Amorphous resin extended porous body

A stretched porous body with a resin composition exceeding 50% amorphous resin addresses pore control issues, achieving high productivity and desirable properties for electronic components.

JP7552172B2Active Publication Date: 2024-09-18MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020152335
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-10
Publication Date
2024-09-18
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

Existing methods for producing porous polymer materials face challenges in controlling pore size and distribution, leading to non-uniform structures, and require significant solvent use, reducing productivity, while dry methods result in material breakage during stretching.

Method used

A stretched porous body with at least one porous layer made of a resin composition containing 50% or more amorphous resin, such as polyphenylene ether, is produced by melt-extrusion, low-temperature stretching, and optional high-temperature stretching to achieve a uniform porous structure with excellent mechanical and electrical properties.

Benefits of technology

The method enables high productivity and produces a porous body with controlled porosity, air permeability, heat resistance, and low dielectric constants, suitable for electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552172000004
    Figure 0007552172000004
  • Figure 0007552172000007
    Figure 0007552172000007
  • Figure 0007552172000006
    Figure 0007552172000006
Patent Text Reader

Abstract

To provide an amorphous resin stretched porous material excellent in porous properties, air infiltration properties, heat resistance, mechanical properties and electrical properties; and to provide a manufacturing method of the stretched porous material, and an electronic member using the stretched porous material.SOLUTION: A stretched porous material has a porous layer, at least one layer, comprising a resin composition containing an amorphous resin (A) as much as 50 mass% or more.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretched porous body using an amorphous resin. More specifically, the present invention relates to a stretched porous body using an amorphous resin that can be used for packaging, sanitation, livestock, agriculture, construction, medical use, separation membranes, water treatment membranes, light diffusion plates, heat insulating materials, buffer materials, foam materials, separators, and low dielectric constant members, and particularly to a low dielectric constant member used in electronic members such as circuit boards typified by flexible printed circuit boards and circuit laminates, and an electronic member made of the low dielectric constant member, an electronic member using the stretched porous body, and a method for producing the stretched porous body. [Background technology]

[0002] Porous polymers having a large number of interconnecting fine pores are used in a wide variety of fields, including as separation membranes for the production of ultrapure water, the purification of chemical solutions, and water treatment; waterproof and moisture-permeable films for clothing and sanitary materials; separators for electronic components such as batteries, including alkaline batteries, nickel metal hydride batteries, lithium batteries, and lithium ion secondary batteries; and capacitors, including electrolytic capacitors, electric double-layer capacitors, and lithium ion capacitors; foam materials for electronic components such as mobile devices; and low-dielectric-constant materials for electronic components, including circuit boards, such as flexible printed circuit boards, and circuit laminates.

[0003] Polymeric porous bodies used in separation membranes are required to have chemical durability such as hypochlorous acid resistance and alkali resistance as well as mechanical strength and water permeability. Polymeric porous bodies used in electronic components such as separators, foam materials, and low dielectric constant components are required to have high heat resistance as well as porosity. In recent electronic components, further lower dielectric constant and lower dielectric loss tangent are required as electrical properties to accommodate high-speed processing of large amounts of information. For this reason, attempts have been made to make polyphenylene ether resins, which have excellent characteristics in mechanical strength, chemical durability, heat resistance, and electrical properties, porous.

[0004] On the other hand, methods for producing a polymeric porous body include a foaming method, a wet method, a dry method, etc. Also included is a method for producing a porous body in the form of a nonwoven fabric as an assembly of fibers.

[0005] The foaming method is a manufacturing method in which a resin is supplied to an extruder and melt-kneaded while simultaneously injecting a volatile foaming agent into the extruder, or a resin is melt-kneaded together with a foaming agent in the extruder, and then extruded through a die to foam. For example, Patent Document 1 discloses a foam sheet for automobile interior materials, which has inside it a foamed sheet of a modified polyphenylene ether resin that has been investigated using the foaming method.

[0006] The wet method is a manufacturing method in which a resin is dissolved in a good solvent, the solution is cast, and then contacted with a poor solvent to form a porous layer. For example, Patent Document 2 discloses a separator made of an amorphous polymer having a glass transition temperature of 150°C or higher, the surface of which has pores with a smaller pore size than those in the central portion, and describes in the examples how polyphenylene ether is made porous using the wet method. Patent Document 3 also discloses a composite porous membrane in which porous membrane A made of a resin with a melting point of 150° C. or less and porous membrane B made of a resin with a glass transition temperature higher than 150° C. are integrated, and a wet method is being considered for making the porous membrane B porous. Furthermore, Patent Document 4 discloses a composite separation membrane having a separation layer on the surface of a porous support membrane containing 50% by mass or more of polyphenylene ether, and a wet method is being considered for making the porous support membrane porous.

[0007] Methods for producing nonwoven porous bodies as fiber aggregates include the spunbond method, in which continuous fibers spun by melting or dissolving are layered on a moving screen to bond the fibers, and the electrostatic spinning method, in which a polymer solution is discharged using a nozzle or other device into an electrostatic field formed between electrodes, where the solution is atomized and solidified by electrostatic force to deposit ultrafine fibrous matter. Patent Document 5 discloses a multi-layer porous membrane including a porous layer made of a thermoplastic resin and a porous layer made of polyphenylene ether, and the porous layer made of polyphenylene ether is investigated by electrostatic spinning. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2005-88873 A [Patent Document 2] JP 2000-138048 A [Patent Document 3] JP 2007-125821 A [Patent Document 4] WO2014 / 054346 International Publication [Patent Document 5] JP 2009-104834 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, in the foamed sheet disclosed in Patent Document 1, since a foaming agent is used to make the pores porous, it is difficult to control the pore size and pore size distribution, and the porous structure is likely to become non-uniform. In addition, the pore size of the resulting porous structure is relatively large, making it difficult to form a dense porous structure required for separation membranes and porous bodies for electronic components.

[0010] In the porous bodies such as the separator, composite porous membrane, and porous support membrane disclosed in Patent Documents 2 to 4, the pores are made by a wet method, so a large amount of good solvent and poor solvent are used, and a process for removing other components is included, so equipment for recovering the solvent and additives is required, which significantly reduces productivity. Also, in the multilayer porous membrane disclosed in Patent Document 5, a porous layer made of polyphenylene ether is deposited by electrostatic spinning, so a large amount of solvent is required as in the wet method, and a special process of applying a high voltage between the nozzle and the collector and depositing fibers while volatilizing the solvent causes difficulties such as increasing the line speed, which significantly reduces productivity.

[0011] On the other hand, as a method for producing a porous body, a dry method is preferred from the viewpoint of productivity. The dry method is a method in which a resin composition is molded, and then stretched to open structurally weak points such as between crystals and crystal lamellae or the interface between an inorganic filler and a resin to form micropores. However, when a dry method is used to make an amorphous resin such as a polyphenylene ether resin porous, there is no element to stop the propagation of the cracks formed by stretching in the flow direction, width direction, and thickness direction of the molded body, so that the conventional dry porosity breaks during stretching, and a good porous body cannot be obtained.

[0012] The present invention has been made in view of the above problems, and has an object to provide an amorphous resin stretched porous body having excellent porosity, air permeability, heat resistance, mechanical properties, and electrical properties with high productivity, and a method for producing the stretched porous body, and also to provide an electronic component using the stretched porous body. [Means for solving the problem]

[0013] As a result of intensive research conducted in consideration of the above-mentioned problems, the present inventors discovered that the above-mentioned problems can be solved by a stretched porous body having at least one porous layer made of a resin composition containing 50% by mass or more of an amorphous resin, and thus completed the present invention.

[0014] That is, the gist of the present invention is as follows. [1] A stretched porous body having at least one porous layer made of a resin composition containing 50% by mass or more of an amorphous resin (A). [2] The stretched porous body according to [1], wherein the amorphous resin (A) is at least one selected from the group consisting of polyphenylene ether resins, polycarbonate resins, thermoplastic polyimide resins, polyamideimide resins, polyarylate resins, polyetherimide resins, polyethersulfone resins, and polysulfone resins. [3] The stretched porous body according to [2], wherein the amorphous resin (A) is a polyphenylene ether resin. [4] The stretched porous body according to any one of [1] to [3], wherein the stretched porous body has a porosity of 15% or more and 80% or less. [5] The stretched porous body according to any one of [1] to [4], which has a linear expansion coefficient of 70 ppm / °C or less from 0°C to 100°C in at least one direction. [6] The stretched porous body according to any one of [1] to [5], which has a relative dielectric constant of 2.5 or less at a measurement frequency of 10 GHz. [7] The stretched porous body according to any one of [1] to [6], which has a dielectric loss tangent of 0.0060 or less at a measurement frequency of 10 GHz. [8] The expanded porous body according to any one of [1] to [7], which has a relative dielectric constant of 2.5 or less at a measurement frequency of 28 GHz. [9] The expanded porous body according to any one of [1] to [8], which has a dielectric tangent of 0.0060 or less at a measurement frequency of 28 GHz.

[10] The stretched porous body according to any one of [1] to [9], wherein the resin composition contains a thermoplastic elastomer (B).

[11] The stretched porous body according to

[10] , wherein the thermoplastic elastomer (B) is contained in the resin composition in an amount of 0.1% by mass or more and 50% by mass or less.

[12] An electronic component comprising the stretched porous body according to any one of [1] to

[11] .

[13] A method for producing a stretched porous body, comprising the steps of: (a) melt-extruding a resin composition containing 50 mass% or more of an amorphous resin (A), cooling and solidifying the extrudate, and molding the extrudate into a molded body having at least one layer made of the resin composition; and (b) stretching the molded body molded in the step (a) at a temperature that is 10°C or more lower than the glass transition temperature (Tg) of the resin composition.

[14] The method for producing a stretched porous body according to

[13] , wherein the amorphous resin (A) is at least one selected from the group consisting of polyphenylene ether-based resins, polycarbonate-based resins, thermoplastic polyimide-based resins, polyamideimide-based resins, polyarylate-based resins, polyetherimide-based resins, polyethersulfone-based resins, and polysulfone-based resins.

[15] The method for producing a stretched porous body according to

[14] , wherein the amorphous resin (A) is a polyphenylene ether resin.

[16] The method for producing a stretched porous body according to any one of

[13] to

[15] , wherein the shaped body is any one selected from the group consisting of a sheet-like body, a fibrous body, and a hollow body.

[17] The method for producing a stretched porous body according to any one of

[13] to

[16] , wherein the resin composition contains a thermoplastic elastomer (B).

[18] The method for producing a stretched porous body according to

[17] , wherein the thermoplastic elastomer (B) is contained in the resin composition in an amount of 0.1 mass % or more and 50 mass % or less.

[19] The method for producing a stretched porous body according to any one of

[13] to

[18] , wherein in the step (b), the stretching temperature is 60° C. or higher and 160° C. or lower.

[20] The method for producing a stretched porous body according to any one of

[13] to

[19] , further comprising, after the step (b), a step (c) of stretching at a temperature higher than the stretching temperature in the step (b).

[21] The method for producing a stretched porous body according to

[20] , wherein the stretching temperature in the step (c) is higher than the stretching temperature in the step (b) and is within ±15°C of the glass transition temperature (Tg) of the resin composition.

[22] The method for producing a stretched porous body according to

[20] or

[21] , wherein the stretching temperature in the step (c) is higher than the temperature in the step (b) and is 160°C or higher and 260°C or lower. Effect of the Invention

[0015] According to the present invention, it is possible to provide an amorphous resin stretched porous body having excellent porous structure, air permeability, heat resistance, mechanical properties, and electrical properties with high productivity. In particular, since this stretched porous body has both excellent mechanical properties and electrical properties, it is expected to be used as an electronic component. [Brief description of the drawings]

[0016] [Figure 1] 1 is a scanning electron microscope photograph of the surface and cross section of the stretched porous film produced in Example 1. [Diagram 2] 1 is a scanning electron microscope photograph of an enlarged surface and cross section of the stretched porous film produced in Example 1. [Diagram 3] 3 is a scanning electron microscope photograph of the surface and cross section of the stretched porous film produced in Example 2. [Figure 4] 3 is a scanning electron microscope photograph of an enlarged surface and cross section of the stretched porous film produced in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, a detailed description will be given of an amorphous resin stretched porous body (hereinafter, also referred to as "the porous body") as one example of an embodiment of the present invention. However, the scope of the present invention is not limited to the embodiment described below.

[0018] In this specification, the term "main component" refers to a component that occupies the largest percentage by mass when the total of the constituent components is 100% by mass, and is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. Furthermore, when it is written "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" and "preferably smaller than Y". Furthermore, even if the upper and lower limits of the numerical ranges in this specification are slightly outside the numerical ranges specified by the present invention, they are included in the equivalent range of the present invention as long as they have the same action and effect as those within the numerical range.

[0019] <This porous body> The porous body is a stretched porous body having at least one porous layer made of a resin composition containing 50% by mass or more of an amorphous resin (A) (hereinafter, simply referred to as "resin composition"). Here, the "stretched porous body" refers to a porous body that is stretched in at least one axial direction.

[0020] The shape of the porous body is not particularly limited, and may be a type of molded product selected from the group consisting of sheet-like, fibrous, and hollow objects. The term "sheet-like" includes a thick (mm order) plate to a thin (μm order) film, the term "fibrous" includes a thick rod to a thin thread, and the term "hollow" means a thick pipe to a thin tube, hollow fiber, inflation film, etc. Of course, it also includes a sheet-like product cut from an inflation film.

[0021] The porous body may have at least one porous layer made of a resin composition described below. That is, the porous body may be formed only of a porous layer made of the resin composition, or may be formed by laminating it with another layer. When the porous body is a sheet-like material, it may be a laminated sheet-like porous body laminated in the thickness direction of the sheet-like material, when it is a fibrous material, it may be a so-called core-sheath structure porous body, and when it is a hollow material, it may be a porous body laminated in the radial direction of the hollow material. In particular, when the porous body is used for an electronic component, a sheet-like material is preferable.

[0022] Furthermore, it is important that the porous layer made of the resin composition in the present porous body is stretched in at least one axial direction. In a preferred embodiment, the porous layer made of the resin composition is stretched in at least one axial direction, preferably in two axial directions, to make the layer porous, and the present porous body has excellent porous properties.

[0023] When the porous body is used as an electronic component, the thickness of the porous body as a sheet is preferably 1 μm to 400 μm, more preferably 5 μm to 300 μm, and even more preferably 10 to 200 μm. When used as an electronic component, a thickness of 1 μm or more can provide the substantially required electrical insulation, and is excellent in safety, for example, being less likely to short circuit even when a large voltage is applied. Furthermore, if the thickness is 400 μm or less, and preferably 300 μm or less, it is easy to ensure that the electronic components are thin and lightweight.

[0024] The air permeability of the porous body is preferably 1 sec / 100 mL to 60,000 sec / 100 mL, more preferably 1 sec / 100 mL to 40,000 sec / 100 mL, and even more preferably 1 sec / 100 mL to 10,000 sec / 100 mL. If the air permeability is 1 sec / 100 mL to 60,000 sec / 100 mL, it indicates that the porous body has interconnectivity and can exhibit excellent air permeability, which is preferable. Air permeability indicates the difficulty of air passing through in the thickness direction, and is specifically expressed as the number of seconds required for 100 mL of air to pass through the porous body. Therefore, a smaller value means that air passes through more easily, and a larger value means that air passes through less easily. In other words, a smaller value means that the interconnectivity in the thickness direction is better, and a larger value means that the interconnectivity in the thickness direction is worse. Interconnectivity is the connection of pores in the thickness direction. If the air permeability of this porous body is low, it can be used for various purposes. The method for measuring air permeability is described in the Examples section below.

[0025] The porosity of the porous body is preferably 15% or more, more preferably 20% or more, and even more preferably 35% or more. If the porosity is 15% or more, the porous body can be made to have excellent air permeability while ensuring interconnectivity. In addition, the relative dielectric constant and dielectric loss tangent of the porous body can be reduced, which is preferable because the transmission loss can be reduced. On the other hand, the upper limit of the porosity is preferably 80% or less, more preferably 75% or less. If the porosity is 80% or less, the problem of the strength of the porous body being reduced too much due to the excessive increase in micropores is eliminated, which is also preferable from the viewpoint of handling. The measurement method of the porosity is described in the Examples section below.

[0026] In the present porous body, the tensile stress at break E in at least one direction is preferably 5 MPa to 100 MPa, more preferably 8 MPa to 90 MPa, and even more preferably 11 MPa to 80 MPa. The tensile stress at break is described in detail below. In this porous body, for example, the tensile breaking stress E MD is preferably 5 MPa or more and 100 MPa or less, more preferably 8 MPa or more and 90 MPa or less, and even more preferably 11 MPa or more and 80 MPa or less. MD If the compressive strength is 5 MPa or more and 100 MPa or less, the porous body can be prevented from breaking when used in various applications. When the porous body is a sheet-like material, the tensile strength E TD is preferably 5 MPa or more and 100 MPa or less, more preferably 8 MPa or more and 90 MPa or less, and even more preferably 11 MPa or more and 80 MPa or less. MD and E TD Ratio to (E MD / E TD ) is preferably 0.2 or more and 5 or less, and more preferably 0.3 or more and 3 or less. MD / E TD By adjusting the thickness to within the above range, damage due to tearing of the porous body can be suppressed.

[0027] Furthermore, in the present porous body, the linear expansion coefficient at 0° C. to 100° C. in at least one direction is preferably 70 ppm / ° C. or less, more preferably 65 ppm / ° C. or less, and even more preferably 60 ppm / ° C. or less. The linear expansion coefficient is described in detail below. In the present porous body, for example, the linear expansion coefficient in the machine direction (MD) from 0°C to 100°C is preferably 70 ppm / °C or less, more preferably 65 ppm / °C or less, and even more preferably 60 ppm / °C or less. The linear expansion coefficient in the machine direction (MD) from 0°C to 100°C of 70 ppm / °C or less is preferable because the present porous body has excellent dimensional stability when used in a high-temperature atmosphere. In particular, when the present porous body is used for electronic components and laminated with a metal such as copper foil, problems due to differences in the linear expansion coefficient between the laminated object, such as curling and peeling during heating, can be suppressed, which is preferable. Furthermore, when the porous body is a sheet-like product, the linear expansion coefficient of the sheet-like product in the transverse direction (TD) from 0°C to 100°C is preferably 70 ppm / °C or less, more preferably 65 ppm / °C or less, and even more preferably 60 ppm / °C or less. The linear expansion coefficient of the transverse direction (TD) from 0°C to 100°C of 70 ppm / °C or less is preferable because the porous body has excellent dimensional stability when used in a high-temperature atmosphere. In particular, when the porous body is used for electronic components and laminated with a metal such as copper foil, problems due to differences in the linear expansion coefficient between the laminated object, such as curling and peeling during heating, can be suppressed, which is preferable. The linear expansion coefficient is measured as follows. Using a tensile probe, confirm the dimensional changes in MD and TD when the temperature is raised from -10°C to 300°C at 5°C / min. Then, from the obtained dimensional change profile, divide the dimensional change ΔL (mm) from 0°C to 100°C and the strain (=ΔL / L) calculated from the initial dimension L (mm) by the temperature change (ΔT=100°C) to calculate the linear expansion coefficient from 0°C to 100°C.

[0028] The relative dielectric constant of the present porous body at a measurement frequency of 10 GHz is preferably 2.5 or less, more preferably 2.4 or less, and even more preferably 2.3 or less. When this porous body is used in electronic components such as circuit boards, such as flexible printed circuit boards, and laminates for circuits, it is required to increase the signal propagation speed in order to speed up information processing. The signal propagation speed V is determined by the proportionality constant k1, the speed of light c, and the relative dielectric constant ε of the board material. r Therefore, V = k1 × c / ε r 1 / 2 Therefore, when the porous body has a relative dielectric constant of 2.5 or less at a measurement frequency of 10 GHz, it is possible to increase the signal propagation speed when the porous body is used in an electronic component, which is preferable.

[0029] Furthermore, the dielectric tangent of the present porous body at a measurement frequency of 10 GHz is preferably 0.0060 or less, more preferably 0.0055 or less, and even more preferably 0.0050 or less. When the porous body is used in electronic components such as circuit boards, such as flexible printed circuit boards, and laminates for circuits, signals are more likely to be converted into thermal energy in the electronic components as the amount of information processed increases and the frequency bands used become higher, resulting in increased signal transmission loss. The signal transmission loss α is expressed as a function of the proportional constant k2, the frequency f, and the relative dielectric constant ε of the board material. r From the dielectric tangent tanδ of the board material, α=k2×f×ε r 1 / 2 × tan δ. Therefore, when the present porous body has a dielectric tangent of 0.0060 or less at a measurement frequency of 10 GHz, it is possible to reduce transmission loss when the present porous body is used in electronic components, which is preferable.

[0030] The relative dielectric constant of the present porous body at a measurement frequency of 28 GHz is preferably 2.5 or less, more preferably 2.4 or less, and even more preferably 2.3 or less. As described above, by reducing the relative dielectric constant, it is possible to improve the signal propagation speed and suppress the transmission loss. On the other hand, due to the increase in communication volume in recent years and the demand for improving information processing speed, the use of high-frequency information communication such as the microwave SHF band of 3 to 30 GHz has been promoted from the ultra-high frequency UHF band of 2 GHz or less that has been used conventionally. As shown in the above-mentioned transmission loss formula, the transmission loss increases as the frequency increases. Therefore, it is preferable that the relative dielectric constant of this porous body at a measurement frequency of 28 GHz is 2.5 or less, because it is possible to reduce the transmission loss even when using this porous body at high frequencies when used in electronic components.

[0031] In addition, the dielectric loss tangent of the porous body at a measurement frequency of 28 GHz is preferably 0.0060 or less, more preferably 0.0055 or less, and even more preferably 0.0050 or less. As described above, the higher the frequency, the greater the transmission loss. When the porous body is used in an electronic component, the dielectric loss tangent of the porous body at a measurement frequency of 28 GHz is preferably 0.0060 or less, because this allows the transmission loss to be reduced even when the porous body is used in an electronic component at high frequencies. Here, the relative dielectric constant and the dielectric loss tangent were measured at the respective measurement frequencies using an AET cavity resonator (TE mode) at room temperature of 26°C and humidity of 40% in accordance with JIS R1641 (2007).

[0032] Although the structural characteristics of the porous body vary depending on the resin composition constituting the porous body and the manufacturing method of the porous body, which will be described later, the porous body has a characteristic porous structure in which crazes are present in the internal structure. The crazes are considered to have been generated when the resin composition constituting the porous body is plastically deformed by stretching, and are observed as microscopic damage. According to the manufacturing method of the present porous body described below, a structural form in which crazes propagate in a direction perpendicular to the stretching direction can be seen, which is one of the characteristics of the porous structure of the present porous body. For example, when the porous body is a sheet-like material and is a stretched porous body stretched in the machine direction (MD), a structural form in which crazes propagate in the width direction (TD) of the sheet-like material is often observed on the surface of the sheet-like material. Also, a structural form in which crazes propagate in the thickness direction (hereinafter sometimes referred to as "THD") of the sheet-like material is often observed on the cross section (MD cross section) of the sheet-like material parallel to the stretching direction. The crazes can be confirmed by a scanning electron microscope, a transmission electron microscope, or the like.

[0033] Each component of the resin composition constituting the present porous body will be described below.

[0034] <Amorphous resin (A)> It is important that the resin composition constituting the present porous body contains 50% by mass or more of the amorphous resin (A). The amount of the amorphous resin (A) contained in the resin composition is preferably 60% by mass or more, and more preferably 70% by mass or more.

[0035] The amorphous resin (A) used in the present invention is not particularly limited as long as it is amorphous, and suitable examples thereof include polyphenylene ether resins, polycarbonate resins, thermoplastic polyimide resins, polyamideimide resins, polyarylate resins, polyetherimide resins, polyethersulfone resins, polysulfone resins, etc. These resins may be used alone or in combination of two or more. Among these amorphous resins (A), polyphenylene ether resins are preferred from the viewpoint of dielectric properties.

[0036] The polyphenylene ether resin preferably used in the present invention is a homopolymer or copolymer having a repeating unit represented by the following general formula (1) as a main repeating unit. Here, the main repeating unit refers to a repeating unit contained in a proportion of 50 mol % or more of all repeating units constituting the polyphenylene ether resin. The polyphenylene ether resin may be used alone or in the form of a blend of two or more kinds of polyphenylene ether resins.

[0037] [ka] ...General formula (1)

[0038] In general formula (1), R1, R2, R3, and R4 are each independently a monovalent residue selected from the group consisting of an alkyl group having 1 to 4 carbon atoms which may have a substituent, an aryl group having 6 to 12 carbon atoms, a halogen atom, and a hydrogen atom. Examples of the substituent include a hydroxyl group and a halogen atom. Furthermore, R3 and R4 are preferably hydrogen atoms, and therefore, the polyphenylene ether resin (A) preferably contains a repeating unit represented by the following general formula (2) as a main repeating unit.

[0039] [ka] ...General formula (2)

[0040] In the general formula (2), R1 and R2 are the same as above. Among these, in the general formula (2), R1 and R2 are preferably an alkyl group having 1 to 4 carbon atoms which may have a substituent, an aryl group having 6 to 8 carbon atoms, or a halogen atom.

[0041] Examples of homopolymers of polyphenylene ether resins used in the present invention include poly(2,6-dimethyl-1,4-phenylene) ether, poly(2-methyl-6-ethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2-ethyl-6-n-propyl-1,4-phenylene) ether, poly(2,6-di-n-propyl-1,4-phenylene) ether, poly(2-methyl-6-n-butyl-1,4-phenylene) ether, poly(2-methyl-6-isopropyl-1,4-phenylene) ether, and poly(2-ethyl-6-isopropyl-1,4-phenylene) ether. ether, poly(2,6-dichloro-1,4-phenylene) ether, poly(2,6-dibromo-1,4-phenylene) ether, poly(2-chloro-6-methyl-1,4-phenylene) ether, poly(2-bromo-6-methyl-1,4-phenylene) ether, poly(2-chloro-6-bromo-1,4-phenylene) ether, poly(2-chloro-6-ethyl-1,4-phenylene) ether, poly(2-bromo-6-ethyl-1,4-phenylene) ether, poly(2-methyl-6-chloroethyl-1,4-phenylene) ether, poly(2-methyl-6-hydroxyethyl-1,4-phenylene) ether, etc. Among these, poly(2,6-dimethyl-1,4-phenylene) ether is preferred from the viewpoints of ease of raw material availability and processability.

[0042] Examples of the copolymer of polyphenylene ether resin used in the present invention include those mainly composed of polyphenylene ether structure, such as a copolymer of 2,6-dimethylphenol and 2,3,6-trimethylphenol, a copolymer of 2,6-dimethylphenol and o-cresol, and a copolymer of 2,3,6-trimethylphenol and o-cresol. Among them, from the viewpoint of easy availability of raw materials and processability, when a copolymer of polyphenylene ether resin is used, it is preferable to use a copolymer of 2,6-dimethylphenol and 2,3,6-trimethylphenol.

[0043] The polyphenylene ether resin may contain various other phenylene ether units other than the general formula (1). Examples of the various other phenylene ether units other than the general formula (1) include, but are not limited to, 2-(dialkylaminomethyl)-6-methylphenylene ether units and 2-(N-alkyl-N-phenylaminomethyl)-6-methylphenylene ether units described in JP-A-01-297428 and JP-A-63-301222. The polyphenylene ether resin may have a small amount of repeating units derived from diphenoquinone or the like bonded to the main chain of the polyphenylene ether.

[0044] The polyphenylene ether resin may contain a functionalized polyphenylene ether in which a part or all of the structural units constituting the polyphenylene ether are reacted (modified) with a functionalizing agent, or may be a functionalized polyphenylene ether. Examples of the functionalized polyphenylene ether include an acyl group (e.g., a carboxyl group, an acid anhydride group, an acid amide group, an imide group, a group derived from an ammonium carboxylate, etc.), an amide group, an orthoester group, and a hydroxyl group.

[0045] The functionalized polyphenylene ether is preferably a functionalized polyphenylene ether obtained by melt-kneading a mixture of polyphenylene ether and unsaturated carboxylic acid or acid anhydride, and more preferably a maleic anhydride-modified polyphenylene ether obtained by melt-kneading a mixture of polyphenylene ether and maleic anhydride. The maleic anhydride-modified polyphenylene ether can be obtained, for example, by feeding 0.1 to 5 parts by mass of maleic anhydride per 100 parts by mass of polyphenylene ether into a twin-screw extruder and melt-kneading at a temperature of 270 to 335°C.

[0046] The weight average molecular weight Mw of the amorphous resin (A) is preferably 40,000 to 400,000, more preferably 50,000 to 300,000, and even more preferably 60,000 to 200,000. The number average molecular weight Mn of the amorphous resin (A) is preferably 5,000 to 200,000, more preferably 10,000 to 150,000, and even more preferably 20,000 to 100,000. The ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn value) is preferably 1.0 or more from the viewpoint of moldability, and is preferably 5.5 or less from the viewpoint of mechanical properties, more preferably 1.5 to 4.5, and even more preferably 2.0 to 4.5. The weight average molecular weight Mw and the number average molecular weight Mn are obtained from the polystyrene equivalent molecular weight measured by GPC (gel permeation chromatography).

[0047] The reduced viscosity of the amorphous resin (A) is preferably 0.25 dL / g or more from the viewpoint of mechanical properties, and is preferably 0.65 dL / g or less from the viewpoint of moldability, more preferably 0.27 to 0.63 dL / g, even more preferably 0.30 to 0.60 dL / g, and particularly preferably 0.33 to 0.55 dL / g. The reduced viscosity can be measured using a 0.5 g / dL chloroform solution at a temperature of 30° C. using an Ubbelohde type viscometer.

[0048] The glass transition temperature of the amorphous resin (A) can be determined depending on the ratio of the constituent monomers, but when the porous body is used in electronic components, the glass transition temperature is preferably 120°C or higher, more preferably 140°C or higher, and even more preferably 160°C or higher, from the viewpoint of the required heat resistance. Here, the glass transition temperature is the midpoint temperature (°C) of the baseline shift part of the thermogram profile measured using a differential scanning calorimeter (DSC) when approximately 10 mg of resin is heated from 0°C to 280°C at a heating rate of 10°C / min, held at 280°C for 1 minute, cooled to 0°C at a cooling rate of 10°C / min, and then heated again to 280°C at a heating rate of 10°C / min.

[0049] The resin composition constituting the present porous body contains, in addition to the amorphous resin (A) represented by a polyphenylene ether-based resin, a thermoplastic elastomer (B), a polystyrene-based resin (C), and a flame retardant (D), which will be described later. Examples of other additives that can be contained in the amorphous resin (A) include heat stabilizers, antioxidants, ultraviolet (UV) absorbers, surfactants, lubricants, fillers, polymer additives, dialkyl peroxides, diacyl peroxides, peroxycarbonates, hydroperoxides, peroxyketals, inorganic fillers (talc, kaolin, xonotlite, wollastonite, titanium oxide, potassium titanate, carbon fiber, glass fiber, etc.), known silane coupling agents for increasing the affinity between the inorganic filler and the resin, fluorine-based polymers exhibiting an anti-dripping effect, plasticizers (oil, low molecular weight polyolefins, polyethylene glycol, fatty acid esters, etc.), flame retardant assistants such as antimony trioxide, colorants such as carbon black, antistatic agents, various peroxides, metal stabilizers such as zinc oxide and zinc sulfide, organic stabilizers such as hindered phenol stabilizers, phosphorus stabilizers, and hindered amine stabilizers, and light stabilizers. In addition, a commercially available resin composition (for example, a resin composition containing a polyphenylene ether resin) containing the amorphous resin (A) and the thermoplastic elastomer (B) or the above-mentioned additives can also be used.

[0050] <Thermoplastic elastomer (B)> The resin composition constituting the porous body preferably contains a thermoplastic elastomer (B). The content of the thermoplastic elastomer (B) is preferably 0.1% by mass or more and 50% by mass or less, more preferably 0.5% by mass or more and 40% by mass or less, and even more preferably 0.5% by mass or more and 30% by mass or less, based on 100% by mass of the resin composition constituting the porous body. The resin composition contains 0.1% by mass or more of the thermoplastic elastomer (B), which is preferable because stress concentration occurs at the interface between the amorphous resin (A) such as the polyphenylene ether resin and the thermoplastic elastomer (B) when the resin composition is stretched at least in one axial direction to form a pore structure, making it easier to generate pore starting points (crazes). In addition, the thermoplastic elastomer (B) plays a role in stopping the propagation of generated crazes within the resin composition, making it less likely to cause problems such as breakage in the production of this porous body. In addition, the thermoplastic elastomer (B) contains 50% by mass or less of the thermoplastic elastomer (B), which is preferable because it is easier to maintain the heat resistance of the resulting porous body.

[0051] The weight average molecular weight Mw of the thermoplastic elastomer (B) is preferably 150,000 or more, more preferably 160,000 or more and 1,000,000 or less, even more preferably 170,000 or more and 800,000 or less, and particularly preferably 180,000 or more and 600,000 or less. The ratio (molecular weight distribution) Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn of the thermoplastic elastomer (B) is preferably 1.00 or more and 2.00 or less, more preferably 1.00 or more and 1.80 or less, and even more preferably 1.00 or more and 1.50 or less.

[0052] The reason why the weight average molecular weight Mw of the thermoplastic elastomer (B) is preferably 150,000 or more is that when a layer made of a resin composition containing the amorphous resin (A) and the thermoplastic elastomer (B) is stretched at least in one axial direction to make it porous, the thermoplastic elastomer (B) is likely to exist as particulate domains in the matrix mainly composed of the amorphous resin (A) in the resin composition before stretching, and it becomes easy to obtain a porous body having a uniform porous structure and excellent air permeability.

[0053] In general, when a resin composition having a sea-island structure of matrix / domain is melt-extruded and cooled to solidify, the resin composition extruded and flowing from a shaping device such as a die or nozzle is cooled and solidified by a cooling and solidifying device such as a cast roll (cooling roll) or air-cooling or water-cooling. At that time, the resin composition melts and elongates in the gap (gap) between the shaping device and the cooling and solidifying device, so that when the weight-average molecular weight Mw of the thermoplastic elastomer (B) which is the domain is small, a resin composition in which the domain is elongated in the flow direction (extrusion direction) is easily obtained. When the resin composition in which the domains are stretched in the flow direction (extrusion direction) is stretched, the stress imparted by the deformation is easily applied uniformly to the entire resin composition, which tends to prevent stress concentration at the matrix / domain interface, because the cross-sectional area of ​​the interface receiving the stress is small due to the domains being stretched in advance.

[0054] On the other hand, when the weight-average molecular weight Mw of the domain is large, the domain is less susceptible to the effect of melt elongation, and the domain in the obtained resin composition before stretching is likely to maintain a particulate shape. Therefore, when the obtained resin composition is stretched, the stress applied by deformation is likely to concentrate at the matrix / domain interface, and the cross-sectional area of ​​the interface receiving the stress is also large, so that interfacial peeling is likely to occur, and as a result, a uniform porous structure is likely to be formed.

[0055] Furthermore, if the weight average molecular weight Mw of the thermoplastic elastomer (B) is less than 150,000, the thermoplastic elastomer (B) is likely to bleed out from the resulting porous body, which tends to accelerate deterioration over time.

[0056] Furthermore, when the ratio (molecular weight distribution) Mw / Mn of the number average molecular weight Mn to the weight average molecular weight Mw of the thermoplastic elastomer (B) is within the above-mentioned preferred range, the dispersed diameter of the formed domains tends to be uniform, which is preferable.

[0057] In the present invention, the weight average molecular weight Mw and number average molecular weight Mn of the thermoplastic elastomer (B) are obtained from the polystyrene equivalent molecular weight measured by GPC (gel permeation chromatography) based on JIS K7252-1 (2008).

[0058] Furthermore, the melt flow rate (MFR) of the thermoplastic elastomer (B) at a temperature of 230°C and a load of 2.16 kg is preferably 30 g / 10 min or less, more preferably 10 g / 10 min or less, even more preferably 5 g / 10 min or less, even more preferably 1 g / 10 min or less, and most preferably does not flow.

[0059] As described above, when the resin composition contains the thermoplastic elastomer (B), it is preferable for the thermoplastic elastomer (B) existing as domains in a particulate form in a matrix mainly composed of the amorphous resin (A) in order to obtain a porous body having a uniform porous structure and excellent air permeability. Therefore, when the MFR of the thermoplastic elastomer (B) at a temperature of 230°C and a load of 2.16 kg is 30 g / 10 min or less, the domains of the thermoplastic elastomer (B) are unlikely to stretch in the flow direction (extrusion direction), and the domains in the resulting resin composition before stretching tend to maintain a particulate shape, which is preferable. The MFR of the thermoplastic elastomer (B) is measured based on JIS K7210-1 (2014).

[0060] The thermoplastic elastomer (B) used in the present invention refers to an amide-based thermoplastic elastomer, an ester-based thermoplastic elastomer, an olefin-based thermoplastic elastomer, a styrene-based thermoplastic elastomer, a urethane-based thermoplastic elastomer, a dynamically vulcanized thermoplastic elastomer, a vinyl chloride-based thermoplastic elastomer, an acrylic-based thermoplastic elastomer, a lactic acid-based thermoplastic elastomer, a diene-based thermoplastic elastomer, a fluorine-based thermoplastic elastomer, a silicone-based thermoplastic elastomer, an ionomer, as well as blends, alloys, modified products, and dynamically crosslinked products thereof, and also includes block copolymers, graft copolymers, random copolymers, and core-shell type multilayer structure rubbers. Among these, olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, acrylic-based thermoplastic elastomers, urethane-based thermoplastic elastomers, and diene-based thermoplastic elastomers are preferred, and from the viewpoints of viscosity and compatibility, styrene-based thermoplastic elastomers, acrylic-based thermoplastic elastomers, and diene-based thermoplastic elastomers are particularly preferred.

[0061] When the thermoplastic elastomer (B) is a styrene-based thermoplastic elastomer, styrene-butadiene copolymer, styrene-butadiene-styrene copolymer, styrene-ethylene-butylene-styrene copolymer, styrene-ethylene-propylene-styrene copolymer, styrene-ethylene-propylene copolymer, styrene-isoprene-styrene copolymer, styrene-ethylene-(ethylene-propylene)-styrene copolymer, styrene-isobutylene-styrene copolymer, and modified products thereof, hydrogenated products, graft copolymers having a styrene structure in the side chain, core-shell type multi-layer structure rubber having a styrene structure, etc. can be suitably used, and may be a blend of two or more kinds. Among them, styrene-ethylene-butylene-styrene copolymer, styrene-ethylene-propylene-styrene copolymer, styrene-ethylene-(ethylene-propylene)-styrene copolymer, and core-shell type multi-layer structure rubber having a styrene structure are preferred.

[0062] When the thermoplastic elastomer (B) is a styrene-based thermoplastic elastomer, the styrene content of the styrene-based thermoplastic elastomer is preferably 1% by mass or more and 90% by mass or less, more preferably 2% by mass or more and 85% by mass or less, further preferably 3% by mass or more and 80% by mass or less, and most preferably 5% by mass or more and 75% by mass or less. The styrene content of a styrene-based thermoplastic elastomer is the ratio of structural units derived from styrene to all structural units (structural units derived from all raw material monomers) that constitute the styrene-based thermoplastic elastomer, and is determined by composition analysis using a nuclear magnetic resonance (NMR) spectrometer.

[0063] When the thermoplastic elastomer (B) is an acrylic thermoplastic elastomer, it is preferably a copolymer having a (meth)acrylic acid ester monomer. Here, the (meth)acrylic acid ester refers to a methacrylic acid ester and / or an acrylic acid ester. Examples of the (meth)acrylic acid ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, stearyl (meth)acrylate, octadecyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, and chloromethyl (meth)acrylate. , 2-chloroethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2,3,4,5-tetrahydroxypentyl (meth)acrylate, aminoethyl (meth)acrylate, propylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, ethylaminopropyl (meth)acrylate, phenylaminoethyl (meth)acrylate, cyclohexylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate. As the acrylic thermoplastic elastomer, methyl (meth)acrylate-butyl (meth)acrylate copolymer, methyl (meth)acrylate-butyl (meth)acrylate-methyl (meth)acrylate copolymer, methyl (meth)acrylate-butadiene-styrene copolymer, methyl (meth)acrylate-silicone copolymer, methyl (meth)acrylate-butyl (meth)acrylate-silicone copolymer, and modified products thereof, hydrogenated products, graft copolymers having a (meth)acrylic acid ester structure in the side chain, core-shell type multi-layer structure rubber having a (meth)acrylic acid ester structure, etc. can be suitably used, and a blend of two or more kinds may be used. Among them, methyl (meth)acrylate-butyl (meth)acrylate copolymer, methyl (meth)acrylate-butyl (meth)acrylate-methyl (meth)acrylate copolymer, and core-shell type multi-layer structure rubber having a (meth)acrylic acid ester structure are preferred.

[0064] When the thermoplastic elastomer (B) is an acrylic thermoplastic elastomer, the methyl methacrylate content of the acrylic thermoplastic elastomer is preferably 1% by mass or more and 90% by mass or less, more preferably 2% by mass or more and 85% by mass or less, further preferably 3% by mass or more and 80% by mass or less, and most preferably 5% by mass or more and 75% by mass or less. The methyl methacrylate content of an acrylic thermoplastic elastomer is the proportion of structural units derived from methyl methacrylate among all structural units (structural units derived from all raw material monomers) constituting the acrylic thermoplastic elastomer, and is determined by composition analysis using a nuclear magnetic resonance (NMR) spectrometer.

[0065] The reason why the styrene content of the styrene-based thermoplastic elastomer is preferably 1% by mass or more and 90% by mass or less, and the reason why the methyl methacrylate content of the acrylic thermoplastic elastomer is preferably 1% by mass or more and 90% by mass or less, is that when the layer made of the resin composition is stretched at least in one axial direction to make it porous, the difference in elastic modulus between the amorphous resin (A) and the thermoplastic elastomer (B) in the resin composition before stretching can be increased, and the starting point (craze) of the porosity due to stress concentration at the interface can be easily formed. Also, the impact absorption of the thermoplastic elastomer (B) can be improved, and the propagation of the crazes generated in the resin composition can be efficiently suppressed.

[0066] When the thermoplastic elastomer (B) is a diene-based thermoplastic elastomer, a thermoplastic elastomer having a carbon-carbon double bond in the main chain, such as polybutadiene, polyisoprene, or polychloroprene, can be preferably used. In addition, a random polymer, block polymer, or graft polymer with other copolymerizable monomers, such as a styrene-isoprene copolymer or a styrene-isoprene-butadiene copolymer, can be preferably used. Examples of the copolymerizable monomer include vinyl aromatic compounds such as styrene and α-methylstyrene, unsaturated carboxylic acids such as acrylic acid and methacrylic acid, and esters thereof, and vinyl cyanide compounds such as acrylonitrile and methacrylonitrile. In addition, modified products thereof, partially hydrogenated products, and core-shell type multilayer rubbers having a carbon-carbon double bond structure can also be preferably used.

[0067] The resin composition constituting the present porous body may contain only one type of the above thermoplastic elastomer (B), or may contain two or more types.

[0068] <Polystyrene resin (C)> The resin composition constituting the porous body may contain a polystyrene resin (C). The polystyrene resin (C) in the present invention is a resin containing more than 90 mass% and not more than 100 mass% of a styrene monomer in the resin. This polystyrene resin (C) may be a homopolymer of a styrene monomer, or a copolymer containing a styrene monomer and another monomer. In addition, the content of the polystyrene resin (C) is preferably 0 mass% or more and 40 mass% or less with respect to 100 mass% of the resin composition constituting the porous body.

[0069] When the polystyrene resin (C) is a copolymer, it may be a multicomponent copolymer containing two or more kinds of other monomer components, and the copolymer may be any copolymer form such as a random copolymer, a block copolymer, or a graft copolymer.

[0070] The polystyrene resin (C) may be a linear polystyrene resin or a hyperbranched polystyrene resin, and may be one type of polystyrene resin (C), or may be a mixture of two or more types of polystyrene resins having different monomer component types, composition ratios, physical properties, etc.

[0071] Examples of the styrene monomer include styrene and its derivatives. For example, alkyl styrenes such as styrene, α-methylstyrene, dimethylstyrene, trimethylstyrene, ethylstyrene, diethylstyrene, triethylstyrene, propylstyrene, butylstyrene, hexylstyrene, heptylstyrene, and octylstyrene, halogenated styrenes such as fluorostyrene, chlorostyrene, bromostyrene, dibromostyrene, and iodostyrene, nitrostyrene, acetylstyrene, and methoxystyrene. Among them, from the viewpoint of heat resistance and processability, it is preferable to use styrene and α-methylstyrene, and styrene is particularly preferable.

[0072] Examples of other monomers used in the copolymer include (meth)acrylic acid, (meth)acrylic acid esters, maleic anhydride, vinyl acetate, acrylonitrile, diene hydrocarbons such as butadiene, isoprene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene, and α-olefins such as ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene.

[0073] In addition, as the polystyrene resin (C), an impact-resistant polystyrene resin can also be suitably used. As the impact-resistant polystyrene resin, a resin obtained by graft-polymerizing a styrene monomer onto the diene thermoplastic elastomer (hereinafter, sometimes referred to as "graft-type HIPS") can be used. The graft-type HIPS can be formed, for example, by dissolving the diene thermoplastic elastomer in a styrene monomer, and then graft-polymerizing the styrene monomer onto the diene thermoplastic elastomer, and the resulting polymer preferably forms a salami structure in which the diene thermoplastic elastomer is dispersed in the polystyrene. In the salami structure, the diene thermoplastic elastomer is bonded to a part of the polystyrene outside the salami.

[0074] The impact-resistant polystyrene resin may be a blend of polystyrene obtained by polymerizing a styrene monomer and a diene thermoplastic elastomer (a blended HIPS). In this case, the polystyrene may be obtained by bulk polymerization or suspension polymerization of the styrene monomer. As a kneading method, a single-screw or multi-screw extruder or a general-purpose kneader such as a Banbury mixer may be used.

[0075] (Flame retardant (D)) The resin composition constituting the porous body may contain a flame retardant (D). The flame retardant (D) is not particularly limited, but is preferably an aromatic phosphate ester flame retardant. The flame retardant (D) may be used alone or in combination of two or more. By containing the flame retardant (D) in the resin composition constituting the porous body, the porous body can be imparted with flame retardancy, and the thermal stability and melt fluidity of the resin composition constituting the porous body can be increased.

[0076] As the aromatic phosphate ester-based flame retardant, for example, triphenyl-substituted aromatic phosphate esters such as triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, xylenyl diphenyl phosphate, dixylenyl phenyl phosphate, hydroxynonbisphenol phosphate, resorcinol bisphosphate, bisphenol A bisphosphate, and condensates of the above aromatic phosphate esters (aromatic condensed phosphate esters) are preferably used, although they are not limited thereto. Among them, bisphenol A bisphosphate, condensates of bisphenol A bisphosphate, trixylenyl phosphate, and condensates of trixylenyl phosphate are more preferably used.

[0077] When the porous body contains a flame retardant (D), the content of the flame retardant (D) is preferably 0.1% by mass or more and 30% by mass or less, more preferably 0.2% by mass or more and 25% by mass or less, and even more preferably 0.5% by mass or more and 20% by mass or less, based on 100% by mass of the resin composition constituting the porous body. If the content of the flame retardant (D) is 0.1% by mass or more, it is preferable to impart the desired flame retardancy. Also, if it is 30% by mass or less, it is preferable to maintain the heat resistance and dimensional stability of the porous body.

[0078] <Resin composition constituting the present porous layer> The porous layer is made of a resin composition containing 50% by mass or more of an amorphous resin (A). On the other hand, the amorphous resin (A) such as polyphenylene ether is often commercially available in a state where various resins and additives are previously contained, and the physical properties such as the weight average molecular weight, number average molecular weight, reduced viscosity, and glass transition temperature of the amorphous resin (A) may change depending on the type and amount of the added resin or additive. Therefore, the preferable range of each physical property value in the resin composition constituting the present porous layer will be explained.

[0079] The weight average molecular weight Mw of the resin composition constituting the porous layer is preferably 40,000 to 400,000, more preferably 50,000 to 300,000, and even more preferably 60,000 to 200,000. The number average molecular weight Mn of the resin composition constituting the porous layer is preferably 5,000 to 200,000, more preferably 10,000 to 150,000, and even more preferably 20,000 to 100,000. The ratio of the weight average molecular weight Mw to the number average molecular weight Mn (Mw / Mn value) is preferably 1.0 or more from the viewpoint of moldability, and is preferably 5.5 or less from the viewpoint of mechanical properties, more preferably 1.5 to 4.5, and even more preferably 2.0 to 4.5. The weight average molecular weight Mw and the number average molecular weight Mn are obtained from the polystyrene equivalent molecular weight measured by GPC (gel permeation chromatography). In addition, when two or more peaks are obtained in the GPC measurement of the resin composition, the weight average molecular weight Mw and the number average molecular weight Mn are calculated from each peak. In this case, the weight average molecular weight Mw and the number average molecular weight Mn of the resin composition mean the weight average molecular weight Mw and the number average molecular weight Mn of the polymer component excluding the monomer component, which are obtained by measuring the resin composition with GPC. In addition, the monomer component is a low molecular weight component having a peak with a weight average molecular weight Mw of less than 900 and a number average molecular weight Mn of less than 900.

[0080] The reduced viscosity of the resin composition constituting the porous layer is preferably 0.25 dL / g or more from the viewpoint of mechanical properties, and is preferably 0.65 dL / g or less from the viewpoint of moldability, more preferably 0.27 to 0.63 dL / g, even more preferably 0.30 to 0.60 dL / g, and particularly preferably 0.33 to 0.55. The reduced viscosity can be measured using a 0.5 g / dL chloroform solution at a temperature of 30° C. using an Ubbelohde type viscometer.

[0081] When the porous body is used in an electronic component, the glass transition temperature of the resin composition constituting the porous layer is preferably 120° C. or higher, more preferably 140° C. or higher, and even more preferably 160° C. or higher, from the viewpoint of required heat resistance. The upper limit of the glass transition temperature of the resin composition is not particularly limited, but is 350° C.

[0082] The resin composition constituting the porous layer may contain other resins (hereinafter, sometimes simply referred to as other resins) other than the amorphous resin (A), the thermoplastic elastomer (B), and the polystyrene-based resin (C) within the range that does not impair the effects of the present invention. Examples of the other resins include polyolefin resins, acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polyester resins, polyamide resins, ethylene vinyl alcohol copolymers, ethylene vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polylactic acid resins, polybutylene succinate resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyurethane resins, polyphenylene sulfide resins, polyvinyl acetal resins, polybutene resins, polyamide bismaleimide resins, polyether ether ketone resins, polyether ketone resins, polyketone resins, aramid resins, and fluorine-based resins.

[0083] In addition to the flame retardant (D) described above, additives generally blended in resin compositions can be appropriately added to the resin composition constituting the porous layer within a range that does not significantly impair the effects of the present invention. Examples of such additives include recycled resins generated from trimming losses such as ears, which are added for the purpose of improving and adjusting molding processability, productivity, and various physical properties, additives such as glass fiber, glass flakes, milled glass fiber, glass beads, calcium sulfate, calcium carbonate, aluminum carbonate, silica, mica, talc, kaolin, chlorite, carbon fiber, carbon black, graphite, titanium oxide, and zinc oxide, additives such as weather resistance stabilizers, heat resistance stabilizers, antistatic agents, melt viscosity improvers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizers, antifogging agents, antiblocking agents, slip agents, and colorants. In particular, it is preferable that zinc oxide is contained from the viewpoint of thermal stability and deodorization.

[0084] <Method of manufacturing the porous body> Next, the method for producing the porous body will be described. As described above, the porous body has at least one porous layer made of a resin composition containing 50% by mass or more of an amorphous resin (A). In the method for producing the porous body, it is important that the layer made of the resin composition is stretched in at least one axial direction to make it porous. A specific example of the method for producing the present porous body is a method for producing a stretched porous body, which comprises, in this order, a step (a) of melt-extruding a resin composition containing 50% by mass or more of an amorphous resin (A), cooling and solidifying the resin composition, and molding the resin composition into a molded body having at least one layer made of the resin composition, and a step (b) of stretching the molded body formed in the step (a) at a temperature at least 10°C lower than the glass transition temperature (Tg) of the resin composition. The amorphous resin (A) and the resin composition are as described above.

[0085] The production method preferably further comprises, after the step (b), a step (c) of stretching at a temperature higher than the stretching temperature in the step (b). The method for producing the porous body will be specifically described below, but the method for producing the porous body is not limited to the method described below.

[0086] [Process (a)] In the step (a), a resin composition containing 50% by mass or more of an amorphous resin (A) is melt-extruded, cooled and solidified, and molded into a molded article having at least one layer made of the resin composition. The molded article is preferably one selected from the group consisting of a sheet-like article, a fibrous article, and a hollow article. The resin composition is melt-extruded, cooled and solidified into a molded product selected from the group consisting of a sheet-like product, a fibrous product, and a hollow product having at least one substantially non-porous layer made of the resin composition, and the method of molding the product is not particularly limited, and a known method may be used. For example, the resin composition is melted using an extruder, extruded from a shaping device such as a T-die, a round die, a nozzle, or a hollow nozzle, and cooled and solidified using a cast roll (cooling roll), air cooling, water cooling, or other equipment. In addition, a method of cutting a film-like product produced by an inflation method or a tubular method into a flat shape can also be applied. The term "substantially non-porous layer" means that no pores are intentionally provided in the layer during the process of melt-extruding the resin composition, cooling, solidifying, and molding it. In addition, when fine pinholes are unintentionally formed due to unforeseen factors during the process, they are included in the term "substantially non-porous layer."

[0087] In the melt extrusion of the resin composition, the extrusion temperature is appropriately adjusted depending on the flow characteristics and moldability of the resin composition, but when a polyphenylene ether resin is used as the amorphous resin (A), in consideration of its thermal decomposition temperature, it is preferably about 230 to 330°C, more preferably 240 to 320°C, and even more preferably 250 to 310°C. When the extrusion temperature is above the lower limit, the viscosity of the molten resin is sufficiently low, and the moldability is excellent, so that the productivity is improved. On the other hand, by setting the extrusion temperature below the upper limit, deterioration and thermal decomposition of the resin composition and a decrease in the mechanical strength of the obtained porous body can be suppressed. The cooling and solidifying temperature, for example, the cooling and solidifying temperature of a casting roll, is preferably 20 to 200° C., more preferably 40 to 190° C., and even more preferably 50 to 180° C. By setting the cooling and solidifying temperature to the above lower limit or higher, the resin composition can be shaped and solidified into a predetermined shape, and a porous body can be easily formed during stretching, which is preferable. By setting the cooling and solidifying temperature to the above upper limit or lower, problems such as the extruded molten resin sticking to and wrapping around the casting roll are less likely to occur, and efficient molding is possible, which is preferable.

[0088] [Step (b)] Step (b) is a step of stretching the molded body formed in step (a) at a temperature at least 10°C lower than the glass transition temperature (Tg) of the resin composition (hereinafter, this step (b) may be referred to as a "low-temperature stretching step"). The stretching method in step (b) includes roll stretching, rolling, tenter stretching, simultaneous biaxial stretching, and the like, which may be performed alone or in combination of two or more. Among them, stretching in the flow direction (i.e., extrusion direction or take-up direction, hereinafter sometimes referred to as "machine direction" or "MD") in step (a) is preferred from the viewpoint of productivity, and roll stretching, which is easy to increase the stretching speed, is preferred from the viewpoint of generating starting points (cracks) for porosity in the resin composition.

[0089] It is important that the stretching temperature is at least 10° C. lower than the glass transition temperature (Tg) of the resin composition. When stretched at such a temperature, the elastic modulus of the amorphous resin (A) in the resin composition does not become too low, and stress concentration in the resin composition occurs appropriately, so that the layer made of the resin composition can be easily made porous. For example, when a polyphenylene ether resin is used as the amorphous resin (A), a specific example of the temperature 10° C. or more lower than the glass transition temperature (Tg) is preferably 60° C. or more and 160° C. or less. Stretching at a temperature of 60° C. or more is preferable in terms of production because no special equipment is required. In addition, the stretching stress in the stretching atmosphere can be adjusted to be lower than the tensile breaking stress of the polyphenylene ether resin, so that deformation can follow the stretching and there is little risk of breakage. On the other hand, when stretching at a temperature of 160° C. or less, the elastic modulus of the polyphenylene ether resin is not too low, and stress concentration in the resin composition is appropriately expressed, so that the layer made of the resin composition can be easily made porous. The temperature in the low-temperature stretching step depends on the type and characteristics of the polyphenylene ether resin used, but is particularly preferably 80° C. or more and 160° C. or less, and more preferably 100° C. or more and 160° C. or less. When a resin other than a polyphenylene ether resin is used as the amorphous resin (A), the temperature in the low-temperature stretching step may be appropriately set depending on the type of resin.

[0090] In addition, the total stretching ratio in this low-temperature stretching step is not particularly limited, but is preferably 1.15 times or more and 4.00 times or less, particularly 1.25 times or more and 3.00 times or less. If the stretching ratio is above the lower limit, stress is concentrated at the matrix / domain interface, and a porous structure is easily formed due to peeling of the interface caused by deformation, and if it is below the upper limit, the formed porous structure is not blocked by excessive deformation and there is little risk of breakage, so this is preferable. In addition, in this low-temperature stretching step, it is preferable to stretch in multiple stages up to the desired stretching ratio from the viewpoint of mitigating sudden deformation and reducing breakage.

[0091] [Process (c)] In step (c), the molded product stretched in step (b) is stretched at a temperature higher than the stretching temperature in step (b) (hereinafter, this step (c) may be referred to as a "high-temperature stretching step"). As for the stretching method in step (c), the same method as in step (b) described above may be adopted, among which, a roll stretching method or a tenter stretching method is preferred, and in particular, from the viewpoint of expanding the holes formed in step (b), it is also preferred to stretch (transverse stretching) in a direction perpendicular to the longitudinal direction (hereinafter, sometimes referred to as the "transverse direction" or "TD") by a tenter stretching method or the like. The temperature in the high-temperature stretching step is preferably higher than the stretching temperature in step (b) and within ±15°C of the glass transition temperature (Tg) of the resin composition, or is preferably higher than the stretching temperature in step (b) and in the range of 160°C to 260°C. Here, the pores formed in step (b) can be stretched and the pore diameter can be enlarged by stretching at a temperature that is −15° C. or higher than the glass transition temperature (Tg) of the resin composition or at a temperature that is 160° C. or higher. On the other hand, the pores formed in step (b) can be prevented from being blocked by stretching at a temperature that is +15° C. or lower than the glass transition temperature (Tg) of the resin composition or at a temperature that is 260° C. or lower.

[0092] The stretching ratio in the high-temperature stretching step is not particularly limited, but is preferably 1.25 to 6.00 times, particularly 1.40 to 5.00 times. When the stretching ratio is equal to or higher than the lower limit, the pore size can be easily enlarged and the porous structure can be easily maintained, whereas when the stretching ratio is equal to or lower than the upper limit, the blocking of the pores can be suppressed, which is preferable.

[0093] In the method for producing the porous body, it is important to carry out each step in the order of step (a), step (b). Furthermore, when step (c) is included, it is preferable to carry out each step in the order of step (a), step (b), and step (c). However, other steps may be included between each of steps (a), (b), and (c). Furthermore, a step other than step (c) may be included after step (b). Furthermore, even when step (c) is included, another step may be included after step (c).

[0094] In particular, after step (b) or step (c), it is preferable to carry out a heat treatment or a relaxation treatment from the viewpoint of improving dimensional stability. In addition, from the viewpoint of further improving dimensional stability, the obtained porous body may be crosslinked by electron beam crosslinking or the like, and the obtained porous body may be surface-treated by corona discharge treatment, plasma treatment or the like from the viewpoint of improving adhesion when laminated with other porous layers as described later.

[0095] In addition, when the porous body has a layer other than the layer made of the resin composition, the layer made of the resin composition and the layer of the composition constituting the other layer may be laminated by a co-extrusion method or a lamination method in the step (a) to prepare a substantially non-porous laminate, and then stretched in the step (b) to make the porous body porous, or the layer made of the resin composition may be made porous through the steps (a) and (b) and then laminated with another layer by a lamination method or a coating method to produce the porous body. In particular, it is preferable to laminate the porous body with copper foil.

[0096] <Electronic components made using the porous body> The stretched porous body of the present invention is preferably used for electronic parts. Examples of electronic parts for which the porous body can be preferably used include batteries such as alkaline batteries, nickel metal hydride batteries, lithium batteries, and lithium ion secondary batteries, capacitors such as electrolytic capacitors, electric double layer capacitors, and lithium ion capacitors, electronic parts for mobile devices, circuit boards such as flexible printed circuit boards, and laminates for circuits, and electronic parts such as the circuit boards and laminates for circuits are particularly preferred. The electronic member of the present invention is not particularly limited in terms of other constituent members, so long as the porous body is used as a separator for electronic members or a low dielectric constant member for circuits. EXAMPLES

[0097] Next, the present porous body will be described in more detail with examples and comparative examples, but the present invention is not limited thereto. Note that, as an embodiment of the present porous body, a sheet-like material is taken as an example, and the present porous body will be referred to as a stretched porous film hereinafter. In addition, the take-up (flow) direction of the stretched porous film is referred to as the "MD" direction, the perpendicular direction thereto as the "TD" direction, and the thickness direction as the "THD" direction.

[0098] [Evaluation method] (1) Thickness The stretched porous films obtained in the Examples and Comparative Examples (hereinafter simply referred to as "stretched porous films") were measured at five random locations in the plane with a 1 / 1000 mm dial gauge, and the average of the measurements was calculated as the thickness. In this evaluation method, the stretched porous film also includes the unstretched film obtained in the Comparative Examples.

[0099] (2) Air permeability The air permeability (sec / 100 mL) of the stretched porous film was measured using an air permeability measuring device (Oken type air permeability measuring device EGO1-55 model manufactured by Asahi Seiko Co., Ltd.) in accordance with JIS P8117 (2009). The measurement was performed at five random points within the plane of the stretched porous film, and the average of the measurements was calculated as the air permeability.

[0100] (3) Porosity The stretched porous film was cut into a piece having a size of 50 mm in the machine direction (MD) and 50 mm in the transverse direction (TD), and the specific gravity (W1) of the stretched porous film was measured. In measuring the specific gravity (W0) of the resin composition forming the stretched porous body of the present invention, the unstretched film obtained in Comparative Example 1 described below was cut into a size of 50 mm in the machine direction (MD) and 50 mm in the transverse direction (TD), and the specific gravity (W0) of the unstretched film was measured. The porosity was calculated from the specific gravity (W1) of the stretched porous film and the specific gravity (W0) of the resin composition according to the following formula. Porosity (%)=[1-(W1 / W0)]×100 The measurement was carried out at three random locations within the plane of the stretched porous film (including the unstretched film obtained in the Comparative Example), and the average was calculated as the porosity.

[0101] (4) Tensile breaking stress The stretched porous film was cut into a size of 120 mm in MD and 15 mm in TD, and a tensile test was performed on the stretched porous film in accordance with JIS K7127, with a chuck distance of 40 mm, a tensile speed of 200 mm / min, and a measurement direction MD at an atmospheric temperature of 23°C. The average value of the tensile breaking stress of three measurements was calculated as the tensile breaking stress in MD. In addition, the stretched porous film was cut into a size of 15 mm in MD and 120 mm in TD, and a tensile test was performed on the stretched porous film in accordance with JIS K7127, with a chuck distance of 40 mm, a tensile speed of 200 mm / min, and a measurement direction TD at an atmospheric temperature of 23°C, and the average value of the tensile breaking stress of three measurements was calculated as the tensile breaking stress in TD.

[0102] (5) Linear expansion coefficient The linear expansion coefficient in MD and TD of the stretched porous film was measured using Hitachi High-Tech Science TMA / SS7100. The measurement was performed using a tensile probe to confirm the dimensional changes in MD and TD when the temperature was raised from -10°C to 300°C at 5°C / min. Then, from the obtained dimensional change profile, the dimensional change amount ΔL (mm) from 0°C to 100°C and the strain (=ΔL / L) calculated from the initial dimension L (mm) were divided by the temperature change amount (ΔT=100°C) to calculate the linear expansion coefficient from 0°C to 100°C.

[0103] (6) High-frequency dielectric constant measurement In accordance with JIS R1641 (2007), the dielectric constant and dielectric loss tangent of the stretched porous film were measured at a measurement frequency of 10 GHz using a cavity resonator (TE mode) manufactured by AET Co., Ltd. at a room temperature of 26°C and a humidity of 40%. The average values ​​of three measurements were calculated as the dielectric constant and dielectric loss tangent at a measurement frequency of 10 GHz. Similarly, the dielectric constant and dielectric loss tangent of the stretched porous film at a measurement frequency of 28 GHz were calculated using a cavity resonator (TE mode) manufactured by AET Co., Ltd. at a room temperature of 26°C and a humidity of 40% in accordance with JIS R1641 (2007). The average values ​​of three measurements were calculated as the dielectric constant and dielectric loss tangent at a measurement frequency of 28 GHz.

[0104] (7) Scanning electron microscope (SEM) observation The film surface, MD cross section, and TD cross section of the stretched porous film obtained in Example 1 were observed with a scanning electron microscope. In addition, the film surface, MD cross section, and TD cross section of the stretched porous film obtained in Example 2 were observed with a scanning electron microscope.

[0105] The raw materials used in the examples and comparative examples are as follows.

[0106] (Resin composition (X)) A resin composition consisting of 75 to 95 mass% poly(2,6-dimethyl-1,4-phenylene) ether, 1 to 10 mass% acrylic thermoplastic elastomer, 1 to 10 mass% phosphorus-based flame retardant, 0.1 to 1 mass% carbon black, and 0.1 to 1 mass% zinc oxide, having a weight average molecular weight Mw1 = 68,200, a number average molecular weight Mn1 = 27,600, Mw1 / Mn1 = 2.47, Mw2 = 708, Mn2 = 678, Mw2 / Mn2 = 1.04, Mw3 = 365, Mn3 = 354, Mw3 / Mn3 = 1.03 (having three peaks in GPC measurement), a reduced viscosity of 0.49 dL / g, and a glass transition temperature Tg = 174°C, hereinafter referred to as resin composition (X).

[0107] [Example 1] The resin composition (X) was put into a single-screw extruder, melt-kneaded at a set temperature of 280 ° C, and shaped into a sheet using a T-die. The sheet was cooled and solidified using a cast roll set at 140 ° C to obtain an unstretched sheet-like material having a thickness of 200 μm. The unstretched sheet-like material obtained under the above conditions was stretched between a roll (P) set at 120 ° C and a roll (Q) set at 120 ° C at a draw ratio of 15% (stretch ratio 1.15 times), then between the roll (Q) and a roll (R) set at 120 ° C at a draw ratio of 15% (stretch ratio 1.15 times), and between the roll (R) and a roll (S) set at 120 ° C at a draw ratio of 15% (stretch ratio 1.15 times), and a three-stage low-temperature stretching (total stretch ratio 1.52 times) was performed to obtain an MD-stretched porous film. The evaluation results of the obtained stretched porous film are summarized in Table 1. SEM photographs of the film surface, MD cross section, and TD cross section of the obtained stretched porous film are shown in Figure 1. An enlarged photograph of the observation surface shown in Figure 1 is shown in Figure 2.

[0108] [Example 2] The resin composition (X) was put into a single-screw extruder, melt-kneaded at a set temperature of 280 ° C., and shaped into a sheet shape with a T-die, then cooled and solidified with a cast roll set at 140 ° C. to obtain an unstretched sheet-like material with a thickness of 200 μm. The unstretched sheet-like material obtained under the above conditions was stretched between a roll (P) set at 120 ° C. and a roll (Q) set at 120 ° C. at a draw ratio of 15% (stretch ratio 1.15 times), then between the roll (Q) and a roll (R) set at 120 ° C. at a draw ratio of 15% (stretch ratio 1.15 times), and between the roll (R) and a roll (S) set at 120 ° C. at a draw ratio of 15% (stretch ratio 1.15 times), and a three-stage low-temperature stretching (total stretch ratio 1.52 times) was performed to obtain an MD-stretched porous film. Thereafter, the film was preheated at 170°C in a film tenter facility manufactured by Kyoto Machinery Co., Ltd., and then hot-stretched in the transverse direction by 2.00 times at a stretching temperature of 170°C, followed by heat treatment at 170°C to obtain a biaxially stretched porous film. The evaluation results of the obtained stretched porous film are summarized in Table 1. SEM photographs of the film surface, MD cross section, and TD cross section of the obtained stretched porous film are shown in Figure 3. An enlarged photograph of the observation surface shown in Figure 3 is shown in Figure 4.

[0109] [Example 3] The resin composition (X) was put into a single screw extruder, melt-kneaded at a set temperature of 280°C, and shaped into a sheet using a T-die. The resin composition was then cooled and solidified using a cast roll set at 140°C to obtain an unstretched sheet having a thickness of 100 μm. Except for this, low-temperature stretching and high-temperature stretching were performed under the same conditions as in Example 2 to obtain a biaxially stretched porous film. The evaluation results of the obtained stretched porous film are summarized in Table 1.

[0110] [Comparative Example 1] Resin composition (X) was fed into a single screw extruder, melt-kneaded at a set temperature of 280° C., and shaped into a sheet using a T-die, and then cooled and solidified using a cast roll set at 140° C. to obtain an unstretched sheet having a thickness of 175 μm. The evaluation results of the obtained unstretched sheet are summarized in Table 1.

[0111] [Comparative Example 2] Resin composition (X) was put into a single screw extruder, melt-kneaded at a set temperature of 280°C, and shaped into a sheet using a T-die, and then cooled and solidified using a cast roll set at 140°C to obtain an unstretched sheet-like product with a thickness of 175 μm. The film was then passed through a Kyoto Machinery Co., Ltd. film tenter facility set at a preheating temperature of 170°C, a stretching temperature of 170°C, and a heat treatment temperature of 170°C, and high-temperature stretching was attempted in the transverse direction at 2.00 times in a stretching zone set at 170°C, but breakage occurred in the stretching zone, and a film could not be obtained.

[0112] [Table 1]

[0113] From Table 1, it can be seen that the stretched porous bodies obtained in Examples 1 to 3 have excellent air permeability and high porosity. In addition, the linear expansion coefficient in the machine direction (MD) from 0°C to 100°C is 70 ppm / °C or less, and it was confirmed that the body has excellent dimensional stability when used in a high-temperature atmosphere. Furthermore, by stretching to make the body porous, a decrease in the relative dielectric constant and dielectric loss tangent was observed at both measurement frequencies of 10 GHz and 28 GHz, and it was found that the body is an excellent stretched porous body with low transmission loss.

[0114] On the other hand, the unstretched sheet obtained in Comparative Example 1 has an air permeability of 99999 sec / 100 mL or more, which exceeds the measurement limit of the measuring device, and has no substantial air permeability, so it is not suitable for applications requiring air permeability or pore interconnectivity in the thickness direction. In addition, the linear expansion coefficient exceeds 70 ppm in both MD and TD, resulting in poor dimensional stability when used in a high temperature atmosphere. In addition, the relative dielectric constant exceeds 2.5 at both measurement frequencies of 10 GHz and 28 GHz, and the dielectric loss tangent also exceeds 0.0060, which indicates that it is insufficient for use as a low dielectric constant member.

[0115] Also, from the scanning electron microscope photographs (FIGS. 1 to 4) of the stretched porous films obtained in Examples 1 and 2, it is confirmed that the porous body of the present invention has a porous structure in which the entire resin composition is made porous starting from the crazes generated during low-temperature stretching, and the propagation of the crazes is suppressed internally. It is also confirmed that the porous structure formed by low-temperature stretching is expanded laterally without being blocked even during stretching, resulting in improved porosity and air permeability. On the other hand, Comparative Example 2 is different from the production method defined by the present invention. Specifically, it is understood that a stretched porous body is not obtained because step (b) is not carried out after step (a). That is, compared with conventional production methods for making amorphous resins, such as polyphenylene ether resins, porous, which have had problems in productivity, such as foaming methods, wet methods, and fiber deposition, the stretched porous body of the present invention has an excellent porous structure, and the production method of the present invention can be produced by a highly productive dry method, and is therefore an excellent production method for forming stretched porous bodies from amorphous resins, such as polyphenylene ether resins. [Industrial Applicability]

[0116] The stretched porous body of the present invention can be used in various applications requiring porous properties.Specifically, it can be used for packaging, sanitation, livestock, agriculture, construction, medical use, separation membranes, water treatment membranes, light diffusion plates, heat insulation materials, buffer materials, foam materials, separators, and low dielectric constant members, and is particularly suitable and useful for low dielectric constant members used in electronic members such as circuit boards, typified by flexible printed circuit boards, and circuit laminates, and electronic members made of the low dielectric constant members.

Claims

1. A stretched porous body having at least one porous layer made of a resin composition containing 50% by mass or more of an amorphous resin (A) and a thermoplastic elastomer (B).

2. 2. The stretched porous body according to claim 1, wherein the amorphous resin (A) is at least one selected from the group consisting of polyphenylene ether-based resins, polycarbonate-based resins, thermoplastic polyimide-based resins, polyamideimide-based resins, polyarylate-based resins, polyetherimide-based resins, polyethersulfone-based resins, and polysulfone-based resins.

3. The stretched porous body according to claim 2 , wherein the amorphous resin (A) is a polyphenylene ether resin.

4. The stretched porous body according to any one of claims 1 to 3, wherein the stretched porous body has a porosity of 15% or more and 80% or less.

5. The stretched porous body according to any one of claims 1 to 4, which has a linear expansion coefficient of 70 ppm / °C or less from 0°C to 100°C in at least one direction.

6. The stretched porous body according to any one of claims 1 to 5, having a relative dielectric constant of 2.5 or less at a measurement frequency of 10 GHz.

7. The stretched porous body according to any one of claims 1 to 6, having a dielectric loss tangent of 0.0060 or less at a measurement frequency of 10 GHz.

8. The stretched porous body according to any one of claims 1 to 7, having a relative dielectric constant of 2.5 or less at a measurement frequency of 28 GHz.

9. The stretched porous body according to any one of claims 1 to 8, having a dielectric loss tangent of 0.0060 or less at a measurement frequency of 28 GHz.

10. The stretched porous body according to any one of claims 1 to 9, wherein the thermoplastic elastomer (B) is contained in the resin composition in an amount of 0.1% by mass or more and 50% by mass or less.

11. An electronic component comprising the stretched porous body according to any one of claims 1 to 10.

12. A step (a) of melt-extruding a resin composition containing 50% by mass or more of an amorphous resin (A) and a thermoplastic elastomer (B), and cooling and solidifying the extrusion, to form a molded article having at least one layer made of the resin composition; and (b) stretching the molded body molded in the step (a) at a temperature 10° C. or more lower than the glass transition temperature (Tg) of the resin composition, in this order.

13. The method for producing a stretched porous body according to claim 12, wherein the amorphous resin (A) is at least one selected from the group consisting of polyphenylene ether resins, polycarbonate resins, thermoplastic polyimide resins, polyamideimide resins, polyarylate resins, polyetherimide resins, polyethersulfone resins, and polysulfone resins.

14. The method for producing a stretched porous body according to claim 13, wherein the amorphous resin (A) is a polyphenylene ether resin.

15. The method for producing a stretched porous body according to any one of claims 12 to 14, wherein the shaped body is any one selected from the group consisting of a sheet-like body, a fibrous body, and a hollow body.

16. The method for producing a stretched porous body according to any one of claims 12 to 15, wherein the thermoplastic elastomer (B) is contained in the resin composition in an amount of 0.1 mass % or more and 50 mass % or less.

17. The method for producing a stretched porous body according to any one of claims 12 to 16, wherein in the step (b), the stretching temperature is 60°C or higher and 160°C or lower.

18. The method for producing a stretched porous body according to any one of claims 12 to 17, further comprising, after the step (b), a step (c) of stretching at a temperature higher than the stretching temperature in the step (b).

19. The method for producing a stretched porous body according to claim 18, wherein the stretching temperature in the step (c) is higher than the stretching temperature in the step (b) and is within ±15°C of the glass transition temperature (Tg) of the resin composition.

20. The method for producing a stretched porous body according to claim 18 or 19, wherein the stretching temperature in the step (c) is higher than the temperature in the step (b) and is 160°C or higher and 260°C or lower.

Citation Information

Patent Citations

  • Porous membrane and manufacture of the same

    JP1995232044A

  • Separator and its manufacture

    JP2000138048A

  • Insulating material for high frequency wiring board and high frequency wiring board

    JP2004082372A

  • Foam sheet for interior material of automobile

    JP2005088873A

  • Composite porous membrane, manufacturing method thereof, and battery separator using the same, battery, and capacitor

    JP2007125821A