Absorbent articles having short cellulose fibers
The absorbent article with a sealed inner core layer between nonwoven fabric layers addresses wet integrity issues in short cellulose fibers, ensuring structural integrity and flexibility, enhancing comfort and fluid management.
Patent Information
- Application Number
- JP2026528559
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-20
- Filing Date
- 2024-11-18
- Publication Date
- 2026-11-20
AI Technical Summary
Conventional absorbent articles using short cellulose fibers face challenges with wet integrity, leading to tearing and loss of shape, which compromises product performance and comfort, while increasing density to address this issue results in reduced flexibility and conformability.
A disposable absorbent article comprising a top sheet, back sheet, and an absorbent core structure with an upper and lower nonwoven fabric layer containing polymer fibers, and an inner core layer with a mixture of cellulose pulp and superabsorbent particles, where the inner core layer is sealed between the nonwoven layers, allowing for structural integrity and flexibility without high density.
The absorbent core structure maintains structural integrity and conforms to the wearer's shape while managing fluid efficiently, even when wet, by using elastic nonwoven layers to recover its shape and resist tearing, thus providing comfort and effective fluid management.
Smart Images

Figure 2026539233000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to an absorbent article having short cellulosic fibers, and more particularly to an absorbent article containing short cellulosic fibers that provides flexibility, conformability, and / or wettability during use. [Background technology]
[0002] Many consumers of disposable absorbent products, such as feminine hygiene pads, are seeking products that contain natural materials, bio-derived materials, recycled materials, and / or more environmentally friendly materials. Conventional cellulose sources, such as pine wood, grow relatively slowly and use a considerable amount of water and / or energy in the kraft pulp production process. In comparison, alternative cellulose sources such as eucalyptus, paulownia, and bamboo are known to grow faster and use less water and / or energy in the kraft pulp production process. Therefore, these alternative cellulose sources may be perceived by consumers as relatively more sustainable and / or environmentally friendly. However, replacing standard pine wood cellulose pulp, which is made from long cellulosic fibers (with an average length of 2.5 mm to 6 mm), with short cellulosic fibers with an average fiber length of less than approximately 2 mm can present challenges. When short cellulosic fibers are used in conventional absorbent core structures, the core may tear and lose its shape when wet, which can negatively impact product performance. The wet integrity problem of such absorbent core structures is often addressed by increasing the density of the absorbent core to help reduce core breakage and / or tearing. However, densification comes at the expense of comfort (rigidity) and the ability of the absorbent core structure and / or absorbent article to easily conform to the wearer's unique anatomical shape. [Overview of the Initiative] [Problems that the invention aims to solve]
[0003] There is a need for disposable absorbent articles containing relatively more sustainable and / or environmentally friendly materials that provide flexibility, conformability, and / or wet integration during use. [Means for solving the problem]
[0004] Disclosed herein are disposable absorbent articles comprising a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet. The absorbent core structure comprises (a) an upper nonwoven fabric layer comprising polymer fibers and having a basis weight of about 30 gsm to about 85 gsm, wherein the upper nonwoven fabric layer comprises a first side region and a second side region facing laterally; (b) a lower nonwoven fabric layer comprising polymer fibers, wherein the lower nonwoven fabric layer comprises a first side region and a second side region facing laterally; and (c) an inner core layer comprising a mixture of cellulose pulp and superabsorbent particles, wherein a portion of the inner core layer is disposed between the upper nonwoven fabric layer and the lower nonwoven fabric layer. The cellulose pulp comprises about 25% to about 70% by weight of short cellulose fibers. Short cellulose fibers have an average fiber length of less than approximately 2 mm. The absorbent core structure has a density of approximately 0.045 g / cm³. 3 ~Approx. 0.15g / cm 3 It has an average density of . A portion of the inner core layer is contained within the upper and lower nonwoven layers by sealing a portion of the first and second side regions of the upper nonwoven layer with a portion of the first and second side regions of the lower nonwoven layer in the peripheral seal.
[0005] Disclosed herein are disposable absorbent articles comprising a top sheet, a back sheet, and an absorbent core structure disposed between the top sheet and the back sheet. The absorbent core structure comprises (a) an upper nonwoven fabric layer containing polymer fibers and having a basis weight of about 30 gsm to about 85 gsm, (b) a lower nonwoven fabric layer containing polymer fibers and having a basis weight of about 7 gsm to about 40 gsm, and (c) an inner core layer containing a mixture of cellulose pulp and superabsorbent particles, with a portion of the inner core layer disposed between the upper and lower nonwoven fabric layers. The cellulose pulp comprises coniferous fibers and short cellulosic fibers in an amount of about 25% to about 70% by weight of the cellulose pulp, the short cellulosic fibers having an average fiber length of about 0.3 mm to about 2 mm. The absorbent core structure includes a plurality of structural binding sites. The structural binding sites are approximately 2 mm 2 ~about 5mm 2 It has a bond area of approximately 0.75% to 4.5% of the total structural bond area of the absorbable core structure, when measured according to the structural bond site pattern spacing and area measurement method. [Brief explanation of the drawing]
[0006] [Figure 1] This is a diagram of the absorbent core structure according to this disclosure. [Figure 2] This is a cross-sectional view of the absorbent core structure along line 2-2 in Figure 1. [Figure 3] This is a plan view of an absorbent material, with the surface facing the wearer oriented towards the viewer. A portion of the structure is cut out to more clearly show the composition of the absorbent core structure. [Figure 4] This is a cross-sectional view along line 4-4 in Figure 3. [Figure 5] This is a plan view of an absorbent article with the surface facing the wearer oriented towards the viewer, showing the arrangement of an example absorbent core structure. [Figure 6A] Figure 5 shows a cross-sectional view of the absorbent material along line 6A-6A. [Figure 6B] Figure 5 shows a cross-sectional view of the absorbent material along line 6B-6B. [Figure 7]This is a cross-sectional view of the absorbent article along line 7-7 in Figure 5. [Figure 8] This is a plan view of an absorbent article with the top sheet removed, where the surface facing the wearer is facing the viewer, and shows the arrangement of an example inner core layer and adhesive. [Figure 9] This is an enlarged view of a structural bonding site, one or more of the configurations shown and described herein. [Figure 10] This is a cross-sectional view of the structural bonding site in Figure 9. [Figure 11A] This is a plan view of an absorbent article in which the surface facing the wearer is oriented towards the viewer, and shows a flex-bonded channel region in one or more configurations shown and described herein. [Figure 11B] This is a plan view of an absorbent article in which the surface facing the wearer is oriented towards the viewer, and shows a flex-bonded channel region in one or more configurations shown and described herein. [Figure 12A] This is the setup for the test method for the wet and dry CD ultra-high sensitivity three-point bending method. [Figure 12B] This is the setup for the test method for the wet and dry CD ultra-high sensitivity three-point bending method. [Figure 12C] This is the setup for the test method for the wet and dry CD ultra-high sensitivity three-point bending method. [Figure 13] This is the configuration of the test method for wet and dry collapse and compression tests. [Figure 14A] This is the configuration of the test method for wet and dry collapse and compression tests. [Figure 14B] This is the configuration of the test method for wet and dry collapse and compression tests. [Figure 15A] This is an exemplary graph of deformation curves obtained from wet and dry deformation compression tests. The graph in Figure 15A is shown to illustrate how calculations in the method may be performed and does not represent the data described herein. [Figure 15B]This is an illustrative graph of deformation curves obtained from wet and dry deformation compression tests. The graph in Figure 15B is shown to illustrate how calculations in the method may be performed and does not represent the data described herein. [Modes for carrying out the invention]
[0007] When used in this specification, “disposable absorbent articles” or “absorbent articles” refer to articles intended for disposal after use, such as diapers, training pants, diaper pants, re-fastening pants, adult incontinence pads, adult incontinence pants, women’s hygiene pads, and cleaning pads.
[0008] As used herein, “absorbent core structure” shall be used in relation to the upper nonwoven layer, the lower nonwoven layer, and the inner core layer positioned between the upper and lower nonwoven layers. As used herein, “absorbent core structure” shall not include any secondary top sheet, top sheet, secondary back sheet, or back sheet of the absorbent article.
[0009] As used herein, “hydrophilic” and “hydrophobic” have well-established meanings in the art with respect to the water contact angle on the surface of a material. Therefore, a material with a water contact angle greater than about 90 degrees is considered hydrophobic, and a material with a water contact angle less than about 90 degrees is considered hydrophilic. A hydrophobic composition increases the water contact angle on the surface of a material, while a hydrophilic composition decreases it. Notwithstanding the foregoing, references to relative hydrophobicity or hydrophilicity between a material and a composition, between two materials, and / or between two compositions do not imply that the material or composition is hydrophobic or hydrophilic. For example, a composition may be more hydrophobic than a material. In this case, neither the composition nor the material may be hydrophobic. However, the contact angle exhibited by the composition is greater than that of the material. As another example, a composition may be more hydrophilic than a material. In this case, neither the composition nor the material may be hydrophilic. However, the contact angle exhibited by the composition is smaller than that of the material.
[0010] As used herein, the term “filament” refers to any type of continuous strand produced through a spinning process, a melt-blown process, a melt-fibrillation or film-fibrillation process, or an electrospinning production process, or any other suitable process for producing a filament. The term “continuous” in the context of filament is distinguished from staple filaments, which are cut to a specific target length. In contrast, a “continuous filament” is not cut to a predetermined length, but can instead break at random lengths, though typically much longer than staple filaments.
[0011] As used herein, “machine direction” refers to the direction in which the web flows through the absorbent material processing process. For brevity, it may be referred to as “MD.”
[0012] In this specification, "machine transverse direction" refers to the direction perpendicular to the MD. For brevity, it may be referred to as "CD".
[0013] As used herein, “elastic” refers to a material that tends to retain its shape in both dry and wet conditions, and, when subjected to a compressive force, tends to recover its original pre-compression shape when such force is removed. In some embodiments, the upper and / or lower nonwoven layers described herein may be elastic.
[0014] Decitex, also known as Dtex, is a measurement used in the textile industry to measure yarn or filament. 1 decitex = 1 gram per 10,000 meters. In other words, if a yarn or filament weighs 500 grams per 10,000 linear meters, then that yarn or filament has 500 decitex.
[0015] As used herein, “facing the wearer” (which may also be referred to as “facing the body”) and “facing the outside” (which may also be referred to as “facing the garment”) refer to the relative position of the surface of an element or group of elements, respectively. “Facing the wearer” means that the element or surface is closer to the wearer during wear than any other element or surface. “Facing the outside” means that the element or surface is further away from the wearer during wear than any other element or surface (i.e., the element or surface is closer to the wearer’s garment that may be worn over an absorbent article).
[0016] It should be understood that all maximum numerical limits given throughout this specification include all lower numerical limits as if they were explicitly stated herein. All minimum numerical limits given throughout this specification include all higher numerical limits as if they were explicitly stated herein. All numerical ranges given throughout this specification include all narrow numerical ranges that fall within such broad numerical ranges as if they were explicitly stated herein.
[0017] This disclosure relates to a disposable absorbent article comprising an absorbent core structure including an upper nonwoven layer and a lower nonwoven layer, together with an inner core layer containing a liquid absorbent material disposed between the upper and lower nonwoven layers. The liquid absorbent material may include a homogeneous mixture of cellulose pulp and superabsorbent particles, referred to herein as "fluff / AGM". At least a portion of the inner core layer may be contained within the upper and lower nonwoven layers by sealing portions of the first and second side regions of the upper nonwoven layer with the first and second side regions of the lower nonwoven layer, thereby defining a periphery seal that positions the adhesive between the upper and lower nonwoven layers and bonds the layers together. In some configurations, the periphery seal may extend around the entire periphery of the inner core layer.
[0018] The absorbent core structures described herein are configured to compress over a range of body movement and compression and to recover their original shape (dry or wet). The flexibility and / or elasticity of the absorbent core structures result in an absorbent article that comfortably conforms to the wearer's anatomical shape while efficiently managing fluid as it leaves the body. Unexpectedly, this can be achieved without typical high-density rigidity (for wet cohesion) by utilizing elastic upper and lower nonwoven fabric layers composed of elastic polymers located above and below the loosely filled liquid-absorbing material of the inner core layer. Remarkably, when the absorbent core structure is wet, it can bear structural loads and recover its shape without physically rigidifying or losing desired structural properties. While not bound by theory, it is believed that when selected elastic upper and lower nonwoven fabrics are positioned above and below the liquid-absorbing material in the inner core layer and bonded to and around the liquid-absorbing material, wet integrity / shape stability in a cellulose-rich absorbent core structure can be achieved without substantial densification and rigidity. The upper and lower nonwoven fabrics may have sufficient resilience to return the liquid-absorbing material to its original state and / or stable fiber orientation after compression. When a cellulose-rich pulp core is wrapped or encapsulated in simple cellulose tissue or a nonwoven fabric with low elasticity, sufficient recovery energy may not be exhibited to restore the shape during use, especially when wet. The structural wet-elastic nonwoven fabrics detailed herein may exhibit post-compression recovery energy sufficient to restore the cellulose-rich fiber matrix and may be selected to provide high compression recovery with relatively low stiffness in both dry and wet conditions. A suitable absorbent core structure is one that exhibits low compressive force (low resistance) and can recover its shape when the user periodically compresses it and releases the compressive force through various bodily movements. To achieve this, the structure should maintain sufficient recovery energy after multiple periodic compressions. Without sufficient recovery energy, the structure will remain in a compressed aggregate state with insufficient force (storage energy) to recover.
[0019] Surprisingly, it has been found that the absorbent core structures described herein can contain cellulose pulp with relatively high levels of short cellulosic fibers while still maintaining structural integrity and fit without requiring high density of the inner core layer. Short cellulosic fibers, such as eucalyptus, in absorbent core structures may be less physically entangled than longer, standard coniferous fibers. As a result, conventional absorbent core structures composed of short cellulosic fibers are more prone to bursting and tearing than core structures containing longer cellulose fibers. While not bound by theory, it is thought that the elastic upper and / or lower nonwoven layers of the inner core layer described herein may help provide structural integrity to the absorbent core structure and may allow the use of more than about 25% by weight of short cellulosic fibers, or about 25% to about 70% by weight of cellulose pulp.
[0020] Described herein is an absorbent core structure comprising a liquid-absorbent material sandwiched between two layers of elastic nonwoven fabric, which can not only bear and manage the mechanical stress exerted by the wearer's body during use, but also allow the absorbent core structure to recover its shape when the wearer compresses and deforms the absorbent article during use. The liquid-absorbent material may comprise a substantially homogeneous mixture of cellulose pulp and superabsorbent particles. The cellulose pulp may comprise about 25% to about 70% short cellulose fibers. The absorbent article has a viscosity of about 0.045 g / cm³. 3 ~Approx. 0.15g / cm 3It may have an average density of . Although not bound by theory, the overall density of the absorbent core structures described herein is thought to allow the cellulosic fibers (regardless of fiber length) to move and / or adjust to the wearer's body movements. The upper and / or lower nonwoven layers can help return the cellulosic fibers to their initial positions when the body's force is removed. In contrast, the high density of conventional cellulose cores substantially fixes the cellulose fibers together closely, reducing the risk of the fibers separating with body movements that could cause tearing and / or deformation. In addition, the absorbent core structures described herein, in which cellulose pulp and superabsorbent particles are substantially homogeneously mixed, are thought to be able to more rapidly dehydrate fluid from the capillary spaces between the cellulosic fibers (because the core is less dense and therefore has weaker capillary forces), and as a result, the cellulosic fibers are thought to resist wet disintegration and / or deformation when saturated with fluid.
[0021] An exemplary absorbent core structure 10 of this disclosure is shown in Figure 1. Figure 2 is a cross-sectional view cut along line 2-2 in Figure 1, with the structural bonding portion 15 removed to more clearly show the absorbent core structure 10.
[0022] Referring to Figures 1 and 2, the absorbent core structure 10 may include an upper nonwoven fabric layer 210 and a lower nonwoven fabric layer 220 (collectively referred to herein as the upper and lower nonwoven fabric layers or upper and lower nonwoven fabric), and an inner core layer 200 disposed between the upper and lower nonwoven fabric layers 210 and 220. The absorbent core structure 10 may also include an inner core layer 200 containing a liquid absorbent material. The liquid absorbent material may include a homogeneous mixture of cellulose pulp and superabsorbent particles. Parts of the upper and lower nonwoven fabric layers 210 and 220 may be joined together by a perimeter seal 230.
[0023] An exemplary absorbent article 20 of this disclosure is shown in Figure 3. To provide a reference frame for this study, the absorbent article 20 in Figure 3 is shown with a longitudinal axis 80 and a transverse axis 90. Figure 3 is a plan view of the absorbent article 20 with the surface 112 facing the wearer facing the viewer, and a portion of the structure is cut off to more clearly show the configuration of the absorbent core structure 10. Figure 4 is a cross-sectional view of the absorbent article 20 along line 4-4 in Figure 3.
[0024] Referring to Figures 3 and 4, the absorbent article 20 may include a top sheet 110, a back sheet 130, and an absorbent core structure 10 disposed between the top sheet 110 and the back sheet 130. The absorbent article 20 may include a surface 112 facing the wearer and a surface 132 facing the clothing. The absorbent article 20 and the absorbent core structure 10 may each include a front region 21, a rear region 23, and an intermediate region 22 disposed between the front region 21 and the rear region 23. In some configurations, the absorbent core structure 10 may have a non-rectangular perimeter. Specifically, the absorbent core may be molded to define a taper along its width toward the intermediate region of the absorbent core structure. The absorbent core structure can conform to the shape of the wearer's inner thigh, such as an hourglass shape, an offset hourglass shape (one end wider than the opposite end and the middle section between the ends narrower), a bicycle seat shape (one end and the middle section narrower than the second end), an ellipse, or a trapezoidal shape.
[0025] In some configurations, the disposable absorbent article 20 may include a structure consisting of a top sheet 110, an upper nonwoven fabric layer 210, an inner core layer 200, a lower nonwoven fabric layer 220, and a back sheet 130 (from the surface facing the wearer to the surface facing the outside). In some embodiments, the top sheet 110 may be in direct contact with the upper nonwoven fabric layer 210, the upper nonwoven fabric layer 210 may be in direct contact with the inner core layer 200, and / or the inner core layer 200 may be in direct contact with the lower nonwoven fabric layer 220. "Direct contact" means that there are no further intermediate component layers between each of the layers that are in direct contact. However, it is not excluded that an adhesive material may be placed between at least a portion of the above-described layers.
[0026] The upper nonwoven fabric layer 210 may include a first side region 210a and a second side region 210b opposite in the transverse direction, and the lower nonwoven fabric layer 220 may include a first side region 220a and a second side region 220b opposite in the transverse direction. In some configurations, the first side regions 210a, 220a of the upper and lower nonwoven fabric layers may extend substantially parallel to the longitudinal axis 80. The upper and lower nonwoven fabric layers 210, 220 may extend outward from the perimeter 200a of the inner core layer and may be joined together using adhesives or other conventional bonding methods including but not limited to ultrasonic bonding, melt bonding, crimping, and combinations thereof to form a perimeter seal 230. In some configurations, the entire inner core layer 200 may be located inside the perimeter seal 230. The periphery seal 230 can help seal the liquid-absorbing material of the inner core layer 200 to the inside of the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220. The periphery seal 230 may include at least a first seal region 231 extending substantially parallel to the longitudinal centerline 80, and a second seal region 231' opposite the first seal region 231. In some configurations, the periphery seal 230 may further include a front periphery seal region 232 and / or a rear periphery seal region 233. In some configurations, the periphery seal 230 may extend around the entire periphery 200a of the inner core layer.
[0027] While not bound by theory, it is conceivable that elastic nonwoven layers may retain their shape when wet and resist plasticization when attached to the inner core layer through the application of a core structure adhesive applied directly to either the inner core layer or the elastic nonwoven layer via a conventional spray coating application selected to achieve bonding but not to obstruct fluid flow to the inner core layer. The periphery seal 230 may be located in at least the intermediate region 22 of the absorbent article 20 and / or absorbent core structure 10. The intermediate region 22 (located between the wearer's thighs during use) is considered to be the area that will experience the most frequent and / or highest forces during use. It has been found that the presence of at least partially periphery seals in the first and second lateral regions of the upper and lower nonwoven layers outside the inner core layer may help ensure that the upper and lower nonwovens do not separate during physical deformation, do not restrict any potential integrity, and maintain their structural function without deformation problems. In addition, the periphery seal may allow any excess nonwoven material to be removed, enabling the absorbent core structure to be molded to conform to the shape of the inner thigh.
[0028] The periphery seal 230 may have a seal width WS of approximately 1 mm to 10 mm, or approximately 2 mm to 8 mm, or approximately 3 mm to 6 mm. The seal width WS may be uniform or may vary around the inner core layer.
[0029] In some configurations, the upper and lower nonwoven layers 210, 220 may be separate materials that can be cut to approximately the size and shape of the inner core layer 200 so as to fit between the top sheet 110 and the back sheet 130. In some configurations, the inner core layer 200, the upper nonwoven layer 210, and / or the lower nonwoven layer 220 may be molded, meaning they are non-rectangular.
[0030] In some configurations, multiple parts of the absorbent core structure may not include a periphery seal. In some configurations, the periphery seal 230 may only partially extend around the inner core layer periphery 200a. Figures 5 to 8 show an absorbent article and an example arrangement of an absorbent core structure. Elements in Figures 5 to 8 having the same reference numerals as those described above in relation to Figures 1 to 4 may be the same elements (e.g., the inner core layer 200). Figure 6A is a cross-sectional view of the absorbent article along line 6A-6A in Figure 5. Figure 6B is a cross-sectional view of the absorbent article along line 6B-6B in Figure 5. Figure 7 is a cross-sectional view of the absorbent article along line 7-7 in Figure 5.
[0031] Referring to Figures 5 to 7, in some configurations, the upper nonwoven fabric layer 210 extends longitudinally between the front edge 403 and the rear edge 404, defining a first side region 210a and a second side region 210b facing each other transversely. The lower nonwoven fabric layer 220 extends longitudinally between the front edge 408 and the rear edge 409, defining a first side region 220a and a second side region 220b facing each other transversely. The upper nonwoven fabric layer 210 may have a first nonwoven transverse width WN1, and the lower nonwoven fabric layer 220 may have a second nonwoven transverse width WN2. In some configurations, the first and second nonwoven transverse widths WN1 and WN2 may be substantially the same. In some configurations, the first and second nonwoven transverse widths WN1 and WN2 may be different. The transverse width WN1 of the first nonwoven fabric and / or the transverse width WN2 of the second nonwoven fabric may be approximately 40 mm to approximately 110 mm, or 45 mm to approximately 90 mm, or approximately 50 mm to approximately 80 mm. The upper and / or lower nonwoven fabric layers 210, 220 may have a longitudinal length of approximately 100 mm to approximately 450 mm, or approximately 150 mm to approximately 375 mm. In some configurations, the upper and / or lower nonwoven fabric layers 210, 220 may extend from the front article edge 30 to the rear article edge 32.
[0032] At least a portion of the inner core layer 200 may be positioned between the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 210. In some configurations, the entire inner core layer 200 may be positioned between the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220.
[0033] The inner core layer 200 extends longitudinally between the front edge 424 and the rear edge 426 of the inner core layer, and extends laterally from the first side edge 250 to the second side edge 252. In some configurations, the inner core layer 200 may be molded. As shown in Figure 8, the inner core layer 200 may define a first inner core layer lateral width WC1, a second inner core layer lateral width WC2, and a third inner core layer lateral width WC3 disposed between them. In some configurations, the first inner core layer lateral width WC1 may be in the front region 21, and the second inner core layer lateral width WC2 may be located in the rear region 23. In some configurations, the third inner core layer lateral width WC3 may be smaller than the first and second inner core layer lateral widths WC1 and WC2. In some configurations, the lateral width WC2 of the second inner core layer may be greater than the lateral widths WC1 and WC3 of the first and third inner core layers. The lateral width WC1 of the first inner core layer may be approximately 50 to 80 mm, the lateral width WC2 of the second inner core layer may be approximately 55 mm to 100 mm, and the lateral width WC3 of the third inner core layer may be approximately 40 mm to 70 mm.
[0034] The adhesive zone 525 may be located between at least one of the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 and the inner core layer 200. The adhesive zone 525 may include an adhesive 528 extending from a first side region 210a to a second side region 210b of the upper nonwoven fabric layer 210, and / or from a first side region 220a to a second side region 220b of the lower nonwoven fabric layer 220. As shown in Figure 8, the adhesive zone 525 may extend from a first edge 525a to a second edge 525b, defining an adhesive zone lateral width WZ of about 35 mm to about 110 mm, or about 40 to about 105 mm. In some configurations, the first and second edges 525a, 525b of the adhesive zone 525 may be adjacent to the lateral edges of the upper and / or lower nonwoven layers 210, 220, or they may be spaced laterally inward from them. In some configurations, as shown in Figure 5, the gap region 530 may be defined on the upper and / or lower nonwoven layers 210, 220 by the absence of adhesive 528 between the first and second edges 525a, 525b of the adhesive zone 525 and the edges of the nonwoven fabric. The gap region 530 may have a width of 5 mm or less, or about 0.1 mm to about 5 mm, or about 0.5 mm to about 3 mm. In some configurations, the upper nonwoven layer 210 and the lower nonwoven layer 220 may substantially surround the adhesive zone 525 and the inner core layer 200.
[0035] In some configurations, a portion of the inner core layer 200 may be contained within the upper and lower nonwoven layers 210 and 220 by sealing a portion of the first side region 210a and the second side region 210b of the upper nonwoven layer 210 with a portion of the first side region 220a and the second side region 220b of the lower nonwoven layer 220, thereby defining a lateral periphery seal 230 in which the adhesive 528 is positioned between the upper and lower nonwoven layers 210 and 220. Thus, the adhesive 528 can bond the upper nonwoven layer 210 to the lower nonwoven layer 220. The lateral periphery seal 230 may be located in an intermediate region 22 and may have a longitudinal seal length LS that is about 45% to about 90% or about 50% to about 85% of the longitudinal inner core length LC.
[0036] Referring to Figure 5, a portion of the inner core layer 200 may extend laterally outward from the adhesive zone 525 to define an unsealed portion 420. The unsealed portion 420 may be located longitudinally outward from the periphery seal 230. It should be understood that the absorbent core structure 10 may include one or more unsealed portions 420, such as two, three, or four, depending on the size and / or arrangement of the upper and lower nonwoven fabric layers relative to the size and / or arrangement of the adhesive zone and the inner core layer.
[0037] The absorbent core structure 10 may include a first unsealed portion 423a, in which a portion of the inner core layer 200 extends laterally outward from the adhesive zone 525. In some configurations, the absorbent core structure 10 may include a second unsealed portion 423b, in which a second portion of the inner core layer 200 extends laterally outward from the adhesive zone 525. The second unsealed portion 423b may be laterally separated from the first unsealed portion 423a by a sealing portion 410. In some configurations, the first and second unsealed portions 423a, 423b may be located in the rear region 23 and may extend longitudinally within a portion of the intermediate region 22. The absorbent core structure 10 may further include a third unsealed portion 421a, in which a third portion of the inner core layer 200 extends laterally outward from the adhesive zone 525. In some configurations, the absorbent core structure 10 may include a fourth unsealed portion 421b, the fourth portion of the inner core layer 200 extending laterally outward from the adhesive zone 525. The fourth unsealed portion 421b may be laterally separated from the third unsealed portion 421a by the sealing portion 410. In some configurations, the third and fourth unsealed portions 421a, 421b may be located within the front region 21 or may extend longitudinally within the intermediate region 22. The unsealed portion 420 may also be formed in a configuration in which a portion of the inner core layer perimeter 200a is adjacent to the first or second edges 525a, 525b of the adhesive zone 525.
[0038] The first and second non-seal portions 423a, 423b may have a non-seal longitudinal length L1U that is about 5% to about 30% or about 8% to about 25% of the longitudinal inner core length LC. The third and fourth non-seal portions 421a, 421b may have a non-seal longitudinal length L2U that is about 5% to about 30% or about 8% to about 25% of the longitudinal inner core length LC. In some configurations, the non-seal longitudinal length L1U of the first or second non-seal portions 423a, 423b may be greater than the non-seal longitudinal length L2U of the third or fourth non-seal portions 421a, 421b.
[0039] Figures 6A and 6B are cross-sectional views of the absorbent article 20 of Figure 5 along lines 6A-6A and 6B-6B, respectively, and show the configuration of the absorbent core structure 10. In particular, Figure 6A is a cross-sectional view passing through the intermediate region 22 of the absorbent article 20, showing that the upper and lower nonwoven fabric layers 210 and 220 extend laterally outward from the first and second side edges 250 and 252 of the inner core layer 200. As described above, a portion of the inner core layer 200 may be housed within the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 by sealing a portion of the first side region 210a and the second side region 210b of the upper nonwoven fabric layer 210 with a portion of the first side region 220a and the second side region 220b of the lower nonwoven fabric layer 220, thereby defining a lateral periphery seal 230. Figure 6B is a cross-sectional view through the rear region 23 of the absorbent article 20, showing that the upper and lower nonwoven layers 210, 220 extend laterally outward from the first and second side edges 250, 252 of the inner core layer 200. As described above, a portion of the inner core layer 200 may extend laterally outward from the adhesive zone 525 (not shown) to define an unsealed portion 420. It should be understood that the garment-facing surface of the upper nonwoven layer 210 and / or the wearer-facing surface of the lower nonwoven layer 220 may be coated with adhesive 528 to provide connection with the inner core layer 200 and / or form a perimeter seal 230. Interlayer adhesives (except for the perimeter seal) are not shown in Figures 6A and 6B for simplification.
[0040] As described above, the upper and lower nonwoven fabric layers 210 and 220 may be further joined by a front periphery seal region 232 and / or a rear periphery seal region 233 located on the longitudinal outer side of the inner core layer 200. The front periphery seal region 232 and / or the rear periphery seal region 233 may extend longitudinally from the periphery 200a of the inner core layer for a distance of approximately 3 mm to approximately 30 mm, or approximately 5 mm to approximately 15 mm. Although not theoretically bound, it is conceivable that front and / or rear periphery seal regions 232 and 233 of less than approximately 3 mm may not provide sufficient distance on the production line to avoid contamination of the liquid absorbent material outside the inner core layer. In some configurations, the front periphery seal region 232 may be adjacent to the leading edge 403 of the upper nonwoven fabric layer 210 and / or the leading edge 406 of the lower nonwoven fabric layer 220, or it may be spaced longitudinally inward from them. In some configurations, the rear peripheral seal 233 may be adjacent to the rear edge 404 of the upper nonwoven fabric layer 210 and / or the rear edge 409 of the lower nonwoven fabric layer 220, or it may be spaced longitudinally inward from them.
[0041] In some structures, the lateral width WC1 and adhesive zone width WZ of the first inner core layer may be substantially the same, and the adhesive 528 does not extend laterally outward around the inner core layer 200a, creating an unsealed portion in this area where the upper nonwoven layer 210 is not bonded to the lower nonwoven layer 220. In some configurations, the lateral width WC2 of the second inner core layer may be substantially the same as the adhesive zone width WZ, and is therefore understood to define an unsealed portion in the rear region 23. In some structures, the lateral width WC1 of the first inner core layer may be smaller than the adhesive zone width WZ. The upper and lower nonwoven layers 210, 220 and the adhesive zone 525 may substantially surround the inner core layer in the front region, and the lateral perimeter seal 230 may extend longitudinally from the intermediate region 22 to the front region 21. In this configuration, the inner core layer is sealed within the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 in the intermediate region 22 and the front region 21. In some configurations, the lateral width WC2 of the second inner core layer may be smaller than the adhesive zone width WZ, and it is understood that a lateral periphery seal 230 is created that extends longitudinally from the intermediate region 22 to the rear region 23.
[0042] In some structures, at least one of the upper nonwoven fabric layer 210 and the lower nonwoven fabric layer 220 may be narrower than at least a portion of the inner core layer. In some configurations, the upper nonwoven fabric layer 210 and / or the lower nonwoven fabric layer 220 may be narrower than the lateral width WC1 of the first inner core layer and / or the lateral width WC2 of the second inner core layer.
[0043] Referring to Figures 5 and 7, the front edge 403 of the upper nonwoven layer 210 and / or the front edge 408 of the lower nonwoven layer 220 may be adjacent to the front article edge 30, or they may be spaced longitudinally inward from the front article edge 30. In some configurations, the rear edge 404 of the upper nonwoven layer 210 and / or the rear edge 409 of the lower nonwoven layer 220 may be adjacent to the rear article edge 32, or they may be spaced longitudinally inward from the rear article edge 32. The absorbent article 20 may further include a crimp seal 500 located in the front region 21 and / or the rear region 23. In some configurations, the crimp seal 500 may extend from the front region 21 and / or the rear region 23 into the intermediate region 22. In some configurations, the crimp seal 500 may be located longitudinally outward of the front and rear perimeter seals 232, 233. In some configurations, the front and / or rear perimeter seal regions 232, 233 may extend within the crimp seal 500.
[0044] The crimp seal 500 may bond a top sheet 110, a back sheet 130, and at least one of an upper nonwoven fabric layer 210 and a lower nonwoven fabric layer 220. In some configurations, the crimp seal 500 may bond the top sheet 110 to the back sheet 130. Surprisingly, it has been found that the crimp seal 500 can include upper and / or lower nonwoven fabric layers 210, 220 without becoming stiff or unpleasant. The crimp seal 500 may substantially not contain any liquid absorbent material.
[0045] Referring to Figure 3, the absorbent article 20 may further include a chassis 100 containing an absorbent core structure 10. The absorbent core structure 10 and / or inner core layer 200 can be molded. The side edges 120 and 125 of the absorbent article 20 may follow the overall contour of the absorbent core structure 10 and / or inner core layer 200. Thus, for example, if the absorbent core structure 10 has an hourglass shape, the side edges 120 and 125 of the absorbent article 20 may similarly be arranged in an hourglass shape. However, there may also be configurations in which the side edges 120 and 125 are generally straight or slightly curved so as not to follow the contour of the absorbent core structure. In some configurations, the absorbent article 20 may be symmetrical with respect to the longitudinal centerline 80 or asymmetrical with respect to the longitudinal centerline 80. Similarly, the absorbent article 20 may be symmetrical with respect to the transverse centerline 90 or asymmetrical with respect to the transverse centerline 90.
[0046] In some structures, the absorbent article and / or absorbent core structure may include a plurality of structural bonding sites 15, as shown in Figures 1, 9, and 10. Figures 9 and 10 show illustrations of example structural bonding sites 15. Figure 9 is a magnified view of an example structural bonding site 15. Figure 10 is a cross-sectional view of the structural bonding site 15 in Figure 9. The structural bonding sites 15 may be symmetrical and / or asymmetrical, and may be any shape, including but not limited to circular, elliptical, heart-shaped, diamond-shaped, triangular, square, star-shaped, and / or X-shaped. While the shape of the structural bonding site 15 may be any shape, preferred shapes may be denser shapes, such as asymmetrical shapes (as opposed to simple dots). The structural bonding sites 15 may be on the absorbent article and / or absorbent core structure. In some configurations, the structural bonding sites are approximately 2 mm 2 ~about 5mm 2The bonding area may be approximately 0.5% to 7.5%, 0.75% to 5%, or 1% to 4% of the absorbent core structure when measured according to the structural bonding site pattern spacing and area measurement method. The average distance between structural bonding sites may be approximately 10 mm to 32 mm. In some configurations, the average distance between structural bonding sites may be greater than approximately 20 mm. In some configurations, the structural bonding sites may have a maximum width of approximately 1 mm to 6 mm, 1.5 mm to 5 mm, or 2 mm to 4 mm. While not limited by theory, the average distance between these structural connection points and / or the size of these structural connection points are thought to help maintain the structural integrity of the absorbent core structure without creating undesirable stiffness that could impair the absorbent article's ability to conform to the body.
[0047] In some configurations, structural bonding sites may be distributed across the absorbent article and / or absorbent core structure, or they may be concentrated in each region of the absorbent article and / or absorbent core structure. In some configurations, structural bonding sites may be concentrated in the intermediate region 22 of the absorbent article and / or absorbent core structure. In some configurations, the intermediate region 22 of the absorbent article and / or absorbent core structure may not contain structural bonding sites, but may be surrounded by the structural bonding sites and / or embossed areas.
[0048] In some configurations, the structural bonding site 15 may bond the top sheet 110, the upper nonwoven layer 210, the absorbent core structure 10, and the lower nonwoven layer 220. In some configurations, the structural bonding site 15 may bond the upper nonwoven layer 210, the absorbent core structure 10, and the lower nonwoven layer 220. The absorbent article 20 and / or absorbent core structure 10 may comprise the upper nonwoven layer 210 and the lower nonwoven layer 220, which are closer to each other in the Z direction at the structural bonding site 15 but are not melted to each other. Since these structural bonding sites are not melted to each other, they may not be permanent in nature and may rather mix the materials within the structural bonding site. In some configurations, the structural bonding site 15 may substantially not contain melt bonding.
[0049] As shown in Figures 11A and 11B, the absorbent article may include one or more flex-bonded channel regions 160, the flex-bonded channel regions may be a series of depressions and / or a series of individually compressed, densely spaced embossed areas.
[0050] A suitable upper nonwoven fabric layer may have a basis weight of approximately 30 gsm to approximately 85 gsm, or approximately 35 gsm to approximately 70 gsm, or approximately 40 to approximately 60 gsm. The upper nonwoven fabric layer may have a tensile stiffness of approximately 0.1 N / mm to approximately 2.2 N / mm, or approximately 0.3 N / mm to approximately 1.6 N / mm, when measured according to the CD periodic stretching method up to 3% strain. The upper nonwoven fabric layer may have a breaking strain of more than approximately 10%, or approximately 10% to approximately 50%, or approximately 20% to approximately 40%, when measured according to the breaking strain method. The upper nonwoven fabric layer may have a permanent strain of approximately 0.005 to approximately 0.013 mm / mm, or 0.005 to approximately 0.0090 mm / mm, when measured according to the CD periodic stretching method up to 3% strain.
[0051] A suitable upper nonwoven fabric layer may have a basis weight of approximately 7 gsm to approximately 40 gsm, approximately 10 gsm to approximately 35 gsm, or approximately 15 gsm to approximately 20 gsm. The lower nonwoven fabric layer may have a tensile stiffness of approximately 0.2 N / mm to approximately 1.6 N / mm when measured according to the CD periodic stretching method up to 3% strain. The lower nonwoven fabric layer may have a fracture strain of more than approximately 10%, or approximately 10% to approximately 50%, or approximately 20% to approximately 40% when measured according to the fracture strain method. The lower nonwoven fabric layer may have a permanent strain of approximately 0.005 to approximately 0.013 mm / mm when measured according to the CD periodic stretching method up to 3% strain.
[0052] The upper and / or lower nonwoven layers may contain polymer fibers. Suitable upper and lower nonwoven fibers may be selected from PET (polyethylene terephthalate), PP (polypropylene), BiCo (two-component fiber) selected from PE / PP (PE sheath and PP core) and / or PE / PET (PE sheath and PET core), PLA (polylactic acid), and combinations thereof. In some configurations, the upper and / or lower nonwoven layers may contain recycled polymer resins, biodegradable polymers, biopolymers, bio-based fibers, and combinations thereof.
[0053] A suitable upper nonwoven fabric may contain approximately 60-100% or 70-100% synthetic fibers, or approximately 0-40% or 0-30% regenerated cellulose fibers such as rayon and / or viscose.
[0054] The upper nonwoven fabric layer may contain fibers with staple lengths of approximately 10 mm or more, or approximately 25 mm or more, or approximately 10 mm to approximately 100 mm, or approximately 20 mm to approximately 75 mm, or approximately 25 mm to approximately 50 mm. The upper nonwoven fabric layer may contain fibers with fiber diameters of approximately 1.3 Dtex to approximately 10.0 Dtex, or approximately 1.3 Dtex to approximately 6.0 Dtex, or approximately 2.0 Dtex to approximately 5.0 Dtex. Although not theoretically bound, it is thought that if the fibers of the upper nonwoven fabric layer are less than approximately 1.3 Dtex, the airflow through the material during manufacturing may be insufficient.
[0055] In some configurations, the upper nonwoven layer may contain a blend of staple fibers. If the upper nonwoven layer contains a blend of staple fibers, the fiber blend preferably contains 30% or less of fibers with a fiber diameter of 1.3 Dtex and / or 30% or less of fibers with a fiber diameter of 10.0 Dtex. In some configurations, the upper nonwoven layer may contain fibers, which are a blend of staple fibers having a fiber diameter of about 2.0 Dtex to about 8.0 Dtex. While not bound by theory, fibers with an average fiber diameter of about 2.0 Dtex to about 8.0 Dtex are thought to help allow sufficient airflow through the material during the fabrication of the absorbent core structure.
[0056] The lower nonwoven layer may contain fibers having staple lengths of approximately 10 mm or more, or approximately 25 mm or more, or approximately 10 mm to approximately 100 mm, or approximately 20 mm to approximately 75 mm, or approximately 25 mm to approximately 50 mm. In some configurations, the lower nonwoven layer may contain continuous fibers. The lower nonwoven layer may contain fibers having a fiber diameter of approximately 1.0 DTex to approximately 5.0 DTex, or approximately 1.3 DTex to approximately 3.3 DTex, or approximately 1.3 DTex to approximately 2.2 DTex, or approximately 2.0 DTex to approximately 10.0 DTex. In some configurations, the lower nonwoven layer may contain fibers, which are a blend of fibers having a fiber diameter of approximately 0.1 DTex to approximately 6.0 DTex.
[0057] In some configurations, the upper nonwoven layer may comprise a blend of fibers, at least a portion of the fibers having a diameter of from about 2.0 DTex to about 10.0 DTex, and the lower nonwoven layer may comprise a blend of fibers, at least a portion of the fibers having a diameter of from about 1.3 DTex to about 5.0 DTex. In some configurations, the upper nonwoven layer may comprise a blend of fibers, at least a portion of the fibers having a diameter of from about 1.3 DTex to about 2.2 DTex, and the lower nonwoven layer may comprise a blend of fibers, the blend of fibers having a diameter of from about 1.0 DTex to about 5.0 DTex.
[0058] Suitable upper and / or lower nonwoven layer materials may bend and substantially recover their original shape after a bending force. Thin or highly flexible materials bend easily at low peak force (load) and low bending energy. Unsuitable materials bend easily but do not have sufficient recovery energy, and thus retain their deformed bent state due to insufficient recovery energy. Suitable materials have sufficient energy to substantially recover their initial pre-bending state. Materials with sufficient bending recovery energy can be regarded as elastic upper and lower nonwoven layers. A particularly suitable upper nonwoven layer is about 0.03 N * mm or more, or about 0.03 N * mm to about 1 N * mm, or about 0.04 N * mm to about 0.5 N * mm of dry recovery energy. A particularly suitable upper nonwoven layer may have a dry bending energy of less than about 1.6 N * mm, or less than about 1.1 N * mm.
[0059] As described above, the upper and lower nonwoven fabrics may contain polymer fibers. Polymer fibers may be included to help provide structural integrity to the upper and lower nonwoven fabrics. Polymer fibers can help increase the structural integrity of the upper and lower nonwoven fabrics in both the machine direction (MD) and the cross-machine direction (CD), thereby facilitating web manipulation of the upper and lower nonwoven fabrics during processing for incorporation into the pad.
[0060] Polymer fibers of any suitable composition can be selected. Some examples of suitable polymer fibers include two-component fibers containing polyethylene (PE) and polyethylene terephthalate (PET) components or polyethylene terephthalate and copolyethylene terephthalate components. The components of the two-component fiber may be arranged in a sheath-core configuration, a parallel configuration, an eccentric sheath-core configuration, a trefoil configuration, or other suitable configurations. In some configurations, the polymer fibers may include two-component fibers having PE / PET components arranged in a concentric sheath-core configuration, where the polyethylene component forms the sheath.
[0061] While other materials may be useful in creating elastic structures, the stiffness of the PET core component in the sheath-core fiber configuration is considered useful in imparting elasticity to the upper and lower nonwoven fabrics. In a synergistic combination, the PE sheath component, which has a lower melting temperature than the PET core component, can be used to provide interfiber melting / fusion bonding brought about by the heat treatment of the precursor butt. This can help provide tensile strength to the web in both MD and CD. Such interfiber bonding helps reduce slippage between fibers, thereby further contributing to imparting dimensional stability and resilience to the material, even when the material is wet.
[0062] When a relatively high weight fraction of polymer fibers is included, more connections can be formed within the structure through heat treatment. However, too many connections can impart greater stiffness to the upper and lower nonwovens than desired. For this reason, selecting the weight fraction of polymer fibers may involve prioritizing and balancing the competing needs for stiffness and flexibility in the upper and lower nonwovens.
[0063] As described above, the upper and lower nonwoven fabrics may further contain polymer fibers that increase the elasticity of the upper and lower nonwoven fabrics. The elastic polymer fibers can help the upper and lower nonwoven fabrics maintain permeability and compression recovery. In some configurations, the upper and lower nonwoven fabrics may contain elastic polymer fibers having various cross-sections, e.g., circular and hollow spiral, and / or elastic fibers having various sizes.
[0064] The polymer fibers may be elastic and may be spun from any suitable thermoplastic resin, such as polypropylene (PP), polyethylene terephthalate (PET), or other suitable thermoplastic plastics known in the art. The elastic polymer fibers may have any suitable structure or shape. For example, the elastic polymer fibers may be circular, or may have other shapes such as helical, wavy elliptical, trefoil, wavy ribbon, and so on. Furthermore, the elastic polymer fibers may be solid, hollow, or multi-hollow. The elastic polymer fibers may be solid and round. In another preferred example, the elastic polymer fibers may include polyester / co-extruded polyester fibers. In one particular example, PET fibers may have a hollow cross-section and may have a curled or helical structure along their length. Optionally, the elastic polymer fibers may be helically crimped or flatly crimped. Elastic polymer fibers may have an average crimp value of about 4 to about 12 crimps / inch (cpi), or about 4 to about 8 cpi, or about 5 to about 7 cpi, or about 9 to about 10 cpi. Specific non-limiting examples of elastic polymer fibers are available from Wellman, Inc. (Ireland) under trade designations H1311 and T5974. Other examples of suitable elastic polymer fibers are disclosed in U.S. Patent No. 7,767,598.
[0065] The rigid polymer fibers and elastic polymer fibers should be carefully selected. For example, the constituent polymers forming the rigid polymer fibers and elastic polymer fibers may have commonalities, but the elastic polymer fibers must be selected such that the melting points of their constituents are higher than those of the bondable components of the rigid polymer fibers. Otherwise, during heat treatment, the elastic polymer fibers may bond to the rigid polymer fibers (or vice versa), thereby forming an excessively rigid structure. To avoid this risk when the rigid polymer fibers include two-component fibers, for example, core-sheath constituent fibers with a sheath component having a relatively low melting temperature at which molten bonding occurs, the elastic polymer fibers may include only the core constituent chemicals, which may be polymers with relatively high melting temperatures.
[0066] Nonwoven fabric performance can be influenced by a combination of the selection of nonwoven fiber polymers, fiber properties, and how the fibers are arranged or connected. The choice of nonwoven fabric can affect the ability of absorbent articles to recover their shape in response to compressive, bending, and stretching forces that occur during use due to body movement. When the fibers are short fibers (less than approximately 10 mm), the fibers are likely to rearrange irreversibly under stretching and compressive forces. Rearranging the fibers in the fiber matrix (changing their orientation / state) dissipates the tensile (stretching) or compressive force, and as a result, the energy used to influence the deformation is not available for recovery to the original shape. Longer fiber networks (typically greater than approximately 10 mm but less than approximately 100 mm) can absorb the tensile / compressive forces typical of body movement along the length of the fibers and across the structure. As a result, the absorbed forces are available to restore the structure to its original state. Longer fibrous network structures composed of finer fibers (approximately 15 microns to less than 20 microns) stretch and compress more easily. As a result, the fluff / AGM structure can deform more easily (and to a greater extent), but the energy associated with these deformations is relatively small and insufficient to return the structure to its original state. Thicker fibers, such as those over approximately 20 microns, or approximately 2.0 DTex to 10 DTex, are both flexible under bodily force, but provide sufficient fiber and web recovery energy to return the structure to its original state.
[0067] From a structural standpoint, the arrangement of fibers in a long-fiber network structure can affect the performance of absorbent articles containing these nonwovens. Long-fiber webs of thicker fibers are typically bulkier than conventional thin spunbond nonwoven webs, which consist of continuous fine fibers that are closely spaced and physically bonded together. By creating webs of thicker fibers arranged in a more random orientation, which can be achieved through carding, water entanglement, and needling, the fibers can be stretched and compressed, thereby allowing them to adjust their arrangement only temporarily (spaces between fibers exist for these arrangements) and to bear / store deformation forces, this energy being available to restore the structural shape.
[0068] Furthermore, thinner synthetic fibers (less than approximately 2.0 DTex), such as BiCo and PP fibers commonly found in spunbond, are densely spaced, aligned relatively parallel to each other, and tightly bonded together. Because these bonded fibers within the spunbond web are interconnected (by closely spaced point bonds), under tension (stretching), the fibers are forced to stretch at the polymer level, and the polymer chains within the fibers are permanently rearranged. As a result, the fibers themselves remain potentially permanently stretched (permanently distorted) and can no longer return to their original state.
[0069] In some configurations, the polymer fibers in the upper nonwoven layer and the polymer fibers in the lower nonwoven layer may be different. In some configurations, the polymer fibers in the upper nonwoven layer and the polymer fibers in the lower nonwoven layer may be the same. In some configurations, the upper nonwoven layer may be a carded nonwoven. In some configurations, the upper nonwoven layer may be air-through bonded, needle-punched, carded, or water-flow entangled. In some configurations, the upper nonwoven layer is not a spunbond material.
[0070] Examples of suitable nonwoven materials, though not limited to them, include: (i) a 40gsm carded elastic nonwoven material manufactured by Yanjan China (material code: ATB Z87G-40-90), which is a carded nonwoven fabric composed of a blend of 60% 2DTex and 40% 4DTex BiCo(PE / PET) fibers. These fibers are bonded together (ATB = "hot" air bond) to form a wet elastic network structure. The basis weight of the material is 40gsm, and its caliper (less than 7kPa) is approximately 0.9mm. Although not bound by theory, due to the presence of 4DTex BiCo fibers and the interfiber-bonded BiCo network structure, the material exhibits low permanent strain (less than approximately 0.013mm / mm) and sufficient dry recovery energy (approximately 0.03N) in wet and dry CD ultra-high sensitivity three-point bending methods. * (ii) A 55gsm elastic spunlace material manufactured by Sandler Germany (material code: 53FC041001), which is a water-flow entangled nonwoven fabric produced by water-flow entanglement using a carding process (as described above for the nonwoven fabric), followed by an upward drying process (as described in U.S. Patent Application Publication No. 2020 / 0315873(A1)) that produces both entangled and BiCo-bonded elastic reticular structures. It contains a fiber blend of 30% 10DTex HS-PET, 50% 2.2DTex BiCo(PE / PET), and 20% 1.3DTex rayon. Thus, this material exhibits low permanent strain (less than approximately 0.013 mm / mm) and sufficient drying recovery energy (approximately 0.03 N) in wet and dry CD ultra-high sensitivity three-point bending methods. *(iii) A water-flow entangled nonwoven fabric produced by Sandler Germany (material code: 53FC041005 opt82), which is produced by water-flow entanglement through a carding process (such as the nonwoven fabric described above) and a subsequent rising drying process (such as the one described in U.S. Patent Application Publication No. 2020 / 0315873(A1)) that produces both entanglement and a BiCo-bonded elastic lattice structure. This material contains a fiber blend of 60% 5.8DTex BiCo(PE / PET), 20% 3.3DTex trefoil-shaped "structure" rayon, and 20% 1.3DTex rayon. Thus, this material exhibits low permanent strain (less than about 0.013 mm / mm) and sufficient drying recovery energy (about 0.03 N) in wet and dry CD ultra-high sensitivity three-point bending methods. * It has a thickness of over mm. This material contains 40% rayon, which can soften when wet, but the use of structural trifoliate rayon fibers helps maintain structural stability in wet conditions.
[0071] In combination with adjusting pore size, volume, and number by selecting appropriate fiber size, basis weight, and degree of compaction, manufacturers may desire to select fiber components to obtain specific surface chemical properties, e.g., fibers with hydrophobic or hydrophilic surfaces, or blends of different fibers and / or fibers with z-directional layering or gradients. Fibers with hydrophilic surfaces tend to attract and move along the aqueous components of menstrual fluid, in a manner that facilitates suction after discharge and rapid fluid acquisition. However, at the same time, the dominance of hydrophilic fiber surfaces in the top sheet may increase the tendency of the top sheet to reacquire fluid from the absorbent components below (re-wetting), which can cause an undesirable wet feeling for the user. On the other hand, fibers with hydrophobic surfaces tend to repel the aqueous components of menstrual fluid and / or resist the movement of fluid along their surfaces, thereby resisting suction, but also resisting re-wetting. Manufacturers may desire to find the right balance when selecting constituent fibers with hydrophilic surfaces, fibers with hydrophobic surfaces, or blends and / or z-directional lamination for any particular product design, in combination with fiber size, fiber reinforcement level, and the resulting top sheet pore size, volume, and number.
[0072] The inner core layer is manufactured by the air-lay method. A flow of cellulose pulp and superabsorbent particles is carried on a high-speed airflow and deposited into a three-dimensional molded pocket on a rotational molding drum with downward vacuum suction to draw the cellulose pulp and superabsorbent particles into the pocket of the laydown station. This molded pocket provides the actual physical shape of the absorbent core structure. The upper or lower nonwoven fabric may be introduced onto the molding drum first, and under vacuum, the upper or lower nonwoven fabric is stretched into the three-dimensional pocket shape. In this case, the flow of cellulose pulp and superabsorbent particle material is deposited directly onto the upper (or lower) nonwoven material at the molding station. Before entering the molding station, the nonwoven fabric is coated with an adhesive to provide a stronger bond between the cellulose and superabsorbent polymer in the nonwoven layer. Particularly suitable adhesives include high-wet-strength adhesives such as Technomelt DM9036U, available from Henkel (Germany). Upon exiting the laydown section, the second remaining nonwoven layer is combined with the nonwoven supporting the cellulose pulp and superabsorbent particle layer exiting the laydown section. This second remaining nonwoven (either the upper or lower nonwoven, depending on which nonwoven passes through the laydown section) is pre-coated with an adhesive to allow for a perimeter seal and to better integrate the cellulose pulp and superabsorbent particles without obstructing the flow of liquid into the cellulose pulp and superabsorbent particle matrix. In an alternative method, the nonwoven is not initially introduced into the molding station, and the mass of cellulose pulp and superabsorbent particles is held on a molding drum under vacuum until discharged onto either the upper or lower nonwoven layer coated with the adhesive as detailed above, and then sealed with the second remaining nonwoven to create an absorbent core structure. The widths of the upper and lower nonwoven webs are typically selected to be wider than the maximum width of the molded cellulose pulp and superabsorbent particle matrix, thereby enabling an effective periphery seal where the two nonwovens connect at least on the leftmost and rightmost sides of the absorbent core structure.
[0073] The inner core layer may contain one of a wide variety of liquid-absorbent materials widely used in disposable absorbent articles, such as crushed wood pulp, commonly known as air felt. One suitable absorbent core material is the air felt material available from Weyerhaeuser Company (Washington, USA) under code number FR516. Other suitable liquid-absorbent materials used in absorbent cores may include crepe cellulose wadding, meltblown polymers including coform, synthetic fibers such as chemically hardened, modified, or crosslinked cellulose fibers or crimped polyester fibers, peat moss, cotton; absorbent polymer materials, or any equivalent materials or combinations thereof.
[0074] In some configurations, the liquid absorbent material may comprise a substantially homogeneous mixture of cellulose pulp and superabsorbent particles. The cellulose pulp may comprise short cellulosic fibers. As used herein, “short cellulosic fibers” means cellulosic fibers having an average fiber length of less than about 2 mm, or about 0.3 mm to about 2 mm, or about 0.5 mm to about 1.5 mm. As used herein, fiber length is defined as “length-weighted average fiber length.” The fiber length distribution can be determined according to ISO 16065-2(2014). In some configurations, short cellulosic fibers can be obtained from hardwood pulp sources such as maple, oak, eucalyptus, poplar, beech, birch, paulownia, and mixtures thereof; non-wood fiber sources such as bamboo, hemp, acacia, wheat straw, rice straw, corn sheath, and mixtures thereof; and combinations of hardwood pulp sources and non-wood fiber sources. In some configurations, short cellulosic fibers can be obtained by chemical pulping processes such as kraft pulping, and / or mechanical pulping processes such as chemical thermomechanical pulping, stone crushed wood pulping, and / or pressure crushed wood pulping. In some configurations, short cellulosic fibers may have an average fiber diameter of about 0.01 mm to about 0.04 mm.
[0075] In some configurations, the cellulose pulp may contain short cellulosic fibers in amounts of approximately 25% to 70% by weight, or approximately 30% to 65% by weight, or approximately 35% to 60% by weight, or approximately 40% to 55% by weight, or approximately 45% to 50% by weight of the cellulose pulp, specifically including all 1% increments within the ranges listed above, and all ranges formed therein or by them. In some configurations, the cellulose pulp may contain short cellulosic fibers in amounts of approximately 25% to 100% by weight, or approximately 30% to 90% by weight, or approximately 50% to 75% by weight of the cellulose pulp, specifically including all 1% increments within the ranges listed above, and all ranges formed therein or by them. In some configurations, the cellulose pulp may contain approximately 25% to 50% by weight, or approximately 30% to 40% by weight, of short cellulosic fibers, specifically all 1% increments within the ranges listed above, and all ranges within or formed thereof.
[0076] In some configurations, cellulose pulp may contain coniferous fibers. As used herein, “coniferous fibers” refers to fibers obtained from coniferous pulp sources such as pine, fir, spruce, cedar, and combinations thereof. In some configurations, coniferous fibers may have an average fiber length of about 2.5 mm to about 6 mm. Cellulose pulp may contain coniferous fibers in amounts of about 30% to about 75% by weight, or about 35% to about 70% by weight, or about 40% to about 65% by weight of the cellulose pulp, specifically all 1% increments within the ranges listed above, and all ranges within or formed thereof.
[0077] In some configurations, the inner core layer may include a ratio of short cellulose fibers to superabsorbent particles of approximately 0.2 to approximately 4.5, or approximately 0.5 to approximately 1.5.
[0078] In some configurations, multiple cellulosic fibers in the inner core layer may penetrate the underside of the upper nonwoven layer. While not theoretically constrained, it is thought that the penetration of multiple cellulosic fibers into the underside of the upper nonwoven layer, and / or the interlacing of the cellulosic fibers with the polymer fibers of the upper nonwoven layer, may result in improved mechanical stability between the upper nonwoven layer and the inner core layer, which may help provide improved fluid transfer from the upper nonwoven layer to the inner core layer during storage.
[0079] Absorbent polymer materials for use in absorbent articles typically include water-insoluble, water-swellable, hydrogel-forming, cross-linked absorbent polymers that can absorb large amounts of liquid and retain such absorbed liquid under moderate pressure.
[0080] The absorbent polymer material for the absorbent core according to this disclosure may include superabsorbent particles, also known as “superabsorbent material” or “absorbent gelling material.” Typically, the absorbent polymer material in particulate form may be selected from polyacrylates and polyacrylate-based materials, such as partially neutralized crosslinked polyacrylates. The term “particles” refers to granules, fibers, flakes, spheres, powders, plates, and other shapes and forms known to those skilled in the art of superabsorbent particles. In some embodiments, the superabsorbent particles may be in the form of fibers, i.e., elongated needle-shaped superabsorbent particles.
[0081] In some structures, the inner core layer may contain cellulose pulp in an amount of about 50% to about 85% by weight, or about 55% to about 80% by weight, or about 60% to about 75% by weight of the inner core layer. The inner core layer may contain superabsorbent particles in an amount of about 15% to about 50% by weight, or about 20% to about 50% by weight, or about 25% to about 40% by weight, or about 30% to about 35% by weight of the inner core layer. In some configurations, the inner core layer may contain cellulose pulp in an amount of about 125 gsm to about 350 gsm. In some configurations, the inner core layer may contain superabsorbent particles in an amount of about 20 gsm to about 125 gsm.
[0082] In some configurations, the inner core layer may contain approximately 50% to 85% cellulose pulp and approximately 15% to 50% superabsorbent particles. The absorbent core structure has a density of approximately 0.045 g / cm³. 3 ~Approx. 0.15g / cm 3 , and / or 0.045 g / cm³ 3 ~0.12 g / cm³ 3 The absorbent article may have an average density of approximately 0.045 g / cm³. 3 ~Approx. 0.16g / cm 3 It may have an average density.
[0083] The absorbent core structure may be compressed after the compression process to restore its original shape. A suitable absorbent core structure requires little force to compress (low resistance), and the structure can restore its shape when the user periodically compresses it and releases the compressive force through various body movements. To achieve this, the structure maintains sufficient recovery energy after multiple periodic compressions. Without sufficient recovery energy, the structure may remain compressed and deformed due to insufficient force (stored energy) to recover.
[0084] The absorbent article 20 may be elastic and conformable, and can provide excellent comfort during use without substantially agglomeration and / or compression. The absorbent article can be subjected to bodily force and can almost return to its original state. The absorbent article has a bending strength of approximately 0.07 to 0.30 N / mm² when measured by wet and dry CD and MD three-point bending methods. 2 , or approximately 0.10 to approximately 0.25 N / mm 2 , or approximately 0.10 to approximately 0.20 N / mm 2 It may have a dry modulus of CD.
[0085] The absorbent article may have a dry caliper of approximately 2.0 mm to 6.0 mm, or approximately 2.0 mm to 4.5 mm, or approximately 2.5 mm to 4.0 mm, when measured according to the wet and dry CD and MD3-point method. In some configurations, the absorbent article has a dry caliper of approximately 0.07 to 0.30 N / mm² when measured according to the wet and dry CD and MD3-point method.2 The dry modulus of CD and dry caliper of approximately 2.0 mm to 4.5 mm, or approximately 0.10 to 0.25 N / mm 2 The CD dry modulus may be of a certain value and the dry caliper may be of approximately 2.5 mm to approximately 4.0 mm. The absorbent article has a dry modulus of approximately 7.0 to approximately 30.0 N when measured by the wet and dry CD and MD three-point bending method. * mm 2 , or approximately 10.0 to 25.0 N * mm 2 , or approximately 10.0 to 20.0 N * mm 2 , or approximately 13.0 to 20.0 N * mm 2 It may have the dry bending rigidity of CD.
[0086] Absorbent materials have a saturation of approximately 1.0 to 3.5 N. * mm, or approximately 1.5 to 3.0 N * mm, or approximately 1.5 to 2.8 N * It may have a fifth-cycle wet recovery energy of mm. Particularly preferred absorbent articles are about 1.0 to 3.5 N. * It may have a fifth-cycle wet recovery energy of mm and a fifth-cycle wet recovery percentage of approximately 29% to approximately 40%.
[0087] Absorbent articles containing absorbent core structures disclosed herein may also need to deliver a dry feel to the consumer after fluid addition, as measured by the light-touch re-wetting method. Absorbent core structures and absorbent articles that satisfy the above characteristics are designed to conform more closely and completely, comfortably and gently, to the wearer's complex anatomical genital shape. Thus, such absorbent articles may also need to be dry to the touch after excretion so as not to irritate sensitive genital tissue. Accordingly, absorbent articles described herein may also maintain a light-touch re-wetting value of less than about 0.15 grams, less than about 0.12 grams, or about 0 to about 0.15 grams, or about 0 to about 0.12 grams.
[0088] Top sheet The top sheet 110 may be formed from any suitable nonwoven web or molded film material. Referring again to the figure, the top sheet 110 is positioned adjacent to the wearer-facing surface of the absorbent article 20 and may be bonded to that surface and to the back sheet 130 by any suitable attachment or bonding method. The top sheet 110 and the back sheet 130 may be directly bonded to each other in the outer peripheral region around the absorbent core structure, or they may be indirectly bonded by directly bonding to the wearer-facing surface and the outer-facing surface of the absorbent article, or to any additional optional layer included in the absorbent article, respectively.
[0089] The absorbent article 20 may have any known or other effective top sheet 110, such as one that conforms to the wearer's skin, is soft to the touch, and is non-irritating. Preferred top sheet materials include liquid-permeable materials that are comfortable when in contact with the wearer's skin and allow discharged menstrual fluid to rapidly permeate through them. Some preferred examples of top sheet materials include laminated structures including films, nonwovens, film / nonwoven layers, film / film layers, and nonwoven / nonwoven layers.
[0090] Non-limiting examples of nonwoven web materials that may be suitable for use in forming the top sheet 110 include fibrous materials made from natural fibers, modified natural fibers, synthetic fibers, or combinations thereof. Several suitable examples are described in U.S. Patents No. 4,950,264, 4,988,344, 4,988,345, 3,978,185, 7,785,690, 7,838,099, 5,792,404, and 5,665,452.
[0091] The top sheet 110 may be adaptable, soft to the touch, and non-irritating to the wearer's skin. Furthermore, the top sheet 110 may be liquid permeable so that liquids (e.g., urine, menstrual blood) can easily penetrate its thickness. Some preferred examples of top sheet materials include laminated structures including films, nonwovens, film / nonwoven layers, film / film layers, and nonwoven / nonwoven layers. Other exemplary top sheet materials and designs are disclosed in U.S. Patent Applications Publications 2016 / 0129661, 2016 / 0167334, and 2016 / 0278986.
[0092] In some examples, the top sheet 110 may include tufts as described in U.S. Patents No. 8,728,049, No. 7,553,532, No. 7,172,801, No. 8,440,286, No. 7,648,752, and No. 7,410,683. The top sheet 20 may have a pattern of individual hair-like fibrils as described in U.S. Patent No. 7,655,176 or No. 7,402,723. Additional examples of preferred top sheet materials are described in U.S. Patents No. 8,614,365, No. 8,704,036, No. 6,025,535, and U.S. Patent Application Publication 2015 / 041640. Another preferred top sheet may be formed from a three-dimensional substrate as detailed in U.S. Patent Application Publication 2017 / 0258647. The top sheet may have one or more layers, as described in U.S. Patent Application Publications 2016 / 0167334, 2016 / 0166443, and 2017 / 0258651.
[0093] In some examples, the top sheet 110 may be formed from a spunbond web nonwoven web material comprising single-component continuous fibers, or alternatively, two-component or multi-component fibers, or a blend of single-component fibers spun from different polymer resins, or any combination thereof. The top sheet may also be a molded nonwoven top sheet, as disclosed in U.S. Patent Application Publication No. 2019 / 0380887.
[0094] To ensure that fluids in contact with the top surface (facing the wearer) of the top sheet move suitably and rapidly in the z-direction to the bottom surface (facing outward) of the top sheet, where they can be drawn into the absorbent layer, it may be important to ensure that the nonwoven web material forming the top sheet has an appropriate weight / volume density, thereby reflecting the suitable presence of pores (also called "pores") in and between the constituent fibers through which fluids can move within the nonwoven material. In some situations, a nonwoven with fibers that are too densely compacted may have an insufficient number and / or volume and / or size of pores, and the nonwoven will hinder rather than facilitate rapid downward z-direction fluid movement. On the other hand, a nonwoven with fibers that are too large and / or not compacted to provide a certain level of opacity (for the purpose of concealing fluids absorbed into the layer below) and a substantial appearance may be perceived negatively by the user.
[0095] The caliper of the top sheet material can be controlled to balance the conflicting needs of opacity and loft (requiring a higher caliper) and the limited z-direction distance required for the discharged fluid to travel through the top sheet from the wearer-facing surface to the outward-facing surface to reach the underlying absorbent core structure. Therefore, it may be desirable to control the production of top sheet materials to produce top sheet materials with calipers of approximately 0.20 mm to 1.0 mm, or approximately 0.25 mm to 0.80 mm, or approximately 0.30 mm to 0.60 mm.
[0096] In some configurations, the absorbent article does not need to include a separate top sheet, and the upper nonwoven fabric layer can function as the top sheet.
[0097] Secondary Top Sheet (STS) In some situations, the STS layer may be included between the top sheet and the absorbent core structure, allowing the absorbent core structure to readily receive the sudden discharge of fluid, and after receiving it, to draw it up along the x and y directions and distribute it across the absorbent core structure below.
[0098] If included, the STS may be a nonwoven fiber structure that may include cellulose fibers, noncellulose fibers (e.g., fibers spun from polymer resins), or blends thereof. To accommodate the folding and lateral gathering of the absorbent article 20 and the absorbent core structure 10, the STS may be formed from a relatively flexible (i.e., relatively low bending stiffness) material, as described herein.
[0099] Several specific examples of preferred STS compositions and structures, and combinations thereof with preferred topsheet compositions and structures, are described in U.S. Patent Applications Nos. 16 / 831,862, 16 / 831,854, 16 / 832,270, 16 / 831,865, 16 / 831,868, 16 / 831,870, and 16 / 831,879, and U.S. Provisional Patent Applications Nos. 63 / 086610 and 63 / 086701. Additional preferred examples are described in U.S. Patent No. 9,504,613, International Publication No. 2012 / 040315, and U.S. Patent Application Publication No. 2019 / 0021917.
[0100] In some configurations, the absorbent material may not include a secondary top sheet.
[0101] Back seat The backsheet 130 can be positioned beneath or adjacent to the outward-facing surface of the absorbent core structure 10 and can be bonded to that surface by any preferred mounting method. For example, the backsheet 130 can be fixed to the absorbent core structure 10 by a uniform, continuous layer of adhesive, a patterned layer of adhesive, or an arrangement of separate lines, spirals, or dots of adhesive. Alternatively, mounting methods may include thermal bonding, pressure bonding, ultrasonic bonding, dynamic mechanical bonding, or any other preferred mounting mechanism, or a combination thereof. In other examples, it is intended that the absorbent core structure 10 is not directly bonded to the backsheet 130.
[0102] The backsheet 130 may be impermeable to or substantially impermeable to aqueous liquids (e.g., urine, menstrual fluid) and may be manufactured from a thin plastic film, although other flexible liquid-impermeable materials may also be used. As used herein, the term “flexible” refers to a material that is adaptable and readily conforms to the general shape and contours of the human body. The backsheet 130 can prevent, or at least substantially prevent, the fluid absorbed and contained within the absorbent core structure 10 from escaping from and reaching articles of the wearer’s clothing that may come into contact with the absorbent articles 20, such as underwear and other clothing. However, in some examples, the backsheet 130 may be manufactured to allow vapors to escape from the absorbent core structure 10 (i.e., the backsheet is made to be breathable), while in other examples, the backsheet 130 may be manufactured not to allow vapors to escape (i.e., it is made to be non-breathable). Thus, the backsheet 130 may include a polymer film, such as a polyethylene or polypropylene thermoplastic film. Suitable materials for the backsheet 130 are, for example, thermoplastic films having a thickness of about 0.012 mm (0.5 mil) to about 0.051 mm (2.0 mil). Any suitable backsheet known in the art may be used in conjunction with the present invention.
[0103] Some preferred examples of materials suitable for forming a backsheet may include tufts as described in U.S. Patents No. 5,885,265, No. 4,342,314, and No. 4,463,045. Suitable single-layer breathable backsheets for use herein include, for example, those described in British Patents Nos. A2184389, A2184390, and A2184391, U.S. Patents No. 4,591,523, No. 3,989,867, and No. 3,156,242, International Publication No. 97 / 24097, U.S. Patents No. 6,623,464, No. 6,664,439, and No. 6,436,508.
[0104] The backsheet 130 may have two layers, as described in U.S. Patent No. 6,462,251: a first layer comprising a vapor-permeable perforated film layer and a second layer comprising a breathable microporous film layer. Other suitable examples of double or multilayer breathable backsheets for use herein include those described in U.S. Patents Nos. 3,881,489, 4,341,216, 4,713,068, 4,818,600, European Patent Application Publications Nos. 203821, 710471, 710472, and 0793952.
[0105] Other features In some configurations, the absorbent article 20 may include panty fastening components such as panty fastening adhesive or components of a hook-and-loop fastening system (such as VELCRO®).
[0106] In some configurations, the absorbent article 20 may include a panty-fastening adhesive disposed on the garment-facing side of the backsheet 130 to provide a mechanism for the user to adhere the absorbent article to the crotch area inside the underwear. The panty-fastening adhesive may include any adhesive or glue used in the art for such purposes. These adhesives are typically pressure-sensitive and maintain tackiness much lower than their application temperature. In some configurations, the panty-fastening adhesive may be a pressure-sensitive hot-melt adhesive. The panty-fastening adhesive may be applied in a pattern such as that described in U.S. Patent Application Publication 2020 / 0281782(A1). When the absorbent article 20 is packaged for transport, handling and storage before use, the panty-fastening adhesive may be covered with a protective cover (not shown), such as silicone-coated release paper, silicone-coated plastic film, or any other easily removable cover. The protective cover may be provided as a single piece or in multiple pieces to cover individual adhesive areas, such as on the backsheet and / or wings. The protective cover may cover / shield the adhesive deposit from contact with other surfaces until the user is ready to remove the protective cover for wearing / use and place the absorbent article in their underwear. The protective cover may also function as individual packaging for the article or provide a disposal function known in the art. Any commercially available release paper or film may be used. Preferred examples include BL 30 MG-A SILOX EI / O and BL 30 MG-A SILOX 4 P / O, available from Akrosil Corporation, and M&W film, available from Gronau, Germany, under code X-5432. In some configurations, the absorbent article may be packaged in a folded or tri-fold state.
[0107] In some configurations, the absorbent article 20 may include opposing wing portions 140, 150 on each side that extend laterally beyond the longitudinal edge of the absorbent portion of the absorbent article by a width dimension relatively larger than the width dimension of the front and rear portions of the absorbent article. Wings are now commonly provided on women's sanitary absorbent articles. As provided, they typically have an adhesive deposit applied to their outward-facing surface (the surface is outward before the absorbent article is placed in the user's underwear and the wings are applied). The wing portions may also include an adhesive deposit as described above, so that the user can wrap the wing portions around the inner edge through the leg opening of the underwear and adhere the wing portions to the outward-facing surface / underside of the underwear in the crotch area, providing auxiliary retaining support for the absorbent article and helping to protect the underwear from soiling in close proximity to the leg edge of the underwear.
[0108] package The absorbent articles of this disclosure may be packaged. The packages may include polymer film, paper, and / or other materials. Figures and / or markings relating to the properties of the absorbent articles may be formed, printed, positioned, and / or placed on the outer portion of the package. Each package may contain multiple absorbent articles. The absorbent articles may be packaged under compression to reduce the package size while still providing a sufficient amount of absorbent articles per package. By packaging the absorbent articles under compression, users and caregivers can easily handle and store the packages, particularly in bathrooms and other places with limited space, and at the same time, the reduced package size also provides manufacturers with reduced logistics costs. The packages may include polymer film containing recycled materials, for example, about 20% to about 100%, about 30% to about 90%, about 30% to about 80%, about 40% to about 60%, or about 50% recycled material. Recycled materials may include post-industrial recycled material (PIR) and / or post-consumer recycled material (PCR). In some cases, the polymer film used for packaging may include two outer layers and one or more inner layers. One or more inner layers may contain recycled material, or contain more recycled material than the outer layers. Recycled materials may include recycled polyethylene. Recycled materials may include recycled polyethylene PIR from cuts from packaging operations.
[0109] The packaging material may include paper, paper-based materials, paper with one or more barrier layers, or paper / film laminates. The packaging material may be in the range of about 50 gsm to about 100 gsm or about 70 gsm to about 90 gsm, and the one or more barrier layers may be in the range of about 3 gsm to about 15 gsm. With or without one or more barrier layers, the paper-based packaging material may exhibit a mechanical tensile strength of at least 5.0 kN / m, at least 3 percent mechanical expansion and contraction, at least 3 kN / m mechanical transverse tensile strength, and at least 4 percent transverse fracture expansion and contraction, as determined by ISO 1924-3.
[0110] Paper-based packaging materials, or paper-based packaging materials including a barrier layer or film, may be recyclable or recyclable in normal paper recycling operations. The degree of recyclability of paper-based packaging can be determined by the recyclability percentage. Paper-based packaging of the Disclosure may exhibit a recyclability percentage of 70 percent or more, 80 percent or more, or 90 percent or more. Paper-based packaging of the Disclosure may have a recyclability percentage of about 70 percent to about 99.9 percent, about 80 percent to about 99.9 percent, or about 90 percent to about 99.9 percent. For example, packaging materials of the Disclosure may exhibit a recyclability percentage of about 95 percent to about 99.9 percent, about 97 percent to about 99.9 percent, or about 98 percent to about 99.9 percent. The recyclability percentage of paper-based packaging can be determined by Category II testing PTS-RH:021 / 97 (draft October 2019), conducted by Papiertechnische Stiftung, located at Pirnaer Strasse 37, 01809 Heidenau, Germany. In another example, the paper-based packaging of this disclosure may show an overall "pass" test result when determined by Category II method PTS-RH:021 / 97 (draft October 2019). Any of the paper-based packaging may have opening features such as perforations and may also have handles.
[0111] Test method Target audience For any of the following methods in which not all constituent layers of the article are tested, the layer to be tested may be separated from the layers not being tested using cryospray as necessary.
[0112] Fracture strain method The force-displacement behavior of the specimen is measured on a universal constant-speed elongation test frame equipped with a load cell in which the measured force is within 1% to 99% of the cell's limit (a suitable instrument is the MTS Alliance with TestSuite Software, available from MTS Systems Corp. (Eden Prairie, MN), or an equivalent). The specimen is subjected to tensile elongation at a constant speed (mm / sec) until fracture, and the fracture strain percentage is measured. All tests are conducted in a controlled room at 23°C ± 3°C and 50% ± 2% relative humidity, and the test specimen is conditioned in this environment for at least 2 hours prior to testing.
[0113] The fixtures used to grip the test specimens are lightweight (<80 grams) vise-type clamps having gripping surfaces of semi-cylindrical steel versus rubber-coated steel, at least 40 mm wide. The fixtures are mounted on a universal test frame and aligned horizontally and vertically to one another.
[0114] Measurements are performed on test specimens taken from raw material rolls or sheets, or from material layers excised from absorbent articles. When excising material layers from absorbent articles, care is taken to avoid any contamination or deformation of the sample layer during the process. The excised layer should not contain any residual adhesive or fibers that may have migrated from the underlying layer. To ensure that all adhesive and migrated fibers are removed, the layer is immersed in a suitable solvent that dissolves the adhesive without adversely affecting the material itself and removes all present migrated fibers. One such solvent is THF (general-purpose tetrahydrofuran, CAS 109-99-9, available from any convenient source). After solvent immersion, the material layer is air-dried completely in a manner that prevents unwanted stretching or other deformation of the material. After the material is dry, test specimens are prepared as follows: The test specimens are cut from an area of the test material that does not contain folds or wrinkles. The test specimen is 100 mm long (parallel to the transverse axis of the article, or the intended transverse axis) and 25.4 mm wide (parallel to the longitudinal axis of the article, or the intended longitudinal axis). Similarly, five duplicate test specimens are prepared.
[0115] Prepare the universal test frame as follows: Set the initial grip separation distance to a nominal gauge length of 80 mm, then zero the crosshead. Program the test frame to bring the grips closer together by intentionally loosening them by 1 mm to ensure that there is no pre-tension in the specimen at the start of the test. (During this movement, the specimen loosens between the grips.) Next, move the grips apart at a loosening rate of 1 mm / s until the loosening preload exceeds 0.05 N. (At this point, use the crosshead position signal to calculate the looseness of the specimen, the adjusted gauge length, and define the strain as zero, i.e., 0.0). Next, move the grips apart at a rate of 1 mm / s until the specimen breaks or exceeds the instrument's extension limit.
[0116] The test is performed by inserting the specimen into the grip so that its long axis is parallel to the movement of the crosshead and positioned at the center of that movement. The test is started and force ("load") and displacement data are continuously collected at a data acquisition rate of 100 Hz.
[0117] Create a graph of load (N) versus displacement (mm). Determine the peak load from the curve, and then determine the fracture sensitivity as follows: Determine the crosshead position at which the load signal decreases by 75% after reaching the peak load, and record this as the final specimen length (Lf) in units of 0.01 mm. Define the initial specimen length by the crosshead position when the loosening preload of 0.05 N is exceeded, and record this value as the initial specimen length (Li) in units of 0.01 mm. Calculate the fracture strain percentage as follows and record it in the nearest 1 percent unit.
[0118] Fracture strain % = ((Lf - Li) / Li) * 100 Repeat this procedure for all five duplicate specimens in the same manner. Calculate the arithmetic mean of the fracture strain % of the five duplicate specimens and report it as fracture strain % in 1-percent increments.
[0119] Wet and dry CD and MD three-point bending method The bending properties of absorbent article test specimens are measured on a universal constant-speed elongation test frame equipped with load cells where the measured force is within 1% to 99% of the cell's limit (a suitable instrument is the MTS Alliance with TestSuite Software, available from MTS Systems Corp. (Eden Prairie, MN), or an equivalent). Tests are performed on both dry and wet specimens. The intention of this method is to simulate the deformation created in the xy plane by the wearer of an absorbent article during normal use. All tests are performed in a room adjusted to 23°C ± 3°C and 50% ± 2% relative humidity.
[0120] The bottom stationary fixture consists of two cylindrical bars made of polished stainless steel, each 3.175 mm in diameter and 110 mm in length, mounted at each end by frictionless rolling bearings. These two bars are mounted horizontally, aligned front to back and parallel to each other, with their upper radii aligned vertically, and rotate freely around the diameter of the cylinder by frictionless bearings. Furthermore, the fixture allows the two bars to move horizontally away from each other on the track, thus allowing a gap to be set between them while maintaining the orientation of the bars. The upper fixture consists of a third cylindrical bar, also made of polished stainless steel, similarly 3.175 mm in diameter and 110 mm in length, mounted at each end by frictionless rolling bearings. When in position, the bars of the upper fixture are parallel to the bars of the lower fixture and aligned front to back, and in the case of the lower fixture, are positioned centered between the bars. Both fixtures include integrated adapters suitable for fitting and securing in place at their respective positions on the universal test frame, so that the bars are perpendicular to the movement of the crossbeams of the test frame.
[0121] Set the gap ("span") between each bar of the lower fixture to 25mm ± 0.5mm (from the center of one bar to the center of the other), and align the center of the upper bar with the midpoint between each lower bar. Set the gauge (from the bottom of the upper bar to the top of the lower bar) to 1.0cm.
[0122] The thickness of the specimen ("caliper") is measured using a manual micrometer equipped with a pressure foot capable of applying a constant pressure of 0.1 psi ± 0.01 psi. The manual micrometer is a self-weight instrument with accurate readings to 0.01 mm. A suitable instrument is the Mitutoyo Series 543 ID-C Digimatic, available from VWR International, or an equivalent. The pressure foot is a circular, movable surface with a flat surface having a diameter of 25.4 mm or less. The specimen is supported by a horizontal, flat reference platform that is larger than the surface of the pressure foot and parallel to the surface of the pressure foot. Zero the micrometer relative to the horizontal, flat reference platform. Place the specimen on the platform and center it under the pressure foot. Lower the pressure foot by hand at a descent rate of 3 + 1 mm / s until the pressure of the entire weight is applied to the specimen. After 5 seconds, record the thickness as caliper in units of 0.01 mm.
[0123] The test fluid to be administered to the wet test specimen is prepared by adding 100.0 grams of sodium chloride (reagent grade, any convenient source) to 900 grams of deionized water in a 1-liter Erlenmeyer flask. Stir until the sodium chloride is completely dissolved.
[0124] Two hours prior to the test, absorbent article samples are conditioned at 23°C ± 3°C and 50% ± 2% relative humidity. Dry test samples are taken from an area of the sample free of seams, folds, or wrinkles, ideally from the center of the absorbent article (the intersection of the longitudinal and transverse centerlines). Dry test pieces are cut to a width of 50.8 mm along the CD (transverse direction, i.e., parallel to the transverse axis of the sample) and a length of 50.8 mm along the MD (parallel to the longitudinal axis of the sample), and prepared for MD (machine direction) bending by maintaining their orientation after cutting and marking the surface facing the body (or the surface intended to face the body in the finished product). The dried specimen is prepared for MD (machine direction) bending by cutting it to a width of 50.8 mm along the MD (transverse direction, i.e., parallel to the transverse axis of the sample) and a length of 50.8 mm along the CD (parallel to the longitudinal axis of the sample), maintaining their orientation after cutting, and marking the surface facing the body (or the surface intended to face the body of the finished product). The thickness of the specimen is measured as described herein and recorded as the dry specimen caliper in units of 0.01 mm. Next, the mass of the specimen is measured and recorded as the dry mass in units of 0.001 grams. Mass (g) is multiplied by the area (0.002581 m²). 2 The basis weight of the test specimen is calculated by dividing by ), and the dry basis weight of the test specimen is 0.01 g / m². 2 Record in units. Basis weight of the sample (g / m²) 2 The bulk density of the sample is calculated by dividing the given value by the sample thickness (mm), and then dividing the resulting quotient by 1000, resulting in a dry sample density of 0.01 g / cm³. 3 Record in units. Similarly, prepare five duplicate dry specimens. Remove the absorbent core so that it separates from the rest of the sample. Measure the thickness of the specimen as described herein and record it in units of 0.01 mm as the dry specimen caliper. Now measure the mass of the specimen and record it in units of 0.001 grams as the dry mass. Record the mass (g) over the area (0.002581 m²). 2 The basis weight of the absorbent core is calculated by dividing by ), and the dry basis weight of the absorbent core is 0.01 g / m². 2 Record in units. Absorbent core basis weight (g / m²) 2The average density of the absorbent core structure is calculated by dividing the given value by the thickness of the absorbent core (mm), and then dividing the quotient by 1000, resulting in a dry absorbent core density of 0.01 g / cm³. 3 Record in units. Similarly, prepare five replicated dry absorbent cores.
[0125] First, the wet test specimen is prepared in exactly the same manner as the dry test specimen, and then the test fluid is added immediately before testing as follows: First, the thickness and mass of the dry test specimen are measured as described herein and recorded as the initial thickness in units of 0.01 mm and the initial mass in units of 0.001 g. Next, the dry test specimen is completely immersed in the test fluid for 60 seconds. After 60 seconds, the specimen is removed from the test fluid and oriented vertically for 30 seconds to allow excess fluid to drip out. At this point, the thickness and mass of the wet test specimen are measured as described herein and recorded as the wet test specimen caliper in units of 0.01 mm and the wet test specimen mass in units of 0.001 g. If desired, the mass of the test fluid in the specimen is calculated by subtracting the initial mass (g) from the wet test specimen mass (g) and recorded as the test specimen fluid volume in units of 0.001 g. The wet test specimen must be tested within 10 minutes after being removed from the test fluid. Similarly, five duplicate wet test specimens are prepared.
[0126] The universal test frame for the deflection bending test is programmed so that the upper fixture moves downward relative to the lower fixture at a speed of 1.0 mm / second until the upper bar touches the top surface of the test specimen with a minimum force of 0.02 N, and then the crosshead is moved so that this continues for a further 12 mm. The crosshead is then immediately returned to its original position at a speed of 1.0 mm / second. Force (N) and displacement (mm) data are collected continuously at 100 Hz throughout the test.
[0127] The dry specimen is loaded so that its sides are parallel to each bar, straddling the two lower bars, and its center is positioned below the upper bar. For MD bending, the MD direction of the specimen is perpendicular to the length of the three bars. The test is started, and force and displacement data are collected continuously.
[0128] Create a graph of force (N) versus displacement (mm). From the graph, determine the maximum peak force and record it as the dry MD peak load in units of 0.01 N. Then, calculate the maximum slope of the curve between the initial force and the maximum force (in the loaded portion of the curve) and record it in units of 0.1. Calculate the modulus of elasticity as follows and record it as the dry MD modulus of elasticity of 0.001 N / mm². 2 Record in units.
[0129] CD or MD dry or wet flexural modulus (N / mm²) 2 ) = (slope × (span) 3 ) / (4 × sample width × (sample caliper 3 )) The bending stiffness was calculated as follows, and the dry MD bending stiffness was 0.1 Nmm. 2 Record in units.
[0130] CD or MD dry or wet bending stiffness (Nmm) 2 ) = modulus of elasticity × moment of inertia In the formula, moment of inertia (mm 4 ) = (sample width × caliper 3 )) / 12 Similarly, the procedure is repeated for all five copies of the dried test specimen. The arithmetic mean of the five duplicate dried test specimens is calculated for each parameter, and the dried test specimen "caliper" is calculated in units of 0.01 mm, 0.01 g / m². 2 The unit of measurement for the dry test piece basis weight is 0.001 g / cm². 3 Dry specimen density in units of 0.01 N, dry CD or MD peak load in units of 0.01 N / mm² 2 The dry CD or MD flexural modulus and Nmm in units of elasticity. 2 Report the bending stiffness in units of dry CD or MD.
[0131] Here, the entire procedure is repeated for all five copies of the wet test specimen, and the results are expressed as wet CD or MD peak load in units of 0.01 N, 0.001 N / mm². 2 Wet CD or MD flexural modulus in units, and Nmm 2 Report the wet CD or MD bending stiffness in units.
[0132] Wet and dry CD ultra-high sensitivity three-point bending method The CD (transverse) bending properties of the test specimen are measured using a highly sensitive three-point bending test on a universal constant-speed elongation test frame equipped with load cells suitable for the force to be measured (preferred equipment is the MTS Alliance using TestSuite Software available from MTS Systems Corp. (Eden Prairie, MN), or equivalent). The test is performed on both dry and wet specimens. The intention of this method is to simulate the deformation created in the xy plane by the wearer of absorbent material during normal use. All tests are performed in a room adjusted to 23°C ± 3°C and 50% ± 2% relative humidity.
[0133] The ultra-high-sensitivity three-point bending method is designed to maximize the force signal-to-noise ratio when testing materials with very low bending forces. The force signal is maximized by using a highly sensitive load cell (e.g., 5N), a small span (load is proportional to the cube of the span), and a wide specimen width (total measured load is directly proportional to the width). The fixture is designed so that the bending measurement is performed under tension, allowing the fixture mass to be kept to a minimum. Noise in the force signal is minimized by keeping the load cell stationary to reduce mechanical vibration and inertial effects, and by keeping the mass of the fixture attached to the load cell as small as possible.
[0134] Referring to Figures 12A to 12C, the load cell 1001 is mounted on the stationary crosshead of the universal test frame. The ultra-high sensitivity fixture 1000 consists of three thin blades constructed from a lightweight rigid material (such as aluminum or equivalent). Each blade has a thickness of 1.0 mm, a rounded edge, and a length capable of accommodating a bending width of 100 mm. Each blade has cavities 1004a and 1004b (outer blades) and 1005 (center blade) cut out along their horizontal edges to create a height h of 5 mm of blade material. The two outer blades 1003a and 1003b are mounted horizontally on the movable crosshead of the universal test frame, aligned parallel to each other, with their horizontal edges aligned vertically. The span s between the two outer blades 1003a and 1003b is 5 mm ± 0.1 mm (inner edge to inner edge). The central blade 1002 is mounted on a load cell on a fixed crosshead of the universal test frame. When in place, the central blade 1002 is parallel to the two outer blades 1003a and 1003b, with its center located midway between the outer blades 1003a and 1003b. The blade fixture includes a one-piece adapter suitable for fitting and securing the blade in place at each position on the universal test frame, so that the horizontal edge of the blade is perpendicular to the movement of the crossbeam of the universal test frame.
[0135] The test fluid to be administered to the wet test specimen is prepared by adding 100.0 grams of sodium chloride (reagent grade, any convenient source) to 900 grams of deionized water in a 1-liter Erlenmeyer flask. Stir until the sodium chloride is completely dissolved.
[0136] Two hours prior to the test, the sample is conditioned at 23°C ± 3°C and 50% ± 2% relative humidity. The dried test specimen is taken from an area of the sample free of seams, folds, or wrinkles. The dried test specimen is cut to a width of 50.0 mm along the CD (transverse direction, i.e., parallel to the transverse axis of the sample) and a length of 100.0 mm along the MD (machine direction, i.e., parallel to the longitudinal axis of the sample), and prepared for the CD bend (i.e., a bend perpendicular to the transverse axis of the sample) by maintaining their orientation after cutting and marking the surface facing the body (or the surface intended to face the body of the finished product). Five duplicate dried test specimens are prepared in the same manner.
[0137] First, prepare the wet test sample in exactly the same manner as the dry test sample, and then add the test fluid immediately before testing as follows: Immerse the dry sample completely in the test fluid for 60 seconds. After 60 seconds, remove the sample from the test fluid and orient it vertically for 30 seconds to allow excess fluid to drip out. After removing the wet test sample from the test fluid, it must be tested within 10 minutes. Similarly, prepare five duplicate wet test samples.
[0138] The universal test frame is programmed so that the movable crosshead moves in the opposite direction to the fixed crosshead at a speed of 1.0 mm / s. The crosshead movement begins with the specimen 1006 flat and unbiased on the outer blades 1003a and 1003b, continues with the inner horizontal edge of the cavity 1005 within the central blade 1002 in contact with the upper surface of the specimen 1006, and is followed by an additional 4 mm crosshead movement. The crosshead stops at 4 mm and then immediately returns to zero at a speed of 1.0 mm / s. Force (N) and displacement (mm) are collected throughout at 50 Hz.
[0139] Before placing specimen 1006, the outer blades 1003a and 1003b are moved toward the central blade 1002 until a clearance C of approximately 3 mm exists between the inner horizontal edges of cavities 1004a and 1004b within the outer blades 1003a and 1003b and the inner horizontal edge of cavity 1005 within the central blade 1002, and then pass through the central blade 1002 (see Figure 12C). Specimen 1006 is positioned within clearance C so as to straddle the inner horizontal edges of cavities 1004a and 1004b within the outer blades 1003a and 1003b, with the MD (short side) of the specimen perpendicular to the horizontal edge of the blade and the body-facing surface of the specimen facing upward. Specimen 1006 is placed at the center between the outer blades 1003a and 1003b. The outer blades 1003a and 1003b are slowly moved in the opposite direction to the fixed crosshead until the inner horizontal edge of the cavity 1005 within the central blade 1002 contacts the upper surface of the test specimen 1006. The test is started, and force and displacement data are collected continuously.
[0140] Plot the force (N) against the displacement (mm). Record the maximum peak force in units of 0.001N. Calculate the area under the curve from the start of loading to the maximum peak force and express it as bending energy of 0.001N. * Record in millimeters. Recovery energy is calculated as the area under the curve where the force is unloaded from the maximum peak to 0.0 N, and is 0.001 N. * The recovery energy is recorded in millimeters. Similarly, the entire test sequence is repeated for a total of five dry specimens and five wet specimens.
[0141] For each test specimen type (dry and wet), the arithmetic mean of the maximum peak force between similar specimens is calculated in units of 0.001 N and recorded as the dry peak load and wet peak load, respectively. For each test specimen type (dry and wet), the arithmetic mean of the bending energy of similar test specimens is calculated in units of 0.001 N. * The calculations are performed in millimeters and reported as dry bending energy and wet bending energy, respectively. For each specimen type (dry and wet), the arithmetic mean of the recovery energy of similar specimens is 0.001 N.* The calculations are performed in millimeters and reported as dry recovery energy and wet recovery energy, respectively.
[0142] Wet and dry cluster compression methods The cluster compression test measures the force-versus-displacement behavior of intentionally "clustered" absorbent article test samples over five cycles of load application ("compression") and load removal ("recovery") using a universal constant-speed elongation test frame (preferred equipment is MTS Alliance using TestSuite software available from MTS Systems Corp. (Eden Prairie, MN), or equivalent) equipped with load cells where the measured force is within 1% to 99% of the cell's limit. This test is performed on dry test samples as well as wet test specimens administered with a specific amount of test fluid. The intent of this method is to simulate the deformation that occurs in the z-plane of the crotch area or its components of an absorbent article when worn by a wearer during a sit-to-stand motion. All tests are performed in a controlled room at 23°C ± 3°C and 50% ± 2% relative humidity.
[0143] Figures 13 to 14B show the test apparatus. The bottom stationary fixture 3000 consists of two matching specimen clamps 3001, each 100 mm wide, and mounted on their respective movable platforms 3002a and 3002b. The clamps have a 110 mm long "knife edge" 3009 that grips a 1 mm thick hard rubber surface 3008. When closed, the clamps are flush with the inside of their respective platforms. The clamps are aligned to hold an unbunched specimen horizontally and perpendicular to the tensile axis of the tensile testing machine. The platforms are mounted on rails 3003, which allow them to be moved horizontally from side to side and locked in place. The rails have adapters 3004 that fit the tensile testing machine, which allow the platforms to be fixed horizontally and perpendicular to the tensile axis of the tensile testing machine. The upper fixture 2000 is a cylindrical plunger 2001 with a total length of 70 mm and a diameter of 25.0 mm. The contact surface 2002 is flat and not curved. The plunger 2001 has an adapter 2003 that is suitable for mounting a load cell, which allows the plunger to be fixed perpendicular to the tensile axis of the tensile testing machine.
[0144] The test specimen is prepared for at least 2 hours before testing at 23°C ± 3°C and 50% ± 2% relative humidity. Prepare the test specimen as follows: When testing an untouched absorbent article, remove any release paper from any panty fastening adhesive on the clothing-facing side of the article, if present. Lightly coat the adhesive with talc powder to reduce stickiness. If there is a cuff, cut it off with scissors, taking care not to disturb the top sheet or any other underlayers of the article. Place the article on a bench with the body-facing surface facing upwards. Mark the intersection of the longitudinal and transverse centerlines on the article. Using a rectangular cutting die or equivalent cutting means, cut the specimen 100 mm longitudinally and 80 mm transversely, centered at the intersection of the centerlines. When testing a material layer or layered component of an absorbent article, place the material layer or component on a bench and orient it as it would be incorporated into the finished product (i.e., identify the surface facing the body, the transverse axis, and the longitudinal axis). Using a rectangular cutting die or equivalent cutting means, cut the sample into sections of 100 mm longitudinal and 80 mm transverse, centered at the intersection of the centerlines. Measure the mass of the sample and record it in units of 0.001 g. Convert the mass (g) to the area (0.008 m²). 2 The basis weight of the sample is calculated by dividing by ), and the basis weight is 1 g / m². 2 Record in units.
[0145] The test specimens can be analyzed in both wet and dry conditions. No further preparation is required for dry specimens. The test fluid to be administered to the wet specimens is prepared by adding 100.0 grams of sodium chloride (reagent grade, any convenient source) to 900 grams of deionized water in a 1-liter Erlenmeyer flask. Stir until the sodium chloride is completely dissolved. A total of 7 mL of the test solution is administered to the wet specimens, as detailed below.
[0146] Add the liquid using a graduated Eppendorf pipette, spreading the fluid over the entire surface of the sample facing the body within approximately 3 seconds. Test the wet sample for 10.0 minutes ± 0.1 minutes after application of the prescribed dosage.
[0147] The tensile testing machine is programmed to zero the load cell, then the upper device is lowered at 2.00 mm / sec until the plunger's contact surface touches the specimen and the load cell reading is 0.02 N. The crosshead is then zeroed. The system is programmed to lower the crosshead by 15.00 mm at a speed of 2.00 mm / sec, and immediately raise it by 15.00 mm at a speed of 2.00 mm / sec. This cycle is repeated for a total of 5 cycles without delay between cycles. Data is collected at 50 Hz during all compression / decompression cycles.
[0148] Position the left platform 3002a 2.5 mm from the side of the upper plunger (distance 3005). Fix the position of the left platform. This platform 3002a remains stationary during the experiment. Align the right platform 3002b 50.0 mm from the stationary clamp (distance 3006). Raise the upper probe 2001 so that it does not obstruct the mounting of the specimen. Open both clamps 3001. Referring to Figure 14A, place the dry specimen so that its longitudinal edge (i.e., the 100 mm long edge) is inside the clamp. Align the lateral center of the dry specimen and firmly secure both edges inside the clamp. Referring to Figure 14B, move the right platform 3002b 20 mm toward the stationary platform 3002a so that a 30.0 mm separation is achieved between the left and right clamps. When the movable platform is positioned, ensure that the dry specimen is curved upwards. Here, manually lower probe 2001 until it is approximately 1 cm above the top of the specimen with the curved lower surface.
[0149] The test is initiated, and force (N) and displacement (mm) data are continuously collected over all five cycles. A force (N) versus displacement (mm) graph is created individually for each cycle. A representative curve is shown in Figure 15A. From the curve, the maximum dry compressive force for each cycle is determined in units of 0.01 N, then multiplied by 101.97, and recorded in units of 1 wt gram. The dry recovery % between the first and second cycles is calculated as (TD-E2) / (TD-E1)×100 (where TD is the total displacement and E2 is the extension in the second compression curve exceeding 0.02 N), and recorded in units of 0.01%. In the same manner, the dry recovery rate % between the first cycle and the other cycles is calculated as (TD-E1) / (TD-E1)×100, and recorded in units of 0.01%. Referring to Figure 15B, the dry compressive energy for cycle 1 is calculated as the area under the compression curve (i.e., area A+B), which is 0.1 N. * Record in millimeters. Calculate the dry energy loss for cycle 1 as the area between the compression curve and the decompression curve (i.e., area A), and set it to 0.1 N. * Record in millimeters. Calculate the drying recovery energy for cycle 1 as the area under the decompression curve (i.e., area B), and value it as 0.1 N. * Record in millimeters. Similarly, for each of the other cycles, record the dry compression energy (N). * (mm), drying energy loss (N) * mm), and drying recovery energy (N * Calculate mm) and 0.1N * Record in millimeters. Similarly, analyze a total of five duplicate dried specimens and report the arithmetic mean of the five dried specimens for each parameter as described above, including basis weight.
[0150] Here, the entire procedure is repeated for a total of five replicated wet specimens, with the maximum wet compressive force in 1 gram force unit for each cycle and 0.1 N for each cycle. * Wet compression energy in millimeter units, 0.1N for each cycle. * Wet energy loss in millimeters, 0.1N per cycle *The results for each of the five cycles are reported as the arithmetic mean of five wet replications for the wet recovery energy in millimeters and the wet recovery percentage for each cycle. Of particular importance are the wet recovery energy and wet recovery percentage characteristics of the fifth cycle from this test method.
[0151] CD periodic stretching method up to 3% distortion The periodic tensile and recovery responses of absorbent material specimens are measured over 10 cycles of load application ("extension") and load removal ("recovery") using a universal constant-rate elongation test frame. The specimen is repeated 10 times up to 3% engineering strain, and then returned to zero engineering strain. For each cycle, stiffness, peak load, normalized peak energy, normalized recovery energy, strain at the start of the cycle, and strain at the end of the cycle (i.e., "permanent strain") are calculated and reported. The intent of this method is to understand the ability of a sample to be stretched in the xy plane as a result of a force on the body and then to recover to their original state. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the specimens are conditioned in this environment for at least 2 hours prior to testing.
[0152] A suitable universal constant-speed elongation test frame is an MTS Alliance or equivalent interfaced to a computer running TestSuite control software (available from MTS Systems Corp, Eden Prairie, MN). The universal test frame is equipped with load cells in which the force to be measured is within 1% to 99% of the cell's limit. The fixtures used to grip the test specimen are lightweight (<80 grams) vise-acting clamps with knife or serrated edge gripping surfaces of at least 40 mm width. The fixtures are mounted on the universal test frame and positioned horizontally and vertically relative to one another.
[0153] Measurements are performed on test specimens taken from raw material rolls or sheets, or from material layers excised from absorbent articles. When excising material layers from absorbent articles, care is taken to avoid any contamination or deformation of the sample layer during the process. The excised layer should not contain any residual adhesive or fibers that may have migrated from the underlying layer. To ensure that all adhesive and migrated fibers are removed, the layer is immersed in a suitable solvent that dissolves the adhesive without adversely affecting the material itself and removes all present migrated fibers. One such solvent is THF (general-purpose tetrahydrofuran, CAS 109-99-9, available from any convenient source). After solvent immersion, the material layer is air-dried completely in a manner that prevents unwanted stretching or other deformation of the material. After the material is dry, test specimens are obtained. Test specimens are cut from an area of the test material that does not have any remaining folds or wrinkles. The test specimen is approximately the same length as the transverse length of the article (parallel to the transverse axis of the article, or the intended transverse axis of the article). When cutting test specimens from absorbent articles of different sizes and widths, the total length of the test specimen (L) total ) may vary from product to product, and therefore the results are normalized to compensate for this variation. The test specimen has a width of 25.4 mm (parallel to the longitudinal axis of the article or the intended longitudinal axis). Test specimen width (w) = 25.4 mm. Total test specimen length (L total Measure the distance and record it in 0.1 mm increments. Prepare five duplicate specimens in the same manner.
[0154] The thickness (t) of the specimen is measured using a manual micrometer equipped with a clamp capable of applying a steady pressure of 0.1 psi ± 0.01 psi. The manual micrometer is a self-weight instrument with accurate readings to 0.01 mm. A suitable instrument is the Mitutoyo Series 543 ID-C Digimatic, available from VWR International, or an equivalent. The clamp is a circular movable surface with a flat surface having a diameter of 25.4 mm or less. The specimen is supported by a horizontal, flat reference platform that is larger than the surface of the clamp and parallel to the surface of the clamp. Zero the micrometer relative to the horizontal, flat reference platform. Place the specimen on the platform and center it under the clamp. Lower the clamp by hand at a descent rate of 3 + 1 mm / s until the pressure of the entire weight is applied to the specimen. After 5 seconds, record the thickness as the specimen thickness (t) in units of 0.01 mm.
[0155] Prepare the universal test frame as follows: Set the initial grip separation distance to a nominal gauge length (L) that is shorter than the total length of the test specimen. nominal Set to (i.e., L) so that the test specimen can be securely gripped at both ends. nominal <L total Next, the crosshead is set to zero. The test frame is programmed to bring the grips closer together by intentionally loosening them by 1 mm to ensure that there is no pre-tension in the specimen at the start of the test. (During this movement, the specimen loosens between the tensile grips.) The grips are then moved apart at a loosening rate of 1 mm / s until the loosening preload exceeds 0.05 N. At this point, the following occurs: 1) The crosshead position signal (mm) is set to the loosening of the specimen (L slack ) is defined as follows: 2) The initial test specimen gauge length (L0) is defined as nominal gauge length + looseness L0 = L nominal +L slackis calculated as. The unit here is millimeter. 3) Set the crosshead elongation (ΔL) to zero (0.0 mm). 4) Set the crosshead displacement (mm) to zero (0.0 mm). At this position, the engineering strain is zero, that is, 0.0. Engineering strain is calculated as the change in length (ΔL) divided by the initial length (L0). Engineering strain = ΔL / L0. For one test cycle, the grips move apart at an initial speed of 1 mm / sec until the engineering strain endpoint of 0.03 mm / mm is exceeded, and immediately thereafter, the grips move toward each other at an initial speed of 1 mm / sec until the crosshead signal is below the 0 mm crosshead return position. The test cycle is repeated until a total of 10 cycles are completed.
[0156] The test is performed by inserting the test specimen into the grips such that the long axis of the test specimen is parallel to the movement of the crosshead and centered in that movement. Start the test and continuously collect time, force and displacement data at a data acquisition rate of 100 Hz.
[0157] A graph of load (N) versus displacement is generated for all 10 cycles. For each cycle, perform the following. Record the peak load in units of 0.01 N. As the area under the load versus displacement curve from the start of the cycle to the strain endpoint of 0.03 mm / mm (during the load portion of the cycle), the peak energy (E peak ) is calculated and recorded in units of 0.01 N·mm. As the area under the load versus displacement curve from the strain endpoint of 0.03 mm / mm to the crosshead return of 0 mm (during the unloading portion of the cycle), the return energy (E return ) is calculated and 0.01 N * recorded as recovery energy in mm units. As the peak energy divided by the initial length, the normalized peak energy (NE peak ) is calculated (NE peak = E peak / L0) and recorded in units of 0.01 mN. As the return energy divided by the initial length, the normalized return energy (NE return ) is calculated (NE return = E returnRecord in units of 0.01 mN (L0). NE peak and NE return The unit is millinewtons (mN).
[0158] Here, we create a graph of engineering stress (σ) versus engineering strain for all 10 cycles, and perform the following for each cycle: N / mm 2 The engineering stress in units of σ is calculated by dividing the load by the cross-sectional area of the specimen, where the cross-sectional area is the width (w) multiplied by the thickness (t) of the specimen (σ = load / (w × t)). The modulus of elasticity, or the slope of the stress-strain curve, is determined for the line between the point of minimum force and the point of maximum force (between the loaded parts of the cycle), and the modulus of elasticity is recorded in units of 0.01 N / mm. The stiffness is calculated by multiplying the modulus of elasticity by the thickness of the specimen, and the tensile stiffness is recorded in units of 0.01 N / mm. The strain of the specimen at the start of the cycle is defined as the strain when the slack preload exceeds 0.05 N for that cycle (between the loaded parts of the cycle), and the initial cycle strain is recorded in units of 0.01 mm / mm. The strain of the specimen at the end of the cycle is defined as the strain when the load falls below 0.05 N for that cycle (between the unloading parts of the cycle), and the permanent strain is recorded in units of 0.01 mm / mm. Similarly, repeat the entire procedure for all five copies.
[0159] The arithmetic mean of five replicated specimens is calculated for each of the 10 cycles for each parameter and reported as peak load in 0.01 N units, normalized energy versus peak in 0.01 mN units, normalized recovery energy in 0.01 mN units, tensile stiffness in 0.01 N / mm units, initial cycle strain in 0.01 mm / mm units, and permanent strain in 0.01 mm / mm units.
[0160] Method for measuring the spacing and area of structural joint site patterns The spacing between inconspicuous structural joints used to create a quilt-like pattern on an absorbent material sample, and the total area occupied by these elements in a specific region of the sample, are measured on an image of the absorbent material sample acquired using a flatbed scanner. The scanner can scan in reflectance mode at a resolution of 2400 dpi and 8-bit grayscale. A suitable scanner is the Epson Perfection V750 Pro from Epson America Inc. (Long Beach, CA, USA) or an equivalent. The scanner is connected to a computer running an image analysis program. A suitable program is ImageJ v.1.52 (National Institute of Health, USA) or an equivalent. The sample image is distance-calibrated against an acquired NIST-certified ruler image. To allow for maximum contrast, the test specimen is backed with a uniformly colored opaque black background before image acquisition. All tests are performed in a humidified room maintained at approximately 23±2°C and approximately 50±2% relative humidity.
[0161] Prepare the test specimen as follows: Remove the absorbent article from its packaging. If the article is folded, gently unfold it and smooth out all wrinkles. If wings are present, extend them, but leave the release paper intact. Prepare the test specimen for approximately 2 hours before testing at approximately 23°C ± 2°C and approximately 50% ± 2% relative humidity.
[0162] The image is obtained as follows: The ruler is placed on the scanner bed so that it is oriented parallel to the side of the scanner glass. The image of the ruler (calibration image) is acquired in reflective mode at a resolution of 2400 dpi (approximately 94 pixels / mm) and 8-bit grayscale. The calibration image is saved as an uncompressed TIFF format file. After acquiring the calibration image, the ruler is removed from the scanner glass and the test specimen is scanned under the same scanning conditions as follows: The test specimen is placed in the center of the scanner glass and, if necessary, secured so that the body-facing surface of the specimen is flat against the scanner's glass surface. The specimen is oriented so that the entire specimen is within the glass surface. A black background is placed over the specimen, the scanner lid is closed, and a scan image of the entire specimen is acquired using the same settings as used for the calibration image. The specimen image is saved as an uncompressed TIFF format file.
[0163] The sample image is analyzed as follows: The calibration image file is opened in the image analysis program, and the image resolution is calibrated using an embossed ruler to determine the number of pixels per millimeter. Next, the sample image is opened in the image analysis program, and the distance scale is set using the image resolution determined from the calibration image. Then, the pattern of embossed elements present on the sample in the image is visually inspected, and the zones of the pattern to be analyzed are identified. For example, an absorbent article can be divided into three equally lengthed zones in the machine direction, such as Zone 1, which is the front 1 / 3 zone; Zone 2, which is the middle 1 / 3 zone; and Zone 3, which is the edge 1 / 3 zone. Using the image analysis tool, the shape is drawn along the perimeter of the first inconspicuous zone to be analyzed. The area of this first zone is measured, and the total area of Zone 1 is 0.01 mm². 2 Record in units of 0.01 mm. Here, measure the area of individual inconspicuous embossed elements located inside the perimeter of Zone 1 as follows: Draw the smallest possible boundary circle around each embossed element so that no part of the embossed element lies outside the boundary circle. Next, measure the area of the boundary circle of that embossed element and record the embossed element area as 0.01 mm. 2Record in units of 0.01 mm. Similarly, measure the area of each embossed element, including the portion of the embossed element located within Zone 1, and record each in units of 0.01 mm. 2 Record in units. Here, the area of all embossed elements within Zone 1 is summed up, and the total embossed element area of Zone 1 is 0.01 mm². 2 Record in units of 0.01 mm. Divide the total embossed element area of Zone 1 by the total area of Zone 1, then multiply by 100 and record as the percentage of the total area of Zone 1 represented by the embossed elements. Measure the spacing between each inconspicuous embossed element inside Zone 1 as follows: Measure the distance from the center of the minimum boundary circle drawn around an inconspicuous embossed element inside Zone 1 to the center of the minimum boundary circle drawn around the nearest adjacent inconspicuous embossed element inside Zone 1, as described herein, and record this distance as the embossed spacing in units of 0.01 mm. Repeat this process for all adjacent embossed elements inside Zone 1, recording each distance in units of 0.01 mm. Next, calculate the arithmetic mean of all measured embossed spacings between the nearest adjacent elements inside Zone 1 and record it as the Zone 1 embossed spacing in units of 0.01 mm.
[0164] Similarly, the entire procedure is repeated for each additional zone containing embossed elements present on the test sample, and these zones are labeled accordingly as Zone 2, Zone 3, etc.
[0165] Nonwoven fabric thickness-pressure method The thickness of the test specimen is measured as the distance between the reference platform on which the test specimen is placed and the presser that applies a specific amount of pressure to the test specimen over a specific period of time. For the purposes of this specification, the thickness is measured under two different confinement pressures (7 g / cm²). 2 and 70g / cm³ 2 The measurements are taken and reported. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity, and the test specimens are conditioned in this environment for at least 2 hours before testing.
[0166] The thickness is determined by a constant pressure (7g / cm²). 2 and 70g / cm³ 2The measurement is performed using a manual micrometer equipped with a clamp capable of applying pressure to the test specimen. The manual micrometer is a self-weight instrument with accurate readings to 0.01 mm. A suitable instrument is the Mitutoyo Series 543 ID-C Digimatic, available from VWR International, or an equivalent. The clamp is a flat, grounded, circular movable surface with a diameter smaller than the test specimen and capable of applying the required pressure. A suitable pressure foot has a diameter of 25.4 mm, but smaller or larger clamps can be used depending on the size of the test specimen being measured. The test specimen is supported by a horizontal, flat reference platform that is larger than the surface of the clamp and parallel to the surface of the clamp. The system is calibrated and operated according to the manufacturer's instructions.
[0167] Measurements are performed on test specimens taken from raw material rolls or sheets, or from material layers excised from absorbent articles. When excising material layers from absorbent articles, care is taken to avoid any contamination or deformation of the sample layer during the process. The excised layer should not contain any residual adhesive or fibers that may have migrated from the underlying layer. To ensure that all adhesive and migrated fibers are removed, the layer is immersed in a suitable solvent that dissolves the adhesive without adversely affecting the material itself and removes all present migrated fibers. One such solvent is THF (general-purpose tetrahydrofuran, CAS 109-99-9, available from any convenient source). After solvent immersion, the material layer is air-dried completely in a manner that prevents unwanted stretching or other deformation of the material. After drying, the test specimen must be obtained from an area free of folds or wrinkles and larger than the presser foot.
[0168] 7g / cm 2To measure the thickness at the confinement pressure, first zero the micrometers against a horizontal, flat reference platform. Place the specimen on the platform with the test position centered under the clamp. Gently lower the clamp at a rate of 3.0 mm ± 1.0 mm / sec until the full pressure is applied to the specimen. After waiting 5 seconds, record the thickness of the specimen in 0.01 mm increments. Repeat the same process for a total of 10 duplicate specimens. 7 g / cm 2 The arithmetic mean of all thickness measurements obtained at the confinement pressure was calculated to be 7 g / cm². 2 The thickness should be reported in units of 0.01 mm.
[0169] 70g / cm 2 To measure the thickness at the confinement pressure, first zero out the micrometers against a horizontal, flat reference platform. Place the specimen on the platform with the test position centered under the clamp. Gently lower the clamp at a rate of 3.0 mm ± 1.0 mm / sec until the full pressure is applied to the specimen. After waiting 5 seconds, record the thickness of the specimen in 0.01 mm increments. Repeat similarly for a total of 10 duplicate specimens. 70 g / cm 2 The arithmetic mean of all thickness measurements obtained at the confinement pressure was calculated to be 70 g / cm². 2 The thickness should be reported in units of 0.01 mm.
[0170] Light touch re-wetting method The light-touch re-wetting method quantitatively measures the mass of liquid that emerges from a test sample of an absorbent article that has been administered a specific amount of artificial menstrual fluid (AMF) (as described herein) when weight is applied over a specific period of time. All measurements are performed in a laboratory maintained at 23°C ± 2°C and 50% ± 2% relative humidity.
[0171] The test sample is administered using a syringe pump equipped with a disposable syringe. A suitable pump is a Perfusor® Compact S (available from B. Braun) or equivalent, which must be capable of accurately dispensing AMF at a rate of 42 mL / min. The disposable syringe is of sufficient capacity (e.g., BD Plastipak 20 mL) and is connected to a flexible tube with a 3 / 16 inch bore (e.g., Original Perfusor® Line, available from Braun, or equivalent). The AMF is prepared as described herein and brought to room temperature (23°C ± 2°C) before use in this test. Before starting the measurement, the syringe is filled with AMF, the flexible tube is primed with the liquid, and the dispensing rate (42 mL / min) and administration volume (4.0 mL + 0.05 mL) are verified according to the manufacturer's instructions. The flexible tube is then mounted so that it is oriented perpendicularly over the test sample and the distance between the tip of the tube and the surface of the test sample is 19 mm. It is important to note that the AMF must be withdrawn from the syringe every 15 minutes and thoroughly mixed.
[0172] The re-wetting weight assembly consists of an acrylic plate and stainless steel weights. The acrylic plate has dimensions of 65mm x 80mm and a thickness of approximately 5mm. Together with the acrylic plate, the stainless steel weights have a total mass of 2 pounds (907.19g) and apply a pressure of 0.25 psi below the surface of the acrylic plate.
[0173] For each test sample, five sheets of filter paper measuring 4 inches x 4 inches are used as the re-wetted substrate. Before testing, the filter paper is conditioned at 23°C ± 2°C and 50% ± 2% relative humidity for at least 2 hours. Suitable filter paper has a basis weight of approximately 139 gsm, a thickness of approximately 700 micrometers, and an absorption rate of approximately 1.7 seconds, and is available from Ahlstrom-Munksjo North America LLC (Alpharetta, GA) and VWR International as Ahlstrom Grade 989 or equivalent.
[0174] Prepare the test samples as follows: Before testing, the test samples are conditioned at 23±2°C and 50%±2% relative humidity for at least 2 hours. Remove the test samples from all packaging, taking care not to press down on or pull the product during handling. Place the test sample horizontally on a hard, flat surface and gently straighten any folds. Determine the test position as follows: For symmetrical samples (i.e., the front side of the sample is the same shape and size as the rear side of the sample when divided laterally along the midpoint of the longitudinal axis of the sample), the test position is the intersection of the midpoint of the longitudinal axis and the midpoint of the transverse axis of the sample. For asymmetrical samples (i.e., the front side of the sample is not the same shape and size as the rear side of the sample when divided laterally along the midpoint of the longitudinal axis of the sample), the test position is the intersection of the midpoint of the longitudinal axis of the sample and the transverse axis located at the midpoint of the wing of the sample. Prepare a total of three test samples.
[0175] Place the test sample horizontally on a flat, hard surface, and position the previously identified test position directly below the tip of the flexible tube. Adjust the height of the tube so that it is 19.0 mm above the surface of the test sample. Start the pump and dispense 4.0 mL + 0.05 mL of AMF at a rate of 42 mL / min. As soon as the AMF is completely dispensed, start a 10-minute timer. At this point, obtain the mass of five sheets of filter paper and record it as the dry mass in units of 0.001 grams. After 10 minutes, place five pre-baked sheets of filter paper on the test sample, centering the stack above the dispensing position. Next, place the acrylic plate centered on top of the filter paper so that its long side is parallel to the longitudinal axis of the test sample. Then, carefully lower the stainless steel weight into the center of the acrylic plate and immediately start a 30-second timer. After 30 seconds, gently remove the re-wetting weight and acrylic plate and set them aside. Obtain the mass of five sheets of filter paper and record it as the wet mass in units of 0.001 grams. Subtract the dry mass from the wet mass of the filter paper and record the re-wetting result in units of 0.001 grams. Before testing the next sample, wipe off any remaining test liquid from the bottom of the acrylic plate. Repeat the same procedure for a total of three duplicate test samples.
[0176] The arithmetic mean of re-wetting between three replicated test samples is calculated and reported as "light touch re-wetting" in units of 0.001 g.
[0177] Preparation of artificial menstrual fluid (AMF) Artificial menstrual fluid (AMF) is composed of a mixture of defibrous sheep blood, phosphate-buffered saline, and mucus components. AMF is prepared to have a viscosity of 7.15–8.65 centistokes at 23°C.
[0178] The viscosity of AMF is measured using a low-viscosity rotational viscometer (a suitable instrument is a Cannon LV-2020 Rotary Viscometer with a UL adapter (Cannon Instrument Co. (State College, PA)) or equivalent). A spindle of the appropriate size for the viscosity range is selected, and the instrument is operated and calibrated according to the manufacturer's instructions. Measurements are taken at 23°C ± 1°C and 60 rpm. Results are reported in 0.01 centistokes units.
[0179] Reagents required for AMF preparation include defibrotic sheep blood with a hematocrit value of 38% or higher (collected under sterile conditions, available from Cleveland Scientific, Inc. (Bath, OH) or equivalent), gastric viscous (crude form, sterile, available from American Laboratories, Inc. (Omaha, NE) or equivalent) with a target viscosity of 3-4 centistokes when prepared as a 2% aqueous solution, 10% v / v lactic acid aqueous solution, 10% w / v potassium hydroxide aqueous solution, dibasic anhydrous sodium phosphate (reagent grade), sodium chloride (reagent grade), monobasic monohydrate sodium phosphate (reagent grade), and distilled water (each available from VWR International or equivalent sources).
[0180] Phosphate-buffered saline consists of two individually prepared solutions (Solution A and Solution B). To prepare 1 L of Solution A, add 1.38 ± 0.005 g of monobasic sodium phosphate monohydrate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the container volume. Mix thoroughly. To prepare 1 L of Solution B, add 1.42 ± 0.005 g of dibasic anhydrous sodium phosphate and 8.50 ± 0.005 g of sodium chloride to a 1000 mL volumetric flask and add distilled water to the container volume. Mix thoroughly. To prepare phosphate-buffered saline, add 450 ± 10 mL of Solution B to a 1000 mL beaker and stir slowly on a stirring plate. Insert a calibrated pH probe (with an accuracy of 0.1) into the beaker of solution B, and while stirring, add a sufficient amount of solution A to adjust the pH to 7.2 ± 0.1.
[0181] The mucus component is a mixture of phosphate-buffered saline, potassium hydroxide aqueous solution, gastric viscous, and lactic acid aqueous solution. The amount of gastric viscous added to the mucus component directly affects the final viscosity of the prepared AMF. To determine the amount of gastric viscous required to obtain AMF within the target viscosity range (7.15–8.65 centistokes at 23°C), three batches of AMF with varying amounts of gastric viscous in the mucus component are prepared, and then a linear fit is performed using the least-squares method through the three points to interpolate the exact required amount from the concentration-viscosity curve. A good range for gastric viscous is usually 38–50 grams.
[0182] To prepare approximately 500 mL of mucus component, add 460 ± 10 mL of pre-prepared phosphate-buffered physiological water and 7.5 ± 0.5 mL of 10% w / v potassium hydroxide aqueous solution to a 1000 mL sturdy glass beaker. Place this beaker on a stirring hot plate and heat it to 45°C ± 5°C while stirring. Weigh the specified amount of gastric viscous (±0.50 g) and gently sprinkle it into the pre-prepared liquid at 45°C to prevent condensation. Cover the beaker and continue mixing. Maintain the temperature of this mixture above 50°C but not above 80°C for 15 minutes. Continue heating for 2.5 hours while gently stirring, maintaining this temperature range. After 2.5 hours, remove the beaker from the hot plate and allow it to cool to below 40°C. Next, add 1.8 ± 0.2 mL of 10% v / v lactic acid aqueous solution and mix thoroughly. Autoclave the mucilage mixture at 121°C for 15 minutes, then allow to cool for 5 minutes. Remove the mucilage mixture from the autoclave and stir until the temperature reaches 23°C ± 1°C.
[0183] Adjust the temperature of the sheep blood and mucus components to 23°C ± 1°C. Using a 500 mL graduated cylinder, measure the total volume of the pre-prepared mucus component batch and add this volume to a 1200 mL beaker. Add an equal volume of sheep blood to the beaker and mix thoroughly. Using the viscosity method described above, confirm that the viscosity of the AMF is 7.15–8.65 centistokes. If not, discard the batch and prepare another batch by adjusting the mucus components as needed.
[0184] Certified AMF should be refrigerated at 4°C unless intended for immediate use. AMF can be stored in an airtight container at 4°C for up to 48 hours after preparation. Before testing, AMF should be brought to 23°C ± 1°C. Any unused portion should be discarded after testing is complete.
[0185] Examples / Data The following data and examples, including comparative examples, are provided to aid in the description of the upper nonwoven layer and lower nonwoven layer, and / or absorbent articles, as described herein. The exemplified structures are provided for illustrative purposes only and many modifications thereto are possible without departing from the spirit and scope of this disclosure, and should not be construed as limiting the invention.
[0186] Testing of nonwoven fabric layer materials A series of measurements are performed on the nonwoven material to evaluate the ability of the material to function as the upper and / or lower nonwoven layer in the absorbent core structure described herein. Samples A to G are examples according to this disclosure. Comparative sample H is a comparative example. Samples A to G and comparative sample H are listed in Table 1 below.
[0187] Samples A-G and comparative sample H were evaluated according to the CD periodic stretching method up to 3% strain, the fracture strain method, the wet and dry CD ultra-high sensitivity three-point bending method, and the nonwoven fabric thickness-pressure method. The results are shown in Table 2.
[0188] [Table 1] 1 Available from Xiamen Yanjan New Material Co. (China) as ATB Z87G-40. 2 Available from Sandler GmbH (Germany) as Sawasoft (registered trademark) 53FC041001. 3 Available from Sandler GmbH (Germany) as Sawasoft® 553FC041005 (Option 82). 4 Available as Aura20 from Xiamen Yanjan New Material Co. (China). 5 Available from Jacob Holms Industries (Germany) as S25000541R01. 6PFN nonwovens is available from Czech SRO (Czech Republic) as PFNZN 18G BICO8020 PHI 6. 7 PFN nonwovens are available from Czech SRO (Czech Republic) as PEGZN25 BICO7030 Phobic. 8 Available from DunnPaper (USA) as product number 3028.
[0189] [Table 2]
[0190] Suitable nonwoven materials for the upper and / or lower nonwoven layers are considered to be able to deform (stretch) with balanced stretching and almost recover to their original state, thus helping to allow the absorbent core structure and / or absorbent article to recover from deformation during body movement. Particularly suitable nonwoven materials for the upper nonwoven layer can provide fluid handling performance, which can help to effectively move fluid deep into the inner core layer to provide a dry-feeling, body-hugging, comfortable fit. To achieve this, suitable nonwoven materials for the upper nonwoven layer exhibit a relatively low density (e.g., 0.03-0.07 g / cm³ under a pressure of 7 g / cm²) to allow fluid to be efficiently discharged from the upper nonwoven layer to the inner core layer below. In addition, suitable nonwoven fabric materials for the upper nonwoven layer can maintain a relatively bulky thickness even under high compressive forces from the body (i.e., a pressure of 70 g / cm²), and as a result, fluid present in the inner core layer is discharged from the absorbent core structure and returned, preventing the body from feeling wet.
[0191] Samples A-C and E were found to be suitable materials for the upper and / or lower nonwoven fabric layers. In particular, samples A-C and E demonstrated that they had a permanent strain of 0.013 mm / mm or less, that the material could stretch and recover, and that they had a fracture strain of more than 10% before tearing. Samples A-C and E also showed a permanent strain of 0.03 N * With a drying recovery energy exceeding 1 mm, less energy was required to bend while recovering from bending (1.6 N). * (Evided by dry bending energy of less than mm). Samples A, B, C, and E are 7 g / cm². 2 Under this pressure, 0.03~0.07 g / cm³ 3 It has a relatively low density, and is 7 g / cm³ in size of 0.80-1.21 mm. 2 The thickness at pressure is shown, demonstrating that these materials have a more open fibrous network structure, which can contribute to bulkier and more efficient fluid handling performance.
[0192] Sample D was found to have a permanent strain of 0.016 mm / mm, demonstrating that the material is likely to stretch significantly during manufacturing and / or use without returning to its initial state. At the same time, sample D was found to be highly compressible under body pressure, as demonstrated by its thickness of 0.19 mm at 70 g / cm², indicating that the material is likely to become denser under body compression and that the inner core layer is unlikely to adequately expel the fluid. Samples F and G were found to have a permanent strain of 0.03 N * It was demonstrated that the material exhibits a dry recovery energy of less than mm, potentially failing to recover from deformation, and therefore being insufficient to function as an upper nonwoven layer. However, when combined with the upper nonwoven layers described herein, samples D, F, and G may be suitable materials for the lower nonwoven layer.
[0193] Comparative sample H exhibited a fracture strain of less than 5% and a thickness of less than 0.2 mm at 70 g / cm². Furthermore, comparative sample H was found to tear when wet. Therefore, comparative sample H is insufficient to function as either an upper or lower nonwoven fabric layer.
[0194] Table 3 is provided for the convenience of the reader. Table 3 includes a non-exhaustive list of properties and a non-exhaustive list of corresponding values for each of the properties that a particularly preferred upper nonwoven layer of this disclosure may exhibit.
[0195] [Table 3]
[0196] Final product testing Absorbent articles are tested to evaluate the effect of short cellulosic fibers on core integrity (i.e., core cracking and / or tearing). Samples 1-3 represent absorbent articles comprising a top sheet, a back sheet, and an absorbent core structure as described herein positioned between them. The absorbent core structures of Samples 1-3 contain varying amounts of short cellulosic fibers. Samples 4-6 represent comparative absorbent articles comprising a top sheet, a back sheet, and an absorbent core disposed between them. The absorbent cores of Samples 4-6 represent conventional high-basis-weight cellulose cores containing varying amounts of short cellulosic fibers.
[0197] Sample 1 Prepare a disposable absorbent article in the form of a women's hygiene pad having the following components:
[0198] Topsheet - Topsheet is a 22.4gsm polyethylene molded film available as DS02-172 from Xiamen Yanjan New Material Co. (India).
[0199] The upper nonwoven layer is a 40gsm carded elastic nonwoven fabric containing BiCo(PE / PET) in a 60% 2DTex / 40% 4DTex blend, available from Xiamen Yanjan New Material Co. (China) as ATB Z87G-40.
[0200] The inner core layer is a homogeneous mixture of 150gsm cellulose pulp and 60gsm superabsorbent particles (available from Nippon Shokubai (Japan) as Aqualic CA L-805). The cellulose pulp is 100% SuperSoft® untreated fluff pulp available from International Paper Company (Memphis, TN).
[0201] The lower nonwoven layer is an 18gsm spunbond nonwoven fabric containing 100% 2.0D Tex polypropylene, available from PFN nonwovens Czech SRO (Czech Republic) as PFNZN 18G 100%PP PHI 6.
[0202] Backsheet - The backsheet is an 18gsm polypropylene film available from Swanson Plastics India (India).
[0203] First, the top sheet is coated with 5gsm adhesive (D3151 NG, available from HBFuller). Next, the upper nonwoven fabric layer is deposited on top of the top sheet. In parallel, the inner core layer is manufactured by the air-lay method. A flow of cellulose pulp and AGM is carried by a high-speed moving airflow and deposited into a three-dimensional molding pocket on a rotational molding drum with a downward vacuum suction to draw the cellulose and AGM into the pocket of the laydown station. The homogeneously mixed mass of cellulose and AGM is held on the forming drum under vacuum until it is deposited directly onto the upper nonwoven fabric layer pre-coated with 5gsm adhesive (D3151 NG, HBFuller), and then sealed with a second remaining nonwoven fabric pre-coated with 5gsm adhesive (D3151 NG, HBFuller) to create an absorbent core. The widths of the upper and lower nonwoven webs are wider than the maximum width of the molded cellulose and AGM inner core layers, thereby enabling an effective periphery seal where the two nonwovens connect, at least on the leftmost and rightmost parts of the absorbent core structure. The flex-bonding channel region is applied to the pattern shown in Figure 11B using a heated embossing unit on the production line. The backsheet is then bonded to the surface facing the outside of the lower nonwoven layer with a 5gsm adhesive (D3151 NG, HBFuller).
[0204] Sample 2: A women's hygiene pad was prepared as in Sample 1, except that the cellulose pulp contained 16% by weight of Eucafluff® (available from Suzanno, Brazil) and 84% by weight of SuperSoft® untreated fluff pulp.
[0205] Sample 3: A women's hygiene pad was prepared as in Sample 1, except that the cellulose pulp contained 32% by weight of Eucafluff® (available from Suzanno) and 68% by weight of SuperSoft® untreated fluff pulp.
[0206] Comparative samples 4-7: Prepare a disposable absorbent article in the form of a women's hygiene pad having the following components:
[0207] Topsheet - The topsheet is a 22.4gsm polyethylene molded film available from Yanjan (Egypt) as MM1-172.
[0208] Core layer - The core layer is 430gsm cellulose pulp. The cellulose pulp is 100% SuperSoft® untreated fluff pulp available from International Paper Company (Memphis, TN).
[0209] Backsheet - The backsheet is a 12gsm polyolefin resin blow film (3 layers) of metallocene-LLDPE, LDPE, and HDPE composition, available from RKW Group (Germany) as Theo 12gsm 168mm film.
[0210] First, a flow of cellulose fibers is carried by a high-speed airflow and deposited into a three-dimensional molded pocket on a rotational molding drum with a downward vacuum suction to draw the cellulose into the pocket of the laydown station. This molded pocket provides the actual physical shape of the core layer, which is deposited directly onto a top sheet pre-coated with 4.1 gsm adhesive (D3151 NG, HBFuller). Next, deep embossed grooves are applied as described in U.S. Patent No. 11,696,858. Channels are formed by heat, compress, and embossing the top sheet and absorbent core material toward the back sheet, so that the channel portion of the absorbent article has a higher density than the rest of the pad, which means that it provides structural wet integrity of the product in use. The product is then closed with a back sheet pre-coated with 9 gsm adhesive (D3151 NG, HBFuller).
[0211] The integrity of the absorbent core is determined by grading the core cracks on the pad after it has been worn during menstruation and collected for testing. Core crack grading is determined by visually inspecting the pad using a lightbox. The returned pads are graded on the following scale: 1. Good - Consumers will likely not see any gaps (cracks or fissures), the length of the cracks is 0-30 mm, the width of the cracks is less than 1 mm, and the number of places where cracks are visible is less than 3. 2. Moderate - Consumers may see cracks, the length of the cracks is more than 30 mm but less than 60 mm, the width of the cracks is more than 1 mm but less than 2 mm, and the number of places where cracks are seen is 4 to 6. 3. Severe - Consumers are very likely to detect core disintegration, can see core missing or very widespread cracks, crack widths exceeding 2mm, and more than 6 locations where cracks are found.
[0212] The results are shown in Table 4 below.
[0213] [Table 4]
[0214] Low basis weight (i.e., 350 gsm or less), low density cellulose pulp absorbent cores have traditionally been considered less structurally stable compared to thicker, higher basis weight (i.e., greater than 350 gsm) cellulose pulp cores, and are at a greater risk of tearing and / or deformation during use. The challenges of structural integrity in low basis weight, low density core structures can be further exacerbated by the inclusion of short cellulosic fibers such as eucalyptus, which are less physically entangled and more susceptible to bursting and tearing than longer, standard southern or northern coniferous fibers. Sample 3, containing the absorbent core structure described herein with 32 wt% eucalyptus fibers of cellulose pulp, was able to maintain structural core integrity during use, and remarkably, core integrity defects were found in only 20% of the returned pads.
[0215] It is believed that high basis weight cellulose pulp absorbent cores with greater mass can allow more fibers to become physically entangled, and typically can retain their structural shape. However, surprisingly, Sample 6 (without upper or lower nonwoven layers) comprising a high basis weight (greater than 350 gsm) cellulose pulp-based core with 32% eucalyptus fibers exhibited significant structural failure of the fiber matrix, and poor core integrity was found in 32% of the returned pads. This level of poor core integrity during use is considered unacceptable to consumers.
[0216] Without being bound by theory, it is believed that the absorbent core structures described herein enable the use of greater than or equal to 32% short cellulosic fibers in relatively low density absorbent core structures (i.e., 0.045 to 0.15 g / cm 3 ) by providing structural integrity through the use of resilient upper and / or lower nonwoven layers. Additional features described herein, such as perimeter seals in the left and right side regions of the upper and lower nonwoven layers, flex-bonded channel regions, and / or structural bond sites, may provide additional structural integrity and help reduce tearing and / or deformation of the core during use.
[0217] Samples 1 to 3 are tested to also evaluate the ability of the absorbent core structures to compress (simulating the compression experienced between a wearer's legs) and recover to their original state. Samples 1 to 3 are evaluated according to the wet and dry CD and MD 3-point bend test, the wet and dry deformation compression test, and the light touch rewet test, as described herein. The results are shown in Table 5.
[0218] [Table 5]
[0219] Sample 1, which contains no short cellulosic fibers, has a CD dry bending stiffness of 15.5 N N * mm 2Furthermore, it exhibited a 30% wet recovery percentage in the fifth cycle in both wet and dry collapse compression methods, demonstrating that Sample 1 would be able to maintain its shape during use. The addition of eucalyptus short cellulosic fibers (Samples 2 and 3) was found not to adversely affect the article's ability to bend and / or compress and recover its original shape. It was also found that Samples 2 and 3 maintained fluid handling performance and could draw fluid deeply into the absorbent core structure, as demonstrated by light touch re-wetting of 0.10 g.
[0220] To provide high biocompatibility, the absorbent articles of this disclosure have a load capacity of approximately 7.0 to 30.0 N. * mm 2 , or approximately 10.0 to approximately 25N * mm 2 It is thought that this can exhibit low CD dry bending stiffness (i.e., high flexibility). Furthermore, in order to provide an absorbent article that can be compressed in accordance with body movement and return to its original pre-compression state relative to the user's body, the absorbent article of this disclosure has a stiffness of approximately 1.0 to approximately 3.5 N. * It is believed that the fifth-cycle wetting recovery energy may be mm and / or a fifth-cycle wetting recovery percentage of about 29% to about 40%. The absorbent articles of this disclosure can also maintain good fluid handling, resulting in low light-touch rewetting of about 0 to about 0.15 g.
[0221] Combinations / Examples Paragraph A. Disposable absorbent articles, Absorbent core structure, a. An upper nonwoven fabric layer containing polymer fibers and having a basis weight of approximately 30 gsm to approximately 85 gsm, wherein the upper nonwoven fabric layer includes a first side region and a second side region facing each other in the transverse direction, b. A lower nonwoven fabric layer containing polymer fibers, wherein the lower nonwoven fabric layer includes a first side region and a second side region facing each other in the transverse direction, c. An absorbent core structure comprising an inner core layer containing a mixture of cellulose pulp and superabsorbent particles, wherein a portion of the inner core layer is disposed between an upper nonwoven fabric layer and a lower nonwoven fabric layer, The cellulose pulp contains short cellulosic fibers in an amount of approximately 25% to 70% by weight, and the short cellulosic fibers have an average fiber length of less than approximately 2 mm, preferably approximately 0.3 mm to approximately 2 mm. The absorbent core structure has a density of approximately 0.045 g / cm³. 3 ~Approx. 0.15g / cm 3 It has an average density, A disposable absorbent article in which a portion of the inner core layer is contained within the upper and lower nonwoven fabric layers by sealing a portion of the first and second side regions of the upper nonwoven fabric with a portion of the first and second side regions of the lower nonwoven fabric layer in a peripheral seal.
[0222] Paragraph B. The disposable absorbent article described in Paragraph A, wherein the short cellulose fibers are selected from the group consisting of maple, oak, eucalyptus, poplar, beech, birch, paulownia, bamboo, hemp, acacia, wheat straw, rice straw, corn sheath, and combinations thereof.
[0223] Paragraph C. A disposable absorbent article according to paragraph A or B, comprising approximately 15% to 50% by weight of superabsorbent particles in the inner core layer.
[0224] Paragraph D. A disposable absorbent article according to any one of paragraphs A to C, wherein the lower nonwoven fabric layer has a basis weight of about 7 gsm to about 40 gsm, preferably about 10 gsm to about 35 gsm, and more preferably about 15 gsm to about 20 gsm.
[0225] Paragraph E. When the absorbent article was measured according to the wet and dry CD and MD 3-point bending method, it was approximately 7.0 N. * mm 2 ~Approx. 30.0N * mm 2A disposable absorbent article according to any of paragraphs A to D, having a CD dry bending stiffness and a 5th cycle wet recovery % of about 29% to about 40% when measured according to the wet and dry collapse compression method.
[0226] Paragraph F. A disposable absorbent article according to any of paragraphs A to E, wherein the upper nonwoven fabric layer is an air-through bonded nonwoven fabric, a needle-punched nonwoven fabric, a carded nonwoven fabric, or a water-entangled nonwoven fabric.
[0227] Paragraph G. The disposable absorbent article described in paragraphs A to F, wherein the polymer fibers of the upper nonwoven fabric layer have a staple length of approximately 10 mm to approximately 100 mm.
[0228] Paragraph H. Disposable absorbent articles as described in paragraphs A to G, wherein the absorbent articles have a dry caliper of approximately 2.0 mm to approximately 6.0 mm when measured according to the wet and dry CD and MD3-point method.
[0229] Paragraph I. The disposable absorbent article according to paragraphs A to H, wherein the polymer fibers of the upper nonwoven fabric layer are selected from two-component fibers comprising polyethylene terephthalate, polypropylene, polylactic acid, polyethylene / polypropylene or polyethylene / polyethylene terephthalate, and combinations thereof.
[0230] Paragraph J. The disposable absorbent article according to paragraphs A to I, wherein the polymer fibers of the lower nonwoven layer are selected from two-component fibers comprising polyethylene terephthalate, polypropylene, polylactic acid, polyethylene / polypropylene or polyethylene / polyethylene terephthalate, and combinations thereof.
[0231] Paragraph K. The disposable absorbent article according to paragraphs A to J, wherein the polymer fibers of the upper nonwoven fabric layer have a fiber diameter of about 2.0 Dtex to about 10.0 Dtex.
[0232] Paragraph L. The disposable absorbent article according to paragraphs A to K, wherein the polymer fibers of the lower nonwoven fabric layer have a fiber diameter of about 1.0 Dtex to about 5.0 Dtex.
[0233] Paragraph M. The disposable absorbent article according to any of paragraphs A to L, wherein the absorbent article has a light touch rewet of 0 to about 0.15 grams as measured according to the light touch rewet method.
[0234] Paragraph N. The disposable absorbent article according to any of paragraphs A to M, wherein the inner core layer comprises superabsorbent particles at from about 20 gsm to about 125 gsm.
[0235] Paragraph O. The disposable absorbent article according to any of paragraphs A to N, wherein the inner core layer comprises cellulose pulp at from about 125 gsm to about 350 gsm.
[0236] Paragraph P. The disposable absorbent article according to any of paragraphs A to O, further comprising a topsheet and a backsheet, wherein the absorbent core structure is disposed between the topsheet and the backsheet.
[0237] Paragraph Q. The disposable absorbent article according to any of paragraphs A to P, wherein at least one of the upper nonwoven layer and the lower nonwoven layer comprises a polymer selected from the group consisting of recycled polymer resins, biodegradable polymers, biopolymers, and combinations thereof.
[0238] Paragraph R. The disposable absorbent article according to any of paragraphs A to Q, wherein the polymer fibers of the upper nonwoven layer comprise from about 60% to about 100% synthetic fibers, and from 0% to 40% regenerated cellulosic fibers including rayon.
[0239] The dimensions and values disclosed herein are not to be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm".
[0240] All documents cited herein, including cross-referenced or related patents or applications, are incorporated herein in their entirety by reference unless expressly excluded or otherwise limited. No citation of any document shall be deemed prior art to any invention disclosed or claimed herein, nor shall it be deemed to teach, suggest or disclose any such invention, either alone or in combination with any one or more other references. Furthermore, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in any document incorporated by reference, the meaning or definition given to that term in this document shall prevail.
[0241] While specific embodiments of the present invention have been illustrated and described, it will be apparent to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. Therefore, it is intended that all such changes and modifications within the scope of the invention be covered in the appended claims.
Claims
1. Disposable absorbent articles, Top sheet and Back seat and, An absorbent core structure disposed between the top sheet and the back sheet, a. An upper nonwoven fabric layer containing polymer fibers and having a basis weight of 30 gsm to 85 gsm, wherein the upper nonwoven fabric layer includes a first side region and a second side region facing each other in the transverse direction. b. A lower nonwoven fabric layer containing polymer fibers, wherein the lower nonwoven fabric layer includes a first side region and a second side region facing each other in the transverse direction, and c. An absorbent core structure comprising an inner core layer containing a mixture of cellulose pulp and superabsorbent particles, wherein a portion of the inner core layer is disposed between the upper nonwoven fabric layer and the lower nonwoven fabric layer, The cellulose pulp contains 25% to 70% by weight of short cellulose fibers, and the short cellulose fibers have an average fiber length of less than 2 mm. The absorbent core structure contains 0.045 g / cm³ 3 ~0.15 g / cm 3 It has an average density, A disposable absorbent article is housed within the upper nonwoven fabric layer and the lower nonwoven fabric layer, wherein a portion of the inner core layer is sealed in a peripheral seal with a portion of the first side region and a portion of the second side region of the upper nonwoven fabric layer and a portion of the first side region and a portion of the second side region of the lower nonwoven fabric layer.
2. The disposable absorbent article according to claim 1, wherein the short cellulose fibers are selected from the group consisting of maple, oak, eucalyptus, poplar, beech, birch, paulownia, bamboo, hemp, acacia, wheat straw, rice straw, corn husk, and combinations thereof.
3. The disposable absorbent article according to claim 1 or 2, comprising 15% to 50% by weight of superabsorbent particles in the inner core layer.
4. The disposable absorbent article according to any one of claims 1 to 3, wherein the lower nonwoven fabric layer has a basis weight of 7 gsm to 40 gsm, preferably 10 gsm to 35 gsm, and more preferably 15 gsm to 20 gsm.
5. The absorbent article measured 7.0 N when subjected to wet and dry CD and MD three-point bending methods. * mm 2 ~30.0N * mm 2 A disposable absorbent article according to any one of claims 1 to 4, wherein the CD dry bending stiffness and, when measured according to the wet and dry collapse compression method, have a fifth cycle wet recovery percentage of 29% to 40%.
6. The disposable absorbent article according to any one of claims 1 to 5, wherein the upper nonwoven fabric layer is an air-through bonded nonwoven fabric, a needle-punched nonwoven fabric, a carded nonwoven fabric, or a water-entangled nonwoven fabric.
7. The disposable absorbent article according to any one of claims 1 to 6, wherein the polymer fibers of the upper nonwoven fabric layer have a staple length of 10 mm to 100 mm.
8. The disposable absorbent article according to any one of claims 1 to 7, wherein the absorbent article has a dry caliper of 2.0 mm to 6.0 mm when measured according to the wet and dry CD and MD 3-point method.
9. A disposable absorbent article according to any one of claims 1 to 8, wherein at least one of the polymer fibers in the upper nonwoven layer and the lower nonwoven layer is selected from two-component fibers including polyethylene terephthalate, polypropylene, polylactic acid, polyethylene / polypropylene or polyethylene / polyethylene terephthalate, and combinations thereof.
10. The disposable absorbent article according to any one of claims 1 to 9, wherein the polymer fibers of the upper nonwoven fabric layer have a fiber diameter of 2.0 Dtex to 10.0 Dtex.
11. The disposable absorbent article according to any one of claims 1 to 10, wherein the polymer fibers of the lower nonwoven fabric layer have a fiber diameter of 1.0 Dtex to 5.0 Dtex.
12. The disposable absorbent article according to any one of claims 1 to 11, wherein the absorbent article has a light touch remoisture of 0 to 0.15 grams when measured according to the light touch remoisture method.
13. The disposable absorbent article according to any one of claims 1 to 12, wherein the inner core layer comprises superabsorbent particles of 20 gsm to 125 gsm and cellulose pulp of 125 gsm to 350 gsm.
14. The disposable absorbent article according to any one of claims 1 to 13, wherein at least one of the upper nonwoven fabric layer and the lower nonwoven fabric layer contains a polymer selected from the group consisting of recycled polymer resin, biodegradable polymer, biopolymer, and combinations thereof.
15. The disposable absorbent article according to any one of claims 1 to 14, wherein the polymer fibers of the upper nonwoven fabric layer comprise 60 to 100% synthetic fibers and 0 to 40% regenerated cellulose fibers including rayon.