Lithium-ion battery
The lithium secondary battery employs a single-crystal cathode and Si-C composite anode to balance irreversible capacities, addressing the reactivity and volume change issues in conventional lithium-ion batteries, resulting in enhanced energy density and lifespan.
Patent Information
- Application Number
- JP2026526768
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-22
- Filing Date
- 2024-12-18
- Publication Date
- 2026-11-24
AI Technical Summary
Lithium-ion batteries face challenges with high reactivity of nickel in positive electrode active materials leading to structural breakdown and rapid degradation, and Si-based anode materials experiencing significant volume changes and poor efficiency, resulting in reduced lifespan and energy density.
A lithium secondary battery design using a single-crystal cathode active material with a medium particle size and a Si-C composite anode active material, where the irreversible capacity of the anode is smaller than that of the cathode, enhancing energy density and lifespan characteristics.
The design minimizes volume expansion of the negative electrode and suppresses rapid degradation of the cathode active material, achieving higher energy density and improved lifespan by balancing irreversible capacities between the electrodes.
Smart Images

Figure 2026539335000001_ABST
Abstract
Description
[Technical Field]
[0001] This invention claims priority under Korean Patent Application No. 10-2023-0190458 dated December 22, 2023, and all content disclosed in the documents of the said Korean Patent Application is incorporated herein by reference.
[0002] The present invention relates to lithium secondary batteries, including all-solid-state lithium secondary batteries, and more particularly to lithium secondary batteries with excellent energy density and life characteristics. [Background technology]
[0003] Lithium-ion batteries generally consist of a positive electrode, a negative electrode, and a separator. 、 The battery consists of a positive electrode and an electrolyte, and the positive electrode and negative electrode contain an active material that allows for the insertion and deintercalation of lithium ions. 、 and a solid electrolyte, wherein the negative electrode includes an active material capable of inserting and removing lithium ions.
[0004] recent years With the rapid growth of the electric vehicle market, there is a growing need for batteries with superior rapid charging performance and high energy density. Consequently, there is an increasing number of attempts to use high-nickel lithium-nickel oxides, which have excellent capacity characteristics, as the positive electrode active material, and Si-based negative electrode active materials, which have excellent rapid charging performance and capacity characteristics, as the negative electrode active material.
[0005] However, while increasing the nickel content in the positive electrode active material improves capacity characteristics, repeated charging and discharging will result in higher reactivity due to the high reactivity of nickel. +4 A large amount of ions are generated, causing structural breakdown of the positive electrode active material. This increases the degradation rate of the positive electrode active material, leading to a problem of reduced lifespan characteristics.
[0006] In addition, the Si-based anode active material has a large irreversible capacity, leading to poor anode efficiency, and undergoes significant volume changes during charge and discharge processes. Consequently, the anode deteriorates rapidly during charge and discharge, resulting in poor lifespan characteristics.
[0007] Accordingly, there is a demand for the development of lithium secondary batteries that achieve high energy density and have excellent lifespan characteristics. [Summary of the Invention] [Problem to be Solved by the Invention]
[0008] The present invention is intended to solve the above problems. It applies a medium particle size single-crystal cathode active material and an anode active material containing a Si-C composite, and is designed such that the irreversible capacity of the anode is smaller than that of the cathode, thereby providing a lithium secondary battery with high energy density and excellent lifespan characteristics. [Means for Solving the Problem]
[0009] According to one embodiment, the present invention provides a lithium secondary battery comprising: a cathode including a single-crystal cathode active material with a D 50 of 5.5 μm to 8 μm; an anode including a first anode active material containing a Si-C composite; and an electrolyte, wherein the irreversible capacity per unit area of the anode is smaller than the irreversible capacity per unit area of the cathode. Here, the ratio of the irreversible capacity per unit area of the cathode to the irreversible capacity per unit area of the anode may be greater than 1, preferably 1.01 to 1.25, and more preferably 1.01 to 1.2.
[0010] Meanwhile, the single-crystal cathode active material may include a lithium nickel-based oxide containing 88 mol% or more, preferably 90 mol% or more of Ni. The lithium nickel-based oxide may be represented by, for example, the following [Chemical Formula 1]. [Chemical Formula 1] Li 1+x [Ni a Co b M 1 c M 2 d]O2 In the above [Chemical Formula 1], M 1 is one or more selected from Mn and Al, and M 2 are Zr, Y, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P 、 It includes one or more selected from the group consisting of and S, where -0.2≦x≦0.2, 0.88≦a<1, 0 <b<0.12、0<c<0.12、0≦d≦0.05である。
[0011] On the other hand, the positive electrode of porosity teeth, The amount may be 16% to 24%, preferably 16% to 23%, and more preferably 17% to 23%.
[0012] The total thickness of the positive electrode may be 90 μm to 120 μm, preferably 90 μm to 110 μm, and more preferably 95 μm to 105 μm.
[0013] The positive electrode of efficiency teeth, It may be less than 90%, preferably 87% or more and less than 90%, and more preferably 87% to 89%.
[0014] The discharge capacity of the positive electrode may be 200mAh / g to 400mAh / g, 200mAh / g to 300mAh / g, 210mAh / g to 300mAh / g, or 210mAh / g to 250mAh / g.
[0015] On the other hand, the negative electrode may further contain a graphite-based negative electrode active material as a second negative electrode active material. Here, the weight ratio of the first negative electrode active material to the second negative electrode active material may be 2:98 to 20:80, preferably 2:98 to 15:85, and more preferably 5:95 to 15:85.
[0016] The negative electrode of porosity teeth, The amount may be 20% to 30%, preferably 22% to 29%, and more preferably 23% to 28%.
[0017] The negative electrode of Full thickness teeth, The particle size may be 80 μm to 130 μm, preferably 90 μm to 120 μm, and more preferably 95 μm to 120 μm.
[0018] The negative electrode of efficiency teeth, It may be 90% or more, preferably 90% to 94%, and more preferably 90% to 93%.
[0019] The discharge capacity of the negative electrode may be 400 mAh / g to 600 mAh / g, preferably 400 mAh / g to 550 mAh / g, and more preferably 450 mAh / g to 550 mAh / g.
[0020] Lithium secondary battery according to the present invention of N / P ratio teeth, It may be 105 or higher, preferably 106 to 110, and more preferably 106.5 to 108.
[0021] On the other hand, the lithium secondary battery has one negative electrode and one positive electrode. 、 It may include at least one unit cell composed of two separators, the thickness of which is 220 μm to 240 μm, or 225 μm to 240 μm. 、 Alternatively, the particle size may be 230 μm to 240 μm. Furthermore, the capacity per unit volume of the unit cell is 270 mAh / cm³. 3 Preferably 270mAh / cm² 3 ~330mAh / cm 3 , more preferably 290mAh / cm² 3 ~320mAh / cm 3 That's fine. [Effects of the Invention]
[0022] The lithium secondary battery according to the present invention includes a positive electrode active material containing a single-particle type lithium nickel-based oxide having a relatively larger average particle size compared to conventional materials, and a negative electrode active material containing a Si-C composite. In the case of a single-particle type positive electrode active material, resistance increases as the particle size increases, therefore, as in the present invention, D 50When a single-particle type cathode active material with a large size is applied, the cathode resistance increases, which in turn increases the irreversible capacitance of the cathode. On the other hand, Si-C composites are conventional from Compared to silicon oxide, which is mainly used as a Si-based negative electrode active material, it has a smaller irreversible capacity. In other words, the lithium secondary battery of the present invention is designed so that the irreversible capacity of the negative electrode is smaller than that of the positive electrode, unlike conventional lithium secondary batteries, by increasing the resistance of the positive electrode to increase the irreversible capacity of the positive electrode and applying a negative electrode active material with a small irreversible capacity. In this way, when the irreversible capacity of the negative electrode is smaller than that of the positive electrode, the use of the low-potential region that causes volume expansion of the negative electrode during charging and discharging is minimized. So This minimizes the volume expansion of the negative electrode, thereby improving the reduction in lifespan characteristics due to the deterioration of the negative electrode.
[0023] On the other hand, the Si-C composite used as the negative electrode active material in this invention has superior capacity characteristics compared to silicon oxide. Therefore, when applied, it is possible to achieve a higher energy density than in the conventional method.
[0024] On the other hand, when a single-particle type cathode active material with a large average particle size is applied, as in the present invention, the rapid degradation of the cathode active material due to an increase in Ni content can be suppressed. Therefore, in the present invention, a high-nickel cathode active material with a high Ni content of 88 mol% or more can be applied, thereby achieving a high energy density. [Brief explanation of the drawing]
[0025] [Figure 1] This is a scanning electron microscope image of a single-particle cathode active material. [Figure 2] This is a scanning electron microscope image of a pseudo-single-particle cathode active material. [Figure 3] This is a scanning electron microscope image of a secondary particle type cathode active material. [Modes for carrying out the invention]
[0026] Terms and words used in this specification and claims are usually of Alternatively, it should not be interpreted in a way that is limited to the dictionary definition, and the inventors is In accordance with the principle that terms can be appropriately defined to best describe the invention, the terms should be interpreted to have meanings and concepts consistent with the technical idea of this invention.
[0027] In this invention, "single-particle type" refers to a particle consisting of 30 or fewer nodules, and is a concept that includes single particles consisting of one nodule and pseudo-single particles which are composites of 2 to 30 nodules. Figure 1 shows a scanning electron microscope image of a single-particle form of positive electrode active material, and Figure 2 shows a scanning electron microscope image of a pseudo-single-particle form of positive electrode active material.
[0028] The aforementioned "nodule" constitutes a single particle and a pseudo-single particle. Sub It is a single crystal consisting of individual particles and lacking crystalline grain boundaries, or 、 Using a scanning electron microscope te5 Even if the material is a polycrystalline material where no grain boundaries are visible when observed at a field of view of 000x to 20000x, it is still acceptable.
[0029] In the present invention, "secondary particles" refer to particles formed by the aggregation of multiple primary particles, for example, tens to hundreds of primary particles. Specifically, secondary particles may be aggregates of 31 or more, 50 or more, 70 or more, or 100 or more primary particles. Figure 3 shows a scanning electron microscope image of a secondary particle type cathode active material.
[0030] In this invention, "particle" refers to a single particle, a pseudo-single particle, a primary particle, or a nodule. 、 This concept includes one or all of the following: and secondary particles.
[0031] In the present invention, the average particle size (D) of the nodule or primary particle mean) After measuring the particle size of the nodules or primary particles observed from the scanning electron microscope image to This refers to the calculated arithmetic mean.
[0032] In the present invention, "D 50 "50% of the volume cumulative particle size distribution of the powder being measured represents the particle size corresponding to 50% of the volume cumulative amount, and can be measured using the laser diffraction method. For example, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac MT 3000), and ultrasonic waves at approximately 28 kHz are irradiated at an output of 60 W. death, After obtaining a volume-cumulative particle size distribution graph, the particle size corresponding to 50% of the cumulative volume can be determined to perform the measurement.
[0033] In the present invention, "irreversible capacity" means the difference between the charging capacity and the discharging capacity, and the irreversible capacity of the negative electrode and the irreversible capacity of the positive electrode can be measured according to the following methods, respectively.
[0034] <Method for measuring the irreversible capacitance of the negative electrode> Prepare a single-sided negative electrode, in which a negative electrode composite layer is formed on one side of the negative electrode current collector. If the negative electrode to be measured is a double-sided negative electrode, in which a negative electrode composite layer is formed on both sides of the negative electrode current collector, clean and remove the negative electrode composite layer formed on one side to prepare a single-sided negative electrode. Fabricate a negative electrode coin half-cell using the single-sided negative electrode prepared as described above and a lithium metal electrode as the counter electrode. death, The battery can be charged to 5mV in 0.1C, CC-CV mode (0.005C cutoff), then discharged to 1V in 0.1C, CC mode to measure the charge and discharge capacities, and the difference between the measured charge and discharge capacities can be calculated as the irreversible capacity. Furthermore, the irreversible capacity per unit area can be calculated by dividing the irreversible capacity by the negative electrode area. There are no particular restrictions on the timing of measurement of the irreversible capacity. The irreversible capacity of the negative electrode can be measured, for example, using a negative electrode obtained by disassembling a battery.
[0035] <Method for measuring irreversible capacitance of the positive electrode> Prepare a single-sided positive electrode, in which a positive electrode composite layer is formed on one side of the positive electrode current collector. If the positive electrode to be measured is a double-sided positive electrode, in which positive electrode composite layers are formed on both sides of the positive electrode current collector, clean and remove the positive electrode composite layer formed on one side to prepare a single-sided positive electrode. Fabricate a positive electrode coin half-cell using the single-sided positive electrode prepared as described above and a lithium metal electrode as the counter electrode. death, The battery can be charged to 4.25V to 4.4V in 0.1C, CC-CV mode (0.05C cut-off), then discharged to 3V in 0.1C, CC mode to measure the charge and discharge capacities. The difference between the measured charge and discharge capacities can then be calculated as the irreversible capacity. Furthermore, the irreversible capacity per unit area can be calculated by dividing the irreversible capacity by the positive electrode area. There are no particular restrictions on the timing of the measurement of the irreversible capacity. The irreversible capacity of the positive electrode can be measured, for example, using a positive electrode obtained by disassembling a battery.
[0036] Here, the charging termination voltage may vary depending on the type of positive electrode active material. For example, if the positive electrode active material is a secondary particle type NCM with a Ni content of 80 mol% or more, the charging termination voltage may be 4.25V to 4.3V, and if the positive electrode active material is a single particle type NCM with a Ni content of 70 mol% or less, the charging termination voltage may be 4.3V to 4.4V.
[0037] In this invention, the "porosity (%)" can be calculated by (1 - electrode density / electrode true density) × 100. The electrode density can be measured by dividing the electrode weight by the electrode volume after measuring the electrode weight and volume, and the electrode true density can be measured using a gas pyrcnometer. A gas pyrcnometer is a device that can measure the density by placing a sample of known weight in a sample chamber, injecting helium or nitrogen gas, and deriving the volume occupied by the sample other than pores. Specifically, after measuring the volume of the sample from the change in pressure between the sample chamber containing the sample and a reference chamber of known volume, idealThe density value of a sample can be calculated by applying the ideal gas law (PV=nRT).
[0038] In this invention, "efficiency" means the ratio of discharge capacity to charge capacity.
[0039] The present invention will be described in more detail below.
[0040] The inventors of this invention have diligently conducted research to develop a lithium secondary battery that achieves high energy density and excellent lifespan characteristics, and as a result, D 50 When manufacturing a lithium secondary battery using a single-particle positive electrode active material with a particle size of 5.5 μm to 8 μm and a negative electrode active material containing a Si-C composite, such that the irreversible capacity per unit area of the negative electrode is smaller than the irreversible capacity per unit area of the positive electrode, the energy density and life characteristics are as follows: 、 We discovered that we could achieve excellent performance in both charging and rapid charging, and thus completed the present invention.
[0041] Specifically, the lithium secondary battery according to the present invention is D 50 The device comprises a positive electrode containing a single-particle positive electrode active material having a particle size of 5.5 μm to 8 μm, a negative electrode containing a first negative electrode active material containing a Si-C composite, and an electrolyte, characterized in that the irreversible capacity per unit area of the negative electrode is smaller than the irreversible capacity per unit area of the positive electrode. Here, the ratio of the irreversible capacity per unit area of the positive electrode to the irreversible capacity per unit area of the negative electrode may be greater than 1, preferably 1.01 to 1.25, and more preferably 1.01 to 1.2.
[0042] Because Si-based negative electrode active materials have a large irreversible capacity, conventional lithium secondary batteries using Si-based negative electrode active materials generally have a negative electrode irreversible capacity greater than that of the positive electrode. On the other hand, when the irreversible capacity of the negative electrode is greater than that of the positive electrode, the range of the drive voltage is limited to a range other than the irreversible capacity of the negative electrode. This results in a loss of the reversible capacity of the positive electrode, reducing the overall capacity, and forcing the use of a low-potential region of the negative electrode where the volume expansion of the Si-based negative electrode active material occurs rapidly, leading to a problem of reduced lifespan characteristics.
[0043] To solve these problems, the present invention provides a positive electrode active material that is D compared to conventional materials. 50 A lithium secondary battery was designed using a large single-particle positive electrode active material and a Si-C composite as the negative electrode active material, such that the irreversible capacity per unit area of the positive electrode is greater than the irreversible capacity per unit area of the negative electrode.
[0044] Single-particle cathode active materials have fewer interparticle interfaces that serve as pathways for lithium ion movement, from Compared to commonly used secondary particles, the resistance is higher, and the resistance increases further as the particle size increases. Therefore, D 50 When a single-particle type positive electrode active material with a large resistance is applied, the efficiency of the positive electrode decreases due to the increase in resistance, and the irreversible capacity increases. Specifically, the positive electrode according to the present invention can have an efficiency of less than 90%, preferably 87% or more and less than 90%, and more preferably 87% to 89%.
[0045] On the other hand, since the Si-C composite has a smaller irreversible capacity compared to the silicon oxide-based anode active material that was previously mainly used, applying it increases the efficiency of the anode and decreases the irreversible capacity compared to conventional materials. Specifically, the anode according to the present invention can have an efficiency of 90% or more, preferably 90% to 94%, and more preferably 90% to 93%.
[0046] Therefore, D 50 When a large single-particle positive electrode active material and a negative electrode active material containing a Si-C composite are used, it is possible to manufacture a lithium-ion secondary battery in which the irreversible capacity per unit area of the positive electrode is greater than the irreversible capacity per unit area of the negative electrode, unlike conventional lithium-ion secondary batteries. In this way, when the irreversible capacity per unit area of the positive electrode is greater than the irreversible capacity per unit area of the negative electrode, the driving voltage range is limited to a range other than the irreversible capacity of the positive electrode. As a result, capacity loss of the positive electrode does not occur, and the use of the low-potential region of the negative electrode where rapid volume expansion of the Si-based negative electrode active material occurs is eliminated, thereby effectively preventing a reduction in lifespan due to volume expansion of the negative electrode.
[0047] The components of the lithium secondary battery according to the present invention will be described in more detail below.
[0048] positive electrode The positive electrode according to the present invention is D 50 The positive electrode comprises a single-particle type positive electrode active material having a particle size of 5.5 μm to 8 μm, and may further include a positive electrode conductive material and a positive electrode binder as needed. Specifically, the positive electrode is a positive electrode current collector. and , a positive electrode composite layer formed on at least one surface of the positive electrode current collector and The positive electrode composite layer includes D 50 Single-particle positive electrode active material and positive electrode conductive material with particle size of 5.5 μm to 8 μm. 、 and includes a positive electrode binder.
[0049] The single-particle type positive electrode active material may contain 30 or fewer nodules, preferably 1 to 25, and more preferably 1 to 15. Because the single-particle type positive electrode active material has a small number of nodules constituting the particle, and therefore fewer interfaces within the particle, the contact area with the electrolyte is small. from Compared to commonly used cathode active materials in the form of secondary particles, which consist of aggregated primary particles ranging from 40 to several hundred, single-particle cathode active materials exhibit fewer side reactions with the electrolyte, resulting in significantly less gas generation. Therefore, when single-particle cathode active materials are applied, excellent lifetime characteristics can be obtained. Furthermore, because single-particle cathode active materials have high resistance due to reduced lithium ion mobility within the particles, their application reduces the efficiency of the cathode, and consequently, the irreversible capacity of the cathode can be made greater than that of the anode.
[0050] On the other hand, in the present invention, as the single-particle type positive electrode active material, D 50 A positive electrode active material is used in which the particle size is 5.5 μm to 8 μm, preferably 5.5 μm to 7.5 μm, and more preferably 6 μm to 7 μm. D of the single-particle positive electrode active material 50 If the above range is satisfied, the resistance of the positive electrode increases further, and the irreversible capacitance of the positive electrode can be made greater than the irreversible capacitance of the negative electrode.
[0051] On the other hand, in the single-particle type positive electrode active material according to the present invention, the nodule of Average particle size teeth, The nodule particle size may be 0.8 μm to 4.0 μm, preferably 0.8 μm to 3 μm, and more preferably 1.0 μm to 3.0 μm. When the average particle size of the nodules satisfies the above range, particle cracking can be minimized during electrode manufacturing, and the increase in resistance can be more effectively suppressed. Here, the average particle size of the nodules refers to the value obtained by measuring the particle size of each nodule observed from the SEM image obtained by analyzing the positive electrode active material powder with a scanning electron microscope, and then calculating the arithmetic mean of the measured values.
[0052] On the other hand, the single-particle positive electrode active material may contain a lithium nickel-based oxide containing 88 mol% or more, preferably 90 mol% or more, of Ni.
[0053] The lithium nickel oxide may be represented, for example, by the following [Chemical Formula 1].
[0054] [Chemical formula 1] Li 1+x [Ni a Co b M 1 c M 2 d ]O2
[0055] In the above [Chemical Formula 1], M 1 This is one or more selected from Mn and Al, and preferably, from the viewpoint of durability, it may be Mn or a combination of Mn and Al.
[0056] Said M 2 are Zr, Y, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P 、 It may include one or more selected from the group consisting of and S.
[0057] The above 1+x represents the atomic fraction of lithium in the lithium nickel oxide, where -0.2≦x≦0.2 and -0.1≦x≦0.1 、Alternatively, 0 ≤ x ≤ 0.1 may also be acceptable.
[0058] The above a is the atomic fraction of nickel among the metal elements other than lithium in the lithium nickel oxide. of The values may also be 0.88 ≤ a < 1, 0.9 ≤ a < 1, or 0.9 ≤ a ≤ 0.97. When the atomic fraction of nickel satisfies the above range, a high energy density can be achieved.
[0059] The above b represents the atomic fraction of cobalt among the metal elements other than lithium in the lithium nickel oxide, and 0 <b<0.12、0.01≦b<0.12 、 Alternatively, 0.01 ≤ b ≤ 0.10 may also apply.
[0060] The aforementioned c is M, which is a metallic element other than lithium in lithium nickel oxides. 1 The atomic fraction of an element is shown, and 0 <c<0.12、0.01≦c<0.12 、 Alternatively, 0.01 ≤ c ≤ 0.10 may also apply.
[0061] The above d is M, which is a metallic element other than lithium in lithium nickel oxide. 2 The atomic fraction of an element is shown, and may be in the form of 0≦d≦0.05, 0≦d≦0.03, or 0≦d≦0.02.
[0062] More preferably, the lithium nickel oxide may be represented, for example, by the following [Chemical Formula 1-1].
[0063] [Chemical formula 1-1] Li 1+x [Ni a Co b Mn c1 Al c2 M 2 d ]O2
[0064] In the above [Chemical Formula 1-1], M 1 M 2x, a, b, and d are defined as in [Chemical Formula 1], and 0 <c1≦0.115、0.01≦c1≦c1≦0.10 、 Or, if 0.01 ≤ c1 ≤ 0.10, then 0 <c2≦0.05、0.005≦c1<0.03 、 Alternatively, 0.01 ≤ c1 ≤ 0.03 may also apply.
[0065] As shown in [Chemical Formula 1-1] above, when the lithium nickel oxide contains both Mn and Al, the particle structure stability of the positive electrode active material can be further improved. However, if the Al content is too high, the capacity characteristics may deteriorate, so it is preferable that the Mn and Al content meet the above range.
[0066] The lithium nickel oxide may be represented, for example, by the following [Chemical Formula 1-2].
[0067] [Chemical formula 1-2] Li 1+x [Ni a Co b Mn c1 Al c2 ]O2
[0068] In the above chemical formula 1-2, 0≦x≦0.1, 0.9≦a≦0.97, 0.01≦b≦0.10, 0.01≦c1≦0.10, and 0.01≦c1≦0.10.
[0069] On the other hand, the positive electrode active material according to the present invention may further include a coating layer on the surface of the lithium nickel oxide. The coating layer may be made of Co, Al, W, Ti, Mg, Zr, Y, Ba, Ca, Sr, Ta, Nb, p, B 、 The coating layer may contain one or more coating elements selected from the group consisting of and Mo. Preferably, the coating layer may contain Co, and more preferably, Co and Al.
[0070] On the other hand, the positive electrode active material is the total weight of the positive electrode composite layer, i.e., positive electrode active material, positive electrode conductive material 、The positive electrode active material can be included in an amount of 93% to 99% by weight, preferably 95% to 98% by weight, and more preferably 95% to 97% by weight, relative to the total amount of the positive electrode binder. When the content of the positive electrode active material satisfies the above range, a high energy density can be achieved.
[0071] On the other hand, the positive electrode conductive material is used to impart conductivity to the electrode and can be used without particular limitations as long as it does not cause chemical changes and has electronic conductivity in the battery it is configured in. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more can be used. The positive electrode conductive material is used in an amount equal to 0.1% of the total weight of the positive electrode composite layer. weight% ~15% by weight in It can be included.
[0072] The positive electrode binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which the hydrogen atoms of these are substituted with Li, Na, or Ca, or various copolymers thereof. One of these alone or a mixture of two or more can be used. The binder is 0.1% of the total weight of the positive electrode composite layer. weight% ~15% by weight in It can be included.
[0073] The positive electrode is manufactured by a conventional method for manufacturing positive electrodes. do Specifically, the positive electrode according to the present invention prepares a positive electrode active material and, if necessary, selectively dissolves or disperses a positive electrode binder, a positive electrode conductive material, and a dispersant in a solvent to produce a positive electrode slurry composition. death, The positive electrode slurry is applied to the positive electrode current collector, then dried and rolled, or the positive electrode slurry composition is cast onto another support, peeled off this support, and the resulting film is laminated onto the positive electrode current collector. do It is possible.
[0074] In other respects, the positive electrode may be manufactured by a solvent-free method, such as the dry method.
[0075] Here, the positive electrode current collector is not particularly limited as long as it can contain a highly conductive metal, the positive electrode composite layer adheres easily, and it is unreactive within the battery voltage range. The positive electrode current collector can be made of, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. Also, the positive electrode current collector is usually 3 μm It can have a thickness of approximately 500 μm, and by forming fine irregularities on the surface of the current collector, it is possible to enhance the adhesion of the positive electrode active material. For example, it can be used in various forms such as films, sheets, foils, meshes, porous materials, foams, and nonwoven fabrics.
[0076] The solvent for the positive electrode slurry may be a common solvent used in the manufacture of positive electrode slurries in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water. 、 Alternatively, mixtures thereof may be used. The amount of solvent used will be determined considering the coating thickness of the slurry and the production yield, in order to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant. What happened after that? Therefore, when coating for the manufacture of the positive electrode, it has a viscosity that can exhibit excellent thickness uniformity. Na That level is sufficient.
[0077] On the other hand, the positive electrode according to the present invention may have a porosity of 16% to 24%, preferably 16% to 23%, and more preferably 16% to 22%. When the porosity of the positive electrode satisfies the above range, excellent energy density can be achieved. If the porosity of the positive electrode is too large, the energy density decreases, and if the porosity of the positive electrode is too small, the electrolyte impregnation decreases, and lithium ion mobility may decrease.
[0078] Furthermore, the total thickness of the positive electrode may be 90 μm to 120 μm, preferably 90 μm to 110 μm, and more preferably 95 μm to 105 μm. When the positive electrode thickness satisfies the above range, the capacity characteristics per unit volume are excellent.
[0079] Furthermore, the positive electrode may have an efficiency of less than 90%, preferably 87% or more and less than 90%, and more preferably 87% to 89%. If the efficiency of the positive electrode is 90% or more, the irreversible capacitance of the positive electrode becomes smaller than the irreversible capacitance of the negative electrode, causing capacitance loss of the positive electrode in the drive voltage range, and making it difficult to obtain the effect of improving lifespan by eliminating the use of the low potential region of the negative electrode.
[0080] On the other hand, the positive electrode according to the present invention may have a discharge capacity of 200 mAh / g to 400 mAh / g, preferably 200 mAh / g to 300 mAh / g, and more preferably 210 mAh / g to 300 mAh / g. Here, the capacity is the discharge capacity measured by charging and discharging a coin-half cell manufactured using the positive electrode according to the present invention and a lithium metal electrode as the counter electrode at 0.1C in a voltage range of 3V to 4.4V. When the capacity of the positive electrode satisfies the above range, structural collapse of the positive electrode can be minimized and durability can be ensured.
[0081] negative electrode The negative electrode according to the present invention comprises a first negative electrode active material containing a Si-C composite, and may further include a negative electrode conductive material and a negative electrode binder as needed. Specifically, the negative electrode is a negative electrode current collector and , a negative electrode composite layer formed on at least one surface of the negative electrode current collector and The negative electrode composite layer includes a first negative electrode active material containing a Si-C composite.
[0082] Si-C composites are materials having a composite structure in which silicon particles are distributed within a carbon matrix, conventionally from Compared to SiOx, which was mainly used as a Si-based negative electrode active material, it has less irreversible capacity and superior conductivity during charging and discharging. body The change in product is small. Therefore, when using Si-C composite... 、The irreversible capacity of the negative electrode is reduced, making it possible to manufacture a negative electrode with a lower irreversible capacity than the positive electrode, thereby improving capacity characteristics and lifespan characteristics.
[0083] Preferably, the Si-C composite is gray stomach The grain size may be 20 nm or less, preferably 1 nm to 20 nm, more preferably 1 nm to 18 nm. stomach When the size meets the aforementioned range, it exhibits excellent improvements in cell resistance characteristics and lifespan characteristics.
[0084] Furthermore, the Si-C composite is D 50 The particle size may be 1 μm to 15 μm, preferably 2 μm to 10 μm, and more preferably 3 μm to 10 μm. Furthermore, the Si-C composite is D 10 D 90 The particle size may be 6 μm to 20 μm, preferably 6 μm to 15 μm. When the particle size distribution of the Si-C composite satisfies the above range, the electrode density of the negative electrode increases, and a high energy density can be achieved.
[0085] On the other hand, the negative electrode may further include a graphite-based negative electrode active material as a second negative electrode active material. The graphite-based negative electrode active material may be, for example, artificial graphite or natural graphite. 、 Alternatively, a combination of these may be used, preferably a mixture of artificial graphite and natural graphite.
[0086] When the second negative electrode active material is a mixture of artificial graphite and natural graphite, the weight ratio of artificial graphite to natural graphite may be 99:1 to 60:40, preferably 90:10 to 60:40, and more preferably 90:10 to 70:30. When the mixing ratio of artificial graphite to natural graphite satisfies the above range, both the lifespan characteristics and rapid charging performance are excellent.
[0087] On the other hand, the weight ratio of the first negative electrode active material to the second negative electrode active material teeth, 2:98~20:80, 2:98~15:85, 5:95~15:85 、Alternatively, the ratio may be 5:95 to 10:90. When the weight ratio of the first negative electrode active material to the second negative electrode active material satisfies the above range, both capacity characteristics and life characteristics are excellent.
[0088] The aforementioned negative electrode active material is 80% of the total weight of the negative electrode composite layer. weight% ~99% by weight, preferably 85% weight% ~99% by weight, comfortable 90 weight% ~99% by weight in It can be included.
[0089] On the other hand, the negative electrode conductive material is used to impart conductivity to the negative electrode and can be used without particular limitations as long as it is used as a conductive material for lithium secondary batteries. Specific examples of the negative electrode conductive material include carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these alone or a mixture of two or more can be used. Preferably, the negative electrode conductive material is carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, or carbon nanotubes. 、 Alternatively, combinations of these materials can be used, and it is more preferable to use both a point-type conductive material and a linear conductive material in terms of improving conductivity. Here, the point-type conductive material is a material having a particle shape and contacting the negative electrode active material in the form of points, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, etc., and the linear conductive material is a material that contacts the negative electrode active material in the form of lines, such as carbon fibers, carbon nanotubes, etc.
[0090] The aforementioned negative electrode conductive material is typically 1 in proportion to the total weight of the negative electrode composite layer. weight% ~20% by weight, preferably 0.1 weight% ~10% by weight, comfort 0.1 weight% ~1% by weight in It can be included.
[0091] Next, the negative electrode binder plays a role in improving adhesion between negative electrode active material particles and adhesion between the negative electrode active material and the negative electrode current collector, and any material used as a negative electrode binder in lithium secondary batteries can be used without particular limitations. Specific examples of negative electrode binders include polyvinylidene fluoride (PVDF), Poly Examples include vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, of which one or more can be used.
[0092] The negative electrode binder is 1 in proportion to the total weight of the negative electrode composite layer. weight% ~20% by weight, preferably 1 weight% ~10% by weight, comfort level 1 weight% ~3% by weight in It can be included.
[0093] The negative electrode is manufactured according to a conventional method for manufacturing negative electrodes. do Specifically, the anode according to the present invention prepares a negative electrode active material and, if necessary, selectively dissolves or disperses a negative electrode binder, a negative electrode conductive material, and a dispersant in a solvent to produce a negative electrode slurry composition. death,The negative electrode slurry is applied to the negative electrode current collector, then dried and rolled, or the negative electrode slurry composition is cast onto another support, peeled off this support, and the resulting film is laminated onto the negative electrode current collector. do It is possible.
[0094] In other respects, the negative electrode may be manufactured by a solvent-free method, such as the dry method.
[0095] Here, the negative electrode current collector can be a negative electrode current collector commonly used in the art, such as copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy. The negative electrode current collector can usually have a thickness of 3 μm to 500 μm, and, similar to the positive electrode current collector, fine irregularities can be formed on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it can be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0096] The solvent for the negative electrode slurry may be a common solvent used in the manufacture of negative electrode slurries in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water. 、 Alternatively, mixtures thereof may be used. The amount of solvent used will be determined considering the coating thickness of the slurry and the production yield, in order to dissolve or disperse the negative electrode active material, conductive material, binder, and dispersant. What happened after that? To have a viscosity that allows for excellent thickness uniformity when applied during the manufacturing of the negative electrode. Na That level is sufficient.
[0097] On the other hand, the negative electrode according to the present invention may have a porosity of 20% to 30%, preferably 22% to 29%, and more preferably 23% to 28%. When the porosity of the negative electrode satisfies the above range, the density of the negative electrode increases, and even if the thickness of the negative electrode is formed thinner than conventionally, the desired capacity characteristics can be achieved.
[0098] The negative electrode may have a total thickness of 80 μm to 130 μm, preferably 90 μm to 120 μm, and more preferably 95 μm to 120 μm. When the thickness of the negative electrode meets the above range, the reaction uniformity of the Si-C composite is improved, and the rapid charging performance is enhanced. of It can be improved.
[0099] On the other hand, the negative electrode may have an efficiency of 90% or more, preferably 90% to 94%, and more preferably 90% to 93%. When the efficiency of the negative electrode satisfies the above range, the irreversible capacitance of the negative electrode becomes smaller than the irreversible capacitance of the positive electrode. This reduces the use of the low-potential region of the negative electrode where rapid expansion of the negative electrode occurs within the driving voltage range, thereby improving the lifespan characteristics.
[0100] The discharge capacity of the negative electrode is 400mAh / g to 600mAh / g, 400mAh / g to 550mAh / g, 400mAh / g to 500mAh / g, and 450mAh / g to 550mAh / g. 、 Alternatively, it may be 450mAh / g to 500mAh / g. Here, the discharge capacity is the discharge capacity measured by charging and discharging a coin-half cell manufactured using the negative electrode and lithium metal electrode according to the present invention as counter electrodes at 0.1C in a voltage range of 0.005V to 1V. When the discharge capacity of the negative electrode satisfies the above range, the capacity per unit volume of the unit cell is 270mAh / cm³. 3 More than 280mAh / cm 3 That's all. 、 Or 290mAh / cm² 3 This can be achieved to the above extent.
[0101] electrolyte The electrolyte used in this invention can be a variety of electrolytes that can be used in lithium secondary batteries, such as organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc., and the types teeth It is not particularly limited.
[0102] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0103] The organic solvent can be used without particular limitations, as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvents include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; and dibutyl ether. Ether-based solvents such as ether or tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethanol and isopropyl alcohol; R-CN (where R is a linear or branched chain of C2-C20 atoms) 、Nitriles such as nitriles (which are hydrocarbon groups with a cyclic structure and may include double-bonded aromatic rings or ether bonds); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes are used. obtain. Among these, carbonate-based solvents are preferred, and cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery, and low viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate) are preferred. 、 A mixture of (or diethyl carbonate, etc.) is more preferable.
[0104] A gas-free organic solvent is preferred as the aforementioned organic solvent. Those skilled in the art will understand that a gas-free solvent means a solvent designed to remove gas-generating sites in its structure. For example, to form a gas-free solvent, dissolved gases can be removed by heating the solvent under pressure for a long period of time.
[0105] The lithium salt can be used without particular limitations as long as it is a compound capable of providing lithium ions for use in lithium secondary batteries. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl O 4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2 、 Alternatively, combinations of these can be used. The concentration of the lithium salt is 0.1 M ~5.0M, 0.1 M ~4.0M, 0.1 M ~3.0M, 0.1 M ~2.0M or 0.1 MIt is preferable to use it within the range of ~1.0M. When the lithium salt concentration falls within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions teeth It allows for effective movement.
[0106] On the other hand, the electrolyte may further contain additives in addition to the above components for purposes such as improving the battery's lifespan, suppressing the decrease in battery capacity, and improving the battery's discharge capacity. For example, the electrolyte may contain cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, phosphate compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, and silane compounds. 、 The additive may include at least one selected from the group consisting of lithium salt compounds.
[0107] Examples of the aforementioned cyclic carbonate compounds include vinylene carbonate (VC) or vinylethylene carbonate.
[0108] An example of the halogen-substituted carbonate compound is fluoroethylene carbonate (FEC).
[0109] Examples of the aforementioned sultone compounds include 、 1,3-Propanesultone (PS), 1,4-Butanesultone, Ethensultone, 1,3-Propensultone (PRS), 1,4-Butensultone 、 Examples include at least one compound selected from the group consisting of and 1-methyl-1,3-propensultone.
[0110] Examples of the sulfate compounds mentioned above include ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS).
[0111] Examples of the aforementioned phosphate compounds include lithium difluoro(bisoxalate) phosphate, lithium difluorophosphate, tetramethyltrimethylsilyl phosphate, trimethylsilyl phosphate, and tris(2,2,2-trifluoroethyl) phosphate. 、 Examples include one or more compounds selected from the group consisting of tris(trifluoroethyl)phosphite.
[0112] Examples of the borate compounds mentioned above include tetraphenyl borate, lithium oxalyl difluoroborate (LiODFB), and lithium bisoxalate borate (LiB(C2O4)2, LiBOB).
[0113] Examples of the aforementioned nitrile compounds include at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonile, cyclohexanecarbonile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.
[0114] Examples of the benzene-based compounds include fluorobenzene, examples of the amine-based compounds include triethanolamine or ethylenediamine, and examples of the silane-based compounds include tetravinylsilane.
[0115] The lithium salt compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, and is lithium difluorophosphate (LiDFP), LiPO2F2 、 Other examples include LiBF4.
[0116] The additive is present in an amount of 0.1% relative to the total weight of the electrolyte. weight%~10wt%, 0.1 weight% ~9wt%, 0.1 weight% ~8wt%, 0.1 weight% ~7% by weight, 0.1 weight% ~6wt%, 0.1 weight% ~5wt%, 0.1 weight% ~4% by weight, or 0.1 weight% ~3% by weight in It can be included.
[0117] Separator The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Regular Any material used as a separator in a lithium secondary battery can be used without particular restrictions. Specifically, the separator can be a porous polymer film, such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, or an ethylene / hexene copolymer. 、 Porous polymer films made from polyolefin polymers such as ethylene / methacrylate copolymers, or laminated structures of two or more layers thereof, can be used. Alternatively, ordinary porous nonwoven fabrics, such as those made from high-melting-point glass fibers or polyethylene terephthalate fibers, can be used. Furthermore, coated separators containing ceramic components or polymeric substances may be used to ensure heat resistance or mechanical strength.
[0118] On one side, the separator has a thickness of 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, and 6 μm or less. 、 Alternatively, the particle size may be 5 μm or less.
[0119] In one aspect, the separator is improved So To provide safety, one or both sides of the surface may be coated with ceramic.
[0120] On one side, in place of or with the separator 、A solid electrolyte layer can be used. The solid electrolyte may contain a solid electrolyte, consist of a solid electrolyte, or have a solid electrolyte or a combination of a solid electrolyte and a liquid electrolyte as its main component. Composition It is possible.
[0121] On the other hand, the lithium secondary battery has one negative electrode and one positive electrode. 、 The lithium secondary battery according to the present invention may contain one unit cell, or two or more unit cells. When multiple unit cells are included, a high energy density can be achieved.
[0122] On the other hand, the total thickness of the unit cell may be 220 μm to 240 μm, preferably 225 μm to 240 μm, more preferably 230 μm to 240 μm, or 235 μm to 240 μm. When the thickness of the unit cell satisfies the above range, the capacity per unit volume of the unit cell is 270 mAh / cm³. 3 More than 280mAh / cm 3 Above, or 290mAh / cm² 3 This can be achieved at an even higher level, enabling the manufacture of batteries with high energy density.
[0123] The lithium secondary battery according to the present invention, configured as described above, has capacity characteristics and life characteristics. 、 It also boasts excellent fast charging performance.
[0124] Specifically, the lithium secondary battery according to the present invention has a capacity of 270 mAh / cm³ per unit cell per unit volume. 3 More than 280mAh / cm 3 Above, or 290mAh / cm² 3 It may be greater than or equal to 270 mAh / cm², preferably 270 mAh / cm². 3 ~350mAh / cm 3 , 280mAh / cm² 3 ~330mAh / cm 3 , or 290mAh / cm² 3 ~320mAh / cm 3 It has high capacitance characteristics.
[0125] Furthermore, the lithium secondary battery according to the present invention has a capacity retention rate of 85% or more after 500 charge-discharge cycles at room temperature, and exhibits excellent lifespan characteristics.
[0126] Furthermore, the lithium secondary battery according to the present invention has a state of charge (SOC) of 45% or higher at the time of lithium deposition during 3C charging, and exhibits excellent rapid charging performance.
[0127] The lithium secondary battery according to the present invention as described above can be used to manufacture a battery pack. The battery pack includes an assembly of electrically connected lithium secondary batteries according to the present invention and a pack housing that houses them, wherein the pack housing is a lithium secondary battery of The battery pack may include busbars for electrical connection, a cooling unit, external terminals, etc. The battery pack can be mounted in an automobile, such as an electric vehicle or a hybrid vehicle. 、 Alternatively, it may be a plug-in hybrid vehicle. The vehicle includes four-wheeled vehicles and two-wheeled vehicles. In particular, the lithium secondary battery according to the present invention has a high energy density, excellent rapid charging performance, and can be usefully used as a battery for electric vehicles.
[0128] The present invention will be described in more detail below with reference to specific examples. However, the following examples are provided to facilitate understanding of the present invention and do not extend to the scope of the invention. teeth These embodiments are not the only ones.
[0129] Example 1 <Manufacturing of positive electrodes> A positive electrode slurry was prepared by mixing positive electrode active material, positive electrode conductive material, and PVDF binder in N-methylpyrrolidone in a weight ratio of 97:1.2:1.4. Here, D was used as the positive electrode active material. 50 =6μm single-particle Li[Ni 0.93 Co 0.05 Mn 0.01 Al 0.01 O2 was used, and carbon nanotubes were used as the positive electrode conductive material.
[0130] The positive electrode slurry was applied to both sides of a 12 μm thick aluminum current collector sheet, dried, and then rolled to obtain a positive electrode with a total thickness of 102.0 μm, a positive electrode porosity of 18%, and a positive electrode loading capacity of 3.5 mAh / cm². 2 We manufactured the positive electrode.
[0131] <Manufacturing of negative electrodes> A negative electrode slurry was prepared by mixing negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) in water in a weight ratio of 96.6:0.5:1.8:1.1. Here, the negative electrode active material used was a mixture of Si-C composite (capacity 1800 mAh / g, efficiency 85%), artificial graphite, and natural graphite in a weight ratio of 7:74.4:18.6, and the negative electrode conductive material used was a mixture of Super C and single-wall carbon nanotubes.
[0132] The negative electrode slurry was applied to both sides of a 6 μm thick copper current collector sheet, dried, and then rolled, resulting in a negative electrode with a total thickness of 110.5 μm, a negative electrode porosity of 25%, and a negative electrode loading capacity of 3.731 mAh / cm². 2 We manufactured the negative electrode.
[0133] <Manufacturing of lithium-ion secondary batteries> As described above, the positive electrode and negative electrode, along with two separators, were stacked in the order of positive electrode / separator / negative electrode / separator to produce a unit cell. Twenty-nine of these unit cells were then stacked to produce an electrode assembly. After that, the electrode assembly was inserted into a battery case, and then an electrolyte was injected to produce a lithium secondary battery.
[0134] Example 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that a mixture of Si-C composite, artificial graphite, and natural graphite in a weight ratio of 10:72:18 was used as the negative electrode active material, and the negative electrode was manufactured so that the total thickness of the negative electrode was 101.8 μm.
[0135] Example 3 A lithium secondary battery was manufactured using the same method as in Example 1, except that a Si-C composite with a capacity of 1800 mAh / g and an efficiency of 82.4% was used.
[0136] Example 4 A lithium secondary battery was manufactured using the same method as in Example 1, except that the positive electrode was manufactured so that its total thickness was 105.4 μm and its porosity was 21%.
[0137] Example 5 A lithium secondary battery was manufactured using the same method as in Example 1, except that the positive electrode was manufactured so that its total thickness was 107.8 μm and its porosity was 23%.
[0138] Comparative Example 1 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the negative electrode was manufactured using a mixture of SiO (capacity 1295 mAh / g, efficiency: 78.7%), artificial graphite, and natural graphite in a weight ratio of 7:74.4:18.6 as the negative electrode active material, and the negative electrode was manufactured so that the total thickness of the negative electrode was 118.6 μm.
[0139] Comparative Example 2 As the positive electrode active material, D 50 Single-particle Li[Ni = 4μm 0.86 Co 0.08 Mn 0.06 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode was manufactured using 2O2, with a total thickness of 109.0 μm and a porosity of 23%, and the negative electrode was manufactured using a mixture of SiO2 (capacity 1295 mAh / g, efficiency: 78.7%), artificial graphite, and natural graphite in a weight ratio of 11:71.2:17.8 as the negative electrode active material, with a total thickness of 109.4 μm.
[0140] Comparative Example 3 As the positive electrode active material, D 50 Single-particle Li[Ni = 4μm 0.86 Co 0.08 Mn 0.06Using O2, the positive electrode was manufactured such that the total thickness of the positive electrode was 109.0 μm and the porosity of the positive electrode was 23%, and SiO (capacity 1295 mAh / g, efficiency: 78.7%) as a negative electrode active material: artificial graphite: natural graphite was mixed at a weight ratio of 4:76.8:19.2 and used, and a lithium secondary battery was manufactured in the same manner as in Example 1, except that the negative electrode was manufactured such that the total thickness of the negative electrode was 126.7 μm.
[0141] Comparative Example 4 At the time of manufacturing the negative electrode, as a negative electrode active material, a Si-C composite: artificial graphite: natural graphite was mixed and used at a weight ratio of 10:72:18, and the total thickness of the negative electrode was 103.7 μm, the porosity of the negative electrode was 25%, and the negative electrode discharge loading amount was 3.801 mAh / cm 2 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the negative electrode was manufactured to be
[0142] Comparative Example 5 As a positive electrode active material, D 50 = 4 μm single-particle type Li[Ni 0.93 Co 0.05 Mn 0.01 Al 0.01 O2 was used, and the positive electrode was manufactured so that the total thickness of the positive electrode was 100.7 μm and the porosity of the positive electrode was 18%, and the negative electrode was manufactured so that the total thickness of the negative electrode was 110.2 μm. A lithium secondary battery was manufactured in the same manner as in Example 1, except that
[0143] The configurations and N / P ratios of the lithium secondary batteries of Examples and Comparative Examples are shown in Table 1 below. Here, the N / P ratio indicates the discharge capacity of the negative electrode per unit area / the discharge capacity of the positive electrode per unit area.
[0144]
Table 1
[0145] Experimental Example 1 The capacities and efficiencies of the positive and negative electrodes manufactured according to Examples and Comparative Examples were measured as follows.
[0146] <Method for measuring positive electrode properties> A positive electrode composite layer formed on one side of the positive electrode current collector in each of the positive electrodes manufactured according to the above examples and comparative examples is cleaned and removed to manufacture a single-sided positive electrode. A separator is interposed between the single-sided positive electrode and the lithium counter electrode. Let A positive electrode coin half-cell was manufactured by injecting an electrolyte. The positive electrode coin half-cell was charged to 4.30V in 0.1C, CC-CV mode (0.05C cut-off), and then discharged to 3V in 0.1C, CC mode to measure the charge capacity and discharge capacity. From the measured charge capacity and discharge capacity, the efficiency of the positive electrode (discharge capacity of the positive electrode / charge capacity of the positive electrode × 100) and the irreversible capacity per unit area of the positive electrode ((charge capacity of the positive electrode - discharge capacity of the positive electrode) / area of the positive electrode) were calculated. Here, the area of the positive electrode is the width of the positive electrode composite layer. of long difference (Units: cm) and height of long difference This value is calculated as a product of units (in cm).
[0147] <Method for measuring the physical properties of the negative electrode> The negative electrode composite layer formed on one side of the negative electrode current collector in each of the negative electrodes manufactured according to the above examples and comparative examples is cleaned and removed to manufacture a single-sided negative electrode. A separator is interposed between the single-sided negative electrode and the lithium counter electrode. Let The negative electrode coin half-cell was manufactured by injecting an electrolyte. coin A half-cell was charged to 5mV at 0.1C, CC-CV mode (0.005C cut-off), then discharged to 1V at 0.1C, CC mode, and the charge and discharge capacities were measured. From the measured charge and discharge capacities, the efficiency of the negative electrode (discharge capacity of the negative electrode / charge capacity of the negative electrode × 100) and the irreversible capacity per unit area of the negative electrode ((charge capacity of the negative electrode - discharge capacity of the negative electrode) / area of the negative electrode) were calculated. Here, the area of the negative electrode is the width of the negative electrode composite layer. of long difference (Units: cm) and height of long difference It can be calculated by the product of (unit: cm)
[0148] Also ,negativeThe ratio of the irreversible capacity per unit area of the positive electrode to the irreversible capacity per unit area of the electrode (RIC) was calculated.
[0149] Measurement results of This is shown in Table 2 below.
[0150] [Table 2]
[0151] Experimental Example 2 The composite material layer formed on one side of the current collector in the positive and negative electrodes manufactured according to the above examples and comparative examples was cleaned and removed to produce a single-sided positive electrode and a single-sided negative electrode.
[0152] Subsequently, the aforementioned one-sided positive electrode and one-sided negative electrode 、 An electrode assembly was manufactured by stacking the separators in the order of one-sided positive electrode / separator / one-sided negative electrode / separator, and the electrode assembly was inserted into a battery case and an electrolyte was injected to manufacture a monocell.
[0153] Each of the monocells manufactured as described above was charged and discharged at 0.1C within a voltage range of 2.5V to 4.25V to measure its cell capacity, and the unit cell capacity per unit volume was measured by substituting these values into the following formula.
[0154] Cell capacity per unit volume (mAh / cm³) 3 ) = (Measured monocell capacity × 2) / ({Positive electrode area × (2 × Thickness of the positive electrode composite layer of the single-sided positive electrode + Thickness of the positive electrode current collector) + (2 × thickness of the negative electrode composite layer of the single-sided negative electrode + thickness of the negative electrode current collector + 2 × thickness of the separator)
[0155] Measurement results of This is shown in Table 3 below.
[0156] Experimental Example 3 The monocell manufactured in Experimental Example 2 was charged and discharged at 3C within a voltage range of 2.5V to 4.25V, and the State of Charge (SOC) at the time of lithium deposition was measured. Measurement results of This is shown in Table 3 below.
[0157] Experimental Example 4 Each lithium secondary battery manufactured according to the examples and comparative examples was charged and discharged at room temperature (0.33C) within a voltage range of 2.5V to 4.25V for 500 cycles, and the capacity retention rate was measured afterward. Measurement results of This is shown in [Table 3] below.
[0158] [Table 3]
[0159] As described in Table 3 above, D 50 Lithium secondary batteries of Examples 1 to 5, which include a single-particle positive electrode active material with a particle size of 5.5 μm to 8 μm and a first negative electrode active material containing a Si-C composite, and in which the irreversible capacity per unit area of the positive electrode is greater than the irreversible capacity per unit area of the negative electrode, have a unit cell capacity of 260 mAhg / cm³ per unit volume. 3 In summary, it boasts excellent capacity characteristics, with a capacity retention rate of over 85% after 500 cycles, demonstrating superior lifespan. Furthermore, lithium deposition occurs after a state of charge (SOC) of 45% during high-rate (3C) charge / discharge, indicating excellent rapid charging performance.
[0160] In contrast, in the case of the lithium secondary battery of Comparative Example 1, in which silicon oxide was used instead of the Si-C composite as the negative electrode active material, the irreversible capacity per unit area of the negative electrode was greater than the irreversible capacity per unit area of the positive electrode, and compared to Examples 1 to 5, the capacity characteristics and life characteristics were different. 、 Furthermore, it had poor fast-charging performance, and lithium deposition occurred when the SOC was below 45%.
[0161] Meanwhile, D 50In the lithium secondary batteries of Comparative Examples 2 and 3, which include a small-particle single-particle positive electrode active material with a D of 5 μm or less and a silicon oxide negative electrode active material, the capacity characteristics and life characteristics were 、 inferior to those of Examples 1 to 5, as well as the rapid charging performance. In particular, in the case of Comparative Example 3, lithium precipitation occurred at a significantly lower SOC compared to Examples 1 to 5. In addition, even if the lithium secondary battery of Comparative Example 4 includes a single-particle positive electrode active material with a D 50 of 5.5 μm to 8 μm and a first negative electrode active material containing a Si-C composite, and the irreversible capacity of the negative electrode is greater than the irreversible capacity of the positive electrode, it can be confirmed that the life characteristics are reduced compared to Examples 1 to 5.
[0162] This indicates that each of the following configurations (1) to (3) is important for achieving improved performance.
[0163] (1) A single-particle positive electrode active material with a D 50 of 5.5 μm to 8 μm. (2) A first negative electrode active material containing a Si-C composite. (3) The irreversible capacity of the negative electrode is smaller than the irreversible capacity of the positive electrode.
[0164] In addition, even if a Si-C composite is used as the negative electrode active material, in the case of Comparative Example 5 using a small-particle single-particle positive electrode active material with a D 50 of less than 5.5 μm, compared to Examples 1 to 5 using a single-particle positive electrode active material with a D 50 of 5.5 μm to 8 μm, it can be confirmed that the life characteristics are significantly reduced.
Claims
1. D 50 A positive electrode containing a single-particle type positive electrode active material having a particle size of 5.5 μm to 8 μm, A negative electrode containing a first negative electrode active material containing a Si-C composite, Contains electrolytes, A lithium secondary battery in which the irreversible capacity per unit area of the negative electrode is smaller than the irreversible capacity per unit area of the positive electrode.
2. The lithium secondary battery according to claim 1, wherein the ratio of the irreversible capacity per unit area of the positive electrode to the irreversible capacity per unit area of the negative electrode is 1.01 or more.
3. The lithium secondary battery according to claim 1, wherein the single-particle positive electrode active material contains a lithium nickel-based oxide in which Ni accounts for 88 mol% or more of the total metals other than lithium.
4. The lithium nickel oxide is represented by the following [Chemical Formula 1], as described in claim 3, for the lithium secondary battery. [Chemical formula 1] Li 1+x [Ni a Co b M 1 c M 2 d ]O 2 In the above [Chemical Formula 1], M 1 is one or more selected from Mn and Al, and M 2 It contains one or more elements selected from the group consisting of Zr, Y, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P, and S, and satisfies -0.2 ≤ x ≤ 0.2, 0.88 ≤ a < 1, 0 < b < 0.12, 0 < c < 0.12, and 0 ≤ d ≤ 0.
05.
5. The lithium secondary battery according to claim 1, wherein the porosity of the positive electrode is 16% to 24%.
6. The lithium secondary battery according to claim 1, wherein the positive electrode has a total thickness of 90 μm to 120 μm.
7. The lithium secondary battery according to claim 1, wherein the positive electrode has an efficiency of less than 90%.
8. The lithium secondary battery according to claim 1, wherein the discharge capacity of the positive electrode is 200 mAh / g to 400 mAh / g.
9. The aforementioned negative electrode further contains a graphite-based negative electrode active material as a second negative electrode active material. The lithium secondary battery according to claim 1, wherein the weight ratio of the first negative electrode active material to the second negative electrode active material is 2:98 to 20:
80.
10. The lithium secondary battery according to claim 1, wherein the negative electrode has a porosity of 20% to 30%.
11. The lithium secondary battery according to claim 1, wherein the negative electrode has a total thickness of 80 μm to 130 μm.
12. The lithium secondary battery according to claim 1, wherein the negative electrode has an efficiency of 90% or more.
13. The lithium secondary battery according to claim 1, wherein the discharge capacity of the negative electrode is 400 mAh / g to 600 mAh / g.
14. The lithium secondary battery includes a unit cell composed of one negative electrode, one positive electrode, and two separators. The lithium secondary battery according to claim 1, wherein the thickness of the unit cell is 220 μm to 240 μm.
15. The capacity per unit volume of the aforementioned unit cell is 270 mAh / cm³. 3 The lithium secondary battery according to claim 14.
16. The lithium secondary battery according to claim 1, wherein the ratio of the irreversible capacity per unit area of the positive electrode to the irreversible capacity per unit area of the negative electrode is 1.01 to 1.
25.
17. The lithium secondary battery according to claim 1, wherein the ratio of the irreversible capacity per unit area of the positive electrode to the irreversible capacity per unit area of the negative electrode is 1.04 to 1.
20.
18. The lithium secondary battery according to claim 9, wherein the weight ratio of the first negative electrode active material to the second negative electrode active material is 5:95 to 15:
85.
19. The lithium secondary battery according to claim 1, wherein the positive electrode has an efficiency of less than 90%, and the negative electrode has an efficiency of 90% or more.