, based on the total mass of the electrolyte.

[0031] By controlling the mass content of cyclic ester compounds containing sulfate and / or sulfite groups within an appropriate range, components containing sulfate and / or sulfite groups are formed in the SEI film, reducing the degree of overall SEI film rupture due to expansion of the sodium secondary battery during the cycle use process, further enhancing the overall protective capacity of the SEI film, and thus improving the storage performance of the sodium secondary battery. Furthermore, it is possible to reduce the degree to which excessive cyclic ester compounds are oxidized and decomposed on the positive electrode side, intensifying gas generation, and the degree to which the oxidative decomposition products accumulate on the surface of the positive electrode, increasing the interfacial resistance of the positive electrode and intensifying the deterioration of the sodium secondary battery's performance. Moreover, by controlling the mass content of cyclic ester compounds to 0.1% to 2%, it is advantageous to balance the storage performance and rapid charging performance of the sodium secondary battery, thereby comprehensively improving the performance of the sodium secondary battery.

[0032] In any of the embodiments, the mass content of the difluoro(oxalato)borate is 0.01% to 5%, and selectively 0.1% to 2%, based on the total mass of the electrolyte.

[0033] By controlling the mass content of difluoro(oxalato)borate within an appropriate range, a borate-containing component is formed in the SEI film, effectively increasing the overall stability of the interfacial SEI film, reducing the degree of gas generation, and thus advantageous for improving the cycle performance and storage performance of sodium secondary batteries. Furthermore, excessively high mass content of difluoro(oxalato)borate can lead to oxidative decomposition of the difluoro(oxalato)borate on the positive electrode side, intensifying gas generation and affecting storage performance. This is achieved by balancing the cycle performance and storage performance of sodium secondary batteries. Moreover, by controlling the mass content of difluoro(oxalato)borate to 0.1% to 2%, it is advantageous for balancing the storage performance and rapid charging performance of sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries.

[0034] In any of the embodiments, the mass content of the sultone compound containing the carbon-carbon double bond is 0.01% to 5%, and selectively 0.1% to 2%, based on the total mass of the electrolyte.

[0035] By controlling the mass content of sultone compounds containing carbon-carbon double bonds within an appropriate range, a sufficient CEI film is formed, direct contact between the positive electrode and the electrolyte is inhibited, reducing oxidation and gas generation on the positive electrode side, and RH + This not only suppresses the generation of sodium deposits and is advantageous for improving the storage and cycle performance of sodium secondary batteries, but also reduces the risk of sodium deposition by increasing the interfacial impedance on the negative electrode side, as sultone compounds containing excess carbon-carbon double bonds are involved in the formation of the SEI film on the negative electrode side, thereby improving the overall performance of sodium secondary batteries.

[0036] A second aspect of this application provides a sodium secondary battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte according to the first aspect of this application.

[0037] In any embodiment, the positive electrode plate includes a positive electrode current collector and a positive electrode material layer located on at least one side of the positive electrode current collector, the positive electrode material layer further includes a positive electrode active material, and the positive electrode active material includes a layered transition metal oxide.

[0038] In any embodiment, the layered transition metal oxide is Na a M b Fe c It contains O2, and M contains at least one of Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, and 0.67 <a<1.1、0.5<b<1、0<c<0.5である。

[0039] Layered transition metal oxide cathode active materials offer advantages at high voltages.

[0040] In any embodiment, the positive electrode material layer includes a layered transition metal oxide containing Cu element, The ratio of the mass content of the sultone compound containing the carbon-carbon double bond in the electrolyte to the mass content of the Cu element in the positive electrode active material is 0.002 or more, and the mass content of the Cu element is based on the total mass of the positive electrode active material.

[0041] Introducing Cu into the positive electrode material layer is advantageous for the stability of the positive electrode active material structure. Furthermore, by controlling the ratio of the mass content of cyclic ester compounds in the electrolyte to the mass content of Cu in the positive electrode active material within an appropriate range, the degree to which gas generation intensifies due to oxidative decomposition of the electrolyte on the positive electrode plate side can be effectively reduced.

[0042] In any of the embodiments, the mass content of Cu element in the positive electrode active material is 23% or less, and selectively 5% to 20%, based on the total mass of the positive electrode active material.

[0043] By controlling the mass content of Cu in the positive electrode active material within an appropriate range, it is advantageous not only to provide sufficient Cu and increase the stability of the positive electrode active material structure, but also to reduce the degree to which excessively high Cu mass content in the positive electrode material layer worsens the oxidative decomposition of the electrolyte and degrades the performance of sodium secondary batteries. Furthermore, controlling the mass content of Cu in the positive electrode active material to 5% to 20% is advantageous for further balancing the storage performance and rapid charging performance of sodium secondary batteries.

[0044] In any embodiment, the negative electrode plate includes a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, and the negative electrode material layer includes the element Ca. The ratio of the mass content of the cyclic ester compound containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is 1 or more, and the mass content of Ca element is based on the total mass of the negative electrode material layer.

[0045] Introducing Ca element into the negative electrode active material is advantageous in reducing the degree of sodium dendrite formation, and also advantageous in forming an SEI film containing organocalcium salt components between the negative electrode active material and cyclic ester compounds containing sulfate and / or sulfite groups, further advantageous in increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. By controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Ca element in the negative electrode material layer within an appropriate range, both the storage performance and rapid charging performance of the sodium secondary battery can be achieved.

[0046] In any embodiment, the mass content of Ca element in the negative electrode material layer is 1 ppm to 3000 ppm, with respect to the total mass of the negative electrode material layer, and is selectively 50 ppm to 1000 ppm or 100 ppm to 1000 ppm.

[0047] By controlling the mass content of Ca element in the negative electrode material layer to an appropriate range, it is possible to form an SEI film that sufficiently contains organic calcium salt components, thereby increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. Furthermore, it is possible to reduce the risk of manufacturing failure of the negative electrode plate due to the gelation phenomenon of the slurry during the manufacturing process caused by an excessively high mass content of Ca element in the negative electrode material layer, the degree of reduction in the initial Coulomb efficiency and the degree of intensification of gas generation due to the formation of Ca(OH)2 during the manufacturing process, or the degree of deterioration of the sodium secondary battery performance due to the increase in the DC impedance of the sodium secondary battery, thereby achieving both the storage performance and rapid charging performance of the sodium secondary battery. Moreover, controlling the mass content of Ca element in the negative electrode material layer to 50 ppm to 1000 ppm or 100 ppm to 1000 ppm is advantageous for further comprehensively improving the storage performance and rapid charging performance of the sodium secondary battery.

[0048] In any embodiment, the negative electrode material layer further comprises a negative electrode active material, the negative electrode active material comprising one or more of hard carbon, tin alloy, and metal oxide.

[0049] A third aspect of this application provides a power consumption device including a sodium secondary battery according to the second aspect of this application. [Brief explanation of the drawing]

[0050] [Figure 1] This is a schematic diagram of a sodium secondary battery according to one embodiment of the present application. [Figure 2] Figure 1 is an exploded view of a sodium secondary battery according to one embodiment of this application. [Figure 3] This is a schematic diagram of a battery module according to one embodiment of the present application. [Figure 4] This is a schematic diagram of a battery pack according to one embodiment of the present application. [Figure 5] Figure 4 is an exploded view of a battery pack according to one embodiment of this application. [Figure 6]This is a schematic diagram of a power consumption device that uses a sodium secondary battery as a power source according to one embodiment of this application. [Modes for carrying out the invention]

[0051] The following describes in detail embodiments of the electrolyte, sodium secondary battery, and power consumption device of this application, with appropriate reference to the drawings. However, unnecessary detailed explanations may be omitted. For example, detailed explanations of well-known matters and redundant explanations of structures that are actually the same may be omitted. This is to avoid making the following explanation unnecessarily long and to make it easily understandable to those skilled in the art. The drawings and the following explanation are provided to enable those skilled in the art to fully understand this application and do not limit the topics described in the claims.

[0052] The “range” disclosed in this application is limited in the form of a lower limit and an upper limit, and a given range is limited by selecting one lower limit and one upper limit, which define the boundary of a particular range. The range thus limited may or may not include the endpoints, and any combination is possible, that is, any lower limit can be combined with any upper limit to form a range. For example, if the ranges 60-120 and 80-110 are listed for a particular parameter, it is understood that the ranges 60-110 and 80-120 can also be assumed. Furthermore, if the minimum range values ​​are listed as 1 and 2, and the maximum range values ​​are listed as 3, 4 and 5, then the ranges 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 can all be assumed. In this application, unless otherwise specified, the numerical range “a-b” represents an abbreviated expression for any combination of real numbers a-b, where a and b are both real numbers. For example, the numerical range "0 to 5" indicates that all real numbers between "0 to 5" have already been listed in this specification, and "0 to 5" is simply an abbreviated representation of combinations of these numbers. Also, when a parameter is described as an integer ≥ 2, it is equivalent to disclosing that this parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0053] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical inventions.

[0054] Unless otherwise specified, all technical features and optional technical features of this application can be combined to form new technical concepts.

[0055] Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, the fact that the method includes steps (a) and (b) means that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, the fact that the method referred to above may further include step (c) means that step (c) may be added to the method in any order, for example the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), and so on.

[0056] Unless otherwise specified, the terms “includes” and “inclusion” as used in this application may be open or closed. For example, “includes” and “inclusion” may mean that other components not listed may be included or inclusion, or that only the listed components may be included or inclusion.

[0057] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the conditions A is true (or exists) and B is false (or does not exist), the condition A is false (or does not exist) but B is true (or exists), and the condition both A and B are true (or exist) all satisfy "A or B."

[0058] Gas generation in sodium-ion batteries has a serious impact on their electrical performance, particularly at low voltages, where gas generation occurs on the negative electrode side. Generally, by introducing film-forming additives into the electrolyte, a Solid Electrolyte Interphase (SEI) film is formed on the surface of the negative electrode. The formation of the SEI film prevents further decomposition of the electrolyte and gas generation to some extent, further improving the performance of sodium-ion batteries. However, sodium-ion batteries still suffer from gas generation problems during cycle use and storage. Therefore, it is necessary to design electrolytes that meet the application requirements of next-generation electrochemical systems.

[0059] [Electrolyte] Based on this, this application proposes an electrolyte for a sodium secondary battery, the electrolyte comprising a first additive, a second additive, and a third additive, wherein the first additive comprises a cyclic ester compound containing a sulfate group and / or a sulfite group, the second additive comprises a difluoro(oxalato)borate, and the third additive comprises a sultone compound containing a carbon-carbon double bond.

[0060] In this specification, "difluoro(oxalato)borate" means an anion [ka] The cation is Li + kaNa + , K + , Rb + , Cs + Mg 2+ Ca 2+ Ba 2+ Fe 2+ Ni 2+ , Al 3+ Fe 3+ Ni 3+ A compound that contains one or more of the following, but is not limited to them.

[0061] In some embodiments, the cyclic ester compound containing a sulfate group and / or a sulfite group comprises at least one of the compounds having the structure shown in formula I-1 and the compounds having the structure shown in formula I-2. [ka] In equation I-1, R1 is [ka] R2 and R3 are independent of each other. [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each include at least one of the following, [ka] It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group. In equation I-2, R7 is [ka] R8 includes, [ka] R9 includes at least one of the following, and C, [ka] It includes at least one of the following, R 14 It includes at least one of a single bond, a C1-C6 alkyl group, a C1-C6 ether group, and a C1-C3 alkoxy group, R 10 , R 11 , R 12 , R 13 Each of these independently contains at least one of the following: a single bond or a C1-C3 alkylene group.

[0062] According to research, there are two reasons why sodium secondary batteries still generate significant gas during cycle use and storage at low voltages. Firstly, the negative electrode potential of sodium secondary batteries is 0.3V higher than that of lithium secondary batteries. The higher the potential, the more the film-forming additives can be driven to form an unstable SEI film mainly composed of several components. Such an unstable SEI film begins oxidative decomposition at 0.5V, generating a large amount of gas. Secondly, the solubility of the SEI film in the electrolyte of sodium secondary batteries is higher than that of the SEI film in lithium secondary batteries. The dissolution of the SEI film exposes the negative electrode plate to the electrolyte, causing a side reaction between the negative electrode plate and the electrolyte, generating a large amount of gas. Additionally, RH on the positive electrode side... + The generation of RH also leads to gas generation problems; for example, in positive electrode active materials containing layered transition metal oxides, the transition metal catalyzes the oxidation of the solvent in the electrolyte, + The anions on the positive electrode plate generate RH, or the high voltage oxidizes the electrolyte solvent. + It can generate RH + It moves from the positive electrode plate side to the negative electrode plate side and accumulates, RH + Li + Similarly, the product can pass through the SEI film and react with the negative electrode plate, forming a product that is not resistant to oxidation, thus exacerbating the gas generation problem on the negative electrode plate side.

[0063] To understand this, the first additive containing a cyclic ester compound with sulfate and / or sulfite groups and the second additive containing difluoro(oxalato)borate are preferentially reduced to the SEI film at the negative electrode rather than the solvent, generating components containing sulfate and / or sulfite groups and other components containing borate in the SEI film. The synergistic effect of both enhances the overall stability of the interfacial SEI film, reduces the degree of oxidation and gas generation during the discharge process of the SEI film, and also reduces the degree of dissolution of the interfacial SEI film in the electrolyte to some extent, thereby reducing the exposure of the negative electrode plate due to the dissolution of the SEI film and thus reducing the electrolysis. It is also possible to reduce the degree to which gas is generated by the reaction between the solvent and the negative electrode plate in the solution. Furthermore, by introducing a third additive containing a sultone compound containing a carbon-carbon double bond into the electrolyte, the sultone compound containing the carbon-carbon double bond preferentially undergoes an oxidative polymerization reaction on the surface of the positive electrode plate, forming a CEI film containing a sulfur-containing polymer that covers the surface of the positive electrode plate and inhibits direct contact between the positive electrode plate and the electrolyte. Thus, the degree to which gas is generated by side reactions between the solvent and the positive electrode plate in the electrolyte can be reduced, while RH generated by the catalytic oxidation of the transition metal in the layered transition metal oxide can be reduced. + The material moves to the negative electrode side, accumulating on the negative electrode side and reducing the degree to which it causes side reactions with the negative electrode, further reducing gas generation on the negative electrode side, and thus comprehensively improving the storage performance, rapid charging performance, and cycle performance of the sodium secondary battery.

[0064] In some embodiments, the difluoro(oxalato)borate comprises the compound shown in formula II, (F2C2O4B) y M y+ Formula II, In equation II, M y+ Li + kaNa + , K + , Rb + , Cs + Mg 2+ Ca 2+ Ba 2+ Fe 2+ Ni 2+, Al 3+ , Fe 3+ , Ni 3+ includes one or more of the above, and y is 1, 2 or 3.

[0065] In some embodiments, the difluoro(oxalato)borate salt comprises sodium difluoro(oxalato)borate. In some embodiments, the difluoro(oxalato)borate salt comprises lithium difluoro(oxalato)borate. In some embodiments, the difluoro(oxalato)borate salt comprises magnesium difluoro(oxalato)borate. In some embodiments, the difluoro(oxalato)borate salt comprises aluminum difluoro(oxalato)borate. In some embodiments, the difluoro(oxalato)borate salt comprises sodium difluoro(oxalato)borate and lithium difluoro(oxalato)borate.

[0066] Any of the above difluoro(oxalato)borate salts can generate other borate-containing components in the SEI film, which can improve the overall stability of the surface SEI film of the negative electrode plate, reduce the degree of oxidative decomposition of the entire SEI film, and reduce the solubility of the entire SEI film in the electrolyte solvent to a certain extent, thereby enhancing the storage performance of the sodium secondary battery.

[0067] In some embodiments, the sultone-based compound containing a carbon-carbon double bond includes a compound having the structure represented by Formula III, [Chemical Formula] In Formula III, R 15 includes at least one of an alkylene group, an alkoxy group, a carbonyl group, and a haloalkylene group, R 16 , R 17Each of these groups independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a phenyl group, an amino group, an amine group, a silyl group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group.

[0068] The above sultone compounds containing carbon-carbon double bonds all form a CEI film of sulfur-containing polymer on the positive electrode side, covering the surface of the positive electrode and inhibiting direct contact between the positive electrode and the electrolyte. This reduces the degree of gas generation due to side reactions between the solvent in the electrolyte and the positive electrode, while simultaneously reducing RH generated by the catalytic oxidation of the transition metal in layered transition metal oxides. + This reduces the extent to which the material moves to the negative electrode side and accumulates on the negative electrode side, causing side reactions with the negative electrode. It also reduces gas generation on both the positive and negative electrode sides, thereby comprehensively improving the storage and cycling performance of the sodium secondary battery.

[0069] In some embodiments, in formula I-1, R1 is [ka] R2 and R3 are independent of each other. [ka] It contains at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and at least one of R2 and R3 is [ka] R4 includes, [ka] R5 and R6 each independently contain at least one of a hydrogen atom, a C1-C6 alkyl group, or a halogen atom, and / or In equation I-2, R7 is

Chemical Formula

Chemical Formula

Chemical Formula

[0070] In some embodiments, the cyclic ester-based compound containing a sulfate group and / or a sulfite group is

Chemical Formula

Chemical Formula

[0071] In the present specification,

Chemical Formula

Chemical Formula

[0072] The above substances are all soluble in the electrolyte as primary additives. The SEI film formed during the charging process covers the surface of the negative electrode plate, reducing the degree to which the negative electrode plate is exposed to the electrolyte, thereby reducing side reactions and gas generation, and improving the performance of the sodium secondary battery. [ka] Compared to the compound with the structure shown, the other compounds have a more stable structure, resulting in superior cycle performance for sodium secondary batteries.

[0073] In some embodiments, in formula II, M y+ Li + kaNa + It includes at least one of the following. In some embodiments, in formula II, M y+ Li + This includes. In some embodiments, in formula II, M y+ is, Na + Includes.

[0074] Li + or Na + Because it has a smaller ionic radius, it can provide higher solubility to sodium difluoro(oxalato)borate or lithium difluoro(oxalato)borate, and further reduce the impact of the introduction of the second additive on the electrolyte conductivity.

[0075] In some embodiments, in Equation III, R 15 It contains at least one of an alkylene group, a carbonyl group, or a haloalkylene group, R 16 , R 17 Each of these groups independently contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 alkoxy group, a phenyl group, an amino group, or a silyl group.

[0076] In some embodiments, the structure shown in Equation III is, [ka] It includes at least one of the following.

[0077] The above-mentioned sultone compounds containing carbon-carbon double bonds are all soluble in the electrolyte, and their introduction as additives reduces the effect on the ionic conductivity of the electrolyte.

[0078] In some embodiments, the mass ratio of the cyclic ester compound containing a sulfate group and / or a sulfite group to the difluoro(oxalato)borate is 0.2 to 500, and selectively 1 to 100. In some embodiments, the mass ratio of the cyclic ester compound containing a sulfate group and / or a sulfite group to the difluoro(oxalato)borate is selectively a value within the range of 0.2, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 200, 300, 400, 500, or any two of the above.

[0079] By controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate within an appropriate range, it is possible to reduce the degree of intensified gas generation due to the intensified oxidative decomposition of the entire SEI film. Furthermore, it is possible to reduce the damage to the SEI film during the cycling process, which is caused by the relatively poor toughness of the entire SEI film and can further seriously affect the cycling performance. An appropriate ratio range allows for a balance between the storage performance and cycling performance of sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries. Moreover, controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate to 0.2 to 100 or 1 to 100 is advantageous for further balancing the storage performance and cycling performance of sodium secondary batteries.

[0080] In some embodiments, the sum of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups and sultone compounds containing carbon-carbon double bonds, based on the total mass of the electrolyte, is 0.1% to 6%, and selectively 0.5% to 5%. In some embodiments, the sum of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups and sultone compounds containing carbon-carbon double bonds, based on the total mass of the electrolyte, is selectively a value within the range of 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, or any two of the above.

[0081] To understand this, both cyclic ester compounds containing sulfate and / or sulfite groups, and sultone compounds containing carbon-carbon double bonds, can form CEI or SEI films on the positive and negative electrode plates, and the formation of CEI or SEI films leads to an increase in the DC impedance of a sodium secondary battery. By controlling the sum of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups and sultone compounds containing carbon-carbon double bonds within an appropriate range, it is possible not only to effectively improve the gas generation problem of sodium secondary batteries, but also to reduce the impact on rapid charging performance due to the increase in DC impedance caused by film formation.

[0082] In some embodiments, the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond is 0.2 to 100, and selectively 1 to 50. In some embodiments, the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond is selectively a value within the range of 0.2, 0.5, 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, or any two of the above.

[0083] To make it clear, difluoro(oxalato)borate not only participates in the formation of the SEI film on the negative electrode plate, but also causes an oxidation reaction on the positive electrode plate side, generating gas. However, sultone compounds containing carbon-carbon double bonds can form films on both the positive and negative electrode plates, and if a film is formed on the negative electrode plate side, it increases the interfacial impedance of the negative electrode plate, intensifying the risk of sodium precipitation. By controlling the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond within an appropriate range, the performance of sodium secondary batteries can be comprehensively improved. If the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond is lower than 0.2, there is too much of the sultone compound containing a carbon-carbon double bond. When a large amount of the sultone compound containing a carbon-carbon double bond forms a film on the negative electrode side, it worsens the interfacial impedance of the negative electrode, hinders sodium movement, and increases the risk of sodium deposition. If the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond is higher than 100, the excess difluoro(oxalato)borate compound oxidizes and decomposes on the positive electrode side, generating gas and degrading the performance of the sodium secondary battery.

[0084] In some embodiments, the product of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borates, and sultone compounds containing carbon-carbon double bonds, based on the total mass of the electrolyte, is 0.005 × 10⁻⁶ ―6 ~10×10 ―6 Therefore, selectively, 0.01 × 10 ―6 ~5×10 ―6 In some embodiments, the product of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borates, and sultone compounds containing carbon-carbon double bonds, based on the total mass of the electrolyte, is selectively 0.005 × 10⁻⁶. ―6 , 0.01 × 10 ―6 , 0.05 × 10 ―6 , 0.1 × 10 ―6 , 0.2 × 10―6 , 0.4 × 10 ―6 , 0.5 × 10 ―6 , 0.6 × 10 ―6 , 0.8 × 10 ―6 , 1 x 10 ―6 , 2×10 ―6 , 4×10 ―6 , 5×10 ―6 , 6×10 ―6 , 8×10 ―6 , 10×10 ―6 , or a numerical value within the range of any two of the above.

[0085] By simultaneously controlling the product of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups, difluoro(oxalato)borate, and sultone compounds containing carbon-carbon double bonds within an appropriate range, it is possible to reduce the impact on the degree of gas generation caused by having too low a mass content of any one of the three additives, as well as reduce the impact on the DC impedance and rapid charging performance of the sodium secondary battery caused by having too high a mass content of any one of the three additives, thereby comprehensively improving the performance of the sodium secondary battery.

[0086] In some embodiments, the mass content of cyclic ester compounds containing sulfate and / or sulfite groups is 0.01% to 5%, and selectively 0.1% to 3%, based on the total mass of the electrolyte. In some embodiments, the mass content of cyclic ester compounds containing sulfate and / or sulfite groups is selectively within the range of 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, or any two of the above.

[0087] By controlling the mass content of cyclic ester compounds containing sulfate and / or sulfite groups within an appropriate range, components containing sulfate and / or sulfite groups are formed in the SEI film, reducing the degree of overall SEI film rupture due to expansion of the sodium secondary battery during the cycle use process, further enhancing the overall protective capacity of the SEI film, and thus improving the storage performance of the sodium secondary battery. Furthermore, it is possible to reduce the degree to which excessive cyclic ester compounds are oxidized and decomposed on the positive electrode side, intensifying gas generation, and the degree to which the oxidative decomposition products accumulate on the surface of the positive electrode, increasing the interfacial resistance of the positive electrode and intensifying the deterioration of the sodium secondary battery's performance. Moreover, by controlling the mass content of cyclic ester compounds to 0.1% to 2%, it is advantageous to balance the storage performance and rapid charging performance of the sodium secondary battery, thereby comprehensively improving the performance of the sodium secondary battery.

[0088] In some embodiments, the mass content of difluoro(oxalato)borate is 0.01% to 5% based on the total mass of the electrolyte, and selectively 0.1% to 2%. In some embodiments, the mass content of difluoro(oxalato)borate is selectively within the range of 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, or any two of the above.

[0089] By controlling the mass content of difluoro(oxalato)borate within an appropriate range, other borate-containing components are formed in the SEI film, effectively enhancing the overall stability of the interfacial SEI film, reducing the degree of gas generation, and advantageously improving the cycle performance and storage performance of sodium secondary batteries. Furthermore, excessively high mass content of difluoro(oxalato)borate can lead to oxidative decomposition of the difluoro(oxalato)borate on the positive electrode side, intensifying gas generation and affecting storage performance. This is achieved by balancing the cycle performance and storage performance of sodium secondary batteries. Moreover, by controlling the mass content of difluoro(oxalato)borate to 0.1% to 2%, it is advantageous to balance the storage performance and rapid charging performance of sodium secondary batteries, thereby comprehensively improving the performance of sodium secondary batteries.

[0090] In some embodiments, the mass content of sultone compounds containing carbon-carbon double bonds is 0.01% to 5% of the total mass of the electrolyte, and selectively 0.1% to 2%. In some embodiments, the mass content of sultone compounds containing carbon-carbon double bonds is selectively 0.01%, 0.05%, 0.1%, 0.2%, 0.5%, 0.7%, 1%, 1.5%, 2%, 3%, 4%, 5%, or any two of the above values.

[0091] By controlling the mass content of sultone compounds containing carbon-carbon double bonds within an appropriate range, a sufficient CEI film is formed, direct contact between the positive electrode and the electrolyte is inhibited, reducing oxidation and gas generation on the positive electrode side, and RH + This not only suppresses the generation of sodium deposits and is advantageous for improving the storage and cycle performance of sodium secondary batteries, but also reduces the risk of sodium deposition by increasing the interfacial impedance on the negative electrode side, as sultone compounds containing excess carbon-carbon double bonds are involved in the formation of the SEI film on the negative electrode side, thereby improving the overall performance of sodium secondary batteries.

[0092] In some embodiments, the electrolyte contains a sodium salt, which includes one or more of NaPF6, NaFSI, NaBF4, NaN(SO2F)2, NaClO4, NaAsF6, NaB(C2O4)2, and NaBF2(C2O4).

[0093] In some embodiments, the sodium salt comprises NaPF6. In some embodiments, the sodium salt comprises NaBF4. In some embodiments, the sodium salt comprises NaFSI. In some embodiments, the sodium salt comprises NaPF6 and NaFSI. In some embodiments, the sodium salt comprises NaPF6 and NaClO4.

[0094] In some embodiments, the electrolyte includes a solvent, the solvent being one or more of a linear carbonate solvent, a linear carboxylic acid ester solvent, a cyclic carbonate solvent, or an ether-based solvent.

[0095] In some embodiments, the linear carbonate solvent includes one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, dipropyl carbonate, and dibutyl carbonate. The chain-like carboxylic acid ester solvent includes one or more of methyl formate, ethyl formate, methyl propionate, ethyl propionate, propyl propionate, ethyl butyrate, methyl acetate, ethyl acetate, and propyl acetate. The cyclic carbonate solvent includes one or more of the following: ethylene carbonate, propylene carbonate, butene carbonate, vinylene carbonate, fluoroethylene carbonate, ethylene sulfite, propylene sulfite, vinylethylene carbonate, 4-ethynyl-1,3-dioxolan-2-one, cis-4,5-difluoro-1,3-dioxolan-2-one, and trans-4,5-difluoro-1,3-dioxolan-2-one. The ether-based solvents include one or more of the following: dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, 1,2-diethoxyethane, and 1,2-dibutoxyethane.

[0096] [Positive electrode plate] The positive electrode plate includes a positive electrode current collector and a positive electrode material layer located on at least one side of the positive electrode current collector.

[0097] For example, a positive electrode current collector has two opposing surfaces in its own thickness direction, and the positive electrode material layer is placed on one or both of the two opposing surfaces of the positive electrode current collector.

[0098] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, aluminum foil may be used as the metal foil sheet. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer material substrate (for example, a substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), or polyethylene (PE)).

[0099] In some embodiments, the positive electrode material layer includes a positive electrode active material, which may be a positive electrode active material known in the art for batteries. For example, the positive electrode active material may include at least one of the following materials: a layered transition metal oxide, a polyanionic compound, or a Prussian blue compound. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may be used. These positive electrode active materials may be used individually or in combination of two or more. Here, the Prussian blue compound is Na x P[R(CN)6] δ·zH2O, wherein P and R are each independently selected from at least one of transition metal elements, 0<x≦2, 0<δ≦1 and 0≦z≦10, and the polyanionic compound comprises Na b Me c (PO4) d , wherein Me includes one or more of Ti, Cr, Mn, Fe, Co, Ni, V, Cu and Zn, 0<b≦4, 0<c≦2, 1≦d≦3, and the layered transition metal oxide comprises Na a M b Fe c O2, M includes a transition metal ion, and 0.67<a<1.1, 0.5<b<1, 0<c<0.5.

[0100] In some embodiments, the positive electrode active material includes a layered transition metal oxide.

[0101] In some embodiments, the layered transition metal oxide comprises Na a M b Fe c O2, M includes at least one of Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, and Pb, and 0.67<a<1.1, 0.5<b<1, 0<c<0.5.

[0102] The layered transition metal oxide positive electrode active material has the advantage of high voltage, but the transition metal therein catalyzes the oxidation of the solvent in the electrolyte to form RH + , and RH + migrates from the positive electrode plate side to the negative electrode plate side and deposits, and RH + is Li +Similarly, it can pass through the SEI film and react with the negative electrode plate, forming a product that is not resistant to oxidation, thus exacerbating the gas generation problem on the negative electrode plate side. A third additive containing a sultone compound with a carbon-carbon double bond preferentially undergoes an oxidative polymerization reaction on the surface of the positive electrode plate, forming a CEI film containing a sulfur-containing polymer that covers the surface of the positive electrode plate and inhibits direct contact between the positive electrode plate and the electrolyte. This reduces the degree of gas generation due to side reactions between the solvent in the electrolyte and the positive electrode plate, while RH generated by the catalytic oxidation of the transition metal in the layered transition metal oxide is reduced. + The material moves to the negative electrode side, accumulating on the negative electrode side and reducing the degree to which it causes side reactions with the negative electrode, further reducing gas generation on the negative electrode side, and thus comprehensively improving the storage performance, rapid charging performance, and cycle performance of the sodium secondary battery.

[0103] In some embodiments, the positive electrode active material is Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 ]O2, Na 7 / 9 [Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 ]O2, NaNi 0.7 Co 0.15 Mn 0.15 Contains at least one of the O2 species.

[0104] In some embodiments, the positive electrode material layer contains a layered transition metal oxide containing Cu, and the ratio of the mass content of sultone compounds containing carbon-carbon double bonds in the electrolyte to the mass content of Cu in the positive electrode active material is 0.002 or greater, with the mass content of Cu being based on the total mass of the positive electrode active material. In some embodiments, the ratio of the mass content of sultone compounds containing carbon-carbon double bonds in the electrolyte to the mass content of Cu in the positive electrode active material is selectively a numerical value within the range of 0.002, 0.004, 0.005, 0.01, 0.05, 0.1, 0.5, 1, 2, 3, 4, 5, 10, 50, 100, 500, 1000, 2000, 5000, or any two of the above, with the mass content of Cu being based on the total mass of the positive electrode active material.

[0105] To understand this, introducing the element Cu into the positive electrode active material is advantageous for the stability of the positive electrode active material structure and improves the cycle performance of sodium secondary batteries. However, at the same time, the Cu element in the positive electrode material layer undergoes a change in valence at high voltage, and Cu 3+ Generates Cu 3+ This has relatively high oxidative activity, which can accelerate the decomposition of the electrolyte and further degrade the performance of sodium secondary batteries. On the other hand, sultone compounds containing carbon-carbon double bonds in the electrolyte preferentially undergo oxidative polymerization reactions on the surface of the positive electrode plate, forming a CEI film containing sulfur-containing polymers that covers the surface of the positive electrode plate, inhibiting direct contact between the positive electrode plate and the electrolyte, and reducing the degree of gas generation due to side reactions between the solvent in the electrolyte and the positive electrode plate. On the other hand, RH generated by the catalytic oxidation of transition metals in layered transition metal oxides + The material can move to the negative electrode side and accumulate there, reducing the extent to which it causes side reactions with the negative electrode, thereby further reducing gas generation on the negative electrode side. By controlling the ratio of the mass content of sultone compounds containing carbon-carbon double bonds in the electrolyte to the mass content of Cu element in the positive electrode active material to an appropriate range, the degree of gas generation on both the positive and negative electrode sides can be effectively reduced.

[0106] In some embodiments, the mass content of Cu in the positive electrode active material is 23% or less, based on the total mass of the positive electrode active material. In some embodiments, the mass content of Cu in the positive electrode active material is selectively a value within the range of 0.01%, 0.1%, 0.5%, 1%, 2%, 5%, 7%, 10%, 12%, 15%, 18%, 20%, 23%, or any two of the above.

[0107] By controlling the mass content of Cu in the positive electrode active material within an appropriate range, it is advantageous not only to provide sufficient Cu to increase the stability of the positive electrode active material structure, but also to reduce the extent to which excessively high Cu mass content in the positive electrode material layer worsens the oxidative decomposition of the electrolyte and degrades the performance of sodium secondary batteries.

[0108] In some embodiments, the mass content of Cu element in the positive electrode active material is 5% to 20% based on the total mass of the positive electrode active material.

[0109] Furthermore, controlling the mass content of Cu element in the positive electrode active material to 5% to 20% is advantageous in further improving both the storage performance and rapid charging performance of sodium secondary batteries.

[0110] In some embodiments, the positive electrode active material does not need to contain the element Cu.

[0111] In some embodiments, the positive electrode material layer further selectively includes an adhesive. For example, the adhesive may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0112] In some embodiments, the positive electrode material layer further selectively includes a conductive agent. For example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0113] In some embodiments, a positive electrode plate can be manufactured by the following method. Components for manufacturing the positive electrode plate, such as a positive electrode active material, a conductive agent, an adhesive, and any other component, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry. The positive electrode slurry is then coated onto a positive electrode current collector, and after processes such as drying and cold pressing, a positive electrode plate is obtained.

[0114] [Negative electrode plate] The negative electrode plate includes a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector.

[0115] For example, the negative electrode current collector has two opposing surfaces in its thickness direction, and the negative electrode material layer is placed on one or both of the two opposing surfaces of the negative electrode current collector.

[0116] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, copper foil may be used as the metal foil sheet. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys) on a polymer material substrate (for example, a substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), or polyethylene (PE)).

[0117] The negative electrode material layer further comprises a negative electrode active material, the negative electrode active material comprising one or more of hard carbon, metallic sodium, sodium-tin alloy, and metal oxide.

[0118] All of the above-mentioned negative electrode active materials possess excellent sodium storage capacity, enabling sodium secondary batteries to have a high energy density.

[0119] In some embodiments, the negative electrode material layer further contains Ca element, and the ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is 1 or more, and the mass content of Ca element is based on the total mass of the negative electrode material layer. In some embodiments, the ratio of the mass content of cyclic ester compounds containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is selectively a numerical value within the range of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 100, 200, 300, 400, 500, 600, 700, 800, 900, 1000, or any two of the above, and the mass content of Ca element is based on the total mass of the negative electrode material layer.

[0120] Introducing Ca element into the negative electrode active material is advantageous in reducing the degree of sodium dendrite formation, and also advantageous in forming an SEI film containing an organic Ca salt component between the negative electrode active material and a cyclic ester compound containing sulfate and / or sulfite groups. Furthermore, it is advantageous in increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. By controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Ca element in the negative electrode material layer within an appropriate range, both the storage performance and rapid charging performance of the sodium secondary battery can be achieved.

[0121] In some embodiments, the mass content of Ca element in the negative electrode material layer is 1 ppm to 3000 ppm, based on the total mass of the negative electrode material layer. In some embodiments, the mass content of Ca element in the negative electrode material layer is selectively a value within the range of 1 ppm, 5 ppm, 10 ppm, 50 ppm, 100 ppm, 200 ppm, 400 ppm, 500 ppm, 600 ppm, 800 ppm, 1000 ppm, 1500 ppm, 2000 ppm, 2500 ppm, 3000 ppm, or any two of the above.

[0122] To make it understandable, the Ca element in the negative electrode material layer is involved in the formation of the SEI film, and by consuming some of the Ca element, the mass content of the Ca element in the negative electrode material layer can be reduced. For example, the mass content of the Ca element in the negative electrode material layer can be reduced to 1 ppm. Therefore, based on the total mass of the negative electrode material layer, the mass content of the Ca element is between 1 ppm and 3000 ppm, all of which are within the range protected in the embodiments of this application.

[0123] By controlling the mass content of Ca element in the negative electrode material layer to an appropriate range, it is possible to form an SEI film that sufficiently contains organic calcium salt components, thereby increasing the toughness of the entire SEI film and reducing the DC impedance of the sodium secondary battery. Furthermore, it is possible to reduce the risk of manufacturing failure of the negative electrode plate due to the gelation phenomenon of the slurry during the manufacturing process caused by an excessively high mass content of Ca element in the negative electrode material layer, the degree of reduction in the initial Coulomb efficiency and the degree of intensification of gas generation due to the formation of Ca(OH)2 during the manufacturing process, or the degree of deterioration of the sodium secondary battery performance due to the increase in the DC impedance of the sodium secondary battery, thereby achieving both the storage performance and rapid charging performance of the sodium secondary battery.

[0124] In some embodiments, the mass content of Ca element in the negative electrode material layer is 50 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.

[0125] In some embodiments, the mass content of Ca element in the negative electrode material layer is 100 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.

[0126] Furthermore, controlling the mass content of Ca element in the negative electrode material layer to 10 ppm to 1000 ppm or 100 ppm to 1000 ppm is advantageous for further comprehensively improving the storage performance and rapid charging performance of sodium secondary batteries.

[0127] In some embodiments, the negative electrode film layer further selectively includes an adhesive. The adhesive may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0128] In some embodiments, the negative electrode film layer further selectively includes a conductive agent. The conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0129] In some embodiments, the negative electrode film layer further selectively includes other auxiliary agents, such as thickeners (e.g., sodium carboxymethylcellulose (CMC-Na)).

[0130] In some embodiments, the negative electrode plate can be manufactured by the following method. Components for manufacturing the negative electrode plate, such as a negative electrode active material, a conductive agent, an adhesive, and any other component, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry. The negative electrode slurry is then coated onto a negative electrode current collector, and after processes such as drying and cold pressing, the negative electrode plate is obtained.

[0131] [Separator] In some embodiments, the sodium secondary battery further includes a separator. Any known porous structure separator with good chemical stability and mechanical stability may be selected.

[0132] In some embodiments, the material of the separator may be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the material of each layer may be the same or different.

[0133] [Sodium Secondary Battery] In some embodiments, the positive electrode plate, the negative electrode plate and the separator can be fabricated into an electrode assembly by a winding process or a lamination process.

[0134] In some embodiments, the sodium secondary battery may include an exterior body. The exterior body may be used to package the above electrode assembly and the electrolyte.

[0135] In some embodiments, the exterior body of the sodium secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, and the like. The exterior body of the sodium secondary battery may be a pouch, for example, a bag-shaped pouch. The material of the pouch may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, polybutylene succinate, and the like.

[0136] In the present application, the shape of the sodium secondary battery may be cylindrical, prismatic or any other shape. For example, FIG. 1 shows a sodium secondary battery 5 having a prismatic structure as an example.

[0137] In some embodiments, referring to Figure 2, the exterior may include a case 51 and a cover plate 53. Here, the case 51 may include a bottom plate and side plates connected to the bottom plate, the bottom plate and side plates enclosing and forming a housing cavity. The case 51 has an opening that communicates with the housing cavity, and the cover plate 53 can cover the opening so as to seal the housing cavity. The positive electrode plate, negative electrode plate and separator can form an electrode assembly 52 by a winding process or a lamination process. The electrode assembly 52 is packaged within the housing cavity. The electrolyte is impregnated into the electrode assembly 52. ​​The number of electrode assemblies 52 included in the sodium secondary battery 5 may be one or more, and those skilled in the art can specifically select them according to their actual needs.

[0138] In some embodiments, the sodium secondary batteries may be assembled into a battery module, and the number of sodium secondary batteries included in the battery module may be one or more, and the specific number can be selected by those skilled in the art depending on the application and capacity of the battery module.

[0139] Figure 3 shows an example of a battery module 4. Referring to Figure 3, in the battery module 4, multiple sodium secondary batteries 5 may be arranged sequentially along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, these multiple sodium secondary batteries 5 may be fixed in place with fasteners.

[0140] Selectively, the battery module 4 may further include a housing having a housing space, in which a plurality of sodium secondary batteries 5 are housed.

[0141] In some embodiments, the battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack may be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery pack.

[0142] Figures 4 and 5 show an example of a battery pack 1. Referring to Figures 4 and 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 can be covered by the lower housing 3 to form a sealed space for housing the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.

[0143] Furthermore, this application provides a power consumption device comprising at least one of a sodium secondary battery, a battery module, or a battery pack according to this application. The sodium secondary battery, battery module, or battery pack may be used as a power source for the power consumption device or as an energy storage unit for the power consumption device. The power consumption device may include, but is not limited to, mobile devices (e.g., mobile phones, laptop computers, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0144] As the power consumption device, a sodium secondary battery, a battery module, or a battery pack can be selected according to the usage demand.

[0145] Figure 6 shows an example of a power consumption device. This power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the demand for high power output and high energy density of sodium secondary batteries in this power consumption device, a battery pack or battery module can be used.

[0146] Other examples of such devices may include mobile phones, tablet computers, and laptop computers. These devices generally require a thin profile and can use sodium-ion batteries as a power source.

[0147] Examples Examples of the present application are described below. The examples described below are illustrative and intended to interpret this application and should not be construed as limitations thereon. Unless otherwise specified in the examples, any specific techniques or conditions are carried out in accordance with the techniques, conditions, or product specifications described in the literature in the art. Unless otherwise specified, the reagents or equipment used are all commonly available commercial products.

[0148] 1. Manufacturing method Example 1 1) Electrolyte In an argon gas-atmosphered glove box (H2O content < 10 ppm, O2 content < 1 ppm), propylene carbonate (PC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 30 / 70, 1 M NaPF6 sodium salt was dissolved, and the first additive was... [ka] , the second additive sodium difluoro(oxalato)borate and the third additive [ka] The following were added and the mixture was uniformly stirred to prepare the electrolyte. Based on the total mass of the electrolyte, the mass content of the first additive, the compound with the structure described in formula I-019, was 1%, the mass content of the second additive, sodium difluoro(oxalato)borate, was 1%, and the mass content of the third additive, the compound with the structure shown in formula III-1, was 1%.

[0149] 2) Manufacturing of positive electrode plates Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3Preparation of O2(13%Cu): A 0.39M Na2CO3, 0.22M CuO, 0.06M Fe2O3, 0.67M MnO2 precursor is ball-milled for 12h in a ball mill using ethanol as a dispersant. After drying, the uniformly mixed powder is pressed into tablets at 20MPa, and sintered at 900°C for 12h to obtain the product. The sintered powder must be quickly transferred to and stored in a glove box, Na of the above positive electrode active material 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, acetylene black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive are fully stirred and uniformly mixed in an N-methylpyrrolidone solvent system at a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is applied at 0.28g (dry weight) / 1540.25mm 2 to uniformly coat an aluminum foil positive electrode current collector with a thickness of 13μm. The aluminum foil is dried at room temperature, then transferred to an oven at 120°C for 1h of drying, and subjected to cold pressing and slitting to obtain a positive electrode plate.

[0150] 3) Preparation of negative electrode plate Preparation of negative electrode material: Negative electrode active material: A biomass material is calcined at 800°C for 2h in a tubular furnace containing an argon gas atmosphere, then washed with hydrochloric acid and deionized water respectively and dried. After grinding, it is calcined at 1550°C for 4h in a tubular furnace under an argon gas atmosphere to obtain hard carbon, Preparation of negative electrode plate: The hard carbon as the above negative electrode active material, acetylene black as a conductive agent, styrene-butadiene rubber (SBR) as an adhesive, sodium carboxymethyl cellulose (CMC-Na) as a thickener, and CaO are fully stirred and uniformly mixed in a deionized water solvent system at a weight ratio of 90:4:4:2:0.014 to obtain a negative electrode slurry. By adding CaO to the negative electrode slurry, Ca contents of different gradients in the negative electrode plate are adjusted. The negative electrode slurry is applied at 0.14g (dry weight) / 1540.25mm 2The material was uniformly applied to an 8 μm thick copper foil negative electrode current collector, dried at room temperature, then transferred to a 120°C oven for 1 hour of drying, followed by cold pressing and slitting to obtain the negative electrode plate.

[0151] 4) Separator A 9 μm polyethylene (PE) porous polymerized film was used as a separator.

[0152] 5) Battery manufacturing The positive electrode plate, separator, and negative electrode plate were stacked in order so that the separator was positioned between the positive and negative electrode plates to isolate them, and the stack was wound up to obtain a bare cell. Tabs were welded on, the bare cell was placed in an outer casing, the electrolyte manufactured above was injected into the dried battery core, and after going through processes such as packaging, settling, chemical conversion, shaping, and capacity testing, the sodium secondary battery product of Example 1 was obtained.

[0153] The secondary batteries of Examples 2-36 and Comparative Examples 1-9 were similar in their manufacturing method to the sodium secondary battery of Example 1, but the composition of the battery electrode plates and product parameters were adjusted. Details of the different product parameters are shown in Tables 1-3. Here, in Examples 2 to 16, the mass content of the first additive, the second additive, and the third additive can be adjusted by adjusting the solvent content in the electrolyte. The first additive in Example 17 is [ka] And, The first additive in Example 18 is [ka] And, The first additive in Example 19 is [ka] And, The third additive in Example 23 is [ka] And, The third additive in Example 24 is [ka] And, The third additive in Example 25 is [ka] And, The negative electrode material layers containing different mass content of Ca element in Examples 26-30 can be adjusted by adding different mass content of CaO during the manufacturing process of the negative electrode plate. The positive electrode active materials containing different mass content of Cu in Examples 31-35 were obtained by adjusting the stoichiometric ratios of the precursor Fe2O3, CuO, MnO2, and Na2CO3 during the sintering process and the formulation of the positive electrode material with different Cu content during the manufacturing process of the positive electrode plate. Specifically, these are as follows: Na 1 / 2 Fe 1 / 2 Mn 1 / 2 Production of O2 (0% Cu): 0.25M Na2CO3, 0.25M Fe2O3, and 0.5M MnO2 precursor are ball-milled for 12 hours using ethanol as a dispersant. After drying, the uniformly mixed powder is pressed into tablets at 20 MPa and sintered at 900°C for 12 hours. The sintered powder must be quickly transferred to a glove box for storage. Na 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 Production of O2 (23% Cu): 0.45M Na2CO3, 0.4M CuO, 0.05M Fe2O3, and a 0.5M MnO2 precursor are ball-milled for 12 hours using ethanol as a dispersant. After drying, the uniformly mixed powder is pressed into tablets at 20 MPa and sintered at 900°C for 12 hours. The sintered powder must be quickly transferred to a glove box for storage. Example 31: Na of the positive electrode active material 1 / 2 Fe1 / 2 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 32: 50% Na of the positive electrode active material 1 / 2 Fe 1 / 2 Mn 1 / 2 O2, 50% Na 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 33: 50% Na of the positive electrode active material 7 / 9 Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 O2, 50% Na 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 34: Na of the positive electrode active material 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. Example 35: Na of the positive electrode active material 9 / 10 Cu 2 / 5 Fe 1 / 10 Mn 1 / 2 O2, the conductive agent acetylene black, and the adhesive polyvinylidene fluoride (PVDF) are thoroughly stirred and homogeneously mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to obtain a positive electrode slurry. The positive electrode slurry is then divided into 0.28 g (dry weight) / 1540.25 mm 2 The amount is uniformly applied to a 13 μm thick positive electrode current collector aluminum foil, the aluminum foil is dried at room temperature, then transferred to a 120°C oven and dried for 1 hour, and then cold-pressed and slit to obtain the positive electrode plate. The first additive in Comparative Example 8 is ethylene carbonate. [ka] And, The third additive in Comparative Example 9 is a vinyl sulfate that does not contain a carbon-carbon double bond. [ka] That is the case.

[0154] 2. Performance Test 1, Negative electrode plate / positive electrode plate 1) Measurement of the mass content of element Ca in the negative electrode material layer. Referring to EPA 6010D-2014, the mass content of element Ca in the negative electrode material layer was tested using inductively coupled plasma atomic emission spectroscopy.

[0155] 2) Measurement of the mass content of Cu element in the positive electrode active material. Referring to EPA 6010D-2014, the mass content of Cu in the positive electrode material layer was tested using inductively coupled plasma atomic emission spectroscopy, i.e., the mass content of Cu in the positive electrode active material = Cu content in the positive electrode material layer / mass content of the positive electrode active material in the positive electrode material layer.

[0156] 2, battery 1) Rate of change in storage volume at high temperature and low voltage. At 25°C, fresh sodium secondary batteries produced in the examples and comparative examples were left for 5 minutes, then charged with a constant current at a 0.5C multiplier up to 4.0V, charged with a constant voltage until the current was 0.05C or less, then left for 5 minutes, discharged with a constant current at a 0.5C multiplier up to 1.5V, the battery volume V1 was tested using the drainage method, and the batteries were then placed in a 70°C oven and stored for 1 month. After removing the batteries and setting the test volume to V2, the rate of change in battery volume at high temperature and low voltage is (V2-V1) / V1 × 100%.

[0157] 2) Rate of change in storage volume at high temperature and high voltage At 25°C, fresh sodium secondary batteries produced in the examples and comparative examples were left for 5 minutes, then charged with a constant current at a rate of 0.5C up to 4.0V, and then charged at a constant voltage until the current was 0.05C or less. The volume V3 of the battery was tested using the drainage method, and the battery was then placed in a 70°C oven and stored for 1 month. After removing the battery, the test volume was set to V4. Therefore, the rate of change in battery volume at high temperature and high voltage is (V4-V3) / V3 × 100%.

[0158] 3) Charging performance at -20℃ Fabrication of a three-electrode battery: First, a vanadium sodium phosphate reference electrode is manufactured. The active material, vanadium sodium phosphate, the conductive agent, acetylene black, and the adhesive, polyvinylidene fluoride (PVDF), are thoroughly stirred and uniformly mixed in an N-methylpyrrolidone solvent system in a weight ratio of 90:5:5 to prepare a slurry. The slurry is uniformly applied to a 10 cm long aluminum wire (where the applied area occupies 1 cm), and after drying at 100°C, the target reference electrode is obtained. In the manufacturing process of a sodium secondary battery, when this reference electrode is placed between the negative electrode plate and the separator, a three-electrode battery is obtained. -20℃ Rapid Charging Capacity Test: A three-electrode battery including the above reference electrode was charged at 25℃ with a constant current of 1C until the voltage reached 4.0V, then charged with a constant voltage until the current was 0.05C or less, left for 5 minutes, discharged with a constant current at a multiplier of 1C until it reached 1.5V, and the discharge capacity was recorded as C1. Then, this battery was placed in a -20℃ environment and left idle for 2 hours, and charged with a constant current of 0.1C until the voltage reached 4.0V, and the charge capacity of the negative electrode potential before the reference potential reached -3.377V was obtained as C2. The charge performance of the battery at -20℃ = C2 / C1 × 100%.

[0159] 4) DC impedance At 25°C, the cell's charge state was adjusted to 50% SOC and left standing for 30 minutes. The battery voltage at this time was recorded as U1 (V). The battery was then discharged for 10 seconds using 4C, and the battery voltage at this time was recorded as U2 (V). The corresponding battery discharge current I (mA) is 4 × battery design capacity (mAh). The DC impedance DCR (mΩ) = (U1 - U2) / I.

[0160] 5) Cycle performance At 25°C, the manufactured battery is charged to 3.8V with a constant current of 1C, then to 3.9V with a constant current of 0.5C, then to 4.0V with a constant current of 0.2C, then charged at a constant voltage of 4.0V until the current drops to 0.05C, left to stand for 10 minutes, and then discharged to 1.5V with a constant current of 1C. This is the battery's first charge / discharge cycle, and the discharge capacity at this point is denoted as the discharge capacity of the battery's first cycle (C0). The above steps are repeated for the same battery, and the discharge capacity after 300 cycles (C1) and the capacity retention rate after 300 cycles = C1 / C0 × 100%. The test process for comparative examples and other examples is the same as above.

[0161] III. Analysis of Test Results for Each Example and Comparative Example Batteries for each example and comparative example were manufactured according to the method described above. The battery parameters were measured according to Tables 1, 2, and 3 below, and the results are shown in Table 4 below.

[0162] [Table 1] TIFF2026539214000154.tif245170TIFF2026539214000155.tif245170TIFF2026539214000156.tif131170

[0163] [Table 2] TIFF2026539214000158.tif133170

[0164] [Table 3] TIFF2026539214000160.tif133170

[0165] [Table 4] TIFF2026539214000162.tif133170

[0166] The electrolytes in Examples 1 to 35 all contained a first additive, a second additive, and a third additive. The first additive contained a compound with the structure shown in formula I-01, a compound with the structure shown in formula I-013, a compound with the structure shown in formula I-014, a compound with the structure shown in formula I-019, or a compound with the structure shown in formula I-022. The second additive contained sodium difluoro(oxalato)borate, lithium difluoro(oxalato)borate, magnesium difluoro(oxalato)borate, or aluminum difluoro(oxalato)borate. The third additive contained a compound with the structure shown in formula III-1, a compound with the structure shown in formula III-4, a compound with the structure shown in formula III-6, or a compound with the structure shown in formula III-8. The sodium secondary batteries containing this electrolyte all exhibited excellent storage performance, cycle performance, and rapid charging performance.

[0167] As can be seen from the comparison between Examples 1 to 25 and Comparative Example 1, the electrolyte containing the first additive, the second additive, and the third additive is advantageous in reducing the volume expansion rate and DC impedance of sodium secondary batteries after storage at high temperature and high voltage / high temperature and low voltage, thereby improving the charging performance and cycle capacity maintenance rate of the sodium secondary batteries.

[0168] As can be seen from the comparison between Examples 1, 7-14 and Comparative Example 2, Examples 1-5, 11-19, 23-25 ​​and Comparative Example 3, Examples 1-10, 17-22 and Comparative Example 4, the electrolyte in this application contains a first additive, a second additive, and a third additive simultaneously, which is advantageous in reducing the volume expansion rate of sodium secondary batteries after storage at high temperature and high voltage / low voltage, and improving the charging performance and cycle capacity maintenance rate of the sodium secondary batteries.

[0169] As can be seen from the comparison between Examples 1, 11-14 and Comparative Example 5, Examples 1, 7-10 and Comparative Example 6, and Examples 1-5, 17-19 and Comparative Example 7, the electrolyte in this application contains the first, second, and third additives simultaneously, whereas the electrolyte contains only two of the first, second, and third additives. This is advantageous in reducing the volume expansion rate of the sodium secondary battery after storage at high temperature and high / low voltage, and in improving the cycle capacity retention rate of the sodium secondary battery.

[0170] As can be seen from the comparison between Examples 1, 17-25 and Comparative Examples 8-9, this application simultaneously contains a compound with the structure shown in formula I-013, I-014, I-019, or I-022 as a first additive, a difluoro(oxalato)borate as a second additive, and a vinyl sulfate containing a carbon-carbon double bond as a third additive, which is advantageous in reducing the volume expansion rate and DC impedance of sodium secondary batteries after storage at high temperature and high / low voltage, and improving the charging performance and cycle capacity retention rate of the sodium secondary batteries.

[0171] As can be seen from Examples 1 to 17, by controlling the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate to 0.2 to 500, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature and high / low voltage, as well as excellent charging and cycling performance. Furthermore, the mass ratio of cyclic ester compounds containing sulfate and / or sulfite groups to difluoro(oxalato)borate was controlled to 1 to 100.

[0172] As can be seen from Examples 1 to 17, by controlling the sum of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups and sultone compounds containing carbon-carbon double bonds to 0.1% to 6% based on the total mass of the electrolyte, the sodium secondary battery was made to have a volume expansion rate and DC impedance after storage at relatively low high temperature and high voltage / low voltage, as well as excellent charging and cycling performance. Furthermore, based on the total mass of the electrolyte, the sum of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups and sultone compounds containing carbon-carbon double bonds was controlled to 0.5% to 5%.

[0173] As can be seen from Examples 1 to 17, by controlling the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond from 0.2 to 100, the sodium secondary battery was made to have a volume expansion rate and DC impedance after storage at relatively low temperature and high / low voltage, as well as excellent charging and cycling performance. Furthermore, the mass ratio of difluoro(oxalato)borate to a sultone compound containing a carbon-carbon double bond was controlled from 1 to 50.

[0174] As can be seen from Examples 1 to 17, the product of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups, difluoro(oxalato)borate, and sultone compounds containing carbon-carbon double bonds, based on the total mass of the electrolyte, is 0.005 × 10⁻⁶. ―6 ~10×10 ―6 By controlling this, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature and high / low voltage, as well as excellent charging and cycling performance. Based on the total mass of the electrolyte, the product of the mass content of cyclic ester compounds containing sulfate groups and / or sulfite groups, difluoro(oxalato)borate, and sultone compounds containing carbon-carbon double bonds was set to 0.01 × 10⁻⁶. ―6 ~5×10 ―6 It was controlled to that extent.

[0175] As can be seen from Examples 1 to 5, by controlling the mass content of the compound with the structure shown in formula I-019 of the first additive to 0.01% to 5% based on the total mass of the electrolyte, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature and high voltage / high temperature and low voltage, as well as excellent charging performance and cycle performance. As can be seen from a comparison between Examples 1, 3 to 4 and Example 5, by further controlling the mass content of the compound with the structure shown in formula I-019 of the first additive to 0.1% to 3% based on the total mass of the electrolyte, it is advantageous to further reduce the DC impedance of the sodium secondary battery and improve its rapid charging performance and cycle capacity retention rate.

[0176] As can be seen from Examples 1, 7-10, by controlling the mass content of the second additive, sodium difluoro(oxalato)borate, to 0.01%-5% based on the total mass of the electrolyte, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature and high voltage / high temperature and low voltage, as well as excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 7-8 and Examples 9-10, by further controlling the mass content of the second additive, sodium difluoro(oxalato)borate, to 0.1%-2% based on the total mass of the electrolyte, the volume expansion rate and DC impedance after storage at high temperature and high voltage of the sodium secondary battery are reduced, which is advantageous in improving the charging performance of the sodium secondary battery.

[0177] As can be seen from Examples 1, 11-14, by controlling the mass content of the compound with the structure shown in formula III-1 of the third additive to 0.01%-5% based on the total mass of the electrolyte, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature / high voltage and high temperature / low voltage, as well as excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 12-13 and Example 11, further controlling the mass content of the compound with the structure shown in formula III-1 of the third additive to 0.1%-2% is advantageous in further reducing the DC impedance of the sodium secondary battery and improving its rapid charging performance and cycle capacity retention rate.

[0178] As can be seen from Examples 1, 17-25, the first additive includes a compound with the structure shown in formula I-01, a compound with the structure shown in formula I-013, a compound with the structure shown in formula I-014, a compound with the structure shown in formula I-019, or a compound with the structure shown in formula I-022; the second additive includes sodium difluoro(oxalato)borate, lithium difluoro(oxalato)borate, magnesium difluoro(oxalato)borate, or aluminum difluoro(oxalato)borate; and the third additive includes a compound with the structure shown in formula III-1, a compound with the structure shown in formula III-2, a compound with the structure shown in formula III-3, or a compound with the structure shown in formula III-9. In all cases, it was possible to make the sodium secondary battery have a volume expansion rate and DC impedance after storage at relatively low temperature high voltage / high temperature low voltage, as well as excellent charging performance and cycle performance.

[0179] As can be seen from a comparison between Examples 1, 26-29 and Example 30, controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Ca element in the negative electrode material layer to 1 or more is advantageous in reducing the volume expansion rate and DC impedance of the sodium secondary battery after storage at high temperature and low voltage, thereby improving the rapid charging performance and cycle capacity maintenance rate of the sodium secondary battery.

[0180] As can be seen from Examples 1, 26-28, by controlling the mass content of Ca element in the negative electrode material layer to 50 ppm to 3000 ppm, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature and high voltage / high temperature and low voltage, as well as excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 26-27 and Example 28, further controlling the mass content of Ca element in the negative electrode material layer to 50 ppm to 1000 ppm is advantageous in further reducing the volume expansion rate and DC impedance of the sodium secondary battery after storage at high temperature and low voltage, thereby improving the rapid charging performance and cycle capacity retention rate of the sodium secondary battery.

[0181] As can be seen from the comparison between Examples 1, 32-35 and Example 31, introducing Cu elements into the positive electrode active material is advantageous for improving the cycle performance of sodium secondary batteries.

[0182] As can be seen from Examples 1, 32-35, by controlling the ratio of the mass content of the first additive in the electrolyte to the mass content of Cu element in the positive electrode active material to 0.002 or higher, the sodium secondary battery was made to have a volume expansion rate and DC impedance after storage at relatively low temperature and high voltage / low voltage, as well as excellent charging and cycling performance.

[0183] As can be seen from Examples 1, 32-34, by controlling the mass content of Cu element in the positive electrode active material to 23% or less, the sodium secondary battery was made to have a relatively low volume expansion rate and DC impedance after storage at high temperature and high voltage / high temperature and low voltage, as well as excellent charging and cycling performance. As can be seen from a comparison between Examples 1, 32-33 and Example 34, controlling the mass content of Cu element in the positive electrode active material to 6.5%-18% further reduces the volume expansion rate and DC impedance of the sodium secondary battery after storage at high temperature and low voltage / high temperature and high voltage, which is advantageous for improving the rapid charging performance of the sodium secondary battery.

[0184] It should be noted that this application is not limited to the embodiments described above. The embodiments described above are merely illustrative, and any embodiments that have substantially the same configuration as the technical idea and produce the same effects within the scope of the technical proposal of this application are included within the scope of the technical proposal. Furthermore, other methods that are constructed by adding various modifications to the embodiments that a person skilled in the art could conceive of, and by combining some of the components of the embodiments, are also included within the scope of this application, without departing from the spirit of this application. [Explanation of Symbols]

[0185] 1. Battery pack, 2. Upper casing, 3. Lower casing, 4. Battery module, 5. Sodium secondary battery, 5. Case, 5. Electrode assembly, 5. Cover plate.

Claims

1. An electrolyte for a sodium secondary battery, comprising a first additive, a second additive, and a third additive, wherein the first additive comprises a cyclic ester compound containing a sulfate group and / or a sulfite group, the second additive comprises a difluoro(oxalato)borate, and the third additive comprises a sultone compound containing a carbon-carbon double bond.

2. The cyclic ester compound containing the sulfate group and / or sulfite group comprises at least one of the compounds having the structure shown in formula I-1 and the compounds having the structure shown in formula I-2. 【Chemistry 1】 In equation I-1, R 1 teeth, 【Chemistry 2】 Includes R 2 , R 3 Each of them operates independently. 【Transformation 3】 , comprising at least one of a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group, and R 2 , R 3 At least one of them is 【Chemistry 4】 Includes R 4 teeth, 【Transformation 5】 It includes at least one of the following, R 5 , R 6 Each of them operates independently. 【Transformation 6】 It contains at least one of the following: a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a C1-C3 olefin group, an ester group, a cyano group, or a sulfonic acid group. In Formula I-2, R 7 is 【Transformation 7】 Includes R 8 teeth, 【Transformation 8】 It includes at least one of the following, R 9 C, 【Chemistry 9】 It includes at least one of the following, R 14 It comprises at least one of a single bond, a C1-C6 alkyl group, a C1-C6 ether group, and a C1-C3 alkoxy group, R 10 , R 11 , R 12 , R 13 Each independently comprises at least one of a single bond, a C1-C3 alkylene group, and / or The aforementioned difluoro(oxalato)borate contains the compound shown in formula II, (F) 2 C 2 O 4 B) y M y+ Formula II In equation II, M y+ Li + Na + _K + , Rb + , Cs + Mg 2+ Ca 2+ Ba 2+ Fe 2+ Ni 2+ Al 3+ Fe 3+ Ni 3+ It includes one or more of the following, where y = 1, 2, or 3, and / or The sultone compound containing the carbon-carbon double bond includes a compound with the structure shown in formula III, 【Chemistry 10】 In equation III, R 15 R includes at least one of an alkylene group, an alkoxy group, a carbonyl group, or a haloalkylene group. 16 , R 17 The electrolyte according to claim 1, wherein each independently comprises at least one of a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 haloalkyl group, a C1-C3 alkoxy group, a C1-C3 haloalkoxy group, a phenyl group, an amino group, an amine group, a silyl group, a C1-C3 olefin group, an ester group, a cyano group, and a sulfonic acid group.

3. In equation I-1, R 1 teeth, 【Chemistry 11】 Includes R 2 , R 3 Each of them operates independently. 【Chemistry 12】 , containing at least one of a hydrogen atom, a C1-C6 alkyl group, and a halogen atom, and R 2 , R 3 At least one of them is 【Chemistry 13】 Includes R 4 teeth, 【Chemistry 14】 It includes at least one of the following, R 5 , R 6 Each independently comprises at least one of a hydrogen atom, a C1-C6 alkyl group, and a halogen atom, and / or In Equation I-2, R 7 teeth, 【Chemistry 15】 Includes R 8 teeth, 【Chemistry 16】 It includes at least one of the following, R 9 C, 【Chemistry 17】 It includes at least one of the following, R 14 R comprises at least one of a single bond, a C1-C6 alkyl group, or a C1-C6 ether group. 10 , R 11 , R 12 , R 13 The electrolyte according to claim 1 or 2, wherein each independently comprises at least one of a single bond and a C1-C3 alkylene group.

4. The cyclic ester compounds containing the aforementioned sulfate group and / or sulfite group are, [Chemistry 18] The electrolyte according to any one of claims 1 to 4, comprising at least one of the following.

6. In equation II, M y+ Li + Na + The electrolyte according to any one of claims 2 to 5, comprising at least one of the following.

7. In equation III, R 15 It contains at least one of an alkylene group, a carbonyl group, or a haloalkylene group, R 16 , R 17 The electrolyte according to any one of claims 2 to 6, wherein each independently comprises at least one of a hydrogen atom, a C1-C6 alkyl group, a halogen atom, a C1-C3 alkoxy group, a phenyl group, an amino group, and a silyl group.

8. The structure shown in formula III above is, 【Chemistry 21】 The electrolyte according to any one of claims 2 to 7, comprising at least one of the following.

9. The electrolyte according to any one of claims 1 to 8, wherein the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the difluoro(oxalato)borate is 0.2 to 500.

10. The electrolyte according to any one of claims 1 to 9, wherein the mass ratio of the cyclic ester compound containing the sulfate group and / or sulfite group to the difluoro(oxalato)borate is 1 to 100.

11. The electrolyte according to any one of claims 1 to 10, wherein, based on the total mass of the electrolyte, the sum of the mass content of the cyclic ester compound containing sulfate groups and / or sulfite groups and the sultone compound containing carbon-carbon double bonds is 0.1% to 6%.

12. The electrolyte according to any one of claims 1 to 11, wherein, based on the total mass of the electrolyte, the sum of the mass content of the cyclic ester compound containing sulfate groups and / or sulfite groups and the sultone compound containing carbon-carbon double bonds is 0.5% to 5%.

13. The electrolyte according to any one of claims 1 to 12, wherein the mass ratio of the difluoro(oxalato)borate to the sultone compound containing the carbon-carbon double bond is 0.2 to 100.

14. The electrolyte according to any one of claims 1 to 13, wherein the mass ratio of the difluoro(oxalato)borate to the sultone compound containing the carbon-carbon double bond is 1 to 50.

15. Based on the total mass of the electrolyte, the product of the mass content of the cyclic ester compound containing a sulfate group and / or a sulfite group, the difluoro(oxalato)borate, and the sultone compound containing a carbon-carbon double bond is 0.005 × 10⁻⁶. ―6 ~10 x 10 ―6 The electrolyte according to any one of claims 1 to 14.

16. Based on the total mass of the electrolyte, the product of the mass content of the cyclic ester compound containing sulfate and / or sulfite groups, the difluoro(oxalato)borate, and the sultone compound containing a carbon-carbon double bond is 0.01 × 10⁻⁶. ―6 ~5 x 10 ―6 The electrolyte according to any one of claims 1 to 15.

17. The electrolyte according to any one of claims 1 to 16, wherein the mass content of the cyclic ester compound containing sulfate and / or sulfite groups is 0.01% to 5% based on the total mass of the electrolyte.

18. The electrolyte according to any one of claims 1 to 17, wherein the mass content of the cyclic ester compound containing sulfate and / or sulfite groups is 0.1% to 3% based on the total mass of the electrolyte.

19. The electrolyte according to any one of claims 1 to 18, wherein the mass content of the difluoro(oxalato)borate is 0.01% to 5% based on the total mass of the electrolyte.

20. The electrolyte according to any one of claims 1 to 19, wherein the mass content of the difluoro(oxalato)borate is 0.1% to 2% based on the total mass of the electrolyte.

21. The electrolyte according to any one of claims 1 to 20, wherein the mass content of the sultone compound containing the carbon-carbon double bond is 0.01% to 5% based on the total mass of the electrolyte.

22. The electrolyte according to any one of claims 1 to 21, wherein the mass content of the sultone compound containing the carbon-carbon double bond is 0.1% to 2% based on the total mass of the electrolyte.

23. A sodium secondary battery comprising a positive electrode plate, a negative electrode plate, and an electrolyte according to any one of claims 1 to 22.

24. The sodium secondary battery according to claim 23, wherein the positive electrode plate includes a positive electrode current collector and a positive electrode material layer located on at least one side of the positive electrode current collector, the positive electrode material layer further includes a positive electrode active material, and the positive electrode active material includes a layered transition metal oxide.

25. The aforementioned layered transition metal oxide is Na a M b Fe c O 2 A sodium secondary battery according to claim 23 or 24, comprising, where M comprises at least one of Sc, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Zr, Nb, Mo, Sn, Hf, Ta, W, Pb, and 0.67 < a < 1.1, 0.5 < b < 1, 0 < c < 0.

5.

26. The positive electrode material layer includes a layered transition metal oxide containing Cu element, The sodium secondary battery according to claim 24 or 25, wherein the ratio of the mass content of the sultone compound containing the carbon-carbon double bond in the electrolyte to the mass content of Cu element in the positive electrode active material is 0.002 or more, and the mass content of Cu element is based on the total mass of the positive electrode active material.

27. A sodium secondary battery according to any one of claims 23 to 26, wherein the mass content of Cu element in the positive electrode active material is 23% or less, based on the total mass of the positive electrode active material.

28. A sodium secondary battery according to any one of claims 23 to 27, wherein the mass content of Cu element in the positive electrode active material is 5% to 20% based on the total mass of the positive electrode active material.

29. The negative electrode plate includes a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, and the negative electrode material layer includes the element Ca. The sodium secondary battery according to any one of claims 23 to 28, wherein the ratio of the mass content of the cyclic ester compound containing sulfate and / or sulfite groups in the electrolyte to the mass content of Ca element in the negative electrode material layer is 1 or more, and the mass content of Ca element is based on the total mass of the negative electrode material layer.

30. A sodium secondary battery according to any one of claims 23 to 29, wherein the mass content of element Ca in the negative electrode material layer is 1 ppm to 3000 ppm, based on the total mass of the negative electrode material layer.

31. A sodium secondary battery according to any one of claims 23 to 30, wherein the mass content of element Ca in the negative electrode material layer is 50 ppm to 1000 ppm or 100 ppm to 1000 ppm, based on the total mass of the negative electrode material layer.

32. The sodium secondary battery according to any one of claims 23 to 31, wherein the negative electrode material layer further comprises a negative electrode active material, the negative electrode active material comprising one or more of hard carbon, tin alloy, and metal oxide.

33. A power consumption device comprising a sodium secondary battery according to any one of claims 23 to 32.