Curable composition and its cured product
A curable composition with urethane (meth)acrylate, thiocarboxylic acid derivative, and triallyl isocyanurate addresses the issues of adhesion and transparency in image display devices, achieving high light transmittance and low haze in cured products.
Patent Information
- Application Number
- JP2019060238
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-03-27
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2039-03-27
AI Technical Summary
Conventional resin compositions used in image display devices do not adequately consider light transmittance and clear visibility, and they lack sufficient adhesion to substrates, limiting the quality of transparent cured products.
A curable composition comprising urethane (meth)acrylate, thiocarboxylic acid derivative, triallyl isocyanurate, and a photopolymerization initiator, with specific mass ratios, to achieve high adhesion, suppressed haze, and high total light transmittance.
The composition results in a highly transparent cured product with excellent adhesion to substrates, maintaining high light transmittance and low haze, even under harsh conditions.
Smart Images

Figure 0007551278000003 
Figure 0007551278000005 
Figure 0007551278000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable composition, for example a curable composition used in the production of transparent displays or adhesives, and a cured product thereof. [Background technology]
[0002] With the recent progress in image forming technology, the image quality of electronic devices such as liquid crystal displays and touch panels has improved remarkably. In order to improve the reproducibility of such high-quality images, it is also desired to improve the quality of the screens of image display devices. That is, in order to enable the image display device to reproduce high-quality moving images and still images with high accuracy, it is essential that the display and its adhesives have excellent transparency, that is, be colorless and transparent.
[0003] In order to obtain a cured resin having high transparency that meets such requirements, an active energy ray-curable resin composition using a photocurable component and specific inorganic particles has been proposed (Patent Document 1). In this document, the haze is controlled as an index of transparency, and a curable composition with excellent transparency is obtained. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-242681 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] There is a demand for transparent cured products of curable compositions used in screens of image display devices etc. to enable brighter and clearer visibility of images. However, while conventional resin compositions such as those shown in Patent Document 1 have a certain degree of transparency, they do not consider light transmittance, and therefore do not necessarily provide sufficient clear visibility of images. In addition, in the manufacture of electronic devices, the curable composition is required to adhere well to the main body (substrate, etc.) of the electronic device. Under such circumstances, there is still room for improvement in conventional resin compositions in terms of maintaining the quality under specified usage conditions and adhesion to the substrate.
[0006] An object of the present invention is to provide a curable composition capable of forming a cured product having excellent adhesion to a substrate, as well as high total light transmittance and well-controlled haze, and a cured product thereof. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted intensive research in light of the above and have found that the above-mentioned problems can be solved by a curable composition comprising (A) a urethane (meth)acrylate, (B) a thiocarboxylic acid derivative, (C) triallyl isocyanurate, and (D) a photopolymerization initiator, the curable composition being characterized in that the curable composition contains 50 parts by mass or more of the (B) thiocarboxylic acid derivative per 100 parts by mass of the (A) urethane (meth)acrylate and 40 parts by mass or more of the (C) triallyl isocyanurate per 100 parts by mass of the (A) urethane (meth)acrylate, and have thus completed the present invention.
[0008] In the curable composition of the present invention, the total mass of (A) the urethane (meth)acrylate, (B) the thiocarboxylic acid derivative, and (C) triallyl isocyanurate is preferably 95% or more of the total mass of the curable composition.
[0009] The object of the present invention is also achieved by a transparent cured product obtained from the curable composition of the present invention. Effect of the Invention
[0010] The curable composition of the present invention has high adhesion to a substrate. Furthermore, by curing the curable composition of the present invention, a highly transparent cured product having reduced haze and high total light transmittance can be obtained. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a schematic diagram showing a plate having recesses used for producing a molded product of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a state in which recesses in a plate are filled with the photocurable composition of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing a process in which a substrate is placed over a plate and ultraviolet light is irradiated from a light source positioned above the substrate. [Figure 4] FIG. 2 is a schematic diagram showing a state in which the substrate and the molded product have been released from the plate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The curable composition of the present invention is a curable composition comprising (A) a urethane (meth)acrylate, (B) a thiocarboxylic acid derivative, (C) triallyl isocyanurate, and (D) a photopolymerization initiator, and is characterized in that the curable composition comprises 40 parts by mass or more of the thiocarboxylic acid derivative (B) per 100 parts by mass of the urethane (meth)acrylate (A), and 50 parts by mass or more of the triallyl isocyanurate (C) per 100 parts by mass of the urethane (meth)acrylate (A). The curable composition of the present invention has excellent adhesion to substrates, and the cured product thereof has high light transmittance and reduced haze, thereby exhibiting excellent transparency and transmittance.
[0013] In the present invention, haze is used as an index of transparency. Haze is the degree of cloudiness, and indicates the degree of transparency of transparent materials such as glass, plastics, and liquids, and is expressed as a percentage of the scattered light transmittance of a test piece divided by the total light transmittance. Therefore, the smaller the value, the less scattered light transmittance there is, and the less haze there is in the material. In the present invention, transmittance (total light transmittance) is used as an index of transparency. Transmittance is the ratio of the amount of transmitted light to the amount of light incident on the material to be measured, and is obtained as a value taking into account reflection on the material surface and absorption inside the material. In the present invention, the haze is measured in accordance with JIS-K-7136:2000, and "transparent" or "highly transparent" means that the haze is less than 5%, preferably less than 1%. Furthermore, in the present invention, the total light transmittance is measured by the method of JIS K7361-1, and the transmittance is high (excellent transmittance). is transparent This means that the rate is 99.0% or higher. Each component will be described in detail below.
[0014] [(A) Urethane (meth)acrylate] The curable composition of the present invention contains (A) a urethane (meth)acrylate. In this specification, the term "(meth)acrylate" is used as a general term for acrylate and methacrylate, and includes either or both of acrylate and methacrylate. The same applies to other similar expressions. The urethane (meth)acrylate resin can be produced, for example, by synthesizing a urethane prepolymer from a polyol and a polyisocyanate, and then adding a (meth)acrylate having a hydroxyl group thereto. Examples of the polyol that can be used include known polyols such as hydrocarbon polyols, polyether polyols, polyester polyols, polycarbonate polyols, etc. Examples of the polyisocyanates that can be used include known polyisocyanates such as aromatic polyisocyanates, aliphatic polyisocyanates, aromatic aliphatic polyisocyanates, alicyclic polyisocyanates, etc. The curable composition of the present invention contains (A) urethane (meth)acrylate, which provides adhesion of the curable composition to a substrate, and further provides flexibility to the cured coating film obtained by curing the curable composition, thereby suppressing the possibility of peeling from the substrate. If the number of (meth)acryloyl functional groups is too large, the crosslinking density increases, which tends to cause the cured product to warp more and to have poor toughness, so bifunctional or trifunctional ones are preferred.
[0015] In the present invention, a urethane resin having two (meth)acryloyl groups is particularly preferably used. Furthermore, the weight average molecular weight of the bifunctional urethane (meth)acrylate is preferably in the range of 1500 to 20000. When the weight average molecular weight of the bifunctional urethane (meth)acrylate is 1500 or more, the curing shrinkage of the bifunctional urethane (meth)acrylate is reduced, and the cured product is less likely to warp. On the other hand, when the weight average molecular weight of the bifunctional urethane (meth)acrylate is 20000 or less, the viscosity is improved, and the handling property in the preparation of the composition is improved.
[0016] Commercially available examples of bifunctional urethane (meth)acrylates include U-108A, U-200AX, UA-112P, UA-5201, U-340AX, UA-511, UA-512, UA-311, UA-412A, UA-4200, UA-4400, UA-340P, UA-2235PE, UA-160TM, UA-6100, U-108, UA-4000, UA-122P, UA-5201, UA-512, UA-W2, UA-7000, U-2PPA, and UA-NDP manufactured by Shin-Nakamura Chemical Co., Ltd.; and CN962, CN963, CN964, CN965, CN980, CN981, CN982, and C manufactured by Sartomer. N983, CN996, CN9001, CN9002, CN9788, CN9893, CN978, CN9782, CN9783; M-1100, M-1200, M-1210, M-1310, M-1600 manufactured by Toagosei Chemical Industry; Art Resin UN-9000PEP, UN-9200A, UN-7600, UN-333, UN-1255, UN-6060PTM, UN-6060P, SH-500B manufactured by Negami Chemical Industry; AH-600, AT-600 manufactured by Kyoeisha Chemical; Ebecryl 280, Ebecryl 284, Ebecryl 402, Ebecryl 8402, Ebecryl 9270 manufactured by Daicel-Allnex, etc.
[0017] Commercially available examples of trifunctional urethane (meth)acrylates include Ebecryl 4513, Ebecryl 4740, KRM8296, Ebecryl 8296, and Ebecryl 8311 manufactured by Daicel-Allnex Corporation.
[0018] The (A) urethane (meth)acrylate may be one of the above-mentioned compounds or a combination of two or more of them.
[0019] The amount of the urethane (meth)acrylate (A) used is preferably within a range from 30 to 40% by mass, and particularly preferably from 34 to 36% by mass, based on the total mass of the curable composition. By using the urethane (meth)acrylate (A) in the above proportions, the adhesion of the curable composition to a substrate to which it is applied and the flexibility of the cured coating film are improved.
[0020] [(B) Thiocarboxylic acid derivatives] The curable composition of the present invention contains (B) a thiocarboxylic acid derivative in an amount of 50 parts by mass or more, preferably in the range of 60 to 120 parts by mass, per 100 parts by mass of (A) the urethane (meth)acrylate. In the present invention, the inclusion of the thiocarboxylic acid derivative (B) can improve the light transmittance of the cured coating film. The thiocarboxylic acid derivative (B) may be used alone or in combination of two or more kinds.
[0021] (B) Thiocarboxylic acid derivatives include [ka] Examples of the compound include compounds having 1 to 6 groups represented by the following formula: Specific examples thereof include linear or branched compounds such as β-mercaptopropionic acid, 2-ethylhexyl-3-mercaptopropionate, n-octyl-3-mercaptopropionate, methoxybutyl-3-mercaptopropionate, stearyl-3-mercaptopropionate, trimethylolpropane tris(3-mercaptopropionate)propionate, pentaerythritol tetrakis(3-mercaptopropionate), and tetraethylene glycol bis(3-mercaptopropionate), and mercaptopropionic acid derivatives including compounds having a cyclic structure such as tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, of which tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate is particularly preferably used in the present invention.
[0022] The amount of the thiocarboxylic acid derivative (B) used is preferably in the range of 25 to 40% by mass, particularly preferably 30 to 38% by mass, based on the total mass of the curable composition. By using an amount of the (B) thiocarboxylic acid derivative of 25 mass % or more, a sufficient light transmittance of the cured coating film can be obtained, and by using an amount of the (B) thiocarboxylic acid derivative of 40 mass % or less, the curable composition can have better adhesion to the substrate than the urethane (meth)acrylate alone.
[0023] [(C) Triallyl isocyanurate] The curable composition of the present invention contains (C) triallyl isocyanurate in an amount of 40 parts by mass or more, preferably in the range of 45 to 95 parts by mass, per 100 parts by mass of (A) urethane (meth)acrylate. Generally, triallyl isocyanurate acts as a crosslinking aid and as an adhesion imparting agent in the curable composition when added in a small amount of about 10 mass % to the curable composition; however, in the present invention, by using 40 parts by mass or more of (C) triallyl isocyanurate, the haze value of the cured coating film can be reduced, the light transmittance can be increased, and heat resistance can also be imparted. The amount of (C) triallyl isocyanurate used is preferably in the range of 20 to 40% by mass, particularly preferably 24 to 33% by mass, based on the total mass of the curable composition. By using (C) triallyl isocyanurate in an amount of 20 mass % or more, it is possible to obtain a cured coating film with sufficient hardness, and by using it in an amount of 40 mass % or less, the transparency and light transmittance become particularly good and heat resistance can also be imparted.
[0024] [(D) Photopolymerization initiator] The curable composition of the present invention contains (D) a photopolymerization initiator. Examples of the photopolymerization initiator that can be used include benzoins such as benzoin, benzil, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; benzoin alkyl ethers; benzophenone, p-methylbenzophenone, Michler's ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone; acetophenone, α- Acetophenones such as hydroxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, N,N-dimethylaminoacetophenone; thioxanthones such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; anthraquinone, chloroanthraquinone, 2-methylanthraquinone, anthraquinones such as anthraquinone, 2-ethyl anthraquinone, 2-tert-butyl anthraquinone, 1-chloro anthraquinone, 2-amyl anthraquinone, and 2-amino anthraquinone; ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoic acid esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethyl benzoate, and p-dimethylbenzoic acid ethyl ester; phenyl disulfide 2-nitrofluorene, butyroin, anisoin ethyl ether, azobisisobutyronitrile, and tetramethylthiuram disulfide.
[0025] The above (D) photopolymerization initiators can be used alone or in combination of two or more. In order to improve the surface characteristics without impairing the flexibility of the cured product, it is preferable to use an α-hydroxyacetophenone-based photopolymerization initiator.
[0026] The photopolymerization initiator (D) is added in an amount of preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, based on 100 parts by mass of the urethane (meth)acrylate (A). .
[0027] The total mass of the above-mentioned (A) urethane (meth)acrylate, (B) thiocarboxylic acid derivative, and (C) triallyl isocyanurate is preferably 95% or more of the total mass of the curable composition, thereby obtaining the properties of high total light transmittance and well-suppressed haze.
[0028] For viscosity adjustment, a known and commonly used diluent, particularly a reactive diluent, can be used. In particular, a monofunctional (meth)acrylate compound, which is a compound having one ethylenically unsaturated group in the molecule, is preferred because of its high dilution effect.
[0029] [Other ingredients] The curable composition of the present invention may contain other components in addition to the above-mentioned components, provided that the effects of the present invention are not impaired. Examples of additives that may be blended include photocurable monomers, silicone-based and fluorine-based defoamers, leveling agents, known and commonly used thermal polymerization inhibitors, ultraviolet absorbers, silane coupling agents, plasticizers, foaming agents, flame retardants, antistatic agents, antioxidants, antibacterial and antifungal agents, etc.
[0030] The curable composition of the present invention may contain a thermosetting component as long as the desired properties are not impaired, but generally does not use a thermosetting component, which results in a cured product with better transparency and light transmittance and less change over time.
[0031] The curable composition of the present invention has high adhesion to a substrate, and therefore can be bonded to the substrate easily and reliably, and can also improve the durability of the device or part to which it is bonded.
[0032] [Method of curing the curable composition] The curable composition of the present invention, which is composed of the above-mentioned components, can be photocured to form a cured product. For curing, the curable composition is applied to a substrate such as quartz glass, and then irradiated with active energy rays to cure. The curable composition of the present invention preferably has a viscosity of 1 to 50 dPa·s.
[0033] The coating method may be any of the following: dip coating, flow coating, bar coating, and screen printing. As the light source for irradiating the active energy rays, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, or a metal halide lamp is suitable. In addition, UV-LED, laser beams, electron beams, and the like can also be used as the active energy rays.
[0034] [Method of curing and molding the curable composition] Here, a method is illustrated with the aid of drawings, in which a plate having recesses on its surface is used, the recesses are filled with the curable composition of the present invention, the filled curable composition is cured by ultraviolet light, and the cured product is removed from the recesses to obtain a molded product.
[0035] Fig. 1 shows a plate (1) having a recess (2) on its surface. Generally, a plate made of metal such as stainless steel is used.
[0036] 2 shows the plate in a state (3) where the plate is filled with the curable composition of the present invention. In general, the curable composition is filled into the recesses of the plate using a doctor knife or the like.
[0037] 3 shows a process in which the curable composition of the present invention is cured by covering the substrate (4) from above and irradiating ultraviolet light from a light source (5) above the substrate (4). Generally, a transparent film made of polyethylene terephthalate or polycarbonate that transmits ultraviolet light is used as the substrate (4).
[0038] Fig. 4 shows the state in which the cured product is released from the plate (1) to obtain a cured molded product (6). The series of steps from Fig. 1 to Fig. 4 can be carried out continuously by using a dedicated known device for each step.
[0039] In this way, the curable composition of the present invention can be molded in advance and used. In the molding method in which the composition is filled in the recesses and then photocured, there is no inhibition of curing by oxygen, so the thickness can be increased, and it is possible to make the composition as thick as 5 mm at its thickest point. The curable composition of the present invention can be used for transparent screens such as touch panels, and as insulating materials such as solder resists, interlayer insulating materials, and coverlays. The curable composition of the present invention may also be used as a solder dam. Furthermore, since the composition of the present invention has good adhesion, it can also be used as an adhesive, particularly a colorless and transparent adhesive used for transparent screens, etc. EXAMPLES
[0040] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the following examples, and "parts" and "%" described below are all based on mass unless otherwise specified.
[0041] [Example 1~ 8, 10, Reference example 9, and Comparative Examples 1 to 3] Each of the components shown in Table 1 below was kneaded in the amount of parts shown for each component in Table 1 using a planetary centrifugal mixer to prepare each of the curable compositions. The resulting curable compositions were evaluated as follows.
[0042] 1. Printability evaluation Example 1 8, 10, Reference example 9, The curable compositions of Comparative Examples 1 to 3 were printed over the entire surface of a quartz glass substrate using a screen printing device equipped with a 300 mesh printing plate made of polyester (Tetron (registered trademark)) so that the film thickness after curing would be 10 μm. The surface condition of the coating film was visually observed 5 minutes after printing and evaluated according to the following criteria. The results are shown in Table 1.
[0043] The entire surface of the substrate is coated smoothly and uniformly with the curable composition. ×: Traces of burst bubbles are observed on the surface of the curable composition, and the coating surface is uneven.
[0044] 2. Evaluation of dryness to the touch (tack evaluation) Example 1 8, 10, Reference example 9, The curable compositions of Comparative Examples 1 to 3 were printed on the entire surface of a quartz glass substrate using a screen printing device equipped with a 300 mesh printing plate made of polyester (Tetron (registered trademark)). The resulting coating film was then exposed to 1000 mJ / cm 2 using a metal halide lamp. 2 The coating film was cured by exposing it to light at an amount of light of 10 μm. The coating film thus obtained (film thickness: 10 μm) was used as a cured film for evaluation and was evaluated according to the following criteria. The results are shown in Table 1.
[0045] ◎ When you touch the coating film with your fingers, your fingerprints will not be left on the surface of the coating film, and the coating film will not stick to your fingers. ○ When you touch the coating with your finger, your fingerprints will be left on the surface of the coating, but the coating will not stick to your finger. × When the coating film is touched with a finger, a fingerprint is left on the surface of the coating film, and the coating film also adheres to the finger.
[0046] 3. Pencil hardness evaluation A cured film similar to the one used in 2. Evaluation of dryness to the touch above was prepared, and its surface hardness was measured using a pencil hardness tester (manufactured by Toyo Seiki Seisakusho Co., Ltd.). In this test, 3H and 4H pencils, sharpened so that the tip is flat, were pressed against each test piece at an angle of about 45° with a load of 1 kg, and moved at least 7 mm at a speed of 0.5 to 1 mm / s, and the state of peeling of the coating film was evaluated according to the following criteria. The results are shown in Table 1.
[0047] ◎ No peeling of the coating with a 4H pencil 〇 No peeling of the coating with a 3H pencil × The paint peels off when using a 3H pencil.
[0048] 4. Adhesion evaluation The adhesion of the cured coating film (10 μm thick) similar to that used in the pencil hardness evaluation above was evaluated by a cross-cut tape peel ring test in accordance with JIS K 5600-5-6, in which cross-cuts were made in a 10 mm x 10 mm grid pattern using a cross-cut guide to form 100 x 100 grids. The number of remaining grids was visually observed according to the following criteria. The results are shown in Table 1.
[0049] ○ No peeling at all in the grid pattern of the coating × Peeling was observed in one or more grids of the coating film.
[0050] 5. Total light transmittance evaluation For the same cured coating film (film thickness 10 μm) used in 3. Pencil hardness evaluation above, the total light transmittance was measured in accordance with JIS K 7361-1 using a UV-visible spectrophotometer V-670EX (manufactured by JASCO Corporation). In this evaluation, the ratio of transmitted light to incident light over the entire wavelength range of 300 to 780 nm used in the evaluation is shown. The measurement results are shown in Table 1.
[0051] 6. Haze rating The same cured coating film (film thickness 10 μm) as that used in 3. Pencil hardness evaluation above was measured using a UV-visible spectrophotometer V-670EX (manufactured by JASCO Corporation) in accordance with JIS K 7136. As described in JIS K 7136, haze is a value expressed as a percentage of the scattered light transmittance of a test piece divided by the total light transmittance, and the total light transmittance value was determined in accordance with JIS K 7361-1. The measurement results are shown in Table 1.
[0052] 7. Heat resistance test (total light transmittance and haze evaluation after heat treatment) 7-1. Preparation of heat-treated samples A cured coating film similar to that used in the above 3. Pencil hardness evaluation was stored in a hot air circulating drying oven at 100° C. for 2 hours to prepare a heat-treated sample. 7-2. Total light transmittance and haze evaluation of heat-treated samples The total light transmittance and haze value of the heat-treated sample thus obtained were determined by the same measurement methods as those in 5. Total Light Transmittance Evaluation and 6. Haze (Cloud Value) Evaluation described above. The measurement results are shown in Table 1.
[0053] 8. Endurance light Property test (total light transmittance and haze evaluation after exposure processing) 8-1. Preparation of exposure-processed samples The same hardened coating film as that used in the pencil hardness evaluation above was exposed to a metal halide lamp at 20 J / cm 2 An exposure-treated sample was prepared by performing full-surface exposure with a light amount of 10 .... 8-2. Evaluation of total light transmittance and haze of exposed samples The total light transmittance and haze value of the thus obtained exposed sample were determined by the same measuring methods as those in 5. Total Light Transmittance Evaluation and 6. Haze (Cloud Value) Evaluation described above. The measurement results are shown in Table 1.
[0054] [Table 1]
[0055] Details of the materials listed in the table are given below. Ebecryl 8402: Bifunctional urethane acrylate, photocurable urethane resin, manufactured by Daicel-Allnex Corporation TAIC: Triallyl isocyanurate , manufactured by Mitsubishi Chemical Corporation TEMPIC: Tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, manufactured by SC Organic Chemicals Co., Ltd. Omnirad® 184: 1-hydroxycyclohexyl-phenyl ketone, IGM Resins KBM-5103: 3-acryloxypropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. Light Ester P-1M: Mono(2-hydroxyethyl methacrylate) phosphate, manufactured by Kyoeisha Chemical Co., Ltd. FLORENE AC-2300C: Olefin polymer (defoamer), manufactured by Kyoeisha Chemical Co., Ltd. Polyflow KL-700: Silicone-containing polymer (substrate wetting agent), manufactured by Kyoeisha Chemical Co., Ltd.
[0056] From the above, it is evident that the curable composition of the present invention has excellent printability, and the cured product thereof has excellent physical properties in terms of dryness to touch, pencil hardness and adhesion. Furthermore, the cured product of the present invention has an initial light transmittance, and a heat resistance test and Lightfastness The haze value was also high, at 99.0% or more after the heat resistance test and after the heat resistance test. Lightfastness Since the change in color was suppressed to 1.5% or less in both cases after the durability test exposure, it is clear that the film is particularly suited as a transparent protective material for LCD displays, touch panels, etc., and that the film will retain its beautiful initial colorless and transparent state even after long-term harsh use.
[0057] The present invention is not limited to the configurations and examples of the above-described embodiment, and various modifications are possible within the scope of the gist of the invention. [Explanation of symbols]
[0058] 1... version 2. Recess 3...Photocurable composition 4...Base material 5...Light source 6...Molded products
Claims
1. (A) urethane (meth)acrylate, (B) a thiocarboxylic acid derivative, (C) triallyl isocyanurate, and (D) a photopolymerization initiator, A curable composition comprising: The (B) thiocarboxylic acid derivative is tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, (B) 50 parts by mass or more of the thiocarboxylic acid derivative per 100 parts by mass of the (A) urethane (meth)acrylate, The composition contains 40 parts by mass or more of the (C) triallyl isocyanurate relative to 100 parts by mass of the (A) urethane (meth)acrylate, The amount of the urethane (meth)acrylate (A) used is 30 to 40% by mass based on the total mass of the curable composition, The curable composition, wherein the amount of the thiocarboxylic acid derivative (B) used is 25 to 40 mass % based on the total mass of the curable composition.
2. The curable composition according to claim 1, wherein a total mass of the urethane (meth)acrylate (A), the thiocarboxylic acid derivative (B), and the triallyl isocyanurate (C) is 95% or more of a total mass of the curable composition.
3. A transparent cured product obtained from the curable composition according to claim 1 or 2.
Citation Information
Patent Citations
Actinically fixable mass and its use
DE102018102916A1
Curable composition
JP1981067333A
The liquid crystal droplets dispersed in the polymer matrix and the manufacturing method and device manufactured therefrom
JP1990502834A
Optical shaping resin composition
JP1991210364A
Liquid crystal injection port-sealant and liquid crystal display cell
JP1999095233A