Electrode compositions for electrodes in electrochemical energy storage devices
The electrode composition for lithium-sulfur batteries, utilizing HNBR as a dispersant for carbon nanotubes, enhances dispersion and electrical properties, overcoming conductivity and volume change challenges in lithium-sulfur batteries.
Patent Information
- Application Number
- JP2026522075
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-10
- Filing Date
- 2024-11-05
- Publication Date
- 2026-11-24
AI Technical Summary
Existing lithium-sulfur batteries face challenges due to the low electrical conductivity of sulfur, the severe polysulfide shuttle effect, and large volume changes during operation, which are exacerbated by the agglomeration of carbon nanotubes into thick bundles, leading to reduced stability and uniformity of the cathode paste.
An electrode composition for lithium-sulfur batteries using carbon nanotubes with a dispersing aid of hydrogenated nitrile-butadiene rubber (HNBR) with specific molecular weight and acrylonitrile content, improving the dispersion of carbon nanotubes and enhancing electrical properties.
The use of HNBR as a dispersant significantly improves the dispersion of carbon nanotubes, resulting in lithium-sulfur batteries with high capacity and capacity retention, addressing the stability and conductivity issues.
Smart Images

Figure 2026539264000001 
Figure 2026539264000002 
Figure 2026539264000003
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to electrochemical energy storage devices, particularly to electrode compositions for lithium-sulfur batteries (LiS). The invention further relates to electrodes, such as cathodes, formed from such compositions and to electrochemical energy storage devices comprising the respective electrodes, in particular as cathodes. BACKGROUND ART
[0002] As small, light, and high-capacity batteries, lithium-ion secondary batteries have been widely used as power sources for portable devices since their inception around 1991. Further applications include energy storage devices for electric vehicles in particular.
[0003] In particular, lithium-sulfur batteries (LiS) have attracted considerable attention due to their high theoretical energy density. However, compared to standard lithium-ion batteries, practical commercial applications of LiS batteries are limited due to various technical challenges based on the low electrical conductivity of sulfur and discharge products, severe polysulfide shuttle effect, and large volume changes during battery operation. To overcome the conductivity problem, various nanostructured carbon materials have been used as conductive additives, whereby carbon nanotubes (CNTs) are superior to other nanostructured carbon materials. Carbon nanotubes tend to bind into more complexly shaped bundles and agglomerates. The agglomeration of carbon nanotubes into long, thick bundles increases the sedimentation rate of dispersed carbon nanotube agglomerates, i.e., decreases the stability of the dispersion or cathode paste. The reduced stability of the dispersion results in a reduced storage time of the dispersion, creates possible transportation and technical scheme constraints, increases the risk of subsequent mixing becoming non-uniform, and consequently increases defects in lithium-ion or lithium-sulfur batteries.
[0004] Conventional technologies have been developed to improve the stability of CNT dispersions in lithium-ion batteries by using dispersants to prevent aggregation of dispersed particles such as carbon nanotubes. However, the preparation of dispersed CNTs for use in LiS batteries can be carried out by various methods, often by modifying CNTs, filtering, or coating them. Modification using a small amount of polymer (less than 10%) on the surface of the CNTs achieves good chemical adsorption, thereby effectively improving the circulation performance of lithium-sulfur batteries, but requires an additional manufacturing step of attaching specific PAA or PEG-based polymers to the CNT surface. Therefore, there is a need for an improved polymer dispersant for CNTs that provides a simpler preparation process for CNT dispersions in LiS batteries.
[0005] (Patent Document 1) describes a conductive material dispersion containing a conductive material including bundled carbon nanotubes; a dispersant containing a hydrogenated nitrile-based rubber; and a dispersion medium, wherein the complex elastic modulus (|G) is measured by a rheometer at a frequency of 1 Hz. * A conductive material dispersion with a pressure (@1Hz) in the range of 20-500 Pa, and a secondary battery manufactured using the same are provided. The conductive material dispersion has a complex modulus controlled to exhibit excellent dispersibility and powder-to-powder resistance characteristics, and as a result, the output characteristics of the battery can be significantly improved. No examples or information regarding the use of LiS batteries were provided.
[0006] (Patent Document 2) relates to carbon / sulfur composite materials containing carbon nanotubes or nanofibers and sulfur elements, which can be identified by their X-ray patterns, their manufacture, and their use as positive electrode active materials, as well as to electrochemical elements containing the said material.
[0007] Patent Document 3 provides a cathode material for a Li-S battery. The cathode material comprises a hydrogenated acrylonitrile-based polymer, sulfur, and GNS (graphene nanosheet), with the cathode material particles being spherical, the hydrogenated acrylonitrile-based polymer content being 20-79% by weight, the sulfur content being 20-79% by weight, and the GNS content being 1-30% by weight. Methods for manufacturing the cathode material, a cathode made from the cathode material, and a Li-S battery containing the cathode are also provided.
[0008] Patent Document 4 provides a cathode material for a Li-S battery comprising a hydrogenated acrylonitrile copolymer, sulfur, and carbon nanotubes, with the weight percentages of these components being as follows: 20% ≤ hydrogenated acrylonitrile copolymer ≤ 80%, 20% ≤ sulfur ≤ 80%, and 1% ≤ carbon nanotubes ≤ 30%. A cathode, a Li-S battery using the cathode material, and a method for preparing the cathode material are also provided.
[0009] (Patent Document 5) relates to a positive electrode active material slurry, a positive electrode including a positive electrode active material layer formed therefrom, and a lithium secondary battery including the positive electrode. The amorphous nature of the positive electrode active material slurry is adjusted by including a rubber-based binder in a predetermined ratio. The positive electrode active material layer formed accordingly from the positive electrode active material slurry can have improved flexibility and hot-rolling properties, and a lithium secondary battery using a positive electrode including the positive electrode active material layer can suppress internal short circuits, high-voltage defects, and capacity reductions.
[0010] Patent Document 6 describes a conductive material dispersion for an electrolyte secondary battery, comprising a conductive material (A), a dispersion medium (B), and a dispersant (C). The dispersant (C) is a copolymer containing (meth)acrylonitrile-derived units and conjugated diene monomer-derived units. The copolymer contains 15 to 50% by mass of (meth)acrylonitrile-derived units. The conductive material dispersion has a weight-average molecular weight of 5,000 to 400,000 g / mol.
[0011] (Patent Document 7) provides a rechargeable alkali metal-sulfur battery comprising an anode layer, an electrolyte and a porous separator, a cathode layer, and separate anode protective layers disposed between the anode layer and the separator, and / or separate cathode protective layers disposed between the separator and the cathode active material layer; wherein the anode protective layer or cathode protective layer comprises a conductive sulfonated elastomer composite material having 0.01 to 50% by weight of a conductive reinforcing material dispersed in a sulfonated elastomer matrix material, and the protective layer has a thickness of 1 nm to 50 μm, a fully recoverable tensile strain of 2 to 500%, and a lithium-ion conductivity of 10 -7 ~5×10 -2 S / cm, and electrical conductivity 10 -7 It has a frequency of ~100 S / cm.
[0012] The scientific publication (Non-Patent Document 1) provides an overview of various applications of CNTs in LiS batteries.
[0013] However, prior art solutions still have room for improvement, and a stable, easily prepared CNT dispersion solution, and its use for LiS batteries, has not yet been provided. [Prior art documents] [Patent Documents]
[0014] [Patent Document 1] European Patent Application Publication No. 3333946A1 [Patent Document 2] International Publication No. 2022 / 136314A Brochure [Patent Document 3] International Publication No. 2014 / 082296A1 Pamphlet [Patent Document 4] International Publication No. 2012 / 040934A1 Pamphlet [Patent Document 5] International Publication No. 2016 / 053063A1 Pamphlet [Patent Document 6] Japanese Patent Publication No. 2020187866 [Patent Document 7] International Publication No. 2019 / 0246068A1 Pamphlet [Non-Patent Literature]
[0015] [Non-Patent Literature 1] Q. Zu, "Carbon nanotube-based materials for lithium-sulfur batteries", J. Mater. Chem. A, 2019, 7, 17204-17241 [Summary of the Invention] [Problem to be Solved by the Invention]
[0016] An object of the present invention is to provide an electrode composition for an electrode that at least partially overcomes at least one of the problems of the prior art. In particular, an object of the present invention is to provide a measure for improving the dispersion of carbon nanotubes in a LiS electrode composition, which enables easy CNT processing and improved LiS battery characteristics. [Means for Solving the Problem]
[0017] These objects are at least partially solved by an electrode composition having the features of claim 1. This object is further solved by an electrode having the features of claim 12, and by an electrochemical energy storage device having the features of claim 13. Preferred embodiments of the present invention are described in the dependent claims, in the specification, or in the examples, and unless the contrary is clearly derived from the context, the further features described or shown in the dependent claims, in the specification, or in the examples individually or in any combination constitute the object of the invention.
[0018] An electrode composition for an electrode of a lithium-sulfur based electrochemical energy storage device is described, the electrode composition comprises a solvent in which a binder and an electrically conductive carbon material are provided, the electrically conductive carbon material comprises carbon nanotubes, and the electrode composition further comprises a dispersing aid for dispersing the carbon nanotubes, the dispersing aid comprises hydrogenated nitrile-butadiene rubber (HNBR), wherein the hydrogenated nitrile-butadiene rubber has a molecular weight Mn > 10 kg / mol to < 83 kg / mol; a molecular weight Mw > 10 kg / mol to < 245 kg / mol; and an acrylonitrile content < 39% by weight .
[0019] It has surprisingly been found that an electrode composition as defined above significantly improves the dispersion of the carbon nanotubes in said composition, thereby enabling very good electrical properties of the electrode and the electrical energy storage device, respectively, when comprising or formed from such an electrode composition. DETAILED DESCRIPTION OF THE INVENTION
[0020] Accordingly, the present invention relates to an electrode composition for an electrode of a lithium-sulfur based electrochemical energy storage device. Such an electrode composition may in particular be a dispersion to be applied to a current collector and thus form an electrode. Before applying it to a current collector, further steps may be carried out with the composition. Thus, the composition may be a starting point for producing an electrode layer. That is, the composition may be a slurry that may be applied to a current collector or may be used to form a slurry. According to an embodiment, the electrode composition may be free of active material. However, as described below, active material may be added to the composition.
[0021] Electrode compositions can be adapted in particular to form a cathode as an electrode. These electrodes can be used in lithium-sulfur batteries (LIS), also known as lithium-sulfur-based electrochemical energy storage devices.
[0022] The electrode composition comprises a solvent in which a binder and a conductive carbon material are provided.
[0023] In general, these compounds are not limited as long as they are usable in LiS batteries.
[0024] Regarding the solvent, it may consist of one material or a combination of different materials. It is preferable to use N-methyl-2-pyrrolidone (NMP) as the solvent.
[0025] Regarding the binder, it may consist of one type of material or a combination of different materials. It is preferable to use polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), or polyvinylidene fluoride (PVDF) as the binder.
[0026] Conductive carbon materials may consist of one type of material or a combination of different materials. However, according to the present invention, it is important that carbon nanotubes form at least a portion of the conductive carbon material. For example, the conductive carbon material may consist of carbon nanotubes. This is particularly advantageous when the composition is used to form LiS batteries. In this regard, it should be noted that the actual commercial applications of LiS batteries are limited compared to standard lithium-ion batteries due to various technical challenges such as the low conductivity and discharge products of sulfur, the severe polysulfide shuttle effect, and the large volume change during battery operation. To overcome these problems, various carbon materials have been used as conductive additives, and thereafter, carbon nanotubes (CNTs) are superior to other carbon materials. Therefore, the use of carbon nanotubes, particularly in LiS batteries, can provide advantageous electrical properties for the electrodes and batteries thus formed.
[0027] However, a problem that may arise when using carbon nanotubes as a conductive material is that carbon nanotubes tend to bond into more complex bundles and aggregates. The aggregation of carbon nanotubes into long, thick bundles increases the sedimentation rate of dispersed carbon nanotube aggregates, thus reducing the stability of the dispersion or cathode paste. To overcome this effect, the composition according to the present invention further includes a dispersion aid for dispersing carbon nanotubes in a solvent. Regarding the dispersion aid, according to the present invention, the dispersion aid includes HNBR, wherein the HNBR is... Molecular weight Mn>10kg / mol~<83kg / mol; Molecular weight Mw > 10 kg / mol to < 245 kg / mol; and Acrylonitrile content <39% by weight It is a condition that it has [the following].
[0028] Surprisingly, such dispersion aids significantly improve the dispersion of carbon nanotubes, thereby further enabling the highly advantageous electrical properties, particularly those of LiS batteries.
[0029] Lithium-ion (LiS) batteries are so-called "post-lithium-ion batteries" and have the potential to complement or replace lithium-ion batteries in the medium or long term. Conductive carbon, particularly carbon nanotubes (CNTs), will likely be used in these battery types, but specific dispersants or processes for this purpose have not yet been made available. Regarding the general use of CNTs in batteries, no specific research or analysis has been conducted for LiS batteries, or for selecting the correct dispersant for their potential effects.
[0030] According to the present invention, it has been found that low molecular weight hydrogenated nitrile rubber having a medium ACN content can be advantageously applied as a CNT dispersion aid, also known as a dispersant used in LiS batteries. However, the application of carbon nanotube dispersions (CNT dispersions) in LiS batteries currently requires dispersants that are more specific than standard CNT dispersants, and are formulated based on low molecular weight HNBR grades with specific ACN content. The direct effects of the dispersant used on cell capacity and stability have been shown, with low molecular weight HNBR grades having a medium ACN content exhibiting the best performance. When using low molecular weight hydrogenated nitrile rubber with a medium ACN content, a simple dispersion process can be established to obtain LiS batteries with high capacity and high capacity retention.
[0031] As is generally known in the art, hydrogenated nitrile rubber is a copolymer formed from acrylonitrile and 1,3-butadiene, wherein the double bonds of the NBR units are hydrogenated to at least a high degree.
[0032] Furthermore, with respect to the degree of hydrogenation of HNBR, a degree of hydrogenation of less than 1%, preferably less than 0.9%, as measured as RDB, is preferred.
[0033] To achieve favorable results, HNBR used as a dispersion aid for the provided carbon nanotubes possesses distinctive properties.
[0034] In detail, the HNBR used in accordance with the present invention should have the following characteristics.
[0035] HNBR should have a molecular weight Mn > 10 kg / mol to < 83 kg / mol.
[0036] Furthermore, HNBR should have a molecular weight Mw > 10 kg / mol to < 245 kg / mol.
[0037] HNBR should have an acrylonitrile content of <39% by weight.
[0038] According to a preferred embodiment, the HNBR should have a molecular weight Mn > 12 to < 75 kg / mol.
[0039] According to a preferred embodiment, HNBR should have a molecular weight Mw ≥ 15 kg / mol to < 240 kg / mol.
[0040] According to a preferred embodiment, the HNBR should have an acrylonitrile content of 25-38% by weight.
[0041] Therefore, HNBR used as a dispersant for carbon nanotubes in electrode compositions has the following properties: Molecular weight Mn > 15 kg / mol to < 75 kg / mol; and / or Molecular weight Mw ≥ 20 kg / mol ~ < 240 kg / mol; and / or Acrylonitrile content: 30-38% by weight It is particularly preferable if it has one, two, or all of the above.
[0042] HNBR, used as a dispersant for carbon nanotubes in electrode compositions, has the following properties: Molecular weight Mn > 15 kg / mol to < 65 kg / mol; and / or Molecular weight Mw ≥ 20 kg / mol ~ < 210 kg / mol; and / or Acrylonitrile content: 32-36% by weight It is even more preferable if it has one, two, or all of the above.
[0043] As described above, it may also be a condition that the composition further contains an active substance. When the composition of the present invention is used in a LiS battery, it is preferable that the active substance contains a lithium-sulfur-based active substance. For example, Li2S can be used as the active substance. However, generally, any active substance that can be used in a LiS battery can be used because it does not degrade the quality of the carbon nanotube dispersion.
[0044] According to a further preferred embodiment, the dispersion aid is present in the electrode composition in an amount of ≥2% to ≤150% by weight relative to the carbon nanotubes, for example, ≥3% to ≤100% by weight, for example, ≥5% to ≤75% by weight relative to the carbon nanotubes. Such an amount of HNBR has already been shown to be sufficient to provide good dispersion of carbon nanotubes in the solvent.
[0045] In a further preferred embodiment, the dispersion aid is present in the electrode composition in an amount of ≥10% to ≤50% by weight, preferably 15 to 25% by weight, relative to the carbon nanotubes.
[0046] In a further preferred embodiment, the dispersing agent is present in the electrode composition in an amount of ≥0.05% to ≤10% by weight, preferably ≥0.05% to ≤5.0% by weight, for example, ≥0.1% to ≤2.5% by weight relative to the electrode composition.
[0047] It is even more preferable that the carbon nanotubes are multi-walled carbon nanotubes (MWCNTs). Such nanotubes have been shown to possess particularly excellent mechanical and especially electrical properties. Therefore, a combination of good dispersion and good electrical properties can be achieved particularly effectively when using this type of nanotube.
[0048] In a further preferred embodiment, the electrode composition forming the carbon nanotube dispersion is: - A solvent in an amount of ≥85 to ≤97% by weight; - Dispersing agent in an amount of ≥0.05 to ≤10% by weight; - Carbon nanotubes in quantities of ≥0.5 to ≤10% by weight; and - Binders with a quantity of ≥0 to ≤10% by weight Includes, The dispersing agent contains HNBR, and HNBR is - Molecular weight Mn>10kg / mol~<83kg / mol; - Molecular weight Mw > 10 kg / mol to < 245 kg / mol; and - Acrylonitrile content <39% by weight It has, The total amount of solvent, binder, carbon nanotubes, and dispersion aid is 98% by weight or more, preferably 100% by weight.
[0049] In this embodiment, if the defined components total less than 100% by weight, the remaining components until the total reaches 100% by weight may be additional additives. However, it is preferable that the components defined above total more than 98% by weight, preferably 100% by weight.
[0050] In this embodiment, the solvent may be provided for N-methyl-2-pyrrolidone (NMP). However, the solvent is not limited to this embodiment.
[0051] In this embodiment, the binder may be provided for polyvinylpyrrolidone (PVP). However, the binder is not limited to this embodiment.
[0052] In a further preferred embodiment, the dispersion aid has a Mooney viscosity ML(1+4)100℃, (MU) ≥ 1 to ≤ 70. Particularly preferred, the dispersion aid has a Mooney viscosity ML(1+4)100℃, (MU) 5 to 60, for example 8 to 50, for example 10 to 45.
[0053] The components of the composition are described in more detail below.
[0054] carbon nanotubes According to the present invention, carbon nanotubes are tubular carbon structures with a diameter of 1 μm or less.
[0055] Carbon nanotubes may include single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs), depending on the number of bonds forming the layers.
[0056] Preferably, the carbon nanotubes may include one or more single-walled, double-walled, and multi-walled carbon nanotubes in the sense of the present invention.
[0057] However, it is particularly preferable that the carbon nanotubes include multi-walled carbon nanotubes. Exemplarily, the carbon nanotubes used in the present invention consist of multi-walled carbon nanotubes.
[0058] The average strand diameter of carbon nanotubes usable in this invention may be 30 nm or less.
[0059] The length of the carbon nanotubes used in accordance with the present invention may be in the range of 1 to 200 μm.
[0060] More preferably, the carbon nanotube may have an aspect ratio of 5 to 50,000, more specifically 10 to 20,000, defined as the ratio of the length of the carbon nanotube (the length of the major axis passing through the center of the carbon nanotube) to the diameter (the length of the minor axis perpendicular to the major axis and passing through the center of the carbon nanotube).
[0061] HNBR In relation to the present invention, "nitrile-diene copolymer" (nitrile-butadiene copolymer, also abbreviated as "NBR," or nitrile rubber) is understood to mean a rubber copolymer, terpolymer, or quarterpolymer of at least one α,β-ethylenically unsaturated nitrile, at least one conjugated diene, and optionally one or more additional copolymerizable monomers. Therefore, this term also encompasses copolymers having two or more α,β-ethylenically unsaturated nitrile monomer units and two or more conjugated diene monomer units.
[0062] "Hydrogenated nitrile-diene copolymer" ("HNBR") is understood to mean a corresponding copolymer, terpolymer, or tetrapolymer in which at least a portion, preferably at least 50%, of the CC double bonds in the copolymerized diene unit are hydrogenated. For sufficient electrochemical stability, it is preferable that the hydrogenated HNBR rubber is completely hydrogenated.
[0063] The term "fully hydrogenated" means that the degree of hydrogenation of the butadiene units in a hydrogenated nitrile-diene copolymer is between 99.1% and 100%.
[0064] At a minimum, the content of residual double bonds is less than 1%.
[0065] The term "copolymer" encompasses polymers that have multiple monomer units.
[0066] α,β-ethylenically unsaturated nitriles: The α,β-ethylenically unsaturated nitrile used to form the α,β-ethylenically unsaturated nitrile unit is acrylonitrile.
[0067] The amount of α,β-ethylenically unsaturated nitrile units is less than 39% by weight, preferably in the range of 20 to 38% by weight, relative to 100% by weight of the total amount of all monomer units in the HNBR rubber.
[0068] Conjugated dienes: The conjugated diene that forms the conjugated diene unit may be any conjugated diene, particularly a C4-C12 conjugated diene. 1,3-butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene (piperylene), 2-chloro-1,3-butadiene, or mixtures thereof are preferred. 1,3-butadiene and isoprene, or mixtures thereof, are particularly preferred. 1,3-butadiene is especially very preferred.
[0069] The amount of conjugated diene is typically in the range of 40 to 90% by weight, preferably 50 to 85% by weight, and more preferably 56 to 83% by weight, relative to 100% by weight of the total amount of all monomer units in the HNBR rubber.
[0070] Further copolymers: Hydrogenated nitrile-diene copolymers may contain at least one additional monomer unit in addition to the monomer units described above. Exemplary additional monomer units are defined below.
[0071] Preferred examples of additional epoxy group-containing monomers are selected from the group consisting of 2-ethylglycidyl acrylate, 2-ethylglycidyl methacrylate, 2-(n-propyl)glycidyl acrylate, 2-(n-propyl)glycidyl methacrylate, 2-(n-butyl)glycidyl acrylate, 2-(n-butyl)glycidyl methacrylate, glycidyl methyl acrylate, glycidyl methyl methacrylate, glycidyl acrylate, and glycidyl methacrylate.
[0072] Most preferably, the epoxy group-containing monomer is a glycidyl (alkyl) acrylate, preferably a glycidyl acrylate and / or a glycidyl methacrylate.
[0073] Furthermore, copolymers used in accordance with the present invention may further comprise one or more units of further copolymerizable monomers known in the art, such as α,β-unsaturated (preferably monounsaturated) monocarboxylic acids, their esters and amides, α,β-unsaturated (preferably monounsaturated) dicarboxylic acids, their mono or diesters, and their respective anhydrides or amides, vinyl esters, vinyl ketones, α-monoolefins, vinyl monomers having a hydroxyl group, and carbon monoxide.
[0074] It is preferable to use acrylic acid and methacrylic acid as α,β-unsaturated monocarboxylic acids.
[0075] Esters of α,β-unsaturated monocarboxylic acids, preferably alkyl esters and alkoxyalkyl esters thereof, can also be used. Alkyl esters of α,β-unsaturated monocarboxylic acids, particularly C1-C18 alkyl esters, are preferred. Alkyl esters of acrylic acid or methacrylic acid, particularly C1-C18 alkyl esters, especially methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, n-dodecyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate and 2-ethylhexyl methacrylate are particularly preferred. Hydroxylalkyl acrylates and hydroxyalkyl methacrylates having 1 to 12 carbon atoms in the hydroxyalkyl group, preferably 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, and 3-hydroxypropyl acrylate, may also be used; α,β-unsaturated carboxylic acid esters containing an amino group, such as dimethylaminomethyl acrylate, N-(2-hydroxyethyl)acrylamide, N-(2-hydroxymethyl)acrylamide, urethane (meth)acrylate, and diethylaminoethyl acrylate, may also be used. Acetoacetoxyethyl methacrylate is another example of a preferred additional monomer.
[0076] Further copolymerizable monomers can also be α,β-unsaturated dicarboxylic acids, preferably maleic acid, fumaric acid, crotonic acid, itaconic acid, citraconic acid, and mesaconic acid.
[0077] Monoesters or diesters of α,β-unsaturated dicarboxylic acids can also be used. These α,β-unsaturated dicarboxylic acid monoesters or diesters may be, for example, alkyl, preferably C1-C10 alkyl, particularly ethyl, n-propyl, isopropyl, n-butyl, t-butyl, n-pentyl or n-hexyl, monoester or diester; alkoxyalkyl, preferably C2-C12 alkoxyalkyl, particularly preferably C3-C8 alkoxyalkyl, monoester or diester; hydroxyalkyl, preferably C1-C12 hydroxyalkyl, particularly preferably C3-C8 hydroxyalkyl, monoester or diester; cycloalkyl, preferably C5-C12 cycloalkyl, particularly preferably C6-C12 cycloalkyl, monoester or diester; alkylcycloalkyl, preferably C6-C12 alkylcycloalkyl, particularly preferably C7-C10 alkylcycloalkyl, monoester or diester; aryl, preferably C6-C14 aryl, monoester or diester, where the diester may be a mixed ester.
[0078] In a particularly preferred embodiment, the fully or partially hydrogenated HNBR rubber contains (01-04)-alkyl methacrylate, most preferably butyl acrylate.
[0079] The manufacture of such rubber is well known in this industry, and is described, for example, in the Handbook of Synthetic Rubber, in Chapter 5, pages 67-86, which deals with rubber in general, and in particular, in Chapter 14, pages 295-314, ARLANXEOD eutschland GmbH, Germany, 2020, which deals with HNBR.
[0080] Monomers used in polymerization are typically obtained from fossil resources, such as by cracking crude oil, but monomers from sustainable resources can also be used. The use of monomers from sustainable resources has the advantage of reducing the carbon footprint of polymers and articles produced therefrom. Examples of monomers from sustainable resources include those obtained from biosources such as plants, fungi, or bacteria. Such monomers are chemically identical to those obtained from fossil resources, but they have a higher carbon-14 isotope content, which allows them to be identified. Other examples of monomers from sustainable resources include those obtained from recycled waste such as recycled biological waste (e.g., wood pulp), recycled rubber waste (e.g., obtained from the pyrolysis of tires), and recycled plastic waste. Monomers derived from recycled materials include ISCC+ certified monomers, which can be used, for example, in so-called mass balance processes to reduce the total CO2 content in the production chain (see, for example, Pete Spanos et al, Sustainable Keltan EPDM, RUBBERWORLD.COM, April 2023. The process is described for EPDM polymers, but the principles described therein can be applied to other polymers accordingly). Unlike monomers derived from fossil resources, monomers from sustainable resources may or may not need to be purified to provide monomers of the same purity.
[0081] solvent Organic solvents enable the dissolution of binders or binder composite materials. They also allow for the dispersion of conductive materials such as carbon nanotubes. Common solvents include NMP, DMF, valerolactone, butyrolactone, xylene, and other aromatics, various esters, ketones, alcohols, ethers, and alkanes. Low-polarity solvents are primarily used in solid-state batteries, and their process solvents must be compatible with the solid electrolyte.
[0082] In accordance with the present invention, NMP is particularly preferred.
[0083] The solvent used in the process must be selected to allow for the dissolution of the binder, while the solubility of a particular HNBR grade depends on its monomer composition.
[0084] binder Polymer binders are a crucial component of electrodes and are used to stabilize active and conductive materials in the slurry during cathode manufacturing, thereby facilitating the processing of these materials and enabling smooth electrodes, such as cathodes with a clear pore structure. During use, cathode cohesion and its adhesion to the current collector are extremely important and are strongly influenced by the type of binder used and the respective functional sites of the polymer. Adhesion and cohesion are important properties of polymer binders that determine the final performance of lithium-ion batteries, especially in the long term. A good polymer binder ensures uniform dispersion of active and conductive materials, along with stable bonding to the metal electrode collector.
[0085] Many types of polymer binders can be used. For example, binders based on PVDF (polyvinylidene fluoride), PTFE, high molecular weight HNBR, PIB, CMC, PAA, PEDOT and PSS, PEO, SBR or PVP, or mixtures thereof, can be used, as they are easily compatible with cathodes operating at high operating voltages.
[0086] However, according to the present invention, PVP and PVDF are particularly preferred as binders, with PVP being particularly preferred.
[0087] Further technical features and advantages of the electrode composition are described in the descriptions of the electrodes, electrochemical energy storage devices, and examples.
[0088] The electrodes of an electrochemical energy storage device are further described, and the electrodes are formed from an electrode composition arranged as described above.
[0089] For example, the electrode composition can be applied to the current collector of the electrode, such as aluminum foil, aluminum foam, foamed aluminum, or carbon nonwoven fabric. In particular, the electrode can form a cathode.
[0090] Thus, the electrode may be formed from the composition described, or it may contain the composition.
[0091] Providing electrode compositions for electrodes such as cathodes offers the aforementioned advantages, particularly with respect to binder compositions.
[0092] In particular, it is possible to achieve extremely good dispersion of carbon nanotubes, thereby enabling even better electronic properties.
[0093] Another advantage is the secure bonding of the electrode material to the current collector, which is generally a thin aluminum foil, aluminum foam, foamed aluminum, or carbon nonwoven fabric. If the bonding is insufficient, the cathode may detach when it is bent in the core of the cylindrical cell. This can lead to a decrease in electrical contact and thus battery failure. Another problem can arise from uneven electrode edges if material is lost during slitting or cutting to size. This can even lead to short circuits.
[0094] Further technical features and advantages of the electrodes are described in the descriptions of the compositions, electrochemical energy storage devices, and examples.
[0095] An electrochemical energy storage device is further described, comprising an anode and a cathode, the cathode arranged as described above.
[0096] In particular, electrochemical energy storage devices are secondary batteries such as lithium-sulfur batteries. They comprise an anode, a cathode, and a separator located between the anode and cathode, by means of known methods. The anode may be formed from graphite or other materials known in the art, and the separator may include a polymer foil or a ceramic structure, as known to those skilled in the art.
[0097] The cathode is arranged as described above, thereby enabling each of the advantages described. In particular, excellent dispersion of carbon nanotubes can be achieved, thereby enabling even better electronic properties.
[0098] Further technical features and advantages of the electrochemical energy storage device are described in the descriptions of the compositions, electrodes, examples, and drawings.
[0099] active substance Many types of active materials can be used in the cathode of a LiS battery. For example, sulfur-containing active materials for the cathode can be based on sulfur, copolymerized sulfur, lithium polysulfide, lithium sulfide, lithium sulfide composite materials, sulfur copolymers such as (poly(S-co-DVB)), or carbon-sulfur polymers, sulfur-transition metal oxide composite materials, sulfur-transition metal sulfide composite materials, and sulfur-carbon composite materials. [Examples]
[0100] The following embodiments further illustrate the present invention in an exemplary manner, but are not intended to limit its scope.
[0101] The following materials were used as provided: Monomer units acrylonitrile (ACN) from Sigma-Aldrich, and 1,3-butadiene from INEOS. Fe(II)SO4 solution: The premix solution is made by adding Fe(II)SO4 to 400g of water. * Contains 0.986g of 7H2O and 6.0g of Rongalit® C. EDTA: Derived from Sigma-Aldrich as a complexing agent. Fatty acid: CAS 67701-08-8, emulsifier for polymerization. t-DDM: Molecular weight modifier. Glidox(registered trademark) 500: 2,6,6-trimethylbicyclo[3.1.1]heptylhydroperoxide from Renessenz, an initiator for emulsion polymerization. Diethylhydroxylamine: polymerization inhibitor, CAS 3710-84-7. Hoveyda-Grubbs catalyst, second generation, double decomposition catalyst, (1,3-bis-(2,4,6-trimethylphenyl)-2-imidazolidinylidene)dichloro(o-isopropoxyphenylmethylene)ruthenium Hydrogen from Nippon Gases. Lithium sulfide: Active substance, Li2S, 99.9% purity, Alfa Aesar Polyvinylpyrrolidone (PVP): Binder, PVP K90, AppliChem Chromium(III) oxide: additive, Cr2O3, 99+%, 60nm, IoLiTec-Ionic Liquids Technologies GmbH Acid-functionalized multilayer carbon nanotubes: Additive, MWCNT, 95+%, OD: 20-30 nm, L: 10-30 μm, IoLiTec-Ionic Liquids Technologies GmbH N-methylpyrrolidone: Solvent, NMP, Purity 99.5%, Acros Organics Carbon nonwoven fabric: current collector, Sigracet28AA, SGL Carbon SE Lithium foil: anode, 380 μm thick, foil punched out onto a 14 mm disc, Alfa Aesar Porous polyolefin film: Separator, Celgard 2500, Film punched out onto 16mm disc, Celgard Electrolyte: Solution of 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 0.2M lithium nitrate (LiNO3) in 1,3-dioxolane (DOL) / 1,2-dimethoxyethane (DME) (1:1 (weight ratio)), e-lyte innovations GmbH Coin cell: Casing, CR2025, Hohsen Corp. Spacer Disk: 16mm x 0.5mm, Hohsen Corp. Wave washer: Spring, 15mm x 1.4mm, Hohsen Corp. Gasket: Polypropylene, Hohsen Corp. Sample F: Fully hydrogenated butadiene acrylonitrile copolymer with less than 1% residual double bonds (ACN content 34 wt%); Mooney viscosity ML(1+4) 100℃ = 70 MU. Sample G: Fully hydrogenated butadiene acrylonitrile polymer with less than 1% residual double bonds (ACN content 21% by weight); Mooney viscosity ML(1+4)100℃ = 39 MU. Sample H: Fully hydrogenated butadiene acrylonitrile copolymer with less than 1% residual double bonds (ACN content 39 wt%); Mooney viscosity ML(1+4)100℃ = 39 MU. Sample I: Partially hydrogenated butadiene acrylonitrile copolymer with 5.5% residual double bonds (ACN content 43 wt%); Mooney viscosity ML(1+4)100℃ = 61 MU.
[0102] Test method Acrylonitrile content: The nitrogen content for determining the acrylonitrile content was determined according to Kjeldahl (DIN 53 625).
[0103] Determination of molecular weight: The molecular weight was determined in the form of number-average molecular weight (Mn) and weight-average molecular weight (Mw) using gel permeation chromatography (GPC) according to DIN55672-1 (Part 1: Tetrahydrofuran THF as solvent).
[0104] Mooney viscosity: The Mooney viscosity (ML 1+4 @ 100°C) is determined by a shear disk viscometer at 100°C according to DIN 53523 / 3 or ASTM D1646.
[0105] Method for evaluating discharge ratio capacity and capacity retention rate: After the formation process, the lithium secondary battery was charged with a constant current of 1C until the voltage reached 2.8V. Once the terminal voltage was reached, a constant voltage phase continued until the current reached 0.083C. After a 3-minute quiescent period, the battery was discharged with a constant current of 1C until the battery voltage reached 1.85V. This cycle was repeated 100 times. The discharge ratio capacity was calculated by taking the average of at least three cells. To evaluate the capacity retention rate, the discharge capacity of the first cycle and the 100th cycle were compared. The capacity retention rate was categorized as follows: A: Capacity retention rate of 95% or more. B: Capacity retention rate is 90% or more, but less than 95%. C: Capacity retention rate less than 90%. D: The cell failed before reaching 100 cycles.
[0106] Polymer manufacturing Low molecular weight hydrogenated butadiene-acrylonitrile copolymers are produced based on base polymers having the formulations specified in Table 1, with all feedstocks expressed in parts by weight per 100 parts by weight of the monomer mixture. Table 1 also shows the respective polymerization conditions.
[0107] [Table 1]
[0108] Each polymer was produced in batches in a 5L autoclave equipped with a stirring system. In each autoclave batch, 1.25 kg of monomer mixture, 2.1 kg of total water, and equimolar amounts of as-is EDTA based on Fe(II) from Fe(II)SO4 were used. This amount of 1.9 kg of water was initially charged into the autoclave with an emulsifier and purged with a nitrogen stream. t-DDM was added and the reactor was closed. When the contents were brought to polymerization temperature, polymerization was initiated by adding the Fe(II)SO4 premix solution and Glidox® 500 as an initiator. Polymerization proceeded at a predetermined temperature of 8–15°C with respect to Glidox® 500 and was monitored by gravimetric analysis of conversion. Once the conversion shown in Table 1 was achieved, polymerization was stopped by adding a 25% aqueous solution of diethylhydroxylamine. Unconverted monomers (i.e., non-polymerized) and remaining volatile substances were removed by steam distillation.
[0109] The antioxidant was mixed with a polymer dispersion to adjust the solid content to 17.5% by weight. Subsequently, the resulting dispersion, containing additional anti-aging components by adding acid according to a procedure known in the art, was subjected to coagulation, pH reduction, washing, dehydration, and drying.
[0110] Prior to the hydrogenation of the polymer, a double decomposition reaction was carried out to reduce the molecular weight of the nitrile rubber. Double decomposition is known, for example, from International Publication A02 / 100941 and International Publication A02 / 100905, and can be used to reduce molecular weight.
[0111] An acrylonitrile butadiene-based polymer was dissolved in monochlorobenzene at a solid concentration of 12-13% in a 10 L high-pressure reactor. Once the nitrile rubber was completely dissolved, 1-hexene 4 phr was added to the reactor, and the solution was stirred at 22°C for 2 hours. At that point, a solution of (1,3-bis-(2,4,6-trimethylphenyl)-2-imidazolidinylidene)dichloro(o-isopropoxyphenylmethylene)ruthenium in monochlorobenzene was added to the reactor. The solution was then stirred at 22°C until the desired molecular weight was achieved.
[0112] After the double decomposition reaction was complete, a monochlorobenzene solution consisting of Wilkinson catalyst and co-catalyst was added, and the pressure was increased to 8.4 MPa while the reactor temperature was adjusted to 137–140°C. Temperature and pressure were kept constant throughout the reaction. The reaction progress was monitored by measuring the residual double bond content by IR spectroscopy using a Perkin Elmer spectrum 100 FT-IR spectrometer. A polymer solution in monochlorobenzene was cast onto KBr disks and dried to form test films. The hydrogenation conversion rate was determined by FT-IR analysis according to ASTM D5670-95.
[0113] The reaction was stopped by releasing the hydrogen pressure when the residual double bond content reached <5%, preferably <1%.
[0114] The resulting hydrogenated polymer was isolated from the solution by vapor solidification. For this purpose, a monochlorobenzene solution was diluted to a polymer content of 7% by weight, filled with water, and continuously supplied by metering into a stirred glass reactor heated to 100°C. Simultaneously, 0.5 bar of steam was used to introduce the solution into the solidification water. The polymer, which precipitated as crumb, was dehydrated and then dried under vacuum at 55°C.
[0115] Table 2 shows the composition, monomer unit content, residual double bond percentage, and molecular weight of each hydrogenated polymer.
[0116] [Table 2]
[0117] General method of manufacturing coin cells The entire manufacturing process is carried out within an argon-filled glove box (Uni-Lab, M. Braun Inertgas-Systeme GmbH, equipped with a heatable antichamber).
[0118] Step (1) - Preparation of MWCNT-containing dispersion: A certain amount of HNBR is dissolved in the solvent (NMP) by mixing two components at room temperature for 24 hours using electromagnetic stirring. Then, MWCNT is added to the solution and the mixture is stirred for 2 hours until a homogeneous dispersion is formed. After that, PVP is added to the dispersion as a binder and the mixture is stirred for 30 minutes. Even when HNBR was not used as a dispersant, the weight of the components used and the procedure remained unchanged.
[0119] [Table 3]
[0120] Step (2) - Preparation of cathode slurry as electrode composition: The solid components Cr2O3, Li2S and the prepared dispersion (Step 1) are homogenized in a planetary ball mill (milling conditions: rotation speed: 500 rpm, duration: 5 minutes, interruption: 30 minutes, 5 cycles).
[0121] [Table 4]
[0122] Step (3) - Fabrication of disk electrodes: The slurry described (Step 2) is coated onto the carbon nonwoven current collector using a quadruple coating frame in the doctor blade process. The slit was 30 μm. The coated current collector is transferred to an oven and oven-dried overnight at 90°C under reduced pressure. The dried electrode sheet is punched out into disk electrodes.
[0123] Process (4) - Coin Cell Assembly: Coin cells are manufactured in a CR2025 housing. A lithium disk as the anode, a porous separator (Celgard 2500), the manufactured cathode, spacers, and springs are placed inside the housing. Each component is placed on top of the previous component. During assembly, 40 μl of electrolyte is added to the separator. The coin cells are then pressed in a coin cell crimper (Automatic Coin Crimper HSACC-10, Hohsen Corp.).
[0124] Figure 5 shows how to determine the initial discharge capacity and capacity retention rate of a lithium-sulfur battery (LSB).
[0125] [Table 5]
[0126] When using low molecular weight HNBR samples with a specific acrylonitrile content, a high discharge capacity greater than 500 mAh / g can be achieved along with excellent capacity retention.
[0127] Thus, the remarkable advantages of the composition according to the present invention are demonstrated.
Claims
1. An electrode composition for an electrode of a lithium-sulfur-based electrochemical energy storage device, comprising (i) a solvent, (ii) a binder, (iii) an active substance, and (iv) a conductive carbon material, wherein the active substance comprises a sulfur-based active substance, the conductive carbon material comprises carbon nanotubes, and the electrode composition further comprises (v) a dispersion aid for dispersing the carbon nanotubes, in the electrode composition, The dispersing agent contains hydrogenated nitrile butadiene rubber, and the hydrogenated nitrile butadiene rubber is Molecular weight Mn>10kg / mol~<83kg / mol; Molecular weight Mw > 10 kg / mol to < 245 kg / mol; and Acrylonitrile content <39% by weight An electrode composition characterized by having [a certain characteristic].
2. The aforementioned hydrogenated nitrile butadiene rubber, Molecular weight Mn > 15 kg / mol to < 75 kg / mol; and / or Molecular weight Mw ≥ 20 kg / mol to < 240 kg / mol; and / or Acrylonitrile content: 30-38% by weight The electrode composition according to claim 1, having at least one of the following.
3. The electrode composition according to claim 1 or 2, wherein the dispersion aid is present in the electrode composition in an amount of ≥2% to ≤150% by weight relative to the carbon nanotubes.
4. The electrode composition according to any one of claims 1 to 3, wherein the dispersion aid is present in the electrode composition in an amount of ≥0.05% by weight to ≤10% by weight relative to the electrode composition.
5. The electrode composition according to any one of claims 1 to 4, wherein the carbon nanotube is a multi-walled carbon nanotube.
6. The electrode composition according to any one of claims 1 to 5, wherein the content of residual double bonds in the dispersant is <1%.
7. The electrode composition according to any one of claims 1 to 6, comprising N-methyl-2-pyrrolidone as a solvent.
8. The electrode composition according to any one of claims 1 to 7, comprising at least one of polyvinylpyrrolidone, polyacrylic acid, or polyvinylidene fluoride as a binder.
9. Solvent in an amount of ≥85 to ≤97% by weight; Dispersing agent in an amount of ≥0.05 to ≤10% by weight; Carbon nanotubes in amounts of ≥0.5 to ≤10% by weight; and Binder in quantities of ≥0 to ≤10% by weight Includes, The aforementioned dispersing agent contains hydrogenated nitrile butadiene rubber, and the hydrogenated nitrile butadiene rubber is Molecular weight Mn>10kg / mol~<83kg / mol; Molecular weight Mw > 10 kg / mol to < 245 kg / mol; and Acrylonitrile content <39% by weight It has, The electrode composition according to any one of claims 1 to 8, wherein the total amount of the solvent, the binder, the carbon nanotubes, and the dispersion aid is 98% by weight or more, preferably 100% by weight.
10. The electrode composition according to any one of claims 1 to 9, wherein the dispersion aid has a Mooney viscosity ML(1+4) at 100°C, (MU) ≤ 70.
11. An electrode for an electrochemical energy storage device, wherein the electrode is formed from an electrode composition, and the electrode composition is arranged according to any one of claims 1 to 10.
12. An electrochemical energy storage device comprising an anode and a cathode, wherein the cathode is arranged according to claim 11.
Citation Information
Patent Citations
Conductor dispersion and secondary battery manufactured using same
EP3333946A1
Conductive material dispersion and utilization thereof
JP2020187866A
Cathode material for li-s battery and method for forming the same
WO2012040934A1
Cathode material for a li-s battery and the method for preparing the same, a cathode made of the cathode material and a li-s battery comprising the cathode
WO2014082296A1
Positive electrode active material slurry comprising rubber-based binder and positive electrode produced from same