Dip coating kit and capillary coating method

The dip coating chamber and method address the challenge of non-uniform deposition on hydrophobic surfaces by controlling evaporation and capillary forces, achieving high-throughput, selective, and reproducible coating on micro/nanostructured surfaces.

JP2026539226APending Publication Date: 2026-11-20SOLNIL +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2026528202
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-09
Filing Date
2024-11-05
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing dip coating methods struggle with the efficient deposition of liquids that do not naturally wet the substrate surface, particularly on microstructured and nanostructured surfaces, leading to non-uniform and reproducibility issues.

Method used

A dip coating chamber and method that controls evaporation conditions and capillary forces to deposit liquids selectively on microscale or nanoscale patterns, even on hydrophobic surfaces, using a dip coating chamber with specific dimensions and controlled atmosphere to ensure homogeneous and reproducible coating.

Benefits of technology

Enables high-throughput, selective deposition of materials on nanoscale or microscale pitches with improved uniformity and reproducibility, reducing process costs and ensuring stable coating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539226000001_ABST
    Figure 2026539226000001_ABST
Patent Text Reader

Abstract

The present invention provides a dip coating kit, a dip coating apparatus equipped with the kit, and a method for depositing a compound onto the surface of a substrate. [Solution] The dip coating kit comprises a substrate (2) and a dip coating chamber (1) for depositing a liquid formulation onto the substantially planar surface (2.1) of the substrate (2), the chamber (1) comprising a tank (3) for storing the liquid formulation, the tank (3) being closed by a removable lid (4) having a slit (5) for dipping and withdrawing the substrate (2). A method for depositing compound C onto the surface of the substrate (2) comprises introducing the substrate (2) into the dip coating chamber (1) through the slit (5) and immersing the entire portion of the surface (2.1) to be coated in the liquid formulation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention is directed to a dip coating chamber, a dip coating kit comprising a substrate and the dip coating chamber, a dip coater comprising the dip coating chamber, and a method of depositing a liquid on the surface of a substrate. The dip coating chamber is particularly efficient for depositing material onto the surface of a substrate from a liquid formulation that wets the surface of the substrate and evaporates. The dip coating chamber enables liquids that do not naturally wet the substrate to be deposited in an efficient and high-speed manner. The present invention applies to the manufacture and use of surfaces composed of at least two different materials accessible at the air / surface interface, with the distribution of both materials controlled at the microscale and nanoscale. The present invention also applies to the selective deposition of molecules or compositions from a solution onto the patterned surface of a device, particularly within the pitch of a micro- or nanopatterned device.

Background Art

[0002] Microstructured and nanostructured surfaces find application in a variety of technical fields including microelectronics, microfluidics, nanotribology and sensing. They are utilized in a wide range of applications in chemistry and biology, particularly for the detection and measurement of various chemical and biological reactions, as well as for the identification, detection and measurement of various compounds.

[0003] Microstructured and nanostructured surfaces can be used to manipulate very small volumes of gas or liquid, or as conductive probes or neurostimulators, or to provide multiple test surfaces for genetic probes. The present invention relates to a novel dip coater and dip coating method for fabricating arrays of such micro-sized and nano-sized structured surfaces.

[0004] The functionalization of micro / nanostructured surfaces, or micro / nanopatterned surfaces, is an essential process for the manufacture and use of miniaturized objects in micro / nanotechnology. This can involve a variety of techniques, including the deposition of liquids onto the micro / nanopatterned surfaces of substrates. In such processes, controlling the zones into which the liquid is deposited is crucial and can be achieved through various methods, including: - Evaporation-induced self-assembly (EISA): The self-assembly of a single material onto a surface of different properties into a periodic arrangement governed by the presence of a template agent such as latex beads or micelles (M. Faustini and D. Grosso; CR Chimie, 19 (2016) 248e265). This method requires the use of a sacrificial organization-directing agent that needs to be removed. This method is limited to long-range ordering and simple periodic patterns. - Colloidal lithography (CL): The self-assembly of individual objects of a single material in a suspension by evaporation or sedimentation (https: / / doi.org / 10.1016 / j.nantod.2018.08.010). This method is limited to long-range ordering and simple periodic patterns. - Induced self-assembly (DSA) of block copolymers on a pattern-forming surface (DOI: 10.3390 / polym12102432). This method requires the pattern-forming surface to already be heterogeneous in composition in order to induce the organization of the material.

[0005] Dip coating is a well-known method for depositing a liquid onto the surface of a substrate. Generally, the liquid is selected based on its ability to wet the surface of the substrate.

[0006] Japanese Patent Publication No. 55-111868 (Patent Document 1) discloses an immersion coating apparatus for coating the metal surface of an object by raising and lowering the object through a vertical channel leading to a tank in the apparatus. The width of the channel and the width of the object are not disclosed. The apparatus is designed to recover solvent gases generated during the coating process.

[0007] Japanese Patent No. 6039394 (Patent Document 2) discloses a coating tank and dip coater for coating the surface of a plate with a film consisting of a solution. The technical problem is to avoid deterioration of the coating solution due to hydrolysis, which leads to poor reproducibility of the film. The lid at the top of the tank has an opening for inserting and removing plates. The width of the opening and the width of the plates are not disclosed.

[0008] Korean Published Patent No. 2015-0127359 (Patent Document 3) discloses a thin film forming apparatus for dip coating. The surface energy of the substrate is increased by irradiation with ultraviolet light. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 55-111868 [Patent Document 2] Patent No. 6039394 [Patent Document 3] Korean Published Patent Publication No. 2015-0127359 [Overview of the Initiative]

[0010] The dip coating chamber and dip coating kit according to the present invention are typically used to deposit a liquid onto the surface of a substrate, usually using a liquid that does not wet the substrate surface. For example, it enables the deposition of a regular and homogeneous layer of aqueous solution on a hydrophobic surface. It also allows for advanced control of evaporation conditions to improve the thickness homogeneity of the deposited material and the reproducibility of the coating. The method according to the present invention can be carried out with any solvent, even if the surface to be coated does not have affinity for the solvent.

[0011] Precisely arranging nanoscale or microscale patterns on a large scale and at a controlled cost remains a challenge. The dip coating method according to the present invention enables high-throughput, selective deposition of material onto nanoscale or microscale pitches on a single-material array surface, thereby significantly reducing process costs. It also enables the homogeneous deposition of a controlled amount of material per pitch across a large surface. The dip coating method according to the present invention enables high-throughput, selective deposition of material onto nanoscale or microscale polar patches dispersed on a hydrophobic material array surface, thereby significantly reducing process costs. It also enables the homogeneous deposition of a controlled amount of material per patch across a large surface. The apparatus and method according to the present invention have the advantage of providing highly reproducible results.

[0012] A first object of the present invention is a dip coating chamber for depositing a formulation F containing compound C in a volatile liquid solvent onto the surface of a substantially planar substrate having a width (W2), wherein the dip coating chamber is - A tank for storing compound F, the tank having an opening at the top, -A removable lid having an upper and lower surface and positioned over the opening of the tank, the lid having a slit leading into the tank as a vertical channel for dipping and lifting the substrate, the vertical channel having an upper end and a lower end and a width (W1), the lid and -A drying chamber located above the lid, the drying chamber having a lower surface located on the upper surface of the lid, the drying chamber having an opening on its lower surface, the opening facing the upper end of the channel, and the drying chamber having an upper surface with a slit that allows the substrate to be introduced and pulled up, and Equipped with, The channel width (W1) and the substrate width (W2) are set so that the value of (W1-W2) / 2 is between 0.2 and 10 mm.

[0013] The present invention also relates to a dip coating kit, which includes a substrate and a dip coating chamber, as defined above and described in detail below.

[0014] According to one embodiment of a dip coating chamber, Vs is the volume of the substrate immersed in the compound F during dipping, and the shape of the tank and the volume of the compound F while stored in the tank cause the compound F to show the upper surface of the surface Sl, and the ratio Vs / Sl satisfies the relationship Vs / Sl ≤ 1 mm.

[0015] According to one embodiment of a dip coating chamber, the channel comprises a vertical wall extending downward from the underside of the lid.

[0016] According to one embodiment of a dip coating chamber, the top surface of the lid has a notch surrounding a slit, and the lower part of the drying chamber is located within the notch.

[0017] In one embodiment of a dip coating chamber, the lid closes the tank in a solvent-sealed manner, except for the slit.

[0018] In one embodiment of a dip coating chamber, the temperature and vapor pressure inside the drying chamber are controlled.

[0019] The present invention is also directed to a dip coating apparatus including a dip coating chamber as disclosed above and described in detail below, the dip coating apparatus further includes - Substrate holding unit, and / or - A lifting device for raising and lowering a substrate holding unit, and / or - A motor for controlling the raising and lowering of the substrate, and / or - Software / hardware coupled to the device to control the device's operating parameters. It is equipped with.

[0020] The present invention is also directed to a method for depositing Compound C on the surface of a substrate, the method comprising: - filling the tank of a dip coating chamber, as disclosed above and described in detail below, with Formulation F comprising Compound C and a volatile liquid solvent; - introducing the substrate through a vertical channel into the dip coating chamber, and immersing the entire portion of the surface to be coated in Formulation F; - lifting the substrate through the vertical channel into a drying chamber; - holding the substrate in the drying chamber for a time sufficient to evaporate the liquid solvent, and controlling the atmosphere .

[0021] According to one embodiment, the surface of the substrate comprises flat regions and microscale to nanoscale topographical features with a lateral dimension (l) of 20 nm to 200000 nm, preferably 50 nm to 50000 nm.

[0022] According to one embodiment, the microscale to nanoscale topographical features comprise nano-sized or micro-sized pitches engraved on the surface of the substrate.

[0023] According to one embodiment, the nano-sized or micro-sized pitches are characterized by an aspect ratio r, where r = depth of the pitch / the smaller lateral dimension, and r ≧ 0.01.

[0024] According to one embodiment, the depth (p) of the pitches of the substrate is 5 nm to 100000 nm, preferably 20 nm to 1000 nm.

[0025] According to one embodiment, the flat regions are composed of a hydrophobic material, and the microscale to nanoscale topographical features are composed of a polar material.

[0026] According to one embodiment, the entire surface of the substrate is flat.

[0027] According to one embodiment, the volatile liquid solvent includes water.

[0028] According to one embodiment, the liquid level of the compound F in the tank is above the lower end of the channel.

[0029] According to one embodiment, the volume and shape of the tank and the shape of the lid are configured such that, during a series of deposition cycles of the compound F onto the substrate, the liquid level of the compound F in the tank remains above the lower end of the channel.

[0030] The dip coating chamber according to the present invention is useful for depositing a coating layer on the surface of a substrate having a micro-size or nano-size design, or alternatively, on a uniform surface of the substrate. In either case, it provides a coating with improved homogeneity and a coating process with improved reproducibility.

[0031] The method according to the present invention can be carried out with any solvent that can solubilize, suspend, or disperse compound C, even if the surface to be coated does not have affinity for that solvent.

[0032] The method according to the present invention has the advantage of enabling the selective deposition of compound C, which is solubilized, suspended, or dispersed in water, a water-rich solvent mixture, or another high-surface-tension solvent, within and / or on a design on the surface of a substrate.

[0033] The method according to the present invention makes it possible to selectively deposit compound C, which is solubilized, suspended, or dispersed in water or other high surface tension solvents, even if the surface flats and design are made of hydrophobic material and would normally repel high surface tension solvent (particularly aqueous) solutions, suspensions, or dispersions of compound C.

[0034] The dip coating chamber design according to the present invention results in improved uniformity and reproducibility of the coating, as well as improved stability of the coating conditions. The resulting coated substrate has the characteristic of high uniformity.

[0035] Combinations of embossed designs on the substrate surface or spotted designs on the substrate surface allow for better control of the capillary forces governing the deposition process, thereby enabling selective deposition of the compound onto the design.

[0036] Detailed explanation The phrase "consists essentially of," followed by one or more features, means that, in addition to the explicitly listed components or processes, components or processes that do not substantially affect the properties and features of the present invention may be included in the processes or materials of the present invention.

[0037] The phrase "comprised between X and Y" includes boundary values ​​unless explicitly stated otherwise. This expression means that the range includes the values ​​of X and Y, as well as all values ​​from X to Y.

[0038] Throughout this specification and its claims, the words “comprise” and “contain,” and their variations, such as “comprising” and “comprises,” mean “include, but not limited to,” and do not exclude other parts, additions, components, elements, or processes. Furthermore, unless otherwise required by context, the singular form includes the plural form. In particular, where the indefinite article is used, this specification is understood to assume both plural and singular forms unless otherwise required by context.

[0039] When upper and lower limits are cited for a characteristic (for example, for the concentration of a component), the range of values ​​defined by any combination of upper and lower limits may also be implied.

[0040] The present invention relates to the functionalization of substrates of various designs, including a flat substrate made of a single material, and a substrate having micro-patterns or nano-patterns within and / or on the surface, wherein the surface and pattern are made of the same or different materials.

[0041] For all types of substrates, the design of the dip coating chamber improves the homogeneity and reproducibility of the coating, as well as the stability of the coating conditions.

[0042] For substrates with flat surfaces and microscale to nanoscale topographic features, thanks to the selection of specific parameters of the dip coater, formulations containing the target compound (compound C) can be selectively deposited within and / or on the pattern, which are zones with higher capillary forces and / or greater concavity, while the flat areas of the surface remain substantially free of compound C.

[0043] In the context of this invention, the terms "cavity," "well," and "pitch" can be used interchangeably and refer to holes engraved on the surface of a substrate in the depth direction of the surface material. The walls and bottom of the pitch are made of the material on which the surface is formed.

[0044] In the context of this invention, the expressions "microscale to nanoscale topographical feature" and "nano-sized or micro-sized pattern" refer to a feature or pattern whose one or more dimensions (depth, length, width, diameter) are in the nanometer range or micrometer range. Preferably, "nano-sized or micro-sized pattern" refers to a pattern whose two or more dimensions (depth, length, width, diameter) are in the nanometer range or micrometer range. The nanometer range means 1 to 1000 nanometers, and the micrometer range means 1 to 1000 micrometers.

[0045] The dimensions of the pattern can be measured by any known method, particularly by analysis of images obtained by scanning electron microscopy (SEM). [Brief explanation of the drawing]

[0046] [Figure 1A] This is a cross-sectional view of the dip coating chamber according to the present invention, showing modified examples of chamber design and operating conditions. [Figure 1B] This is a cross-sectional view of the dip coating chamber according to the present invention, showing modified examples of chamber design and operating conditions. [Figure 2] This is a cross-sectional view of a part of the dip coating chamber according to the present invention, focusing on the vertical channel that can be used for dipping and pulling up the substrate. [Figure 3] This is a plan view of the dip coating chamber according to the present invention. [Figure 4A] In Example 1, this is a photograph of a coated plate obtained by dip-coating a silicon plate in the dip-coating chamber according to the present invention (Example 1 - Figure 4A). [Figure 4B] In Example 2, this is a photograph of a coated plate obtained by dip-coating a silicon plate in a conventional dip-coating chamber (Example 2 - Figure 4B). [Figure 4C] In Example 3, this is a photograph of a coated plate obtained by dip-coating a silicon plate in a conventional dip-coating chamber (Example 3 - Figure 4C). [Figure 5A] This is a plan view showing an example of a substrate having a flat surface including pitch. [Figure 5B] This is a cross-sectional view showing an example of a substrate having a flat surface including pitch. [Figure 6A] This is an SEM image corresponding to a substrate obtained by dip coating a plate having a nanopitch pattern in a dip coating chamber in which TiO2 is deposited from an aqueous formulation of TiCl4 into nanocavities on the surface of SiO2. In Example 4-Figure 6A, the dip coating chamber is according to the present invention. [Figure 6B]This is an SEM image corresponding to a substrate obtained by dip coating a plate having a nanopitch pattern in a dip coating chamber where TiO2 is deposited from an aqueous TiCl4 mixture into nanocavities on the surface of SiO2. In Example 5-Figure 6B, the dip coating chamber is based on conventional technology. [Modes for carrying out the invention]

[0047] To facilitate the reading of drawings, objects or parts of objects with the same function are represented by the same reference numeral in different drawings.

[0048] In the drawing, axes XX and ZZ are horizontal, and axis YY is vertical. The "up" and "down" indications are based on the vertical axis YY.

[0049] [Dip coating chamber] The dip coating chamber 1 according to the present invention is shown in Figures 1A, 1B, 2, and 3 together with a substrate 2 introduced into the dip coating chamber 1 to deposit compound C from a formulation F onto one surface of the substrate. The substrate 2 is a rectangular plate.

[0050] The dip coating chamber 1 includes a tank 3 for storing a formulation F containing compound C in a volatile liquid solvent.

[0051] In Figure 1A, the tank 3 is rectangular in shape, the bottom 3.2 of the tank 3 is flat and horizontal, and the walls 3.8 of the tank 3 are vertical.

[0052] In Figure 1B, tank 3 has a more complex shape, the details of which will be explained in a specific chapter.

[0053] Tank 3 has an opening 3.1 at its top.

[0054] Tank 3 is made of a material suitable for storing liquids; for example, the tank may be made of glass or polymer.

[0055] The dip coating chamber 1 is equipped with a removable lid 4 having an upper surface 4.1 and a lower surface 4.2, the lower surface 4.2 resting on the tank wall 3.8 and positioned over the tank opening 3.1, and partially closing the tank opening 3.1. The lid 4 prevents evaporation of the solvent of the compound F when the dip coating chamber is in use.

[0056] The tank 3 can be filled and / or cleaned by removing the lid 4. The lid 4 has a substantially rectangular shaped slit 5 that leads into the tank 3.

[0057] Slit 5 has a longitudinal shape parallel to axis ZZ.

[0058] The slit 5 leads into the tank 3 and extends into the tank 3 as a vertical channel 6 through which the substrate 2 can be dipped and pulled out.

[0059] When the lid 4 is placed on the tank 3, the slit 5 allows communication between the internal volume of the tank 3 and the internal volume of the drying chamber 7.

[0060] In Figures 1A and 1B, the lid 4 consists of two levels: an upper level 4.3 located at its periphery and part of its central region, and a lower level 4.4 located above part of the central region. The lower level 4.4 is above the area of ​​the tank 3 that is deep enough to dip the substrate 2. The upper level 4.3 and the lower level 4.4 are connected by a vertical wall 4.5.

[0061] The lower level 4.4 of the lid 4 is centered around the slit 5, and the portion of the lid 4 consisting of the wall 4.5 and the lower level 4.4 forms a notch or recess 8 that accommodates the lower part 7.6 of the drying chamber 7. Other arrangements between the lid 4 and the drying chamber 7 are possible, as long as it is possible to close off the lower part 7.6 of the drying chamber 7 and thereby control the atmosphere in the channel 6 and the drying chamber 7.

[0062] In Figures 1A and 1B, the lid 4 is placed on the side wall 3.8 of the tank 3, except for the slit 5, to close the tank 3 in a solvent-sealed manner. Other arrangements are possible to avoid evaporation of the solvent contained in the tank 3.

[0063] In Figures 1A and 1B, the slit 5 and the drying chamber 7 are located on one side of the lid 4. This arrangement facilitates the combination of the dip coating chamber 1 with a mechanized arm (not shown) for handling the substrate 2 in and out of the dip coating chamber 1. Alternatively, the slit 5 can be located in a more central part of the lid 4.

[0064] The lid 4 is made of a material suitable for this application. For example, the lower surface 4.2 of the lid 4, which is partially immersed in or in contact with the solution F in Figures 1A and 1B, is covered with a hydrophobic layer, preferably a layer of polytetrafluoroethylene.

[0065] The vertical channel 6 has an upper end 6.1 and a lower end 6.2. In Figures 1A and 1B, the channel 6 extends below the level of the lower surface 4.2 of the lid 4. Other configurations are possible, and the channel 6 may be defined by a simple opening of the slit 5 within the lid 4 without extending below the lower surface 4.2 of the lid.

[0066] The slits 5 and channels 6 are sized such that the substrate can be introduced into and pulled up from the tank 3 without contacting the wall 6.3 of channel 6 (shown in Figure 2). They are sized such that the distance between the wall 6.3 of channel 6 and the surface 2.1 of the substrate 2 is minimized.

[0067] As shown in Figure 2, the channel 6 has a width W1 and the substrate has a width W2. The distance between the surface 2.1 of the substrate 2 and the wall 6.3 of the channel 6 is denoted as d, and by controlling this parameter, the regular deposition of the liquid formulation F onto the surface 2.1 of the substrate 2 as it is immersed and withdrawn through the channel 6 can be controlled. Controlling the width W1 also leads to minimizing evaporation from the tank to the drying chamber 7.

[0068] A simple way to control the distance d is to position the substrate 2 substantially in the center relative to the channel 6 and to control W1 and W2 so that the distance between the surface 2.1 of the substrate 2 and the wall 6.3 of the channel 6 is approximately equal to (W1-W2) / 2.

[0069] According to the present invention, (W1-W2) / 2 is 0.2 mm to 10 mm, preferably 0.2 mm to 5 mm, more preferably 0.5 to 4 mm, and even more preferably 1 to 2 mm. This value range allows for control of the distance d between the surface 2.1 of the substrate 2 and the wall 6.3 of the channel 6, and enables the regular and homogeneous deposition of the compound F on the surface 2.1 of the substrate 2.

[0070] If the distance d exceeds 10 mm, evaporation of the solvent from tank 3 occurs more rapidly. If the distance d is less than 0.2 mm, the meniscus at the liquid / gas / substrate interface may be disturbed.

[0071] The distance between the side surface of the substrate 2 and the end wall of the channel 6 should also be kept small (e.g., 0.2 mm to 10 mm), thereby minimizing solvent evaporation.

[0072] According to the modified examples shown in Figures 1A, 1B, and 2, the volume and shape of the tank 3 and the shape of the lid 4 (particularly the channel 6) are configured such that, during a series of cycles of depositing the compound F onto the substrate 2, the liquid level 10 of the liquid (compound F) in the tank 3 remains above the lower end 6.2 of the channel 6.

[0073] As shown in Figure 2, when the substrate 2 is removed from the compound F, the proximity of the surface 2.1 to the wall 6.3 results in a stable meniscus 9 and regular deposition of the compound F on the surface 2.1 of the substrate 2.

[0074] Since the slits 5 and channels 6 have a small width W1, the transfer of volatile solvents (from the formulation F) by evaporation from the tank 3 to the drying chamber 7 is minimized.

[0075] In a preferred modification, the surface 10 of the liquid formulation F in the tank 3 is large enough so that the liquid level of the liquid formulation F in the tank 3 does not fluctuate substantially due to repeated immersion and withdrawal of the substrate 2 into the formulation F.

[0076] To obtain this constant liquid level in tank 3, the shape and volume of tank 3 must be controlled as a function of the volume of the substrate 2 immersed in the liquid. The portion of the substrate 2 immersed in the liquid induces a change in the volume of the liquid. The volume of the substrate 2 immersed in the liquid is denoted as Vs. Due to the shape of tank 3 and the volume of the mixture F in tank 3, the mixture F has an upper surface 10 on its surface Sl.

[0077] To obtain a substantially constant liquid level in tank 3, the ratio Vs / Sl is advantageously satisfied with the relationship Vs / Sl ≤ 1 mm.

[0078] In a more preferred embodiment, Vs / Sl ≤ 0.5 mm.

[0079] The tank 3 shown in Figure 1B is designed to reduce the volume of liquid stored in the tank 3 compared to the apparatus in Figure 1A, while ensuring that the liquid formulation F has a large upper surface 10 of surface Sl. The bottom 3.2 of the tank 3 is not flat, but has a flat horizontal section 3.3 located at a lower level below the channel 6, thereby ensuring that a sufficient volume of formulation F is stored below the slit 5 for the substrate 2 to be immersed in the liquid. The tank 3 also has a flat horizontal section 3.6 located at a higher level compared to the lower section 3.3, as well as legs 3.5 for leveling the tank 3. The flat horizontal sections 3.3 and 3.6 are connected by a vertical wall 3.4 which may be linear or may form an angle 3.7 as shown in Figure 1B.

[0080] Other configurations of the tank 3 are also possible, as long as there is enough liquid volume below the channel 6 to allow the substrate 2 to be dipped into the liquid. A configuration of the tank 3 with two different bottom levels, 3.3 and 3.6, allows for maximizing the surface area 10 of the liquid formulation F while minimizing the volume of the liquid formulation F.

[0081] As shown in Figures 1A, 1B, and 3, the dip coating chamber 1 further comprises a drying chamber 7 which is substantially rectangular in shape and defines an internal space 7.5. The drying chamber 7 has a bottom surface 7.1 located on the top surface 4.1 of the lid 4 and cooperates with the lid 4 in a manner that allows for control of the atmosphere in the channel 6 and the internal space 7.5 of the drying chamber 7. Preferably, the bottom surface 7.1 of the drying chamber 7 and the top surface 4.1 of the lid 4 cooperate in a solvent-sealed manner to prevent evaporation of the solvent from the tank 3 and to maintain control of the atmosphere in the internal space 7.5 of the drying chamber 7.

[0082] The drying chamber 7 has an opening 7.2 on its bottom surface 7.1, which faces the upper end 6.1 of the channel 6, so that the substrate 2 is directly pulled up from the tank 3 into the internal space 7.5 of the drying chamber 7 through the channel 6. The top surface 7.3 of the drying chamber 7 has a slit 7.4 through which the substrate 2 can be introduced and pulled up. The slit 7.4, the opening 7.2, the slit 5, and the channel 6 define a vertical plane parallel to the plane defined by (YY) and (ZZ), and vertical movement of the substrate 2 can be carried out through this vertical plane.

[0083] In the dip coating chamber 1 according to the present invention, the temperature in the internal space 7.5 of the drying chamber 7 is advantageously controlled to allow evaporation of the solvent (from the compound F). Preferably, the atmosphere is controlled at a temperature of 20°C or higher. The temperature is adapted by those skilled in the art depending on other parameters (such as the material deposited on the substrate and the risk of ignition of the solvent).

[0084] Advantageously, the dip coating chamber is used in combination with a substrate holding unit, which is not shown in the drawings but is well known in the art.

[0085] The drying chamber 7 is designed to allow minimal exchange with the atmosphere in order to maintain drying conditions within the internal space 7.5. Means for achieving such results include, for example, a solvent-sealed joint between the chamber bottom 7.1 and the lid 4, a reduced size of the slit 7.4, and a system for closing the opening 7.4 around the substrate holding unit.

[0086] The drying chamber 7 is constructed of a material suitable for controlling the atmosphere inside the chamber. For example, the drying chamber 7 can be made of stainless steel. Controlling the atmosphere inside the chamber means controlling the temperature and vapor pressure.

[0087] The dip coating chamber according to the present invention may be part of a dip coating apparatus (dip coater) further equipped with other devices to facilitate handling of the substrate, as is well known to those skilled in the art. In particular, the following can be mentioned: - A lifting device for raising and lowering the substrate holding unit. - A motor for controlling the raising and lowering of the substrate, and / or - Software / hardware integrated into the device to control parameters (speed, temperature, pressure, etc.) of the dip coating method.

[0088] The dip coating chamber 1 according to the present invention enables the deposition of compound C onto the surface 2.1 of a substrate 2 from a volatile liquid formulation F stored in a tank 3.

[0089] Advantageously, the substrate 2 is substantially planar.

[0090] According to the first embodiment shown in Figure 5A, the surface 2.1 of the substrate 2 is patterned. According to another embodiment, the surface 2.1 of the substrate 2 is flat, that is, it does not have any pattern.

[0091] In Figures 1A, 1B, and 2, the substrate 2 is introduced into the dip coater through slit 7.4, then immersed in the liquid formulation F through slit 5 and channel 6 of the lid 4, and subsequently pulled up through the same path and returned to the internal space 7.5 of the drying chamber 7.

[0092] As the substrate 2 is pulled up through the channel 6, controlling the distance d between the surface 2.1 of the substrate 2 and the wall 6.3 of the channel 6, combined with controlling the atmosphere in the drying chamber 7, results in the stable meniscus 9 shown in Figure 2, as well as the controlled deposition of the liquid formulation F and the evaporation of the solvent therefrom.

[0093] Compound C is dissolved, suspended, or dispersed in the formulation F, and so, after the formulation F is deposited on the surface 2.1, the solvent is evaporated in the internal space 7.5 of the drying chamber 7.

[0094] Suitable substrates for implementing this method are described in detail below.

[0095] [Base material] The present invention relates to a method for functionalizing a substrate in which the substrate is substantially planar. Advantageously, and as shown in the drawings, the substrate 2 is rectangular in shape, and more advantageously, the substrate 2 is a plate.

[0096] According to the first embodiment, the surface 2.1 of the substrate 2 is flat and consists of a single material. The design of the coating chamber has the advantage of allowing homogeneous and reproducible deposition of the coating onto the surface 2.1 of the substrate 2 for such a substrate, as shown in the experimental section (Examples 1 and Comparative Examples 2 and 3). This advantage is particularly evident when the solvent of the substrate 2 and the formulation F do not have affinity, for example, when the surface consists of a hydrophobic material such as silicate and the solvent is an aqueous solvent such as water or a mixture of water and another high surface tension solvent.

[0097] The present invention is further particularly useful in the deposition of liquids within and / or on nano-sized or micro-sized patterns on the surface of a substrate, as shown in Figures 5A and 5B.

[0098] Advantageously, the substrate includes a flat region 2.2 and a surface 2.1 having nano-sized or micro-sized patterns 2.3, 2.3.1 provided within and / or on the surface 2.1.

[0099] Preferably, the patterns 2.3, 2.3.1 within and / or on the substrate 2 are arranged regularly or in an array, meaning that their size and spacing are uniform. Regular arrangement facilitates large-scale processing of samples for analysis or to carry out other reactions. However, substrates in which the patterns have an irregular shape and an irregular or random surface distribution are also within the scope of the present invention.

[0100] According to the first embodiment, the nano-sized or micro-sized pattern consists of micro-sized or nano-sized reliefs 2.3.1 on the surface 2.1 of the substrate 2. Thus, the substrate includes substantially flat regions 2.2, as well as micro-sized or nano-sized reliefs 2.3.1 arranged on the surface 2.1.

[0101] Preferably, the nano-sized or micro-sized pattern is a nano-sized or micro-sized pitch or cavity 2.3.1 engraved or embossed on the surface 2.1 of the substrate 2.

[0102] In a preferred embodiment, the surface pattern of the substrate is designed such that the liquid formulation F is held in the pitch or cavity 2.3.1 by capillary force, and that the flat areas 2.2 of the surface 2.1 are not wetted by the liquid formulation F after the substrate 2 is removed from the tank 3.

[0103] Preferably, the surface 2.1 of the substrate 2 is substantially flat, and more preferably, the surface 2.1 of the substrate 2 is flat except for the pattern 2.3.1 provided thereon. The portion of the surface 2.1 not occupied by the pattern is indicated as a flat region 2.2. The flat region 2.2 represents a continuous surface interrupted by the pattern.

[0104] Nano-sized or micro-sized patterns are preferably pitches or cavities. In the context of the present invention, the terms “cavity,” “well,” and “pitch” can be used interchangeably and refer to micro-sized or nano-sized holes engraved on the surface 2.1 in the depth direction of the surface material. The walls and bottoms of the pitch may be made of the material constituting the surface or of another material. According to a preferred embodiment, the walls and bottoms of the pitch are made of the material constituting the surface.

[0105] A pattern (especially a micro / nanopitch) is defined by its shape and dimensions. The cross-sectional dimensions of a pattern (especially a micro / nanopitch) are shown by l in Figure 5A and can range from a few nanometers to a few millimeters. A pattern (especially a pitch) can be a centrally symmetric shape, such as a circle, as shown in Figure 5A, but it may also be a triangle, square, or polygon. Alternatively, a pattern (especially a micro / nanopitch) may be a planar symmetric shape; for example, a pattern (especially a micro / nanopitch) may be an oval, rectangular, or linear shape with one cross-sectional dimension being micro / nanometer-sized and the other cross-sectional dimension being on a larger scale. Alternatively, a pattern (especially a micro / nanopitch) may be asymmetric.

[0106] If desired, patterns of different dimensions and shapes (especially pitches) may exist within a single substrate; however, for the manufacture and use of patterned substrates, it is generally more convenient if all patterns (more specifically, all pitches) have the same dimensions and shape.

[0107] According to a preferred embodiment relating to a substrate having a nano-sized or micro-sized pitch, these pitches are characterized by their aspect ratio r. In defining the aspect ratio r of the pitch, the ratio of the pitch depth to the minimum cross-sectional dimension is adopted. For a circular pitch, r is the ratio of the pitch depth, indicated by p in Figure 5B, to the pitch diameter, indicated by l in Figure 5A. For a linear pitch, r is the ratio of the depth to the width of the line segment.

[0108] According to a preferred embodiment, the substrate 2 includes nano-sized or micro-sized pitches having an aspect ratio of r = pitch depth / smaller lateral dimension, and r ≥ 0.01, advantageously r ≥ 0.03, and even more preferably r ≥ 0.1.

[0109] For the substrates shown in Figures 5A and 5B, r = p / l.

[0110] According to a preferred embodiment, the pitch depth p of the substrate 2 is 5 nm to 100,000 nm, preferably 20 to 1,000 nm.

[0111] According to a preferred embodiment, the substrate 2 includes microscale to nanoscale topographic features having a lateral dimension l of 20 nm to 200,000 nm, preferably 50 to 50,000 nm.

[0112] This parameter selection results in efficient capillary action of the formulation F into the pitch when using the dip coating chamber according to the present invention.

[0113] The pitch distance can range from 10 nm to approximately 100 mm.

[0114] According to this preferred embodiment, the surface of the substrate 2 may contain other pitches with an aspect ratio r < 0.01, which are not affected by the deposition of the compound on the surface.

[0115] According to a preferred embodiment, the substrate preferably includes a support and a layer of material M on the surface of the support. The support may be composed of any material suitable for the future use of the substrate, such as metal, glass, or polymer.

[0116] For example, material M may be a hydrophobic material selected from metals, ceramics, hydrophobic polymers, or hybrid materials.

[0117] Examples of metals include aluminum, silicon, or gold.

[0118] Examples of ceramics include SiO2, Al2O3, SiC, SiN, and TiN.

[0119] Among hybrid materials, silicone or PDMS can be mentioned.

[0120] Examples of hydrophobic polymers include PTFE, PS, and PET.

[0121] In a preferred modification, the surface of the substrate is made of a material M selected from hybrid metal oxides such as PDMS, and preferably the surface of the substrate is made of SiO2 functionalized with methyl groups using a coupling agent such as (Si(OEt)3(Me)1).

[0122] The thickness of the surface material is advantageously greater than the depth of the pitch, so that the pitch is engraved within the surface material and does not communicate with the support.

[0123] Alternatively, the substrate surface is substantially flat and includes a dominant region of hydrophobic material M and a pattern of polar patches located within or on the surface of material M. Such a surface can be obtained by methods such as those disclosed in Polymers 2020, 12(10), 2432; DOI: 10.3390 / polym12102432. When the substrate is dipped in a formulation F containing compound C and an aqueous solvent, the hydrophobic surface does not retain the formulation F, while the polar patches fix the formulation. After drying, this results in selective coating of compound C on the polar patches.

[0124] [Formulation F] The present invention enables the deposition of compound C, which is solubilized, suspended, or dispersed in a solvent composition. Formulation F comprises compound C and a liquid solvent composition.

[0125] Formula F is designed to satisfy the following constraints. -It is the vehicle of compound C, - The liquid solvent composition is evaporable.

[0126] Formulation F is said to be a vehicle for compound C, meaning that compound C is suspended, dispersed, or solubilized in the solvent or solvent mixture of formulation F.

[0127] According to a preferred embodiment, the compound F does not wet the material in the flat areas of the substrate surface. This means that if the substrate 2 is flat or contains a pitch of r < 0.01, the solution F does not wet the surface of the substrate 2. This characteristic is determined experimentally by dipping the substrate 2 into the solvent or solvent mixture of the compound F and observing the result, without using the dip coating chamber according to the present invention.

[0128] Alternatively, those skilled in the art know of many examples of materials that are not wetted by solvents or solvent mixtures. For example, metal surfaces such as silica, or metal oxide surfaces such as silica or titanium oxide, are not wetted by water, or by mixtures of water with a slightly less polar solvent such as THF or acetone.

[0129] In the case of substrates exhibiting an entirely flat surface, i.e., a non-pattern-forming surface, the inventors observed that even when the solvent of the formulation F does not normally wet the substrate surface, such as an aqueous solvent and a silicon surface, the deposition of formulation F in the dip coating chamber according to the present invention is extremely homogeneous compared to the deposition of the same formulation in a conventional dip coating chamber. The specific configuration of the dip coating chamber provides control of capillary forces and enables extremely regular coating of the substrate by the liquid formulation compared to conventional coating chambers.

[0130] When the surface of the substrate is patterned, compound C is deposited within and / or in the design, preferably in the pitch or cavity, on the surface of the substrate.

[0131] If a design (preferably a pitch or cavity 2.3.1) is present, the compound F is held in place by the design (preferably a pitch or cavity 2.3.1), while on the flat area 2.2 of the substrate surface, the compound F is rapidly removed. Finally, the liquid is fixed onto the cavity 2.3.1 by capillary force. Compound C dries and aggregates at the bottom of the cavity 2.3.1.

[0132] This combination of features makes it possible to deposit liquid only within the cavities or pitch of the substrate, and not on the flat areas of the substrate surface.

[0133] According to a preferred embodiment, formulation F comprises a mixture of a high surface tension solvent A and a low surface tension solvent B, and the presence of both solvents makes it possible to form a homogeneous wetting layer on the pattern-forming surface.

[0134] According to a preferred embodiment, the high surface tension solvent A is water.

[0135] According to a preferred embodiment, the low surface tension solvent B is selected from THF, acetone, and mixtures thereof.

[0136] According to one embodiment, water is the solvent of compound F.

[0137] [Compound C] Compound C may be a single compound or a composition of substances such as a mixture or complex structure of molecules. For example, Compound C may be a dissolved salt, suspended nanoparticles, a macromolecule such as RNA, DNA, or polymer, or a chemical composition.

[0138] In the method according to the present invention, compound C is ultimately deposited on the flat surface of the substrate 2 if the entire substrate 2 is flat, or within and / or on the design of the substrate surface (e.g., within the bottom of the pitch or cavity 2.3.1 of the substrate), and provides functionalization of the design (preferably pitch or cavity) that is different from the flat region 2.2 of the substrate surface.

[0139] According to a preferred embodiment, compound C is a metal oxide and is different from any metal oxide that may constitute the surface. When compound C is a metal oxide, it can be selected from, for example, TiO2, SnO2, or Y2O3, and is obtained by sol-gel chemistry in solution, in which a precursor (salt, organometallic, etc.) is hydrolyzed and partially condensed into a final metal oxide intermediate, which is a hydroxo-oxocluster or nanoparticle. According to a preferred embodiment, compound C is TiO2 and is obtained by hydrolysis / condensation of TiCl4 in formulation F according to well known sol-gel chemistry.

[0140] According to a preferred embodiment, compound C is a metal salt, such as a metal chloride. When compound C is a metal salt, it can be selected from, for example, AuCl3, AgNO3, and the like.

[0141] The dip coating chamber according to the present invention is particularly useful in that it allows a material (compound C) dispersed, suspended, or solubilized in an aqueous solvent to be deposited onto a surface made of a material that is not normally wetted by an aqueous composition.

[0142] This invention enables access to material arrangements (surface materials, pitch materials) that are difficult or costly to obtain by conventional methods.

[0143] This invention enables access to a coated substrate obtained by coating it from a liquid formulation that does not have affinity with the surface material of the substrate.

[0144] [Deposition method] The method for depositing solute C onto the surface of a substrate, as shown in Figures 1A, 1B, and 2, includes filling a tank 3 of a dip coating chamber 1 with a formulation F containing solute C and a liquid solvent.

[0145] Next, the substrate 2 is introduced into the dip coating chamber 1 through the drying chamber 7 and vertical channel 6, and the entire surface 2.1 to be coated is immersed in the formulation F.

[0146] The substrate 2 is lifted into the drying chamber 7 in a vertical plane through the channel 6, and the distance between the coated surface 2.1 of the substrate 2 and the wall 6.3 of the channel 6 is controlled to 0.2 to 10 mm. Controlling the distance between the coated surface 2.1 and the wall 6.3 of the channel 6 results in a stable meniscus at the interface between the surface 2.1, air, and liquid mixture, which in turn results in the regular deposition of the liquid on the surface 2.1 of the substrate.

[0147] The substrate 2 emerges from the liquid into the drying chamber 7, where it is held for a sufficient amount of time to evaporate the liquid solvent.

[0148] Preferably, the shape of the tank 3 and the volume of the compound F inside the tank 3 are such that the volume of the substrate 2 immersed in the compound F induces a change in the liquid level of the compound F that is negligible.

[0149] Furthermore, the volume of liquid deposited on the surface 2.1 of the substrate 2 represents a negligible proportion of the volume of the compound F. Therefore, even if this method is repeated, the liquid level 10 on the surface of the compound F does not change significantly, and generally constant deposition conditions are applied.

[0150] In summary, part or all of the tank 3 has sufficient depth to allow the substrate 2 to be immersed in the compound F. In a preferred embodiment, the tank 3 has a very large top surface 10, so that the compound F spreads widely within the tank 3, and the immersion of the substrate in the compound F does not significantly change the liquid level within the tank 3.

[0151] Most preferably, if Vs is the volume of the substrate 2 immersed in the compound F, then, depending on the shape of the tank 3 and the volume of the compound F in the tank 3, the compound F will show the upper surface 10 of the surface Sl, and the ratio Vs / Sl will satisfy the relationship Vs / Sl ≤ 1 mm.

[0152] Deposition can be carried out in a single step for a given substrate and compound.

[0153] Alternatively, the deposition process can be repeated to deposit a larger amount of compound C on the substrate surface. If deposition of two or more different materials is required, the sequential deposition of materials can be carried out using different compositions.

[0154] If compound C deposited on the surface of the substrate is soluble in the solvent of the subsequent deposition formulation, it is recommended to perform a treatment step on the coated substrate before subsequent deposition to prevent the dissolution of the first coating during subsequent deposition. This applies, for example, when compound C is a salt or polymer.

[0155] In other cases, the deposition process can be repeated without intermediate treatment. For example, if compound F is a sol-gel composition, deposition can be repeated several times on the same substrate without intermediate treatment.

[0156] [Application] The present invention is applied to the manufacture of a substrate in which the surface is composed of at least two different materials accessible at the air / surface interface, and the distribution of these two materials is controlled. Here, the two materials are a material that constitutes a flat region surface and a material that is deposited in the pitch and covers at least a portion of the bottom of the pitch.

[0157] Furthermore, the present invention applies to the manufacture of a substrate coated with a uniform and continuous material deposited on its surface, wherein the material is dispersible or soluble in a solvent that does not normally wet the surface.

[0158] In microfluidics and combinatorial chemistry, it is often necessary to manipulate extremely small volumes of gas or liquid, such as picoliters, and selectively deposit them into cavities or wells of a substrate. Fabricating substrates that contain cavities sized to meet such requirements and that allow for the selective and inexpensive deposition of liquids is challenging.

[0159] The method according to the present invention makes it possible to functionalize pitch in a substrate with a material different from the substrate surface material. For example, it makes it possible to functionalize pitch in a substrate with a metal salt or metal oxide, and to functionalize a flat region of the substrate with another material, such as another metal oxide, particularly SiO2. It also makes it possible to functionalize pitch in a substrate with a polymer such as DNA or RNA, either directly or in a subsequent selective deposition step based on the affinity of the polymer to the material deposited at the bottom of the pitch.

[0160] This method is easy to implement and does not require any specific tools. It also offers high selectivity for deposits.

[0161] This method can be applied to the dispensing and manipulation of DNA or RNA samples, combinatorial chemistry, or materials science applications. For example, it can be applied to the manufacture of micro- and nano-sized electrodes, or micro- and nano-sized heating devices. It can also be applied to optoelectronics, the manufacture of metasurfaces, the manufacture of metalens, and so on. Functionalized substrates obtained from this method can be applied to the detection and measurement of one or more analytes, the analysis of numerous genes, and so on.

[0162] Laboratory Department: The methods of Example 1 and Example 4 are carried out in a dip coater according to the present invention, which is equipped with a dip coating chamber corresponding to that shown in Figure 1A and has the following features.

[0163] The slit is 5mm wide and 100mm long.

[0164] The base material is a plate with a width of 9.6 mm and an immersion length of 100 mm.

[0165] The tank is a rectangular prism with dimensions of 21cm x 21cm x 15cm (height).

[0166] The lifting speed is 0.2 mm·s. -1 It is controlled by [something].

[0167] The drying chamber is under controlled temperature.

[0168] The methods in Examples 2, 3, and 5 are carried out in a conventional dip coater with the same characteristics except for the presence of slits in the lid, and the tank is largely open at its top surface.

[0169] Example 1 and Comparative Examples 2 and 3: Functionalization of Si flat plates using TiO2 The base material is a silicon plate with no pattern whatsoever.

[0170] Formulation F is a solution of TiCl4 in H2O at a concentration of 5 wt / wt%.

[0171] Example 1: Plate A is immersed in a dip coating chamber according to the present invention (Figure 1A), and the temperature inside the drying chamber is controlled to T=70°C.

[0172] Example 2 (Comparative Example): Plate B is immersed in a dip coating chamber B that does not have slits 5, and the temperature inside the drying chamber is controlled to T=25°C.

[0173] Example 3 (Comparative Example): Plate C is immersed in a dip coating chamber B that does not have slits 5, and the temperature inside the drying chamber is controlled to T = 70°C.

[0174] The results are shown in Figures 4A, 4B, and 4C, which are photographs of the plates after dipping and drying. The dip coating chamber according to the present invention provides a regular and homogeneous coating layer (Figure 4A). Conventional dip coating chambers provide a non-uniform surface where a material is deposited only on a portion of the surface in an uncontrolled and unpredictable manner (Figures 4B and 4C).

[0175] Examples 4 and 5: Functionalization of Me-functionalized SiO2 nanopatterned plates using TiO2 from TiCl4 aqueous formulations The substrate is a plate corresponding to Figures 5A and 5B, having an SiO2 surface with a nanopitch of diameter l = 250 nm and depth p = 70 nm, and r = 0.28.

[0176] Formulation F is a solution of TiCl4 in H2O at a concentration of 5 wt / wt%.

[0177] The drying chamber is under a controlled temperature of T=70°C.

[0178] Example 4: A functionalized substrate obtained using the chamber that is the subject of this invention is shown in Figure 6A.

[0179] It can be observed that the final TiO2 material is deposited within the pitch on the substrate surface in a homogeneous manner (substantially similar amounts of material are deposited in all pitches) and selective manner (no material is visible on the substrate surface).

[0180] Example 5 (Comparative Example): This method is carried out in a dip coating chamber without slits. A functionalized substrate obtained according to the conventional method is shown in Figure 6B. It can be observed that no material is deposited inside or outside the pitch.

Claims

1. A dip coating kit comprising a substrate (2) and a dip coating chamber (1) for depositing a formulation F containing compound C in a volatile liquid solvent onto the surface (2.1) of the substrate (2), wherein the substrate (2) is substantially planar and has a width (W2), and the chamber (1) is - A tank (3) for storing the aforementioned compound F, the tank (3) having an opening (3.1) at its upper part, - A removable lid (4) having an upper surface (4.1) and a lower surface (4.2), positioned over the opening (3.1) of the tank (3), wherein the lid (4) is provided with a slit (5) leading into the tank (3) as a vertical channel (6) for dipping and lifting the substrate (2), the vertical channel (6) having an upper end (6.1) and a lower end (6.2), and the channel (6) having a width (W1), the lid (4) and - A drying chamber (7) located above the lid (4), wherein the drying chamber (7) has a lower surface (7.1) located on the upper surface (4.1) of the lid (4), the drying chamber (7) has an opening (7.2) on its lower surface (7.1), the opening (7.2) faces the upper end (6.1) of the channel (6), and the drying chamber (7) has an upper surface (7.3) with a slit (7.4) through which the substrate (2) can be introduced and pulled up, and Equipped with, The width (W1) of the channel (6) and the width (W2) of the substrate (2) are set such that the value of (W1 - W2) / 2 is between 0.2 and 10 mm. Dip coating kit.

2. The dip coating kit according to claim 1, wherein the volume of the substrate (2) immersed in the compound F during dipping is Vs, and due to the shape of the tank (3) and the volume of the compound F while stored in the tank (3), the compound F shows the upper surface (10) of the surface Sl, and the ratio Vs / Sl satisfies the relationship Vs / Sl ≤ 1 mm.

3. The dip coating kit according to claim 1 or 2, wherein the channel (6) comprises a vertical wall (6.3) extending downward from the lower surface (4.2) of the lid (4).

4. The dip coating kit according to any one of claims 1 to 3, wherein the upper surface (4.1) of the lid is provided with a notch (8) surrounding the slit (5), and the lower part (7.6) of the drying chamber (7) is located within the notch (8).

5. The dip coating kit according to any one of claims 1 to 4, wherein the lid (4) closes the tank (3) in a solvent-sealed manner, except for the slit (5).

6. The dip coating kit according to any one of claims 1 to 5, wherein the temperature and vapor pressure inside the drying chamber (7) are controlled.

7. The dip coating kit according to any one of claims 1 to 6, wherein the surface (2.1) of the substrate (2) includes a flat region (2.2) and microscale to nanoscale topographic features (2.3, 2.3.1) having a lateral dimension (l) of 20 nm to 200,000 nm.

8. The dip coating kit according to claim 7, wherein the microscale to nanoscale topographical features (2.3, 2.3.1) comprises nanoscale or microscale pitches (2.3.1) engraved on the surface (2.1) of the substrate.

9. The dip coating kit according to claim 8, wherein the nano-sized or micro-sized pitch is characterized by an aspect ratio where r = pitch depth / smaller lateral dimension, and r ≥ 0.

01.

10. The dip coating kit according to claim 8 or 9, wherein the depth (p) of the pitch (2.3.1) of the substrate (2) is 5 nm to 100,000 nm.

11. The dip coating kit according to any one of claims 7 to 10, wherein the flat region (2.2) is composed of a hydrophobic material and the microscale to nanoscale topographical feature (2.3) is composed of a polar material.

12. The dip coating kit according to any one of claims 1 to 11, wherein the entire surface (2.1) of the substrate (2) is flat.

13. A dip coating apparatus comprising a dip coating kit according to any one of claims 1 to 12, further, - Substrate holding unit, and / or - A lifting device for raising and lowering the substrate holding unit, and / or - A motor that controls the raising and lowering of the base material (2), and / or - Software / hardware coupled to the device to control the usage parameters of the device. A dip coating apparatus equipped with the following features.

14. A method for depositing compound C onto the surface of a substrate (2), - Fill the tank (3) of the dip coating chamber (1) according to any one of claims 1 to 6 with a formulation F containing the compound C and a volatile liquid solvent, - The substrate (2) is introduced into the dip coating chamber (1) through the vertical channel (6), and the entire portion of the surface (2.1) to be coated is immersed in the compound F. - Lifting the substrate (2) into the drying chamber (7) through the vertical channel (6), - To hold the substrate (2) in the drying chamber (7) for a sufficient amount of time to evaporate the liquid solvent and to control the atmosphere. Methods that include...

15. The method according to claim 14, wherein the surface (2.1) of the substrate (2) includes a flat region (2.2) and microscale to nanoscale topographic features (2.3, 2.3.1) having a lateral dimension (l) of 20 nm to 200,000 nm.

16. The method according to claim 15, wherein the microscale to nanoscale topographical features (2.3, 2.3.1) comprises nanoscale or microscale pitches (2.3.1) engraved on the surface (2.1) of the substrate.

17. The method according to claim 16, wherein the nano-sized or micro-sized pitch is characterized by an aspect ratio where r = pitch depth / smaller lateral dimension, and r ≥ 0.

01.

18. The method according to claim 16 or 17, wherein the depth (p) of the pitch (2.3.1) of the substrate (2) is 5 nm to 100,000 nm.

19. The method according to any one of claims 14 to 18, wherein the flat region (2.2) is composed of a hydrophobic material and the microscale to nanoscale topographic feature (2.3) is composed of a polar material.

20. The method according to claim 14, wherein the entire surface (2.1) of the substrate (2) is flat.

21. The method according to any one of claims 14 to 20, wherein the volatile liquid solvent comprises water.

22. The method according to any one of claims 14 to 21, wherein the liquid level (10) of the compound F in the tank (3) is above the lower end (6.2) of the channel (6).

23. The method according to any one of claims 14 to 22, wherein the volume and shape of the tank (3) and the shape of the lid (4) are configured such that during a series of deposition cycles of the compound F on the substrate (2), the liquid level (10) of the compound F in the tank (3) remains above the lower end (6.2) of the channel (6).

Citation Information

Patent Citations

  • Solvent gas recovery at immersion coating procedure

    JP1980111868A

  • Speed controller of motor

    JP1985039394A

  • KR2015-0127359