Cathode material, cathode containing the same, and lithium secondary battery
The cathode material with controlled surface area and crystallite size, coated with boron, addresses particle cracking and gas generation issues, enhancing the output and storage performance of lithium secondary batteries.
Patent Information
- Application Number
- JP2026526371
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-11-20
- Filing Date
- 2024-12-20
- Publication Date
- 2026-11-24
AI Technical Summary
Conventional cathode materials using lithium nickel cobalt manganese oxide face issues such as particle cracking during electrode manufacturing, frequent side reactions with the electrolyte, excessive gas generation during high-temperature storage, and increased initial resistance due to high specific surface area or low surface area, which affect the output and storage characteristics of lithium secondary batteries.
A cathode material comprising lithium nickel-based oxide particles with a controlled BET specific surface area of 0.41 m²/g to 0.59 m²/g and an average crystallite size of 155 nm or more, coated with boron, which minimizes particle cracking and gas generation while maintaining low resistance and excellent output characteristics.
The cathode material achieves reduced initial resistance and gas generation during high-temperature storage, resulting in improved output characteristics and high-temperature storage performance.
Smart Images

Figure 2026539323000001 
Figure 2026539323000002 
Figure 2026539323000003
Abstract
Description
Technical Field
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2023-0189917 filed on December 22, 2023 and Korean Patent Application No. 10-2024-0166754 filed on November 20, 2024, the entire contents of which are incorporated herein by reference. The present invention relates to a positive electrode material, a positive electrode including the same, and a lithium secondary battery.
Background Art
[0002] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, and the positive electrode and the negative electrode include an active material capable of intercalating and deintercalating lithium ions.
[0003] As the positive electrode active material of a lithium secondary battery, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (such as LiMnO2 or LiMnO4), lithium iron phosphate (LiFePO4), and the like have been used. Among them, lithium cobalt oxide has advantages of high operating voltage and excellent capacity characteristics, but it is difficult to commercially apply it to high-capacity batteries due to the high price of cobalt as a raw material and unstable supply. Lithium nickel oxide is inferior in structural stability and it is difficult to achieve sufficient lifespan characteristics. On the other hand, lithium manganese oxide is excellent in stability but has a problem of being inferior in capacity characteristics. Accordingly, lithium composite transition metal oxides containing two or more types of transition metals have been developed to complement the problems of lithium transition metal oxides containing Ni, Co, or Mn alone, and among them, lithium nickel cobalt manganese oxide containing Ni, Co, and Mn is widely used in the field of batteries for electric vehicles.
[0004] On the other hand, conventional cathode materials using lithium nickel cobalt manganese oxide have a high specific surface area and excellent resistance characteristics, but they have problems such as the particles being prone to cracking during electrode manufacturing, generating a lot of fine powder, frequent side reactions with the electrolyte, and generating a lot of gas during high-temperature storage. To solve this, measures to reduce the specific surface area have been proposed, but if the specific surface area is too low, the initial resistance increases, the output characteristics deteriorate, and the initial capacitance characteristics deteriorate. Therefore, there is a need for the development of cathode materials that have low resistance, excellent output characteristics, and excellent high-temperature storage characteristics. [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] The present invention aims to solve the above-mentioned problems and to provide a cathode material with low resistance, excellent output characteristics, and excellent high-temperature storage characteristics, as well as a cathode containing the same and a lithium secondary battery. [Means for solving the problem]
[0006] [1] The present invention relates to a positive electrode material comprising a positive electrode active material comprising lithium nickel-based oxide particles in the form of secondary particulate matter formed by aggregation of multiple primary particles, wherein the content of Ni among all metals excluding lithium is 50 mol% to 90 mol%, and a coating layer containing boron (B) formed on the surface of the lithium nickel-based oxide particles, wherein the BET specific surface area of the positive electrode material is 0.41 m². 2 / g~0.59m 2 The present invention provides a cathode material having a density of / g and an average crystallite size of 155 nm or more.
[0007] [2] In the present invention, in [1] above, the average crystallite size of the positive electrode material may be 155 nm to 170 nm.
[0008] [3] In the present invention, in [1] or [2] above, the lithium nickel oxide particles may be represented by the following chemical formula 1.
[0009] [Chemical Formula 1] Li a [Ni b Co c M 1 d M 2 e O2
[0010] In Chemical Formula 1, M 1 is Mn, Al, or a combination thereof, and M 2 is at least one selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo, and satisfies 0.80≦a≦1.20, 0.50≦b≦0.90, 0<c≦0.40, 0<d≦0.40, and 0≦e≦0.10.
[0011] [4] The present invention is the positive electrode material according to any one of [1] to [3], wherein the boron (B) may be included in an amount of 500 ppm to 1000 ppm based on the total weight of the positive electrode material.
[0012] [5] The present invention is the positive electrode material according to any one of [1] to [4], wherein the amount of residual lithium in the positive electrode material may be 0.2 wt% to 0.4 wt%.
[0013] [6] The present invention is the positive electrode material according to any one of [1] to [5], wherein the cation mixing rate of the positive electrode material may be 2.5 at% or less.
[0014] [7] The present invention is the positive electrode material according to any one of [1] to [6], wherein the positive electrode material has an average particle diameter D 50 of 6 μm to 20 μm, and an average particle diameter D 50 of 0.1 μm to 5.5 μm.
[0015] [8] The present invention is the positive electrode material according to any one of [1] to [7], wherein the positive electrode material has an average particle diameter D 50 of 6 μm to 20 μm, and an average particle diameter D 50The material contains small particles ranging from 0.1 μm to 5.5 μm, and the large particles and small particles may be present in a weight ratio of 60:40 to 80:20.
[0016] [9] The present invention provides a positive electrode comprising the positive electrode material described in any one of the above [1] to [8].
[0017]
[10] The present invention provides a lithium secondary battery including the positive electrode described in [9] above. [Effects of the Invention]
[0018] The cathode material according to the present invention has a BET specific surface area of 0.41 m². 2 / g~0.59m 2 It is characterized by having a density of / g and an average crystallite size of 155 nm or larger. In the case of a lithium secondary battery using a cathode material that satisfies all of the above conditions, it exhibits excellent initial resistance characteristics and high-temperature storage characteristics. [Modes for carrying out the invention]
[0019] The present invention will be described more preferably below. The terms and words used in this specification and in the claims are not to be interpreted in a manner limited to their ordinary or dictionary meanings, but rather in a manner consistent with the technical idea of the present invention, in accordance with the principle that inventors may appropriately define the concepts of terms in order to best describe their invention.
[0020] In this invention, the "specific surface area" is measured by the BET method, and preferably can be calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using BELSORP-mini II manufactured by BEL Japan.
[0021] In this invention, "single-particle form" means a particle consisting of 50 or fewer nodules, and is a concept that includes single particles consisting of one nodule and pseudo-single particles which are composites of 2 to 50 nodules.
[0022] The aforementioned "nodule" may be a single crystal without crystalline grain boundaries, or a polycrystalline material in which no grain boundaries are visible when observed with a scanning electron microscope at a field of view of 5,000 to 20,000 times magnification, as the lower particle unit constituting a single particle or pseudo-single particle.
[0023] In the present invention, "secondary particle" means a particle formed by the aggregation of multiple primary particles, for example, tens to hundreds of primary particles. Preferably, the secondary particle may be an aggregate of 51 or more primary particles.
[0024] In this invention, "particle" is a concept that includes one or all of the following: single particles, pseudo-single particles, primary particles, nodules, and secondary particles. In this invention, "average particle size D 50 "Cumulative particle size distribution" refers to the particle size at 50% of the volume-cumulative particle size distribution of the positive electrode active material powder or positive electrode material powder, and can be measured using the laser diffraction method. For example, after dispersing the positive electrode active material powder or positive electrode material powder in a dispersion medium, it can be introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac MT 3000), irradiated with ultrasound at approximately 28 kHz at an output of 60 W, and after obtaining a graph of the volume-cumulative particle size distribution, the particle size corresponding to 50% of the volume-cumulative amount can be determined to measure the particle size.
[0025] In this invention, "crystallite" refers to a particle unit having substantially the same crystal orientation, which can be confirmed by EBSD (Electron Backscatter Diffraction) analysis. Preferably, it refers to the smallest particle unit that is displayed in the same color in the IPF (Inverse Pole Figure Orientation) map obtained by EBSD analysis of a cross section of the positive electrode active material cut by ion milling.
[0026] In the present invention, the "average crystallite size" can be quantitatively analyzed using X-ray diffraction analysis (XRD) with Cu Kα X-rays. Preferably, the average crystal size of the crystal grains can be quantitatively analyzed by placing the particles to be measured in a holder, irradiating the particles with X-rays, and analyzing the resulting diffraction pattern. Sampling involves placing a powder sample of the target particles into the central groove of a standard powder holder, leveling the surface using a glass slide, and preparing the sample so that its height aligns with the edge of the holder. Next, X-ray diffraction analysis is performed using a Bruker D8 Endeavor (light source: Cu Kα, λ=1.54Å) equipped with a LynxEye XE-T position-sensitive detector, in the region of FDS 0.5°, 2θ=10°~125°, with a step size of 0.02 degrees and a total scanning time of approximately 60 minutes. Rietveld refinement is then performed on the measured data, considering the charge at each site (metal ions at transition metal sites are +3, Ni ions at Li sites are +2) and cation mixing. During the analysis of crystal grain size, instrumental broadening is performed using the Fundamental Parameter Analysis (FPA) implemented in the Bruker TOPAS program. The approach is considered, and during fitting, all peaks within the measurement range are used. Of the peak types available in TOPAS, only the FP (First Principle) and Lorentzian contribution are used for fitting, and strain is not considered.
[0027] In this invention, "cation mixing rate" refers to the amount of nickel ions (Ni) in the lithium layer of a layered lithium nickel oxide, based on the total amount of lithium sites (Li sites). 2+This refers to the percentage (%) of the material present, and is the value measured by X-ray diffraction analysis (XRD). Preferably, the X-ray diffraction analysis can be performed as follows: Using a Bruker D8 Endeavor (light source: Cu Kα, λ=1.54Å) equipped with a LynxEye XE-T position-sensitive detector, X-ray diffraction analysis was performed on the region FDS 0.5°, 2θ=10°~125°, with a step size of 0.02 degrees and a total scanning time of approximately 60 minutes. Rietveld refinement was then performed on the measured data, taking into account the charge at each site (metal ions at transition metal sites are +3, Ni ions at Li sites are +2) and cation mixing. During the analysis of crystal grain size, instrumental broadening was considered using the Fundamental Parameter Approach (FPA) implemented in the Bruker TOPAS program. All peaks within the measurement range were used during fitting, and the peak shape was fitted using only the Lorentzian contribution (FP) from the peak types available in TOPAS, without considering strain.
[0028] The positive electrode material, positive electrode containing the same, and lithium secondary battery according to the present invention include at least one of the following disclosed configurations, and may include any combination of technically possible configurations from the following configurations.
[0029] Cathode material The cathode material according to the present invention will be described below. The cathode material according to the present invention comprises a cathode active material comprising lithium nickel-based oxide particles in the form of secondary particulate matter formed by the aggregation of multiple primary particles, wherein the Ni content among all metals excluding lithium is 50 mol% to 90 mol%, and a coating layer containing boron (B) formed on the surface of the lithium nickel-based oxide particles, wherein the BET specific surface area of the cathode material is 0.41 m². 2 / g~0.59m 2 The coefficient is / g, and the average crystallite size of the positive electrode material is 155 nm or larger.
[0030] Lithium nickel oxide particles, which have been conventionally used as positive electrode active materials, are generally 0.6 m 2 / g~1.9m 2 It has a specific surface area at the / g level. Conventional positive electrode active materials have high internal porosity and excellent resistance characteristics, but they have problems such as particles being prone to cracking during electrode manufacturing, generating a lot of fine powder, frequent side reactions with the electrolyte, and excessive gas generation during high-temperature storage. Conversely, reducing the specific surface area of the positive electrode active material reduces particle cracking and gas generation during high-temperature storage, but it leads to problems such as increased initial resistance and a decrease in output characteristics and capacitance characteristics.
[0031] The inventors conducted extensive research to solve these problems and found that the BET specific surface area of the positive electrode material was 0.41 m². 2 / g~0.59m 2 We discovered that by controlling the resistance to the / g level and adjusting the average crystallite size of the cathode material to 155 nm or higher, the initial resistance is reduced, resulting in excellent output characteristics, and the amount of gas generated during high-temperature storage is reduced, resulting in excellent high-temperature storage characteristics. This led to the completion of the present invention.
[0032] According to one embodiment of the present invention, the BET specific surface area of the cathode material is 0.41 m². 2 / g~0.59m 2 It is / g. Preferably 0.41m 2 / g or more, or 0.42m 2 It may be 0.59m or more. 2 / g or less, 0.58m 2 / g or less, 0.57m 2 / g or less, 0.56m 2 Less than / g, or 0.55m 2 It may be less than or equal to / g, and more preferably 0.41m 2 / g~0.55m 2 It may also be / g. The BET specific surface area of the positive electrode material is 0.41 m². 2 If the value is less than / g, problems arise such as over-calcination during the manufacturing of the positive electrode material or instability of the crystal structure due to increased calcination temperature, leading to an increase in the amount of residual lithium on the surface and an increase in gas generation during high-temperature storage. The specific surface area of the positive electrode material is 0.59 m². 2 If the value exceeds / g, particle cracking during rolling increases, the contact area with the electrolyte increases, and the hygroscopicity of the electrolyte at the interface increases, leading to a problem of increased gas generation during high-temperature storage. Therefore, when the above range is met, the initial resistance decreases, excellent power characteristics are achieved, and excellent high-temperature storage characteristics can be achieved by reducing gas generation during high-temperature storage.
[0033] According to one embodiment of the present invention, the average crystallite size of the cathode material is 155 nm or more, preferably 155 nm or more, but may also be 190 nm or less, 185 nm or less, 180 nm or less, 175 nm or less, or 170 nm or less, and more preferably 155 nm to 170 nm. If the average crystallite size of the cathode material is less than 155 nm, many primary particles within the secondary particles are randomly arranged, which diversifies the movement pathways for lithium ions within the secondary particles, resulting in increased movement of unwanted lithium ions. In other words, this hinders the movement of lithium through the primary particle interface within the secondary particles, leading to an increase in initial resistance, an increase in specific surface area, and an increase in gas generation. Therefore, when the above range is met, excellent initial resistance characteristics and high-temperature storage characteristics can be achieved.
[0034] Furthermore, our research has revealed that when the BET specific surface area range and average crystallite size range of the cathode material are simultaneously satisfied, excellent power characteristics and excellent high-temperature storage characteristics are achieved simultaneously. Specifically, the BET specific surface area of the cathode material is 0.41 m². 2 / g~0.59m 2 Even if the / g requirement is met, if the average crystallite size is less than 155 nm, or if the BET specific surface area falls outside the aforementioned range even if the average crystallite size of the cathode material is 155 nm or more, it has become clear that the improvement in output characteristics and the reduction in gas generation during high-temperature storage are minimal.
[0035] For example, if both the BET specific surface area and average crystallite size of the cathode material are not controlled within a certain range, the contact area with the electrolyte, the stability of the crystal structure, and the efficiency of the lithium pathway due to the size of the crystal grains will not be combined in a favorable and organic way. This leads to problems such as a decrease in output characteristics and an increase in gas generation during high-temperature storage.
[0036] On the other hand, the BET specific surface area and average crystallite size of the cathode material are controlled by a combination of factors, including the BET specific surface area and average crystallite size of the cathode active material contained in the cathode material, the BET specific surface area and average particle size of the precursor used in the manufacture of the cathode active material, the molar ratio of lithium to transition metal during precursor calcination, the calcination temperature during the manufacture of the cathode active material and cathode material, and the content of coating elements. In this case, if the cathode material has a bimodal particle size distribution with cathode active material having a large average particle size and cathode active material having a small average particle size, the BET specific surface area and average crystallite size of each cathode active material and the content of coating elements can be combined to control the BET specific surface area and average crystallite size of the cathode material, but this is not limited to this case.
[0037] In this case, the BET specific surface area and average crystallite size of the cathode material are values measured from the cathode material powder and are distinct from the BET specific surface area and average crystallite size of individual cathode active material particles. For example, if the cathode active material contains both a cathode active material with a large average particle size and a cathode active material with a small average particle size, the BET specific surface area and average crystallite size of each may differ from the BET specific surface area and average crystallite size of the cathode material as a whole.
[0038] The cathode material according to the present invention will be described below in detail. According to one embodiment of the present invention, the positive electrode material comprises a positive electrode active material including lithium nickel oxide particles in the form of secondary particulate matter in which a plurality of primary particles are aggregated, and a coating layer formed on the surface of the lithium nickel oxide particles and containing boron (B).
[0039] According to one embodiment of the present invention, the lithium nickel oxide particles have a Ni content of 50 mol% to 90 mol% among the metal elements other than lithium, preferably 60 mol% to 90 mol%, more preferably 60 mol% to 85 mol%, and even more preferably 65 mol% to 80 mol%. For example, the lithium nickel oxide particles may be represented by the following chemical formula 1.
[0040] [Chemical formula 1] Li a [Ni b Co c M 1 d M 2 e ]O2
[0041] In the above chemical formula 1, M 1 This can be Mn, Al, or a combination of these. M 2This may be one or more selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo, and preferably one or more selected from the group consisting of Ti, Zr, Y, and Mg. When the above conditions are met, it is preferable in that it can promote particle growth during firing or improve the stability of the crystal structure.
[0042] The above 'a' represents the molar ratio of lithium in lithium nickel oxide particles, and may be 0.80 ≤ a ≤ 1.20, 0.90 ≤ a ≤ 1.10, or 1.00 ≤ a ≤ 1.10. When the above range is satisfied, it is preferable in that the amount of gas generated can be reduced and the resistance can be reduced.
[0043] The above b represents the molar ratio of nickel among the metals excluding lithium in the lithium nickel oxide particles, and may be 0.50 ≤ b ≤ 0.90, 0.60 ≤ b ≤ 0.90, 0.60 ≤ b ≤ 0.85, or 0.65 ≤ b ≤ 0.80.
[0044] The aforementioned c represents the molar ratio of cobalt among the metals excluding lithium in lithium nickel oxide particles, and 0 <c≦0.40、0<c≦0.25、または0<c≦0.15であってもよい。
[0045] The above d is M, which is the metal excluding lithium in the lithium nickel oxide particles. 1 This indicates the molar ratio of elements, and 0 <d≦0.40、0<d≦0.30、または0<d≦0.25であってもよい。
[0046] The aforementioned e is M, which is the metal excluding lithium in the lithium nickel oxide particles. 2 This represents the molar ratio of elements, and may be 0≦e≦0.10, 0≦e≦0.08, or 0≦e≦0.05.
[0047] According to one embodiment of the present invention, the lithium nickel oxide particles are in the form of secondary particles formed by the aggregation of multiple primary particles. When the lithium nickel oxide particles are in the form of secondary particles, a high rolling density can be achieved, and thus the energy density per unit volume can be increased. Furthermore, when the aforementioned BET specific surface area range and average crystallite size range of the cathode material are met, and a coating layer containing boron (B) is formed on the surface of the lithium nickel oxide particles, these may be favorable conditions for achieving better power characteristics and high-temperature storage characteristics.
[0048] For example, if the lithium nickel oxide particles are single-particle rather than secondary-particle, a large amount of inert rock salt-type structure is formed on the particle surface, making ion transfer difficult. This results in an excessively high average crystallite size and low lithium ion movement, leading to poor resistance characteristics. Furthermore, in the case of single-particle lithium nickel oxide, an inert structure is formed on the surface during the water washing process, increasing resistance. Since the water washing process is not performed, it becomes difficult to control the amount of residual lithium on the surface. Therefore, the effects of the present invention are best realized when the lithium nickel oxide particles are secondary-particle.
[0049] According to one embodiment of the present invention, the coating layer is formed on the surface of the lithium nickel oxide particles and contains boron(B). When a coating layer containing boron(B) is formed on the surface of the lithium nickel oxide particles, the coating layer minimizes contact between the electrolyte and the lithium nickel oxide particles, suppresses the occurrence of side reactions between the electrolyte and the lithium nickel oxide and the elution of transition metals, and improves the lifetime characteristics.
[0050] According to one embodiment of the present invention, the boron (B) may be present in an amount of 500 ppm to 1000 ppm, preferably 600 ppm to 900 ppm, and more preferably 700 ppm to 900 ppm, based on the total weight of the positive electrode material. When the above range is met, it is preferable in that the elution of transition metals can be suppressed, particle cracking during rolling can be reduced, and the resistance does not increase excessively.
[0051] According to one embodiment of the present invention, the residual lithium content of the positive electrode material may be 0.2% to 0.4% by weight, preferably 0.25% to 0.35% by weight, and more preferably 0.25% to 0.30% by weight. When the above range is satisfied, it is preferable in that it is possible to prevent the problem of the surface of the positive electrode active material vagina collapsing due to excessive washing and to prevent an increase in resistance due to residual lithium.
[0052] According to one embodiment of the present invention, the cation mixing rate of the positive electrode active material may be 2.5 at% or less, preferably 1.0 at% to 2.5 at%, and more preferably 1.0 at% to 2.0 at%. When this range is met, the resistance characteristics can be improved due to the high degree of perfection of the crystal structure. In this case, at% means atomic%.
[0053] According to one embodiment of the present invention, the positive electrode material has an average particle size D 50 This includes large particles ranging from 6 μm to 20 μm, and average particle size D 50 It may also contain small particles ranging from 0.1 μm to 5.5 μm.
[0054] The average particle size D is larger than the aforementioned large particles. 50 When the material contains small particles, during the manufacturing of the positive electrode, the small particles fill the gaps between the larger particles with a larger average particle size, thereby increasing the electrode density, increasing the contact area between particles, and improving the energy density.
[0055] According to one embodiment of the present invention, the average particle size D of the large particles 50The particle size may be 6 μm to 20 μm, preferably 6 μm to 15 μm, and more preferably 7 μm to 11 μm.
[0056] According to one embodiment of the present invention, the average particle size D of the small particles 50 The particle size may be between 0.1 μm and 5.5 μm, preferably between 1 μm and 5 μm, and more preferably between 2 μm and 5 μm. When the above range is satisfied, excellent energy density can be achieved.
[0057] According to one embodiment of the present invention, the large particles include lithium nickel oxide particles in the form of secondary particulate matter in which a plurality of primary particles are aggregated, and the lithium nickel oxide particles may be represented by the following chemical formula 2.
[0058] [Chemical formula 2] Li a1 Ni b1 Co c1 M 3 d1 M 4 e1 O2
[0059] In the above chemical formula 2, M 3 This can be Mn, Al, or a combination of these. M 4 This may be one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo.
[0060] The above a1 represents the molar ratio of lithium in lithium nickel oxide particles, and may be 0.80 ≤ a1 ≤ 1.20, 0.90 ≤ a1 ≤ 1.10, or 1.00 ≤ a1 ≤ 1.10.
[0061] The b1 value represents the molar ratio of nickel among the metals excluding lithium in the lithium-nickel oxide particles, and may be 0.30 ≤ b1 < 1.00, 0.40 ≤ b1 ≤ 0.90, 0.50 ≤ b1 ≤ 0.85, or 0.65 ≤ b ≤ 0.80.
[0062] The aforementioned c1 represents the molar ratio of cobalt among the metals excluding lithium in lithium nickel oxide particles, and 0 <c1≦0.70、0<c1≦0.40、または0<c1≦0.20であってもよい。
[0063] The aforementioned d1 is M, which is the metal excluding lithium in the lithium nickel oxide particles. 1 This indicates the molar ratio of elements, and 0 <d1≦0.70、0<d1≦0.40、または0<d1≦0.30であってもよい。
[0064] The aforementioned e1 is M, which is the metal excluding lithium in the lithium nickel oxide particles. 2 This represents the molar ratio of elements, and may be 0≦e1≦0.10, 0≦e1≦0.08, or 0≦e1≦0.05.
[0065] According to one embodiment of the present invention, the large particles may include lithium nickel oxide particles and a coating layer formed on the surface of the lithium nickel oxide particles and containing boron (B). When a coating layer is formed on the surface of the lithium nickel oxide particles, the coating layer suppresses contact between the electrolyte and the lithium nickel oxide particles, thereby reducing the elution of transition metals and gas generation due to side reactions with the electrolyte.
[0066] According to one embodiment of the present invention, the coating layer may further contain one or more coating elements selected from the group consisting of Al, Ti, W, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, and S. When the above conditions are met, it is preferable in that the occurrence of side reactions of the electrolyte can be suppressed.
[0067] According to one embodiment of the present invention, the small particles include lithium nickel oxide particles in the form of secondary particulate matter in which a plurality of primary particles are aggregated, and the lithium nickel oxide particles may be represented by the following chemical formula 3.
[0068] [Chemical formula 3] Li a2 Ni b2 Co c2 M 5 d2 M 6 e2 O2
[0069] In the above chemical formula 3, M 5 This can be Mn, Al, or a combination of these. M 6 This may be one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo.
[0070] The a2 mentioned above represents the molar ratio of lithium in the lithium nickel oxide particles, and may be 0.80 ≤ a2 ≤ 1.20, 0.90 ≤ a2 ≤ 1.10, or 1.00 ≤ a2 ≤ 1.10.
[0071] The b2 value represents the molar ratio of nickel among the metals excluding lithium in the lithium-nickel oxide particles, and may be 0.30 ≤ b2 < 1.00, 0.40 ≤ b2 ≤ 0.90, 0.50 ≤ b2 ≤ 0.85, or 0.65 ≤ b2 ≤ 0.80.
[0072] The aforementioned c2 represents the molar ratio of cobalt among the metals excluding lithium in lithium nickel oxide particles, and 0 <c2≦0.70、0<c2≦0.40、または0<c2≦0.20であってもよい。
[0073] The aforementioned d2 is M, which is the metal excluding lithium in the lithium nickel oxide particles. 1 This indicates the molar ratio of elements, and 0 <d2≦0.70、0<d2≦0.40、または0<d2≦0.30であってもよい。
[0074] The aforementioned e2 is M, which is the metal excluding lithium in the lithium nickel oxide particles. 2 This represents the molar ratio of elements, and may be 0 ≤ e² ≤ 0.10, 0 ≤ e² ≤ 0.08, or 0 ≤ e² ≤ 0.05.
[0075] According to one embodiment of the present invention, the small particles may include lithium nickel oxide particles and a coating layer formed on the surface of the lithium nickel oxide particles and containing boron (B). When a coating layer is formed on the surface of the lithium nickel oxide particles, the coating layer suppresses contact between the electrolyte and the lithium nickel oxide particles, thereby reducing the elution of transition metals and gas generation due to side reactions with the electrolyte.
[0076] According to one embodiment of the present invention, the large particles and small particles may be present in a weight ratio of 60:40 to 80:20, preferably 65:35 to 75:25. When the above range is satisfied, excellent suppression of particle cracking during rolling and energy density can be achieved.
[0077] positive electrode Next, the positive electrode according to the present invention will be described. The positive electrode according to the present invention includes the positive electrode material according to the present invention as described above. Preferably, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and containing the positive electrode material of the present invention as described above.
[0078] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. may be used. The positive electrode current collector may also have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the positive electrode current collector to increase the adhesion strength of the positive electrode active material. For example, it may be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0079] Furthermore, the positive electrode active material layer may also include a conductive material and a binder, along with the positive electrode material described above. The conductive material is used to impart conductivity to the electrodes and can be used in any battery without particular limitations as long as it has electronic conductivity without causing a chemical change. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these may be used alone or in mixtures of two or more. The conductive material is usually included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, relative to the total weight of the positive electrode active material layer.
[0080] The binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The binder may be present in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, relative to the total weight of the positive electrode active material layer.
[0081] The positive electrode can be manufactured by a conventional method for manufacturing a positive electrode. For example, the positive electrode can be manufactured by mixing a positive electrode active material, a binder, and / or a conductive material in a solvent to produce a positive electrode slurry, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling it. In this case, the types and contents of the positive electrode active material, binder, and conductive material are as described above.
[0082] The solvent may be a solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of solvent used should be sufficient to dissolve or disperse the cathode active material, conductive material, and binder, and to have a viscosity that allows for excellent thickness uniformity when applied for cathode manufacturing, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0083] Alternatively, the positive electrode can be manufactured by casting the positive electrode slurry onto another support, peeling it off the support, and then laminating the resulting film onto the positive electrode current collector.
[0084] Lithium-ion battery The lithium secondary battery according to the present invention will be described below. The lithium secondary battery of the present invention includes the positive electrode according to the present invention as described above. Preferably, it may also include the positive electrode, negative electrode, separator, and electrolyte. The lithium secondary battery may further selectively include a battery container for housing the electrode assembly of the positive electrode, negative electrode, and separator, and a sealing member for sealing the battery container.
[0085] (Negative electrode) The negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0086] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. The negative electrode current collector may also have a thickness of 3 to 500 μm, and, similar to the positive electrode current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it may be used in various forms such as film, sheet, foil, mesh, porous material, foam, and nonwoven fabric.
[0087] The negative electrode active material layer selectively includes a binder and a conductive material together with the negative electrode active material. As the negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO2. β Examples include lithium-doped and dedoped metal oxides such as (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compound and carbonaceous material, such as Si-C composites or Sn-C composites. One or more of these mixtures may be used.
[0088] Furthermore, a metallic lithium thin film may be used as the negative electrode active material. In addition, either low-crystalline carbon or high-crystalline carbon may be used as the carbon material. Typical low-crystalline carbons include soft carbon and hard carbon, while typical high-crystalline carbons include amorphous, plate-like, flaky, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0089] The conductive material is used to impart conductivity to the electrodes and can be used in any battery without particular limitations as long as it has electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these may be used alone or in mixtures of two or more. The conductive material is usually included in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, relative to the total weight of the negative electrode active material layer.
[0090] The binder plays a role in improving adhesion between negative electrode active material particles and adhesion between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. The binder may be present in an amount of 1 to 30% by weight, preferably 1 to 20% by weight, and more preferably 1 to 10% by weight, relative to the total weight of the negative electrode active material layer.
[0091] The negative electrode active material layer can be manufactured, for example, by applying a negative electrode slurry containing a negative electrode active material and selectively a binder and conductive material onto a negative electrode current collector and drying it, or by casting the negative electrode slurry onto another support, peeling it off the support, and then laminating the resulting film onto the negative electrode current collector.
[0092] (Separator) On the other hand, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Generally, any separator commonly used in lithium secondary batteries can be used without particular limitations, but it is especially preferable that it has low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity. Preferably, a porous polymer film, such as a porous polymer film made from polyolefin polymers like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. Alternatively, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, to ensure heat resistance or mechanical strength, a coated separator containing ceramic components or polymeric substances may be used, and it may be selectively used as a single-layer or multi-layer structure.
[0093] (electrolyte) Furthermore, the electrolytes used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0094] Preferably, the electrolyte may include an organic solvent and a lithium salt. The organic solvent can be any solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move, and is not particularly limited. Preferably, the organic solvent is an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene Carbonate solvents such as carbonate (PC); alcoholic solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon group of C2-C20, which may include a double-bonded aromatic ring or ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes may be used. Among these, carbonate solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery, and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.
[0095] The lithium salt can be any compound capable of providing lithium ions for use in lithium secondary batteries, and is not particularly limited. Preferably, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO2, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1 to 5.0 M, more preferably 0.1 to 3.0 M. When the concentration of the lithium salt falls within this range, the electrolyte has suitable conductivity and viscosity, exhibiting excellent electrolyte performance and allowing lithium ions to move effectively.
[0096] The electrolyte may further contain additives in addition to the components of the electrolyte to improve battery life characteristics, suppress the decrease in battery capacity, and improve battery discharge capacity. For example, the additives may be, but are not limited to, haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethyl phosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, either alone or in combination. The additives may be present in an amount of 0.1 to 10% by weight, preferably 0.1 to 5% by weight, relative to the total weight of the electrolyte.
[0097] As described above, the lithium secondary battery according to the present invention exhibits excellent output characteristics and is therefore useful not only in the electric vehicle field, such as hybrid electric vehicles (HEVs), but also in fields such as portable devices, including mobile phones, laptop computers, and digital cameras.
[0098] Accordingly, another embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same. The battery module or battery pack may be used as a power source for one or more medium- and large-sized devices selected from among power tools; electric vehicles including Electric Vehicles (EVs), hybrid electric vehicles, and Plug-in Hybrid Electric Vehicles (PHEVs); or power storage systems.
[0099] Hereinafter, embodiments of the present invention will be described in detail to enable a person of ordinary skill in the art to easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein.
[0100] Example 1 As large particles, Li 50 with an average particle diameter D 1.0 of 9.9 μm was used 0.7 [Ni 0.1 Co 0.2 Mn 50 O2, and as small particles, Li 1.0 with an average particle diameter (D 0.7 ) of 4 μm was used 0.1 [Ni 0.2 Co 2 Mn 0.7 O2 was mixed at a weight ratio of 70:30 to prepare a mixed cathode active material. Here, the large particles and small particles were in the form of secondary particles, and the large particles were prepared by mixing a composite transition metal precursor (Ni 0.1 Co 0.2 Mn(OH)2) having a BET specific surface area of 5.7 m2 / g with a lithium source (Li2CO3) such that the molar ratio of Li:Ni+Co+Mn was 1.03:1, followed by calcination.
[0101] After mixing the mixed cathode active material with H3BO3, the mixture was calcined at a temperature of 320° C. for 6 hours to prepare a cathode material in which a coating layer containing boron (B) was formed on the surface of cathode active material particles.
[0102] Boron (B) was present at a concentration of 800 ppm based on the total weight of the positive electrode material. Subsequently, the positive electrode material, carbon black as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in N-methyl-2-pyrrolidone (NMP) in a weight ratio of 96:1:3 to produce a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried at 130°C, and then rolled to produce a positive electrode.
[0103] A negative electrode slurry was prepared by mixing artificial graphite as the negative electrode active material, carbon black as the conductive material, and carboxymethylcellulose (CMC) as the binder in a weight ratio of 97:1.5:1.5. This slurry was then applied to one side of a copper current collector, dried at 110°C, and then rolled to produce the negative electrode.
[0104] An electrode assembly was manufactured by interposing a separator between the positive electrode and the negative electrode, then the assembly was placed inside a battery case, and finally, an electrolyte was injected into the case to manufacture a lithium secondary battery. The electrolyte was a mixed organic solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 30:40:30, to which 1 M of LiPF6 was dissolved.
[0105] Examples 2-3 and Comparative Examples 1-5 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the ratio of the number of moles of lithium (Li) contained in Li2CO3 to the total number of moles of transition metals (Ni+Co+Mn, Me) in the composite transition metal precursor (Li / Me) and the BET specific surface area of the composite transition metal precursor were adjusted as shown in Table 1 below during the production of large particles. Furthermore, the average particle size of the large particles used in the examples and comparative examples is shown in Table 1 below.
[0106] [Table 1]
[0107] Experimental Example 1: Measurement of BET specific surface area and average crystallite size of cathode material The BET specific surface area was measured for the cathode material powders produced in Examples 1-3 and Comparative Examples 1-5 using the BET method, and the average crystallite size was measured by X-ray diffraction analysis (XRD, Bruker D8 Endeavor). The conditions for performing the BET method and X-ray diffraction analysis were the same as described above. The measurement results are shown in Table 2 below.
[0108] [Table 2]
[0109] Experimental Example 2: Measurement of Residual Lithium Content and Cation Mixing Rate 5 g of the cathode material powder produced in Examples 1-3 and Comparative Examples 1-5 was dispersed in 100 ml of distilled water, and the amount of residual lithium dissolved in the distilled water was measured by pH titration. The measured amount of residual lithium is expressed as a weight percentage of the total weight of the cathode material.
[0110] Furthermore, the cation mixing rate of the cathode materials produced in Examples 1-3 and Comparative Examples 1-5 was measured by XRD analysis. The XRD analysis was performed using an X-ray diffraction analyzer (Bruker AXS D4-Endeavor XRD) with a Cu-Ka light source and under an acceleration voltage of 10kV. The measurement results are shown in Table 3 below.
[0111] [Table 3]
[0112] Experiment Example 3: Measurement of Initial Resistance Each lithium secondary battery manufactured in Examples 1-3 and Comparative Examples 1-5 was charged at 25°C with a constant current of 0.3C until it reached 4.25V, and then discharged to 3.0V with a constant current of 39mAh / g. This constituted one charge-discharge cycle, and three such cycles were performed.
[0113] Next, the battery was charged to 4.25V at 25°C under constant current-constant voltage (CC-CV) charging conditions using 0.3C CC. Then, pulse discharge was performed at a rate of 2.5C under conditions of 50% and 10% SOC, and the voltage drop over 10 seconds was measured to determine the initial resistance. The initial resistance values are shown in Table 4 below.
[0114] Experimental Example 4: Evaluation of Gas Generation Amount Each lithium secondary battery manufactured in Examples 1-3 and Comparative Examples 1-5 was charged to 4.25V with a constant current of 0.3C, and then charged again with a constant voltage of 4.25V until the charging current became 0.05C (cutoff current). After that, each lithium secondary battery was stored at 60°C for 4 weeks, and the amount of gas generated was measured. The amount of gas generated is shown in Table 4 below.
[0115] [Table 4]
[0116] From Table 4 above, it can be seen that in Examples 1 to 3, where the BET specific surface area and average crystallite size of the positive electrode material satisfy the scope of the present invention, the amount of gas generated is less and the initial resistance value is at a similar level or smaller compared to Comparative Examples 1 to 5.
Claims
1. A positive electrode material comprising a positive electrode active material comprising lithium nickel-based oxide particles in the form of secondary particles formed by the aggregation of multiple primary particles, wherein the Ni content among all metals excluding lithium is 50 mol% to 90 mol%, and a coating layer containing boron (B) formed on the surface of the lithium nickel-based oxide particles, The BET specific surface area of the aforementioned positive electrode material is 0.41 m². 2 / g ~ 0.59m 2 / g, A cathode material having an average crystallite size of 155 nm or more.
2. The cathode material according to claim 1, wherein the average crystallite size of the cathode material is 155 nm to 170 nm.
3. The lithium nickel oxide particles are represented by the following chemical formula 1, [Chemical formula 1] Li a [Ni b Co c M 1 d M 2 e ]O 2 In the above chemical formula 1, M 1 M is Mn, Al, or a combination thereof. 2 The positive electrode material according to claim 1, wherein is one or more selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo, and satisfies 0.80 ≤ a ≤ 1.20, 0.50 ≤ b ≤ 0.90, 0 < c ≤ 0.40, 0 < d ≤ 0.40, and 0 ≤ e ≤ 0.
10.
4. The positive electrode material according to claim 1, wherein the boron (B) is contained in an amount of 500 ppm to 1000 ppm based on the total weight of the positive electrode material.
5. The positive electrode material according to claim 1, wherein the residual lithium content of the positive electrode material is 0.2% by weight to 0.4% by weight.
6. The cathode material according to claim 1, wherein the cation mixing rate of the cathode material is 2.5 at% or less.
7. The aforementioned positive electrode material is Average particle size D 50 These are large particles ranging from 6 μm to 20 μm, Average particle size D 50 The positive electrode material according to claim 1, comprising small particles of 0.1 μm to 5.5 μm.
8. The positive electrode material according to claim 7, wherein the large particles and the small particles are contained in a weight ratio of 60:40 to 80:
20.
9. A positive electrode comprising the positive electrode material described in claim 1.
10. A lithium secondary battery comprising the positive electrode described in claim 9.