Electrolyte and sodium-ion batteries

The electrolyte composition for sodium-ion batteries, using sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, addresses stability issues, improving high-temperature performance and reducing costs by forming a stable solvation structure.

JP2026539307APending Publication Date: 2026-11-24GUANGZHOU TINCI MATERIALS TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026525239
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-02
Filing Date
2024-10-31
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Sodium-ion batteries face challenges with high-temperature cycling and storage due to the instability of current electrolytes, which require strict environmental control and result in shorter shelf life and higher costs.

Method used

An electrolyte composition comprising sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, with specific mass percentages, forms a stable solvation structure that enhances high-temperature stability and reduces decomposition, allowing for relaxed environmental conditions during preparation, storage, and use.

Benefits of technology

The electrolyte improves the stability and conductivity of sodium-ion batteries, extending shelf life, reducing costs, and ensuring good wetting between electrolyte and electrodes, thereby enhancing cycle life and safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539307000001
    Figure 2026539307000001
  • Figure 2026539307000002
    Figure 2026539307000002
  • Figure 2026539307000003
    Figure 2026539307000003
Patent Text Reader

Abstract

The electrolyte comprises a sodium salt, an additive, and an organic solvent. The sodium salt includes sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide, and the additive includes 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide. The electrolyte contains, by mass percentage, 2 to 15% by weight of sodium hexafluorophosphate, 0.1 to 20% by weight of sodium bis(fluorosulfonyl)imide, and 0.1 to 5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, with the remainder being an organic solvent. Because the electrolyte has high stability at room temperature or high temperature environments, it can alleviate strict environmental requirements in the preparation, transportation, and storage processes of the electrolyte, effectively suppress manufacturing costs, and improve the cycle stability of batteries when applied to sodium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority based on the Chinese patent application filed with the China National Intellectual Property Administration on November 2, 2023, with application number 202311449268.9 and the invention titled "Electrolyte and Use Thereof", the entire contents of which are incorporated herein by reference.

[0002] The present invention belongs to the field of sodium-ion batteries, and relates to an electrolyte, in particular to an electrolyte and a sodium-ion battery.

Background Art

[0003] Lithium-ion batteries are widely used in new energy vehicles, various portable electronic devices, and energy storage fields due to their advantages such as high energy density, long cycle life, and small volume. However, since lithium has small reserves and uneven resource distribution, the cost of lithium-ion batteries is increasing year by year, and there is an urgent need to develop new battery systems. Sodium is in the same group as lithium and has similar chemical properties, and its reserves are extremely abundant at 2.36%, with lower cost and better safety. Furthermore, sodium-ion batteries have the advantages of high energy density and excellent cost performance, and can meet the needs of future sustainable energy development. However, sodium-ion batteries still have some challenges in terms of high-temperature cycling and high-temperature storage.

[0004] The electrolyte is a crucial component of sodium-ion batteries, occupying a large proportion of the battery's composition; therefore, its properties significantly impact the battery's overall performance. Currently, sodium difluorophosphate and ethylene sulfate are widely used as electrolyte additives to effectively improve the lifespan and reliability of sodium-ion batteries under high-temperature storage conditions. However, electrolytes containing sodium difluorophosphate require low-temperature storage to maintain stability and avoid decomposition at room temperature or high temperatures. Furthermore, the presence of trace amounts of water in the electrolyte makes ethylene sulfate susceptible to hydrolysis at room temperature or high temperatures. The hydrolysis products include sulfuric acid and glycol sulfate monoesters, increasing the overall acidity of the electrolyte, and this reaction intensifies under high-temperature storage conditions. This limits the broad applicability of ethylene sulfate.

[0005] Therefore, electrolytes containing ethylene sulfate and / or sodium difluorophosphate always require stricter environmental control during preparation, transportation, and storage, and the electrolyte has a shorter shelf life and consistently higher costs. [Overview of the Initiative]

[0006] To solve the above problems, the present invention provides an electrolyte that has high stability in room temperature or high temperature environments, thereby easing to some extent the strict environmental requirements in the preparation, transportation, and storage processes of the electrolyte, extending the shelf life of the electrolyte, and effectively suppressing manufacturing costs. In a first embodiment of the present invention, an electrolyte is provided comprising a sodium salt, an additive, and an organic solvent, wherein the sodium salt comprises sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide, and the additive comprises 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide.

[0007] The electrolyte contains, by mass percentage, 2 to 15% by weight of sodium hexafluorophosphate, 0.1 to 20% by weight of sodium bis(fluorosulfonyl)imide, and 0.1 to 5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, with the remainder being an organic solvent.

[0008] Furthermore, the mass percentage of sodium hexafluorophosphate in the electrolyte is 6 to 14% by weight.

[0009] Furthermore, the mass percentage of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in the electrolyte is 1-2% by weight.

[0010] Furthermore, the mass percentage of bis(fluorosulfonyl)imide sodium in the electrolyte is 2 to 8% by weight.

[0011] Furthermore, the organic solvent includes at least one of the following: carbonates, fluorocarbonates, carboxylic acid esters, fluorocarboxylic acid esters, ethers, and fluoroethers.

[0012] Furthermore, the electrolyte further comprises a sodium salt additive, the sodium salt additive comprising at least one of sodium perchlorate, sodium bis(oxalato)borate, sodium difluoro(oxalato)borate, and sodium bis(trifluoromethanesulfonyl)imide.

[0013] Furthermore, the mass percentage of the sodium salt additive in the electrolyte is 0.01 to 1% by weight.

[0014] Furthermore, the electrolyte further contains an organic additive, the organic additive comprising at least one of vinylethylene carbonate, fluoroethylene carbonate, vinylene carbonate, hexamethylene diisocyanate, ethynylethylene carbonate, trans-difluoroethylene carbonate, 1,3-propanesultone, 1,4-propanesultone, propa-1-ene-1,3-sultone, 1,3,2-dioxathiolan-2,2-dioxide, 4-propyl-1,3,2-dioxathiolan-2,2-dioxide, methylene methane disulfonate, 1,2-ethanedisulfonic anhydride, tris(trimethylsilyl)borate, succinanitrile, ethoxy(pentafluoro)cyclotriphosphazene, tert-butylbenzene, tert-amylbenzene, fluorobenzene, and cyclohexylbenzene.

[0015] Furthermore, the mass percentage of the organic additive in the electrolyte is 0.1 to 20% by weight.

[0016] In a second aspect of the present invention, a sodium-ion battery is provided comprising an electrolyte provided according to the first aspect of the present invention, the sodium-ion battery provided according to the second aspect of the present invention having good cycle characteristics.

[0017] The electrolyte of the present invention contains sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide. Of these, sodium hexafluorophosphate has high conductivity and ion transport rate, and can improve the overall conductivity of the electrolyte system, but its stability is poor and its safety is not high. In contrast, the present invention uses sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide as the main sodium salts, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide as an additive. By limiting the mass percentages of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in the electrolyte, a synergistic effect is obtained between the three, ultimately resulting in an electrolyte with high storage stability. Therefore, the environmental temperature control conditions can be relaxed during the preparation, storage, and use processes, the electrolyte can be stored in harsh environments such as high temperatures, and the objectives of extending the shelf life of the electrolyte and reducing storage and transportation costs can be achieved. Furthermore, because the electrolyte has good high-temperature stability, it can accelerate penetration at high temperatures, ensuring good wetting between the electrolyte, electrodes, and separators, thereby improving the problem of insufficient electrolyte penetration in sodium-ion batteries. [Modes for carrying out the invention]

[0018] To further clarify the object, technical solution, and advantages of the present invention, the technical solution in the embodiments of the present invention will be described in detail below with reference to the embodiments of the present invention. It will be clear that the embodiments described are merely a part of the embodiments of the present invention, and not all embodiments. Any other embodiments that a person skilled in the art can obtain based on the embodiments of the present invention without requiring any creative work will fall within the scope of the protection of the present invention.

[0019] In a first aspect of the present invention, an electrolyte is provided, comprising a sodium salt, an additive and an organic solvent, wherein the sodium salt comprises sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide, and the additive comprises 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide.

[0020] The electrolyte contains, by mass percentage, 2 to 15% by weight of sodium hexafluorophosphate, 0.1 to 20% by weight of sodium bis(fluorosulfonyl)imide, and 0.1 to 5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, with the remainder being an organic solvent.

[0021] The present invention does not limit the origin of each component, and commercially available products known to those skilled in the art or products prepared by conventional preparation methods may be used.

[0022] In the technical solution provided by the present invention, the electrolyte comprises sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, of which sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide are the main salts of the complex sodium salt, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide is used as an electrolyte additive, while limiting the mass percentages of these three in the electrolyte. This significantly improves the storage stability of the electrolyte, especially under harsh high-temperature environments, thereby extending the shelf life of the electrolyte and reducing storage and transportation costs. Based on this phenomenon, the inventors have analyzed raw materials that improve stability and have concluded the following. In other words, the combination of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide changes the solvation structure of the electrolyte system, forming a more stable solvation structure with sodium ions as the core, 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide and organic solvent molecules as the intermediate layer, and hexafluorophosphate ions and bis(fluorosulfonyl)imide anions as the outer layer. This suppresses the decomposition of sodium hexafluorophosphate at high temperatures. Furthermore, when the mass percentages of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in the electrolyte are within a limited range, the decomposition rate of sodium salts can be further reduced in high-temperature environments, significantly improving the stability of the electrolyte under room temperature or high-temperature storage conditions. As a result, the environmental requirements in the preparation, storage, or use processes of the electrolyte can be relaxed, and the objective of reducing costs can be achieved.

[0023] Furthermore, sodium-ion batteries containing the above-mentioned electrolyte also possess excellent ionic conductivity, electrical conductivity, and penetration characteristics. The reason for this is as follows: By limiting the mass percentages of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in the electrolyte of the present invention, the three components cooperate and influence each other, thereby giving the electrolyte good ionic conductivity and electrical conductivity, further reducing the internal resistance of the sodium-ion battery and improving the initial efficiency and rate characteristics. At the same time, because the electrolyte has good high-temperature stability, penetration at high temperatures can be accelerated, allowing for good wetting between the electrolyte and the electrodes and separator, thus improving the problem of insufficient electrolyte penetration in sodium-ion batteries.

[0024] In one specific embodiment, the mass percentage of sodium hexafluorophosphate in the electrolyte is 6 to 14% by weight. Within this range, sodium hexafluorophosphate can form a good synergistic effect with sodium bis(fluorosulfonyl)imide and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, thereby providing the electrolyte with good high-temperature stability and high ionic conductivity.

[0025] In a specific embodiment, the mass percentage of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in the electrolyte is 1-2 wt%. Within this range, 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide can better synergize with sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide, further improving the high-temperature storage stability of the electrolyte. At the same time, when applied to sodium-ion batteries, 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide can rapidly form a stable and dense SEI film on the surfaces of the positive and negative electrodes during charge and discharge processes. This effectively suppresses side reactions between the electrolyte and the positive and negative electrodes, making the effect of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in improving electrolyte stability more prominent, and endowing sodium-ion batteries with better cycle life and safety performance.

[0026] In a specific embodiment, the mass percentage of sodium bis(fluorosulfonyl)imide in the electrolyte is 2-8 wt%. Within this range, it can be better formulated with 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide and sodium hexafluorophosphate, improving the high-temperature storage stability of the electrolyte, reducing the temperature sensitivity of the electrolyte, and lowering costs. At the same time, sodium bis(fluorosulfonyl)imide and sodium hexafluorophosphate can better synergize to effectively suppress the corrosion of aluminum foil caused by sodium bis(fluorosulfonyl)imide.

[0027] In a specific embodiment, the organic solvent includes at least one of carbonates, fluorocarbonates, carboxylates, fluorocarboxylates, ethers, and fluoroethers. For example, the organic solvent may be at least one of propylene carbonate, ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, propylene carbonate, diethyl carbonate, ethyl acetate, methyl acetate, propyl acetate, butyl acetate, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and trifluoroethyl methyl carbonate, and is not particularly limited in the present invention. When the organic solvent is a mixture of the above-mentioned specific compounds, the ratio between the specific compounds is not particularly limited in the present invention.

[0028] In a specific embodiment, the electrolyte further includes a sodium salt additive, which includes at least one of sodium perchlorate, sodium bis(oxalato)borate, sodium difluoro(oxalato)borate, and sodium bis(trifluoromethanesulfonyl)imide. By adding the sodium salt additive to introduce anions, the anions participate in constructing the outer layer of the solvation structure together with hexafluorophosphate ions and bis(fluorosulfonyl)imide anions, thereby making the electrolyte system more stable and further improving the stability of the electrolyte at room temperature or high temperatures.

[0029] Further, when the sodium salt additive is further added to the electrolyte, the formation of the SEI film can be further promoted in the obtained sodium-ion battery, side reactions between the electrolyte and the positive and negative electrodes can be better avoided, and the stability of the electrolyte system can be improved. Meanwhile, the anions in the sodium salt additive contribute to controlling the solvation shell of sodium ions, improving the ionic conductivity of the electrolyte, and reducing the migration resistance of sodium ions in the electrolyte. As a result, the sodium-ion battery can have high initial efficiency and rate performance.

[0030] In one specific embodiment, the mass percentage of the sodium salt additive in the electrolyte is 0.01 to 1% by weight. Within this range, the stability of the electrolyte system at room temperature or high temperature can be further improved. Furthermore, the effect of the sodium salt additive on improving the ion conductivity and electrical conductivity of the electrolyte can be made more pronounced, resulting in better initial efficiency and rate characteristics of the sodium-ion battery.

[0031] In one specific embodiment, the electrolyte further comprises an organic additive, the organic additive comprising at least one of vinylethylene carbonate, fluoroethylene carbonate, vinylene carbonate, hexamethylene diisocyanate, ethynylethylene carbonate, trans-difluoroethylene carbonate, 1,3-propanesultone, 1,4-propanesultone, prop-1-ene-1,3-sultone, 1,3,2-dioxathiolan-2,2-dioxide, 4-propyl-1,3,2-dioxathiolan-2,2-dioxide, methylene methane disulfonate, 1,2-ethanedisulfonic anhydride, tris(trimethylsilyl)borate, succinanitrile, ethoxy(pentafluoro)cyclotriphosphazene, tert-butylbenzene, tert-amylbenzene, fluorobenzene, and cyclohexylbenzene. The above organic additive has good compatibility with 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide. Furthermore, it can contribute to the construction of an intermediate layer in the solvation structure, thereby obtaining a more stable electrolyte and further improving the stability of the electrolyte at room temperature or high temperature.

[0032] Furthermore, by adding organic additives, the SEI film can be formed more quickly on the surfaces of the positive and negative electrodes, further reducing side reactions between the electrolyte and the positive and negative electrodes, improving the stability of the electrolyte, and improving the penetration effect between the electrolyte and the positive and negative electrode pieces. This solves the problem of insufficient penetration in sodium-ion batteries and improves the safety characteristics of sodium-ion batteries.

[0033] In one specific embodiment, the mass percentage of the organic additive in the electrolyte is 0.1 to 20% by weight. Within this range, the electrolyte can be given good stability, and the permeability between the electrolyte and the positive and negative electrode pieces can be further improved, thereby shortening the transport path of sodium ions. As a result, the cycle life and rate characteristics of the sodium-ion battery can be improved.

[0034] In a second aspect of the present invention, a sodium-ion battery is provided comprising an electrolyte according to any one of the above-mentioned items, wherein the synergistic and mutual effects between sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, and 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide contained in the electrolyte effectively improve the stability of the electrolyte at room temperature or high temperature, reduce costs, and simultaneously improve the conductivity and ion transport rate of the electrolyte. Therefore, the sodium-ion battery not only has high cycle stability and low internal resistance at high temperatures, but also has a good filtration effect, effectively reducing the manufacturing, storage, and transportation costs of the sodium-ion battery.

[0035] The sodium-ion battery containing the electrolyte of the present invention will be described in detail below with reference to specific examples.

[0036] Example 1 In a glove box under an argon atmosphere, 40% by weight of propylene carbonate, 20% by weight of ethyl methyl carbonate, and 20% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0037] Example 2 In a glove box under an argon atmosphere, 40.66% by weight of propylene carbonate, 20.32% by weight of ethyl methyl carbonate, and 20.32% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 0.2% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 8.5% by weight of sodium hexafluorophosphate and 6.5% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0038] Example 3 In a glove box under an argon atmosphere, 38.24% by weight of propylene carbonate, 19.13% by weight of ethyl methyl carbonate, and 19.13% by weight of diethyl carbonate, all organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 11.5% by weight of sodium hexafluorophosphate and 3.5% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0039] Example 4 In a glove box under an argon atmosphere, 40% by weight of propylene carbonate, 20% by weight of ethyl methyl carbonate, and 20% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 14.5% by weight of sodium hexafluorophosphate and 0.5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0040] Example 5 In a glove box under an argon atmosphere, 40% by weight of propylene carbonate, 20% by weight of ethyl methyl carbonate, and 20% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 7% by weight of sodium hexafluorophosphate and 8% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0041] Example 6 In a glove box under an argon atmosphere, 35% by weight of propylene carbonate, 17.5% by weight of ethyl methyl carbonate, and 17.5% by weight of diethyl carbonate, all organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 15% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0042] Example 7 In a glove box under an argon atmosphere, 39.7% by weight of propylene carbonate, 19.9% ​​by weight of ethyl methyl carbonate, and 19.9% ​​by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate, 5% by weight of sodium bis(fluorosulfonyl)imide, and 0.5% of sodium perchlorate were added and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0043] Example 8 In a glove box under an argon atmosphere, 39.4% by weight of propylene carbonate, 19.7% by weight of ethyl methyl carbonate, and 19.7% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate, 5% by weight of sodium bis(fluorosulfonyl)imide, and 1.2% of sodium perchlorate were added and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0044] Example 9 In a glove box under an argon atmosphere, 30.5% by weight of propylene carbonate, 15.5% by weight of ethyl methyl carbonate, and 15.5% by weight of diethyl carbonate, all organic solvents, were mixed. Then, 6% by weight of fluoroethylene carbonate, 6% by weight of vinylene carbonate, 6% by weight of 1,3-propanesultone, 4% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0045] Example 10 In a glove box under an argon atmosphere, 41.5% by weight of propylene carbonate, 21% by weight of ethyl methyl carbonate, and 21% by weight of diethyl carbonate, which are organic solvents, were mixed. Next, 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide was added. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was homogenized to obtain the electrolyte of this example.

[0046] Example 11 In a glove box under an argon atmosphere, 43% by weight of propylene carbonate, 22% by weight of ethyl methyl carbonate, and 22% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 3% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was homogenized to obtain the electrolyte of this example.

[0047] Example 12 In a glove box under an argon atmosphere, 39.5% by weight of propylene carbonate, 19.5% by weight of ethyl methyl carbonate, and 19.5% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 3% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0048] Example 13 In a glove box under an argon atmosphere, 40.7% by weight of propylene carbonate, 20.35% by weight of ethyl methyl carbonate, and 20.35% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 0.1% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was homogenized to obtain the electrolyte of this example.

[0049] Example 14 In a glove box under an argon atmosphere, 40.25% by weight of propylene carbonate, 20.125% by weight of ethyl methyl carbonate, and 20.125% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0050] Example 15 In a glove box under an argon atmosphere, 39.75% by weight of propylene carbonate, 19.875% by weight of ethyl methyl carbonate, and 19.875% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 2% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was homogenized to obtain the electrolyte of this example.

[0051] Example 16 In a glove box under an argon atmosphere, 44% by weight of propylene carbonate, 22% by weight of ethyl methyl carbonate, and 22% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 2% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0052] Example 17 In a glove box under an argon atmosphere, 42% by weight of propylene carbonate, 21% by weight of ethyl methyl carbonate, and 21% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 6% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0053] Example 18 In a glove box under an argon atmosphere, 38% by weight of propylene carbonate, 19% by weight of ethyl methyl carbonate, and 19% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 14% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0054] Example 19 In a glove box under an argon atmosphere, 37.5% by weight of propylene carbonate, 18.75% by weight of ethyl methyl carbonate, and 18.75% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 15% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0055] Example 20 In a glove box under an argon atmosphere, 42.45% by weight of propylene carbonate, 21.225% by weight of ethyl methyl carbonate, and 21.225% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 0.1% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0056] Example 21 In a glove box under an argon atmosphere, 41.5% by weight of propylene carbonate, 20.75% by weight of ethyl methyl carbonate, and 20.75% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 2% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was stirred uniformly to obtain the electrolyte of this example.

[0057] Example 22 In a glove box under an argon atmosphere, 32.5% by weight of propylene carbonate, 16.25% by weight of ethyl methyl carbonate, and 16.25% by weight of diethyl carbonate, all organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 20% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0058] Example 23 In a glove box under an argon atmosphere, 41.7% by weight of propylene carbonate, 20.85% by weight of ethyl methyl carbonate, and 20.85% by weight of diethyl carbonate, which are organic solvents, were mixed. Next, 0.1% by weight of fluoroethylene carbonate and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in sequence. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added, and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0059] Example 24 In a glove box under an argon atmosphere, 31.75% by weight of propylene carbonate, 15.875% by weight of ethyl methyl carbonate, and 15.875% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 6% by weight of fluoroethylene carbonate, 6% by weight of vinylene carbonate, 6% by weight of 1,3-propanesultone, 2% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate and 5% by weight of sodium bis(fluorosulfonyl)imide were added and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0060] Example 25 In a glove box under an argon atmosphere, 39.994% by weight of propylene carbonate, 19.998% by weight of ethyl methyl carbonate, and 19.998% by weight of diethyl carbonate, all organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate, 5% by weight of sodium bis(fluorosulfonyl)imide, and 0.01% of sodium perchlorate were added and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0061] Example 26 In a glove box under an argon atmosphere, 39.5% by weight of propylene carbonate, 19.75% by weight of ethyl methyl carbonate, and 19.75% by weight of diethyl carbonate, which are organic solvents, were mixed. Then, 1% by weight of fluoroethylene carbonate, 1% by weight of vinylene carbonate, 1% by weight of 1,3-propanesultone, 0.5% by weight of propa-1-ene-1,3-sultone, and 1.5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide were added in order. Finally, 10% by weight of sodium hexafluorophosphate, 5% by weight of sodium bis(fluorosulfonyl)imide, and 1% of sodium perchlorate were added and the mixture was uniformly stirred to obtain the electrolyte of this example.

[0062] Comparative Example 1 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that ethylene sulfate was used instead of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide.

[0063] Comparative Example 2 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that sodium difluorophosphate was used instead of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide.

[0064] Comparative Example 3 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that a mixture of ethylene sulfate and sodium difluorophosphate was used instead of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, the mass percentage of sodium difluorophosphate in the electrolyte was set to 0.75% by weight, the mass percentage of ethylene sulfate in the electrolyte was set to 0.75% by weight, and the other components remained unchanged.

[0065] Comparative Example 4 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that sodium perchlorate was used instead of sodium bis(fluorosulfonyl)imide.

[0066] Comparative Example 5 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that the mass percentage of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide in the electrolyte was 6% by weight, and in this case, the mass percentage of propylene carbonate, which is the organic solvent in the electrolyte, was 37.76% by weight, the mass percentage of ethyl methyl carbonate was 18.87% by weight, and the mass percentage of diethyl carbonate was 18.87% by weight.

[0067] Comparative Example 6 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that lithium hexafluorophosphate was used instead of sodium hexafluorophosphate, and lithium bis(fluorosulfonyl)imide was used instead of sodium bis(fluorosulfonyl)imide.

[0068] Comparative Example 7 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that the mass percentage of sodium hexafluorophosphate in the electrolyte was 17% by weight, the mass percentage of propylene carbonate (an organic solvent in the electrolyte) was 37% by weight, the mass percentage of ethyl methyl carbonate was 18% by weight, the mass percentage of diethyl carbonate was 18% by weight, and the other components remained unchanged.

[0069] Comparative Example 8 The method for preparing the electrolyte in this comparative example was substantially the same as in Example 1, except that the mass percentage of bis(fluorosulfonyl)imide sodium in the electrolyte was 22% by weight, the mass percentage of propylene carbonate (an organic solvent in the electrolyte) was 31% by weight, the mass percentage of ethyl methyl carbonate was 16% by weight, the mass percentage of diethyl carbonate was 16% by weight, and the other components remained unchanged.

[0070] Test example The electrolytes prepared in the above examples and comparative examples were divided into three groups: Group 1 electrolyte, Group 2 electrolyte, and Group 3 electrolyte. Group 1 electrolyte was the electrolyte immediately after preparation, Group 2 electrolyte was stored at 45°C for 24 hours, and Group 3 electrolyte was stored at room temperature (25°C) for 180 days. Sodium-ion batteries were manufactured using each of the three electrolyte groups. The manufacturing steps for the sodium-ion batteries were as follows.

[0071] 90% by weight of NaNi 1 / 3 Mn 1 / 3 Fe 1 / 3A slurry of positive electrode active material was obtained by mixing and stirring O2 powder, 5% by weight of polyvinylidene fluoride, 5% by weight of acetylene black, and the solvent N-methylpyrrolidone. This slurry was applied to both sides of an aluminum foil with a thickness of 16 μm and dried at 130°C for 12 hours. After drying, a positive electrode piece was obtained by roll pressing, slitting, and tab welding. The thickness of the positive electrode material layer on one side was 58 μm, and the dimensions of the cut positive electrode piece were 558 mm in length and 55 mm in width. A slurry of negative electrode active material was obtained by mixing and stirring 89% by weight of hard carbon, 1% by weight of conductive carbon black Super-P, and 10% by weight of polyvinylidene fluoride. This slurry was applied to both sides of an aluminum foil with a thickness of 16 μm and dried at 120°C for 12 hours. After drying, a negative electrode piece was obtained by roll pressing, slitting, and tab welding. The thickness of the negative electrode material layer on one side was 67 μm, and the dimensions of the negative electrode piece after cutting were 708 mm in length and 59 mm in width. A ceramic-coated PE separator was used as the separator. The separator was purchased from Shenzhen Senior Technology Material Co., Ltd., model number PE Ceramics 16+4, and the total thickness of the separator was 20 μm.

[0072] An electrode assembly was obtained by sequentially stacking and winding the prepared positive electrode piece, separator, and negative electrode piece so that the separator would act as an intermediary between the positive electrode piece and the negative electrode piece to provide isolation. The electrode assembly was placed in an aluminum plastic film outer bag, moisture was removed at 85°C, and the first, second, and third groups of electrolytes prepared above were injected, with an injection coefficient of 5 g / Ah. Subsequently, a sodium-ion battery was obtained through processes such as vacuum sealing, standing, formation, shaping, and sorting. The standing time was 48 hours, and the formation process involved charging to 3.4V at 0.02C, then to 3.8V at 0.2C, and finally to the formation upper limit voltage of 4V at 0.5C. The formation temperature was 45°C.

[0073] Initial efficiency, cycle characteristics, DCR DC internal resistance, and smearability measurements were performed on sodium-ion batteries containing the first group electrolyte, the second group electrolyte, and the third group electrolyte.

[0074] (1) Initial efficiency measurement at 25℃ After the sodium-ion battery formation was complete, the total charge capacity of the entire formation process was recorded as C1. After aging at a high temperature of 45°C for 24 hours, the initial efficiency measurement was performed at a temperature of 25°C. The measurement procedure was as follows: After charging to 4.0V with a current of 0.2C, the charge was switched to constant voltage charging with a cutoff current of 0.05C, and the total charge capacity of the charging process was recorded as C2. After standing for 5 minutes, the battery was discharged to 1.5V with a current of 0.2C, and the discharge capacity was recorded as C3. The initial efficiency at 25°C was calculated using the following formula: Initial efficiency = C3 / (C1 + C2) × 100%.

[0075] (2) Cycle characteristics Under conditions of 25°C and 45°C, the prepared sodium-ion batteries were charged with a constant current of 0.2C until the voltage reached 3.9V, then charged again with a constant voltage of 3.9V until the cutoff current reached 0.05C, left for 10 minutes, and then discharged to 3.0V with a constant current of 0.5C. This procedure was repeated as a cycle, and the number of cycles until the capacity decayed to 80% of the initial cycle capacity was recorded. The measurement results are shown in Tables 1, 2, and 3.

[0076] (3)DCR DC internal resistance measurement The DC internal resistance of the prepared sodium-ion batteries was measured and calculated under conditions of 0°C, 25°C, and 45°C. The measurement procedure was as follows: The batteries were charged with a constant current of 0.2C until the voltage reached 4V, then charged with a constant voltage of 4V until the cutoff current reached 0.05C, left for 5 minutes, discharged with a current of 1C for 30 minutes, and then placed in a high / low temperature charge / discharge test chamber, set to a predetermined measurement temperature, and left for 2 hours. After that, they were discharged with a current of 2C for 10 seconds, and the voltage values ​​at the 1st second and the final second of discharge were recorded as V1 and V2, respectively. The DC internal resistance was calculated using the following formula: DCR = (V1 - V2) / 2C. The measurement results are shown in Tables 1, 2, and 3.

[0077] (4) Infiltration measurement At 25°C, the electrolyte was filled into a glove box using a pipette with a measuring range of 1-5 μL and dropped onto the positive and negative electrode pieces, respectively. The compressed density of the positive electrode material layer was 3.5 g / cm³. 3 The positive electrode material layer had a thickness of 58 μm on one side, and the positive electrode piece was a square with a side length of 55 mm. The compressed density of the negative electrode material layer was 1.65 g / cm³. 3 The negative electrode material layer had a thickness of 67 μm on one side, and the negative electrode piece was a square with a side length of 59 mm. The time required for one drop of the electrolyte prepared in the above examples and comparative examples to be completely absorbed by the electrode piece was recorded. The measurement results are shown in Tables 1, 2, and 3. Table 1 shows the measurement results for sodium-ion batteries containing the electrolyte of Group 1, Table 2 shows the measurement results for sodium-ion batteries containing the electrolyte of Group 2, and Table 3 shows the measurement results for sodium-ion batteries containing the electrolyte of Group 3.

[0078] [Table 1]

[0079] [Table 2]

[0080] [Table 3]

[0081] [Table 4]

[0082] [Table 5]

[0083] [Table 6]

[0084] [Table 7]

[0085] As can be seen from Tables 1 and 2, the electrolytes of Examples 1 to 26 exhibit high high-temperature stability. After storage at high temperatures for 24 hours, the decrease in cycle characteristics, wetting properties, initial efficiency, and DC internal resistance of sodium-ion batteries containing these electrolytes was small. As can be seen from Table 2, the maximum number of cycles reached 1570 under 25°C conditions and 1152 under 45°C conditions. In contrast, after storing the electrolytes of Comparative Examples 1 to 8 at high temperatures, the cycle characteristics, wetting properties, initial efficiency, and DC internal resistance of sodium-ion batteries containing these electrolytes all decreased significantly. Of these, the maximum number of cycles under 25°C conditions was only 1128, and the maximum number of cycles under 45°C conditions was 633. As can be seen from the above, the electrolyte of the present invention has high high-temperature storage characteristics.

[0086] As can be seen from Tables 2 and 3, the electrolytes used in Examples 1 to 26 showed no significant change in the related characteristics of the manufactured sodium-ion batteries after storage at 45°C for 24 hours and after storage at 25°C for 180 days, although they showed a slight decrease. On the other hand, the electrolytes used in Comparative Examples 1 to 8 showed a significant decrease in the related characteristics of the manufactured sodium-ion batteries after storage under the same conditions. As can be seen from this, the electrolyte of the present invention has excellent stability, can be stored in harsh environments such as high temperatures, and has a long storage life.

[0087] The above embodiments are merely for illustrating the technical solutions of the present invention and do not limit them. Although the present invention has been described in detail with reference to the embodiments described above, those skilled in the art should understand that it is still possible to modify the technical solutions described in the embodiments described above, or to make equivalent substitutions for some or all of the technical features therein. Furthermore, these modifications and substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. An electrolyte containing a sodium salt, additives and an organic solvent, The sodium salt comprises sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide. The aforementioned additive comprises 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, The electrolyte is characterized by containing, by mass percentage, 2 to 15% by weight of sodium hexafluorophosphate, 0.1 to 20% by weight of sodium bis(fluorosulfonyl)imide, and 0.1 to 5% by weight of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide, with the remainder being an organic solvent. Electrolyte.

2. The electrolyte is characterized in that the mass percentage of sodium hexafluorophosphate is 6 to 14% by weight. The electrolyte according to claim 1.

3. The electrolyte is characterized in that the mass percentage of 2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane 3,3,9,9-tetraoxide is 1 to 2% by weight. The electrolyte according to claim 1 or 2.

4. The electrolyte is characterized in that the mass percentage of bis(fluorosulfonyl)imide sodium is 2 to 8% by weight. The electrolyte according to any one of claims 1 to 3.

5. The organic solvent is characterized by containing at least one of the following: carbonates, fluorocarbonates, carboxylic acid esters, fluorocarboxylic acid esters, ethers, and fluoroethers. The electrolyte according to any one of claims 1 to 4.

6. The electrolyte further contains a sodium salt additive, The sodium salt additive is characterized by containing at least one of sodium perchlorate, sodium bis(oxalato)borate, sodium difluoro(oxalato)borate, and sodium bis(trifluoromethanesulfonyl)imide. The electrolyte according to any one of claims 1 to 5.

7. The sodium salt additive in the electrolyte is characterized by having a mass percentage of 0.01 to 1% by weight. The electrolyte according to claim 6.

8. The electrolyte further contains an organic additive, The organic additive is characterized by containing at least one of vinylethylene carbonate, fluoroethylene carbonate, vinylene carbonate, hexamethylene diisocyanate, ethynylethylene carbonate, trans-difluoroethylene carbonate, 1,3-propanesultone, 1,4-propanesultone, propa-1-ene-1,3-sultone, 1,3,2-dioxathiolan-2,2-dioxide, 4-propyl-1,3,2-dioxathiolan-2,2-dioxide, methylene methane disulfonate, 1,2-ethane disulfonic anhydride, tris(trimethylsilyl)borate, succinanitrile, ethoxy(pentafluoro)cyclotriphosphazene, tert-butylbenzene, tert-amylbenzene, fluorobenzene, and cyclohexylbenzene. The electrolyte according to any one of claims 1 to 7.

9. The organic additive in the electrolyte is characterized by having a mass percentage of 0.1 to 20% by weight. The electrolyte according to claim 8.