Positive electrode active material, method for manufacturing the same, and positive electrode and lithium secondary battery containing the same
A lithium composite transition metal oxide with controlled nickel, yttrium, and zirconium content in single-particle form addresses thermal instability and particle cracking issues, enhancing the capacity and lifespan of lithium secondary batteries.
Patent Information
- Application Number
- JP2026526378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-03
- Filing Date
- 2024-10-31
- Publication Date
- 2026-11-24
AI Technical Summary
Conventional lithium nickel composite transition metal oxides used in positive electrodes of lithium secondary batteries suffer from poor thermal stability, particle cracking during manufacturing and charge-discharge processes, leading to increased gas generation and reduced lifespan due to side reactions with the electrolyte, and high production costs.
A positive electrode active material comprising lithium composite transition metal oxide in single-particle form with specific nickel, yttrium, and zirconium content, controlled particle size, and composition, produced through a controlled calcination process, which enhances structural stability and uniformity.
The solution improves the capacity and lifespan characteristics of lithium secondary batteries by reducing particle cracking, side reactions, and maintaining thermal stability, while offering cost-effective production.
Smart Images

Figure 2026539327000001_ABST
Abstract
Description
[Technical Field]
[0001] This application claims priority under Korean Patent Application No. 10-2023-0151119 dated November 3, 2023, and all content disclosed in the documents of the said Korean Patent Application is incorporated herein by reference.
[0002] The present invention relates to a positive electrode active material, a method for producing the same, and a positive electrode and lithium secondary battery containing the same. [Background technology]
[0003] As technological development and demand for mobile devices increase, the demand for rechargeable batteries as an energy source is rapidly growing. Among these rechargeable batteries, lithium-ion batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Lithium-complex transition metal oxides are used as the positive electrode active material for lithium secondary batteries, and among them, lithium-cobalt complex metal oxide (LiCoO2), which has a high operating voltage and excellent capacity characteristics, is mainly used. However, LiCoO2 has very poor thermal properties due to the destabilization of its crystal structure by delithiation, and it is also expensive, so there are limitations to its large-scale use as a power source in fields such as electric vehicles.
[0005] To replace LiCoO2, various materials have been developed, including lithium manganese composite metal oxides (such as LiMnO2 or LiMn2O4), lithium iron phosphate compounds (such as LiFePO4), and lithium nickel composite metal oxides (such as LiNiO2). Among these, research and development on lithium nickel composite metal oxides are particularly active because they have a high reversible capacity of approximately 200 mAh / g and facilitate the realization of high-capacity batteries. However, LiNiO2 has poorer thermal stability than LiCoO2, and if an internal short circuit occurs due to external pressure while charged, the positive electrode active material itself decomposes, leading to battery rupture and fire.
[0006] Therefore, in order to maintain the excellent reversible capacity of LiNiO2 and improve its low thermal stability, nickel-cobalt-manganese lithium composite transition metal oxides in which some of the Ni is replaced with Mn and Co, and nickel-manganese-aluminum lithium composite transition metal oxides in which some of the Ni is replaced with Mn and Al have been developed.
[0007] Conventional nickel-cobalt-manganese lithium composite transition metal oxides typically have a spherical secondary particle morphology, consisting of tens to hundreds of primary particles aggregated together. However, in the case of nickel-cobalt-manganese lithium composite transition metal oxides with this secondary particle morphology, particle cracking, where primary particles detach during the rolling process, is likely to occur during the manufacturing of the positive electrode, and cracks can develop inside the particles during the charge-discharge process. When particle cracking or cracking occurs in the positive electrode active material, the contact area with the electrolyte increases, leading to problems such as increased gas generation due to side reactions with the electrolyte and increased degeneration of the active material.
[0008] On the other hand, in the case of lithium-compound transition metal oxides in which the nickel content among the total metals other than lithium is 50 mol% or more, structural and chemical stability are further reduced, ensuring thermal stability becomes more difficult, and there are also cost issues associated with high heat treatment temperatures.
[0009] Therefore, there is a need to develop positive electrode active materials that can realize lithium secondary batteries with improved capacity and lifespan characteristics. [Prior art documents] [Patent Documents]
[0010] [Patent Document 1] Korean Published Patent Gazette No. 10-2023-0013396 [Overview of the Initiative] [Problems that the invention aims to solve]
[0011] The present invention aims to solve the above-mentioned problems and to provide a positive electrode active material and a method for producing the same that can improve the capacity and life characteristics of a battery.
[0012] Furthermore, the present invention aims to provide a positive electrode and a lithium secondary battery with excellent capacity and lifespan characteristics by including the positive electrode active material described above. [Means for solving the problem]
[0013] (1) The present invention provides a positive electrode active material comprising a lithium composite transition metal oxide in single-particle form consisting of 10 or fewer primary particles, wherein the lithium composite transition metal oxide has a nickel (Ni) content of 50 mol% or more of the total metals other than lithium, contains yttrium (Y) and zirconium (Zr), and the average particle size (D'50) of the primary particles is 2.0 μm or more and 3.5 μm or less.
[0014] (2) The present invention provides a positive electrode active material in which, in the lithium composite transition metal oxide, the nickel (Ni) content among the total metals other than lithium is 59 mol% or more and 70 mol% or less.
[0015] (3) The present invention provides a positive electrode active material in which the lithium composite transition metal oxide has a composition represented by the following chemical formula 1, in (1) or (2) above. [Chemical formula 1] Li 1+x Ni a Co b Mn c Y d Zr e M f O2 In the above chemical formula 1, M is one or more selected from B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La, and -0.1≦x≦0.1, 0.59≦a<1, 0 <b<0.41、0<c<0.41、0<d≦0.1、0<e≦0.1、0≦f≦0.1である。
[0016] (4) The present invention provides a positive electrode active material in any one of (1) to (3) above, wherein the lithium composite transition metal oxide has a single-particle degree (χ) of 0.4 or more according to the following formula 1.
number
[0017] (5) The present invention provides a positive electrode active material in which the degree of single particle formation (χ) is 0.55 or more and 0.65 or less, as described in (4) above.
[0018] (6) The present invention relates to any one of (1) to (5) above, wherein the average particle size (D) of the lithium composite transition metal oxide. 50 The present invention provides a positive electrode active material having a diameter of 2.0 μm or more and 5.0 μm or less.
[0019] (7) The present invention provides a positive electrode active material in which, in any one of (1) to (6) above, the ratio of the area of primary particles with a particle size of 1 μm or less to the total area of primary particles present in the positive electrode active material is 20% or less.
[0020] (8) The present invention provides a positive electrode active material in any one of (1) to (7) above, wherein the yttrium (Y) content in the lithium composite transition metal oxide is 500 ppm or more and 4,000 ppm or less with respect to the total weight of the lithium composite transition metal oxide.
[0021] (9) The present invention provides a positive electrode active material in any one of (1) to (8) above, wherein the zirconium (Zr) content in the lithium composite transition metal oxide is 500 ppm or more and 4,000 ppm or less with respect to the total weight of the lithium composite transition metal oxide.
[0022] (10) A method for producing a positive electrode active material according to any one of (1) to (9) above, comprising the steps of (A) mixing a nickel-containing composite transition metal hydroxide, a lithium (Li)-containing raw material, a yttrium (Y)-containing raw material, and a zirconium (Zr)-containing raw material to produce a mixture, and (B) calcining the mixture to produce a lithium composite transition metal oxide, wherein the calcination is performed at a temperature of 920°C or higher and 980°C or lower.
[0023] (11) The present invention provides a method for producing a positive electrode active material, wherein in step (A) of (10), the yttrium (Y)-containing raw material is mixed such that the yttrium (Y) content is 500 ppm or more and 4,000 ppm or less with respect to the total weight of the composite transition metal hydroxide.
[0024] (12) The present invention provides a method for producing a positive electrode active material, wherein in step (A) of (10) or (11), the zirconium (Zr)-containing raw material is mixed such that the zirconium (Zr) content is 500 ppm or more and 4,000 ppm or less relative to the total weight of the composite transition metal hydroxide.
[0025] (13) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (9) above.
[0026] (14) The present invention provides a lithium secondary battery including a positive electrode according to (13) above. [Effects of the Invention]
[0027] The positive electrode active material according to the present invention contains zirconium (Zr) and yttrium (Y), and by adjusting the particle size of the primary particles, the structural stability of the positive electrode active material and the uniformity of particle size and shape are achieved. As a result, the capacity characteristics and life characteristics of the positive electrode and secondary battery containing the positive electrode active material are improved.
[0028] Furthermore, the method for producing the positive electrode active material of the present invention makes it possible to effectively produce the above-mentioned positive electrode active material. [Brief explanation of the drawing]
[0029] [Figure 1] This is an SEM image of the positive electrode active material produced in Example 1. [Figure 2] This is an SEM image of the positive electrode active material produced in Example 2. [Figure 3] This is an SEM image of the positive electrode active material produced in Comparative Example 1. [Figure 4] This is an SEM image of the positive electrode active material produced in Comparative Example 2. [Figure 5] This is an SEM image of the positive electrode active material produced in Comparative Example 3. [Figure 6] This is an SEM image of the positive electrode active material produced in Comparative Example 4. [Figure 7] This is an SEM image of the positive electrode active material produced in Comparative Example 5. [Figure 8] This is an SEM image of the cathode active material according to one embodiment of the present invention. [Figure 9] This image shows the boundaries of primary particles within a cathode active material, using an SEM image of the cathode active material according to one embodiment of the present invention. [Figure 10] This image shows the boundaries of primary particles within a cathode active material separated by random colors, using an SEM image of a cathode active material according to one embodiment of the present invention. [Modes for carrying out the invention]
[0030] The present invention will be described in more detail below to aid in understanding the present invention.
[0031] The terms and words used herein and in the claims should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather in a manner consistent with the technical idea of the present invention, in accordance with the principle that inventors may define the concepts of terms as appropriate to best describe their invention.
[0032] In this specification, terms such as "comprise", "include" or "have" specify the presence of implemented features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the presence or possibility of addition of one or more other features, numbers, steps, components, or combinations thereof.
[0033] In this specification, the term "on" means to include not only the case where a certain structure is formed immediately on top of another structure, but also the case where a third structure is interposed between these structures.
[0034] In this specification, the "single particle form" is a concept contrasted with the spherical secondary particle form formed by agglomeration of tens to hundreds of primary particles produced by a conventional method, and means a form consisting of 10 or less primary particles. Specifically, in the present invention, the single particle form may be a single particle consisting of one primary particle, or may be a secondary particle form in which several primary particles are agglomerated.
[0035] In this specification, the "primary particle" means the minimum unit of particles recognized when observing the positive electrode active material using a scanning electron microscope (SEM), and the "secondary particle" means a secondary structure formed by agglomeration of a plurality of primary particles.
[0036] In this specification, the content of each element in the lithium composite transition metal oxide can be measured by ICP (Inductive Coupled Plasma) analysis using an inductively coupled plasma optical emission spectrometer (ICP-OES; Aligent5110, manufactured by Aligent).
[0037] In this specification, the average particle size (D of the lithium composite transition metal oxide 50Each of these can be defined as the particle size corresponding to 50% of the cumulative volume distribution in the particle size distribution curve (graph curve of the particle size distribution diagram). The average particle size of the lithium composite transition metal oxide can be measured by dispersing the powder to be measured in a dispersion medium, introducing it into a commercially available laser diffraction particle size analyzer (for example, Microtrac's S3500), measuring the difference in diffraction patterns due to particle size as the particles pass through the laser beam to calculate the particle size distribution, and then calculating the particle size at the point where the cumulative volume distribution by particle size in the measuring device reaches 50%.
[0038] In this specification, the particle size of a primary particle may be calculated by determining the area of each primary particle based on the number of pixels corresponding to each of the n primary particles present in the SEM image, and then using the radius of a circle having the same area as the area of each primary particle to calculate the particle size of each primary particle present in the SEM image. In this specification, the average particle size of the primary particles (D') 50 ) can be defined as the particle size that corresponds to 50% of the volume cumulative distribution in the particle size distribution curve (graph curve of the particle size distribution diagram). The average particle size (D') of the primary particles. 50 The particle diameter can be measured by first determining the volume of a sphere with a radius equal to half the particle size of the primary particle, and then calculating the particle diameter at the point where the cumulative volume distribution by particle size, calculated from the volume of the primary particle, reaches 50%.
[0039] In this specification, fine powder is defined as primary particles whose particle size is 1 μm or less, calculated by determining the area of each primary particle based on the number of pixels corresponding to each of the n primary particles present in the SEM image, and then calculating the particle size of each primary particle present in the SEM image using the radius of a circle having the same area as the area of each primary particle.
[0040] positive electrode active material The positive electrode active material according to the present invention will be described below.
[0041] The positive electrode active material according to the present invention comprises a lithium composite transition metal oxide in single-particle form consisting of 10 or fewer primary particles, wherein the lithium composite transition metal oxide has a nickel (Ni) content of 50 mol% or more of the total metals other than lithium, and also contains yttrium (Y) and zirconium (Zr), and the average particle size (D') of the primary particles is 50 The diameter is between 2.0 μm and 3.5 μm.
[0042] The lithium composite transition metal oxide is in a single-particle form consisting of 10 or fewer primary particles. That is, the lithium composite transition metal oxide is in the form of a single particle or a single particle formed by the aggregation of 2 to 10 particles. The single-particle form is distinguished from secondary particles formed by the aggregation of more than 10 primary particles. When the lithium composite transition metal oxide has a single-particle form, it has excellent stability, and even when the positive electrode active material containing it is rolled, the positive electrode active material does not crack or break, and side reactions between the positive electrode active material and the electrolyte can be reduced. As a result, durability against volume changes during battery charging and discharging can be improved, and the lifespan characteristics can be improved. When the lithium composite transition metal oxide is in a secondary-particle form, the positive electrode active material containing it cracks or breaks, and there is a problem of poor lifespan characteristics due to side reactions between the positive electrode active material and the electrolyte.
[0043] The primary particles that make up the single particle have an average particle size (D' 50 The particle size is 2.0 μm or more and 3.5 μm or less. Specifically, the primary particles have an average particle size (D' 50 The average particle size (D') of the primary particles may be 2.0 μm or larger, 2.1 μm or larger, 2.2 μm or larger, 2.3 μm or larger, 2.4 μm or larger, or 2.5 μm or larger, and may be 2.6 μm or smaller, 2.7 μm or smaller, 2.8 μm or smaller, 2.9 μm or smaller, 3.0 μm or smaller, 3.1 μm or smaller, 3.2 μm or smaller, 3.3 μm or smaller, 3.4 μm or smaller, or 3.5 μm or smaller. 50 When the average particle size (D') of the primary particles is within the above range, side reactions between the positive electrode active material and the electrolyte can be reduced, improving lifetime characteristics, and the lithium diffusion pathway within the particles can be shortened, improving resistance characteristics. 50If the average particle size (D') of the primary particles is less than 2.0 μm, the area of the grain boundaries in contact with the electrolyte is large, and there is a problem that the lifespan characteristics of the secondary battery are poor due to the generation of gas due to side reactions with the electrolyte. 50 If the particle size exceeds 3.5 μm, there is a problem where the lithium diffusion path inside the particle is long, resulting in poor resistance characteristics.
[0044] The aforementioned lithium composite transition metal oxide has a nickel (Ni) content of 50 mol% or more among the total metals other than lithium. When the nickel (Ni) content is within the aforementioned range, the capacity characteristics of the positive electrode active material can be improved. Specifically, when the Ni content is between 59 mol% and 70 mol%, the lifetime characteristics can be maintained while the capacity characteristics can be improved. When the nickel (Ni) content among the total metals other than lithium is less than 50 mol%, there is a problem of inferior charge-discharge capacity of the positive electrode active material.
[0045] The present inventors have found that when a lithium composite transition metal oxide, in which the nickel (Ni) content among the total metals other than lithium is 50 mol% or more, contains yttrium (Y) and zirconium (Zr), specifically when yttrium (Y) is doped, the yttrium (Y) ions in the positive electrode active material structure are Y 3+ It exists in form, Y 3+ O has a bonding strength with oxygen of 512 kJ / mol, while Ni has a bonding strength with oxygen of 392 kJ / mol. 2+ -Co has a bonding strength of 368 kJ / mol with oxygen. 3+ -O has a stronger bonding force with oxygen, which can improve structural stability, Y 3+ Ni is found in the tetrahedral sites within the structure. 2+ By suppressing cation mixing, which leads to greater stability, structural stability can be improved, and it has been found that acting as a flux can make the particle size and shape of the positive electrode active material uniform. Furthermore, when zirconium (Zr) is doped, the zirconium (Zr) ions in the positive electrode active material structure are Zr 4+ It exists in form, Ni 3+ Part of Ni2+ By changing it, the charging and discharging capacity can be increased, and zirconium (Zr) ions occupy the lithium ion sites, Ni 2+ We discovered that by suppressing the diffusion of to lithium ion sites, structural stability can be improved by suppressing deformation from a layered structure to a spinel structure. This led to the discovery that life characteristics at high temperatures and high voltages can be improved, thus completing the present invention. On the other hand, when a lithium composite transition metal oxide contains 50 mol% or more nickel (Ni) among the total metals other than lithium, and does not contain yttrium (Y) or zirconium (Zr), the particle shape of the lithium composite transition metal oxide is not uniform, the particle size is non-uniform, and there are problems with capacity characteristics and life characteristics.
[0046] According to one embodiment of the present invention, the lithium composite transition metal oxide has a composition represented by the following chemical formula 1.
[0047] [Chemical formula 1] Li 1+x Ni a Co b Mn c Y d Zr e M f O2
[0048] In the aforementioned chemical formula 1, M is one or more elements selected from B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La. -0.1≦x≦0.1, 0.59≦a<1, 0 <b<0.41、0<c<0.41、0<d≦0.1、0<e≦0.1、0≦f≦0.1である。
[0049] The aforementioned M is a doping element, and specifically, M may be one or more selected from B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La. The aforementioned M is not necessarily included, but when included in an appropriate amount, the particle shape of the positive electrode active material can be improved and the stability of the crystal structure can be enhanced.
[0050] According to one embodiment of the present invention, the lithium composite transition metal oxide may contain only one M selected from B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La. When M contains only one selected from B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La, M is appropriately substituted for the transition metal and lithium ion sites, which has the effect of improving the capacity characteristics.
[0051] On the other hand, x may be -0.1 or greater, -0.09 or greater, -0.08 or greater, -0.07 or greater, -0.06 or greater, -0.05 or greater, -0.04 or greater, -0.03 or greater, -0.02 or greater, -0.01 or greater, 0 or greater, 0.01 or greater, or 0.02 or greater, and may be 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.1 or less. When x satisfies the above range, high capacity characteristics and high energy density per unit volume can be achieved.
[0052] The above a is the mole fraction of nickel (Ni) among the total metals other than lithium in the lithium composite transition metal oxide, and may be 0.59 or more, and may be 0.60 or less, 0.61 or less, 0.62 or less, 0.63 or less, 0.64 or less, 0.65 or less, 0.66 or less, 0.67 or less, 0.68 or less, 0.69 or less, 0.7 or less, 0.8 or less, 0.9 or less, or less than 1. When a is within the above range, the capacity characteristics of the positive electrode active material can be improved. In particular, when a is 0.59 or more and 0.7 or less, it is possible to have superior price competitiveness and improve the structural stability and thermal stability of the positive electrode active material.
[0053] The above b is the mole fraction of cobalt (Co) among the total metals other than lithium in the lithium composite transition metal oxide, and may be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, or 0.04 or more, and may be 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, 0.1 or less, 0.2 or less, 0.25 or less, 0.3 or less, 0.35 or less, or less than 0.41. When b satisfies the above range, the output characteristics can be improved during the charge and discharge process.
[0054] The above-mentioned c is the mole fraction of manganese (Mn) among the total metals other than lithium in the lithium composite transition metal oxide, and may be greater than 0, 0.1 or more, 0.15 or more, 0.2 or more, 0.25 or more, 0.3 or more, 0.31 or more, 0.32 or more, 0.33 or more, or 0.34 or more, and may be 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.41. When c satisfies the above range, structural stability is increased and the decomposition reaction of the electrolyte can be relatively reduced.
[0055] The above d is the mole fraction of yttrium (Y) among the total metals other than lithium in the lithium composite transition metal oxide, and may be greater than 0, 0.0001 or more, 0.0002 or more, 0.0003 or more, 0.0004 or more, 0.0005 or more, 0.0006 or more, 0.0007 or more, 0.0008 or more, 0.0009 or more, 0.001 or more, or 0.002 or more, and may be 0.003 or less, 0.004 or less, 0.005 or less, 0.006 or less, 0.007 or less, 0.008 or less, 0.009 or less, 0.01 or less, 0.02 or less, 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.1 or less. When d satisfies the above range, the structural stability of the positive electrode active material can be improved. Specifically, the yttrium (Y) ions in the positive electrode active material structure are Y 3+ It exists in form, Y 3+ -O has a bonding strength with oxygen of 512 kJ / mol, and Ni has a bonding strength with oxygen of 392 kJ / mol. 2+-Co has a bonding strength of 368 kJ / mol with oxygen. 3+ Because it has a stronger bond with oxygen than -O, it can improve structural stability, and Ni can form at tetrahedral sites within the structure. 2+ Because it is more stable, cation mixing is suppressed, and structural stability can be improved. In addition, it acts as a flux, making the particle size and shape of the positive electrode active material uniform.
[0056] The above e is the mole fraction of zirconium (Zr) among the total metals other than lithium in the lithium composite transition metal oxide, and may be greater than 0, 0.0001 or more, 0.0002 or more, 0.0003 or more, 0.0004 or more, 0.0005 or more, 0.0006 or more, 0.0007 or more, 0.0008 or more, 0.0009 or more, or 0.001 or more, and may be 0.002 or less, 0.003 or less, 0.004 or less, 0.005 or less, 0.006 or less, 0.007 or less, 0.008 or less, 0.009 or less, 0.01 or less, 0.02 or less, 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.1 or less. When e satisfies the above range, the capacity characteristics and lifetime characteristics of the positive electrode active material can be improved. Specifically, the zirconium (Zr) ions in the positive electrode active material structure are Zr 4+ It exists in form, Ni 3+ Part of Ni 2+ By changing it, the charging and discharging capacity can be increased. Also, zirconium (Zr) ions can occupy lithium ion sites, Ni 2+ By suppressing diffusion to lithium ion sites, deformation from a layered structure to a spinel structure is inhibited, thereby improving structural stability. Furthermore, it acts as a flux, making the particle size and shape of the positive electrode active material uniform. This improves lifetime characteristics at high temperatures and high voltages.
[0057] The above f is the mole fraction of M among the total metals other than lithium in the lithium composite transition metal oxide, and may be 0 or more, 0.001 or more, 0.002 or more, or 0.003 or more, and may be 0.004 or less, 0.005 or less, 0.006 or less, 0.007 or less, 0.008 or less, 0.009 or less, 0.01 or less, 0.02 or less, 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.1 or less. When f satisfies the above range, the stability of the positive electrode active material crystal structure is improved and the grain shape can be improved.
[0058] The terms a, b, c, d, e, and f may also be a+b+c+d+e+f=1.
[0059] In this invention, the degree of single-particle formation is evaluated and expressed by the parameter shown in the following formula 1. The degree of single-particle formation as used in this invention is the average particle size (D') of the primary particles that make up a single particle. 50 ) and the average particle size (D) of lithium composite transition metal oxides which are single particles 50 This value is adjusted according to the average particle size (D') of the primary particles present in the lithium composite transition metal oxide. 50 ) is the average particle size (D) of lithium composite transition metal oxides. 50 The closer it is to ), the higher the degree of single-particle separation.
[0060] For example, the maximum value of the single-particle degree is 1, which means that one single particle consists of one primary particle.
[0061] According to one embodiment of the present invention, the lithium composite transition metal oxide may have a degree of single-particle formation (χ) of 0.4 or higher according to the following formula 1.
[0062]
number
[0063] The degree of single-particle formation (χ) may be 0.4 or higher, 0.45 or higher, 0.5 or higher, 0.55 or higher, 0.56 or higher, 0.57 or higher, 0.58 or higher, 0.59 or higher, or 0.6 or higher, and may also be 0.61 or lower, 0.62 or lower, 0.63 or lower, 0.64 or lower, 0.65 or lower, 0.66 or lower, 0.67 or lower, 0.68 or lower, 0.69 or lower, 0.7 or lower, 0.71 or lower, 0.72 or lower, 0.73 or lower, 0.74 or lower, or 0.75 The following ranges may also be 0.76 or less, 0.77 or less, 0.78 or less, 0.79 or less, 0.8 or less, 0.81 or less, 0.82 or less, 0.83 or less, 0.84 or less, 0.85 or less, 0.86 or less, 0.87 or less, 0.88 or less, 0.89 or less, 0.91 or less, 0.92 or less, 0.93 or less, 0.94 or less, 0.95 or less, 0.96 or less, 0.97 or less, 0.98 or less, 0.99 or less, or 1 or less. When the above ranges are satisfied, it can be seen that the lithium composite transition metal oxide of the present invention is in a single-particle form in which aggregation between particles is suppressed. As a result, structural stability is improved, particle cracking is suppressed when rolling for electrode manufacturing or when driving cells, the grain boundary area in contact with the electrolyte is reduced, the generation of gas due to side reactions with the electrolyte is reduced, and the life characteristics of secondary batteries can be improved. In particular, when the degree of single-particle formation is 0.55 or higher and 0.65 or lower, the capacity characteristics and lifetime characteristics can be improved.
[0064] According to one embodiment of the present invention, the average particle size (D) of the lithium composite transition metal oxide is 50 The average particle size (D) of the lithium composite transition metal oxide may be 2.0 μm or more and 5.0 μm or less. Specifically, the average particle size (D) of the lithium composite transition metal oxide may be 2.0 μm or more and 5.0 μm or less. 50The average particle size (D) of the lithium composite transition metal oxide may be 2.0 μm or larger, 2.1 μm or larger, 2.2 μm or larger, 2.3 μm or larger, 2.4 μm or larger, 2.5 μm or larger, 2.6 μm or larger, 2.7 μm or larger, 2.8 μm or larger, 2.9 μm or larger, 3.0 μm or larger, 3.1 μm or larger, 3.2 μm or larger, 3.3 μm or larger, 3.4 μm or larger, 3.5 μm or larger, 3.6 μm or larger, 3.7 μm or larger, 3.8 μm or larger, 3.9 μm or larger, 4.0 μm or larger, or 4.1 μm or larger, and may be 4.2 μm or smaller, 4.3 μm or smaller, 4.4 μm or smaller, 4.5 μm or smaller, 4.6 μm or smaller, 4.7 μm or smaller, 4.8 μm or smaller, 4.9 μm or smaller, or 5.0 μm or smaller. 50 When the above range is present, an excellent electrode density can be achieved, and capacitance characteristics can be improved.
[0065] According to one embodiment of the present invention, the ratio of the area of primary particles with a particle size of 1 μm or less to the total area of primary particles present in the positive electrode active material may be 20% or less. Specifically, the ratio of the area of primary particles with a particle size of 1 μm or less to the total area of primary particles present in the positive electrode active material may be 10% or less, 11% or less, 12% or less, 13% or less, 14% or less, 15% or less, 16% or less, 17% or less, 18% or less, 19% or less, or 20% or less. The ratio can serve as a measure of particle growth. The closer the ratio is to 0, the fewer primary particles have not yet completed their growth. The more particles that have not yet completed their growth, i.e., fine powder, there are, the more the lifetime characteristics can deteriorate due to side reactions with the electrolyte, the more gas is generated, and the lower the stability can be. When the ratio is within the range, gas generation due to side reactions with the electrolyte is reduced, degeneration is suppressed, and stability can be improved.
[0066] According to one embodiment of the present invention, the yttrium (Y) content in the lithium composite transition metal oxide may be 500 ppm or more and 4,000 ppm or less relative to the total weight of the lithium composite transition metal oxide. Specifically, the yttrium (Y) content in the lithium composite transition metal oxide may be 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, 900 ppm or more, 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, 1,400 ppm or more, 1,500 ppm or more, 1,600 ppm or more, 1,700 ppm or more, 1,800 ppm or more, 1,900 ppm or more, 2,000 ppm or more, and 2,100 ppm relative to the total weight of the lithium composite transition metal oxide. The yttrium (Y) content may be m or more, 2,200 ppm or more, 2,300 ppm or more, 2,400 ppm or more, 2,500 ppm or more, 2,600 ppm or more, or 2,700 ppm or more, and may be 2,800 ppm or less, 2,900 ppm or less, 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less. When the yttrium (Y) content is within the above range, the structural stability of the positive electrode active material can be improved. Specifically, the yttrium (Y) ions in the positive electrode active material structure are Y 3+ It exists in form, Y 3+ -O has a bonding strength with oxygen of 512 kJ / mol, and Ni has a bonding strength with oxygen of 392 kJ / mol. 2+ -Co has a bonding strength of 368 kJ / mol with oxygen. 3+ Because it has a stronger bond with oxygen than -O, it can improve structural stability. Also, at the tetrahedral sites within the structure, Ni 2+ Because it is more stable, cation mixing is suppressed, and structural stability can be improved. In addition, it acts as a flux, making the particle size and shape of the positive electrode active material uniform.
[0067] According to one embodiment of the present invention, the zirconium (Zr) content in the lithium composite transition metal oxide may be 500 ppm or more and 4,000 ppm or less relative to the total weight of the lithium composite transition metal oxide. Specifically, the zirconium (Zr) content in the lithium composite transition metal oxide may be 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, 900 ppm or more, 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, or 1,300 ppm or more relative to the total weight of the lithium composite transition metal oxide, and may be 1,400 ppm or less, 1,500 ppm or less, 1,600 ppm or less, 1,700 ppm or less, 1,800 ppm or less, 1,900 ppm or less, or 2,000 ppm or less. The zirconium (Zr) content may be less than or equal to m, less than or equal to 2,100 ppm, less than or equal to 2,200 ppm, less than or equal to 2,300 ppm, less than or equal to 2,400 ppm, less than or equal to 2,500 ppm, less than or equal to 2,600 ppm, less than or equal to 2,700 ppm, less than or equal to 2,800 ppm, less than or equal to 2,900 ppm, less than or equal to 3,000 ppm, less than or equal to 3,100 ppm, less than or equal to 3,200 ppm, less than or equal to 3,300 ppm, less than or equal to 3,400 ppm, less than or equal to 3,500 ppm, less than or equal to 3,600 ppm, less than or equal to 3,700 ppm, less than or equal to 3,800 ppm, less than or equal to 3,900 ppm, or less than or equal to 4,000 ppm. When the zirconium (Zr) content is within the above range, the capacity characteristics and lifetime characteristics of the positive electrode active material can be improved. Specifically, the zirconium (Zr) ions in the positive electrode active material structure are Zr 4+ It exists in form, Ni 3+ Part of Ni 2+ By changing it, the charging and discharging capacity can be increased. Also, zirconium (Zr) ions can occupy lithium ion sites, Ni 2+ By suppressing diffusion to lithium ion sites, deformation from a layered structure to a spinel structure is inhibited, thereby improving structural stability. Furthermore, it acts as a flux, making the particle size and shape of the positive electrode active material uniform. This can improve lifetime characteristics at high temperatures and high voltages.
[0068] Method for manufacturing positive electrode active material Next, the method for producing the positive electrode active material of the present invention will be described. The method for producing the positive electrode active material of the present invention is the method for producing the positive electrode active material according to the present invention.
[0069] The method for producing a positive electrode active material according to the present invention includes the steps of (A) mixing a nickel-containing composite transition metal hydroxide, a lithium (Li)-containing raw material, a yttrium (Y)-containing raw material, and a zirconium (Zr)-containing raw material to produce a mixture, and (B) calcining the mixture to produce a lithium composite transition metal oxide.
[0070] The positive electrode active material according to the present invention described above can be manufactured by appropriately adjusting the type of raw material, the mixing ratio of the raw material, the firing step, the firing atmosphere, and so on.
[0071] The steps of the present invention will be described in detail below.
[0072] (A) Step The present invention relates to a method for producing a positive electrode active material, which includes step (A) of mixing a nickel-containing composite transition metal hydroxide, a lithium (Li)-containing raw material, a yttrium (Y)-containing raw material, and a zirconium (Zr)-containing raw material to produce a mixture.
[0073] Specifically, the mixing can be carried out by dry mixing or wet mixing. When the components are mixed by dry mixing, the calcination process can be performed without a separate drying step. When the components are mixed by wet mixing, they can be produced by adding them to a mixture of water and a solvent, specifically water, or an organic solvent that can be uniformly mixed with water (specifically, alcohol, etc.), or by producing a solution containing each raw material, specifically an aqueous solution, mixing these solutions, spray-drying the mixed components, and then performing the calcination process. Each raw material and composite transition metal hydroxide can be used in appropriate amounts, taking into account the content of each metal element in the final lithium composite transition metal oxide produced.
[0074] The aforementioned complex transition metal hydroxide can be produced by a coprecipitation reaction in which an aqueous solution of the complex transition metal, an ammonium cation complex, and a basic compound are introduced into a reactor.
[0075] The aforementioned complex transition metal aqueous solution can be produced by dissolving a transition metal-containing raw material in a solvent such as water. For example, it can be produced by dissolving nickel (Ni), cobalt (Co), or manganese (Mn)-containing raw material in water. That is, the complex transition metal-containing solution contains nickel (Ni), cobalt (Co), and manganese (Mn). Furthermore, if necessary, the complex transition metal-containing solution may further contain metal-containing raw material that contains a transition metal other than nickel (Ni), cobalt (Co), and manganese (Mn) (for example, one or more selected from Y, Zr, B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La).
[0076] The nickel (Ni)-containing raw material may be at least one selected from the group consisting of NiO, Ni(OH)2, NiO·OH, NiCO3·2Ni(OH)2·4H2O, NiC2O4·2H2O, Ni(NO3)2·6H2O, fatty acid nickel, and nickel halides, and one or more of these can be used as a mixture.
[0077] The cobalt (Co)-containing raw material may be at least one selected from the group consisting of Co(OH)2, CO3O4, CoO·OH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, or Co(SO4)2·7H2O, fatty acid cobalt, and cobalt halides, and one or more of these can be used as a mixture.
[0078] The manganese (Mn)-containing raw material may be at least one selected from the group consisting of MnCO3, Mn2O3, MnO2, Mn3O4, Mn(NO3)2, manganese acetate, manganese dicarboxylate, manganese citrate, manganese salts of fatty acid manganese, oxyhydroxides, and halides of manganese chloride, and one or more of these can be used as a mixture.
[0079] Nickel (Ni), cobalt (Co), manganese (Mn), and other raw materials can be used in appropriate amounts, taking into account the content of each metal element in the resulting composite transition metal hydroxide.
[0080] On the other hand, the ammonium cation complex-forming agent may contain at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3, and the compound may be introduced into the reactor in the form of a solution in which it is dissolved in a solvent. Here, the solvent may be water, or a mixture of water and an organic solvent that can be homogeneously mixed with water (specifically, an alcohol, etc.).
[0081] The basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and the compound can be introduced into the reactor in the form of a solution in which it is dissolved in a solvent. Here, the solvent can be water, or a mixture of water and an organic solvent that can be homogeneously mixed with water (specifically, an alcohol, etc.).
[0082] As described above, when a complex transition metal aqueous solution, an ammonium cation complex-forming agent, and a basic compound are added to the reactor, the transition metal in the complex transition metal aqueous solution undergoes a coprecipitation reaction to generate precursor particles in the form of complex transition metal hydroxides.
[0083] Here, the basic compound can be added in an amount such that the pH of the reaction solution falls within the desired range.
[0084] When the precursor particles are formed by the method as described above, the particles are separated from the reaction solution to obtain a composite transition metal hydroxide. Specifically, after filtering the reaction solution to separate the precursor particles from the reaction solution, the separated precursor particles are washed with water and dried to obtain the composite transition metal hydroxide. Here, if necessary, processes such as pulverization and / or classification may be performed.
[0085] The composite transition metal hydroxide is Ni p Co q Mn r M 1 s (OH)2 (where M 1 is at least one selected from the group consisting of Y, Zr, B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La, and p, q, r, and s satisfy 0.59 ≤ p < 1, 0 < q < 0.41, 0 < r < 0.41, and 0 ≤ s ≤ 0.1).
[0086] The lithium (Li)-containing source material may be at least one selected from the group consisting of LiOH, Li2CO3, LiNO3, LiNO2, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, lithium acetate, lithium dicarboxylate, lithium citrate, lithium fatty acid salt, alkyl lithium, and lithium halide, and one or a mixture of two or more of these may be used. Specifically, LiOH or Li2CO3 may be used.
[0087] The yttrium (Y)-containing source material may be at least one selected from the group consisting of Y2O3, Y2(CO3)3·xH2O, Y(C5H7O2)3·xH2O, (CH3CO2)3Y·xH2O, Y(OH)3·xH2O, Y2(SO4)3·8H2O, and Y(NO3)3·xH2O, and one or a mixture of two or more of these may be used. Specifically, considering process convenience, Y2O3 may be used.
[0088] The zirconium (Zr)-containing raw material may be at least one selected from the group consisting of ZrO2, Zr(OH)4, Zr(OC2H5)4, Zr(SO4)2·xH2O, and Zr[OC(CH3)3]4, and one or more of these can be used as a mixture. Specifically, considering the convenience of the process, ZrO2 can be used.
[0089] According to one embodiment of the present invention, the yttrium (Y)-containing raw material may be mixed such that the yttrium (Y) content is 500 ppm or more and 4,000 ppm or less relative to the total weight of the composite transition metal hydroxide. Specifically, the yttrium (Y)-containing raw material may contain 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, 900 ppm or more, 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, or 1,400 ppm or more, and 1,500 ppm or less, 1,600 ppm or less, 1,700 ppm or less, 1,800 ppm or less, 1,900 ppm or less, 2,000 ppm or less, or 2,100 ppm relative to the total weight of the composite transition metal hydroxide. The materials may be mixed to contain yttrium (Y) or less, 2,200 ppm or less, 2,300 ppm or less, 2,400 ppm or less, 2,500 ppm or less, 2,600 ppm or less, 2,700 ppm or less, 2,800 ppm or less, 2,900 ppm or less, 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less. When the amount of yttrium (Y)-containing raw material added is within the above range, the structural stability of the positive electrode active material can be improved. Specifically, the yttrium (Y) ions in the positive electrode active material structure are Y 3+ It exists in form, Y 3+ -O has a bonding strength with oxygen of 512 kJ / mol, and Ni has a bonding strength with oxygen of 392 kJ / mol. 2+ -Co has a bonding strength of 368 kJ / mol with oxygen. 3+Because it has a stronger bonding force with oxygen than with -O, it can improve structural stability. Ni at the tetrahedral site within the structure 2+ Because it is more stable, cation mixing is suppressed, and structural stability can be improved. In addition, it acts as a flux, making the particle size and shape of the positive electrode active material uniform.
[0090] According to one embodiment of the present invention, the zirconium (Zr)-containing raw material may be mixed such that the zirconium (Zr) content is 500 ppm or more and 4,000 ppm or less relative to the total weight of the composite transition metal hydroxide. Specifically, the zirconium (Zr)-containing raw material may be mixed such that the zirconium (Zr) content is 500 ppm or more, 600 ppm or more, 700 ppm or more, 800 ppm or more, 900 ppm or more, 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, 1,400 ppm or more, 1,500 ppm or more, 1,600 ppm or more, 1,700 ppm or more, 1,800 ppm or more, 1,900 ppm or more, 2,000 ppm or more, 2,100 ppm or more, relative to the total weight of the composite transition metal hydroxide. The materials may be mixed to contain 2,200 ppm or more, 2,300 ppm or more, 2,400 ppm or more, 2,500 ppm or more, 2,600 ppm or more, 2,700 ppm or more, 2,800 ppm or more, or 2,900 ppm or more, and 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less. When the amount of the zirconium (Zr)-containing raw material mixed is within the above range, the capacity characteristics and lifetime characteristics of the positive electrode active material can be improved. Specifically, the zirconium (Zr) ions in the positive electrode active material structure are Zr 4+ It exists in form, Ni 3+ Part of Ni 2+By changing it, the charging and discharging capacity can be increased. Also, zirconium (Zr) ions can occupy lithium ion sites, Ni 2+ By suppressing diffusion to lithium ion sites, deformation from a layered structure to a spinel structure is inhibited, thereby improving structural stability. Furthermore, it acts as a flux, making the particle size and shape of the positive electrode active material uniform. This improves lifetime characteristics at high temperatures and high voltages.
[0091] According to one embodiment of the present invention, in step (A), a nickel-containing composite transition metal hydroxide, a lithium (Li)-containing raw material, a yttrium (Y)-containing raw material, and a zirconium (Zr)-containing raw material can be mixed in amounts such that they have the composition represented by the chemical formula 1.
[0092] (B) Step The method for producing a positive electrode active material according to the present invention includes, after step (A), step (B) of calcining the mixture to produce a lithium composite transition metal oxide.
[0093] The aforementioned firing may be carried out at temperatures of 920°C or higher and 980°C or lower. Specifically, the firing may be carried out at temperatures of 920°C or higher, 930°C or higher, 940°C or higher, and 950°C or lower, 960°C or lower, or 970°C or lower. By firing in this manner, lithium composite transition metal oxide in single-particle form can be formed. When lithium composite transition metal oxide is in single-particle form, there are fewer particle interfaces, and during rolling, deterioration due to particle cracking at the interface or side reactions with the electrolyte can be suppressed. This makes it possible to improve the life characteristics of secondary batteries, especially at high voltages. On the other hand, when the firing is carried out at temperatures below 920°C, sufficient thermal energy is not supplied for the formation of lithium composite transition metal oxide in single-particle form, and sufficient thermal energy necessary for the growth of primary particles is not supplied. When the firing is carried out at temperatures above 980°C, over-firing occurs, generating a rock salt phase, which leads to excessive growth of primary particles and the problem of agglomeration.
[0094] The aforementioned firing may be carried out for a period of 6 hours or more and 20 hours or less. When this range is met, highly crystalline particles with an appropriate size can be obtained, resulting in excellent production efficiency.
[0095] The aforementioned firing may be carried out in an air atmosphere, an oxidizing atmosphere, or an inactive atmosphere.
[0096] positive electrode Next, the positive electrode according to the present invention will be described.
[0097] The positive electrode according to the present invention includes a positive electrode active material layer containing the positive electrode active material according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, which contains the positive electrode active material. Since the positive electrode active material has been described above, a detailed explanation will be omitted, and only the remaining components will be described in detail below.
[0098] The positive electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and is conductive. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., can be used. The positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to improve the adhesion of the positive electrode active material. For example, it may be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0099] The positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material. Here, the positive electrode active material can be included in an amount of 80% to 99% by weight, more specifically 85% to 98.5% by weight, relative to the total weight of the positive electrode active material layer, and within this range, excellent capacitance characteristics can be observed.
[0100] The conductive material is used to impart conductivity to the electrodes and can be used without particular limitations in the battery it is configured in, as long as it does not cause chemical changes and has electronic conductivity. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. Of these, one or more can be used. The conductive material can be included in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.
[0101] The binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more can be used. The binder can be included in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.
[0102] The positive electrode can be manufactured by a conventional method for manufacturing a positive electrode, except that the positive electrode active material described above is used. Specifically, the positive electrode can be manufactured by coating a positive electrode active material layer-forming composition, which is prepared by dissolving or dispersing the positive electrode active material and, selectively, a binder and a conductive material in a solvent, onto a positive electrode current collector, followed by drying and rolling. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above. Alternatively, the positive electrode can also be manufactured by casting the positive electrode active material layer-forming composition onto another support, peeling it off this support, and then laminating the resulting film onto a positive electrode current collector.
[0103] The solvent may be any solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more can be used. The amount of solvent used should be sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to have a viscosity that allows for excellent thickness uniformity when applied for the manufacture of the positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0104] Lithium-ion battery Next, the lithium secondary battery according to the present invention will be described.
[0105] The present invention makes it possible to manufacture an electrochemical element including the positive electrode. Specifically, the electrochemical element may be a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.
[0106] The lithium secondary battery specifically includes a positive electrode, a negative electrode located opposite the positive electrode, and a separator and electrolyte interposed between the positive and negative electrodes. As the positive electrode has been described previously, a detailed explanation will be omitted, and only the remaining components will be described in detail below.
[0107] Furthermore, the lithium secondary battery may selectively further include a battery container for housing the electrode assembly comprising the positive electrode, negative electrode, and separator, and a sealing member for sealing the battery container.
[0108] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0109] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloys can be used. The negative electrode current collector can usually have a thickness of 3 μm to 500 μm, and, similar to the positive electrode current collector, fine irregularities can be formed on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it can be used in various forms such as film, sheet, foil, mesh, porous material, foam, and nonwoven fabric.
[0110] The negative electrode active material layer selectively includes a binder and a conductive material together with the negative electrode active material.
[0111] As the negative electrode active material, compounds capable of reversible intercalation and deintercalation of lithium can be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO2. βExamples include metallic oxides that can be doped and dedoped with lithium, such as (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compound and carbonaceous material, such as Si-C composites or Sn-C composites; and any one or more mixtures thereof can be used. A metallic lithium thin film can also be used as the negative electrode active material. Furthermore, both low-crystallinity carbon and high-crystallinity carbon can be used as the carbon material. Examples of low-crystalline carbon include soft carbon and hard carbon, while examples of high-crystalline carbon include amorphous, plate-like, flaky, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0112] The anode active material can be present in an amount of 80% to 99% by weight relative to the total weight of the anode active material layer.
[0113] The binder is a component that helps to bond the conductive material, active material, and current collector, and is usually added in an amount of 0.1% to 10% by weight relative to the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0114] The conductive material is a component for further improving the conductivity of the negative electrode active material, and can be added in an amount of 10% by weight or less, specifically 5% by weight or less, relative to the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives can be used.
[0115] The negative electrode active material layer can be manufactured by coating a negative electrode active material layer-forming composition, which is prepared by dissolving or dispersing a negative electrode active material and, selectively, a binder and a conductive material in a solvent, onto a negative electrode current collector and drying it, or by casting the negative electrode active material layer-forming composition onto another support, peeling it off the support, and then laminating the resulting film onto the negative electrode current collector.
[0116] On the other hand, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Generally, any separator used in lithium secondary batteries can be used without particular limitations, but those with low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity are particularly preferred. Specifically, porous polymer films, such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or laminated structures of two or more layers thereof can be used. Ordinary porous nonwoven fabrics, such as nonwoven fabrics made of high-melting-point glass fibers or polyethylene terephthalate fibers, can also be used. Furthermore, coated separators containing ceramic components or polymeric substances can be used to ensure heat resistance or mechanical strength, and may be selectively used in single-layer or multi-layer structures.
[0117] Furthermore, the electrolytes used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0118] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0119] The organic solvent can be used without particular limitations, as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvents include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (propylene Carbonate solvents such as carbonate (PC); alcoholic solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms, and can include a double-bonded aromatic ring or ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, carbonate solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery, and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred. In this case, mixing the cyclic carbonate and linear carbonate in a volume ratio of about 1:1 to about 1:9 can improve the performance of the electrolyte.
[0120] The lithium salt can be any compound capable of providing lithium ions for use in lithium secondary batteries, without any particular limitations. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, etc. The concentration of the lithium salt is preferably in the range of 0.1 to 5.0 M, specifically 0.1 to 3.0 M. When the concentration of the lithium salt falls within this range, the electrolyte has appropriate conductivity and viscosity, exhibiting excellent electrolyte performance and allowing lithium ions to move effectively.
[0121] In addition to the components of the electrolyte, the electrolyte may further contain one or more additives for purposes such as improving battery life characteristics, suppressing battery capacity reduction, and improving battery discharge capacity. These additives may include, for example, haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride. Here, the additive may be present in an amount of 0.1 to 10% by weight, specifically 0.1 to 5% by weight, relative to the total weight of the electrolyte.
[0122] As described above, lithium secondary batteries containing the positive electrode active material according to the present invention exhibit excellent lifespan and capacity characteristics, making them useful in portable devices such as mobile phones, notebook computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0123] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0124] The aforementioned battery module or battery pack can be used as a power source for one or more medium-to-large devices, including power tools; electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.
[0125] The external shape of the lithium secondary battery of the present invention is not particularly limited, but may be cylindrical, rectangular, pouch-type, or coin-type using a can.
[0126] In addition to being usable as a battery cell for powering small devices, the lithium secondary battery according to the present invention can also be preferably used as a unit battery in medium- and large-sized battery modules containing a large number of battery cells.
[0127] Hereinafter, embodiments of the present invention will be described in detail so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention can be realized in various different forms and is not limited to the embodiments described herein. [Examples]
[0128] The present invention will be described in detail below with reference to examples. However, the examples of the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples detailed below. The examples of the present invention are provided to give a more complete explanation of the present invention to a person of average skill in the art.
[0129] Examples and Comparative Examples Example 1 Ni0.60 Co 0.05 Mn 0.35 A composite transition metal hydroxide having a composition represented by (OH)2 (product name: Nickel cobalt manganese hydroxide, D 50 : 3.5 μm ± 0.2 μm, secondary particles) and Li2CO3 were introduced such that the molar ratio of (Ni+Co+Mn):Li was 1:1.05, and Y2O3 was added to Ni 0.60 Co 0.05 Mn 0.35 ZrO2 was added such that the Y content was 1,500 ppm based on the total weight of (OH)2, and Ni 0.60 Co 0.05 Mn 0.35 was introduced such that the Zr content was 3,000 ppm based on the total weight of (OH)2, followed by mixing to prepare a mixture.
[0130] The mixture was heated from 25°C to 950°C at a rate of 3°C / min in an air atmosphere, and then calcined at 950°C for 14 hours to prepare a single-particle lithium composite transition metal oxide (positive electrode active material).
[0131] Example 2 The mixture prepared in Example 1 was heated from 25°C to 960°C at a rate of 3°C / min in an air atmosphere, and then calcined at 960°C for 14 hours to prepare a single-particle lithium composite transition metal oxide (positive electrode active material).
[0132] Comparative Example 1 Ni 0.60 Co 0.05 Mn 0.35 A composite transition metal hydroxide having a composition represented by (OH)2 (product name: Nickel cobalt manganese hydroxide, D 50 : 3.5 μm ± 0.2 μm, secondary particles) and Li2CO3 were introduced such that the molar ratio of (Ni+Co+Mn):Li was 1:1.05, followed by mixing to prepare a mixture. A positive electrode active material was prepared in the same manner as in Example 1, except for the above.
[0133] Comparative Example 2 Ni 0.60 Co0.05 Mn 0.35 A composite transition metal hydroxide having a composition represented by (OH)2 (product name: Nickel cobalt manganese hydroxide, D 50 : 3.5μm ± 0.2μm, secondary particles) and Li2CO3 were added such that the molar ratio of (Ni+Co+Mn):Li was 1:1.05, and ZrO2 was added to Ni 0.60 Co 0.05 Mn 0.35 A positive electrode active material was manufactured in the same manner as in Example 1, except that Zr was added to a content of 3,000 ppm based on the total weight of (OH)2 and mixed to prepare a mixture.
[0134] Comparative Example 3 Ni 0.60 Co 0.05 Mn 0.35 A composite transition metal hydroxide having a composition represented by (OH)2 (product name: Nickel cobalt manganese hydroxide, D 50 : 3.5μm ± 0.2μm, secondary particles) and Li2CO3 were added such that the molar ratio of (Ni+Co+Mn):Li was 1:1.05, and Y2O3 was added to Ni 0.60 Co 0.05 Mn 0.35 A positive electrode active material was manufactured in the same manner as in Example 1, except that Y was added to a content of 1,500 ppm based on the total weight of (OH)2 and mixed to prepare a mixture.
[0135] Comparative Example 4 The mixture prepared in Example 1 was heated from 25°C to 900°C at a rate of 3°C / min in an air atmosphere, and then calcined for 14 hours while maintaining the temperature at 900°C to prepare a single-particle lithium composite transition metal oxide (positive electrode active material).
[0136] Comparative Example 5 The mixture prepared in Example 1 was heated from 25°C to 995°C at a rate of 3°C / min in an air atmosphere, and then calcined for 14 hours while maintaining the temperature at 995°C to prepare a single-particle lithium composite transition metal oxide (positive electrode active material).
[0137] Experimental example Experimental Example 1: Analysis of Cathode Active Material - Confirmation of the composition ratio and doping element content of the positive electrode active material by ICP analysis. The composition and doping element content of the positive electrode active materials produced in Examples 1 and 2 and Comparative Examples 1 to 5 were confirmed by the following methods and are shown in Table 1 below.
[0138] To each of the positive electrode active material particles produced in Examples 1 and 2 and Comparative Examples 1 to 5, 1 ml of hydrochloric acid was added and heated to dissolve the positive electrode active material. Next, a small amount of hydrogen peroxide solution was added to accelerate the reaction and completely dissolve the positive electrode active material to prepare a solution. Then, the solution was diluted with deionized water to a total volume of 10 ml to prepare an analytical sample. The composition of the positive electrode active material and the weight (ppm) of the doping elements present in the analytical sample were confirmed using ICP-OES (Aligent 5100, manufactured by Aligent), and these are shown in Table 1 below.
[0139] - Morphological analysis of positive electrode active material Scanning electron microscope (SEM) images were acquired for the positive electrode active materials produced in Examples 1 and 2 and Comparative Examples 1 to 5, and these are shown in Figures 1 to 7.
[0140] Figure 1 is an SEM image of the positive electrode active material produced in Example 1.
[0141] Figure 2 is an SEM image of the positive electrode active material produced in Example 2.
[0142] Figure 3 is an SEM image of the positive electrode active material produced in Comparative Example 1.
[0143] Figure 4 is an SEM image of the positive electrode active material produced in Comparative Example 2.
[0144] Figure 5 is an SEM image of the cathode active material produced in Comparative Example 3.
[0145] Figure 6 is an SEM image of the positive electrode active material produced in Comparative Example 4.
[0146] Figure 7 is an SEM image of the cathode active material produced in Comparative Example 5.
[0147] As shown in Figures 1 to 7, it was confirmed that the positive electrode active material produced in Example 1 according to the present invention was in single-particle form. Furthermore, it was confirmed that the positive electrode active material produced in Example 1 had superior single-particle formation and improved particle shape compared to Comparative Examples 1 to 3, which were not doped with Zr and / or Y, Comparative Example 4, which was produced by firing at a temperature below 920°C, and / or Comparative Example 5, which was produced by firing at a temperature above 980°C.
[0148] [Table 1]
[0149] Referring to Table 1, it was confirmed that the positive electrode active materials produced in Examples 1 and 2 had a composition represented by chemical formula 1, with a nickel (Ni) content of 59 mol% or more and 70 mol% or less among the total metals other than lithium, a yttrium (Y) content of 500 ppm or more and 4,000 ppm or less relative to the total weight of the lithium composite transition metal oxide, and a zirconium (Zr) content of 500 ppm or more and 4,000 ppm or less relative to the total weight of the lithium composite transition metal oxide.
[0150] - Evaluation of the degree of single particle formation and fine powder content of the positive electrode active material Using PSA (S3500, manufactured by Microtrac), the average particle size (D) of the lithium composite transition metal oxides produced in Examples 1 and 2 and Comparative Examples 1 to 5 was measured. 50 The following measurements were taken and are shown in Table 2 below.
[0151] Furthermore, using a SEM (FEI, Inspect F), SEM images (5K magnification) of the lithium composite transition metal oxides produced in Examples 1 and 2 and Comparative Examples 1 to 5 were acquired. Using an image processing program (LG Chem, DX program), images were obtained in which the boundaries of primary particles present in the SEM images were separated and displayed in random colors. Using the images in which the boundaries of primary particles were separated and displayed in random colors, the area of each primary particle was calculated based on the number of pixels corresponding to each of the n primary particles (an average of 50,000 or more primary particles). The average particle size (D') of the primary particles present in the lithium composite transition metal oxides produced in Examples 1 and 2 and Comparative Examples 1 to 5 was calculated using the radius of a circle having the same area as each of the primary particles. 50 The average particle size (D) of the lithium composite transition metal oxide was measured and is shown in Table 2 below. 50 ) with respect to the average particle size (D' of primary particles 50 The value of (single particle degree (χ)) was calculated and is shown in Table 2 below.
[0152] Regarding the fine particles present in the positive electrode active material, the ratio (%) of the area of the fine particles to the total area of the primary particles present in the positive electrode active material, i.e., the area of primary particles with a particle size of 1 μm or less, was calculated and the results are shown in Table 2 below. Specifically, the area of each primary particle was calculated based on the number of pixels corresponding to each of the n primary particles present in the SEM image, and the percentage of the area of the fine particles to the total area of the primary particles (the ratio (%) of the area of primary particles with a particle size of 1 μm or less) is shown in Table 2 below.
[0153] The steps of the aforementioned SEM image processing program (manufactured by LG Chem, DX program) are shown in Figures 8 to 10.
[0154] Figure 8 is an SEM image of the cathode active material according to one embodiment of the present invention.
[0155] Figure 9 is an SEM image of the cathode active material according to one embodiment of the present invention, showing the boundaries of primary particles within the cathode active material separated.
[0156] Figure 10 is an SEM image of a positive electrode active material according to one embodiment of the present invention, showing the boundaries of primary particles within the positive electrode active material separated and indicated by random colors.
[0157] [Table 2]
[0158] Referring to Table 2, the positive electrode active materials produced in Examples 1 and 2, i.e., positive electrode active materials containing yttrium (Y) and zirconium (Zr), have an average particle size (D') of primary particles. 50 The particle size is 2.0 μm or larger and 3.5 μm or smaller, and the average particle size (D) of the lithium composite transition metal oxide is 2.0 μm or larger. 50 It was confirmed that the particle size (D') was 2.0 μm or more and 5.0 μm or less, the degree of single-particle formation (χ) according to Formula 1 described herein was 0.4 or more, and the ratio of the area of primary particles with a particle size of 1 μm or less to the total area of primary particles present in the positive electrode active material was 20% or less. On the other hand, the positive electrode active materials produced in Comparative Examples 1, 2, 4 and 5 had an average particle size (D') of primary particles. 50 It was confirmed that the particle size was less than 2.0 μm or greater than 3.5 μm. Furthermore, it was confirmed that in the positive electrode active materials produced in Comparative Examples 1, 2, and 4, the ratio of the area of primary particles with a particle size of 1 μm or less to the total area of primary particles present in the positive electrode active material was greater than 20%.
[0159] Experimental Example 2: Evaluation of Battery Characteristics - Manufacturing of pouch-type monocell batteries A positive electrode slurry was prepared by mixing 95% by weight of the positive electrode active material produced in Examples 1 and 2 and Comparative Examples 1 to 5, 2.0% by weight of Super P as a conductive material, and 3.0% by weight of polyvinylidene fluoride (PVDF) as a binder in an N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then rolled to produce a positive electrode.
[0160] A negative electrode slurry was prepared by mixing a negative electrode active material consisting of natural graphite and artificial graphite in a 5:5 weight ratio, Super C conductive material, additives (Daicel, DAIEL2200), and binder (ZEON, BML302) in water in a weight ratio of 95.6:1.0:2.3:1.1. After applying the negative electrode slurry to one surface of a copper current collector, it was dried at 130°C and rolled to produce a negative electrode.
[0161] An electrode assembly was manufactured by interposing a porous polyethylene separator between the positive and negative electrodes. This assembly was placed inside a battery case, and an electrolyte solution prepared by dissolving 0.7 M LiPF6 and 0.3 M LiFSI in an organic solvent mixture of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7 was injected to manufacture a pouch-type monocell battery.
[0162] - Evaluation of battery capacity characteristics and life characteristics Using the pouch-type monocell manufactured as described above, it was charged to 4.4V at 25°C using the CC-CV method (0.1C), and then discharged to 2.5V using the CC method (0.1C). The discharge capacity at this time was measured and is shown in Table 3 below.
[0163] After charging to 4.4V using the CC-CV method (0.1C) at 25°C and discharging to 2.5V using the CC method (0.1C), the SOC state was set based on the measured discharge capacity. The initial SOC50 resistance (Ω) was then measured at 25°C. One cycle consisted of charging to 4.4V using the CC-CV method (0.33C) at 45°C and discharging to 2.5V using the CC method (0.33C). This cycle was repeated 100 times. Immediately after the 100th cycle at 25°C, the SOC50 resistance (Ω) was measured. The percentage of the SOC50 resistance immediately after the 100th cycle relative to the initial SOC50 resistance (resistance increase rate (%)) is shown in Table 3 below. The SOC50 resistance was calculated by applying a discharge current of 2.5C to the SOC50 for 30 seconds at 25°C, measuring the voltage drop, and then dividing the voltage drop during the first 10 seconds by the applied current.
[0164] The battery was charged to 4.4V at 45°C using the CC-CV method (0.33C), and then discharged to 2.5V using the CC method (0.33C). This cycle was defined as one cycle, and a total of 100 charge-discharge cycles were repeated. The discharge capacity was measured for the first cycle and the 100th cycle, and the percentage of the discharge capacity at the 100th cycle relative to the discharge capacity at the first cycle (capacity retention rate (%)) is shown in Table 3 below.
[0165] [Table 3]
[0166] Referring to Table 3, it was confirmed that batteries containing the positive electrode active materials produced in Examples 1 and 2, i.e., positive electrode active materials containing yttrium (Y) and zirconium (Zr), had high discharge capacity and capacity retention rates in the first and 100th cycles at 45°C, and low resistance increase rate at 25°C. On the other hand, batteries containing the positive electrode active materials produced in Comparative Examples 1 to 3, i.e., positive electrode active materials that do not contain yttrium (Y) and / or zirconium (Zr), and the positive electrode active materials produced in Comparative Examples 4 and 5, i.e., the average particle size (D') of the primary particles, were compared. 50 Batteries containing positive electrode active material with a diameter of less than 2.0 μm or greater than 3.5 μm were found to have low discharge capacity and capacity retention rate in the first and 100th cycles at 45°C, and a high resistance increase rate at 25°C.
[0167] In conclusion, the positive electrode active material according to the present invention is stable because its structure does not change significantly even during charge-discharge cycles.
Claims
1. It contains a lithium composite transition metal oxide in single-particle form consisting of 10 or fewer primary particles, The aforementioned lithium composite transition metal oxide has a nickel (Ni) content of 50 mol% or more of the total metals other than lithium, and also contains yttrium (Y) and zirconium (Zr). A positive electrode active material having an average particle size (D'50) of the primary particles of 2.0 μm or more and 3.5 μm or less.
2. The positive electrode active material according to claim 1, wherein the lithium composite transition metal oxide has a nickel (Ni) content of 59 mol% or more and 70 mol% or less among the total metals other than lithium.
3. The lithium composite transition metal oxide has a composition represented by the following chemical formula 1, wherein it is the positive electrode active material according to claim 1: [Chemical formula 1] Li 1+x Ni a Co b Mn c Y d Zr e M f O 2 In the aforementioned chemical formula 1, M is one or more selected from B, Al, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, Ce, F, P, S, and La. -0.1 ≤ x ≤ 0.1, 0.59 ≤ a < 1, 0 < b < 0.41, 0 < c < 0.41, 0 < d ≤ 0.1, 0 < e ≤ 0.1, 0 ≤ f ≤ 0.
1.
4. The positive electrode active material according to claim 1, wherein the lithium composite transition metal oxide has a degree of single-particle formation (χ) of 0.4 or more according to the following formula 1. [Math 1]
5. The positive electrode active material according to claim 4, wherein the degree of single-particle formation (χ) is 0.55 or more and 0.65 or less.
6. The positive electrode active material according to claim 1, wherein the average particle diameter (D 50 ) of the lithium composite transition metal oxide is 2.0 μm or more and 5.0 μm or less.
7. The positive electrode active material according to claim 1, wherein the ratio of the area of primary particles with a particle size of 1 μm or less to the total area of primary particles present in the positive electrode active material is 20% or less.
8. The positive electrode active material according to claim 1, wherein the yttrium (Y) content in the lithium composite transition metal oxide is 500 ppm or more and 4,000 ppm or less relative to the total weight of the lithium composite transition metal oxide.
9. The positive electrode active material according to claim 1, wherein the zirconium (Zr) content in the lithium composite transition metal oxide is 500 ppm or more and 4,000 ppm or less based on the total weight of the lithium composite transition metal oxide.
10. (A) A step of mixing nickel-containing composite transition metal hydroxide, lithium (Li)-containing raw material, yttrium (Y)-containing raw material, and zirconium (Zr)-containing raw material to produce a mixture, (B) The step of calcining the mixture to produce a lithium composite transition metal oxide, The method for producing a positive electrode active material according to claim 1, wherein the firing is carried out at a temperature of 920°C or higher and 980°C or lower.
11. The method for producing a positive electrode active material according to claim 10, wherein in step (A), the yttrium (Y)-containing raw material is mixed such that the content of yttrium (Y) is 500 ppm or more and 4,000 ppm or less with respect to the total weight of the composite transition metal hydroxide.
12. The method for producing a positive electrode active material according to claim 10, wherein in step (A), the zirconium (Zr)-containing raw material is mixed such that the zirconium (Zr) content is 500 ppm or more and 4,000 ppm or less with respect to the total weight of the composite transition metal hydroxide.
13. A positive electrode comprising the positive electrode active material according to any one of claims 1 to 9.
14. A lithium secondary battery comprising the positive electrode described in claim 13.
Citation Information
Patent Citations
Positive electrode active material for lithium secondary battery, preparing method of the same