High strength, heat stable nickel-based alloy
A nickel-based alloy with tailored compositions addresses the challenges of strength and ductility in high-temperature environments, achieving performance comparable to Alloy 740H while reducing cobalt content and enhancing thermal stability.
Patent Information
- Application Number
- JP2023542585
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-13
- Filing Date
- 2022-01-13
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2042-01-13
AI Technical Summary
Existing nickel-based alloys used in harsh environments like advanced ultra-supercritical boilers lack a desirable combination of strength, ductility, and thermal stability, particularly at high temperatures, which affects their performance and manufacturing processes.
A nickel-based alloy composition with specific weight percentages of elements such as aluminum, cobalt, chromium, molybdenum, niobium, titanium, tungsten, and carbon, along with incidental impurities, providing enhanced mechanical properties and thermal stability, including a stress rupture life of at least 300 hours at 700°C and 393.7 MPa, and room temperature elongation of at least 15% after aging at 700°C for 1,000 hours.
The alloy achieves high strength and ductility, with mechanical properties comparable to Alloy 740H but at reduced cobalt content, offering improved thermal stability and cost-effectiveness for use in high-temperature environments.
Smart Images

Figure 0007551935000019 
Figure 0007551935000021 
Figure 0007551935000020
Abstract
Description
Cross-reference to related application
[0001] This application claims priority to and the benefit of U.S. Patent Application No. 63 / 136,668, filed January 13, 2021, the disclosure of which is incorporated herein by reference. [Technical field]
[0002] The present disclosure relates to nickel-base alloys, and more particularly to high strength, thermally stable nickel-base alloys for use at high temperatures. [Background technology]
[0003] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0004] Alloys used in harsh environments, such as advanced ultra-supercritical (A-USC) boilers, require a combination of ductility at room temperature for fabrication, and strength and oxidation resistance at temperatures approaching 815 °C (1500 °F) during service. Thus, conventional alloys use combinations of nickel and chromium for high temperature oxidation resistance, titanium, aluminum and niobium for high temperature strength through precipitation hardening, and nickel and cobalt for ductility after the alloy is in service at room temperature and at high temperatures, and for fabrication and repair of the alloy after its use at high temperatures.
[0005] The present disclosure addresses the problem of alloys having the desired strength and ductility for use in A-USC boilers, as well as other problems associated with nickel-base precipitation hardenable alloys for use in high temperature corrosive environments. Summary of the Invention
[0006] This section provides a general overview of the disclosure and is not an exhaustive disclosure of its entire scope or all of its features.
[0007] In one aspect of the disclosure, the alloy comprises, in weight percent (weight percentages are used throughout unless otherwise noted), about 1.3% to about 1.8% aluminum, about 1.5% to about 4.0% cobalt, about 18.0% to about 22.0% chromium, about 4.0% to about 10.0% iron, about 1.0% to about 3.0% molybdenum, about 1.0% to about 2.5% niobium, about 1.3% to about 1.8% titanium, about 0.8% to about 1.2% tungsten, about 0.01% to about 0.08% carbon, and the balance nickel and incidental impurities. In some variations, the alloy has a stress rupture life at 700° C. and 393.7 MPa (57.1 ksi) of at least 300 hours, and a room temperature elongation of at least 15% after aging at 700° C. for 1,000 hours.
[0008] In some variations, the cobalt content of the alloy is about 2.0% to about 3.0%. In at least one variation, the molybdenum content of the alloy is about 1.0% to about 2.75%. In some variations, the niobium content of the alloy is about 1.0% to about 1.75%.
[0009] In at least one variation, the cobalt content in the alloy is about 2.0% to about 3.0% and the molybdenum content in the alloy is about 1.0% to about 2.75%. In some variations, the cobalt content in the alloy is about 2.0% to about 3.0% and the niobium content in the alloy is about 1.0% to about 1.75%.
[0010] In at least one variation, the molybdenum content in the alloy is from about 1.0% to about 2.75%, and the niobium content in the alloy is from about 1.0% to about 1.75%.
[0011] In some variations, the cobalt content in the alloy is from about 2.0% to about 3.0%, the molybdenum content in the alloy is from about 1.0% to about 2.75%, and the niobium content in the alloy is from about 1.0% to about 1.75.
[0012] In at least one variation, the stress rupture life of the alloy at 700° C. and 393.7 MPa (57.1 ksi) is at least 500 hours.
[0013] In some variations, the room temperature elongation of the alloy is at least 20% after aging for 1000 hours at 700° C. In at least one variation, the room temperature elongation of the alloy is at least 22% after aging for 1000 hours at 700° C.
[0014] In at least one variation, the alloy has a room temperature elongation of at least 15% after aging for 5000 hours at 700° C. In some variations, the alloy has a room temperature elongation of at least 20% after aging for 5000 hours at 700° C.
[0015] In some variations, the alloy has a room temperature impact energy of at least 12 ft-lb after aging for 1000 hours at 700° C. In at least one variation, the alloy has a room temperature impact energy of at least 15 ft-lb after aging for 1000 hours at 700° C., and in some variations, the alloy has a room temperature impact energy of at least 20 ft-lb after aging for 1000 hours at 700° C.
[0016] In at least one variation, the alloy has a room temperature impact energy of at least 10 ft-lb after aging for 5000 hours at 700° C. In some variations, the alloy has a room temperature impact energy of at least 12 ft-lb after aging for 5000 hours at 700° C., and in at least one variation, the alloy has a room temperature impact energy of at least 15 ft-lb after aging for 5000 hours at 700° C.
[0017] In some variations, the alloy has a room temperature (RT) ultimate tensile strength of between about 160 ksi (1104 MPa) and about 175 ksi (1207 MPa), a RT 0.2% proof stress of between about 95 ksi (655 MPa) and 115 ksi (793 MPa), and a RT elongation of between about 30% and 45% after the alloy is annealed at 788°C (1450°F) for four hours and then air cooled, and in at least one variation, the RT ultimate tensile strength of between about 160 ksi (1104 MPa) and about 170 ksi (1172 MPa), the RT 0.2% proof stress of between about 95 ksi (655 MPa) and 110 ksi (758 MPa), and the RT elongation of between about 35% and 45% after the alloy is annealed at 788°C (1450°F) for four hours and then air cooled.
[0018] In some variations, the alloy has a room temperature (RT) ultimate tensile strength of between about 175 ksi (1207 MPa) and about 195 ksi (1344 MPa), an RT 0.2% yield strength of between about 105 ksi (724 MPa) and 125 ksi (861 MPa), and an RT elongation of between about 15% and 30% after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours, followed by air cooling. And, in at least one variation, after annealing the alloy at 788°C (1450°F) for 4 hours followed by air cooling and aging the alloy at 700°C (1292°F) for 1000 hours followed by air cooling, the RT ultimate tensile strength is between about 175 ksi (1207 MPa) and about 185 ksi (1275 MPa), the RT 0.2% proof stress is between about 105 ksi (724 MPa) and 120 ksi (827 MPa), and the RT elongation is between about 22% and 30%.
[0019] In some variations, the alloy has an RT ultimate tensile strength of between about 170 ksi (1172 MPa) and about 200 ksi (1379 MPa), an RT 0.2% proof strength of between about 100 ksi (689 MPa) and about 120 ksi (827 MPa), and an RT elongation of between about 16% and 30% after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours, followed by air cooling. And, in at least one variation, after annealing the alloy at 788°C (1450°F) for 4 hours followed by air cooling and aging the alloy at 700°C (1292°F) for 5000 hours followed by air cooling, the RT ultimate tensile strength is between about 175 ksi (1207 MPa) and about 190 ksi (1310 MPa), the RT 0.2% proof stress is between about 105 ksi (724 MPa) and about 115 ksi (793 MPa), and the RT elongation is between about 20% and 30%.
[0020] In some variations, the alloy has a 700°C ultimate tensile strength of between about 130 ksi (896 MPa) and about 155 ksi (1069 MPa), a 700°C 0.2% yield strength of between about 90 ksi (620 MPa) and about 105 ksi (724 MPa), and a 700°C elongation of between about 9% and 25% after the alloy is annealed at 788°C (1450°F) for four hours followed by air cooling. And, in at least one variation, the alloy, after annealing at 788°C (1450°F) for four hours followed by air cooling, has a 700°C ultimate tensile strength of between about 125 ksi (861 MPa) and about 140 ksi (965 MPa), a 700°C 0.2% yield strength of between about 90 ksi (620 MPa) and about 100 ksi (689 MPa), and a 700°C elongation of between about 14% and 20%.
[0021] In some variations, the alloy has a 700°C ultimate tensile strength of between about 135 ksi (931 MPa) and about 155 ksi (1069 MPa), a 700°C 0.2% yield strength of between about 95 ksi (655 MPa) and about 110 ksi (758 MPa), and a 700°C elongation of between about 12% and 30% after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours, followed by air cooling. And, in at least one variation, after annealing the alloy at 788°C (1450°F) for 4 hours and then air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours and then air cooling, the 700°C ultimate tensile strength is between about 135 ksi (931 MPa) and about 150 ksi (1034 MPa), the 700°C 0.2% yield strength is between about 95 ksi (655 MPa) and 105 ksi (724 MPa), and the 700°C elongation is between about 15% and 30%.
[0022] In some variations, the alloy has a 700°C ultimate tensile strength of between about 130 ksi (896 MPa) and about 150 ksi (1034 MPa), a 700°C 0.2% yield strength of between about 90 ksi (620 MPa) and about 110 ksi (758 MPa), and a 700°C elongation of between about 15% and 28% after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours, followed by air cooling. And, in at least one variation, after annealing the alloy at 788°C (1450°F) for 4 hours and then air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours and then air cooling, the 700°C ultimate tensile strength is between about 130 ksi (896 MPa) and about 145 ksi (1034 MPa), the 700°C 0.2% yield strength is between about 90 ksi (620 MPa) and 102 ksi (703 MPa), and the 700°C elongation is between about 15% and 25%.
[0023] In some variations, the alloy has a composition including, in weight percent, about 0.02% to about 0.3% manganese, about 0.05% to about 0.3% silicon, about 0.005% to about 0.2% vanadium, about 0.005% to about 0.2% zirconium, about 0.001% to about 0.025% boron, and about 0.001% to about 0.02% nitrogen.
[0024] In another aspect of the present disclosure, the alloy contains, in weight percent, about 1.3% to about 1.8% aluminum, about 0.001% to about 0.025% boron, about 0.01% to about 0.05% carbon, about 2.0% to about 3.0% cobalt, about 18.0% to about 22.0% chromium, about 4.0% to about 10.0% iron, about 0.02% to about 0.3% manganese, about 1.0% to about 3.0% chromium. The alloy has a composition consisting essentially of molybdenum, about 1.0% to about 2.5% niobium, about 0.001% to about 0.02% nitrogen, about 0.05% to about 0.3% silicon, about 1.3% to about 1.8% titanium, about 0.8% to about 1.2% tungsten, about 0.005% to about 0.2% vanadium, about 0.005% to about 0.2% zirconium, the balance nickel and incidental impurities. In some variations, the alloy has a stress rupture life of at least 300 hours at 700°C and 393.7 MPa (57.1 ksi), and a room temperature elongation of at least 15% after aging for 1,000 hours at 700°C.
[0025] Further areas of applicability will become apparent from the description provided herein. It should be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. [Brief description of the drawings]
[0026] In order that the present disclosure may be more fully understood, various forms thereof will now be described by way of example only and with reference to the accompanying drawings, in which:
[0027] [Figure 1] FIG. 1 is an SEM micrograph showing the microstructure of a high strength, thermally stable nickel-base alloy according to the teachings of the present disclosure.
[0028] [Diagram 2] FIG. 2 shows a higher magnification of a portion of the micrograph of FIG. 1 with multiple locations analyzed by energy dispersive spectroscopy (EDS).
[0029] [Diagram 3] FIG. 3 shows the results of EDS analysis of a portion of the microstructure of FIGS.
[0030] The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way. Detailed Description of the Invention
[0031] The following description is merely exemplary in nature and is not intended to limit the present disclosure, application, or uses. It should be understood that corresponding reference numerals throughout the drawings indicate like or corresponding parts and features. It should be understood that composition values in this application are expressed as weight percent (hereinafter "wt %" or simply "%") unless otherwise specified.
[0032] With reference to Table 1, the compositions of eighteen experimental heats (heats 1-18) and one heat (heat 19) of a commercially available alloy are shown. The commercially available alloy heat is an Inconel® nickel-chromium brand alloy, more specifically 740H® (hereinafter referred to as "Alloy 740H"). With reference to Table 2, three additional experimental heats (heats 20-22) are shown.
[0033] The experimental alloys contain various ranges of carbon (C), iron (Fe), silicon (Si), nickel (Ni), chromium (Cr), aluminum (Al), titanium (Ti), cobalt (Co), molybdenum (Mo), niobium (Nb), and tungsten (W). Additionally, small amounts (i.e., less than about 0.10 wt%) of manganese (Mn), sulfur (S), copper (Cu), tantalum (Ta), phosphorus (P), boron (B), vanadium (V), and zirconium (Zr) are included as impurities, trace elements, deoxidizing elements, and / or grain boundary strengthening additions, as described in more detail below. Additionally, calcium (Ca), magnesium (Mg), and rare earth metals such as cesium, lanthanum, and yttrium may be present as trace elements with desulfurizing and deoxidizing properties. [Table 1] [Table 2]
[0034] Carbon (C) is added to control grain growth during processing and to increase creep strength. Excessive amounts of grain boundary carbides can impair the ductility of the alloys in the present disclosure. Primary MC-type carbides formed with niobium and titanium can also form large amounts of stringers, which also impacts the amount of gamma prime strengthening phase that can form. Thus, the amount of C is between about 0.005% and about 0.1%. In some variations, the amount of C in the alloy is between about 0.0075% and about 0.075%, such as between about 0.01% and about 0.075%. In at least one variation, the amount of C in the alloy is between about 0.01% and about 0.05%.
[0035] Manganese (Mn) is added as a deoxidizer. However, excessive amounts of Mn can impair the thermal stability and ductility of the disclosed alloys. Thus, the amount of Mn is between about 0.05% and about 0.3%. In some variations, the amount of Mn in the alloy is between about 0.075% and about 0.25%, such as between about 0.075% and about 0.2%. In at least one variation, the amount of Mn in the alloy is between about 0.09% and about 0.15%.
[0036] Iron (Fe) is added to reduce the manufacturing cost of the alloy. However, the addition of excessive Fe may impair the thermal stability and ductility of the alloy of the present disclosure. Thus, the amount of Fe is between about 3.0% and about 15.0%. In some variations, the amount of Fe in the alloy is between about 4.0% and about 12.5%, such as between about 4.0% and about 10.0%. In at least one variation, the amount of Fe in the alloy is between about 4.0 and about 9.0%, such as between about 5.0 and about 10.0%.
[0037] Silicon (Si) is added as a deoxidizer, similar to Mn. However, excessive amounts of Si may impair the weldability, thermal stability, and ductility of the alloys of the present disclosure. Thus, the amount of Si is between about 0.05% and about 0.3%. In some variations, the amount of Si in the alloy is between about 0.075% and about 0.25%, such as between about 0.1% and about 0.2%. In at least one variation, the amount of Si in the alloy is between about 0.11% and about 0.18%.
[0038] Nickel (Ni) improves metallurgical stability, high temperature corrosion resistance, and weldability, and also provides for the formation of the gamma prime strengthening phase.
[0039] Chromium (Cr) is added to enhance high temperature corrosion resistance. However, excessive Cr addition can impair high temperature strength and promote the formation of deleterious sigma phases in the disclosed alloys. Thus, the amount of Cr is between about 17.0% and about 23.0%. In some variations, the amount of Cr in the alloy is between about 18.0% and about 22.0%, such as between about 19.0% and about 21.0%.
[0040] Aluminum (Al) is added to form the Ni3Al gamma prime phase. However, excessive Al additions may impair the hot formability of the disclosed alloys. Thus, the amount of Al is between about 1.0% and about 2.5%. In some variations, the amount of Al in the alloy is between about 1.1% and about 2.0%, e.g., between about 1.3% and about 1.9%. In at least one variation, the amount of Al in the alloy is between about 1.2% and about 1.8%, e.g., between about 1.3% and about 1.9%.
[0041] Titanium (Ti) may also be added to form the gamma prime phase and may substitute for Al. However, excessive Ti addition may impair the hot formability of the disclosed alloys. Thus, the amount of Ti is between about 1.0% and about 2.5%. In some variations, the amount of Ti in the alloy is between about 1.1% and about 2.0%, e.g., between about 1.3% and about 1.9%. In at least one variation, the amount of Ti in the alloy is between about 1.2 and about 1.8%, e.g., between about 1.3 and about 1.9%.
[0042] Cobalt (Co) promotes high temperature strength and correlates with improved fracture ductility. However, excessive Co additions increase the cost of the disclosed alloys. Thus, the amount of Co is between about 1.0% and about 3.0%. In some variations, the amount of Co in the alloy is between about 1.5% and about 3.0%, such as between about 1.6% and about 3.0%. In at least one variation, the amount of Co in the alloy is between about 1.7% and about 3.0%, such as between about 1.8% and about 3.0%.
[0043] Molybdenum (Mo) provides a solid solution strengthening effect, thereby promoting fracture strength at high temperatures. However, excessive Mo additions can result in the formation of topologically close packed (TCP) phases that can impair the ductility of the disclosed alloys after prolonged exposure to high temperatures. Thus, the amount of Mo is between about 0.8% and about 3.5%. In some variations, the amount of Mo in the alloy is between about 1.0% and about 3.0%, such as between about 1.0% and about 2.9%. In at least one variation, the amount of Mo in the alloy is between about 1.0% and about 2.8%, such as between about 1.0% and about 2.7%.
[0044] Niobium (Nb) is added for solid solution strengthening and can replace Al in the gamma prime phase. However, excessive Nb addition can impair the hot formability, ductility and impact strength of the alloys of the present disclosure after prolonged exposure to high temperatures. Thus, the amount of Nb is between about 1.0% and about 3.0%. In some variations, the amount of Nb in the alloy is between about 1.0% and about 2.8%, such as between about 1.0% and about 2.7%. In at least one variation, the amount of Nb in the alloy is between about 1.0% and about 2.6%, such as between about 1.2% and about 2.7%. It should be understood that in some variations of the present disclosure, tantalum (Ta) can replace some or all of the Nb. For example, in at least one variation, Nb is less than 1.0% and Ta is added up to 1.0%.
[0045] The addition of boron (B) and zirconium (Zr) provides grain boundary strengthening and improves high temperature ductility. However, excessive addition of B and / or Zr may impair the hot formability and weldability of the alloys in the present disclosure. Thus, the amount of B is between about 0.001% and about 0.025%. In some variations, the amount of B in the alloy is between about 0.002% and about 0.02%, such as between about 0.003% and about 0.015%. In at least one variation, the amount of B is between about 0.003% and about 0.01%. Also, the amount of Zr is between about 0.001% and about 0.05%. In some variations, the amount of Zr in the alloy is between about 0.005% and about 0.04%, such as between about 0.0075% and about 0.03%. In at least one variation, the amount of Zr is between about 0.01% and about 0.02%.
[0046] Similar to Mo, tungsten (W) provides a solid solution strengthening effect, thereby promoting high temperature fracture strength. However, excessive W addition can result in the formation of TCP (topologically close packed) phases that can impair the alloys of the present disclosure after prolonged exposure to high temperatures. Thus, the amount of W is between about 0.75% and about 2.0%. In some variations, the amount of W in the alloy is between about 0.8% and about 1.5%, such as between about 0.9% and about 1.3%. In at least one variation, the amount of W in the alloy is between about 0.9% and about 1.2%, such as between about 0.8% and about 1.2%.
[0047] It should also be understood that the element ranges discussed herein include all increments between the minimum and maximum alloying element composition values. That is, the minimum alloying element composition values can range from the minimum to the maximum. Similarly, the maximum alloying element composition values can range from the maximum values shown to the minimum values discussed. For example, the minimum Ti content can be 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, and any values between these increments, and the maximum Ti content can be 2.5, 2.4, 2.3, 2.2, 2.1, 2.0, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, 1.1, 1.0, and any values between these increments.
[0048] With further reference to Tables 1 and 2, heats 2, 5, 6, 7, 10, 12, and 20-22 are examples of compositions according to the teachings of the present disclosure. In particular, heats 2, 5, 6, 7, 10, 12, and 20-22 have chemical compositions within the scope of the teachings of the present disclosure. Additionally, heats 2, 5, 6, 7, 10, 12, and 20-22 have at least one desirable property with respect to cost, mechanical strength, ductility, thermal stability, and / or high temperature corrosion.
[0049] In some variations of the present disclosure, alloys according to the teachings of the present disclosure have a combination of desirable properties with respect to cost, mechanical strength, ductility, and / or high temperature corrosion, as described in more detail below.
[0050] Experimental alloy heats were melted in a vacuum induction melting (VIM) furnace and cast into 4-inch (10.2 cm) diameter molds to form 50 pound (22.7 kg) ingots. The ingots were heated at 2200 °F (1204 °C) for 16 hours, then the temperature was reduced to 2100 °F (1149 °C) for initial hot rolling, and reheated at 2075 °F (1135 °C) for additional hot rolling until a 0.5-inch (1.27 cm) thick hot rolled plate was produced. The 0.5-inch (1.27 cm) thick hot rolled plate was "solution annealed" at 2000 °F (1093 °C) for 1 hour, then water cooled, and then "aged" at 1450 °F (788 °C) for 4 hours. All experimental heat samples examined in this "solution annealed + aged" condition had an ASTM #2-4 grain size.
[0051] The commercial alloy heat (i.e., Heat 19) was initially hot rolled from 1.5 inch (3.8 cm) commercial plate at 2100°F (1149°C) and reheated at 2075°F (1135°C) when the material was processed into 0.5 inch (1.27 cm) thick hot rolled plate. The 0.5 inch (1.27 cm) thick hot rolled plate of Heat 19 was solution annealed at 2025°F (1107°C) for 1 hour, then water quenched and aged at 1472°F (800°C) for 4 hours, then air cooled. All commercial alloy heat samples tested in this solution annealed + aged condition also had an ASTM #2-4 grain size.
[0052] In addition to the heat samples shown in Tables 1 and 2 that were provided (and tested) in the solution annealed + aged condition, some solution annealed + aged samples were subjected to an additional aging of 1,000 hours at 700°C (1292°F) ("700°C / 1,000 hours / AC") and then air cooled or subjected to an additional aging of 5.0 hours at 700°C (1292°F). Thus, the samples were divided into solution annealed + aged condition, solution annealed + aged + 700°C / 1,000hr / AC condition (also referred to herein simply as the "700°C / 1,000hr / AC condition" or the "700°C / 1,000hr / AC sample"), and solution annealed + aged + 700°C / 5,000hr / AC condition (also referred to herein simply as the "700°C / 5,000hr / AC condition" or the "700°C / 5,000hr / AC sample").
[0053] Referring to Tables 3 and 4, room temperature (RT) tensile data is provided for samples tested in the solution annealed + aged condition. [Table 3] [Table 4]
[0054] As shown in Tables 3 and 4, heats having compositions within the teachings of the present disclosure (i.e., heats 2, 5, 6, 7, 10, 12, and 20-21) have a minimum RT ultimate tensile strength (UTS) of 1108.7 megapascals (MPa) (160.8 kilopounds per square inch (ksi)), a minimum RT 0.2% yield strength (YS) of 680.5 MPa (98.7 ksi), a minimum RT elongation of 35%, and a minimum RT reduction in area (ROA) of 37%. That is, in some variations, alloys having compositions within the teachings of the present disclosure in the solution annealed + aged condition have a minimum RT UTS of 1108.7 MPa (160.8 ksi), a minimum RT YS of 680.5 MPa (98.7 ksi), a minimum RT elongation of 35%, and a minimum RT ROA of 37%. In comparison, heat 9 in the solution annealed + aging condition has an RT elongation of 31%, an RT ROA of 28%, heat 11 in the solution annealed + aging condition has an RT elongation of 33%, heat 13 in the solution annealed + aging condition has an RT elongation of 34%, and heat 17 in the solution annealed + aging condition has an RT elongation of 33%.
[0055] Additionally, commercial alloy heat 19 has an RT UTS of 167.5 ksi, an RT 0.2% YS of 103.6 ksi, an RT elongation of 37%, and an RT ROA of 45%. Thus, an alloy having a composition within the teachings of the present disclosure in the solution annealed + aged condition has an RT UTS equal to about 0.96 of the RT UTS of alloy 740H, an RT YS equal to about 0.95 of the RT YS of alloy 740H, an RT elongation equal to about 0.95 of the RT elongation of alloy 740H, and an RT ROA equal to about 0.82 of the RT ROA of alloy 740H. Also, an alloy having a composition within the teachings of the present disclosure has a Co content that is only about 0.125 of the Co content of alloy 740H.
[0056] Referring to Tables 5 and 6 below, RT tensile data for samples tested at 700° C. / 1,000 hr / AC conditions is shown. [Table 5] [Table 6]
[0057] As shown in Tables 5 and 6, heats 2, 5, 6, 7, 10, 12, and 20-21 have a minimum RT UTS of 1211.5 MPa (175.7 ksi), a minimum RT YS of 746 MPa (108.2 ksi), a minimum RT Elongation of 19%, and a minimum RT ROA of 20%. That is, in some variations, alloys having compositions within the teachings of the present disclosure at the 700°C / 1,000 hr / AC condition have a minimum RT UTS of 1211.5 MPa (175.7 ksi), a minimum RT YS of 746 MPa (108.2 ksi), a minimum RT Elongation of 19%, and a minimum RT ROA of 19%. In comparison, heats 16 and 18 in the 700°C / 1000hr / AC condition have an RT elongation of less than 19%, and heats 16, 17, and 18 in the 700°C / 1000hr / AC condition have an RT ROA of less than 20%. Additionally, commercial alloy heat 19 in the 700°C / 1000hr / AC condition has an RT UTS of 1249.4 MPa (181.2 ksi), an RT 0.2% YS of 810.9 MPa (117.6 ksi), an RT elongation of 26%, and an RT ROA of 29%. Thus, an alloy having a composition within the teachings of the present disclosure at the 700°C / 1,000hrs / AC condition has an RT UTS equal to about 0.97 of alloy 740H, an RT YS equal to about 0.92 of alloy 740H, an RT elongation equal to about 0.73 of alloy 740H, and an RT ROA equal to about 0.69 of alloy 740H.
[0058] Referring to Tables 7 and 8, the RT tensile data for samples at 700° C. / 5000 hr / AC conditions is shown. [Table 7] [Table 8]
[0059] As shown in Tables 7 and 8, heats 2, 5, 6, 10, 12, and 20-22 (heat 7 was not tested) have a minimum RT UTS of 1235.6 MPa (179.2 ksi), a minimum RT YS of 730.9 MPa (106.0 ksi), a minimum RT Elongation of 17%, and a minimum RT ROA of 18%. That is, in some variations, alloys having compositions within the teachings of the present disclosure at the 700°C / 5,000 hr / AC condition have a minimum RT UTS of 1235.6 MPa (179.2 ksi), a minimum RT YS of 730.9 MPa (106 ksi), a minimum RT Elongation of 17%, and a minimum RT ROA of 18%. Additionally, commercial alloy heat 19 at 700°C / 5,000hr / AC condition has an RT UTS of 1266.6 MPa (183.7 ksi), an RT 0.2% YS of 759.1 MPa (110.1 ksi), an RT elongation of 26%, and an RT ROA of 30%. Thus, an alloy having a composition within the teachings of the present disclosure at 700°C / 5,000hr / AC condition has an RT UTS equal to about 0.98 of the RT UTS of alloy 740H, an RT YS equal to about 0.96 of the RT YS of alloy 740H, an RT elongation equal to about 0.65 of the RT elongation of alloy 740H, and an RT ROA equal to about 0.60 of the RT ROA of alloy 740H.
[0060] Referring to Tables 9 and 10, 700°C (1292°F) tensile data for samples in the solution annealed + aged condition is shown. [Table 9] [Table 10]
[0061] As shown in Tables 9 and 10, heats having compositions within the teachings of the present disclosure in the solution annealed + aged condition (i.e., heats 2, 5, 6, 7, 10, 12, and 20-21) have a minimum 700°C UTS of 909.5 MPa (131.9 ksi), a minimum 700°C YS of 651.6 MPa (94.5 ksi), a minimum 700°C elongation of 16.7%, and a minimum 700°C reduction in area (ROA) of 19.5%. That is, in some variations of the present disclosure, alloys having compositions within the teachings of the present disclosure in the solution annealed + aged condition have a minimum 700°C UTS of 909.5 MPa (131.9 ksi), a minimum 700°C YS of 651.6 MPa (94.5 ksi), a minimum 700°C elongation of 16.7%, and a minimum 700°C ROA of 19.5%. In comparison, heat 1 in the solution annealed + aged condition has a 700°C elongation of 11.3% and a 700°C ROA of 15.3%, heat 3 in the solution annealed + aged condition has a 700°C elongation of 15.2% and a 700°C ROA of 16.4%, and heat 11 in the solution annealed + aged condition has a 700°C elongation and 700°C ROA of 9.5%, and a minimum 700°C ROA of 19.5%. Heat 13 in the solution annealed + aged condition has a 700°C elongation of 15.0% and a 700°C ROA of 16.5%, Heat 17 in the solution annealed + aged condition has a 700°C elongation of 14.7% (2 samples) average and a 700°C ROA of 19.0%, and Heat 18 in the solution annealed + aged condition has a 700°C elongation of 15.0% (2 samples) average and a 700°C ROA of 18.3%.
[0062] Additionally, commercial alloy heat 19 in the solution annealed + aged condition has a 700°C UTS of 960.5 MPa (139.3 ksi), a 700°C 0.2% YS of 630.2 MPa (91.4 ksi), a 700°C elongation of 29.5%, and a 700°C ROA of 30%. Thus, an alloy having a composition within the teachings of the present disclosure in the solution annealed + aged condition has a 700°C UTS equal to about 0.95 of the 700°C UTS of alloy 740H, a 700°C YS equal to about 1.0 of the 700°C YS of alloy 740H, a 700°C elongation equal to about 0.57 of the 700°C elongation of alloy 740H, and a 700°C ROA equal to about 0.65 of the 700°C ROA of alloy 740H.
[0063] Referring to Tables 11 and 12, 700°C (1292°F) tensile data for samples in the 700°C / 1,000hr / AC condition is shown. [Table 11] [Table 12]
[0064] As shown in Tables 11 and 12, heats 2, 5, 6, 10, 12, and 20-21 (heat 7 was not tested) in the 700°C / 1,000hr / AC condition have a minimum 700°C UTS of 142.7 ksi, a minimum 700°C YS of 98.8 ksi, a minimum 700°C elongation of 20.5%, and a minimum 700°C ROA of 22.0%. That is, in some variations of the present disclosure, alloys having compositions within the teachings of the present disclosure in the 700°C / 1,000hr / AC condition have a minimum 700°C UTS of 142.7 ksi, a minimum 700°C YS of 98.8 ksi, a minimum 700°C elongation of 20.5%, and a minimum 700°C ROA of 22.0%. In comparison, heat 11 at 700°C / 1000hr / AC has a 700°C elongation of 15.0% and a 700°C ROA of 16.5%. Additionally, commercial alloy heat 19 at 700°C / 1000hr / AC has a 700°C UTS of 987.4 MPa (143.2 ksi), a 700°C 0.2% YS of 686.7 MPa (99.6 ksi), a 700°C elongation of 25.5%, and a 700°C ROA of 31%. Thus, an alloy having a composition within the teachings of the present disclosure at the 700°C / 1,000hrs / AC condition will have a 700°C UTS equal to about 1.0 of the 700°C UTS of alloy 740H, a 700°C YS equal to about 1.0 of the 700°C YS of alloy 740H, a 700°C elongation equal to about 0.80 of the 700°C elongation of alloy 740H, and a 700°C ROA equal to about 0.71 of the 700°C ROA of alloy 740H.
[0065] Referring to Tables 13 and 14, 700°C (1292°F) tensile data for samples in the 700°C / 5,000hr / AC condition is shown. [Table 13] [Table 14]
[0066] As shown in Tables 13 and 14, heats 2, 5, 6, 10, 12, and 20-22 (heat 7 was not tested) in the 700°C / 5,000hr / AC condition have a minimum 700°C UTS of 940.5 MPa (136.4 ksi), a minimum 700°C YS of 667.4 MPa (96.8 ksi), a minimum 700°C elongation of 20.0%, and a minimum 700°C ROA of 26.0%. That is, in some variations of the present disclosure, alloys having compositions within the teachings of the present disclosure in the 700°C / 5,000hr / AC condition have a minimum 700°C UTS of 940.5 MPa (136.4 ksi), a minimum 700°C YS of 667.4 MPa (96.8 ksi), a minimum 700°C elongation of 20.0%, and a minimum 700°C ROA of 26.0%. In comparison, Heat 11 at 700°C / 5,000hrs / AC condition has a 700°C elongation of 18.0% and a 700°C ROA of 22.5%.
[0067] Additionally, commercial alloy heat 19 at 700°C / 5000hrs / AC condition has a 700°C UTS of 137.6ksi, a 700°C 0.2% YS of 99.5ksi, a 700°C elongation of 26.5%, and a 700°C ROA of 37.5%. Thus, an alloy having a composition within the teachings of the present disclosure at 700°C / 5000hrs / AC condition has a 700°C UTS equal to about 0.99 of alloy 740H's 700°C UTS, a 700°C YS equal to about 0.97 of alloy 740H's 700°C YS, a 700°C elongation equal to about 0.76 of alloy 740H's 700°C elongation, and a 700°C ROA equal to about 0.69 of alloy 740H's 700°C ROA.
[0068] Referring to Table 15, RT impact test data for samples in the solution annealed + aged condition is shown. [Table 15]
[0069] As shown in Table 15, heats having compositions within the teachings of the present disclosure in the solution annealed + aged condition (i.e., heats 2, 5, 6, 7, 10, and 12) had a melting point of 87.0 J / cm 2 (51.3 Ft.lb), i.e., in some variations of the present disclosure, alloys having compositions within the teachings of the present disclosure in the solution annealed + aged condition have a minimum RT impact energy of 87.0 J / cm 2 (51.3 Ft.lb) minimum RT impact energy, compared to 80.9 J / cm for Heat 1 in the solution annealed + aged condition. 2 (47.7 ft.lb) RT impact energy, and Heat 8 in the solution annealed + aged condition had an RT impact energy of 77.6 J / cm 2 (45.8 ft.lb) RT impact energy, and Heat 9 in the solution annealed + aged condition had an RT impact energy of 76.8 J / cm 2 (45.3 ft.lb). Additionally, commercial alloy heat 19 in the solution annealed + aged condition has an RT impact energy of 114.7 J / cm 2 (67.7 ft.lb). Thus, an alloy having a composition within the teachings of the present disclosure in the solution annealed + aged condition has an RT impact energy equal to about 0.76 of the RT impact energy of alloy 740H.
[0070] Referring to Tables 16 and 17, RT impact test data for samples at 700° C. / 1000 hr / AC conditions is shown. [Table 16] [Table 17]
[0071] As shown in Tables 16 and 17, heats having compositions within the teachings of the present disclosure (i.e., heats 2, 5, 6, 7, 10, 12, and 20-22) at 700°C / 1,000hr / AC conditions had a yield of 23.7 J / cm 2(14.0 Ft.lb), i.e., in some variations of the present disclosure, alloys having compositions within the teachings of the present disclosure at 700°C / 1,000hr / AC conditions have a minimum RT impact energy of 23.7 J / cm 2 (14.0 Ft.lb) minimum RT impact energy. In comparison, Heat 4 at 700°C / 1,000hrs / AC had a minimum RT impact energy of 23.2 J / cm 2 (13.7 ft.lb) RT impact energy, and Heat 15 at 700°C / 1,000hrs / AC is 17.3 J / cm 2 (10.2 ft.lb) RT impact energy, and Heat 16 at 700°C / 1,000hrs / AC is 15.7 J / cm 2 (9.3 ft.lb) RT impact energy, and Heat 17 at 700°C / 1,000hrs / AC was 13.4 J / cm 2 (7.9 ft.lb) RT impact energy, and Heat 18 at 700°C / 1,000hrs / AC is 12.3 J / cm 2 (7.2 ft.lb). Additionally, commercial alloy heat 19 at 700°C / 1,000hrs / AC has an RT impact energy of 24.3 J / cm 2 (14.3 ft.lb). Thus, alloys having compositions within the teachings of the present disclosure in the solution annealed + aged condition have RT impact energies equal to about 0.98 of the 700°C RT impact energy of alloy 740H.
[0072] Referring to Table 18, stress rupture data at 700°C (1292°F) is shown for samples in the solution annealed + aged condition. As shown in Table 18, heats 2, 5, 6, and 10 (heat 7 was not tested) in the solution annealed + aged condition have minimum stress rupture lives of 1,396 hours (h) at 700°C (1292°F) under a stress of 393.7 MPa (57.1 ksi). In comparison, heats 1, 3, 8, 9, 11, 13, and 14 in the solution annealed + aged condition have stress rupture lives of 1197.5 hours, 1055 hours, 1124.5 hours, 1079 hours, 464 hours, 678 hours, and 692 hours, respectively, at 700°C (1292°F) under a load of 393.7 MPa (57.1 ksi). [Table 18]
[0073] Additionally, alloys having compositions within the teachings of the present disclosure in the solution annealed + aged condition have a minimum stress rupture life at 700°C (1292°F) equal to about 0.99 (as an estimate from a combination of known data for Alloy 740H) of the minimum stress rupture life at 700°C (1292°F) of Alloy 740H under a stress of 393.7 MPa (57.1 ksi).
[0074] As discussed above with respect to Tables 1-18, the teachings of the present disclosure provide Ni-base alloys having a desirable combination of mechanical properties and low Co content. In other words, the teachings of the present disclosure provide Ni-base alloys having similar mechanical properties to alloy 740H, but with significantly less Co, and therefore reduced cost. In particular, alloys having compositions within the scope of the teachings of the present disclosure have an RT UTS of at least 0.96 of alloy 740H, an RT YS of at least 0.92 of alloy 740H, an RT elongation of at least 0.65 of alloy 740H, and an RT ROA of at least 0.60 of alloy 740H. Also, alloys having compositions within the teachings of the present disclosure have a 700° C. UTS of at least 0.95 of the 700° C. UTS of alloy 740H, a 700° C. YS of at least 0.97 of the 700° C. YS of alloy 740H, a 700° C. elongation of at least 0.57 of the 700° C. elongation of alloy 740H, and a 700° C. ROA of at least 0.65 of the 700° C. ROA of alloy 740H, and an RT impact energy equal to at least 0.76 of the RT impact energy of alloy 740H, and a stress rupture life at 700° C. (1292° F.) and 393.7 MPa (57.1 ksi) of at least 0.99 of the stress rupture life at 700° C. (1292° F.) and 393.7 MPa (57.1 ksi) of alloy 740H. Thus, an alloy is provided with lower cost, higher temperature mechanical and corrosion resistance properties compared to Alloy 740H for use in environments or industries such as USC and A-USC boilers, and power systems using supercritical CO2 (sCO2) as the heat transfer medium, which can be used in high temperature fasteners, springs and valves. Additionally, the high nickel content provides the alloy with good weldability and fabricability.
[0075] Referring to Figures 1-2, SEM (Scanning Electron Microscopy) images of stress fracture specimens from one heat are shown and Energy Dispersive Spectroscopy (EDS) results are shown in Figure 3. Based on EDS analysis, two types of precipitates were identified. First, Nb, Ti and carbide precipitates were identified and second, Cr, Mo precipitates were identified. As shown, the grain boundaries of the alloy according to the present disclosure are well defined and in some forms of the present disclosure, the grain size is ASTM#2-4 with an average grain size of about 100 μm. SEM and X-ray diffraction analysis showed mainly chromium rich carbides (M23C6) on the grain boundaries with MC type carbonitrides (Nb, Ti rich) mainly intragranularly.
[0076] Unless expressly indicated herein, all numerical values expressing mechanical / thermal properties, composition percentages, dimensions and / or tolerances, or other characteristics should be understood as being modified by the word "about" or "approximately" when describing the scope of this disclosure. This variation is desirable for a variety of reasons, including industrial practices, materials, manufacturing, assembly tolerances, and testing capabilities.
[0077] As used herein, the phrase "at least one of A, B, and C" should be interpreted to mean (A or B or C) using a non-exclusive logical OR, and not to mean "at least one of A, at least one of B, and at least one of C."
[0078] The description of the disclosure is merely exemplary in nature and, thus, variations that do not depart from the gist of the disclosure are intended to be within the scope of the disclosure. Such variations should not be considered as a departure from the spirit and scope of the disclosure.
Claims
1. In weight percent: 1.3% to 1.8% aluminum; 1.5% to 4.0% Cobalt; 18.0% to 22.0% chromium; 4.0% to 10.0% iron; 1.0% to 3.0% molybdenum; 1.0% to 2.5% niobium; 1.3% to 1.8% titanium; 0.8% to 1.2% tungsten; 0.01% to 0.08% carbon; and Remaining nickel and incidental impurities; having a composition consisting of: A stress rupture life at 700° C. and 393.7 MPa (57.1 ksi) of at least 300 hours; and An alloy having a room temperature elongation of at least 19% after aging at 700°C for 1,000 hours.
2. 2. The alloy of claim 1, wherein said cobalt is from 2.0% to 3.0%.
3. 2. The alloy of claim 1, wherein said molybdenum is from 1.0% to 2.75%.
4. 2. The alloy of claim 1, wherein said niobium is from 1.0% to 1.75%.
5. 2. The alloy of claim 1, wherein said cobalt is from 2.0% to 3.0% and said molybdenum is from 1.0% to 2.75%.
6. 2. The alloy of claim 1, wherein said cobalt is from 2.0% to 3.0% and said niobium is from 1.0% to 1.75%.
7. 2. The alloy of claim 1, wherein said molybdenum is from 1.0% to 2.75% and said niobium is from 1.0% to 1.75%.
8. 2. The alloy of claim 1, wherein said cobalt is 2.0% to 3.0%, said molybdenum is 1.0% to 2.75%, and said niobium is 1.0% to 1.75%.
9. 10. The alloy of claim 1, having a stress rupture life at 700°C and 393.7 MPa (57.1 ksi) of at least 500 hours.
10. 2. The alloy of claim 1, wherein said room temperature elongation is at least 20% after aging at 700°C for 1000 hours.
11. 2. The alloy of claim 1, wherein said room temperature elongation is at least 22% after aging at 700°C for 1000 hours.
12. The alloy of claim 1, having a room temperature elongation of at least 15% after aging at 700°C for 5000 hours.
13. 2. The alloy of claim 1, wherein said room temperature elongation is at least 20% after aging at 700°C for 5000 hours.
14. The alloy of claim 1, having a room temperature impact energy of at least 16.272 Nm (12 ft-lb) when aged for 1000 hours at 700°C.
15. 15. The alloy of claim 14, wherein the room temperature impact energy is at least 20.34 Nm (15 ft-lb) when aged for 1000 hours at 700°C.
16. 16. The alloy of claim 15, wherein the room temperature impact energy is at least 27.12 Nm (20 ft-lb) when aged for 1000 hours at 700°C.
17. The alloy of claim 1, having a room temperature impact energy of at least 13.56 Nm (10 ft-lb) when aged for 5000 hours at 700°C.
18. 2. The alloy of claim 1, wherein the room temperature impact energy of the alloy is at least 12 ft-lb (16.272 Nm) when aged for 5000 hours at 700°C.
19. 2. The alloy of claim 1, wherein the room temperature impact energy of the alloy is at least 20.34 Nm (15 ft-lb) when aged at 700° C. for 5000 hours.
20. 2. The alloy of claim 1, wherein the alloy has a room temperature (RT) ultimate tensile strength of between 1104 MPa (160 ksi) and 1207 MPa (175 ksi), a RT 0.2% yield strength of between 655 MPa (95 ksi) and 793 MPa (115 ksi), and a RT elongation of between 30% and 45%, after annealing at 788°C (1450°F) for 4 hours followed by air cooling.
21. 21. The alloy of claim 20, wherein, after annealing at 788°C (1450°F) for 4 hours followed by air cooling, the RT ultimate tensile strength is between 1104 MPa (160 ksi) and 1172 MPa (170 ksi), the RT 0.2% yield strength is between 655 MPa (95 ksi) and 758 MPa (110 ksi), and the RT elongation is between 35% and 45%.
22. 2. The alloy of claim 1, wherein the room temperature (RT) ultimate tensile strength is between 1207 MPa (175 ksi) and 1344 MPa (195 ksi), the RT 0.2% proof stress is between 724 MPa (105 ksi) and 861 MPa (125 ksi), and the RT elongation is between 15% and 30%, after annealing at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours, followed by air cooling.
23. 23. The alloy of claim 22, wherein after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours, followed by air cooling, the RT ultimate tensile strength is between 1207 MPa (175 ksi) and 1275 MPa (185 ksi), the RT 0.2% proof stress is between 724 MPa (105 ksi) and 827 MPa (120 ksi), and the RT elongation is between 22% and 30%.
24. 2. The alloy of claim 1, wherein the room temperature (RT) ultimate tensile strength is between 1172 MPa (170 ksi) and 1379 MPa (200 ksi), the RT 0.2% yield strength is between 689 MPa (100 ksi) and 827 MPa (120 ksi), and the RT elongation is between 16% and 30%, after annealing at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours, followed by air cooling.
25. 25. The alloy of claim 24, wherein after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours, followed by air cooling, the RT ultimate tensile strength is between 1207 MPa (175 ksi) and 1310 MPa (190 ksi), the RT 0.2% proof stress is between 724 MPa (105 ksi) and 793 MPa (115 ksi), and the RT elongation is between 20% and 30%.
26. 2. The alloy of claim 1, wherein the alloy has a 700°C ultimate tensile strength of between 896 MPa (130 ksi) and 1069 MPa (155 ksi), a 700°C 0.2% yield strength of between 620 MPa (90 ksi) and 724 MPa (105 ksi), and a 700°C elongation of between 9% and 25%, after annealing at 788°C (1450°F) for four hours followed by air cooling.
27. 27. The alloy of claim 26, wherein after annealing the alloy at 788°C (1450°F) for 4 hours followed by air cooling, the 700°C ultimate tensile strength is between 861 MPa (125 ksi) and 965 MPa (140 ksi), the 700°C 0.2% yield strength is between 620 MPa (90 ksi) and 689 MPa (100 ksi), and the 700°C elongation is between 14% and 20%.
28. 2. The alloy of claim 1, wherein after annealing at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours, followed by air cooling, the 700°C ultimate tensile strength is between 931 MPa (135 ksi) and 1069 MPa (155 ksi), the 700°C 0.2% yield strength is between 655 MPa (95 ksi) and 758 MPa (110 ksi), and the 700°C elongation is between 12% and 30%.
29. 29. The alloy of claim 28, wherein after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 1000 hours, followed by air cooling, the 700°C ultimate tensile strength is between 931 MPa (135 ksi) and 1034 MPa (150 ksi), the 700°C 0.2% proof stress is between 655 MPa (95 ksi) and 724 MPa (105 ksi), and the 700°C elongation is between 15% and 30%.
30. 2. The alloy of claim 1, wherein after annealing at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours, followed by air cooling, the 700°C ultimate tensile strength is between 896 MPa (130 ksi) and 1034 MPa (150 ksi), the 700°C 0.2% proof stress is between 620 MPa (90 ksi) and 758 MPa (110 ksi), and the 700°C elongation is between 15% and 28%.
31. 31. The alloy of claim 30, wherein after annealing the alloy at 788°C (1450°F) for 4 hours, followed by air cooling, and aging the alloy at 700°C (1292°F) for 5000 hours, followed by air cooling, the 700°C ultimate tensile strength is between 896 MPa (130 ksi) and 1000 MPa (145 ksi), the 700°C 0.2% proof stress is between 620 MPa (90 ksi) and 703 MPa (102 ksi), and the 700°C elongation is between 15% and 25%.
32. In weight percent: 1.3% to 1.8% aluminum; 1.5% to 4.0% Cobalt; 18.0% to 22.0% chromium; 4.0% to 10.0% iron; 1.0% to 3.0% molybdenum; 1.0% to 2.5% niobium; 1.3% to 1.8% titanium; 0.8% to 1.2% tungsten; 0.01% to 0.08% carbon; 0.02% to 0.3% manganese; 0.05% to 0.3% silicon; 0.005% to 0.2% Vanadium; 0.005% to 0.2% zirconium; 0.001% to 0.025% boron; 0.001% to 0.02% nitrogen; and Remaining nickel and incidental impurities; having a composition consisting of: A stress rupture life at 700° C. and 393.7 MPa (57.1 ksi) of at least 300 hours; and An alloy having a room temperature elongation of at least 19% after aging at 700°C for 1,000 hours.
Citation Information
Patent Citations
Free cutting ni based heat resistant alloy
JP2002363674A
Tube alloys for modern supercritical boilers
JP2002518599A
Ni-BASED HEAT-RESISTANT ALLOY
JP2013036086A
Ni-BASED HEAT-RESISTANT ALLOY AND METHOD FOR MANUFACTURING SAME
WO2018151222A1