Semiconductor wafer having a multilayer structure and method for manufacturing the same
A semiconductor wafer with a multilayer structure using AlGaN island-like parts and a superlattice structure addresses the defect density and thickness limitations of GaN layers, enabling crack-free and cost-effective growth for medium-voltage devices.
Patent Information
- Application Number
- JP2026521780
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-10-12
- Filing Date
- 2024-03-07
- Publication Date
- 2026-11-24
AI Technical Summary
Existing GaN power devices face limitations due to high defect density and thickness restrictions in the GaN layer, which affect performance and are prone to cracking due to lattice mismatch and thermal expansion coefficient differences.
A semiconductor wafer with a multilayer structure comprising a single-crystal silicon substrate, AlGaN island-like parts, and a superlattice structure is developed, which reduces dislocation density and maintains sufficient compressive stress, allowing for thick GaN layers with low defects.
The method enables the growth of crack-free GaN layers with reduced dislocation density, enhancing heat transport and reducing manufacturing costs, suitable for industrial applications in medium-voltage devices.
Smart Images

Figure 2026539263000001_ABST
Abstract
Description
[Technical Field]
[0001] Technical field The present invention relates to a semiconductor wafer having a multilayer structure and a method for manufacturing the same. [Background technology]
[0002] Examination of the most recent prior art In modern electronics, gallium nitride (GaN) power devices are attracting increasing attention due to their superior high-voltage and high-current capacities. In particular, vertical GaN power devices are promising candidates for next-generation high-voltage and high-current power switching applications in electric vehicles, smart grids, and renewable energy processes.
[0003] In such devices, a relatively thin layer of heteroepitaxial GaN film is deposited on a silicon wafer via a buffer layer. The buffer layer is necessary because the lattice mismatch between Si and GaN results in mismatched thermal expansion coefficients.
[0004] Even with one or more buffer layers present, lattice mismatches result in a relatively high defect density in the GaN layer. Furthermore, differing thermal expansion coefficients can lead to cracking once the GaN layer exceeds a certain thickness. To account for these differing thermal expansion coefficients, sufficient compressive stress must be incorporated into the GaN layer during growth to counteract the tensile stresses experienced during the cooling process. If the defect density of the GaN layer is relatively high and its thickness is limited, the performance of the power device will be restricted, for example, with respect to its breakdown voltage.
[0005] Therefore, there is a need for improvements to GaN structures with new buffer layers that enable the fabrication of GaN drift layers with low defect density and large thicknesses exceeding 5 μm.
[0006] EP 2 727 133 B1 contains composition B w Al x Ga y Inz A GaN structure is disclosed having a buffer layer containing two N transition layers. This makes it possible to obtain a GaN layer with a thickness of more than 5 μm and a relatively low dislocation density.
[0007] However, the buffer layer is relatively thick and complex, and the thickness of the GaN drift layer is limited.
[0008] In Y. Zhang et al., J. Phys. D: Appl. Phys. 51 (2018) 273001, 2 × 10 8 cm -2 A buffer layer is described that enables the fabrication of GaN layers with a dislocation density and a thickness of less than 6 μm.
[0009] A. Dadgar et al., Phys. Stat. Sol. (C) 0, No. 6 (2003), describe the reduction of dislocations by a superlattice structure with 15 periods. They explain that dislocations are bent at the interfaces of the superlattice layers, thereby increasing the probability of recombination and annihilation with other dislocations having opposite Burgers vectors. The mechanism of dislocation annihilation in such multilayer structures is also discussed by AERomanov and JSSpeck, Appl. Phys. Lett. 83.13 (2003): 2569-2571, B. Daudin, B. et al., Phys. Rev. B 56.12 (1997): R7069, and M. Imura et al., J. Cryst. Growth 300.1 (2007): 136-140. [Overview of the Initiative] [Problems that the invention aims to solve]
[0010] Objects and solutions of the present invention The present invention aims to provide a novel GaN structure having a GaN drift layer with increased thickness and reduced dislocation density and stress within the GaN drift layer. [Means for solving the problem]
[0011] The aforementioned problems are solved by a semiconductor wafer having a multilayer structure according to the first aspect of the present invention.
[0012] In a second aspect, the present invention relates to a method for manufacturing a semiconductor wafer having a multilayer structure. This method is suitable for manufacturing a semiconductor wafer having a multilayer structure according to the first aspect of the present invention.
[0013] In particular, the inventors have found that certain process conditions can induce the growth of Al islands with 0.7≦x≦1.0 and 0≦y≦0.5 x Ga 1-x N islands and Al y Ga 1-y N islands, and subsequently induce a superlattice composed of layers of these materials. Surprisingly, it has been found that the presence of islands reduces dislocations in a relatively narrow region of the buffer layer. These islands annihilate dislocations and reduce compressive stress relaxation during GaN growth. Therefore, a sufficiently high compressive stress can be maintained, which can compensate for tensile stress during cooling. As a result, a GaN drift layer with large thickness and low dislocation density can be obtained in a process suitable for industrial applications. Furthermore, since dislocations, especially threading dislocations, can be efficiently reduced in a relatively narrow region of the buffer layer, the overall thickness of the buffer layer can be reduced. This is advantageous because it enables a reduction in manufacturing costs and enhances heat transport through the buffer layer during device operation.
[0014] Increased accumulation of compressive stress compensates for thermal mismatch, enables the growth of thick GaN layers, and results in crack-free wafers with low residual stress and wafer bow (warpage). This achievement is the key to achieving thick GaN layers on silicon substrates.
[0015] A semiconductor wafer having a multilayer structure according to the first aspect of the present invention has a diameter of 150 mm or more and 300 mm or less. The multilayer structure of the semiconductor wafer includes a single crystal silicon substrate having a {111} orientation, At least one AlN nucleating layer, Al z Ga 1-z N layer and Al x Ga 1-x N island-like parts and Al y Ga 1-y The island-like part of N, A superlattice structure containing periods 20 to 120, where each period is Al x Ga 1-x N layer and Al y Ga 1-y A superlattice structure consisting of N layers, It comprises one or more single-crystal doped GaN layers having a total thickness of 6 μm or more, in this order. At least one of the one or more single-crystal doped GaN layers is 5.0 × 10 8 cm -2 It has the following penetrating dislocation density, 0.3 ≤ z ≤ 0.7, 0.7 ≤ x ≤ 1.0, and 0 ≤ y ≤ 0.5.
[0016] In a second embodiment of the present invention, a method for manufacturing a semiconductor wafer having a multilayer structure is provided. The method is as follows: (i) The step of providing a single crystal silicon substrate having a {111} orientation, (ii) A step of flowing a gas stream containing an aluminum precursor but not a nitrogen precursor onto a substrate at a temperature of 700°C to 900°C such that the total amount of aluminum flowed onto the substrate is 0.1 μmol or more and 250 μmol or less, (iii) A step of forming a low-temperature AlN nucleation layer by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto a substrate at a temperature of 700°C to 900°C, (iv) A step of forming a high-temperature AlN nucleation layer by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto a substrate at a temperature of 950°C to 1100°C, (v) By flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor onto a substrate at a temperature between 950°C and 1050°C, Al 0.3 ≤ z ≤ 0.7z Ga 1-z The steps include: forming an N-layer film, (vi) By flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor onto a substrate at a temperature between 950°C and 1100°C, Al 0.7 ≤ x ≤ 1.0 x Ga 1-x N and Al where 0 ≤ y ≤ 0.5 y Ga 1-y The step involves alternately depositing N and N for 20 to 120 cycles, where the alternating deposition is achieved by changing the composition of the gas flow. (vii) The procedure comprises the steps of (vii) depositing one or more single-crystal doped GaN layers by flowing a gas stream containing a gallium precursor, a nitrogen precursor, and a dopant precursor onto a substrate at a temperature of 900°C to 1200°C, in this order.
[0017] The method according to the second aspect of the present invention is more economical in terms of process time and cost because it does not require ELOG technology or in-situ masking with silicon nitride. Therefore, the method is more suitable for industrial applications. Furthermore, the method according to the second aspect of the present invention makes it possible to obtain specific shapes and dimensions of the island-like portions formed in step (vi).
[0018] The growth of island-like structures and superlattice structures is an effective method for bending and eliminating dislocations, resulting in a dramatic reduction in dislocation density in narrow regions of the buffer, as shown in Figure 8. Therefore, it is possible to avoid using time-consuming conventional methods such as ELOG and thick buffer structures to achieve similar dislocation densities. The method of the present invention enables the fabrication of superlattice structures in which sufficient compressive stress is maintained in the crystal lattice. As a result, the amount of positive warp per unit thickness during the growth of GaN on the superlattice structure is large enough to compensate for the tensile stress generated during cooling. In the definition of the present invention, positive warp indicates that the semiconductor wafer has a convex shape. In the definition of the present invention, negative warp indicates that the semiconductor wafer has a concave shape.
[0019] Furthermore, a lower dislocation density results in a higher critical breakdown field, and thus the required thickness of GaN to achieve the same breakdown voltage can be reduced. This makes it possible to grow sufficiently thick GaN device layers to manufacture PIN diodes and transistors for medium-voltage applications (600-1700V) in either fully vertical or pseudo-vertical configurations. [Brief explanation of the drawing]
[0020] [Figure 1] This figure shows a plan view image of a semiconductor wafer recorded with a scanning electron microscope (SEM) after performing five cycles of alternately depositing AlxGa1-xN (0.7 ≤ x ≤ 1.0) and AlyGa1-yN (0 ≤ y ≤ 0.5) according to steps (i) to (vi) of the method of the present invention. [Figure 2a] This figure shows the reverse current-voltage curves (IV curves) at different temperatures for a PIN diode manufactured according to the method of the present invention and equipped with a drift layer having a thickness of 3 μm. [Figure 2b] The temperature-dependent breakdown voltage of a PIN diode with a drift layer having a thickness of 3 μm is shown in Figure 2a. The PIN diode is formed from a semiconductor wafer manufactured according to the method of the present invention and is the same PIN diode studied in Figure 2a. [Figure 3] The figure shows the inverse IV curves of two PIN diodes with drift layers having thicknesses of 3.5 μm and 4.5 μm, respectively. The inverse IV curves were measured at room temperature, and both samples were fabricated from semiconductor wafers prepared according to the present invention. [Figure 4a] This is a schematic diagram showing the multilayer structure of a PIN stacked semiconductor wafer according to the present invention. [Figure 4b] This figure shows a cross-sectional image of a PIN stack similar to that shown in Figure 4a, recorded with a scanning electron microscope. [Figure 5] This figure shows a plan view image of the surface of a semiconductor wafer according to the present invention, recorded with an optical microscope. [Figure 6] This figure shows a cross-sectional TEM image of a semiconductor wafer fabricated according to the method of the present invention, illustrating that dislocations are bent and eliminated by island-like structures. [Figure 7] The figure shows a cross-sectional SEM image of a buffer layer in a multilayer structure of a semiconductor wafer according to the first aspect of the present invention, showing the maximum thickness (h) of the island-like portion and the value corresponding to half of the maximum thickness (h / 2), where h / 2 corresponds to the thickness for which the density of the island-like portion of 6 × 10⁷ cm⁻² was determined. [Figure 8] The figure shows a TEM image of a cross-section of a buffer layer in a multilayer structure of a semiconductor wafer according to a first aspect of the present invention, where circles highlight locations where threading dislocations merge to form new dislocations or disappear. [Figure 9] This figure shows the inverse JV characteristics of the PIN structure of Example 6. [Modes for carrying out the invention]
[0021] Detailed description of the present invention A semiconductor wafer having a multilayer structure according to a first aspect of the present invention is disclosed below. The multilayer structure of the wafer is A single-crystal silicon substrate having {111} orientation, At least one AlN nucleating layer, Al z Ga 1-z N layer and Al x Ga 1-x N island-like parts and Al y Ga 1-y The island-like part of N, A superlattice structure containing periods 20 to 120, where each period is Al x Ga 1-x N layer and Al y Ga 1-y A superlattice structure consisting of N layers, It comprises one or more single-crystal doped GaN layers having a total thickness of 6 μm or more, in this order. At least one of the one or more single-crystal doped GaN layers is 5.0 × 10 8 cm -2It has the following penetrating dislocation density, 0.3 ≤ z ≤ 0.7, 0.7 ≤ x ≤ 1.0, and 0 ≤ y ≤ 0.5.
[0022] The single-crystal silicon substrate has a {111} orientation. The substrate is preferably a single-crystal silicon wafer having a diameter of 150 mm to 300 mm, preferably 150 mm to 210 mm. In a particularly preferred embodiment, the single-crystal silicon substrate has a diameter of 150 mm or 200 mm. The single-crystal silicon substrate preferably has a thickness of 625 μm to 1500 μm. The single-crystal silicon substrate may be doped as needed and may have a silicon oxide protective layer or a silicon nitride protective layer on its back surface.
[0023] The substrate is preferably made of boron-doped single-crystal silicon. At least one AlN nucleation layer preferably includes a low-temperature AlN nucleation layer and a high-temperature AlN nucleation layer. The total thickness of the at least one AlN nucleation layer is preferably 50 nm to 500 nm. Preferably, the high-temperature AlN nucleation layer is placed on top of the low-temperature AlN nucleation layer.
[0024] In the definition of this invention, a low-temperature AlN nucleation layer is a layer of AlN composition deposited by metal-organic chemical vapor deposition (MOCVD) at a temperature of 900°C or lower. The low-temperature AlN nucleation layer is formed on a single-crystal silicon substrate. The low-temperature AlN nucleation layer preferably has a thickness of 1 nm to 50 nm. The purpose of the low-temperature AlN nucleation layer is to provide a high density of nucleation sites on the silicon substrate in order to promote the growth of a continuous high-temperature AlN layer while avoiding large pits. The low-temperature AlN nucleation layer is formed by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto the substrate at a temperature of 700°C to 900°C.
[0025] In the definition of this invention, a high-temperature AlN nucleation layer is a layer of AlN composition deposited by metal-organic vapor deposition (MOCVD) at a temperature of 950°C or higher. The high-temperature AlN nucleation layer is formed on top of a low-temperature AlN layer. The high-temperature AlN nucleation layer preferably has a thickness of 50 nm to 500 nm, more preferably 100 nm to 300 nm. The high-temperature AlN layer is deposited to protect the silicon substrate from melt-back etching that occurs when Ga comes into contact with silicon at high temperatures. In the initial growth stage, island-like structures are formed and coalesce. As a result of high lattice mismatch between AlN and silicon and subsequent coalescing of the island-like structures, the high-temperature AlN nucleation layer has a high density of threading dislocations. Since the AlN layer grows under tensile stress, concave warps occur in the wafer as the thickness of the AlN increases. The high-temperature AlN nucleation layer is formed at high temperatures by flowing a gas stream containing aluminum precursors and nitrogen precursors onto a substrate having a low-temperature AlN layer on top of it at a temperature between 950°C and 1100°C.
[0026] Al z Ga 1-z The N layer is formed on at least one AlN nucleating layer, preferably on a high-temperature AlN nucleating layer, and has an Al content defined by 0.3 ≤ z ≤ 0.7. More preferably Al z Ga 1-z The N layer has a composition defined by 0.4 ≤ z ≤ 0.6, most preferably 0.45 ≤ z ≤ 0.55. z Ga 1-z The N layer preferably has a thickness of 10 nm to 400 nm, more preferably 20 nm to 200 nm, and most preferably 100 nm or less. z Ga 1-z The effect of the N layer is to smooth the surface after AlN growth and eliminate dislocations. Preferably, Al z Ga 1-z Compressive stress is applied to the N layer. z Ga 1-z When compressive stress is applied to the N layer, a change in wafer curvature begins, and as a result, the multilayer structure is formed after the AlN layer is deposited and Al z Ga 1-zCompared to the curvature of N before film deposition, the concave shape is relaxed. z Ga 1-z The N layer is formed by flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor, as well as a carrier gas such as hydrogen or nitrogen as needed, onto a substrate having low-temperature and high-temperature AlN layers at a temperature of 950°C to 1050°C.
[0027] Al z Ga 1-z On top of the N layer, Al has 0.7≦x≦1.0 and 0≦y≦0.5, preferably 0.80≦x≦1.00 and 0.05≦y≦0.4, most preferably 0.90≦x≦1.00 and 0.10≦y≦0.20. x Ga 1-x N island-like parts and Al y Ga 1-y An island-like section of N is formed.
[0028] Al x Ga 1-x The island-like part of N is Al x Ga 1-x It includes at least one layer of N, Al y Ga 1-y The island-like part of N is Al y Ga 1-y It includes at least one layer of N. Preferably, Al x Ga 1-x N island-like parts and Al y Ga 1-y The island-like portions of N have a layered structure. More preferably, Al x Ga 1-x N island-like parts and Al y Ga 1-y The island-like part of N is Al x Ga 1-x N and Al y Ga 1-y It consists of alternating layers of N. In a preferred embodiment, the island-like portion consists of 5 to 20 layers.
[0029] Al x Ga 1-x N island-like parts and Al y Ga 1-yThe total density of N island-like portions is preferably 1.0×10 7 cm -2 or more and 1.0×10 10 cm -2 or less, more preferably 5.0×10 7 cm -2 or more and 5.0×10 9 cm -2 or less. According to the definition of the present invention, the total density of island-like portions is determined from a plan view, i.e., when viewed from the axial direction. In other words, the density of island-like portions refers to the density of island-like portions in a plane that is parallel to the wafer surface and located between the Al z Ga 1-z N layer and the GaN layer. The density of island-like portions is preferably determined after at least 5 cycles of alternately forming Al x Ga 1-x N with 0.7≦x≦1.0 and Al y Ga 1-y N with 0≦y≦0.5, more preferably after at least 10 cycles and 20 cycles or less. In other words, it is preferable to determine the density of island-like portions immediately before the coalescence stage, before the formation of continuous layers in the superlattice structure is induced.
[0030] The density of island-like portions decreases as the thickness of the superlattice increases due to coalescence of adjacent island-like portions. Therefore, the density of island-like portions is most preferably determined when the thickness of the island-like portions corresponds to half of their maximum thickness. In the present invention, the terms "height" and "maximum thickness" are used synonymously with respect to island-like portions. FIG. 7 shows a scanning electron microscope (SEM) image of the buffer layer of the multilayer structure of the semiconductor wafer according to the first aspect of the present invention, showing the maximum thickness (h) of the island-like portions and the value (h / 2) corresponding to half of the maximum thickness. h / 2 corresponds to the thickness at which the density and geometry of the island-like portions are preferably determined. The density ρ of the island-like portions is determined by taking a cross-sectional view of an SEM image such that a surface perpendicular to the (111) orientation of the single-crystal silicon substrate is shown in the SEM image, counting the number n of island-like portions along a horizontal line of length L in the SEM image (as shown in FIG. 7), and using the formula ρ=n / L 2The density ρ can be determined by the following equation, where n is the number of island-like parts counted along a horizontal line of length L.
[0031] The mechanism of island formation will be discussed in more detail below in relation to the method according to a second aspect of the present invention. Figure 6 is a cross-sectional image of a semiconductor wafer fabricated according to the method of the present invention, showing that dislocations are bent and eliminated by island-like structures. This image was recorded with a transmission electron microscope.
[0032] When the density of the island-like regions is within the above range, dislocation disappearance is improved, and the dislocation density in the subsequently deposited layer becomes lower. More specifically, when the density of the island-like regions is 1.0 × 10⁻⁶ 7 cm -2 If the density is lower, the distance between adjacent island-like regions is too large for them to merge. Instead, the layer is closed by vertical growth between the island-like regions. As a result, the region between the island-like regions has a high dislocation density. Furthermore, if the density of the island-like regions is 1.0 × 10⁻⁶ 7 cm -2 If the density is lower, the thickness of adjacent island-like structures increases when they merge. Since the island-like structures grow under low stress, the tensile stress induced during cooling is not compensated for. The density of the island-like structures is 1.0 × 10⁻⁶. 10 cm -2 In cases exceeding this limit, the elimination of the transposition is also ineffective.
[0033] Preferably, the island portion has a height of 100 nm to 1000 nm. More preferably, the island portion has a height (or maximum thickness) of 160 nm to 450 nm. The height or maximum thickness preferably corresponds to the thickness at the time of coalescence. The height is the maximum length of the island portion in the direction perpendicular to the wafer surface, i.e., perpendicular to the plane of the single-crystal silicon substrate having a {111} orientation. The height refers to the height of the island portion at the time of coalescence. When the height of the island portion is in the range of 100 to 1000 nm, dislocation annihilation is promoted and thermally induced stress is compensated. In this invention, the height of the island portion is also referred to as the thickness of the island portion. Preferably, the island portion has an aspect ratio of 0.1 to 100, more preferably 0.1 to 10. The aspect ratio is the ratio of the width to the height of the island portion. The width is the maximum diameter of the island in a plane parallel to the wafer surface, i.e., the maximum width in a plane parallel to the {111} orientation of the single-crystal silicon substrate. Therefore, the maximum width is determined in the plan view of the wafer. The height and diameter of the island, as well as the density of the island, can be determined by scanning electron microscopy (SEM). The height and diameter of the island, as well as the density of the island, can also be determined by transmission electron microscopy (TEM) or atomic force microscopy (AFM), although the latter requires interruption of growth at different stages of island growth. SEM is a relatively rapid method for analyzing the geometry of the island, i.e., the height and width of the island. In addition, SEM allows for the analysis of larger areas, and the cross-section to be analyzed can be easily prepared by mechanically dicing the wafer. Therefore, the total density of the island, their aspect ratio, and the height of the island are preferably determined by scanning electron microscopy (SEM).
[0034] In the definition of this invention, the aspect ratio is preferably the median aspect ratio, which is the median of the aspect ratios of at least 100 island-like regions. When the aspect ratio is greater than 100, the height of the island-like regions at the time of coalescence is low. As a result, dislocations reach the top surface without interacting with dislocations bent in adjacent island-like regions, resulting in a high dislocation density in the doped or undoped GaN layer of the semiconductor wafer. When the aspect ratio is less than 0.1, the height of the island-like regions is relatively high, so thermally induced stresses are not compensated during cooling.
[0035] Preferably, the island portion has inclined lateral facets. The inclined lateral facets cause bending of dislocations, thus further promoting dislocation disappearance. More specifically, dislocations, particularly through dislocations, are bent at the facets of the island portion and concentrated at the boundary of the island portion, increasing the probability of these dislocations disappearing.
[0036] Al x Ga 1-x N and Al y Ga 1-y After 5 to 20 cycles of alternating N film deposition, coalescence occurs, and the deposition of a continuous layer begins on the island-like regions.
[0037] When the deposition of the continuous layer begins, a superlattice structure is formed. A superlattice is a periodic structure of layers of two or more materials, with the thickness of one period being in the nanometer range. In this invention, the term superlattice structure refers to a periodic structure of two materials, each period having a thickness in the nanometer range and comprising two continuous layers. In the definition of this invention, the term continuous layer refers to a uniform layer that covers more than 90%, preferably more than 95%, and most preferably more than 98% of the substrate surface of the semiconductor wafer to which the film is deposited.
[0038] In the periodic structure, the layers are preferably continuous layers. In the present invention, the superlattice structure includes a period of 20 to 120, preferably 20 to 100, more preferably 20 to 60, where each period is preferably continuous Al, with 0.7 ≤ x ≤ 1.0 and 0.0 ≤ y ≤ 0.5, preferably 0.80 ≤ x ≤ 1.00 and 0.05 ≤ y ≤ 0.40, most preferably 0.90 ≤ x ≤ 1.00 and 0.10 ≤ y ≤ 0.20. x Ga 1-x A layer of N and preferably a continuous layer of Al y Ga 1-y It includes a layer of N. In a particularly preferred embodiment, the superlattice structure includes 20 to 40 periods. Preferably, each period of the superlattice structure has a thickness of 18 nm to 50 nm. More preferably, in each period of the superlattice structure, Al x Ga 1-x The N layer preferably has a thickness of 3 nm to 15 nm, and A y Ga 1-y The N layer preferably has a thickness of 15 nm to 35 nm. The average Al content of the superlattice structure is preferably less than 50% by weight. Dislocations are caused by the strain field, Al x Ga 1-x Each layer of N and Al y Ga 1-y Although dislocations can be bent at the interfaces between each N layer, the probability of dislocation annihilation is higher. Therefore, the superlattice structure promotes dislocation annihilation, and as a result, doped or undoped GaN single crystal layers with lower dislocation densities can be deposited on the superlattice structure. The desired degree of dislocation annihilation is achieved when the superlattice structure includes continuous layers with 20 to 120 periods, preferably 20 to 100 periods, more preferably 20 to 60 periods, and most preferably 20 to 40 periods.
[0039] In a preferred embodiment, the total thickness of the layer located between the single-crystal silicon substrate and one or more single-crystal doped GaN layers is 0.7 μm or more and 1.5 μm or less. Therefore, since the semiconductor wafer according to the first aspect of the present invention has a relatively thin buffer layer, it provides a basis for a simpler manufacturing process and the manufacture of thinner structures.
[0040] The multilayer structure may also include a second superlattice structure located between the first superlattice structure and one or more single-crystal doped GaN layers. The second superlattice structure includes periods, each period being m <xおよびn<yであるAl m Ga 1-m N layer and Al n Ga 1-n It consists of layers of N. The second superlattice structure has a lower average Al content compared to the superlattice structure defined in claim 1.
[0041] Essentially, Al x Ga 1-x N and Al y Ga 1-y The presence of N island-like regions and superlattice structures with continuous layers made of these materials enables the deposition of relatively thick single-crystal doped GaN layers that are crack-free and have low dislocation density. At the same time, the total thickness of the layers located between the single-crystal silicon substrate and one or more single-crystal doped GaN layers is relatively thin. This is due to the fact that the growth of both the superlattice structure and the island-like regions is an effective method for bending and eliminating dislocations, resulting in a dramatic reduction in dislocation density in a series of relatively thin layers. Therefore, it is possible to avoid time-consuming conventional methods such as ELOG and thick buffer structures to achieve a similar dislocation density. In addition, sufficient compressive stress can be obtained by the deposition of island-like regions and superlattice structures, so tensile stress during cooling can be compensated for.
[0042] Since one or more single-crystal doped GaN layers deposited on a superlattice function as device layers, their composition, structure, and stacking order are determined by the application. One or more single-crystal doped GaN layers have a thickness of 6 μm or more, preferably 7 μm or more. One or more single-crystal doped GaN layers preferably include a drain layer, a drift layer, and a p-type doped GaN layer in this order. In a preferred embodiment, one or more single-crystal doped GaN layers preferably include an n-type doped GaN layer as a drain layer, another n-type doped GaN layer as a drift layer, and a p-type doped GaN layer in this order. The n-type dopant is preferably Si, and the p-type dopant is preferably Mg.
[0043] At least one of the one or more single-crystal doped GaN layers is 5.0 × 10 8 cm -2 The following through-dislocation densities are observed. The through-dislocation density can be determined by various methods. In the present invention, the through-dislocation density is preferably determined using a transmission electron microscope (TEM) or scanning electron microscope (SEM) by recording an image of a plan view of a semiconductor wafer having one or more single-crystal doped GaN layers and counting the dislocations on the recorded image. In another embodiment of the present invention, at least one of the one or more single-crystal doped GaN layers is 8.5 × 10 8 cm -2 ~1.2 × 10 9 cm -2 It has a threading dislocation density (TDD) in the range of [specified range].
[0044] In a more preferred embodiment, the drift layer has a thickness of 3 μm or more, preferably 4 μm or more, and most preferably 6 μm or more.
[0045] Generally, one or more single-crystal doped GaN layers may contain p-type dopants and / or n-type dopants. The p-type dopant is preferably one or more elements selected from the group consisting of Mg, Be, Zn, and C. The n-type dopant is preferably one or more elements selected from the group consisting of Si, Ge, Sn, O, and C. The Si concentration in the Si-doped GaN layer is preferably 1.0 × 10⁻⁶. 15 cm -3 The above 5.0 x 10 19 cm -3 The following is more comfortable: 1.0 × 10 15 cm -3 The above 1.0 × 10 18 cm -3 The following applies: When a Si-doped GaN layer is used as a drift layer, the Si concentration is preferably 1.0 × 10⁻⁶. 15 cm -3 The above 5.0 x 10 16 cm -3 The following applies:
[0046] The Mg concentration in the Mg-doped GaN layer is preferably 1.0 × 10⁻⁶. 18 cm -3 The above 5.0 x 10 20 cm -3 The following is more comfortable: 1.0 × 10 19 cm -3 The above 5.0 x 10 20 cm -3 The following applies: In the case of PIN diodes, the application of another thin cap layer is advantageous. Such a cap layer has a thickness of 10 nm to 50 nm, more preferably 10 nm to 30 nm, and is 5.0 × 10 19 cm -3 The above 5.0 x 10 20 cm -3 The following dopant concentrations are present. Most preferably, the cap layer is 5.0 × 10 19 cm -3 The above 1.0 × 10 20 cm -3 The following dopant concentrations are present, and the dopant is Mg.
[0047] The oxygen concentration in one or more single-crystal doped GaN layers is preferably 1.0 × 10⁻⁶. 16 cm -3 It is less than 1.0 × 10⁻¹⁰. The carbon concentration in one or more single-crystal doped GaN layers is preferably 1.0 × 10⁻¹⁰. 18 cm -3 Less than 5.0 × 10 17 cm -3 Less than 5.0 × 10 16 cm -3 It is less than.
[0048] For example, one or more single-crystal doped GaN layers may include one or more Si-doped GaN layers and one or more Mg-doped GaN layers. The semiconductor wafer of claim 1 may also include one or more Sn-doped GaN layers.
[0049] For example, in one embodiment of the present invention, the following layers can be deposited on the superlattice structure in this order.
[0050] The laminate consists of a first Si-doped GaN layer, a second Si-doped GaN layer, and an Mg-doped GaN layer. The first Si-doped GaN layer has a higher Si concentration and a thinner thickness compared to the second Si-doped GaN layer. If necessary, another Mg-doped GaN layer may be deposited as a capping layer. Such a laminate is suitable for use as a PIN diode. This structure can also be used as a template for a DMOSFET.
[0051] In another embodiment of the present invention, the following layers can be deposited on the superlattice structure in this order.
[0052] The layers consist of a first Si-doped GaN layer, a second Si-doped GaN layer, an Mg-doped GaN layer, a third Si-doped GaN layer, and a fourth Si-doped GaN layer. The second Si-doped GaN layer has a lower Si concentration and a greater thickness compared to the other Si-doped GaN layers. Such a structure is suitable for trench MOSFET structures.
[0053] Preferably, the semiconductor wafer according to the first aspect of the present invention has an absolute wafer bow of 80 μm or less, more preferably 50 μm or less, and most preferably 40 μm or less at room temperature.
[0054] In a second embodiment of the present invention, a method for manufacturing a semiconductor wafer having a multilayer structure is provided. The method is as follows: (i) The step of providing a single crystal silicon substrate having a {111} orientation, (ii) A step of flowing a gas stream containing an aluminum precursor but not a nitrogen precursor onto a substrate at a temperature of 700°C to 900°C such that the total amount of aluminum flowed onto the substrate is 0.1 μmol or more and 250 μmol or less, (iii) A step of forming a low-temperature AlN nucleation layer by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto a substrate at a temperature of 700°C to 900°C, (iv) A step of forming a high-temperature AlN nucleation layer by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto a substrate at a temperature of 950°C to 1100°C, (v) By flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor onto a substrate at a temperature between 950°C and 1050°C, Al 0.3 ≤ z ≤ 0.7 z Ga 1-z The steps include: forming an N-layer film, (vi) By flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor onto a substrate at a temperature between 950°C and 1100°C, Al 0.7 ≤ x ≤ 1.0 x Ga 1-x Al where N and 0 ≤ y ≤ 0.5 y Ga 1-y This step involves alternately depositing N over 20 to 120 cycles, with the alternating deposition achieved by changing the gas flow composition. (vii) The procedure comprises the steps of (vii) depositing one or more single-crystal doped GaN layers by flowing a gas stream containing a gallium precursor, a nitrogen precursor, and a dopant precursor onto a substrate at a temperature of 900°C to 1200°C, in this order.
[0055] In a method according to a second aspect of the present invention, various gas streams containing a precursor compound are sequentially passed over a heated semiconductor wafer in a reactor equipped with a reactor chamber. The reactor may be a horizontal laminar reactor, for example a planetary reactor commercially available from AIXTRON, or a vertical reactor, for example a vertical rotating disk reactor commercially available from Veeco Instruments.
[0056] Various precursors are used. In the definition of this invention, the aluminum precursor is preferably an organoaluminum compound, more preferably a trialkylaluminum compound, and most preferably trimethylaluminum or triethylaluminum. In the definition of this invention, the nitrogen precursor is preferably ammonia or a trialkylammonium compound, more preferably ammonia. Inert compounds such as nitrogen are not considered nitrogen precursors in the definition of this invention. The Ga precursor is preferably a trialkylgallium compound, more preferably trimethylgallium or triethylgallium. Preferably, in each of steps (ii) to (vii), a carrier gas comprising one or more selected from the group consisting of helium, argon, nitrogen, and hydrogen is used. It is particularly preferable to use hydrogen and / or nitrogen as the carrier gas. Most preferably, hydrogen is used as the carrier gas throughout steps (ii) to (vi).
[0057] The total pressure in steps (ii) to (vii) is preferably 50 mbar or more and 1000 mbar or less, more preferably 500 mbar or less, even more preferably 300 mbar or less, and most preferably 250 mbar or less. The total pressure in steps (ii) to (vii) refers to the total pressure in the reaction chamber during each step. In one embodiment, the total pressure in steps (ii) to (vi) is preferably in the range of 50 to 150 mbar.
[0058] The single-crystal silicon substrate used in the method according to the second aspect of the present invention is preferably the single-crystal silicon substrate described in relation to the first aspect of the present invention. Preferably, the single-crystal silicon substrate is annealed at a temperature above 800°C, preferably above 1000°C, to remove surface oxides and contaminants from the substrate surface.
[0059] In step (ii), a gas stream containing an aluminum precursor but not a nitrogen precursor is flowed onto the substrate at a temperature of 700°C to 900°C, so that the total amount of aluminum flowed onto the substrate is between 0.1 μmol and 250 μmol.
[0060] The partial pressure of the aluminum precursor in the gas stream (i.e., the aluminum concentration within it), the volumetric flow rate, and the duration of step (ii) are adjusted so that the total amount of aluminum flowed onto the substrate in this step is 0.1 μmol or more and 250 μmol or less, preferably 1 or more and 100 μmol or less. The total amount of aluminum flowed onto the substrate in step (ii) is calculated from the volumetric flow rate of the gas stream, the concentration or partial pressure of the aluminum precursor in the gas stream, and the flow time, i.e., the time the gas stream flows over the semiconductor wafer. Preferably, the time the gas stream flows over the semiconductor wafer is 2 seconds or more and 60 seconds or less, more preferably 2 seconds or more and 20 seconds or less. This step is beneficial in preventing the single-crystal silicon substrate from being nitrided before the AlN film is deposited.
[0061] In step (iii), a low-temperature AlN nucleation layer is formed by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto the substrate at a temperature of 700°C to 900°C, preferably 750°C to 850°C. The low-temperature AlN nucleation layer is preferably the layer defined in the first aspect of the present invention and serves to provide nucleation sites for the growth of the high-temperature AlN layer.
[0062] In step (iv), a high-temperature AlN nucleation layer is formed by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto the substrate at a temperature of 950°C to 1100°C, preferably 1000°C to 1050°C. The high-temperature AlN nucleation layer is preferably the high-temperature AlN nucleation layer defined in the first aspect of the present invention.
[0063] In step (v), a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor, as well as a carrier gas such as hydrogen as needed, is flowed onto the substrate at a temperature of 950°C to 1050°C, preferably 980°C to 1030°C, thereby producing Al with a coefficient of 0.3 ≤ z ≤ 0.7. z Ga 1-z The N layer is deposited.
[0064] Under the above conditions, V-pits are formed in the AlN layer. V-pits are voids with an inverted hexagonal pyramidal shape. The density and size of the V-pits are determined by the conditions of AlN deposition. More specifically, under the conditions defined in steps (iii) and (iv), the deposition of the AlN layer is 5.0 × 10⁻¹⁰. 7 cm -2 The above 5.0 x 10 9 cm -2 The following V-pit density results. The V-pits were found to be associated with helical dislocations within the AlN layer and to function as a source of island-like growth. Subsequently, the Al z Ga 1-z The N layer is preferably deposited within the V pit, and the subsequent growth of island-like structures is such that Al z Ga 1-zThis occurs on V-pits filled with N. Consequently, the density of the island regions is determined, in particular, by the growth conditions in steps (iii) to (v). As described above, island region densities within the above range promote dislocation annihilation and thus reduce the dislocation density in one or more single-crystal doped GaN layers.
[0065] In step (vi), a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor, as well as a carrier gas such as hydrogen as needed, is flowed onto the substrate at a temperature of 950°C to 1100°C, preferably 1000°C to 1100°C, thereby producing Al 0.7 ≤ x ≤ 1.0 x Ga 1-x Al where N and 0 ≤ y ≤ 0.5 y Ga 1-y N is deposited alternately for 20 to 120 cycles, preferably 20 to 100 cycles. The deposition can be performed alternately by changing the composition of the gas flow. Preferably, in step (vi), Al is 0.80 ≤ x ≤ 1.00. x Ga 1-x N and Al where 0.05 ≤ y ≤ 0.40 y Ga 1-y N is deposited. Most preferably, Al is 0.90 ≤ x ≤ 1.00. x Ga 1-x N and Al where 0.10 ≤ y ≤ 0.20 y Ga 1-y A film of N is formed.
[0066] In this step, island-like structures and superlattice structures are formed. During the first few cycles of step (vi), preferably at least 5 cycles, more preferably the first 10 to 20 cycles, the vertical growth rate, i.e., the growth rate in the direction perpendicular to the plane of the single-crystal silicon substrate having {111} orientation, is much faster than the horizontal growth rate, i.e., the growth rate along the plane of the single-crystal silicon substrate having {111} orientation. This causes island-like structures to form during the first few cycles, preferably at least 5 cycles, more preferably the first 10 to 20 cycles. The dimensions, shape, and density of the island-like structures are controlled by process conditions, particularly temperature, pressure, and the atomic ratio of group (v) and group (iii) elements in the gas phase, where only group (V) and group (III) elements from the precursor compound are considered. The process of island-like structure formation is also determined by the strain of the underlying layer. After the first few cycles, preferably 20 cycles or less, the ratio of vertical growth rate to horizontal growth rate decreases, resulting in the coalescence of the island-like structures and the formation of a continuous layer. During the transition from island-like growth to continuous layer deposition, new dislocations, particularly through dislocations, may be generated at the coalescence boundaries. To further reduce dislocation density, the superlattice is maintained for at least 10 periods to prevent high dislocation density and thus prevent rapid relaxation of the initially compressively stressed GaN layer. Furthermore, compressively stressed Al y Ga 1-y N layer and Al under tensile stress x Ga 1-x The N layer collectively generates the effective lattice constant, which can be altered by changing the Ga / Al ratio in the superlattice. This lattice constant influences the amount of compressive stress in GaN.
[0067] Generally, in each of steps (ii) to (v), the gas flow satisfies the requirement that the atomic ratio of Group (V) elements derived from the nitrogen precursor to Group (III) elements derived from the aluminum precursor and, if present, the gallium precursor is between 5 and 100. Preferably, the ratio is between 10 and 60. Since N2 is not considered a precursor in the definition of this invention, nitrogen derived from N2 in the carrier gas is not considered when calculating the above ratio. Preferably, the gas flow in steps (ii) to (vi) contains one or more carrier gases selected from the group of hydrogen, nitrogen, helium, and argon. More preferably, the gas flow in each of steps (ii) to (vi) contains hydrogen as the carrier gas. In one embodiment, the aluminum precursor is trimethylaluminum, the gallium precursor is trimethylgallium, and the nitrogen precursor is ammonia. Generally, the chemical composition of the deposited layer is determined by the atomic ratio of Group (V) elements derived from the nitrogen precursor to Group (III) elements derived from the aluminum precursor and, if present, the gallium precursor. The growth mode is also determined by this ratio.
[0068] Preferably, the alternating film formation in each cycle of step (vi) is achieved by varying the composition of the gas stream such that the atomic ratio of group (V) elements derived from the nitrogen precursor in the gas stream and group (III) elements derived from the aluminum precursor and, if present, the gallium precursor alternates between a first value of 100 or less and a second value of 200 or more. In addition, the ratio of Al to Ga in the gas stream can be adjusted to control the composition of the layers formed in steps (v) and (vi). More preferably, the first value is 50 or less and the second value is 300 or more. Most preferably, the first value is 5 to 50 and the second value is 300 to 500. In a particularly preferred embodiment, the first value is 10 to 30 and the second value is 350 to 400.
[0069] In one embodiment, the method is carried out in a reactor chamber having a total pressure of 50 mbar to 500 mbar throughout steps (ii) to (vii). The total pressure in the reaction chamber in step (iv) is preferably 50 mbar to 300 mbar. Most preferably, the total pressure in the reaction chamber in step (iv) is 50 mbar to 150 mbar.
[0070] The growth rate in steps (i) to (iv) is preferably in the range of 100 to 1500 nm / h. In steps (i) to (iii), the growth rate is more preferably in the range of 100 to 300 nm / h. Preferably, in step (vi), Al x Ga 1-x The growth rate of N is in the range of 100-500 nm / h, and Al y Ga 1-y The growth rate of N is in the range of 700 to 1300 nm / h. The growth rate can be influenced by adjusting the temperature, flow rate, total pressure in the reaction chamber, and precursor concentration in the gas stream. In step (vii), the gas stream is preferably adjusted for each layer to be deposited according to the desired composition of the doped GaN layer.
[0071] If one or more single-crystal doped GaN layers of a semiconductor wafer include p-type doped GaN layers, the wafer may be annealed in-situ in a hydrogen-free atmosphere as needed. Preferably, the in-situ annealing is performed at a temperature between 700°C and 900°C. In-situ annealing enables the electrical activation of the p-type doped GaN layers, particularly the Mg-doped GaN layers.
[0072] Examples A semiconductor wafer according to the first aspect of the present invention is manufactured as follows using the method for manufacturing a semiconductor wafer according to the second aspect of the present invention.
[0073] The coalescence of island-like regions was investigated using a cross-sectional SEM operated in in-lens mode. Defect-selective etching was performed in a KOH / NaOH melt at 465°C for 4 minutes, and the etch pit density was determined by observation with SEM, thereby measuring the threading dislocation density (TDD). Defect counting was performed using an automated method on 10 individual SEM images per sample to ensure the statistical significance of the TDD. The dislocation network was further analyzed by weak-beam dark-field TEM using an FEI Titan 80-300 operating at 300 keV. Cross-sectional samples were prepared by conventional mechanical polishing followed by chemical mechanical polishing and ion milling with an Ar ion beam. Finally, the TDD was determined using TEM in the plan view, thereby complementing the TDD determination by DSE.
[0074] A silicon substrate wafer (111) with a diameter of 150 mm and a thickness of 750 μm is used as the substrate.
[0075] The nitride layer is deposited by metal-organic vapor deposition (MOCVD) using trimethylgallium, trimethylaluminum, bismethylcyclopentadienylmagnesium, silane, and ammonia as precursors, and hydrogen and nitrogen as carrier gases.
[0076] In Examples 1-5, the deposition of layers on the substrate by MOCVD was carried out in a commercially available vertical rotating disk reactor from Veeco Instruments. The pressure in steps (ii)-(vi) was approximately 100 mbar, and the pressure in step (vii) was approximately 200 mbar.
[0077] The film deposition process is carried out in the following steps, in this order. The substrate is heated and annealed at 1050°C to remove surface oxides and contaminants from the substrate surface. A gas stream containing an aluminum precursor is flowed over the substrate at a temperature of 800°C, adjusting the gas flow rate, precursor concentration / partial pressure, and flow time so that the total amount of aluminum flowed over the substrate is approximately 10 μmol.
[0078] Next, the temperature is lowered to 800°C, and a 1nm thick low-temperature AlN nucleation layer is deposited at 800°C, after which growth is stopped. The temperature is raised to 1050°C, and a 200nm thick high-temperature AlN nucleation layer is deposited at 1050°C, after which growth is stopped. The temperature is lowered to 1010°C, and a 25nm thick Al 0.51 Ga 0.49 After depositing the N layer at 1010°C, growth is interrupted. Next, 6nm thick AlN and 26nm thick Al 0.12 Ga 0.88 The sequence for depositing N was repeated 41 times at 1010°C, followed by interruption of growth. Then, 5.0 × 10 18 cm -3 After depositing an 800nm thick GaN:Si layer with a silicon concentration as the drain layer, growth is interrupted. 4.0 × 10 16 cm -3 After depositing a 3.5 μm thick GaN:Si layer with a silicon concentration as a drift layer, growth is interrupted. 5.0 × 10 19 cm -3 After depositing a 700 nm thick GaN:Mg layer with a magnesium concentration of , growth was interrupted and the layer was cooled to room temperature. The penetration dislocation density was determined using a transmission electron microscope (TEM), particularly a planar transmission electron microscope. TEM analysis revealed a density of 3.5 × 10⁻⁶. 8 cm -2 The density of penetrating dislocations was revealed.
[0079] The material obtained in Example 1 was a PIN diode, and its electrical properties were subsequently tested by measuring the current at different voltages. The reverse current-voltage curves obtained from these measurements are shown in Figure 2a. Figure 2b shows the temperature-dependent breakdown voltage of the PIN diode manufactured in Example 1. The curve shows an increase in breakdown voltage with temperature, which is characteristic of avalanche breakdown. This is evidence of the good electrical properties of the material obtained in Example 1. In contrast, poor material quality can lead to premature dielectric breakdown due to high leakage currents that cannot maintain avalanche breakdown.
[0080] Example 2 involved 6 nm thick AlN and 26 nm thick Al before interrupting growth and recording a planar image with a scanning electron microscope (SEM). 0.12 Ga 0.88 The procedure was carried out under the same process conditions as in Example 1, except that the sequence / cycle for depositing N was performed only 5 times. Figure 1 shows the recorded SEM image. x Ga 1-x N island-like parts and Al y Ga 1-y The total density of the island-like parts of N can be determined from the image, and is 1.0 × 10⁻⁶. 9 cm -2 It is less than.
[0081] Examples 3 and 4 were carried out under the same conditions as Example 1, except that GaN drift layers with thicknesses of 3 μm and 4.5 μm, respectively, were deposited so that the total thickness of the series of GaN layers deposited on the buffer layer was 4.5 μm and 6 μm, respectively. Subsequently, PIN diodes were fabricated from these materials. The two PIN diodes obtained in Examples 3 and 4 were both tested for electrical properties by measuring inverse IV curves at room temperature. These inverse IV curves are shown in Figure 3, providing evidence of the good electrical properties of these materials.
[0082] In Example 5, the same buffer layer as in Example 1 was prepared. After preparing the buffer layer, 5.0 × 10 18 cm -3 A 400 nm thick GaN:Si layer with a silicon concentration is deposited on a superlattice structure as a drain layer, and then growth is interrupted. 4.0 × 10 16 cm -3 After depositing a 6 μm thick GaN:Si layer with a silicon concentration of 2.0 × 10 as a drift layer, growth is interrupted. 19 cm -3 After depositing a 600nm thick GaN:Mg layer with a magnesium concentration, growth is interrupted. Finally, a 30nm thick and 1.0 × 10⁻⁶ layer is formed. 20 cm -3After depositing an Mg cap layer having a magnesium concentration, growth is interrupted. Before cooling to room temperature, the sample may be annealed at 800°C in a nitrogen atmosphere. A schematic diagram is shown in Figure 4a, and an SEM image of the semiconductor wafer obtained in Example 5 is shown in Figure 4b. Figure 5 shows an image of the wafer obtained in Example 5 recorded with an optical microscope. Figure 5 demonstrates that the present invention enables the deposition of a series of crackless GaN layers with a total thickness of 7 μm, including a crackless drift layer with a thickness of 6 μm.
[0083] In Example 6, the same buffer layer as in Example 1 was fabricated. By using the buffer consisting of island-like portions described, it became possible to realize a crack-free GaN layer with a total thickness exceeding 7 μm on a Si(111) substrate having a diameter of 150 mm. An absolute wafer bow of less than 50 μm was observed. PIN diodes were processed on a wafer having the following active layer stack, namely, a 500 nm thick n-type GaN drain layer, a 6500 nm thick n-type drift layer, and a 630 nm thick p-type GaN layer. The JV blocking characteristics of such diodes revealed hard dielectric breakdown at approximately 1130 V, as shown in Figure 9.
Claims
1. A semiconductor wafer having a multilayer structure and a diameter of 150 mm to 300 mm, wherein the multilayer structure is A single-crystal silicon substrate having a {111} orientation, At least one AlN nucleating layer, Al z Ga 1-z N layer and Al x Ga 1-x Island-shaped parts of N and Al y Ga 1-y The island-like part of N, comprising 20 to 120 periods, each period comprising an Al x Ga 1-x N layer and an Al y Ga 1-y N layer; and a superlattice structure It comprises one or more single-crystal doped GaN layers having a total thickness of 6 μm or more, in this order. At least one of the one or more single-crystal doped GaN layers is 5.0 × 10 8 cm -2 It has the following penetrating dislocation density, A semiconductor wafer where 0.3 ≤ z ≤ 0.7, 0.7 ≤ x ≤ 1.0, and 0 ≤ y ≤ 0.
5.
2. The semiconductor wafer according to claim 1, wherein 0.80 ≤ x ≤ 1.00 and 0.05 ≤ y ≤ 0.
40.
3. The semiconductor wafer according to claim 1 or 2, wherein each period of the superlattice structure has a thickness of 18 nm or more and 50 nm or less.
4. The semiconductor wafer according to any one of claims 1 to 3, wherein the average Al content of the superlattice structure is less than 50% by weight.
5. The aforementioned Al x Ga 1-x N's island-shaped portion and the Al y Ga 1-y The total density of the island-like parts of N is 5.0 × 10 7 cm -2 The above 5.0 x 10 9 cm -2 The semiconductor wafer according to any one of claims 1 to 4, which is as follows:
6. The aforementioned Al x Ga 1-x N's island-shaped portion and the Al y Ga 1-y The semiconductor wafer according to any one of claims 1 to 5, wherein the island-like portion of N has an aspect ratio of 0.1 or more and 10 or less.
7. The aforementioned Al x Ga 1-x N's island-shaped portion and the Al y Ga 1-y The semiconductor wafer according to any one of claims 1 to 6, wherein the height of the island-like portion of N is 100 nm or more and 1000 nm or less.
8. The semiconductor wafer according to any one of claims 1 to 7, wherein the total thickness of the layers provided between the single-crystal silicon substrate and the one or more single-crystal doped GaN layers is 0.7 μm or more and 1.5 μm or less.
9. The semiconductor wafer according to any one of claims 1 to 8, wherein the total thickness of the at least one AlN nucleation layer is 50 nm or more and 500 nm or less.
10. The semiconductor wafer according to any one of claims 1 to 9, wherein the multilayer structure includes a second superlattice structure provided between a first superlattice structure and one or more single-crystal doped GaN layers, and the second superlattice structure has a lower average Al content than the superlattice structure defined in claim 1.
11. A method for manufacturing a semiconductor wafer having a multilayer structure, (i) The step of providing a single crystal silicon substrate having a {111} orientation, (ii) A step of flowing a gas stream containing an aluminum precursor but not a nitrogen precursor onto the single crystal silicon substrate at a temperature of 700°C to 900°C such that the total amount of aluminum flowed onto the single crystal silicon substrate is 0.1 μmol or more and 250 μmol or less, (iii) A step of forming a low-temperature AlN nucleation layer by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto the single-crystal silicon substrate at a temperature of 700°C to 900°C, (iv) A step of forming a high-temperature AlN nucleation layer by flowing a gas stream containing an aluminum precursor and a nitrogen precursor onto the single-crystal silicon substrate at a temperature of 950°C to 1100°C, (v) By flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor over the single-crystal silicon substrate at a temperature of 950°C to 1050°C, Al is obtained such that 0.3 ≤ z ≤ 0.7 z Ga 1-z The step of forming the N layer, (vi) By flowing a gas stream containing an aluminum precursor, a gallium precursor, and a nitrogen precursor over the single-crystal silicon substrate at a temperature of 950°C to 1100°C, Al is obtained such that 0.7 ≤ x ≤ 1.0 x Ga 1-x N and Al where 0 ≤ y ≤ 0.5 y Ga 1-y A step of alternately depositing N and for 20 to 120 cycles, wherein the alternating deposition is achieved by changing the composition of the gas flow, A method comprising, in this order, (vii) forming one or more single-crystal doped GaN layers by flowing a gas stream containing a gallium precursor, a nitrogen precursor, and a dopant precursor onto the single-crystal silicon substrate at a temperature of 900°C to 1200°C.
12. A method for producing a semiconductor wafer having a multilayer structure according to claim 11, wherein in each of steps (ii) to (iv), the gas flow satisfies the condition that the atomic ratio of group (V) elements derived from the nitrogen precursor to group (III) elements derived from the aluminum precursor is 5 or more and 100 or less.
13. A method for manufacturing a semiconductor wafer having a multilayer structure according to claim 11 or 12, wherein the alternating film deposition in each cycle of step (vi) is achieved by changing the composition of the gas stream such that the atomic ratio of group (V) elements derived from the nitrogen precursor and group (III) elements derived from the aluminum precursor and, if applicable, the gallium precursor, alternates between a first value of 100 or less and a second value of 200 or more.
14. A method for producing a semiconductor wafer having a multilayer structure according to any one of claims 11 to 13, wherein the method is carried out in a reaction chamber having a total pressure of 50 mbar or more and 300 mbar or less throughout steps (ii) to (vii).
15. In step (vi), Al x Ga 1-x The growth rate of N is in the range of 100 to 500 nm / h, and Al y Ga 1-y A method for manufacturing a semiconductor wafer having a multilayer structure according to any one of claims 11 to 14, wherein the growth rate of N is in the range of 700 to 1300 nm / h.