Positive electrode active material configuration for all-solid-state batteries, positive electrode for all-solid-state batteries containing the same, and all-solid-state battery
The positive electrode active material configuration with a lithium titanium compound and concentration gradient addresses interfacial resistance issues in all-solid-state batteries, enhancing their lifespan and stability.
Patent Information
- Application Number
- JP2025573850
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-12
- Filing Date
- 2025-04-04
- Publication Date
- 2026-11-24
AI Technical Summary
Conventional all-solid-state batteries using sulfide-based solid electrolytes face high interfacial resistance due to the formation of a lithium-deficient layer and impurity layers at the interface between the positive electrode active material and the solid electrolyte, leading to reduced capacity and degradation over cycles.
A positive electrode active material configuration is developed with a core portion containing a lithium titanium compound and a coating portion with a concentration gradient, where titanium concentration decreases from the surface towards the center, reducing interfacial resistance and side reactions.
The configuration improves the lifespan characteristics of all-solid-state batteries by minimizing interfacial resistance and preventing degradation, enabling stable operation for several hundred cycles.
Smart Images

Figure 2026539251000001_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to and the benefit of Korean Patent Application No. 10-2024-0049273, filed on April 12, 2024, the entire contents of which are incorporated herein by reference.
[0002] The present disclosure relates to a positive electrode active material composition for all-solid-state batteries, a positive electrode for all-solid-state batteries including the same, and an all-solid-state battery.
Background Art
[0003] Lithium secondary batteries are widely used as power sources for portable devices including IT and mobile devices, and in recent years, the market has been steadily expanding from small-sized lithium secondary batteries to medium- and large-sized secondary batteries. In particular, the use of lithium secondary batteries as automotive batteries is showing a rapid growth trend. In order to use lithium secondary batteries as power sources for electric vehicles, high energy density and high output characteristics are required, and ensuring safety is particularly important.
[0004] Conventional lithium secondary batteries use liquid non-aqueous organic electrolytes, which pose a risk of ignition and explosion. Since explosion accidents involving products using such electrolytes have occurred continuously, there is an urgent need to address these issues.
[0005] All-solid-state batteries replace such organic electrolytes with solid electrolytes, and are batteries in which all components including electrodes and electrolytes are made of solid materials. Due to the high intrinsic safety of the solid electrolyte contained therein, the risk of ignition and explosion can be fundamentally eliminated.
[0006] Candidates for use as solid electrolytes in all-solid-state lithium-ion secondary batteries include gel-type polymer electrolytes, sulfide-based solid electrolytes, and oxide-based solid electrolytes. Among these, sulfide-based solid electrolytes have a lithium ion conductivity of 1×10 -2It exhibits high lithium-ion conductivity values of S / cm or higher and has a wide potential window of 5V or more, resulting in less degradation of characteristics even in extreme environments, and offering significant advantages in the design of high-energy-density lithium-ion secondary batteries.
[0007] In all-solid-state batteries using sulfide-based solid electrolytes, there is a problem in that the capacity is not properly realized due to high interfacial resistance generated at the interface between the positive electrode active material and the sulfide-based solid electrolyte. The main causes of such interfacial resistance have been proposed to be: 1) the space charge layer phenomenon in which a lithium-deficient layer is formed at the solid electrolyte interface due to the chemical potential difference between lithium ions in the positive electrode active material and the solid electrolyte, and 2) the formation of an interfacial impurity layer due to chemical reactions at the interface between the positive electrode active material and the solid electrolyte.
[0008] To solve the aforementioned problems, a technique has been applied to introduce a coating layer on the surface of the positive electrode active material, and lithium oxide of Li-MO (where M is B, Al, Zr, P, Ti, Nb, or W) is known as the material for the coating layer. However, even with the introduction of a coating layer on the surface of the positive electrode active material, degradation of all-solid-state batteries that occurs over long cycles has not been prevented. [Prior art documents] [Patent Documents]
[0009] [Patent Document 1] Korean Published Patent No. 2017-0074624 [Overview of the Initiative] [Problems that the invention aims to solve]
[0010] To solve the aforementioned problems, the inventors conducted multifaceted research and discovered that coating the surface of the positive electrode active material with a lithium titanium compound can reduce the interfacial resistance between the positive electrode active material and the solid electrolyte. Furthermore, they discovered that positioning the lithium titanium compound at the interface of the positive electrode active material, which is a secondary particle formed by the aggregation of multiple primary particles, can reduce side reactions and improve the lifespan characteristics of the all-solid-state battery, thus completing this disclosure.
[0011] Therefore, the present disclosure aims to provide a positive electrode active material configuration for an all-solid-state battery that can not only reduce the interfacial resistance between the positive electrode active material and the solid electrolyte, but also improve the lifespan characteristics of the all-solid-state battery.
[0012] Furthermore, this disclosure aims to provide a positive electrode including the positive electrode active material configuration for the all-solid-state battery and an all-solid-state battery including the same. [Means for solving the problem]
[0013] In order to achieve the aforementioned objective, This disclosure includes a core portion comprising a positive electrode active material and a lithium titanium compound; and A coating portion located on the surface of the core portion and containing a lithium titanium compound; The core portion provides a positive electrode active material configuration for an all-solid-state battery, having a concentration gradient in which the titanium concentration decreases from the outermost surface towards the center.
[0014] Furthermore, this disclosure provides a positive electrode for an all-solid-state battery, comprising the positive electrode active material configuration, solid electrolyte, conductive material, and binder described herein.
[0015] Furthermore, this disclosure provides an all-solid-state battery comprising a positive electrode; a negative electrode; and a solid electrolyte layer between the positive electrode and the negative electrode. [Effects of the Invention]
[0016] The positive electrode active material configuration for all-solid-state batteries disclosed herein involves coating the surface of the positive electrode active material with a lithium titanium compound and positioning the lithium titanium compound at the interface of the positive electrode active material, which is a secondary particle formed by the aggregation of multiple primary particles. This suppresses side reactions occurring between the positive electrode active material and the solid electrolyte and reduces interfacial resistance.
[0017] As a result, the all-solid-state battery, including the positive electrode active material configuration, can have improved lifespan characteristics. [Brief explanation of the drawing]
[0018] [Figure 1] This is a cross-sectional view of the positive electrode active material configuration for an all-solid-state battery in this disclosure. [Modes for carrying out the invention]
[0019] The terms and words used in this specification and in the claims should not be construed to be limited to their ordinary or dictionary meanings, but rather to be construed in a sense and concept consistent with the technical idea of this disclosure, based on the principle that inventors may appropriately define the concepts of terms in order to best describe their inventions.
[0020] The terms used in this disclosure are used solely to describe specific embodiments and are not intended to limit this disclosure. Singular expressions include plural expressions unless they are clearly different in context. In this disclosure, terms such as “includes” or “having” specify the existence of features, figures, stages, operations, components, parts or combinations thereof described in the specification, and should not be understood to preemptively exclude the existence or possibility of adding one or more other features, figures, stages, operations, components, parts or combinations thereof.
[0021] The following provides a more detailed explanation of this disclosure.
[0022] Solid-state batteries use a solid electrolyte to conduct lithium ions, so the movement of lithium ions during charging and discharging occurs in a solid state. In other words, since lithium ions can only move through the actual contact area between the positive electrode and the solid electrolyte, minimizing the interfacial resistance between the positive electrode and the solid electrolyte can improve the performance of solid-state batteries.
[0023] However, side reactions occur at the actual contact site between the positive electrode and the solid electrolyte, leading to increased interfacial resistance. Furthermore, when all-solid-state batteries are operated for hundreds of cycles or more, side reactions occur from the surface of the positive electrode active material, causing problems such as the positive electrode active material entering a rock salt phase.
[0024] Therefore, in this disclosure, we aimed to provide a positive electrode active material configuration that can improve the long-term life characteristics of an all-solid-state battery while reducing the interfacial resistance between the positive electrode and the solid electrolyte.
[0025] Composition of positive electrode active material for all-solid-state batteries This disclosure includes a core portion comprising a positive electrode active material and a lithium titanium compound; and A coating portion located on the surface of the core portion and containing a lithium titanium compound; The present invention relates to a positive electrode active material configuration for an all-solid-state battery, wherein the core portion has a concentration gradient in which the titanium concentration decreases from the outermost surface towards the center.
[0026] The positive electrode active material configuration of this disclosure is a core-shell structure, wherein the core portion contains the positive electrode active material and a lithium titanium compound, and the coating portion corresponding to the shell may also contain a lithium titanium compound.
[0027] The lithium titanium compound acts as a buffer and is included not only in the coating but also in the core. If the lithium titanium compound were included only in the coating, a side reaction could occur from the outermost surface of the core when the all-solid-state battery is operated for several hundred cycles or more, potentially causing the positive electrode active material to become rock salt. However, this disclosure solves the above problem by including the lithium titanium compound not only in the coating but also in the core, and provides an all-solid-state battery that can be operated for several hundred cycles or more.
[0028] The core portion comprises a positive electrode active material and a lithium titanium compound, and the lithium titanium compound in the core portion may have a concentration gradient in which the concentration of titanium decreases from the outermost surface of the core portion toward the center.
[0029] The concentration gradient refers to the existence of a slope between the concentration at any point on the outermost surface of the core and the concentration at any point in the center of the core.
[0030] The positive electrode active material is a lithium metal oxide, and the lithium metal oxide may be secondary particles formed by the aggregation of multiple primary particles. Therefore, the lithium metal oxide may be in a polycrystalline form. The primary particle refers to a single grain (grain or crystallite). Voids and grain boundaries may exist between the primary particles constituting the secondary particle. For example, the primary particles may form internal voids by separating from adjacent primary particles within the secondary particle. Alternatively, the primary particles may form grain boundaries by touching adjacent primary particles. In the core portion, the lithium titanium compound may be present in the internal voids.
[0031] If, by any chance, the concentration of titanium on the outermost surface of the core part is the same as the concentration of titanium in the central part of the core part, or if the concentration of titanium increases from the outermost surface of the core part toward the central part, the movement of lithium ions between the primary particles is hindered, Ohmic resistance and charge transfer resistance increase, and the performance of the all-solid-state battery may deteriorate.
[0032] The diameter of the core part may be the diameter of secondary particles, and the diameter of the secondary particles may vary depending on the number of aggregated primary particles, and may be 3 to 10 μm. Accordingly, the diameter of the core part may be 3 to 10 μm.
[0033] Further, in the core part, the lithium-titanium compound may exist within a distance of 5 μm, 4 μm, 3 μm, 2 μm, 1 μm, or 0.5 μm from the outermost surface of the core part toward the center. Accordingly, only the lithium metal oxide, which is a positive electrode active material, may be present in the absolute center of the core part.
[0034] The lithium metal oxide is a material capable of intercalating and deintercalating lithium ions, and is not particularly limited as long as it can be used as a positive electrode active material for a lithium ion secondary battery.
[0035] For example, the positive electrode active material may include layered compounds such as lithium cobalt oxide (LiCoO2) and lithium nickel oxide (LiNiO2), or compounds substituted with one or more transition metals; chemical formula Li x M y O2 (M is at least one selected from the group consisting of Co, Mn, Ni, Al, Fe, V, Zn, Cr, Ti, Ta, Mg, Mo, Zr, W, Sn, Hf, Nd, and Gd, x satisfies 0<x≦1.5, and y satisfies 0<y≦1); chemical formula Li 1+x Mn 2-x O4 (0≦x≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8; chemical formula LiNi 1-x Mx Ni-site type lithium nickel oxide represented by O2 (M=Co, Mn, Al, Cu, Fe, Mg, B, or Ga; 0.01≦x≦0.3); chemical formula LiMn 2-x M x Lithium manganese composite oxide represented by O2 (M=Co, Ni, Fe, Cr, Zn, or Ta; 0.01≦x≦0.1) or Li2Mn3MO8 (M=Fe, Co, Ni, Cu, or Zn); LiNi x Mn 2-x Lithium manganese composite oxide with a spinel structure represented by O4; LiCoPO4; or LiFePO4; etc., but are not limited to these.
[0036] The lithium titanium compound located in the core part and the coating part may be lithium titanium oxide. The lithium titanium oxide is Li x Ti y O4 (0.8≦x≦1.4, 1.6≦y≦2.2), but is not limited thereto.
[0037] The coating part is located on the surface of the core part, and more specifically, may be located on the surface of the secondary particles. In addition, the coating part includes the lithium titanium compound, and preferably may be composed of the lithium titanium compound.
[0038] The coating portion can mean a portion in which the lithium titanium compound is physically and / or chemically bonded to the surface of the core portion. The lithium titanium compound may cover the entire surface of the core portion, or it may be distributed on the surface of the core portion in an island type or flake form, and if it is distributed in an island type or flake form, it may be separated from each other at predetermined intervals. Preferably, the lithium titanium compound may be distributed in a form that uniformly covers the entire surface of the core portion. When the lithium titanium compound is uniformly coated on the entire surface of the core portion, the coating layer of the lithium titanium compound prevents direct contact between the positive electrode active material and the solid electrolyte, thereby suppressing interfacial side reactions due to the chemical potential difference of lithium ions. At the same time, the lithium concentration increases, and a path for lithium ion movement is secured, so the interfacial resistance with the solid electrolyte can be reduced.
[0039] Furthermore, the thickness of the coating portion is not particularly limited in this disclosure, but is preferably 10 to 200 nm, and more preferably 50 to 150 nm.
[0040] The lithium titanium compound in the coating portion is present in an amount of 0.1 to 5 parts by weight, preferably 1 to 3 parts by weight, based on 100 parts by weight of the core portion. Within the range of 0.1 to 5 parts by weight, an effect of reducing interfacial resistance can be obtained, but outside this range, the interfacial resistance increases, which presents a problem in that the electrochemical properties of the all-solid-state battery containing it cannot be improved.
[0041] The positive electrode active material configuration for the all-solid-state battery described herein may be such that, in the final stage of the core manufacturing process, a precursor of a titanium compound is mixed together and fired to form a coating portion containing a lithium titanium compound, the lithium titanium compound in the coating portion is absorbed into the core portion containing the positive electrode active material, and finally a core portion containing the positive electrode active material and a lithium titanium compound, and a coating portion containing a lithium titanium compound are formed. Furthermore, since the lithium titanium compound is absorbed from the coating portion into the core portion, the concentration of the lithium titanium compound present in the coating portion may be higher than the concentration of the lithium titanium compound present in the core portion. In addition, in the core portion, titanium may have a concentration gradient in which the concentration decreases from the outermost surface of the core portion toward the center.
[0042] Positive electrode for all-solid-state batteries This disclosure relates to a positive electrode for an all-solid-state battery, wherein the positive electrode may include a positive electrode active material, a solid electrolyte, a conductive material, and a binder, and the positive electrode active material is the positive electrode active material configuration of this disclosure described above.
[0043] The positive electrode may include a positive electrode current collector and a positive electrode active material layer coated on one or both sides of the positive electrode current collector. Therefore, the positive electrode active material, solid electrolyte, conductive material, and binder may be included in the positive electrode active material layer.
[0044] The positive electrode current collector is for supporting the positive electrode active material layer and is not particularly limited as long as it has excellent conductivity and is electrochemically stable in the voltage range of the lithium secondary battery. For example, the positive electrode current collector may be any one metal selected from the group consisting of copper, aluminum, stainless steel, titanium, silver, palladium, nickel, alloys thereof, and combinations thereof. The stainless steel may be surface-treated with carbon, nickel, titanium, or silver. As the alloy, an aluminum-cadmium alloy may be preferably used. Other options include calcined carbon, a non-conductive polymer surface-treated with a conductive material, or a conductive polymer.
[0045] The positive electrode current collector can have fine irregularities formed on its surface to strengthen its bonding force with the positive electrode active material, and may be used in various forms such as film, sheet, foil, mesh, net, porous material, foam, nonwoven fabric, etc.
[0046] The solid electrolyte may include one or more selected from the group consisting of sulfide-based solid electrolytes, polymer-based solid electrolytes, and oxide-based solid electrolytes, and preferably includes a sulfide-based solid electrolyte.
[0047] The sulfide-based solid electrolyte contains sulfur (S) and has ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS glass or Li-PS glass ceramic.
[0048] Specifically, the sulfide-based solid electrolyte may contain one or more selected from the group consisting of Li6PS5Cl, Li6PS5Br, Li6PS5I, Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, and Li2S-GeS2-ZnS, and preferably contains one or more selected from the group consisting of Li6PS5Cl, Li6PS5Br, and Li6PS5I. The Li6PS5Cl, Li6PS5Br, and Li6PS5I mentioned above may be argyrodite-type solid electrolytes. Furthermore, the sulfide-based solid electrolyte may be in a form doped with trace amounts of elements; for example, Li6PS5Cl may be further doped with bromine (Br).
[0049] The aforementioned polymer solid electrolyte is a composite of a lithium salt and a polymer resin, that is, a polymer electrolyte material formed by adding a polymer resin to a solvated lithium salt, and is approximately 1 × 10⁻⁶ -7S / cm or more, preferably about 1 × 10 -5 It can exhibit ionic conductivity of S / cm or higher.
[0050] Non-limiting examples of the polymer resin include polyether polymers, polycarbonate polymers, acrylate polymers, polysiloxane polymers, phosphazene polymers, polyethylene derivatives, alkylene oxide derivatives such as polyethylene oxide, phosphate ester polymers, agitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, polymers containing ionic dissociation groups, and may contain one or more of these. Furthermore, as the polymer electrolyte, examples of polymer resins include branched copolymers obtained by copolymerizing a PEO (polyethylene oxide) main chain with amorphous polymers such as PMMA, polycarbonate, polysiloxane (pdms) and / or phosphazene as copolymerizers, comb-like polymers, and crosslinked polymers, and may contain one or more of these.
[0051] In the polymer solid electrolyte, the lithium salt is an ionizable lithium salt, Li + X - It can be expressed as follows. There are no particular restrictions on the anion of such lithium salt, but F - Cl - , Br - , I - NO3 - , N(CN)2 - BF4 - ClO4 - PF6 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - CF3CF2SO3 - (CF3SO2)2N - , (FSO2)2N- CF3CF2(CF3)2CO - (CF3SO2) 2CH - (SF5)3C - , (CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - , (CF3CF2SO2)2N - Examples include the following.
[0052] The oxide-based solid electrolyte may contain oxygen (O) and have ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table. For example, LLTO compounds, Li6La2CaTa2O 12 Li6La2ANb2O 12 (A is Ca or Sr), Li2Nd3TeSbO 12 Li3BO 2.5 N 0.5 , Li9SiAlO8, LAGP compounds, LATP compounds, Li 1+x Ti 2-x Al x Si y (PO4) 3-y (Here, 0≦x≦1, 0≦y≦1), LiAl x Zr 2-x (PO4)3 (where 0≦x≦1), LiTi x Zr 2-x (PO4)3 (where 0 ≤ x ≤ 1), may contain one or more compounds selected from LISICON compounds, LIPON compounds, perovskite compounds, NASICON compounds, and LLZO compounds.
[0053] The conductive material electrically connects the current collector and the positive electrode active material, acting as a pathway for electrons to move from the current collector to the positive electrode active material. It can be used without limitation as long as it does not undergo chemical changes in a lithium secondary battery and is porous and conductive.
[0054] For example, the conductive material can be a porous carbon-based material, such as carbon black, graphite, graphene, activated carbon, carbon fiber, metallic fibers such as metal mesh; metallic powders such as copper, silver, nickel, and aluminum; or organic conductive materials such as polyphenylene derivatives. The conductive materials can be used individually or in combination.
[0055] Currently, commercially available conductive materials include the acetylene black series (products from Chevron Chemical Company or Gulf Oil Company, etc.), the Ketjen Black EC series (products from Armak Company), Vulcan XC-72 (products from Cabot Company), and Super P (products from MMM). Examples include acetylene black, carbon black, and graphite.
[0056] Furthermore, the binder enhances the bonding force between the components constituting the positive electrode and between them and the current collector, and any binder known in the industry can be used.
[0057] For example, the binder may be one, a mixture of two or more, or a copolymer selected from the group consisting of: fluororesin binders containing polyvinylidenefluoride (PVdF) or polytetrafluoroethylene (PTFE); rubber binders containing styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, or styrene-isoprene rubber; cellulose binders containing carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, or regenerated cellulose; polyalcohol binders; polyolefin binders containing polyethylene or polypropylene; polyimide binders; polyester binders; and silane binders.
[0058] All solid state battery This disclosure relates to an all-solid-state battery comprising a positive electrode; a negative electrode; and a solid electrolyte layer between the positive electrode and the negative electrode, wherein the positive electrode is the positive electrode of the present disclosure described above.
[0059] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector. Furthermore, the negative electrode, like the positive electrode, may optionally include a conductive material and a binder. In this case, the negative electrode current collector, conductive material, and binder are as described above.
[0060] The aforementioned negative electrode active material is lithium ion (Li + Any substance that can reversibly intercalate or deintercalate lithium, or react with lithium ions to reversibly form lithium-containing compounds, is acceptable.
[0061] For example, the negative electrode active material may be one or more carbon-based materials selected from the group consisting of crystalline artificial graphite, crystalline natural graphite, amorphous hard carbon, low-crystalline soft carbon, carbon black, acetylene black, Ketjen black, Super P, graphene, and fibrous carbon, a Si-based material, Li x Fe2O3(0≦x≦1), Li x WO2(0≦x≦1), Sn x Me 1-x Me' y O z metal composite oxides such as (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0<x≦1; 1≦y≦3; 1≦z≦8); lithium metal; lithium alloys; silicon-based alloys; tin-based alloys; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; titanium oxide; lithium titanium oxide, etc., but are not limited thereto.
[0062] In addition, the negative electrode may include a negative electrode current collector and a coating layer including metal-carbon composite particles positioned on the negative electrode current collector. This may mean an anodeless electrode that does not include a negative electrode active material.
[0063] When charging the all-solid-state battery, lithium ions may pass through the coating layer of the negative electrode to reach the surface of the negative electrode current collector, where they are electrodeposited to form a lithium metal layer.
[0064] The metal-carbon composite particles may have a form in which carbon particles and metal particles are attached to each other, or one is coated on the surface of the other, or may be physically or chemically bonded.
[0065] The aforementioned carbon particles may include natural graphite, artificial graphite, hard carbon, soft carbon, carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon nanotubes, fullerenes, carbon fibers, and fluorinated carbon.
[0066] The aforementioned metal particles are lithiophilic metals, such as Ni, Cu, Ag, Au, Pt, Al, Zn, and Bi, and may be one or more of these in combination. Introducing these lithium-philic metals is advantageous for forming a stable and uniform lithium layer on the surface of the current collector.
[0067] The negative electrode may be manufactured by mixing a binder solution and the composite particles to produce a slurry for forming a coating layer, and then applying and drying the slurry onto a negative electrode current collector. In this case, the binder may be a conventional binder used in the industry.
[0068] The solid electrolyte layer consists of a solid electrolyte in a layered structure, and the solid electrolyte is as described above. Therefore, the solid electrolyte may contain one or more selected from the group consisting of sulfide-based solid electrolytes, polymer-based solid electrolytes, and oxide-based solid electrolytes, and preferably contains a sulfide-based solid electrolyte.
[0069] As described above, the positive electrode active material configuration of this disclosure includes a coating portion containing the lithium titanium compound on the surface of the core portion, thereby preventing the lithium metal oxide, which is the positive electrode active material, from coming into direct contact with the solid electrolyte, reducing side reactions between the positive electrode active material and the solid electrolyte, and thereby reducing interfacial resistance. Furthermore, by including not only the lithium metal oxide, which is the positive electrode active material, but also the lithium titanium compound in the core portion, the long-term life characteristics of the all-solid-state battery can be improved. More specifically, when an all-solid-state battery is operated for several hundred cycles or more, side reactions occur from the outermost surface even if the positive electrode active material configuration includes a coating layer, but by including the lithium titanium compound in the core portion, this can be prevented, and the long-term life characteristics of the all-solid-state battery can be improved.
[0070] The present disclosure will be further described below with reference to examples, but these examples are for illustrative purposes only and the scope of the present disclosure is not limited to them.
[0071] < Manufacturing of positive electrode active material components for all-solid-state batteries > Example 1. LiOH·H2O and Ni 0.8 Co 0.1 Mn 0.1 (OH)2 was mixed in a weight ratio of 1.05:1, and then titanium isopropoxide was added. The mixture was placed in a stainless steel crucible and heat-treated at a temperature of 750°C at a heating rate of 3°C / min in an air atmosphere for 10 hours until the particle size (D 50 ) manufactured a 5μm positive electrode active material configuration.
[0072] The positive electrode active material configuration of the above-described embodiment 1 is a core-shell structure including a core portion and a coating portion on the surface of the core portion, wherein the core portion is made of LiNi 0.8 Co 0.1 Mn 0.1The material contained O2 and a lithium titanium compound, exhibiting a concentration gradient in which the titanium concentration decreased from the outermost surface of the core towards the center. The coating also contained a lithium titanium compound, with the amount of the lithium titanium compound in the coating being 0.5 parts by weight based on 100 parts by weight of the core.
[0073] Comparative Example 1. LiOH·H2O and Ni 0.8 Co 0.1 Mn 0.1 (OH)2 was mixed in a weight ratio of 1.1:1, and the mixture was placed in a stainless steel crucible and subjected to primary heat treatment at 600°C in an air atmosphere for 5 hours to form a plastic mixture, after which it was cooled. After that, it was crushed and sieved, and the crushed plastic mixture was placed in an aluminum crucible and subjected to secondary heat treatment at 800°C in an air atmosphere for 10 hours to form a particle size (D 50 ) is 5μm LiNi 0.8 Co 0.1 Mn 0.1 O2 was produced.
[0074] The LiSu 0.8 Co 0.1 Mn 0.1 O2 powder, titanium isopropoxide, and lithium ethoxide were added to ethanol and mixed for 24 hours. The mixture was then vacuum-dried to remove the ethanol solvent.
[0075] The positive electrode active material was manufactured by charging a circular furnace (tube furnace) with an inner diameter of 50 mm and a length of 1000 mm, and then heat-treating it at 400°C for 4 hours.
[0076] The positive electrode active material configuration of Comparative Example 1 is a core-shell structure including a core portion and a coating portion on the surface of the core portion, wherein the core portion is made of LiNi 0.8 Co 0.1 Mn 0.1 The material contains O2, and the coating portion contains a lithium titanium compound, with the lithium titanium compound in the coating portion being present in an amount of 0.5 parts by weight based on 100 parts by weight of the core portion.
[0077] Comparative Example 2. LiOH·H2O and Ni 0.8 Co 0.1 Mn 0.1 (OH)2 were mixed at a weight ratio of 1.05:1, and then titanium isopropoxide was added. The mixture was placed in a stainless steel crucible and heat-treated at a heating rate of 0.5°C / min at 650°C in an air atmosphere for 20 hours to prepare a positive electrode active material composition having a particle diameter (D 50 ) of 5 μm.
[0078] The positive electrode active material composition of Comparative Example 2 had a core-shell structure including a core portion and a coating portion on the surface of the core portion, and the core portion was made of LiNi 0.8 Co 0.1 Mn 0.1 O2 and a lithium titanium compound, but did not exhibit a concentration gradient in which the concentration of titanium decreases from the outermost surface of the core portion toward the center portion. In addition, the coating part included a lithium titanium compound, and the lithium titanium compound in the coating part was included in an amount of 0.5 parts by weight based on 100 parts by weight of the core part.
[0079] Experimental Example 1. Component analysis of the core and coating portions of the positive electrode active material. Using SEM-EDS (Scanning electron microscope energy dispersive spectrometer), the cross-section of the positive electrode active material composition prepared in Example 1, Comparative Example 1, and Comparative Example 2 was analyzed, and the content of titanium (Ti) distributed from the outermost surface of the coating part and the core part toward the center part was confirmed for each section, and the results are shown in Table 1 below. [Table 1]
[0080] From the results in Table 1, it was found that in Comparative Example 1, the lithium titanium compound was measured only in the coating portion because the core portion of the positive electrode active material configuration did not contain a lithium titanium compound. In Example 1 and Comparative Example 2, lithium titanium compounds were present in both the coating portion and the core portion of the positive electrode active material configuration. In the core portion of the positive electrode active material configuration of Example 1, the titanium concentration decreased from the outermost surface towards the center. On the other hand, in the positive electrode active material configuration of Comparative Example 2, titanium did not show a concentration gradient in the core portion, indicating that titanium was uniformly distributed in the core portion.
[0081] Experimental Example 2. Measurement of Life Characteristics of All-Solid-State Batteries 81.9% by weight of the positive electrode active material, 15.6% by weight of the solid electrolyte (Li6PS5Cl, LPS), 1.5% by weight of the conductive material (carbon black powder), and 1% by weight of the binder (PTFE) from Example 1, Comparative Example 1, and Comparative Example 2 were primary-mixed for 1 minute at 5000 rpm without solvent using a Lab Blender (Waring). Subsequently, a shear force of 100 N was applied to the mixture for high-shear mixing (using PBV-0.1L, Irie Shokai), and secondary mixing was performed to produce a dough. A free-standing positive electrode active material layer was produced from the dough using a Two-roll mill MR-3 (Inoue).
[0082] The positive electrode was manufactured by positioning the positive electrode active material layer on one surface of an aluminum current collector with a thickness of 15 μm and applying pressure.
[0083] All-solid-state batteries (jig cells) for Example 1, Comparative Example 1, and Comparative Example 2 were manufactured by using a 40 μm thick lithium metal negative electrode, interposing a 50 μm thick Li6PS5Cl solid electrolyte membrane between the positive and negative electrodes, and then pressurizing them at a pressure of 500 MPa to produce a drive pressure of 3 MPa and a capacity of 5 mAh.
[0084] The all-solid-state batteries of Example 1, Comparative Example 1, and Comparative Example 2 were charged at a rate of 0.33C until the voltage reached 4.25V (vs.Li), and then cut-off was performed at a rate of 0.1C while maintaining the voltage of 4.25V (vs.Li). Subsequently, one discharge cycle was performed at a rate of 0.33C (C-rate) until the voltage reached 3.0V (vs.Li). The capacity retention rate of the discharged capacity was measured after repeating the charge-discharge cycle 50 times, and the results are shown in Table 2 below. [Table 2]
[0085] As shown in Table 2 above, the all-solid-state batteries in Example 1 and Comparative Example 1 showed similar results in initial capacity and initial efficiency, but differed in lifespan characteristics. From this, it was found that including a lithium titanium compound in the core portion of the positive electrode active material configuration results in superior lifespan characteristics.
[0086] Furthermore, the all-solid-state battery in Comparative Example 2 showed poor results in initial capacity, initial efficiency, and lifespan characteristics. From this, it was found that even if a lithium titanium compound is present in the core of the positive electrode active material, if there is no concentration gradient in which the titanium concentration decreases from the outermost surface to the center of the core, the initial capacity, initial efficiency, and lifespan characteristics will all be poor.
[0087] The positive electrode active material configuration of this disclosure includes a lithium titanium compound in the coating portion and the core portion. In particular, the lithium titanium compound in the core portion has a concentration gradient in which the titanium concentration decreases from the outermost surface of the core portion toward the center. This results in excellent initial capacity, initial efficiency, and life characteristics for all-solid-state batteries containing this configuration.
Claims
1. Core portion containing positive electrode active material and lithium titanium compound; and A coating portion located on the surface of the core portion and containing a lithium titanium compound; The core portion has a concentration gradient in which the titanium concentration decreases from the outermost surface towards the center, providing a positive electrode active material configuration for an all-solid-state battery.
2. The positive electrode active material configuration for an all-solid-state battery according to claim 1, wherein the diameter of the core portion is 3 to 10 μm.
3. The positive electrode active material configuration for an all-solid-state battery according to claim 1, wherein the lithium titanium compound is present within a distance of 5 μm from the outermost surface of the core towards the center of the core.
4. The positive electrode active material of the core is a lithium metal oxide. The positive electrode active material configuration for an all-solid-state battery according to claim 1, wherein the lithium metal oxide is a secondary particle formed by the aggregation of a plurality of primary particles.
5. The primary particles separate from adjacent primary particles within the secondary particles, forming internal voids. The lithium titanium compound in the core portion is present in the internal void, as described in claim 4 for the positive electrode active material configuration for an all-solid-state battery.
6. The coating portion contains the lithium titanium compound in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the core portion, wherein this is the positive electrode active material configuration for an all-solid-state battery according to claim 1.
7. The positive electrode active material configuration for an all-solid-state battery according to claim 1, wherein the concentration of titanium present in the coating portion is higher than the concentration of titanium present in the core portion.
8. A positive electrode configuration for an all-solid-state battery comprising a positive electrode active material, a solid electrolyte, a conductive material, and a binder as described in any one of claims 1 to 7.
9. A solid-state battery configuration comprising a positive electrode; a negative electrode; and a solid electrolyte layer between the positive electrode and the negative electrode, as described in claim 8.
10. The all-solid-state battery configuration according to claim 9, wherein the solid electrolyte includes one or more selected from the group consisting of sulfide-based solid electrolytes, polymer-based solid electrolytes, and oxide-based solid electrolytes.
11. The all-solid-state battery configuration according to claim 10, wherein the solid electrolyte includes a sulfide-based solid electrolyte.
Citation Information
Patent Citations
KR2017-0074624