Positive electrode active material, method for manufacturing the same, and positive electrode and lithium secondary battery containing the same
The single-particle lithium composite transition metal oxide active material addresses structural breakdown and mobility issues, enhancing energy density, output, and resistance characteristics in lithium-ion batteries.
Patent Information
- Application Number
- JP2026526379
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-03
- Filing Date
- 2024-11-04
- Publication Date
- 2026-11-24
AI Technical Summary
Conventional lithium composite transition metal oxides used in lithium-ion secondary batteries face issues such as structural breakdown, increased degradation, and reduced lifespan due to high nickel content, particle cracking during manufacturing and charging, and poor lithium mobility, leading to inferior energy density, output characteristics, and resistance characteristics.
A positive electrode active material composed of single-particle lithium composite transition metal oxide with specific nickel content, single crystallinity, and crystal grain size, optimized for improved lithium mobility and reduced side reactions.
Enhances energy density, output characteristics, and resistance characteristics by minimizing particle cracking and improving lithium mobility, resulting in superior battery performance and stability.
Smart Images

Figure 2026539328000001_ABST
Abstract
Description
[Technical Field]
[0001] This application claims priority under Korean Patent Application No. 10-2023-0151122 dated November 3, 2023, and all content disclosed in the documents of the said Korean Patent Application is incorporated herein by reference.
[0002] The present invention relates to a positive electrode active material, a method for producing the same, and a positive electrode and lithium secondary battery containing the same. [Background technology]
[0003] A lithium secondary battery generally consists of a positive electrode, a negative electrode, a separator, and an electrolyte, and the positive electrode and negative electrode contain an active material that allows for the insertion and deintercalation of lithium ions.
[0004] Lithium-ion oxides (LiFePO4), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMnO4, etc.), and lithium iron phosphate compounds (LiFePO4) are used as positive electrode active materials in lithium-ion secondary batteries. Of these, lithium cobalt oxide has the advantage of a high operating voltage and excellent capacity characteristics, but the price of cobalt, which is the raw material, is high and the supply is unstable, making it difficult to commercially apply to high-capacity batteries. Lithium nickel oxide has poor structural stability, making it difficult to achieve sufficient lifespan characteristics. On the other hand, lithium manganese oxide has excellent stability but has the problem of poor capacity characteristics. Therefore, lithium composite transition metal oxides containing two or more transition metals have been developed to complement the problems of lithium transition metal oxides containing Ni, Co, or Mn alone, and among them, lithium composite transition metal oxides containing Ni, Co, and Mn are widely used in the electric vehicle battery field.
[0005] Recently, there has been an increasing demand for high-power, high-capacity batteries, such as those for electric vehicles, and consequently, the nickel content in lithium-ion composite transition metal oxides is tending to increase. When the nickel content in lithium-ion composite transition metal oxides increases, the initial capacity characteristics improve, but with repeated charging and discharging, the highly reactive nickel... +4 The generation of a large amount of ions causes structural breakdown of the positive electrode active material, which increases the rate of degradation of the positive electrode active material, reduces its lifespan characteristics, and compromises battery safety.
[0006] Furthermore, conventional lithium composite transition metal oxides typically exist in the form of spherical secondary particles, which are aggregates of tens to hundreds of primary particles. However, in the case of lithium composite transition metal oxides with secondary particle forms in which a large number of primary particles are aggregated in this way, during the manufacturing of the positive electrode, primary particles tend to detach during the rolling process, meaning that particle cracking is likely to occur, and cracks can develop inside the particles during the charge and discharge process. When particle cracking or cracking occurs in the positive electrode active material, the contact area with the electrolyte increases, leading to side reactions with the electrolyte, increased gas generation and degradation of the active material, and a decrease in lifetime characteristics.
[0007] To address the above issues, a technique has been proposed to manufacture lithium composite transition metal oxides in single-particle form rather than secondary particles by increasing the firing temperature. In the case of single-particle form positive electrode active materials, the contact area with the electrolyte is smaller compared to conventional secondary-particle form positive electrode active materials, resulting in fewer side reactions with the electrolyte and superior particle strength, thus reducing particle cracking during electrode manufacturing. Therefore, applying single-particle form positive electrode active materials offers the advantage of superior gas generation and lifespan characteristics.
[0008] However, single-particle lithium composite transition metal oxide particles have relatively larger primary particle sizes and fewer interfaces between primary particles that serve as diffusion pathways for lithium ions compared to conventional secondary-particle lithium composite transition metal oxide particles, resulting in inferior lithium mobility. Furthermore, because they are manufactured at relatively high firing temperatures, a rock salt phase forms on the particle surface, leading to high surface resistance. In addition, single-particle lithium composite transition metal oxide particles have high lithium diffusion resistance, which causes uneven lithium ion movement during charging and discharging, leading to deformation of the crystal structure and subsequent particle cracking, thus reducing battery performance. [Prior art documents] [Patent Documents]
[0009] [Patent Document 1] Korean Published Patent Gazette No. 10-2019-0131842 [Overview of the Initiative] [Problems that the invention aims to solve]
[0010] The present invention aims to solve the above-mentioned problems and to provide a positive electrode active material and a method for manufacturing the same that can improve the rolling density of the positive electrode active material and improve the output characteristics, rate characteristics, resistance characteristics, etc., of a battery.
[0011] Furthermore, the present invention aims to provide a positive electrode and a lithium secondary battery that are excellent in terms of energy density, output characteristics, rate characteristics, resistance characteristics, etc., by including the positive electrode active material described above. [Means for solving the problem]
[0012] (1) The present invention provides a positive electrode active material which is in the form of single particles composed of 10 or fewer primary particles, includes a lithium composite transition metal oxide containing nickel in an amount of 50 mol% or more based on the total amount of metals other than lithium, has a single crystallinity (χ) of 0.500 or more and 0.850 or less as calculated by the following Formula 1, and has a crystal grain size (D) of 2.00 μm or more and 5.00 μm or less. [Equation]
[0013] (2) The present invention provides the positive electrode active material of (1), wherein the lithium composite transition metal oxide has a composition represented by the following Chemical Formula 1. [Chemical Formula 1] Li 1+x Ni a Co b Mn c M 1 d O2 In Chemical Formula 1, M 1 is one or more selected from the group consisting of Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si, and -0.10≤x≤0.10, 0.500≤a<1.000, 0<b<0.500, 0<c<0.500, 0≤d≤0.100, and a+b+c+d=1.
[0014] (3) The present invention provides the positive electrode active material of (1) or (2), wherein the lithium composite transition metal oxide includes one or more doping elements selected from the group consisting of Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si.
[0015] (4) The present invention provides the positive electrode active material of any one of (1) to (3), wherein the average particle diameter (D 50 ) of the primary particles is 2.35 μm or more and 6.00 μm or less.
[0016] (5) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (4) above.
[0017] (6) The present invention provides a lithium secondary battery including the positive electrode according to (5) above. [Effects of the Invention]
[0018] The positive electrode active material according to the present invention is in single-particle form and contains a lithium composite transition metal oxide that includes 50 mol% or more nickel among the total metals other than lithium, has a specific range of single crystallinity, and has a specific range of crystal grain size, and is effective in improving the energy density, output characteristics, rate characteristics, and resistance characteristics of batteries containing it.
[0019] This makes it possible to improve the performance of the positive electrode containing the positive electrode active material and the secondary battery, particularly the energy density, output characteristics, and resistance characteristics. [Brief explanation of the drawing]
[0020] [Figure 1] This is an SEM image of the positive electrode active material produced in Example 1. [Figure 2] This is an SEM image of the positive electrode active material produced in Example 2. [Figure 3] This is an SEM image of the positive electrode active material produced in Comparative Example 1. [Figure 4] This is an SEM image of the positive electrode active material produced in Comparative Example 2. [Figure 5] This is an SEM image of the positive electrode active material produced in Comparative Example 3. [Figure 6] This is an SEM image of the positive electrode active material produced in Comparative Example 4. [Figure 7] This is an IPF map obtained by performing EBSD analysis on a cathode for EBSD analysis manufactured using the cathode active material produced in Example 1. [Figure 8] This is an IPF map obtained by performing EBSD analysis on a cathode for EBSD analysis manufactured using the cathode active material produced in Example 2. [Figure 9] This is an IPF map obtained by performing EBSD analysis on a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 1. [Figure 10] This is an IPF map obtained by performing EBSD analysis on a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 2. [Figure 11] This is an IPF map obtained by performing EBSD analysis on a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 3. [Figure 12] This is an IPF map obtained by performing EBSD analysis on a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 4. [Modes for carrying out the invention]
[0021] The present invention will be described in more detail below to aid in understanding the present invention.
[0022] The terms and words used herein and in the claims should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather in a manner consistent with the technical idea of the present invention, in accordance with the principle that inventors may define the concepts of terms as appropriate to best describe their invention.
[0023] In this specification, terms such as “includes,” “equip,” or “have” specify the presence of implemented features, figures, steps, components, or combinations thereof, but should be understood not to preclude the existence or possibility of adding one or more other features, figures, steps, components, or combinations thereof.
[0024] In this specification, the term "single-particle form" includes all forms in which the positive electrode active material and / or lithium composite transition metal oxide particles are single particles and forms in which two to ten particles aggregate together. That is, the single-particle form positive electrode active material and / or single-particle form lithium composite transition metal oxide of the present invention may include one or more types of particles selected from the group consisting of single particles and particles in which two to ten particles aggregate together.
[0025] In this specification, "primary particle" refers to the smallest particle unit recognized when observing a positive electrode active material using a scanning electron microscope (SEM), and "secondary particle" refers to a secondary structure formed by the aggregation of multiple primary particles.
[0026] In this specification, "crystal grain" refers to a particle unit having substantially the same crystal orientation, which can be measured by EBSD (Electron Backscatter Diffraction). Specifically, it refers to the smallest particle unit represented by the same color in an IPF map obtained by EBSD analysis of a cross-section of a positive electrode active material cut by ion milling.
[0027] In this specification, the particle size of a primary particle may be calculated by determining the area of each primary particle based on the number of pixels corresponding to each of the n primary particles present in the SEM image, and then using the radius of a circle having the same area as the area of each primary particle to calculate the particle size of each primary particle present in the SEM image. In addition, in this specification, the average particle size of the primary particles (D 50 ) can be defined as the particle size that corresponds to 50% of the volume cumulative distribution in the particle size distribution curve (graph curve of particle size distribution). The average particle size (D) of the primary particles. 50 The particle diameter can be measured by first calculating the volume of a sphere with a radius equal to half the particle size of the primary particle, then determining the particle diameter at the point where the cumulative volume distribution by particle size, calculated from the volume of the primary particle, reaches 50%.
[0028] In this specification, the grain size (D) may be the arithmetic mean of the grain size. The grain size can be measured by image analysis. Specifically, the grain size can be calculated by obtaining an IPF map of the particles using EBSD, calculating the grain size from the area of the grains confirmed from the obtained map image, and then taking the arithmetic mean of these values.
[0029] In this specification, the content of each element in lithium composite transition metal oxide may be measured by ICP (Inductive Coupled Plasma) analysis using an inductively coupled plasma emission spectrometer (ICP-OES; Agilent 5100, manufactured by Agilent Technologies).
[0030] positive electrode active material The positive electrode active material according to the present invention will be described below.
[0031] The positive electrode active material according to the present invention is in a single-particle form consisting of 10 or fewer primary particles, and contains a lithium composite transition metal oxide in which nickel accounts for 50 mol% or more of the total metals other than lithium, and has a single crystallinity degree (χ) of 0.500 or more and 0.850 or less according to the following formula 1, and a crystal grain size (D) of 2.00 μm or more and 5.00 μm or less.
[0032]
number
[0033] On the other hand, when the lithium composite transition metal oxide is not in a single-particle form consisting of 10 or fewer primary particles, but rather contains less than 50 mol% nickel among the total metals other than lithium, has a single crystallinity degree according to Equation 1 of less than 0.500 or greater than 0.850, and has a crystal grain size (D) of less than 2.00 μm or greater than 5.00 μm as a positive electrode active material, there were problems with inferior energy density, output characteristics, rate characteristics, and resistance characteristics.
[0034] The inventors of the present invention have diligently conducted research to develop a positive electrode active material with excellent output characteristics, rate characteristics, and resistance characteristics. As a result, they have found that in the case of a positive electrode active material that is in a single-particle form consisting of 10 or fewer primary particles, contains a lithium composite transition metal oxide with 50 mol% or more of nickel among the total metals other than lithium, has a single crystallinity degree (χ) of 0.500 or more and 0.850 or less according to Formula 1 described herein, and has a crystal grain size (D) of 2.00 μm or more and 5.00 μm or less according to Formula 1 described herein, lithium mobility can be improved by increasing the rolling density and adjusting the inter-grain interfaces that serve as pathways for lithium ion movement within the positive electrode active material particles. This led to the completion of the present invention. As described above, a battery to which the positive electrode active material according to the present invention is applied can have excellent energy density, output characteristics, rate characteristics, and resistance characteristics.
[0035] The lithium composite transition metal oxide is in a single-particle form consisting of 10 or fewer primary particles. That is, the lithium composite transition metal oxide is in a single-particle form or a single-particle form in which 2 to 10 particles are aggregated. The single-particle form is distinguished from secondary particles in which more than 10 primary particles are aggregated. When the lithium composite transition metal oxide has a single-particle form, it has excellent stability, and even when the positive electrode active material containing it is rolled, the positive electrode active material does not crack or break. As a result, side reactions between the positive electrode active material and the electrolyte can be reduced, and the life characteristics of the battery to which it is applied can be improved. On the other hand, when the lithium composite transition metal oxide is in a secondary-particle form, the particle strength is low, and when the electrode is rolled after manufacturing, particle cracking is severe, and when the cell is driven, a large amount of gas is generated, which leads to problems of reduced stability and life characteristics.
[0036] The lithium composite transition metal oxide contains 50 mol% or more of nickel among the total metals other than lithium. Specifically, it contains 50 mol% or more, 55 mol% or more, 60 mol% or more, or 61 mol% or more of nickel among the total metals other than lithium. When the nickel content among the total metals other than lithium is within the above range, high capacity characteristics can be achieved. When the nickel content among the total metals other than lithium is less than 50 mol%, there is a problem of inferior capacity characteristics.
[0037] The inventors evaluated the degree of single crystallinity and expressed it using the parameter represented by Formula 1 above. The degree of single crystallinity as used in this invention refers to the size (D) of the crystal grains that make up a single particle and the average particle size (D) of the primary particles that make up the lithium composite transition metal oxide, which is a single particle. 50 This value is adjusted according to ). The size of the crystal grains (D) is measured using an EBSD instrument, and the average particle size (D) of the primary particles is determined. 50 The above equation 1 was derived by measuring the size of the crystal grains using a scanning electron microscope (SEM). The inventors considered the large size of the crystal grains, specifically, when the crystal grain size is 150-200 nm or larger, it is difficult to trust XRD data using FWHM, so they measured the size of the crystal grains using an EBSD device, and considering that the lithium composite transition metal oxide is a single particle, specifically, in order to distinguish adjacent single particles, they measured the average particle size of the primary particles using a scanning electron microscope (SEM) and derived equation 1.
[0038] First, in Equation 1, the grain size (D) refers to the average grain size measured by electron backscatter diffraction (EBSD) analysis of a cross-section of an electrode obtained by ion milling an electrode manufactured using the positive electrode active material. Specifically, the area of each grain is calculated by the number of pixels corresponding to each of the n grains present in the IPF map image obtained by EBSD analysis, and the diameter of the circle having the same area as the area of each grain is taken as the grain size. The grain size (D) refers to the arithmetic mean of the grain sizes, and this value can be obtained using the software of the EBSD instrument.
[0039] In the above formula 1, the average particle size of the primary particles (D 50 This refers to the diameter of the primary particle at the point where the cumulative volume distribution by particle size of the primary particle, obtained by analyzing an SEM image of the positive electrode active material, reaches 50%. Specifically, it can be measured by first determining the volume of the primary particle by the volume of a sphere with a radius equal to half the particle size of the primary particle, and then calculating the particle diameter at the point where the cumulative volume distribution by particle size, based on the calculated volume of the primary particle, reaches 50%.
[0040] Equation 1 above expresses the difference between the size of crystal grains (D) measured by EBSD analysis and the average particle size (D) of primary particles measured by SEM image analysis. 50 This is obtained by dividing by ), and the size of the crystal grains (D) is the average grain size of the primary particles (D 50 The closer it is to ), the higher the degree of single crystallinity. That is, the maximum value of the degree of single crystallinity is 1, which means that one primary particle consists of one crystal grain.
[0041] The positive electrode active material has a single crystallinity degree (χ) according to Formula 1 described herein of 0.500 or higher and 0.850 or lower. The single crystallinity degree (χ) is 0.500 or higher, 0.510 or higher, 0.520 or higher, 0.530 or higher, 0.540 or higher, 0.550 or higher, 0.560 or higher, 0.570 or higher, 0.580 or higher, 0.590 or higher, 0.60 or higher, 0.610 or higher, 0.620 or higher, 0.630 or higher, 0.640 or higher, 0.650 or higher, 0.660 or higher, 0.670 or higher, and 0.680. The values above may be 0.690 or higher, 0.700 or higher, 0.710 or higher, 0.720 or higher, 0.730 or higher, 0.740 or higher, 0.750 or higher, 0.760 or higher, 0.770 or higher, 0.780 or higher, 0.790 or higher, 0.800 or higher, 0.810 or higher, or 0.820 or higher, and may also be 0.830 or lower, 0.840 or lower, or 0.850 or lower. In particular, when the single crystallinity (χ) is 0.800 or higher and 0.850 or lower, it means that the lithium composite transition metal oxide has two or more crystal grains, which adjusts the inter-grain interfaces that serve as pathways for lithium ion movement within the positive electrode active material particles, improving lithium mobility and thus improving the output characteristics, rate characteristics, and resistance characteristics of the secondary battery. On the other hand, if the single crystallinity is less than 0.500, there are too many inter-grain interfaces within the lithium composite transition metal oxide particles that serve as pathways for lithium ions, resulting in poor efficiency and resistance characteristics. Specifically, in the case of secondary particles rather than single particles, the single crystallinity is less than 0.500. If the single crystallinity is greater than 0.850, there are fewer inter-grain interfaces within the lithium composite transition metal oxide particles that serve as pathways for lithium ions, resulting in reduced lithium mobility and poor output characteristics, rate characteristics, and resistance characteristics of the secondary battery.
[0042] According to the present invention, the crystal grain size (D) is 2.00 μm or more and 5.00 μm or less. Specifically, the crystal grain size (D) may be 2.00 μm or more, 2.10 μm or more, 2.20 μm or more, 2.30 μm or more, 2.40 μm or more, or 2.50 μm or more, and may be 2.60 μm or less, 2.70 μm or less, 2.80 μm or less, 2.90 μm or less, 3.00 μm or less, 3.10 μm or less, 3.20 μm or less, 3.30 μm or less, 3.4 The grain size (D) may be 0 μm or less, 3.50 μm or less, 3.60 μm or less, 3.70 μm or less, 3.80 μm or less, 3.90 μm or less, 4.00 μm or less, 4.10 μm or less, 4.20 μm or less, 4.30 μm or less, 4.40 μm or less, 4.50 μm or less, 4.60 μm or less, 4.70 μm or less, 4.80 μm or less, 4.90 μm or less, or 5.00 μm or less. When the grain size (D) is within the above range, the lithium mobility is improved by the presence of an appropriate number of inter-grain interfaces that serve as lithium ion migration pathways within the positive electrode active material particles, thereby improving the output characteristics, rate characteristics, and resistance characteristics of the secondary battery. If the crystal grain size (D) is less than 2.00 μm or greater than 5.00 μm, there is a problem of reduced lithium mobility due to an excessive or insufficient number of inter-grain interfaces within the positive electrode active material particles, which serve as pathways for lithium ion movement. As a result, the output characteristics, rate characteristics, and resistance characteristics of the secondary battery are inferior. Furthermore, since manufacturing positive electrode active materials with a crystal grain size (D) greater than 5.00 μm requires firing at high temperatures exceeding 1000°C, it is practically difficult to manufacture positive electrode active materials with a crystal grain size (D) greater than 5.00 μm.
[0043] According to one embodiment of the present invention, the lithium composite transition metal oxide may have a composition represented by the following chemical formula 1.
[0044] [Chemical formula 1] Li 1+x Ni a Co b Mn c M 1 d O2
[0045] In the aforementioned chemical formula 1, Said M 1 x is one or more elements selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si, and -0.10 ≤ x ≤ 0.10, 0.500 ≤ a < 1.000, 0 <b<0.500、0<c<0.500、0≦d≦0.100、a+b+c+d=1である。
[0046] The aforementioned M1 is a doping element, specifically, the aforementioned M 1 is one or more selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si. 1 While not necessarily included, it can improve capacity characteristics and lifetime characteristics. In particular, M 1 When the material is Zr or Y, a fluxing effect is achieved during firing, improving resistance characteristics and lifespan characteristics.
[0047] The aforementioned x may be -0.10 or greater, -0.09 or greater, -0.08 or greater, -0.07 or greater, -0.06 or greater, -0.05 or greater, -0.04 or greater, -0.03 or greater, -0.02 or greater, -0.01 or greater, 0 or greater, 0.01 or greater, 0.02 or greater, 0.03 or greater, 0.04 or greater, or 0.05 or greater, and may also be 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.10 or less. When x satisfies the above range, high safety and high energy density per unit volume can be achieved.
[0048] The above a is the molar ratio of nickel (Ni) among the total metals other than lithium in the lithium composite transition metal oxide, and may be 0.500 or more, 0.510 or more, 0.520 or more, 0.530 or more, 0.540 or more, 0.550 or more, 0.560 or more, 0.570 or more, 0.580 or more, 0.590 or more, 0.600 or more, or 0.610 or more, and may be 0.620 or less, 0.630 or less, 0.640 or less, 0.650 or less, 0.660 or less, 0.670 or less, 0.680 or less, 0.690 or less, 0.700 or less, 0.710 or less, 0. It may be 720 or less, 0.730 or less, 0.740 or less, 0.750 or less, 0.760 or less, 0.770 or less, 0.780 or less, 0.790 or less, 0.800 or less, 0.810 or less, 0.820 or less, 0.830 or less, 0.840 or less, 0.850 or less, 0.860 or less, 0.870 or less, 0.880 or less, 0.890 or less, 0.900 or less, 0.910 or less, 0.920 or less, 0.930 or less, 0.940 or less, 0.950 or less, 0.960 or less, 0.970 or less, 0.980 or less, 0.990 or less, or less than 1.000. When a satisfies the above range, high energy characteristics can be achieved. In particular, when a is 0.600 or more and 0.700 or less, high energy density is observed during high-voltage driving, high capacitance characteristics can be achieved, and high safety can be ensured.
[0049] The above b is the molar ratio of cobalt (Co) among the total metals other than lithium in the lithium composite transition metal oxide, and may be greater than 0, 0.010 or more, 0.020 or more, 0.030 or more, 0.040 or more, 0.050 or more, or 0.060 or more, and may be 0.070 or less, 0.080 or less, 0.090 or less, 0.100 or less, 0.110 or less, 0.120 or less, 0.130 or less, 0.140 or less, 0.150 or less, 0.160 or less, 0.170 or less, 0.180 or less, 0.190 or less, 0.200 or less, 0.210 or less, 0.220 The following ranges may also be 0.230 or less, 0.240 or less, 0.250 or less, 0.260 or less, 0.270 or less, 0.280 or less, 0.290 or less, 0.300 or less, 0.310 or less, 0.320 or less, 0.330 or less, 0.340 or less, 0.350 or less, 0.360 or less, 0.370 or less, 0.380 or less, 0.390 or less, 0.400 or less, 0.410 or less, 0.420 or less, 0.430 or less, 0.440 or less, 0.450 or less, 0.460 or less, 0.470 or less, 0.480 or less, 0.490 or less, or less than 0.500. When b satisfies the above range, stability during the charge-discharge process can be improved and rate characteristics can be enhanced.
[0050] The above c is the molar ratio of manganese (Mn) among the total metals other than lithium in the lithium composite transition metal oxide, and is greater than 0, 0.010 or more, 0.020 or more, 0.030 or more, 0.040 or more, 0.050 or more, 0.060 or more, 0.070 or more, 0.080 or more, 0.090 or more, 0.100 or more, 0.110 or more, 0.120 or more, 0.130 or more, 0.140 or more, 0.150 or more, 0.160 or more, 0.170 or more, 0.180 or more, 0.190 or more, 0.200 or more, 0.210 or more, 0.220 or more, 0.230 or more. It may be 0.240 or higher, 0.250 or higher, 0.260 or higher, 0.270 or higher, 0.280 or higher, 0.290 or higher, 0.300 or higher, or 0.310 or higher, and may be 0.320 or lower, 0.330 or lower, 0.340 or lower, 0.350 or lower, 0.360 or lower, 0.370 or lower, 0.380 or lower, 0.390 or lower, 0.400 or lower, 0.410 or lower, 0.420 or lower, 0.430 or lower, 0.440 or lower, 0.450 or lower, 0.460 or lower, 0.470 or lower, 0.480 or lower, 0.490 or lower, or less than 0.500. When c satisfies the above range, high-temperature stability can be increased and side reactions with the electrolyte can be relatively reduced.
[0051] The above d is M, which is the total amount of metal other than lithium in the lithium composite transition metal oxide. 1 This is the molar ratio, which may be 0 or greater, or 0.010 or greater, and may be 0.020 or less, 0.030 or less, 0.040 or less, 0.050 or less, 0.060 or less, 0.070 or less, 0.080 or less, 0.090 or less, or 0.100 or less. When d satisfies the above range, the stability of the crystal structure of the positive electrode active material is improved, and the grain shape can be improved.
[0052] According to one embodiment of the present invention, the lithium composite transition metal oxide may contain one or more doping elements selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si, i.e., it may be doped with doping elements. In this case, the stability of the positive electrode active material crystal structure can be improved and the grain shape can be improved.
[0053] According to one embodiment of the present invention, the average particle size (D 50 The average particle size (D) of the primary particles may be 2.35 μm or more and 6 μm or less. Specifically, the average particle size (D) of the primary particles may be 2.35 μm or more and 6 μm or less. 50 ) may be 2.35 μm or larger, or 2.40 μm or larger, and 3.10 μm or smaller, 3.20 μm or smaller, 3.30 μm or smaller, 3.40 μm or smaller, 3.50 μm or smaller, 3.60 μm or smaller, 3.70 μm or smaller, 3.80 μm or smaller, 3.90 μm or smaller, 4.00 μm or smaller, 4.10 μm or smaller, 4.20 μm or smaller, 4.30 μm or smaller, 4.40 μm or smaller The average particle size may be 4.50 μm or less, 4.60 μm or less, 4.70 μm or less, 4.80 μm or less, 4.90 μm or less, 5.00 μm or less, 5.10 μm or less, 5.20 μm or less, 5.30 μm or less, 5.40 μm or less, 5.50 μm or less, 5.60 μm or less, 5.70 μm or less, 5.80 μm or less, 5.90 μm or less, or 6.00 μm or less. The average particle size (D 50 When the above range is present, excellent electrode density can be achieved and structural stability can be improved.
[0054] Method for manufacturing positive electrode active material Next, the method for producing the positive electrode active material of the present invention will be described. The method for producing the positive electrode active material of the present invention is the method for producing the positive electrode active material according to the present invention.
[0055] The positive electrode active material according to the present invention can be manufactured by either manufacturing method 1 or manufacturing method 2 described below. The methods for manufacturing method 1 and manufacturing method 2 will be described in detail below.
[0056] <Manufacturing method 1> The method for producing a positive electrode active material according to the present invention comprises (A1) the step of mixing a composite transition metal hydroxide and a lithium-containing raw material to produce a mixture, and (B1) the step of calcining the mixture to produce a lithium composite transition metal oxide, and is carried out under conditions that satisfy the following formula 2.
[0057] [Formula 2] 30.30 ≤ (0.055 × T1) - (20 × P1) ≤ 31.00
[0058] In the above equation 2, P1 is the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide in step (A1), and T1 is the firing temperature in step (B1).
[0059] The positive electrode active material according to the present invention described above can be manufactured by appropriately adjusting the type of raw material, firing temperature, firing atmosphere, and so on.
[0060] The steps of the present invention will be described in detail below.
[0061] (A1) Step The method for producing a positive electrode active material according to the present invention includes the step of mixing a composite transition metal hydroxide with a lithium-containing raw material to produce a mixture (A1).
[0062] The aforementioned complex transition metal hydroxide can be produced by a coprecipitation reaction in which a complex transition metal-containing solution, an ammonium cation complex-forming agent, and a basic compound are introduced into a reactor.
[0063] The aforementioned complex transition metal-containing solution may also contain nickel (Ni), cobalt (Co), and manganese (Mn).
[0064] The composite transition metal-containing solution can be produced by dissolving a transition metal-containing raw material in a solvent such as water. For example, it can be produced by dissolving nickel (Ni), cobalt (Co), and manganese (Mn)-containing raw materials in water. That is, the composite transition metal-containing solution may contain nickel (Ni), cobalt (Co), and manganese (Mn)-containing raw materials. Furthermore, if necessary, the composite transition metal-containing solution may further contain metal-containing raw materials that contain transition metals other than nickel (Ni), cobalt (Co), and manganese (Mn) (for example, one or more selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si).
[0065] The nickel (Ni)-containing raw material may be at least one selected from the group consisting of nickel-containing acetates, nitrates, sulfates, halides, sulfides, hydroxides, oxides, oxyhydroxides, NiSO4, NiSO4·6H2O, NiCO3·2Ni(OH)2·4H2O, NiC2O4·2H2O, Ni(NO3)2·6H2O, fatty acid nickel, and nickel halides, and one or more of these can be used as a mixture. Specifically, considering ease of manufacturing processes such as pH adjustment and solubility, as well as economic efficiency, NiSO4·6H2O can be used as the nickel (Ni)-containing raw material.
[0066] The aforementioned cobalt (Co)-containing raw material may be at least one selected from the group consisting of cobalt-containing acetates, nitrates, sulfates, halides, sulfides, hydroxides, oxides, oxyhydroxides, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, Co(SO4)2·7H2O, fatty acid cobalt, and cobalt halides, and one or more of these can be used as a mixture. Specifically, considering ease of manufacturing processes such as pH adjustment and solubility, as well as economic efficiency, Co(SO4)2·7H2O can be used as the cobalt (Co)-containing raw material.
[0067] The manganese (Mn)-containing raw material may be at least one selected from the group consisting of manganese-containing acetates, nitrates, sulfates, halides, sulfides, hydroxides, oxides, oxyhydroxides, MnSO4·H2O, MnCO3, manganese dicarboxylates, manganese citrate, manganese salts of fatty acid manganese, and halides of manganese chloride, and one or more of these can be used as a mixture. Considering ease of manufacturing processes such as pH adjustment and solubility, as well as economic efficiency, MnSO4·H2O can be used as the manganese (Mn)-containing raw material.
[0068] Nickel (Ni), cobalt (Co), and manganese (Mn)-containing raw materials can be used in appropriate amounts, taking into account the content of each metal element in the resulting composite transition metal hydroxide.
[0069] On the other hand, the ammonium cation complex-forming agent may contain at least one compound selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4CO3, and the compound may be introduced into the reactor in the form of a solution in which it is dissolved in a solvent. Here, the solvent may be water, or a mixture of water and an organic solvent that is homogeneously miscible with water (specifically, an alcohol, etc.).
[0070] The basic compound may be at least one compound selected from the group consisting of NaOH, KOH, and Ca(OH)2, and the compound can be introduced into the reactor in the form of a solution in which it is dissolved in a solvent. Here, the solvent can be water, or a mixture of water and an organic solvent that is homogeneously miscible with water (specifically, an alcohol, etc.).
[0071] As described above, when a complex transition metal-containing solution, an ammonium cation complex-forming agent, and a basic compound are introduced into the reactor, a coprecipitation reaction occurs between the transition metal ions in the complex transition metal-containing solution and the hydroxide ions of the basic compound, generating precursor particles in the form of complex transition metal hydroxides.
[0072] The coprecipitation reaction can be carried out for a period of 12 hours or more and 100 hours or less. When the coprecipitation reaction is carried out for a period of time within the above range, particles with uniform particle size and shape can be produced.
[0073] Here, the basic compound can be added in an amount such that the pH of the reaction solution falls within the desired range.
[0074] Once the precursor particles are formed by the method described above, the particles are separated from the reaction solution to obtain the composite transition metal precursor. Specifically, the reaction solution is filtered to separate the composite transition metal precursor from the reaction solution, and then the separated composite transition metal precursor is washed with water and dried to obtain the composite transition metal precursor. Here, if necessary, steps such as grinding and / or classification may be performed.
[0075] According to one embodiment of the present invention, the composite transition metal hydroxide may have a composition represented by the following chemical formula 2.
[0076] [Chemical formula 2] Ni a1 Co b1 Mn c1 M 2 d1 (OH)2
[0077] In the aforementioned chemical formula 2, Said M 2 is one or more selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si. 0.50 ≤ a1 < 1.00, 0 <b1<0.50、0<c1<0.50、0≦d1≦0.10、a1+b1+c1+d1=1である。
[0078] Said M 2 This is a doping element, specifically, the aforementioned M 2 The M may be one or more selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si. 2 Although not necessarily present, when present in appropriate amounts, it can improve the particle shape of the positive electrode active material and enhance the stability of its crystal structure.
[0079] The above a1 is the molar ratio of nickel (Ni) among the total metals other than lithium in the lithium composite transition metal oxide, and may be 0.50 or more, 0.51 or more, 0.52 or more, 0.53 or more, 0.54 or more, 0.55 or more, 0.56 or more, 0.57 or more, 0.58 or more, 0.59 or more, 0.60 or more, or 0.61 or more, and may be 0.62 or less, 0.63 or less, 0.64 or less, 0.65 or less, 0.66 or less, 0.67 or less, 0.68 or less, 0.69 or less, 0.70 or less, or 0.71 or less. It may also be 0.72 or less, 0.73 or less, 0.74 or less, 0.75 or less, 0.76 or less, 0.77 or less, 0.78 or less, 0.79 or less, 0.80 or less, 0.81 or less, 0.82 or less, 0.83 or less, 0.84 or less, 0.85 or less, 0.86 or less, 0.87 or less, 0.88 or less, 0.89 or less, 0.91 or less, 0.92 or less, 0.93 or less, 0.94 or less, 0.95 or less, 0.96 or less, 0.97 or less, 0.98 or less, 0.99 or less, or less than 1.00. When a1 satisfies the above range, high energy characteristics can be achieved, and in particular, when a1 is 0.60 or more and 0.70 or less, high energy density is shown during high-voltage driving, high capacity characteristics can be achieved, and high safety can be achieved.
[0080] The above b1 is the molar ratio of cobalt (Co) among the total metals other than lithium in the lithium composite transition metal oxide, and may be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, or 0.06 or more, and may be 0.07 or less, 0.08 or less, 0.09 or less, 0.10 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, 0.18 or less, 0.19 or less, 0.20 or less, 0.21 or less, It may be 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.30 or less, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, 0.40 or less, 0.41 or less, 0.42 or less, 0.43 or less, 0.44 or less, 0.45 or less, 0.46 or less, 0.47 or less, 0.48 or less, 0.49 or less, or less than 0.50. When b1 satisfies the above range, stability during the charge-discharge process can be improved and rate characteristics can be enhanced.
[0081] The above c1 is the molar ratio of manganese (Mn) among the total metals other than lithium in the lithium composite transition metal oxide, and can be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.10 or more, 0.11 or more, 0.12 or more, 0.13 or more, 0.14 or more, 0.15 or more, 0.16 or more, 0.17 or more, 0.18 or more, 0.19 or more, 0.20 or more, 0.21 or more, 0.22 or more, or 0.2 It may be 3 or more, 0.24 or more, 0.25 or more, 0.26 or more, 0.27 or more, 0.28 or more, 0.29 or more, 0.30 or more, or 0.31 or more, and may be 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, 0.40 or less, 0.41 or less, 0.42 or less, 0.43 or less, 0.44 or less, 0.45 or less, 0.46 or less, 0.47 or less, 0.48 or less, 0.49 or less, or less than 0.50. When c1 satisfies the above range, high-temperature stability can be increased and side reactions with the electrolyte can be relatively reduced.
[0082] The aforementioned d1 is M, which is the total amount of metal other than lithium in the lithium composite transition metal oxide. 1 This is the molar ratio, which may be 0 or greater, or 0.01 or greater, and may be 0.02 or less, 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.10 or less. When d1 satisfies the above range, the stability of the positive electrode active material crystal structure is improved and the grain shape can be improved.
[0083] The lithium (Li)-containing raw material may be at least one selected from the group consisting of LiOH, Li2CO3, LiNO3, LiNO2, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li acetate, Li dicarboxylic acid, Li citrate, Li fatty acid, alkyl lithium, and lithium halides, and one or more of these can be used as a mixture. Specifically, considering economics, Li2CO3 can be used as the lithium (Li)-containing raw material.
[0084] The mixing can be carried out by dry mixing or wet mixing. When the components are mixed by dry mixing, the calcination process can be performed without a separate drying step. When the components are mixed by wet mixing, they may be prepared by adding them to a mixture of water and a solvent, specifically water, or an organic solvent that can be uniformly mixed with water (specifically, alcohol, etc.), or by preparing a solution containing each raw material, specifically an aqueous solution, mixing these solutions, spray-drying the mixed components, and then performing the calcination process. Each raw material and composite transition metal hydroxide can be used in an appropriate content, taking into account the content of each metal element in the final lithium composite transition metal oxide produced.
[0085] According to one embodiment of the present invention, in step (A1), the composite transition metal hydroxide and the lithium (Li)-containing raw material can be mixed in an amount such that they have the composition represented by the chemical formula 1.
[0086] According to one embodiment of the present invention, the composite transition metal hydroxide and the lithium-containing raw material may be mixed such that the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide is 1.00 or more and 1.10 or less. Specifically, the mixture may be mixed such that the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide is 1.00 or more, 1.01 or more, 1.02 or more, 1.03 or more, 1.04 or more, 1.05 or more, or 1.06 or more, and 1.07 or less, 1.08 or less, 1.09 or less, or 1.10 or less. When the mixture is mixed such that the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide is within the above range, the shape of the single particles can be adjusted to improve capacitance characteristics, resistance characteristics, and rate characteristics. In particular, when the molar ratio (Li / M) is 1.02 or higher and 1.07 or lower, there is sufficient lithium for the reaction, and after the reaction, the amount of residual lithium is small, resulting in improved capacity characteristics, resistance characteristics, and rate characteristics of the secondary battery produced.
[0087] (B1) Step The method for producing a positive electrode active material according to the present invention includes, after step (A1), step (B1) of calcining the mixture to produce a lithium composite transition metal oxide.
[0088] According to one embodiment of the present invention, the firing may be carried out at a temperature of 700°C or higher and 1,000°C or lower. Specifically, the firing may be carried out at a temperature of 700°C or higher, 710°C or higher, 720°C or higher, 730°C or higher, 740°C or higher, 750°C or higher, 760°C or higher, 770°C or higher, 780°C or higher, 790°C or higher, 800°C or higher, 810°C or higher, 820°C or higher, 830°C or higher, 840°C or higher, 850°C or higher, 860°C or higher, 870°C or higher, 880°C or higher, 890°C or higher, 900°C or higher, 910°C or higher, 920°C or higher, or 930°C or higher, and 940°C or lower, 950°C or lower, 960°C or lower, 970°C or lower, 980°C or lower, 990°C or lower, or 1,000°C or lower. When the firing temperature is within the aforementioned range, the particle size and specific surface area of the positive electrode active material can be easily adjusted, and the capacity characteristics and resistance characteristics of the secondary battery to which it is applied can be improved.
[0089] According to one embodiment of the present invention, the firing may be carried out for a period of 5 hours or more and 20 hours or less. Specifically, the firing may be carried out for a period of 5 hours or more, 6 hours or more, 7 hours or more, or 8 hours or more, and 9 hours or less, 10 hours or less, 11 hours or less, 12 hours or less, 13 hours or less, 14 hours or less, 15 hours or less, 16 hours or less, 17 hours or less, 18 hours or less, 19 hours or less, or 20 hours or less. When the firing time is within the above range, a positive electrode active material having a layered structure and excellent structural stability can be produced, and the particle size of the positive electrode active material can be grown to an appropriate degree. The firing may be carried out while maintaining the firing temperature during the firing time.
[0090] The method for producing a positive electrode active material according to the present invention may be carried out under conditions that satisfy the following formula 2.
[0091] [Formula 2] 30.3 ≤ (0.055 × T1) - (20 × P1) ≤ 31.0
[0092] In the above formula 2, P1 is the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide in step (A1), and T1 is the firing temperature in step (B1).
[0093] The inventors have determined the average particle size (D) of the primary particles. 50 ) and the relationship with firing temperature, the average particle size of primary particles (D 50 The inventors derived the relationship between the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide, and the relationship between the crystal grain size (D) and the firing temperature, thereby finding a method for producing a positive electrode active material with improved output characteristics, rate characteristics, and resistance characteristics. Specifically, the inventors found that for every approximately 10°C increase in firing temperature, the average particle size (D) of the primary particles increases. 50 ) increases by 0.55 μm, and for every approximately 0.01 increase in the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide, the average particle size (D) of the primary particles increases. 50 We discovered that the grain size increases by 0.2 μm and that the crystal grain size (D) increases with increasing firing temperature. Using this, we were able to complete a method for manufacturing positive electrode active material with improved output characteristics, rate characteristics, and resistance characteristics.
[0094] Equation 2, i.e., (0.055 × T1) - (20 × P1) (where P1 is the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide in step (A1), T1 is the firing temperature in step (B1), and P and T are dimensionless numbers without units), may be 30.3 or less, or 31.0 or less. Specifically, it may be greater than 28.5, 29 or more, 29.1 or more, 29.2 or more, 29.3 or more, 29.4 or more, 29.5 or more, 29.6 or more, 29.7 or more, 29.8 or more, 29.9 or more, 30.0 or more, 30.1 or more, or 30.2 or more, and may be 30.3 or less, 30.4 or less, 30.5 or less, 30.6 or less, 30.7 or less, 30.8 or less, 30.9 or less, or 31.0 or less. When formula 2 satisfies the above range, it is a single-particle form consisting of 10 or fewer primary particles, and a positive electrode active material with improved lithium mobility can be manufactured by adjusting the average particle size of the primary particles and the size of the crystal grains. On the other hand, if the value of Equation 2 is less than 30.3, there is a problem of poor lifetime characteristics because there are too many inter-grain interfaces that serve as lithium ion migration pathways within the lithium composite transition metal oxide particles. If the value of Equation 2 is greater than 31.0, there is a problem of poor lithium mobility because there are too few inter-grain interfaces that serve as lithium ion migration pathways within the lithium composite transition metal oxide particles, resulting in poor output characteristics, rate characteristics, and resistance characteristics of the secondary battery.
[0095] <Manufacturing method 2> The method for producing a positive electrode active material according to the present invention includes the steps of (A2) mixing a composite transition metal hydroxide and a lithium (Li)-containing raw material to produce a mixture, (B2) calcining the mixture to produce a calcined product, and (C2) heat-treating the calcined product at a temperature of 400°C or higher and 900°C or lower to produce a lithium composite transition metal oxide, and is carried out under conditions that satisfy the following formula 3.
[0096] [Formula 3] 26.0 ≤ (0.055 × T²) - (20 × P²) ≤ 31.5
[0097] In the above equation 3, P2 is the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide in step (A2), and T2 is the firing temperature in step (B2).
[0098] The positive electrode active material according to the present invention described above can be manufactured by appropriately adjusting the type of raw material, firing temperature, firing atmosphere, and so on.
[0099] (A2) Step The method for producing a positive electrode active material according to the present invention includes the step of mixing a composite transition metal hydroxide with a lithium-containing raw material to produce a mixture (A2).
[0100] Step (A2) can be carried out in the same way as step (A1) of the method for producing the positive electrode active material 1, and since step (A1) has been described in detail in the method for producing the positive electrode active material 1, a detailed explanation will be omitted.
[0101] (B2) Step The method for producing a positive electrode active material according to the present invention includes, after step (A2), step (B2) of calcining the mixture to produce a calcined product.
[0102] According to one embodiment of the present invention, the firing may be carried out at a temperature of 700°C or higher and 1,000°C or lower. Specifically, the firing may be carried out at a temperature of 700°C or higher, 710°C or higher, 720°C or higher, 730°C or higher, 740°C or higher, 750°C or higher, 760°C or higher, 770°C or higher, 780°C or higher, 790°C or higher, 800°C or higher, 810°C or higher, 820°C or higher, 830°C or higher, 840°C or higher, 850°C or higher, 860°C or higher, 870°C or higher, 880°C or higher, 890°C or higher, 900°C or higher, 910°C or higher, 920°C or higher, or 930°C or higher, and 940°C or lower, 950°C or lower, 960°C or lower, 970°C or lower, 980°C or lower, 990°C or lower, or 1,000°C or lower. When the firing temperature is within the aforementioned range, the particle size and specific surface area of the positive electrode active material can be easily adjusted, and the capacity characteristics and resistance characteristics of the secondary battery to which it is applied can be improved.
[0103] According to one embodiment of the present invention, the firing may be carried out for a period of 5 hours or more and 20 hours or less. Specifically, the firing may be carried out for a period of 5 hours or more, 6 hours or more, 7 hours or more, or 8 hours or more, 9 hours or more, 10 hours or more, 11 hours or more, 12 hours or more, 13 hours or more, or 14 hours or more, and 15 hours or less, 16 hours or less, 17 hours or less, 18 hours or less, 19 hours or less, or 20 hours or less. When the firing time is within the above range, a positive electrode active material having a layered structure and excellent structural stability can be produced. In particular, when the firing time is 14 hours or more and 20 hours or less, the particle size of the positive electrode active material can be grown to an appropriate degree.
[0104] (C2) Step The method for producing a positive electrode active material according to the present invention includes, after step (B2), step (C2), in which the calcined product is heat-treated at a temperature of 400°C or higher and 900°C or lower.
[0105] The (C2) step can be included to reduce the size of the crystal grains. This improves the lithium mobility of the positive electrode active material, and thus improves the output characteristics, rate characteristics, and resistance characteristics of the secondary battery to which it is applied. The heat treatment is a step distinct from the (B2) step, and the heat treatment temperature may be 50°C or more lower than the firing temperature. Specifically, the heat treatment may be performed at temperatures of 400°C or higher, 500°C or higher, 600°C or higher, or 700°C or higher, and 800°C or lower, or 900°C or lower. When the heat treatment is within the above temperature range, the surface crystals are stabilized, the interface between crystal grains increases due to the reduction in crystal grain size, lithium mobility is improved, and the output characteristics, rate characteristics, and resistance characteristics of the secondary battery to which it is applied can be improved. When the heat treatment is 400°C or lower, there is insufficient thermal energy to stabilize the surface crystals, and the surface crystals are not sufficiently stabilized. When the heat treatment is 900°C or higher, there is a problem that the size of the crystal grains does not decrease.
[0106] According to one embodiment of the present invention, the heat treatment may be performed for a period of 2 hours or more and 10 hours or less. Specifically, the heat treatment may be performed for a period of 2 hours or more, 3 hours or more, or 4 hours or more, and 5 hours or less, 6 hours or less, 7 hours or less, 8 hours or less, 9 hours or less, or 10 hours or less. When the time is within the above range, the surface crystal is stabilized, the interface between crystal grains increases due to the reduction in crystal grain size, lithium mobility is improved, and the output characteristics, rate characteristics, and resistance characteristics of the secondary battery to which this is applied can be improved.
[0107] The method for producing a positive electrode active material according to the present invention (2) is carried out under conditions that satisfy the following formula 3.
[0108] [Formula 3] 26.0 ≤ (0.055 × T²) - (20 × P²) ≤ 31.5
[0109] In the above formula 3, P2 is the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide in step (A2), and T2 is the firing temperature in step (B2).
[0110] The above equation 3, i.e., (0.055 × T2) - (20 × P2) (where P2 is the molar ratio (Li / M) of lithium (Li) present in the lithium-containing raw material to the transition metal (M) present in the composite transition metal hydroxide in step (A2), T2 is the firing temperature in step (B2), and P and T are dimensionless numbers without units), may be between 26.0 and 31.5. Specifically, it may be 26.0 or higher, 26.5 or higher, 27.0 or higher, 27.5 or higher, 28.0 or higher, 28.5 or higher, 29.0 or higher, 29.1 or higher, 29.2 or higher, 29.3 or higher, 29.4 or higher, 29.5 or higher, 29.6 or higher, 29.7 or higher, 29.8 or higher, 29.9 or higher, 30.0 or higher, 30.1 or higher, 30.2 or higher, 30.3 or higher, 30.4 or higher, 30.5 or higher, 30.6 or higher, 30.7 or higher, 30.8 or higher, 30.9 or higher, or 31.0 or higher, and may also be 31.1 or lower, 31.2 or lower, 31.3 or lower, 31.4 or lower, or 31.5 or lower. When equation 3 satisfies the range, it is a single-particle form consisting of 10 or fewer primary particles, and by adjusting the average particle size of the primary particles and the size of the crystal grains, a positive electrode active material with improved lithium mobility can be manufactured. On the other hand, if step (C2) is not included and equation 3 is less than 26.0, there is a problem of poor lifetime characteristics due to too many inter-grain interfaces that serve as lithium ion migration pathways within the lithium composite transition metal oxide particles, and when equation 3 is greater than 31.5, there is a problem of poor lithium mobility due to fewer inter-grain interfaces that serve as lithium ion migration pathways within the lithium composite transition metal oxide particles, resulting in poor output characteristics, rate characteristics, and resistance characteristics of the secondary battery.
[0111] positive electrode Next, the positive electrode according to the present invention will be described.
[0112] The positive electrode according to the present invention includes a positive electrode active material layer containing the positive electrode active material according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, which contains the positive electrode active material. Since the positive electrode active material has been described above, a detailed explanation will be omitted, and only the remaining components will be described in detail below.
[0113] The positive electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and is conductive. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., can be used. The positive electrode current collector can usually have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on the surface of the current collector to improve the adhesion of the positive electrode active material. For example, it may be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0114] The positive electrode active material layer may include a conductive material and a binder together with the positive electrode active material. Here, the positive electrode active material can be included in an amount of 80% to 99% by weight, more specifically 85% to 98.5% by weight, relative to the total weight of the positive electrode active material layer, and within this range, excellent capacitance characteristics can be observed.
[0115] The conductive material is used to impart conductivity to the electrodes and can be used without particular limitations in the battery it is configured in, as long as it does not cause chemical changes and has electronic conductivity. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. Of these, one or more can be used. The conductive material can be included in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.
[0116] The binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more can be used. The binder can be included in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.
[0117] The positive electrode can be manufactured by a conventional method for manufacturing a positive electrode, except that the positive electrode active material described above is used. Specifically, the positive electrode can be manufactured by coating a positive electrode active material layer-forming composition, which is prepared by dissolving or dispersing the positive electrode active material and, selectively, a binder and a conductive material in a solvent, onto a positive electrode current collector, followed by drying and rolling. Here, the types and contents of the positive electrode active material, binder, and conductive material are as described above. Alternatively, the positive electrode can also be manufactured by casting the positive electrode active material layer-forming composition onto another support, peeling it off this support, and then laminating the resulting film onto a positive electrode current collector.
[0118] The solvent may be any solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more can be used. The amount of solvent used should be sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to have a viscosity that allows for excellent thickness uniformity when applied for the manufacture of the positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.
[0119] Lithium-ion battery Next, the lithium secondary battery according to the present invention will be described.
[0120] The present invention makes it possible to manufacture an electrochemical element including the positive electrode. Specifically, the electrochemical element may be a battery, a capacitor, or the like, and more specifically, a lithium secondary battery.
[0121] The lithium secondary battery specifically includes a positive electrode, a negative electrode located opposite the positive electrode, and a separator and electrolyte interposed between the positive and negative electrodes. As the positive electrode has been described previously, a detailed explanation will be omitted, and only the remaining components will be described in detail below.
[0122] Furthermore, the lithium secondary battery may selectively further include a battery container for housing the electrode assembly comprising the positive electrode, negative electrode, and separator, and a sealing member for sealing the battery container.
[0123] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0124] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloys can be used. The negative electrode current collector can usually have a thickness of 3 μm to 500 μm, and, similar to the positive electrode current collector, fine irregularities can be formed on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it can be used in various forms such as film, sheet, foil, mesh, porous material, foam, and nonwoven fabric.
[0125] The negative electrode active material layer selectively includes a binder and a conductive material together with the negative electrode active material.
[0126] As the negative electrode active material, compounds capable of reversible intercalation and deintercalation of lithium can be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO2. βExamples include metallic oxides that can be doped and dedoped with lithium, such as (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compound and carbonaceous material, such as Si-C composites or Sn-C composites; and any one or more mixtures thereof can be used. A metallic lithium thin film can also be used as the negative electrode active material. Furthermore, both low-crystallinity carbon and high-crystallinity carbon can be used as the carbon material. Examples of low-crystalline carbon include soft carbon and hard carbon, while examples of high-crystalline carbon include amorphous, plate-like, flaky, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0127] The anode active material can be present in an amount of 80% to 99% by weight relative to the total weight of the anode active material layer.
[0128] The binder is a component that helps to bond the conductive material, active material, and current collector, and is usually added in an amount of 0.1% to 10% by weight relative to the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0129] The conductive material is a component for further improving the conductivity of the negative electrode active material, and can be added in an amount of 10% by weight or less, specifically 5% by weight or less, relative to the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives can be used.
[0130] The negative electrode active material layer can be manufactured by coating a negative electrode active material layer-forming composition, which is prepared by dissolving or dispersing a negative electrode active material and, selectively, a binder and a conductive material in a solvent, onto a negative electrode current collector and drying it, or by casting the negative electrode active material layer-forming composition onto another support, peeling it off the support, and then laminating the resulting film onto the negative electrode current collector.
[0131] On the other hand, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Generally, any separator used in lithium secondary batteries can be used without particular limitations, but those with low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity are particularly preferred. Specifically, porous polymer films, such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, ethylene / hexene copolymers, and ethylene / methacrylate copolymers, or laminated structures of two or more layers thereof can be used. Ordinary porous nonwoven fabrics, such as nonwoven fabrics made of high-melting-point glass fibers or polyethylene terephthalate fibers, can also be used. Furthermore, coated separators containing ceramic components or polymeric substances can be used to ensure heat resistance or mechanical strength, and may be selectively used in single-layer or multi-layer structures.
[0132] Furthermore, the electrolytes used in the present invention include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0133] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0134] The organic solvent can be used without particular limitations, as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvents include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (propylene Carbonate solvents such as carbonate (PC); alcoholic solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms, and can include a double-bonded aromatic ring or ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, carbonate solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery, and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred. In this case, mixing the cyclic carbonate and linear carbonate in a volume ratio of about 1:1 to about 1:9 can improve the performance of the electrolyte.
[0135] The lithium salt can be any compound capable of providing lithium ions for use in lithium secondary batteries, without any particular limitations. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, etc. The concentration of the lithium salt is preferably in the range of 0.1 to 5.0 M, specifically 0.1 to 3.0 M. When the concentration of the lithium salt falls within this range, the electrolyte has appropriate conductivity and viscosity, exhibiting excellent electrolyte performance and allowing lithium ions to move effectively.
[0136] In addition to the components of the electrolyte, the electrolyte may further contain one or more additives for purposes such as improving battery life characteristics, suppressing battery capacity reduction, and improving battery discharge capacity. These additives may include, for example, haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride. Here, the additive may be present in an amount of 0.1 to 10% by weight, specifically 0.1 to 5% by weight, relative to the total weight of the electrolyte.
[0137] As described above, lithium secondary batteries containing the positive electrode active material according to the present invention exhibit excellent energy density, efficiency characteristics, resistance characteristics, and rate characteristics, making them useful in portable devices such as mobile phones, notebook computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0138] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0139] The aforementioned battery module or battery pack can be used as a power source for one or more medium-to-large devices, including power tools; electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.
[0140] The external shape of the lithium secondary battery of the present invention is not particularly limited, but may be cylindrical, rectangular, pouch-type, or coin-type using a can.
[0141] In addition to being usable as a battery cell for powering small devices, the lithium secondary battery according to the present invention can also be preferably used as a unit battery in medium- and large-sized battery modules containing a large number of battery cells. [Examples]
[0142] Hereinafter, embodiments of the present invention will be described in detail so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention can be realized in various different forms and is not limited to the embodiments described herein.
[0143] Examples and Comparative Examples Example 1 Ni 0.62 Co 0.06 Mn 0.32A composite transition metal hydroxide (product name: Nickel cobalt manganese hydroxide, average particle size: 3-4 μm, secondary particles) having a composition represented by (OH)2, Li2CO3 was mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.07, and ZrO2 and Y2O3 were mixed to produce a mixture. Here, ZrO2 is the same as the Ni 0.62 Co 0.06 Mn 0.32 Mix (OH)2 so that the Zr content is 1,500 ppm relative to the total weight, and Y2O3 is Ni 0.62 Co 0.06 Mn 0.32 The mixture was prepared so that Y contained 3,000 ppm relative to the total weight of (OH)2.
[0144] The aforementioned mixture was calcined in an air atmosphere at a temperature of 940°C for 9 hours to produce a lithium composite transition metal oxide (cathode active material).
[0145] Example 2 Ni 0.62 Co 0.06 Mn 0.32 A composite transition metal hydroxide (product name: Nickel cobalt manganese hydroxide, average particle size: 3-4 μm, secondary particles) having a composition represented by (OH)2, Li2CO3 was mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.06, and ZrO2 and Y2O3 were mixed to produce a mixture. Here, ZrO2 is the same as the Ni 0.62 Co 0.06 Mn 0.32 Mix (OH)2 so that the Zr content is 1,500 ppm relative to the total weight, and Y2O3 is Ni 0.62 Co 0.06 Mn 0.32 The mixture was prepared so that Y contained 3,000 ppm relative to the total weight of (OH)2.
[0146] The mixture was fired in an air atmosphere at a temperature of 950°C for 14 hours to produce a fired product. Then, the fired product was heat-treated in an air atmosphere at a temperature of 800°C for 4 hours to produce a lithium composite transition metal oxide (cathode active material).
[0147] Comparative Example 1 Ni 0.62 Co 0.06 Mn 0.32 A composite transition metal hydroxide (product name: Nickel cobalt manganese hydroxide, average particle size: 3-4 μm, secondary particles) having a composition represented by (OH)2, Li2CO3 was mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.06, and ZrO2 and Y2O3 were mixed to produce a mixture. Here, ZrO2 is the same as the Ni 0.62 Co 0.06 Mn 0.32 Mix (OH)2 so that the Zr content is 1,500 ppm relative to the total weight, and Y2O3 is Ni 0.62 Co 0.06 Mn 0.32 The mixture was prepared so that Y contained 3,000 ppm relative to the total weight of (OH)2.
[0148] The aforementioned mixture was calcined in an air atmosphere at a temperature of 950°C for 9 hours to produce a lithium composite transition metal oxide (cathode active material).
[0149] Comparative Example 2 Ni 0.62 Co 0.06 Mn 0.32 A composite transition metal hydroxide (product name: Nickel cobalt manganese hydroxide, average particle size: 3-4 μm, secondary particles) having a composition represented by (OH)2, Li2CO3 was mixed so that the molar ratio of (Ni+Co+Mn):Li was 1:1.04, and ZrO2 and Y2O3 were mixed to produce a mixture. Here, ZrO2 is the same as the Ni 0.62 Co 0.06 Mn 0.32 Mix (OH)2 so that the Zr content is 1,500 ppm relative to the total weight, and Y2O3 is Ni 0.62 Co 0.06 Mn 0.32 The mixture was prepared so that Y contained 3,000 ppm relative to the total weight of (OH)2.
[0150] The mixture was calcined in an air atmosphere at a temperature of 960°C for 9 hours to prepare a lithium composite transition metal oxide (cathode active material).
[0151] Comparative Example 3 The calcined product of Example 2 was used as the cathode active material of Comparative Example 3.
[0152] Comparative Example 4 Ni 0.62 Co 0.06 Mn 0.32 A composite transition metal hydroxide having a composition represented by (OH)2 (product name: Nickel cobalt manganese hydroxide, average particle size: 3~4μm, secondary particles) and Li2CO3 were mixed such that the molar ratio of (Ni+Co+Mn):Li was 1:1.06, and ZrO2 and Y2O3 were mixed to prepare a mixture. Here, ZrO2 is the above Ni 0.62 Co 0.06 Mn 0.32 It was mixed such that the content of Zr was 1,500 ppm relative to the total weight of (OH)2, and Y2O3 was mixed such that the content of Ni 0.62 Co 0.06 Mn 0.32 It was mixed such that the content of Y was 3,000 ppm relative to the total weight of (OH)2.
[0153] The mixture was calcined in an air atmosphere at a temperature of 909°C for 9 hours to prepare a lithium composite transition metal oxide (cathode active material).
[0154] [Table 1]
[0155] Experimental example Experimental Example 1: ICP Analysis After taking 0.1 g each of the positive electrode active materials produced in Examples 1-2 and Comparative Examples 1-4, 1 ml of hydrochloric acid was added and heated to dissolve the positive electrode active materials. Next, a small amount of hydrogen peroxide was added to accelerate the reaction and completely dissolve the positive electrode active materials to prepare a solution. Then, the solution was diluted with deionized water to a total volume of 10 ml to prepare the analytical sample. Using an ICP instrument (ICP-OES; Agilent 5100, manufactured by Agilent Technologies), the weight ratio of the constituent elements present in the analytical sample was measured to determine the composition of the positive electrode active material, M 1 The content (ppm) is shown in Table 2 below.
[0156] [Table 2]
[0157] Referring to Table 2 above, it was confirmed that the lithium composite transition metal oxides produced in Examples 1 and 2 have the composition represented by Chemical Formula 1 and contain the doping elements Zr and Y.
[0158] Experimental Example 2: Analysis of Single Crystallinity - Measurement of the average particle size of primary particles Using a SEM (FEI, Inspect F), SEM images (5K magnification) of the positive electrode active materials manufactured in Examples 1-2 and Comparative Examples 1-4 were acquired. Using an image processing program (LG Chem, DX program), images were obtained that separated the boundaries of primary particles present in the SEM images and displayed them in random colors. These images are shown in Figures 1-6 below. Using the images that separated the boundaries of primary particles and displayed them in random colors, the area of each primary particle was calculated based on the number of pixels corresponding to each of the n primary particles (an average of 50,000 or more primary particles). The average particle size (D) of the primary particles present in the positive electrode active materials manufactured in Examples 1, 2 and Comparative Examples 1-4 was calculated using the radius of a circle having the same area as each primary particle. 50 The following measurements were taken and are shown in Table 3 below.
[0159] Figure 1 is an SEM image of the positive electrode active material produced in Example 1.
[0160] Figure 2 is an SEM image of the positive electrode active material produced in Example 2.
[0161] Figure 3 is an SEM image of the positive electrode active material produced in Comparative Example 1.
[0162] Figure 4 is an SEM image of the positive electrode active material produced in Comparative Example 2.
[0163] Figure 5 is an SEM image of the cathode active material produced in Comparative Example 3.
[0164] Figure 6 is an SEM image of the positive electrode active material produced in Comparative Example 4.
[0165] - Measurement of grain size (D) For each of the positive electrode active materials produced in Examples 1 and 2 and Comparative Examples 1 to 4, a positive electrode slurry was prepared by mixing 95% by weight of the positive electrode active material, 2.0% by weight of carbon black as a conductive material, and 3.0% by weight of polyvinylidene fluoride (PVDF) as a binder in an N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of an aluminum current collector and dried at 130°C to produce a positive electrode for EBSD analysis. No rolling was performed during the production of the positive electrode.
[0166] The cross-section of the positive electrode was cut using an ion milling device (HITACHI IM-400, accelerating voltage 6kV), and an EBSD analysis was performed on the cross-section of the positive electrode using an FE-SEM (FEI Corporation, QuantaFEG 250) equipped with an electron backscatter diffraction pattern analyzer (EBSD) to obtain an IPF map, which is shown in Figures 7 to 12 below.
[0167] EBSD analysis was performed on a scale where the grain size was approximately 0.5 μm or larger, under conditions of an acceleration voltage of 20 kV and a working width (WD) of 16 mm.
[0168] After calculating the grain size from the grain area observed in the IPF map image, the measured grain size (D) obtained by calculating the arithmetic mean of these values is shown in Table 3 below.
[0169] And the average particle size of the primary particles (D 50 The degree of single crystallinity (χ) calculated by substituting the crystal grain size (D) and the crystal grain size (D) into Equation 1 described herein is shown in Table 3 below.
[0170] Figure 7 shows the IPF map obtained by EBSD analysis of a cathode for EBSD analysis manufactured using the cathode active material produced in Example 1.
[0171] Figure 8 shows the IPF map obtained by EBSD analysis of a cathode for EBSD analysis manufactured using the cathode active material produced in Example 2.
[0172] Figure 9 shows the IPF map obtained by EBSD analysis of a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 1.
[0173] Figure 10 shows the IPF map obtained by EBSD analysis of a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 2.
[0174] Figure 11 shows the IPF map obtained by EBSD analysis of a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 3.
[0175] Figure 12 shows the IPF map obtained by EBSD analysis of a cathode for EBSD analysis manufactured using the cathode active material produced in Comparative Example 4.
[0176] [Table 3]
[0177] Refer to Table 3. The positive electrode active materials produced in Examples 1 and 2 have an average particle size (D) of primary particles. 50) was 2.35 μm or more and 6.00 μm or less, the grain size (D) was 2.00 μm or more and 5.00 μm or less, and the single crystallinity (χ) calculated by Equation 1 described in this specification was 0.500 or more and 0.850 or less. On the other hand, it was confirmed that the positive electrode active materials prepared in Comparative Examples 1 to 3 had a single crystallinity (χ) of more than 0.850, and the positive electrode active material prepared in Comparative Example 4 had a single crystallinity (χ) of 0.500 or more and 0.850 or less, and the grain size (D) was less than 2.00 μm.
[0178] Experimental Example 3: Measurement of Rolling Density 5 g of each positive electrode active material of Examples and Comparative Examples was put into a circular 4-point probe (Gold Pin) mold of a resistance measuring instrument (manufactured by Hantech) having a diameter of 2.2 cm, and force was applied until a force corresponding to 2,000 kgf was reached. The heights of the pellets formed (the difference between the height of the mold before charging the positive electrode active material and the height of the mold after applying a force of 2,000 kgf) were measured, respectively. From the height of the pellet, the rolling density (g / cm 3 ) was calculated and shown in Table 4 below.
[0179] [Equation 4] Volume of pellet (cm 3 ) = π (radius of circular pellet holder) 2 × Height of pellet
[0180] [Equation 5] Rolling density (g / cm 3 ) = Weight of positive electrode active material (g) / Volume of pellet (cm 3 )
[0181] [Table 4]
[0182] Referring to Table 4, it was confirmed that the positive electrode active materials prepared in Examples 1 and 2 had higher rolling densities than the positive electrode active materials prepared in Comparative Examples 2 to 4.
[0183] In particular, we confirmed that the positive electrode active material produced in Comparative Example 4, i.e., when the crystal grain size (D) was less than 2.00 μm, had too many inter-grain interfaces that served as pathways for lithium ions within the positive electrode active material particles, resulting in the lowest rolling density.
[0184] Experimental Example 4: Evaluation of Battery Characteristics - Manufacturing of coin-type half-cells A positive electrode slurry was prepared by mixing 95% by weight of the positive electrode active material produced in Examples 1 and 2 and Comparative Examples 1 to 4, 2.0% by weight of carbon black as a conductive material, and 3.0% by weight of polyvinylidene fluoride (PVDF) as a binder in an N-methylpyrrolidone (NMP) solvent. The prepared positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C, and then rolled to produce a positive electrode.
[0185] An electrode assembly was manufactured using a lithium metal electrode as the negative electrode, with a porous polyethylene separator interposed between the positive and negative electrodes. This assembly was placed inside a battery case, and an electrolyte solution prepared by dissolving 1.0 M LiPF6 in an organic solvent mixture of ethylene carbonate (EC): ethyl methyl carbonate (EMC): diethyl carbonate (DEC) in a volume ratio of 3:3:4 was injected to manufacture a coin-type half-cell.
[0186] - Evaluation of battery characteristics Using the coin-type half-cell manufactured as described above, it was charged to 4.45V at 25°C using the CC-CV method (0.1C), and then discharged to 2.5V using the CC method (0.1C). The charge and discharge capacities were measured during this process. The percentage of the discharge capacity relative to the measured charge capacity (efficiency (%)) is shown in Table 5 below.
[0187] Next, the battery was charged to 4.25V using the CC-CV method at 25°C (0.1C), and then discharged to 2.5V using the CC method (2.0C). The charge and discharge capacities during this process were then measured.
[0188] Table 5 below shows the percentage of the discharge capacity at 2.0C to the measured discharge capacity at 0.1C (2C / 0.1C).
[0189] Furthermore, the DC internal resistance (DCIR) was calculated and is shown in Table 5 below. The DCIR value is calculated by dividing the difference between the voltage at which 60 seconds of discharge with a constant current of 0.1C occurred and the initial voltage by the applied current during the initial charge and discharge.
[0190] [Table 5]
[0191] Referring to Table 5, it was confirmed that the batteries containing the positive electrode active materials manufactured in Examples 1 and 2 had an efficiency (%) of 89.7% or higher at 0.1C, a DCIR of 33.7Ω or less at 0.1C, an efficiency of 94.0% or higher at 2C, and a 2C / 0.1C ratio of 85.0% or higher.
[0192] On the other hand, the batteries containing the positive electrode active materials produced in Comparative Examples 1 and 2 had an efficiency (%) of less than 89.7% at 0.1C, a DCIR of more than 33.7Ω at 0.1C, an efficiency of less than 94.0% at 2C, and a 2C / 0.1C ratio of less than 85.0%, confirming that their output, resistance, and rate characteristics were inferior to those of the batteries containing the positive electrode active materials produced in Examples 1 and 2. Furthermore, the battery containing the positive electrode active material produced in Comparative Example 3 had an efficiency of less than 94.0% at 2C and a 2C / 0.1C ratio of less than 85.0%, confirming that its output and rate characteristics were inferior to those of the batteries containing the positive electrode active materials produced in Examples 1 and 2.
[0193] For reference, the battery containing the positive electrode active material manufactured in Comparative Example 4 did not undergo separate evaluation of its battery characteristics due to its inferior rolling density.
[0194] In other words, referring to Tables 4 and 5, it was confirmed that the positive electrode active material according to the present invention is in single-particle form, contains a lithium composite transition metal oxide with nickel at a concentration of 50 mol% or more of the total metals other than lithium, has a specific range of single crystallinity, has a specific range of crystal grain size, improves the rolling density of the positive electrode active material, and improves the electrochemical properties of a battery containing it.
Claims
1. It is a single-particle form consisting of 10 or fewer primary particles, and contains a lithium composite transition metal oxide in which nickel accounts for 50 mol% or more of the total metal other than lithium. The degree of single crystallinity (χ) calculated by formula 1 below is 0.500 or greater and 0.850 or less. A positive electrode active material having a crystal grain size (D) of 2.00 μm or more and 5.00 μm or less. [Math 1]
2. The lithium composite transition metal oxide has a composition represented by the following chemical formula 1, wherein it is the positive electrode active material according to claim 1: [Chemical formula 1] Li 1+x Ni a Co b Mn c M 1 d O 2 In the aforementioned chemical formula 1, Said M 1 is one or more selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si. -0.10 ≤ x ≤ 0.10, 0.500 ≤ a < 1.000, 0 < b < 0.500, 0 < c < 0.500, 0 ≤ d ≤ 0.100, and a + b + c + d = 1.
3. The positive electrode active material according to claim 1, wherein the lithium composite transition metal oxide comprises one or more doping elements selected from Al, W, Co, B, Zr, Y, Ce, Hf, La, Ba, F, P, S, Nb, Ta, Sc, Cr, V, Cu, Sr, Ti, Mg, Mo, Sn, Fe, Zn, and Si.
4. The average particle size (D 50 ) of the primary particles is 2.35 μm or more and 6.00 μm or less, The positive electrode active material according to claim 1.
5. A positive electrode comprising the positive electrode active material described in any one of claims 1 to 4.
6. A lithium secondary battery comprising the positive electrode described in claim 5.
Citation Information
Patent Citations
Positive electrode active material for secondary battery, method for preparing the same and lithium secondary battery comprising the same
KR1020190131842A