Galvanic nickel or nickel alloy electroplating bath for depositing semi-bright nickel or semi-bright nickel alloy coatings
A modified nickel electroplating bath using acetylene compounds and reduced chloral hydrate addresses the challenges of achieving good gloss, leveling, and low stress in nickel coatings, offering stable and cost-effective semi-bright nickel alloy deposition.
Patent Information
- Application Number
- JP2021560982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-15
- Filing Date
- 2020-04-14
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2040-04-14
AI Technical Summary
Existing nickel electroplating baths struggle to achieve a combination of good gloss properties, low internal stress, and effective leveling without producing high internal stress values, and often require costly and time-consuming processes to remove harmful decomposition products.
A modified galvanic nickel or nickel alloy electroplating bath comprising specific acetylene compounds and reduced chloral hydrate concentration, along with other additives, to deposit semi-bright nickel or semi-bright nickel alloy coatings with improved gloss and leveling properties while minimizing internal stress and cracks.
The modified bath achieves semi-bright nickel coatings with excellent gloss and leveling, low internal stress, and minimal cracks, providing stability and cost-effectiveness by reducing chloral hydrate usage.
Smart Images

Figure 0007551647000006 
Figure 0007551647000001 
Figure 0007551647000004
Abstract
Description
[Technical field]
[0001] The present invention relates to galvanic nickel or nickel alloy electroplating baths and methods for depositing semi-bright nickel or semi-bright nickel alloy coatings on conductive workpieces. The present invention is further directed generally to the use of such galvanic nickel or nickel alloy electroplating baths for depositing semi-bright nickel or semi-bright nickel alloy coatings by practicing the methods of the present invention. [Background technology]
[0002] Bright nickel electroplating baths are used in the automotive, electrical, appliance, hardware and other industries. The most important function of bright nickel plating is as an undercoat for chrome plating, helping the finisher achieve a smooth, bright finish and providing a significant amount of corrosion protection.
[0003] For decorative plated parts requiring a high level of base metal corrosion protection, Semi-bright nickel deposits are most often used in combination with subsequent bright nickel and chromium deposits. The Semi-bright nickel deposit is typically about 60-70% of the total nickel deposited on the part, which provides the highest level of base metal corrosion protection, minimizes total nickel thickness, and provides the best appearance.
[0004] Typically, a workpiece, particularly a metal substrate, is covered by a semi-bright nickel deposit, which is covered by a bright nickel deposit, which is covered by a chromium outer deposit.
[0005] The most common nickel electroplating baths are sulfate baths, also known as Watts baths. In addition, organic and inorganic agents (brighteners) are often added to the electrolyte to achieve a bright and shiny appearance of the nickel plating deposit. The type of brightener added and its concentration determine the appearance of the nickel deposit: bright, shiny, semi-bright, satin, etc.
[0006] Traditionally, coumarins have been used to obtain high leveling, ductile, semi-bright, sulfur-free nickel deposits from Watts nickel baths. However, coumarin-free solutions are now available. Semi-bright nickel finishes are as the name suggests, semi-lustrous, but were specifically developed to be easy to polish and buff. Alternatively, buffing can be eliminated by subsequently plating bright nickel. Brightness and smoothness will vary with service conditions.
[0007] One of the reasons why semi-bright nickel finishes are so easily buffed and / or polished is because the deposit structure is columnar, whereas bright nickel finishes have a plate-like (lamellar) structure. However, the deposit structure can be altered by various additives, changes in pH, current density, or increased agitation of the solution, which is not an issue as long as it does not affect the deposit properties such as internal stress.
[0008] The internal stresses in plated nickel deposits can be compressive or tensile. Compressive stresses are when the deposit expands to relieve the stress. In contrast, tensile stresses are when the deposit contracts. Highly compressive deposits can blister, warp, or cause the deposit to separate from the workpiece, while deposits with high tensile stresses can cause warping as well as cracking and reduced fatigue strength.
[0009] It is well known to use coumarin as an additive in nickel electroplating baths, especially in semi-bright nickel processes, to produce ductile, bright deposits with excellent leveling. While a high concentration of coumarin in the bath gives the best leveling results on the one hand, such a high concentration of coumarin on the other hand gives a high rate of formation of harmful decomposition or decomposition products. These decomposition products are objectionable in that they can result in non-uniform, dull gray areas that are not easily lightened by the subsequent bright nickel deposit, can reduce the leveling obtained from a given concentration of coumarin in the electroplating bath, and can reduce the beneficial physical properties of the nickel deposit.
[0010] The use of various additives such as formaldehyde and chloral hydrate has also been proposed to help overcome the undesirable effects of the coumarin degradation products, but there are certain limitations to the use of such additives, since even moderate concentrations of these materials not only increase the tensile stress of the nickel electrodeposit, but also significantly reduce the leveling action of the coumarin.
[0011] Over the decades, plating suppliers have offered numerous bath formulations that claim to have the same leveling effect as coumarin baths, but until now, few bath formulations have met all the necessary criteria.
[0012] As explained above, coumarin leveling is exceptional, but coumarin has an unpleasant odor and decomposes to form harmful degradation products that can only be removed by batch carbon treatment of the electroplating bath. These treatments are expensive and time consuming, and must usually be performed at least monthly, and sometimes weekly.
[0013] DE 19610361 A1 discloses a process for the galvanic deposition of semi-bright nickel coatings on substrates, the said substrates being treated with an acidic aqueous galvanic bath which contains as brightener additives cyclic N-allyl- or N-vinyl-ammonium compounds, in particular based on pyridinium.
[0014] EP 2,852,698 B1 discloses a galvanic nickel or nickel alloy electroplating bath for depositing a semi-bright nickel or nickel alloy coating on an electrically conductive workpiece; and a method thereof.
[0015] U.S. Pat. No. 5,164,069(A) discloses an acidic aqueous electroplating solution containing nickel ions and one or more acetylenic compounds, specifically mono- and polyglycerol ethers of acetylenic alcohols, and a method for electrolytically depositing a bright nickel deposit on a surface.
[0016] EP 2 801 640 A1 discloses a galvanic nickel or nickel alloy electroplating bath for depositing semi-bright nickel or nickel alloy coatings on conductive workpieces.
[0017] China Patent Publication No. 108950617(A) discloses a nickel-nickel alloy plating solution containing bismuth and an electroplating method thereof.
[0018] However, there is very little known prior art that suggests how to achieve the desired complex combination of good deposition properties for Semi-bright nickel or Semi-bright nickel alloy coatings with good brightness properties without producing high internal stress values. Prior art baths have been mostly successful in achieving Semi-bright nickel or Semi-bright nickel alloy coatings that exhibit some good properties, while other properties have been or become poor, such as a combination of good brightness and high internal stress, or poor brightness and low internal stress. [Prior art documents] [Patent documents]
[0019] [Patent Document 1] DE 19610361 A1 [Patent Document 2] European Patent No. 2,852,698(B1) [Patent Document 3] U.S. Patent No. 5,164,069(A) [Patent Document 4] European Patent Application Publication No. 2801640(A1) [Patent Document 5] Chinese Patent Application Publication No. 108950617(A) Summary of the Invention [Problem to be solved by the invention]
[0020] In view of the prior art, it was therefore an object of the present invention to provide a modified galvanic nickel or nickel alloy electroplating bath for depositing Semi-bright nickel or Semi-bright nickel alloy coatings on workpieces which does not exhibit the above-mentioned drawbacks of the known prior art nickel electroplating baths.
[0021] In particular, it was an object of the present invention to provide a modified galvanic nickel or nickel alloy electroplating bath capable of depositing Semi-bright nickel or Semi-bright nickel alloy coatings on a number of different types of workpieces.
[0022] Therefore, what is needed is a method for depositing a semi-bright nickel or semi-bright nickel alloy coating that has good gloss characteristics and good leveling.
[0023] Another object of the present invention is to provide a coumarin-free galvanic nickel or nickel alloy electroplating bath that approaches or matches the leveling characteristics of coumarin baths.
[0024] Furthermore, it was an object of the present invention to provide a semi-bright nickel or semi-bright nickel alloy coating having low internal stresses, in particular in combination with good gloss properties.
[0025] Furthermore, it was an object of the present invention, particularly when the workpiece to be coated comprises a metal, such as steel, to provide a Semi-bright nickel or Semi-bright nickel alloy coating having only minimal cracks and pores to avoid undesirable corrosion of the metal surface.
[0026] It is yet another object of the present invention to provide a galvanic nickel or nickel alloy electroplating bath that provides good stability over the life of the bath.
[0027] It was further an object of the present invention to provide a modified galvanic nickel or nickel alloy electroplating bath that is also suitable for use in depositing semi-bright nickel or semi-bright nickel alloy coatings.
[0028] It was further an object of the present invention to provide a modified galvanic nickel or nickel alloy electroplating bath which contains the simplest possible general bath composition and preferably contains the cheapest possible chemicals. [Means for solving the problem]
[0029] These objects, as well as further objects not explicitly stated but which can be readily derived or discerned from the connections discussed herein in the introduction, are achieved by a galvanic nickel or nickel alloy electroplating bath having all the features of claim 1 according to a first aspect of the present invention. Appropriate modifications of the galvanic nickel or nickel alloy electroplating bath of the present invention are contained in dependent claims 2 to 7. Furthermore, claim 8 comprises a method for depositing a Semi-bright nickel or Semi-bright nickel alloy coating on a conductive workpiece according to the second aspect of the present invention. According to a third aspect of the present invention, claim 9 comprises the use of a galvanic nickel or nickel alloy electroplating bath according to the first aspect for carrying out a method according to the second aspect to deposit a Semi-bright nickel or Semi-bright nickel alloy coating.
[0030] The invention is particularly suitable for depositing decorative coatings on conductive workpieces, for example in the field of decorative coatings for sanitary or automotive equipment, where an intermediate nickel or nickel alloy layer is required for the subsequent deposition of a different metal layer for corrosion protection and / or decorative layers. Typical workpieces are substrates from the automotive industry having a surface to be plated with a metallic coating, such as interior parts of cars, front grilles or emblems, or workpieces from the white goods industry having a surface to be plated with a metallic coating, such as doors, refrigerator handles, knobs, microwaves, shower heads, etc., parts of kitchen and bathroom appliances. The base material of the substrate can be known plastics, such as polycarbonate (PC), polyimide (PI), polyethylene (PE), acrylonitrile butadiene styrene (ABS), or mixtures thereof, which are made conductive by known methods and which ultimately provide a conductive surface (e.g. copper or nickel or combinations thereof), or it can be a metal substrate (further having a conductive surface, such as copper or nickel or combinations thereof).
[0031] The present invention according to a first aspect provides a galvanic nickel or nickel alloy electroplating bath for depositing a semi-bright nickel or semi-bright nickel alloy coating, the electroplating bath comprising a nickel alloy having general formula (I):
[0032] [ka]
[0033] (In the formula, R1 = C1-C containing SO3 group 18 C1-C containing a hydrocarbon group or a carboxyl group 18 Hydrocarbon groups or C1-C containing aromatic and / or heteroaromatic groups 18 is a hydrocarbon group; R2=NR3R4 group, OR5 group, or cyclic NR6 group; R3, R4, R5 = hydrogen or C1-C 18C1-C containing aliphatic hydrocarbon groups, or aromatic and / or heteroaromatic groups 18 is a hydrocarbon group, R3, R4 and R5 are the same or different; R6 = a C3-C8 hydrocarbon group or a C3-C8 hydrocarbon group in which at least one carbon atom is substituted with a heteroatom; n=1 to 3) and / or a salt thereof; The electroplating bath further comprises at least one acetylenic compound and / or a salt thereof in a total concentration ranging from 0.002 g / l to 0.15 g / l; at least one acetylenic compound and / or salt thereof is selected from the group consisting of HC≡C-CH2-N(ethyl)2, HC≡C-CH2-O-CH2-CH2-OH, CH3-CH(OH)-C≡C-CH(OH)-CH3, CH3-C(CH3)(OH)-C≡CC(CH3)(OH)-CH3, HO-CH2-C≡C-CH2-OH, HO-CH2-CH2-O-CH2-C≡C-CH2-O-CH2-CH2-OH, HC≡C-CH2-O-CH2-CH2-CH2-OH and HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH; The electroplating bath includes chloral hydrate, and the chloral hydrate has a concentration of less than 0.07 g / l.
[0034] It has therefore unexpectedly been possible to provide a modified galvanic nickel or nickel alloy electroplating bath for depositing Semi-bright nickel or Semi-bright nickel alloy coatings on workpieces, which does not exhibit the aforementioned disadvantages of the known prior art nickel electroplating baths.
[0035] In particular, the modified galvanic nickel or nickel alloy electroplating baths according to the present invention are suitable for depositing semi-bright nickel or semi-bright nickel alloy coatings while reducing the concentration of chloral hydrate in the electroplating bath.
[0036] In particular, the modified galvanic nickel or nickel alloy electroplating baths according to the present invention are suitable for depositing Semi-bright nickel or Semi-bright nickel alloy coatings on several different types of workpieces.
[0037] The present invention provides a coumarin-free galvanic nickel or nickel alloy electroplating bath that at least approaches the leveling characteristics of coumarin baths.
[0038] The achieved semi-bright nickel or semi-bright nickel alloy coating has good gloss properties and good leveling.
[0039] Furthermore, the resulting semi-bright nickel or semi-bright nickel alloy coating has low internal stresses, particularly in combination with good gloss properties.
[0040] Additionally, the present invention provides a galvanic nickel or nickel alloy electroplating bath that offers good stability over the life of the bath.
[0041] Furthermore, the resulting Semi-bright nickel or Semi-bright nickel alloy coating has minimal cracks and pores in the final outer coating, which helps to avoid undesirable corrosion of the metal surface when the workpiece to be coated includes metals, such as steel, or conductive plastics (e.g., metallized with copper or nickel coatings or combinations thereof).
[0042] Moreover, the modified galvanic nickel or nickel alloy electroplating baths of the present invention include very simple general bath compositions having mostly inexpensive single chemicals.
[0043] Brief explanation of the table The objects, features and advantages of the present invention will also become apparent from the following description taken in conjunction with the tables. Table 1 shows experimental semi-bright nickel coatings according to embodiments of the present invention. Table 2 shows the experimental results of a semi-bright nickel coating according to a comparative embodiment other than the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0044] In order to distinguish between embodiments within the scope of the present invention and embodiments outside the scope of the present invention, the latter embodiments will be referred to below as "according to the present invention" embodiments. In many cases, features apply equally to both.
[0045] A first aspect according to the present specification is a galvanic nickel or nickel alloy electroplating bath for depositing a semi-bright nickel or semi-bright nickel alloy coating, the electroplating bath comprising a nickel alloy having a general formula (I):
[0046] [ka]
[0047] (In the formula, R1 = C1-C containing SO3 group 18 C1-C containing a hydrocarbon group or a carboxyl group 18 Hydrocarbon groups or C1-C containing aromatic and / or heteroaromatic groups 18 is a hydrocarbon group; R2=NR3R4 group, OR5 group, or cyclic NR6 group; R3, R4, R5 = hydrogen or C1-C 18 C1-C containing aliphatic hydrocarbon groups, or aromatic and / or heteroaromatic groups 18 is a hydrocarbon group, R3, R4 and R5 are the same or different; R6 = a C3-C8 hydrocarbon group or a C3-C8 hydrocarbon group in which at least one carbon atom is substituted with a heteroatom; n=1 to 3) and / or a salt thereof; The present invention relates to an electroplating bath, the electroplating bath further comprising at least one acetylenic compound and / or a salt thereof in a total concentration ranging from 0.001 g / l to 0.5 g / l.
[0048] According to the present specification, at least one acetylene compound and / or a salt thereof is represented by the general formula (V): R7-C≡C-R8 (V) (In the formula, R7=hydrogen or a C1-C8 hydrocarbon group containing at least one OR9 group; R9=hydrogen or a C1-C8 hydrocarbon group containing at least one OH group; R8 = at least one OR 10 C1-C8 hydrocarbon group containing a group, or at least one NR 11 R 12 is a C1-C8 hydrocarbon group containing a group, R 10 = hydrogen or a C1-C8 hydrocarbon group containing at least one OH group; R 11 , R 12 = hydrogen or a C1-C8 hydrocarbon group, R 11 and R 12 are the same or different), Electroplating baths are preferred.
[0049] According to the present specification, at least one acetylene compound and / or a salt thereof is represented by the general formula (V): R7-C≡C-R8 (V) (In the formula, R7=hydrogen or a C1-C4, preferably C1 or C2 or C3 alkyl group containing at least one OR9 group; R9=hydrogen or a C1-C8 hydrocarbon group containing at least one OH group; R8 = at least one OR 10 a C1-C4, preferably C1 or C2 or C3 alkyl group containing a group, or at least one NR 11 R 12 is a C1 to C4, preferably C1 or C2 alkyl group containing a group, R 10 = hydrogen or a C1-C8 hydrocarbon group containing at least one OH group; R 11 , R 12= hydrogen or a C1-C8 hydrocarbon group, R 11 and R 12 are the same or different), Electroplating baths are preferred.
[0050] According to the present specification, at least one acetylene compound and / or a salt thereof is represented by the general formula (V): R7-C≡C-R8 (V) (In the formula, R7=hydrogen or a C1-C4, preferably C1 or C2 or C3 alkyl group containing at least one OR9 group; R9=hydrogen or a C1-C3, preferably C1 or C2 alkyl group containing at least one OH group; R8 = at least one OR 10 a C1-C4, preferably C1 or C2 or C3 alkyl group containing a group, or at least one NR 11 R 12 is a C1 to C4, preferably C1 or C2 alkyl group containing a group, R 10 = hydrogen or a C1-C3, preferably C1 or C2 alkyl group containing at least one OH group; R 11 , R 12 = hydrogen or a C1 to C4, preferably C1 or C2 alkyl group; R 11 and R 12 are the same or different), Electroplating baths are preferred.
[0051] According to the present specification, at least one acetylene compound and / or a salt thereof is represented by the general formula (V): R7-C≡C-R8 (V) (In the formula, R7=hydrogen, or CH2-OH, or CH(OH)-CH3, C(CH3)(OH)-CH3, or CH2-O-CH2-CH2-OH, or CH2-O-CH2-CH2-CH2-OH; R8=CH2-OH, or CH(OH)-CH3, C(CH3)(OH)-CH3, or CH2-O-CH2-CH2-OH, or CH2-O-CH2-CH2-CH2-OH, or CH2-N(ethyl)2; Electroplating baths are preferred.
[0052] According to the present specification, electroplating baths are preferred, wherein the at least one acetylenic compound and / or salt thereof is selected from the group consisting of HC≡C-CH2-N(ethyl)2, HC≡C-CH2-O-CH2-CH2-OH, CH3-CH(OH)-C≡C-CH(OH)-CH3, CH3-C(CH3)(OH)-C≡CC(CH3)(OH)-CH3, HO-CH2-C≡C-CH2-OH, HO-CH2-CH2-O-CH2-C≡C-CH2-O-CH2-CH2-OH, HC≡C-CH2-O-CH2-CH2-CH2-OH, HC≡C-CH2-OH, and HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH.
[0053] According to this specification, preferred are electroplating baths comprising at least one acetylenic compound and / or salt thereof in a total concentration in the range of 0.001 g / l to 0.4 g / l, preferably 0.001 g / l to 0.25 g / l, more preferably 0.002 g / l to 0.15 g / l, even more preferably 0.003 g / l to 0.1 g / l, even more preferably 0.004 g / l to 0.08 g / l, and most preferably 0.001 g / l to 0.08 g / l.
[0054] According to this specification, preferred are electroplating baths which contain chloral hydrate, preferably in a concentration ranging from 0.005 g / l to 0.5 g / l, more preferably from 0.01 g / l to 0.1 g / l, and most preferably from 0.04 g / l to 0.085 g / l.
[0055] According to this specification, electroplating baths are preferred which contain chloral hydrate in a concentration of less than 0.07 g / l, preferably less than 0.045 g / l.
[0056] According to this specification, preferred are electroplating baths, which further comprise at least one bright nickel additive and / or salts thereof, preferably PPS, PES and / or PPS-OH, preferably in a total concentration in the range of 0.005 g / l to 10 g / l, more preferably 0.005 g / l to 1 g / l, and most preferably 0.01 g / l to 0.1 g / l.
[0057] According to this specification, electroplating baths are preferred which are formaldehyde-free or which contain formaldehyde in a concentration of less than 0.1 g / l, preferably less than 0.05 g / l, more preferably less than 0.025 g / l, even more preferably less than 0.01 g / l, and most preferably less than 0.005 g / l.
[0058] According to this specification, preferred are electroplating baths, wherein the electroplating bath does not contain aromatic sulfonic acids and / or salts thereof, preferably does not contain 1,3,6-naphthalene trisulfonic acid and / or salts thereof, and / or wherein the electroplating bath does not contain benzoic acid sulfimide (saccharin).
[0059] According to the present specification, preferred are electroplating baths, wherein the electroplating bath further comprises at least one compound selected from internal stress reducing agents and / or salts thereof, wherein the at least one internal stress reducing agent is selected as salicylic acid and / or salts thereof, preferably in a total concentration in the range of 0.1 g / l to 10 g / l, more preferably 0.3 g / l to 6 g / l, and most preferably 0.5 g / l to 3.5 g / l.
[0060] A second aspect according to the present specification is a method for depositing a Semi-bright nickel or Semi-bright nickel alloy coating on an electrically conductive workpiece, comprising the following method steps: i) contacting a workpiece with a galvanic nickel or nickel alloy electroplating bath according to the first aspect of the present specification; ii) contacting at least one anode with a galvanic nickel or nickel alloy electroplating bath according to the first aspect of the present specification; iii) applying a voltage between the workpiece and at least one anode; and iv) electrodepositing a semi-bright nickel or semi-bright nickel alloy coating onto the workpiece. The present invention is directed to a method, comprising:
[0061] A third aspect hereof is directed to the use of a galvanic nickel or nickel alloy electroplating bath according to the first aspect hereof for depositing a Semi-bright nickel or Semi-bright nickel alloy coating by carrying out a method according to the second aspect hereof. The present invention will now be described in more detail.
[0062] The present invention according to a first aspect provides a galvanic nickel or nickel alloy electroplating bath for depositing a semi-bright nickel or semi-bright nickel alloy coating, the electroplating bath comprising a nickel alloy having general formula (I): (In the formula, R1 = C1-C containing SO3 group 18 C1-C containing a hydrocarbon group or a carboxyl group 18 Hydrocarbon groups or C1-C containing aromatic and / or heteroaromatic groups 18 is a hydrocarbon group; R2=NR3R4 group, OR5 group, or cyclic NR6 group; R3, R4, R5 = hydrogen or C1-C 18 C1-C containing aliphatic hydrocarbon groups, or aromatic and / or heteroaromatic groups 18 is a hydrocarbon group, R3, R4 and R5 are the same or different; R6 = a C3-C8 hydrocarbon group or a C3-C8 hydrocarbon group in which at least one carbon atom is substituted with a heteroatom; n=1 to 3) and / or a salt thereof; The electroplating bath further comprises at least one acetylenic compound and / or a salt thereof in a total concentration ranging from 0.002 g / l to 0.15 g / l; at least one acetylenic compound and / or salt thereof is selected from the group consisting of HC≡C-CH2-N(ethyl)2, HC≡C-CH2-O-CH2-CH2-OH, CH3-CH(OH)-C≡C-CH(OH)-CH3, CH3-C(CH3)(OH)-C≡CC(CH3)(OH)-CH3, HO-CH2-C≡C-CH2-OH, HO-CH2-CH2-O-CH2-C≡C-CH2-O-CH2-CH2-OH, HC≡C-CH2-O-CH2-CH2-CH2-OH and HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH; The electroplating bath includes chloral hydrate, and the chloral hydrate has a concentration of less than 0.07 g / l.
[0063] By adding at least one acetylene compound and / or salt thereof in a total concentration ranging from 0.002 g / l to 0.15 g / l, an electroplating bath capable of depositing semi-bright nickel or semi-bright nickel alloy coatings having advanced properties such as good or even better brightness properties and good or even better leveling is provided.
[0064] The galvanic nickel or nickel alloy electroplating baths for depositing the Semi-bright nickel or Semi-bright nickel alloy coatings according to the invention contain nickel ions. This applies equally to the electroplating baths according to the present specification.
[0065] According to the present invention / specification, the salts include, but are not limited to, alkali metal salts, such as sodium salts, potassium salts, etc.; alkaline earth metal salts, such as calcium salts, magnesium salts, etc.; organic amine salts, such as triethylamine salts, pyridine salts, picoline salts, ethanolamine salts, triethanolamine salts, dicyclohexylamine salts, etc.; inorganic acid salts, such as halides, preferably chlorides, bromides, fluorides and / or iodides, hydrochlorides, hydrobromides, sulfates, phosphates, etc.; organic acid salts, such as formates, acetates, trifluoroacetates, maleates, tartarates, etc.; sulfonates, such as methanesulfonates, benzenesulfonates, p-toluenesulfonates, etc.; amino acid salts, such as alginates, aspartates, glutamates, etc.
[0066] Preferably, the salts include alkali metal salts, such as sodium salts, potassium salts, etc.; alkaline earth metal salts, such as calcium salts, magnesium salts, etc.; and / or inorganic acid salts, such as halides, more preferably chlorides, bromides, fluorides and / or iodides, sulfates, etc.
[0067] According to the present specification, electroplating baths are preferred, wherein the at least one acetylenic compound and / or salt thereof is an aliphatic acetylenic compound and / or salt thereof. Generally, providing the electroplating bath with at least one aliphatic acetylenic compound, as opposed to an aromatic acetylenic compound, improves the properties of the deposited Semi-bright nickel or Semi-bright nickel alloy coating.
[0068] According to the present specification, electroplating baths are preferred in which the at least one acetylenic compound and / or salt thereof comprises at least one OH group or at least one N(ethyl)2 group. Generally, the hydroxyl or diethylamine group provides the acetylenic compound with polarity, thereby improving the deposition process.
[0069] According to this specification, when R7 is selected as hydrogen, R8 cannot be selected as CH2-OH, and thus the electroplating bath is preferred.
[0070] The selection of an acetylenic compound as a substituted alkyne group according to formula (V) improves the brightness and leveling of the deposited semi-bright nickel or semi-bright nickel alloy coating. The alkyl groups utilized in the context of the present invention may include n-alkyl groups, iso-alkyl groups, or tert-alkyl groups.
[0071] According to the present specification, the compound according to formula (V) is selected from the group consisting of HC≡C-CH2-N(ethyl)2 (Golpanol DEP), HC≡C-CH2-O-CH2-CH2-OH (Golpanol PME), HO-CH2-C≡C-CH2-OH (Golpanol BOZ), CH3-CH(OH)-C≡C-CH(OH)-CH3 (Golpanol HD), CH3-C(CH3)(OH)-C≡CC(CH3)(OH)-CH3, HO-CH2-CH2-O-CH2-C≡C-CH2-O Preferred are electroplating baths selected as -CH2-CH2-OH (Golpanol BEO), HC≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol PAP), HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol BMP), HC≡C-CH2-OH (Golpanol PA) and / or salts thereof, preferably Golpanol DEP, Golpanol PME, Golpanol BOZ, Golpanol HD, and / or salts thereof.
[0072] However, according to the present invention, at least one acetylenic compound is selected from the group consisting of HC≡C-CH2-N(ethyl)2 (Golpanol DEP), HC≡C-CH2-O-CH2-CH2-OH (Golpanol PME), HO-CH2-C≡C-CH2-OH (Golpanol BOZ), CH3-CH(OH)-C≡C-CH(OH)-CH3 (Golpanol HD), CH3-C(CH3)(OH)-C≡CC(CH3)(OH)-CH3, HO-CH2-CH2-O Preferred are electroplating baths selected as -CH2-C≡C-CH2-O-CH2-CH2-OH (Golpanol BEO), HC≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol PAP), HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol BMP) and / or salts thereof, preferably Golpanol DEP, Golpanol PME, Golpanol BOZ, Golpanol HD, and / or salts thereof.
[0073] Preferably, when the electroplating bath contains CH3-CH(OH)-C≡C-CH(OH)-CH3 (Golpanol HD), the electroplating bath cannot contain chloral hydrate in a concentration greater than 0.15 g / l, preferably cannot contain chloral hydrate in a concentration greater than 0.20 g / l, and more preferably cannot contain chloral hydrate in a concentration greater than 0.25 g / l.
[0074] Preferably, when the electroplating bath comprises CH3-CH(OH)-C≡C-CH(OH)-CH3 (Golpanol HD), the electroplating bath cannot contain a salicylic acid concentration greater than 1.5 g / l, preferably cannot contain a salicylic acid concentration greater than 2.0 g / l, and more preferably cannot contain a salicylic acid concentration between 2.4 g / l and 2.6 g / l.
[0075] Preferably, when the electroplating bath contains CH3-CH(OH)-C≡C-CH(OH)-CH3 (Golpanol HD), the electroplating bath cannot contain HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol BMP) in a concentration of less than 0.050 g / l, preferably cannot contain HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol BMP) in a concentration of less than 0.030 g / l, and more preferably cannot contain HO-CH2-C≡C-CH2-O-CH2-CH2-CH2-OH (Golpanol BMP) in a concentration of 0.010 g / l to 0.020 g / l.
[0076] Preferably, when the electroplating bath contains CH3-CH(OH)-C≡C-CH(OH)-CH3 (Golpanol HD), the electroplating bath cannot contain HO-CH2-C≡C-CH2-OH (Golpanol BOZ) in a concentration of less than 0.060 g / l, preferably cannot contain HO-CH2-C≡C-CH2-OH (Golpanol BOZ) in a concentration of less than 0.050 g / l, and more preferably cannot contain HO-CH2-C≡C-CH2-OH (Golpanol BOZ) in a concentration of 0.030 g / l to 0.040 g / l.
[0077] Preferably, when the electroplating bath contains HO-CH2-CH2-O-CH2-C≡C-CH2-O-CH2-CH2-OH (Golpanol BEO) and / or HC≡C-CH2-O-CH2-CH2-OH (Golpanol PME), the electroplating bath cannot contain 1-benzylpyridinium-3-carboxylate at a concentration of 0.05 ml / l to 0.5 ml / l.
[0078] Preferably, the electroplating bath of the present invention comprises at least one acetylenic compound and / or salt thereof in a total concentration in the range of 0.003 g / l to 0.1 g / l, even more preferably 0.004 g / l to 0.08 g / l, and most preferably 0.001 g / l to 0.08 g / l.
[0079] Preferably, the electroplating bath of the present invention contains at least one acetylene compound and / or salt thereof at a concentration of 0.005 g / l to 0.15 g / l, more preferably 0.010 g / l to 0.15 g / l, even more preferably 0.015 g / l to 0.15 g / l, even more preferably 0.020 g / l to 0.15 g / l, even more preferably 0.030 g / l to 0.15 g / l, even more preferably 0.040 g / l to 0.15 g / l, even more preferably 0.050 g / l to 0.15 g / l, even more preferably 0.06 and even more preferably 0.14 g / l to 0.15 g / l, more preferably 0.070 g / l to 0.15 g / l, even more preferably 0.080 g / l to 0.15 g / l, even more preferably 0.090 g / l to 0.15 g / l, even more preferably 0.10 g / l to 0.15 g / l, even more preferably 0.11 g / l to 0.15 g / l, even more preferably 0.12 g / l to 0.15 g / l, even more preferably 0.13 g / l to 0.15 g / l, and even more preferably 0.14 g / l to 0.15 g / l.
[0080] Preferably, the electroplating bath of the present invention contains at least one acetylene compound and / or salt thereof at a concentration of from 0.005 g / l to 0.15 g / l, even more preferably from 0.005 g / l to 0.14 g / l, even more preferably from 0.005 g / l to 0.13 g / l, even more preferably from 0.005 g / l to 0.12 g / l, even more preferably from 0.005 g / l to 0.11 g / l, even more preferably from 0.005 g / l to 0.10 g / l, even more preferably from 0.005 g / l to 0.090 g / l, even more preferably from 0.005 g / l to 0.15 ... The total concentration is preferably in the range of 0.005 g / l to 0.080 g / l, even more preferably 0.005 g / l to 0.070 g / l, even more preferably 0.005 g / l to 0.060 g / l, even more preferably 0.005 g / l to 0.050 g / l, even more preferably 0.005 g / l to 0.040 g / l, even more preferably 0.005 g / l to 0.030 g / l, even more preferably 0.005 g / l to 0.020 g / l, and even more preferably 0.005 g / l to 0.010 g / l.
[0081] By selecting the total concentration of the at least one acetylenic compound in a preferred concentration range, the properties of the deposited Semi-bright nickel or Semi-bright nickel alloy coating can be improved.
[0082] Preferably, the electroplating bath comprises at least two acetylenic compounds and / or salts thereof, preferably at least three acetylenic compounds and / or salts thereof.
[0083] As used herein, the term "galvanic nickel or nickel alloy electroplating bath", when applied to deposit Semi-bright nickel or Semi-bright nickel alloy coatings, refers to galvanic nickel baths based on so-called "Watts electrolytic baths", which have the general composition: 240~550g / l Nickel sulfate (NiSO4·7H2O or NiSO4·6H2O), 30-150g / l Nickel chloride (NiCl2·6H2O), and 30~55g / l boric acid (H3BO3).
[0084] Large amounts of nickel sulfate provide the necessary concentration of nickel ions, nickel chloride improves anode corrosion and increases electrical conductivity, and boric acid is used as a weak buffer to maintain pH value.
[0085] Preferably, the galvanic nickel and nickel alloy electroplating baths have a chloride content in the range of 10 g / l to 50 g / l, preferably in the range of 15 g / l to 40 g / l, and more preferably in the range of 20 g / l to 30 g / l.
[0086] The nickel chloride may be partially or completely replaced by sodium chloride.
[0087] Additionally, the chloride in the electrolyte may be partially or completely replaced by an equivalent amount of bromide.
[0088] In general, chloral hydrate serves to set the electrical potential and also serves to modify the gloss and throwing power characteristics of the deposited coating.
[0089] Preferably, the electroplating bath of the present invention contains chloral hydrate at a concentration in the range of 0.001 g / l to 0.069 g / l, more preferably at a concentration in the range of 0.005 g / l to 0.069 g / l, even more preferably at a concentration in the range of 0.010 g / l to 0.069 g / l, even more preferably at a concentration in the range of 0.020 g / l to 0.069 g / l, even more preferably at a concentration in the range of 0.025 g / l to 0.069 g / l, even more preferably at a concentration in the range of 0.030 g / l to 0.069 g / l, and even more preferably at a concentration in the range of 0.010 g / l to 0.069 g / l. More preferably, it is contained in a concentration in the range of 0.035 g / l to 0.069 g / l, even more preferably in a concentration in the range of 0.040 g / l to 0.069 g / l, even more preferably in a concentration in the range of 0.045 g / l to 0.069 g / l, even more preferably in a concentration in the range of 0.050 g / l to 0.069 g / l, even more preferably in a concentration in the range of 0.055 g / l to 0.069 g / l, even more preferably in a concentration in the range of 0.060 g / l to 0.069 g / l, and even more preferably in a concentration in the range of 0.065 g / l to 0.069 g / l.
[0090] Preferably, the electroplating bath of the present invention contains chloral hydrate at a concentration in the range of 0.001 g / l to 0.069 g / l, more preferably at a concentration in the range of 0.001 g / l to 0.065 g / l, even more preferably at a concentration in the range of 0.001 g / l to 0.060 g / l, even more preferably at a concentration in the range of 0.001 g / l to 0.055 g / l, even more preferably at a concentration in the range of 0.001 g / l to 0.050 g / l, even more preferably at a concentration in the range of 0.001 g / l to 0.045 g / l, and even more preferably at a concentration in the range of 0.001 g / l to 0.040 g / l. More preferably, the concentration of the glycerol is in the range of 0.001 g / l to 0.035 g / l, even more preferably, in the range of 0.001 g / l to 0.030 g / l, even more preferably, in the range of 0.001 g / l to 0.025 g / l, even more preferably, in the range of 0.001 g / l to 0.020 g / l, even more preferably, in the range of 0.001 g / l to 0.015 g / l, even more preferably, in the range of 0.001 g / l to 0.010 g / l, and even more preferably, in the range of 0.001 g / l to 0.005 g / l.
[0091] By selecting the concentration of chloral hydrate in a preferred concentration range, the overall consumption of chloral hydrate can be reduced, thereby reducing costs, while optimizing the properties of the deposited Semi-bright nickel or Semi-bright nickel alloy coating.
[0092] Preferably, the electroplating baths of the present invention contain chloral hydrate in a concentration of less than 0.045 g / l.
[0093] Preferably, the electroplating baths of the present invention contain chloral hydrate at a concentration of less than 0.065 g / l, more preferably less than 0.060 g / l, even more preferably less than 0.055 g / l, even more preferably less than 0.050 g / l, even more preferably less than 0.045 g / l, even more preferably less than 0.040 g / l, even more preferably less than 0.040 g / l, in some cases even more preferably less than 0.035 g / l, even more preferably less than 0.030 g / l, even more preferably less than 0.025 g / l, even more preferably less than 0.020 g / l, even more preferably less than 0.015 g / l, and even more preferably less than 0.010 g / l.
[0094] Preferably, the electroplating bath may contain at least one compound selected from an internal stress reducing agent, such as benzoic acid, acetic acid and / or salicylic acid, and / or a salt thereof, and a wetting agent, such as succinic acid, sulfosuccinic acid, 2-ethylhexyl sulfate, dihexylsulfosuccinic acid, and / or diamylsulfosuccinic acid, and / or a salt thereof, preferably in a total concentration ranging from 0.001 g / l to 8 g / l, more preferably from 0.01 g / l to 2 g / l, and most preferably from 0.02 g / l to 1 g / l.
[0095] Preferably, the electroplating baths may contain at least one wetting agent, such as succinic acid, sulfosuccinic acid, 2-ethylhexyl sulfate, dihexylsulfosuccinic acid, and / or diamylsulfosuccinic acid, and / or their salts, preferably the sodium salt, preferably in a total concentration in the range of 0.005 g / l to 0.5 g / l, more preferably 0.01 g / l to 0.35 g / l, and most preferably 0.02 g / l to 0.1 g / l.
[0096] Preferably, the electroplating bath may contain at least one compound selected from internal stress reducing agents and / or salts thereof, the at least one internal stress reducing agent being preferably selected as salicylic acid and / or salts thereof in a total concentration ranging from 0.1 g / l to 10 g / l, more preferably from 0.3 g / l to 6 g / l, and most preferably from 0.5 g / l to 3.5 g / l. Such additives have a positive effect on the hardness, durability, and optical properties of the achieved coating.
[0097] Preferably, the electroplating bath further comprises an alkali metal benzoate, preferably sodium benzoate, preferably in a concentration ranging from 0.005 g / l to 5 g / l, more preferably from 0.02 g / l to 2 g / l, and most preferably from 0.05 g / l to 0.5 g / l. Such additive compounds aid in reducing internal stresses in the deposited coating.
[0098] Preferably, the electroplating bath of the present invention further comprises at least one bright nickel additive and / or salt thereof, preferably PPS (3-(pyridinium-1-yl)-propane-1-sulfonate), PES (3-(pyridinium-1-yl)-ethane-1-sulfonate), and / or PPS-OH (3-(pyridinium-1-yl)-(2-hydroxy-propane-1-sulfonate)), preferably in a total concentration ranging from 0.005 g / l to 10 g / l, more preferably from 0.005 g / l to 1 g / l, and most preferably from 0.01 g / l to 0.1 g / l. Preferably, the concentration ratio between the at least one additional bright nickel additive and / or salt thereof, e.g., PPS, PES, and / or PPS-OH, and the at least one compound having the general formula (I) and / or salt thereof is less than 10:1, more preferably less than 5:1, and most preferably less than 3:1. This applies equally to the electroplating baths according to the present invention.
[0099] This provides a huge advantage by allowing large quantities of expensive compounds having formula (I) to be replaced with cheaper known bright nickel additives, such as PPS, PES, and / or PPS-OH, without the known drawbacks of PPS, PES, and PPS-OH.
[0100] Preferably, the electroplating baths of the present invention are formaldehyde-free or contain formaldehyde in a concentration of less than 0.1 g / l, preferably less than 0.05 g / l, more preferably less than 0.025 g / l, even more preferably less than 0.01 g / l, and most preferably less than 0.005 g / l.
[0101] The presence of formaldehyde in a galvanic nickel or nickel alloy electroplating bath affects the brightness of the nickel or nickel alloy coating deposited on the workpiece. By preferably omitting formaldehyde or preferably reducing the concentration of formaldehyde, one can advantageously ensure that a Semi-bright nickel or Semi-bright nickel alloy coating is deposited. In particular, this is in contrast to the prior art, where a high concentration of formaldehyde in the electroplating bath results in the deposition of a bright nickel or bright nickel alloy coating rather than a Semi-bright nickel or Semi-bright nickel alloy coating.
[0102] Preferably, the electroplating baths of the present invention are free of aromatic sulfonic acids and / or salts thereof, preferably free of 1,3,6-naphthalene trisulfonic acid and / or salts thereof, and / or the electroplating baths are free of benzoic acid sulfimide (saccharin).
[0103] The presence of aromatic sulfonic acids or benzoic acid sulfimides (also known as saccharin) in galvanic nickel or nickel alloy electroplating baths affects the brightness, crystal structure and potential of the nickel or nickel alloy coating deposited on the workpiece. By preferably omitting the aromatic sulfonic acids or benzoic acid sulfimides from the electroplating bath, one can advantageously ensure that a semi-bright nickel or semi-bright nickel alloy coating is deposited.
[0104] Preferably, the cathode current density is 1 to 10 A / dm 2 in the range of 2 to 7 A / dm 2 and more preferably 3 to 5 A / dm 2 The value will be in the range.
[0105] Preferably, the operating temperature is in the range of 40°C to 70°C, more preferably 45°C to 65°C, and most preferably 50°C to 60°C.
[0106] Preferably, the pH value of the electroplating bath is in the range of 2 to 6, more preferably 3 to 5, and most preferably 3.5 to 4.5.
[0107] The galvanic nickel or nickel alloy electroplating baths can be deposited on several different types of workpieces based on metals and / or metal alloys, in particular steel, copper, brass and / or zinc die casting; or on "POP" workpieces. "POP" workpieces stand for "plating on plastic" workpieces. POPs therefore include synthetic workpieces, preferably based on at least one polymeric compound, more preferably based on acrylonitrile-butadiene-styrene (ABS), polyamide, polypropylene or ABS / PC (polycarbonate).
[0108] The expression n=1-3, 1 or 2, or 1 in the general formula (I) defines the number of substituents on the ring system of the general formula (I). Thus, when n=3, the ring system of the general formula (I) contains three substituents, which can be located in the ortho, meta and / or para positions relative to the nitrogen atom of the ring system according to the generally known substitution rules of organic chemistry. In conclusion, when n=2, there are two such substituents, and when n=1, there is only one such substituent on the ring system present.
[0109] In contrast, electrolytes for obtaining matte nickel or nickel alloy deposits do not form part of the present invention.
[0110] Preferably, the electroplating bath comprises at least one compound having the general formula (I): R1 = a C1-C8, preferably C1-C4, hydrocarbon group containing an SO3 group, or a C1-C8, preferably C1-C4, hydrocarbon group containing a carboxyl group, or a C1-C8, preferably C1-C4, hydrocarbon group containing an aromatic and / or heteroaromatic group; R2=NR3R4 group, OR5 group, or cyclic NR6 group; R3, R4, R5 = hydrogen or C1-C 18 C1-C containing aliphatic hydrocarbon groups, or aromatic and / or heteroaromatic groups 18 is a hydrocarbon group, R3, R4 and R5 are the same or different; R6 = a C4-C8 hydrocarbon group or a C3-C8 hydrocarbon group in which at least one carbon atom is substituted with a heteroatom; n=1 or 2.
[0111] Preferably, the electroplating bath comprises at least one compound having the general formula (I): R1 = a C1-C8, preferably C1-C4, hydrocarbon group containing an SO3 group, or a C1-C8, preferably C1-C4, hydrocarbon group containing a carboxyl group, or a C1-C8, preferably C1-C4, hydrocarbon group containing an aromatic and / or heteroaromatic group; R2=NR3R4 group, OR5 group, or cyclic NR6 group; R3, R4, R5=hydrogen, or a C1-C8, preferably C1-C4 aliphatic hydrocarbon group, or a C1-C8, preferably C1-C4 hydrocarbon group containing aromatic and / or heteroaromatic groups, where R3, R4 and R5 are the same or different; R6=C4 or C5 hydrocarbon group, or a C4-C5 hydrocarbon group in which at least one carbon atom is substituted with a sulfur or oxygen atom; n=1.
[0112] Preferably, the electroplating bath comprises at least one compound having the general formula (I): R1 = n-ethyl-SO3-, or n-propyl-SO3-, or n-butyl-SO3-, or benzyl, or CH2-COOH and / or salts thereof, preferably sodium salts CH2-COONa groups; R2=NH2, or N(ethyl)2, or O(ethyl), or an OH group, or a cyclic NR6 group; R6=C4 or C5 hydrocarbon group, or a C4-C5 hydrocarbon group in which at least one carbon atom is substituted with a sulfur or oxygen atom; n=1.
[0113] Preferably, the electroplating bath comprises at least one compound having the general formula (I) and / or a salt thereof, wherein R1 is not hydrogen.
[0114] Preferably, the electroplating bath comprises at least one compound having the general formula (I) and / or a salt thereof, wherein at least one group C(O)R2 is in the ortho, meta and / or para position of an aromatic ring.
[0115] Preferably, the electroplating bath comprises at least one compound having general formula (I) and / or a salt thereof in a total concentration in the range of 0.005 g / l to 10 g / l, more preferably 0.008 g / l to 5 g / l, even more preferably 0.01 g / l to 1 g / l, and most preferably 0.01 g / l to 0.1 g / l.
[0116] All preferred features of the electroplating bath according to the first aspect of the invention preferably also constitute the method according to the second aspect of the invention and the use according to the third aspect of the invention. In other words, what is stated above regarding the first aspect of the invention / first aspect hereof (i.e. the electroplating bath, most preferably including its preferred variants) preferably also applies analogously to the method of the invention (second aspect of the invention) and the second aspect hereof, respectively.
[0117] The present invention according to a second aspect provides a method for depositing a Semi-bright nickel or Semi-bright nickel alloy coating on an electrically conductive workpiece comprising the following method steps: i) contacting a workpiece with a galvanic nickel or nickel alloy electroplating bath according to the first aspect of the present invention; ii) contacting at least one anode with a galvanic nickel or nickel alloy electroplating bath; iii) applying a voltage between the workpiece and at least one anode; and iv) electrodepositing a semi-bright nickel or semi-bright nickel alloy coating onto the workpiece. The present invention provides a method comprising:
[0118] In the method, the cathode current density is preferably 1 to 10 A / dm 2 in the range of 2 to 7 A / dm 2 and more preferably 3 to 5 A / dm 2 The value will be in the range.
[0119] Preferably, the process has a working temperature in the range of 40°C to 70°C, more preferably 45°C to 65°C, and most preferably 50°C to 60°C.
[0120] Preferably, the pH value of the electroplating bath is in the range of 2 to 6, more preferably 3 to 5, and most preferably 3.5 to 4.5.
[0121] The present invention according to a third aspect provides the use of a galvanic nickel or nickel alloy electroplating bath according to the first aspect of the invention for carrying out a method according to the second aspect of the invention to deposit a Semi-bright nickel or Semi-bright nickel alloy coating.
[0122] Preferably, the features of the electroplating bath according to the first aspect of the present invention / herein (including most preferably preferred variants thereof) apply analogously to the use according to the third aspect of the present invention / herein, respectively.
[0123] Preferably, the compounds of general formula (I) for the electroplating bath, method and / or use include in particular chemical compounds having the following formulae (II), (III) and (IV):
[0124] [ka]
[0125] The synthesis procedure is summarized below.
[0126] 3-(3-(diethylcarbamoyl)pyridinium-1-yl)propane-1-sulfonate(II) 10 g (0.0555 mol) of nicotinic acid diethylamide (99%) is dissolved in 50 ml of ethanol. Subsequently, 6.78 g (0.0555 mol) of 1,3-propane sultone is added. The reaction mixture is then heated under reflux at 78° C. for 48 hours.
[0127] After the reaction is completed, the reaction mixture is cooled, and then 100 ml of diethyl ether is added at room temperature. The resulting white solid is filtered at 4°C, washed with another 100 ml of diethyl ether, and finally dried in vacuum. 9.00 g of a white solid are obtained (54% of theory).
[0128] 3-(3-(pyrrolidine-1-carbonyl)pyridinium-1-yl)propane-1-sulfonate(III) 10 g (0.056747 mol) of 3-(pyrrolidine-1-carbonyl)pyridine is dissolved in 50 ml of ethanol. Then, 6.93 g (0.056747 mol) of 1,3-propane sultone is added. The reaction mixture is then heated under reflux at 78° C. for 48 hours.
[0129] After the reaction is completed, the reaction mixture is cooled, and then 100 ml of diethyl ether is added at room temperature. The resulting white solid is filtered at 4°C, washed with another 100 ml of diethyl ether, and finally dried in vacuum. 8.635 g of a white solid are obtained (51% of theory).
[0130] 3-(3-(morpholine-4-carbonyl)pyridinium-1-yl)propane-1-sulfonate(IV) 10 g (0.05206 mol) of 3-(morpholine-1-carbonyl)pyridine is dissolved in 50 ml of ethanol. Then, 6.36 g (0.05206 mol) of 1,3-propane sultone is added. The reaction mixture is then heated under reflux at 78° C. for 48 hours.
[0131] After the reaction is completed, the reaction mixture is cooled, and then 100 ml of diethyl ether is added at room temperature. The resulting white solid is filtered at 4°C, washed with another 100 ml of diethyl ether, and finally dried in vacuum. 8.10 g of a white solid are obtained (49.5% of theory).
[0132] Thus, the present invention addresses the problem of providing a modified galvanic nickel or nickel alloy electroplating bath for depositing semi-bright nickel or semi-bright nickel alloy coatings on a number of different types of workpieces, as well as the method and use thereof. The electroplating bath according to the present invention provides a method for achieving semi-bright nickel or semi-bright nickel alloy coatings with a good and unique combination of desired properties such as brightness, leveling, ductility, etc., whereas known prior art baths can in most cases only provide some of these properties, and in most cases at least one serious drawback exists in the form of poor underside properties. The electroplating bath according to the present invention provides, for example, for steels, a combination of desired properties with good leveling, low hardness and high ductility, and for POPs, a combination of good brightness and simultaneously low internal stress values.
[0133] The following non-limiting examples are provided to illustrate embodiments of the present invention and to facilitate an understanding of the present invention, but are not intended to limit the scope of the invention, which is defined by the claims appended hereto.
[0134] In general, it should be mentioned that all the experiments, including those according to the invention as well as comparative embodiments other than the invention, were carried out using a so-called "Watts-based electrolytic bath" having the following composition: 280g / l Nickel sulfate (NiSO4·6H2O), 40g / l Nickel chloride (NiCl2·6H2O), 45g / l boric acid (H3BO3), 0.300g / l sodium benzoate, 0.025 g / l of a compound of formula (II), 0.067g / l PPS, 0.0425g / l chloral hydrate, and 0.05g / l Sodium dihexyl sulfosuccinate.
[0135] Nickel deposition was carried out using a Hull Cell at a temperature of 55° C.±3° C., pH 4.2, and 2.5 amperes for 10 minutes. In addition, compressed air was introduced at 3 liters / minute during nickel deposition.
[0136] The workpieces were pretreated before being used for nickel deposition in the following manner. i) Degreasing with hot soak cleaner ii) Electrolytic degreasing iii) Washing with water iv) Acid immersion with 10 vol% sulfuric acid
[0137] Copper and brass sample workpieces were scratched to determine leveling by subjective optical judgement, and the brightness of the resulting nickel deposits on the workpieces was also judged optically.
[0138] All results shown in Tables 1 and 2 for leveling and gloss were qualitatively ranked using the following synonyms: +++ Excellent ++ Good + Medium - bad
[0139] All concentrations given in Tables 1 and 2 for the different bath components are given in mg / l unless otherwise stated. The basic electroplating bath components (Watts bath) are described above and are not repeated in the tables, even if they are included. Golpanol DEP (N,N-diethyl-2-propyne-1-amine), Golpanol PME (propargyl alcohol ethoxylate), Golpanol BOZ (2-butyne-1,4-diol), and Golpanol HD (3-hexyne-2,5-diol) are commercially available brighteners.
[0140] The experiments shown in Tables 1 and 2 are numbered in order of outcome, with the second number in parentheses being Applicant's internal experiment number.
[0141] Returning to tables, Table 1 shows experiments carried out primarily on semi-bright nickel coatings according to embodiments of the present invention.
[0142] [Table 1]
[0143] Table 2 shows the experiments of semi-bright nickel coating according to comparative embodiments other than the present invention where no acetylenic compound was added to the electroplating bath (Experiments 15 and 16), and Table 1 shows Experiment 13, which is also a comparative example, with a total chloral hydrate concentration of 80 mg / l.
[0144] For experiments 1 to 14 according to embodiments of the invention (experiment 13 is a comparative example), the gloss values are good or excellent, whereas comparative experiment 15 often shows good results in terms of leveling, but at the same time a poor gloss value.
[0145] [Table 2]
[0146] The particular surprising effects of preferred embodiments of the present invention are outlined by a direct comparison of Experiments 1-14 and Comparative Experiment 15. In Comparative Experiment 15, no acetylenic compounds were added as additives to the electroplating bath. In contrast, in Experiments 1-14, Golpanol DEP, Golpanol PME, Golpanol BOZ, and / or Golpanol HD were added in various combinations as acetylenic additives, resulting in good or excellent gloss values in contrast to the poor gloss values of Comparative Experiment 15.
[0147] Furthermore, a direct comparison of Comparative Runs 13 and 16 highlights that the addition of 3 mg / l Golpanol PME, 3 mg / l Golpanol DEP, and 15 mg / l Golpanol BOZ as acetylenic compounds clearly improves the gloss values from good (see Comparative Run 16) to excellent (see Example 13). However, this is achieved in the presence of a relatively high concentration of chloral hydrate, i.e., 80 mg / l.
[0148] In particular, a direct comparison of Run 14 and Comparative Run 15 highlights that the addition of 10 mg / l Golpanol HD as the acetylenic compound clearly improves the gloss value from poor (see Comparative Example 15) to excellent (see Example 14). This was achieved in the presence of a relatively low concentration of chloral hydrate, i.e., 42.5 mg / l, which was an unexpected result.
[0149] Therefore, with regard to Experiment 12 and Comparative Experiment 13, it must be emphasized that excellent gloss values were achieved by adding acetylenic compounds at specific concentrations and at the same time, the concentration of chloral hydrate could be reduced to 42.5 mg / l (see Experiment 12 vs Comparative Experiment 13) without reducing the gloss value, since the gloss values are excellent in both Experiment 12 and Comparative Experiment 13.
[0150] As a result, the concentration of chloral hydrate in the electroplating bath can be significantly reduced without impairing the leveling or gloss value of the Semi-bright nickel or Semi-bright nickel alloy coating, thereby significantly reducing production costs.
[0151] While the principles of the invention have been described in relation to certain specific embodiments, provided for purposes of illustration, it should be understood that various modifications thereof will become apparent to those skilled in the art upon reading the specification. It is therefore to be understood that the invention disclosed herein includes such modifications as fall within the scope of the appended claims. The scope of the invention is limited only by the scope of the appended claims.
Claims
1. A galvanic nickel or nickel alloy electroplating bath for depositing a semi-bright nickel or semi-bright nickel alloy coating, said electroplating bath comprising a nickel alloy having general formula (I): [Formula 1] (In the formula, R 1 =SO 3 C containing groups 1 ~C 18 C containing a hydrocarbon group or a carboxyl group 1 ~C 18 C containing hydrocarbon groups, or aromatic and / or heteroaromatic groups 1 ~C 18 is a hydrocarbon group; R 2 =NR 3 R 4 Group or OR 5 group, or cyclic NR 6 It is based on R 3 , R 4 , R 5 = Hydrogen or C 1 ~C 18 C containing aliphatic hydrocarbon groups, or aromatic and / or heteroaromatic groups 1 ~C 18 is a hydrocarbon group, R 3 , R 4 and R 5 are the same or different; R 6 =C 3 ~C 8 A hydrocarbon group or a C group in which at least one carbon atom is replaced by a heteroatom 3 ~C 8 is a hydrocarbon group; n=1-3) and / or salts thereof; the electroplating bath further comprises at least one acetylenic compound and / or a salt thereof in a total concentration ranging from 0.002 g / l to 0.15 g / l; The at least one acetylenic compound and / or salt thereof is HC≡C-CH 2 -N(ethyl) 2, HC≡C-CH 2 -O-CH 2 -CH 2 -OH, CH 3 -CH(OH)-C≡C-CH(OH)-CH 3 , C.H. 3 -C(CH 3 )(OH)-C≡CC(CH 3 )(OH)-CH 3 , H.O.-C.H. 2 -C≡C-CH 2 -OH, HO-CH 2 -CH 2 -O-CH 2 -C≡C-CH 2 -O-CH 2 -CH 2 -OH, HC≡C-CH 2 -O-CH 2 -CH 2 -CH 2 -OH, and HO-CH 2 -C≡C-CH 2 -O-CH 2 -CH 2 -CH 2 -OH; 1. The electroplating bath, comprising chloral hydrate, the chloral hydrate having a concentration of less than 0.07 g / l.
2. 2. The galvanic nickel or nickel alloy electroplating bath according to claim 1, characterized in that the electroplating bath comprises the at least one acetylenic compound and / or salt thereof in a total concentration in the range from 0.003 g / l to 0.1 g / l.
3. 3. The galvanic nickel or nickel alloy electroplating bath according to claim 1 or 2, characterized in that the electroplating bath contains chloral hydrate in a concentration of less than 0.045 g / l.
4. 4. The galvanic nickel or nickel alloy electroplating bath according to claim 1, characterized in that the electroplating bath further comprises at least one bright nickel additive and / or salts thereof.
5. 5. The galvanic nickel or nickel alloy electroplating bath according to claim 1 , characterized in that the electroplating bath is formaldehyde-free or contains formaldehyde in a concentration of less than 0.1 g / l.
6. 6. The galvanic nickel or nickel alloy electroplating bath according to claim 1, characterized in that the electroplating bath does not contain aromatic sulfonic acids and / or salts thereof and / or the electroplating bath does not contain benzoic acid sulfimide.
7. 7. The galvanic nickel or nickel alloy electroplating bath according to claim 1, characterized in that the electroplating bath further comprises at least one compound selected from internal stress reducing agents and / or salts thereof, the at least one internal stress reducing agent being selected as salicylic acid and / or salts thereof.
8. 1. A method for depositing a semi-bright nickel or semi-bright nickel alloy coating on an electrically conductive workpiece, comprising the following method steps: i) contacting a workpiece with the galvanic nickel or nickel alloy electroplating bath according to any one of claims 1 to 7; ii) contacting at least one anode with said galvanic nickel or nickel alloy electroplating bath; iii) applying a voltage between the workpiece and the at least one anode; and iv) electrodepositing a semi-bright nickel or semi-bright nickel alloy coating onto said workpiece. A method comprising:
9. Use of the galvanic nickel or nickel alloy electroplating bath according to any one of claims 1 to 7 for depositing a Semi-bright nickel or Semi-bright nickel alloy coating by carrying out the method according to claim 8.
Citation Information
Patent Citations
Tellurium-containing zinc-nickel alloy electroplating solution and electroplating process thereof
CN108950617A
Bath and method for the electroplating of semi-bright nickel
DE19610361A1
EP2,852,698B1
Galvanic nickel or nickel alloy electroplating bath for depositing a semi-bright nickel or nickel alloy
EP2801640A1
Use of 2-substituted ethanesulfone compound as electroplating aid
JP1990073990A