Secondary batteries
Incorporating alkali metal variscite and functional additives into lithium-ion batteries stabilizes the electrode structure, addressing capacity loss and safety issues by reducing active metal consumption and enhancing performance.
Patent Information
- Application Number
- JP2026528544
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-14
- Filing Date
- 2024-12-12
- Publication Date
- 2026-11-24
AI Technical Summary
Lithium-ion batteries face issues such as decreased capacity and shortened cycle life due to consumption of active metals, large volume changes in the positive electrode, fragmentation of material powder particles, migration and dissolution of transition metal ions, continuous electrolyte depletion, increased SEI film thickness, and internal resistance, leading to degraded cycle performance and safety concerns.
Incorporating alkali metal variscite MAlPO4(OH)x F1-x into the positive and negative electrodes, along with specific functional additives in the electrolyte, to stabilize the electrode structure, suppress side reactions, and improve conductivity and ion transfer.
Enhances battery performance by reducing active metal consumption, preventing dendrite growth, and stabilizing the electrode structure, thereby improving initial efficiency, rate performance, and cycle characteristics.
Smart Images

Figure 2026539352000001 
Figure 2026539352000002 
Figure 2026539352000003
Abstract
Description
[Technical Field]
[0001] This disclosure relates to the technology of lithium-ion batteries, and more specifically to secondary batteries. [Background technology]
[0002] As battery energy density continues to improve, the driving range of mainstream car models now exceeds 400 km, and that of luxury models exceeds 700 km, largely alleviating concerns about the range of electric vehicles. However, compared to the refueling time of gasoline cars, fast charging of electric vehicles remains a bottleneck.
[0003] During its initial charge-discharge cycle, batteries need to consume active metals such as lithium and sodium as an interfacial film forms. Especially when silicon or amorphous carbon is used as the negative electrode, more active metals are consumed, resulting in the battery's actual capacity falling below its design capacity.
[0004] During the battery cycle, problems arise at the positive electrode, such as large volume changes in the unit cell, increased fragmentation of material powder particles, and migration and dissolution of transition metal ions. At the negative electrode, problems occur such as continuous electrolyte depletion, increased SEI film thickness, increased internal resistance, and depletion of active metals. This degrades the battery's cycle performance, accelerating the decrease in specific capacity and energy density. As a result, it leads to a decrease in battery capacity and a shortened cycle life, which has a significant negative impact on safety. [Overview of the Initiative]
[0005] This disclosure aims to provide a secondary battery with high initial efficiency, high rate performance, high voltage, and excellent cycle characteristics. [Means for solving the problem]
[0006] To achieve the above-mentioned objectives of this disclosure, the following technical proposals are adopted.
[0007] The present disclosure provides a secondary battery. The secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte. The positive electrode and / or the negative electrode includes alkali metal variscite MAlPO4(OH) x F 1-x , where 0≦x<1, M is an alkali metal Li or Na. The electrolyte includes a functional additive, and the functional additive is any one selected from compounds having structures represented by Formula I, Formula II, and Formula III.
[0008] [Chemical] R1, R2, and R3 are each independently one selected from a hydrocarbyl group, a hydrocarbyl group substituted with B, N, F, Si, P, S, Cl, Br, or I elements, an alkoxy group, an aryl group, or a heteroaryl group.
[0009] The hydrocarbyl group is C a H 2a+1 , C b H 2b-1 , C c H 2c-3 , where 0<a≦6, 0<b≦6, 0<c≦6.
[0010] The alkoxy group is C a H 2a+1 O, C b H 2b-1 O, C c H 2c-3 O, where 0<a≦6, 0<b≦6, 0<c≦6.
[0011] The aryl group includes any one of a phenyl group, an anthryl group, a naphthyl group, and a biphenyl group.
[0012] The heteroaryl group has 1 to 20 carbon atoms and includes 1 to 3 heteroatoms selected from O, S, P, and N.
[0013] Furthermore, the heteroaryl groups include pyridyl group, indolyl group, pyrrolyl group, imidazolyl group, thienyl group, furyl group, 1,2-thiazolyl group, 1,3-thiazolyl group, 1,2,3-oxadiazolyl group, 1,2,4-oxadiazolyl group, thiadiazolyl group, 1,2,3-triazole group, 1,2,4-triazole group, pyridyl group, pyrazyl group, pyrimidyl group, 1,3,5-triazinyl group, 1,2,4-triazinyl group, and 1,2,3-triazinyl group. It contains one of the following groups: azinyl group, isoindolyl group, benzimidazolyl group, naphthoimidazolyl group, phenanthroimidazolyl group, benzotriazole group, benzoxazolyl group, naphthoxazolyl group, phenanthroxazolyl group, benzothiadiazolyl group, benzotriazole group, quinolyl group, isoquinolyl group, benzopyradyl group, benzothienyl group, benzofuryl group, benzopyrrolyl group, carbazolyl group, or naphthothiadiazolyl group.
[0014] Furthermore, the functional additive is one or more compounds selected from the following:
[0015] [ka]
[0016] Furthermore, the electrolyte solution comprises 0.1 wt% to 20 wt% of an electrolyte salt, 0.1 wt% to 10 wt% of a functional additive, 0.1 wt% to 10 wt% of an auxiliary additive, and 60 wt% to 90 wt% of a solvent.
[0017] Furthermore, the electrolyte salt includes one or more of the following: lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(oxalate)borate, lithium difluoro(oxalato)borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, sodium hexafluorophosphate, sodium tetrafluoroborate, sodium difluorophosphate, sodium bis(oxalate)borate, sodium difluoro(oxalato)borate, sodium bis(trifluoromethanesulfonyl)imide, and sodium bis(fluorosulfonyl)imide.
[0018] The solvent includes one or more mixtures of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, methylpropyl carbonate, γ-butyrolactone, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, ethyl butyrate, and halogenated derivatives thereof.
[0019] The aforementioned auxiliary additive includes one or more of the following: vinylene carbonate, fluoroethylene carbonate, 1,3-propanesultone, 1-propene-1,3-sultone, methylene methanedisulfonate, succinonitrile, adiponitrile, bis(fluorosulfonyl)imide lithium, ethylene sulfate, tris(trimethylsilyl) borate, tris(trimethylsilyl) phosphite, and tris(trimethylsilyl) phosphate.
[0020] Furthermore, the alkali metal varisite is LiAlPO4F, LiAlPO4(OH) 0.9 F 0.1 LiAlPO4(OH) 0.5 F 0.5 NaAlPO4F, NaAlPO4(OH) 0.9 F 0.1 NaAlPO4(OH) 0.5 F 0.5 They are selected from among them.
[0021] Furthermore, the positive electrode comprises a current collector and a positive electrode film piece, the positive electrode film piece being prepared from a positive electrode active material, a conductive agent, a binder, and alkali metal variscite, wherein the alkali metal variscite is present in an amount of 0.1% to 5% by mass relative to the positive electrode film piece.
[0022] Furthermore, the negative electrode comprises a current collector and a negative electrode film piece, the negative electrode film piece being prepared from a negative electrode active material, a conductive agent, a binder, and alkali metal variscite, wherein the alkali metal variscite is present in an amount of 0.1% to 5% by mass relative to the negative electrode film piece.
[0023] Furthermore, the secondary battery is either a lithium-ion battery or a sodium-ion battery. [Modes for carrying out the invention]
[0024] The present disclosure provides a secondary battery in several embodiments. The secondary battery comprises a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode and / or negative electrode is alkali metal varicite MAlPO4(OH) x F 1-x The electrolyte contains , where 0 ≤ x < 1, M is an alkali metal Li or Na, and the electrolyte contains a functional additive, which is selected from compounds having structures represented by formulas I, II, and III.
[0025] [ka]
[0026] R1, R2, and R3 are each independently selected from a hydrocarbyl group, a hydrocarbyl group substituted with elements B, N, F, Si, P, S, Cl, Br, or I, an alkoxy group, an aryl group, or a heteroaryl group.
[0027] In some embodiments of this disclosure, the hydrocarbyl group is C a H 2a+1 , C b H 2b-1 , C c H2c-3 and 0 <a≦6、0<b≦6、0<c≦6である。
[0028] The aforementioned alkoxy group is C a H 2a+1 O, C b H 2b-1 O, C c H 2c-3 O and 0 <a≦6、0<b≦6、0<c≦6である。
[0029] The aforementioned aryl group includes one of the following: a phenyl group, anthryl group, naphthyl group, or biphenyl group.
[0030] The aforementioned heteroaryl group has 1 to 20 carbon atoms and contains 1 to 3 heteroatoms from among O, S, and N.
[0031] In some embodiments of this disclosure, the heteroaryl group is specifically a pyridyl group, an indolyl group, a pyrrolyl group, an imidazolyl group, a thienyl group, a furyl group, a 1,2-thiazolyl group, a 1,3-thiazolyl group, a 1,2,3-oxadiazolyl group, a 1,2,4-oxadiazolyl group, a thiadiazolyl group, a 1,2,3-triazole group, a 1,2,4-triazole group, a pyridyl group, a pyrazyl group, a pyrimidyl group, a 1,3,5-triazinyl group, or a 1,2,4-triazinyl group. It contains one of the following groups: 1,2,3-triazinyl group, isoindolyl group, benzimidazolyl group, naphthoimidazolyl group, phenanthroimidazolyl group, benzotriazole group, benzoxazolyl group, naphthoxazolyl group, phenanthroxazolyl group, benzothiadiazolyl group, benzotriazole group, quinolyl group, isoquinolyl group, benzopyradyl group, benzothienyl group, benzofuryl group, benzopyrrolyl group, carbazolyl group, or naphthothiadiazolyl group.
[0032] In some embodiments of this disclosure, the functional additive is selected from the following specific compounds.
[0033] [ka]
[0034] In some embodiments of the present disclosure, the electrolyte comprises 0.1 wt% to 20 wt% of an electrolyte salt, 0.1 wt% to 10 wt% of a functional additive, 0.1 wt% to 10 wt% of an auxiliary additive, and 60 wt% to 90 wt% of a solvent.
[0035] In some embodiments of this disclosure, the electrolyte contains 0.1 wt% to 20 wt% of an electrolyte salt, which may be 0.1 wt%, 0.5 wt%, 1 wt%, 3 wt%, 5 wt%, 10 wt%, 15 wt%, 20 wt%, or any value between 0.1 wt% and 20 wt%.
[0036] In some embodiments of the present disclosure, the electrolyte salt comprises one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(oxalate)borate, lithium difluoro(oxalato)borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, sodium hexafluorophosphate, sodium tetrafluoroborate, sodium difluorophosphate, sodium bis(oxalate)borate, sodium difluoro(oxalato)borate, sodium bis(trifluoromethanesulfonyl)imide, and sodium bis(fluorosulfonyl)imide.
[0037] In some embodiments of this disclosure, the electrolyte further comprises 0.1 wt% to 10 wt% of a functional additive, which may be 0.1 wt%, 0.5 wt%, 1 wt%, 3 wt%, 5 wt%, 10 wt%, or any value between 0.1 wt% and 10 wt%. The functional additive is selected from the above functional additives.
[0038] In some embodiments of the present disclosure, the electrolyte further comprises 0.1 wt% to 10 wt% of auxiliary additives, which may be 0.1 wt%, 0.5 wt%, 1 wt%, 3 wt%, 5 wt%, 10 wt%, or any value between 0.1 wt% and 10 wt%.
[0039] In some embodiments of this disclosure, the auxiliary additive comprises one or more of the following: vinylene carbonate, fluoroethylene carbonate, 1,3-propanesultone, 1-propene-1,3-sultone, methylene methanedisulfonate, succinonitrile, adiponitrile, lithium bis(fluorosulfonyl)imide, ethylene sulfate, tris(trimethylsilyl) borate, tris(trimethylsilyl) phosphite, and tris(trimethylsilyl) phosphate. This auxiliary additive can form a film on the positive and negative electrodes, thereby suppressing the continuous decomposition of the electrolyte.
[0040] In some embodiments of the present disclosure, the electrolyte further comprises 60 wt% to 90 wt% of a solvent, which may be 60 wt%, 65 wt%, 70 wt%, 75 wt%, 80 wt%, 85 wt%, 90 wt%, or any value between 60 wt% and 90 wt%.
[0041] In some embodiments of the present disclosure, the solvent includes one or more mixtures of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, methylpropyl carbonate, γ-butyrolactone, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, ethyl butyrate, and halogenated derivatives thereof.
[0042] In some embodiments of the present disclosure, the secondary battery further comprises a positive electrode and a negative electrode, wherein the positive electrode and / or negative electrode comprises alkali metal varicite.
[0043] The general formula for the alkali metal varisite is MAlPO4(OH) x F 1-x That is the case.
[0044] Here, 0 ≤ x < 1, and M is an alkali metal, either Li or Na.
[0045] In some embodiments of this disclosure, the alkali metal varisite is LiAlPO4F, LiAlPO4(OH) 0.9 F 0.1 LiAlPO4(OH) 0.5 F 0.5 NaAlPO4F, NaAlPO4(OH) 0.9 F 0.1 NaAlPO4(OH) 0.5 F 0.5 They are selected from among them.
[0046] In some embodiments of the present disclosure, the positive electrode comprises a current collector and a positive electrode film, the positive electrode film being prepared from a positive electrode active material, a conductive agent, a binder, and alkali metal variscite, wherein the alkali metal variscite is present in an amount of 0.1% to 5% by mass relative to the positive electrode film. This could be 0.1%, 0.3%, 0.5%, 1.0%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any value between 0.1% and 5%.
[0047] The negative electrode comprises a current collector and a negative electrode film piece, the negative electrode film piece being prepared from a negative electrode active material, a conductive agent, a binder, and alkali metal variscite, wherein the alkali metal variscite is present in an amount of 0.1% to 5% by mass relative to the negative electrode film piece. It may also be 0.1%, 0.3%, 0.5%, 1.0%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%, and any value between 0.1% and 5%.
[0048] This disclosure does not particularly limit the method for preparing the positive and negative electrodes, and any preparation method well known to those skilled in the art may be used.
[0049] In this disclosure, alkali metal variscite is added to the cathode and anode slurries in the form of a solid or slurry. A solid or non-aqueous slurry is used for the cathode, and a solid or aqueous slurry is used for the anode. After the electrode pieces are dried, the alkali metal variscite is uniformly distributed on the electrode pieces.
[0050] The secondary battery according to this disclosure further includes a separator, and this disclosure does not particularly limit the type of the separator, and a separator well known to those skilled in the art may be used.
[0051] In some embodiments of this disclosure, the secondary battery may be a lithium-ion battery or a sodium-ion battery.
[0052] The secondary battery according to this disclosure improves the battery's rate performance by forming a porous electrode through the dissolution of alkali metal variscite from the positive and negative electrodes by incorporating functional additives -CN and B into the electrolyte, thereby creating voids. The alkali metal aluminum phosphate dissolved from the positive electrode forms AlF, Li3PO4, and Na3PO4 at the positive electrode, stabilizing the electrode structure, suppressing the elution of transition metal ions, and preventing continuous side reactions by the electrolyte. By coating the surface of the positive electrode material with a metal oxide, a physical barrier can be formed, suppressing side reactions, removing HF, preventing chemical erosion by the electrolyte, and reducing the dissolution of transition metals. In addition, it is possible to improve the conductivity of electrons and ions, chemically modify the surface, promote the transfer of ionic charge at the interface, stabilize the structure, and reduce stress due to phase transitions.
[0053] The alkali metal variscite dissolved from the negative electrode forms LiF and NaF at the negative electrode, reducing the consumption of active metals, improving initial efficiency, suppressing dendrite formation, and preventing continuous side reactions by the electrolyte. LiF has low electronic conductivity, a large band gap, high electrochemical stability at the negative electrode, and low Li + Energy barrier of diffusion, high interfacial energy, and Li + SEI has a weak bonding affinity to lithium fluoride (LiF), and because it is rich in lithium fluoride (LiF), it can suppress the growth of dendrites at the negative electrode.
[0054] Further explanation will be provided below with reference to specific examples and comparative examples.
[0055] Example 1 Synthesis of additives: [ka] (1) Pretreatment of raw materials: Tetrahydrofuran was heated and distilled, and dried and dehydrated using metallic sodium to achieve a purity of over 99.9% of tetrahydrofuran and reduce the water content to 50 ppm or less. Triethylamine was heated and fractionally distilled to obtain a colorless and transparent triethylamine solution. Activated 4A molecular sieve was then added to reduce the water content of triethylamine (Et3N) to less than 50 ppm. Activated 4A molecular sieve was added to 2-thienylboronic acid and chloroacetonitrile, respectively, to reduce the water content of 2-thienylboronic acid and chloroacetonitrile to less than 50 ppm.
[0056] (2) The additive preparation reaction according to this example was carried out in a nitrogen gas atmosphere. After filling the reactor with nitrogen gas, 50 mL of tetrahydrofuran was added.
[0057] (3) 0.2 mol of chloroacetonitrile and 0.2 mol of triethylamine were added to the reactor in sequence.
[0058] (4) The reaction system temperature was maintained at 0°C to 5°C, and 0.1 mol of 2-thienylboronic acid was slowly added while constantly stirring, and the mixture was stirred at room temperature for 12 hours.
[0059] (5) The white precipitate of triethylamine hydrochloride was removed by filtration.
[0060] (6) Triethylamine, 2-thienylboronic acid, and tetrahydrofuran, which are low-boiling components in the filtrate, were removed by several vacuum distillations, and after washing, additive A was obtained.
[0061] The product after washing was dissolved in dimethyl sulfoxide (DMSO), and proton nuclear magnetic resonance analysis and structural determination were performed. The result was GC-MS (m / z): calcd.for C8H7BN2O2S[M+1]+, 206.03, found 206.01.
[0062] Making a battery: LiNi 0.6 Co 0.2 Mn 0.2 O2 was selected, and LiNi was used as the positive electrode material. 0.6 Co 0.2 Mn 0.2 O2, LiAlPO4F, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 95.4:2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0063] Artificial graphite was selected as the negative electrode material. Graphite, CMC, carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) as a binder were uniformly mixed in a mass ratio of 95.3:1.3:1.4:2.0 and coated onto a copper foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0064] A ceramic-coated polyethylene (PE) membrane was selected as the separator. Its thickness was 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0065] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and 0.5 wt% of a functional additive was added. [ka] Adding this, the concentration of LiPF6 becomes 1 mol·L -1 Then, 0.5 wt% fluoroethylene carbonate (FEC) was added.
[0066] Example 2 Synthesis of additives: [ka]
[0067] (1) Pretreatment of raw materials: Tetrahydrofuran was heated and distilled, and dried and dehydrated using metallic sodium to achieve a purity of over 99.9% of tetrahydrofuran and reduce the water content to 50 ppm or less. Triethylamine was heated and fractionally distilled to obtain a colorless and transparent triethylamine solution. Activated 4A molecular sieve was then added to reduce the water content of triethylamine (Et3N) to less than 50 ppm. Activated 4A molecular sieve was added to cyclohexen-1-ylboronic acid and chloroacetonitrile, respectively, to reduce the water content of cyclohexen-1-ylboronic acid and chloroacetonitrile to less than 50 ppm.
[0068] (2) The additive preparation reaction according to this example was carried out in a nitrogen gas atmosphere. After filling the reactor with nitrogen gas, 50 mL of tetrahydrofuran was added.
[0069] (3) 0.2 mol of chloroacetonitrile and 0.2 mol of triethylamine were added to the reactor in sequence.
[0070] (4) The reaction system temperature was maintained at 0°C to 5°C, and 0.1 mol of cyclohexen-1-ylboronic acid was slowly added while constantly stirring, and the mixture was stirred at room temperature for 12 hours.
[0071] (5) The white precipitate of triethylamine hydrochloride was removed by filtration.
[0072] (6) Triethylamine, cyclohexen-1-ylboronic acid, and tetrahydrofuran, which are low-boiling components in the filtrate, were removed by several vacuum distillations, and after washing, additive B was obtained.
[0073] The washed product was dissolved in dimethyl sulfoxide (DMSO), and proton nuclear magnetic resonance analysis and structural determination were performed. The results were obtained using GC-MS (m / z): calcd.for C 10 H 13 The result was BN2O2[M+1]+, 204.11, found as 204.14.
[0074] Making a battery: LiNi 0.6 Co 0.2 Mn 0.2 O2 was selected, and LiNi was used as the positive electrode material. 0.6 Co 0.2 Mn 0.2 O2, LiAlPO4(OH) 0.9 F 0.1 Carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 96.4:1:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0075] Artificial graphite was selected as the negative electrode material. Graphite, CMC, carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) as a binder were uniformly mixed in a mass ratio of 95.3:1.3:1.4:2.0 and coated onto a copper foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0076] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0077] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and 0.5 wt% of a functional additive was added. [ka] Adding this, the concentration of LiPF6 becomes 1 mol·L -1 Then, 0.5 wt% of bis(fluorosulfonyl)imide lithium (LiFSI) was added.
[0078] Example 3 Synthesis of additives: [ka]
[0079] (1) Pretreatment of raw materials: Tetrahydrofuran was heated and distilled, and dried and dehydrated using metallic sodium to achieve a purity of over 99.9% of tetrahydrofuran and reduce the water content to 50 ppm or less. Triethylamine was heated and fractionally distilled to obtain a colorless and transparent triethylamine solution. Activated 4A molecular sieve was then added to reduce the water content of triethylamine (Et3N) to less than 50 ppm. Activated 4A molecular sieve was added to phenylboronic acid and chloroacetonitrile, respectively, to reduce the water content of phenylboronic acid and chloroacetonitrile to less than 50 ppm.
[0080] (2) The additive preparation reaction according to this example was carried out in a nitrogen gas atmosphere. After filling the reactor with nitrogen gas, 50 mL of tetrahydrofuran was added.
[0081] (3) 0.2 mol of chloroacetonitrile and 0.2 mol of triethylamine were added to the reactor in sequence.
[0082] (4) The reaction system temperature was maintained at 0°C to 5°C, and 0.1 mol of phenylboronic acid was slowly added while constantly stirring, and the mixture was stirred at room temperature for 12 hours.
[0083] (5) The white precipitate of triethylamine hydrochloride was removed by filtration.
[0084] (6) Triethylamine, phenylboronic acid, and tetrahydrofuran, which are low-boiling components in the filtrate, were removed by several vacuum distillations, and after washing, additive C was obtained.
[0085] The washed product was dissolved in dimethyl sulfoxide (DMSO), and proton nuclear magnetic resonance analysis and structural determination were performed. The results were obtained using GC-MS (m / z): calcd.for C 10The result was H9BN2O2[M+1]+, 200.08, found at 200.12.
[0086] Making a battery: LiNi 0.6 Co 0.2 Mn 0.2 O2 was selected, and LiNi was used as the positive electrode material. 0.6 Co 0.2 Mn 0.2 O2, LiAlPO4(OH) 0.5 F 0.5 Carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 96.9:0.5:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0087] Artificial graphite was selected as the negative electrode material. Graphite, CMC, carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) as a binder were uniformly mixed in a mass ratio of 95.3:1.3:1.4:2.0 and coated onto a copper foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0088] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0089] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and 0.5 wt% of a functional additive was added. [ka] Adding this, the concentration of LiPF6 becomes 1 mol·L -1 Then, 0.5 wt% ethylene sulfate (DTD) was added.
[0090] Example 4 Synthesis of additives: [ka]
[0091] (1) Pretreatment of raw materials: Tetrahydrofuran was heated and distilled, and dried and dehydrated using metallic sodium to achieve a purity of over 99.9% of tetrahydrofuran and reduce the water content to 50 ppm or less. Triethylamine was heated and fractionally distilled to obtain a colorless and transparent triethylamine solution. Activated 4A molecular sieve was then added to reduce the water content of triethylamine (Et3N) to less than 50 ppm. Activated 4A molecular sieve was added to propylboronic acid and chloroacetonitrile, respectively, to reduce the water content of propylboronic acid and chloroacetonitrile to less than 50 ppm.
[0092] (2) The additive preparation reaction according to this example was carried out in a nitrogen gas atmosphere. After filling the reactor with nitrogen gas, 50 mL of tetrahydrofuran was added.
[0093] (3) 0.2 mol of chloroacetonitrile and 0.2 mol of triethylamine were added to the reactor in sequence.
[0094] (4) The reaction system temperature was maintained at 0°C to 5°C, and 0.1 mol of propylboronic acid was slowly added while constantly stirring, and the mixture was stirred at room temperature for 12 hours.
[0095] (5) The white precipitate of triethylamine hydrochloride was removed by filtration.
[0096] (6) Triethylamine, propylboronic acid, and tetrahydrofuran, which are low-boiling components in the filtrate, were removed by several vacuum distillations, and after washing, additive D was obtained.
[0097] The washed product was dissolved in dimethyl sulfoxide (DMSO), and proton nuclear magnetic resonance analysis and structural determination were performed. The results were as follows: GC-MS (m / z): calcd.for C7H 11 The result was BN2O2[M+1]+, 166.09, found at 166.11.
[0098] Sodium-ion battery positive electrode: Na as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2 was selected, and Na was used as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2, NaAlPO4F, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 97.2:0.2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0099] Negative electrode of sodium-ion battery: Hard carbon was selected as the negative electrode material. Hard carbon, sodium carboxymethylcellulose (CMC), carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) were uniformly mixed in a ratio of 95.8:1.4:0.8:2.0 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0100] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0101] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and 0.5 wt% of a functional additive was added. [ka] Adding this, the concentration of LiPF6 becomes 1 mol·L -1 Then, 0.5 wt% of 1-propene-1,3-sultone (PS) was added.
[0102] Example 5 Synthesis of additives: [ka]
[0103] (1) Pretreatment of raw materials: Tetrahydrofuran was heated and distilled, and dried and dehydrated using metallic sodium to achieve a purity of over 99.9% of tetrahydrofuran and reduce the water content to 50 ppm or less. Triethylamine was heated and fractionally distilled to obtain a colorless and transparent triethylamine solution, and activated 4A molecular sieve was added to reduce the water content of triethylamine (Et3N) to less than 50 ppm. Activated 4A molecular sieve was added to 1-methylpyrimidine-4-boronic acid and chloroacetonitrile, respectively, to reduce the water content of 1-methylpyrimidine-4-boronic acid and chloroacetonitrile to less than 50 ppm.
[0104] (2) The additive preparation reaction according to this example was carried out in an inert gas atmosphere. After filling the reactor with inert gas, 50 mL of tetrahydrofuran was added.
[0105] (3) 0.2 mol of chloroacetonitrile and 0.2 mol of triethylamine were added to the reactor in sequence.
[0106] (4) The reaction system temperature was maintained at 0°C to 5°C, and 0.1 mol of 1-methylpyrimidine-4-boronic acid was slowly added while constantly stirring, and the mixture was stirred at room temperature for 12 hours.
[0107] (5) The white precipitate of triethylamine hydrochloride was removed by filtration.
[0108] (6) Low-boiling components including triethylamine, 1-methylpyrimidine-4-boronic acid, and tetrahydrofuran in the filtrate were removed through several rounds of vacuum distillation, and the additive E was obtained after washing.
[0109] The washed product was dissolved in dimethyl sulfoxide (DMSO), and subjected to proton nuclear magnetic resonance analysis and structural determination. The results were GC-MS (m / z): calcd. for C 10 H 16 BN3O2 [M+1]+, 221.13; found 221.08.
[0110] Battery fabrication: Positive electrode of sodium-ion battery: Na was selected as the positive electrode material 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2 was selected, and the positive electrode material Na 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2, NaAlPO4(OH) 0.9 F 0.1 , carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed at a mass ratio of 97.2:0.2:1.3:1.3, and the mixture was coated onto an aluminum foil current collector. It was then dried in an oven and rolled with a roll press to produce the desired positive electrode sheet.
[0111] Negative electrode of sodium-ion battery: Hard carbon was selected as the negative electrode material. Hard carbon, sodium carboxymethyl cellulose (CMC), carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) were uniformly mixed at a ratio of 95.8:1.4:0.8:2.0, and the mixture was coated onto an aluminum foil current collector. It was then dried in an oven and rolled with a roll press to produce the desired negative electrode sheet.
[0112] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al2O3 + 9 μm PE + 2 μm Al2O3. The electrode sheets were assembled into a 2 Ah small soft-pack battery by a lamination method for use in electrolyte tests.
[0113] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and 0.5 wt% of a functional additive was added. [ka] Adding this, the concentration of LiPF6 becomes 1 mol·L -1 Then, 0.5 wt% methylene methanedisulfonate (MMDS) was added.
[0114] Example 6 Sodium-ion battery positive electrode: Na as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2 was selected, and Na was used as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2, NaAlPO4(OH) 0.5 F 0.5 Carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 97.2:0.2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0115] Sodium-ion battery negative electrode: Hard carbon was selected as the negative electrode material, and NaAlPO4(OH) 0.5 F 0.5 Sodium carboxymethylcellulose (CMC), carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) were uniformly mixed in a ratio of 95.7:0.1:1.4:0.8:2.0 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0116] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0117] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and the concentration of NaPF6 was 1 mol·L. -1 This results in a 0.5 wt% functional additive. [ka] This was added, followed by 0.5 wt% vinylene carbonate (VC).
[0118] Comparative Example 1 Making a battery: LiNi 0.6 Co 0.2 Mn 0.2 O2 was selected, and LiNi was used as the positive electrode material. 0.6 Co 0.2 Mn 0.2 O2, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 97.4:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0119] Artificial graphite was selected as the negative electrode material. Graphite, CMC, carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) as a binder were uniformly mixed in a mass ratio of 95.3:1.3:1.4:2.0 and coated onto a copper foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0120] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0121] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and the concentration of LiPF6 was 1 mol·L. -1 Then, 0.5 wt% fluoroethylene carbonate (FEC) was added.
[0122] Comparative Example 2 Sodium-ion battery positive electrode: Na as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2 was selected, and Na was used as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 97.4:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0123] Negative electrode of sodium-ion battery: Hard carbon was selected as the negative electrode material. Hard carbon, sodium carboxymethylcellulose (CMC), carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) were uniformly mixed in a ratio of 95.8:1.4:0.8:2.0 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0124] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0125] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and the concentration of NaPF6 was 1 mol·L. -1 Then, 0.5 wt% vinylene carbonate (VC) was added.
[0126] Comparative Example 3 Making a battery: LiNi 0.6 Co 0.2 Mn 0.2 O2 was selected, and LiNi was used as the positive electrode material. 0.6 Co 0.2 Mn 0.2 O2, LiAlPO4F, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 95.4:2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0127] Artificial graphite was selected as the negative electrode material. Graphite, CMC, carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) as a binder were uniformly mixed in a mass ratio of 95.3:1.3:1.4:2.0 and coated onto a copper foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0128] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0129] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and the concentration of LiPF6 was 1 mol·L. -1 Then, 0.5 wt% fluoroethylene carbonate (FEC) was added.
[0130] Comparative Example 4 Sodium-ion battery positive electrode: Na as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2 was selected, and Na was used as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2, NaAlPO4F, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 97.2:0.2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0131] Negative electrode of sodium-ion battery: Hard carbon was selected as the negative electrode material. Hard carbon, sodium carboxymethylcellulose (CMC), carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) were uniformly mixed in a ratio of 95.8:1.4:0.8:2.0 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0132] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0133] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and the concentration of NaPF6 was 1 mol·L. -1 Then, 0.5 wt% vinylene carbonate (VC) was added.
[0134] Comparative Example 5 LiNi 0.6 Co 0.2 Mn 0.2 O2 was selected, and LiNi was used as the positive electrode material. 0.6 Co 0.2 Mn 0.2 O2, LiAlPO4F, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 95.4:2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0135] Artificial graphite was selected as the negative electrode material. Graphite, CMC, carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) as a binder were uniformly mixed in a mass ratio of 95.3:1.3:1.4:2.0 and coated onto a copper foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0136] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0137] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and 0.5 wt% of a functional additive was added. [ka] Adding this, the concentration of LiPF6 becomes 1 mol·L -1 Then, 0.5 wt% fluoroethylene carbonate (FEC) was added.
[0138] Comparative Example 6 Making a battery: Sodium-ion battery positive electrode: Na as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2 was selected, and Na was used as the positive electrode material. 0.9 Cu 0.22 Fe 0.30 Mn 0.48 O2, NaAlPO4F, carbon nanotubes (CNTs), and polyvinylidene fluoride (PVDF) were uniformly mixed in a mass ratio of 97.2:0.2:1.3:1.3 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired positive electrode piece.
[0139] Negative electrode of sodium-ion battery: Hard carbon was selected as the negative electrode material. Hard carbon, sodium carboxymethylcellulose (CMC), carbon nanotubes (CNTs), and styrene-butadiene rubber (SBR) were uniformly mixed in a ratio of 95.8:1.4:0.8:2.0 and coated onto an aluminum foil current collector. The mixture was then dried in an oven and rolled in a roll press to produce the desired negative electrode piece.
[0140] A ceramic-coated polyethylene (PE) membrane was selected as the separator, with a thickness of 2 μm Al₂O₃ + 9 μm PE + 2 μm Al₂O₃. The electrode pieces were assembled into a 2Ah small soft pack battery using a lamination method and used for electrolyte testing.
[0141] Preparation of electrolyte: In a glove box under an argon gas atmosphere with less than 0.1 ppm of moisture and less than 0.1 ppm of oxygen, ethylene carbonate (EC), propylene carbonate (PC), and dimethyl carbonate (DMC) were uniformly mixed in a mass ratio of 1:1:1, and the concentration of NaPF6 was 1 mol·L. -1 This results in a 0.5 wt% functional additive. [ka] This was added, followed by 0.5 wt% vinylene carbonate (VC).
[0142] Test conditions for lithium-ion batteries: The charge / discharge voltage range is 2.75 to 4.3V, with 1000 cycles at a 2C rate, discharge at a 5C rate, and discharge at a 10C rate.
[0143] For Comparative Examples 1, 3, 5, 1, 2, and 3, tests were conducted using lithium-ion batteries, and the specific results are shown in Table 1.
[0144] Test conditions for sodium-ion batteries: The charge and discharge voltage range of sodium-ion batteries is 1.5 to 4.0V, and they can be discharged for 1000 cycles at a 2C rate, 5C rate, and 10C rate.
[0145] For Comparative Examples 2, 4, and 6, and Examples 4, 5, and 6, tests were conducted using sodium-ion batteries, and the specific results are shown in Table 2.
[0146] [Table 1]
[0147] [Table 2]
[0148] As is clear from Comparative Examples 1 and 3, and Comparative Examples 2 and 4, the electrochemical performance was not significantly improved even when alkali metal variscite was added to the positive and negative electrodes. Also, as is clear from Comparative Examples 1 and 5, the electrochemical performance was not significantly improved even when alkali metal variscite was added to the positive and negative electrodes and only additive B was included in the electrolyte. As is clear from Comparative Examples 2 and 6, the electrochemical performance was not significantly improved even when alkali metal variscite was added to the positive and negative electrodes and only additive -CN was included in the electrolyte. From Comparative Examples 1, 3, 5 and Examples 1, 2, 3 and Comparative Examples 2, 4, 6 and Examples 4, 5, 6, it was confirmed that when alkali metal variscite was added to the positive and negative electrodes and additives B and -CN were simultaneously included in the electrolyte, the initial efficiency, 1000 cycles at 2C rate, 5C rate discharge, 10C rate discharge, and internal resistance were significantly improved in lithium-ion batteries and sodium-ion batteries.
[0149] The secondary battery according to this disclosure comprises a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode and / or negative electrode are alkali metal varicite MAlPO4(OH) x F 1-x The electrolyte contains 0 ≤ x < 1, M is an alkali metal Li or Na, the electrolyte contains a functional additive, the functional additive is selected from compounds having a structure represented by formula I, and R1, R2, and R3 are each independently selected from a hydrocarbyl group, a hydrocarbyl group substituted with element B, N, F, Si, P, S, Cl, Br, I, an alkoxy group, an aryl group, or a heteroaryl group. In this disclosure, the B atom in the functional additive added to the electrolyte is sp 2 In covalent molecules formed by hybrid orbitals, the remaining empty orbitals accept lone pairs of electrons from the outside as Lewis acids, sp 3A tetrahedral complex can be formed by hybrid orbitals. The fluorine atom in alkali metal variscite has strong electronegativity and can form a complex FB with the B atom through the action of the electron cloud. The -CN group in the functional additive added to the electrolyte is an unsaturated group and has electron-withdrawing properties, so it can complex with metal ions to form a complex. The functional additive contains both a cyano group and a B atom, allowing it to bond simultaneously with the fluorine ions and metal ions in the alkali metal variscite, dissociating the alkali metal variscite, increasing its solubility, and dissolving it in the electrolyte. This forms a porous structure on the electrode pieces, and the dissolved alkali metal variscite forms AlF, Li3PO4, and Na3PO4 at the positive electrode and LiF and NaF at the negative electrode under the action of an electric field, resulting in improved initial efficiency, rate performance, and cycle performance of the battery.
[0150] Industrial applicability This disclosure provides a secondary battery. The secondary battery according to this disclosure comprises a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode and / or negative electrode are alkali metal varicite MAlPO4(OH) x F 1-x The electrolyte contains a B-containing functional additive. This improves the battery's initial efficiency, rate performance, and cycle performance.
[0151] Cross-references of related applications This application claims priority based on a Chinese application filed with the China Patent Office on November 14, 2023, with application number 2023115126694, titled "Secondary Battery," all of which are incorporated into this application by reference.
Claims
1. It comprises a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode and / or the negative electrode is alkali metal varicite MAlPO 4 (OH) x F 1-x The electrolyte contains , where 0 ≤ x < 1, M is an alkali metal Li or Na, the electrolyte contains a functional additive, and the functional additive is selected from any one of the compounds having a structure represented by formula I, formula II, or formula III. 【Chemistry 1】 R 1 , R 2 , R 3 Each of these is independently selected from a hydrocarbyl group, a hydrocarbyl group substituted with elements B, N, F, Si, P, S, Cl, Br, or I, an alkoxy group, an aryl group, or a heteroaryl group. A secondary battery characterized by the following features.
2. The hydrocarbyl group is C a H 2a+1 , C b H 2b-1 , C c H 2c-3 , and satisfies 0<a≤6, 0<b≤6, 0<c≤6, The alkoxy group is C a H 2a+1 O, C b H 2b-1 O, C c H 2c-3 O is true, and 0 < a ≤ 6, 0 < b ≤ 6, 0 < c ≤ 6, The aforementioned aryl group includes one of the following: a phenyl group, anthryl group, naphthyl group, or biphenyl group. The aforementioned heteroaryl group has 1 to 20 carbon atoms and contains 1 to 3 heteroatoms from among O, S, P, and N. The secondary battery according to claim 1.
3. The aforementioned heteroaryl groups include pyridyl group, indolyl group, pyrrolyl group, imidazolyl group, thienyl group, furyl group, 1,2-thiazolyl group, 1,3-thiazolyl group, 1,2,3-oxadiazolyl group, 1,2,4-oxadiazolyl group, thiadiazolyl group, 1,2,3-triazole group, 1,2,4-triazole group, pyridyl group, pyrazyl group, pyrimidyl group, 1,3,5-triazinyl group, 1,2,4-triazinyl group, and 1,2,3-triazinyl group. Contains one of the following groups: dinyl group, isoindolyl group, benzimidazolyl group, naphthoimidazolyl group, phenanthroimidazolyl group, benzotriazole group, benzoxazolyl group, naphthoxazolyl group, phenanthroxazolyl group, benzothiadiazolyl group, benzotriazole group, quinolyl group, isoquinolyl group, benzopyradyl group, benzothienyl group, benzofuryl group, benzopyrrolyl group, carbazolyl group, or naphthothiadiazolyl group. The secondary battery according to claim 1.
4. The functional additive is one or more compounds selected from the following: 【Chemistry 2】 The secondary battery according to claim 1.
5. The aforementioned electrolyte is 0.1 wt% to 20 wt% of electrolyte salts, Functional additives in amounts of 0.1 wt% to 10 wt%, 0.1 wt% to 10 wt% of auxiliary additives, Contains 60 wt% to 90 wt% solvent, The secondary battery according to claim 1.
6. The aforementioned electrolyte salt includes one or more of the following: lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(oxalate)borate, lithium difluoro(oxalato)borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, sodium hexafluorophosphate, sodium tetrafluoroborate, sodium difluorophosphate, sodium bis(oxalate)borate, sodium difluoro(oxalato)borate, sodium bis(trifluoromethanesulfonyl)imide, and sodium bis(fluorosulfonyl)imide. The solvent comprises one or more mixtures of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethylmethyl carbonate, methylpropyl carbonate, γ-butyrolactone, methyl formate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, ethyl butyrate, and halogenated derivatives thereof. The aforementioned auxiliary additive includes one or more of the following: vinylene carbonate, fluoroethylene carbonate, 1,3-propanesultone, 1-propene-1,3-sultone, methylene methanedisulfonate, succinonitrile, adiponitrile, bis(fluorosulfonyl)imide lithium, ethylene sulfate, tris(trimethylsilyl) borate, tris(trimethylsilyl) phosphite, and tris(trimethylsilyl) phosphate. The secondary battery according to feature 5.
7. The alkali metal varisite is LiAlPO 4 F, LiAlPO 4 (OH) 0.9 F 0.1 LiAlPO 4 (OH) 0.5 F 0.5 NaAlPO 4 F, NaAlPO 4 (OH) 0.9 F 0.1 NaAlPO 4 (OH) 0.5 F 0.5 Selected from The secondary battery according to claim 1.
8. The positive electrode comprises a current collector and a positive electrode film piece, the positive electrode film piece being prepared from a positive electrode active material, a conductive agent, a binder, and alkali metal variscite, wherein the alkali metal variscite is present in an amount of 0.1% to 5% by mass relative to the positive electrode film piece. The secondary battery according to claim 1.
9. The negative electrode comprises a current collector and a negative electrode film piece, the negative electrode film piece being prepared from a negative electrode active material, a conductive agent, a binder, and alkali metal variscite, wherein the alkali metal variscite is present in an amount of 0.1% to 5% by mass relative to the negative electrode film piece. The secondary battery according to claim 1.
10. The aforementioned secondary battery is either a lithium-ion battery or a sodium-ion battery. The secondary battery according to claim 1.