Secondary battery and method for manufacturing the same

The secondary battery design with a center pin and melting polymer electrolyte addresses electrolyte impregnation and stability issues, ensuring consistent performance and extended lifespan.

JP2026539274APending Publication Date: 2026-11-24LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026523927
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-11-27
Filing Date
2024-12-05
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Secondary batteries face issues with electrolyte impregnation and stability, particularly in large-scale batteries, leading to decreased capacity and shortened lifespan due to insufficient electrolyte quantity and loss during charging and discharging.

Method used

A secondary battery design incorporating a center pin with multiple holes and a polymer electrolyte that melts at a predetermined temperature, along with electrolyte sheets, ensures improved electrolyte impregnation and stability by replenishing electrolyte during operation.

Benefits of technology

The design enhances electrolyte impregnation and output stability in large-scale batteries, maintaining capacity and extending lifespan by replenishing electrolyte within the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539274000001_ABST
    Figure 2026539274000001_ABST
Patent Text Reader

Abstract

The present invention relates to a secondary battery comprising: an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separation membrane interposed between the positive and negative electrode plates are wound in one direction and impregnated with an electrolyte; a hollow center pin located on the winding shaft of the electrode assembly and having a plurality of holes formed on its outer circumferential surface; an electrolyte solid disposed inside the hollow of the center pin and containing a first polymer electrolyte having a melting point of 60°C to 73°C; a battery case housing the electrode assembly and the center pin; and a seal that seals the open end of the battery case. By applying the electrolyte solid to the secondary battery, a secondary battery with improved electrolyte impregnation can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims priority rights based on Korean Patent Application No. 10-2023-0176098, filed on December 6, 2023, and Korean Patent Application No. 10-2024-0172904, filed on November 27, 2024, and all content disclosed in the documents of said Korean patent applications is incorporated herein by reference.

[0002] The present invention relates to a secondary battery, and more particularly to a secondary battery with improved output stability and impregnation properties. [Background technology]

[0003] With technological advancements in electric vehicles and portable devices, the demand for rechargeable batteries as an energy source is rapidly increasing. In particular, as the application range of rechargeable batteries expands to electric vehicles (EVs) and hybrid electric vehicles (HEVs), there is a growing demand for rechargeable batteries with superior capacity and output stability.

[0004] In particular, to achieve high-capacity secondary batteries, secondary batteries are being manufactured on a larger scale. As the capacity and size of secondary batteries increase, more electrolyte needs to be injected into the battery. Here, it is important to ensure that the enlarged electrode assemblies are sufficiently impregnated with the electrolyte. If the electrode assemblies of the secondary battery are not sufficiently impregnated with the electrolyte, it can lead to problems such as a decrease in the capacity of the secondary battery, accelerated electrode degradation, and a shortened lifespan of the secondary battery.

[0005] Furthermore, the above problems can also occur if the amount of electrolyte is insufficient. For example, the amount of electrolyte is determined by the initial amount injected, but repeated charging and discharging during the use of a secondary battery can reduce the amount of electrolyte, potentially leading to electrolyte loss.

[0006] Therefore, technologies are needed to complement the electrolyte impregnation properties and electrolyte quantity of secondary batteries. [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] To solve the above-mentioned problems, the first technical problem that the present invention aims to solve is to provide a secondary battery with improved electrolyte impregnation and output stability by arranging a polymer electrolyte that melts at a predetermined temperature or above inside a center pin having multiple pores.

[0008] To solve the above-mentioned problems, the second technical problem that the present invention aims to solve is to provide a method for manufacturing a secondary battery in which electrolyte impregnation and output stability are improved by arranging a polymer electrolyte that melts at a predetermined temperature or above inside a center pin having a plurality of pores. [Means for solving the problem]

[0009] [1] The present invention provides a secondary battery comprising: an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separation membrane interposed between the positive electrode plate and the negative electrode plate are wound in one direction and impregnated with an electrolyte; a hollow center pin located on the winding shaft of the electrode assembly and having a plurality of holes formed on its outer peripheral surface; an electrolyte solid disposed inside the hollow of the center pin and containing a first polymer electrolyte having a melting point of 60°C to 73°C; a battery case in which the electrode assembly and the center pin are housed; and a seal that seals the open end of the battery case.

[0010] [2] The present invention provides a secondary battery in which the first polymer electrolyte comprises a main component comprising polyethylene oxide (PEO) and a secondary component comprising one or more selected from the group consisting of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and aluminum oxide (Al2O3).

[0011] [3] In the present invention, in the above [1] or [2], the diameter of the center pin (D c ) and the diameter of each of the plurality of holes (D h The present invention provides a secondary battery such that ) satisfies the following equation 1.

[0012] [Formula 1] D c / 10≦D h ≤D c / 3

[0013] [4] The present invention provides a secondary battery in which, in at least one of the above [1] to [3], the plurality of holes are arranged at predetermined intervals in the circumferential direction.

[0014] [5] The present invention provides a secondary battery in which, in at least one of the above [1] to [4], the plurality of holes are arranged at predetermined intervals in a direction perpendicular to the circumferential direction.

[0015] [6] The present invention provides a secondary battery in which, in at least one of the above [1] to [5], the electrolyte solid further comprises a second polymer electrolyte, the melting point of the second polymer electrolyte is even lower than the melting point of the first polymer electrolyte.

[0016] [7] The present invention provides a secondary battery in which the melting point of the second polymer electrolyte is 35°C to 55°C, as described in [6] above.

[0017] [8] The present invention provides a secondary battery in which the second polymer electrolyte, as described in [6] above, comprises a main component comprising succinonitrile (SN) and a secondary component comprising one or more selected from the group consisting of polycarboxylate ether (PCE), polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), polyethylene carbonate (PEC), and polyacrylonitrile (PAN).

[0018] [9] The present invention provides the secondary battery according to at least one of [1] to [8], further comprising a first electrolyte sheet including a first polymer electrolyte, wherein the first electrolyte sheet is disposed on at least one surface selected from the surface of the separator and the outermost surface of the electrode assembly.

[0019]

[10] The present invention provides the secondary battery according to [9], further comprising a second electrolyte sheet including a second polymer electrolyte, wherein the second electrolyte sheet is disposed on at least one surface selected from the surface of the separator and the outermost surface of the electrode assembly, and the melting point of the second polymer electrolyte is lower than the melting point of the first polymer electrolyte.

[0020]

[11] The present invention provides the secondary battery according to at least one of [1] to

[10] , wherein the secondary battery is a cylindrical secondary battery.

[0021]

[12] The present invention provides a method for manufacturing a secondary battery, comprising: winding a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate in one direction to manufacture an electrode assembly; accommodating the electrode assembly in a battery case; injecting a solid electrolyte body including a first polymer electrolyte into a hollow center pin positioned on a winding axis of the electrode assembly; injecting an electrolyte into the battery case and sealing the battery case with a sealing member to prepare an inactive secondary battery, wherein the melting point of the first polymer electrolyte is 60°C to 73°C.

[0022]

[13] The present invention provides the method for manufacturing a secondary battery according to

[12] , wherein the solid electrolyte body further includes a second polymer electrolyte, and the melting point of the second polymer electrolyte is 35°C to 55°C.

[0023]

[14] The present invention provides the method for manufacturing a secondary battery according to

[13] , further comprising activating the inactive secondary battery, wherein the center pin includes a plurality of holes, and during the step of activating the inactive secondary battery, the second polymer electrolyte melts and moves from the plurality of holes to a gap of the electrode assembly.

[0024]

[15] The present invention provides a method for manufacturing a secondary battery, wherein the step of manufacturing the electrode assembly in

[13] above includes one or more steps selected from: manufacturing a first electrolyte sheet containing a first polymer electrolyte and arranging the first electrolyte sheet on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly; and manufacturing a second electrolyte sheet containing a second polymer electrolyte and arranging the second electrolyte sheet on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly. [Effects of the Invention]

[0025] The secondary battery according to the present invention provides a secondary battery with improved electrolyte impregnation by replenishing the electrolyte that decreases during the charging and discharging process by placing a polymer electrolyte that melts at a predetermined temperature or above inside the center pin. Furthermore, by placing a first electrolyte sheet and a second electrolyte sheet with different melting points in the electrode assembly, a secondary battery is provided that is large in size but has excellent electrolyte impregnation and output stability.

[0026] The effects obtained by exemplary embodiments of the present invention are not limited to those mentioned above, and other effects not mentioned can be clearly derived and understood from the following description by a person with ordinary skill in the art to which the exemplary embodiments of this disclosure belong. That is, unintended effects of carrying out exemplary embodiments of this disclosure can also be derived from exemplary embodiments of this disclosure by a person with ordinary skill in the art. [Brief explanation of the drawing]

[0027] [Figure 1] This is a perspective view showing a secondary battery according to one embodiment. [Figure 2] This is a diagram illustrating a secondary battery according to one embodiment. [Figure 3a] This is a projection view showing a center pin according to one embodiment. [Figure 3b]This is a projection view showing a center pin according to one embodiment. [Figure 3c] This is a projection view showing a center pin according to one embodiment. [Figure 4] This figure shows a first electrolyte sheet placed on the surface of a separation membrane according to one embodiment. [Figure 5] This figure shows a first electrolyte sheet and a second electrolyte sheet arranged on an electrode assembly according to one embodiment. [Modes for carrying out the invention]

[0028] The terms and words used in this specification and in the claims should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather should be interpreted in a manner consistent with the technical concept of the present invention, in accordance with the principle that inventors can appropriately define the concepts of terms in order to best describe their invention.

[0029] In this specification, "electrolyte solid" and "electrolyte sheet" refer to a substance that functions as an electrolyte for a secondary battery, for example, a polymer electrolyte, which has a sheet-like shape due to maintaining a solid state at room temperature.

[0030] In this specification, "polymer electrolyte" means a substance that maintains a solid state at room temperature and can be molded into shapes such as sheets or bands, and that undergoes a phase transition to a liquid or gel above its melting temperature (Tm) to change into an amorphous state. The polymer electrolyte may also be called a solid polymer electrolyte (SPE) or a solid electrolyte.

[0031] In this specification, terms such as “includes,” “equip,” and “have” specify the presence of implemented features, figures, steps, components, or combinations thereof, and should be understood not to preemptively exclude the existence or possibility of adding one or more other features, figures, steps, components, or combinations thereof.

[0032] Each of the phrases such as "A or B," "A and at least one of B," "A or at least one of B," "A, B or C," "A, B and at least one of C," and "A, B or at least one of C" may include any one of the items listed together in the phrase, or any possible combination thereof.

[0033] Terms such as "first," "second," etc., may be used simply to distinguish the relevant component from other relevant components and do not limit the relevant component in any other way (e.g., importance or order).

[0034] The present invention will be described in detail below.

[0035] The secondary battery according to the present invention includes at least one of the configurations disclosed below, and may include any combination of technically feasible configurations from the following.

[0036] The secondary battery according to the present invention includes an electrode assembly in which a positive electrode plate, a negative electrode plate, and a separation membrane interposed between the positive electrode plate and the negative electrode plate are wound in one direction and impregnated with an electrolyte; a hollow center pin located on the winding shaft of the electrode assembly and having a plurality of holes formed on its outer circumferential surface; an electrolyte solid disposed inside the hollow of the center pin and containing a first polymer electrolyte having a melting point of 60°C to 73°C; a battery case housing the electrode assembly and the center pin; and a seal that seals the open end of the battery case.

[0037] The secondary battery according to the present invention can replenish the amount of electrolyte in the secondary battery by applying an electrolyte solid containing a first polymer electrolyte that melts within the normal operating temperature range of the secondary battery to the inside of a hollow center pin, thereby improving output stability.

[0038] Furthermore, the electrolyte solid may further contain a second polymer electrolyte, and the melting point of the second polymer electrolyte may be lower than the melting point of the first polymer electrolyte, ranging from 35°C to 55°C. By applying a second polymer electrolyte that can dissolve during the activation process to the electrolyte solid, a secondary battery with excellent electrolyte impregnation properties can be realized.

[0039] In other words, the electrolyte solid located inside the center pin improves the impregnation of the central part of the electrode assembly, thereby enabling the realization of a secondary battery that is both high-capacity and has excellent electrolyte impregnation properties.

[0040] On the other hand, each of the first electrolyte sheet containing the first polymer electrolyte and the second electrolyte sheet containing the second polymer electrolyte may be placed on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly. For example, the first electrolyte sheet may be placed on the surface of the separation membrane, and the second electrolyte sheet may be placed on the outermost surface of the electrode assembly. This allows the first electrolyte sheet located on the separation membrane of the electrode assembly to improve the electrolyte impregnation of the electrode assembly, replenish the amount of electrolyte and improve output stability. In addition, the second electrolyte sheet located on the outer surface of the electrode assembly can improve the electrolyte impregnation of the electrode assembly.

[0041] Thus, when the electrolyte solid and electrolyte sheet are used as means for replenishing or impregnating the electrolyte during the activation process or between charge and discharge of a secondary battery, the means for replenishing or impregnating the electrolyte are present both inside and outside the electrode assembly. This allows for uniform impregnation and supply of the electrolyte throughout, and stable performance can be expected.

[0042] <Secondary battery> Figure 1 is a perspective view showing a secondary battery 100 according to one embodiment.

[0043] Referring to Figure 1, the secondary battery 100 includes an electrode assembly 200, a battery case 400, and a sealing body 410. The external shape of the secondary battery 100 is not particularly limited and may be cylindrical, rectangular, or the like using a can. For example, the secondary battery 100 may be a cylindrical secondary battery, and the battery case 400 may be a cylindrical can. In that case, the electrode assembly 200 may be a winding type, or a jelly roll type electrode assembly.

[0044] The battery case 400 may be a metal container, for example, containing aluminum or an aluminum alloy. The open top of the battery case 400 may be covered by a seal 410. The seal 410 is for sealing the open end of the battery case 400 and may be coupled to the open end of the battery case 400.

[0045] According to another embodiment of the present invention, a battery module including a secondary battery 100 as a unit cell and a battery pack including the same can be provided. Since the battery module and battery pack include the secondary battery having high capacity, high rate-limiting characteristics and cycle characteristics, they can be used as a power source for medium to large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles and power storage systems.

[0046] electrode assembly Figure 2 is a diagram illustrating a secondary battery 100 according to one embodiment.

[0047] Referring to Figure 2, the secondary battery 100 according to the present invention includes an electrode assembly 200 in which a positive electrode plate 210, a negative electrode plate 220, and a separation membrane 230 interposed between the positive electrode plate 210 and the negative electrode plate 220 are wound in one direction. The electrode assembly 200 may be formed in the shape of a jelly roll in which the positive electrode plate 210, the negative electrode plate 220, and the separation membrane 230 are wound. The electrode assembly 200 includes a winding shaft in its center, and the winding center is an empty space where a center pin 300 may be located. The electrode assembly 200 may also be impregnated with an electrolyte (not shown) that is poured into the battery case 400.

[0048] (1) Positive electrode plate The positive electrode plate 210 according to the present invention may include a positive electrode current collector and a positive electrode active material layer (not shown) coated on the positive electrode current collector. The positive electrode plate 210 may have a structure in which a positive electrode active material layer is formed on a positive electrode current collector. The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or those obtained by surface-treating the surface of aluminum or stainless steel with carbon, nickel, titanium, silver, etc. can be used.

[0049] The positive electrode active material layer includes a positive electrode active material, a positive electrode conductive material, and a positive electrode binder. The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; chemical formula Li 1+a1 Mn 2-a1 Lithium manganese oxides such as O4 (0≦a1≦0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, and Cu2V2O7; chemical formula LiNi 1-a2 M c2 Ni-site type lithium nickel oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≦a2≦0.3); chemical formula LiMn 2-a3 M c3Lithium manganese composite oxides represented by O2 (where M is selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01 ≤ a3 ≤ 0.1) or Li2Mn3MO8 (where M is selected from the group consisting of Fe, Co, Ni, Cu, and Zn); LiMn2O4 in which part of the Li in the chemical formula is substituted with alkaline earth metal ions, etc., are examples, but are not limited to these. The positive electrode may also be Li-metal.

[0050] The positive electrode conductive material is used to impart conductivity to the electrode and can be used without particular limitations as long as it does not cause chemical changes in the battery it is constructed from and possesses electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives. One of these can be used alone or in mixtures of two or more.

[0051] Next, the positive electrode binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one or more of these can be used individually or in mixtures of two or more.

[0052] The positive electrode plate 210 can be manufactured by a conventional electrode manufacturing method. For example, a positive electrode slurry can be produced by mixing a positive electrode active material, a positive electrode binder, and / or a positive electrode conductive material in a positive electrode slurry solvent, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling it to produce a positive electrode current collector with a positive electrode active material layer 222 formed thereon.

[0053] On the other hand, as the solvent for the positive electrode slurry, solvents commonly used in the art can be used. For example, dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., can be used individually or in combination of two or more.

[0054] (2) Negative plate The negative electrode plate 220 according to the present invention may have a structure in which a negative electrode active material layer (not shown) is formed on a negative electrode current collector (not shown). The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. Examples thereof include copper, stainless steel, aluminum, nickel, titanium, calcined carbon, those obtained by surface-treating the surface of copper or stainless steel with carbon, nickel, titanium, silver or the like, and aluminum-cadmium alloys.

[0055] As the negative electrode active material, a compound generally used in the art that enables reversible intercalation and deintercalation of lithium can be used, and the type thereof is not particularly limited. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fibers, and amorphous carbon; Si, Si-Me alloy (wherein Me is at least one selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti and Ni), SiO y (wherein 0<y<2), silicon-based materials such as Si-C composites; lithium metal thin films; metal materials capable of being alloyed with lithium such as Sn and Al, and the like, and any one or a mixture of two or more thereof can be used.

[0056] The negative electrode conductive material is used to impart conductivity to the negative electrode, and can be used without particular limitation as long as it does not cause chemical changes in the configured battery and has electron conductivity. The negative electrode conductive material may be the same as the positive electrode conductive material.

[0057] The negative electrode binder plays a role in improving adhesion between negative electrode active material particles and adhesion between the negative electrode active material and the negative electrode current collector. The negative electrode binder may be the same as the positive electrode binder.

[0058] On the other hand, the negative electrode plate 220 can be manufactured by a conventional electrode manufacturing method. For example, a negative electrode slurry can be produced by mixing a negative electrode active material, a negative electrode binder, and / or a negative electrode conductive material in a negative electrode slurry solvent, applying the negative electrode slurry onto a negative electrode current collector, and then drying and rolling it to produce a negative electrode current collector on which a negative electrode active material layer 212 is formed.

[0059] As the solvent for the negative electrode slurry, solvents commonly used in the art can be used, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, and water, either individually or in combination of two or more.

[0060] (3) Separation membrane The separation membrane 230 according to the present invention is located between electrodes and can provide a passage for lithium ions to move. It can be used without particular limitations as long as it is a separation membrane that is normally used in secondary batteries. Specifically, the separation membrane can be a porous polymer film, for example, a porous polymer film made from polyolefin polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, or ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof. Alternatively, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, can also be used. Furthermore, a coated separation membrane containing ceramic components or polymeric substances can be used to ensure heat resistance or mechanical strength.

[0061] Center pin Figures 3a to 3c show a center pin according to one embodiment.

[0062] Referring to Figures 2 and 3a to 3c, the hollow center pin 300 is located on the winding shaft of the electrode assembly 200. The center pin 300 is located in the center of the electrode assembly 200 and may be formed in a hollow cylindrical shape. The center pin 300 can be inserted into the winding shaft of the electrode assembly 200 to prevent deformation of the electrode assembly 200.

[0063] Furthermore, multiple holes 320 may be arranged on the outer surface of the center pin 300, and an electrolyte solid 310 may be placed inside the hollow space. When the electrolyte solid 310 melts at a predetermined temperature or higher and undergoes a phase transition to an amorphous state such as a liquid or gel, the multiple holes 320 can serve as passages for the electrolyte solid 310 to move from the inside of the center pin 300 towards the electrode assembly 200.

[0064] Specifically, referring to Figure 3b, the multiple holes 320 may be arranged at predetermined intervals in the circumferential direction, and referring to Figure 3a, the multiple holes 320 may be arranged at predetermined intervals in a direction perpendicular to the circumferential direction. Referring to Figure 3c, the multiple holes 320 may be arranged on the outer surface of the center pin 300 in both the circumferential and perpendicular directions. The multiple holes 320 can be arranged on the center pin 300 in an appropriate number as needed, and the direction and speed of electrolyte movement can be adjusted by the arrangement position and number of the multiple holes 320, so the arrangement position and number of the multiple holes 320 can be adjusted depending on the type of electrolyte solid 310.

[0065] Also, the diameter of the center pin (D c ) and the diameter of each of the multiple holes 320 (D h ) may also satisfy the following formula 1.

[0066] [Formula 1] D c / 10≦D h ≤D c / 3

[0067] The diameter of each of the multiple holes 320 (D h ) is the diameter of the center pin (D cIf the diameter of each of the multiple holes 320 is 1 / 10 or more, the electrolyte solid 310 located inside the center pin 300 can easily move to the electrode assembly 200. h ) is the diameter of the center pin (D c If the diameter of each of the multiple holes 320 is 1 / 3 or less, the center pin 300 can be designed to have excellent durability and to prevent the movement speed of the electrolyte solid 310 from being too fast. By applying a center pin 300 with multiple holes 320 that satisfy the above range, a secondary battery that can maintain electrolyte impregnation and output stability can be realized. Therefore, preferably, the diameter of each of the multiple holes 320 (D h ) is the diameter of the center pin (D c ) may be 1 / 10 or more, 1 / 9 or more, 1 / 8 or more, or 1 / 7 or more, preferably the diameter of each of the multiple holes 320 (D h ) is the diameter of the center pin (D c It may be 1 / 3 or less, 1 / 4 or less, 1 / 5 or less, or 1 / 6 or less of )

[0068] electrolyte solid body The electrolyte solid 310 according to the present invention is placed inside the hollow of the center pin 300. The form of the electrolyte solid 310 is not particularly limited as long as it can be placed inside the center pin 300. For example, the form of the electrolyte solid 310 may be cylindrical, prismatic, or irregular. Furthermore, the electrolyte solid 310 may contain one or more solids, for example, two solids with different compositions.

[0069] Furthermore, the electrolyte solid 310 contains a first polymer electrolyte having a melting point of 60°C to 73°C. The first polymer electrolyte may contain polyethylene oxide (PEO), and preferably contains a main component containing polyethylene oxide (PEO) and a secondary component containing one or more selected from the group consisting of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and aluminum oxide (Al2O3). If polyethylene oxide (PEO), which has a melting point of about 75°C, is used alone as the first polymer electrolyte, it will not melt at the normal operating temperature of the secondary battery. Therefore, by mixing polyethylene oxide (PEO) with lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or aluminum oxide (Al2O3), the electrolyte solid 310 containing the first polymer electrolyte can be made to melt during operation of the secondary battery. This allows the electrolyte to be replenished in the electrode assembly 200, improves electrolyte impregnation, and enables the realization of a secondary battery 100 with excellent performance.

[0070] Specifically, the first polymer electrolyte may contain polyethylene oxide (PEO) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) in a weight ratio of 40:1 to 80:1, preferably 40:1 to 60:1. Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) can change the structure of polyethylene oxide (PEO) from crystalline to amorphous, thereby lowering the melting point of the first polymer electrolyte. When the weight ratio of polyethylene oxide (PEO) and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) satisfies the above range, the first electrolyte sheet does not melt during the manufacturing process of the secondary battery 100, but can melt during the operation of the secondary battery 100.

[0071] Furthermore, the melting point of the first polymer electrolyte may be 60°C to 73°C, preferably 60°C to 70°C, and more preferably 60°C to 66°C. If the melting point of the first polymer electrolyte is lower than 60°C, it will all melt during the manufacturing process of the secondary battery 100, and will not be present inside the center pin 300 after the secondary battery 100 is completed, making it impossible to replenish the electrolyte after the manufacturing of the secondary battery 100 is complete. On the other hand, if the melting point of the first polymer electrolyte is higher than 73°C, the first electrolyte sheet 230_1 will not melt within the normal operating temperature range of the secondary battery 100, and will not be able to perform its role of replenishing the electrolyte. Therefore, preferably, the melting point of the first polymer electrolyte may be 60°C or higher, 61°C or higher, or 62°C or higher, and the melting point of the first polymer electrolyte may be 73°C or lower, 71°C or lower, 70°C or lower, 68°C or lower, or 66°C or lower.

[0072] The first polymer electrolyte can partially dissolve during the activation process of the secondary battery, and the remainder can dissolve during the operation of the secondary battery. That is, the first polymer electrolyte contained in the electrolyte solid can be located within the hollow of the center pin 300 once the manufacturing of the secondary battery is complete.

[0073] Furthermore, the electrolyte solid 310 may further contain a second polymer electrolyte. The second polymer electrolyte may contain a main component containing succinonitrile (SN) and a secondary component containing one or more selected from the group consisting of polycarboxylate ether (PCE), polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), polyethylene carbonate (PEC), and polyacrylonitrile (PAN). In exemplary embodiments, the second polymer electrolyte may include, as the secondary component, a combination of polycarboxylate (PCE) and polyethylene oxide (PEO), a combination of polycarboxylate (PCE) and polyvinylpyrrolidone (PVP), a combination of polycarboxylate (PCE) and polyethylene carbonate (PEC), or a combination of polycarboxylate (PCE) and polyacrylonitrile (PAN).

[0074] In exemplary embodiments, the molecular weight of the polycarboxylate (PCE) may be approximately 165 g / mol, the molecular weight of the polyethylene oxide (PEO) may be approximately 100 g / mol, and the molecular weight of the polyvinylpyrrolidine (PVP) may be approximately 25 g / mol.

[0075] The melting point of the second polymer electrolyte may be even lower than the melting point of the first polymer electrolyte. Specifically, the melting point of the second polymer electrolyte may be about 35°C to 55°C, preferably about 35°C to 53°C, and more preferably about 40°C to 50°C. The second polymer electrolyte can melt during the manufacturing process of the secondary battery 100, and after the second polymer electrolyte melts during the process, it is impregnated into the positive electrode plate 210, negative electrode plate 220, separation membrane 230, etc., within the electrode assembly 200, and does not return to its original state even if the temperature drops again, thereby improving the electrolyte impregnation of the secondary battery 100 during the manufacturing process. Therefore, preferably, the melting point of the second polymer electrolyte may be 35°C or higher, 37°C or higher, 40°C or higher, or 42°C or higher, and the melting point of the second polymer electrolyte may be 55°C or lower, 53°C or lower, 52°C or lower, 50°C or lower, or 48°C or lower.

[0076] In other words, the second polymer electrolyte contained in the electrolyte solid can dissolve during the activation process of the secondary battery 100, thereby realizing a secondary battery 100 with improved electrolyte impregnation.

[0077] In conclusion, the electrolyte solid 310 may include one or more selected from the group consisting of a first polymer electrolyte and a second polymer electrolyte. By applying the first and second polymer electrolytes, which have different melting points, to the electrolyte solid 310, the electrolyte impregnation of the secondary battery 100 can be improved during the manufacturing process of the secondary battery and during the operation of the manufactured secondary battery. In particular, the electrolyte solid located inside the center pin 300 melts and moves to the center of the electrode assembly 200, thereby impregnating the electrode assembly 200 up to the center of the enlarged electrode assembly 200. Therefore, the electrolyte impregnation of the enlarged secondary battery can be improved without performing any additional steps.

[0078] Furthermore, the electrolyte solid 310 to which the first polymer electrolyte is applied can replenish the electrolyte that has decreased during the operation of the manufactured secondary battery, thereby improving output stability.

[0079] Electrolyte sheet Figure 4 shows a first electrolyte sheet placed on a separation membrane according to one embodiment.

[0080] Figure 5 shows a first electrolyte sheet and a second electrolyte sheet arranged on an electrode assembly according to one embodiment.

[0081] The first electrolyte sheet 240_1 contains a first polymer electrolyte, and since the first polymer electrolyte is as described above, a detailed explanation is omitted. The second electrolyte sheet 240_2 contains a second polymer electrolyte, and since the second polymer electrolyte is as described above, a detailed explanation is omitted.

[0082] Referring to Figures 4 and 5, each of the first electrolyte sheet 240_1 and the second electrolyte sheet 240_2 may be placed on one or more surfaces selected from the surface of the separation membrane 230 and the outermost surface of the electrode assembly 200. Specifically, the first electrolyte sheet 240_1 and the second electrolyte sheet 240_2 may be alternately positioned on the surface of the separation membrane 230.

[0083] Furthermore, the first electrolyte sheet 240_1 may be located on the upper part of the outermost surface of the electrode assembly 200, and the second electrolyte sheet 240_2 may be located on the lower part of the outermost surface of the electrode assembly 200. Here, the first electrolyte sheet 240_1 and the second electrolyte sheet 240_2 can maintain the shape of the electrode assembly 200 before it is placed in the battery case 400. The first electrolyte sheet 240_1 can dissolve during the operation of the secondary battery 100, so that it does not compress the electrode assembly 200 when a swelling phenomenon occurs in which the electrode assembly 200 expands. The second electrolyte sheet 240_2 can dissolve during the activation process of the secondary battery 100 after the electrode assembly 200 has been placed in the battery case 400.

[0084] On the other hand, the first electrolyte sheet 240_1 and the second electrolyte sheet 240_2 according to the present invention may be arranged in different positions within the secondary battery 100. Specifically, the first electrolyte sheet 240_1 may be arranged on the surface of the separation membrane 230, and the second electrolyte sheet 240_2 may be arranged on the outermost surface of the electrode assembly 200.

[0085] Here, there may be two or more first electrolyte sheets 240_1, and multiple first electrolyte sheets 240_1 may be arranged on the surface of the separation membrane at predetermined intervals. Furthermore, multiple first electrolyte sheets 240_1 may be arranged on both sides of the separation membrane. That is, by positioning the first electrolyte sheets 240_1 on the surface of the separation membrane 230, the first electrolyte sheets 240_1 can provide electrolyte to the positive electrode plate 210 and the negative electrode plate 220 inside the electrode assembly 200 during operation of the secondary battery 100. This makes it possible to realize a secondary battery 100 with improved lifespan for the positive electrode plate 210 and the negative electrode plate 220.

[0086] Furthermore, the second electrolyte sheet 240_2 may be positioned in the middle with respect to the height of the electrode assembly 200. In addition, there may be multiple second electrolyte sheets 240_2. For example, each of the multiple second electrolyte sheets 240_2 may be positioned near each of the ends of the electrode assembly 200.

[0087] In other words, the first electrolyte sheet 240_1 and the second electrolyte sheet 240_2 are means for replenishing or impregnating the electrolyte during the activation process of the secondary battery or between charge and discharge, and can stably maintain the output performance of the secondary battery.

[0088] electrolyte The secondary battery 100 according to the present invention further includes an electrolyte (not shown) that is injected into the inside of the battery case 400. The electrolyte is for moving lithium ions generated by the electrochemical reaction of electrodes during charging / discharging of the secondary battery, and may include a non-aqueous organic electrolyte which is a mixture of a lithium salt and organic solvents.

[0089] The organic solvent can be any solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move, without any particular limitations. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; a carbonate solvent such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethylmethyl carbonate (EMC), ethylene carbonate (EC), or propylene carbonate (PC); or an alcohol solvent such as ethyl alcohol or isopropyl alcohol. Among these, carbonate-based solvents are preferred, and more preferably are mixtures of cyclic carbonates (e.g., ethylene carbonate, propylene carbonate, etc.) having high ionic conductivity and high dielectric constant to enhance the charge and discharge performance of the battery, and low-viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.).

[0090] The lithium salt can be used without particular limitations, as long as it is a compound that can provide lithium ions for use in lithium secondary batteries. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The concentration of the lithium salt is preferably within the range of 0.1M to 2.0M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, exhibiting excellent electrolyte performance and allowing lithium ions to move effectively.

[0091] <Manufacturing method for secondary batteries> The method for manufacturing a secondary battery 100 according to the present invention includes the steps of: manufacturing an electrode assembly 200 by winding a positive electrode plate 210, a negative electrode plate 220, and a separation membrane 230 interposed between the positive electrode plate 210 and the negative electrode plate 220 in one direction; housing the electrode assembly 200 in a battery case 400; introducing an electrolyte solid 310 containing a first polymer electrolyte into a hollow center pin 300 located on the winding shaft of the electrode assembly 200; and preparing an inert secondary battery by introducing the electrolyte into the battery case 400 and sealing the battery case 400 with a sealant 410. Here, the melting point of the first polymer electrolyte is 60°C to 73°C.

[0092] On the other hand, the electrolyte solid 310 may further contain a second polymer electrolyte, and the melting point of the second polymer electrolyte may be 35°C to 55°C.

[0093] Steps for manufacturing an electrode assembly The steps for manufacturing the electrode assembly 200 may include one or more selected steps from the following: manufacturing a first electrolyte sheet 240_1 containing a first polymer electrolyte and placing the first electrolyte sheet 240_1 on one or more surfaces selected from the surface of the separation membrane 230 and the outermost surface of the electrode assembly 200; and manufacturing a second electrolyte sheet 240_2 containing a second polymer electrolyte and placing the second electrolyte sheet 240_2 on one or more surfaces selected from the surface of the separation membrane 230 and the outermost surface of the electrode assembly 200. When the first electrolyte sheet 240_1 and the second electrolyte sheet each contain a first polymer electrolyte and a second polymer electrolyte, the first electrolyte sheet 240_1 or the second electrolyte sheet 240_2 can be manufactured by applying a conventional molding method.

[0094] Step of storing the electrode assembly in the battery case. The step of housing the electrode assembly 200 in the battery case 400 may also involve inserting the electrode assembly 200 from the open end of the battery case 400. The electrode assembly 200 can enter and exit from the open end of the battery case 400.

[0095] Step 1: Place an electrolyte solid containing a first polymer electrolyte inside a hollow center pin.

[0096] The step of introducing an electrolyte solid containing a first polymer electrolyte into the hollow center pin may include a step of manufacturing an electrolyte solid 310, and if the electrolyte solid 310 contains a first polymer electrolyte as a component, a conventional method can be applied as the molding method to manufacture the electrolyte solid 310.

[0097] Furthermore, the electrolyte solid may further contain a second polymer electrolyte, the characteristics of which are the same as those of the second polymer electrolyte described above. Therefore, the step of adding the electrolyte solid may include the step of producing an electrolyte solid containing the second polymer electrolyte.

[0098] Steps to prepare an inert secondary battery The step of preparing the inert secondary battery may involve filling the battery case 400 with an electrolyte and sealing the battery case 400 with a sealant 410. The sealant 410 may be bonded to the battery case 400. Sealing the battery case 400 with the sealant 410 prevents the electrode assembly 200 from being deformed or damaged by the external environment.

[0099] Steps to activate an inactive secondary battery On the other hand, the method for manufacturing the secondary battery 100 may further include a step of activating the inactive secondary battery. The activation step may involve charging and discharging the secondary battery 100 at 45°C to 59°C. In an exemplary embodiment, the temperature of the activation step may be 50°C to 59°C.

[0100] Furthermore, the activation step may include a step in which the electrolyte solid 310 containing the second polymer electrolyte dissolves within the battery case 400. Specifically, during the activation step, the second polymer electrolyte can dissolve and move through the multiple holes 320 of the center pin 300 into the voids of the electrode assembly. The voids of the electrode assembly 200 may include the voids of the positive electrode plate 210, the negative electrode plate 220, and the separation membrane 230. This improves the electrolyte impregnation of the central part of the electrode assembly 200, even though the electrode assembly 200 is larger.

[0101] The following describes in detail embodiments of the present invention so that those with ordinary skill in the art to which the present invention pertains can easily implement it. However, the present invention can be realized in a variety of different forms and is not limited to the embodiments described below.

[0102] Example 1 (1) Production of electrolyte solids containing the first polymer electrolyte Lithium bis(trifluoromethanesulfonyl)imide (LiTFSI with a purity of 99.9%) was prepared by storing it in a dry room at 110°C for more than 24 hours, and polyethylene oxide (PEO) was prepared by storing it at 45°C for 48 hours. Then, the polyethylene oxide and LiTFSI were mixed in a weight ratio of 50:1 and stirred for 12 hours to produce a first polymer electrolyte. Using this first polymer electrolyte, a cylindrical electrolyte solid with a melting point of approximately 60°C that could be placed inside a center pin was produced.

[0103] (2) Manufacturing of secondary batteries A jelly roll type electrode assembly was manufactured by winding a material with a separation membrane interposed between the positive electrode plate and the negative electrode plate. The electrode assembly was then placed in a battery case, and a hollow center pin was positioned on the winding shaft of the electrode assembly. An electrolyte solid containing the first polymer electrolyte was placed inside the hollow center pin, and ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 30:70. Subsequently, the electrolyte, dissolved to a concentration of 1.0 M of LiPF6, was injected into the battery case. After that, the open end of the battery case was sealed with a sealant to prepare an inactivated secondary battery.

[0104] Subsequently, the deactivated secondary battery was subjected to an activation process at 45°C to 59°C, followed by an additional 3-day aging process to manufacture the secondary battery.

[0105] Example 2 A secondary battery was manufactured in the same manner as in Example 1, except that the first polymer electrolyte was manufactured as described below.

[0106] A first polymer electrolyte with a melting point of approximately 73°C was produced by mixing lithium salt (LiTFSI) with polyethylene oxide (PEO) and aluminum oxide (Al2O3) in a mass ratio of 9:1 and stirring for 12 hours.

[0107] Example 3 A secondary battery was manufactured in the same manner as in Example 1, except that an electrolyte solid containing a second polymer electrolyte was manufactured as described below and additionally inserted into the center pin.

[0108] (1) Production of electrolyte solids containing the second polyelectrolyte Polycarboxylate (PCE) and polyethylene oxide (PEO) were prepared by drying them in a dry room for 24 hours. Then, a mixture of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI with a purity of 99.9%) and succinonitrile (SN) was added to a mixture of polycarboxylate (PCE) and polyethylene oxide (PEO) in a mass ratio of 9:1 to a total of 10 wt%, and the mixture was then stirred at 70°C to produce a second polymer electrolyte. Using this second polymer electrolyte, a cylindrical electrolyte solid with a melting point of 42°C that could be placed inside a center pin was produced.

[0109] Example 4 A secondary battery was manufactured in the same manner as in Example 3, except that the second polymer electrolyte was manufactured as described below.

[0110] Polycarboxylate (PCE) and polyvinylpyrrolidine (PVP) were prepared by drying them in a dry room for 24 hours. Then, a mixture of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) with a purity of 99.9% and succinonitrile (SN) was added to a mixture of polycarboxylate (PCE) and polyvinylpyrrolidine (PVP) in a mass ratio of 9:1 to a total of 10 wt%, and the mixture was then stirred at 70°C to produce a second polymer electrolyte with a melting point of approximately 52°C.

[0111] Example 5 A secondary battery was manufactured in the same manner as in Example 3, except that a first electrolyte sheet was manufactured and placed on the outermost surface of the electrode assembly, and a second electrolyte sheet was manufactured and placed on the surface of the separation membrane.

[0112] The first electrolyte sheet was manufactured by casting an electrolyte solid containing the first polymer electrolyte into a glass container to form a film, and then drying it in a vacuum oven at 50°C for 24 hours.

[0113] The second electrolyte sheet was manufactured by casting an electrolyte solid containing the second polymer electrolyte into a glass container to form a film, and then drying it in a vacuum oven at 35°C for 24 hours.

[0114] Comparative Example 1 A secondary battery was manufactured in the same manner as in Example 1, except that an electrolyte solid was not applied.

[0115] Experimental Example 1: Impregnation Evaluation For each of the secondary batteries produced in Examples 1-5 and Comparative Example 1, one cycle was defined as charging and discharging at 1 C-rate. After 100 cycles, the batteries were disassembled, and the electrolyte impregnation properties were relatively evaluated, as shown in Table 1 below.

[0116] In Table 1 below, "○" indicates good condition, meaning that the electrolyte impregnation area covers 80% or more of the entire surface of the electrode and separation membrane. "△" indicates average condition, meaning that the electrolyte impregnation area covers 50% to 80% of the entire surface of the electrode and separation membrane.

[0117] Experimental Example 2: Evaluation of Electrolyte Depletion During Secondary Battery Use For each of the secondary batteries manufactured in Examples 1-5 and Comparative Example 1, one cycle was defined as charging and discharging at 1C-rate, and after 100 cycles, the batteries were disassembled and the battery cases were opened. The weight of the secondary batteries before and after 100 cycles was then compared to confirm the amount of residual electrolyte. The amount of residual electrolyte was evaluated to assess the performance in terms of electrolyte reduction, and the results are shown in Table 1 below.

[0118] In Table 1 below, a "○" indicates that the residual electrolyte level is 90% or higher, based on the results of the pouch-type secondary battery manufactured in Example 1, while a "×" indicates that the level is less than 80%, based on the results of Example 1.

[0119] [Table 1]

[0120] Referring to Table 1 above, it can be confirmed that the secondary batteries of Examples 1 to 5 have superior electrolyte impregnation properties and a larger amount of residual electrolyte compared to the secondary battery of Comparative Example 1. This is judged to be because an electrolyte solid that can replenish the electrolyte or impregnate the electrode assembly during the activation process of the secondary battery or between charge and discharge was applied. [Explanation of Symbols]

[0121] 100 Secondary battery 200 electrode assembly 210 Positive plate 220 Negative electrode plate 230 Separation membrane 240_1 Electrolyte Sheet 1 240_2 Second Electrolyte Sheet 300 Center Pin 310 Solid electrolyte 320 Multiple holes 400 Battery Case 410 Sealed body

Claims

1. An electrode assembly comprising a positive electrode plate, a negative electrode plate, and a separation membrane interposed between the positive and negative electrode plates, which are wound in one direction and impregnated with an electrolyte, A hollow center pin located on the winding shaft of the electrode assembly, with multiple holes formed on its outer surface, An electrolyte solid containing a first polymer electrolyte having a melting point of 60°C to 73°C is disposed inside the hollow of the center pin, A battery case in which the electrode assembly and the center pin are housed, A secondary battery comprising a sealing body that seals the open end of the battery case.

2. The first polymer electrolyte comprises a main component containing polyethylene oxide, The secondary battery according to claim 1, comprising a minor component comprising one or more selected from the group consisting of lithium bis(trifluoromethanesulfonyl)imide and aluminum oxide.

3. The diameter of the aforementioned center pin (D c ) and the diameter of each of the plurality of holes (D h The secondary battery according to claim 1, wherein ) satisfies the following formula 1. [Formula 1] D c / 10≦D h ≦D c / 3

4. The secondary battery according to claim 1, wherein the plurality of holes are arranged at predetermined intervals in the circumferential direction.

5. The secondary battery according to claim 1, wherein the plurality of holes are arranged at predetermined intervals in a direction perpendicular to the circumferential direction.

6. The electrolyte solid further comprises a second polymer electrolyte, The secondary battery according to claim 1, wherein the melting point of the second polymer electrolyte is even lower than the melting point of the first polymer electrolyte.

7. The secondary battery according to claim 6, wherein the melting point of the second polymer electrolyte is 35°C to 55°C.

8. The second polymer electrolyte comprises a main component containing succinonitrile, The secondary battery according to claim 6, comprising a secondary component comprising one or more selected from the group consisting of polycarboxylate, polyethylene oxide, polyvinylpyrrolidine, polyethylene carbonate, and polyacrylonitrile.

9. The secondary battery further comprises a first electrolyte sheet containing a first polymer electrolyte, The secondary battery according to claim 1, wherein the first electrolyte sheet is arranged on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly.

10. The secondary battery further comprises a second electrolyte sheet containing a second polymer electrolyte, The second electrolyte sheet is placed on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly. The secondary battery according to claim 9, wherein the melting point of the second polymer electrolyte is even lower than the melting point of the first polymer electrolyte.

11. The secondary battery according to claim 1, wherein the secondary battery is a cylindrical secondary battery.

12. A step of manufacturing an electrode assembly by winding a positive electrode plate, a negative electrode plate, and a separation film interposed between the positive electrode plate and the negative electrode plate in one direction, The steps include: housing the electrode assembly in a battery case, The steps include: placing an electrolyte solid containing a first polymer electrolyte into the hollow center pin located on the winding shaft of the electrode assembly; The process includes the steps of preparing an inert secondary battery by filling the battery case with an electrolyte and sealing the battery case with a sealing body, A method for manufacturing a secondary battery, wherein the melting point of the first polymer electrolyte is 60°C to 73°C.

13. The electrolyte solid further comprises a second polymer electrolyte, The method for manufacturing a secondary battery according to claim 12, wherein the melting point of the second polymer electrolyte is 35°C to 55°C.

14. The method further includes the step of activating the inactive secondary battery, The center pin includes a plurality of holes, The method for manufacturing a secondary battery according to claim 13, wherein during the step of activating the inert secondary battery, the second polymer electrolyte dissolves and moves from the plurality of pores into the voids of the electrode assembly.

15. The step of manufacturing the electrode assembly is, The steps include: manufacturing a first electrolyte sheet containing a first polymer electrolyte, and placing the first electrolyte sheet on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly; A method for manufacturing a secondary battery according to claim 13, comprising one or more steps selected from: manufacturing a second electrolyte sheet containing a second polymer electrolyte; and arranging the second electrolyte sheet on one or more surfaces selected from the surface of the separation membrane and the outermost surface of the electrode assembly.