Absorbent products with improved packaging efficiency
Elastic nonwoven fabric layers in absorbent core structures address the rigidity and material creep issues of conventional absorbent articles, ensuring comfort and efficient fluid management with reduced packaging and shipping needs.
Patent Information
- Application Number
- JP2026528545
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-20
- Filing Date
- 2024-11-18
- Publication Date
- 2026-11-20
AI Technical Summary
Conventional absorbent core structures for absorbent articles, such as women's pads, are rigid and uncomfortable due to their densification for improved absorbency, leading to reduced flexibility and conformability, and they suffer from material creep during packaging and shipping, affecting absorption efficiency and comfort.
Incorporating elastic upper and lower nonwoven fabric layers with a liquid-absorbing inner core layer containing cellulose fibers and superabsorbent particles, sealed together to maintain structural integrity and flexibility, allowing the absorbent articles to recover their shape after compression.
The absorbent articles maintain comfort and conformability while efficiently managing fluid absorption, reducing environmental impact by minimizing packaging and shipping volume, and lowering costs through optimized delivery and shipment.
Smart Images

Figure 2026539232000001_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure relates to absorbent products in general, and more specifically to a flexible, adaptable package for containing disposable absorbent articles that exhibits improved packaging efficiency and results in smaller, more environmentally friendly products. [Background technology]
[0002] Absorbent articles, such as diapers, training pants, women's pads, and adult incontinence pads, are widely used among consumers. Generally, these absorbent articles include a top sheet and a back sheet, with an absorbent core structure positioned between them. These absorbent articles are designed to absorb and retain fluids and other discharges from the human body to prevent soiling of the body and clothing.
[0003] Historically, absorbent core structures for women's pad applications have utilized cellulose fibers in various ways to manage the complex and diverse rheological properties of menstrual fluid and vaginal secretions. Conventional cellulose-based absorbent core structures can be thick, rigid, bulky, and uncomfortable to wear. Over time, these thick, cellulose-rich absorbent cores have been made thinner by incorporating absorbent polymer materials such as absorbent gelling materials ("AGMs") to further enhance their absorbent properties. However, these absorbent core structures have low mechanical strength and an even lower ability to maintain their shape, especially when filled with fluid exudate. These thinner structures also tend to be denser (and therefore more rigid) and are often wrapped in a simple cellulose tissue or thin nonwoven fabric layer to hold the AGM inside the core structure. Another approach combines these wrapped cellulose and AGM cores with additional fluid-trapping-distributing layers. However, these trapping-distributing layers are not ideal for complex viscous fluids that need to move across the boundaries between these layers. To facilitate the fractional distillation of fluid from the capture-distribution system to the core, the core is often made denser to increase capillary action and the core's ability to effectively draw fluid from the upper capture-distribution layer. However, such densification of the absorbent system comes at the expense of comfort (rigidity) and the ability of the absorbent core structure and / or absorbent article to easily conform to the wearer's unique anatomical shape.
[0004] While relatively low-density, flexible, and conformable cellulose-based absorbent core structures are desirable for comfort and performance, maintaining the intended density of such cores during manufacturing, packaging, shipping, and storage is challenging. Cellulose-rich absorbent core structures are known to be sensitive to compression during manufacturing and / or packaging processes. For example, prolonged compression of a typical cellulose-rich absorbent core structure, such as within a package, can cause the article and / or absorbent core structure to lose its ability to recover to its pre-compression state. This is a process called material (or product) creep, where the system readjusts to prolonged mechanical compression or stress to find a new equilibrium. Absorbent articles held in a package under compression may become denser, resulting in a stiff article that may be less conformable to the user's anatomical features and uncomfortable to wear. Furthermore, prolonged compression can reduce absorption efficiency, resulting in an article that feels wet and exhibits larger stain sizes. Absorbent materials are also typically compressed during packaging to reduce their volume for storage and transport, and to lessen the space they require on store shelves. Compressing a product can increase packaging efficiency, but it typically comes at the expense of the product's flexibility, conformability, and / or absorbency. [Overview of the project] [Problems that the invention aims to solve]
[0005] There is a need for absorbent materials that can be compressed during manufacturing and packaging, and can then nearly recover to their original state, providing a comfortable and adaptable fit. Furthermore, there is a need for mechanisms that fully optimize the product delivery and shipment of such materials (optimization in terms of more materials per unit volume and fewer packages per number of materials packed). These types of shipping efficiencies can reduce the environmental impact of shipping such materials by reducing the number of pallets and trucks required to ship the materials to various store locations and warehouses. [Means for solving the problem]
[0006] This disclosure reduces the cost and environmental impact of packing and shipping cellulose-based absorbent articles having conforming features. The absorbent articles of this disclosure include an absorbent core structure comprising an upper nonwoven layer and a lower nonwoven layer sandwiching an inner core layer containing a liquid absorbent material containing cellulosic fibers. The absorbent articles described herein are compressed and retained in a package, but maintain a relatively low density and can recover almost their pre-compression caliper after being removed from the package.
[0007] This specification discloses an absorbent product including a package with an internal space and an external surface. Multiple disposable feminine hygiene pads are arranged within the internal space of the package. Each disposable feminine hygiene pad includes a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet. The absorbent core structure includes an upper nonwoven fabric layer, a lower nonwoven fabric layer, and an inner core layer containing cellulosic fibers, with at least a portion of the inner core layer disposed between the upper and lower nonwoven fabric layers. The disposable feminine hygiene pad has a weight of approximately 0.20 g / cm³ when measured according to the in-bag compression recovery method. 3 The following average pad density is observed within the bag, and caliper recovery percentage is at least 4% in 2 minutes.
[0008] This specification also discloses absorbent products including packaging, which includes an internal space and an external surface. Multiple disposable feminine hygiene pads are arranged within the internal space of the packaging. Each disposable feminine hygiene pad includes a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet. The absorbent core structure includes an upper nonwoven fabric layer containing polymer fibers and having a basis weight of about 30 gsm to about 85 gsm, a lower nonwoven fabric layer containing polymer fibers and having a basis weight of about 7 gsm to about 40 gsm, and an inner core layer containing a mixture of cellulose fibers and superabsorbent particles. At least a portion of the inner core layer is disposed between the upper and lower nonwoven fabric layers. The feminine hygiene pad has a viscosity of 0.20 g / cm³ when measured according to the in-bag compression recovery method. 3 The following average padding density is observed within the bag.
[0009] This specification also discloses absorbent products including packaging, which includes an internal space and an external surface. Multiple disposable feminine hygiene pads are arranged within the internal space of the packaging. Each disposable feminine hygiene pad includes a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet. The absorbent core structure includes an upper nonwoven fabric layer containing polymer fibers and having a basis weight of about 30 gsm to about 85 gsm, a lower nonwoven fabric layer containing polymer fibers, and an inner core layer containing about 50% to about 85% by weight of cellulose fibers and about 15% to about 50% by weight of superabsorbent particles. At least a portion of the inner core layer is disposed between the upper and lower nonwoven fabric layers. The feminine hygiene pads exhibit a caliper recovery percentage of about 4% to about 35% in 2 minutes, as measured according to the in-bag compression recovery method.
[0010] Furthermore, this specification discloses a process for packaging multiple disposable feminine hygiene pads, the process of providing multiple disposable feminine hygiene pads, each of which comprises a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet, the absorbent core structure comprising an upper nonwoven fabric layer containing polymer fibers and having a basis weight of about 30 gsm to about 85 gsm, a lower nonwoven fabric layer containing polymer fibers and having a basis weight of about 7 gsm to about 40 gsm, and an inner core layer containing cellulosic fibers and superabsorbent particles, the process of providing multiple disposable feminine hygiene pads, each of which comprises folding each disposable feminine hygiene pad to form multiple folded disposable feminine hygiene pads, and arranging the multiple folded disposable feminine hygiene pads. The method includes forming a laminate of folded disposable feminine hygiene pads, compressing the laminate of folded disposable feminine hygiene pads along a compression axis to form a compressed laminate of folded disposable feminine hygiene pads, and placing the compressed laminate of folded disposable feminine hygiene pads into the internal space of a package such that the compressed laminate of folded disposable feminine hygiene pads is placed into the internal space of the package such that the compression axis of the laminate of folded disposable feminine hygiene pads is oriented substantially along the width dimension of the package, and closing the package such that the folded disposable feminine hygiene pads exhibit an average in-bag folded caliper of about 7.0 to about 15.0 mm, and when removed from the package, the disposable feminine hygiene pads exhibit a caliper recovery percentage of at least 4% in 2 minutes when measured according to the in-bag compression recovery method. [Brief explanation of the drawing]
[0011] [Figure 1] This is a diagram of the absorbent core structure according to this disclosure. [Figure 2] This is a cross-sectional view of the absorbent core structure along line 2-2 in Figure 1. [Figure 3]This is a plan view of an absorbent material, with the surface facing the wearer oriented towards the viewer. A portion of the structure is cut out to more clearly show the composition of the absorbent core structure. [Figure 4] This is a cross-sectional view along line 4-4 in Figure 3. [Figure 5] This is a plan view of an absorbent article with the surface facing the wearer oriented towards the viewer, showing the arrangement of an example absorbent core structure. [Figure 6A] Figure 5 shows a cross-sectional view of the absorbent material along line 6A-6A. [Figure 6B] Figure 5 shows a cross-sectional view of the absorbent material along line 6B-6B. [Figure 7] This is a cross-sectional view of the absorbent article along line 7-7 in Figure 5. [Figure 8] This is a plan view of an absorbent article with the top sheet removed, where the surface facing the wearer is facing the viewer, and shows the arrangement of an example inner core layer and adhesive. [Figure 9] This is an enlarged view of a structural bonding site, one or more of the configurations shown and described herein. [Figure 10] This is a cross-sectional view of the structural bonding site in Figure 9. [Figure 11A] This is a plan view of an absorbent article in which the surface facing the wearer is oriented towards the viewer, and shows a flex-bonded channel region in one or more configurations shown and described herein. [Figure 11B] This is a plan view of an absorbent article in which the surface facing the wearer is oriented towards the viewer, and shows a flex-bonded channel region in one or more configurations shown and described herein. [Figure 12A] This is a side view of the package for the absorbent article according to this disclosure, showing the width of the filled bag. The outer surface is shown transparently for clarity. [Figure 12B] This is a side view of the package for the absorbent article according to this disclosure, showing the height of the filled bag in the package. The outer surface is shown transparently for clarity. [Figure 13]This is a perspective view of the package for the absorbent article according to this disclosure, showing the depth of the filled bag in the package. [Figure 14A] This is the setup for the test method for the wet and dry CD ultra-high sensitivity three-point bending method. [Figure 14B] This is the setup for the test method for the wet and dry CD ultra-high sensitivity three-point bending method. [Figure 14C] This is the setup for the test method for the wet and dry CD ultra-high sensitivity three-point bending method. [Figure 15] This is the configuration of the test method for wet and dry collapse and compression tests. [Figure 16A] This is the configuration of the test method for wet and dry collapse and compression tests. [Figure 16B] This is the configuration of the test method for wet and dry collapse and compression tests. [Figure 17A] These are exemplary graphs of deformation curves obtained from wet and dry deformation compression tests. The graphs in Figures 17A and 17B are shown to illustrate how calculations in the method may be performed and do not represent the data described herein. [Figure 17B] These are exemplary graphs of deformation curves obtained from wet and dry deformation compression tests. The graphs in Figures 17A and 17B are shown to illustrate how calculations in the method may be performed and do not represent the data described herein. [Figure 18] This is a top view of the permeable plate used in the capture time and re-wetting method described herein. [Figure 19] This is a bottom view of the permeable plate used in the capture time and re-wetting method described herein. [Figure 20A] This is a cross-sectional view of the permeable plate used in the capture time and re-wetting method described herein, defined by the z-direction and along the line 20A-20A shown in Figure 18. [Figure 20B] This is a cross-sectional view of the permeable plate used in the capture time and re-wetting method described herein, defined by the z-direction and along the line 20B-20B shown in Figure 18. [Modes for carrying out the invention]
[0012] When used in this specification, “disposable absorbent articles” or “absorbent articles” refer to articles intended for disposal after use, such as diapers, training pants, diaper pants, re-fastening pants, adult incontinence pads, adult incontinence pants, women’s hygiene pads, and cleaning pads.
[0013] As used herein, “absorbent core structure” shall be used in relation to the upper nonwoven layer, the lower nonwoven layer, and the inner core layer positioned between the upper and lower nonwoven layers. As used herein, “absorbent core structure” shall not include any secondary top sheet, top sheet, secondary back sheet, or back sheet of the absorbent article.
[0014] As used herein, “hydrophilic” and “hydrophobic” have well-established meanings in the art with respect to the water contact angle on the surface of a material. Therefore, a material with a water contact angle greater than about 90 degrees is considered hydrophobic, and a material with a water contact angle less than about 90 degrees is considered hydrophilic. A hydrophobic composition increases the water contact angle on the surface of a material, while a hydrophilic composition decreases it. Notwithstanding the foregoing, references to relative hydrophobicity or hydrophilicity between a material and a composition, between two materials, and / or between two compositions do not imply that the material or composition is hydrophobic or hydrophilic. For example, a composition may be more hydrophobic than a material. In this case, neither the composition nor the material may be hydrophobic. However, the contact angle exhibited by the composition is greater than that of the material. As another example, a composition may be more hydrophilic than a material. In this case, neither the composition nor the material may be hydrophilic. However, the contact angle exhibited by the composition is smaller than that of the material.
[0015] As used herein, the term “filament” refers to any type of continuous strand produced through a spinning process, a melt-blown process, a melt-fibrillation or film-fibrillation process, or an electrospinning production process, or any other suitable process for producing a filament. The term “continuous” in the context of filament is distinguished from staple filaments, which are cut to a specific target length. In contrast, a “continuous filament” is not cut to a predetermined length, but can instead break at random lengths, though typically much longer than staple filaments.
[0016] As used herein, “machine direction” refers to the direction in which the web flows through the absorbent material processing process. For brevity, it may be referred to as “MD.”
[0017] In this specification, "machine transverse direction" refers to the direction perpendicular to the MD. For brevity, it may be referred to as "CD."
[0018] As used herein, “elastic” refers to a material that tends to retain its shape in both dry and wet conditions, and, when subjected to a compressive force, tends to recover its original pre-compression shape when such force is removed. In some embodiments, the upper and / or lower nonwoven layers described herein may be elastic.
[0019] Decitex, also known as Dtex, is a measurement used in the textile industry to measure yarn or filament. 1 decitex = 1 gram per 10,000 meters. In other words, if a yarn or filament weighs 500 grams per 10,000 linear meters, then that yarn or filament has 500 decitex.
[0020] As used herein, “facing the wearer” (which may also be referred to as “facing the body”) and “facing the outside” (which may also be referred to as “facing the garment”) refer to the relative position of the surface of an element or group of elements, respectively. “Facing the wearer” means that the element or surface is closer to the wearer during wear than any other element or surface. “Facing the outside” means that the element or surface is further away from the wearer during wear than any other element or surface (i.e., the element or surface is closer to the wearer’s garment that may be worn over an absorbent article).
[0021] It should be understood that all maximum numerical limits given throughout this specification include all lower numerical limits as if they were explicitly stated herein. All minimum numerical limits given throughout this specification include all higher numerical limits as if they were explicitly stated herein. All numerical ranges given throughout this specification include all narrow numerical ranges that fall within such broad numerical ranges as if they were explicitly stated herein.
[0022] This disclosure relates to a disposable absorbent article comprising an absorbent core structure including an upper nonwoven layer and a lower nonwoven layer, together with an inner core layer containing a liquid absorbent material disposed between the upper and lower nonwoven layers. The liquid absorbent material may include a homogeneous mixture of cellulosic fibers and superabsorbent particles, referred to herein as "fluff / AGM". At least a portion of the inner core layer may be contained within the upper and lower nonwoven layers by sealing portions of the first and second side regions of the upper nonwoven layer with the first and second side regions of the lower nonwoven layer, thereby defining a periphery seal that positions the adhesive between the upper and lower nonwoven layers and bonds the layers together. In some configurations, the periphery seal may extend around the entire periphery of the inner core layer.
[0023] The absorbent core structures described herein are configured to compress over a range of body movement and compression and to recover their original shape (dry or wet). The flexibility and / or elasticity of the absorbent core structures result in an absorbent article that comfortably conforms to the wearer's anatomical shape while efficiently managing fluid as it leaves the body. Unexpectedly, this can be achieved without typical high-density rigidity (for wet cohesion) by utilizing elastic upper and lower nonwoven fabric layers composed of elastic polymers located above and below the loosely filled liquid-absorbing material of the inner core layer. Remarkably, when the absorbent core structure is wet, it can bear structural loads and recover its shape without physically rigidifying or losing desired structural properties. While not bound by theory, it is believed that when selected elastic upper and lower nonwoven fabrics are positioned above and below the liquid-absorbing material in the inner core layer and bonded to and around the liquid-absorbing material, wet integrity / shape stability in a cellulose-rich absorbent core structure can be achieved without substantial densification and rigidity. The upper and lower nonwoven fabrics may have sufficient resilience to return the liquid-absorbing material to its original state and / or stable fiber orientation after compression. When a cellulose-rich pulp core is wrapped or encapsulated in simple cellulose tissue or a nonwoven fabric with low elasticity, sufficient recovery energy may not be exhibited to restore the shape during use, especially when wet. The structural wet-elastic nonwoven fabrics detailed herein may exhibit post-compression recovery energy sufficient to restore the cellulose-rich fiber matrix and may be selected to provide high compression recovery with relatively low stiffness in both dry and wet conditions. A suitable absorbent core structure is one that exerts low compressive force (low resistance) and can almost recover its shape when the user periodically compresses it and releases the compressive force through various bodily movements. To achieve this, the structure should maintain sufficient recovery energy after multiple periodic compressions. Without sufficient recovery energy, the structure will remain in a compressed aggregate state with insufficient force (storage energy) to recover.
[0024] Absorbent articles are typically compressed strongly during manufacturing and packaging to help minimize shipping and / or warehousing costs. Typical fluff and airlaid absorbent products are manufactured to have a high-density absorbent system, and therefore compression during manufacturing and / or packaging does not significantly affect the intended product caliper, density, and / or performance, and is therefore typically not a concern for manufacturers. However, in the case of relatively low-density flexible absorbent articles and / or absorbent core structures as described herein, strong compression can significantly affect the ability of the absorbent article and / or absorbent structure to recover its caliper after the compression is removed, which may result in a wet feel and increased stain size during use. Surprisingly, it has been found that the absorbent articles and / or absorbent core structures described herein can be compressed to a relatively high level and retained in packaging without permanent densification, and the absorbent articles and / or absorbent core structures can recover almost their pre-compression caliper after being removed from packaging. While not bound by theory, increased compression ratios are thought to offer multiple cost-saving benefits, such as lower shipping costs, lower storage / warehouse storage costs, reduced packaging costs, and reduced shelf / inventory costs, as well as smaller package sizes and more environmentally friendly packaging.
[0025] An exemplary absorbent core structure 10 of this disclosure is shown in Figure 1. Figure 2 is a cross-sectional view along line 2-2 in Figure 1, with the structural bonding site 15 removed to more clearly show the absorbent core structure 10.
[0026] Referring to Figures 1 and 2, the absorbent core structure 10 may include an upper nonwoven fabric layer 210 and a lower nonwoven fabric layer 220 (collectively referred to herein as the upper and lower nonwoven fabric layers or upper and lower nonwoven fabric), and an inner core layer 200 disposed between the upper and lower nonwoven fabric layers 210 and 220. The absorbent core structure 10 may also include an inner core layer 200 containing a liquid absorbent material. The liquid absorbent material may include a homogeneous mixture of cellulose pulp and superabsorbent particles. Parts of the upper and lower nonwoven fabric layers 210 and 220 may be joined together by a perimeter seal 230.
[0027] An exemplary absorbent article 20 in the form of a women's hygiene pad is shown in Figure 3. To provide a reference frame for this study, the absorbent article 20 in Figure 3 is shown with its longitudinal axis 80 and transverse axis 90. Figure 3 is a plan view of the absorbent article 20 with the surface 112 facing the wearer facing the viewer, and a portion of the structure is cut out to more clearly show the configuration of the absorbent core structure 10. Figure 4 is a cross-sectional view of the absorbent article 20 along line 4-4 in Figure 3.
[0028] Referring to Figures 3 and 4, the absorbent article 20 may include a top sheet 110, a back sheet 130, and an absorbent core structure 10 disposed between the top sheet 110 and the back sheet 130. The absorbent article 20 may include a surface 112 facing the wearer and a surface 132 facing the clothing. The absorbent article 20 and the absorbent core structure 10 may each include a front region 21, a rear region 23, and an intermediate region 22 disposed between the front region 21 and the rear region 23. In some configurations, the absorbent core structure 10 may have a non-rectangular perimeter. Specifically, the absorbent core may be molded to define a taper along its width toward the intermediate region of the absorbent core structure. The absorbent core structure can conform to the shape of the wearer's inner thigh, such as an hourglass shape, an offset hourglass shape (one end wider than the opposite end and the middle section between the ends being narrower), a bicycle seat shape (one end and the middle section being narrower than the second end), an ellipse, or a trapezoidal shape.
[0029] In some configurations, the disposable absorbent article 20 may include a structure consisting of a top sheet 110, an upper nonwoven fabric layer 210, an inner core layer 200, a lower nonwoven fabric layer 220, and a back sheet 130 (from the surface facing the wearer to the surface facing the outside). In some embodiments, the top sheet 110 may be in direct contact with the upper nonwoven fabric layer 210, the upper nonwoven fabric layer 210 may be in direct contact with the inner core layer 200, and / or the inner core layer 200 may be in direct contact with the lower nonwoven fabric layer 220. "Direct contact" means that there are no further intermediate component layers between each of the layers that are in direct contact. However, it is not excluded that an adhesive material may be placed between at least a portion of the above-described layers.
[0030] The upper nonwoven fabric layer 210 may include a first side region 210a and a second side region 210b opposite in the transverse direction, and the lower nonwoven fabric layer 220 may include a first side region 220a and a second side region 220b opposite in the transverse direction. In some configurations, the first side regions 210a, 220a of the upper and lower nonwoven fabric layers may extend substantially parallel to the longitudinal axis 80. The upper and lower nonwoven fabric layers 210, 220 may extend outward from the perimeter 200a of the inner core layer and may be joined together using adhesives or other conventional bonding methods including but not limited to ultrasonic bonding, melt bonding, crimping, and combinations thereof to form a perimeter seal 230. In some configurations, the entire inner core layer 200 may be located inside the perimeter seal 230. The periphery seal 230 can help seal the liquid-absorbing material of the inner core layer 200 to the inside of the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220. The periphery seal 230 may include at least a first seal region 231 extending substantially parallel to the longitudinal centerline 80, and a second seal region 231' opposite the first seal region 231. In some configurations, the periphery seal 230 may further include a front periphery seal region 232 and / or a rear periphery seal region 233. In some configurations, the periphery seal 230 may extend around the entire periphery 200a of the inner core layer.
[0031] While not bound by theory, elastic nonwoven layers containing polymer fibers may retain their shape when wet and resist plasticization when attached to the inner core layer through the application of a core structure adhesive applied directly to either the inner core layer or the elastic nonwoven layer via a conventional spray coating application selected to achieve bonding but not to obstruct fluid flow to the inner core layer. The periphery seal 230 may be located in at least the intermediate region 22 of the absorbent article 20 and / or absorbent core structure 10. The intermediate region 22 (located between the wearer's thighs during use) is considered to be the area that will experience the most frequent and / or highest forces during use. It has been found that the presence of at least partially periphery seals in the first and second lateral regions of the upper and lower nonwoven layers outside the inner core layer may help ensure that the upper and lower nonwovens do not separate during physical deformation, do not restrict any potential integrity, and maintain their structural function without deformation problems. In addition, the periphery seal may allow any excess nonwoven material to be removed, enabling the absorbent core structure to be molded to conform to the shape of the inner thigh.
[0032] The periphery seal 230 may have a seal width WS of approximately 1 mm to 10 mm, or approximately 2 mm to 8 mm, or approximately 3 mm to 6 mm. The seal width WS may be uniform or may vary around the inner core layer.
[0033] In some configurations, the upper and lower nonwoven layers 210, 220 may be separate materials that can be cut to approximately the size and shape of the inner core layer 200 so as to fit between the top sheet 110 and the back sheet 130. In some configurations, the inner core layer 200, the upper nonwoven layer 210, and / or the lower nonwoven layer 220 may be molded, meaning they are not rectangular. In some configurations, the upper and / or lower nonwoven layers 210, 220 may be rectangular.
[0034] In some configurations, multiple parts of the absorbent core structure may not include a periphery seal. In some configurations, the periphery seal 230 may only partially extend around the inner core layer periphery 200a. Figures 5 to 8 show an absorbent article and an example arrangement of an absorbent core structure. Elements in Figures 5 to 8 having the same reference numerals as those described above in relation to Figures 1 to 4 may be the same elements (e.g., the inner core layer 200). Figure 6A is a cross-sectional view of the absorbent article along line 6A-6A in Figure 5. Figure 6B is a cross-sectional view of the absorbent article along line 6B-6B in Figure 5. Figure 7 is a cross-sectional view of the absorbent article along line 7-7 in Figure 5.
[0035] Referring to Figures 5 to 7, in some configurations, the upper nonwoven fabric layer 210 extends longitudinally between the front edge 403 and the rear edge 404, defining a first side region 210a and a second side region 210b facing each other transversely. The lower nonwoven fabric layer 220 extends longitudinally between the front edge 408 and the rear edge 409, defining a first side region 220a and a second side region 220b facing each other transversely. The upper nonwoven fabric layer 210 may have a first nonwoven transverse width WN1, and the lower nonwoven fabric layer 220 may have a second nonwoven transverse width WN2. In some configurations, the first and second nonwoven transverse widths WN1 and WN2 may be substantially the same. In some configurations, the first and second nonwoven transverse widths WN1 and WN2 may be different. The transverse width WN1 of the first nonwoven fabric and / or the transverse width WN2 of the second nonwoven fabric may be approximately 40 mm to approximately 110 mm, or 45 mm to approximately 90 mm, or approximately 50 mm to approximately 80 mm. The upper and / or lower nonwoven fabric layers 210, 220 may have a longitudinal length of approximately 100 mm to approximately 450 mm, or approximately 150 mm to approximately 375 mm. In some configurations, the upper and / or lower nonwoven fabric layers 210, 220 may extend from the front article edge 30 to the rear article edge 32.
[0036] At least a portion of the inner core layer 200 may be positioned between the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 210. In some configurations, the entire inner core layer 200 may be positioned between the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220.
[0037] The inner core layer 200 extends longitudinally between the front edge 424 and the rear edge 426 of the inner core layer, and extends laterally from the first side edge 250 to the second side edge 252. In some configurations, the inner core layer 200 may be molded. As shown in Figure 8, the inner core layer 200 may define a first inner core layer lateral width WC1, a second inner core layer lateral width WC2, and a third inner core layer lateral width WC3 disposed between them. In some configurations, the first inner core layer lateral width WC1 may be in the front region 21, and the second inner core layer lateral width WC2 may be located in the rear region 23. In some configurations, the third inner core layer lateral width WC3 may be smaller than the first and second inner core layer lateral widths WC1 and WC2. In some configurations, the lateral width WC2 of the second inner core layer may be greater than the lateral widths WC1 and WC3 of the first and third inner core layers. The lateral width WC1 of the first inner core layer may be approximately 50 to 80 mm, the lateral width WC2 of the second inner core layer may be approximately 55 mm to 100 mm, and the lateral width WC3 of the third inner core layer may be approximately 40 mm to 70 mm.
[0038] The adhesive zone 525 may be located between at least one of the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 and the inner core layer 200. The adhesive zone 525 may include an adhesive 528 extending from a first side region 210a to a second side region 210b of the upper nonwoven fabric layer 210, and / or from a first side region 220a to a second side region 220b of the lower nonwoven fabric layer 220. As shown in Figure 8, the adhesive zone 525 may extend from a first edge 525a to a second edge 525b, defining an adhesive zone lateral width WZ of about 35 mm to about 110 mm, or about 40 to about 105 mm. In some configurations, the first and second edges 525a, 525b of the adhesive zone 525 may be adjacent to the lateral edges of the upper and / or lower nonwoven layers 210, 220, or may be spaced laterally inward from them. In some configurations, as shown in Figure 5, the gap region 530 may be defined on the upper and / or lower nonwoven layers 210, 220 by the absence of adhesive 528 between the first and second edges 525a, 525b of the adhesive zone 525 and the edges of the nonwoven fabric. The gap region 530 may have a width of less than 5 mm, or about 0.1 mm to about 5 mm, or about 0.5 mm to about 3 mm. In some configurations, the upper nonwoven layer 210 and the lower nonwoven layer 220 may substantially surround the adhesive zone 525 and the inner core layer 200.
[0039] In some configurations, a portion of the inner core layer 200 may be contained within the upper and lower nonwoven layers 210 and 220 by sealing a portion of the first side region 210a and the second side region 210b of the upper nonwoven layer 210 with a portion of the first side region 220a and the second side region 220b of the lower nonwoven layer 220, thereby defining a lateral periphery seal 230 in which the adhesive 528 is positioned between the upper and lower nonwoven layers 210 and 220. Thus, the adhesive 528 can bond the upper nonwoven layer 210 to the lower nonwoven layer 220. The lateral periphery seal 230 may be located in an intermediate region 22 and may have a longitudinal seal length LS that is about 45% to about 90% or about 50% to about 85% of the longitudinal inner core length LC.
[0040] Referring to Figure 5, a portion of the inner core layer 200 may extend laterally outward from the adhesive zone 525 to define an unsealed portion 420. The unsealed portion 420 may be located longitudinally outward from the periphery seal 230. It should be understood that the absorbent core structure 10 may include one or more unsealed portions 420, such as two, three, or four, depending on the size and / or arrangement of the upper and lower nonwoven fabric layers relative to the size and / or arrangement of the adhesive zone and the inner core layer.
[0041] The absorbent core structure 10 may include a first unsealed portion 423a, in which a portion of the inner core layer 200 extends laterally outward from the adhesive zone 525. In some configurations, the absorbent core structure 10 may include a second unsealed portion 423b, in which a second portion of the inner core layer 200 extends laterally outward from the adhesive zone 525. The second unsealed portion 423b may be laterally separated from the first unsealed portion 423a by a sealing portion 410. In some configurations, the first and second unsealed portions 423a, 423b may be located in the rear region 23 and may extend longitudinally within a portion of the intermediate region 22. The absorbent core structure 10 may further include a third unsealed portion 421a, in which a third portion of the inner core layer 200 extends laterally outward from the adhesive zone 525. In some configurations, the absorbent core structure 10 may include a fourth unsealed portion 421b, the fourth portion of the inner core layer 200 extending laterally outward from the adhesive zone 525. The fourth unsealed portion 421b may be laterally separated from the third unsealed portion 421a by the sealing portion 410. In some configurations, the third and fourth unsealed portions 421a, 421b may be located within the front region 21 or may extend longitudinally within the intermediate region 22. The unsealed portion 420 may also be formed in a configuration in which a portion of the inner core layer perimeter 200a is adjacent to the first or second edges 525a, 525b of the adhesive zone 525.
[0042] The first and second non-seal portions 423a, 423b may have a non-seal longitudinal length L1U that is about 5% to about 30% or about 8% to about 25% of the longitudinal inner core length LC. The third and fourth non-seal portions 421a, 421b may have a non-seal longitudinal length L2U that is about 5% to about 30% or about 8% to about 25% of the longitudinal inner core length LC. In some configurations, the non-seal longitudinal length L1U of the first or second non-seal portions 423a, 423b may be greater than the non-seal longitudinal length L2U of the third or fourth non-seal portions 421a, 421b.
[0043] Figures 6A and 6B are cross-sectional views of the absorbent article 20 of Figure 5 along lines 6A-6A and 6B-6B, respectively, and show the configuration of the absorbent core structure 10. In particular, Figure 6A is a cross-sectional view passing through the intermediate region 22 of the absorbent article 20, showing that the upper and lower nonwoven fabric layers 210 and 220 extend laterally outward from the first and second side edges 250 and 252 of the inner core layer 200. As described above, a portion of the inner core layer 200 may be housed within the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 by sealing a portion of the first side region 210a and the second side region 210b of the upper nonwoven fabric layer 210 with a portion of the first side region 220a and the second side region 220b of the lower nonwoven fabric layer 220, thereby defining a lateral periphery seal 230. Figure 6B is a cross-sectional view through the rear region 23 of the absorbent article 20, showing that the upper and lower nonwoven layers 210, 220 extend laterally outward from the first and second side edges 250, 252 of the inner core layer 200. As described above, a portion of the inner core layer 200 may extend laterally outward from the adhesive zone 525 (not shown) to define an unsealed portion 420. The garment-facing surface of the upper nonwoven layer 210 and / or the wearer-facing surface of the lower nonwoven layer 220 may be coated with adhesive 528 to provide connection with the inner core layer 200 and / or to form a perimeter seal 230. Interlayer adhesives (except in the perimeter seal) are not shown in Figures 6A and 6B for simplification.
[0044] As described above, the upper and lower nonwoven fabric layers 210 and 220 may be further joined by a front periphery seal region 232 and / or a rear periphery seal region 233 located on the longitudinal outer side of the inner core layer 200. The front periphery seal region 232 and / or the rear periphery seal region 233 may extend longitudinally from the periphery 200a of the inner core layer for a distance of approximately 3 mm to approximately 30 mm, or approximately 5 mm to approximately 15 mm. Although not theoretically bound, it is conceivable that front and / or rear periphery seal regions 232 and 233 of less than approximately 3 mm may not provide sufficient distance on the production line to avoid contamination of the liquid absorbent material outside the inner core layer. In some configurations, the front periphery seal region 232 may be adjacent to the leading edge 403 of the upper nonwoven fabric layer 210 and / or the leading edge 406 of the lower nonwoven fabric layer 220, or it may be spaced longitudinally inward from them. In some configurations, the rear peripheral seal 233 may be adjacent to the rear edge 404 of the upper nonwoven fabric layer 210 and / or the rear edge 409 of the lower nonwoven fabric layer 220, or it may be spaced longitudinally inward from them.
[0045] In some structures, the lateral width WC1 and adhesive zone width WZ of the first inner core layer may be substantially the same, and the adhesive 528 does not extend laterally outward around the inner core layer 200a, creating an unsealed portion in this area where the upper nonwoven layer 210 is not bonded to the lower nonwoven layer 220. In some configurations, the lateral width WC2 of the second inner core layer may be substantially the same as the adhesive zone width WZ, and is therefore understood to define an unsealed portion in the rear region 23. In some structures, the lateral width WC1 of the first inner core layer may be smaller than the adhesive zone width WZ. The upper and lower nonwoven layers 210, 220 and the adhesive zone 525 may substantially surround the inner core layer in the front region, and the lateral perimeter seal 230 may extend longitudinally from the intermediate region 22 to the front region 21. In this configuration, the inner core layer is sealed within the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 in the intermediate region 22 and the front region 21. In some configurations, the lateral width WC2 of the second inner core layer may be smaller than the adhesive zone width WZ, and it is understood that a lateral periphery seal 230 is created that extends longitudinally from the intermediate region 22 to the rear region 23.
[0046] In some structures, at least one of the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 may be narrower than at least a portion of the inner core layer 210. In some configurations, the upper nonwoven fabric layer 210 and / or the lower nonwoven fabric layer 220 may be narrower than the lateral width WC1 of the first inner core layer and / or the lateral width WC2 of the second inner core layer.
[0047] Referring to Figures 5 and 7, the front edge 403 of the upper nonwoven layer 210 and / or the front edge 408 of the lower nonwoven layer 220 may be adjacent to the front article edge 30, or they may be spaced longitudinally inward from the front article edge 30. In some configurations, the rear edge 404 of the upper nonwoven layer 210 and / or the rear edge 409 of the lower nonwoven layer 220 may be adjacent to the rear article edge 32, or they may be spaced longitudinally inward from the rear article edge 32. The absorbent article 20 may further include a crimp seal 500 located in the front region 21 and / or the rear region 23. In some configurations, the crimp seal 500 may extend from the front region 21 and / or the rear region 23 into the intermediate region 22. In some configurations, the crimp seal 500 may be located longitudinally outward of the front and rear perimeter seals 232, 233. In some configurations, the front and / or rear perimeter seal regions 232, 233 may extend within the crimp seal 500. The crimp seal 500 may be bonded to a top sheet 110, a back sheet 130, and at least one of an upper nonwoven fabric layer 210 and a lower nonwoven fabric layer 220. In some configurations, the crimp seal 500 may bond the top sheet 110 to the back sheet 130. Surprisingly, it has been found that the crimp seal 500 can include upper and / or lower nonwoven fabric layers 210, 220 without becoming stiff or unpleasant. The crimp seal 500 may substantially not contain any liquid absorbent material.
[0048] Referring to Figure 3, the absorbent article 20 may further include a chassis 100 containing an absorbent core structure 10. The absorbent core structure 10 and / or inner core layer 200 can be molded. The side edges 120 and 125 of the absorbent article 20 may follow the overall contour of the absorbent core structure 10 and / or inner core layer 200. Thus, for example, if the absorbent core structure 10 has an hourglass shape, the side edges 120 and 125 of the absorbent article 20 may similarly be arranged in an hourglass shape. However, there may also be configurations in which the side edges 120 and 125 are generally straight or slightly curved so as not to follow the contour of the absorbent core structure. In some configurations, the absorbent article 20 may be symmetrical with respect to the longitudinal centerline 80 or asymmetrical with respect to the longitudinal centerline 80. Similarly, the absorbent article 20 may be symmetrical with respect to the transverse centerline 90 or asymmetrical with respect to the transverse centerline 90.
[0049] In some structures, the absorbent article and / or absorbent core structure may include a plurality of structural bonding sites 15, as shown in Figures 1, 9, and 10. Figures 9 and 10 show illustrations of example structural bonding sites 15. Figure 9 is a magnified view of an example structural bonding site 15. Figure 10 is a cross-sectional view of the structural bonding site 15 in Figure 9. The structural bonding sites 15 may be symmetrical and / or asymmetrical, and may be any shape, including but not limited to circular, elliptical, heart-shaped, diamond-shaped, triangular, square, star-shaped, and / or X-shaped. While the shape of the structural bonding site 15 may be any shape, preferred shapes may be denser shapes, such as asymmetrical shapes (as opposed to simple dots). The structural bonding sites 15 may be on the absorbent article and / or absorbent core structure. In some configurations, the structural bonding sites are approximately 2 mm 2 ~about 5mm 2The bonding area may be approximately 0.5% to 7.5%, 0.75% to 5%, or 1% to 4% of the absorbent core structure when measured according to the structural bonding site pattern spacing and area measurement method. The average distance between structural bonding sites may be approximately 10 mm to 32 mm. In some configurations, the average distance between structural bonding sites may be greater than approximately 20 mm. In some configurations, the structural bonding sites may have a maximum width of approximately 1 mm to 6 mm, 1.5 mm to 5 mm, or 2 mm to 4 mm. While not limited by theory, the average distance between these structural connection points and / or the size of these structural connection points are thought to help maintain the structural integrity of the absorbent core structure without creating undesirable stiffness that could impair the absorbent article's ability to conform to the body.
[0050] In some configurations, structural bonding sites may be distributed across the absorbent article and / or absorbent core structure, or they may be concentrated in each region of the absorbent article and / or absorbent core structure. In some configurations, structural bonding sites may be concentrated in the intermediate region 22 of the absorbent article and / or absorbent core structure. In some configurations, the intermediate region 22 of the absorbent article and / or absorbent core structure may not substantially contain structural bonding sites and may be surrounded by the structural bonding sites and / or embossed areas.
[0051] In some configurations, the structural bonding site 15 may bond the top sheet 110, the upper nonwoven layer 210, the absorbent core structure 10, and the lower nonwoven layer 220. In some configurations, the structural bonding site 15 may bond the upper nonwoven layer 210, the absorbent core structure 10, and the lower nonwoven layer 220. The absorbent article 20 and / or absorbent core structure 10 may comprise the upper nonwoven layer 210 and the lower nonwoven layer 220, which are closer to each other in the Z direction at the structural bonding site 15 but are not melted to each other. Since these structural bonding sites are not melted to each other, they may not be permanent in nature and may rather mix the materials within the structural bonding site. In some configurations, the structural bonding site 15 may substantially not contain melt bonding.
[0052] As shown in Figures 11A and 11B, the absorbent article may include one or more flex-bonded channel regions 160, the flex-bonded channel regions may be continuous depressions and / or a series of individually compressed, densely spaced embossed areas.
[0053] A suitable upper nonwoven fabric layer may have a basis weight of approximately 30 gsm to approximately 85 gsm, or approximately 35 gsm to approximately 70 gsm, or approximately 40 to approximately 60 gsm. The upper nonwoven fabric layer may have a tensile stiffness of approximately 0.1 N / mm to approximately 2.2 N / mm, or approximately 0.3 N / mm to approximately 1.6 N / mm, when measured according to the CD periodic stretching method up to 3% strain. The upper nonwoven fabric layer may have a breaking strain of more than approximately 10%, or approximately 10% to approximately 50%, or approximately 20% to approximately 40%, when measured according to the breaking strain method. The upper nonwoven fabric layer may have a permanent strain of approximately 0.005 to approximately 0.013 mm / mm, or 0.005 to approximately 0.0090 mm / mm, when measured according to the CD periodic stretching method up to 3% strain.
[0054] A suitable upper nonwoven fabric layer may have a basis weight of approximately 7 gsm to approximately 40 gsm, approximately 10 gsm to approximately 35 gsm, or approximately 15 gsm to approximately 20 gsm. The lower nonwoven fabric layer may have a tensile stiffness of approximately 0.2 N / mm to approximately 1.6 N / mm when measured according to the CD periodic stretching method up to 3% strain. The lower nonwoven fabric layer may have a fracture strain of more than approximately 10%, or approximately 10% to approximately 50%, or approximately 20% to approximately 40% when measured according to the fracture strain method. The lower nonwoven fabric layer may have a permanent strain of approximately 0.005 to approximately 0.013 mm / mm when measured according to the CD periodic stretching method up to 3% strain.
[0055] The upper and / or lower nonwoven layers may contain polymer fibers. Suitable upper and lower nonwoven fibers may be selected from PET (polyethylene terephthalate), PP (polypropylene), BiCo (two-component fiber) selected from PE / PP (PE sheath and PP core) and / or PE / PET (PE sheath and PET core), PLA (polylactic acid), and combinations thereof. In some configurations, the upper and / or lower nonwoven layers may contain recycled polymer resins, biodegradable polymers, biopolymers, bio-based fibers, and combinations thereof.
[0056] A suitable upper nonwoven fabric may contain approximately 60-100% or 70-100% synthetic fibers, or approximately 0-40% or 0-30% regenerated cellulose fibers such as rayon and / or viscose.
[0057] The upper nonwoven fabric layer may contain fibers with staple lengths of approximately 10 mm or more, or approximately 25 mm or more, or approximately 10 mm to approximately 100 mm, or approximately 20 mm to approximately 75 mm, or approximately 25 mm to approximately 50 mm. The upper nonwoven fabric layer may contain fibers with fiber diameters of approximately 1.3 Dtex to approximately 10.0 Dtex, or approximately 1.3 Dtex to approximately 6.0 Dtex, or approximately 2.0 Dtex to approximately 5.0 Dtex. Although not theoretically bound, it is thought that if the fibers of the upper nonwoven fabric layer are less than approximately 1.3 Dtex, the airflow through the material during manufacturing may be insufficient.
[0058] In some configurations, the upper nonwoven layer may contain a blend of staple fibers. If the upper nonwoven layer contains a blend of staple fibers, the fiber blend preferably contains 30% or less of fibers with a fiber diameter of 1.3 Dtex and / or 30% or less of fibers with a fiber diameter of 10.0 Dtex. In some configurations, the upper nonwoven layer may contain fibers, which are a blend of staple fibers having a fiber diameter of about 2.0 Dtex to about 8.0 Dtex. While not bound by theory, fibers with an average fiber diameter of about 2.0 Dtex to about 8.0 Dtex are thought to help allow sufficient airflow through the material during the fabrication of the absorbent core structure.
[0059] The lower nonwoven layer may contain fibers having a short fiber length of approximately 10 mm or more, or approximately 25 mm or more, or approximately 10 mm to approximately 100 mm, or approximately 20 mm to approximately 75 mm, or approximately 25 mm to approximately 50 mm. In some configurations, the lower nonwoven layer may contain continuous fibers. The lower nonwoven layer may contain fibers having a fiber diameter of approximately 1.0 DTex to approximately 5.0 DTex, or approximately 1.3 DTex to approximately 3.3 DTex, or approximately 1.3 DTex to approximately 2.2 DTex, or approximately 2.0 DTex to approximately 10.0 DTex. In some configurations, the lower nonwoven layer may contain fibers, which are a blend of fibers having a fiber diameter of approximately 0.1 DTex to approximately 6.0 DTex.
[0060] In some configurations, the upper nonwoven layer may comprise a blend of fibers, at least a portion of the fibers having a denier of from about 2.0 DTex to about 10.0 DTex, and the lower nonwoven layer may comprise a blend of fibers, at least a portion of the fibers having a denier of from about 1.3 DTex to about 5.0 DTex. In some configurations, the upper nonwoven layer may comprise a blend of fibers, at least a portion of the fibers having a denier of from about 1.3 DTex to about 2.2 DTex, and the lower nonwoven layer may comprise a blend of fibers, the blend of fibers having a denier of from about 1.0 DTex to about 5.0 DTex.
[0061] Suitable upper nonwoven layer materials and / or lower nonwoven layer materials may bend and return to their original shape in response to bending forces. Thin or highly flexible materials bend easily at low peak force (load) and low bending energy. Unsuitable materials bend easily but do not have sufficient recovery energy, and thus retain their deformed, bent state due to insufficient recovery energy. Suitable materials have sufficient energy to substantially recover their initial pre-bending state. Materials with sufficient bend recovery energy can be considered elastic upper and lower nonwoven layers. A particularly suitable upper nonwoven layer has about 0.03 N * mm or more, or about 0.03 N * mm to about 1 N * mm, or about 0.04 N * mm to about 0.5 N * mm of dry recovery energy. A particularly suitable upper nonwoven layer may have a dry bending energy of less than about 1.6 N * mm, or less than about 1.1 N * mm.
[0062] As noted above, the upper and lower nonwovens may comprise polymeric fibers. Polymeric fibers may be included to help impart structural integrity to the upper and lower nonwovens. The polymeric fibers can help increase the structural integrity of the upper and lower nonwovens in both the machine direction (MD) and the cross-machine direction (CD), which can facilitate web handling during processing of the upper and lower nonwovens for incorporation into a pad.
[0063] Polymer fibers of any suitable composition can be selected. Some examples of suitable polymer fibers include two-component fibers containing polyethylene (PE) and polyethylene terephthalate (PET) components or polyethylene terephthalate and copolyethylene terephthalate components. The components of the two-component fiber may be arranged in a sheath-core configuration, a parallel configuration, an eccentric sheath-core configuration, a trefoil configuration, or other suitable configurations. In some configurations, the polymer fibers may include two-component fibers having PE / PET components arranged in a concentric sheath-core configuration, where the polyethylene component forms the sheath.
[0064] While other materials may be useful in creating elastic structures, the stiffness of the PET core component in the sheath-core fiber configuration is considered useful in imparting elasticity to the upper and lower nonwoven fabrics. In a synergistic combination, the PE sheath component, which has a lower melting temperature than the PET core component, can be used to provide interfiber melting / fusion bonding brought about by the heat treatment of the precursor butt. This can help provide tensile strength to the web in both MD and CD. Such interfiber bonding helps reduce slippage between fibers, thereby further contributing to imparting dimensional stability and resilience to the material, even when the material is wet.
[0065] When a relatively high weight fraction of polymer fibers is included, more connections can be formed within the structure through heat treatment. However, too many connections can impart greater stiffness to the upper and lower nonwovens than desired. For this reason, selecting the weight fraction of polymer fibers may involve prioritizing and balancing the competing needs for stiffness and flexibility in the upper and lower nonwovens.
[0066] As described above, the upper and lower nonwoven fabrics may further contain polymer fibers that increase the elasticity of the upper and lower nonwoven fabrics. The elastic polymer fibers can help the upper and lower nonwoven fabrics maintain permeability and compression recovery. In some configurations, the upper and lower nonwoven fabrics may contain elastic polymer fibers having various cross-sections, e.g., circular and hollow spiral, and / or elastic fibers having various sizes.
[0067] The polymer fibers may be elastic and may be spun from any suitable thermoplastic resin, such as polypropylene (PP), polyethylene terephthalate (PET), or other suitable thermoplastic plastics known in the art. The elastic polymer fibers may have any suitable structure or shape. For example, the elastic polymer fibers may be circular, or may have other shapes such as helical, wavy elliptical, trefoil, wavy ribbon, and so on. Furthermore, the elastic polymer fibers may be solid, hollow, or multi-hollow. The elastic polymer fibers may be solid and round. In another preferred example, the elastic polymer fibers may include polyester / co-extruded polyester fibers. In one particular example, PET fibers may have a hollow cross-section and may have a curled or helical structure along their length. Optionally, the elastic polymer fibers may be helically crimped or flatly crimped. Elastic polymer fibers may have an average crimp value of about 4 to about 12 crimps / inch (cpi), or about 4 to about 8 cpi, or about 5 to about 7 cpi, or about 9 to about 10 cpi. Specific non-limiting examples of elastic polymer fibers are available from Wellman, Inc. (Ireland) under trade designations H1311 and T5974. Other examples of suitable elastic polymer fibers are disclosed in U.S. Patent No. 7,767,598.
[0068] The rigid polymer fibers and elastic polymer fibers should be carefully selected. For example, the constituent polymers forming the rigid polymer fibers and elastic polymer fibers may have commonalities, but the elastic polymer fibers must be selected such that the melting points of their constituents are higher than those of the bondable components of the rigid polymer fibers. Otherwise, during heat treatment, the elastic polymer fibers may bond to the rigid polymer fibers (or vice versa), thereby forming an excessively rigid structure. To avoid this risk when the rigid polymer fibers include two-component fibers, for example, core-sheath constituent fibers with a sheath component having a relatively low melting temperature at which molten bonding occurs, the elastic polymer fibers may include only the core constituent chemicals, which may be polymers with relatively high melting temperatures.
[0069] Nonwoven fabric performance can be influenced by a combination of the selection of nonwoven fiber polymers, fiber properties, and how the fibers are arranged or connected. The choice of nonwoven fabric can affect the ability of an absorbent article to recover its shape after compressive, bending, and stretching forces that occur during use due to body movement. When the fibers are short fibers (less than approximately 10 mm), the fibers are likely to rearrange irreversibly under stretching and compressive forces. Rearranging the fibers in the fiber matrix (changing their orientation / state) dissipates the tensile (stretching) or compressive force, and as a result, the energy used to affect the deformation is not available for recovery to the original shape. Longer fiber networks (typically longer than approximately 10 mm but less than approximately 100 mm) can absorb the tensile / compressive forces typical of body movement along the length of the fibers and across the structure. As a result, the absorbed forces are available to restore the structure to its original state. Longer fibrous network structures composed of finer fibers (approximately 15 to less than 20 micrometers) stretch and compress more easily. As a result, fluff / AGM structures can deform more easily (and to a greater extent), but the energy associated with these deformations is relatively small and insufficient to return the structure to its original state. Thicker fibers, such as those over approximately 20 micrometers or approximately 2.0 DTex to 10 DTex, are both flexible under bodily force but provide sufficient fiber and web recovery energy to return the structure to its original state.
[0070] From a structural standpoint, the arrangement of fibers in a long-fiber network structure can affect the performance of absorbent articles containing these nonwovens. Long-fiber webs of thicker fibers are typically bulkier than conventional thin spunbond nonwoven webs, which consist of continuous fine fibers that are closely spaced and physically bonded together. By creating webs of thicker fibers arranged in a more random orientation, which can be achieved through carding, water entanglement, and needling, the fibers can be stretched and compressed, thereby allowing them to adjust their arrangement only temporarily (spaces between fibers exist for these arrangements) and to bear / store deformation forces, this energy being available to restore the structural shape.
[0071] Furthermore, thinner synthetic fibers (less than approximately 2.0 DTex), such as BiCo and PP fibers commonly found in spunbond, are densely spaced, aligned relatively parallel to each other, and tightly bonded together. Because these bonded fibers within the spunbond web are interconnected (by closely spaced point bonds), under tension (stretching), the fibers are forced to stretch at the polymer level, and the polymer chains within the fibers are permanently rearranged. As a result, the fibers themselves remain potentially permanently stretched (permanently distorted) and can no longer return to their original state.
[0072] In some configurations, the polymer fibers in the upper nonwoven layer and the polymer fibers in the lower nonwoven layer may be different. In some configurations, the polymer fibers in the upper nonwoven layer and the polymer fibers in the lower nonwoven layer may be the same. In some configurations, the upper nonwoven layer may be a carded nonwoven fabric. In some configurations, the upper nonwoven layer may be air-through bonded or water-flow entangled. In some configurations, the upper nonwoven layer may not be a spunbond material.
[0073] Examples of suitable nonwoven materials, though not limited to them, include: (i) a 40gsm carded elastic nonwoven material manufactured by Yanjan China (material code; ATB Z87G-40-90), which is a carded nonwoven composed of a blend of 60% 2DTex and 40% 4DTex BiCo(PE / PET) fibers. These fibers are bonded together (ATB = "hot" air bond) to form a wet elastic network structure. The basis weight of the material is 40gsm, and its caliper (under 7kPa) is approximately 0.9mm. Although not bound by theory, due to the presence of 4DTex BiCo fibers and the interfiber-bonded BiCo network structure, the material exhibits low permanent strain (less than approximately 0.013mm / mm) and sufficient dry recovery energy (approximately 0.03N) in wet and dry CD ultra-high sensitivity three-point bending methods. * (ii) A 55gsm elastic spunlace material manufactured by Sandler Germany (material code: 53FC041001), which is a water-flow entangled nonwoven fabric produced by water-flow entanglement using a carding process (as described above for the nonwoven fabric), followed by an upward drying process (as described in U.S. Patent Application Publication No. 2020 / 0315873(A1)) that produces both entangled and BiCo-bonded elastic reticular structures. It contains a fiber blend of 30% 10DTex HS-PET, 50% 2.2DTex BiCo(PE / PET), and 20% 1.3DTex rayon. Thus, this material exhibits low permanent strain (less than approximately 0.013 mm / mm) and sufficient drying recovery energy (approximately 0.03 N) in wet and dry CD ultra-high sensitivity three-point bending methods. *(iii) A water-flow entangled nonwoven fabric produced by Sandler Germany (material code: 53FC041005 opt82), which is produced by water-flow entanglement through a carding process (such as the nonwoven fabric described above) and a subsequent rising drying process (such as the one described in U.S. Patent Application Publication No. 2020 / 0315873(A1)) that produces both entanglement and a BiCo-bonded elastic lattice structure. This material contains a fiber blend of 60% 5.8DTex BiCo(PE / PET), 20% 3.3DTex trefoil-shaped "structure" rayon, and 20% 1.3DTex rayon. Thus, this material exhibits low permanent strain (less than about 0.013 mm / mm) and sufficient drying recovery energy (about 0.03 N) in wet and dry CD ultra-high sensitivity three-point bending methods. * It has a thickness of over mm. This material contains 40% rayon, which can soften when wet, but the use of structural trifoliate rayon fibers helps maintain structural stability in wet conditions.
[0074] In combination with adjusting pore size, volume, and number by selecting appropriate fiber size, basis weight, and degree of compaction, manufacturers may wish to select fiber components to obtain specific surface chemical properties, such as hydrophobic or hydrophilic surfaces, or blends of different fibers and / or fibers with z-directional layering or gradients. Fibers with hydrophilic surfaces tend to attract and move along the aqueous components of menstrual fluid, in a manner that facilitates suction after discharge and rapid fluid acquisition. However, at the same time, the dominance of hydrophilic fiber surfaces in the top sheet may increase the tendency of the top sheet to reacquire fluid from the absorbent components below (re-wetting), which can cause an undesirable wet feeling for the user. On the other hand, fibers with hydrophobic surfaces tend to repel the aqueous components of menstrual fluid and / or resist the movement of fluid along their surfaces, thereby resisting suction, but also resisting re-wetting. Manufacturers may desire to find the right balance when selecting constituent fibers with hydrophilic surfaces, fibers with hydrophobic surfaces, or blends and / or z-directional lamination for any particular product design, in combination with fiber size, fiber reinforcement level, and the resulting top sheet pore size, volume, and number.
[0075] The inner core layer is manufactured by the air-lay method. A flow of cellulose and superabsorbent particles is carried on a high-speed airflow and deposited into a three-dimensional molded pocket on a rotational molding drum with downward vacuum suction to draw the cellulose and superabsorbent particles into the pocket of the laydown station. This molded pocket provides the actual physical shape of the absorbent core structure. The upper or lower nonwoven fabric may be introduced onto the molding drum first, and under vacuum, the upper or lower nonwoven fabric is stretched into the three-dimensional pocket shape. In this case, the flow of cellulose and superabsorbent particle material is deposited directly onto the upper (or lower) nonwoven fabric material at the molding station. Before entering the molding station, the nonwoven fabric is coated with an adhesive to provide a stronger bond between the cellulose and superabsorbent polymer in the nonwoven layer. Particularly suitable adhesives include high-wet-strength adhesives such as Technomelt DM9036U, available from Henkel (Germany). Upon exiting the laydown section, the second remaining nonwoven layer is combined with the nonwoven supporting the cellulose and superabsorbent particle layer exiting the laydown section. This second remaining nonwoven (either the upper or lower nonwoven, depending on which nonwoven passes through the laydown section) is pre-coated with an adhesive to allow for a perimeter seal and to better integrate the cellulose and superabsorbent particles without obstructing the flow of liquid into the cellulose and superabsorbent particle matrix. In an alternative method, the nonwoven is not initially introduced into the molding station, and the mass of cellulose and superabsorbent particles is held on a molding drum under vacuum until it is discharged onto either the upper or lower nonwoven layer coated with the adhesive as detailed above, and then sealed with the second remaining nonwoven to create an absorbent core structure. The widths of the upper and lower nonwoven webs are typically selected to be wider than the maximum width of the molded cellulose and superabsorbent particle matrix, thereby enabling an effective periphery seal where the two nonwovens connect at least on the leftmost and rightmost sides of the absorbent core structure.
[0076] The inner core layer may contain one of a wide variety of liquid-absorbent materials widely used in disposable absorbent articles, such as crushed wood pulp, commonly known as air felt. One suitable absorbent core material is the air felt material available from Weyerhaeuser Company (Washington, USA) under code number FR516. Other suitable liquid-absorbent materials used for the absorbent core include crepe cellulose wadding, meltblown polymers including coform, synthetic fibers such as chemically hardened, modified, or crosslinked cellulose fibers or crimped polyester fibers, peat moss, cotton, bamboo, eucalyptus, absorbent polymer materials, or any equivalent materials or combinations thereof.
[0077] Absorbent polymer materials for use in absorbent articles typically include water-insoluble, water-swellable, hydrogel-forming, cross-linked absorbent polymers that can absorb large amounts of liquid and retain such absorbed liquid under moderate pressure.
[0078] The absorbent polymer material for the absorbent core according to this disclosure may include superabsorbent particles, also known as “superabsorbent material” or “absorbent gelling material.” Typically, the absorbent polymer material in particulate form may be selected from polyacrylates and polyacrylate-based materials, such as partially neutralized crosslinked polyacrylates. The term “particles” refers to granules, fibers, flakes, spheres, powders, plates, and other shapes and forms known to those skilled in the art of superabsorbent particles. In some embodiments, the superabsorbent particles may be in the form of fibers, i.e., elongated needle-shaped superabsorbent particles.
[0079] In some configurations, the inner core layer may contain cellulose fibers and superabsorbent particles. In some structures, the inner core layer may contain cellulose fibers in an amount of about 50% to about 85% by weight, or about 55% to about 80% by weight, or about 60% to about 75% by weight of the inner core layer. The inner core layer may contain superabsorbent particles in an amount of about 15% to about 50% by weight, or about 20% to about 50% by weight, or about 25% to about 40% by weight, or about 30% to about 35% by weight of the inner core layer. In some configurations, the inner core layer may contain cellulose fibers in an amount of about 125 gsm to about 350 gsm. In some configurations, the inner core layer may contain superabsorbent particles in an amount of about 20 gsm to about 125 gsm.
[0080] In some configurations, the inner core layer may contain approximately 50% to 85% cellulosic fibers and approximately 15% to 50% superabsorbent particles. The absorbent core structure has a density of approximately 0.045 g / cm³. 3 ~Approx. 0.15g / cm 3 , and / or 0.045 g / cm³ 3 ~0.12 g / cm³ 3 The absorbent article may have an average density of approximately 0.045 g / cm³. 3 ~Approx. 0.16g / cm 3 It may have an average density.
[0081] Absorbent core structures can be compressed and then nearly recover to their original shape after the compression process. A suitable absorbent core structure requires little force to compress (low resistance), and the structure can nearly recover its shape when the user periodically compresses it and releases the compressive force through various body movements. To achieve this, the structure maintains sufficient recovery energy after multiple periodic compressions. Without sufficient recovery energy, the structure may remain compressed and deformed due to insufficient force (stored energy) to recover.
[0082] The absorbent article 20 may be elastic and conformable, and can provide excellent comfort during use without substantially agglomeration and / or compression. The absorbent article can be subjected to bodily force and can almost return to its original state. The absorbent article has a bending strength of approximately 0.07 to 0.30 N / mm² when measured by wet and dry CD and MD three-point bending methods. 2 , or approximately 0.10 to approximately 0.25 N / mm 2 , or approximately 0.10 to approximately 0.20 N / mm 2 It may have a dry modulus of CD.
[0083] The absorbent article may have a dry caliper of approximately 2.0 mm to 6.0 mm, or approximately 2.0 mm to 4.5 mm, or approximately 2.5 mm to 4.0 mm, when measured according to the wet and dry CD and MD3-point method. In some configurations, the absorbent article has a dry caliper of approximately 0.07 to 0.30 N / mm² when measured according to the wet and dry CD and MD3-point method. 2 The dry modulus of CD and dry caliper of approximately 2.0 mm to 4.5 mm, or approximately 0.10 to 0.25 N / mm 2 The CD dry modulus may be 0.5 mm to 0.4 mm and the dry caliper may be 0.4 mm. The absorbent article has a dry modulus of approximately 7.0 to 0.30.0 N when measured by the wet and dry CD and MD three-point bending method. * mm 2 , or approximately 10.0 to approximately 25.0 N * mm 2 , or approximately 10.0 to 20.0 N * mm 2 , or approximately 13.0 to 20.0 N * mm 2 It may have the dry bending rigidity of CD.
[0084] Absorbent materials have a condensation capacity of approximately 1.0 to 3.5 N. * mm, or approximately 1.5 to 3.0 N * mm, or approximately 1.5 to 2.8 N * It may have a fifth-cycle wetting recovery energy of mm. Particularly preferred absorbent articles are about 1.0 to 3.5 N. * It may have a fifth-cycle wet recovery energy of mm and a fifth-cycle wet recovery percentage of approximately 29% to approximately 40%.
[0085] Top sheet The top sheet 110 may be formed from any suitable nonwoven web or molded film material. Referring again to the figure, the top sheet 110 is positioned adjacent to the wearer-facing surface of the absorbent article 20 and may be bonded to the surface and to the back sheet 130 by any suitable attachment or bonding method. The top sheet 110 and the back sheet 130 may be directly bonded to each other in the outer peripheral region around the absorbent core structure, or they may be indirectly bonded by directly bonding to the wearer-facing surface and the outer-facing surface of the absorbent article, or to any additional optional layer included in the absorbent article, respectively.
[0086] The absorbent article 20 may have any known or other effective top sheet 110, such as one that conforms to the wearer's skin, is soft to the touch, and is non-irritating. Preferred top sheet materials include liquid-permeable materials that are comfortable when in contact with the wearer's skin and allow discharged menstrual fluid to rapidly permeate through them. Some preferred examples of top sheet materials include laminated structures including films, nonwovens, film / nonwoven layers, film / film layers, and nonwoven / nonwoven layers.
[0087] Non-limiting examples of nonwoven web materials that may be suitable for use in forming the top sheet 110 include fibrous materials made from natural fibers, modified natural fibers, synthetic fibers, or combinations thereof. Several suitable examples are described in U.S. Patents No. 4,950,264, 4,988,344, 4,988,345, 3,978,185, 7,785,690, 7,838,099, 5,792,404, and 5,665,452.
[0088] The top sheet 110 may be adaptable, soft to the touch, and non-irritating to the wearer's skin. Furthermore, the top sheet 110 may be liquid permeable so that liquids (e.g., urine, menstrual blood) can easily penetrate its thickness. Some preferred examples of top sheet materials include laminated structures including films, nonwovens, film / nonwoven layers, film / film layers, and nonwoven / nonwoven layers. Other exemplary top sheet materials and designs are disclosed in U.S. Patent Applications Publications 2016 / 0129661, 2016 / 0167334, and 2016 / 0278986.
[0089] In some examples, the top sheet 110 may include tufts as described in U.S. Patents No. 8,728,049, 7,553,532, 7,172,801, 8,440,286, 7,648,752, and 7,410,683. The top sheet 20 may have a pattern of individual hair-like fibrils as described in U.S. Patent No. 7,655,176 or 7,402,723. Additional examples of preferred top sheet materials are described in U.S. Patents No. 8,614,365, 8,704,036, 6,025,535, and U.S. Patent Application Publication 2015 / 041640. Another preferred top sheet may be formed from a three-dimensional substrate as detailed in U.S. Patent Application Publication 2017 / 0258647. The top sheet may have one or more layers, as described in U.S. Patent Application Publications 2016 / 0167334, 2016 / 0166443, and 2017 / 0258651.
[0090] In some examples, the top sheet 110 may be formed from a spunbond web nonwoven web material comprising single-component continuous fibers, or alternatively, two-component or multi-component fibers, or a blend of single-component fibers spun from different polymer resins, or any combination thereof. The top sheet may also be a molded nonwoven top sheet, as disclosed in U.S. Patent Application Publication No. 2019 / 0380887.
[0091] To ensure that fluids in contact with the top surface (facing the wearer) of the top sheet move suitably and rapidly in the z-direction to the bottom surface (facing outward) of the top sheet, where they can be drawn into the absorbent layer, it may be important to ensure that the nonwoven web material forming the top sheet has an appropriate weight / volume density, thereby reflecting the suitable presence of pores (also called "pores") in and between the constituent fibers through which fluids can move within the nonwoven material. In some situations, a nonwoven with fibers that are too densely compacted may have an insufficient number and / or volume and / or size of pores, and the nonwoven will hinder rather than facilitate rapid downward z-direction fluid movement. On the other hand, a nonwoven with fibers that are too large and / or not compacted to provide a certain level of opacity (for the purpose of concealing fluids absorbed into the layer below) and a substantial appearance may be perceived negatively by the user.
[0092] The caliper of the top sheet material can be controlled to balance the conflicting needs of opacity and loft (requiring a higher caliper) and the limited z-direction distance through the top sheet from the wearer-facing surface to the outward-facing surface in order for the discharged fluid to reach the underlying absorbent core structure. Therefore, it may be desirable to control the production of top sheet materials to produce top sheet materials with calipers of approximately 0.20 mm to 1.0 mm, or approximately 0.25 mm to 0.80 mm, or approximately 0.30 mm to 0.60 mm.
[0093] In some configurations, the absorbent article does not need to include a separate top sheet, and the upper nonwoven fabric layer can function as the top sheet.
[0094] Secondary Top Sheet (STS) In some situations, the STS layer may be included between the top sheet and the absorbent core structure, allowing the absorbent core structure to readily receive the sudden discharge of fluid, and after receiving it, to draw it up along the x and y directions and distribute it across the absorbent core structure below.
[0095] If included, the STS may be a nonwoven fiber structure that may include cellulose fibers, noncellulose fibers (e.g., fibers spun from polymer resins), or blends thereof. To accommodate the folding and lateral gathering of the absorbent article 20 and the absorbent core structure 10, the STS may be formed from a relatively flexible (i.e., relatively low bending stiffness) material, as described herein.
[0096] Several specific examples of preferred STS compositions and structures, and combinations thereof with preferred topsheet compositions and structures, are described in U.S. Patent Applications Nos. 16 / 831,862, 16 / 831,854, 16 / 832,270, 16 / 831,865, 16 / 831,868, 16 / 831,870, and 16 / 831,879, and U.S. Provisional Patent Applications Nos. 63 / 086,610 and 63 / 086,701. Additional preferred examples are described in U.S. Patent No. 9,504,613, International Publication No. 2012 / 040315, and U.S. Patent Application Publication No. 2019 / 0021917.
[0097] In some configurations, the absorbent material may not include a secondary top sheet.
[0098] Back seat The backsheet 130 can be positioned beneath or adjacent to the outward-facing surface of the absorbent core structure 10 and can be bonded to that surface by any preferred mounting method. For example, the backsheet 130 can be fixed to the absorbent core structure 10 by a uniform, continuous layer of adhesive, a patterned layer of adhesive, or an arrangement of separate lines, spirals, or dots of adhesive. Alternatively, mounting methods may include thermal bonding, pressure bonding, ultrasonic bonding, dynamic mechanical bonding, or any other preferred mounting mechanism, or a combination thereof. In other examples, it is intended that the absorbent core structure 10 is not directly bonded to the backsheet 130.
[0099] The backsheet 130 may be impermeable to or substantially impermeable to aqueous liquids (e.g., urine, menstrual fluid) and may be manufactured from a thin plastic film, although other flexible liquid-impermeable materials may also be used. As used herein, the term “flexible” refers to a material that is adaptable and readily conforms to the general shape and contours of the human body. The backsheet 130 can prevent, or at least substantially prevent, the fluid absorbed and contained within the absorbent core structure 10 from escaping from and reaching articles of the wearer’s clothing that may come into contact with the absorbent articles 20, such as underwear and other clothing. However, in some examples, the backsheet 130 may be manufactured to allow vapors to escape from the absorbent core structure 10 (i.e., the backsheet is made to be breathable), while in other examples, the backsheet 130 may be manufactured not to allow vapors to escape (i.e., it is made to be non-breathable). Thus, the backsheet 130 may include a polymer film, such as a polyethylene or polypropylene thermoplastic film. Suitable materials for the backsheet 130 are, for example, thermoplastic films having a thickness of about 0.012 mm (0.5 mil) to about 0.051 mm (2.0 mil). Any suitable backsheet known in the art may be used in conjunction with the present invention.
[0100] Some preferred examples of materials suitable for forming a backsheet may include tufts as described in U.S. Patents Nos. 5,885,265, 4,342,314, and 4,463,045. Suitable single-layer breathable backsheets for use herein include, for example, those described in UK Patent Application Publications Nos. 2184389(A), 2184390(A), and 2184391(A), U.S. Patents Nos. 4,591,523, 3,989,867, and 3,156,242, International Publication No. 97 / 24097, U.S. Patents Nos. 6,623,464, 6,664,439, and 6,436,508.
[0101] The backsheet 130 may have two layers: a first layer comprising a vapor-permeable perforated film layer, and a second layer comprising a breathable microporous film layer, as described in U.S. Patent No. 6,462,251. Other suitable examples of double or multilayer breathable backsheets for use herein include those described in U.S. Patents No. 3,881,489, No. 4,341,216, No. 4,713,068, No. 4,818,600, European Patent Application Publications No. 203821, No. 710471, No. 710472, and No. 0793952.
[0102] Other features In some configurations, the absorbent article 20 may include panty fastening components such as panty fastening adhesive or components of a hook-and-loop fastening system (such as VELCRO®).
[0103] In some configurations, the absorbent article 20 may include a panty-fastening adhesive disposed on the garment-facing side of the backsheet 130 to provide a mechanism for the user to adhere the absorbent article to the crotch area inside the underwear. The panty-fastening adhesive may include any adhesive or glue used in the art for such purposes. These adhesives are typically pressure-sensitive and maintain tackiness much lower than their application temperature. In some configurations, the panty-fastening adhesive may be a pressure-sensitive hot-melt adhesive. The panty-fastening adhesive may be applied in a pattern such as that described in U.S. Patent Application Publication 2020 / 0281782(A1). When the absorbent article 20 is packaged for transport, handling and storage before use, the panty-fastening adhesive may be covered with a protective cover (not shown), such as silicone-coated release paper, silicone-coated plastic film, or any other easily removable cover. The protective cover may be provided as a single piece or in multiple pieces to cover individual adhesive areas, such as on the backsheet and / or wings. The protective cover may cover / shield the adhesive deposit from contact with other surfaces until the user is ready to remove the protective cover for wearing / use and place the absorbent article in their underwear. The protective cover may also function as individual packaging for the article or provide a disposal function known in the art. Any commercially available release paper or film may be used. Preferred examples include BL 30 MG-A SILOX EI / O and BL 30 MG-A SILOX 4 P / O, available from Akrosil Corporation, and M&W film, available from Gronau, Germany, under code X-5432. In some configurations, the absorbent article may be packaged in a folded or tri-fold state.
[0104] In some configurations, the absorbent article 20 may include opposing wing portions 140, 150 on each side that extend laterally beyond the longitudinal edge of the absorbent portion of the absorbent article by a width dimension relatively larger than the width dimension of the front and rear portions of the absorbent article. Wings are now commonly provided on women's sanitary absorbent articles. As provided, they typically have an adhesive deposit applied to their outward-facing surface (the surface is outward before the absorbent article is placed in the user's underwear and the wings are applied). The wing portions may also include an adhesive deposit as described above, so that the user can wrap the wing portions around the inner edge through the leg opening of the underwear and adhere the wing portions to the outward-facing surface / underside of the underwear in the crotch area, providing auxiliary retaining support for the absorbent article and helping to protect the underwear from soiling in close proximity to the leg edge of the underwear.
[0105] package Typically, products such as absorbent articles are not sold individually, but rather in packages containing multiple absorbent articles, such as packages containing approximately 5 to 30 absorbent articles. The absorbent articles of this disclosure may be packaged. The packages may include polymer film, paper material, cardboard for cartons, and / or other materials. Figures and / or markings relating to the properties of the absorbent articles may be formed, printed, positioned, and / or placed on the outer portion of the package. Each package may contain multiple absorbent articles. The absorbent articles may be packaged under compression to reduce the package size while still providing a sufficient quantity of absorbent articles per package. By packaging absorbent articles under compression, users and caregivers can easily handle and store the packages, particularly in bathrooms and other places with limited space, and at the same time, it also provides manufacturers with reduced logistics costs due to the package size.
[0106] In some configurations, the absorbent articles may be packaged in a polybag. In some configurations, the package may be a plastic "shrink-package" container. As shown in Figure 12A, package 500 is a polybag. Package 500 has an internal space 502, an external surface 512, and dimensions of height, width, and depth. Package 500 may be any shape known in the art. For example, package may have the shape of a polyhedron defining or forming a polyhedron enclosure. The interior 502 defines an internal space for containing the absorbent articles 20. In some configurations, the absorbent articles may all be identical to one another.
[0107] The absorbent articles 20 may be arranged to form a laminate 506 inside the package 500 502. The articles may be stacked in any direction. As used herein, the term “laminated” means a regular stack. For example, the articles may be stacked vertically, horizontally, or at any angle inside the package. As shown in Figure 12A, the package 500 has a filled bag width (FBW) 508, defined as the maximum distance between two highest bulging points along the same compression laminate axis 510 of the package. As shown in Figure 12B, the package 500 has a filled bag height (FBH) 520, defined as the maximum distance between the highest points of the bottom panel and the top panel. As shown in Figure 13, the package 500 has a filled bag depth (FBD) 530, defined as the maximum distance between the front panel and the back panel of the package 500. The absorbent articles according to this disclosure may be folded in half, folded in thirds, rolled up, unfolded, or in any other configuration suitable for packaging absorbent articles. The package 500 may also include mechanisms or means for accessing the internal space, such as gussets, perforations, tabs, adhesive openings, or any other means known in the art.
[0108] Package 500 may consist of different materials or substantially the same type of materials. Package 500 may consist of a single layer or laminate. This material may include blown or cast films in blends with low-density polyethylene and linear low-density polyethylene, metallocene, ethylene vinyl acetate, surlyn, polyethylene terephthalate, biaxially oriented polypropylene, and / or nylon.
[0109] In some structures, package 500 may include a polymer film containing recycled material, e.g., about 20% to about 100%, about 30% to about 90%, about 30% to about 80%, about 40% to about 60%, or about 50% recycled material. The recycled material may include post-industrial recycled material (PIR) and / or post-consumer recycled material (PCR). In some cases, the polymer film used for the package may include two outer layers and one or more inner layers. One or more inner layers may contain recycled material, or may contain more recycled material than the outer layers. The recycled material may include recycled polyethylene. The recycled material may include recycled polyethylene PIR from cuts from packaging operations.
[0110] The packaging material may include paper, paper-based materials, paper with one or more barrier layers, or paper / film laminates. The packaging material may be in the range of about 50 gsm to about 100 gsm or about 70 gsm to about 90 gsm, and the one or more barrier layers may be in the range of about 3 gsm to about 15 gsm. With or without one or more barrier layers, the paper-based packaging material may exhibit a mechanical tensile strength of at least 5.0 kN / m, at least 3 percent mechanical expansion and contraction, at least 3 kN / m mechanical transverse tensile strength, and at least 4 percent transverse fracture expansion and contraction, as determined by ISO 1924-3.
[0111] Paper-based packaging materials, or paper-based packaging materials including a barrier layer or film, may be recyclable or recyclable in normal paper recycling operations. The degree of recyclability of paper-based packaging can be determined by the recyclability percentage. Paper-based packaging of the Disclosure may exhibit a recyclability percentage of 70 percent or more, 80 percent or more, or 90 percent or more. Paper-based packaging of the Disclosure may have a recyclability percentage of about 70 percent to about 99.9 percent, about 80 percent to about 99.9 percent, or about 90 percent to about 99.9 percent. For example, packaging materials of the Disclosure may exhibit a recyclability percentage of about 95 percent to about 99.9 percent, about 97 percent to about 99.9 percent, or about 98 percent to about 99.9 percent. The recyclability percentage of paper-based packaging can be determined by Category II testing PTS-RH:021 / 97 (draft October 2019), conducted by Papiertechnische Stiftung, located at Pirnaer Strasse 37, 01809 Heidenau, Germany. In another example, the paper-based packaging of this disclosure may show an overall "pass" test result when determined by Category II method PTS-RH:021 / 97 (draft October 2019). Any of the paper-based packaging may have opening features such as perforations and may also have handles.
[0112] Surprisingly, the absorbent articles described herein have been found to be able to be compressed, retained in a package for extended periods, and still largely recover their pre-compression caliper height. For example, the absorbent products according to this disclosure may have in-bag compression of about 40% or less, or about 5% to about 35%, or about 15% to about 30%, without adversely affecting the flexibility, conformability, or fluid handling performance of the absorbent articles. As used herein, “in-bag compression” is the number obtained by subtracting from 1 the number obtained by dividing the height of a stack of 10 absorbent articles in millimeters, measured under in-bag compression, by the height of a stack of 10 absorbent articles of the same type before compression, multiplying by 100. This number is reported as a percentage.
[0113] In some configurations, the absorbent product may include absorbent articles having an average in-bag pad caliper of approximately 2.0 mm to 5.5 mm, or approximately 2.5 mm to 4.0 mm, or approximately 2.75 mm to 3.5 mm, when measured according to the in-bag compression recovery method.
[0114] In some configurations, the absorbent product may include an absorbent article having an average outer bag pad caliper of approximately 2.0 mm to approximately 6.0 mm, or approximately 3.0 mm to approximately 5.0 mm, two minutes after being removed from the package, as measured according to the in-bag compression recovery method. In some configurations, the absorbent product may include an absorbent article having an average outer bag pad caliper of approximately 2.0 mm to approximately 6.0 mm, or approximately 3.0 mm to approximately 5.0 mm, four hours after being removed from the package, as measured according to the in-bag compression recovery method.
[0115] In some configurations, the absorbent product may include absorbent articles having a caliper recovery percentage of at least 4%, or at least 10%, or at least 15% two minutes after being removed from the package, as measured according to the in-bag compression recovery method. In some configurations, the absorbent product may include absorbent articles having a caliper recovery percentage of about 3% to about 35%, or about 10% to about 30%, or about 12% to about 25% two minutes after being removed from the package, as measured according to the in-bag compression recovery method.
[0116] In some configurations, the absorbent product may include absorbent articles having a caliper recovery percentage of at least 4%, or at least 10%, or at least 15% four hours after being removed from the package, as measured according to the in-bag compression recovery method. In some configurations, the absorbent product may include absorbent articles having a caliper recovery percentage of about 4% to about 35%, or about 10% to about 30%, or about 15% to about 30%, as measured according to the in-bag compression recovery method, four hours after being removed from the package.
[0117] In some configurations, the absorbent product weighs approximately 0.20 g / cm³ when measured according to the in-bag compression recovery method. 3 The following, or approximately 0.07 g / cm³ 3 ~Approx. 0.17g / cm 3 , or approximately 0.10 g / cm³ 3 ~Approx. 0.15g / cm 3 It may also include absorbent articles having an average pad density within the bag.
[0118] In some configurations, the absorbent product, when measured according to the in-bag compression recovery method, measured approximately 0.06 g / cm³ two minutes after being removed from the package. 3 ~Approx. 0.16g / cm 3 The absorbent article may include an average outer-bag pad density of 0.06 g / cm³. In some configurations, the absorbent product, when measured according to the in-bag compression recovery method, has a density of approximately 0.06 g / cm³ four hours after being removed from the package. 3 ~Approx. 0.16g / cm 3 It may also include absorbent articles having an average outer bag pad density.
[0119] This disclosure also relates to a process for packaging multiple disposable absorbent articles, such as feminine hygiene pads. This process is a. A process for providing a plurality of disposable absorbent articles, wherein each disposable absorbent article includes an absorbent core structure disposed between a top sheet and a back sheet, the absorbent core structure includes an upper nonwoven fabric layer containing polymer fibers and having a basis weight of about 30 gsm to about 85 gsm, a lower nonwoven fabric layer containing polymer fibers and having a basis weight of about 7 gsm to about 40 gsm, and an inner core layer containing cellulose fibers and superabsorbent particles, and at least a portion of the inner core layer is disposed between the upper nonwoven fabric layer and the lower nonwoven fabric layer. b. A step of folding each of the multiple disposable absorbent articles to form multiple folded disposable absorbent articles, c. A step of arranging multiple folded disposable absorbent articles to form a laminate of folded disposable absorbent articles, d. A step of compressing a laminate of folded disposable absorbent articles along a compression axis to form a compressed laminate of folded disposable absorbent articles, e. A step of placing a compressed laminate of folded disposable absorbent articles into the internal space of a package, wherein the compressed laminate of folded disposable absorbent articles is placed into the internal space of the package such that the compression axis of the laminate of folded disposable absorbent articles is oriented substantially along the width dimension of the package. f. The package may include a step of closing the package such that the folded disposable absorbent article exhibits an average in-bag folded caliper of less than 18 mm, or about 7.0 to about 15.0 mm, or about 8.0 mm to about 13.0 mm, and when removed from the package, the disposable feminine hygiene pad exhibits a caliper recovery percentage of at least 4% in 2 minutes, as measured according to the in-bag compression recovery method.
[0120] In some configurations, multiple disposable absorbent articles may not need to be folded and may be arranged to form a substantially flat layer of disposable absorbent articles. In such configurations, the disposable absorbent articles may exhibit an average in-bag pad caliper of about 2.5 mm to about 5.5 mm.
[0121] Test method Target audience For any of the following methods in which not all constituent layers of the article are tested, the layer to be tested may be separated from the layers not being tested using cryospray as necessary.
[0122] Fracture strain method The force-displacement behavior of the specimen is measured on a universal constant-speed elongation test frame equipped with a load cell in which the measured force is within 1% to 99% of the cell's limit (a suitable instrument is the MTS Alliance with TestSuite Software, available from MTS Systems Corp. (Eden Prairie, MN), or an equivalent). The specimen is subjected to tensile elongation at a constant speed (mm / sec) until fracture, and the fracture strain percentage is measured. All tests are conducted in a room controlled at 23°C ± 3°C and 50% ± 2% relative humidity, and the test specimen is conditioned in this environment for at least 2 hours prior to testing.
[0123] The fixtures used to grip the test specimens are lightweight (<80 grams) vise-type clamps having gripping surfaces of semi-cylindrical steel versus rubber-coated steel, at least 40 mm wide. The fixtures are mounted on a universal test frame and aligned horizontally and vertically to one another.
[0124] Measurements are performed on test specimens taken from raw material rolls or sheets, or from material layers excised from absorbent articles. When excising material layers from absorbent articles, care is taken to avoid any contamination or deformation of the sample layer during the process. The excised layer should not contain any residual adhesive or fibers that may have migrated from the underlying layer. To ensure that all adhesive and migrated fibers are removed, the layer is immersed in a suitable solvent that dissolves the adhesive without adversely affecting the material itself and removes all present migrated fibers. One such solvent is THF (general-purpose tetrahydrofuran, CAS 109-99-9, available from any convenient source). After solvent immersion, the material layer is air-dried completely in a manner that prevents unwanted stretching or other deformation of the material. After the material is dry, test specimens are prepared as follows: The test specimens are cut from a region of the test material that does not contain folds or wrinkles. The test specimen is 100 mm long (parallel to the transverse axis of the article, or the intended transverse axis) and 25.4 mm wide (parallel to the longitudinal axis of the article, or the intended longitudinal axis). Similarly, five duplicate test specimens are prepared.
[0125] Prepare the universal test frame as follows: Set the initial grip separation distance to the nominal gauge length of 80 mm, then zero the crosshead. Program the test frame to bring the grips closer together by intentionally loosening them by 1 mm to ensure that there is no pre-tension in the specimen at the start of the test. (During this movement, the specimen loosens between the grips.) Next, move the grips apart at a loosening rate of 1 mm / second until the loosening preload exceeds 0.05 N. (At this point, use the crosshead position signal to calculate the looseness of the specimen, the adjusted gauge length, and define the strain as zero, i.e., 0.0). Next, move the grips apart at a rate of 1 mm / second until the specimen breaks or exceeds the instrument's extension limit.
[0126] The test is performed by inserting the specimen into the grip so that its long axis is parallel to the movement of the crosshead and positioned at the center of that movement. The test is started and force ("load") and displacement data are continuously collected at a data acquisition rate of 100 Hz.
[0127] Create a graph of load (N) versus displacement (mm). Determine the peak load from the curve, and then determine the fracture sensitivity as follows: Determine the crosshead position at which the load signal decreases by 75% after reaching the peak load, and record this as the final specimen length (Lf) in units of 0.01 mm. Define the initial specimen length by the crosshead position when the loosening preload of 0.05 N is exceeded, and record this value as the initial specimen length (Li) in units of 0.01 mm. Calculate the fracture strain percentage as follows and record it in the nearest 1 percent unit. Fracture strain % = ((Lf - Li) / Li) * 100
[0128] Repeat this procedure for all five duplicate specimens in the same manner. Calculate the arithmetic mean of the fracture strain % of the five duplicate specimens and report it as fracture strain % in 1-percent increments.
[0129] Wet and dry CD and MD three-point bending method The bending properties of absorbent material test specimens are measured on a universal constant-speed elongation test frame equipped with load cells where the measured force is within 1% to 99% of the cell's limit (preferred instruments are the MTS Alliance with TestSuite Software, available from MTS Systems Corp. (Eden Prairie, MN), or equivalent). Tests are performed on both dry and wet specimens. The intention of this method is to simulate the deformation created in the xy plane by the wearer of an absorbent material during normal use. All tests are performed in a room adjusted to 23°C ± 3°C and 50% ± 2% relative humidity.
[0130] The bottom stationary fixture consists of two cylindrical bars made of polished stainless steel, each 3.175 mm in diameter and 110 mm in length, mounted at each end by frictionless rolling bearings. These two bars are mounted horizontally, aligned front to back and parallel to each other, with their upper radii aligned vertically, and rotate freely around the diameter of the cylinder by frictionless bearings. Furthermore, the fixture allows the two bars to move horizontally away from each other on the track, thus allowing a gap to be set between them while maintaining the orientation of the bars. The upper fixture consists of a third cylindrical bar, also made of polished stainless steel, similarly 3.175 mm in diameter and 110 mm in length, mounted at each end by frictionless rolling bearings. When in position, the bars of the upper fixture are parallel to the bars of the lower fixture and aligned front to back, and in the case of the lower fixture, are positioned centered between the bars. Both fixtures include integrated adapters suitable for fitting and securing in place at their respective positions on the universal test frame, so that the bars are perpendicular to the movement of the crossbeams of the test frame.
[0131] Set the gap ("span") between each bar of the lower fixture to 25mm ± 0.5mm (from the center of one bar to the center of the other), and align the center of the upper bar with the midpoint between each lower bar. Set the gauge (from the bottom of the upper bar to the top of the lower bar) to 1.0cm.
[0132] The thickness of the specimen ("caliper") is measured using a manual micrometer equipped with a pressure foot capable of applying a constant pressure of 0.1 psi ± 0.01 psi. The manual micrometer is a self-weight instrument with accurate readings to 0.01 mm. A suitable instrument is the Mitutoyo Series 543 ID-C Digimatic, available from VWR International, or an equivalent. The pressure foot is a circular, movable surface with a flat surface and a diameter of 25.4 mm or less. The specimen is supported by a horizontal, flat reference platform that is larger than the surface of the pressure foot and parallel to the surface of the pressure foot. Zero the micrometer relative to the horizontal, flat reference platform. Place the specimen on the platform and center it under the pressure foot. Lower the pressure foot by hand at a rate of 3 ± 1 mm / sec until the pressure of the entire weight is applied to the specimen. After 5 seconds, record the thickness as caliper in 0.01 mm increments.
[0133] The test fluid to be administered to the wet test specimen is prepared by adding 100.0 grams of sodium chloride (reagent grade, any convenient source) to 900 grams of deionized water in a 1-liter Erlenmeyer flask. Stir until the sodium chloride is completely dissolved.
[0134] Two hours prior to the test, absorbent article samples are conditioned at 23°C ± 3°C and 50% ± 2% relative humidity. Dry test samples are taken from an area of the sample free of seams, folds, or wrinkles, ideally from the center of the absorbent article (the intersection of the longitudinal and transverse centerlines). Dry test pieces are cut to a width of 50.8 mm along the CD (transverse direction, i.e., parallel to the transverse axis of the sample) and a length of 50.8 mm along the MD (parallel to the longitudinal axis of the sample), and prepared for MD (machine direction) bending by maintaining their orientation after cutting and marking the surface facing the body (or the surface intended to face the body in the finished product). The dried specimen is prepared for CD (machine direction) bending by cutting it to a width of 50.8 mm along the MD (transverse direction, i.e., parallel to the transverse axis of the sample) and a length of 50.8 mm along the CD (parallel to the longitudinal axis of the sample), maintaining their orientation after cutting, and marking the surface facing the body (or the surface intended to face the body of the finished product). The thickness of the specimen is measured as described herein and recorded as the dry specimen caliper in units of 0.01 mm. Next, the mass of the specimen is measured and recorded as the dry mass in units of 0.001 grams. The mass (g) is multiplied by the area (0.002581 m²). 2 The basis weight of the test specimen is calculated by dividing by ), and the dry basis weight of the test specimen is 0.01 g / m². 2 Record in units. Basis weight of the sample (g / m²) 2 The bulk density of the sample is calculated by dividing the given value by the sample thickness (mm), and then dividing the resulting quotient by 1000, resulting in a dry sample density of 0.01 g / cm³. 3 Record in units. Similarly, prepare five duplicate dried test specimens.
[0135] First, the wet test specimen is prepared in exactly the same manner as the dry test specimen, and then the test fluid is added immediately before testing as follows: First, the thickness and mass of the dry test specimen are measured as described herein and recorded as the initial thickness in units of 0.01 mm and the initial mass in units of 0.001 g. Next, the dry test specimen is completely immersed in the test fluid for 60 seconds. After 60 seconds, the specimen is removed from the test fluid and oriented vertically for 30 seconds to allow excess fluid to drip out. At this point, the thickness and mass of the wet test specimen are measured as described herein and recorded as the wet test specimen caliper in units of 0.01 mm and the wet test specimen mass in units of 0.001 g. If desired, the mass of the test fluid in the specimen is calculated by subtracting the initial mass (g) from the wet test specimen mass (g) and recorded as the test specimen fluid volume in units of 0.001 g. The wet test specimen must be tested within 10 minutes after being removed from the test fluid. Similarly, five duplicate wet test specimens are prepared.
[0136] The universal test frame for the deflection bending test is programmed so that the upper fixture moves downward relative to the lower fixture at a speed of 1.0 mm / second until the upper bar touches the top surface of the test specimen with a minimum force of 0.02 N, and then the crosshead is moved so that this continues for a further 12 mm. The crosshead is then immediately returned to its original position at a speed of 1.0 mm / second. Force (N) and displacement (mm) data are collected continuously at 100 Hz throughout the test.
[0137] The dry specimen is loaded so that its sides are parallel to each bar, straddling the two lower bars, and its center is positioned below the upper bar. For MD bending, the MD direction of the specimen is perpendicular to the length of the three bars. The test is started, and force and displacement data are collected continuously.
[0138] Create a graph of force (N) versus displacement (mm). From the graph, determine the maximum peak force and record it as the dry MD peak load in units of 0.01 N. Then, calculate the maximum slope of the curve between the initial force and the maximum force (in the loaded portion of the curve) and record it in units of 0.1. Calculate the modulus of elasticity as follows and record it as the dry MD modulus of elasticity of 0.001 N / mm².2 Record in units. CD or MD dry or wet flexural modulus (N / mm²) 2 ) = (slope × (span) 3 )) / (4 × sample width × (sample caliper 3 ))
[0139] The bending stiffness was calculated as follows, and the dry MD bending stiffness was 0.1 Nmm. 2 Record in units. CD or MD dry or wet bending stiffness (Nmm) 2 ) = modulus of elasticity × moment of inertia In the formula, moment of inertia (mm 4 ) = (sample width × (sample caliper 3 )) / 12
[0140] Similarly, the procedure is repeated for all five copies of the dried test specimen. The arithmetic mean of the five duplicate dried test specimens is calculated for each parameter, and the dried test specimen "caliper" is calculated in units of 0.01 mm, 0.01 g / m². 2 The unit of measurement for the dry test piece basis weight is 0.001 g / cm². 3 Dry specimen density in units of 0.01 N, dry CD or MD peak load in units of 0.01 N / mm² 2 The dry CD or MD flexural modulus and Nmm in units of elasticity. 2 Report the bending stiffness in units of dry CD or MD.
[0141] Here, the entire procedure is repeated for all five copies of the wet test specimen, and the results are expressed as wet CD or MD peak load in units of 0.01 N, 0.001 N / mm². 2 Wet CD or MD flexural modulus in units, and Nmm 2 Report the wet CD or MD bending stiffness in units.
[0142] Wet and dry CD ultra-high sensitivity three-point bending method The CD (transverse) bending properties of the test specimen are measured using a highly sensitive three-point bending test on a universal constant-speed elongation test frame equipped with load cells suitable for the force to be measured (preferred equipment is the MTS Alliance using TestSuite Software available from MTS Systems Corp. (Eden Prairie, MN), or equivalent). The test is performed on both dry and wet specimens. The intention of this method is to simulate the deformation created in the xy plane by the wearer of absorbent material during normal use. All tests are performed in a room adjusted to 23°C ± 3°C and 50% ± 2% relative humidity.
[0143] The ultra-high-sensitivity three-point bending method is designed to maximize the force signal-to-noise ratio when testing materials with very low bending forces. The force signal is maximized by using a highly sensitive load cell (e.g., 5N), a small span (load is proportional to the cube of the span), and a wide specimen width (total measured load is directly proportional to the width). The fixture is designed so that the bending measurement is performed under tension, allowing the fixture mass to be kept to a minimum. Noise in the force signal is minimized by keeping the load cell stationary to reduce mechanical vibration and inertial effects, and by keeping the mass of the fixture attached to the load cell as small as possible.
[0144] Referring to Figures 14A to 14C, the load cell 1001 is mounted on the stationary crosshead of the universal test frame. The ultra-high sensitivity fixture 1000 consists of three thin blades constructed from a lightweight rigid material (such as aluminum or equivalent). Each blade has a thickness of 1.0 mm, a rounded edge, and a length capable of accommodating a bending width of 100 mm. Each blade has cavities 1004a and 1004b (outer blades) and 1005 (center blade) cut out along their horizontal edges to create a height h of 5 mm of blade material. The two outer blades 1003a and 1003b are mounted horizontally on the movable crosshead of the universal test frame, aligned parallel to each other, with their horizontal edges aligned vertically. The span s between the two outer blades 1003a and 1003b is 5 mm ± 0.1 mm (inner edge to inner edge). The central blade 1002 is mounted on a load cell on a fixed crosshead of the universal test frame. When in place, the central blade 1002 is parallel to the two outer blades 1003a and 1003b, with its center located midway between the outer blades 1003a and 1003b. The blade fixture includes a one-piece adapter suitable for fitting and securing the blade in place at each position on the universal test frame, so that the horizontal edge of the blade is perpendicular to the movement of the crossbeam of the universal test frame.
[0145] The test fluid to be administered to the wet test specimen is prepared by adding 100.0 grams of sodium chloride (reagent grade, any convenient source) to 900 grams of deionized water in a 1-liter Erlenmeyer flask. Stir until the sodium chloride is completely dissolved.
[0146] Two hours prior to the test, the sample is conditioned at 23°C ± 3°C and 50% ± 2% relative humidity. The dried test specimen is taken from an area of the sample free of seams, folds, or wrinkles. The dried test specimen is cut to a width of 50.0 mm along the CD (transverse direction, i.e., parallel to the transverse axis of the sample) and a length of 100.0 mm along the MD (machine direction, i.e., parallel to the longitudinal axis of the sample), and prepared for the CD bend (i.e., a bend perpendicular to the transverse axis of the sample) by maintaining their orientation after cutting and marking the surface facing the body (or the surface intended to face the body of the finished product). Five duplicate dried test specimens are prepared in the same manner.
[0147] First, prepare the wet test sample in exactly the same manner as the dry test sample, and then add the test fluid immediately before testing as follows: Immerse the dry sample completely in the test fluid for 60 seconds. After 60 seconds, remove the sample from the test fluid and orient it vertically for 30 seconds to allow excess fluid to drip out. After removing the wet test sample from the test fluid, it must be tested within 10 minutes. Similarly, prepare five duplicate wet test samples.
[0148] The universal test frame is programmed so that the movable crosshead moves in the opposite direction to the fixed crosshead at a speed of 1.0 mm / second. The crosshead movement begins with the specimen 1006 flat and unbiased on the outer blades 1003a and 1003b, continues with the inner horizontal edge of the cavity 1005 within the central blade 1002 in contact with the upper surface of the specimen 1006, and is followed by an additional 4 mm crosshead movement. The crosshead stops at 4 mm and then immediately returns to zero at a speed of 1.0 mm / second. Force (N) and displacement (mm) are collected throughout at 50 Hz.
[0149] Before placing specimen 1006, the outer blades 1003a and 1003b are moved toward the central blade 1002 until a clearance C of approximately 3 mm exists between the inner horizontal edges of cavities 1004a and 1004b within the outer blades 1003a and 1003b and the inner horizontal edge of cavity 1005 within the central blade 1002, and then pass through the central blade 1002 (see Figure 14C). Specimen 1006 is positioned within clearance C so as to straddle the inner horizontal edges of cavities 1004a and 1004b within the outer blades 1003a and 1003b, with the MD (short side) of the specimen perpendicular to the horizontal edge of the blade and the body-facing surface of the specimen facing upward. Specimen 1006 is placed at the center between the outer blades 1003a and 1003b. The outer blades 1003a and 1003b are slowly moved in the opposite direction to the fixed crosshead until the inner horizontal edge of the cavity 1005 within the central blade 1002 contacts the upper surface of the test specimen 1006. The test is started, and force and displacement data are collected continuously.
[0150] Plot the force (N) against the displacement (mm). Record the maximum peak force in units of 0.001N. Calculate the area under the curve from the start of loading to the maximum peak force and express it as bending energy of 0.001N. * Record in millimeters. Recovery energy is calculated as the area under the curve where the force is unloaded from the maximum peak to 0.0 N, and is 0.001 N. * The recovery energy is recorded in millimeters. Similarly, the entire test sequence is repeated for a total of five dry specimens and five wet specimens.
[0151] For each test specimen type (dry and wet), the arithmetic mean of the maximum peak force between similar specimens is calculated in units of 0.001 N and recorded as the dry peak load and wet peak load, respectively. For each test specimen type (dry and wet), the arithmetic mean of the bending energy of similar test specimens is calculated in units of 0.001 N. * The calculations are performed in millimeters and reported as dry bending energy and wet bending energy, respectively. For each specimen type (dry and wet), the arithmetic mean of the recovery energy of similar specimens is 0.001 N.* The calculations are performed in millimeters and reported as dry recovery energy and wet recovery energy, respectively.
[0152] Wet and dry cluster compression methods The cluster compression test measures the force-versus-displacement behavior of intentionally "clustered" absorbent article test samples over five cycles of load application ("compression") and load removal ("recovery") using a universal constant-speed elongation test frame (preferred equipment is MTS Alliance using TestSuite software available from MTS Systems Corp. (Eden Prairie, MN), or equivalent) equipped with load cells where the measured force is within 1% to 99% of the cell's limit. This test is performed on dry test samples as well as wet test specimens administered with a specific amount of test fluid. The intent of this method is to simulate the deformation that occurs in the z-plane of the crotch area or its components of an absorbent article when worn by a wearer during a sit-to-stand motion. All tests are performed in a controlled room at 23°C ± 3°C and 50% ± 2% relative humidity.
[0153] Figures 15 to 16B show the test apparatus. The bottom stationary fixture 3000 consists of two matching specimen clamps 3001, each 100 mm wide, and mounted on their respective movable platforms 3002a and 3002b. The clamps have a 110 mm long "knife edge" 3009 that grips a 1 mm thick hard rubber surface 3008. When closed, the clamps are flush with the inside of their respective platforms. The clamps are aligned to hold an unbunched specimen horizontally and perpendicular to the tensile axis of the tensile testing machine. The platforms are mounted on rails 3003, which allow them to be moved horizontally from side to side and locked in place. The rails have adapters 3004 that fit the tensile testing machine, which allow the platforms to be fixed horizontally and perpendicular to the tensile axis of the tensile testing machine. The upper fixture 2000 is a cylindrical plunger 2001 with a total length of 70 mm and a diameter of 25.0 mm. The contact surface 2002 is flat and not curved. The plunger 2001 has an adapter 2003 that is suitable for mounting a load cell, which allows the plunger to be fixed perpendicular to the tensile axis of the tensile testing machine.
[0154] The test specimen is prepared for at least 2 hours before testing at 23°C ± 3°C and 50% ± 2% relative humidity. Prepare the test specimen as follows: When testing an untouched absorbent article, remove any release paper from any panty fastening adhesive on the clothing-facing side of the article, if present. Lightly coat the adhesive with talc powder to reduce stickiness. If there is a cuff, cut it off with scissors, taking care not to disturb the top sheet or any other underlayers of the article. Place the article on a bench with the body-facing surface facing upwards. Mark the intersection of the longitudinal and transverse centerlines on the article. Using a rectangular cutting die or equivalent cutting means, cut the specimen 100 mm longitudinally and 80 mm transversely, centered at the intersection of the centerlines. When testing a material layer or layered component of an absorbent article, place the material layer or component on a bench and orient it as it would be incorporated into the finished product (i.e., identify the surface facing the body, the transverse axis, and the longitudinal axis). Using a rectangular cutting die or equivalent cutting means, cut the sample into sections of 100 mm longitudinal and 80 mm transverse, centered at the intersection of the centerlines. Measure the mass of the sample and record it in units of 0.001 g. Convert the mass (g) to the area (0.008 m²). 2 The basis weight of the sample is calculated by dividing by ), and the basis weight is 1 g / m². 2 Record in units.
[0155] The test specimens can be analyzed in both wet and dry conditions. No further preparation is required for dry specimens. The test fluid to be administered to the wet specimens is prepared by adding 100.0 grams of sodium chloride (reagent grade, any convenient source) to 900 grams of deionized water in a 1-liter Erlenmeyer flask. Stir until the sodium chloride is completely dissolved. A total of 7 ml of the test solution is administered to the wet specimens, as detailed below.
[0156] Add the liquid using a graduated Eppendorf pipette, spreading the fluid over the entire surface of the sample facing the body within approximately 3 seconds. Test the wet sample for 10.0 minutes ± 0.1 minutes after application of the liquid.
[0157] The tensile testing machine is programmed to zero the load cell, then the upper device is lowered at 2.00 mm / second until the plunger's contact surface touches the specimen and the load cell reading is 0.02 N. The crosshead is then zeroed. The system is programmed to lower the crosshead by 15.00 mm at a speed of 2.00 mm / second, and immediately raise it by 15.00 mm at a speed of 2.00 mm / second. This cycle is repeated for a total of 5 cycles without delay between cycles. Data is collected at 50 Hz during all compression / decompression cycles.
[0158] Position the left platform 3002a 2.5 mm from the side of the upper plunger (distance 3005). Fix the position of the left platform. This platform 3002a remains stationary during the experiment. Align the right platform 3002b 50.0 mm from the stationary clamp (distance 3006). Raise the upper probe 2001 so that it does not obstruct the mounting of the specimen. Open both clamps 3001. Referring to Figure 16A, place the dry specimen so that its longitudinal edge (i.e., the 100 mm long edge) is inside the clamp. Align the lateral center of the dry specimen and firmly secure both edges inside the clamp. Referring to Figure 16B, move the right platform 3002b 20 mm toward the stationary platform 3002a so that a 30.0 mm separation is achieved between the left and right clamps. When the movable platform is positioned, ensure that the dry specimen is curved upwards. Here, manually lower probe 2001 until it is approximately 1 cm above the top of the specimen with the curved lower surface.
[0159] The test is initiated, and force (N) and displacement (mm) data are continuously collected over all five cycles. A force (N) versus displacement (mm) graph is created individually for each cycle. A representative curve is shown in Figure 17A. From the curves, the maximum dry compressive force for each cycle is determined in units of 0.01 N, then multiplied by 101.97, and recorded in units of 1 wt gram. The dry recovery % between the first and second cycles is calculated as (TD-E2) / (TD-E1).* Calculate using 100 (where TD is the total deviation and E2 is the extension in the second compression curve above 0.02N), and record in units of 0.01%. In the same manner, calculate the drying recovery rate % between the first cycle and the other cycles as (TD-E1) / (TD-E1) * Calculate using 100 and record in units of 0.01%. Referring to Figure 17B, the dry compression energy for cycle 1 is calculated as the area under the compression curve (i.e., area A + B), which is 0.1N. * Record in millimeters. Calculate the dry energy loss for cycle 1 as the area between the compression curve and the decompression curve (i.e., area A), and set it to 0.1 N. * Record in millimeters. Calculate the drying recovery energy for cycle 1 as the area under the decompression curve (i.e., area B), and value it as 0.1 N. * Record in millimeters. Similarly, for each of the other cycles, record the dry compression energy (N * (mm), drying energy loss (N) * mm), and drying recovery energy (N * Calculate the basis weight (mm) and record it in units of 0.1 N-mm. Similarly, analyze a total of five duplicate dried specimens and report the arithmetic mean of the five dried specimens for each parameter as described above, including basis weight.
[0160] Here, the entire procedure is repeated for a total of five replicated wet specimens, with the maximum wet compressive force in 1 gram force unit for each cycle and 0.1 N for each cycle. * Wet compression energy in millimeter units, 0.1N for each cycle. * Wet energy loss in millimeters, 0.1N per cycle * The results for each of the five cycles are reported as the arithmetic mean of five wet replications for the wet recovery energy in millimeters and the wet recovery percentage for each cycle. Of particular importance are the wet recovery energy and wet recovery percentage characteristics of the fifth cycle from this test method.
[0161] CD periodic stretching method up to 3% distortion The periodic tensile and recovery responses of absorbent material specimens are measured over 10 cycles of load application ("extension") and load removal ("recovery") using a universal constant-rate elongation test frame. The specimen is repeated 10 times up to 3% engineering strain, and then returned to zero engineering strain. For each cycle, stiffness, peak load, normalized peak energy, normalized recovery energy, strain at the start of the cycle, and strain at the end of the cycle (i.e., "permanent strain") are calculated and reported. The intent of this method is to understand the ability of a sample to be stretched in the xy plane as a result of a force on the body and then to recover to their original state. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the specimens are conditioned in this environment for at least 2 hours prior to testing.
[0162] A suitable universal constant-speed elongation test frame is an MTS Alliance or equivalent interfaced to a computer running TestSuite control software (available from MTS Systems Corp, Eden Prairie, MN). The universal test frame is equipped with load cells in which the force to be measured is within 1% to 99% of the cell's limit. The fixtures used to grip the test specimen are lightweight (<80 grams) vise-acting clamps with knife or serrated edge gripping surfaces of at least 40 mm width. The fixtures are mounted on the universal test frame and positioned horizontally and vertically relative to one another.
[0163] Measurements are performed on test specimens taken from raw material rolls or sheets, or from material layers excised from absorbent articles. When excising material layers from absorbent articles, care is taken to avoid any contamination or deformation of the sample layer during the process. The excised layer should not contain any residual adhesive or fibers that may have migrated from the underlying layer. To ensure that all adhesive and migrated fibers are removed, the layer is immersed in a suitable solvent that dissolves the adhesive without adversely affecting the material itself and removes all present migrated fibers. One such solvent is THF (general-purpose tetrahydrofuran, CAS 109-99-9, available from any convenient source). After solvent immersion, the material layer is completely air-dried in a manner that prevents unwanted stretching or other deformation of the material. After the material is dry, test specimens are obtained. The test specimens are cut from an area of the test material that does not have any folds or wrinkles remaining. The test specimen is approximately the same length as the transverse length of the article (parallel to the transverse axis of the article, or the intended transverse axis of the article). When cutting test specimens from absorbent articles of different sizes and widths, the total length of the test specimen (L) total ) may vary from product to product, and therefore the results are normalized to compensate for this variation. The test specimen has a width of 25.4 mm (parallel to the longitudinal axis of the article or the intended longitudinal axis). Test specimen width (w) = 25.4 mm. Total test specimen length (L total Measure the distance and record it in 0.1 mm increments. Prepare five duplicate specimens in the same manner.
[0164] Measure the thickness (t) of the test specimen using a manual micrometer equipped with a presser capable of applying a steady pressure of 0.1psi±0.01psi. The manual micrometer is a self-standing instrument with an accurate reading up to 0.01mm. A suitable instrument is the Mitutoyo Series 543 ID-C Digimatic available from VWR International, or an equivalent. The presser is a circular movable surface with a flat surface having a diameter of 25.4mm or less. The test specimen is larger than the surface of the presser and is supported by a horizontal flat reference platform parallel to the surface of the presser. Zero the micrometer against the horizontal flat reference platform. Place the test specimen on the platform and center it under the presser. Manually lower the presser at a descent rate of 3±1mm / sec until the full weight pressure is applied to the test specimen. After 5 seconds have elapsed, record the thickness in 0.01mm units as the test specimen thickness (t).
[0165] Prepare the universal test frame as follows. Set the initial grip separation distance to a nominal gauge length (L nominal ) that is shorter than the total length of the test specimen, to ensure that the test specimen can be gripped at both ends (i.e., L nominal <L total ). Then zero the crosshead. Program the test frame to bring the grips closer to each other by intentionally loosening 1mm, to ensure that no pre-tension exists in the test specimen at the start of the test. (During this movement, the test specimen loosens between the tensile grips.) Next, the grips move apart at a loosening speed of 1mm / sec until a loosening preload of 0.05N is exceeded. At this time: 1) Define the crosshead position signal (mm) as the slack of the test specimen (L slack ). 2) The initial test specimen gauge length (L0) is defined as nominal gauge length + slack, L0=L nominal +L slackis calculated as. Here, the unit is millimeter. 3) Set the crosshead elongation (ΔL) to zero (0.0 mm). 4) Set the crosshead displacement (mm) to zero (0.0 mm). At this position, the engineering strain is zero, that is, 0.0. Engineering strain is calculated as the change in length (ΔL) divided by the initial length (L0). Engineering strain = ΔL / L0. For one test cycle, the grips move apart at an initial speed of 1 mm / sec until the engineering strain endpoint of 0.03 mm / mm is exceeded, and immediately thereafter, the grips move toward each other at an initial speed of 1 mm / sec until the crosshead signal is below the crosshead return position of 0 mm. The test cycle is repeated until a total of 10 cycles are completed.
[0166] The test is performed by inserting the test specimen into the grips such that the long axis of the test specimen is parallel to the movement of the crosshead and centered on that movement. Start the test and continuously collect time, force and displacement data at a data acquisition rate of 100 Hz.
[0167] A graph of load (N) versus displacement is generated for all 10 cycles. For each cycle, perform the following. Record the peak load in units of 0.01 N. As the area under the load versus displacement curve from the start of the cycle to the strain endpoint of 0.03 mm / mm (during the load portion of the cycle), the peak energy (E peak ) is calculated and recorded in units of 0.01 N * mm. As the area under the load versus displacement curve from the strain endpoint of 0.03 mm / mm to the crosshead return of 0 mm (during the unloading portion of the cycle), the return energy (E return ) is calculated and recorded as the recovery energy in units of 0.01 N * mm. As the peak energy divided by the initial length, the normalized peak energy (NE peak ) is calculated (NE peak =E peak / L0) and recorded in units of 0.01 mN. As the return energy divided by the initial length, the normalized return energy (NE return ) is calculated (NE return =E returnRecord in units of 0.01 mN (L0). NE peak and NE return The unit is millinewtons (mN).
[0168] Here, we create a graph of engineering stress (σ) versus engineering strain for all 10 cycles, and perform the following for each cycle: N / mm 2 The engineering stress in units of σ is obtained by dividing the load by the cross-sectional area of the test specimen, where the cross-sectional area is the width (w) multiplied by the thickness (t) of the test specimen (σ = load / (w)). * t)). Determine the modulus of elasticity, or the slope of the stress-strain curve, along the line between the point of minimum force and the point of maximum force (between the loaded parts of the cycle), and record it as the modulus of elasticity in units of 0.01 N / mm. Calculate the stiffness by multiplying the modulus of elasticity by the thickness of the specimen, and record it as the tensile stiffness in units of 0.01 N / mm. Define the strain of the specimen at the start of the cycle as the strain when the load exceeds 0.05 N of loosening preload for that cycle (between the loaded parts of the cycle), and record it as the initial strain of the cycle in units of 0.01 mm / mm. Define the strain of the specimen at the end of the cycle as the strain when the load falls below 0.05 N of preload for that cycle (between the unloading parts of the cycle), and record it as the permanent strain in units of 0.01 mm / mm. Repeat the entire procedure in the same manner for all five copies.
[0169] The arithmetic mean of five replicated specimens is calculated for each of the 10 cycles for each parameter and reported as peak load in 0.01 N units, normalized energy versus peak in 0.01 mN units, normalized recovery energy in 0.01 mN units, tensile stiffness in 0.01 N / mm units, initial cycle strain in 0.01 mm / mm units, and permanent strain in 0.01 mm / mm units.
[0170] Nonwoven fabric thickness-pressure method The thickness of the test specimen is measured as the distance between the reference platform on which the test specimen is placed and the presser that applies a specific amount of pressure to the test specimen over a specific period of time. For the purposes of this specification, the thickness is measured under two different confinement pressures (7 g / cm²).2 and 70g / cm³ 2 The measurements are taken and reported. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the test specimens are conditioned in this environment for at least 2 hours before testing.
[0171] The thickness is determined by a constant pressure (7g / cm²). 2 and 70g / cm³ 2 The measurement is performed using a manual micrometer equipped with a clamp capable of applying pressure to the test specimen. The manual micrometer is a self-weight instrument with accurate readings to 0.01 mm. A suitable instrument is the Mitutoyo Series 543 ID-C Digimatic, available from VWR International, or an equivalent. The clamp is a flat, grounded, circular movable surface with a diameter smaller than the test specimen and capable of applying the required pressure. A suitable pressure foot has a diameter of 25.4 mm, but smaller or larger clamps can be used depending on the size of the test specimen being measured. The test specimen is supported by a horizontal, flat reference platform that is larger than the surface of the clamp and parallel to the surface of the clamp. The system is calibrated and operated according to the manufacturer's instructions.
[0172] Measurements are performed on test specimens taken from raw material rolls or sheets, or from material layers excised from absorbent articles. When excising material layers from absorbent articles, care is taken to avoid any contamination or deformation of the sample layer during the process. The excised layer should not contain any residual adhesive or fibers that may have migrated from the underlying layer. To ensure that all adhesive and all migrated fibers are removed, the layer is immersed in a suitable solvent that dissolves the adhesive without adversely affecting the material itself and removes all present migrated fibers. One such solvent is THF (general-purpose tetrahydrofuran, CAS 109-99-9, available from any convenient source). After solvent immersion, the material layer is air-dried completely in a manner that prevents unwanted stretching or other deformation of the material. After drying, the test specimen must be obtained from an area free of folds or wrinkles and must be larger than the presser foot.
[0173] 7g / cm 2 To measure the thickness at the confinement pressure, first zero the micrometers against a horizontal, flat reference platform. Place the specimen on the platform with the test position centered under the clamp. Gently lower the clamp at a rate of 3.0 mm ± 1.0 mm / sec until the full pressure is applied to the specimen. After waiting 5 seconds, record the thickness of the specimen in 0.01 mm increments. Repeat the same process for a total of 10 duplicate specimens. 7 g / cm 2 The arithmetic mean of all thickness measurements obtained at the confinement pressure was calculated to be 7 g / cm². 2 The thickness should be reported in units of 0.01 mm.
[0174] 70g / cm 2 To measure the thickness at the confinement pressure, first zero out the micrometers against a horizontal, flat reference platform. Place the specimen on the platform with the test position centered under the clamp. Gently lower the clamp at a rate of 3.0 mm ± 1.0 mm / sec until the full pressure is applied to the specimen. After waiting 5 seconds, record the thickness of the specimen in 0.01 mm increments. Repeat similarly for a total of 10 duplicate specimens. 70 g / cm2 The arithmetic mean of all thickness measurements obtained at the confinement pressure was calculated to be 70 g / cm². 2 The thickness should be reported in units of 0.01 mm.
[0175] Capture time and re-wetting method This method describes how to measure the ejection capture time, interfacial free fluid volume, and low-pressure and high-pressure re-wetting values for an absorbent article loaded with new artificial menstrual fluid (nAMF; preparation is provided separately herein). Following a pretreatment step, a known volume of nAMF is introduced into the absorbent article three times. The time required for the absorbent article to capture each dose of nAMF is measured using a permeation plate and an electronic circuit interval timer. After each fluid dose, the interfacial free fluid (IFF) is measured by gravimetric method as the fluid moves from the bottom of the permeation plate to the filter paper. Subsequently, low-pressure and high-pressure re-wetting are measured after the final fluid dosing. The surface free fluid (SFF) is the amount of fluid remaining within the top sheet of the absorbent article. The SFF is measured by performing re-wetting at low pressure (0.1 psi). Immediately after measuring the SFF, re-wetting at higher pressure (0.5 psi) is performed to determine the overall re-wetting of the absorbent article. All tests are conducted in a room maintained at 23°C ± 2°C and 50% ± 2% relative humidity.
[0176] Referring to Figures 18-20B, the permeable plate 9001 is made of plexiglass or equivalent having overall dimensions of 10.2 cm in length, 10.2 cm in width, and 3.1 cm in height. The central test fluid well 9008 has a circular opening with a diameter of 25 mm and is located on the top surface of the plate. The first side wall extends to a depth of 15 mm at a 90° angle, and then inclined downward at an 82° angle for an additional depth of 7.5 mm to reach the test fluid reservoir 9003. The test fluid reservoir 9003 is concentric with the test fluid well 9008, has a diameter of 6.6 mm, and has a side wall extending to a depth of 5 mm at a 90° angle. The test fluid reservoir 9003 opens into a longitudinal fluid channel 9007 located at the bottom of the plate. The longitudinal fluid channel 9007 has side walls that initially extend to a depth of 3.5 mm at the midpoint of the channel (directly below the test fluid reservoir 9003), and then incline downward toward each longitudinal end of the channel at an angle of 0.72° 9007a to a final depth of 3 mm. The longitudinal fluid channel opens to the bottom surface of the plate so that fluid is introduced onto the test sample below. The longitudinal fluid channel 9007 is centered on the test fluid reservoir 9003 and extends perpendicular to the electrode 9004. The longitudinal fluid channel 9007 has a width of 5 mm and a length of 80 mm and has a lateral edge that is rounded with a radius of 1.0 mm 9007b. The longitudinal end of the longitudinal fluid channel 9007 is rounded with a radius of 2.5 mm 9009. Two wells (80.5 mm long x 24.5 mm wide x 25 mm deep) located outside the fluid reservoir are filled with stainless steel shot (or equivalent) to adjust the total mass of the plate and apply 0.10 psi (7.0 g / cm³) to the test area. 2) provides a restraining pressure. The procedure for determining the test area is described later in this specification. Electrode 9004 is embedded in plate 9001 and an external banana jack 9006 is connected to the inner wall 9005 of the longitudinal fluid channel 9003. A circuit interval timer is plugged into jack 9006 and monitors the impedance between the two electrodes 9004, measuring the time from the introduction of nAMF into reservoir 9003 until the nAMF is discharged from the reservoir. The timer has a resolution of 0.01 seconds.
[0177] A pretreatment plate is used in combination with a pretreatment weight to pre-coat the surface of a test sample with nAMF droplets as a means of priming the surface of the test sample before the introduction of the full fluid dose. The pretreatment plate is made of plexiglass or equivalent, measuring 14 inches (35.6 cm) in length and 8 inches (20.3 cm) in width, with a thickness of approximately 0.25 inches (6.4 mm). The pretreatment plate has five circular markers, each 5 mm in diameter, spaced 1 cm apart (center to center), and arranged along the longitudinal axis of the plate. The center marker is centered at the midpoint of the plate in the transverse direction. These markers indicate the placement of the nAMF droplets. The markers are located on the underside of the pretreatment plate and can be milled or easily drawn with a permanent marker or equivalent. The pretreatment weight measures 10.2 cm × 10.2 cm and is made of a flat, smooth, rigid material (e.g., stainless steel) with an optional handle. The pre-treatment weight (including the optional handle) has a total mass of 726 g ± 0.5 g and a pressure of 0.10 psi (7.0 g / cm²) across the bottom surface area of the weight. 2 ) brings about pressure.
[0178] When measuring interfacial fluid volume, a rubber pad is used to provide a reproducibly flat surface that allows for a uniform pressure distribution. The IFF rubber pad is constructed from high-strength neoprene rubber (available from WVGrainger, Inc., part number 1DUV4, or equivalent) with a 40A durometer and 1 / 8 inch thickness, and cut to dimensions of 6 inches (15.2 cm) x 6 inches (15.2 cm).
[0179] For the entire re-wetting portion of the test, apply 0.5 psi (35.1 g / cm³) to the test area. 2 A padded weight assembly is required to apply the following. The procedure for determining the test area will be described later in this specification. The re-wet weight is constructed as follows: A piece of polyethylene film (approximately 25 micrometers thick, from any convenient source) is placed horizontally and flat on the surface of a rigid bench. A piece of polyurethane foam (25 mm thick, density 1.0 lb / ft) is placed. 3 Cut a piece of plexiglass (IDL 24 psi, available from Concord-Renn Co., Cincinnati, OH, or equivalent) to 10.2 cm × 10.2 cm and place it in the center of the film. Next, stack a piece of plexiglass (10.2 cm × 10.2 cm, and approximately 6.4 mm thick) on top of the polyurethane foam. Then, wrap the polyurethane foam and plexiglass plate with polyethylene film and secure it with clear tape. The total mass of the padded weight assembly should be 0.5 psi (35.1 g / cm³) in the test area. 2 Stack and secure metal weights with handles on top of the plexiglass plate so that the pressure can be adjusted to apply.
[0180] Various filter paper layers are required for the IFF, SFF, and overall re-wetting processes. Before testing, the filter paper is conditioned at 23°C ± 2°C and 50% ± 2% relative humidity for at least 2 hours. A suitable filter paper has a basis weight of approximately 88 gsm, a thickness of approximately 249 micrometers, and an absorption rate of approximately 5 seconds, and is available from Ahlstrom-Munksjo (Mt. Holly Springs, PA) as Grade 632 or equivalent. The filter paper has dimensions of 5 inches × 5 inches (12.7 cm × 12.7 cm).
[0181] Prior to testing, test samples are conditioned at 23°C ± 2°C and 50% ± 2% relative humidity for at least 2 hours. Remove the test samples from their packaging and, if necessary, open the packaging and spread out the product, taking care not to press or pull the product during handling. No attempt has been made to smooth out wrinkles. If applicable, tear the release paper between the wings and place the sample horizontally on a flat, rigid surface with the body side facing upward (e.g., the panty side facing downward). Determine the administration site as follows: For symmetrical products (i.e., the front side of the product is the same shape and size as the rear side of the product when divided laterally along the midpoint of the longitudinal axis of the product), the administration site is the intersection of the midpoint of the longitudinal axis and the midpoint of the transverse axis of the absorbent core. For symmetrical products (i.e., the front side of the sample is the same shape and size as the rear side of the product when divided laterally along the midpoint of the longitudinal axis of the product), the administration site is the midpoint of the product wing at the midpoint of the transverse axis of the absorbent core. For products with a foam core having punched or printed holes and slits, the dosage site is the longitudinal midpoint of the area where the holes are punched (or printed) at the lateral midpoint of the absorbent core. Once determined, mark the dosage site with a small dot using a black, thin-tipped permanent marker. If wings are present, fold them to the back of the product.
[0182] The test area of the test sample is determined as follows. This area is used to appropriately adjust the mass of the permeation plate and the mass of the re-wetting weight so that the required pressure (0.1 psi and 0.5 psi, respectively) can be delivered. The width of the absorbent core of the test sample is measured as the distance between one side edge of the core and the other side edge of the core, along a line placed at the administration site and extending perpendicular to the longitudinal axis of the test sample, and recorded as the core width in units of 0.01 cm. Here, the core width is multiplied by 10.2 cm (length of the permeation plate and re-wetting weight) and 0.1 cm 2 The unit is recorded as the test area. The total mass of the permeability plate is 7 g / cm² of the test area. 2 This is calculated by multiplying by . The total mass of the re-wetting weight is 35.1 g / cm² of the test area. 2It is the result of multiplying by .
[0183] Pre-treat the test sample with nAMF as follows: Place the pre-treatment plate horizontally on a flat, rigid surface with the side containing the circular markers facing downwards. Using a single-channel fixed-volume pipette, dispense 50 μL of nAMF precisely onto the upper side of the pre-treatment plate at the positions of each of the five circular markers. Place the test sample on the pre-treatment plate so that the body side of the sample faces the plate, the longitudinal axes of the sample and the plate are aligned, and the pre-marked dose positions on the test sample are centered on the central droplet of nAMF on the pre-treatment plate. After proper positioning, place the test sample in contact with the pre-treatment plate, then immediately apply the pre-treatment weight to the back of the test sample, centering it on the dose position / central droplet of nAMF on the pre-treatment plate. Start a 40-second timer. After 40 seconds, remove the pre-treatment weight from the test sample and remove the test sample from the pre-treatment plate. The test sample is flipped over so that the body side faces upwards, then placed horizontally on a flat, rigid surface, and the process proceeds quickly to the next step.
[0184] The first capture time (ACQ-1) is measured as follows: Connect the electronic circuit interval timer to the permeable plate 9001 and set the timer to zero. Position the permeable plate 9001 above the main body of the test sample so that the long axis of the longitudinal fluid channel 9007 on the underside of the permeable plate 9001 aligns with the longitudinal axis of the test sample, and ensure that the fluid reservoir 9003 is centered at the pre-marked dosing site on the test sample. Note that the nAMF should be visible through the fluid reservoir 9003 at the dosing site on the test sample. After proper positioning, gently place the permeable plate 9001 over the test sample. Using an adjustable volume pipette, accurately dispense 2.0 mL of nAMF into the fluid well 9008 of the permeable plate 9001. The fluid should be dispensed without splashing along the inclined wall of the fluid well 9008 within a period of 3 seconds or less. Immediately after capturing the fluid, record the first capture time (ACQ-1) displayed on the circuit interval timer in 0.1-second increments. Leave the permeable plate 9001 in place on the test sample and immediately start the 2-minute timer.
[0185] After 2 minutes have elapsed, the first interfacial free fluid (IFF-1) is measured as follows: Place the IFF rubber pad horizontally on a flat, rigid surface. Measure the mass of one layer of filter paper to the nearest 0.0001 g and measure the IFF-1. initial Record as follows: Place the filter paper in the center of the IFF rubber pad. Transfer the permeability plate 9001 to the pre-weighed filter paper from the test sample, ensuring the plate is in the center of the filter paper, and immediately start the 8-minute timer. After 10 seconds have elapsed on the 8-minute timer, remove the permeability plate from the filter paper and gently return it to the test sample in the exact same position as before. Within the next 10 seconds, measure the mass of the filter paper to the nearest 0.0001g and record as IFF-1 final Record it as such.
[0186] The second capture time (ACQ-2) is measured as follows: After 8 minutes have elapsed, a second ejection of the fluid is applied using an adjustable volume pipette to precisely dispense 4.0 mL of nAMF into the fluid well 9008 in the permeation plate 9001, as described above. Immediately after the fluid is captured, the second capture time (ACQ-2) displayed on the circuit interval timer is recorded in 0.1-second increments. The permeation plate 9001 is left in place on the test sample, and the 2-minute timer is immediately started.
[0187] After 2 minutes, measure the second interfacial free fluid (IFF-2) as follows: Place the IFF rubber pad horizontally on a flat, rigid surface. Measure the mass of a new single layer of filter paper to the nearest 0.0001 g and measure the IFF-2. initial Record as follows: Place the filter paper in the center of the IFF rubber pad. Transfer the permeability plate 9001 to the pre-weighed filter paper from the test sample, ensuring the plate is in the center of the filter paper, and immediately start the 8-minute timer. After 10 seconds have elapsed on the 8-minute timer, remove the permeability plate 9001 from the filter paper and gently return it to the test sample in the exact same position as before. Within the next 10 seconds, measure the mass of the filter paper to the nearest 0.0001g and record as IFF-2 final Record it as such.
[0188] The third capture time (ACQ-3) is measured as follows: After 8 minutes have elapsed, as described above, a third ejection of fluid is applied using an adjustable volume pipette to precisely dispense 2.0 mL of nAMF into the fluid well 9008 in the permeation plate 9001. Immediately after the fluid is captured, the third capture time (ACQ-3) displayed on the circuit interval timer is recorded in 0.1-second increments. The permeation plate 9001 is left in place on the test sample, and the 2-minute timer is immediately started.
[0189] After 2 minutes have elapsed, measure the third interfacial free fluid (IFF-3) as follows: Place the IFF rubber pad horizontally on a flat, rigid surface. Measure the mass of a new single layer of filter paper to the nearest 0.0001 g and measure the IFF-3. initialRecord as follows: Place the filter paper in the center of the IFF rubber pad. Transfer the permeability plate 9001 to the pre-weighed filter paper from the test sample, ensuring the plate is in the center of the filter paper, and immediately start the 8-minute timer. After 10 seconds have elapsed on the 8-minute timer, remove the permeability plate 9001 from the filter paper and place it to the side, ensuring the pad side of the plate does not touch the bench. Within the next 10 seconds, measure the mass of the filter paper to the nearest 0.0001g and record as IFF-3. final Record it as such.
[0190] The surface free fluid (SFF) is measured as follows: After 8 minutes, the mass of a new stack of five filter papers is measured to the nearest 0.0001 g, and the SFF is measured. initial Record as follows: Place the stack of filter paper on the body side of the test sample, centered at the top of the administration site. Gently place the permeation plate 9001 on top of the filter paper, with the pad side of the plate centered on the filter paper, and immediately start a 10-second timer. After 10 seconds, remove the permeation plate 9001 from the filter paper and set it aside. Measure the mass of the stack of five filter papers to the nearest 0.0001g and record as SFF. final Record this as such. Proceed immediately to the next step.
[0191] The overall rewetting is measured as follows: The mass of a new stack of 5 filter papers is measured to the nearest 0.0001g, and REWET initial Record as follows: Place the filter paper on the body side of the test sample, so that it is centered at the top of the administration site. Next, place the padded rewetting weight on top of the filter paper stack so that the weight is centered on the filter paper stack, and immediately start the 30-second timer. After 30 seconds, remove the rewetting weight, measure the mass of the five filter paper stacks to the nearest 0.0001g, and then REWET final Record this as follows. Discard the sample, thoroughly clean it, and dry the bottom surfaces of the fluid well 9008, fluid reservoir 9003, longitudinal fluid channel 9007, and permeation plate 9001 before testing the next sample.
[0192] The following calculations are performed for each of the measured parameters as follows: The total ejection and absorption time is calculated as the sum of ACQ-1, ACQ-2, and ACQ-3, and recorded in units of 0.1 seconds. IFF-1 final From IFF-1 initial IFF-1 is calculated by subtracting [a certain value] and recorded in units of 0.0001g. IFF-2 final From IFF-2 initial IFF-2 is calculated by subtracting [a certain value] and recorded in units of 0.0001g. IFF-3 final From IFF-3 initial Subtracting from IFF-3 calculates IFF-3 and records it in units of 0.0001g. Calculate the total IFF as the sum of IFF-1, IFF-2, and IFF-3 and record it in units of 0.1g. SFF final From SFF initial Subtracting the specified value (SFF) calculates the SFF and records it in units of 0.0001g. Calculate the total IFF + SFF as the sum of the total IFF and SFF, and record it in units of 0.1g. REWET final REWET initial The total re-wetting is calculated by subtracting the value of the value and recorded in units of 0.0001g.
[0193] The entire procedure is repeated for a total of three replicated test samples. For each parameter, the reported value is the arithmetic mean of three individually recorded measurements for each capture time (ACQ-1, ACQ-2, and ACQ-3) in 0.1-second units, total ejection and absorption time in 0.1-second units, interfacial free fluid (IFF-1, IFF-2, and IFF-3) in 0.0001 g units, total IFF in 0.1 g units, surface free fluid (SFF) in 0.0001 g units, total IFF + SFF in 0.1 g units, and overall re-wetting in 0.0001 g units.
[0194] Preparation of new artificial menstrual fluids (nAMF) This formulation of artificial menstrual fluid (nAMF) consists of a mixture of defibrous sheep blood, phosphate-buffered saline, and mucus components. The nAMF is prepared to have a viscosity of 7.40–9.00 centipoise at 23°C.
[0195] The viscosity of nAMF is measured using a low-viscosity rotational viscometer (a suitable instrument is the Brookfield DV2T with a Brookfield UL adapter, available from AMETEK Brookfield, Middleboro, MA, or an equivalent). A spindle of the appropriate size for the viscosity range is selected, and the instrument is operated and calibrated according to the manufacturer's instructions. Measurements are performed at 23°C ± 1°C and 60 rpm. Results are reported in 0.01 centipoise units.
[0196] Reagents required for nAMF preparation include defibrated sheep blood with a filling cell volume of 38% or more (collected under sterile conditions, available from Cleveland Scientific, Inc., Bath, OH, or an equivalent source), gastric viscous (crude form, sterile, available from American Laboratories, Inc., Omaha, NE, or an equivalent source) with a target viscosity of 3-4 centistokes when prepared as a 2% aqueous solution, dibasic anhydrous sodium phosphate (reagent grade), sodium chloride (reagent grade), monobasic monohydrate sodium phosphate (reagent grade), sodium benzoate (reagent grade), benzyl alcohol (reagent grade), and distilled water (each available from VWR International or an equivalent source).
[0197] Phosphate-buffered saline consists of two individually prepared solutions (Solution A and Solution B). To prepare 1 L of Solution A, add 1.38 ± 0.005 g of monobasic sodium phosphate monohydrate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the container volume. Mix thoroughly. To prepare 1 L of Solution B, add 1.42 ± 0.005 g of dibasic anhydrous sodium phosphate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the container volume. Mix thoroughly. To prepare approximately 200 mL of phosphate-buffered saline solution, add 49.50 g ± 0.10 g of Solution A and 157.50 g ± 0.10 g of Solution B to a sufficiently sized bottle with a tightly sealing lid. Next, add 1.0 g of sodium benzoate and 1.60 g of benzyl alcohol to the bottle along with the stirring rod, and set it aside.
[0198] The mucus component of nAMF is a mixture of phosphate-buffered saline and gastric viscous. The amount of gastric viscous added to the mucus component directly affects the final viscosity of the prepared nAMF. To determine the amount of gastric viscous required to obtain nAMF within the target viscosity range (7.4–9.0 centipoise at 23°C and 60 rpm), three batches of nAMF with varying amounts of gastric viscous in the mucus component are prepared, and then a linear fit is performed using the least-squares method through the three points to interpolate the exact required amount from the concentration-viscosity curve. The appropriate range for gastric viscous is usually 13–15 grams per 400 mL batch of nAMF, but this can vary considerably depending on the mucin supplier, age, and lot.
[0199] To prepare approximately 200 mL of mucus, a predetermined amount of gastric viscous is added to a bottle containing a pre-prepared phosphate-buffered solution, and then the bottle is capped. The bottle is placed on a wrist-action shaker at maximum speed for 5 minutes. After 5 minutes, the flask containing the mucus is removed from the wrist-action shaker and placed on a magnetic stirring plate. The mixture is stirred for at least 2 hours until no mucin clumps remain, and then the stirring rod is removed from the flask. The mucus is mixed using a homogenizer at 10,000 rpm for 5 minutes. A suitable homogenizer is the T18 Ultra-Turrax with the S18N-19G dispersion tool (19 mm stator diameter, 12.7 mm rotor diameter, 0.4 mm gap between rotor and stator), both of which are available from IKA Works, Inc., Wilmington, NC or equivalent sources. After the final mixing step, the viscosity of the viscous component is measured and recorded in 0.01 centipoise units using a viscometer equipped with a UL adapter at 23°C ± 1°C and 20 rpm. It is then confirmed that the viscosity of the prepared viscous component is within the target range of 9.0–11.0 centipoise.
[0200] nAMF is a 50:50 mixture of mucus and sheep blood. Ensure the temperature of the sheep blood and mucus is 23°C ± 1°C. To prepare approximately 400 mL of nAMF, add 200 g of mucus to a glass bottle with a capacity of at least 500 mL. Next, add 200 g of sheep blood to the bottle along with a stirring rod. Mix on a magnetic stirring plate until completely combined. Ensure that the viscosity of the prepared nAMF is within the target range of 7.4–9.0 centipoise when measured at 23°C ± 1°C and 60 rpm using a viscometer equipped with a UL adapter. If the viscosity is too high, the viscosity can be adjusted by adding 0.5 g of the previously prepared phosphate-buffered saline solution at a time, followed by stirring for 2 minutes, and then rechecking the viscosity until it reaches the target range.
[0201] Certified nAMF must be refrigerated at 4°C unless intended for immediate use. After preparation, nAMF can be stored in an airtight container at 4°C for up to 48 hours. Before testing, nAMF must be kept at 23°C ± 1°C. Any unused portion should be discarded after testing is complete.
[0202] Bag compression recovery method In the product development of bulky, cellulose-rich absorbent materials, it is crucial to understand the caliper recovery of the material after it has been compressed and held in a package for an extended period. The in-bag compression recovery method measures the caliper recovery of the laminate of an absorbent material after it has been removed from a sealed full-bag package subjected to prolonged compressive force. Caliper recovery is calculated by comparing the initial laminate height inside the package with the laminate height measured at a specific point in time after the absorbent material has been removed from the package. All tests are conducted in a controlled room at 23°C ± 3°C and 50% ± 2% relative humidity.
[0203] Package dimensions and stack height are measured using a Universal Package Tester (UPT) equipped with an electric test stand including a control box with a touchscreen. A suitable instrument is available from Alluris GmbH & Co. (Freiburg, Germany) as model FMT-310 or equivalent. The UPT's stationary base plate has a surface area greater than the surface area of the test specimen's stack. A compression plate with a diameter of 150 mm is mounted on a load cell (5N) attached to the movable crossbeam of the test stand. The compression plate is zeroed out, and the reference (i.e., "home") position is set according to the manufacturer's instructions so that the precise distance between the contact surface of the base plate and the contact surface of the compression plate can be measured. Ensure that the compression plate is fixed so that its contact surface is parallel to the base plate and oriented perpendicular to the movement of the crossbeam of the test stand. The system is calibrated according to the manufacturer's instructions before testing.
[0204] The test specimens are prepared as follows: A full bag test package of absorbent article pads having a manufacturing date at least one week prior to the test date is obtained. Referring to Figures 12A to 13 as guidance, the orientation of the compression laminate axis 510 of the full bag test package 500 is determined, where the compression laminate axis is defined as a dashed line, which starts from the flat surface of the first folded absorbent article pad in the laminate, passes through the regular stack of folded pads, and ends on the flat surface of the last folded absorbent article pad in the laminate contained within the package. The compression laminate axis is perpendicular to the flat surface of the folded absorbent article pads and represents the direction in which the filled bag width (FBW) 508 of the package will be measured, as described herein. Using a permanent ink pen, the orientation of the compression laminate axis is marked on the outside of the package. Similarly, a total of three duplicate full bag test packages are prepared. Before testing, the full bag test packages are conditioned for at least two hours in a laboratory maintained at 23°C ± 3°C and 50% ± 2% relative humidity.
[0205] Using the UPT, measure the package dimensions and stack height of a full bag test package as follows: Place the test package on the UPT base plate so that the predetermined direction of the compression stack axis is parallel to the movement of the crossbeam of the test stand and perpendicular to the contact surface of the base plate. Position the test package so that a single stack of folded pads within the package is centered under the compression plate. Set the starting position on the UPT so that the distance between the compression plate and the base plate is approximately 1 cm greater than the approximate filled bag width (FBW) of the package. Program the UPT as follows: Lower the compression plate from the home position to the preset starting position at a speed of 180 mm / min. Then, lower the compression plate further at a speed of 12 mm / min until it contacts the test package, then continue lowering until a force of 1 N (+0.05 N) is reached, pause briefly, and then immediately return to the preset starting position. The height of the compression plate when the force of 1 N is reached is the filled bag width (FBW) and is recorded as the stack height within the bag in 0.1 mm units. Here, the test package is positioned on the UPT baseplate so that the package height can be measured. To measure the package height, the package is positioned such that the predetermined direction of the compression stack axis is perpendicular to the movement of the crossbeam of the test stand and parallel to the contact surface of the baseplate. The test package is placed in the center under the compression plate. The starting position is set on the UPT such that the distance between the compression plate and the baseplate is approximately 1 cm greater than the height of the nearly filled bag of the package. The filled bag height is measured using the UPT in the same manner as described for FBW measurement, here by moving the compression plate from the preset starting position toward the full bag package at a speed of 12 mm / min until a force of 1 N is applied to the package, and then immediately returning the plate to the preset starting position. The height of the compression plate when the force of 1 N is reached is recorded as the filled bag height (FBH) in 0.1 mm increments. Here, the test package is positioned on the UPT baseplate so that the depth of the package can be measured.To measure the package depth, position the package so that the side of the package marked with the direction of the compression stack axis faces the base plate of the UPT. Place the test package in the center under the compression plate. Set the starting position on the UPT so that the distance between the compression plate and the base plate is approximately 1 cm greater than the approximate filled bag depth of the package. Measure the filled bag depth using the UPT in the same manner as described for FBW measurement, here by moving the compression plate from the preset starting position toward the full bag package at a speed of 12 mm / min until a force of 1 N is applied to the package, and then immediately returning the plate to the preset starting position. Record the height of the compression plate when the force of 1 N is reached as the filled bag depth (FBD) in 0.1 mm increments. Now measure the mass of the full bag test package and record it as the filled bag mass (FBM) in 0.01 g increments.
[0206] The stack height measurement of the pad stacks is performed as follows after they have been removed from the test package: Carefully open the full bag test package, taking care not to apply pressure to the package or the folded pads inside it. Now, remove the pads from the package and stack them to mimic the stacked state inside the package, and start a 2-minute timer. Set the empty package aside temporarily. Without excessive delay, count the number of folded pads that make up the single stack that the FBW has just measured, and record this value as the number of pads per stack in the bag. Also, count the number of individual stacks of pads present in the full bag package, and record this value as stacks per bag (SPB). Without opening or unfolding the pads, transfer the pad stacks to the UPT base plate. Ensure that the stacks are properly aligned with the individual pads overlapping each other, and that the number of pads in the stacks is equal to the number of pads per stack in the bag. Orient the laminate in the same manner as described for FBW measurement, so that the compressed laminate axis is parallel to the movement of the crossbeam of the test stand and perpendicular to the contact surface of the compression plate. Position the laminate so that it is centered under the compression plate but does not touch the compression plate, and set the starting position on the UPT so that the distance between the compression plate and the base plate is approximately 1 cm greater than the approximate height of the pad laminate. Allow the laminate to relax without disturbing it for the remainder of the 2-minute relaxation time. After 2 minutes, measure the laminate height using the UPT in the same manner as described for FBW measurement, and move the compression plate from the preset starting position toward the full bag package at a speed of 12 mm / min until a force of 1 N is applied to the package, and then immediately return the plate to the preset starting position. Record the height of the compression plate when the force of 1 N is reached as the recovered laminate height in 0.1 mm increments. Allow the pad laminate to rest undisturbed on the UPT base plate for a 4-hour relaxation time. During this time, the mass of the empty package is measured and recorded as the empty bag mass (EBM) in units of 0.01g.After 4 hours, the laminate height is measured using UPT as described above. The height of the compressed plate that has reached a force of 1N is recorded in 0.1mm increments as the recovered laminate height after 4 hours. At this point, one of the pads is removed from the laminate, unfolded, and the number of folds is recorded in units of folds per pad (Folds Per Pad, FPP). For example, a tri-fold pad has an FPP equal to 3.
[0207] The following calculations are performed inside the bag to determine the pad density and pad caliper. The volume of the full bag test package is calculated as FBW × FBH × FBD, and the full bag volume (FBV) is 0.1 mm³. 3 Record in units. Here, the volume of each individual layer of pads inside the test package is calculated by dividing the full bag volume (FBV) by the stack per bag (SPB), and the stack volume inside the bag is 0.1 mm. 3 Record in units. Calculate the mass of the stack inside the bag by subtracting the mass of the empty bag (EBM) from the mass of the filled bag (FBM), then divide by the stack per bag (SPB), and record in units of 0.01g. Here, divide the mass of the stack inside the bag by the number of pads per stack, then divide by the volume of the stack inside the bag divided by the number of pads per stack, then multiply by 1000 to get the average pad density inside the bag of 0.01g / cm³. 3 Record in units of 0.1 mm. The folded pad caliper within the bag is calculated by dividing the stack height (FBW) value by the number of pads per stack within the bag, and recorded in units of 0.1 mm. Here, the folded pad caliper value within the bag is divided by the fold per pad (FPP), and the average pad caliper within the bag is recorded in units of 0.1 mm.
[0208] Perform the following out-of-bag calculations to determine the pad caliper and density after a specified relaxation time. Calculate the folded pad caliper outside the bag at 2 minutes by dividing the value of the recovered stack height at 2 minutes by the value of the number of pads per stack in the bag, and record it in units of 0.1 mm. Here, divide the folded pad caliper value outside the bag at 2 minutes by the number of folds per pad (FPP), and record the average out-of-bag pad caliper at 2 minutes in units of 0.1 mm. Calculate the out-of-bag stack volume at 2 minutes by multiplying the recovered stack height at 2 minutes, the filled bag height (FBH), and the filled bag depth (FBD) together, then dividing by the number of stacks per bag (SPB), and record it in 0.1 mm 3 units. Here, calculate the pad density at 2 minutes by dividing the in-bag stack mass by the out-of-bag stack volume at 2 minutes, then multiply by 1000, and record the average out-of-bag pad density at 2 minutes in units of 0.01 g / cm 3 units. Similarly, calculate the average out-of-bag pad caliper at 4 hours and the average out-of-bag pad density at 4 hours, and record them in units of 0.1 mm and 0.01 g / cm respectively 3 units.
[0209] Calculate the caliper recovery percent after 2 minutes and after 4 hours as follows, and record each value in units of 1 percent.
[0210] [Equation]
[0211] Similarly, repeat the entire procedure until a total of 3 replicate full bag test packages are measured. Calculate the arithmetic mean of all 3 replicates, and record the in-bag stack height in units of 0.1 mm, the average in-bag pad caliper in units of 0.1 mm, and the average in-bag pad density in units of 0.01 g / cm 3 units, the average out-of-bag pad caliper at 2 minutes in units of 0.1 mm, and the average out-of-bag pad density at 2 minutes in units of 0.01 g / cm 3in units, the average out-of-bag pad caliper at 4 hours in 0.1 mm units, and the average out-of-bag pad density in 0.01 g / cm 3 in units, the caliper recovery % at 2 minutes in 1 percent units, and the caliper recovery % at 4 hours in 1 percent units are reported.
[0212] Examples / Data The following data and examples, including comparative examples, are provided to assist in the description of the upper nonwoven layer and lower nonwoven layer, and / or the absorbent articles described herein. The illustrated structures are provided for illustrative purposes only, and many modifications thereof are possible without departing from the spirit and scope of the present disclosure, and therefore should not be construed as limiting the present invention.
[0213] Testing of Nonwoven Layer Materials A series of measurements are performed on nonwoven materials to evaluate the ability of the materials to function as the upper nonwoven layer and / or lower nonwoven layer in the absorbent core structures described herein. Samples A to G are examples according to the present disclosure. Comparative Sample H is a comparative example. Samples A to G and Comparative Sample H are set forth in Table 1 below.
[0214] Samples A to G and Comparative Sample H were evaluated according to the CD cyclic stretch method up to 3% strain, the break strain method, the wet and dry CD ultra-sensitive 3-point bending method, and the nonwoven thickness-pressure method. The results are shown in Table 2.
[0215] [Table 1] 1 Available as ATB Z87G-40 from Xiamen Yanjan New Material Co. (China) 2 Available as Sawasoft® 53FC041001 from Sandler GmbH (Germany) 3 Available as Sawasoft® 553FC041005 (Option 82) from Sandler GmbH (Germany) 4 Available as Aura20 from Xiamen Yanjan New Material Co. (China). 5 Available from Jacob Holms Industries (Germany) as S25000541R01. 6 Available from PFN nonwovens Czech SRO (Czech Republic) as PFNZN 18G BICO8020 PHI 6. 7 PFN nonwovens are available from Czech SRO (Czech Republic) as PEGZN25 BICO7030 Phobic. 8 Available from DunnPaper (USA) as product number 3028.
[0216] [Table 2]
[0217] Suitable nonwoven materials for the upper and / or lower nonwoven layers are considered to be able to deform (stretch) with balanced stretching and almost recover to their original state, thus helping to allow the absorbent core structure and / or absorbent article to recover from deformation during body movement. Particularly suitable nonwoven materials for the upper nonwoven layer can provide fluid handling performance, which can help to effectively move fluid deep into the inner core layer to provide a dry-feeling, body-hugging, comfortable fit. To achieve this, suitable nonwoven materials for the upper nonwoven layer exhibit a relatively low density (e.g., 0.03-0.07 g / cm³ under a pressure of 7 g / cm²) to allow fluid to be efficiently discharged from the upper nonwoven layer to the inner core layer below. In addition, suitable nonwoven fabric materials for the upper nonwoven layer can maintain a relatively bulky thickness even under high compressive forces from the body (i.e., a pressure of 70 g / cm²), and as a result, fluid present in the inner core layer is discharged from the absorbent core structure and returned, preventing the body from feeling wet.
[0218] Samples A-C and E were found to be suitable materials for the upper and / or lower nonwoven fabric layers. In particular, samples A-C and E demonstrated that they had a permanent strain of 0.013 mm / mm or less, that the material could stretch and recover, and that they had a fracture strain of more than 10% before tearing. Samples A-C and E also showed a permanent strain of 0.03 N * With a drying recovery energy exceeding 1 mm, less energy was required to bend while recovering from bending (1.6 N). * (Evided by dry bending energy of less than mm). Samples A-C and E are 7 g / cm². 2 Under this pressure, 0.03~0.07 g / cm³ 3 It has a relatively low density, and is 7 g / cm³ in size of 0.80-1.21 mm. 2 The thickness at pressure is shown, demonstrating that these materials have a more open fibrous network structure, which can contribute to bulkier and more efficient fluid handling performance.
[0219] Sample D was found to have a permanent strain of 0.016 mm / mm, demonstrating that the material is likely to stretch significantly during manufacturing and / or use without returning to its initial state. At the same time, sample D was found to be highly compressible under body pressure, as demonstrated by its thickness of 0.19 mm at 70 g / cm², indicating that the material is likely to become denser under body compression and that the inner core layer is unlikely to adequately expel the fluid. Samples F and G were found to have a permanent strain of 0.03 N * It was demonstrated that the material exhibits a dry recovery energy of less than mm, potentially failing to recover from deformation, and therefore being insufficient to function as an upper nonwoven layer. However, when combined with the upper nonwoven layers described herein, samples D, F, and G may be suitable materials for the lower nonwoven layer.
[0220] Comparative sample H exhibited a fracture strain of less than 5% and a thickness of less than 0.2 mm at 70 g / cm². Furthermore, comparative sample H was found to tear when wet. Therefore, comparative sample H is insufficient to function as either an upper or lower nonwoven fabric layer.
[0221] Table 3 is provided for the convenience of the reader. Table 3 includes a non-exhaustive list of properties and a non-exhaustive list of corresponding values for each of the properties that a particularly preferred upper nonwoven layer of this disclosure may exhibit.
[0222] [Table 3]
[0223] Compression test inside the bag Absorbent products are tested to evaluate the effect of compression within the bag on the caliper and density of the absorbent articles. The following examples provide a comparison between commercially available feminine hygiene products and feminine hygiene products according to this disclosure.
[0224] Examples 1-5: Prepare a disposable absorbent article in the form of a women's hygiene pad (280 mm in length) as described herein, having the following components: Top sheet - The top sheet is a 24 gsm carded nonwoven fabric comprising 100% 4 denier BiCo (PE / PET), available from Xiamen Yanjan New Material Co.. Upper nonwoven layer - The upper nonwoven layer is a 40 gsm carded elastic nonwoven fabric comprising BiCo (PE / PET) in a 60% 2DTex / 40% 4DTex blend, available as ATB Z87G-40 from Xiamen Yanjan New Material Co. (China). Inner core layer - The inner core layer is a homogeneous mixture of 180 gsm cellulose pulp (100% SuperSoft® untreated fluff pulp, available from International Paper Company (Memphis, TN)) and 70 gsm superabsorbent particles (available as Aqualic CA L-805 from Nippon Shokubai (Japan)). Lower nonwoven layer - The lower nonwoven layer is an 18 gsm spunbond nonwoven fabric comprising 100% 2.0 DTex polypropylene, available as PFNZN 18G 100% PP PHI 6 from PFN nonwovens Czech S.R.O (Czech Republic). Back sheet - The back sheet is a 12 gsm polyolefin resin-based blown film (3 layers) of metallocene-LLDPE, LDPE and HDPE composition, available as Theo 12gsm film from RKW Group (Germany).
[0225] First, the top sheet is coated with 5gsm adhesive (D3151 NG, available from HB Fuller). Next, the upper nonwoven fabric layer is deposited on top of the top sheet. In parallel, the inner core layer is manufactured by the air-lay method. A flow of cellulose fibers and AGM is carried on a high-speed moving airflow and deposited into a three-dimensional molding pocket on a rotational molding drum with a downward vacuum suction to draw the cellulose and AGM into the pocket of the laydown station. The homogeneously mixed mass of cellulose and AGM is held on the forming drum under vacuum until it is deposited directly onto the upper nonwoven fabric layer pre-coated with 5gsm adhesive (D3151 NG, HB Fuller), and then sealed with a second remaining nonwoven fabric pre-coated with 5gsm adhesive (D3151 NG, HB Fuller) to create an absorbent core. The widths of the upper and lower nonwoven webs are wider than the maximum width of the molded cellulose and AGM inner core layers, thereby enabling an effective periphery seal where the two nonwovens connect, at least on the leftmost and rightmost parts of the absorbent core structure. The flex-bonding channel region is applied to the pattern shown in Figure 11B using a heated embossing unit on the production line. The backsheet is then bonded to the surface facing the outside of the lower nonwoven layer with a 5gsm adhesive (D3151 NG, HB Fuller).
[0226] Apply panty-fastening adhesive to the surface of the pad that faces the clothing, then cover it with silicone-treated kraft paper. Fold the pad into thirds, then wrap it in a non-silicone-treated 14gsm polyolefin film pouch and seal it. Place the stack of 10 folded pads into a polybag package. The package is compressed to various levels of compression within the bag and then sealed.
[0227] The packages were evaluated according to the in-bag compression recovery method, and the results are shown in Tables 4a and 4b.
[0228] [Table 4]
[0229] [Table 5]
[0230] Surprisingly, the feminine hygiene pads described herein were found to be compressible and retained within the package without adversely affecting the caliper or density. Two minutes after removal from the package, the feminine hygiene pads of Examples 2-5 exhibited a caliper recovery percentage of 4%-23%. Four hours after removal from the package, the feminine hygiene pads of Examples 3-5 continued to recover the caliper, exhibiting a caliper recovery percentage of 15%-26%. The feminine hygiene pads of Examples 2-5 had a density of 0.16 g / cm³ both inside and outside the bag. 3 It exhibited a density of less than . Thus, Examples 2-5 demonstrate that the absorbent articles described herein can be compressed and retained in smaller packages requiring less packaging material, reduced shipping volume, and lower transport and storage costs, while nearly recovering to their pre-packaging caliper and density.
[0231] Example 6 is a commercially available Always® ultra-thin feminine hygiene product (size 1 normal, bag count 13, lot number D DE 3 291 0314 20 08:33 P:181023) sold by The Procter & Gamble Company in Western Europe.
[0232] Example 7 is a commercially available Bodyform® feminine hygiene product (size 1, bag count 12, lot number 160923 GH 16 20:42) sold by Essity in Western Europe.
[0233] Example 8 is a commercially available Always® Maxi feminine hygiene product (size 2 long, bag count 12, lot number HU 3048208001 11 18:45 PROD:17 / 02 / 23 7657) sold by The Procter & Gamble Company in Western Europe.
[0234] Example 9 is a commercially available Sofy® antibacterial slim feminine hygiene product (size XL 290mm, bag count 14, lot number SEP22 01 / 09 / 22 B21F3U) sold by Unicharm in India.
[0235] Example 10 is a commercially available Sofy® Naked Feel feminine hygiene product (pad length 25cm, bag count 13, lot number 20200120D2082) sold by Unicharm in China.
[0236] Example 11 is a commercially available Always® ultra-thin feminine hygiene product (size 3 extra-long, oversized, bag count 32 (2 x 16), lot number 230047860063 3010032) sold by The Procter & Gamble Company in North America.
[0237] Examples 6-11 were evaluated according to the in-bag compression recovery method, and the results are shown in Tables 5a and 5b.
[0238] [Table 6]
[0239] [Table 7]
[0240] Examples 6-11, which are commercially available women's hygiene products, did not recover their caliper and / or density 4 hours after being removed from the package.
[0241] The absorbent products will be tested to evaluate the effect of compression within the bag on the pads' ability to compress and return to their original state, and on their fluid handling performance.
[0242] Examples 12-13: Prepare a disposable absorbent article in the form of a women's hygiene pad (280 mm in length) as described herein, having the following components: Topsheet - Topsheet is a 22.4gsm polyethylene molded film available as DS02-172 from Xiamen Yanjan New Material Co. (India). The upper nonwoven layer is a 40gsm carded elastic nonwoven fabric containing BiCo(PE / PET) in a 60% 2DTex / 40% 4DTex blend, available from Xiamen Yanjan New Material Co. (China) as ATB Z87G-40. The inner core layer is a homogeneous mixture of 150gsm cellulose pulp (100% SuperSoft® untreated fluff pulp, available from International Paper Company (Memphis, TN)) and 60gsm superabsorbent particles (available from Nippon Shokubai (Japan) as Aqualic CA L-805). The lower nonwoven layer is an 18gsm spunbond nonwoven fabric containing 100% 2.0DTex polypropylene, available from PFN nonwovens Czech SRO (Czech Republic) as PFNZN 18G 100% polypropylene PHI 6. Backsheet - The backsheet is a 12gsm polyolefin resin blow film (3 layers) of metallocene-LLDPE, LDPE, and HDPE composition, available from RKW Group, Germany as Theo 12gsm film.
[0243] Examples 12 and 13 were manufactured as described above for Examples 1 to 5. Examples 12 and 13 were evaluated according to the wet and dry CD and MD three-point bending method, and the wet and dry collapse compression method, the results of which are shown in Table 6, and according to the capture time and re-wetting method, the results of which are shown in Table 7.
[0244] [Table 8]
[0245] [Table 9]
[0246] It was found that prolonged compression (Example 12) did not adversely affect the bending and / or compression of the article and its ability to recover to its original shape. It was also found that even after being held in the package at a 26% compression level in the bag, Example 12 could efficiently manage the fluid at a level comparable to that of Example 11, which was not compressed.
[0247] Combinations / Examples Paragraph A. Women's hygiene products, Package including internal space and external surface, A plurality of disposable feminine hygiene pads disposed within the internal space of a package, each of which includes an absorbent core structure, the absorbent core structure comprising an upper nonwoven fabric layer, a lower nonwoven fabric layer, and an inner core layer containing cellulose fibers, and at least a portion of the inner core layer disposed between the upper nonwoven fabric layer and the lower nonwoven fabric layer, comprising a plurality of disposable feminine hygiene pads, Disposable feminine hygiene pads, when measured according to the in-bag compression recovery method, weigh approximately 0.20 g / cm³. 3 A women's hygiene product exhibiting the following average pad density within the bag and a caliper recovery percentage of at least 4%, preferably at least 10%, in 2 minutes.
[0248] Paragraph B. Disposable feminine hygiene pads, when measured according to the in-bag compression recovery method, are approximately 0.07 g / cm³. 3 ~Approx. 0.17g / cm 3 The feminine hygiene product described in paragraph A exhibits the average pad density inside the bag.
[0249] Paragraph C. The disposable feminine hygiene pad exhibits a caliper recovery percentage of approximately 4% to approximately 35% in 2 minutes, as measured according to the in-bag compression recovery method, as described in Paragraph A or B.
[0250] Paragraph D. A disposable feminine hygiene pad exhibits a caliper recovery percentage of approximately 4% to approximately 35% in 4 hours, as measured according to the in-bag compression recovery method, as described in any of paragraphs A to C.
[0251] Paragraph E. A feminine hygiene product according to any of paragraphs A to D, wherein the inner core layer contains cellulose fibers in an amount of approximately 50% to approximately 85% by weight of the inner core layer.
[0252] Paragraph F. A feminine hygiene product according to any of paragraphs A to E, wherein the inner core layer further comprises superabsorbent particles in an amount of approximately 15% to approximately 50% by weight of the inner core layer.
[0253] Paragraph G. A feminine hygiene product according to any of paragraphs A to F, wherein the upper nonwoven fabric layer has a basis weight of approximately 30 gsm to approximately 85 gsm.
[0254] Paragraph H. A feminine hygiene product according to any of paragraphs A to G, wherein the lower nonwoven fabric layer has a basis weight of approximately 7 gsm to approximately 40 gsm.
[0255] Paragraph I. When measured according to the in-bag compression recovery method, the femininity of a sanitary pad is approximately 0.06 g / cm³. 3 ~Approx. 0.16g / cm 3 A feminine hygiene product described in any of paragraphs A to H, exhibiting an average outer pad density of the bag at 2 minutes.
[0256] Paragraph J. A feminine hygiene product according to any of paragraphs A to I, wherein the packaging includes packaging material selected from the group consisting of polymer film, paper material, cardboard for cartons, and combinations thereof.
[0257] Paragraph K. When measured according to the wet and dry CD and MD 3-point bending method, the female hygiene pad was approximately 7.0 N. * mm2 ~ approx. 30N * mm 2 A women's hygiene product described in any of paragraphs A to J, exhibiting the dry bending rigidity of CD.
[0258] Paragraph L. A feminine hygiene product as described in any of paragraphs A to K, wherein the feminine hygiene pad exhibits an average internal pad caliper of approximately 2.0 mm to approximately 5.5 mm when measured according to the internal compression recovery method.
[0259] Paragraph M. A feminine hygiene product according to any one of paragraphs A to L, wherein at least one of the upper nonwoven fabric layer and the lower nonwoven fabric layer contains a polymer selected from the group consisting of recycled polymer resin, biodegradable polymer, biopolymer, and combinations thereof.
[0260] Paragraph N. A feminine hygiene product according to any of paragraphs A to M, wherein the polymer fibers of the upper nonwoven fabric layer consist of approximately 60 to 100% synthetic fibers and 0 to 40% regenerated cellulose fibers, including rayon.
[0261] Paragraph O. A feminine hygiene product according to any of paragraphs A to N, wherein each disposable feminine hygiene pad further comprises a top sheet and a back sheet, and an absorbent core structure is disposed between the top sheet and the back sheet.
[0262] Paragraph P. A process for packaging multiple disposable feminine hygiene pads, wherein this process is: To provide a plurality of disposable feminine hygiene pads, each of which comprises an absorbent core structure, the absorbent core structure comprising an upper nonwoven fabric layer containing polymer fibers and having a basis weight of approximately 30 gsm to approximately 85 gsm, a lower nonwoven fabric layer containing polymer fibers and having a basis weight of approximately 7 gsm to approximately 40 gsm, and an inner core layer containing cellulose fibers and superabsorbent particles, wherein at least a portion of the inner core layer is disposed between the upper nonwoven fabric layer and the lower nonwoven fabric layer. Folding each of the multiple disposable feminine hygiene pads to form multiple folded disposable feminine hygiene pads, By arranging multiple folded disposable feminine hygiene pads to form a laminate of folded disposable feminine hygiene pads, Compressing a laminate of folded disposable feminine hygiene pads along a compression axis to form a compressed laminate of folded disposable feminine hygiene pads, The process involves placing a compressed laminate of folded disposable feminine hygiene pads into the internal space of a package such that the compressed laminate of folded disposable feminine hygiene pads is oriented substantially along the width dimension of the package. The process includes closing the package such that the folded disposable feminine hygiene pads exhibit an average folded caliper of approximately 7.0 to 15.0 mm within the bag, and that when removed from the package, the disposable feminine hygiene pads exhibit a caliper recovery percentage of at least 4% within 2 minutes, as measured according to the in-bag compression recovery method.
[0263] Paragraph Q. The feminine hygiene product according to Paragraph P, wherein each disposable feminine hygiene pad further comprises a top sheet and a back sheet, and an absorbent core structure is disposed between the top sheet and the back sheet.
[0264] The dimensions and values disclosed herein should not be understood as being strictly limited to the exact numerical values listed. Instead, unless otherwise specified, each such dimension is intended to mean both the listed value and the functionally equivalent range encompassing that value. For example, a dimension disclosed as "40 mm" is intended to mean "approximately 40 mm."
[0265] All documents cited herein, including cross-referenced or related patents or applications, are incorporated herein by reference in their entirety unless expressly excluded or otherwise limited. No citation of any document shall be deemed prior art to any invention disclosed or claimed herein, nor shall it be deemed to teach, suggest or disclose any such invention, either alone or in combination with any other reference. Furthermore, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in any document incorporated by reference, the meaning or definition given to that term in this document shall prevail.
[0266] While specific embodiments of the present invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. Therefore, it is intended that all such changes and modifications within the scope of the invention be covered in the appended claims.
Claims
1. A women's hygiene product, Package including internal space and external surface, A plurality of disposable feminine hygiene pads disposed within the internal space of the package, each of the disposable feminine hygiene pads comprising a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet, wherein the absorbent core structure comprises an upper nonwoven fabric layer, a lower nonwoven fabric layer, and an inner core layer comprising cellulosic fibers, and at least a portion of the inner core layer disposed between the upper nonwoven fabric layer and the lower nonwoven fabric layer, The aforementioned disposable feminine hygiene pad, when measured according to the bag compression recovery method, measured 0.20 g / cm³. 3 A women's hygiene product exhibiting the following average pad density within the bag and a caliper recovery percentage of at least 4%, preferably at least 10%, in 2 minutes.
2. The disposable feminine hygiene pad, when measured according to the bag compression recovery method, weighs approximately 0.07 g / cm³. 3 ~Approx. 0.17g / cm 3 A women's hygiene product according to claim 1, which exhibits an average pad density inside the bag.
3. The women's hygiene product according to claim 1 or 2, wherein the inner core layer contains 50% to 85% by weight of cellulose fibers in the inner core layer.
4. The feminine hygiene product according to any one of claims 1 to 3, wherein the inner core layer further comprises superabsorbent particles in an amount of 15% to 50% by weight of the inner core layer.
5. The women's hygiene product according to any one of claims 1 to 4, wherein the upper nonwoven fabric layer has a basis weight of 30 gsm to 85 gsm.
6. The feminine hygiene product according to any one of claims 1 to 5, wherein the lower nonwoven fabric layer has a basis weight of 7 gsm to 40 gsm.
7. The feminine hygiene product according to any one of claims 1 to 6, wherein the disposable feminine hygiene pad exhibits a caliper recovery percentage of 4% to 35% in 4 hours when measured according to the bag compression recovery method.
8. The feminine hygiene product according to any one of claims 1 to 7, wherein the package comprises a packaging material selected from the group consisting of polymer film, paper material, cardboard for cartons, and combinations thereof.
9. The feminine hygiene product according to any one of claims 1 to 8, wherein the inner core layer contains cellulose fibers of 125 gsm to 350 gsm.
10. The feminine hygiene product according to any one of claims 1 to 9, wherein the inner core layer contains superabsorbent particles of about 20 gsm to about 125 gsm.
11. The aforementioned women's hygiene pad measured 7.0 N when subjected to wet and dry CD and MD three-point bending tests. * mm 2 ~30N * mm 2 A women's hygiene product according to any one of claims 1 to 10, which exhibits the CD dry bending rigidity.
12. A feminine hygiene product according to any one of claims 1 to 11, wherein the absorbent article exhibits a fifth-cycle wet recovery percentage of 29% to 40% when measured according to the wet and dry collapse compression method.
13. The feminine hygiene product according to any one of claims 1 to 12, wherein the feminine hygiene pad exhibits an average internal pad caliper of 2.0 mm to 5.5 mm when measured according to the internal compression recovery method.
14. The feminine hygiene product according to any one of claims 1 to 13, wherein the feminine hygiene pad exhibits an average outer pad caliper of 2.0 to 6.0 mm over 2 minutes when measured according to the inner bag compression recovery method.
15. The feminine hygiene pad has, when measured according to the in-bag compression recovery method, 0.06 g / cm 3 to 0.16 g / cm 3 exhibiting an average out-of-bag pad density at 2 minutes, the feminine hygiene product according to any one of claims 1 to 14.