Ultra-low sparkle glass film

A glass sheet with tailored composition and surface roughness parameters addresses the challenge of balancing sparkle and diffusion in high-resolution displays, achieving low sparkle and moderate diffusion for improved image quality and tactile comfort at a lower cost.

JP2026539262APending Publication Date: 2026-11-24AGC GLASS EUROPE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026520522
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-14
Filing Date
2024-11-06
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Existing glass sheets for high-resolution displays face challenges in achieving a balance between low sparkling and moderate diffusion, leading to a grainy appearance and reduced image quality, while also being cost-effective for mass production.

Method used

A glass sheet with a specific composition and surface roughness parameters, including 0.020 ≤ Ra ≤ 0.400 micrometers and 7 ≤ RSm ≤ 30 micrometers, combined with optical properties of 1.50% to 8.00% sparkling and 2% to 50% diffusion, is developed to achieve ultra-low sparkle and moderate diffusion, providing a comfortable touch sensation.

Benefits of technology

The solution effectively reduces sparkling and maintains acceptable anti-glare properties, enhancing image quality and user experience with a soft touch feel, while being cost-effective for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539262000001_ABST
    Figure 2026539262000001_ABST
Patent Text Reader

Abstract

The present invention relates to a glass sheet having a glass composition containing, in percentages of the total weight of the glass, SiO2 55% to 85%, preferably 55% to 78%, Al2O 30% to 5%, preferably 0% to 4%, B2O 30% to 20%, preferably 0% to 18%, Na2O 0% to 25%, preferably 5% to 20%, CaO 0% to 20%, preferably 2% to 12%, MgO 0% to 15%, preferably 0% to 12%, K2O 0% to 20%, preferably 0% to 10%, and BaO 0% to 20%, preferably 0% to 5%. The glass sheet includes at least one etched surface having a surface roughness defined as 0.020 ≤ Ra ≤ 0.400 micrometers and 7 ≤ RSm ≤ 30 micrometers when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm at an evaluation length of 4 mm. The glass sheet, when measured from the etched surface, has optical properties of a sparkling value of 1.50% to 8.00% and a diffusion value of 2% to 50% when measured at a display resolution of 264 PPI.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to glass sheets that are particularly suitable for high-resolution display applications as cover glass. In particular, the present invention relates to glass sheets that exhibit moderate anti-glare optical properties with very low sparkle. Additionally, the glass sheets of the present invention also provide a "soft touch". BACKGROUND ART

[0002] Surface texturing of glass is widely used in the display industry to achieve specific optical properties. This texturing can be produced by several known methods such as (i) removing material from a smooth glass surface by chemical etching or sandblasting or laser ablation, (ii) applying a rough coating on a smooth surface, for example by spraying, polymer web coating or dip coating, etc.

[0003] It has been recognized that texturing must be used to reach a compromise between reducing glare on the surface of the glass and reducing transmission / resolution properties. Furthermore, with recent increases in brightness and high resolution of marketed displays, there is also a growing demand for maintaining / reaching a comfortable smooth touch feeling (often called satin, silk, or soft touch) while providing anti-glare / anti-sparkle solutions for cover glass sheets.

[0004] In fact, sparkling can result from the interaction between two structured layers: the regular pixel matrix that makes up the display and the irregularly structured surface of the anti-glare cover glass. It is known that sparkling increases as the resolution of new displays, characterized by higher pixel density and increasingly smaller sizes, increases. Fine-tuning the morphology of the anti-glare glass microstructure (size, height, shape, distribution, etc.) is crucial to achieving the right balance between a good level of anti-glare (maximum possible diffusion of reflected light) and the lowest sparkling effect in high-resolution displays. It is well recognized in the art that achieving both properties simultaneously is extremely difficult. Typically, current glass sheets for display applications either result in low levels of sparkling but insufficient anti-glare with very low levels of light diffusion, or a good level of anti-glare with higher diffusion levels but significant levels of sparkling.

[0005] Therefore, there is still a need to provide cover glass sheets that exhibit very low sparkling while maintaining low to moderate diffusion. In particular, there is still a need to provide such glass sheets that are cost-effective for the mass production market. [Overview of the Initiative]

[0006] The present invention relates to a glass sheet having a glass composition containing the following, expressed as a percentage of the total weight of the glass: SiO2 55%~85%, preferably 55%~78%; Al2O30-5%, preferably 0-4%; B2O 30-20%, preferably 0-18%; Na2O 0-25%, preferably 5-20%; CaO 0-20%, preferably 2-12%; MgO 0-15%, preferably 0-12%; K2O 0-20%, preferably 0-10%; and BaO 0-20%, preferably 0-5%.

[0007] The glass sheet includes at least one etched surface having a surface roughness defined by 0.020 ≤ Ra ≤ 0.400 micrometers and 7 ≤ RSm ≤ 30 micrometers when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

[0008] The glass sheet has the following optical properties when measured from the etched surface: a sparkling value of 1.50% to 8.00%, preferably 1.75% to 7.00%, more preferably 2.00% to 5.00%, and a diffusion value of 2% to 50%, preferably ≥2.5%, preferably ≥3.0%, more preferably ≥4.0% to ≤40%, preferably ≤35%, preferably ≤30%, and more preferably ≤25%.

[0009] At least one etched surface of the glass sheet of the present invention has a surface roughness preferably defined by 0.025 ≤ Ra ≤ 0.300 micrometers, more preferably 0.035 ≤ Ra ≤ 0.250 micrometers, when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

[0010] At least one etched surface of the glass sheet of the present invention has a surface roughness preferably defined by 10 ≤ Rsm ≤ 28 micrometers, more preferably 15 ≤ Rsm ≤ 25 micrometers, when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

[0011] In a preferred embodiment, at least one etched surface of the glass sheet of the present invention has a surface roughness defined by: 0.10 ≤ Rz ≤ 2.00 micrometers; preferably: 0.12 ≤ Rz ≤ 1.50 micrometers, when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

[0012] In a preferred embodiment, the glass sheet of the present invention has a clarity of 30% to 100%, preferably 45% to 100%, more preferably 60% to 100%, and / or a haze value of 1% to 50%, preferably 2% to 40%, more preferably 3% to 35%, as measured from the etched surface.

[0013] Preferably, the glass composition of the glass sheet of the present invention contains 0 to 4 wt%, preferably 0 to 3 wt%, more preferably 0 to 2 wt% Al2O3, expressed as a percentage of the total weight of the glass, and / or 3 wt% to 10 wt%, preferably 5 wt% to 10 wt%, more preferably 6 wt% to 10 wt% CaO, expressed as a percentage of the total weight of the glass.

[0014] The glass composition of the glass sheet of the present invention further contains a total amount of iron (expressed in the form of Fe2O3) preferably in the range of 0.002 to 0.06 wt%, preferably in the range of 0.002 to 0.04 wt%, more preferably in the range of 0.002 to 0.02 wt%, and most preferably in the range of 0.002 to 0.015 wt%. The glass composition of the glass sheet of the present invention further contains chromium preferably in the range of 0.0001% ≤ Cr2O3 ≤ 0.06%, expressed as a percentage of the total weight of the glass, preferably in the range of 0.002% ≤ Cr2O3 ≤ 0.06%.

[0015] Typically, the glass sheet has a glass thickness of 0.1 to 6 mm, preferably 0.1 to 2.2 mm, and more preferably 0.5 mm to 1.5 mm. In a preferred embodiment, the glass sheet is heat-strengthened glass, heat-reinforced safety glass, or chemically strengthened glass, preferably chemically strengthened glass. The glass sheet may be coated with at least one anti-reflective layer, preferably the glass sheet is coated with the anti-reflective layer on the same glass surface as the etching surface. Typically, the anti-reflective layer consists of a stack of dielectric material layers that alternately include layers of low refractive index and high refractive index, and end with layers of low refractive index.

[0016] The present invention further relates to a display device comprising the glass sheet of the present invention. [Brief explanation of the drawing]

[0017] [Figure 1-3] An optical microscope image of the glass sheet according to the present invention is shown. [Modes for carrying out the invention]

[0018] The object of the present invention is to improve upon the aforementioned shortcomings and solve the technical problems, namely, to provide a glass sheet that allows for ultra-low sparkle while simultaneously considering a certain degree of acceptable and controlled diffusion of reflected light, which is the cause of the anti-glare effect.

[0019] The objective of the present invention is, in practice, to find the best compromise between sparkling and diffusion, particularly in high-resolution display applications. Sparkling should be avoided because, especially in high-resolution displays, it results in a grainy appearance that interferes with color rendering and image display for the user. Anti-glare treatment reduces the adverse effects of incident light on the glass sheet by diffusing light reflection. However, it is recognized in the art that a reduction in sparkling adversely affects diffusion. Similarly, it is recognized that an increase in diffusion adversely affects sparkling.

[0020] Another object of the present invention in at least one of its embodiments is to provide a glass sheet that exhibits ultra-low sparkle, ultra-low to moderate diffusion, and a "soft touch".

[0021] Another object of the present invention in at least one of its embodiments is to provide a glass sheet that exhibits ultra-low sparkle, ultra-low to moderate diffusion, and is chemically or thermally strengthenable.

[0022] Finally, another object of the present invention is to provide a solution to the drawbacks of the prior art which is simple, quick and, above all, economical.

[0023] The object of the present invention is therefore to provide glass sheets that exhibit the best compromise between sparkling and diffusion. It has surprisingly been found that maintaining relatively moderate structural features on the etched surface of a soda-lime-silica glass sheet makes it possible to achieve excellent low sparkling with low to moderate diffusion, for good anti-glare, good haze and excellent clarity optical properties.

[0024] The present invention, when measured over an evaluation length of 4 mm with a Gaussian filter with cut-off wavelength of 0.8 mm: 0.020 ≤ Ra ≤ 0.40 micrometres, 7 ≤ Rsm ≤ 30 micrometres, glass sheet comprising at least one etched surface having a surface roughness defined by when measured from said etched surface, the following optical properties, - a diffusion value of from 2% to 50%; - a sparkling value of from 1.50% to 8.00%, measured at a display resolution of 264 PPI, relates to a glass sheet having

[0025] The inventors have found that it is possible to obtain an anti-sparkle glass sheet with a comfortable smooth touch sensation while reducing the anti-glare effect by considering glass surfaces with specific finely tuned roughness in conjunction with specific optical properties. It has been found that such optical properties can be obtained even in the case of glass sheets used with thin and / or high-resolution displays.

[0026] Throughout this document, where a range is indicated, the values ​​at the ends are included. Furthermore, integer values ​​and subdomain values ​​within all numerical ranges are explicitly included, as if explicitly stated. Other features and advantages of the present invention will become clearer from the following description of preferred embodiments, illustrated by simple, descriptive, and non-limiting examples.

[0027] According to the present invention, the glass sheet includes at least one etched surface. In practice, both surfaces of the glass sheet can be etched, but for typical display applications and processing, it is preferable that only one of the two surfaces of the glass sheet is etched. "Etched surface" means a surface that has been eroded by mechanical or chemical means, from which a certain amount of glass material has been removed and a certain surface texture / roughness has been imparted. When the removal of material is carried out by a chemical reaction / erosion (i.e., acid etching), it is called chemically etched glass. When the removal of material is carried out by a mechanical reaction / erosion (i.e., sandblasting), it is called mechanically etched glass. In a preferred embodiment of the present invention, the glass sheet is chemically etched glass, and more preferably oxidatively etched glass. According to the present invention, the at least one etched surface can advantageously be etched over substantially the entire glass surface, i.e., over at least 90% of the glass surface.

[0028] The etched surface of a glass sheet is typically characterized by its surface texture or roughness, particularly by the Ra, Rz, and Rsm values ​​(expressed in micrometers) defined in the ISO 4287-1997 standard. Texture / roughness is a result of surface irregularities / patterns. These irregularities consist of protrusions called "peaks" and depressions called "valleys." In a cross-section perpendicular to the etched surface, the peaks and valleys are distributed on either side of the "centerline" (algebraic mean), also known as the "mean line." For a given profile, with respect to measurements along a certain length (referred to as the "evaluation length"), the following applies: - Ra (amplitude value) corresponds to the arithmetic mean of the average difference in texture, i.e., the absolute difference between peaks and valleys. Ra measures the distance between this mean and the "line," thereby providing an indicator of the height of the pattern on the etched surface. - Rz (amplitude value) corresponds to the sum of the peak height Rp of the maximum profile within the evaluation length range and the height of the maximum profile plus the depth Rv. - Rsm (interval value, sometimes called Sm) is the average distance between two consecutive points in the profile passing through the "mean line," thereby giving the average distance between "peaks" and therefore the average width of the pattern.

[0029] The roughness value according to the present invention can be measured with a surface roughness gauge using a 2D profile (according to ISO 4287 standard). Alternatively, a 3D surface roughness gauge method (according to ISO 25178 standard) can be used, but the 2D profile is isolated and then the parameters defined in ISO 4287 standard can be accessed.

[0030] According to the present invention, the roughness value is measured using a Gaussian filter, which is a long-wavelength filter and a profile filter λ C Also known as [another term]. This is used to separate the roughness / texture component from the undulation component of the profile.

[0031] According to the present invention, the evaluation length L is the length of the profile used to evaluate roughness. The base length l is the portion of the evaluation length used to identify the irregularities that characterize the profile under assessment. The evaluation length L is divided / cut into n base lengths l, which depend on the irregularities of the profile. The base length l corresponds to the "cutoff" wavelength of the Gaussian filter (l=λ C Typically, the evaluation length is at least 5 times the base length. In roughness measurement, a short-wavelength filter (profile filter λ) is used. S ) is also commonly used to eliminate the effects of very short wavelengths, which are background noise.

[0032] The surface roughness of the etched surface of the glass sheet of the present invention is, for example, 0.020 ≤ Ra ≤ 0.400 micrometers. Preferably, the surface roughness of the etched surface of the present invention is, for example, 0.025 ≤ Ra ≤ 0.300 micrometers, and more preferably, for example, 0.035 ≤ Ra ≤ 0.250 micrometers.

[0033] The surface roughness of the etched surface of the present invention is, for example, 7 ≤ Rsm ≤ 30 micrometers. Preferably, the surface roughness of the etched surface of the present invention is, for example, 10 ≤ Rsm ≤ 28 micrometers, and more preferably, for example, 15 ≤ Rsm ≤ 25 micrometers.

[0034] According to another advantageous embodiment of the present invention, the surface roughness of the etched surface of the present invention is, for example, 0.10 ≤ Rz ≤ 2.00 micrometers, preferably, for example, 0.12 ≤ Rz ≤ 1.50 micrometers.

[0035] Such a limited range of roughness values ​​for Ra, Rsm, and preferably Rz yields a glass sheet of the present invention having a low to moderate diffusion level for a lower haze value, along with an excellent anti-sparkling effect.

[0036] It is recognized in the art that a decrease in sparkling has a negative impact on diffusion. Similarly, it is recognized that an increase in diffusion has a negative impact on sparkling. Surprisingly, the best compromise between sparkling and diffusion for coverslip sheets of high commercial viability has been found to be as follows:

[0037] The glass sheet of the present invention has a sparkling value of 1.50% to 8.00% when measured from the etched surface. Preferably, the glass sheet of the present invention exhibits a sparkling value of 1.75% to 7.00%, more preferably 2.00% to 5.00%. Here, sparkling is measured using an SMS-1000 instrument with an iPad® screen (264 PPI pixel resolution) using the Sparkling Image Difference method as recommended by the system manufacturer Display-Messtechnik & Systeme (Germany), with a focal length of 50 mm and an aperture of 5.6 mm, with no distance and no optical coupling between the glass sheet and the display. The iPad® is typically an iPad® 4 with a Retina display (264 PPI pixel resolution) that displays a completely green background image (RGB color 0,255,0). A lens with a focal length of 50mm and an aperture of 5.6mm typically has a pixel ratio of 2.47.

[0038] "Sparkle" refers to tiny bright spots (roughly pixel-level in size) that appear momentarily in the texture of an image on a display screen through an anti-glare glass surface, giving the transmitted image a grainy appearance. Thus, the "sparkling effect" is an optical interaction between two surface regions: the regular display pixel matrix (light source) and the anti-glare glass surface with its less regular microstructure. This manifests as irregular fluctuations in intensity on the display (accompanied by refraction, diffraction, and diffusion phenomena) as the observer's head moves from side to side.

[0039] In sparkle measurements, the sparkle level and intensity modulation (normal modulation) caused by the display's pixel matrix must be separated from the irregular intensity modulation perceived as sparkle. A glass sheet sample is mounted on the display screen at a specific pitch in the pixel matrix (display resolution of 264 PPI), and an image of this combination is captured by the SMS-1000 camera. For this measurement, the glass sheet has a thickness of 1 mm. During sparkle measurement, usually only the green subpixels of the display are active because, under these conditions, the human eye is very sensitive to detecting small features. Exposure is set on the SMS-1000 instrument without the sample, and positioned at the highest setting that does not overexpose the image. The pixel ratio (ratio of pixels on the target to pixels on the camera) is set, with the standard being set to 0. The sample is placed on the target, and the first data point is collected. The sample is placed on the target again, and the second data point is collected. To achieve the limited angular resolution of the human eye and to separate display pixel modulation from sparkle, the recorded image is passed through a numerical low-pass filter. The sparkle level is evaluated as the standard deviation of the tonal distribution of the filtered image divided by the mean (similar to speckle contrast).

[0040] To obtain the benefits of anti-glare, the glass sheet of the present invention exhibits a diffusion value between a minimum of ≥2.0%, preferably ≥2.5%, more preferably ≥3.0%, and even more preferably ≥4.0%, and a maximum of ≤50%, preferably ≤40%, preferably ≤35%, preferably ≤30%, and more preferably ≤25%, when measured from the etched surface. The greater the diffusion of the glass sheet, the better the anti-glare optical properties.

[0041] Diffuse reflection of a glass surface, also called scattering or diffusion, represents the relative intensity of reflected light scattered by the surface. This corresponds to the portion of light reflected in all directions, not just the specular reflection direction. This is referred to as "diffusion" in this specification. Unroughened glass surfaces are generally considered to have a diffusion value close to 0%. The rougher the surface, the more reflected and scattered light becomes, and therefore the larger the diffusion value. Diffusion values ​​are measured using a DM&S (Display-Messtechnik & Systeme) SMS-1000 apparatus, according to the system manufacturer's procedure, with an incident light angle of 6°, a distance of 260 mm between the glass and the lens, and a focal length of 16 mm and a lens with an aperture of 5.6 mm. The DM&S SMS-1000 apparatus typically operates using an isotropic linear light source incorporated within the SMS-1000 apparatus, according to the reflectance distribution function method of the system manufacturer's procedure.

[0042] The glass sheet of the present invention exhibits ultra-low sparkling while maintaining acceptable anti-glare with a diffusion value in a range of ultra-low to moderate diffusion: • Very low diffusion (VLD): 1 ≤ diffusion (%) < 10 • Low diffusion (LD): 10 ≤ diffusion (%) < 30 • Medium diffusion (MD): 30 ≤ diffusion (%) < 60

[0043] The optical properties of a glass sheet can be characterized by the following: • Direct total light transmittance (or normal light transmittance); (i) Diffuse light transmittance measured by "haze" and (ii) "transparency": "haze" corresponds to the diffuse transmittance in wide-angle scattering, while "transparency" corresponds to the diffuse transmittance in narrow-angle scattering; For example, gloss, which characterizes the brightness or sheen of a surface, particularly the specular reflection of the surface with respect to a standard at a specific angle according to ASTM standard D523 (e.g., a certified black glass standard), is expressed as SGU (Standard Gloss).

[0044] The term "diffuse" as used in relation to light transmission refers to the ratio of light deflected from the incident beam by scattering more than 2.5° after passing through glass. The term "diffuse" as used in relation to light transmission also refers to the ratio of light deflected from the specularly reflected beam by scattering more than 2.5° due to reflection at the glass / air interface. Haze and transparency can be measured using light source C according to ASTM standard D1003.

[0045] In a preferred embodiment, the glass sheet of the present invention has one or more of the following further optical properties when measured from the etched surface. According to an advantageous embodiment of the present invention, the glass sheet has a transparency of 30% to 100%, preferably 45% to 100%, and more preferably 60% to 100%. Typically, the haze of the glass sheet of the present invention is in the range of 1% to 50%, preferably 2% to 40%, and more preferably 3% to 35%.

[0046] The glass sheet according to the present invention preferably has a light transmittance TLD4 of at least 85%, preferably at least 90%. To quantify the transmittance of glass in the visible range, the inventors define the light transmittance (TL) calculated between wavelengths of 380 and 780 nm according to the ISO 9050 standard, such as that defined by the ISO / CIE 10526 standard, using illumination D65, taking into account the colorimetric standard observer CIE 1931 as defined by the ISO / CIE 10527 standard. As used herein, the light transmittance is measured according to the said standard and obtained at a thickness of 4 mm at a stereoscopic viewing angle of 2° (TLD4).

[0047] composition The glass sheet of the present invention has the following composition in terms of content expressed as a percentage of the total weight of the glass. According to preferred and more preferred embodiments of the present invention, the glass sheet of the present invention has the following composition in terms of content expressed as a percentage of the total weight of the glass.

[0048] TIFF2026539262000002.tif80170

[0049] Such basic soda-lime glass compositions have the advantage of being inexpensive even if they do not have very high mechanical resistance. In a preferred embodiment, the glass composition contains 0 to 4 wt%, preferably 0 to 3 wt%, preferably 0 to 2 wt%, more preferably 0 to 1 wt%, of Al2O3 as expressed as a percentage of the total weight of the glass, and / or in a preferred embodiment, the glass composition contains 3 wt% to 10 wt%, preferably 5 wt% to 10 wt%, more preferably 6 wt% to 10 wt%, of CaO as expressed as a percentage of the total weight of the glass.

[0050] Ideally, according to embodiments of the present invention, the composition of the glass sheet is boron-free. This means that boron is not intentionally added to the glass batch / raw material, and if it were present, the B2O3 content in the composition of the glass sheet would only reach the amount of impurity that would be unavoidable during manufacturing. For example, the B2O3 content in the composition of the glass sheet of the present invention is less than 0.01 wt%, or even less than 0.005 wt%.

[0051] According to an advantageous embodiment of the present invention, which can combine the above-described embodiments with the basic glass composition, the glass sheet has a composition containing iron (expressed as Fe2O3) in the range of 0.002 to 0.06 wt%. When the total content of iron (expressed as Fe2O3) is 0.06 wt% or less, it is possible to obtain a glass sheet that has almost no visible color and allows for high flexibility in terms of aesthetic design (for example, no distortion occurs when white silk printing is performed on some glass elements of a smartphone). This minimum value does not cause excessive damage from the perspective of the cost of the glass, and low iron values ​​often require expensive, very high-purity starting materials and their refining. Preferably, the composition contains a total amount of iron (expressed as Fe2O3) in the range of 0.002 to 0.04 wt%. More preferably, the composition contains a total amount of iron (expressed as Fe2O3) in the range of 0.002 to 0.02 wt%. In the most preferred embodiment, the composition contains a total amount of iron (represented in the form of Fe2O3) in the range of 0.002 to 0.015 wt%.

[0052] According to another embodiment of the present invention, in combination with the above embodiment regarding the Fe2O3 content, the glass has a composition containing chromium in an amount of, for example, 0.0001% ≤ Cr2O3 ≤ 0.06% expressed as a percentage of the total weight of the glass. Preferably, the glass has a composition containing chromium in an amount of, for example, 0.002% ≤ Cr2O3 ≤ 0.06%. This chromium content makes it possible to obtain glass with a higher IR transmittance, which is therefore advantageous when using a glass sheet in a touch panel that uses optical IR touch technology such as plane scattering detection (PSD) or leak total internal reflection (FTIR) (or any other technology that requires high IR radiative transmittance) to detect the position of one or more objects (e.g., a finger or stylus) on the surface of the glass sheet.

[0053] According to a preferred embodiment, the glass sheet of the present invention is a float glass sheet. The term “float glass sheet” should be understood to mean a glass sheet formed by a float process, which involves pouring molten glass onto a molten tin bath under reducing conditions. A float glass sheet includes, as is known, a “tin surface,” i.e., a tin-enriched surface in the glass body near the sheet surface. The term “tin-enriched” should be understood to mean a high concentration of tin with respect to the composition of the glass in the core, which may be substantially zero (tin-free) or none at all. Thus, a float glass sheet can be easily distinguished from sheets obtained by other glass manufacturing processes by its oxide content, which can be measured, for example, by an electron microprobe at a depth of about 10 micrometers.

[0054] Advantageously, for display applications, the glass sheet according to the present invention preferably has a thickness of 0.1 to 6 mm. More preferably, for display applications, for weight reasons, the thickness of the glass sheet according to the present invention is 0.1 to 2.2 mm, and even more preferably 0.5 mm to 1.5 mm.

[0055] The glass sheet according to the present invention may, advantageously, be prestressed glass. Prestressed glass means heat-strengthened glass, heat-reinforced safety glass, or chemically strengthened glass. Preferably, the glass sheet of the present invention is chemically strengthened glass.

[0056] Heat-strengthened glass is heat-treated using a controlled heating and cooling method that compresses the outer glass surface and stretches the inner glass surface. This heat treatment method imparts a bending strength to the glass that is higher than that of annealed glass but lower than that of heat-reinforced safety glass. Heat-reinforced safety glass is heat-treated using a controlled heating and cooling method that compresses the outer glass surface and stretches the inner glass surface. This stress causes the glass to shatter into small granular particles rather than breaking into sharp shards when impacted. These granular particles are less likely to injure an occupant or damage an object. Chemical strengthening of glass products is a thermal induction ion exchange, which involves replacing smaller alkaline sodium ions in the glass surface layer with larger ions, such as alkaline potassium ions. The larger ions "wedge" into the smaller bonding positions previously occupied by sodium ions, resulting in greater surface compressive stress in the glass. Such chemical treatments are generally carried out by immersing the glass in an ion-exchange melting tank containing one or more larger ion-containing molten salts, while precisely controlling the temperature and time.

[0057] Depending on the field of application, intended use, and / or desired properties, various layers / treatments can be deposited / performed on the same surface as the etched surface according to the present invention and / or on the opposite surface of the glass sheet according to the present invention.

[0058] According to one embodiment of the present invention, a glass sheet is coated with at least one thin transparent conductive layer. The thin transparent conductive layer according to the present invention may be, for example, a layer based on SnO2:F, SnO2:Sb, or ITO (indium tin oxide), ZnO:Al, or ZnO:Ga. Advantageously, according to this embodiment, the glass surface of the glass sheet opposite to the etched surface is coated with the thin transparent conductive layer.

[0059] According to another embodiment of the present invention, the glass sheet is coated with at least one anti-reflective layer. Advantageously, according to this embodiment, the anti-reflective layer is coated on the same glass surface as the etched surface. This embodiment is advantageous when the glass sheet of the present invention is used as a front cover for a screen. The anti-reflective layer according to the present invention may be, for example, a layer based on porous silica with a low refractive index, or it may consist of a stack of layers, particularly a stack of dielectric material layers alternating between layers with low and high refractive indices and ending with a layer with a low refractive index.

[0060] In another embodiment, the glass sheet has at least one anti-fingerprint layer / treatment to reduce or prevent fingerprint adhesion. Advantageously, in this embodiment, the glass sheet has the anti-fingerprint layer / treatment on the same glass surface as the etched surface. This embodiment is also advantageous in the case of using the glass sheet of the present invention as a front cover for a touchscreen. Such a layer / treatment can be combined with a thin, transparent, dielectric layer deposited on the opposite surface. Such a layer / treatment can be combined with an anti-reflective layer deposited on the same surface.

[0061] According to yet another embodiment of the present invention, the glass sheet has an antimicrobial layer / treatment. Advantageously, according to this embodiment, the glass sheet has the antimicrobial layer / treatment on the same glass surface as the etched surface. For example, such an antimicrobial treatment may be the diffusion of silver ions into the portion of the glass sheet closer to the outer surface.

[0062] Furthermore, the glass sheet according to the present invention exhibits excellent mechanical properties. In particular, it exhibits excellent abrasion resistance.

[0063] Finally, the present invention also relates to a display device comprising a glass sheet according to the present invention. All of the above embodiments of the glass sheet also apply to the present invention of the display device.

[0064] Herein, embodiments of the present invention will be described further, along with several comparative examples that do not conform to the present invention, for illustrative purposes only. The following examples are provided for illustrative purposes and do not limit the scope of the present invention. [Examples]

[0065] Comparative Examples 1-2: Soda-lime (SL) etched "LST" (or "LSTouch" or "low sparkling touch") glass from AGC Glass Europe, primarily sold for display applications.

[0066] Comparative Examples 3-4: Soda-lime (SL) etched "VRD" (or "Verre a Reflexion Diffuse") glass from AGC Glass Europe, primarily sold for display purposes.

[0067] Examples 5-7 (according to the present invention) - Based on soda-lime composition (SL) For each of Examples 5-7, a 1.0 mm thick sheet of ultra-transparent glass (10 cm x 10 cm) was cleaned with an aqueous cleaning agent and dried. Tape was attached to one side of the glass to protect it during the etching process. The glass was then immersed in 200 mL of acid etching solution at 20-25°C for time t. Finally, the glass was removed and immediately cleaned with an aqueous cleaning agent.

[0068] The soda-lime (SL) composition of the glass was as follows, expressed as a weight percentage: SiO2 72.8% Al2O3 0.9% Na2O 13.8% CaO 8.0% MgO 4.48% K2O 0.02%

[0069] Example 5 (based on SL): The acid etching aqueous solution is • (NH4)HF 24.75 mol% • KHF 21.5 mol% • Citric acid 0.5 mol% Glycerol 0.5 mol% It included. The glass sample was removed after 12 seconds.

[0070] Example 6 (based on SL): The acid etching aqueous solution is: • (NH4)HF 27.0 mol% • KHF 21.2 mol% • HF 1.0 mol% • TWEEN (registered trademark) 60 0.035 mol% It included.

[0071] The glass sample was removed after 40 seconds. After washing and drying the glass sheet, • HF 25mol% • H2SO4 100 mol% • HCl 8 mol% • (NH4)HF 20.4 mol% • Xanthan gum 0.15 mol% It is immersed in a second acid etching aqueous solution composed of [components]. The glass sample was removed after 90 seconds.

[0072] Example 7 (based on SL): The acid etching aqueous solution is • (NH4)HF 27.0 mol% • KHF 21.8 mol% • HF 0.5 mol% It included. The glass sample was removed after 30 seconds. After cleaning and drying the glass sheet, • HF 20mol% • H2SO4 100 mol% • (NH4)HF 21.0 mol% Glycerol 0.8 mol% It is immersed in a second acid etching aqueous solution composed of [components]. The glass sample was removed after 120 seconds.

[0073] Texture and optical properties Each glass sheet from Examples 1-7 was analyzed in terms of texture / surface roughness and optical properties.

[0074] Surface roughness measurements were performed using a SensoFar Model S neox 090 3D optical profiler equipped with a Nikon 50x lens and SensoSCAN S neox 7.7 software, with a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm. Roughness values ​​were calculated from profiles measured according to the ISO 4287 standard. Samples were first cleaned with a cleaning agent and dried. They were then placed in the microscope, and after conventional setup, 2D profile acquisition was started. Optical microscope images were taken of several samples using a Leica DM2700 M instrument equipped with a 50x lens.

[0075] Diffusion and sparkling measurements were performed using an SMS-1000 instrument from the manufacturer Display-Messtechnik & Systeme (Germany). Sparkling was evaluated using the Sparkling Image Difference method provided by the system manufacturer Display-Messtechnik & Systeme (Germany), with an iPad® screen (264 PPI pixel resolution), a 50 mm focal length, and a 5.6 mm aperture lens, without distance between the glass object and the display, and without optical coupling. Diffusion was measured according to the system manufacturer's procedure, with an incident light angle of 6°, a distance of 260 mm between the glass and the lens, and a 16 mm focal length and a 5.6 mm aperture lens. The iPad® is an iPad® 4 with a Retina display (264 PPI pixel resolution) displaying a completely green background image (RGB color 0,255,0), and the lens has a pixel ratio of 2.47.

[0076] To highlight the advantages of the present invention, the measured sparkling (S) can also be expressed as “anti-sparkling (AS)” characterized by the formula: AS = 1 - (S / Sref) (where AS and S are the anti-sparkling and sparkling properties of the sample under consideration, respectively, and Sref is the measured sparkling of a standard sample having a very high sparkling value). The selected standard sample is VRD140, a soda-lime (SL) etched “VRD” (or “Verre a Reflexion Diffuse”) glass, a commercial product of AGC Glass Europe, having a sparkling of 26.6%.

[0077] Haze and transparency measurements were performed using a BYK Haze-gard i instrument and light source C, according to ASTM standard D1003. Gloss measurements were performed using a BYK micro-TRI-gloss instrument at a specific angle of 60°, according to ASTM standard D523.

[0078] The obtained roughness parameters and the results of the optical properties of the examples are shown in the table below.

[0079] TIFF2026539262000003.tif112170

[0080] observation The sparkling values ​​for Comparative Examples 3-6 were measured at thicknesses of 1.9 mm or 2.9 mm. Therefore, as is well known to those skilled in the art, sparkling values ​​measured with thicker glass sheet samples show even worse sparkling values ​​when measured at the required thickness of 1 mm, which is only about 20-30%. All other values ​​of diffusion, haze, and clarity remained unchanged.

[0081] The optical microscope images of Examples 5, 6, and 7 shown in Figures 1, 2, and 3 respectively illustrate the morphological / geometric structures that can be obtained while achieving the roughness parameters and optical properties according to the present invention.

[0082] The results in the table show that, compared to existing commercialized glass sheets, the glass sheet according to the present invention represents the best compromise between the excellent anti-sparkle effect required in the cover glass market and moderate, acceptable, and controlled low to medium diffusion. The glass sheets according to the present invention shown in Examples 5-7 yield lower levels of sparkling than Comparative Examples 1-4, resulting in better color rendering and display images, and good diffusion with a very acceptable anti-glare effect. Each sample according to the present invention exhibits a tactile feel that it is a softer glass sheet than the comparative examples.

Claims

1. The content is expressed as a percentage of the total weight of the glass: SiO 2 55% to 85%, preferably 55% to 78%; Al 2 O 3 0-5%, preferably 0-4%; B 2 O 3 0-20%, preferably 0-18%; Na 2 O 0-25%, preferably 5-20%; CaO 0-20%, preferably 2-12%; MgO 0-15%, preferably 0-12%; K 2 O 0-20%, preferably 0-10%; and BaO 0-20%, preferably 0-5% A glass sheet having a glass composition including, When measured using a Gaussian filter with a cutoff wavelength of 0.8 mm at an evaluation length of 4 mm: 0.020 ≤ Ra ≤ 0.400 micrometers, 7 ≤ RSm ≤ 30 micrometers It includes at least one etched surface having a surface roughness defined as, When measured from the aforementioned etched surface: A glass sheet having optical properties with a sparkling value of 1.50% to 8.00% and a diffusion value of 2% to 50% when measured at a display resolution of 264 PPI.

2. The glass sheet according to claim 1, having a sparkling value of 1.75% to 7.00%, preferably 2.00% to 5.00%.

3. The glass sheet according to claim 1 or 2, having a diffusion value between a minimum value of ≥2.5%, preferably ≥3.0%, more preferably ≥3.5%, and even more preferably ≥4.0%, and a maximum value of ≤40%, preferably ≤35%, preferably ≤30%, and more preferably ≤25%.

4. The glass sheet according to any one of claims 1 to 3, wherein the at least one etched surface has a surface roughness defined as 0.025 ≤ Ra ≤ 0.300 micrometers, preferably 0.035 ≤ Ra ≤ 0.250 micrometers, when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

5. The glass sheet according to any one of claims 1 to 4, wherein the at least one etched surface has a surface roughness defined as 7 ≤ Rsm ≤ 28 micrometers, preferably 10 ≤ Rsm ≤ 25 micrometers, when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

6. The glass sheet according to any one of claims 1 to 5, wherein the at least one etched surface has a surface roughness defined as 0.10 ≤ Rz ≤ 2.00 micrometers, preferably 0.12 ≤ Rz ≤ 1.50 micrometers, when measured using a Gaussian filter with a cutoff wavelength of 0.8 mm over an evaluation length of 4 mm.

7. The glass sheet according to any one of claims 1 to 6, wherein the glass sheet has a transparency of 30% to 100%, preferably 45% to 100%, and more preferably 60% to 100%, when measured from the etched surface.

8. The glass sheet according to any one of claims 1 to 7, wherein the glass sheet has a haze value of 1% to 50%, preferably 2% to 40%, and more preferably 3% to 35%.

9. The glass sheet according to any one of claims 1 to 8, wherein the glass composition comprises Al in a content expressed as a percentage of the total weight of the glass of 0 to 4 wt%, preferably 0 to 3 wt%, more preferably 0 to 2 wt% 2 O 3 .

10. The glass sheet according to any one of claims 1 to 9, wherein the glass composition contains 3 wt% to 10 wt%, preferably 5 wt% to 10 wt%, and more preferably 6 wt% to 10 wt%, of CaO as expressed as a percentage of the total weight of the glass.

11. A glass sheet according to any one of claims 1 to 10, characterized in that it is heat-strengthened glass, heat-reinforced safety glass, or chemically strengthened glass, preferably chemically strengthened glass.

12. The glass sheet according to any one of claims 1 to 11, wherein the glass sheet is coated with at least one anti-reflective layer, preferably the anti-reflective layer is coated on the same surface as the etched surface.

13. The glass sheet according to claim 12, wherein the anti-reflective layer is a stack of dielectric material layers that alternately include layers of low refractive index and high refractive index, and end with layers of low refractive index.

14. A glass sheet according to any one of claims 1 to 13, having a glass thickness of 0.1 to 6 mm, preferably 0.1 to 2.2 mm, and more preferably 0.5 mm to 1.5 mm.

15. A display device comprising a glass sheet according to any one of claims 1 to 14.