Lithium-ion battery

The lithium secondary battery addresses low-temperature degradation by optimizing the ratio of conductive material, active material particle sizes, and N/P ratio, achieving stable high-voltage operation and high energy density using graphite-based and single-particle lithium nickel oxide components.

JP2026539336APending Publication Date: 2026-11-24LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026526770
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-22
Filing Date
2024-12-13
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Lithium-ion batteries face challenges in achieving high energy density and suppressing cell degradation at low temperatures due to reduced conductive material content, leading to increased internal resistance and lithium plating.

Method used

A lithium secondary battery design that includes specific ratios and relationships between negative electrode conductive material, negative electrode active material particle sizes, and N/P ratio, using graphite-based materials and single-particle lithium nickel oxide with a nickel content of 70 mol% or less, along with optimized electrolyte composition.

Benefits of technology

The design suppresses lithium plating at low temperatures, improving low-temperature life characteristics and enabling stable high-voltage operation with high energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539336000001_ABST
    Figure 2026539336000001_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery having excellent low-temperature life characteristics. The lithium secondary battery of the present invention includes: a negative electrode including a negative electrode mixture layer containing a first negative electrode active material, a second negative electrode active material, a negative electrode conductive material, and a negative electrode binder; a positive electrode including a positive electrode mixture layer containing a positive electrode active material, a positive electrode conductive material, and a positive electrode binder; and an electrolyte, wherein a CFC defined by the following formula (1) is 0.38 to 1.962. Formula (1): CFC=100×W c -{(D 50、a1 ×D 50、a2 ×L×R N / P ×10 10 ) / MW C} In Formula (1), W c is the ratio of the weight of the negative electrode conductive material to the total weight of the negative electrode mixture layer, MW C is the value of the weight of 1 mole of carbon measured in units of g, D 50、a1 is the value of D 50 of the first negative electrode active material measured in units of m, D 50、a2 is the value of D 50 of the second negative electrode active material measured in units of m, L is the value of the weight of the negative electrode active material per unit area of the negative electrode mixture layer disposed in the cross-section of the negative electrode measured in units of g / 25 cm 2 , and R N / P is the ratio of the negative electrode capacity to the positive electrode capacity.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to lithium secondary batteries, and more particularly to high-voltage lithium secondary batteries with excellent low-temperature life characteristics. [Background technology]

[0002] With the advancement of technologies such as electric vehicles, energy storage systems (ESS), and portable electronic devices, the demand for lithium-ion batteries as an energy source is rapidly increasing.

[0003] On the other hand, in the electric vehicle sector, cells with high energy density are required to extend the driving range on a single charge, and therefore, within the electrode composite layer in Research is being conducted to increase the active material content. In order to increase the active material content, it is necessary to reduce the content of other components, namely conductive materials and / or binders. However, when the content of conductive materials is reduced, electrical conductivity decreases, the internal resistance of the cell increases, lithium plating (Li plating) occurs at low temperatures, and the cell's capacity deteriorates rapidly.

[0004] Therefore, there is a need to develop lithium secondary batteries that have high energy density and can suppress cell degradation at low temperatures. [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] The present invention aims to solve the above-mentioned problems and provides a lithium secondary battery that can be driven stably at high voltage, achieve high energy density, and have excellent low-temperature life characteristics. [Means for solving the problem]

[0006] In one aspect, the present invention relates to a negative electrode active material comprising a first negative electrode active material and a second negative electrode active material, and a negative electrode conductive material. 、and a negative electrode including a negative electrode mixture layer containing a negative electrode binder, a positive electrode including a positive electrode mixture layer containing a positive electrode active material, a positive electrode conductive material 、 and a positive electrode binder, and an electrolyte, wherein CFC defined by the following formula (1) is 0.38 to 1.962, preferably 0.39 to 1.962, more preferably 0.40 to 1.962 、 provided is a lithium secondary battery. Formula (1): CFC = 100 × W c - {(D 50、a1 × D 50、a2 × L × R N / P × 10 10 ) / MW C} In the formula (1), W c is the ratio of the weight of the negative electrode conductive material to the total weight of the negative electrode mixture layer, MW C is the value of the weight of 1 mole of carbon measured in units of g, D 50、a1 is the value of D 50 of the first negative electrode active material measured in units of m, D 50、a2 is the value of D 50 of the second negative electrode active material measured in units of m, L is the value of the weight of the negative electrode active material per unit area of the negative electrode mixture layer disposed on the cross-section of the negative electrode measured in units of g / 25 cm 2 , R N / P is the ratio of the negative electrode capacity to the positive electrode capacity.

[0007] In the formula (1), the W c may be 0.001 to 0.05, preferably 0.002 to 0.03, and more preferably 0.003 to 0.03.

[0008] In the formula (1), the L may be 0.2 to 0.5, preferably 0.3 to 0.4, and more preferably 0.3 to 0.35.

[0009] In the formula (1), the R N / P may be 1.05 to 1.10, preferably 1.06 to 1.09, and more preferably 1.07 to 1.08.

[0010] The first negative electrode active material and the second negative electrode active material may each be independently graphite-based materials, preferably the first negative electrode active material is artificial graphite and the second negative electrode active material is natural graphite.

[0011] On the other hand, the D of the first negative electrode active material 50 The diameter of the second negative electrode active material is 10 μm to 30 μm, preferably 10 μm to 20 μm. 50 is 5μm~25 μm Preferably, the particle size may be 5 μm to 20 μm.

[0012] The negative electrode conductive material may be a point-type conductive material.

[0013] On the other hand, the positive electrode active material may include a single-particle lithium nickel oxide having a Ni content of 70 mol% or less. Here, the single-particle lithium nickel oxide may contain 30 or fewer nodules, and the average particle size of the nodules may be 0.8 μm to 4.0 μm.

[0014] Preferably, the single-particle lithium nickel oxide is represented by the following [Chemical Formula 1] thing That's fine. [Chemical formula 1] Li 1+x [Ni a Co b Mn c M 1 d ]O2 In the above [Chemical Formula 1], M 1 It contains one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo, and -0.1 ≤ x ≤ 0.1, 0.5 ≤ a ≤ 0.7, 0 <b<0.5、0<c<0.5、0≦d≦0.2である。

[0015] The single-particle lithium nickel oxide may further include a coating layer on its surface containing one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo.

[0016] The lithium secondary battery according to the present invention may have an energy density of 260 Wh / kg or more, and a charge cut-off voltage of 4.35 V or more. [Effects of the Invention]

[0017] The lithium secondary battery according to the present invention has a particle size of the negative electrode active material, a negative electrode cross-sectional loading amount, and a negative electrode conductive material. 、 The invention is characterized in that the CFC, which is the relationship between the N / P ratio, is designed to satisfy a specific range. As in the present invention, when the CFC value defined by formula (1) of the lithium secondary battery satisfies the range of 0.38 to 1.962, degradation due to lithium plating is suppressed at low temperatures, and the effect of significantly improving life characteristics can be obtained.

[0018] On the other hand, the lithium secondary battery according to the present invention can use a single-particle type positive electrode active material having a nickel content of 70 mol% or less, preferably 50 to 70 mol%, as the positive electrode active material. In this case, it can be stably driven at a high voltage of 4.35V or higher, and a high energy density can be achieved. [Brief explanation of the drawing]

[0019] [Figure 1] This is a scanning electron microscope image of a single-particle cathode active material. [Figure 2] This is a scanning electron microscope image of a pseudo-single-particle cathode active material. [Figure 3] This is a scanning electron microscope image of a secondary particle type cathode active material. [Modes for carrying out the invention]

[0020] The present invention will be described in more detail below.

[0021] Terms and words used in this specification and claims are, general It should not be interpreted in a way that is limited to its literal or dictionary meaning, and the inventors isIn accordance with the principle that terms can be appropriately defined to best describe the invention, the terms should be interpreted to have meanings and concepts consistent with the technical idea of ​​this invention.

[0022] In the present invention, "D 50 "50% of the volume cumulative particle size distribution of the powder being measured represents the particle size corresponding to 50% of the volume cumulative amount, and can be measured using the laser diffraction method. For example, after dispersing the powder to be measured in a dispersion medium, it is introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac MT 3000), and ultrasonic waves at approximately 28 kHz are irradiated at an output of 60 W. death, After obtaining a volume-cumulative particle size distribution graph, the particle size corresponding to 50% of the volume-cumulative amount can be determined to perform the measurement.

[0023] In this invention, "single-particle type" refers to a particle formed by the aggregation of 30 or fewer sub-particles. The sub-particle unit constituting a single-particle type particle is called a nodule. Single-particle type particles include single particles consisting of one nodule and pseudo-single particles which are composites of 2 to 30 nodules. Figure 1 shows a scanning electron microscope image of a positive electrode active material in single-particle form, and Figure 2 shows a scanning electron microscope image of a positive electrode active material in pseudo-single-particle form.

[0024] The aforementioned "nodule" constitutes a single particle and a pseudo-single particle. Sub It is a single crystal consisting of individual particles and lacking crystalline grain boundaries, or 、 Even if the material is a polycrystalline material with no visible grain boundaries when observed using a scanning electron microscope at a field of view of 5,000x to 20,000x, it is still acceptable.

[0025] In this invention, "secondary particle type" refers to a particle formed by the aggregation of more than 30 sub-particles. To distinguish it from the sub-particles that constitute single-particle type particles, the sub-particles that constitute secondary particles are referred to as "primary particles." Figure 3 shows a scanning electron microscope (SEM) image of a secondary particle type cathode active material.

[0026] In this invention, "particle" refers to a single particle, a pseudo-single particle, a primary particle, or a nodule. 、 It is a concept that includes one or all of these, including secondary particles.

[0027] In the present invention, the average particle size (D) of the nodule or primary particle mean ) refers to the arithmetic mean of these values, calculated after measuring the particle sizes of nodules or primary particles observed from scanning electron microscope images.

[0028] The inventors of this invention have diligently conducted research to develop a lithium secondary battery with excellent low-temperature life characteristics, and as a result, have found that the particle size of the negative electrode active material, the amount of negative electrode cross-sectional loading, and the negative electrode conductive material 、 Furthermore, we discovered that when the CFC, which is the relationship between the N / P ratio, satisfies the range of 0.38 to 1.962, degradation due to lithium plating is suppressed at low temperatures, and low-temperature life characteristics are significantly improved, thus completing the present invention.

[0029] Specifically, the lithium secondary battery according to the present invention comprises a negative electrode active material including a first negative electrode active material and a second negative electrode active material, and a negative electrode conductive material. 、 and a negative electrode including a negative electrode composite layer containing a negative electrode binder, positive electrode active material, positive electrode conductive material 、 The cathode comprises a positive electrode including a positive electrode composite layer containing a positive electrode binder, and an electrolyte, wherein the CFC defined by the following formula (1) is 0.38 to 1.962, preferably 0.39 to 1.962, and more preferably 0.40 to 1.962.

[0030] Formula (1): CFC=100×W c -{(D 50、a1 ×D 50、a2 ×L×RN / P ×10 10 ) / MW C}

[0031] In equation (1) above, W c This is the ratio of the weight of the negative electrode conductive material to the total weight of the negative electrode composite layer, MW C This is the value of the weight of 1 mole of carbon measured in grams, D 50、a1 This is the D of the first negative electrode active material, measured in units of meters. 50 x, D 50、a2 This is the D of the second negative electrode active material, measured in units of meters. 50 The value is L, where g / 25cm 2 This is the value of the weight of the negative electrode active material per unit area of ​​the negative electrode composite layer arranged in the cross-section of the negative electrode, measured in units of R. N / P This is the ratio of the negative electrode capacity to the positive electrode capacity.

[0032] When a lithium secondary battery is designed so that the CFC value meets the aforementioned range, the low-temperature life characteristics are significantly improved. If the CFC is less than 0.38 or greater than 1.962, lithium plating occurs during low-temperature charging and discharging, causing a rapid decrease in cell capacity. Generally, at low temperatures, Li ions have low conductivity, which increases resistance during low-temperature charging and discharging. This prevents lithium ions from being completely inserted into the negative electrode in the high-voltage region during charging, causing them to accumulate on the surface of the negative electrode and resulting in lithium plating. However, as in the present invention, when the negative electrode is designed so that the CFC is between 0.38 and 1.962 by adjusting the weight of the negative electrode conductive material in the negative electrode composite layer, the particle size and content of the negative electrode active material, and the N / P ratio, the electron and ionic conductivity of the negative electrode increases, improving lithium mobility. As a result, the internal resistance of the electrode and lithium plating decrease, improving the low-temperature life characteristics.

[0033] On the other hand, the ratio W of the weight of the negative electrode conductive material to the total weight of the negative electrode composite layer c This may be 0.001 to 0.05, preferably 0.002 to 0.03, and more preferably 0.003 to 0.03. c When the above range is satisfied, the electrical conductivity and capacitance characteristics of the negative electrode are excellent. cIf it is too small, the battery conductivity of the negative electrode decreases, increasing the internal resistance of the cell, and lithium plating may occur at low temperatures. c If it is too large, the negative electrode capacity may decrease.

[0034] The aforementioned MW C This is the weight value of 1 mole of carbon measured in grams. can be, It is 12.

[0035] On the other hand, L is the unit area (25 cm²) of the negative electrode composite layer arranged in the cross-section of the negative electrode. 2 This is the weight of the negative electrode active material per unit area, and may be 0.2 to 0.5, preferably 0.3 to 0.4, and more preferably 0.3 to 0.35. When L satisfies the above range, the ratio of negative electrode conductive material to negative electrode active material is appropriately maintained, lithium plating can be effectively suppressed during low-temperature charging and discharging, and a high energy density can be achieved.

[0036] Furthermore, R is the ratio of the negative electrode capacity to the positive electrode capacity. N / P The negative electrode capacity may be 1.05 to 1.10, preferably 1.06 to 1.09, and more preferably 1.07 to 1.08. If the negative electrode capacity is too small relative to the positive electrode capacity, lithium plating may occur; if it is too large, the energy density may decrease.

[0037] The aforementioned W c , D 50、a1 , D 50、a2 , L, R N / P This is a unitless number that does not contain any units.

[0038] The components of the lithium secondary battery according to the present invention will be described in more detail below.

[0039] negative electrode The lithium secondary battery according to the present invention comprises a first negative electrode active material, a second negative electrode active material, and a negative electrode conductive material. 、 and a negative electrode including a negative electrode binder. Specifically, the negative electrode is a negative electrode current collector and, a negative electrode composite layer formed on at least one surface of the negative electrode current collector and The negative electrode composite layer includes a negative electrode active material and a negative electrode conductive material. 、 and a negative electrode binder. The negative electrode active material comprises a first negative electrode active material and a second negative electrode active material.

[0040] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy can be used. obtain. Furthermore, the negative electrode current collector is typically 3 μm It can have a thickness of ~500 μm, and, similar to the positive electrode current collector, it is possible to form fine irregularities on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it can be used in various forms such as films, sheets, foils, meshes, porous materials, foams, and nonwoven fabrics.

[0041] On the other hand, the first negative electrode active material and the second negative electrode active material may each be independently a graphite-based material such as natural graphite or artificial graphite. Preferably, the first negative electrode active material is artificial graphite, and the second negative electrode active material may be natural graphite. The graphite-based materials for the first negative electrode active material and the second negative electrode active material may each be independently the graphite system The negative electrode active material may or may not include a coating layer formed on its surface. The coating layer may be a carbon coating layer.

[0042] The carbon coating layer is made of coal tar pitch and rayon. 、 and one or more substances selected from the group consisting of polyacrylonitrile resins. 、 or 、The carbon coating layer can be formed by providing a precursor of the substance to the surface of the graphite-based substance and then thermally decomposing it. Preferably, the carbon coating layer contains soft carbon and can be formed by the calcination and thermal decomposition process of the coal tar pitch. The heat treatment process for forming the carbon coating layer can be carried out in a temperature range of 1000°C to 4000°C. However, if the heat treatment process is carried out at a temperature below 1000°C, it may be difficult to form a uniform carbon coating layer, and if it is carried out at a temperature above 4000°C, there is a problem of excessive carbon coating layer formation during the process. The first negative electrode active material and the second negative electrode active material are D 50 They may be the same or different. D of the first negative electrode active material and the second negative electrode active material 50 If they differ, the first negative electrode active material is either larger or smaller than the second negative electrode active material. 50 It can have.

[0043] On the other hand, the D of the first negative electrode active material 50 The diameter of the second negative electrode active material may be 10 μm to 30 μm, preferably 10 μm to 20 μm. 50 The diameter may be 5 μm to 25 μm, preferably 5 μm to 20 μm. The D of the first negative electrode active material and the second negative electrode active material 50 When the above range is met, the CFC value is more likely to meet the range of the present invention, and the difference in particle size of each negative electrode active material makes the packing between particles smoother, reducing internal voids. As a result, the degree of electrode orientation decreases during rolling, and the effect of suppressing electrode expansion during charging and discharging can be obtained.

[0044] On the other hand, in the present invention, the first negative electrode active material and the second negative electrode active material can be mixed in a weight ratio of 90:10 to 50:50, preferably 90:10 to 60:40, and more preferably 90:10 to 70:30. When the mixing ratio of the first negative electrode active material and the second negative electrode active material satisfies the above range, superior electrochemical performance is observed.

[0045] On the other hand, the total content of the negative electrode active material, including the first negative electrode active material and the second negative electrode active material, may be 80% to 98% by weight, preferably 90% to 98% by weight, and more preferably 93% to 98% by weight, relative to the total weight of the negative electrode composite layer. When the content of the negative electrode active material satisfies the above range, an excellent energy density can be achieved.

[0046] Next, the negative electrode conductive material is used to impart conductivity to the negative electrode, and can be used without particular limitations in the battery it is configured in, as long as it does not cause a chemical change and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, etc. nine Examples include carbon-based materials such as carbon fibers and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these materials alone or a mixture of two or more materials is used. obtain.

[0047] Preferably, the negative electrode conductive material may be a point-type conductive material. A point-type conductive material means a conductive material that has a particulate form and makes point-like contact with the active material. Specific examples of point-type conductive materials include, but are not limited to, carbon-based particles such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and porous carbon. Because point-type conductive materials have a low molecular weight and excellent dispersibility, when used, the conductive material can be uniformly dispersed in the negative electrode slurry, reducing viscosity and thereby improving the coating properties of the negative electrode slurry.

[0048] The aforementioned negative electrode conductive material is typically 0.1% of the total weight of the negative electrode active material layer. weight%The negative electrode conductive material can be included in an amount of ~5% by weight, preferably 0.2% to 3% by weight, and more preferably 0.3% to 3% by weight. If the content of the negative electrode conductive material is too low, the electrical conductivity of the negative electrode will decrease, which may cause lithium plating during low-temperature operation. If the content of the negative electrode conductive material is too high, the content of the negative electrode active material will decrease, which may degrade the capacitance characteristics.

[0049] The aforementioned negative electrode binder plays a role in improving adhesion between negative electrode active material particles and the adhesion between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), Poly Examples include vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more is used. obtain.

[0050] The negative electrode binder is 1 in proportion to the total weight of the positive electrode active material layer. weight% ~10% by weight, preferably 1 weight% ~8% by weight, more preferably 1 weight% ~5% by weight in It can be included.

[0051] The aforementioned negative electrode is manufactured by a conventional negative electrode manufacturing method. do This is possible. For example, the negative electrode may consist of a negative electrode active material and a negative electrode binder. 、 and / or a negative electrode slurry is produced by mixing a negative electrode conductive material in a solvent, applying the negative electrode slurry onto a negative electrode current collector, and then drying and rolling it. do or 、The negative electrode slurry is cast onto another support, and the resulting film, obtained by peeling it off the support, is then laminated onto the negative electrode current collector. do It is possible.

[0052] On the other hand, the solvent for the negative electrode slurry is a solvent commonly used in the relevant technical field. of for There are For example, one of the following can be used: dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc. in, Alternatively, two or more types can be mixed and used. The amount of solvent used will be determined considering the slurry coating thickness and manufacturing yield, and the negative electrode active material, conductive material 、 and dissolve or disperse the binder, after that Therefore, when coating for the manufacture of the positive electrode, it has a viscosity that can exhibit excellent thickness uniformity. Na That level is sufficient.

[0053] positive electrode The lithium secondary battery according to the present invention comprises a positive electrode active material and a positive electrode conductive material. 、 and a positive electrode including a positive electrode binder. Specifically, the positive electrode includes a positive electrode current collector. and , a positive electrode active material layer formed on at least one surface of the positive electrode current collector and The positive electrode active material layer comprises a positive electrode active material and a positive electrode conductive material. 、 and includes a positive electrode binder.

[0054] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. can be used. obtain. Furthermore, the positive electrode current collector is typically 3 μmIt can have a thickness of ~500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to enhance the adhesion of the positive electrode active material. For example, it can be used in various forms such as films, sheets, foils, meshes, porous materials, foams, and nonwoven fabrics.

[0055] On the other hand, in the present invention, the positive electrode active material may include a single-particle lithium nickel-based oxide having a Ni content of 70 mol% or less, preferably 50 mol% to 70 mol%.

[0056] As described above, when using single-particle lithium nickel oxide with a relatively low nickel content as the positive electrode active material, side reactions with the electrolyte are suppressed under high temperature and high voltage conditions, reducing gas generation and achieving excellent lifespan characteristics.

[0057] In the case of lithium nickel oxides in secondary particle form, where 40 to several hundred primary particles aggregate, the large contact area with the electrolyte leads to numerous side reactions with the electrolyte, generating gas during these side reaction processes. In particular, under high temperature and / or high voltage conditions, the amount of gas generated increases significantly, leading to rapid cell degradation. In contrast, single-particle lithium nickel oxides have fewer nodules constituting the particles, resulting in fewer interfaces within the particles and a smaller contact area with the electrolyte. Therefore, compared to secondary particles, there are fewer side reactions with the electrolyte, and consequently, the amount of gas generated is significantly less. Consequently, when single-particle lithium nickel oxides are used as positive electrode active materials, excellent lifetime characteristics can be obtained even under high voltage and high temperature conditions.

[0058] Furthermore, in the case of single-particle lithium nickel oxides with a relatively low nickel content, the structural stability at high voltages is higher compared to lithium nickel oxides with a high nickel content or those with a secondary particle form, thus minimizing the degradation of life characteristics when driven at high voltages. Specifically, the higher the nickel content in the lithium nickel oxide, the more reactive the Ni... +4The increased ion content reduces the structural stability of the positive electrode active material during charging and discharging, leading to rapid degradation of the positive electrode. This phenomenon worsens under high-voltage operation. Therefore, in this invention, by applying a lithium nickel-based oxide with a low Ni content of 70 mol% or less, it is possible to suppress the reduction in lifespan due to degradation of the active material under high-voltage operation. However, if the Ni content is too low, the capacity characteristics will deteriorate, so the Ni content of the lithium nickel-based oxide is preferably around 50 mol% to 70 mol%.

[0059] Specifically, the single-particle lithium nickel oxide is made of nickel, manganese 、 It may also be a lithium transition metal oxide containing cobalt, which can be represented, for example, by the following [Chemical Formula 1].

[0060] [Chemical formula 1] Li 1+x [Ni a Co b Mn c M 1 d ]O2

[0061] In the above [Chemical Formula 1], M 1 It may contain one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo. 1 When elements are included, the structural stability of lithium nickel oxide particles is improved, and better life characteristics can be achieved when driven at high voltage. Preferably, the M 1 The elements are Ti, Mg, Al, Zr 、 It may include one or more selected from the group consisting of and Y, and more preferably Ti, Mg, Al, Zr 、 It may include two or more types selected from the group consisting of and Y.

[0062] The aforementioned 1+x represents the lithium molar ratio within the lithium nickel oxide, and may be -0.1 ≤ x ≤ 0.1, 0 ≤ x ≤ 0.1, or 0 ≤ x ≤ 0.07. When 1+x satisfies the above range, a stable layered crystal structure is formed. obtain.

[0063] The value of 'a' represents the molar ratio of nickel to the total metals other than lithium in the lithium nickel oxide, and may be 0.5 ≤ a ≤ 0.7, 0.55 ≤ a ≤ 0.7, or 0.55 ≤ a ≤ 0.65. When 'a' satisfies the above range, it can be driven stably at high voltage and achieve high capacity.

[0064] The above b represents the molar ratio of cobalt among the total metals other than lithium in the lithium nickel oxide, and 0 <b<0.5、0.05≦b≦0.4 、 Alternatively, 0.1 ≤ a ≤ 0.4 may also be acceptable.

[0065] The aforementioned c represents the molar ratio of manganese to the total metals other than lithium in the lithium nickel oxide, and 0 <c<0.5、0.05≦c≦0.4 、 Alternatively, 0.1 ≤ c ≤ 0.4 may also be acceptable.

[0066] The above d is M, which is the total amount of metals other than lithium in the lithium nickel oxide. 1 The molar ratio of the elements is shown, with 0≦d≦0.2 and 0≦d≦0.1. 、 or 0 <d≦0.1であってもよい。M 1 When the molar ratio of the elements satisfies the aforementioned range, the structural stability and capacity of the positive electrode active material can all be excellent.

[0067] On the other hand, the single-particle lithium nickel oxide may further include a coating layer on its surface containing one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo.

[0068] When a coating layer is present on the surface of a lithium nickel oxide, the coating layer suppresses contact between the electrolyte and the lithium nickel oxide, thereby reducing the elution of transition metals and the generation of gases due to side reactions with the electrolyte, and thus improving the lifespan characteristics. Preferably, the coating layer may contain two or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo, and more preferably Ti, Mg, Al, Zr, Y 、 It may contain two or more elements selected from the group consisting of and W.

[0069] On the other hand, the single-particle lithium nickel oxide preferably contains 30 or fewer nodules, preferably 1 to 25, and more preferably 1 to 15. This is because if the number of nodules constituting the lithium nickel oxide exceeds 30, particle cracking increases during electrode manufacturing, and the occurrence of internal cracks due to volume expansion / contraction of nodules increases during charging and discharging, which can reduce the improvement effect on high-temperature lifetime characteristics and high-temperature storage characteristics.

[0070] On the other hand, the nodule of Average particle size teeth, The nodule particle size may be 0.8 μm to 4.0 μm, preferably 0.8 μm to 3 μm, and more preferably 1.0 μm to 3.0 μm. When the average particle size of the nodules satisfies the above range, particle cracking during electrode manufacturing is minimized, and the increase in resistance can be more effectively suppressed. Here, the average particle size of the nodules refers to the value obtained by measuring the particle size of each nodule observed from the SEM image obtained by analyzing the positive electrode active material powder with a scanning electron microscope, and then calculating the arithmetic mean of the measured values.

[0071] On the other hand, the single-particle lithium nickel oxide having a nickel content of 70 mol% or less constitutes 50% by weight or more, preferably 70% by weight or more, and more preferably 100% by weight of the total positive electrode active material in the positive electrode active material layer. in can be included . NiSingle-particle lithium nickel oxide with a nickel content of 70 mol% or less Relative to the total weight of the positive electrode active material When the ratio satisfies the aforementioned range, it can be driven stably at high voltage.

[0072] The positive electrode active material layer may contain a portion of a positive electrode active material other than single-particle lithium nickel oxide with a nickel content of 70 mol% or less, i.e., lithium nickel oxide in secondary particle form and / or single-particle lithium nickel oxide with a nickel content exceeding 70 mol%. However, if the proportion of secondary particles and / or lithium nickel oxide with a nickel content exceeding 70 mol% exceeds 50% by weight of the total positive electrode active material, the lifetime characteristics may deteriorate during high-voltage operation.

[0073] On the other hand, the positive electrode active material of D 50 teeth, The particle size may be 3.0 μm to 8.0 μm, preferably 3.0 μm to 7.5 μm. More preferably, it is about 3.5 μm to 7.5 μm. D of lithium nickel oxide 50 If it is too small, the processability during electrode manufacturing may decrease, the electrolyte impregnation may decrease, and the electrochemical properties may increase. 50 If the value is too large, the resistance increases, leading to a problem of reduced output characteristics.

[0074] On the other hand, the positive electrode active material is the total weight of the positive electrode active material layer, i.e., positive electrode active material, positive electrode conductive material 、 Based on the total amount of the cathode binder, the cathode active material can be included in an amount of 93% to 99% by weight, preferably 95% to 98% by weight, and more preferably 95% to 97% by weight. When the content of the cathode active material satisfies the above range, a high energy density can be achieved.

[0075] Next, the positive electrode conductive material is used to impart conductivity to the positive electrode, and can be used without particular limitations as long as it does not cause chemical changes and has electronic conductivity in the battery it is configured in. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and from these, one or more materials may be used. obtain.

[0076] Preferably, the positive electrode conductive material may include a linear conductive material and a point conductive material. When both a linear conductive material and a point conductive material are used as the positive electrode conductive material, excellent conductivity can be achieved even with a small amount of conductive material, thus allowing for an increase in the positive electrode active material content within the positive electrode.

[0077] Here, the linear conductive material refers to a conductive material that makes line contact with the active material, and the point conductive material refers to a conductive material that makes point contact with the active material.

[0078] Examples of the linear conductive material include fibrous carbon materials such as carbon fibers and carbon nanotubes, and metal fibers such as copper, nickel, aluminum, and silver, but are not limited to these, and various conductive materials in fibrous form can be used.

[0079] Examples of the point-like conductive material that can be used include carbon-based particles such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and porous carbon.

[0080] The positive electrode conductive material is usually the total weight of the positive electrode active material layer, i.e., positive electrode active material, positive electrode conductive material、 And the total weight including the positive electrode binder do, The positive electrode conductive material can be included in an amount of 0.5 to 2% by weight, preferably 0.5 to 1.8% by weight, and more preferably 0.8 to 1.8% by weight. When the content of the positive electrode conductive material satisfies the above range, the positive electrode conductivity is excellent, the active material content in the positive electrode can be increased, and high capacity can be achieved.

[0081] Next, the positive electrode binder plays a role in improving adhesion between positive electrode active material particles and adhesion between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), Poly Examples include vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more is used. obtain.

[0082] The positive electrode binder is 0.5% to 5% by weight of the total weight of the positive electrode active material layer, preferably 1 weight% ~4% by weight, comfort, 1 weight% ~3% by weight in It can be included.

[0083] The positive electrode is manufactured by a conventional method for manufacturing positive electrodes. do This is possible. For example, the positive electrode may consist of a positive electrode active material and a positive electrode binder. 、 and / or a positive electrode slurry is produced by mixing positive electrode conductive material in a solvent, applying the positive electrode slurry onto a positive electrode current collector, and then drying and rolling it. do or 、The positive electrode slurry can be cast onto another support, and the resulting film, obtained by peeling it off the support, can be laminated onto the positive electrode current collector.

[0084] On the other hand, the solvent for the positive electrode slurry is a solvent commonly used in the relevant technical field. of for There are For example, one of the following can be used: dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc. in, Alternatively, two or more types can be mixed and used. The amount of solvent used will be determined considering the coating thickness of the slurry and the manufacturing yield, and will be the amount of the positive electrode active material and conductive material. 、 and dissolve or disperse the binder, after that Therefore, when coating for the manufacture of the positive electrode, it has a viscosity that can exhibit excellent thickness uniformity. Na That level is sufficient.

[0085] electrolyte The electrolyte may include an organic solvent and a lithium salt.

[0086] The aforementioned organic solvent can be used without particular limitations, as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the aforementioned organic solvents include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (propylene Carbonate solvents such as carbonate (PC); alcoholic solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear or branched hydrocarbon group of C2-C20 or a cyclic hydrocarbon group of C3-C20, and can include a double-bonded aromatic ring or ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes are used. obtain. In particular, carbonate-based solvents are preferred, and in terms of improving the charge and discharge performance of the battery, cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant are preferred. low High viscosity linear carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate) 、 A mixture of (or diethyl carbonate, etc.) is more preferable.

[0087] The lithium salt can be any compound capable of providing lithium ions for use in lithium secondary batteries, without any particular limitations. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAl O 4. LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used. The concentration of the lithium salt is 0.1 M ~3.0M, preferably 0.1 M ~2.0M, more preferably 0.5 M It is preferable to use it within a range of ~1.5M. When the lithium salt concentration falls within the above range, the electrolyte can exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions teeth It allows for effective movement.

[0088] The electrolyte may further contain additives in addition to the constituent components of the electrolyte, for purposes such as improving the battery's lifespan, suppressing the decrease in battery capacity, and improving the battery's discharge capacity. For example, the additives may include various additives used in the art, such as fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinylethylene carbonate (VEC), ethylene sulfate (ESa), lithium difluorophosphate (LiPO2F2), lithium bisoxalate borate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium difluorooxalate borate (LiDFOB), lithium difluorobisoxalate phosphate (LiDFBP), and lithium tetrafluorooxalate phosphate (LiTF OP), lithium methyl sulfate (LiMS), lithium ethyl sulfate (LiES), propanesultone (PS), propensultone (PRS), succinonitrile (SN), adiponitrile (AND), 1,3,6-hexanetricarbonite (HTCN), 1,4-dicyano-2-butene (DCB), fluorobenzene (FB), ethyldi(pro-2-i-1-nyl)phosphate (EDP), 5-methyl-5-propargyloxylcarbonyl-1,3-dioxan-2-one (MPOD), etc., can be used alone or in combination, but are not limited thereto. The additives can be added in an amount of 0.1% of the total weight of the electrolyte. weight% ~10% by weight, preferably 0.1 weight% ~5% by weight in It can be included.

[0089] Separator The lithium secondary battery according to the present invention may further include a separator between the positive electrode and the negative electrode, if necessary. The separator separates the negative electrode and the positive electrode and provides a passage for the movement of lithium ions. RegularAny material used as a separator in a lithium secondary battery can be used without particular restrictions, but materials that have low resistance to ion movement of the electrolyte and excellent electrolyte moisture absorption capacity are particularly preferred. Specifically, porous polymer films, such as ethylene homopolymers, propylene homopolymers, ethylene / butene copolymers, and ethylene / hexene copolymers are preferred. 、 and porous polymer films made from polyolefin polymers such as ethylene / methacrylate copolymers. 、 Alternatively, a laminated structure of two or more layers may be used. obtain. Alternatively, ordinary porous nonwoven fabrics, such as those made of high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, to ensure heat resistance or mechanical strength, coated separators containing ceramic components or polymeric substances may be used, and these can be selectively used in single-layer or multi-layer structures.

[0090] The lithium secondary battery of the present invention, as described above, can operate stably at high voltage to achieve high energy density and exhibits excellent lifespan characteristics at low temperatures.

[0091] Preferably, the lithium secondary battery according to the present invention of Charging cutoff voltage teeth, The voltage is preferably 4.35V or higher, more preferably 4.35V to 5V, and more preferably 4.35V to 4.5V. When the charge cut-off voltage meets the above range during operation, a high energy density can be achieved. Specifically, the lithium secondary battery according to the present invention of Energy density teeth, The 260 Wh / kg or more, preferably 260 Wh / kg to 330 Wh / kg, and more preferably 270 Wh / kg to 320 Wh / kg.

[0092] The capacity of a lithium secondary battery is affected not only by the type of active material used but also by the range of the driving voltage. In particular, when lithium nickel cobalt manganese oxide is used as the positive electrode active material, higher driving voltages can be achieved to realize higher capacity. However, when the driving voltage is high, side reactions with the electrolyte increase during charging and discharging, leading to a problem where the structural breakdown of the positive electrode active material occurs rapidly, and the life characteristics deteriorate rapidly. This problem is more pronounced in high-nickel lithium nickel cobalt manganese oxides with a high nickel content. However, when lithium nickel oxide with a Ni content of 70 mol% or less and in single-particle form is used as the positive electrode active material, stable operation is possible even at high voltages of 4.35V or higher, and high energy density can be achieved.

[0093] The lithium secondary battery according to the present invention can be usefully applied in portable devices such as mobile phones, notebook computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs). Because the lithium secondary battery according to the present invention is driven at high voltage, achieves high energy density, and offers excellent safety in the event of thermal runaway, it can be particularly useful in the field of electric vehicles.

[0094] According to another embodiment of the present invention, a battery module and a battery pack including the lithium secondary battery according to the present invention as a unit cell are provided.

[0095] The aforementioned battery module or battery pack can be used as a power source for one or more medium-to-large devices, including power tools; electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems.

[0096] Hereinafter, embodiments of the present invention will be described in detail so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention can be realized in various different forms and is not limited to the embodiments described herein.

[0097] Example 1 <Manufacturing of negative electrodes> A negative electrode slurry was prepared by mixing negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) in water in a weight ratio of 96.15:0.5:2.3:1.05. Here, the negative electrode active material was D 50 Artificial graphite and D 50 Natural graphite with a particle size of 18 μm was used in a mixture of 8:2 by weight, and Super C 65 was used as the negative electrode conductive material.

[0098] A negative electrode slurry is spread on the copper current collector sheet over a 25 cm area on one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3415 g / 25 cm². 2 The material was applied in this manner, dried, and then rolled to produce the negative electrode.

[0099] <Manufacturing of positive electrodes> A cathode slurry (solid content 75 wt%) was prepared by mixing a cathode active material, cathode conductive material, and PVDF binder in N-methylpyrrolidone in a weight ratio of 97:1.2:1.8. Here, single-particle Li[Ni 0.60 Co 0.10 Mn 0.30 100% O2 was used, and as the positive electrode conductive material, a mixture of carbon nanotubes and acetylene black in a 2:1 weight ratio was used.

[0100] The positive electrode slurry is placed on the aluminum current collector sheet at a ratio of negative electrode capacity to positive electrode capacity (R N / P The material was coated to a ratio of 1.07, dried, and then rolled to produce the positive electrode.

[0101] <Manufacturing of lithium-ion secondary batteries> As stated above Made in A separator is interposed between the manufactured positive and negative electrodes. Let An electrode assembly was manufactured, and after inserting the electrode assembly into a battery case, an electrolyte was injected to manufacture a lithium secondary battery cell.

[0102] Here, the electrolyte used was prepared by dissolving 61.0M LiPF in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and then adding 0.5% by weight of vinylene carbonate (VC), 0.5% by weight of propane sultone (PS), 1% by weight of ethylene sulfate (ESa), 1% by weight of lithium difluorophosphate, and 40.2% by weight of LiBF as additives.

[0103] Example 2 A lithium secondary battery was manufactured using the same method as in Example 1, except that carbon nanotubes were used alone as the positive electrode conductive material.

[0104] Example 3 During the manufacturing of the negative electrode, the negative electrode slurry is applied to one side of the copper current collector in a 25cm layer. 2 The weight of the negative electrode active material per unit area (L) is 0.3175 g / 25 cm². 2 The mixture is applied in such a way that, during the manufacturing of the positive electrode, the ratio of the negative electrode capacity to the positive electrode capacity (R) is determined. N / P A lithium secondary battery was manufactured in the same manner as in Example 1, except that the material was coated to a ratio of 1.072, and a mixture of carbon nanotubes and acetylene black in a weight ratio of 5:1 was used as the positive electrode conductive material.

[0105] Example 4 <Manufacturing of negative electrodes> A negative electrode slurry was prepared by mixing negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) in water in a weight ratio of 94.65:2:2.3:1.05. Here, D was used as the negative electrode active material. 50 Artificial graphite and D 50and natural graphite with an average particle diameter of 9 μm at a weight ratio of 8:2, and Super C 65 was used as the negative electrode conductive material.

[0106] The negative electrode slurry was applied onto one surface of a copper current collector sheet at 25 cm 2 per unit area such that the weight (L) of the negative electrode active material per unit area was 0.3513 g / 25 cm 2 . After drying, the coated sheet was rolled to prepare a negative electrode.

[0107] <Preparation of Positive Electrode> A positive electrode active material, a positive electrode conductive material, and a PVDF binder were mixed in N-methylpyrrolidone at a weight ratio of 97:1.2:1.8 to prepare a positive electrode slurry (solid content: 75 wt%). Here, single-crystal Li[Ni 0.60 Co 0.10 Mn 0.30 O2 was used as the positive electrode active material in an amount of 100%, and carbon nanotubes and acetylene black were mixed at a weight ratio of 2:1 and used as the positive electrode conductive material.

[0108] The positive electrode slurry was applied onto an aluminum current collector sheet such that the ratio (R N / P ) of the negative electrode capacity to the positive electrode capacity was 1.0945. After drying, the coated sheet was rolled to prepare a positive electrode.

[0109] <Preparation of Lithium Secondary Battery> A separator was interposed between the positive electrode and the negative electrode prepared as described above to prepare an electrode assembly. After the electrode assembly was inserted into a battery case, an electrolyte was injected to prepare a lithium secondary battery cell. Let

[0110] Here, as the electrolyte, 1.0 M LiPF6 was dissolved in a mixed solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a volume ratio of 3:7, and then 0.5 wt% of vinylene carbonate (VC), 0.5 wt% of propane sultone (PS), 1 wt% of ethylene sulfate (ESa), 1 wt% of lithium difluorophosphate, and 0.2 wt% of LiBF4 were added as additives to prepare the electrolyte.​

[0111] Example 5 An anode slurry was prepared by mixing an anode active material:an anode conductive material:styrene-butadiene rubber (SBR):carboxymethyl cellulose (CMC) in water at a weight ratio of 95.90:0.75:2.3:1.05. Here, as the anode active material, D 50 of 16 μm artificial graphite and D 50 of 18 μm natural graphite were mixed at a weight ratio of 8:2 for use, and Super C 65 was used as the anode conductive material.

[0112] The anode slurry was coated on a copper current collector sheet such that the weight (L) of the anode active material per 25 cm 2 area of one surface of the copper current collector was 0.3391 g / 25 cm 2 , and after drying, the sheet was rolled to manufacture an anode.

[0113] <Manufacture of Cathode> A cathode slurry (solid content: 75 wt%) was prepared by mixing a cathode active material:a cathode conductive material:a PVDF binder in N-methylpyrrolidone at a weight ratio of 97:1.2:1.8. Here, as the cathode active material, 100% of single-crystal Li[Ni 0.60 Co 0.10 Mn 0.30 O2 was used, and as the cathode conductive material, carbon nanotubes and acetylene black were mixed at a weight ratio of 2:1 for use.

[0114] The cathode slurry was coated on an aluminum current collector sheet such that the ratio (R N / P ) of the anode capacity to the cathode capacity was 1.0730, and after drying, the sheet was rolled to manufacture a cathode.

[0115] <Manufacture of Lithium Secondary Battery> An electrode assembly was manufactured by interposing a separator between the cathode and the anode manufactured as described above, and after inserting the electrode assembly into a battery case, an electrolyte was injected to manufacture a lithium secondary battery cell. Let

[0116] ​Here, the electrolyte used was prepared by dissolving 61.0M LiPF in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and then adding 0.5% by weight of vinylene carbonate (VC), 0.5% by weight of propane sultone (PS), 1% by weight of ethylene sulfate (ESa), 1% by weight of lithium difluorophosphate, and 40.2% by weight of LiBF as additives.

[0117] Example 6 A negative electrode slurry was prepared by mixing negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) in water in a weight ratio of 95.65:1:2.3:1.05. Here, the negative electrode active material was D 50 Artificial graphite and D 50 Natural graphite with a particle size of 18 μm was used in a mixture of 8:2 by weight, and Super C 65 was used as the negative electrode conductive material.

[0118] A negative electrode slurry is spread on the copper current collector sheet over a 25 cm area on one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3512 g / 25 cm². 2 The material was applied in this manner, dried, and then rolled to produce the negative electrode.

[0119] <Manufacturing of positive electrodes> A positive electrode slurry (solid content 75 wt%) was prepared by mixing positive electrode active material, positive electrode conductive material, and PVDF binder in N-methylpyrrolidone in a weight ratio of 97:1.2:1.8. Here, single-particle Li[Ni 0.60 Co 0.10 Mn 0.30 100% O2 was used, and as the positive electrode conductive material, a mixture of carbon nanotubes and acetylene black in a 2:1 weight ratio was used.

[0120] The positive electrode slurry is placed on the aluminum current collector sheet at a ratio of negative electrode capacity to positive electrode capacity (R N / P The material was coated to a ratio of 1.0950, dried, and then rolled to produce the positive electrode.

[0121] <Manufacturing of lithium-ion secondary batteries> A separator is interposed between the positive electrode and the negative electrode manufactured as described above. Let An electrode assembly was manufactured, and after inserting the electrode assembly into a battery case, an electrolyte was injected to manufacture a lithium secondary battery cell.

[0122] Here, the electrolyte used was prepared by dissolving LiPF61.0M in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and then adding the following additives: vinylene carbonate (VC) 0.5% by weight, propane sultone (PS) 0.5% by weight, ethylene sulfate (ESa) 1% by weight, lithium difluorophosphate 1% by weight, and LiBF 40.2% by weight.

[0123] Example 7 A negative electrode slurry was prepared by mixing negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) in water in a weight ratio of 95.40:1.25:2.3:1.05. Here, the negative electrode active material was D 50 Artificial graphite and D 50 Natural graphite with a particle size of 18 μm was used in a mixture of 8:2 by weight, and Super C 65 was used as the negative electrode conductive material.

[0124] A negative electrode slurry is spread on the copper current collector sheet over a 25 cm area on one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3182 g / 25 cm². 2 The material was applied in this manner, dried, and then rolled to produce the negative electrode.

[0125] <Manufacturing of positive electrodes> A positive electrode slurry (solid content 75 wt%) was prepared by mixing positive electrode active material, positive electrode conductive material, and PVDF binder in N-methylpyrrolidone in a weight ratio of 97:1.2:1.8. Here, single-particle Li[Ni 0.60 Co 0.10 Mn0.30 100% O2 was used, and as the positive electrode conductive material, a mixture of carbon nanotubes and acetylene black in a 2:1 weight ratio was used.

[0126] The positive electrode slurry is placed on the aluminum current collector sheet at a ratio of negative electrode capacity to positive electrode capacity (R N / P The material was coated to a ratio of 1.058, dried, and then rolled to produce the positive electrode.

[0127] <Manufacturing of lithium-ion secondary batteries> A separator is interposed between the positive electrode and the negative electrode manufactured as described above. Let An electrode assembly was manufactured, and after inserting the electrode assembly into a battery case, an electrolyte was injected to manufacture a lithium secondary battery cell.

[0128] Here, the electrolyte used was prepared by dissolving LiPF61.0M in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and then adding the following additives: vinylene carbonate (VC) 0.5% by weight, propane sultone (PS) 0.5% by weight, ethylene sulfate (ESa) 1% by weight, lithium difluorophosphate 1% by weight, and LiBF 40.2% by weight.

[0129] Example 8 A negative electrode slurry was prepared by mixing negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) in water in a weight ratio of 94.90:1.75:2.3:1.05. Here, the negative electrode active material was D 50 Artificial graphite and D 50 Natural graphite with a particle size of 18 μm was used in a mixture of 8:2 by weight, and Super C 65 was used as the negative electrode conductive material.

[0130] A negative electrode slurry is spread on the copper current collector sheet over a 25 cm area on one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3460 g / 25 cm². 2The material was applied in this manner, dried, and then rolled to produce the negative electrode.

[0131] <Manufacturing of positive electrodes> A positive electrode slurry (solid content 75 wt%) was prepared by mixing positive electrode active material, positive electrode conductive material, and PVDF binder in N-methylpyrrolidone in a weight ratio of 97:1.2:1.8. Here, single-particle Li[Ni 0.60 Co 0.10 Mn 0.30 100% O2 was used, and as the positive electrode conductive material, a mixture of carbon nanotubes and acetylene black in a 2:1 weight ratio was used.

[0132] The positive electrode slurry is placed on the aluminum current collector sheet at a ratio of negative electrode capacity to positive electrode capacity (R N / P The material was coated to a ratio of 1.083, dried, and then rolled to produce the positive electrode.

[0133] <Manufacturing of lithium-ion secondary batteries> A separator is interposed between the positive electrode and the negative electrode manufactured as described above. Let An electrode assembly was manufactured, and after inserting the electrode assembly into a battery case, an electrolyte was injected to manufacture a lithium secondary battery cell.

[0134] Here, the electrolyte used was prepared by dissolving LiPF61.0M in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and then adding the following additives: vinylene carbonate (VC) 0.5% by weight, propane sultone (PS) 0.5% by weight, ethylene sulfate (ESa) 1% by weight, lithium difluorophosphate 1% by weight, and LiBF 40.2% by weight.

[0135] Comparative Example 1 During the production of the negative electrode slurry, the negative electrode active material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) are mixed in water in a weight ratio of 96.65:2.3:1.05 to produce the negative electrode slurry, and this negative electrode slurry is then placed on a copper current collector sheet, covering 25 cm of one side of the copper current collector.2 The weight of the negative electrode active material per unit area (L) is 0.3205 g / 25 cm². 2 The negative electrode is manufactured by coating it in such a way, and carbon nanotubes are used alone as the positive electrode conductive material during the manufacturing of the positive electrode, and the positive electrode slurry is made with a ratio of negative electrode capacity to positive electrode capacity (R N / P A lithium secondary battery was manufactured in the same manner as in Example 1, except that the coating was applied so that the ratio was 1.072.

[0136] Comparative Example 2 During the production of the negative electrode slurry, the negative electrode active material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) are mixed in water in a weight ratio of 96.65:2.3:1.05 to produce the negative electrode slurry, and this negative electrode slurry is then placed on a copper current collector sheet, covering 25 cm of one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3375 g / 25 cm². 2 The negative electrode is manufactured by coating it in such a way, and when manufacturing the positive electrode, a mixture of carbon nanotubes and acetylene black in a weight ratio of 5:1 is used as the positive electrode conductive material, and the positive electrode slurry is made with a ratio of negative electrode capacity to positive electrode capacity (R N / P A lithium secondary battery was manufactured in the same manner as in Example 1, except that the coating was applied so that the ratio was 1.075.

[0137] Comparative Example 3 During the production of the negative electrode slurry, the negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) are mixed in water in a weight ratio of 96.4:0.25:2.3:1.05 to produce the negative electrode slurry, and this negative electrode slurry is then placed on a copper current collector sheet on a surface of 25 cm on one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3167 g / 25 cm². 2 The negative electrode is manufactured by coating it in such a way, and when manufacturing the positive electrode, carbon nanotubes and acetylene black are mixed in a weight ratio of 5:1 as the positive electrode conductive material, and the positive electrode slurry is made with a ratio of negative electrode capacity to positive electrode capacity (R N / P A lithium secondary battery was manufactured in the same manner as in Example 1, except that the coating was applied so that the ratio was 1.072.

[0138] Comparative Example 4 During the production of the negative electrode slurry, the negative electrode active material, negative electrode conductive material, styrene-butadiene rubber (SBR), and carboxymethylcellulose (CMC) are mixed in water in a weight ratio of 96.4:0.25:2.3:1.05 to produce the negative electrode slurry, and this negative electrode slurry is then placed on a copper current collector sheet on a surface of 25 cm on one side of the copper current collector. 2 The weight of the negative electrode active material per unit area (L) is 0.3428 g / 25 cm². 2 The negative electrode is manufactured by coating it in such a way, and when manufacturing the positive electrode, carbon nanotubes are used alone as the positive electrode conductive material, and the positive electrode slurry is made with a ratio of negative electrode capacity to positive electrode capacity (R N / P A lithium secondary battery was manufactured in the same manner as in Example 1, except that the coating was applied so that the ratio was 1.070.

[0139] Comparative Example 5 During the manufacturing of the negative electrode, the negative electrode slurry is applied to one side of the copper current collector in a 25cm layer. 2 The weight of the negative electrode active material per unit area (L) is 0.3915 g / 25 cm². 2 The mixture is applied in such a way that, during the manufacturing of the positive electrode, the ratio of the negative electrode capacity to the positive electrode capacity (R) is determined. N / P A lithium secondary battery was manufactured in the same manner as in Example 1, except that the coating was applied so that the ratio was 1.3362.

[0140] Comparative Example 6 During the manufacturing of the negative electrode, the negative electrode slurry is applied to one side of the copper current collector in a 25cm layer. 2 The weight of the negative electrode active material per unit area (L) is 0.2986 g / 25 cm². 2 The mixture is applied in such a way that, during the manufacturing of the positive electrode, the ratio of the negative electrode capacity to the positive electrode capacity (R) is determined. N / P A lithium secondary battery was manufactured in the same manner as in Example 4, except that the coating was applied so that the ratio was 1.0010.

[0141] For each of the lithium secondary batteries manufactured according to Examples 1 to 8 and Comparative Examples 1 to 6, the CFC value represented by the following formula (1) is calculated and shown in Table 1 below. Here, MW C It was calculated to be 12g.

[0142] Formula (1): CFC=100×W c -{(D 50、a1 ×D 50、a2 ×L×R N / P ×10 10 ) / MW C}

[0143] In equation (1) above, W c This is the ratio of the weight of the negative electrode conductive material to the total weight of the negative electrode composite layer, MW C This is the value of the weight of 1 mole of carbon measured in grams, D 50、a1 This is the D of the first negative electrode active material, measured in units of meters. 50 x, D 50、a2 This is the D of the second negative electrode active material, measured in units of meters. 50 The value is L, where g / 25cm 2 This is the value of the weight of the negative electrode active material per unit area of ​​the negative electrode composite layer arranged in the cross-section of the negative electrode, measured in units of R. N / P This is the ratio of the negative electrode capacity to the positive electrode capacity.

[0144] [Table 1]

[0145] Experimental Example 1: Evaluation of Low-Temperature Characteristics Each lithium secondary battery manufactured according to Examples 1-8 and Comparative Examples 1-6 was charged to 4.35V at -10°C at 0.2C, and then discharged to 2.5V at 0.33C. This constituted one charge-discharge cycle. After 50 charge-discharge cycles, the capacity retention rate was measured using a PNE cycler.

[0146] Furthermore, the energy density of each lithium secondary battery manufactured according to Examples 1 to 8 and Comparative Examples 1 to 6 was measured when operated within a voltage range of 2.5V to 4.35V. The measurement results are shown in Table 2.

[0147] [Table 2]

[0148] As shown in Table 2 above, the lithium secondary batteries of Examples 1 to 8, in which the CFC satisfies the scope of the present invention, have a capacity retention rate of 87% or more after 50 cycles at a low temperature of -10°C. and In contrast to the high CFCs, the lithium secondary batteries of Comparative Examples 1-6, in which the CFCs deviate from the scope of the present invention, retained a capacity of 37%-80% after 50 cycles at a low temperature of -10°C. and It was very low.

Claims

1. A negative electrode comprising a negative electrode active material including a first negative electrode active material and a second negative electrode active material, a negative electrode conductive material and a negative electrode binder, and a negative electrode composite layer comprising a negative electrode active material, A positive electrode comprising a positive electrode composite layer containing a positive electrode active material, a positive electrode conductive material, and a positive electrode binder, and an electrolyte, A lithium secondary battery having a CFC defined by the following formula (1) between 0.38 and 1.

962. Equation (1): CFC = 100 × W c -{(D) 50、a1 ×D 50、a2 ×L×R N/P ×10 10 ) / MW C } In the above Formula (1), W c is a ratio of a weight of the negative electrode conductive material to a total weight of the negative electrode mixture layer, MW C is a value of a weight of 1 mol of carbon measured in units of g, D 50、a1 is a value of D of a first negative electrode active material measured in units of m, D 50 is a value of D of a second negative electrode active material measured in units of m, L 50、a2 is a value of a weight of the negative electrode active material per unit area of the negative electrode mixture layer disposed in the cross-section of the negative electrode measured in units of g / 25 cm 50 , and R 2 is a ratio of a negative electrode capacity to a positive electrode capacity. N/P ​

2. The lithium secondary battery according to claim 1, wherein the first negative electrode active material and the second negative electrode active material are graphite-based materials.

3. The first negative electrode active material is artificial graphite, The lithium secondary battery according to claim 1, wherein the second negative electrode active material is natural graphite.

4. The lithium secondary battery according to claim 1, wherein the first negative electrode active material and the second negative electrode active material are contained in a weight ratio of 90:10 to 50:

50.

5. The lithium secondary battery according to claim 1, wherein the negative electrode conductive material is a point-type conductive material.

6. The aforementioned W c The lithium secondary battery according to claim 1, wherein the value is 0.001 to 0.

05.

7. D of the first negative electrode active material 50 The size is 10 μm to 30 μm. The second negative electrode active material D 50 The lithium secondary battery according to claim 1, wherein the particle size is 5 μm to 25 μm.

8. The lithium secondary battery according to claim 1, wherein L is 0.2 to 0.

5.

9. The aforementioned R N/P The lithium secondary battery according to claim 1, wherein the ratio is 1.05 to 1.

10.

10. The lithium secondary battery according to claim 1, wherein the positive electrode active material comprises a single-particle type lithium nickel oxide having a Ni content of 70 mol% or less.

11. The lithium secondary battery according to claim 10, wherein the single-particle lithium nickel oxide is contained in an amount of 50% by weight or more relative to the total weight of the positive electrode active material.

12. The aforementioned single-particle lithium nickel oxide contains 30 or fewer nodules. The lithium secondary battery according to claim 10, wherein the average particle size of the nodule is 0.8 μm to 4.0 μm.

13. The lithium secondary battery according to claim 10, wherein the single-particle lithium nickel oxide is represented by the following [Chemical Formula 1]. [Chemical formula 1] Li 1+x [Ni a Co b Mn c M 1 d ]O 2 In the above [Chemical Formula 1], M 1 It contains one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo, and satisfies -0.1 ≤ x ≤ 0.1, 0.5 ≤ a ≤ 0.7, 0 < b < 0.5, 0 < c < 0.5, and 0 ≤ d ≤ 0.

2.

14. The lithium secondary battery according to claim 10, wherein the single-particle lithium nickel oxide further comprises a coating layer on its surface containing one or more elements selected from the group consisting of Ti, Mg, Al, Zr, Y, Ba, Ca, Sr, W, Ta, Nb, and Mo.

15. The positive electrode active material is D 50 The lithium secondary battery according to claim 1, wherein the particle size is 3.0 μm to 8 μm.

16. The lithium secondary battery according to claim 1, wherein the positive electrode conductive material includes a linear conductive material and a point conductive material.

17. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has an energy density of 260 Wh / kg or more.

18. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has a charge cutoff voltage of 4.35V or higher.

19. A battery module comprising the lithium secondary battery described in claim 1.