Method for producing copolymer

The copolymerization of specific monomers with an aqueous surfactant solution at controlled temperatures produces high molecular weight copolymers for semiconductor manufacturing, addressing low molecular weight issues and improving solubility and clarity in positive resists.

JP7552095B2Active Publication Date: 2024-09-18ZEON CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020107296
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-22
Publication Date
2024-09-18
Estimated Expiration
2040-06-22

AI Technical Summary

Technical Problem

Existing copolymers used as main chain cleavage type positive resists have low molecular weights, limiting their effectiveness in semiconductor manufacturing processes, particularly in terms of solubility differences and pattern clarity.

Method used

A method involving the copolymerization of a monomer composition containing specific monomers represented by formulas (I) and (II) with an aqueous surfactant solution, optimized at a polymerization temperature of 10°C to 90°C, without reaction aids, buffers, or polymerization initiators, to produce high molecular weight copolymers.

Benefits of technology

This method efficiently produces high molecular weight copolymers that are highly sensitive to ionizing radiation, enhancing solubility differences and pattern clarity, while reducing metal content and production time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552095000009
    Figure 0007552095000009
  • Figure 0007552095000010
    Figure 0007552095000010
  • Figure 0007552095000015
    Figure 0007552095000015
Patent Text Reader

Abstract

To provide a method of efficiently manufacturing a polymer having a high molecular weight useful as a main-chain cutting type positive resist.SOLUTION: The method comprises a step of copolymerizing a monomer composition containing a monomer (a) represented by formula (I) and a monomer (b) represented by formula (II). In formula (I), X is a halogen atom, a cyano group or the like. R1 is an organic group in which the number of fluorine atoms is 3 or larger and 10 or smaller. In formula (II), R2 is an alkyl group, a halogen atom, a cyano group, an alkyl sulfonyl group, an alkoxy group, a nitro group, etc. and R3 is an alkyl group, a halogen atom, a hydroxy group, etc.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a copolymer, and more particularly to a method for producing a copolymer that can be suitably used as a positive resist. [Background technology]

[0002] Conventionally, in the field of semiconductor manufacturing and the like, polymers whose main chains are cleaved and whose solubility in a developer is increased by irradiation with ionizing radiation such as electron beams or short-wavelength light such as ultraviolet light (hereinafter, ionizing radiation and short-wavelength light may be collectively referred to as "ionizing radiation, etc.") have been used as main-chain scission type positive resists.

[0003] Specifically, for example, Patent Document 1 discloses a positive resist made of a copolymer containing α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units and α-methylstyrene units, as a main chain cleavage type positive resist that is excellent in heat resistance and is capable of forming a resist pattern with excellent resolution and clarity.

[0004] In Patent Document 1, the copolymer is obtained by reacting a monomer composition containing α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl, α-methylstyrene, and azobisisobutyronitrile as a polymerization initiator. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2020 / 066806 Summary of the Invention [Problem to be solved by the invention]

[0006] Here, from the viewpoint of increasing the difference in solubility in a developer between the portion irradiated with ionizing radiation or the like and the unirradiated portion, and thereby improving the clarity of the obtained resist pattern, a high molecular weight copolymer is required as a copolymer used as a main chain scission type positive resist.

[0007] However, the copolymer obtained by the method described in Patent Document 1 has a low molecular weight, leaving room for improvement.

[0008] It is therefore an object of the present invention to provide a method for efficiently producing a high molecular weight copolymer useful as a main chain scission type positive resist. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to achieve the above object, and have found that a high molecular weight copolymer useful as a main chain scission type positive resist can be efficiently produced by copolymerizing a monomer composition containing a specific monomer and an aqueous surfactant solution, thereby completing the present invention.

[0010] That is, the present invention aims to advantageously solve the above-mentioned problems, and the copolymerization production method of the present invention is characterized by comprising a step of copolymerizing a monomer composition containing a monomer (a) represented by the following formula (I), a monomer (b) represented by the following formula (II), and an aqueous surfactant solution. [ka] [In formula (I), X is a halogen atom, a cyano group, an alkylsulfonyl group, an alkoxy group, a nitro group, an acyl group, an alkyl ester group, or a halogenated alkyl group; R 1 is an organic group having 3 to 10 fluorine atoms. In formula (II), R 2 is an alkyl group, a halogen atom, a cyano group, an alkylsulfonyl group, an alkoxy group, a nitro group, an acyl group, an alkyl ester group, or a halogenated alkyl group; R 3is an alkyl group, a halogen atom, a hydroxyl group, or a halogenated alkyl group, p is an integer of 0 to 5, R 3 When a plurality of are present, they may be the same or different. In this way, by copolymerizing a monomer composition containing a predetermined monomer and an aqueous surfactant solution, a high molecular weight copolymer useful as a main chain scission type positive resist can be efficiently produced.

[0011] In the method for producing the copolymer of the present invention, in the formula (I), X is a chlorine atom, and in the formula (II), R 2 is preferably an alkyl group. By using such a monomer, it becomes easier to efficiently produce a high molecular weight copolymer useful as a main chain scission type positive resist.

[0012] In addition, in the method for producing the copolymer of the present invention, the copolymerization is preferably carried out at a polymerization temperature of 10° C. or more and 90° C. or less. In this way, by copolymerizing a predetermined monomer at a polymerization temperature of 10° C. or more and 90° C. or less, the reaction efficiency can be increased.

[0013] In the method for producing the copolymer of the present invention, the weight average molecular weight of the copolymer obtained is preferably 200,000 or more and 700,000 or less. If the weight average molecular weight of the copolymer is 200,000 or more and 700,000 or less, the usefulness as a main chain cleavage type positron is improved. The weight average molecular weight of the copolymer can be measured by the method described in the examples of this specification.

[0014] Furthermore, in the method for producing a copolymer of the present invention, it is preferable that the monomer composition does not contain a reaction aid. If a monomer composition that does not contain a reaction aid is used, the amount of metal that may be contained in the obtained copolymer can be reduced.

[0015] In the method for producing a copolymer of the present invention, the amount of the buffer in the monomer composition is preferably 0.2% by mass or less relative to the mass of the aqueous surfactant solution. If the amount of the buffer is 0.2% by mass or less relative to the mass of the aqueous surfactant solution, the amount of metal that may be contained in the obtained copolymer can be further reduced.

[0016] In the method for producing the copolymer of the present invention, the amount of the polymerization initiator in the monomer composition is preferably 0.005 equivalent or less. If the amount of the polymerization initiator is 0.005 equivalent or less, the amount of metal that may be contained in the obtained copolymer can be further reduced. In the present invention, the term "equivalent" refers to a molar equivalent relative to the amount of monomer (a). Effect of the Invention

[0017] According to the method for producing a copolymer of the present invention, it is possible to efficiently produce a high molecular weight copolymer that is useful as a main chain scission type positive resist. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail.

[0019] Here, the copolymer produced by the copolymer production method of the present invention can be suitably used as a main chain scission type positive resist in which the main chain is scissed and the molecular weight is reduced by irradiation with ionizing radiation such as an electron beam or short wavelength light such as ultraviolet light.

[0020] (Method of Producing Copolymer) The method for producing the copolymer of the present invention includes a step (copolymerization step) of copolymerizing a monomer composition containing a monomer (a) represented by the following formula (I), a monomer (b) represented by the following formula (II), and an aqueous surfactant solution, and may optionally further include a step (recovery step) of recovering the obtained copolymer. In addition, the method for producing the copolymer of the present invention may further include a step (purification step) of purifying the recovered copolymer. [ka] [In formula (I), X is a halogen atom, a cyano group, an alkylsulfonyl group, an alkoxy group, a nitro group, an acyl group, an alkyl ester group, or a halogenated alkyl group; R 1 is an organic group having 3 to 10 fluorine atoms. In formula (II), R 2 is an alkyl group, a halogen atom, a cyano group, an alkylsulfonyl group, an alkoxy group, a nitro group, an acyl group, an alkyl ester group, or a halogenated alkyl group; R 3 is an alkyl group, a halogen atom, a hydroxyl group, or a halogenated alkyl group, p is an integer of 0 to 5, R 3 When a plurality of are present, they may be the same or different.

[0021] <Copolymerization process> In the copolymerization step, a monomer composition containing a predetermined monomer and an aqueous surfactant solution is copolymerized to synthesize a copolymer. Since the monomer composition containing a predetermined monomer and an aqueous surfactant solution is copolymerized in the copolymerization step, a high molecular weight copolymer useful as a main chain scission type positive resist can be efficiently produced.

[0022] [Monomer composition] Here, the monomer composition contains a monomer (a), a monomer (b) and an aqueous surfactant solution.

[0023] [Monomer (a)] The monomer (a) is a compound having a structure represented by the above formula (I). The ratio of the monomer (a) in the total monomers contained in the monomer composition is not particularly limited, and can be, for example, 30 mol% or more, preferably 40 mol% or more, and more preferably 45 mol% or more, and can be 70 mol% or less, preferably 60 mol% or less, and more preferably 55 mol% or less.

[0024] Here, examples of halogen atoms that can constitute X in formula (I) include chlorine, fluorine, bromine, iodine, and astatine atoms. Examples of alkylsulfonyl groups that can constitute X in formula (I) include methylsulfonyl and ethylsulfonyl groups. Examples of alkoxy groups that can constitute X in formula (I) include methoxy, ethoxy, and propoxy groups. Examples of acyl groups that can constitute X in formula (I) include formyl, acetyl, and propionyl groups. Examples of alkyl ester groups that can constitute X in formula (I) include methyl ester and ethyl ester groups. Examples of halogenated alkyl groups that can constitute X in formula (I) include halogenated methyl groups having 1 to 3 halogen atoms. Among these, from the viewpoint of more efficiently producing a high molecular weight copolymer useful as a main chain scission type positive resist, X is preferably a halogen atom, and more preferably a chlorine atom.

[0025] In addition, R in formula (I) 1 must be an organic group having 3 to 10 fluorine atoms, and R 1 The number of fluorine atoms contained in R is preferably 3 or more and 8 or less. 1 If the number of fluorine atoms contained therein is equal to or greater than the above lower limit, a high molecular weight copolymer useful as a main chain scission type positive resist can be obtained. 1 When the number of fluorine atoms contained therein is equal to or less than the above upper limit, the production efficiency of a high molecular weight copolymer is improved.

[0026] The organic group having 3 or more and 10 or less fluorine atoms is not particularly limited, and examples thereof include fluoroalkyl groups having 3 or more and 10 fluorine atoms, such as the following (a-1) to (a-30); fluoroalkoxyalkyl groups having 3 or more and 10 fluorine atoms, such as the following (a-31) to (a-54); fluoroalkoxyalkenyl groups having 3 or more and 10 fluorine atoms, such as a fluoroethoxyvinyl group; and an organic group represented by the following formula (A) (hereinafter referred to as "organic group (A)"). -L-Ar···(A) [In the organic group (A), L is a divalent linking group, Ar is an aromatic ring group which may have a substituent, and the number of fluorine atoms contained in the organic group (A) is 3 to 10. In the present invention, "may have a substituent" means "unsubstituted or substituted."]

[0027] [ka] [ka]

[0028] The divalent linking group that can constitute L in the organic group (A) is not particularly limited, and examples thereof include an alkylene group which may have a substituent, and an alkenylene group which may have a substituent.

[0029] The alkylene group of the alkylene group which may have a substituent is not particularly limited, and examples thereof include linear alkylene groups such as methylene, ethylene, propylene, n-butylene, and isobutylene, and cyclic alkylene groups such as 1,4-cyclohexylene. Among them, the alkylene group is preferably a linear alkylene group having 1 to 6 carbon atoms such as methylene, ethylene, propylene, n-butylene, and isobutylene, more preferably a linear alkylene group having 1 to 6 carbon atoms such as methylene, ethylene, propylene, and n-butylene, and even more preferably a linear alkylene group having 1 to 3 carbon atoms such as methylene, ethylene, and propylene.

[0030] The alkenylene group of the alkenylene group which may have a substituent is not particularly limited, and examples thereof include chain alkenylene groups such as ethenylene group, 2-propenylene group, 2-butenylene group, and 3-butenylene group, and cyclic alkenylene groups such as cyclohexenylene group. Among them, the alkenylene group is preferably a straight-chain alkenylene group having 2 to 6 carbon atoms such as ethenylene group, 2-propenylene group, 2-butenylene group, and 3-butenylene group.

[0031] Among the above, from the viewpoint of sufficiently improving the sensitivity of the resulting copolymer to ionizing radiation and the like, the divalent linking group is preferably an alkylene group which may have a substituent, more preferably a chain alkylene group having 1 to 6 carbon atoms which may have a substituent, still more preferably a linear alkylene group having 1 to 6 carbon atoms which may have a substituent, and particularly preferably a linear alkylene group having 1 to 3 carbon atoms which may have a substituent.

[0032] From the viewpoint of further improving the sensitivity of the resulting copolymer to ionizing radiation, etc., it is preferable that the divalent linking group capable of constituting L of the organic group (A) has one or more electron-withdrawing groups. In particular, when the divalent linking group is an alkylene group having an electron-withdrawing group as a substituent or an alkenylene group having an electron-withdrawing group as a substituent, it is preferable that the electron-withdrawing group is bonded to the carbon bonded to O adjacent to the carbonyl carbon in formula (I).

[0033] The electron-withdrawing group capable of sufficiently improving the sensitivity to ionizing radiation and the like is not particularly limited, and may be, for example, at least one selected from the group consisting of a fluorine atom, a fluoroalkyl group, a cyano group, and a nitro group. The fluoroalkyl group is not particularly limited, and may be, for example, a fluoroalkyl group having 1 to 5 carbon atoms. Among them, the fluoroalkyl group is preferably a perfluoroalkyl group having 1 to 5 carbon atoms, and more preferably a trifluoromethyl group.

[0034] From the viewpoint of more efficiently producing a high molecular weight copolymer useful as a main chain scission type positive resist, L in the organic group (A) is preferably a divalent linking group containing 3 or more and 10 or less fluorine atoms, more preferably a divalent linking group containing 3 or more and 6 or less fluorine atoms, and further preferably a trifluoromethylmethylene group, a pentafluoroethylmethylene group or a bis(trifluoromethyl)methylene group.

[0035] Examples of Ar in the organic group (A) include aromatic hydrocarbon ring groups which may have a substituent and aromatic heterocyclic groups which may have a substituent.

[0036] The aromatic hydrocarbon ring group is not particularly limited, and examples thereof include a benzene ring group, a biphenyl ring group, a naphthalene ring group, an azulene ring group, an anthracene ring group, a phenanthrene ring group, a pyrene ring group, a chrysene ring group, a naphthacene ring group, a triphenylene ring group, an o-terphenyl ring group, an m-terphenyl ring group, a p-terphenyl ring group, an acenaphthene ring group, a coronene ring group, a fluorene ring group, a fluoranthrene ring group, a pentacene ring group, a perylene ring group, a pentaphene ring group, a picene ring group, and a pyranthrene ring group.

[0037] Furthermore, examples of the aromatic heterocyclic group include, but are not limited to, a furan ring group, a thiophene ring group, a pyridine ring group, a pyridazine ring group, a pyrimidine ring group, a pyrazine ring group, a triazine ring group, an oxadiazole ring group, a triazole ring group, an imidazole ring group, a pyrazole ring group, a thiazole ring group, an indole ring group, a benzimidazole ring group, a benzothiazole group, a benzoxazole ring group, a quinoxaline ring group, a quinazoline ring group, a phthalazine ring group, a benzofuran ring group, a dibenzofuran ring group, a benzothiophene ring group, a dibenzothiophene ring group, and a carbazole ring group.

[0038] Furthermore, the substituent that Ar may have is not particularly limited, and examples thereof include an alkyl group, a fluorine atom, and a fluoroalkyl group. Examples of the alkyl group as the substituent that Ar may have include a chain alkyl group having 1 to 6 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an n-butyl group, and an isobutyl group. Examples of the fluoroalkyl group as the substituent that Ar may have include a fluoroalkyl group having 1 to 5 carbon atoms, such as a trifluoromethyl group, a trifluoroethyl group, and a pentafluoropropyl group.

[0039] Among these, from the viewpoint of more efficiently producing a high molecular weight copolymer useful as a main chain scission type positive resist, Ar in the organic group (A) is preferably an aromatic hydrocarbon ring group which may have a substituent, more preferably an unsubstituted aromatic hydrocarbon ring group, and even more preferably a benzene ring group (phenyl group).

[0040] The monomer (a) represented by formula (I) is not particularly limited, and examples thereof include α-chloroacrylic acids such as 2,2,2-trifluoroethyl α-chloroacrylate, 2,2,3,3,3-pentafluoropropyl α-chloroacrylate, 3,3,4,4,4-pentafluorobutyl α-chloroacrylate, 1H-1-(trifluoromethyl)trifluoroethyl α-chloroacrylate, 1H,1H,3H-hexafluorobutyl α-chloroacrylate, 1,2,2,2-tetrafluoro-1-(trifluoromethyl)ethyl α-chloroacrylate, and 2,2,3,3,4,4,4-heptafluorobutyl α-chloroacrylate. α-chloroacrylic acid fluoroalkoxyalkyl esters such as α-chloroacrylic acid pentafluoroethoxymethyl ester and α-chloroacrylic acid pentafluoroethoxyethyl ester; α-chloroacrylic acid fluoroalkoxyalkenyl esters such as α-chloroacrylic acid pentafluoroethoxyvinyl ester; α-chloroacrylic acid-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl, α-chloroacrylic acid-1-phenyl-2,2,2-trifluoroethyl, and α-chloroacrylic acid-1-phenyl-2,2,3,3,3-pentafluoropropyl. From the viewpoint of more efficiently producing a high molecular weight copolymer useful as a main chain cleavage type positive resist, the monomer (a) represented by formula (I) is preferably α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl, α-chloroacrylate-1-phenyl-2,2,2-trifluoroethyl, or α-chloroacrylate-1-phenyl-2,2,3,3,3-pentafluoropropyl.

[0041] [Monomer (b)] The monomer (b) is a compound having a structure represented by the above formula (II). The ratio of the monomer (b) in the total monomers contained in the monomer composition is not particularly limited, and can be, for example, 30 mol% or more, preferably 40 mol% or more, more preferably 45 mol% or more, and can be 70 mol% or less, preferably 60 mol% or less, and more preferably 55 mol% or less.

[0042] Here, R in formula (I) 2 and R 3 The alkyl group that can constitute the above group is not particularly limited, and examples thereof include unsubstituted alkyl groups having 1 to 5 carbon atoms.

[0043] In addition, R in formula (II) 2 and R 3 The halogen atoms and halogenated alkyl groups that can constitute R are not particularly limited, and examples thereof include the same halogen atoms and halogenated alkyl groups as those described in formula (I). 3 The alkyl halide that can constitute the above group is preferably a perfluoroalkyl group having 1 to 5 carbon atoms, more preferably a trifluoromethyl group.

[0044] Furthermore, R in formula (II) 2 The cyano group, alkylsulfonyl group, alkoxy group, nitro group, acyl group, and alkyl ester group that can constitute the formula (I) are not particularly limited, and examples thereof include the cyano group, alkylsulfonyl group, alkoxy group, nitro group, acyl group, and alkyl ester group described in formula (I).

[0045] From the viewpoint of easiness in preparation of the copolymer and improvement in severability of the main chain when irradiated with ionizing radiation or the like, R 2 As the alkyl group, an alkyl group is preferable, and a methyl group or an ethyl group is preferable.

[0046] From the viewpoints of easiness in preparation of the copolymer and improvement in severability of the main chain upon irradiation with ionizing radiation or the like, p in formula (II) is preferably 0 or 1, and more preferably 0.

[0047] The monomer (b) represented by the above formula (II) is not particularly limited, and examples thereof include α-methylstyrene and its derivatives such as the following (b-1) to (b-12). [ka]

[0048] From the viewpoint of more efficiently producing a high molecular weight copolymer useful as a main chain scission type positive resist, the monomer (b) is preferably α-methylstyrene or 1-chloro-4-(1-propen-2-yl)benzene, and more preferably α-methylstyrene.

[0049] [Surfactant Aqueous Solution] The surfactant aqueous solution is a solution in which a surfactant is dissolved or dispersed in water. In the present invention, by using a monomer composition containing the surfactant aqueous solution, it is possible to emulsion-polymerize the monomer (a) and the monomer (b), and as a result, it is possible to efficiently produce a high molecular weight copolymer.

[0050] Here, the surfactant used in the aqueous surfactant solution is not particularly limited, and for example, a surfactant that contains a hydrophilic group and a lipophilic group and can form micelles for emulsion polymerization can be used. Specifically, a nonionic surfactant, a cationic surfactant, an anionic surfactant, an amphoteric surfactant, etc. can be used.

[0051] Examples of nonionic surfactants include polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, polyoxyethylene higher alcohol ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene alkyl ether, polyoxyethylene myristyl ether, polyoxyethylene octyldodecyl ether, polyoxyethylene alkylene alkyl ether, polyoxyethylene distyrenated phenyl ether, polyoxyethylene derivatives, polyoxyethylene polyoxypropylene glycol, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tri ... areate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, polyoxyethylene sorbitan tetraoleate, glycerol monostearate, glycerol monooleate, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, sorbitan monooleate, sorbitan trioleate, sorbitan sesquioleate, polyethylene glycol monolaurate, polyethylene glycol monostearate, polyethylene glycol distearate, polyethylene glycol monooleate, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkylamines, alkyl alkanolamides, stearic acid monoglyceride, polyoxyethylene-polyoxypropylene block polymers, and the like.

[0052] Examples of cationic surfactants include coconut amine acetate, stearylamine acetate, lauryl trimethyl ammonium chloride, stearyl trimethyl ammonium chloride, cetyl trimethyl ammonium chloride, distearyl dimethyl ammonium chloride, alkyl benzyl dimethyl ammonium chloride, hydrochlorides of primary amines such as monomethylamine, monoethylamine, and monostearylamine; hydrochlorides of secondary amines such as dimethylamine, diethylamine, and distearylamine; hydrochlorides of tertiary amines such as trimethylamine, triethylamine, and stearyl dimethylamine; hydrochlorides of ethanolamines such as monoethanolamine, diethanolamine, and triethanolamine; hydrochlorides of polyethylene polyamines such as ethylene diamine and diethylene triamine; and hydrochlorides of amines such as pyridine, morpholine, and hydrazine.

[0053] Examples of anionic surfactants include mixed fatty acid soda soap, semi-hardened beef tallow fatty acid soda soap, sodium stearate soap, semi-hardened beef tallow fatty acid potassium soap, potassium oleate soap, castor oil potassium soap, sodium lauryl sulfate, sodium higher alcohol sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzene sulfonate, sodium alkyl naphthalene sulfonate, sodium dialkyl sulfosuccinate, sodium alkyl diphenyl ether disulfonate, potassium alkyl phosphate, sodium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene alkyl ether sulfate, triethanolamine polyoxyethylene alkyl ether sulfate, sodium polyoxyethylene alkyl phenyl ether sulfate, sodium alkane sulfonate, sodium salt of β-naphthalene sulfonic acid formalin condensate, alkoxyalkyl phosphate, alkyl phosphate, diethanolamine alkyl phosphate, sodium alkyl sulfonate special aromatic sulfonic acid formalin condensate, and special carboxylic acid surfactant.

[0054] Examples of amphoteric surfactants include lauryl betaine, stearyl betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, lauryl dimethylamine oxide, alkyl dimethylamine oxide, and alkyl carboxy betaine.

[0055] Here, the surfactant aqueous solution can be prepared by mixing the above-mentioned surfactant with water by a known method. In this case, the concentration of the surfactant in the surfactant aqueous solution is not particularly limited, and can be, for example, 0.1% by mass or more and 10% by mass or less, and preferably 0.5% by mass or more and 3% by mass or less.

[0056] The monomer composition used in the method for producing the copolymer of the present invention may contain the above-mentioned monomer (a), monomer (b) and an aqueous surfactant solution, but the monomer composition may further contain other components as desired. The other components are not particularly limited, and examples thereof include other monomers, other solvents, reaction auxiliaries, buffers and polymerization initiators.

[0057] [Other monomers] The other monomer may be any monomer copolymerizable with the monomer (a) and the monomer (b). However, the ratio of the other monomer to the total monomers contained in the monomer composition is preferably 10 mol% or less, and more preferably 0 mol% (i.e., the monomer composition contains only the monomer (a) and the monomer (b) as monomers).

[0058] [Other Solvents] The other solvent is not particularly limited, and for example, cyclopentanone can be used.

[0059] [Reaction aid] According to the method for producing a copolymer of the present invention, even if the monomer composition does not contain a reaction auxiliary, the copolymerization reaction between the monomer (a) and the monomer (b) can be sufficiently advanced to produce a high molecular weight copolymer. However, if necessary, the monomer composition may contain a reaction auxiliary.

[0060] Here, the reaction aid that can be contained in the monomer composition is not particularly limited, and examples thereof include sodium dithionite, sodium iron ethylenediaminetetraacetate trihydrate, tetrasodium ethylenediaminetetraacetate tetrahydrate, sodium formaldehyde sulfoxylate, and cumene hydroperoxide.

[0061] The amount of the reaction aid in the monomer composition is not particularly limited, and is preferably 0.008 equivalents or less, more preferably 0.006 equivalents or less, and even more preferably 0.004 equivalents or less. If the amount of the reaction aid is equal to or less than the upper limit, the amount of metal that may be contained in the obtained copolymer can be reduced.

[0062] Preferably, the monomer composition used in the method for producing the copolymer of the present invention does not contain the above-mentioned reaction aid. If a monomer composition that does not contain a reaction aid is used, a copolymer with an effectively reduced amount of metal can be obtained.

[0063] [Buffer] According to the method for producing a copolymer of the present invention, even if the monomer composition does not contain a buffer agent, the copolymerization reaction between the monomer (a) and the monomer (b) can be sufficiently advanced to produce a high molecular weight copolymer. However, if necessary, the monomer composition may contain a buffer agent.

[0064] The buffer that can be contained in the monomer composition is not particularly limited, and for example, sodium carbonate can be used.

[0065] The amount of the buffer in the monomer composition is preferably 0.2% by mass or less, more preferably 0.15% by mass or less, based on the mass of the above-mentioned aqueous surfactant solution. If the amount of the buffer in the monomer composition is equal to or less than the upper limit value based on the mass of the aqueous surfactant solution, the amount of metal that may be contained in the obtained copolymer can be further reduced.

[0066] [Polymerization initiator] According to the method for producing a copolymer of the present invention, even if the monomer composition does not contain a polymerization initiator, it is possible to produce a high molecular weight copolymer by sufficiently proceeding the copolymerization reaction between the monomer (a) and the monomer (b). However, if necessary, the monomer composition may contain a polymerization initiator.

[0067] The polymerization initiator that can be contained in the monomer composition is not particularly limited, and for example, a radical polymerization initiator such as potassium persulfate or azobisisobutyronitrile can be used.

[0068] The amount of the polymerization initiator in the monomer composition is not particularly limited, but is preferably 0.005 equivalents or less, more preferably 0.002 equivalents or less. If the amount of the polymerization initiator is equal to or less than the upper limit, the amount of metal that may be contained in the obtained copolymer can be further reduced.

[0069] [Polymerization temperature] The polymerization temperature when copolymerizing the monomer composition in the copolymerization step is not particularly limited, and is preferably 10°C or higher, more preferably 25°C or higher, and even more preferably 30°C or higher, and is preferably 90°C or lower, more preferably 80°C or lower, and even more preferably 70°C or lower. If the polymerization temperature is 10°C or higher, freezing of the monomer can be prevented, and the reaction efficiency can be improved. Also, if the polymerization temperature is 90°C or lower, a good balance between the reaction efficiency and the molecular weight of the resulting copolymer can be achieved.

[0070] [Other polymerization conditions] The time (reaction time) for copolymerizing the monomer composition is not particularly limited, and is preferably 4 hours or more, more preferably 5 hours or more, more preferably 10 hours or more, and more preferably 24 hours or less, and more preferably 20 hours or less. If the reaction time is equal to or more than the above lower limit, the resulting copolymer can be sufficiently highly molecular weighted. If the reaction time is equal to or less than the above upper limit, the time required for synthesizing the copolymer can be sufficiently shortened.

[0071] [Copolymer] The copolymer obtained in the copolymerization step contains a repeating unit derived from monomer (a) represented by formula (III) below and a repeating unit derived from monomer (b) represented by formula (IV) below, and optionally further contains repeating units derived from other monomers. [ka] [In the formula (III), X and R 1 is the same as in formula (I), and in formula (IV), R 2 and R 3 is the same as in formula (II).

[0072] Since the copolymer contains both the repeating unit represented by the above formula (III) and the repeating unit represented by the above formula (IV), the main chain is easily cleaved when irradiated with ionizing radiation or the like (e.g., electron beam, KrF laser, ArF laser, EUV laser, etc.) (i.e., the sensitivity to ionizing radiation or the like is high). Therefore, the copolymer is useful as a main chain cleavage type positive resist.

[0073] The weight average molecular weight of the copolymer obtained in the copolymerization step is preferably 200,000 or more, more preferably 250,000 or more, even more preferably 300,000 or more, and preferably 700,000 or less, more preferably 500,000 or less, and even more preferably 400,000 or less. If the weight average molecular weight is the above lower limit or more, when the copolymer is used as a main chain cleavage type positive resist, the clarity of the obtained resist pattern can be improved. In addition, if the weight average molecular weight is the above upper limit or less, the time required for synthesizing the copolymer can be sufficiently shortened.

[0074] <Recovery process> In the optional recovery step, the copolymer is recovered from the polymer solution containing the copolymer obtained in the copolymerization step.

[0075] Specifically, in the recovery step, for example, a good solvent such as tetrahydrofuran is added to a polymer solution containing the copolymer, and then the solution to which the good solvent has been added is dropped into a poor solvent such as methanol to coagulate the copolymer, thereby recovering the copolymer.

[0076] <Purification process> In the purification step that can be optionally performed, the copolymer can be purified using a known purification method such as a reprecipitation method or a column chromatography method without any particular limitation. By performing purification using any of the known purification methods such as the reprecipitation method or the column chromatography method, the amount of metal that can be contained in the copolymer can be further reduced. Among them, from the viewpoint of ease, it is preferable to use the reprecipitation method as the purification method. The purification of the copolymer may be performed repeatedly multiple times.

[0077] The purification of the copolymer by the reprecipitation method is preferably carried out, for example, by dissolving the obtained copolymer in a good solvent such as tetrahydrofuran, and then dropping the obtained solution into a mixed solvent of a good solvent such as tetrahydrofuran and a poor solvent such as methanol to precipitate a part of the copolymer. In this way, if the copolymer solution is dropped into a mixed solvent of a good solvent and a poor solvent to perform purification, the molecular weight distribution, weight average molecular weight, and number average molecular weight of the obtained copolymer can be easily adjusted by changing the type and mixing ratio of the good solvent and the poor solvent. Specifically, for example, the molecular weight of the copolymer precipitated in the mixed solvent can be increased by increasing the ratio of the good solvent in the mixed solvent.

[0078] When purifying the copolymer by the reprecipitation method, the copolymer may be one that has precipitated in a mixed solvent of a good solvent and a poor solvent, or one that has not precipitated in the mixed solvent (i.e., one that is dissolved in the mixed solvent). The copolymer that has not precipitated in the mixed solvent can be recovered from the mixed solvent by a known method such as concentration to dryness. EXAMPLES

[0079] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "%" representing an amount is based on mass unless otherwise specified. In the examples and comparative examples, the weight average molecular weight, number average molecular weight and molecular weight distribution of the copolymer, and the amount of metal in the solution were measured and evaluated by the following methods. The aqueous solution of the semi-hardened beef tallow fatty acid potassium soap with a solid content of 18% used in the examples and comparative examples was prepared as follows.

[0080] <Weight average molecular weight, number average molecular weight and molecular weight distribution> For the copolymers obtained in the Examples and Comparative Examples, the weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by gel permeation chromatography, and the molecular weight distribution (Mw / Mn) was calculated. Specifically, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer were determined in terms of standard polystyrene using gel permeation chromatography (Tosoh Corporation, HLC-8220) and tetrahydrofuran as a developing solvent, and the molecular weight distribution (Mw / Mn) was calculated.

[0081] <Amount of metal in solution> The polymer solution containing the copolymer obtained in the Examples and Comparative Examples, or the isoamyl acetate solution with a copolymer concentration of 1.5% prepared using the copolymer obtained in the Examples and Comparative Examples, was heated on a heater with a hood, and the sample was dried and solidified, and then incinerated in an electric furnace. After cooling, the ash was completely dissolved in acid to prepare a test solution, which was appropriately diluted and measured with an ICP mass spectrometer (Agilent Technologies, Inc., "Agilent7900 ICP-MS"). The calibration curve was obtained using the absolute calibration curve method, and the measurement mode was set to cool mode. The amount of metal contained in each of the polymer solution and the isoamyl acetate solution with a copolymer concentration of 1.5% was evaluated according to the following criteria. A: The amount of metal in the solution is more than 1 ppb and less than 10 ppb B: The amount of metal in the solution is more than 10 ppb and less than 100 ppb C: The amount of metal in the solution is more than 100 ppb and less than 1000 ppb D: The amount of metal in the solution is more than 1000 ppb and less than 10,000 ppb E: The amount of metal in the solution is greater than 10,000 ppb

[0082] <Preparation of an aqueous solution of partially hardened beef tallow fatty acid potassium soap with a solid content of 18%> 100g of ion-exchanged water was prepared, heated to 70°C while stirring, and 8.40g of potassium hydroxide (49% aqueous solution) was added. Next, 19.6g of beef tallow 45° hydrogenated fatty acid HFA (manufactured by NOF Corporation) was added at a rate of 1.28g / min, followed by 0.126g of potassium silicate. The mixture was then stirred at 80°C for more than 2 hours to obtain an aqueous solution of semi-hydrogenated beef tallow fatty acid potassium soap with a solid content of 18%.

[0083] Example 1 <Preparation of copolymers by emulsion polymerization> A monomer composition containing 3.0000 g (1.0000 equivalents) of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl as monomer (a) represented by the following formula, 2.7120 (2.5444 equivalents) g of α-methylstyrene as monomer (b), 0.0114 g (0.0047 equivalents) of potassium persulfate as a polymerization initiator, 0.5463 g of an aqueous solution of half-hardened beef tallow fatty acid potassium soap with a solid content of 18% as an aqueous surfactant solution, 6.7708 g of ion-exchanged water, and 0.0073 g of sodium carbonate as a buffer was added to a glass ampoule containing a stirrer, and the ampoule was sealed, and the system was pressurized and depressurized 10 times with nitrogen gas to remove oxygen from the system. [ka] Next, the system was heated to 30°C and reacted for 6 hours to obtain a polymer solution containing a copolymer. Then, 10g of tetrahydrofuran as a good solvent was added to the obtained polymer solution, and the polymer solution to which the good solvent was added was dropped into 200g of methanol as a poor solvent to precipitate the copolymer. The precipitated copolymer was then recovered by filtration, and the weight average molecular weight and number average molecular weight of the obtained copolymer were measured to determine the molecular weight distribution. The results are shown in Table 1. Furthermore, the copolymer was used to prepare an isoamyl acetate solution with a copolymer concentration of 1.5%, and the amount of metal in the isoamyl acetate solution was measured. The results are shown in Table 1. The resulting copolymer contained 50 mol % each of α-methylstyrene units and α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units.

[0084] (Examples 2 to 5) During the preparation of the copolymer, the temperature at which the system was heated was changed to 40°C (Example 2), 50°C (Example 3), 60°C (Example 4), and 70°C (Example 5), respectively. In the same manner as in Example 1, a polymer solution, a copolymer, and an isoamyl acetate solution with a copolymer concentration of 1.5% were obtained. Various measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 1.

[0085] [Table 1]

[0086] Example 6 In preparing the copolymer, potassium persulfate as a polymerization initiator and sodium carbonate as a buffer were not used, and the reaction time was changed to 13 hours, but the same procedure as in Example 1 was repeated to obtain a polymer solution, a copolymer, and an isoamyl acetate solution with a copolymer concentration of 1.5%. Various measurements and evaluations were then performed in the same manner as in Example 1. The results are shown in Table 2.

[0087] (Examples 7 to 10) During the preparation of the copolymer, the temperature at which the system was heated was changed to 40°C (Example 7), 50°C (Example 8), 60°C (Example 9), and 70°C (Example 10), respectively. In the same manner as in Example 6, a polymer solution, a copolymer, and an isoamyl acetate solution with a copolymer concentration of 1.5% were obtained. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.

[0088] [Table 2]

[0089] Comparative Example 1 <Preparation of copolymer by solution polymerization> 3.0000 g (1.0000 equivalents) of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl as monomer (a), 2.4930 g (2.3389 equivalents) of α-methylstyrene as monomer (b), and 0.0040 g (0.0027 equivalents) of azobisisobutyronitrile as a polymerization initiator were added to a glass ampoule containing a stirrer, and the ampoule was sealed. Pressurization and depressurization with nitrogen gas were repeated 10 times to remove oxygen from the system. Next, the system was heated to 78°C and reacted for 3.5 hours to obtain a polymer solution containing a copolymer. Then, 10g of tetrahydrofuran as a good solvent was added to the obtained copolymer solution, and the polymer solution to which the good solvent had been added was dropped into 200g of methanol as a poor solvent to precipitate the copolymer. The precipitated copolymer was then recovered by filtration, and the weight average molecular weight and number average molecular weight of the obtained copolymer were measured to obtain the molecular weight distribution. The results are shown in Table 3. Furthermore, the copolymer was used to prepare an isoamyl acetate solution with a copolymer concentration of 1.5%, and the amount of metal in the isoamyl acetate solution was measured. The results are shown in Table 3. The resulting copolymer contained 50 mol % each of α-methylstyrene units and α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units.

[0090] Comparative Example 2 <Preparation of copolymers by emulsion polymerization> In a glass ampoule containing a stirrer, 3.0000 g (1.0000 equivalents) of methyl α-chloroacrylate instead of 1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl α-chloroacrylate as monomer (a), 7.2267 g (2.4568 equivalents) of α-methylstyrene as monomer (b), 0.0027 g of sodium dithionite as a reaction aid, 0.0010 g of sodium ferric ethylenediaminetetraacetate trihydrate, and ethylene A monomer composition containing 0.0025 g of tetrasodium diaminetetraacetate tetrahydrate, 0.0015 g of sodium formaldehyde sulfoxylate, 0.0052 g of cumene hydroperoxide, 1.5000 g of an aqueous solution of half-hardened beef tallow fatty acid potassium soap with a solid content of 18% as an aqueous surfactant solution, 18.3333 g of ion-exchanged water, and 0.0200 g of sodium carbonate as a buffer was added and sealed, and the system was pressurized and depressurized with nitrogen gas 10 times to remove oxygen from the system. Next, the system was cooled to 5°C, and the reaction was carried out for 24 hours to obtain a polymer solution containing a copolymer. Then, 10g of tetrahydrofuran as a good solvent was added to the obtained polymer solution, and the polymer solution to which the good solvent was added was dropped into 400g of methanol as a poor solvent to precipitate the copolymer. Then, the precipitated copolymer was recovered by filtration, and the weight average molecular weight and number average molecular weight of the obtained copolymer were measured to obtain the molecular weight distribution. The results are shown in Table 3. Furthermore, the copolymer was used to prepare an isoamyl acetate solution with a copolymer concentration of 1.5%, and the amount of metal in the isoamyl acetate solution was measured. The results are shown in Table 3. The resulting copolymer contained 50 mol % each of α-methylstyrene units and α-methyl chloroacrylate units.

[0091] Comparative Example 3 Except for changing the reaction time to 48 hours during preparation of the copolymer, a polymer solution, a copolymer, and an isoamyl acetate solution with a copolymer concentration of 1.5% were obtained in the same manner as in Comparative Example 2. Various measurements and evaluations were then carried out in the same manner as in Example 1. The results are shown in Table 3.

[0092] Comparative Example 4 The reaction was carried out in the same manner as in Comparative Example 2, except that sodium dithionite, sodium iron ethylenediaminetetraacetate trihydrate, tetrasodium ethylenediaminetetraacetate tetrahydrate, sodium formaldehyde sulfoxylate, and cumene hydroperoxide as reaction aids, and sodium carbonate as a buffer were not used during the preparation of the copolymer, and the system was heated to 40°C and the reaction time was changed to 13 hours. However, a polymer solution containing the copolymer could not be obtained. The results are shown in Table 3.

[0093] [Table 3]

[0094] Example 11 <Preparation of copolymers by emulsion polymerization> A monomer composition containing 3.0000 g (1.0000 equivalents) of α-chloroacrylate-1-phenyl-2,2,2-trifluoroethyl as monomer (a) represented by the following formula (a), 3.4089 g (2.5444 equivalents) of α-methylstyrene as monomer (b), 0.6866 g of an aqueous solution of semi-hardened beef tallow fatty acid potassium soap with a solid content of 18% as an aqueous surfactant solution, and 8.5107 g of ion-exchanged water was added to a glass ampoule containing a stirrer, and the ampoule was sealed. The system was pressurized and depressurized with nitrogen gas 10 times to remove oxygen from the system. [ka] Next, the system was heated to 40°C and reacted for 13 hours to obtain a polymer solution containing a copolymer. Then, 10g of tetrahydrofuran as a good solvent was added to the obtained polymer solution, and the polymer solution to which the good solvent was added was dropped into 200g of methanol as a poor solvent to precipitate the copolymer. Then, the precipitated copolymer was recovered by filtration, and the weight average molecular weight and number average molecular weight of the obtained copolymer were measured to obtain the molecular weight distribution. The results are shown in Table 4. Furthermore, the copolymer was used to prepare an isoamyl acetate solution with a copolymer concentration of 1.5%, and the amount of metal in the isoamyl acetate solution was measured. The results are shown in Table 4. The resulting copolymer contained 50 mol % each of α-methylstyrene units and α-chloroacrylate-1-phenyl-2,2,2-trifluoroethyl units.

[0095] Example 12 A monomer composition containing 3.0000 g (1.0000 equivalents) of α-chloroacrylate-1-phenyl-2,2,3,3,3-pentafluoropropyl as monomer (a) represented by the following formula, 2.8671 g (2.5444 equivalents) of α-methylstyrene as monomer (b), 0.5775 g of an aqueous solution of half-hardened beef tallow fatty acid potassium soap with a solid content of 18% as an aqueous surfactant solution, and 7.1580 g of ion-exchanged water was added to a glass ampoule containing a stirrer, and the ampoule was sealed, and the system was pressurized and depressurized with nitrogen gas 10 times to remove oxygen from the system. [ka]

[0096] Next, the system was heated to 40°C and reacted for 13 hours to obtain a polymer solution containing a copolymer. Then, 10g of tetrahydrofuran as a good solvent was added to the obtained polymer solution, and the polymer solution to which the good solvent was added was dropped into 200g of methanol as a poor solvent to precipitate the copolymer. Then, the precipitated copolymer was recovered by filtration, and the weight average molecular weight and number average molecular weight of the obtained copolymer were measured to obtain the molecular weight distribution. The results are shown in Table 4. Furthermore, the copolymer was used to prepare an isoamyl acetate solution with a copolymer concentration of 1.5%, and the amount of metal in the isoamyl acetate solution was measured. The results are shown in Table 4. The resulting copolymer contained 50 mol % each of α-methylstyrene units and α-chloroacrylate-1-phenyl-2,2,3,3,3-pentafluoropropyl units.

[0097] [Table 4]

[0098] Example 13 <Preparation of copolymers by emulsion polymerization> A monomer composition containing 3.0000 g (1.0000 equivalents) of α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl as the monomer (a) used in Example 1, 3.5024 g (2.5444 equivalents) of 1-chloro-4-(1-propen-2-yl)benzene as the monomer (b), 0.5463 g of an aqueous solution of half-hardened beef tallow fatty acid potassium soap with a solid content of 18% as an aqueous surfactant solution, and 6.7708 g of ion-exchanged water was added to a glass ampoule containing a stirrer, and the ampoule was sealed, and the system was pressurized and depressurized 10 times with nitrogen gas to remove oxygen from the system. Next, the system was heated to 40°C and reacted for 13 hours to obtain a polymer solution containing a copolymer. Then, 10g of tetrahydrofuran as a good solvent was added to the obtained polymer solution, and the polymer solution to which the good solvent was added was dropped into 200g of methanol as a poor solvent to precipitate the copolymer. The precipitated copolymer was then recovered by filtration, and the weight average molecular weight and number average molecular weight of the obtained copolymer were measured to obtain the molecular weight distribution. The results are shown in Table 5. Furthermore, the copolymer was used to prepare an isoamyl acetate solution with a copolymer concentration of 1.5%, and the amount of metal in the isoamyl acetate solution was measured. The results are shown in Table 5. The resulting copolymer contained 50 moles each of 1-chloro-4-(1-propen-2-yl)benzene units and α-chloroacrylate-1-phenyl-1-trifluoromethyl-2,2,2-trifluoroethyl units.

[0099] [Table 5]

[0100] From Tables 1 to 5, it can be seen that when the monomer compositions of Examples 1 to 13 were used, higher molecular weight copolymers could be produced compared to the case where a monomer composition not containing an aqueous surfactant solution was used (Comparative Example 1). It can also be seen that when the monomer compositions of Examples 1 to 13 were used, the amount of metal contained in the resulting copolymer could be reduced compared to when a monomer composition containing a reaction aid was used (Comparative Example 2 and Comparative Example 3). Furthermore, it is clear that when a monomer composition not containing the monomer (a) was used (Comparative Example 4), no copolymer was obtained. Furthermore, it is understood from Examples 6 to 13 that a high molecular weight copolymer could be produced even when the monomer composition did not contain a polymerization initiator. [Industrial Applicability]

[0101] According to the method for producing a copolymer of the present invention, it is possible to efficiently produce a high molecular weight copolymer that is useful as a main chain scission type positive resist.

Claims

1. A method for producing a copolymer, comprising a step of copolymerizing a monomer composition comprising a monomer (a) represented by the following formula (I), a monomer (b) represented by the following formula (II), and an aqueous surfactant solution: [Formula 1] [In formula (I), X is a halogen atom, a cyano group, an alkylsulfonyl group, an alkoxy group, a nitro group, an acyl group, an alkyl ester group, or a halogenated alkyl group; R 1 is an organic group having 3 to 10 fluorine atoms. In formula (II), R 2 is an alkyl group, a halogen atom, a cyano group, an alkylsulfonyl group, an alkoxy group, a nitro group, an acyl group, an alkyl ester group, or a halogenated alkyl group; R 3 is an alkyl group, a halogen atom, a hydroxyl group, or a halogenated alkyl group; p is an integer of 0 to 5; R 3 When a plurality of are present, they may be the same or different.

2. In the formula (I), X is a chlorine atom, and in the formula (II), R 2 The method for producing a copolymer according to claim 1 , wherein is an alkyl group.

3. The method for producing a copolymer according to claim 1 or 2, wherein the copolymerization is carried out at a polymerization temperature of 10° C. or higher and 90° C. or lower.

4. The method for producing a copolymer according to any one of claims 1 to 3, wherein the weight average molecular weight of the resulting copolymer is 200,000 or more and 700,000 or less.

5. The method for producing a copolymer according to any one of claims 1 to 4, wherein the monomer composition does not contain a reaction aid.

6. The method for producing a copolymer according to any one of claims 1 to 5, wherein the amount of the buffer in the monomer composition is 0.2 mass % or less based on the mass of the aqueous surfactant solution.

7. The method for producing a copolymer according to any one of claims 1 to 6, wherein the amount of the polymerization initiator in the monomer composition is 0.005 equivalent or less.

Citation Information

Patent Citations

  • Crosslinkable copolymer and positive type resist composed of its copolymer

    JP1987079446A

  • Copolymer and positive resist composition

    JP2018154754A

  • Method for forming resist pattern

    JP2020086063A

  • Copolymer and positive resist composition

    WO2020066806A1