Polyimide film with improved dielectric breakdown properties and method for manufacturing the same
Patent Information
- Application Number
- JP2026523928
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-23
- Filing Date
- 2024-10-16
- Publication Date
- 2026-11-24
Smart Images

Figure 2026539275000001 
Figure 2026539275000002 
Figure 2026539275000003
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide film with improved dielectric breakdown characteristics and a method for manufacturing the same. More particularly, the present invention relates to a polyimide film with improved dielectric breakdown characteristics by including nanoparticles having an average particle diameter of 100 to 500 nm, and a method for manufacturing the same.
Background Art
[0002] Generally, a polyimide (PI) film is a film formed from a polyimide resin. The polyimide resin refers to a super heat-resistant resin produced by solution-polymerizing an aromatic dianhydride and an aromatic diamine or an aromatic diisocyanate to prepare a polyamic acid derivative, followed by ring closure and dehydration at a high temperature for imidization.
[0003] As an insoluble and infusible super heat-resistant resin, the polyimide resin has a high glass transition temperature and exhibits excellent heat-resistant oxidation resistance, heat resistance, radiation resistance, low-temperature properties, chemical resistance, and electrical properties, and thus is used in various forms such as films, resins, molded parts, adhesives, and insulators in the electric, electronic, automotive, and aerospace industries. In particular, the polyimide resin, which is excellent in insulation properties and thermal and chemical stability as an electronic industry material, has expanded applications to an interlayer insulating film of a semiconductor chip and the like.
[0004] Among various applications, a polyimide film used in a secondary battery is required to have a dielectric breakdown voltage (BDV) as a main physical property. In addition, dielectric breakdown resistance is proportional to the thickness of a film, and a film having a high dielectric breakdown voltage per unit thickness can satisfy the required dielectric breakdown voltage at a lower thickness, and thus can be reduced in size and weight. On the other hand, in a roll-to-roll process of a polyimide film, it is essential to secure required roughness using a filler in order to secure sample winding property.
[0005] Accordingly, there is a need to develop a polyimide film that satisfies both the required roughness and the enhanced dielectric breakdown voltage.
Summary of Invention
[0006] The present invention aims to provide a polyimide film with improved dielectric breakdown properties and a roughness that meets the required level for ensuring the windability of the sample, as well as a method for producing the same.
[0007] Furthermore, the present invention aims to provide a secondary battery containing the above-mentioned polyimide film. [Means for solving the problem]
[0008] Because the present invention can be modified in various ways and has various embodiments, specific embodiments will be illustrated and described in detail. However, this should not be understood as limiting the present invention to specific embodiments, but rather as including all modifications, equivalents, or substitutions that fall within the spirit and technical scope of the present invention.
[0009] The terms used in this application are used solely to describe specific embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise. In this application, terms such as “includes” or “having” specify the presence of features, figures, steps, actions, components, parts, or combinations thereof described in the specification, and should be understood not to preclude the presence or possibility of adding one or more different features, figures, steps, actions, components, parts, or combinations thereof.
[0010] Wherever a quantity, concentration, or other value or parameter is given in this specification by enumeration of ranges, preferred ranges, preferred upper limits, and preferred lower limits, it should be understood that this specifically discloses all ranges formed by any pair of limits or preferred values of any upper range and any limits or preferred values of any lower range, regardless of whether the ranges are disclosed separately.
[0011] Where a range of numerical values is referred to herein, unless otherwise specified, that range is intended not to be limited to the specific values referred to when defining the range, including its endpoints and the models within that range.
[0012] In this specification, “dianhydride” is intended to include its precursors or derivatives, but it may also be referred to as “dianhydric acid,” “dianhydride,” or “acidic dianhydride.” These may not be technically dianhydrides, but nevertheless react with diamines to form polyamic acids, which can also be converted to polyimides.
[0013] In this specification, “diamine” is intended to include its precursors or derivatives, which may not be technically diamines, but nevertheless react with dianhydride acids to form polyamic acids, which can also be converted to polyimides.
[0014] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the same meaning as those generally understood by a person of ordinary skill in the art to which this invention pertains. Terms such as those defined in commonly used dictionaries should be interpreted as having the meaning consistent with their meaning in the context of the relevant art, and should not be interpreted in an ideal or overly formal sense unless explicitly defined in this application. The specific details for realizing the invention are described below.
[0015] The present invention relates to a polyimide film with improved dielectric breakdown properties and a method for producing the same.
[0016] Polyimide film
[0017] The present invention provides a polyimide film comprising a polyimide containing dianhydride monomers and diamine monomers as polymerization units, and nanoparticles having an average particle diameter of 100 to 500 nm, having a dielectric breakdown voltage (BDV) of 350 kV / mm or more, and a roughness (Ra) value of 0.01 nm or more.
[0018] The average particle diameter of the nanoparticles may be 100 to 500 nm, preferably 100 nm or more and less than 500 nm, more preferably 110 to 400 nm, 120 to 350 nm, 130 to 300 nm, 135 to 290 nm, 140 to 280 nm, 145 to 270 nm, 148 to 260 nm, and even more preferably 150 to 250 nm. If the average particle diameter of the nanoparticles is less than 100 nm, the roughness (Ra) value is low and undesirable, and if it exceeds 500 nm, a dispersion problem of nanoparticles within the film may occur and is therefore undesirable.
[0019] In one embodiment, the average particle size of the nanoparticles can be measured using a laser diffraction particle size analyzer (SHIMADZU, model SALD-2201).
[0020] The dielectric breakdown voltage (BDV) of the polyimide film may be 350kV / mm or higher. For example, the lower limit of the dielectric breakdown voltage may be 353kV / mm, 355kV / mm, 358kV / mm, or 360kV / mm or higher. The upper limit of the dielectric breakdown voltage is not particularly limited, but may be 500kV / mm or lower, 400kV / mm or lower, 350kV / mm or lower, 330kV / mm or lower, or 320kV / mm or lower.
[0021] The dielectric breakdown voltage (BDV) can be measured by methods known in the industry. For example, the dielectric breakdown voltage can be measured in accordance with the ASTM D149 standard. Specifically, the polyimide film is pre-treated in a 100°C oven to remove moisture, then fixed in a measuring device (PHENIX, TECHNOLOGIES 6CCE50-5) set to a room temperature atmosphere, and a voltage of 10 kVAc is applied to the upper electrode at the bottom, and the BDV can be measured by increasing the AC voltage from 0 at a constant rate.
[0022] The roughness (Ra) value of the polyimide film may be 0.01 nm or greater. For example, the lower limit of the roughness (Ra) value may be 0.0105 nm, 0.0108 nm, 0.0110 nm, 0.0115 nm, 0.0118 nm, or 0.012 nm or greater. The upper limit of the roughness (Ra) value is not particularly limited, but may be 0.05 nm or less, 0.04 nm or less, 0.035 nm or less, or 0.03 nm or less.
[0023] The aforementioned roughness (Ra) refers to the arithmetic mean roughness and can be measured by methods known in the industry. In one example, the roughness (Ra) can be measured using a film roughness analyzer manufactured by Kosaka Laboratory Ltd.
[0024] The aforementioned nanoparticles may contain nanosilica.
[0025] The polyimide film may contain 1,000 to 5,000 ppm of the nanoparticles, preferably 1,500 to 4,500 ppm, 1,800 to 4,200 ppm, 2,000 to 4,000 ppm, 2,300 to 3,700 ppm, 2,500 to 3,500 ppm, and more preferably 2,800 to 3,200 ppm.
[0026] When the polyimide film contains the nanoparticles in an amount of less than 1,000 ppm, the dielectric breakdown voltage value is low, which is not preferable. When the content exceeds 5,000 ppm, the improvement degree of the dielectric breakdown voltage is insignificant compared with the amount of the nanoparticles used, which is inefficient and thus not preferable.
[0027] The aforementioned dianhydride monomers include pyromeretic dianehydride (PMDA), 3,3',4,4'-benzophenone tetracarboxylic dianehydride (BTDA), biphenyl tetracarboxylic dianehydride (BPDA), oxydiphthalic dianehydride (ODPA), diphenylsulfone-3,4,3',4'-tetracarboxylic dianehydride (DSDA), and bis(3,4-dicarboxyphenyl) sulfide dianehydride. 2,2-Bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropanedianehydride, 2,3,3',4'-benzophenone tetracarboxylic dianehydride, bis(3,4-dicarboxyphenyl)methanedianehydride, 2,2-bis(3,4-dicarboxyphenyl)propanedianehydride, p-phenylenebis(trimeric monoester acid anhydride), p-biphenylenebis(trimeric (Rhizonium ester acid anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic dianehydride, p-terphenyl-3,4,3',4'-tetracarboxylic dianehydride, 1,3-bis(3,4-dicarboxyphenoxy)benzenedianehydride, 1,4-bis(3,4-dicarboxyphenoxy)benzenedianehydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyldianehydride, 2,2- It may contain one or more selected from the group consisting of bis[(3,4-dicarboxyphenoxy)phenyl]propanedianehydride (BPADA), 2,3,6,7-naphthalenetetracarboxylic acid dianehydride, 1,4,5,8-naphthalenetetracarboxylic dianehydride, and 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianehydride, and preferably pyromeretic dianehydride (PMDA).
[0028] The aforementioned diamine monomers are 1,4-diaminobenzene (PPD), 4,4'-diaminodiphenyl ether (ODA), 2,2-bisaminophenoxyphenylpropane (BAPP), metaphenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (DABA), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl (m-tolidine), and 2,2'-bis(trifluoromethyl (Cyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diamino Nodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-amino Phenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(3-aminophenoxy)benzene (TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenylphenoxy)benzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3 -Bis(3-aminophenylsulfone)benzene, 1,3-bis(4-aminophenylsulfone)benzene, 1,4-bis(4-aminophenylsulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl] ether, bis[3-(4-aminophenoxy)phenyl] ether, bis[4-(3-aminophenoxy)phenyl] ether, bis[4-(4-aminophenoxy)phenyl] ether, bis[3-(3-aminophenoxy)phenyl] ketone, bis[3-(4-aminophenoxy)phenyl] ketone, bis[4-(3-aminophenoxy)phenyl] ketone, bis[4-(4-aminophenoxy)phenyl] ketone, bis[3-(3-aminophenoxy)phenyl] sulfide, bis[3-(4-aminophenoxy)phenyl] sulfide, bis[4-(3-aminophenoxy)phenyl] sulfide, bis[4-(4-aminophenoxy)phenyl] sulfide, bis[3-(3-aminophenoxy)phenyl] sulfone, bis[3-(4-aminophenoxy)phenyl] sulfone, bis[4-(3-aminophenoxy)phenyl] sulfone, bis[4-(4-aminophenoxy)phenyl] sulfone, bis[3-(3-aminophenoxy)phenyl] methane, bis[3-(4-aminophenoxy)phenyl] methane, bis[4-(3-aminophenoxy)phenyl] methane, bis[4-(4-aminophenoxy)phenyl] methane, 2,2-bis[3-(3-aminophenoxy)phenyl] propane, 2,2-bis[3-(4-aminophenoxy)phenyl] propane, 2,2-bis[4-(3-aminophenoxy)phenyl] propane, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and may preferably include 1,4-diaminobenzene (PPD) and 4,4'-diaminodiphenyl ether (ODA).
[0029] In one embodiment, the content of 1,4-diaminobenzene (PPD) in the total diamine monomer may be greater than 0 mol% and 50 mol% or less. For example, the upper limit may be 48 mol% or less, 45 mol% or less, 43 mol% or less, 40 mol% or less, 38 mol% or less, 35 mol% or less, 32 mol% or less, or 30 mol% or less, and the lower limit may be 1 mol% or more, 2 mol% or more, 3 mol% or more, 4 mol% or more, 5 mol% or more, 6 mol% or more, 7 mol% or more, 8 mol% or more, 9 mol% or more, 10 mol% or more, 12 mol% or more, 14 mol% or more, 16 mol% or more, 18 mol% or more, or 20 mol% or more. Preferably, the content of 1,4-diaminobenzene (PPD) in the total diamine monomer may be 20 to 30 mol%.
[0030] When the content of 1,4-diaminobenzene (PPD) exceeds 50 mol%, the heat resistance increases, but the manufactured film is brittle and undesirable. On the other hand, when the content of 1,4-diaminobenzene (PPD) is 0 mol%, the heat resistance is low and undesirable.
[0031] In one embodiment, the content of 4,4'-diaminodiphenyl ether (ODA) in the total diamine monomer may be 50 mol% or more and less than 100 mol%. For example, the upper limit may be 99 mol% or less, 98 mol% or less, 97 mol% or less, 96 mol% or less, 95 mol% or less, 94 mol% or less, 93 mol% or less, 92 mol% or less, 91 mol% or less, 90 mol% or less, 88 mol% or less, 86 mol% or less, 84 mol% or less, 82 mol% or less, or 80 mol% or less, and the lower limit may be 52 mol% or more, 55 mol% or more, 57 mol% or more, 60 mol% or more, 62 mol% or more, 65 mol% or more, 68 mol% or more, or 70 mol% or more. Preferably, the content of 4,4'-diaminodiphenyl ether (ODA) in the total diamine monomer may be 70 to 80 mol%.
[0032] When the content of 4,4'-diaminodiphenyl ether (ODA) is less than 50 mol%, the heat resistance increases, but the manufactured film is brittle, which is undesirable. On the other hand, when the content of 4,4'-diaminodiphenyl ether (ODA) is 100 mol%, the flexibility (elongation) of the film increases, but the heat resistance decreases (Tg decrease), which is undesirable.
[0033] The molar ratio of the dianhydride monomer to the diamine monomer may be 1:2 to 2:1, and preferably 1:1.
[0034] The polyimide may contain 90 to 110 mol% of the diamine monomer, preferably 95 to 105 mol%, more preferably 98 to 102 mol%, and even more preferably 99 to 101 mol%.
[0035] The polyimide may contain 90 to 110 mol% of the dianhydride monomer, preferably 95 to 105 mol%, more preferably 98 to 102 mol%, and even more preferably 100 mol%.
[0036] The polyimide may contain 95 to 105 mol% of the dianhydride monomer, based on 100 mol% of the diamine monomer. For example, the lower limit may be 95.5 mol% or more, 96 mol% or more, 96.5 mol% or more, 97 mol% or more, 97.5 mol% or more, 98 mol% or more, 98.5 mol% or more, 99 mol% or more, or 99.5 mol% or more. The upper limit may be 105 mol% or less, 104 mol% or less, 103 mol% or less, 102 mol% or less, 101 mol% or less, or 100 mol% or less.
[0037] The thickness of the polyimide film can be appropriately selected considering the application, usage environment, and physical properties of the polyimide film. For example, the thickness of the polyimide film may be 1 to 100 μm, 15 to 70 μm, 25 to 50 μm, or 30 to 45 μm, but is not limited thereto.
[0038] Another embodiment of the present invention provides a secondary battery comprising the polyimide film.
[0039] Method for manufacturing polyimide films
[0040] The following describes a method for manufacturing polyimide film. The method for manufacturing polyimide film according to the present invention excludes any overlap with the content described in the above-mentioned polyimide film; however, the content described in the above-mentioned polyimide film also applies to the method for manufacturing polyimide film described below.
[0041] The present invention provides a method for producing a polyimide film, comprising the steps of (a) preparing a polyamic acid solution by introducing a dianhydride monomer and a diamine monomer into a solvent and carrying out an imidation reaction; (b) preparing a mixed solution by introducing nanoparticles having an average particle size of 100 to 500 nm into the polyamic acid solution and stirring; and (c) preparing a polyimide film by coating the mixed solution and drying, wherein the dielectric breakdown voltage (BDV) of the polyimide film is 350 kV / mm or higher and the roughness (Ra) value of the polyimide film is 0.01 nm or higher.
[0042] The mixed solution may contain 1,000 to 5,000 ppm of the nanoparticles, preferably 1,500 to 4,500 ppm, 1,800 to 4,200 ppm, 2,000 to 4,000 ppm, 2,300 to 3,700 ppm, 2,500 to 3,500 ppm, and more preferably 2,800 to 3,200 ppm.
[0043] If the mixed solution contains less than 1,000 ppm of the nanoparticles, the dielectric breakdown voltage of the manufactured polyimide film is low, which is undesirable. If it exceeds 5,000 ppm, the improvement in dielectric breakdown voltage is minimal and inefficient compared to the nanoparticles used, which is also undesirable.
[0044] The solvent may contain one or more selected from the group consisting of N,N'-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), N,N'-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), diethylacetamide (DEAc), N-ethyl-2-pyrrolidone (NEP), N,N'-diethylformamide (DEF), dimethylpropanamide (DMPA), and γ-butyrolactone (GBL).
[0045] In the present invention, the polyamic acid solution may have a solid content of 15 to 50% by weight based on 100 parts by weight of the polyamic acid solution. The lower limit of the solid content by weight may be 16, 17, 18, 19, or 20% or more, and the upper limit of the solid content by weight may be 45, 40, 35, 30, 27, or 25% or less. By adjusting the solid content of the polyamic acid solution, the increase in viscosity can be controlled, and the process time during the curing process can be shortened.
[0046] Another embodiment of the present invention provides a secondary battery comprising a polyimide film manufactured by the method for manufacturing the polyimide film described above. [Effects of the Invention]
[0047] The polyimide film and its manufacturing method according to the present invention improve electrical properties by strengthening dielectric breakdown strength and increasing dielectric breakdown voltage through the inclusion of nanoparticles with an average particle size of 100 to 500 nm, thereby enhancing the practicality of films for secondary batteries.
[0048] Furthermore, the polyimide film and its manufacturing method according to the present invention have the effect of satisfying the required roughness for ensuring the windability of the sample in the roll-to-roll process.
[0049] Furthermore, the polyimide film according to the present invention has the effect of being applicable to secondary batteries. [Modes for carrying out the invention]
[0050] To aid in understanding the present invention, examples are provided below. The following examples are provided to facilitate understanding of the present invention and do not limit the scope of the invention.
[0051] <Example: Manufacturing of polyimide film>
[0052] Examples
[0053] A polyamic acid solution was prepared by mixing 100 mol% of dimethylformamide (DMF) as a solvent with 100 mol% of a diamine monomer and 100 mol% of a dianhydride monomer. Here, the diamine monomer contained 25 mol% of 1,4-diaminobenzene (PPD) and 75 mol% of 4,4'-diaminodiphenyl ether (ODA), and the dianhydride monomer contained 100 mol% of pyromeretic dianehydride (PMDA).
[0054] To the aforementioned polyamic acid solution, 3,000 ppm of nanosilica with an average particle size of 100 nm and a catalyst were added and stirred to prepare a mixed solution.
[0055] The degassed mixed solution was applied to a glass plate. Next, the solvent-to-solids ratio was calculated and the solution was spread using an applicator to ensure uniform distribution across the surface. The solution was then cured at 130°C (3 mins) → 280°C (4 mins) → 420°C (4 mins) to obtain a polyimide film. The film thickness was manufactured to 12.5 μm.
[0056] Examples 2-5
[0057] As shown in Table 1 below, polyimide films were manufactured using the same method as in Example 1, except that the average particle size of the nanosilica was varied.
[0058] Comparative Examples 1-4
[0059] As shown in Table 1 below, polyimide films were manufactured using the same method as in Example 1, except that calcium phosphate was used instead of nanosilica, and the average particle size and content of calcium phosphate were varied.
[0060] Comparative Examples 5-7
[0061] As shown in Table 1 below, polyimide films were manufactured using the same method as in Example 1, except that the average particle size of the nanosilica was varied.
[0062] Table 1 below lists the types, average particle size, and content of nanoparticles (nanosilica, calcium phosphate) used in the production of polyimide films according to Examples 1-5 and Comparative Examples 1-7.
[0063] [Table 1]
[0064] <Experimental Example: Evaluation of Physical Properties of Polyimide Film>
[0065] Experimental Example 1. Evaluation of Dielectric Breakdown Voltage (BDV)
[0066] The dielectric breakdown voltage (BDV) of the polyimide films produced in the above examples and comparative examples was measured in accordance with the ASTM D149 standard. Specifically, the polyimide films were pre-treated in a 100°C oven to remove moisture, then fixed in a measuring device (PHENIX, TECHNOLOGIES 6CCE50-5) set to a room temperature atmosphere. A voltage of 10 kVAc was applied to the upper electrode at the bottom, and the BDV was measured by increasing the AC voltage from 0 at a constant rate. The measurement results are shown in Table 2 below.
[0067] Experimental Example 2. Measurement of Roughness (Ra) Value
[0068] The roughness (Ra) values of the polyimide films produced in the above examples and comparative examples were measured using a film roughness analyzer manufactured by Kosaka Laboratory Ltd. The measurement results are shown in Table 2 below.
[0069] [Table 2]
[0070] Table 2 shows that Examples 1 to 5, which use nanosilica with an average particle size of 100 to 500 nm, all exhibit excellent BDV values (≧350 kV / mm) and roughness (Ra) values (≧0.010 nm).
[0071] On the other hand, Comparative Examples 1-4, which used calcium phosphate with average particle sizes of 1 μm and 2 μm, showed excellent roughness (Ra) values, but it was confirmed that they had low BDV values.
[0072] Furthermore, it can be confirmed that Comparative Examples 5-7, which use nanosilica with an average particle diameter of less than 100 nm, have low roughness values.
[0073] On the other hand, in Example 5, which uses nanosilica with an average particle size of 500 nm, it has excellent BDV values (≧350 kV / mm) and roughness (Ra) values (≧0.010 nm), but it is undesirable because it may cause filler dispersion problems.
[0074] These results indicate that the polyimide film and its manufacturing method of the present invention, by including nanoparticles with an average particle size of 100 to 500 nm, can enhance the dielectric breakdown strength and improve the dielectric breakdown voltage, thereby improving electrical properties and increasing the practicality of the film for secondary batteries.
[0075] Furthermore, the polyimide film and its manufacturing method according to the present invention, by including nanoparticles with an average particle diameter of 100 to 500 nm, have the effect of satisfying the required roughness for ensuring the winding ability of the sample in a roll-to-roll process.
[0076] Furthermore, the polyimide film according to the present invention has the effect of being applicable to secondary batteries.
[0077] This specification omits detailed descriptions of matters that can be easily understood and inferred by a person with ordinary skill in the art of the present invention. Beyond the specific examples provided herein, various modifications are possible without altering the technical concept or essential configuration of the present invention. Therefore, the present invention can be implemented in ways different from those specifically described and illustrated herein, and this is understandable to a person with ordinary skill in the art of the present invention.
Claims
1. A polyimide containing dianhydride monomers and diamine monomers as polymerization units, It contains nanoparticles with an average particle size of 100 to 500 nm. The dielectric breakdown voltage (BDV) is 350 kV / mm or higher. A polyimide film having a roughness (Ra) value of 0.01 nm or greater.
2. The polyimide film according to claim 1, wherein the nanoparticles include nanosilica.
3. The polyimide film according to claim 1, wherein the polyimide film contains 1,000 to 5,000 ppm of the nanoparticles.
4. The aforementioned dianhydride monomers include pyromeretic dianehydride (PMDA), 3,3',4,4'-benzophenone tetracarboxylic dianehydride (BTDA), biphenyl tetracarboxylic dianehydride (BPDA), oxydiphthalic dianehydride (ODPA), diphenyl sulfone-3,4,3',4'-tetracarboxylic dianehydride (DSDA), and bis(3,4-dicarboxyphenyl) sulfide dianehydride. Hydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropanedianehydride, 2,3,3',4'-benzophenonetetracarboxylic dianehydride, bis(3,4-dicarboxyphenyl)methanedianehydride, 2,2-bis(3,4-dicarboxyphenyl)propanedianehydride, p-phenylenebis(trimeltic monoester acid anhydride), p-bife Nilenbis(trimeltic monoester acid anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic dianehydride, p-terphenyl-3,4,3',4'-tetracarboxylic dianehydride, 1,3-bis(3,4-dicarboxyphenoxy)benzenedianehydride, 1,4-bis(3,4-dicarboxyphenoxy)benzenedianehydride, 1,4-bis(3,4-dicarboxyphenoxy The polyimide film according to claim 1, comprising one or more selected from the group consisting of biphenyl dianehydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propanedianehydride (BPADA), 2,3,6,7-naphthalenetetracarboxylate dianehydride, 1,4,5,8-naphthalenetetracarboxylate dianehydride, and 4,4'-(2,2-hexafluoroisopropylidene)diphthalate dianehydride.
5. The polyimide film according to claim 4, wherein the dianhydride monomer comprises pyromeretic dianehydride (PMDA).
6. The aforementioned diamine monomers are 1,4-diaminobenzene (PPD), 4,4'-diaminodiphenyl ether (ODA), 2,2-bisaminophenoxyphenylpropane (BAPP), metaphenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (DABA), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl (m-tolidine), and 2,2'-bis(trifluoromethyl 3,3'-Dimethyl-4,4'-Diaminobiphenyl, 3,3'-Dicarboxy-4,4'-Diaminodiphenylmethane, 3,3'-5,5'-Tetramethyl-4,4'-Diaminodiphenylmethane, 4,4'-Diaminobenzanilide, 3,3'-Dimethoxybenzidine, 2,2'-Dimethoxybenzidine, 3,3'-Diaminodiphenyl ether, 3,4'-Diaminodiphenyl ether, 3,3'-Diaminodiphenyl sulfide, 3,4'-Diaminodiphenyl sulfide, 4,4'-Diamino Nodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-amino Phenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(3-aminophenoxy)benzene (TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenylphenoxy)benzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3 -Bis(3-aminophenylsulfone)benzene, 1,3-bis(4-aminophenylsulfone)benzene, 1,4-bis(4-aminophenylsulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-Bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl] ether, bis[3-(4-aminophenoxy)phenyl] ether, bis[4-(3-aminophenoxy)phenyl] ether, bis[4-(4-aminophenoxy)phenyl] ether, bis[3-(3-aminophenoxy)phenyl] ketone, bis[3-(4-aminophenoxy)phenyl] ketone, bis[4-(3-aminophenoxy)phenyl] ketone, bis[4-(4-aminophenoxy) [xy)phenyl]ketone, bis[3-(3-aminophenoxy)phenyl]sulfide, bis[3-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl] [Nyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[3-(3-aminophenoxy A polyimide film according to claim 1, comprising one or more selected from the group consisting of [(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.
7. The polyimide film according to claim 6, wherein the diamine monomer comprises 1,4-diaminobenzene (PPD) and 4,4'-diaminodiphenyl ether (ODA).
8. Of the total diamine monomers, the content of 1,4-diaminobenzene (PPD) is greater than 0 mol% and 50 mol% or less. The polyimide film according to claim 7, wherein the content of 4,4'-diaminodiphenyl ether (ODA) in the total diamine monomer is 50 mol% or more and less than 100 mol%.
9. The polyimide film according to claim 1, wherein the thickness of the polyimide film is 1 to 100 μm.
10. A secondary battery comprising the polyimide film described in claim 1.
11. (a) A step of adding a dianhydride monomer and a diamine monomer to a solvent and polymerizing them to produce a polyamic acid solution, (b) A step of adding nanoparticles having an average particle size of 100 to 500 nm to the polyamic acid solution and stirring to produce a mixed solution, (c) The step of applying the mixed solution and drying it to produce a polyimide film, The dielectric breakdown voltage (BDV) of the polyimide film is 350 kV / mm or higher. A method for producing a polyimide film, wherein the roughness (Ra) value of the polyimide film is 0.01 nm or greater.
12. The method for producing a polyimide film according to claim 11, wherein the mixed solution contains 1,000 to 5,000 ppm of the nanoparticles.
13. A method for producing a polyimide film according to claim 11, wherein the solvent comprises one or more selected from the group consisting of N,N'-dimethylacetamide (DMAc), N-methyl-2-pyrrolidone (NMP), N,N'-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), diethylacetamide (DEAc), N-ethyl-2-pyrrolidone (NEP), N,N'-diethylformamide (DEF), dimethylpropanamide (DMPA), and γ-butyrolactone (GBL).