Lithium-ion battery

Optimized electrical conductivity ranges in the electrolyte, undercoat, and positive electrode material layers in lithium-ion batteries address safety and performance issues, reducing short circuits and improving cycle life and test results.

JP2026539308APending Publication Date: 2026-11-24SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026525240
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-19
Filing Date
2024-12-30
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Lithium-ion batteries face safety issues due to short circuits, particularly between the positive electrode current collector and negative electrode active layer, which generate excessive heat, and electrical conductivity imbalances affect charge/discharge and cycle performance.

Method used

A lithium-ion battery design with specific electrical conductivity ranges for the electrolyte, undercoat layer, and positive electrode material layer, optimized to prevent short circuits and improve cycle performance, using a primer layer and positive electrode material layer on the positive electrode current collector.

Benefits of technology

Reduces short circuit occurrences, minimizes heat generation, prevents high-temperature combustion or explosion, and enhances cycle life and nail-piercing test performance by maintaining optimal electrical conductivity levels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539308000001_ABST
    Figure 2026539308000001_ABST
Patent Text Reader

Abstract

In conventional lithium-ion batteries, high electrical conductivity makes the battery prone to short circuits, and low electrical conductivity affects the battery's electrical performance. To solve this problem, a lithium-ion battery is provided. The battery comprises a positive electrode sheet and an electrolyte, the positive electrode sheet comprising a positive electrode current collector, a primer layer, and a positive electrode material layer, the primer layer located on the surface of the positive electrode current collector, and the positive electrode material layer located on the surface of the primer layer opposite to the positive electrode current collector, and the electrical conductivity of the electrolyte, the primer layer, and the positive electrode material layer satisfy the following conditions: JPEG2026539308000024.jpg20170 Here, σ e σ is the electrical conductivity of the electrolyte, and its unit is mS / cm. a σ represents the electrical conductivity of the undercoat layer, and its unit is mS / cm. c σ represents the electrical conductivity of the positive electrode material layer, in units of mS / cm, and is the electrical conductivity of the electrolyte. e The electrical conductivity is 6.5~8.5 mS / cm, and the electrical conductivity of the undercoat layer is σ a The conductivity is 1-6 mS / cm, and the electrical conductivity of the positive electrode material layer is σ c The voltage range is 1.6 to 12.5 mS / cm. The lithium-ion battery provided by this invention helps to reduce short circuits inside the battery, improve battery cycle performance, avoid high-temperature combustion or explosion of the battery, and also improve the pass rate of the battery in nail-piercing tests.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] <Cross-reference of related applications> This application is based on a Chinese patent application filed on January 19, 2024, with application number 202410081615.5, titled "Lithium-ion battery," and claims priority therefrom. This application belongs to the technical field of lithium-ion batteries, and more specifically, relates to lithium-ion batteries. [Background technology]

[0002] As lithium-ion batteries become increasingly widely used in production and daily life, it is essential to place a high degree of emphasis on their safety during use. There are four types of short-circuit modes that can occur when a lithium-ion battery experiences a safety failure: positive electrode current collector-negative electrode active layer, positive electrode current collector-negative electrode current collector, positive electrode active layer-negative electrode current collector, and positive electrode active layer-negative electrode active layer. Of these, the short circuit between the positive electrode current collector and the negative electrode active layer is the most dangerous because it generates the highest amount of heat. To improve the safety of lithium-ion batteries, a safety coating layer is applied to the surface of the positive electrode current collector to prevent short circuits between the positive electrode current collector and the negative electrode active layer, and simultaneously convert the short circuit into a short circuit between the safety coating layer and the negative electrode current collector, and a short circuit between the safety coating layer and the negative electrode active layer. The electrical conductivity of the safety coating layer affects the magnitude of the short-circuit current and the heat generated. A safety coating layer with high electrical conductivity generates heat quickly, affecting the safety of the battery. A safety coating layer with low electrical conductivity offers high safety, but significantly inhibits electron conduction between the positive electrode active layer and the positive electrode current collector, affecting the charge / discharge and cycle performance of the lithium-ion battery. Since the positive electrode active layer has short-circuit modes with the negative electrode active layer and the negative electrode current collector, the magnitude of the electrical conductivity of the positive electrode active layer also affects the safety, charge / discharge, and cycle performance of the lithium-ion battery. High electrical conductivity of the positive electrode active layer is advantageous for lithium ion movement and electron conduction during the charge / discharge process, but it increases the short-circuit current and heat generated during a short circuit, which is detrimental to improving safety. While the low electrical conductivity of the positive electrode active layer is advantageous for reducing short-circuit current and heat generation, it affects lithium ion movement and electron conduction, impacting the charge / discharge and cycle performance of lithium-ion batteries. In addition, the electrical conductivity of the electrolyte also affects the safety, charge / discharge, and cycle performance of lithium-ion batteries. High electrical performance requirements must be met while maintaining high safety. If the electrical conductivity of the electrolyte is high, the internal resistance of the battery decreases, increasing the risk of thermal degradation due to short circuits during nail-piercing tests. On the other hand, if the electrical conductivity of the electrolyte is too low, it will affect the electrical performance of the battery. [Overview of the Initiative] [Problems that the invention aims to solve]

[0003] This invention provides a lithium-ion battery that addresses the problems in conventional lithium-ion batteries, where high electrical conductivity makes the battery prone to short circuits, and insufficient electrical conductivity affects the battery's electrical performance. [Means for solving the problem]

[0004] The technical means employed in this invention to solve the above technical problems are as follows.

[0005] The present invention provides a lithium-ion battery comprising a positive electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector, a primer layer and a positive electrode material layer, the primer layer is located on the surface of the positive electrode current collector and the positive electrode material layer is located on the surface of the primer layer opposite to the positive electrode current collector, and the electrical conductivity of the electrolyte, the electrical conductivity of the primer layer and the electrical conductivity of the positive electrode material layer are as follows: The file JPEG2026539308000002.jpg20170 satisfies the conditions, and here, σ e This is the electrical conductivity of the electrolyte, and its unit is mS / cm. σ a This represents the electrical conductivity of the undercoat layer, and its unit is mS / cm. σ c This represents the electrical conductivity of the positive electrode material layer, and its unit is mS / cm. Electrical conductivity σ of the aforementioned electrolyte e The value is 6.5-8.5 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a The temperature is 1-6 mS / cm. Electrical conductivity σ of the positive electrode material layer c The intensity is 1.6 to 12.5 mS / cm.

[0006] Selectively, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: The file JPEG2026539308000003.jpg19170 is satisfied. Selectively, the electrical conductivity of the electrolyte is 7.14 to 8.05 mS / cm. Selectively, the electrical conductivity of the undercoat layer is 1.2 to 5.5 mS / cm. Selectively, the electrical conductivity of the positive electrode material layer is 2.2 to 6.5 mS / cm.

[0007] Selectively, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: JPEG2026539308000004.jpg20170 is satisfied, the electrical conductivity σ of the electrolyte e is 7.14 to 8.05 mS / cm, the electrical conductivity σ of the undercoat layer a is 1.2 to 2.3 mS / cm, the electrical conductivity σ of the positive electrode material layer c is 3.04 to 4.5 mS / cm.

[0008] Optionally, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer satisfy the following conditions. JPEG2026539308000005.jpg20170 the electrical conductivity σ of the electrolyte e is 7.14 to 8.05 mS / cm, the electrical conductivity σ of the undercoat layer a is 1.6 to 5.5 mS / cm, the electrical conductivity σ of the positive electrode material layer c is 2.2 to 6.5 mS / cm.

[0009] Optionally, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer satisfy the following conditions. JPEG2026539308000006.jpg23170 the electrical conductivity σ of the electrolyte e is 7.14 to 8.05 mS / cm, the electrical conductivity σ of the undercoat layer a is 2.2 to 2.4 mS / cm, the electrical conductivity σ of the positive electrode material layer c is 3.04 to 4.5 mS / cm.

[0010] Optionally, the undercoat layer includes a first active material and an inorganic filler, the positive electrode material layer includes a second active material, a proportion of the mass of the first active material in the undercoat layer is 0% to 98%, a proportion of the inorganic filler in the undercoat layer is 0% to 98%, and a proportion of the mass of the second active material in the positive electrode material layer is 95% to 98.5%.

[0011] Selectively, the inorganic filler comprises one or more of aluminum oxide, magnesium oxide, and calcium carbonate. [Effects of the Invention]

[0012] The lithium-ion battery provided by the present invention has an electrical conductivity of 6.5 to 8.5 mS / cm for the electrolyte, an electrical conductivity of 1 to 6 mS / cm for the undercoat layer, and an electrical conductivity of 1.6 to 12.5 mS / cm for the positive electrode material layer, and all three of the above electrical conductivity values ​​are related by the formula If the conditions in JPEG2026539308000007.jpg19170 are met, the occurrence of short circuits in lithium-ion batteries can be effectively reduced, and the battery's cycle performance can be improved at the same time. Short circuits where the positive electrode current collector and the negative electrode active material layer are in direct contact have the highest heat generation rate and adversely affect the safety of lithium-ion batteries. Therefore, by providing the undercoat layer and the positive electrode material layer on the positive electrode sheet, and by ensuring that the electrical conductivity of both satisfies a specific numerical range in the above relational expression, the short circuit situation in batteries caused by excessively fast heat generation rates at high electrical conductivity, and the adverse effects of excessively low electrical conductivity on the battery's cycle performance can be improved. The electrical conductivity of the electrolyte also affects the safety and cycle performance of the battery. As a result of numerous tests on the electrical conductivity of the electrolyte, the inventors found that when the electrical conductivity of the electrolyte is in the range of 6.5 to 8.5 mS / cm and similarly satisfies the above relational expression, the occurrence of short circuits in the corresponding lithium-ion batteries is mitigated, and the cycle performance is effectively improved. Based on the above, when the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer of the present invention satisfy the above relationship, the probability of short circuits occurring inside the lithium-ion battery can be effectively reduced, thereby reducing heat generation in the battery, avoiding high-temperature combustion or explosion of the lithium-ion battery, improving the battery's cycle life, and also being advantageous in improving the pass rate of the lithium-ion battery in the nail-piercing test. [Modes for carrying out the invention]

[0013] To further clarify the technical problems, technical means, and beneficial effects that this invention aims to solve, the invention will be described in more detail below with reference to examples. Please understand that the specific examples described herein are merely for illustrative purposes and do not limit the invention.

[0014] The present invention provides a lithium-ion battery comprising a positive electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector, a primer layer and a positive electrode material layer, the primer layer is located on the surface of the positive electrode current collector and the positive electrode material layer is located on the surface of the primer layer opposite to the positive electrode current collector, and the electrical conductivity of the electrolyte, the electrical conductivity of the primer layer and the electrical conductivity of the positive electrode material layer are as follows: The condition JPEG2026539308000008.jpg21170 is satisfied. Here, σ e This is the electrical conductivity of the electrolyte, and its unit is mS / cm. σ a This represents the electrical conductivity of the undercoat layer, and its unit is mS / cm. σ c This represents the electrical conductivity of the positive electrode material layer, and its unit is mS / cm. Electrical conductivity σ of the aforementioned electrolyte e The value is 6.5-8.5 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a The temperature is 1-6 mS / cm. Electrical conductivity σ of the positive electrode material layer c The intensity is 1.6 to 12.5 mS / cm.

[0015] Specifically, the lithium-ion battery provided by the present invention has an electrical conductivity of 6.5 to 8.5 mS / cm for the electrolyte, an electrical conductivity of 1 to 6 mS / cm for the undercoat layer, and an electrical conductivity of 1.6 to 12.5 mS / cm for the positive electrode material layer, and all three of the above electrical conductivity values ​​are related by the formula If the conditions in JPEG2026539308000009.jpg18170 are met, the occurrence of short circuits in lithium-ion batteries can be effectively reduced, and the battery's cycle performance can be improved at the same time. Short circuits where the positive electrode current collector and the negative electrode active material layer are in direct contact have the highest heat generation rate and adversely affect the safety of lithium-ion batteries. Therefore, by providing the undercoat layer and the positive electrode material layer on the positive electrode sheet, and by ensuring that the electrical conductivity of both satisfies a specific numerical range in the above relational expression, the short circuit situation in batteries caused by excessively fast heat generation rates at high electrical conductivity, and the adverse effects of excessively low electrical conductivity on the battery's cycle performance can be improved. The electrical conductivity of the electrolyte also affects the safety and cycle performance of the battery. As a result of numerous tests on the electrical conductivity of the electrolyte, the inventors found that when the electrical conductivity of the electrolyte is in the range of 6.5 to 8.5 mS / cm and similarly satisfies the above relational expression, the occurrence of short circuits in the corresponding lithium-ion batteries is mitigated, and the cycle performance is effectively improved. Based on the above, when the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer of the present invention satisfy the above relationship, the probability of short circuits occurring inside the lithium-ion battery is effectively reduced, thereby reducing heat generation in the battery, avoiding high-temperature combustion or explosion of the lithium-ion battery, improving the battery's cycle life, and also being advantageous in improving the pass rate of the lithium-ion battery in the nail-piercing test.

[0016] In some embodiments, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: The file JPEG2026539308000010.jpg24170 is satisfied.

[0017] By further limiting the electrical conductivity of the electrolyte, the undercoat layer, and the positive electrode material layer to satisfy the above conditions, it is possible to effectively reduce the probability of short circuits occurring inside the lithium-ion battery and achieve the objective of improving the battery's cycle performance, which is also advantageous for improving the pass rate in the nail-piercing test of lithium-ion batteries.

[0018] In specific embodiments, the electrical conductivity of the electrolyte can be 6.5 mS / cm, 7.0 mS / cm, 7.14 mS / cm, 7.2 mS / cm, 7.4 mS / cm, 7.6 mS / cm, 7.8 mS / cm, 7.9 mS / cm, 8.0 mS / cm, 8.02 mS / cm, 8.03 mS / cm, 8.05 mS / cm, 8.07 mS / cm, or 8.5 mS / cm.

[0019] In a preferred embodiment, the electrical conductivity of the electrolyte is 7.14 to 8.05 mS / cm.

[0020] In specific embodiments, the electrical conductivity of the undercoat layer can be 1.0 mS / cm, 1.2 mS / cm, 1.4 mS / cm, 1.6 mS / cm, 1.8 mS / cm, 2.0 mS / cm, 2.3 mS / cm, 2.5 mS / cm, 2.7 mS / cm, 3.0 mS / cm, 3.2 mS / cm, 3.4 mS / cm, 3.6 mS / cm, 3.8 mS / cm, 4.2 mS / cm, 4.4 mS / cm, 4.6 mS / cm, 5.0 mS / cm, 5.2 mS / cm, 5.5 mS / cm, or 6.0 mS / cm.

[0021] In a preferred embodiment, the electrical conductivity of the undercoat layer is 1.2 to 5.5 mS / cm.

[0022] By applying a coating layer to the surface of the positive electrode current collector, short circuits between the positive electrode current collector and the negative electrode active material layer can be prevented. The electrical conductivity of the coating layer also affects the safety, charge / discharge performance, and cycle performance of the lithium-ion battery. A coating layer with high electrical conductivity generates heat quickly, which affects the safety of the battery. A coating layer with low electrical conductivity offers high safety, but it significantly inhibits electron conduction between the positive electrode active layer and the positive electrode current collector, affecting the charge / discharge and cycle performance of the lithium-ion battery.

[0023] In specific embodiments, the electrical conductivity of the positive electrode material layer can be 2.0 mS / cm, 2.2 mS / cm, 2.3 mS / cm, 2.6 mS / cm, 3.1 mS / cm, 3.5 mS / cm, 4.0 mS / cm, 4.6 mS / cm, 5.0 mS / cm, 5.5 mS / cm, 6.0 mS / cm, 6.5 mS / cm, or 7.0 mS / cm.

[0024] In a preferred embodiment, the electrical conductivity of the positive electrode material layer is 2.2 to 6.5 mS / cm.

[0025] In some embodiments, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: The file JPEG2026539308000011.jpg19170 is satisfied. Electrical conductivity σ of the aforementioned electrolyte e The values ​​are 7.14-8.05 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a It is 1.2~2.3 mS / cm, Electrical conductivity σ of the positive electrode material layer c The value is 3.04-4.5 mS / cm.

[0026] Furthermore, the inventors have verified through experiments that when the lithium-ion battery simultaneously satisfies the above-mentioned limiting conditions and setting parameters, it effectively reduces the probability of short circuits occurring inside the lithium-ion battery, reduces heat generation in the battery, avoids high-temperature combustion or explosion of the lithium-ion battery, and consequently enhances the effectiveness of the lithium-ion battery in nail-piercing tests.

[0027] In some embodiments, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: Satisfy the requirements of JPEG2026539308000012.jpg23170. Electrical conductivity σ of the aforementioned electrolyte e The values ​​are 7.14-8.05 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer aThe values ​​are 1.6 to 5.5 mS / cm. Electrical conductivity σ of the positive electrode material layer c The value is 2.2 to 6.5 mS / cm.

[0028] Furthermore, if the electrical conductivity of the undercoat layer and the positive electrode material layer is relatively low or relatively high, it is also detrimental to improving the safety and cycle performance of the battery. As a result of numerous experimental studies conducted in the previous period, the inventors have proven that when the electrical conductivity of the electrolyte, the undercoat layer, and the positive electrode material layer in the lithium-ion battery are within the above range, the cycle retention rate of the corresponding lithium-ion battery is effectively improved, that is, lithium-ion batteries under the above limiting conditions and parameter settings have superior cycle performance.

[0029] In some embodiments, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: The file JPEG2026539308000013.jpg21170 is satisfied. Electrical conductivity σ of the aforementioned electrolyte e The values ​​are 7.14-8.05 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a It is 2.2~2.4 mS / cm, Electrical conductivity σ of the positive electrode material layer c The value is 3.04-4.5 mS / cm.

[0030] Furthermore, after numerous experimental verifications in the preceding period, it has been found that when the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer of the lithium-ion battery are within the above numerical range, the nail-piercing test pass rate and cycle retention rate of the corresponding lithium-ion battery improve. In other words, when the parameter settings of the lithium-ion battery simultaneously satisfy the above-mentioned limiting conditions and relational formulas of this application, the nail-piercing test pass rate and cycle performance of the lithium-ion battery are simultaneously improved.

[0031] In some embodiments, the thickness of the undercoat layer is 3 to 8 μm.

[0032] The thickness of the primer layer affects the distance electrons travel within the coating. A thin primer layer shortens the electron conduction distance, resulting in improved electrical conductivity. Conversely, if the primer layer is excessively thick, it becomes difficult for current to pass through the coating, leading to a decrease in electrical conductivity.

[0033] Through numerous experimental measurements in the preceding period, the inventor confirmed that when the thickness of the undercoat layer is 3 to 8 μm, the electrical conductivity of the positive electrode material layer satisfies the above-mentioned relational equation.

[0034] In some embodiments, the undercoat layer comprises a first active material and an inorganic filler, the cathode material layer comprises a second active material, the proportion of the mass of the first active material to the undercoat layer is 0% to 98%, the proportion of the inorganic filler to the undercoat layer is 0% to 98%, and the proportion of the mass of the second active material to the cathode material layer is 95% to 98.5%.

[0035] In some embodiments, the electrical conductivity (σ) of the undercoat layer a ) is the electrical conductivity (σ) of the positive electrode material layer. c ) is smaller than, i.e., σ a <σ c That is the case.

[0036] Furthermore, the undercoat layer contains the aforementioned inorganic filler, and theoretically, the electrical conductivity of the undercoat layer is lower than that of the positive electrode material layer. An undercoat layer with high electrical conductivity generates heat quickly, which affects the safety of the battery. Therefore, in this invention, adding an inorganic filler to the undercoat layer is advantageous in improving the safety of lithium-ion batteries.

[0037] This point should be recognized from the description of the "safety coating layer" in the technical specifications and from the specific examples provided. This point refers to the difference between the undercoat layer and the cathode material layer. By defining this point, the undercoat layer and the normal cathode material layer can be clearly distinguished.

[0038] In some embodiments, the first active material and the second active material include one or more of lithium iron phosphate, lithium cobaltate, lithium manganeseate, and nickel-cobalt-lithium manganeseate ternary materials.

[0039] In some embodiments, the inorganic filler includes one or more of aluminum oxide, magnesium oxide, and calcium carbonate.

[0040] Furthermore, the undercoat layer and the positive electrode material layer further contain a positive electrode binder and a positive electrode conductive agent. The undercoat layer is obtained by co-mixing the positive electrode binder, the positive electrode conductive agent and the first active material, and the positive electrode material layer is obtained by co-mixing the positive electrode binder, the positive electrode conductive agent and the second active material.

[0041] The positive electrode binder includes at least one of the following: polyvinylidene fluoride, vinylidene fluoride copolymer, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-fluoroethylene copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, and styrene-butadiene rubber.

[0042] The positive electrode conductive agent includes at least one of conductive carbon black, conductive graphite, conductive carbon fiber, carbon nanotube, graphene, and reduced graphene oxide.

[0043] In some embodiments, the positive electrode sheet further includes a positive electrode current collector, the positive electrode current collector being aluminum foil.

[0044] In some embodiments, the lithium-ion battery further includes a separator and a negative electrode sheet, wherein the separator is positioned between the positive electrode sheet and the negative electrode sheet to form the lithium-ion battery.

[0045] The negative electrode sheet further includes a negative electrode coating, the negative electrode coating includes a negative electrode active material, and the negative electrode active material includes one or more of the following: a carbon-based negative electrode, a silicon-based negative electrode, and a lithium negative electrode.

[0046] The carbon-based anode is selected from at least one of graphite, hard carbon, soft carbon, graphene, and mesocarbon microbeads; the silicon-based anode is selected from at least one of silicon material, silicon oxide, silicon-carbon composite material, and silicon alloy material; and the lithium anode is specifically selected from metallic lithium or lithium alloy.

[0047] Specifically, when the lithium-ion battery is formed using the positive electrode sheet, the negative electrode sheet, and the separator, and the relational expression described in this application is satisfied, the probability of a short circuit occurring inside the lithium-ion battery can be effectively reduced, thereby reducing heat generation in the battery, avoiding high-temperature combustion or explosion of the lithium-ion battery, improving the battery's cycle life, and also being advantageous in improving the pass rate of the lithium-ion battery in nail penetration tests and screw pressing tests.

[0048] The present invention will be described in more detail below with reference to examples.

[0049] JPEG2026539308000014.jpg128170

[0050] Example 1 This embodiment is intended to illustrate the lithium-ion battery and method for manufacturing the same disclosed in the present invention, and includes the following steps.

[0051] Manufacturing of positive electrode sheets A predetermined weight of binder PVDF, conductive agent SuperP, CNT, and lithium iron phosphate are added to NMP solvent, and the mixture is thoroughly stirred to obtain a primer layer slurry. The electrical conductivity of the primer layer is 2.3 mS / cm. A predetermined weight of binder PVDF, conductive agent SuperP, CNT, and lithium cobalt oxide are added to NMP solvent, and the mixture is thoroughly stirred to obtain a positive electrode material layer slurry. The electrical conductivity of the positive electrode material layer is 3.04 mS / cm. The primer layer slurry is uniformly applied onto the positive electrode current collector, then the positive electrode material layer slurry is applied to the surface of the first coated slurry, and the positive electrode sheet is obtained through drying, roll pressing, and slitting.

[0052] Manufacturing of negative electrode sheets Take graphite, conductive carbon, sodium carboxymethylcellulose, and styrene-butadiene rubber (in mass ratio), first add sodium carboxymethylcellulose to pure water and stir thoroughly until homogenized, then add conductive carbon and stir thoroughly until homogenized, then add graphite and stir thoroughly until homogenized to obtain the desired negative electrode slurry. The manufactured negative electrode slurry is uniformly applied onto the negative electrode current collector, and then dried, roll-pressed, and slit to obtain a negative electrode sheet.

[0053] Manufacturing of electrolyte Ethylene carbonate, diethyl carbonate, and ethylmethyl carbonate are mixed to obtain an organic solvent, a lithium salt is dissolved in the organic solvent, and after uniform mixing, an electrolyte is obtained, the electrical conductivity of the electrolyte is 8.05 mS / cm.

[0054] Manufacturing of lithium-ion batteries A separator is placed between the positive electrode sheet and the negative electrode sheet, and tabs are welded to the positive and negative electrode positions, respectively. A bare cell is manufactured by a winding or lamination process. The bare cell is placed in a battery case, the electrolyte is injected and sealed, and after standing, heat pressing, and chemical conversion processes, a lithium-ion battery is obtained.

[0055] Examples 2-8 Examples 2 to 8 are intended to illustrate the lithium-ion battery and method for manufacturing the same disclosed in the present invention, and include most of the operations of Example 1, with the following differences. The electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer, as well as the values ​​of the related formulas in Examples 2 to 8, are specifically in accordance with the parameters set in Examples 2 to 8 in Table 1.

[0056] Comparative Examples 1-14 Comparative Examples 1 to 14 are provided to illustrate the lithium-ion battery and its manufacturing method disclosed in the present invention, and include most of the operations of Example 1, with the following differences. The electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer in Comparative Examples 1 to 14 are specifically those listed in Comparative Examples 1 to 14 in Table 1.

[0057] Performance testing The following performance tests were performed on Examples 1-8 and Comparative Examples 1-14, which were manufactured as described above.

[0058] Test method for electrical conductivity The pole pieces were cut into 6cm x 10cm rectangles, placed flat in a jig, and the jig was placed in an IESTBER1300 pole piece resistance meter. The test was performed under a pressure of 25MPa, with a holding time of 15s, a temperature of 25℃, and a humidity of 70%RH.

[0059] Method for testing lithium-ion batteries by nail penetration: Using the BE9002CY battery nail penetration tester, a fully charged battery is placed in the device, and a 3mm diameter steel nail is driven into the geometric center of the cell plane at a speed of 15mm / s until the entire battery is penetrated. After nail penetration, the steel nail is held inside the battery for 30 seconds before being withdrawn.

[0060] Room temperature cycling performance test The sodium-ion battery after chemical formation is placed at room temperature (25°C ± 3°C), charged to 3.9V with a constant current of 1C, then charged again with a constant voltage of 3.9V, with a cutoff current of 0.05C, and discharged to 1.5V with a constant current of 1C. This cycle is repeated 1000 times. The following formula is used to calculate the capacity retention rate after 1000 cycles at 25°C: Capacity retention rate (%) after 1000 cycles at 25°C = Discharge capacity at 1000 cycles / Discharge capacity at 1 cycle × 100%.

[0061] Enter the test results in Table 2.

[0062] JPEG2026539308000015.jpg151170

[0063] As can be seen from the test results in Table 2, the sodium-ion batteries manufactured using the parameters set in Examples 1 to 8 generally showed better nail-piercing pass rates and room-temperature cycle capacity retention rates than Comparative Examples 1 to 14. As can be seen from the test results of Examples 1 to 8 and Comparative Examples 1 to 14, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are conditions The conditions for JPEG2026539308000016.jpg19170 are met, and the electrical conductivity of the electrolyte is σ e The electrical conductivity of the undercoat layer is 6.5~8.5 mS / cm, and the electrical conductivity of the undercoat layer is σ a The electrical conductivity of the positive electrode material layer is 1-6 mS / cm, and the electrical conductivity of the positive electrode material layer is σ c When the conductivity is between 1.6 and 12.5 mS / cm, it is advantageous in improving the adverse effects on battery cycle performance due to short-circuit conditions and excessively low electrical conductivity, thereby mitigating the occurrence of short circuits in the corresponding lithium-ion battery and effectively improving cycle performance. Furthermore, in Example 7, the electrical conductivity of the undercoat layer and the positive electrode material layer were generally lower compared to the other examples, and in Example 8, the electrical conductivity values ​​of the undercoat layer and the positive electrode material layer were high. Since relatively low or relatively high electrical conductivity of the undercoat layer and the positive electrode material layer is also disadvantageous in improving battery safety and cycle performance, the overall test results of Examples 7 and 8 are somewhat inferior to those of the other examples.

[0064] As can be seen by comparing the test results of Examples 1-8 and Comparative Examples 1-14, in Comparative Examples 1-3, the electrical conductivity of the undercoat layer and JPEG2026539308000017.jpg18170 does not meet the range limitations, and in Comparative Examples 4-13, the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, the electrical conductivity of the positive electrode material layer, and One or more of the elements in JPEG2026539308000018.jpg18170 do not satisfy the range limitations. Under these conditions, all of them are detrimental to improving the battery's cycle performance and short-circuit conditions. Therefore, when the electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer simultaneously satisfy the numerical values ​​and relational formulas within the limit range of this application, it is possible to effectively reduce the probability of short circuits occurring inside the lithium-ion battery, reduce heat generation in the battery, avoid high-temperature combustion or explosion of the lithium-ion battery, and improve the battery's cycle performance.

[0065] The foregoing are merely preferred embodiments of the present invention and do not limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall all be within the scope of protection of the present invention.

Claims

1. Lithium-ion battery, The positive electrode sheet comprises a positive electrode sheet and an electrolyte, the positive electrode sheet comprising a positive electrode current collector, a primer layer and a positive electrode material layer, the primer layer located on the surface of the positive electrode current collector, the positive electrode material layer located on the surface of the primer layer opposite to the positive electrode current collector, and the electrical conductivity of the electrolyte, the electrical conductivity of the primer layer and the electrical conductivity of the positive electrode material layer are as follows: Satisfying the conditions, here, σ e This is the electrical conductivity of the electrolyte, and its unit is mS / cm. σ a This represents the electrical conductivity of the undercoat layer, and its unit is mS / cm. σ c This represents the electrical conductivity of the positive electrode material layer, and its unit is mS / cm. Electrical conductivity σ of the aforementioned electrolyte e The values ​​are 6.5 to 8.5 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a The temperature range is 1 to 6 mS / cm. Electrical conductivity σ of the positive electrode material layer c A lithium-ion battery characterized by having a capacitance of 1.6 to 12.5 mS / cm.

2. The electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: A lithium-ion battery according to claim 1, characterized in that it satisfies the requirements.

3. The lithium-ion battery according to claim 1, characterized in that the electrical conductivity of the electrolyte is 7.14 to 8.05 mS / cm.

4. The lithium-ion battery according to claim 1, characterized in that the electrical conductivity of the undercoat layer is 1.2 to 5.5 mS / cm.

5. The lithium-ion battery according to claim 1, characterized in that the electrical conductivity of the positive electrode material layer is 2.2 to 6.5 mS / cm.

6. The electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: Satisfying the conditions, Electrical conductivity σ of the aforementioned electrolyte e The values ​​were 7.14–8.05 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a The value is 1.2–2.3 mS / cm. The electrical conductivity σ of the positive electrode material layer c The lithium-ion battery according to claim 1, characterized in that it is 3.04 to 4.5 mS / cm.

7. The electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: Satisfying the conditions, Electrical conductivity σ of the aforementioned electrolyte e The values ​​were 7.14–8.05 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a The values ​​are 1.6 to 5.5 mS / cm. Electrical conductivity σ of the positive electrode material layer c The lithium-ion battery according to claim 1, characterized in that the current is 2.2 to 6.5 mS / cm.

8. The electrical conductivity of the electrolyte, the electrical conductivity of the undercoat layer, and the electrical conductivity of the positive electrode material layer are as follows: Satisfying the conditions, Electrical conductivity σ of the aforementioned electrolyte e The values ​​were 7.14–8.05 mS / cm. Electrical conductivity σ of the aforementioned undercoat layer a The value is 2.2–2.4 mS / cm. Electrical conductivity σ of the positive electrode material layer c The lithium-ion battery according to claim 1, characterized in that the current is 3.04 to 4.5 mS / cm.

9. The lithium-ion battery according to claim 1, characterized in that the undercoat layer comprises a first active material and an inorganic filler, the positive electrode material layer comprises a second active material, the proportion of the mass of the first active material to the undercoat layer is 0% to 98%, the proportion of the inorganic filler to the undercoat layer is 0% to 98%, and the proportion of the mass of the second active material to the positive electrode material layer is 95% to 98.5%.

10. The lithium-ion battery according to claim 9, characterized in that the inorganic filler includes one or more of aluminum oxide, magnesium oxide, and calcium carbonate.