Resin composition, prepreg and method for manufacturing the same, and laminate and method for manufacturing the same

A resin composition with modified bismaleimide prepolymer and naphthalene bisallyl ether trimer improves thermal and dielectric properties, addressing the limitations of conventional BT substrates for high-performance semiconductor package substrates.

JP2026539355APending Publication Date: 2026-11-24GUANGDONG HINNO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026528934
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-11
Filing Date
2024-09-27
Publication Date
2026-11-24

AI Technical Summary

Technical Problem

Conventional BT substrates face challenges in meeting the requirements for high-performance semiconductor package substrates in the AI era due to issues with thermal expansion coefficient, heat resistance, and dielectric properties.

Method used

A resin composition comprising modified bismaleimide prepolymer, cyanate ester resin, functional resin, and inorganic filler, with a naphthalene bisallyl ether trimer as a modifying agent, is used to produce prepregs and laminates, enhancing thermal and dielectric properties.

Benefits of technology

The composition achieves a low coefficient of thermal expansion, high heat resistance, and excellent dielectric properties, suitable for high-performance semiconductor package substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539355000001
    Figure 2026539355000001
  • Figure 2026539355000002
    Figure 2026539355000002
  • Figure 2026539355000003
    Figure 2026539355000003
Patent Text Reader

Abstract

The present invention relates to a resin composition, a prepreg and a method for producing the same, and a laminate and a method for producing the same. The resin composition comprises parts by mass of 20 to 50 parts of a modified bismaleimide prepolymer, 10 to 40 parts of a cyanate ester resin, 30 to 60 parts of a functional resin, and 50 to 200 parts of an inorganic filler. The raw materials for the modified bismaleimide prepolymer include a bismaleimide resin and a modifier, and the modifier includes a naphthalene bisallyl ether trimer. The cured product of the resin composition has an extremely low coefficient of thermal expansion, excellent high-temperature modulus retention, and extremely high heat resistance, as well as excellent dielectric properties, making it suitable for the manufacture of high-performance semiconductor package substrates.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to the technical field of modified resins, and more particularly to resin compositions, prepregs and methods for producing the same, and laminates and methods for producing the same. [Background technology]

[0002] In recent years, with the miniaturization and multi-functionalization of electronic devices, semiconductor package substrates have also been required to be thinner and more highly integrated. Furthermore, to ensure the reliability of interconnection and mounting, they are required to possess characteristics such as a high glass transition temperature, high elastic modulus, and low thermal expansion coefficient. Additionally, with the advent of the "artificial intelligence (AI)" era, the amount and speed of information processing have increased exponentially, and semiconductor package substrates are increasingly required to have lower dielectric constants and dielectric losses to reduce transmission loss.

[0003] Currently, most semiconductor package substrates use BT substrates, which are a type of resin-based package substrate formed by thermosetting, with bismaleimide (BMI) and cyanate ester resin (triazine A, also known as TA) as the main resin components. However, conventional BT substrates have difficulty meeting the requirements for high-performance substrates in the AI ​​era in terms of thermal expansion coefficient, heat resistance, and dielectric properties. [Overview of the Initiative] [Problems that the invention aims to solve]

[0004] Based on this, in order to overcome the problem that conventional BT substrates have difficulty meeting the requirements for high-performance substrates in the AI ​​era in terms of thermal expansion coefficient, heat resistance, and dielectric properties, it is necessary to provide resin compositions, prepregs and methods for manufacturing the same, as well as laminates and methods for manufacturing the same. [Means for solving the problem]

[0005] The above objectives of the present invention are achieved by the following technical means.

[0006] A first aspect of the present invention is: Modified bismaleimide prepolymer 20 to 50 parts, 10 to 40 parts of cyanate ester resin, 30 to 60 parts of functional resin, and It contains 50 to 200 parts by mass of inorganic filler as raw material. The present invention provides a resin composition comprising a bismaleimide resin and a modifying agent as raw materials for the modified bismaleimide prepolymer, wherein the modifying agent comprises a naphthalene bisallyl ether trimer.

[0007] In one embodiment, the mass ratio of the bismaleimide resin to the naphthalene bisallyl ether trimer in the raw materials for the modified bismaleimide prepolymer is 100:(60~100).

[0008] In one embodiment, the modifying agent further comprises one or more of diallylbisphenol A, diallylbisphenol S, diallylbisphenol F, and bisphenol A bisallyl ether.

[0009] In one embodiment, the bismaleimide resin includes one or more of the following: N,N'-(4,4'-methylenediphenyl)bismaleimide, N,N'-(1,4-phenylene)bismaleimide, N,N'-(4-methyl-1,3-phenylene)bismaleimide, N,N'-m-phenylenebismaleimide, di(4-maleimidophenyl)methane, 2,2-di(4-(4-maleimidophenoxy)-phenyl)propane, di(3,5-dimethyl-4-maleimidophenyl)methane, di(3-ethyl-5-methyl-4-maleimidophenyl)methane, di(3,5-diethyl-4-maleimidophenyl)methane, polyphenylmethanebismaleimide, and bismaleimides containing a biphenyl structure.

[0010] In one embodiment, the method for producing the modified bismaleimide prepolymer is as follows: The process includes the step of heating the modifying agent until it melts, adding the bismaleimide resin, and carrying out a prepolymerization reaction to produce the modified bismaleimide prepolymer.

[0011] In one embodiment, the temperature of the preliminary polymerization reaction is 140°C to 170°C.

[0012] In one embodiment, the duration of the preliminary polymerization reaction is 60 min to 180 min.

[0013] In one embodiment, the cyanate ester resin includes one or more of the following: bisphenol A type cyanate ester resin, novolac type cyanate ester resin, bisphenol F type cyanate ester resin, bisphenol M type cyanate ester resin, bisphenol E type cyanate ester resin, naphthalene type cyanate ester resin, biphenyl type cyanate ester resin, bisphenol S type cyanate ester resin, and dicyclopentadiene bisphenol type cyanate ester resin.

[0014] In one embodiment, the functional resin includes one or more of the following: a benzoxazine resin, a modified polyphenylene ether resin, and a hydrocarbon resin.

[0015] In one embodiment, the benzoxazine resin includes one or more of the following: bisphenol A type benzoxazine resin, bisphenol F type benzoxazine resin, bisphenol S type benzoxazine resin, main chain type benzoxazine resin, phosphorus-containing benzoxazine resin, dicyclopentadiene benzoxazine resin, biphenyl type benzoxazine resin, tetraphenolethane benzoxazine resin, and naphthalene type benzoxazine resin.

[0016] In one embodiment, the modified polyphenylene ether resin has a structure represented by general formula (II), [ka] (II) m and n are each independently a positive integer, and the sum of m and n ranges from 5 to 60, Y is absent or selected from alkylene groups having 1 to 3 carbon atoms.

[0017] In one embodiment, the hydrocarbon resin includes one or more of polybutadiene and styrene-butadiene copolymers.

[0018] In one embodiment, the inorganic filler includes one or more of zirconium vanadate, zirconium tungstate, hafnium tungstate, crystallized glass, eucryptite, silica, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc powder, alumina, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay, and kaolin.

[0019] In one embodiment, the resin composition further includes one or more of a flame retardant, a curing accelerator, a solvent, and an auxiliary agent, and the auxiliary agent includes one or more of a dispersant, a defoaming agent, a leveling agent, a coupling agent, a surfactant, and an ultraviolet absorber.

[0020] A second aspect of the present invention provides a method for producing a prepreg, including the steps of: coating the surface of a reinforcing material with the resin composition, and performing a semi-curing treatment to produce the prepreg.

[0021] In one embodiment, the method of coating the surface of the reinforcing material with the resin composition includes one or more of an immersion method, a padding method, and a coating method.

[0022] In one embodiment, the reinforcing material includes one or more of inorganic fiber materials and organic fiber materials.

[0023] In one embodiment, the temperature of the semi-curing treatment is 120°C to 230°C.

[0024] In one embodiment, the time for the semi-curing treatment is 3 min to 15 min.

[0025] A third aspect of the present invention provides a prepreg whose raw materials include a reinforcing material and the resin composition described above, or a prepreg manufactured by the method for manufacturing the prepreg described above.

[0026] A fourth aspect of the present invention provides a laminate whose raw material includes the above-mentioned prepreg.

[0027] In one embodiment, one or both sides of the laminate are covered with metal foil.

[0028] In one embodiment, the metal foil includes copper foil.

[0029] In one embodiment, the thickness of the metal foil is 3 μm to 105 μm.

[0030] A fifth aspect of the present invention provides a method for manufacturing the laminate, which includes the step of performing a vacuum heat press treatment on the prepreg.

[0031] In one embodiment, the temperature of the vacuum heat press treatment is 150°C to 300°C.

[0032] In one embodiment, the pressure of the vacuum heat press treatment is 10 kgf / cm². 2 ~50 kgf / cm² 2 That is the case.

[0033] In one embodiment, the vacuum level of the vacuum heat press treatment is 2 kPa or less.

[0034] In one embodiment, the time for the vacuum heat press treatment is 200 min to 400 min. [Effects of the Invention]

[0035] The present invention has the following beneficial effects.

[0036] In the resin composition according to the present invention, a modified bismaleimide prepolymer is produced using a bismaleimide resin and a modifying agent containing a naphthalene bisallyl ether trimer. The naphthalene bisallyl ether trimer can introduce multiple high-rigidity naphthalene ring structures into the molecular structure of the modified bismaleimide prepolymer. This not only reduces its structural symmetry and improves the compatibility of the prepolymer with other resins, but is also advantageous for reducing the coefficient of thermal expansion, improving the glass transition temperature, high-temperature modulus, and dielectric properties. By blending the modified bismaleimide prepolymer with components such as cyanate ester resin, functional resin, and inorganic filler in a specific blending ratio, the cured product of the resin composition exhibits an extremely low coefficient of thermal expansion, excellent retention of high-temperature modulus, and extremely high heat resistance, as well as excellent dielectric properties, making it suitable for the manufacture of high-performance semiconductor package substrates. [Modes for carrying out the invention]

[0037] To make the above-mentioned objectives, features, and advantages of the present invention clearer and easier to understand, specific embodiments of the present invention will be described in detail below. The following description includes many specific details to facilitate a full understanding of the present invention. However, the present invention can be implemented in many ways different from those described herein, and those skilled in the art can make similar improvements without contradicting the present invention; therefore, the present invention is not limited to the specific embodiments disclosed below.

[0038] Furthermore, the terms “first” and “second” are used solely for descriptive purposes and should not be understood as indicating or implying relative importance, or implicitly indicating the number of technical features shown. Therefore, features defined as “first” and “second” may explicitly or implicitly include at least one such feature. In the description of this invention, “multiple” means at least two, for example, two, three, etc., unless otherwise specified.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. Terms used herein are for the purpose of describing specific embodiments and do not limit the invention. The terms “and / or” as used herein include any and all combinations of one or more related items.

[0040] BT substrates are a type of resin-based package substrate formed by thermosetting, primarily using bismaleimide (BMI) resin and cyanate ester (TA) resin. They possess properties such as a high glass transition temperature (Tg), excellent dielectric properties, and a low coefficient of thermal expansion (CTE). However, their dielectric properties are not ideal, with a dielectric constant (Dk) of 4.3 and a dielectric loss (dissipation factor (Df) of 0.008, making it difficult to meet the demands of the explosively increasing amount of information processing and processing speed in the AI ​​era.

[0041] On the other hand, bismaleimide resin has excellent heat resistance and thermal stability, low curing shrinkage rate, low coefficient of thermal expansion, and good dielectric properties, making it a commonly used resin matrix for semiconductor package substrates. Unmodified bismaleimide has drawbacks such as low solubility, excessively high curing temperature, excessively high crosslinking density, and excessive brittleness of the cured product due to the high symmetry of its structure, making it difficult to use alone, and it usually becomes usable only after modification. Conventional technology often uses modified bismaleimide resin to manufacture BT substrates, but it has defects such as a high coefficient of thermal expansion, low heat resistance, and high dielectric loss, making it difficult to apply to high-performance integrated circuits in the AI ​​era.

[0042] Based on this, a first aspect of the present invention provides a resin composition that effectively solves the problem that conventional BT substrates have difficulty meeting the requirements for high-performance substrates in the AI ​​era in terms of thermal expansion coefficient, heat resistance, and dielectric properties.

[0043] In some embodiments, the resin composition is Modified bismaleimide prepolymer 20 to 50 parts, 10 to 40 parts of cyanate ester resin, 30 to 60 parts of functional resin, and It contains 50 to 200 parts by mass of inorganic filler as raw material. The raw materials for the modified bismaleimide prepolymer include a bismaleimide resin and a modifying agent, the modifying agent containing a naphthalene bisallyl ether trimer.

[0044] Furthermore, the naphthalene bisallyl ether trimer has a structure represented by general formula (I). [ka] (I)

[0045] In the resin composition according to the present invention, a modified bismaleimide prepolymer is produced using a bismaleimide resin and a modifying agent containing a naphthalene bisallyl ether trimer. The naphthalene bisallyl ether trimer can introduce multiple high-rigidity naphthalene ring structures into the molecular structure of the modified bismaleimide prepolymer. This not only reduces its structural symmetry and improves the compatibility of the prepolymer with other resins, but is also advantageous for reducing the coefficient of thermal expansion, improving the glass transition temperature, high-temperature modulus, and dielectric properties. By blending the modified bismaleimide prepolymer with components such as cyanate ester resin, functional resin, and inorganic filler in a specific blending ratio, the cured product of the resin composition exhibits an extremely low coefficient of thermal expansion, excellent retention of high-temperature modulus, and extremely high heat resistance, as well as excellent dielectric properties, making it suitable for the manufacture of high-performance semiconductor package substrates.

[0046] In the resin composition, the amount of modified bismaleimide prepolymer may be 20, 25, 30, 35, 40, 45, or 50 parts by mass, but is not limited to these amounts. Preferably, the amount of modified bismaleimide prepolymer is 20 to 40 parts by mass. More preferably, in the resin composition, the amount of modified bismaleimide prepolymer is 25 to 35 parts by mass.

[0047] In the resin composition, the cyanate ester resin may be present in amounts of 10, 15, 20, 25, 30, 35, or 40 parts by mass, but is not limited to these amounts. Preferably, the cyanate ester resin is present in amounts of 10 to 30 parts by mass. More preferably, the cyanate ester resin is present in amounts of 15 to 25 parts by mass in the resin composition.

[0048] In the resin composition, the functional resin may include, but is not limited to, 30, 35, 40, 45, 50, 55, or 60 parts by mass. Preferably, the functional resin is 30 to 50 parts by mass. More preferably, the functional resin is 35 to 45 parts by mass.

[0049] In the resin composition, the parts by mass of inorganic filler may include, but are not limited to, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, or 200 parts. Preferably, the parts by mass of inorganic filler is 80 to 160 parts. More preferably, the parts by mass of inorganic filler is 100 to 140 parts.

[0050] Preferably, the resin composition is Modified bismaleimide prepolymer 20 to 40 parts, 10 to 30 parts of cyanate ester resin, 30 to 50 parts of functional resin, and It contains 80 to 160 parts by mass of inorganic filler as raw material.

[0051] More preferably, the resin composition is 25 to 35 parts of modified bismaleimide prepolymer, 15 to 25 parts of cyanate ester resin, 35 to 45 parts of functional resin, and It contains 100 to 140 parts by mass of inorganic filler as raw material.

[0052] Preferably, in the raw materials for the modified bismaleimide prepolymer, the mass ratio of the bismaleimide resin to the naphthalene bisallyl ether trimer is 100:(60~100), for example, 100:60, 100:65, 100:70, 100:75, 100:80, 100:85, 100:90, 100:95, or 100:100. By controlling the mass ratio of the bismaleimide resin to the naphthalene bisallyl ether trimer, the naphthalene ring content in the modified bismaleimide prepolymer can be controlled, thereby improving its compatibility, thermal expansion coefficient, glass transition temperature, and dielectric properties.

[0053] Furthermore, when modifying bismaleimide resin with a modifying agent, naphthalene bisallyl ether trimer can be used alone or in combination with conventional bismaleimide resin modifying agents, and the mixing ratio is not particularly limited.

[0054] Furthermore, the denaturing agent further comprises one or more of the following: diallylbisphenol A, diallylbisphenol S, diallylbisphenol F, and bisphenol A bisallyl ether. Preferably, the denaturing agent is at least one selected from the group consisting of a combination of naphthalene bisallyl ether trimer and diallylbisphenol A, a combination of naphthalene bisallyl ether trimer and diallylbisphenol S, a combination of naphthalene bisallyl ether trimer and diallylbisphenol F, and a combination of naphthalene bisallyl ether trimer and diallylbisphenol F.

[0055] The bismaleimide resin is selected from organic compounds containing at least two maleimide groups in its molecular structure. Preferably, the bismaleimide resin includes one or more of the following: N,N'-(4,4'-methylenediphenyl)bismaleimide, N,N'-(1,4-phenylene)bismaleimide, N,N'-(4-methyl-1,3-phenylene)bismaleimide, N,N'-m-phenylenebismaleimide, di(4-maleimoidphenyl)methane, 2,2-di(4-(4-maleimoidphenoxy)-phenyl)propane, di(3,5-dimethyl-4-maleimoidphenyl)methane, di(3-ethyl-5-methyl-4-maleimoidphenyl)methane, di(3,5-diethyl-4-maleimoidphenyl)methane, polyphenylmethanebismaleimide, and bismaleimides containing a biphenyl structure.

[0056] In some embodiments, the method for producing a modified bismaleimide prepolymer includes the steps of heating a modifying agent until it melts, adding a bismaleimide resin, and carrying out a prepolymerization reaction to produce a modified bismaleimide prepolymer.

[0057] Selectively, the temperature at which the denaturing agent is heated until it melts is between 100°C and 150°C, including but not limited to 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, and 150°C. Preferably, the temperature at which the denaturing agent is heated until it melts is between 100°C and 130°C.

[0058] Selectively, the temperature of the prepolymerization reaction is 140°C to 170°C, including but not limited to 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, and 170°C. Preferably, the temperature of the prepolymerization reaction is 140°C to 160°C. More preferably, the temperature of the prepolymerization reaction is 145°C to 155°C.

[0059] Selectively, the process further includes a step of cooling to room temperature after the prepolymerization reaction.

[0060] Selectively, the prepolymerization reaction time is 60 min to 180 min, including but not limited to 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, and 180 min. Preferably, the prepolymerization reaction time is 80 min to 150 min. More preferably, the prepolymerization reaction time is 90 min to 120 min.

[0061] In some embodiments, the cyanate ester resin includes one or more of the following: bisphenol A type cyanate ester resin, novolac type cyanate ester resin, bisphenol F type cyanate ester resin, bisphenol M type cyanate ester resin, bisphenol E type cyanate ester resin, naphthalene type cyanate ester resin, biphenyl type cyanate ester resin, bisphenol S type cyanate ester resin, and dicyclopentadiene bisphenol type cyanate ester resin.

[0062] In some embodiments, the functional resin includes one or more of benzoxazine resins, modified polyphenylene ether resins, and hydrocarbon resins.

[0063] Hydrocarbon resins have excellent dielectric properties and are widely used in the field of electronic equipment. However, due to their flexibility and non-polar carbon chain structure, cured products lack rigidity, have low strength, poor heat resistance, and a low glass transition temperature, and also have poor compatibility with strongly polar bismaleimide resins. Polyphenylene ether (PPO) resins have a molecular structure that contains numerous benzene rings and lacks strongly polar groups, resulting in excellent properties such as a high glass transition temperature, a low coefficient of linear expansion, a low dielectric constant, and low dielectric loss. By modifying polyphenylene ether resins, unsaturated groups such as alkenyl groups, alkynyl groups, or acrylate groups can be introduced to improve compatibility and reduce melt viscosity. Benzoxazine resin is an organic compound containing a six-membered oxazine ring in its molecular structure. It has high heat resistance, a glass transition temperature of 150°C or higher, near-zero curing shrinkage, good flame retardancy, low water absorption, good elastic modulus, and low dielectric constant, but it is highly brittle and has a high curing temperature.

[0064] In the functional resins described above, the dielectric properties, from best to worst, are hydrocarbon resins, modified polyphenylene ether resins, and benzoxazine resins. By combining functional resins with different components, the number of polar groups in the cured resin composition can be significantly reduced, thereby effectively improving its dielectric properties.

[0065] The functional resin may be just one selected from the group consisting of benzoxazine resin, modified polyphenylene ether resin, and hydrocarbon resin, or it may be at least two selected from the group consisting of benzoxazine resin, modified polyphenylene ether resin, and hydrocarbon resin. Preferably, the functional resin includes benzoxazine resin and modified polyphenylene ether resin.

[0066] Selectively, the benzoxazine resin includes one or more of the following: bisphenol A type benzoxazine resin, bisphenol F type benzoxazine resin, bisphenol S type benzoxazine resin, main chain type benzoxazine resin, phosphorus-containing benzoxazine resin, dicyclopentadiene benzoxazine resin, biphenyl type benzoxazine resin, tetraphenolethane benzoxazine resin, and naphthalene type benzoxazine resin.

[0067] Selectively, modified polyphenylene ether resins have a structure represented by general formula (II). [ka] (II) In the formula, m and n are both positive integers, and the sum of m and n is between 5 and 60. Y is either absent or selected from alkylene groups having 1 to 3 carbon atoms.

[0068] Selectively, the hydrocarbon resin comprises one or more of polybutadiene and styrene-butadiene copolymers. Preferably, the hydrocarbon resin is polybutadiene.

[0069] In some embodiments, the inorganic filler includes one or more of the following: zirconium vanadate, zirconium tungstate, hafnium tungstate, crystallized glass, eucryptite, silica, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc powder, alumina, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay, and kaolin. Here, silica may be at least one of spherical silica, fused silica, and composite silica. Preferably, the inorganic filler is spherical silica.

[0070] By adding an appropriate inorganic filler to the resin composition, a synergistic effect with the modified maleimide prepolymer is achieved, resulting in a significant reduction in the thermal expansion coefficient of the resin composition.

[0071] In some embodiments, the resin composition further comprises one or more of a flame retardant, a curing accelerator, a solvent, and an auxiliary agent, the auxiliary agent comprising one or more of a dispersant, an antifoaming agent, a leveling agent, a coupling agent, a surfactant, and an ultraviolet absorber.

[0072] Adding flame retardants improves the flame retardancy of the resin composition. Adding curing accelerators lowers the curing temperature of the resin composition, improves the curing speed, and reduces the difficulty of processing the resin composition. Adding solvents improves the compatibility between multiple components, preventing defects such as delamination and precipitation. Adding auxiliary agents improves the dispersibility, fluidity, uniformity, and bonding ability between different components of the resin composition, further improving the curability of the resin composition and enhancing the various properties of the cured product.

[0073] Selectively, the resin composition is Flame retardant 10 to 40 units, 1 to 10 parts of hardening accelerator, 50 to 150 parts of solvent, and It contains 1 to 5 parts by mass of raw materials as an auxiliary agent.

[0074] In the resin composition, the amount of flame retardant may be 10, 15, 20, 25, 30, 35, or 40 parts by mass, but is not limited to these amounts. Preferably, the amount of flame retardant is 10 to 30 parts by mass. More preferably, the amount of flame retardant is 15 to 25 parts by mass.

[0075] In the resin composition, the parts by mass of the curing accelerator may be 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts, but is not limited to these amounts. Preferably, the parts by mass of the curing accelerator is 2 to 8 parts. More preferably, the parts by mass of the curing accelerator is 4 to 6 parts.

[0076] In the resin composition, the amount of solvent may be 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, or 150 parts by mass, but is not limited to these amounts. Preferably, the amount of solvent is 80 to 120 parts by mass. More preferably, the amount of solvent is 90 to 110 parts by mass.

[0077] In the resin composition, the amount of the additive may be 1, 2, 3, 4, or 5 parts by mass, but is not limited to these amounts. Preferably, the amount of the additive is 2 to 4 parts by mass. More preferably, the amount of the additive is 3 parts by mass.

[0078] Selectively, the flame retardant includes one or more halogen-containing flame retardants and non-halogen flame retardants. The halogen-containing flame retardants include one or more ethylenebispentabromophenyl, decabromodiphenylethane, tetrabromobisphenol A, ethylenebistetrabromoimide, and tetradecabromodiphenoxybenzene, while the non-halogen flame retardants include one or more phosphazene compounds, phosphate ester compounds, bisdiphenylphosphine oxide compounds, and phosphinate compounds.

[0079] Selectively, the curing accelerator includes one or more of the following: tertiary amine accelerators, imidazole accelerators, peroxide accelerators, organophosphorus accelerators, and transition metal carboxylate accelerators. Tertiary amine accelerators include, but are not limited to, tris(dimethylaminomethyl)phenol, triethylenediamine, and dimethylaniline; imidazole accelerators include, but are not limited to, 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole; peroxide accelerators include, but are not limited to, dicumyl peroxide, tert-butyl peroxybenzoate, and tert-butyl peroxyoctoate; and transition metal carboxylate accelerators include, but are not limited to, cobalt acetylacetonate, nickel acetylacetonate, and zinc acetylacetonate. Organophosphorus accelerators include, but are not limited to, triphenylphosphine.

[0080] Selectively, the solvent comprises one or more of the following: ethanol, acetone, cyclohexanone, methyl ethyl ketone, toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, and propylene glycol monomethyl ether. Preferably, the solvent comprises methyl ethyl ketone, toluene, and propylene glycol monomethyl ether. More preferably, in the solvent, the mass ratio of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether is 1:1:1.

[0081] Selectively, the coupling agent includes one or more of the following: silane coupling agents, titanate coupling agents, and zirconate coupling agents. Preferably, the coupling agent is a silane coupling agent.

[0082] A second aspect of the present invention provides a method for producing a prepreg using the above-mentioned resin composition.

[0083] In some embodiments, the method for producing a prepreg includes the steps of coating the surface of a reinforcing material with the resin composition and performing a semi-curing treatment to produce a prepreg.

[0084] Prepregs, also known as semi-cured sheets, are compositions of resin matrix / reinforcement materials formed by combining a resin matrix with reinforcing materials (continuous fibers, woven fabrics, or chopped strands), and represent one form of material used to manufacture advanced composite components.

[0085] Selectively, the method for coating the surface of the reinforcing material with the resin composition includes one or more of the following: immersion, padding, and coating. Preferably, the method for coating the surface of the reinforcing material with the resin composition is immersion.

[0086] Selectively, the reinforcing material includes one or more types of inorganic fiber materials and organic fiber materials. Inorganic fiber materials include one or more types of glass fibers, carbon fibers, silicon carbide fibers, and asbestos fibers, and glass fibers include one or more types of E-type glass fibers, NE-type glass fibers, D-type glass fibers, S-type glass fibers, and T-type glass fibers. Organic fiber materials include one or more types of nylon fibers, polyethylene fibers, aramid fibers, polyimide fibers, polyester fibers, and cotton fibers, and polyethylene fibers include one or more types of high-density polyethylene (HDPE) fibers, low-density polyethylene (LDPE) fibers, linear low-density polyethylene (LLDPE) fibers, and ultra-high molecular weight polyethylene (UHMWPE) fibers.

[0087] Selectively, the semi-curing temperature is 120°C to 230°C, including but not limited to 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, and 230°C. Preferably, the semi-curing temperature is 140°C to 180°C. More preferably, the semi-curing temperature is 150°C to 170°C.

[0088] Selectively, the semi-curing time is 3 min to 15 min, including but not limited to 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, and 15 min. Preferably, the semi-curing time is 3 min to 10 min. More preferably, the semi-curing time is 4 min to 8 min.

[0089] A third aspect of the present invention provides a prepreg whose raw materials include a reinforcing material and the resin composition described above, or a prepreg manufactured by the method for manufacturing the prepreg described above.

[0090] A fourth aspect of the present invention provides a laminate containing the above-mentioned prepreg.

[0091] Furthermore, in the raw materials for laminated boards, the number of prepregs may be one or more.

[0092] Selectively, one or both sides of the laminate are covered with metal foil.

[0093] Selectively, the metal foil includes copper foil. Selectively, the thickness of the metal foil is 3 μm to 105 μm, including, but not limited to, 3 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, and 105 μm.

[0094] A fifth aspect of the present invention provides a method for manufacturing the laminate, which includes the step of performing a vacuum heat press treatment on the prepreg.

[0095] Selectively, the temperature for vacuum hot pressing is 150°C to 300°C, including, but not limited to, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, and 300°C.

[0096] Selectively, the pressure for vacuum heat pressing is 10 kgf / cm². 2~50 kgf / cm 2 , including but not limited to 10 kgf / cm 2 , 20 kgf / cm 2 , 30 kgf / cm 2 , 40 kgf / cm 2 , 50 kgf / cm 2 .

[0097] Optionally, the vacuum degree of the vacuum hot pressing treatment is ≤ 2 kPa, including but not limited to 2 kPa, 1.5 kPa, 1 kPa, 0.5 kPa, 0.2 kPa, 0.1 kPa, 0.05 kPa, 0.02 kPa, 0.01 kPa, and 0.001 kPa.

[0098] Optionally, the duration of the vacuum hot pressing treatment is 200 min to 400 min, including but not limited to 200 min, 220 min, 240 min, 260 min, 280 min, 300 min, 320 min, 340 min, 360 min, 380 min, and 400 min. [Examples]

[0099] [0000366]The present invention will be described in more detail below with reference to specific examples.

[0100] In the following specific examples and comparative examples, unless otherwise specified, the raw materials used are all commercially available products, the equipment used is all commercially available products, and the processes used are all well known to those skilled in the art unless otherwise specified. The sources of some of the raw materials are as follows.

[0101] Naphthalene bis-allyl ether trimer is available from Shanghai Kungang New Material Technology Co., Ltd. Bismaleimide resin is purchased from Daiwa Kasei Co., Ltd., with model number BMI-5100 and chemical name bis(3-ethyl-5-methyl-4-maleimidophenyl)methane. The bisphenol A type cyanate ester resin was purchased from the Lonza Group, and its model number is BA-230S. The modified polyphenylene ether resin was purchased from Savic, and its model number is SA9000. Polybutadiene was purchased from Soda Chemical, and its model number is B1000. The flame retardant was purchased from Daihachi Chemical Industry Co., Ltd., its model number is PX-200, and it is an organophosphate ester-based non-halogen flame retardant. The spherical silica was purchased from Admatex Co., Ltd., and its model number is SO-E6. Diallylbisphenol A will be purchased from Honghu Shuangma Resin Plant. Dicumyl peroxide will be purchased from Domyo Chemical. The auxiliary agent was purchased from Dow Corning, its model number is Z-6011, and it is a silane coupling agent.

[0102] <Example 1> (1) Preparation of modified bismaleimide prepolymer: As shown in Table 1, take 60 parts by mass of naphthalene bisallyl ether trimer, heat to molten state at 120°C, add 100 parts of bismaleimide resin, carry out a prepolymerization reaction at 150°C, cool to room temperature after 90 min to obtain a modified bismaleimide prepolymer, which is designated as prepolymer A.

[0103] [Table 1]

[0104] (2) Preparation of the resin composition: As shown in Table 2, 20 parts by mass of prepolymer A, 10 parts by mass of bisphenol A type cyanate ester resin, 15 parts by mass of modified polyphenylene ether resin, 15 parts by mass of polybutadiene, and 10 parts by mass of flame retardant were dissolved in 80 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 80 parts by mass of spherical silica, 1 part by mass of an auxiliary agent, and 1 part by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0105] [Table 2]

[0106] (3) Production of prepreg: 2116 type glass fiber cloth was immersed in the resin composition and placed in a hot air circulating oven, baked at 160°C for 5 minutes to obtain a semi-cured sheet (i.e., prepreg).

[0107] (4) Manufacturing of laminates: A laminate was obtained by laminating eight semi-cured sheets. One sheet of electrolytic copper foil with a thickness of 12 μm was coated on both the top and bottom surfaces of the laminate, and it was placed in a vacuum press machine capable of programmed temperature and pressure control, under a vacuum of 2 kPa or less and a pressure of 28 kgf / cm². 2 Under pressure, a 0.8 mm thick copper-clad laminate was manufactured by vacuum heat pressing at 180°C for 2 hours, followed by vacuum heat pressing at 220°C for 2 hours.

[0108] <Example 2> (1) Preparation of the modified bismaleimide prepolymer: Same as in Example 1, i.e., prepolymer A.

[0109] (2) Preparation of the resin composition: As shown in Table 2, 30 parts by mass of prepolymer A, 20 parts by mass of bisphenol A type cyanate ester resin, 20 parts by mass of modified polyphenylene ether resin, 20 parts by mass of polybutadiene, and 20 parts by mass of flame retardant were dissolved in 100 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 120 parts by mass of spherical silica, 3 parts by mass of auxiliary agent, and 5 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0110] (3) Manufacturing of prepreg: Same as in Example 1.

[0111] (4) Manufacturing of laminates: Same as in Example 1.

[0112] <Example 3> (1) Preparation of the modified bismaleimide prepolymer: Same as in Example 1, i.e., prepolymer A.

[0113] (2) Preparation of the resin composition: As shown in Table 2, 40 parts by mass of prepolymer A, 30 parts by mass of bisphenol A type cyanate ester resin, 25 parts by mass of modified polyphenylene ether resin, 25 parts by mass of polybutadiene, and 30 parts by mass of flame retardant were dissolved in 120 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 160 parts by mass of spherical silica, 5 parts by mass of auxiliary agent, and 10 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0114] (3) Manufacturing of prepreg: Same as in Example 1.

[0115] (4) Manufacturing of laminates: Same as in Example 1.

[0116] <Example 4> (1) Preparation of modified bismaleimide prepolymer: As shown in Table 1, take 100 parts by mass of naphthalene bisallyl ether trimer, heat to molten state at 120°C, add 100 parts of bismaleimide resin, carry out a prepolymerization reaction at 150°C, cool to room temperature after 120 min to obtain a modified bismaleimide prepolymer, which is designated as prepolymer B.

[0117] (2) Preparation of the resin composition: As shown in Table 2, 30 parts by mass of prepolymer B, 15 parts by mass of bisphenol A type cyanate ester resin, 20 parts by mass of modified polyphenylene ether resin, 20 parts by mass of polybutadiene and 20 parts by mass of flame retardant were dissolved in 100 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 120 parts by mass of spherical silica, 3 parts by mass of auxiliary agent and 5 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0118] (3) Manufacturing of prepreg: Same as in Example 1.

[0119] (4) Manufacturing of laminates: Same as in Example 1.

[0120] <Example 5> (1) Preparation of modified bismaleimide prepolymer: As shown in Table 1, take 80 parts by mass of naphthalene bisallyl ether trimer, heat to molten state at 120°C, add 100 parts of bismaleimide resin, carry out a prepolymerization reaction at 150°C, cool to room temperature after 100 min to obtain a modified bismaleimide prepolymer, which is designated as prepolymer C.

[0121] (2) Preparation of the resin composition: As shown in Table 2, 30 parts by mass of prepolymer C, 20 parts by mass of bisphenol A type cyanate ester resin, 20 parts by mass of modified polyphenylene ether resin, 20 parts by mass of polybutadiene, and 20 parts by mass of flame retardant were dissolved in 100 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 120 parts by mass of spherical silica, 3 parts by mass of auxiliary agent, and 5 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0122] (3) Manufacturing of prepreg: Same as in Example 1.

[0123] (4) Manufacturing of laminates: Same as in Example 1.

[0124] <Example 6> (1) Preparation of modified bismaleimide prepolymer: As shown in Table 1, take 60 parts by mass of naphthalene bisallyl ether trimer and 20 parts by mass of diallylbisphenol A, heat to 130°C until molten, add 100 parts of bismaleimide resin, carry out a prepolymerization reaction at 150°C, and after 120 minutes cool to room temperature to obtain a modified bismaleimide prepolymer, which is designated as prepolymer D.

[0125] (2) Preparation of the resin composition: As shown in Table 2, 30 parts by mass of prepolymer C, 40 parts by mass of bisphenol A type cyanate ester resin, 20 parts by mass of modified polyphenylene ether resin, 20 parts by mass of polybutadiene, and 20 parts by mass of flame retardant were dissolved in 100 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 120 parts by mass of spherical silica, 3 parts by mass of auxiliary agent, and 5 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0126] (3) Manufacturing of prepreg: Same as in Example 1.

[0127] (4) Manufacturing of laminates: Same as in Example 1.

[0128] <Comparative Example 1> (1) Preparation of modified bismaleimide prepolymer: As shown in Table 1, 80 parts by mass of diallylbisphenol A are taken and heated to a molten state at 100°C, 100 parts of bismaleimide resin are added, a prepolymerization reaction is carried out at 150°C, and after 120 minutes it is cooled to room temperature to obtain a modified bismaleimide prepolymer, which is designated as prepolymer E.

[0129] (2) Preparation of the resin composition: As shown in Table 2, 30 parts by mass of prepolymer C, 20 parts by mass of bisphenol A type cyanate ester resin, 20 parts by mass of modified polyphenylene ether resin, 20 parts by mass of polybutadiene, and 20 parts by mass of flame retardant were dissolved in 100 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene, and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 120 parts by mass of spherical silica, 3 parts by mass of auxiliary agent, and 5 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0130] (3) Manufacturing of prepreg: Same as in Example 1.

[0131] (4) Manufacturing of laminates: Same as in Example 1.

[0132] <Comparative Example 2> (1) Preparation of the resin composition: As shown in Table 2, 30 parts by mass of unmodified bismaleimide resin, 20 parts by mass of bisphenol A type cyanate ester resin, 20 parts by mass of modified polyphenylene ether resin, 20 parts by mass of polybutadiene and 20 parts by mass of flame retardant were dissolved in 100 parts by mass of solvent (a mixture of methyl ethyl ketone, toluene and propylene glycol monomethyl ether in a mass ratio of 1:1:1) to obtain a mixture. Under stirring conditions, 120 parts by mass of spherical silica, 3 parts by mass of an auxiliary agent and 5 parts by mass of dicumyl peroxide were added to the mixture and stirred until uniformly mixed to obtain a gel-like resin composition.

[0133] (2) Prepreg manufacturing: Same as in Example 1.

[0134] (3) Manufacturing of laminates: Same as in Example 1.

[0135] <Example Test> The following tests were conducted on the above-mentioned resin composition and laminate, and the results are shown in Table 3. (1) Resin compatibility: After standing for 1 day, visually observe for the presence or absence of precipitation or delamination. (2) Peel strength: The test method shall be in accordance with IPC-TM-6502.4.8. (3) Glass transition temperature (Tg) and high-temperature modulus: Test in accordance with IPC-TM650 2.4.25D. (4) Coefficient of thermal expansion (XYZ-CTE): Test in accordance with IPC-TM650 2.4.24. (5) Dielectric properties test: Test in accordance with IPC-TM650 2.5.5.2. (6) Flame retardancy level: Test in accordance with IPC-TM650 2.3.10.

[0136] [Table 3]

[0137] As can be seen from Table 3, in Comparative Example 2, an unmodified bismaleimide resin was used, resulting in precipitation in the resin composition, poor compatibility between different resins, and poor performance in all aspects of the laminate produced using this resin composition. In Comparative Example 1, diallylbisphenol A, a conventional modifier, was used to modify the prepolymer E produced by diallylbisphenol A, and the compatibility between the prepolymer E and other resins was good, and the peel strength was also significantly improved. However, the glass transition temperature, high-temperature modulus, coefficient of thermal expansion, and dielectric properties were only slightly improved, and the requirements for a high-performance package substrate could not be met.

[0138] The composition of Example 2 is basically the same as that of Comparative Examples 1 and 2, the only difference being the use of a modified bismaleimide prepolymer obtained by prepolymerizing bismaleimide resin and naphthalene bisallyl ether trimer. Compared to Comparative Example 2, the modified bismaleimide prepolymer of Example 2 not only has better compatibility but also shows a very significant improvement in peel strength, glass transition temperature, high-temperature modulus, thermal expansion coefficient, and dielectric properties. Compared to Comparative Example 1, Example 2 showed a slight decrease in peel strength, but the glass transition temperature and high-temperature modulus were clearly improved, the thermal expansion coefficient was clearly reduced, and it also had a lower dielectric constant and dielectric loss. This indicates that by using naphthalene bisallyl ether trimer as a modifier, various properties of the resin composition such as thermal expansion coefficient, high-temperature modulus, heat resistance, and dielectric properties can be significantly improved, and as a result the laminate has an extremely low thermal expansion coefficient, excellent retention of high-temperature modulus, extremely high heat resistance, extremely low dielectric constant, and dielectric loss, making it very suitable for the manufacture of high-performance semiconductor package substrates.

[0139] The technical features of the embodiments described above can be combined in any way, and for the sake of brevity, not all possible combinations of the technical features in the embodiments described above have been described. However, as long as these combinations of technical features are inconsistent, they should be considered to fall within the scope described herein.

[0140] The embodiments described above merely illustrate some of the embodiments of the present invention, and while a more specific and detailed description is available, it does not limit the scope of the claims. Furthermore, those skilled in the art can make some modifications and improvements without departing from the spirit of the present invention, and all of these fall within the scope of protection of the present invention. Therefore, the scope of patent protection for the present invention is determined by the attached claims, and the specification is intended to explain the content of those claims.

Claims

1. 20 to 50 parts of modified bismaleimide prepolymer, 10 to 40 parts of cyanate ester resin, 30 to 60 parts of functional resin, and It contains 50 to 200 parts by mass of inorganic filler as raw material. The resin composition is characterized in that the raw materials for the modified bismaleimide prepolymer include a bismaleimide resin and a modifier, wherein the modifier includes a naphthalene bisallyl ether trimer.

2. The resin composition according to claim 1, characterized in that, in the raw materials for the modified bismaleimide prepolymer, the mass ratio of the bismaleimide resin to the naphthalene bisallyl ether trimer is 100:(60-100).

3. The resin composition according to claim 2, characterized in that the modifying agent further comprises one or more of diallylbisphenol A, diallylbisphenol S, diallylbisphenol F, and bisphenol A bisallyl ether.

4. The resin composition according to claim 1, characterized in that the bismaleimide resin comprises one or more of the following: N,N'-(4,4'-methylenediphenyl)bismaleimide, N,N'-(1,4-phenylene)bismaleimide, N,N'-(4-methyl-1,3-phenylene)bismaleimide, N,N'-m-phenylenebismaleimide, di(4-maleimidophenyl)methane, 2,2-di(4-(4-maleimidophenoxy)-phenyl)propane, di(3,5-dimethyl-4-maleimidophenyl)methane, di(3-ethyl-5-methyl-4-maleimidophenyl)methane, di(3,5-diethyl-4-maleimidophenyl)methane, polyphenylmethanebismaleimide, and bismaleimides containing a biphenyl structure.

5. The method for producing the modified bismaleimide prepolymer is as follows: The resin composition according to any one of claims 1 to 4, characterized in that it includes the step of heating the modifying agent until it melts, adding the bismaleimide resin, and carrying out a prepolymerization reaction to produce the modified bismaleimide prepolymer.

6. The method for producing the modified bismaleimide prepolymer is as follows: (1) The temperature of the prepolymerization reaction is 140°C to 170°C, (2) The resin composition according to claim 5, characterized in that it satisfies one or more of the conditions that the time of the prepolymerization reaction is 60 min to 180 min.

7. The resin composition according to any one of claims 1 to 4, characterized in that the cyanate ester resin comprises one or more of the following: bisphenol A type cyanate ester resin, novolac type cyanate ester resin, bisphenol F type cyanate ester resin, bisphenol M type cyanate ester resin, bisphenol E type cyanate ester resin, naphthalene type cyanate ester resin, biphenyl type cyanate ester resin, bisphenol S type cyanate ester resin, and dicyclopentadiene bisphenol type cyanate ester resin.

8. The resin composition according to any one of claims 1 to 4, characterized in that the functional resin comprises one or more of the following: a benzoxazine resin, a modified polyphenylene ether resin, and a hydrocarbon resin.

9. The aforementioned functional resin is (1) The benzoxazine resin includes one or more of the following: bisphenol A type benzoxazine resin, bisphenol F type benzoxazine resin, bisphenol S type benzoxazine resin, main chain type benzoxazine resin, phosphorus-containing benzoxazine resin, dicyclopentadiene benzoxazine resin, biphenyl type benzoxazine resin, tetraphenolethane benzoxazine resin, and naphthalene type benzoxazine resin. (2) The modified polyphenylene ether resin has a structure represented by general formula (II), 【Chemistry 1】 (II) In the formula, m and n are both positive integers, and the sum of m and n is between 5 and 60. Y is either absent or selected from alkylene groups having 1 to 3 carbon atoms. (3) The resin composition according to claim 8, characterized in that the hydrocarbon resin satisfies one or more of the conditions that it contains one or more of polybutadiene and styrene-butadiene copolymers.

10. The resin composition according to any one of claims 1 to 4, characterized in that the inorganic filler includes one or more of the following: zirconium vanadate, zirconium tungstate, hafnium tungstate, crystallized glass, eucryptite, silica, mica powder, titanium dioxide, magnesium oxide, magnesium hydroxide, talc powder, alumina, silicon carbide, boron nitride, aluminum nitride, molybdenum oxide, barium sulfate, zinc molybdate, zinc borate, zinc stannate, zinc oxide, strontium titanate, barium titanate, calcium titanate, clay, and kaolin.

11. The resin composition according to any one of claims 1 to 4, further comprising one or more of a flame retardant, a curing accelerator, a solvent, and an auxiliary agent, wherein the auxiliary agent comprises one or more of a dispersant, an antifoaming agent, a leveling agent, a coupling agent, a surfactant, and an ultraviolet absorber.

12. A method for producing a prepreg, comprising the step of coating the surface of a reinforcing material with the resin composition described in any one of claims 1 to 11 and performing a semi-curing treatment to produce the prepreg.

13. (1) The method of coating the surface of the reinforcing material with the resin composition includes one or more of the dipping method, padding method and coating method, (2) The reinforcing material includes one or more types of inorganic fiber materials and organic fiber materials, (3) The temperature of the semi-curing treatment is 120°C to 230°C. (4) The method for producing a prepreg according to 12, characterized in that the time for the semi-curing treatment satisfies one or more of the conditions of 3 min to 15 min.

14. A prepreg characterized in that its raw materials include a reinforcing material and a resin composition according to any one of claims 1 to 11, or is manufactured by a method for manufacturing a prepreg according to claim 12 or 13.

15. A laminate characterized in that the raw material includes the prepreg described in claim 14.

16. The laminate according to claim 15, characterized in that one or both sides of the laminate are covered with metal foil.

17. (1) The metal foil includes copper foil, (2) The laminate according to claim 16, characterized in that the thickness of the metal foil satisfies one or more of the conditions of 3 μm to 105 μm.

18. A method for manufacturing a laminate according to any one of claims 15 to 17, characterized by including the step of performing a vacuum heat press treatment on the prepreg.

19. The aforementioned vacuum heat pressing process is (1) The temperature of the vacuum heat press treatment is 150°C to 300°C, (2) The pressure of the vacuum heat press treatment is 10 kgf / cm 2 ~50 kgf / cm² 2 And, (3) The vacuum level of the vacuum heat press treatment is ≤ 2 kPa, (4) The method for manufacturing a laminate according to 18, characterized in that one or more of the conditions that the time of the vacuum heat press treatment is 200 min to 400 min are met.