Silanol-functionalized polyolefins
The synthesis of silanol-functionalized polyolefins is achieved through a thermal process combining silyl hydride-functionalized polyolefin with peroxy acid, addressing catalyst incompatibilities and cost issues, resulting in efficient and controlled polar functionality.
Patent Information
- Application Number
- JP2026517958
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-27
- Filing Date
- 2024-09-27
- Publication Date
- 2026-11-24
AI Technical Summary
Existing methods for synthesizing polar polyolefins face challenges such as high capital intensity, branching issues, limited graftable monomers, incompatibility with catalysts, and the use of expensive and difficult-to-remove transition metal compounds, making it difficult to achieve controlled silanol functionality.
A method involving the combination of silyl hydride-functionalized polyolefin, peroxy acid, and optionally a solvent and neutralizing agent, under thermal conditions to form silanol-functionalized polyolefin, bypassing catalyst incompatibilities and additional reactions.
This approach allows for the controlled synthesis of silanol-functionalized polyolefins without the drawbacks of high capital costs and catalyst incompatibilities, providing a cost-effective and efficient method for introducing polar functionality.
Smart Images

Figure 2026539255000001 
Figure 2026539255000002 
Figure 2026539255000003
Abstract
Description
[Technical Field]
[0001] Embodiments of this disclosure relate to polyolefins, more specifically to silanol-functionalized polyolefins. [Background technology]
[0002] The synthesis of polar polyolefins has been a long-standing problem for at least some of the following reasons: Polar comonomers can copolymerize with ethylene monomers, but this is a capital-intensive, high-pressure process, and the resulting polymers have extensive branching and other property / compositional limitations. Radical grafting can be performed on high-density polyethylene or linear low-density polyethylene polymers, but the range of graftable monomers is limited, and heterogeneous mixtures of graft points and lengths (e.g., mono, oligo, polygrafts) are usually all that can be obtained. In addition, commercial in-reactor solution-phase polyolefin synthesis cannot tolerate polar monomers due to their incompatibility with catalysts.
[0003] Another approach involves incorporating the silane (-SiH) functional group "in-reactor," which is compatible with conventional catalysts but nonpolar, requiring additional reactions to obtain polar functionality. The simplest reaction of -SiH to obtain polar functionality is to obtain SiOH (silanol) through oxidation or hydrolysis. However, silanols are difficult to synthesize in a controlled manner without further condensation to Si-O-Si. Transition metal compounds can also be used (e.g., Pd, Ru, Ir, Cr, and Rh), but these compounds are expensive and require separation from the final reaction product, which is also a problem. Furthermore, several methods for silane hydrolysis using stoichiometric oxidizing agents such as dioxiranes and potassium permanganate have been reported. Unfortunately, dioxiranes are unstable and unsuitable for the temperatures required for polyolefin functionalization, and potassium permanganate is expensive, highly discolorative, and difficult to remove from the final product. Therefore, it is desirable to develop alternative, ideally in-reactor approaches for the synthesis of polar polyolefins that do not have these drawbacks. [Overview of the Initiative]
[0004] This disclosure provides various embodiments that address the above-mentioned drawbacks by providing a method for preparing silanol-functionalized polyolefins, comprising combining starting materials comprising A) a silyl hydride-functionalized polyolefin, optionally B) a solvent, C) a peroxy acid, and optionally D) a neutralizing agent, under thermal conditions for the synthesis of a silanol moiety, thereby forming a reaction mixture that produces a silanol-functionalized polyolefin having a silanol moiety under thermal conditions. As disclosed herein, the silyl hydride-functionalized polyolefin may comprise a silyl hydride moiety of formula I, -SiR2H Formula I (For example, including the silyl hydride moiety of formula I), where each R is independently selected from the group consisting of alkyl groups of 1 to 4 carbon atoms and aryl groups of 6 to 10 carbon atoms. As disclosed herein, each R can be methyl (for example, each R is methyl). In addition, as disclosed herein, a silyl hydride-functionalized polyolefin may contain 0.10% by weight (wt%) to 10% by weight of the silyl hydride moiety of formula I based on the total weight of the silyl hydride-functionalized polyolefin (for example, a silyl hydride-functionalized polyolefin may contain 0.10% by weight to 10% by weight of the silyl hydride moiety of formula I based on the total weight of the silyl hydride-functionalized polyolefin). In specific embodiments, the silyl hydride-functionalized polyolefin can be selected from the group consisting of silyl hydride-functionalized polyethylene and silyl hydride-functionalized polypropylene (for example, the silyl hydride-functionalized polyolefin is selected from the group consisting of silyl hydride-functionalized polyethylene and silyl hydride-functionalized polypropylene). In one embodiment, the silyl hydride-functionalized polyolefin can be a branched silyl hydride-functionalized polyolefin (for example, the silyl hydride-functionalized polyolefin is a branched silyl hydride-functionalized polyolefin).
[0005] As disclosed herein, thermal conditions for resulting in the synthesis of a silanol moiety include melt-blending the reaction mixture at a temperature of 100°C to 180°C for a duration of 30 seconds to 60 minutes (for example, thermal conditions for resulting in the synthesis of a silanol moiety include melt-blending the reaction mixture at a temperature of 100°C to 180°C for a duration of 30 seconds to 60 minutes). As disclosed herein, the method can be carried out in the absence of a solvent (for example, it can be carried out). As disclosed herein, thermal conditions for resulting in the synthesis of a silanol moiety include dissolving the silyl hydride-functionalized polyolefin in solvent B) of the reaction mixture. As disclosed herein, thermal conditions for resulting in the synthesis of a silanol moiety include heating the reaction mixture at a temperature of 60°C to 120°C for a duration of 1 minute to 60 minutes. As disclosed herein, the method of this disclosure further includes separating the silanol-functionalized polyolefin from the reaction mixture.
[0006] As disclosed herein, peroxy acid is used in the method of this disclosure in an amount of 1 to 3 molar equivalents of peroxy acid, based on the silicon-bonded hydrogen content of A) silyl hydride-functionalized polyolefin. As disclosed herein, peroxyacetic acid can be selected from the group consisting of peracetic acid, meta-chloroperbenzoic acid, perbenzoic acid, and combinations thereof (e.g., selected). As disclosed herein, a neutralizing agent D) may be present in the reaction mixture (e.g., present). As disclosed herein, this disclosure provides silanol-functionalized polyolefins formed by the method disclosed herein. [Modes for carrying out the invention]
[0007] The following detailed description provides, among other things, approaches to the synthesis of polar polyolefins (e.g., in-reactor approaches). As discussed herein, typical commercial in-reactor solution-phase polyolefin synthesis cannot tolerate polar monomers due to their incompatibility with catalysts and therefore cannot produce polar polyolefins. Furthermore, while silane (-SiH) functional groups can be incorporated “in-reactor” and are compatible with conventional catalysts, they are nonpolar and require additional reactions to obtain polar functionality. The simplest reaction of silane to obtain polar functionality for polyolefins is to form silanols (-SiOH) through oxidation or hydrolysis of the silane. However, silanols are difficult to synthesize in a controlled manner without further condensation of Si-OH to Si-O-Si, which is unacceptable. In addition, transition metal compounds (e.g., Pd, Ru, Ir, Cr, and Rh) can be used in these processes, but they are expensive and need to be separated from the final reaction product. Furthermore, silane hydrolysis methods using stoichiometric oxidizing agents such as dioxirane are unstable and unsuitable for the temperatures required for polyolefin functionalization, while methods using potassium permanganate are too expensive, highly discolored, and contain by-products that are difficult to remove.
[0008] Depending on the drawbacks discussed herein, embodiments of the present disclosure provide a method for preparing a silanol-functionalized polyolefin, comprising combining starting materials comprising A) a silyl hydride-functionalized polyolefin, optionally B) a solvent, C) a peroxy acid, and optionally D) a neutralizing agent, under thermal conditions for the synthesis of a silanol moiety, thereby forming a reaction mixture that produces a silanol-functionalized polyolefin having a silanol moiety under thermal conditions.
[0009] As used herein, "optionally" means "including or not including." For example, "optionally, solvent" means including or not including the solvent.
[0010] Unless otherwise stated, implied by the context, or customary in the art, all parts and percentages are based on weight, and all test methods are current as of the filing date of this disclosure.
[0011] Where used herein, “a,” “an,” and “the” are used following open-ended terms such as “comprising” to mean “at least one.” In any aspect or embodiment of the Disclosure described herein, the term “about” in a numerical phrase may be omitted to give another aspect or embodiment of the Disclosure. In the original aspect or embodiment in which the term “about” is used, the meaning of “about” may be interpreted from the context of its use.
[0012] The terms “comprising,” “including,” and “having,” and their derivatives, are not intended to exclude the existence of any additional components, processes, or procedures, whether or not they are specifically disclosed. To avoid any doubt, all compositions claimed through the use of the term “comprising” may, unless otherwise stated, include any additional additives, adjuvants, or compounds, whether polymeric or not. In contrast, the term “consisting essentially of” excludes any other components, processes, or procedures from the scope of any subsequent description, except those not essential to operability. The term “consisting of” excludes any components, processes, or procedures not specifically described or listed.
[0013] Preferably, “approximately” means 90 percent to 100 percent of a number, 100 percent to 110 percent of a number, or 90 percent to 110 percent of a number. In any aspect or embodiment of the Disclosure described herein, open-ended terms such as “comprising,” “comprises” (synonymous with “including,” “having,” and “characterized by”) may be replaced by their respective partially closed phrases such as “consisting essentially of,” “consists essentially of,” or their respective closed phrases such as “consisting of,” “consists of,” to give another aspect or embodiment of the Disclosure. Partially closed phrases such as “consisting essentially of” limit the claims to materials or processes enumerated herein and materials or processes that do not substantially affect the basic and novel features of the claimed Disclosure. The term “characterized” means open-ended and distinguishable.
[0014] As used herein, the term “composition” includes mixtures of materials comprising the composition, as well as reaction and decomposition products formed from the materials of the composition. Any reaction or decomposition products are typically present in trace or residual amounts.
[0015] As used herein, the term “polymer” refers to a polymer compound prepared by polymerizing monomers, whether of the same or different types. Thus, the general term polymer includes the terms homopolymer (used to refer to a polymer prepared from only one type of monomer, under the understanding that trace amounts of impurities may be incorporated into the polymer structure) and interpolymer, as defined below. Trace amounts of impurities, such as catalyst residues, can be incorporated into and / or within the polymer. Typically, polymers are stabilized with one or more stabilizers in very small amounts ("ppm").
[0016] As used herein, the term “interpolymer” refers to a polymer prepared by the polymerization of at least two different types of monomers. Thus, the term interpolymer includes the term copolymer (used to refer to a polymer prepared from two different types of monomers) and polymers prepared from three or more different types of monomers (e.g., terpolymer).
[0017] As used herein, the term “olefinic polymer” means a polymer that, in its polymeric form, contains 50% by weight or more than half by weight percent of an olefin such as ethylene or propylene (based on the weight of the polymer), and may optionally contain one or more comonomers.
[0018] As used herein, the term “propylene polymer” means a polymer in which, in its polymerized form, contains 50% by weight or a majority by weight of propylene (based on the weight of the polymer) and may optionally contain one or more comonomers.
[0019] As used herein, the term “ethylene-based polymer” means a polymer in which, in its polymerized form, contains 50% by weight or more than half by weight of ethylene (based on the weight of the polymer) and may optionally contain one or more comonomers.
[0020] As used herein, the term "ethylene / alpha-olefin interpolymer" refers to a random interpolymer in which, in its polymerized form, comprises 50% by weight or more than half by weight of ethylene and alpha-olefin (based on the weight of the interpolymer).
[0021] As used herein, the term "ethylene / alpha-olefin copolymer" refers to a random copolymer in which, in its polymerized form, ethylene and alpha-olefin are present in 50% by weight or more than half by weight (based on the weight of the copolymer) as only two monomers.
[0022] As used herein, the term "propylene / alpha-olefin interpolymer" refers to a random interpolymer comprising, in its polymerized form, 50% by weight or more than half by weight of propylene and alpha-olefin (based on the weight of the interpolymer).
[0023] As used herein, the term "propylene / alpha-olefin copolymer" refers to a random copolymer in which, in its polymerized form, propylene and alpha-olefin are present in 50% by weight or more than half by weight (based on the weight of the copolymer) as only two monomers.
[0024] As used herein, the term “silyl hydride-functionalized polyolefin” refers to a random interpolymer in polymerization form comprising 50% by weight or more than half by weight of an olefin and a silane monomer (based on the weight of the interpolymer). As used herein, the interpolymer comprises at least one Si-H group, and the phrase “at least one Si-H group” refers to the type of “Si-H” group. In the art, it is understood that an interpolymer may contain a number of these groups. Silyl hydride-functionalized polyolefins are formed by copolymerization of at least an olefin (e.g., ethylene and / or propylene) and a silane monomer (e.g., using a bis-biphenyl-phenoxy metal complex), as provided herein. An example of a silane monomer is shown in Formula 1, as described herein.
[0025] As used herein, the term “ethylene / silane interpolymer” refers to a random interpolymer in polymerization form comprising 50% by weight or more than half by weight of ethylene and silane monomer (based on the weight of the interpolymer). As used herein, the interpolymer includes at least one Si-H group and the phrase “at least one Si-H group,” as discussed above. Ethylene / silane interpolymers are formed by copolymerization of at least ethylene and silane monomer.
[0026] As used herein, the term “ethylene / alpha-silylhydride functionalized polyolefin” refers to a random interpolymer in polymerization form comprising 50% by weight or more than half by weight of ethylene, alpha-olefin, and silane monomer (based on the weight of the interpolymer). As used herein, these interpolymers contain at least one Si-H group, as discussed above. Ethylene / silane interpolymers are formed by copolymerization of at least ethylene, alpha-olefin, and silane monomer.
[0027] As used herein, the term “ethylene / alpha-olefin / silant polymer” refers to a random terpolymer in which, in its polymerized form, ethylene, alpha-olefin, and silane monomers are present in 50% by weight or more than half by weight (based on the weight of the terpolymer) as only three monomers. As used herein, the terpolymer contains at least one Si-H group, as discussed above. Ethylene / silant polymers are formed by copolymerization of ethylene, alpha-olefin, and silane monomers.
[0028] In this application, when referring to a preceding listing of elements (e.g., components), phrases such as “their mixture” or “their combination” mean any two or more (including all) of the listed elements. The term “or” used in listing members, unless otherwise stated, refers to the listed members individually and in any combination, and supports additional embodiments that list any one of the individual members (for example, in embodiments that list the phrase “10 percent or more,” “or” supports another embodiment that lists “10 percent,” and yet another embodiment that lists “greater than 10 percent”). The term “plural” means two or more, and each plural is selected independently unless otherwise indicated. Terms such as “first,” “second,” etc., serve as a convenient means of distinguishing two or more elements or limitations (e.g., the first chair and the second chair) and do not mean quantity or order unless specifically indicated. The symbols “<” and “>” mean less than or equal to, and greater than or equal to, respectively. The symbols "<" and ">" mean "less than" and "greater than," respectively.
[0029] As used herein, the term “alkyl group” means unsubstituted or at least one R sThis refers to saturated linear or branched (if possible) hydrocarbon radicals of the provided number of carbon atoms that are substituted by R. Therefore, for example, alkyl groups of 1 to 4 carbon atoms include, but are not limited to, methyl, ethyl, 1-propyl, 2-propyl, 1-butyl, 2-butyl, 2-methylpropyl, and 1,1-dimethylethyl. Examples of substituted alkyl groups of 1 to 4 carbon atoms include, but are not limited to, those with at least one hydrogen atom and one R s Replaced by each R s Examples provided herein include those in which the elements are independently halogen atoms.
[0030] As used herein, the term “aryl group” means an unsubstituted or substituted ring carbon atom (at least one R) of 6 to 10 carbon atoms. s This refers to monocyclic or bicyclic aromatic hydrocarbon radicals (e.g., aryl groups of 6 to 10 carbon atoms), where each monocyclic or bicyclic radical contains one or two rings, one and two rings being aromatic, and the two rings being condensed or uncondensed to one ring. Examples of substituted aryl groups of 6 to 10 carbon atoms include, but are not limited to, groups with at least one hydrogen atom in one R s Replaced by each R s Examples provided herein include those in which the elements are independently halogen atoms.
[0031] As used herein, the term “silyl hydride-functionalized polyolefin” is used to describe either a polyolefin copolymer formed using alpha-olefin monomers and alpha-silyl monomers, or b) a polyolefin terpolymer formed using alpha-olefin monomers, olefin comonomers, and alpha-silyl monomers. As used herein, the term “alpha-olefin monomer” may include ethylene (CH2=CH2), propylene (CH2=CH2-CH3), or a combination thereof. As used herein, the term “olefin comonomer” may include vinyl acetate, 1-butene, 2-butene, iso-butene, styrene, acrylic acid, methyl acrylate, vinyl chloride, 1-hexene, 1-octene, and dienes such as butadiene and isoprene. Other olefin comonomers are also possible. In addition, the silyl hydride-functionalized polyolefins of this disclosure may be formed as block copolymers / terpolymers or as random copolymers / terpolymers, as considered herein.
[0032] As discussed herein, the method disclosed herein provides thermal conditions for the synthesis of the silanol moiety. A) Silyl hydride-functionalized polyolefins, Optionally, B) Solvent, C) Peroxy acid, Optional: D) Neutralizing agent This invention relates to the preparation of silanol-functionalized polyolefins, including the combination of starting materials. As discussed herein, by combining the above-mentioned starting materials, a reaction mixture is formed to produce a silanol-functionalized polyolefin having a silanol moiety according to the present disclosure under the thermal conditions discussed herein. Each of the starting materials A), C), and optionally B) and / or D) listed above, along with the thermal conditions for resulting in the synthesis of the silanol moiety, is discussed herein. In the present disclosure, the preparation of the silanol-functionalized polyolefin according to the present disclosure is carried out without a catalyst or in the presence of a catalyst.
[0033] Silyl hydride-functionalized polyolefins The silyl hydride-functionalized polyolefins of this disclosure can be prepared in accordance with any one of U.S. Patent Publication No. 2023 / 0272206, U.S. Patent No. 6,624,254, International Publication Nos. 2012 / 027448, 2012 / 027448, and 1995 / 000526, each of which is incorporated herein by reference in whole.
[0034] In this disclosure, a silyl hydride-functionalized polyolefin comprises at least one of the silyl hydride moieties of formula I, -SiR2H Formula I In the formula, each R is independently selected from the group consisting of alkyl groups of 1 to 4 carbon atoms and aryl groups of 6 to 10 carbon atoms (both as defined herein). Preferably, each R is a methyl group. In this disclosure, the silyl hydride-functionalized polyolefin contains 0.10 wt percent (W%) to 10 wt percent of the silyl hydride moiety of formula I, based on the total weight of the silyl hydride-functionalized polyolefin. All individual values and sub-ranges of 0.10 wt percent to 10 wt percent are included, for example, the Wt% of the silyl hydride moiety of formula I can have a lower limit of 0.10, 0.20, 0.40, or 1.0 wt percent to an upper limit of 10, 8, 6, or 4 wt percent, based on the total weight of the silyl hydride-functionalized polyolefin.
[0035] In this disclosure, the silyl hydride-functionalized polyolefin is selected from the group consisting of silyl hydride-functionalized polyethylene and silyl hydride-functionalized polypropylene. In addition, the silyl hydride-functionalized polyolefin may be a branched silyl hydride-functionalized polyolefin. For example, the silyl hydride-functionalized polyolefin may be a branched silyl hydride-functionalized polyethylene or a branched silyl hydride-functionalized polypropylene.
[0036] In this disclosure, the silyl hydride moiety of formula I is derived from a silane monomer selected from formula II.
[0037] [ka] In the formula, A is an alkenyl group having 2 to 12 carbon atoms, B is a hydrocarbyl group having 1 to 10 carbon atoms, R is as defined above, H is hydrogen, and x is 0 to 10. In this disclosure, x can be 0 to 8, or 0 to 6, or 0 to 4, or 0 to 2, or 0 or 1, or 0. In this disclosure, A can be a C2-C12 alkenyl group, a C2-C8 alkenyl group, a C2-C6 alkenyl group, or a C2-C4 alkenyl group. In one embodiment, or a combination of two or more embodiments, each of which is described herein, formula II can be selected from the following compounds a) to h).
[0038] [ka]
[0039] Some examples of silane monomers of formula II include hexenylsilane, allylsilane, vinylsilane, octenylsilane, hexenyldimethylsilane, octenyldimethylsilane, vinyldimethylsilane, vinyldiethylsilane, vinyldi(n-butyl)silane, vinylmethyloctadecylsilane, allyldimethylsilane, allyldiethylsilane, allyldi(n-butyl)silane, allylmethyloctadecylsilane, and bishexenylsilane. Mixtures of the aforementioned alkenylsilanes may also be used. More specific examples of silane monomers of formula II include 5-hexenyl-dimethylsilane (HDMS), 7-octenyldimethylsilane (ODMS), allyldimethylsilane (ADMS), 3-butenyldimethylsilane, 1-(buta-3-en-1-yl)-1,1,3,3-tetramethyldisiloxane (BuMMH), and 1-(hexa-5-en-1-yl)-1,1,3,3-tetramethyldisiloxane (HexMMH). Mixtures of the aforementioned alkenylsilanes may also be used.
[0040] Additional monomers used in the formation of the silylhydride-functionalized polyolefins of this disclosure include addition polymerizable monomers comprising olefins or mixtures of olefins and diolefins. The most preferred olefin is C 2-20 The material is an α-olefin or a mixture thereof, most preferably ethylene, propylene, or a mixture of ethylene and propylene, 1-butene, 1-hexene, or 1-octene.
[0041] The process for forming the silyl hydride-functionalized polyolefins of this disclosure using monomers of formula II may be carried out under slurry, solution, bulk, gas phase, or suspension polymerization conditions, or other suitable reaction conditions. Polymerization may be carried out at a temperature of 0°C to 180°C, preferably 25°C to 170°C, for a sufficient time to produce the desired polymer. Typical reaction times are 1 minute to 100 hours, preferably 1 to 10 hours. The optimal reaction time or reactor residence time will vary depending on the temperature, solvent, and other reaction conditions used. Polymerization may be carried out at pressures below atmospheric pressure and above atmospheric pressure, preferably in the range of 1 to 800 psig (6.9 kPa to 5,515 kPa).
[0042] Suitable catalysts and co-catalysts for use herein are preferably those provided in International Publication Nos. 2012 / 027448, 2012 / 027448, and 1995 / 000526. Examples of such catalysts and co-catalysts are provided in the Examples section herein. For example, a catalyst may include the following structure:
[0043] [ka] In the formula, M is one metal from groups 3-6 of the periodic table, and metal M is in a formal oxidation state of +2, +3, +4, +5, or +6; n is an integer from 0 to 5, and when n is 0, X is absent; each X is independently a monodentate ligand that is neutral, monoanionic, or dianionic; or two Xs together form a bidentate ligand that is neutral, monoanionic, or dianionic; X and n are selected such that the metal-ligand complex of formula (I) as a whole is neutral; each Z is independently O, S, N(Ci-C4g) hydrocarbyl, or P(C j -C4Q)hydrocarbyl, where L is (Ci-C4Q)hydrocarbylene or (Ci-C4Q)heterohydrocarbylene. (C1-C40) hydrocarbylene has a moiety containing a linker skeleton of 1 carbon atom to 18 carbon atoms connecting the Z atoms in formula (I), and (C1-C40) heterohydrocarbylene has a moiety containing a linker skeleton of 1 atom to 12 atoms connecting the Z atoms in formula (I), wherein each of the 1 to 18 atoms in the linker skeleton of 1 atom to 18 atoms of (C1-C40) heterohydrocarbylene is independently a carbon atom or a heteroatom, and each heteroatom is independently O, S, S(O), S(O)2, Si(R c )2, P(R P ), or N(R N ), and each R is independently c is unsubstituted (C1-C18) hydrocarbyl, each R p is unsubstituted (C1-C18) hydrocarbyl, each R N is unsubstituted (C1-C18) hydrocarbyl or is absent, and each of R^ a , R^ a , R^b, and R^b is independently a hydrogen atom (C r C 40 ) hydrocarbyl; (C r C 40 ) heterohydrocarbyl; -; Si(R c )3; O(R C ); S(R C ); N(R N )2; P(R P )2, or a halogen atom, R 6c , R 7c , and R 8c at least one of, and R 6d , R 7d , and R 8d at least one of is independently (C2-C40) hydrocarbyl, Si(R c )3, and R^ c , R 7c , R 8c , R 6d , R 7d , and R 8d each of the others is independently a hydrogen atom; (C1-C40) hydrocarbyl; (C r C40) heterohydrocarbyl; -; Si(Rc )3;0(R C );S(R C );N(R N )2, and P(R P )2 or halogen atoms, optionally two or more R groups (R^ a ~R 8d These can combine to form a ring structure, which has 3 to 50 atoms in the ring, without considering hydrogen atoms. The molar ratio of polymerizable monomer to catalyst is 100:1 to 1 × 10⁻⁶. 10 :1, preferably 1000:1~1×10 6 It can be in the range of :1.
[0044] Another example of a suitable catalyst is the following:
[0045] [ka] In the formula, each instance of R' is independently selected from hydrogen, hydrocarbyl, silyl, germyl, cyano, halo, and combinations thereof, and the R' has up to 20 nonhydrogen atoms, and optionally two R' groups (if R' is not hydrogen, halo, or cyano) come together to form a fused ring structure by forming its divalent derivative bonded adjacent to the cyclopentadienyl ring, and X is a neutral q having up to 30 nonhydrogen atoms that forms a π complex with M. 4 -A bonded diene group, where Y is -0-, -S-, -NR * -,-PR * - and M is titanium or zirconium in a +2 formal oxide state, Z * is SiR * 2. CR * 2. SiR * 2SiR * 2. CR * 2CR I 2CR * =CR * CR * 2SιR * 2, or GeR * 2, R *Each instance of R is independently selected from hydrogen, or hydrocarbyl, silyl, alkyl halide, aryl halide, and combinations thereof, and * It has up to 10 non-hydrogen atoms, and optionally, 2 R * Base, or Z * R from * Base, and R from Y * (R * If (is not hydrogen), a ring system is formed. The molar ratio of polymerizable monomer to catalyst is 100:1 to 1 × 10⁻⁶. 10 :1, preferably 1000:1~1×10 6 It can be in the range of :1.
[0046] The support may optionally be present in the catalyst formulation, particularly in gas-phase or slurry polymerization. Suitable supports include any inert granular material, most preferably a metal oxide, preferably alumina, silica, or aluminosilicate material. Suitable particle sizes are 1 to 1000 μm, preferably 10 to 100 μm. The most desired support is calcined silica, which can be treated to reduce surface hydroxyl groups by reaction with silane or a similar reactive compound. Any suitable means may be used to include such a support in the catalyst formulation, for example, by spraying or coating the support with such a liquid and then removing the liquid by dispersing the components in a liquid and bringing it into contact with the support and then drying, or by co-precipitating the co-catalyst and support material from the liquid medium.
[0047] Polymerization can be carried out in the presence or absence of an inert diluent or solvent, i.e., in the presence of an excess monomer. Examples of suitable diluents or solvents include C 6-20 Examples include aliphatic, alicyclic, aromatic, and halogenated aliphatic or aromatic hydrocarbons, as well as mixtures thereof. Preferred diluents are C 6-10The compound contains alkanes, toluene, and mixtures thereof. Particularly preferred diluents for polymerization are iso-octane, iso-nonane, or blends thereof such as Isopar-E®, available from Exxon Chemical Company. A suitable amount of solvent is used to provide monomer concentrations of 5% to 100% by weight. Polymerization can be carried out in the presence of hydrogen.
[0048] Polymerization is preferably carried out as continuous polymerization (where catalyst components, monomers, and optionally a solvent are continuously supplied to the reaction zone, and the polymer product is continuously removed therefrom). When used in this context, the terms “continuous” and “continuously” refer to processes in which there is intermittent addition of reactants and removal of products at regular intervals, and therefore the overall process is continuous over time.
[0049] In this disclosure, silyl hydride-functionalized polyolefins are defined as having a concentration of 10,000 g / mol or more, or 12,000 g / mol or more, or 14,000 g / mol or more, or 16,000 g / mol or more, or 18,000 g / mol or more, or 20,000 g / mol or more, or 22,000 g / mol or more, or 24,000 g / mol or more, 26,000 g / mol or more, or 28,000 g / mol or more, or 30,000 g / mol or more, or 32,000 g / mol or more. It can have a number-average molecular weight (Mn) of 100,000 g / mol or less, or 95,000 g / mol, or 90,000 g / mol, or 85,000 g / mol or less, or 80,000 g / mol or less, or 75,000 g / mol, or 70,000 g / mol or less, or 68,000 g / mol or less, or 66,000 g / mol or less, or 64,000 g / mol or less, or 62,000 g / mol or less, or 60,000 g / mol or less. In this disclosure, the silyl hydride-functionalized polyolefin is defined as having a concentration of 20,000 g / mol or more, or 25,000 g / mol or more, or 30,000 g / mol or more, or 35,000 g / mol or more, or 40,000 g / mol or more, or 45,000 g / mol or more, or 50,000 g / mol or more, or 52,000 g / mol or more, or 54,000 g / mol or more, or 56,000 g / mol or more, or 58,000 g / mol or more, or 60,000 g / mol or more, or 62,000 g / mol or more, up to 300,000 g / mol. It may have a weight-average molecular weight (Mw) of 250,000 g / mol or less, or 200,000 g / mol or less, or 190,000 g / mol or less, or 180,000 g / mol or less, or 170,000 g / mol or less, or 160,000 g / mol or less, or 150,000 g / mol or less, or 148,000 g / mol or less, or 146,000 g / mol or less, or 144,000 g / mol or less, or 142,000 g / mol or less, or 140,000 g / mol or less, or 138,000 g / mol or less.In this disclosure, silyl hydride-functionalized polyolefins may also have a molecular weight distribution (MWD = Mw / Mn) ranging from 1.5 or more, or 1.6 or more, or 1.7 or more, or 1.8 or more, or 1.9 or more, to 5.0 or less, or 4.5 or less, or 4.0 or less, or 3.5 or less, or 3.0 or less, or 2.9 or less, or 2.8 or less, or 2.7 or less, or 2.6 or 2.5, or 2.4 or less, or 2.3 or less. The techniques for measuring Mw and Mn are described in the Examples section of this specification.
[0050] In this disclosure, silyl hydride-functionalized polyolefins are defined as having a concentration of 0.855 g / cc or more, or 0.856 g / cc or more, or 0.857 g / cc or more, or 0.858 g / cc or more, or 0.859 g / cc or more, or 0.860 g / cc or more, or 0.861 g / cc or more, or 0.862 g / cc or more, or 0.863 g / cc or more, or 0.864 g / cc or more, or 0.865 g / cc or more, or 0.866 g / cc or more, or 0.867 g / cc or more (1 cc = 1 cm³) 3 The density can range from 0.950 g / cc or less, or 0.920 g / cc or less, or 0.900 g / cc or less, or 0.890 g / cc or less, or 0.888 g / cc or less, or 0.886 g / cc or less, or 0.884 g / cc or less, or 0.882 g / cc or less, or 0.880 g / cc or less, or 0.878 g / cc or less, or 0.876 g / cc or less, or 0.874 g / cc or less. The density measurement technique is as described in the Examples section.
[0051] In this disclosure, silyl hydride-functionalized polyolefins may have a melt index (I2) of 0.5 dg / min or more, or 1.0 dg / min or more, or 2.0 dg / min or more, or 5.0 dg / min or more, or 10 dg / min or more to 100 dg / min or less, or 50 dg / min or less, or 30 dg / min or less, or 20 dg / min or less, or 15 dg / min or less. The technique for measuring the melt index (I2) is described in the Examples section of this specification.
[0052] Thermal conditions for the synthesis of the silanol moiety In this disclosure, a method for preparing a silanol-functionalized polyolefin involves combining A), C), and optionally B) and / or D), under thermal conditions to produce a silanol-functionalized polyolefin having a silanol moiety as discussed herein. In embodiments, the thermal conditions include heating the reaction mixture to a temperature near or above the melting temperature (Tm) of the silylhydride-functionalized polyolefin, as discussed herein. For example, while forming a reaction mixture by combining A), C), and optionally B) and / or D), providing thermal conditions for producing a silanol-functionalized polyolefin having a silanol moiety can also be achieved by melt blending using a number of different devices. For various embodiments, a number of different devices are designed to heat, mix, and process a molten reaction mixture to produce a silanol-functionalized polyolefin having a silanol moiety as discussed herein. Examples of such devices include single-screw extruders, twin-screw extruders, internal batch mixers (e.g., Banbury mixers and Intermix mixers), and kneaders or Sigma-Blade mixers. Each device can provide heat in addition to the friction of mixing by the container or housing in which the reaction mixture is being processed. For example, a single-screw or twin-screw extruder may have a heating barrel for adding heat to the reaction mixture as needed.
[0053] As disclosed herein, the thermal conditions for resulting in the synthesis of the silanol moiety include combining (e.g., melt blending) the reaction mixture over a duration of 30 seconds to 60 minutes at a temperature of 100°C to 180°C, as considered herein. All individual values and subranges of 100°C to 180°C are included, for example, the thermal conditions can range from a lower limit of 100, 110, 120, or 130°C to an upper limit of 180, 170, 160, or 150°C. All individual values and subranges of duration (e.g., reaction time) are included, for example, the duration can range from a lower limit of 30, 60, 90, 120, or 150 seconds to an upper limit of 60, 45, 30, 20, 10, or 5 minutes. Any combination of the above individual values for temperature and duration is also possible.
[0054] B) Solvent As disclosed herein, the methods of this disclosure may also optionally use solvent B) to aid in the mixing of the starting materials A) and C) of the reaction mixture. For example, A) silyl hydride-functionalized polyolefin may be dissolved in solvent B) before combining A) silyl hydride-functionalized polyolefin and C) peroxy acid. The solvents that can be used herein are those that help in the fluidization of the starting materials A) and C) but do not react with the starting materials in an essential manner. The solvent may be selected based on the solubility of the starting materials A) and C) and the volatility of the solvent. Solubility refers to the solvent being sufficient to dissolve and / or disperse the starting materials (e.g., A)). Volatility refers to the vapor pressure of the solvent. For example, if the solvent is not sufficiently volatile (vapor pressure is too low), the solvent may be difficult to remove at the end of the process.
[0055] If present, the solvent is a nonpolar solvent that, in particular, helps to control the exothermic reaction of this method and can act to dissolve the silylhydride-functionalized polyolefin. Examples of suitable nonpolar solvents include C6-C 20 Examples include aliphatic, alicyclic, aromatic, and halogenated aliphatic or aromatic hydrocarbons, as well as mixtures thereof. Preferred nonpolar solvents include C6-C10 Examples include alkanes, toluene, and mixtures thereof. Particularly desirable nonpolar solvents for the synthesis of the silanol moiety are toluene, iso-octane, iso-nonane, or blends thereof such as Isopar-E®, available from Exxon Chemical Company.
[0056] B) If a solvent is present, the thermal conditions for resulting in the synthesis of the silanol moiety include dissolving the silyl hydride-functionalized polyolefin in solvent B) of the reaction mixture. The amount of solvent depends on various factors, including the type of solvent selected, as well as the amount and type of other starting materials selected for use in the method. In this disclosure, a suitable solvent-to-silyl hydride-functionalized polyolefin ratio for dissolving the silyl hydride-functionalized polyolefin in solvent B) can be in the range of 15:1 to 1:1 (milliliters of solvent:grams of silyl hydride-functionalized polyolefin). As disclosed herein, the thermal conditions for resulting in the synthesis of the silanol moiety when solvent B) is present in the reaction mixture include heating the reaction mixture at a temperature of 60°C to 120°C for a duration of 1 minute to 60 minutes. All individual values and subranges from 60 to 120°C are included; for example, thermal conditions can range from a lower limit of 60, 65, 70, or 75°C to an upper limit of 120, 115, 110, 105, or 100°C. For duration (e.g., reaction time), all individual values and subranges from 1 to 60 minutes are included; for example, duration can range from a lower limit of 1, 2, 3, 4, or 5 minutes to an upper limit of 60, 45, 30, 20, or 10 minutes. Any combination of the above individual values for temperature and duration is also possible.
[0057] In one embodiment, the method of the present disclosure, as discussed herein, is carried out in the absence of solvent B). Thus, for example, the melt blending of the reaction mixture under thermal conditions to result in the synthesis of a silanol moiety, as discussed herein, can be carried out in the absence of the solvent (e.g.).
[0058] C) Peroxy acid As disclosed herein, a method for preparing silanol-functionalized polyolefins involves the use of peroxy acids. As used herein, peroxy acids are a class of organic compounds containing a peroxide group (OO) bonded to a carboxylic acid group (-COOH), thereby making peroxy acids oxidizing agents. While we do not wish to be bound by theory, it is assumed that peroxy acids act as oxidizing agents, thereby forming the silanol (Si-OH) moiety from the Si-H moiety of the starting material A) of the method described herein. In this disclosure, peroxy acids are selected from the group consisting of peracetic acid, meta-chloroperbenzoic acid, perbenzoic acid, and combinations thereof. In particular, the use of peracetic acid for -SiH to -SiOH conversion is surprising, as peracetic acid is typically considered a milder oxidizing agent and is therefore expected to give somewhat poorer reaction efficiency. Another surprising result of this disclosure is that for peroxy acids, the molecular weight change (crosslinking) at the high temperature required for the reaction is small. Thus, the results of this disclosure are surprising in that peracetic acid is effective for this conversion.
[0059] In this disclosure, the amount of peroxy acid used in a method for preparing a silanol-functionalized polyolefin comprises 1 to 3 molar equivalents of peroxy acid, based on A) the silicon-bonded hydrogen content of the silyl hydride-functionalized polyolefin. Other ranges for the amount of peroxy acid used in a method for preparing a silanol-functionalized polyolefin are also possible. For example, the amount of peroxy acid used in a method for preparing a silanol-functionalized polyolefin may include not only 1 to 3, but also 1.2 to 2, 1.2 to 3, or 2 to 3 molar equivalents of peroxy acid, based on A) the silicon-bonded hydrogen content of the silyl hydride-functionalized polyolefin. As used herein, the molar equivalent of peroxy acid based on the silicon-bonded hydrogen content of the silyl hydride-functionalized polyolefin is the molar amount of peroxy acid used in the method to react with 1 mole of -SiH moiety present in the silyl hydride-functionalized polyolefin (e.g., 1 to 3 moles of peroxy acid).
[0060] In this disclosure, peroxy acids can be used as is or as aqueous solutions. When used in aqueous solutions, the peroxy acid is present in an amount of 5 to 50% by weight based on the total weight of the aqueous solution. In this disclosure, the discovery that aqueous peracetic acid is a stoichiometric oxidizing agent for synthesizing -SiH to -SiOH is remarkable. For example, the use of aqueous peracetic acid as described herein allows for a high conversion rate from -SiH to -SiOH with a short reaction time (less than 20 minutes) and at the high temperatures required for melting or solution functionalization, and such reactions can be carried out in the molten state of the polymer in the presence of any nonpolar solvent such as toluene or others provided herein. In addition, the peroxy acids provided herein are commercially available. Furthermore, the peroxy acids in this disclosure are decomposable into relatively safe and volatile by-products (e.g., which can be stripped) such as hydrogen peroxide, acetic acid, and water, making the method considerably "environmentally friendly." Low / controllable molecular weight growth during functionalization and stable molecular weight of the SiOH polymer during long-term storage.
[0061] An aqueous solution of peroxy acid may also contain other compounds to adjust the pH of the aqueous solution, such as other mineral acids, including acetic acid, sulfuric acid, nitric acid, phosphoric acid, perchloric acid, and hydrochloric acid. In this disclosure, the pKa of the peroxy acid in the aqueous solution may be in the range of 4 to 10.
[0062] D) Neutralizing agent As disclosed herein, the method of this disclosure may also optionally use a neutralizing agent D) in the reaction mixture. While we do not wish to be bound by theory, the peroxy acids provided herein are considered to contain residual mineral acids (for example, commercially available peracetic acid has a pH of less than 1). The neutralizing agent may be added to prevent or minimize undesirable condensation. For example, a sufficient amount of a weakly basic neutralizing agent may be added to C) peracetic acid to give it a pH of 3-4, in which case the condensation will be relatively slow. The starting material D) neutralizing agent may be added together with the other starting materials A) and C), or the starting material containing C) peroxy acid may be combined with the neutralizing agent D) before being combined with starting material A). Suitable neutralizing agents include sodium carbonate, sodium bicarbonate, calcium carbonate CaO3, and potassium carbonate, all of which are commercially available, for example, from Sigma-Aldrich, Inc.
[0063] additives The silanol-functionalized polyolefins of this disclosure may also comprise one or more additives. These additives include, but are not limited to, UV stabilizers, antioxidants, fillers, scorch retarders, tackifiers, waxes, compatibilizers, adhesion promoters, plasticizers (e.g., oils), blocking agents, anti-blocking agents, antistatic agents, release agents, anti-tack additives, colorants, dyes, pigments, and combinations thereof.
[0064] Separation of silanol-functionalized polyolefins from reaction mixtures As disclosed herein, the method of this disclosure further comprises separating silanol-functional polyolefins from a reaction mixture. Separation of silanol-functional polyolefins from a reaction mixture in or without solvent B) can be achieved by a variety of techniques, including precipitation in a suitable polar solvent, cooling the silanol-functional polyolefins to below their glass transition temperature, a salting-out process (e.g., in the presence of solvent B), or a spray-drying process (e.g., in the presence of solvent B). Examples of suitable polar solvents for separating silanol-functional polyolefins from a reaction mixture include polar aprotic solvents such as acetone and acetonitrile, which are known in the art. Other polar solvents, such as alcohols, are undesirable because they may result in alkoxysilane byproducts. After separation, the silanol-functional polyolefins can be washed once or more times with a polar aprotic solvent and then dried (e.g., under dry nitrogen at high temperature, 30–50°C). [Examples]
[0065] The Inventive Example (IE) and Comparative Example (CE) of the present invention were derived using the following materials and methods. Table 1 provides the materials used in the IE and CE.
[0066] General process The polymer substrates are provided in Table 1A, where each polymer substrate is a --SiH-containing polyolefin. For each IE and CE, the respective polymer substrate was melt-blended in a twin-screw extruder (Thermo Fisher Scientific Process 11 twin-screw extruder) to a temperature above the melting temperature of the polymer substrate (Tables 1A and 2A / 2B) as discussed herein, or dissolved in the solvent and at the temperature provided in Tables 1A and 3A / 3B as discussed herein. Peracids were introduced in equimolar to 3-fold molar excess relative to the moles of silane groups (-SiH), as provided in the following tables.
[0067] [Table 1] AcOH - Acetic Acid
[0068] Polymer synthesis and properties Polymers 1 to 5 (Poly1 to Poly5, Table 1A) were each prepared in a 1-gallon polymerization reactor filled with hydraulic pressure and operated under steady-state conditions. Detailed synthesis information is provided below. The solvent was ISOPAR-E supplied by ExxonMobil Chemical Company. 5-Hexenyldimethylsilane (HDMS), supplied by Gelest, was used as the ter monomer and purified with AZ-300 alumina supplied by UOP Honeywell before use. HDMS was supplied to the reactor as a 22 wt% solution in ISOPAR-E. The reactor temperature was measured at or near the outlet of the reactor. The polymers were isolated and pelletized. The polymerization conditions are listed in Tables 1C to 1E, and the catalysts are shown in Table 1B. The polymer properties of each ethylene / octene / silane polymer (SiH-POE) and ethylene / octene interpolymer (polyolefin elastomer, "POE") are shown in Tables 2A and 2B.
[0069] [Table 2]
[0070] [Table 3]
[0071] [Table 4] * The amount in "ppm" is based on the weight of each catalyst supply solution.
[0072] [Table 5] * The amount in "ppm" is based on the weight of the co-catalyst supply solution. ** The amount of Al in "ppm" based on the weight of the co-catalyst supply solution.
[0073] [Table 6] * Silane molar percentage based on the total moles of monomers in the polymer ** Calculated from mol%, based on the weight of the interpolymer, and representing silane weight%. F:HDMS = 5-hexenyldimethylsilane.
[0074] [Table 7] * Preparation using PE CAT3: Each ethylene / octene copolymer was prepared in the same manner as the ethylene / octene / silane interpolymers discussed above, except that it lacked silane. ** Preparation using PE CAT4: The ethylene / octene copolymer was prepared in a similar manner to the ethylene / octene / silane interpolymer discussed above.
[0075] Testing methods for POLY1 to POLY5 Gel permeation chromatography The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high-temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The autosampler's oven compartment was set to 160°C, and the column compartment to 150°C. The column consisted of four AGILENT "Mixed A" 30 cm, 20 micron linear mixed-bed columns. The chromatography solvent was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was spurged with nitrogen. The injection volume used was 200 microliters, and the flow rate was 1.0 ml / min.
[0076] Calibration of the GPC column set was performed using 21 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000, prepared as six "cocktail" mixtures with at least a 10-fold gap between individual molecular weights. The standards were purchased from Agilent Technologies. Polystyrene standards were prepared at a concentration of 0.025 grams per 50 ml of solvent for molecular weights greater than 1,000,000, and 0.05 grams per 50 ml of solvent for molecular weights less than 1,000,000. The polystyrene standards were dissolved at 80°C with gentle stirring for 30 minutes. The peak molecular weights of the polystyrene standards were converted to polyethylene molecular weights using Equation 1 (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)),
[0077]
number
[0078] A quintic polynomial was used to fit the respective polyethylene equivalent calibration points. A slight adjustment (approximately 0.375 to 0.445) was made for A to correct for column resolution and band expansion effects so that linear homopolymer polyethylene standards could be obtained at 120,000 Mw. The total plate count of the GPC column set was performed using decane (prepared with 0.04 g in 50 ml of TCB and dissolved for 20 minutes with gentle stirring). Plate count (Equation 2) and symmetry (Equation 3) were measured with 200 microliter injections according to the following equations:
[0079]
number
[0080]
number
[0081] The sample was prepared semi-automatically using PolymerChar's "Instrument Control" software, with a target weight of 2 mg / ml. The solvent (containing 200 ppm BHT) was added to a pre-spurged nitrogen-filled vial with a septum cap via PolymerChar's high-temperature autosampler. The sample was dissolved for 2 hours under "low-speed" shaking at 160°C.
[0082] Mn (GPC) , Mw (GPC) , and Mz (GPC) The calculations were based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph, according to Equations 4-6, using the PolymerChar GPCOne® software, the IR chromatogram with the baseline subtracted at each equally spaced data acquisition point (i), and the polyethylene equivalent molecular weight obtained from the narrow standard calibration curve for point (i) in Equation 1. Equations 4-6 are as follows:
[0083]
number
[0084] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by a PolymerChar GPC-IR system. Using this flow rate marker (FM), the pump flow rate (apparent flow rate) for each sample was linearly corrected by matching the RV (RV(FM sample)) of each decane peak in the sample with the RV (RV(FM calibrated)) of the decane peak within a narrow standard calibration. Any temporal changes in the decane marker peak were then assumed to be related to a linear shift in the overall flow rate (effective flow rate). To facilitate the highest accuracy of RV measurements of the flow marker peaks, a least-squares fitting routine was used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation was then used to solve for the true peak location. After calibrating the system based on the flow marker peaks, the effective flow rate (relative to the narrow standard calibration) was calculated as shown in Equation 7. Effective flow rate = Apparent flow rate × (RV (FM calibrated) / RV (FM sample)) (Equation 7)
[0085] Peak processing for the flow marker was performed via PolymerChar GPCOne™ software. For acceptable flow rate correction, the effective flow rate must be within ±0.7% of the apparent flow rate.
[0086] Melt Index The melt index I2 of each polymer was measured according to ASTM D-1238, condition 190°C / 2.16 kg (melt index I at 190°C / 10.0 kg 10 ). I 10 / I2 was calculated from the ratio of I 10 to I2. The melt flow rate MFR of each polymer was measured according to ASTM D-1238, condition 230°C / 2.16 kg.
[0087] Density Polymer plaques for density analysis were prepared using ASTM D4703. The density of each polymer was measured using ASTM D792, Method B.
[0088] NMR Characterization of Terpolymers 13 For 13C NMR experiments, samples were dissolved in tetrachloroethane-d2 (with or without 0.025 M Cr(acac)3) in 10 mm NMR tubes. The concentration was approximately 300 mg / 2.8 mL. Each tube was then heated in a heating block set to 110°C. The sample tubes were repeatedly vortexed and heated to obtain a homogeneous flowing fluid. 13 13C NMR spectra were obtained on a BRUKER AVANCE 600 MHz spectrometer equipped with a 10 mm C / H DUAL cryoprobe. The following acquisition parameters were used: 60 s repetition delay, 12.0 μs 90° pulse, 256 scans. The spectral center was 100 ppm, and the spectral width was 250 ppm. All measurements were acquired at 110°C without sample spinning. 13C NMR spectrum was referenced to the solvent resonance peak at "74.5 ppm". For samples containing Cr, data was acquired with a "7-second repetition delay" and 1024 scans.
[0089] Differential Scanning Calorimetry (DSC) Differential Scanning Calorimetry (DSC) is used to measure the T m , T c , T g , and crystallinity of each polymer sample. Each sample (0.5 g) was compression molded into a film at 5000 psi for 2 minutes at 190°C. Approximately 5-8 mg of the film sample was weighed and placed into a DSC pan. The lid was crimped onto the pan to ensure a sealed atmosphere. Unless otherwise stated, the sample pan was placed in the DSC cell, then heated at a rate of 10°C / min to a temperature of 180°C for PE (230°C for PP). The sample was held at this temperature for 3 minutes. The sample was then cooled at a rate of 10°C / min to -90°C for PE (-60°C for PP) and held isothermally at that temperature for 3 minutes. Next, the sample was heated at a rate of 10°C / min until completely melted (second heating). Unless otherwise stated, the melting point (T m ) and glass transition temperature (T g ) of each polymer were determined from the second heating curve, and the crystallization temperature (T c ) was determined from the first cooling curve. The peak temperatures of T m and T c were recorded. The percent crystallinity can be calculated by dividing the heat of fusion (H f ) determined from the second heating curve by the theoretical heat of fusion of 292 J / g for PE (165 J / g for PP), and multiplying this value by 100 (e.g., % crystallinity = (Hf / 292 J / g) × 100 for PE). In DSC measurements, multiple T m peaks are typically observed, and the highest temperature peak is recorded as the polymer's T m .
[0090] Experimental Procedures IE1-IE10: Oxidative extrusion The oxidation reaction extrusions for IE1–IE10 were performed in an 11 mm diameter Thermo Fisher Scientific Process 11 twin-screw extruder (TSE) held in a chemical fume hood. This is a small parallel co-rotating TSE with a clamshell barrel. The extruder length is 44 L / D, including a 40 L / D barrel and a 4 L / D extension. The barrel has six multi-functional barrel ports for reagent injection or vacuum, and eight separate heating zones along the barrel. The polymer substrate was ground to a particle size of less than 2 mm before use to facilitate its feeding. For IE1–IE10, Poly1 was used as the substrate and mCPBA as the oxidizing agent, with the polymer powder and mCPBA being dry-blended. The polymer substrate was fed into the extruder at a rate of 180 g / hour using a MovaColor MCBALANCE uni-screw weight feeder. A residence time of 2.5 minutes was used. Generally, the extruder was run for approximately 5 minutes to equalize, and then approximately 10-20 g of sample was collected for analysis.
[0091] Purification was carried out by precipitation of the functionalized polymer from hot toluene in methanol. The resulting purified functionalized polymer was characterized by proton NMR spectroscopy as discussed herein.
[0092] IE11~IE18: Solvent oxidation Solvent oxidation of IE11-IE18 was carried out as follows: Under a dry nitrogen atmosphere, the polymer substrate was dissolved in toluene (Table 4A) in a three-necked round-bottom flask equipped with an overhead stirrer and reflux condenser. The solution was heated to the temperature provided in Table 4A. An oxidizing agent as provided in Table 4A was added, and the mixture was vigorously stirred for the time shown in Table 4A. During the reaction, both NMR and ATR FT-IR analysis were performed on aliquots precipitated in methanol, as discussed herein, and briefly dried in an aluminum pan at 120°C to provide the conversion of -SiH to Si-OH. The analysis was carried out until no further change was observed in -SiH. The hot polymer solution was then precipitated in acetone at atmospheric pressure at room temperature (23°C). The resulting precipitated polymer was blended in acetone, filtered, resuspended in acetone, filtered again, and dried at high temperature (50°C) under a nitrogen sweep.
[0093] Tested characteristic results Tables 3A / 3B and 4A / 4B provide test results for IE1 to IE18. Mn and Mw were determined as described herein.
[0094] [Table 8]
[0095] [Table 9]
[0096] [Table 10]
[0097] [Table 11]
[0098] Data Analysis As can be seen from the above, IE1 to IE10 demonstrate that oxidation of TSE with mCPBA provides an extremely high conversion rate of -SiH to the -SiOH moiety in the polymer substrate. This is achieved with stoichiometric equivalents of oxidizing agent to -SiH ranging from as little as 1:1 to a maximum of 3:1. The reaction temperature for the conversion was also reasonable in the range of 100°C to 180°C, especially when the reaction was carried out at atmospheric pressure.
[0099] The solvent oxidation processes of IE11-IE18 demonstrated that mCPBA and PAA are effective oxidizing agents in solution, while CE1 showed that tBHP is not an effective oxidizing agent.
[0100] IE and CE measurement information GPC The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high-temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5). The autosampler's oven compartment was set to 160°C, and the column compartment to 150°C. The column consisted of four AGILENT "Mixed A" 30 cm, 20 micron linear mixed-bed columns. The chromatography solvent was 1,2,4-trichlorobenzene containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was spurged with nitrogen. The injection volume used was 200 microliters, and the flow rate was 1.0 ml / min.
[0101] Calibration of the GPC column set was performed using 21 narrow molecular weight distribution polystyrene standards with molecular weights ranging from 580 to 8,400,000, prepared as six "cocktail" mixtures with at least a 10-fold gap between individual molecular weights. The standards were purchased from Agilent Technologies. Polystyrene standards were prepared at a concentration of 0.025 grams per 50 ml of solvent for molecular weights greater than 1,000,000, and 0.05 grams per 50 ml of solvent for molecular weights less than 1,000,000. The polystyrene standards were dissolved at 80 degrees Celsius for 30 minutes with gentle stirring. The peak molecular weights of the polystyrene standards were converted to polyethylene molecular weights using Equation 1 (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)),
[0102]
number
[0103] A quintic polynomial was used to fit the respective polyethylene equivalent calibration points. A slight adjustment (approximately 0.375 to 0.445) was made for A to correct for column resolution and band expansion effects so that linear homopolymer polyethylene standards could be obtained at 120,000 Mw. The total plate count of the GPC column set was performed using decane (prepared with 0.04 g in 50 ml of TCB and dissolved for 20 minutes with gentle stirring). Plate count (Equation 2) and symmetry (Equation 3) were measured with 200 microliter injections according to the following equations:
[0104]
number
[0105]
number
[0106] The sample was prepared semi-automatically using PolymerChar's "Instrument Control" software, with a target weight of 2 mg / ml. The solvent (containing 200 ppm BHT) was added to a pre-spurged nitrogen-filled vial with a septum cap via PolymerChar's high-temperature autosampler. The sample was dissolved for 2 hours under "low-speed" shaking at 160°C.
[0107] Mn (GPC) , Mw (GPC) , and Mz (GPC) The calculations were based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph, according to Equations 4-6, using the PolymerChar GPCOne® software, the IR chromatogram with the baseline subtracted at each equally spaced data acquisition point (i), and the polyethylene equivalent molecular weight obtained from the narrow standard calibration curve for point (i) in Equation 1. Equations 4-6 are as follows:
[0108]
number
[0109] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by a PolymerChar GPC-IR system. Using this flow rate marker (FM), the pump flow rate (apparent flow rate) for each sample was linearly corrected by matching the RV (RV(FM sample)) of each decane peak within the sample with the RV (RV(FM calibrated)) of the decane peak within a narrow standard calibration. Any temporal changes in the decane marker peak were then assumed to be related to a linear shift in the overall flow rate (effective flow rate). To facilitate the highest accuracy of RV measurements of the flow marker peaks, a least-squares fitting routine was used to fit the peaks of the flow marker concentration chromatogram to a quadratic equation. The first derivative of the quadratic equation was then used to solve for the true peak location. After calibrating the system based on flow marker peaks, the effective flow rate (with respect to a narrow standard calibration) was calculated using Equation 7: Flow rate (effective) = Flow rate (apparent) × (RV (FM calibrated) / RV (FM sample)) (Equation 7). Flow marker peak processing was performed via PolymerChar GPCOne® software. For an acceptable flow rate correction, the effective flow rate must be within ±0.7% of the apparent flow rate.
[0110] NMR The extruded polymer was subjected to Varian 500 MHz NMR. 1 H and 29 Analysis was performed by Si NMR. 1 ¹H NMR samples were prepared using 10–15 mg of polymer dissolved in 550 μL of TCE-d2, with a D1 of 10 seconds, 16–32 scans, and other standard methods. 29 Si NMR samples were prepared using 100 mg of polymer and 500 μL of TCE-d2 together with 4 mM Cr(acac)3, with a D1 of 5 seconds, 256 scans, and the QA-RINEPT method. 1The conversion of SiH by 1H NMR was determined by comparing the change in the integral of the SiH resonance at 3.95 ppm after extrusion with that of the unextruded sample and normalizing it against the integral of the aliphatic resonance. All spectra were collected with a Varian 500 MHz spectrometer equipped with a liquid N2 cooled cryoprobe.
[0111] FTIR-ATR Infrared spectra were collected using a Perkin Elmer Frontier Fourier transform infrared spectrometer (FT-IR) equipped with an attenuated total reflection (ATR) accessory (single bounce diamond / ZnSe). The sample was cut with scissors to expose a clean inner surface, then placed inside the accessory and held with a force that resulted in a peak absorbance of approximately 0.4. Four to 16 scans were collected depending on the spectral quality. Spectra were collected at least three times to ensure a representative sample of the entire sample.
[0112] The SiH conversion rate is the molar percentage of SiH bonds in a polymer source that become Si-OH bonds as a result of an oxidation reaction. The SiH conversion rate is 2920 cm⁻¹. -1 The peak was normalized at 942 cm, and the baseline was set to 942 cm. -1 This is determined by setting it to 0, and then 887cm -1 The conversion rate was determined using the Si-H peak in the following case: %SiH conversion rate = 100 × (887 cm after oxidation reaction) -1 Absorbance at (887 cm² before oxidation reaction) / (887 cm² before oxidation reaction) -1 Absorbance in [location].
Claims
1. A method for preparing silanol-functionalized polyolefins, Under the thermal conditions necessary to bring about the synthesis of the silanol moiety, A) Silyl hydride-functionalized polyolefins, Optionally, B) Solvent, C) Peroxy acid, Optional choice: D) Neutralizing agent Combining the starting materials, A method comprising forming a reaction mixture that, under the aforementioned thermal conditions, produces the silanol-functionalized polyolefin having the silanol portion.
2. The silyl hydride-functionalized polyolefin comprises the silyl hydride moiety of formula I, -SiR 2 H (I) The method according to claim 1, wherein each R is independently selected from the group consisting of alkyl groups of 1 to 4 carbon atoms and aryl groups of 6 to 10 carbon atoms.
3. The method according to claim 2, wherein each R is a methyl group.
4. The method according to claim 2 or 3, wherein the silyl hydride-functionalized polyolefin contains 0.10 weight percent (wt%) to 10 weight percent of the silyl hydride portion of formula I, based on the total weight of the silyl hydride-functionalized polyolefin.
5. The method according to any one of claims 1 to 4, wherein the silyl hydride-functionalized polyolefin is selected from the group consisting of silyl hydride-functionalized polyethylene and silyl hydride-functionalized polypropylene.
6. The method according to any one of claims 1 to 5, wherein the silyl hydride-functionalized polyolefin is a branched silyl hydride-functionalized polyolefin.
7. The method according to any one of claims 1 to 6, wherein the thermal conditions for producing the synthesis of the silanol portion include melt-blending the reaction mixture at a temperature of 100°C to 180°C for a duration of 30 seconds to 60 minutes.
8. The method according to claim 7, wherein the method is carried out in the absence of a solvent.
9. The method according to any one of claims 1 to 6, wherein the thermal conditions for producing the synthesis of the silanol portion include dissolving the silyl hydride-functionalized polyolefin in the solvent of the reaction mixture.
10. The method according to claim 9, wherein the thermal conditions for producing the synthesis of the silanol moiety include heating the reaction mixture at a temperature of 60°C to 120°C for a duration of 1 minute to 60 minutes.
11. The method according to any one of claims 1 to 10, further comprising separating the silanol-functionalized polyolefin from the reaction mixture.
12. C) The method according to any one of claims 1 to 11, wherein the peroxy acid is used in an amount of 1 to 3 molar equivalents of peroxy acid based on A) the silicon bond hydrogen content of the silyl hydride-functionalized polyolefin.
13. The method according to any one of claims 1 to 12, wherein the peroxy acid is selected from the group consisting of peracetic acid, meta-chloroperbenzoic acid, perbenzoic acid, and combinations thereof.
14. D) The method according to any one of claims 1 to 13, wherein the neutralizing agent is present in the reaction mixture.
15. A silanol-functionalized polyolefin formed according to any one of claims 1 to 14.