Hot-dip galvanized steel sheet and method for manufacturing the same

The method of spraying a mixed aqueous solution of water, urea, and alcohol on hot-dip galvanized steel sheets enhances spangle refinement and reduces carbon content, addressing issues of corrosion resistance and paint adhesion, resulting in improved surface quality for automotive and construction uses.

JP2026539267APending Publication Date: 2026-11-24POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026522586
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-17
Filing Date
2023-12-20
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Conventional methods for reducing spangle size in hot-dip galvanized steel sheets are inadequate, leading to poor corrosion resistance, paint adhesion, and surface appearance due to residual phosphate components and large spangle sizes.

Method used

A method involving the formation of a hot-dip galvanized steel sheet with fine spangles by spraying a mixed aqueous solution of water, urea, and alcohol, along with air, to increase solidification nuclei density and control the spangle size to 150 μm or less, while maintaining a carbon content of 0.2% by weight or less in the surface layer.

Benefits of technology

The method results in a hot-dip galvanized steel sheet with improved corrosion resistance, paint adhesion, and surface appearance, suitable for automotive and construction applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539267000001_ABST
    Figure 2026539267000001_ABST
Patent Text Reader

Abstract

One aspect of the present invention is to provide a hot-dip galvanized steel sheet and a method for manufacturing the same. Another aspect of the present invention is to provide a hot-dip galvanized steel sheet having fine spangles and good paint quality, and a method for manufacturing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to hot-dip galvanized steel sheets and a method for manufacturing the same. [Background technology]

[0002] Generally, hot-dip galvanized steel sheets are manufactured by immersing a steel sheet that has passed through an annealing furnace in a hot-dip galvanizing bath, and then allowing the applied molten zinc to solidify. As the molten zinc plated onto the steel sheet cools, spangles, which are dendritic crystal grains, are formed on the surface of the plating layer. When zinc solidifies, dendritic crystals (dendrites) grow very rapidly in the initial stages of solidification due to solidification nuclei, forming a coarse spangle pattern. Therefore, it can be said that the size of the spangles is determined in the initial stages of solidification.

[0003] The coarse spangles formed on the surface of the plating layer degrade the corrosion resistance, paint adhesion, and surface appearance after painting of the plating layer.

[0004] Therefore, the quality of the plated steel sheet can be improved by reducing the size of the spangles formed on the hot-dip galvanized steel sheet.

[0005] Conventional methods for reducing the size of spangles include, for example, (1) using a plating bath that does not contain antimony (Sb) or lead (Pb) to form the spangles, (2) applying pressure with a skin pass roll after plating, or (3) spraying water or a phosphate solution before the coated zinc solidifies.

[0006] However, this conventional method has the problem that not only does the spangle size not become small enough, but phosphate components remain, leading to the side effect of poor coating quality in additional processes.

[0007] Therefore, there is a need for a method that precisely reduces the size of the spangles in hot-dip galvanized steel sheets while simultaneously improving the surface appearance and quality without the side effects mentioned above. [Overview of the Initiative] [Problems that the invention aims to solve]

[0008] One aspect of the present invention is to provide a hot-dip galvanized steel sheet and a method for manufacturing the same.

[0009] Another aspect of the present invention is to provide a hot-dip galvanized steel sheet having fine spangles and good paint quality, and a method for manufacturing the same. [Means for solving the problem]

[0010] One embodiment of the present invention provides a hot-dip galvanized steel sheet comprising a base steel sheet and a hot-dip galvanized layer formed on at least one surface of the base steel sheet, wherein the average size of spangles formed on the surface of the hot-dip galvanized layer is 150 μm or less (excluding 0 μm), and the carbon content in a region within 2 μm in the thickness direction from the surface of the hot-dip galvanized layer is 0.2% by weight or less (including 0%).

[0011] Another embodiment of the present invention provides a method for manufacturing a hot-dip galvanized steel sheet, comprising the steps of: forming a hot-dip galvanized layer on at least one surface of a base steel sheet; spraying an aqueous solution onto the hot-dip galvanized layer; and cooling the hot-dip galvanized layer onto which the aqueous solution has been sprayed, wherein the step of spraying the aqueous solution includes spraying a mixed aqueous solution and air, the mixed aqueous solution consisting of water, urea, and alcohol, the average droplet size of the mixed aqueous solution when sprayed being 10 to 50 μm, the urea content being 0.1 to 5.0% by weight, and the alcohol content being 0.1 to 5.0% by weight.

[0012] The step of adjusting the amount of hot-dip galvanized layer deposited may be further included between the step of forming the hot-dip galvanized layer and the step of spraying the aqueous solution.

[0013] The mixed aqueous solution can be sprayed with the steel sheet temperature during hot-dip galvanizing of ~419°C as the spray start temperature and the steel sheet temperature of 417~415°C as the spray end temperature.

[0014] The mixed aqueous solution can be sprayed by passing through a charging electrode.

[0015] When the mixed aqueous solution passes through the charging electrode, the voltage applied to the charging electrode may be -1 to -50 kV.

[0016] The alcohol may be at least one selected from the group consisting of ethanol, propanol, isopropanol, butanol, and isobutanol.

[0017] The spray pressure of the air is 1.5 to 5.0 kgf / cm 2 .

[0018] The spray pressure of the mixed aqueous solution is 0.5 to 2.5 kgf / cm 2 .

[0019] The mixed aqueous solution and air may be sprayed at a pressure ratio of 0.3 to 0.9. [Advantageous Effects of the Invention]

[0020] According to one aspect of the present invention, a hot-dip galvanized steel sheet and a method of manufacturing the same can be provided.

[0021] According to another aspect of the present invention, a hot-dip galvanized steel sheet which has fine spangles, has good coating quality, and is preferably used for inner and outer plates of automobile bodies, home appliances, construction materials, and the like, and a method of manufacturing the same can be provided. [Brief Description of the Drawings]

[0022] [Figure 1] is a schematic view showing an embodiment of an apparatus for manufacturing a hot-dip galvanized steel sheet applicable to the present invention. [Figure 2]These are the EPMA analysis results for the hot-dip galvanized coating of Invention Example 1 according to an embodiment of the present invention. [Figure 3] These are the EPMA analysis results for the hot-dip galvanized coating of Comparative Example 6, which deviates from an embodiment of the present invention. [Embodiments for Carrying Out the Invention]

[0023] Hereinafter, a hot-dip galvanized steel sheet according to an embodiment of the present invention will be described.

[0024] The hot-dip galvanized steel sheet according to an embodiment of the present invention includes a base steel sheet and a hot-dip galvanized coating formed on at least one surface of the base steel sheet. In the present invention, the type of the base steel sheet is not particularly limited, and any steel sheet for hot-dip galvanized steel sheets commonly used in the technical field can be used. In addition, the type of the hot-dip galvanized coating is not particularly limited in the present invention. However, as an example, the hot-dip galvanized coating may be made of pure zinc (Zn), and may further include one or more of aluminum (Al), magnesium (Mg), antimony (Sb), and lead (Pb). More specifically, the hot-dip galvanized coating may include Al: 0.13 to 0.3 wt% and the balance Zn, and may be a binary Zn-Al hot-dip galvanized coating or a ternary Zn-Al-Mg hot-dip galvanized coating. In the case of the binary Zn-Al hot-dip galvanized coating, it may include 40 to 95 wt% of Al, and in the case of the ternary Zn-Al-Mg hot-dip galvanized coating, it may include 0.1 to 30% of each of Al and Mg.

[0025] In the present invention, it is preferable that the average size of the spangles formed on the surface of the hot-dip galvanized layer of the hot-dip galvanized steel sheet is 150 μm or less (excluding 0 μm). By forming such fine spangles, the corrosion resistance, paint adhesion, and surface appearance of the hot-dip galvanized steel sheet can be improved. If the average size of the spangles exceeds 150 μm, it is difficult to sufficiently ensure the spangle refinement effect described above. Therefore, it is preferable that the average size of the spangles is 150 μm or less (excluding 0 μm). It is more advantageous that the average size of the spangles is 140 μm or less, even more advantageous that it is 130 μm or less, and most advantageous that it is 120 μm or less.

[0026] In the present invention, it is preferable that the carbon content in the region within 2 μm of the surface of the hot-dip galvanized layer in the thickness direction is 0.2% by weight or less (including 0%). When carbon is present in the surface layer of the hot-dip galvanized layer, problems such as reduced weldability and paint adhesion may occur. In the present invention, by controlling the carbon content in the surface layer of the hot-dip galvanized layer as described above, it is possible to improve the usability of the steel sheet while also achieving a beautiful surface. However, in the present invention, the upper limit of the carbon content in the surface layer of the hot-dip galvanized layer is limited to 0.2% by weight, and if the carbon content exceeds 0.2% by weight, the above-mentioned problems may occur. Therefore, it is preferable that the carbon content in the region within 2 μm of the surface of the hot-dip galvanized layer in the thickness direction is 0.2% by weight or less (including 0%). It is even more advantageous that the carbon content in the region within 2 μm of the surface of the hot-dip galvanized layer in the thickness direction is 0.1% by weight or less.

[0027] Figure 1 is a schematic diagram showing one embodiment of a manufacturing apparatus for hot-dip galvanized steel sheets applicable to the present invention. The method for manufacturing hot-dip galvanized steel sheets according to one embodiment of the present invention will be described below with reference to Figure 1.

[0028] First, a hot-dip galvanized layer is formed on at least one surface of the base steel sheet. In this invention, the method for forming the hot-dip galvanized layer is not particularly limited, and all methods for forming a hot-dip galvanized layer commonly used in the art can be used. For example, as shown in Figure 1, a method of immersing the base steel sheet 2 in a hot-dip galvanizing bath 1 can be used.

[0029] On the other hand, after forming the hot-dip galvanized layer, the process may further include a step to adjust the amount of the hot-dip galvanized layer. Through this step of adjusting the amount of the hot-dip galvanized layer, excess plating metal can be removed to appropriately control the amount of plating. In this invention, the method for adjusting the amount of the hot-dip galvanized layer is not particularly limited, and as an example, an air wiping process using an air knife 3 can be used. Furthermore, in this invention, the amount of plating is not particularly limited and can be appropriately controlled depending on the intended use of the hot-dip galvanized steel sheet. However, as an example, the amount of plating is 20 to 500 g / m² on a single-sided basis. 2 It can have a range.

[0030] Next, an aqueous solution is sprayed onto the hot-dip galvanized layer. When spraying the aqueous solution, it is preferable to spray a mixed aqueous solution and air. Generally, spangles are formed when a molten galvanized layer cools, and solidification nuclei are generated and grown through this process. In order to refine the size of the spangles, the density of solidification nuclei must be increased during the solidification reaction stage of the plating layer, so that solidification ends before dendritic crystals can grow. Therefore, in this invention, by spraying air together with the aqueous solution, the droplets of the aqueous solution are turned into mist, increasing the density of solidification nuclei and allowing them to act as solidification nuclei on the surface of the steel sheet. On the other hand, conventionally, aqueous solutions of the phosphate series have been used to promote nucleation on the surface of the plating layer, but their use has been limited because they contaminate surrounding equipment after drying or remain on the surface of the steel sheet as a glassy film, inducing a secondary deterioration of physical properties. In particular, the glassy phosphate remaining on the surface of the steel sheet reduces paint adhesion during painting and can also cause low-temperature joint brittleness. In this invention, in order to improve upon this, the cooling rate of the plating layer during the spraying of the aqueous solution is increased, and a mixed aqueous solution consisting of water, urea, and alcohol is sprayed so that no residue is generated after drying. The spraying of the mixed aqueous solution and air can be performed via a spray nozzle 5.

[0031] In other words, when a mixed aqueous solution consisting of water, urea, and alcohol is sprayed instead of a conventional phosphate aqueous solution, the solidification rate of the steel plate surface is accelerated by the endothermic reaction heat of urea, the evaporation heat of alcohol, and the vaporization heat of water, as shown in [Equation 1], [Equation 2], and [Equation 3] below. Furthermore, the alcohol reduces the surface tension of the aqueous solution, causing the droplets to become even finer during spraying compared to a phosphate aqueous solution, forming more solidification nuclei, and allowing the molten zinc to cool rapidly, resulting in even finer spangles. On the other hand, the water and urea constituting the mixed aqueous solution can be added using urea solution commonly used in the art. In this invention, there are no particular limitations on the type of urea solution, but for example, AdBlue (registered trademark) consisting of 67.5% purified water and 32.5% urea ((NH2)2CO) can be diluted and used. [Equation 1] (NH2)2CO + H2O → 2NH3 + CO2ΔH° (heat of reaction) = 185.5 kJ / mol [Equation 2] C2H5OH(l) → C2H5OH(g) ΔH° (heat of vaporization) = 39.3 kJ / mol [Equation 3] H2O(l) → H2O(g) ΔH° (heat of vaporization) = 43.1 kJ / mol

[0032] The above mixed aqueous solution can be sprayed with a steel plate temperature of ~419°C (hot-dip galvanizing temperature) as the spraying start temperature and a steel plate temperature of 417~415°C as the spraying end temperature. This is because applying solidification nuclei from the outside is effective in promoting the formation of solidification nuclei. The above "hot-dip galvanizing temperature" refers to the steel plate temperature when the amount of hot-dip galvanizing layer is adjusted, more specifically, when the steel plate has undergone air wiping treatment during the plating process. By spraying the aqueous solution onto the steel plate from the hot-dip galvanizing temperature, the steel plate is cooled and the molten zinc solidifies. However, experiments have shown that only droplets that adhere at around 419°C can act as solidification nuclei, and aqueous solution sprayed onto the steel plate before or after the solidification of molten zinc begins only serves to remove heat from the steel plate. Therefore, in order to form a large number of solidification nuclei, it is preferable to spray the aqueous solution onto the steel plate at around 419°C. In other words, if the steel plate temperature at the start of aqueous solution spraying is lower than 419°C, the spangles will become larger, and there is a risk of dendritic crystal formation. However, since it is difficult to accurately measure the temperature of the steel sheet being produced, the coarsening of the plating structure can be prevented by spraying at 419°C or higher, when the hot-dip galvanized layer is in a completely molten state. Therefore, the spraying start temperature of the above mixed aqueous solution may be a steel sheet temperature between the hot-dip galvanizing temperature and 419°C, more preferably between 460°C and 419°C, and even more preferably between 430°C and 419°C. Furthermore, if the spraying end temperature of the mixed aqueous solution exceeds 417°C, the solidification nuclei that have been formed may remelt, and if it is below 415°C, the solidification and cooling effects will saturate. Therefore, the spraying end temperature of the above mixed aqueous solution may be between 417°C and 415°C.

[0033] It is important to deposit as many liquid droplets as possible onto the steel plate within the above-mentioned injection start and end temperature ranges. Considering this, smaller droplets are advantageous for the same solution injection volume, as they allow for a greater number of droplets to be formed.

[0034] For this purpose, the above mixed aqueous solution can be sprayed by passing it through the high-voltage charged electrode 6. This causes the aqueous solution droplets to generate static electricity, which can then adhere to the steel plate due to the electrical attraction between the droplets and the steel plate. On the other hand, using a mesh-type charged electrode as the high-voltage charged electrode allows for the formation of a uniform electric field, further improving the effect of the high voltage. Furthermore, it is possible to miniaturize the droplets, preventing the pitting phenomenon that occurs when large droplets collide with the molten plating layer, thus preventing damage to the appearance.

[0035] This effect becomes more pronounced with higher applied voltages, and for this reason, the voltage applied to the charging electrode when the mixed aqueous solution passes through it can be between -1 and -50kV. If the voltage is less than -1kV, coarse spangles may form, and if the voltage is increased excessively, electrical sparks may occur between the charging electrode and the steel plate, so it is preferable to keep it below -50kV. On the other hand, the charging electrode is for creating negatively charged droplets (mist), and the negative sign of the voltage indicates polarity.

[0036] The average size of the droplets when the above mixed aqueous solution is sprayed is preferably 10 to 50 μm. By controlling the average size of the droplets in this way, a spangle of uniform size can be formed, resulting in a more beautiful surface appearance. If the average size of the droplets is less than 10 μm, the amount of droplets reaching the steel plate may be small, and if the average size of the droplets exceeds 50 μm, there is a disadvantage that the spangle refinement effect will be small. Therefore, the average size of the droplets is preferably 10 to 50 μm. The lower limit of the average size of the droplets is more advantageous at 15 μm, and even more advantageous at 20 μm. The upper limit of the average size of the droplets is more advantageous at 45 μm, and even more advantageous at 40 μm.

[0037] On the other hand, as shown in [Equation 1], [Equation 2], and [Equation 3] above, the urea solution absorbs the latent heat of the steel sheet through an endothermic reaction as the urea decomposes along with the evaporation of alcohol and water. It temporarily remains on the surface and acts as a solidification nucleus, and the plating layer solidifies around this nucleus. In addition, the alcohol reduces the surface tension of the aqueous solution, reducing the size of the droplets during spraying and increasing the cooling effect on the surface due to the heat of vaporization. Generally, one solidification nucleus forms one spangle, so the smaller the droplets of aqueous solution sprayed with the same amount of aqueous solution, the higher the density of solidification nuclei, which is advantageous for manufacturing hot-dip galvanized steel sheets with small spangle sizes. Therefore, it is preferable to spray a mixed aqueous solution of appropriate concentration to further promote the formation of solidification nuclei in the solidification reaction.

[0038] The urea content is preferably 0.1 to 5.0% by weight. If the urea content is less than 0.1%, the spangle refinement effect cannot be sufficiently obtained, and if it exceeds 5.0%, not only will manufacturing costs increase, but the urea may turn into a solid powder upon drying, contaminating surrounding equipment. In addition, problems may arise such as poor weldability and paint adhesion as a large amount of carbon remains on the surface of the plating layer. Therefore, the content of the above element is preferably 0.1 to 5.0% by weight. The lower limit of the content of the above element is more advantageous at 0.2% by weight, and even more advantageous at 0.3% by weight. The upper limit of the content of the above element is more advantageous at 4.5% by weight, and even more advantageous at 4.0% by weight.

[0039] The alcohol content is preferably 0.1 to 5.0% by weight. If the alcohol content is less than 0.1%, the spangle refinement effect cannot be sufficiently obtained, and if it exceeds 5.0%, not only will the manufacturing cost increase, but there may also be damage due to odor due to volatility. Therefore, the alcohol content is preferably 0.1 to 5.0% by weight. The lower limit of the alcohol content is more advantageous at 0.3% by weight, and even more advantageous at 0.5% by weight. The upper limit of the alcohol content is more advantageous at 4.0% by weight, and even more advantageous at 3.0% by weight. On the other hand, the present invention does not particularly limit the type of alcohol, but for example, one or more selected from the group consisting of ethanol, propanol, isopropanol, butanol, and isobutanol can be used.

[0040] On the other hand, the air injection pressure is 1.5 to 5.0 kgf / cm². 2 This is possible. The above air injection pressure is 1.5 kgf / cm². 2 If the pressure is less than 5.0 kgf / cm², the injection pressure is too low, making it difficult for the droplets of the injected aqueous solution to adhere to the steel plate. 2If it exceeds this range, the kinetic energy of the injected aqueous solution droplets becomes excessively high, which may cause pitting marks on the plating layer surface due to indentation by the droplets, thereby damaging the surface appearance.

[0041] The injection pressure of the mixed aqueous solution may be 0.5 to 2.5 kgf / cm 2 . If the injection pressure of the mixed aqueous solution is less than 0.5 kgf / cm 2 , the spangle refinement effect may be reduced. If the injection pressure of the mixed aqueous solution exceeds 2.5 kgf / cm 2 , pitting marks may occur due to the impact of aqueous solution droplets on the steel sheet surface, damaging the appearance.

[0042] The mixed aqueous solution and air may be injected at a pressure ratio of 0.3 to 0.9. If the pressure ratio between the mixed aqueous solution and air is less than 0.3, the aqueous solution may not be injected, making it difficult to achieve the spangle refinement effect. If the pressure ratio exceeds 0.9, drop marks may occur, damaging the surface appearance.

[0043] Thereafter, the hot-dip galvanized layer onto which the aqueous solution was injected is cooled. Through the above cooling process, a hot-dip galvanized layer with refined spangles can be formed. In the present invention, the cooling process is not particularly limited, and all cooling conditions commonly used in the relevant technical field may be employed. [Examples]

[0044] Hereinafter, the present invention will be described more specifically through examples. However, it should be noted that the following examples are only for illustrating and explaining the present invention in more detail, and are not intended to limit the scope of the present invention. This is because the scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.

[0045] (Example) A 0.8 mm thick base steel sheet containing, by weight, C: 0.03%, Si: 0.01%, Mn: 0.15%, P: 0.008%, the remainder Fe and other unavoidable impurities, in a hot-dip galvanizing bath containing Al: 0.18 wt% and the remainder Zn, was immersed at a moving speed of 80 m / min and air-wiped to achieve a plating rate of 70 g / m² per side. 2 A hot-dip galvanized layer was formed on the base steel sheet to have the specified plating adhesion amount. Afterward, a mixed aqueous solution having the composition shown in Table 1 below and air were simultaneously sprayed onto the surface of the hot-dip galvanized layer through a two-fluid spray nozzle. At this time, the spraying start temperature of the mixed aqueous solution was 420°C (steel sheet temperature), and the spraying end temperature was 417°C (steel sheet temperature). Afterward, the hot-dip galvanized layer to which the aqueous solution had been sprayed was cooled. In contrast, in Comparative Example 10, the above-described spraying of the mixed aqueous solution and air was not performed.

[0046] The average spangle size, carbon content of the surface layer, corrosion resistance, paint adhesion, and surface appearance of the hot-dip galvanized steel sheets manufactured in this manner were measured, and the results are shown in Table 2 below.

[0047] The average size of the spangles was measured as follows: Ten straight lines were drawn vertically and horizontally at equal intervals on photographs of the hot-dip galvanized layer taken using an optical microscope and SEM, and the total number of spangles through which these lines passed was counted. After calculating the sum of the lengths of these lines, the average length of a single spangle was measured by dividing it by the total number of spangles. This average length was then considered as the equivalent diameter of a circle and used to determine the average size of the spangles (sum of straight line lengths / total number of spangles = average length of a single spangle).

[0048] The carbon content of the surface layer of the hot-dip galvanized layer was measured using the EDS carbon atom surface analysis method, within a region of 2 μm in the thickness direction from the surface of the hot-dip galvanized layer.

[0049] On the other hand, to evaluate the corrosion resistance and paint adhesion after painting, test specimens were prepared from the hot-dip galvanized steel sheets manufactured as described above. These test specimens were prepared by coating the hot-dip galvanized steel sheets with melamine-alkyd resin to a thickness of approximately 20 μm using a roll-coater coating test machine, baking them at a post-mass temperature (PMT) of 160°C for 30 seconds, and then cooling them with water to room temperature.

[0050] The corrosion resistance after painting was tested by applying 1 kg / m² of 5% NaCl at 35°C to the above test specimen using a salt spray apparatus (Japanese Industrial Standard Test Method JIS E2731). 2 After spraying at the specified pressure, the time required until 5% white rust appeared was evaluated. A time of 480 hours or more but 680 hours or less was rated ○ (Excellent), 360 hours or more but less than 480 hours was rated △ (Average), and less than 360 hours was rated × (Poor).

[0051] Paint adhesion was evaluated by immersing the test specimen in distilled water at 50°C for 240 hours, allowing it to air dry, creating 100 checkerboard markings at 1mm intervals on the paint film surface, and then counting the number of paint film pieces that peeled off onto the tape when the paint film was removed with Scotch tape. At this time, no peeling was evaluated as ○ (excellent), a peeling rate of more than 0% but less than or equal to 3% was evaluated as △ (average), and a peeling rate of more than 3% was evaluated as × (poor).

[0052] The surface appearance was evaluated as follows: the color difference (ΔE) compared to Comparative Example 10 was measured, and a value of 0.5 or greater was rated as ○, a value of 0.3 or greater but less than 0.5 was rated as △ (normal), and a value of less than 0.3 was rated as × (poor).

[0053] [Table 1]

[0054] [Table 2]

[0055] As can be seen from Tables 1 and 2 above, in the case of Invention Examples 1 to 12, which satisfy the conditions proposed by the present invention, corrosion resistance, paint adhesion, and surface appearance are good. On the other hand, in the case of Comparative Examples 1 to 10, which do not satisfy the conditions proposed by the present invention, one or more of the corrosion resistance, paint adhesion, and surface appearance are not good.

[0056] Figure 2 shows the EPMA analysis results for the hot-dip galvanized layer of Invention Example 1. Figure 3 shows the EPMA analysis results for the hot-dip galvanized layer of Comparative Example 23. As can be seen from Figures 2 and 3, in Invention Example 1, almost no carbon is observed, but in Comparative Example 6, a relatively large amount of carbon is observed. [Explanation of Symbols]

[0057] 1. Hot-dip zinc plating bath 2. Untreated steel sheet 3. Air knife 4 Injection tank 5 spray nozzles 6. Charged electrodes 7 Air Curtain 8. Intake Hood 9 pyrometer

Claims

1. The material comprises a base steel sheet and a hot-dip galvanized layer formed on at least one surface of the base steel sheet. The average size of the spangles formed on the surface of the hot-dip galvanized layer is 150 μm or less (excluding 0 μm), A hot-dip galvanized steel sheet in which the carbon content in a region within 2 μm in the thickness direction from the surface of the hot-dip galvanized layer is 0.2% by weight or less (including 0%).

2. A step of forming a hot-dip galvanized layer on at least one surface of the base steel sheet; The step of spraying an aqueous solution onto the molten zinc plating layer; and The step includes cooling the molten zinc plating to which the aqueous solution has been sprayed, The step of spraying the aqueous solution includes spraying the mixed aqueous solution and air, The aforementioned mixed aqueous solution consists of water, urea, and alcohol. The average size of the droplets during the spraying of the mixed aqueous solution is 10 to 50 μm. The urea content is 0.1 to 5.0% by weight. A method for manufacturing a hot-dip galvanized steel sheet, wherein the alcohol content is 0.1 to 5.0% by weight.

3. The method for manufacturing a hot-dip galvanized steel sheet according to claim 2, further comprising a step of adjusting the amount of hot-dip galvanized layer deposited between the step of forming the hot-dip galvanized layer and the step of spraying the aqueous solution.

4. The method for manufacturing a hot-dip galvanized steel sheet according to claim 2, wherein the mixed aqueous solution is sprayed with a steel sheet temperature of 417 to 415°C as the spraying start temperature and a steel sheet temperature of 417 to 415°C as the spraying end temperature.

5. The method for manufacturing a hot-dip galvanized steel sheet according to claim 2, wherein the mixed aqueous solution is sprayed after passing through a charging electrode.

6. The method for manufacturing a hot-dip galvanized steel sheet according to claim 5, wherein the voltage applied to the charging electrode when the mixed aqueous solution passes through the charging electrode is -1 to -50 kV.

7. The method for producing a hot-dip galvanized steel sheet according to claim 2, wherein the alcohol is one or more selected from the group consisting of ethanol, propanol, isopropanol, butanol, and isobutanol.

8. The air injection pressure is 1.5 to 5.0 kgf / cm². 2 The method for manufacturing a hot-dip galvanized steel sheet according to claim 2.

9. The injection pressure of the mixed aqueous solution is 0.5 to 2.5 kgf / cm². 2 The method for manufacturing a hot-dip galvanized steel sheet according to claim 2.

10. The method for manufacturing a hot-dip galvanized steel sheet according to claim 2, wherein the mixed aqueous solution and air are sprayed at a pressure ratio of 0.3 to 0.9.