Negative electrode active material, negative electrode containing the same, and secondary battery

A negative electrode active material with controlled nitrogen, oxygen, and hydrogen content in artificial graphite particles addresses surface peeling and side reactions, maintaining discharge capacity and efficiency in lithium ion batteries.

JP2026539321APending Publication Date: 2026-11-24LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026526369
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-12-18
Filing Date
2024-12-18
Publication Date
2026-11-24

Smart Images

  • Figure 2026539321000001_ABST
    Figure 2026539321000001_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode active material. Specifically, the negative electrode active material comprises artificial graphite particles and nitrogen, oxygen, and hydrogen elements present on the surface, inside, or both on the surface and inside the artificial graphite particles, wherein the nitrogen content is 80 mg to 180 mg per kilogram of the negative electrode active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative electrode active material, a negative electrode including the same, and a secondary battery.

Background Art

[0002] As interest in environmental issues has increased, research has been conducted on electric vehicles (EVs), hybrid electric vehicles (HEVs), and the like, which can replace vehicles using fossil fuels, such as gasoline vehicles and diesel vehicles, which are one of the main causes of air pollution. As a power source for such electric vehicles (EVs), hybrid electric vehicles (HEVs), and the like, secondary batteries for electric vehicles are used, and currently, as commercialized secondary batteries for electric vehicles, there are nickel cadmium batteries, nickel hydrogen batteries, nickel zinc batteries, lithium ion batteries, and the like. Among these secondary batteries for electric vehicles, lithium ion batteries have little memory effect compared to nickel-based batteries, are free to charge and discharge, have a low self-discharge rate, and have high energy density, high discharge voltage, and output stability. Various studies have been conducted due to the advantages of exhibiting properties.

Summary of Invention

Problem to be Solved by the Invention

[0003] One object of the present invention is to prevent a decrease in discharge capacity and prevent surface peeling of an artificial graphite-based negative electrode active material and a problem of a side reaction of an electrolyte resulting therefrom, thereby improving initial efficiency and maintaining discharge capacity. An object of the present invention is to provide a negative electrode active material capable of exhibiting an effect and having improved rapid charging performance.

[0004] In addition, another object of the present invention is to provide a negative electrode including the above negative electrode active material.

[0005] In addition, another object of the present invention is to provide a lithium secondary battery including the above negative electrode. Means for Solving the Problem

[0006] [1] The present invention provides a negative electrode active material comprising artificial graphite particles and nitrogen, oxygen, and hydrogen elements present on the surface, inside, or on the surface and inside of the artificial graphite particles, wherein the nitrogen element is present in an amount of 80 mg to 180 mg per kg of the negative electrode active material.

[0007] [2] The present invention provides a negative electrode active material in which, in the present invention, the oxygen element is contained in an amount of 650 mg to 1,000 mg per 1 kg of the negative electrode active material, and the hydrogen element is contained in an amount of 300 mg to 500 mg per 1 kg of the negative electrode active material.

[0008] [3] The present invention provides a negative electrode active material in which, in any one or more of the above [1] to [2], the ratio of the weight of nitrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material is 0.12 or more.

[0009] [4] The present invention provides a negative electrode active material in which, in any one or more of the above [1] to [3], the ratio of the weight of hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material is 0.47 or more.

[0010] [5] The present invention provides a negative electrode active material in which, in any one or more of the above [1] to [4], the ratio of the total weight of nitrogen and hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material is 0.5 or more.

[0011] [6] The present invention provides a negative electrode active material in which, in any one or more of the above [1] to [5], the total weight of nitrogen, oxygen, and hydrogen elements present in the negative electrode active material is 1,000 mg to 1,600 mg per 1 kg of the negative electrode active material.

[0012] [7] The present invention provides a negative electrode active material in which, in any one or more of the above [1] to [6], the artificial graphite particles are in the form of secondary particles formed by granulating two or more primary particles.

[0013] [8] The present invention provides a negative electrode active material in which, in any one or more of the above [1] to [7], the degree of graphitization of the negative electrode active material is 90% to 99%.

[0014] [9] In the present invention, in any one or more of the above [1] to [8], the BET specific surface area of ​​the negative electrode active material is 1 m² 2 / g~8m 2 We provide a negative electrode active material with a value of / g.

[0015]

[10] The present invention provides a negative electrode active material in any one or more of the above [1] to [9], wherein the negative electrode active material further comprises an amorphous carbon coating layer located on the artificial graphite particles.

[0016]

[11] The present invention provides a negative electrode comprising a negative electrode active material according to one or more of the above [1] to

[10] .

[0017]

[12] The present invention also provides a lithium secondary battery comprising a negative electrode according to

[11] , a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and a non-aqueous electrolyte. [Effects of the Invention]

[0018] The negative electrode active material according to the present invention comprises artificial graphite particles and elements of nitrogen, oxygen, and hydrogen. The elements of nitrogen, oxygen, and hydrogen may be present in or doped into the artificial graphite particles. The elements of nitrogen are present in the negative electrode active material in a specific amount. The range of nitrogen content present in the negative electrode active material can be interpreted as an indicator of the degree of graphitization of the surface of the negative electrode active material. The present invention makes it possible to lower the degree of graphitization of the surface of the negative electrode active material to an appropriate level by adjusting the nitrogen content present in the negative electrode active material to a specific range. As a result, the negative electrode active material according to the present invention can prevent or suppress peeling phenomena caused by organic solvents contained in non-aqueous electrolytes, and can exhibit the desired level of discharge capacity. [Brief explanation of the drawing]

[0019] The following drawings accompanying this specification illustrate embodiments of the present invention and, together with the detailed description of the invention described later, serve to further illustrate the technical concept of the present invention. The present invention should not be construed as being limited solely to the matters described in such drawings.

[0020] [Figure 1] This is a flowchart illustrating the manufacturing process of the negative electrode active material according to one embodiment of the present invention. [Modes for carrying out the invention]

[0021] The terms and words used herein and in the claims should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather in a manner consistent with the technical idea of ​​the present invention, in accordance with the principle that inventors may define the concepts of terms as appropriate to best describe their invention.

[0022] The terms used herein are for illustrative purposes only and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise.

[0023] In this specification, terms such as “include,” “equip,” or “have” indicate the presence of implemented features, figures, steps, components, or combinations thereof, and should be understood not to preclude the existence or possibility of adding one or more different features, figures, steps, components, or combinations thereof.

[0024] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50The particle size can be measured, for example, using the laser diffraction method. This laser diffraction method can generally measure particle sizes from the submicron region to several millimeters in size, and can yield highly reproducible and high-resolution results.

[0025] In this specification, "primary particle" means a single particle, and "secondary particle" means an aggregate formed by the aggregation of multiple primary particles through an intentional granulation or bonding process.

[0026] As used herein, “approximately,” “essentially,” and “substantially” are used to mean a range of numerical values ​​or degrees, or something close thereto, in light of inherent manufacturing and material tolerances.

[0027] A lithium secondary battery is composed of a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode and negative electrode are manufactured by mixing positive electrode active material and negative electrode active material with a binder, etc., dispersing them in a solvent to produce a slurry, applying the slurry to the surface of an electrode current collector, and drying it to form an electrode active material layer.

[0028] As the negative electrode active material, carbon-based active materials can be used that allow for reversible insertion and removal of lithium ions while maintaining structural and electrical properties. Various forms of carbon-based materials are used as carbon-based active materials, including artificial graphite, natural graphite, and hard carbon. Among these, graphite-based active materials are widely used because their excellent reversibility ensures the lifespan characteristics of lithium secondary batteries. Since graphite-based active materials have a relatively low discharge voltage of -0.2V compared to lithium, batteries using graphite-based active materials can exhibit a high discharge voltage of, for example, around 3.6V, providing many advantages in terms of energy density for lithium batteries.

[0029] Among carbon-based active materials, artificial graphite has advantages over natural graphite in that it exhibits a relatively lower degree of orientation during electrode rolling and good lithium ion ingress and egress characteristics, resulting in superior rapid charging performance, lower expansion due to charging and discharging, and excellent lifespan characteristics. Artificial graphite is produced by heat-treating amorphous carbon such as coke at high temperatures (e.g., 2,500°C to 3,200°C) and is distinguished from natural graphite by being artificially synthesized. Such artificial graphite has a high degree of graphitization due to the aforementioned high-temperature heat treatment, and there is a problem that its surface peels off upon contact with organic solvents (e.g., ethyl methyl carbonate) in the non-aqueous electrolyte. Such surface peeling of artificial graphite can cause various problems, such as increased side reactions of the electrolyte, low initial efficiency, loss of energy density, and gas generation. On the other hand, if the degree of graphitization of artificial graphite is excessively reduced in order to prevent or suppress such problems, the capacity itself may decrease.

[0030] The present invention will be described in detail below.

[0031] <Negative electrode active material> The present invention relates to a negative electrode active material, for example, a negative electrode active material for lithium secondary batteries.

[0032] The negative electrode active material comprises artificial graphite particles and nitrogen (N), oxygen (O), and hydrogen (H) elements present on the surface, inside, or on the surface and inside the artificial graphite particles, wherein the nitrogen element is present in an amount of approximately 80 mg to 180 mg per 1 kg of the negative electrode active material.

[0033] The negative electrode active material according to the present invention comprises artificial graphite particles and elements of nitrogen, oxygen, and hydrogen. The elements of nitrogen, oxygen, and hydrogen may be present in the artificial graphite particles or may be doped into them. The elements of nitrogen are present in the negative electrode active material in a specific amount. The range of nitrogen content present in the negative electrode active material can be interpreted as an indicator of the degree of graphitization of the surface of the negative electrode active material, and the present invention makes it possible to lower the degree of graphitization of the surface of the negative electrode active material to an appropriate level by adjusting the nitrogen content present in the negative electrode active material to a specific range. As a result, the negative electrode active material according to the present invention can prevent or suppress peeling phenomena caused by organic solvents contained in non-aqueous electrolytes, and can exhibit the desired level of discharge capacity.

[0034] Generally, graphite can be artificially produced through a series of complex processes that transform raw materials into a highly orderly crystalline structure. For example, to produce such artificial graphite, coke and graphite are crushed and mixed with a binder (e.g., pitch) to form a homogeneous mass. This mixture can then be shaped using techniques such as isotropic pressing, extrusion, or die molding. The shaped material then undergoes a carbonization process in an oxygen-free environment at approximately 1000°C. In the next step, graphitization, the material is heat-treated in an inert atmosphere to a temperature of approximately 2,500°C to 3,200°C, thereby partially or completely converting amorphous or non-crystalline carbon into graphite. The graphitization process in such artificial graphite production is the main step of the carbon-graphite process. For example, the high-temperature treatment in the graphitization process aligns the carbon atoms into the characteristic layered structure of graphite, improving properties such as strength and conductivity. The degree of graphitization is a measure of how closely a material resembles a hexagonal graphite crystal structure, where carbon atoms are densely packed together. An ideal graphite crystal structure exhibits a dense arrangement of hexagons with lattice constants a=0.2461 nm and c=0.6708 nm. Generally, the closer the lattice dimensions are to the ideal graphite lattice constants, the higher the degree of graphitization is considered to be.

[0035] The negative electrode active material includes artificial graphite particles. These artificial graphite particles are produced by heat-treating amorphous carbon at high temperatures (e.g., 2,500°C to 3,200°C) and are distinguished from natural graphite by being artificially synthesized.

[0036] The artificial graphite particles may be in the form of primary particles, or in the form of secondary particles formed by granulating two or more primary particles. For example, the artificial graphite particles may be in the form of secondary particles formed by granulating two or more primary particles. The primary particles contained in the artificial graphite particles may mean artificial graphite in the form of primary particles.

[0037] When the artificial graphite particles are in a secondary particle form, voids can be formed within the artificial graphite particles, and these voids may be empty spaces formed between primary particles, amorphous, or two or more voids may exist.

[0038] If the artificial graphite particles are in secondary particle form, they can be produced by mixing primary particle-form artificial graphite particles with a binder substance (e.g., pitch), mechanically milling, molding or spheroidizing them, and heat-treating them to aggregate the primary particle-form artificial graphite particles into secondary particles. Alternatively, if the artificial graphite particles are in secondary particle form, they can be produced by mixing a carbon precursor and a binder substance, performing mechanical milling (or molding) and granulation steps to produce an intermediate in secondary particle form, and heat-treating the intermediate at a temperature of 3,000°C or higher to graphitize it. Here, the carbon precursor may be coal-based heavy oil, petroleum-based heavy oil, tar, pitch, coke, etc., and may be at least one selected from the group consisting of, for example, needle coke, mosaic coke, and coal tar pitch. The production method is not particularly limited as long as it satisfies the range of nitrogen element content present in the negative electrode active material.

[0039] The negative electrode active material may include nitrogen, oxygen, and hydrogen elements present on, inside, or both on the surface and inside the artificial graphite particles. In one embodiment, the nitrogen, oxygen, and hydrogen elements may be doped into the artificial graphite particles.

[0040] In the present invention, the nitrogen element content in the artificial graphite particles may be about 80 mg to 180 mg per 1 kg of the negative electrode active material.

[0041] The nitrogen, oxygen, and hydrogen elements may be introduced into or present in the artificial graphite particles during the manufacturing process, for example, during processes such as crushing, mechanical milling, and granulation. Typically, during the manufacturing process of the artificial graphite particles, for example, during the graphitization process, the nitrogen elements are removed or present at low levels. On the other hand, if the graphitization of the artificial graphite is carried out sufficiently, the nitrogen content in the artificial graphite particles will be at a relatively low level. In this case, surface peeling of the artificial graphite may occur during the process in which electrolyte components such as ethyl methyl carbonate (EMC) are impregnated into the artificial graphite. Such surface peeling of the artificial graphite causes a side reaction between the non-aqueous electrolyte and the artificial graphite surface, leading to the problem of continuous consumption of the organic solvent in the non-aqueous electrolyte. On the other hand, if the degree of graphitization of the entire artificial graphite is reduced to prevent such problems, the discharge capacity itself decreases, making it difficult to achieve the desired energy density.

[0042] In this regard, the present invention prevents or suppresses electrolyte side reactions and improves discharge capacity by adjusting the nitrogen element content present in the artificial graphite particles within a specific range. The reason for this effect is understood to be that when the nitrogen element content present or introduced during the graphitization process of the artificial graphite particles meets a specific range, the degree of graphitization of the surface of the artificial graphite particles decreases to an appropriate level, and surface peeling by non-aqueous electrolyte organic solvents decreases to a significant level. Furthermore, the negative electrode active material according to the present invention can prevent or suppress electrolyte side reactions without lowering the overall degree of graphitization of the artificial graphite particles, and can also achieve a high level of discharge capacity.

[0043] Furthermore, by adjusting the nitrogen content in the artificial graphite particles to a specific range, it is possible to improve the rapid charging performance of the negative electrode active material by generating localized electrochemically active sites through nitrogen doping.

[0044] In one embodiment, the nitrogen content in the artificial graphite particles may be about 80 mg to 180 mg per 1 kg of the negative electrode active material, for example, about 100 mg to 170 mg, or about 110 mg to 160 mg, or about 120 mg to 140 mg, and within this range, the effect of improving initial efficiency and discharge capacity and the effect of preventing electrolyte side reactions can be expressed at a better level.

[0045] In the present invention, the oxygen content in the negative electrode active material may be about 650 mg to 1,000 mg per 1 kg of the negative electrode active material, for example, about 650 mg to 900 mg, or about 680 mg to 850 mg, or about 700 mg to 800 mg. Furthermore, the hydrogen content in the negative electrode active material may be about 300 mg to 500 mg per 1 kg of the negative electrode active material, for example, about 310 mg to 480 mg, or about 320 mg to 450 mg, or about 350 mg to 420 mg.

[0046] The total weight of nitrogen, oxygen, and hydrogen elements present in the negative electrode active material may be approximately 1,000 mg to 1,600 mg per 1 kg of the negative electrode active material, for example, approximately 1,050 mg to 1,500 mg, or approximately 1,110 mg to 1,460 mg, or approximately 1,200 mg to 1,400 mg.

[0047] The ratio of the weight of nitrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be about 0.12 or more, for example, 0.15 or more, or 0.16 or more. The ratio of the weight of nitrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be, for example, about 0.20 or less, or about 0.19 or less. The ratio of the weight of nitrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be about 0.12 to 0.20, for example, about 0.15 to 0.20, or 0.16 to 0.19, or about 0.165 to 0.185.

[0048] The ratio of the weight of hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be about 0.47 or more, for example, about 0.47 to 0.55, or for example, about 0.48 to 0.51.

[0049] The ratio of the total weight of nitrogen and hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be about 0.5 or more, for example, 0.55 or more, or 0.6 or more. The ratio of the total weight of nitrogen and hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be about 0.75 or less. For example, the ratio of the total weight of nitrogen and hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material may be about 0.5 to 0.75, for example, 0.6 to 0.72, or 0.65 to 0.70.

[0050] The aforementioned nitrogen, oxygen, and hydrogen content, and the relationships between their content, can improve initial efficiency and discharge capacity, as well as prevent or suppress electrolyte side reactions.

[0051] The nitrogen, oxygen, and / or hydrogen content can be measured using an ONH analyzer. For example, 0.1 g of a negative electrode active material sample can be placed in a crucible and then put into an ONH analyzer to measure the nitrogen, oxygen, and / or hydrogen content. For example, the NOH836 Analyzer manufactured by LECO Korea can be used as the ONH analyzer. In the case of the nitrogen, oxygen, and / or hydrogen content, three identical negative electrode active material samples can be prepared, and after performing analysis with the ONH analyzer three times, the average value obtained can be defined as the nitrogen, oxygen, and / or hydrogen content.

[0052] In the present invention, the nitrogen, oxygen, and hydrogen content in the negative electrode active material can be adjusted by adjusting the conditions of the manufacturing process of artificial graphite particles, such as grinding, molding by mechanical milling, granulation, graphitization, and additional molding steps. In one embodiment, the negative electrode active material according to the present invention can have its nitrogen, oxygen, and hydrogen content adjusted by adjusting the conditions of the mechanical milling or spheroidization step while performing an additional molding step, such as mechanical milling or spheroidization, after the graphitization step for manufacturing artificial graphite particles. Here, the mechanical milling or spheroidization conditions can be adjusted, for example, by considering the size of the reactor and the weight of the precursor introduced.

[0053] Figure 1 is a flowchart illustrating the artificial graphite manufacturing process (100) according to one embodiment.

[0054] In step S110, the coke, which is the raw material for artificial graphite, is first crushed to the desired size. In this process, the size of the coke is adjusted by controlling the rounds per minute (RPM) of the milling equipment, such as an air classifier mill, roll mill, or hammer mill.

[0055] In step S120, a primary molding process is performed. The primary molding process not only smooths the surface of the coke, which has been reduced to the desired size through the previous grinding process, but also shapes it into a non-pointed form. The primary molding process may use the same equipment as the grinding process, or different equipment may be used.

[0056] In step S130, a granulation process is carried out. In the case of artificial graphite, the granulation process is the process of producing secondary particles by agglomerating multiple primary particles, which are made by crushing coke and using additives such as pitch. The granulation process is carried out using a vertical or horizontal granulator, which is equipment for mixing the primary particles, which are crushed coke, with additives such as pitch. The mixing ratio with the additives can be adjusted by adjusting the RPM of the equipment to form the desired particle size.

[0057] In step S140, a graphitization process is carried out. In one embodiment, an Acheson furnace is used in the graphitization process, and graphite is produced by heat-treating coke at a temperature of, for example, about 3,000°C.

[0058] Step S150 involves a secondary molding process, which is an additional molding process that can cause artificial damage to the surface of the graphite. The equipment used in the previous molding and grinding process can be used in the secondary molding process. However, the RPM and process time are significantly reduced compared to the previous molding and grinding process, for example, by performing relatively weak milling.

[0059] The degree of graphitization of the negative electrode active material may be about 90% to 99%, for example, about 92% to 99%, or about 92% to 96%, or about 92% to 94%. When it is within this range, the degree of graphitization of the entire negative electrode active material can be increased to a specific level to ensure excellent initial efficiency and discharge capacity, and to prevent or suppress side reactions of the electrolyte due to surface peeling of the negative electrode active material.

[0060] The graphitization degree of the negative active material can be calculated by measuring the interplanar spacing d002 of the graphite (002) plane obtained from XRD data according to Bragg's Law.

[0061] For example, the graphitization degree can be derived by the following Equation 1.

[0062] [Equation 1] Graphitization degree (%) = (3.44-d002) / (0.086) × 100

[0063] (In Equation 1, d002 is the interplanar spacing (nm) of the (002) plane of artificial graphite particles present in the negative active material)

[0064] The average particle diameter (D 50 ) of the negative active material may be about 10 μm to 30 μm, for example, about 12 μm to 25 μm.

[0065] The BET (Brunauer, Emmett, Teller) specific surface area of the negative active material is about 1 m 2 / g to 8 m 2 / g, for example, about 1.2 m 2 / g to 5 m 2 / g, or about 1.4 m 2 / g to 3.2 m 2 / g, or about 1.6 m 2 / g to 2.5 m 2 / g. When the specific surface area is within the above range, a smooth movement path for lithium ions can be secured, excellent initial efficiency and discharge capacity can be achieved, and the effect of improving side reactions of the electrolyte by reducing the graphitization degree of the surface portion of the negative active material can be realized. The BET specific surface area can be measured using, for example, a BEL Sorption device (manufactured by BEL Japan).

[0066] The negative electrode active material may further include an amorphous carbon coating layer located on the surface of the artificial graphite particles. The amorphous carbon coating layer can improve the structural stability of the artificial graphite particles and help prevent or suppress side reactions between the negative electrode active material and the electrolyte.

[0067] The amorphous carbon coating layer can be formed in an amount of about 0.1% to 10% by weight, for example, about 1% to 5% by weight, relative to the total weight of the anode active material. The presence of the amorphous carbon coating layer can improve the structural stability of the anode active material. However, excessive formation of the amorphous carbon coating layer may cause a decrease in initial efficiency due to an increase in specific surface area during rolling of the anode, and may lead to a decrease in high-temperature storage performance. Therefore, the carbon coating layer is formed within the above-mentioned content range.

[0068] The amorphous carbon coating layer can be formed by providing a carbon coating layer precursor to artificial graphite particles and then heat-treating them.

[0069] The carbon coating layer precursor may include at least one selected from the group consisting of polymer resins and pitch. For example, the polymer resin may include at least one selected from the group consisting of sucrose, phenol resin, naphthalene resin, polyvinyl alcohol resin, furfuryl alcohol resin, polyacrylonitrile resin, polyamide resin, furan resin, cellulose resin, styrene resin, polyimide resin, epoxy resin, vinyl chloride resin, and polyvinyl chloride. The pitch may include at least one selected from the group consisting of coal-based pitch, petroleum-based pitch, and mesophase pitch. The heat treatment step for forming the amorphous carbon coating layer may be carried out at about 1,000°C to 1,500°C in order to ensure uniform formation of the amorphous carbon coating layer.

[0070] <Negative electrode> The present invention provides a negative electrode, for example, a negative electrode for a lithium secondary battery. The negative electrode may be a negative electrode containing the negative electrode active material described above.

[0071] In one embodiment, the negative electrode includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector, and the negative electrode active material layer may include the negative electrode active material described above.

[0072] The negative electrode current collector can be any negative electrode current collector commonly used in the art, and is not particularly limited, as long as it does not cause chemical changes in the lithium secondary battery and has high conductivity. For example, the negative electrode current collector may contain at least one selected from copper, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum-cadmium alloy, depending on one embodiment.

[0073] The negative electrode current collector may have fine irregularities formed on the surface thereof to enhance the binding force of the negative electrode active material, and may be used in various forms such as films, sheets, foils, meshes, porous bodies, foams, and non-woven fabrics.

[0074] The negative electrode current collector may generally have a thickness of 3 μm to 500 μm.

[0075] The negative electrode active material layer is disposed on at least one surface of the negative electrode current collector. For example, the negative electrode active material layer may be disposed on one surface or both surfaces of the negative electrode current collector.

[0076] The negative electrode active material layer may include the above-mentioned negative electrode active material.

[0077] The negative electrode active material layer may further include a silicon-based active material in addition to the above-mentioned negative electrode active material.

[0078] The silicon-based active material may include, for example, at least one of silicon (Si), silicon oxide (SiO x , 0<x<2), and a silicon-carbon composite.

[0079] The negative electrode active material or a mixture of the negative electrode active material and the silicon-based active material may be included in the negative electrode active material layer in an amount of about 80 wt% to 99 wt%, for example, about 88 wt% to 98 wt%.

[0080] In addition, the description of the negative electrode active material is as described above.

[0081] The negative electrode active material layer may further include a binder, a conductive material, and / or a thickener in addition to the above-mentioned negative electrode active material.

[0082] The binder is a component that contributes to the bonding between the active material and / or the current collector, and may be generally included in the negative electrode active material layer in an amount of about 1 wt% to 30 wt%, for example, about 1 wt% to 10 wt%.

[0083] The binder may include at least one selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, for example, at least one selected from the group consisting of polyvinylidene fluoride and styrene-butadiene rubber.

[0084] As the aforementioned thickening agent, all thickening agents conventionally used in lithium secondary batteries can be used, one example being carboxymethylcellulose (CMC).

[0085] The conductive material is a component for further improving the conductivity of the negative electrode active material, and can be included in the negative electrode active material layer in an amount of about 1% to 30% by weight, for example, 1% to 10% by weight.

[0086] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. Examples of usable conductive materials include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Examples of commercially available conductive materials include acetylene black (such as products from Chevron Chemical Company), Denka Black (manufactured by Denka Singapore Private Limited), products from Gulf Oil Company, Ketjen black, EC series (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).

[0087] The thickness of the negative electrode active material layer may be approximately 10 μm to 300 μm, for example, approximately 50 μm to 200 μm, but is not limited thereto.

[0088] The negative electrode active material layer can be manufactured by applying, rolling, and drying a negative electrode slurry, which is produced by selectively adding a negative electrode active material, a binder, a thickener, and / or a conductive material to a solvent, to the negative electrode current collector. Here, the solvent may include water or an organic solvent such as NMP (N-methyl-2-pyrrolidone), for example, water.

[0089] <Secondary battery> Furthermore, the present invention provides a secondary battery including the above-described negative electrode, such as a lithium secondary battery.

[0090] The secondary battery may include the negative electrode described above, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte.

[0091] The positive electrode can face the negative electrode.

[0092] The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.

[0093] The positive electrode current collector can be any positive electrode current collector commonly used in the art, and is not particularly limited as long as it does not cause chemical changes in the secondary battery and has relatively high conductivity. For example, the positive electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, and aluminum-cadmium alloy, and depending on one embodiment, aluminum.

[0094] The positive electrode current collector can also have fine irregularities formed on its surface to strengthen the bonding force of the positive electrode active material, and can be used in various forms such as films, sheets, foils, meshes, porous materials, foams, and nonwoven fabrics.

[0095] The positive electrode current collector can generally have a thickness of 3 μm to 500 μm.

[0096] The positive electrode active material layer may contain a positive electrode active material.

[0097] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium composite metal oxide containing lithium and at least one metal such as cobalt, manganese, nickel or aluminum. According to one embodiment, the lithium composite metal oxide may be a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2 (where 0<Y<1), LiMn 2-z Ni z O4 (where 0<Z<2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co Y1 O2 (where 0<Y1<1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0<Y2<1), LiMn 2-z1 Co z1 O4 (where 0<Z1<2), etc.), a lithium-nickel-manganese-cobalt-based oxide (e.g., Li(Ni p Co q Mn r1 )O2 (where 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0<p1<2, 0<q1<2, 0<r2<2, p1+q1+r2=2), etc.), or a lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (wherein M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, and p2, q2, r3 and s2 are each independently an atomic fraction of an element satisfying 0<p2<1, 0<q2<1, 0<r3<1, 0<s2<1, and p2+q2+r3+s2=1), and the like, and any one or two or more of these compounds may be included. Among them, from the viewpoint of improving the capacity characteristics and stability of the battery, the lithium composite metal oxide may be LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Mn 0.15 Co 0.05 )O2, etc.). Considering the remarkable improvement effect by controlling the types and content ratios of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., and any one or a mixture of two or more of these may be used.

[0098] The cathode active material may be included in an amount of about 80% by weight to 99% by weight in the cathode active material layer.

[0099] The positive electrode active material layer may further include, together with the positive electrode active material, at least one selected from the group consisting of a binder and a conductive material.

[0100] The binder is a component that facilitates the bonding of the active material to the conductive material and to the current collector, and is usually added in an amount of 1 to 30% by weight relative to the total weight of the positive electrode mixture. Examples of such binders include at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber.

[0101] The binder can be contained in the positive electrode active material layer in an amount of about 1% to 30% by weight.

[0102] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. Examples of usable conductive materials include graphite; carbon-based materials such as carbon black, acetylene black, Ketjenblack, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Examples of commercially available conductive materials include acetylene black (such as products from Chevron Chemical Company), Denka Black (manufactured by Denka Singapore Private Limited), products from Gulf Oil Company, Ketjenblack, EC series (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).

[0103] The conductive material can be added to the positive electrode active material layer in an amount of about 1% to 30% by weight.

[0104] The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. It can be used without particular limitations as long as it is a separator commonly used in lithium secondary batteries. For example, a separator with low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity can be used. In one embodiment, a porous polymer film, such as a porous polymer film made from polyolefin polymers like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, can be used. Alternatively, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymeric substances may be used to ensure heat resistance or mechanical strength, and can be selectively used in single-layer or multi-layer structures.

[0105] Furthermore, the electrolytes used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.

[0106] For example, the electrolyte may include an organic solvent and a lithium salt.

[0107] The aforementioned organic solvent can be used without particular limitations, as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. For example, the organic solvents that can be used include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon element group of C2-C20, and may include a double-bonded aromatic ring or ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Depending on the embodiment, a carbonate-based solvent may be used, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant, which can improve the charge and discharge performance of the battery, and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) may be used. In this case, the electrolyte can exhibit excellent performance by mixing the cyclic carbonate and the linear carbonate in a volume ratio of about 1:1 to about 1:9.

[0108] The lithium salt can be used without particular limitations as long as it is a compound that can provide lithium ions for use in lithium secondary batteries. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, etc. The concentration of the lithium salt is preferably in the range of about 0.1 to 2.0 M. When the concentration of the lithium salt falls within this range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions can move effectively.

[0109] As described above, the lithium secondary battery according to the present invention exhibits excellent discharge capacity, rapid charging characteristics, and stable capacity retention, making it useful in portable devices such as mobile phones, notebook computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs). In particular, it can be used as a component battery in medium- and large-sized battery modules. Therefore, the present invention also provides a medium- and large-sized battery module that includes the above-described secondary battery as a unit battery.

[0110] These medium- and large-sized battery modules can be applied to power sources that require high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage devices.

[0111] Hereinafter, embodiments of the present invention will be described in detail so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention can be realized in various different forms and is not limited to the embodiments described herein.

[0112] <Examples and Comparative Examples> Example 1 The coke raw material was crushed, air-classified, and mechanically milled to produce a primary particle form carbon precursor. The carbon precursor and pitch were then mixed and fed into a granulation facility containing blades. Mixing and mechanical milling were performed simultaneously at 400°C to 800°C to produce a secondary particle form intermediate. The intermediate was then graphitized by heat treatment at 3,000°C for 2 hours in a graphitization furnace with a capacity of approximately 100 kg.

[0113] After the graphitization process, the obtained material was subjected to additional mechanical milling in a granulation facility at room temperature and a speed of 30 Hz. This produced artificial graphite particles in the form of secondary particles, each containing two or more primary artificial graphite particles, which were then used as the negative electrode active material.

[0114] The average particle size (D) of the negative electrode active material 50 The surface area is 17 μm, and the BET specific surface area is 1.4 m². 2 It was / g.

[0115] Example 2 The negative electrode active material was manufactured in the same manner as in Example 1, except that the additional mechanical milling after graphitization was performed at room temperature and at a speed of 40 Hz, which is higher than the 30 Hz used in Example 1.

[0116] The average particle size (D) of the negative electrode active material 50 The surface area is 16 μm, and the BET specific surface area is 1.8 m². 2 It was / g.

[0117] Example 3 The negative electrode active material was manufactured in the same manner as in Example 1, except that additional mechanical milling after graphitization was performed at room temperature and at a speed of 50 Hz, which is higher than the 40 Hz used in Example 2.

[0118] The average particle size (D) of the negative electrode active material 50 The surface area is 15 μm, and the BET specific surface area is 3.2 m². 2 It was / g.

[0119] Comparative Example 1 The negative electrode active material was manufactured in the same manner as in Example 1, except that no additional mechanical milling was performed after graphitization.

[0120] The average particle size (D) of the negative electrode active material 50 The surface area is 19 μm, and the BET specific surface area is 1.2 m². 2 It was / g.

[0121] Comparative Example 2 The negative electrode active material was manufactured in the same manner as in Example 1, except that the heat treatment time during graphitization was adjusted to 3 hours and no additional mechanical milling was performed after graphitization.

[0122] The average particle size (D) of the negative electrode active material 50 The surface area was 19 μm, and the BET specific surface area was 1.0 m² / g.

[0123] Comparative Example 3 The negative electrode active material was manufactured in the same manner as in Example 1, except that the heat treatment time during graphitization was adjusted to 1 hour and no additional mechanical milling was performed after graphitization.

[0124] The average particle size (D) of the negative electrode active material 50 The surface area is 20 μm, and the BET specific surface area is 3.5 m². 2 It was / g.

[0125] [Table 1]

[0126] 1) Analysis of nitrogen, oxygen, and hydrogen content 0.1 g of the negative electrode active material sample was placed in a crucible and then put into an ONH analyzer (NOH836 Analyzer, manufactured by LECO Korea) to measure the nitrogen, oxygen, and / or hydrogen content. Three samples were prepared for each example and comparative example, and the measurement test was performed three times. The average values ​​are shown in Table 1.

[0127] 2) Degree of graphitization The degree of graphitization of the negative electrode active material was calculated by measuring the interplanar spacing d002 of the graphite (002) planes obtained from XRD data using Bragg's law, and then calculating according to Equation 1.

[0128] 3) Average particle size (D 50 ) Average particle size of negative electrode active material (D 50 ) is determined by obtaining a particle size distribution curve using laser diffraction, then finding the particle size corresponding to 50% of the cumulative volume, and using this as the average particle size (D) of the negative electrode active material. 50 ) was defined as follows.

[0129] 4) BET specific surface area The BET specific surface area of ​​the negative electrode active material was measured using a BEL Sorption instrument (manufactured by BEL Japan).

[0130] <Example of experiment> Experimental Example 1: Evaluation of Initial Efficiency and Discharge Capacity (Manufacturing of lithium-ion batteries) A negative electrode slurry was prepared by adding the negative electrode active material manufactured according to Example 1, carbon black as a conductive material, styrene-butadiene rubber as a binder, and CMC as a thickener in a weight ratio of 95.6:1.0:1.1:2.3 to water as a solvent. The negative electrode slurry was applied to a copper current collector, dried at 130°C, and rolled to produce a negative electrode.

[0131] A lithium metal was prepared as a counter electrode to the aforementioned negative electrode.

[0132] An electrode assembly was manufactured by interposing a porous polyethylene separator between the negative electrode and the lithium metal counter electrode, the electrode assembly was placed inside a case, a non-aqueous electrolyte was injected into the case, and the case was sealed to manufacture the lithium secondary battery of Example 1.

[0133] The non-aqueous electrolyte used was prepared by dissolving LiPF6 at a concentration of 1.0 M in an organic solvent mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 20:80.

[0134] Lithium secondary batteries of Examples 2-3 and Comparative Examples 1-4 were manufactured using the same method as in Example 1, except that the negative electrode active materials of Examples 2-3 and Comparative Examples 1-3 were used.

[0135] (Evaluation of initial efficiency and discharge capacity) The lithium secondary batteries of Examples 1-3 and Comparative Examples 1-3 manufactured as described above were charged at 25°C in CC / CV mode at 0.1C (0.005V, 0.005C cut-off), and discharged in CC mode at 0.1C to confirm their initial efficiency and discharge capacity.

[0136] The results are shown in Table 2 below.

[0137] [Table 2]

[0138] Referring to Table 2, it can be confirmed that the lithium secondary batteries of Examples 1 to 3, which contain the negative electrode active material according to the present invention, have superior initial efficiency and discharge capacity compared to Comparative Examples 1 to 3. For example, the initial efficiencies of Examples 1, 2, and 3 were 91%, 2%, 93.8%, and 92.2%, respectively, which were higher than the 88.6%, 78.3%, and 84.2% of Comparative Examples 1, 2, and 3. Similarly, the discharge capacities of Examples 1, 2, and 3 were 347 mAh / g, 350 mAh / g, and 345 mAh / g, respectively, which were higher than the 336 mAh / g, 343 mAh / g, and 320 mAh / g of Comparative Examples 1, 2, and 3.

[0139] While the embodiments of this disclosure have been described above with reference to those embodiments, a person skilled in the art or with ordinary knowledge in the art can understand that various modifications and changes to the various embodiments of this disclosure can be made in various ways without departing from the technical scope of the various embodiments of this disclosure as described in the claims below. Accordingly, the technical scope of the various embodiments of this disclosure is not limited to what is described in the detailed description of the specification, but must be determined by the claims.

Claims

1. It is a negative electrode active material, The negative electrode active material comprises artificial graphite particles and nitrogen, oxygen, and hydrogen elements present on the surface, inside, or both on the surface and inside the artificial graphite particles. The negative electrode active material contains the nitrogen element in an amount of 80 mg to 180 mg per kg of the negative electrode active material.

2. The aforementioned oxygen element is contained in an amount of 650 mg to 1,000 mg per 1 kg of the negative electrode active material. The negative electrode active material according to claim 1, wherein the hydrogen element is contained in an amount of 300 mg to 500 mg per 1 kg of the negative electrode active material.

3. The negative electrode active material according to claim 1, wherein the ratio of the weight of nitrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material is 0.12 or more.

4. The negative electrode active material according to claim 1, wherein the ratio of the weight of hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material is 0.47 or more.

5. The negative electrode active material according to claim 1, wherein the ratio of the total weight of nitrogen and hydrogen elements in the negative electrode active material to the weight of oxygen elements in the negative electrode active material is 0.5 or more.

6. The negative electrode active material according to claim 1, wherein the total weight of nitrogen, oxygen, and hydrogen elements present in the negative electrode active material is 1,000 mg to 1,600 mg per 1 kg of the negative electrode active material.

7. The negative electrode active material according to claim 1, wherein the artificial graphite particles are in the form of secondary particles obtained by granulating two or more primary particles.

8. The negative electrode active material according to claim 1, wherein the degree of graphitization of the negative electrode active material is 90% to 99%.

9. The BET specific surface area of ​​the negative electrode active material is 1 m² 2 / g to 8m 2 The negative electrode active material according to claim 1, wherein the value is / g.

10. The negative electrode active material according to claim 1, further comprising an amorphous carbon coating layer located on the artificial graphite particles.

11. A negative electrode comprising the negative electrode active material described in claim 1.

12. The negative electrode according to claim 11, A positive electrode opposite the negative electrode, A separator interposed between the negative electrode and the positive electrode, A lithium secondary battery containing a non-aqueous electrolyte.