film

The biodegradable polyester film, made from an aliphatic polyester resin, polyhydroxyalkanoate, and inorganic filler, achieves enhanced biodegradability and mechanical properties, overcoming the limitations of existing biodegradable resins in environmental and marine conditions.

JP7552198B2Active Publication Date: 2024-09-18MITSUBISHI CHEM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020161041
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-25
Publication Date
2024-09-18
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing biodegradable resins have low biodegradability at room temperature and in marine environments, failing to meet the demand for complete biodegradation and mechanical properties required for films used in agricultural and packaging materials.

Method used

A biodegradable polyester film composed of an aliphatic polyester resin, polyhydroxyalkanoate, and an inorganic filler, with specific mass ratios and properties to enhance biodegradability and mechanical strength, transparency, and moldability.

Benefits of technology

The film exhibits high biodegradability at room temperature and in marine environments, with excellent mechanical properties, transparency, and moldability, addressing the limitations of conventional biodegradable resins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552198000002
    Figure 0007552198000002
  • Figure 0007552198000001
    Figure 0007552198000001
Patent Text Reader

Abstract

To provide a biodegradable polyester film that has high biodegradability at room temperature, is excellent also in marine degradability, is excellent also in moldability when obtaining films, and has excellent balance in characteristics such as mechanical properties such as rigidity or tensile strength, transparency and port opening property.SOLUTION: A film is made of an aliphatic polyester resin composition that comprises: an aliphatic polyester resin (A) containing a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid as a main constituent unit, polyhydroxyalkanoate (B) and an inorganic filler (C), in which the polyhydroxyalkanoate (B) contains 3-hydroxybutyrate unit and 3-hydroxyhexanoate unit as main constituent, a mass ratio of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B) is 95 / 5 to 70 / 30, a content ratio of the inorganic filler (C) to a total 100 pts.mass of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B) is 0.1 to 15 pts.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film made of an aliphatic polyester resin composition. [Background technology]

[0002] In recent years, there has been active development of biodegradable plastics as a solution to problems caused by plastic waste, such as its impact on the ecosystem, the generation of harmful gases during combustion, and global warming due to the large amount of heat generated by combustion, which places a heavy burden on the global environment. In particular, the carbon dioxide emitted when biodegradable plastics derived from plants are burned is carbon that was originally in the air, and does not increase the amount of carbon dioxide in the atmosphere. This is called carbon neutrality, and is considered important under the Kyoto Protocol, which imposed carbon dioxide reduction targets, and active use of biodegradable plastics is desired.

[0003] Recently, from the standpoint of biodegradability and carbon neutrality, aliphatic polyester resins have been attracting attention as plant-derived plastics, and in particular polyhydroxyalkanoate (hereinafter sometimes referred to as PHA) resins, and among PHA resins, poly(3-hydroxybutyrate) homopolymer resin (hereinafter sometimes referred to as PHB), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) copolymer resin (hereinafter sometimes referred to as PHBV), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin (hereinafter sometimes referred to as PHBH), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) copolymer resin, polylactic acid, etc. have been attracting attention.

[0004] For example, Patent Document 1 discloses a molded article made of an aliphatic polyester resin composition containing a compound having an amide bond in a polyhydroxyalkanoate and pentaerythritol, and describes that the moldability in molding processes such as injection molding and sheet processing is improved.

[0005] Meanwhile, in recent years, the use of biodegradable resins in films for agricultural materials, packaging materials, and the like has also been considered. For example, Patent Document 2 discloses a method for stably producing a biodegradable polyester film containing polyhydroxyalkanoate under practical processing conditions by inflation molding by mixing a master batch containing polyhydroxyalkanoate and fatty acid amide with an aliphatic aromatic polyester. Patent Document 3 discloses a resin composition containing a poly(3-hydroxybutyrate) copolymer and polybutylene succinate, and a film using the same. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2014 / 068943 [Patent Document 2] International Publication No. 2018 / 181500 [Patent Document 3] International Publication No. 2017 / 087658 Summary of the Invention [Problem to be solved by the invention]

[0007] In recent years, due to the strong social trend towards environmental protection, especially environmental pollution caused by the disposal of used plastic products (especially the impact of microplastics caused by the disposal of used plastic products in the ocean), resins that are completely biodegradable, rather than only partially biodegradable, are required. In addition, in terms of the biodegradation environment, not only is biodegradability required in an aerobic compost environment (in soil) at relatively high temperatures (58°C or higher), but also in an aerobic compost environment (in soil) at room temperature (28°C) and in the ocean. If a product shows not only room temperature biodegradability but also ocean biodegradability (marine biodegradability), for example, a film made of biodegradable resin can be treated as a home compost after use, and furthermore, it can be biodegraded in the ocean, eliminating the adverse effects of microplastics on marine life.

[0008] The above Patent Documents 2 and 3 disclose the use of a composition combining polyhydroxyalkanoate with an aliphatic aromatic polyester or polybutylene succinate as a film material. However, the biodegradable resins proposed therein have low biodegradability at room temperature and in the sea, and do not satisfy the rapidly increasing demand for reducing environmental impact today. Furthermore, in the case of agricultural materials (mulch films) and packaging materials such as plastic shopping bags, not only biodegradation rate but also properties such as mechanical strength, transparency, and ease of opening during inflation molding are required, but conventionally proposed film compositions have been insufficient to satisfy these required properties.

[0009] The present invention has been made in view of the above background, and aims to provide a biodegradable polyester film which, compared to films using conventional biodegradable resins, has a higher degree of biodegradability at room temperature, is also excellent in marine biodegradability, and is also excellent in formability when obtaining a film, while also having a well-balanced combination of mechanical properties such as rigidity and tensile strength, and properties such as transparency and opening ability. [Means for solving the problem]

[0010] As a result of intensive research into solving the above-mentioned problems, the inventors have found that the above-mentioned problems can be solved by a biodegradable polyester film obtained by molding an aliphatic polyester resin composition containing an aliphatic polyester resin (A) containing, as main structural units, a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid, a polyhydroxyalkanoate (B), and further an inorganic filler (C) in a predetermined ratio, and have thus arrived at the present invention. That is, the gist of the present invention resides in the following [1] to

[10] .

[0011] [1] A film using an aliphatic polyester resin composition comprising an aliphatic polyester resin (A) containing, as main structural units, a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid, a polyhydroxyalkanoate (B), and an inorganic filler (C), wherein the polyhydroxyalkanoate (B) is a copolymer containing, as main structural units, 3-hydroxybutyrate units and 3-hydroxyhexanoate units, the mass ratio of the aliphatic polyester resin (A) to the polyhydroxyalkanoate (B) is 95 / 5 to 70 / 30, and the content of the inorganic filler (C) per 100 parts by mass of the total amount of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B) is 0.1 to 15 parts by mass.

[0012] [2] The film according to [1], wherein the repeating units derived from the aliphatic dicarboxylic acid contained in the aliphatic polyester resin (A) contain succinic acid units and adipic acid units.

[0013] [3] The film according to [1] or [2], wherein the amount of adipic acid units contained in the repeating units derived from the aliphatic dicarboxylic acid contained in the aliphatic polyester resin (A) is 18 mol % or more and 32 mol % or less.

[0014] [4] The film according to any one of [1] to [3], wherein the inorganic filler (C) is one or more selected from the group consisting of anhydrous silica, calcium carbonate, talc, silicates, and zeolites.

[0015] [5] The film according to any one of [1] to [4], wherein the inorganic filler (C) has an average particle size of 30 μm or less.

[0016] [6] The film according to any one of [1] to [5], having a tensile breaking strength of 25 MPa or more.

[0017] [7] The film according to any one of [1] to [6], having a haze of 40 or less.

[0018] [8] The film according to any one of [1] to [7], which is formed by an inflation method.

[0019] [9] The film according to any one of [1] to [7], which is formed by a T-die method.

[0020]

[10] An inflation film, which has a peel strength of 12 N or less in the MD direction between inner surfaces of the inflation film based on ASTM D1893-67 (1985), and is characterized in that it is made of an aliphatic polyester resin composition containing: (A) an aliphatic polyester resin containing, as main structural units, a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid; (B) a polyhydroxyalkanoate which is a copolymer containing, as main structural units, 3-hydroxybutyrate units and 3-hydroxyhexanoate units; and (C) an inorganic filler. Effect of the Invention

[0021] According to the present invention, there is provided a biodegradable polyester film that has excellent formability, a high degree of biodegradability at room temperature, excellent marine biodegradability, and a well-balanced combination of mechanical properties such as rigidity and tensile strength, and properties such as transparency and opening property. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The following describes in detail the embodiments of the present invention; however, the present invention is not limited to the following description, and can be modified in any manner without departing from the gist of the present invention. In this specification, when "~" is used to express a numerical value or a physical property value, the values ​​before and after the "~" are included. In this specification, "mass %" and "parts by mass" have the same meaning as "weight %" and "parts by weight", respectively. The MD direction of the film refers to the extrusion direction (or take-up direction or flow direction) during film formation and is also called the longitudinal direction, and the TD direction refers to the direction perpendicular to the MD direction and is also called the transverse direction or width direction.

[0023] The film of the present invention uses an aliphatic polyester resin composition (hereinafter sometimes referred to as "the aliphatic polyester resin composition of the present invention") that contains an aliphatic polyester resin (A) containing, as main structural units, a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid, a polyhydroxyalkanoate (B), and an inorganic filler (C), wherein the polyhydroxyalkanoate (B) is a copolymer containing, as main structural units, 3-hydroxybutyrate units and 3-hydroxyhexanoate units, the mass ratio of the aliphatic polyester resin (A) to the polyhydroxyalkanoate (B) is 95 / 5 to 70 / 30, and the content of the inorganic filler (C) per 100 parts by mass of the total amount of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B) is 0.1 to 15 parts by mass.

[0024] The inflation film of the present invention is characterized in that the peel strength in the MD direction between the inner faces of the inflation film is 12 N or less based on ASTM D1893-67 (1985), and is made of an aliphatic polyester resin composition containing an aliphatic polyester resin (A) containing, as main structural units, a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid, a polyhydroxyalkanoate (B) which is a copolymer containing, as main structural units, 3-hydroxybutyrate units and 3-hydroxyhexanoate units, and an inorganic filler (C), preferably the aliphatic polyester resin composition of the present invention.

[0025] In the present invention, an aliphatic diol refers to an aliphatic hydrocarbon group to which two hydroxyl groups are bonded. As the aliphatic hydrocarbon group, a straight-chain aliphatic hydrocarbon group is usually used, but it may have a branched structure or a cyclic structure, or may have a plurality of these structures. Furthermore, an aliphatic dicarboxylic acid refers to an aliphatic hydrocarbon group to which two carboxyl groups are bonded. As the aliphatic hydrocarbon group, a straight-chain aliphatic hydrocarbon group is usually used, but it may have a branched structure or a cyclic structure, or may have multiple of these.

[0026] The aliphatic polyester resin (A) contained in the aliphatic polyester resin composition of the present invention is a polymer having repeating units, and each repeating unit is also called a compound unit corresponding to the compound from which the repeating unit is derived. For example, a repeating unit derived from an aliphatic diol is also called an "aliphatic diol unit", and a repeating unit derived from an aliphatic dicarboxylic acid is also called an "aliphatic dicarboxylic acid unit". The "main structural unit" in the aliphatic polyester resin (A) generally refers to a structural unit that is contained in the aliphatic polyester resin (A) at 80% by mass or more, and may not contain any structural units other than the main structural unit. The same applies to the "main structural unit" in the polyhydroxyalkanoate (B).

[0027] [mechanism] The aliphatic polyester resin (A) and polyhydroxyalkanoate (B) contained in the aliphatic polyester resin composition of the present invention have high biodegradability at room temperature and in the sea, so that the film of the present invention made of the aliphatic polyester resin composition of the present invention containing the aliphatic polyester resin (A) and polyhydroxyalkanoate (B) as resin components has excellent biodegradability at room temperature and in the sea. In addition, the rigidity can be improved by using the aliphatic polyester resin (A) and polyhydroxyalkanoate (B) in a predetermined ratio. The aliphatic polyester resin composition of the present invention contains an inorganic filler (C) in a predetermined ratio in addition to the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B), and can impart opening properties and appropriate rigidity during inflation molding, thereby making it possible to obtain an aliphatic polyester resin composition with excellent moldability. Furthermore, the addition of inorganic filler (C) increases the surface area of ​​the molded article, and when decomposition is accelerated, the inorganic filler falls off, increasing the contact area with the decomposition enzymes produced by microorganisms, thereby accelerating the biodegradation rate of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B). In addition, the inorganic filler (C) also works as a nucleating agent, which effectively improves moldability, so that by including inorganic filler (C) in a specified ratio, it becomes possible to provide a film with even better room temperature and marine biodegradability with good moldability and productivity.

[0028] [Aliphatic polyester resin composition] The aliphatic polyester resin composition of the present invention containing the aliphatic polyester resin (A), the polyhydroxyalkanoate (B), and the inorganic filler (C) will be described below.

[0029] <Aliphatic polyester resin (A)> The aliphatic polyester resin (A) used in the present invention (hereinafter sometimes referred to as "polyester resin (A)") is an aliphatic polyester resin containing aliphatic diol units and aliphatic dicarboxylic acid units as main constituent units.

[0030] The polyester resin (A) used in the present invention preferably contains succinic acid units and adipic acid units in all dicarboxylic acid units. In this case, the polyester resin (A) preferably contains succinic acid units in an amount of 5 mol% to 90 mol% in all dicarboxylic acid units, and adipic acid units in an amount of 10 mol% to 95 mol% in all dicarboxylic acid units. The polyester resin (A) may be a mixture of aliphatic polyester resins having different amounts of succinic acid units and adipic acid units. That is, it may be a mixture of an aliphatic polyester resin containing succinic acid units and adipic acid units and an aliphatic polyester resin not containing succinic acid units and adipic acid units, or it is possible to blend an aliphatic polyester resin containing only one of succinic acid units and adipic acid units and use the resulting mixture by adjusting the amounts of succinic acid units and adipic acid units in the polyester resin (A) to fall within the above-mentioned preferred ranges. When the polyester resin (A) is a copolymer polyester resin containing succinic acid units and adipic acid units, the degree of crystallization of the polyester resin (A) is reduced, and biodegradability can be further increased, which is preferable.

[0031] More specifically, the polyester resin (A) is a polyester resin containing an aliphatic diol unit represented by the following formula (1) and an aliphatic dicarboxylic acid unit represented by the following formula (2). -OR 1 -O- (1) -OC-R 2 -CO- (2)

[0032] In formula (1), R 1 represents a divalent aliphatic hydrocarbon group. 2represents a divalent aliphatic hydrocarbon group. The aliphatic diol unit and the aliphatic dicarboxylic acid unit represented by the above formula (1) and (2) may be derived from a compound derived from petroleum or a compound derived from a plant raw material, but are preferably derived from a compound derived from a plant raw material.

[0033] When the polyester-based resin (A) is a copolymer, the polyester-based resin (A) may contain two or more types of aliphatic diol units represented by formula (1), and the polyester-based resin (A) may contain two or more types of aliphatic dicarboxylic acid units represented by formula (2).

[0034] As described above, the aliphatic dicarboxylic acid unit represented by formula (2) contains succinic acid units and adipic acid units, and preferably contains 5 mol% to 90 mol% of succinic acid units and 10 mol% to 95 mol% of adipic acid units relative to the total dicarboxylic acid units. When the polyester resin (A) contains succinic acid units and adipic acid units and the succinic acid unit and adipic acid unit contents are within the above-mentioned predetermined ranges, it is possible to obtain an aliphatic polyester resin composition having improved moldability and excellent heat resistance and biodegradability. For the same reason, the amount of succinic acid units in the polyester resin (A) is more preferably 10 mol% or more, even more preferably 50 mol% or more, particularly preferably 64 mol% or more, especially preferably 68 mol% or more, more preferably 88 mol% or less, even more preferably 86 mol% or less, especially preferably 84 mol% or less, especially preferably 82 mol% or less relative to the total dicarboxylic acid units. On the other hand, the amount of adipic acid units in the polyester resin (A) is more preferably 12 mol% or more, even more preferably 14 mol% or more, particularly preferably 16 mol% or more, and especially preferably 18 mol% or more, based on the total dicarboxylic acid units, and is more preferably 90 mol% or less, even more preferably 50 mol% or less, particularly preferably 36 mol% or less, and especially preferably 32 mol% or less.

[0035] The aliphatic dicarboxylic acid unit represented by formula (2) may contain an aliphatic dicarboxylic acid unit other than a succinic acid unit and an adipic acid unit. The aliphatic dicarboxylic acid units other than the succinic acid unit and the adipic acid unit are not particularly limited, but are preferably aliphatic dicarboxylic acid units having 2 to 40 carbon atoms, particularly preferably 4 to 10 carbon atoms, and examples thereof include one or more of a suberic acid unit, a sebacic acid unit, a dodecanedioic acid unit, a dimer acid unit, etc. Among these, a sebacic acid unit is preferred. When the polyester resin (A) contains aliphatic dicarboxylic acid units other than succinic acid units and adipic acid units, the content thereof is preferably 45 mol % or less, particularly preferably 40 mol % or less, of the total dicarboxylic acid units.

[0036] The aliphatic dicarboxylic acid component that gives the aliphatic dicarboxylic acid unit represented by formula (2) is not particularly limited, and may be one or more of the above-mentioned succinic acid unit, adipic acid unit, aliphatic dicarboxylic acids other than the succinic acid unit and the adipic acid unit, and derivatives thereof such as alkyl esters.

[0037] The aliphatic diol that gives the diol unit represented by formula (1) is not particularly limited, but from the viewpoint of moldability and mechanical strength, an aliphatic diol having 2 to 10 carbon atoms is preferred, and an aliphatic diol having 4 to 6 carbon atoms is particularly preferred. For example, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, etc. are included, and among them, 1,4-butanediol is particularly preferred. Note that two or more kinds of the above aliphatic diols can be used.

[0038] The polyester resin (A) may have a repeating unit (aliphatic oxycarboxylic acid unit) derived from an aliphatic oxycarboxylic acid. Specific examples of the aliphatic oxycarboxylic acid component that gives the aliphatic oxycarboxylic acid unit include, for example, lactic acid, glycolic acid, 2-hydroxy-n-butyric acid, 2-hydroxycaproic acid, 6-hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, and the like, or derivatives thereof such as lower alkyl esters or intramolecular esters. When optical isomers exist in these, they may be any of D-form, L-form, or racemic form, and may be in the form of a solid, liquid, or aqueous solution. Among these, lactic acid or glycolic acid or derivatives thereof are particularly preferred. These aliphatic oxycarboxylic acids may be used alone or as a mixture of two or more.

[0039] When the polyester resin (A) contains these aliphatic oxycarboxylic acid units, from the viewpoint of moldability, the content thereof is preferably 20 mol % or less, more preferably 10 mol % or less, even more preferably 5 mol % or less, and most preferably 0 mol % (not included), based on 100 mol % of all constituent units constituting the polyester resin (A).

[0040] The polyester resin (A) may have an increased melt viscosity by copolymerizing a trifunctional or higher aliphatic polyhydric alcohol, a trifunctional or higher aliphatic polycarboxylic acid or its acid anhydride, or a trifunctional or higher aliphatic polyoxycarboxylic acid component.

[0041] Specific examples of trifunctional aliphatic polyhydric alcohols include trimethylolpropane, glycerin, etc., and specific examples of tetrafunctional aliphatic polyhydric alcohols include pentaerythritol, etc. These may be used alone or in combination of two or more. A specific example of a trifunctional aliphatic polycarboxylic acid or its anhydride is propanetricarboxylic acid or its anhydride, and a specific example of a tetrafunctional polycarboxylic acid or its anhydride is cyclopentanetetracarboxylic acid or its anhydride, etc. These may be used alone or in combination of two or more.

[0042] In addition, trifunctional aliphatic oxycarboxylic acids are divided into (i) a type having two carboxyl groups and one hydroxyl group in the same molecule, and (ii) a type having one carboxyl group and two hydroxyl groups. Either type can be used, but from the viewpoint of moldability, mechanical strength, and appearance of molded products, (i) a type having two carboxyl groups and one hydroxyl group in the same molecule, such as malic acid, is preferred, and more specifically, malic acid is preferably used. In addition, tetrafunctional aliphatic oxycarboxylic acid components are divided into (i) a type having three carboxyl groups and one hydroxyl group in the same molecule, (ii) a type having two carboxyl groups and two hydroxyl groups in the same molecule, and (iii) a type having three hydroxyl groups and one carboxyl group in the same molecule. Either type can be used, but those having multiple carboxyl groups are preferred, and more specifically, citric acid, tartaric acid, etc. can be mentioned. These can be used alone or in a mixture of two or more types.

[0043] When the polyester resin (A) contains such structural units derived from trifunctional or higher components, the content thereof, based on all structural units constituting the aliphatic polyester resin (A) being 100 mol %, is generally 0 mol % or more in lower limit, preferably 0.01 mol % or more in upper limit, and generally 5 mol % or less, preferably 2.5 mol % or less in upper limit.

[0044] The method for producing the aliphatic polyester resin (A) according to the present invention can adopt a known method for producing polyester. In addition, the polycondensation reaction at this time can set appropriate conditions that have been used in the past, and is not particularly limited. Usually, a method is adopted in which the polymerization degree is further increased by carrying out a decompression operation after the esterification reaction has progressed.

[0045] In the case where a diol component forming a diol unit and a dicarboxylic acid component forming a dicarboxylic acid unit are reacted during the production of the aliphatic polyester resin (A), the amounts of the diol component and the dicarboxylic acid component used are set so that the aliphatic polyester resin (A) produced has a desired composition. Usually, the diol component and the dicarboxylic acid component react in substantially equimolar amounts, but the diol component is usually used in an excess of 1 to 20 mol % over the dicarboxylic acid component because it is distilled off during the esterification reaction.

[0046] When the aliphatic polyester resin (A) contains components (optional components) other than the essential components such as aliphatic oxycarboxylic acid units and polyfunctional component units, the corresponding compounds (monomers and oligomers) are reacted so that the aliphatic oxycarboxylic acid units and polyfunctional component units have the desired compositions. At this time, there is no limitation on the timing and method of introducing the optional components into the reaction system, and they are optional as long as the aliphatic polyester resin (A) suitable for the present invention can be produced.

[0047] For example, the timing and method of introducing the aliphatic oxycarboxylic acid into the reaction system is not particularly limited as long as it is before the polycondensation reaction between the diol component and the dicarboxylic acid component. Examples of the method include (1) a method in which the catalyst is dissolved in an aliphatic oxycarboxylic acid solution in advance and mixed, and (2) a method in which the catalyst is introduced into the reaction system and mixed at the same time when the raw materials are charged.

[0048] The timing of introducing the compound that forms the polyfunctional component unit may be such that it is charged simultaneously with other monomers or oligomers at the initial stage of polymerization, or it may be charged after the ester exchange reaction and before the start of pressure reduction. However, charging the compound simultaneously with other monomers or oligomers is preferred from the viewpoint of process simplification.

[0049] Aliphatic polyester resin (A) is usually produced in the presence of a catalyst. As the catalyst, any catalyst that can be used in the production of known polyester resins can be selected as long as it does not significantly impair the effects of the present invention. For example, metal compounds such as germanium, titanium, zirconium, hafnium, antimony, tin, magnesium, calcium, and zinc are suitable. Among them, germanium compounds and titanium compounds are suitable.

[0050] Examples of germanium compounds that can be used as catalysts include organic germanium compounds such as tetraalkoxygermanium, and inorganic germanium compounds such as germanium oxide and germanium chloride. Among these, germanium oxide, tetraethoxygermanium, and tetrabutoxygermanium are preferred in terms of cost and availability, and germanium oxide is particularly preferred.

[0051] Examples of titanium compounds that can be used as catalysts include organic titanium compounds such as tetraalkoxytitanium compounds such as tetrapropyl titanate, tetrabutyl titanate, tetraphenyl titanate, etc. Among these, tetrapropyl titanate, tetrabutyl titanate, etc. are preferred in terms of cost and availability.

[0052] In addition, other catalysts may be used in combination as long as the object of the present invention is not impaired. The catalysts may be used alone or in any combination and ratio of two or more.

[0053] The amount of catalyst used is arbitrary as long as it does not significantly impair the effects of the present invention, but is usually 0.0005% by mass or more, more preferably 0.001% by mass or more, and usually 3% by mass or less, preferably 1.5% by mass or less, based on the amount of monomer used. If the amount is below the lower limit of this range, the effect of the catalyst may not be exhibited, and if the amount is above the upper limit, the production cost may increase, the obtained polymer may be significantly colored, or the hydrolysis resistance may decrease.

[0054] The timing of introducing the catalyst is not particularly limited as long as it is before the polycondensation reaction, and it may be introduced when the raw materials are charged, or may be introduced when the pressure reduction is started. When an aliphatic oxycarboxylic acid unit is introduced, it is preferable to introduce it simultaneously with a monomer or oligomer that forms an aliphatic oxycarboxylic acid unit, such as lactic acid or glycolic acid, when the raw materials are charged, or to dissolve the catalyst in an aqueous aliphatic oxycarboxylic acid solution and introduce it, and in particular, the method of dissolving the catalyst in an aqueous aliphatic oxycarboxylic acid solution and introducing it is preferable in terms of accelerating the polymerization rate.

[0055] The reaction conditions such as temperature, polymerization time, and pressure when producing the aliphatic polyester resin (A) are arbitrary as long as they do not significantly impair the effects of the present invention. The reaction temperature of the esterification reaction and / or transesterification reaction between the dicarboxylic acid component and the diol component is usually 150°C or more, preferably 180°C or more, and usually 260°C or less, preferably 250°C or less. The reaction atmosphere is usually an inert atmosphere such as nitrogen or argon. The reaction pressure is usually normal pressure to 10 kPa, and normal pressure is preferable. The reaction time is usually 1 hour or more, and usually 10 hours or less, preferably 6 hours or less, more preferably 4 hours or less. If the reaction temperature is too high, excessive generation of unsaturated bonds occurs, gelation caused by the unsaturated bonds occurs, and polymerization control may become difficult.

[0056] In addition, the pressure for the polycondensation reaction after the esterification reaction and / or transesterification reaction between the dicarboxylic acid component and the diol component is usually at a lower limit of 0.01×10 3 Pa or more, preferably 0.03×10 3 Pa or higher, with an upper limit of 1.4×10 3 Pa or less, preferably 0.4×10 3It is desirable to carry out the reaction under a vacuum of 0.1 Pa or less. The lower limit of the reaction temperature is usually 150° C. or more, preferably 180° C. or more, and the upper limit is usually 260° C. or less, preferably 250° C. or less. The lower limit of the reaction time is usually 2 hours or more, and the upper limit is usually 15 hours or less, preferably 10 hours or less. If the reaction temperature is too high, gelation caused by the unsaturated bonds due to excessive generation of unsaturated bonds may occur, making it difficult to control the polymerization.

[0057] When producing the aliphatic polyester resin (A), a chain extender such as a carbonate compound or a diisocyanate compound can also be used. In this case, the amount of the chain extender is usually 10 mol% or less, preferably 5 mol% or less, and more preferably 3 mol% or less, as the ratio of carbonate bonds or urethane bonds in the polyester resin (A) when the total structural units constituting the aliphatic polyester resin are 100 mol%. However, if urethane bonds or carbonate bonds are present in the aliphatic polyester resin (A), biodegradability may be inhibited. Therefore, in the present invention, the carbonate bonds are less than 1 mol%, preferably 0.5 mol% or less, more preferably 0.1 mol% or less, and the urethane bonds are 0.55 mol% or less, preferably 0.3 mol% or less, more preferably 0.12 mol% or less, and even more preferably 0.05 mol% or less, relative to the total structural units constituting the aliphatic polyester resin (A). This amount is 0.9 parts by mass or less, preferably 0.5 parts by mass or less, more preferably 0.2 parts by mass or less, and further preferably 0.1 parts by mass or less, calculated per 100 parts by mass of the aliphatic polyester resin (A). In particular, if the amount of urethane bonds exceeds the upper limit, the decomposition of the urethane bonds may cause problems in the film formation process, such as smoke or odor from the molten film exiting the die, and film breakage due to foaming may occur in the molten film, making it impossible to mold stably. The carbonate bond amount and urethane bond amount in the aliphatic polyester resin (A) are 1 H-NMR and 13 It can be determined by calculation from the results of NMR measurements such as C-NMR.

[0058] Specific examples of carbonate compounds as the chain extender include diphenyl carbonate, ditolyl carbonate, bis(chlorophenyl) carbonate, m-cresyl carbonate, dinaphthyl carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, ethylene carbonate, diamyl carbonate, dicyclohexyl carbonate, etc. In addition, carbonate compounds consisting of the same or different hydroxy compounds derived from hydroxy compounds such as phenols and alcohols can also be used.

[0059] Specific examples of the diisocyanate compound include known diisocyanates such as 2,4-tolylene diisocyanate, a mixture of 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate, 1,5-naphthylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, tetramethylxylylene diisocyanate, 2,4,6-triisopropylphenyl diisocyanate, 4,4'-diphenylmethane diisocyanate, and tolidine diisocyanate.

[0060] Other chain extenders such as dioxazoline and silicate esters may also be used. Specific examples of the silicate ester include tetramethoxysilane, dimethoxydiphenylsilane, dimethoxydimethylsilane, and diphenyldihydroxysilane.

[0061] It is also possible to produce high molecular weight polyester resins using these chain extenders (coupling agents) using conventional techniques. After the polycondensation is completed, the chain extender is added to the reaction system in a homogeneous molten state without a solvent, and reacted with the polyester obtained by the polycondensation.

[0062] More specifically, a polyester resin having a higher molecular weight can be obtained by reacting the chain extender with a polyester having a terminal group substantially containing a hydroxyl group and a weight average molecular weight (Mw) of 20,000 or more, preferably 40,000 or more, obtained by catalytically reacting a diol component with a dicarboxylic acid component. A prepolymer having a weight average molecular weight of 20,000 or more can be produced by using a small amount of chain extender without generating gel during the reaction, since it is not affected by the remaining catalyst even under severe conditions such as a molten state. Here, the weight average molecular weight (Mw) of the polyester resin is calculated as a monodisperse polystyrene conversion value from the measured value by gel permeation chromatography (GPC) at a measurement temperature of 40°C using chloroform as a solvent.

[0063] Therefore, for example, when the polyester resin is further increased in molecular weight using the above-mentioned diisocyanate compound as a chain extender, it is preferable to use a prepolymer having a weight average molecular weight of 20,000 or more, preferably 40,000 or more. If the weight average molecular weight is less than 20,000, the amount of diisocyanate compound used for increasing the molecular weight increases, and the heat resistance may decrease. Using such a prepolymer, a polyester resin having urethane bonds having a linear structure linked via urethane bonds derived from the diisocyanate compound is produced.

[0064] The pressure during chain extension is usually 0.01 MPa or more and 1 MPa or less, preferably 0.05 MPa or more and 0.5 MPa or less, more preferably 0.07 MPa or more and 0.3 MPa or less, and most preferably normal pressure.

[0065] The reaction temperature during chain extension has a lower limit of usually 100° C. or more, preferably 150° C. or more, more preferably 190° C. or more, and most preferably 200° C. or more, and an upper limit of usually 250° C. or less, preferably 240° C. or less, and more preferably 230° C. or less. If the reaction temperature is too low, the viscosity will be high, making it difficult to achieve a uniform reaction, and high stirring power will tend to be required, while if the reaction temperature is too high, gelation or decomposition of the polyester resin will tend to occur concomitantly.

[0066] The time for chain extension is usually 0.1 minutes or more, preferably 1 minute or more, more preferably 5 minutes or more, and usually 5 hours or less, preferably 1 hour or less, more preferably 30 minutes or less, and most preferably 15 minutes or less. If the time for chain extension is too short, the effect of adding the chain extender tends not to be exerted, and if it is too long, gelation or decomposition of the polyester resin tends to occur concomitantly.

[0067] The molecular weight of the aliphatic polyester resin (A) used in the present invention can be measured by gel permeation chromatography (GPC). The weight average molecular weight (Mw) of the aliphatic polyester resin (A) using monodisperse polystyrene as the standard is usually 10,000 or more and 1,000,000 or less, but is preferably 20,000 or more and 500,000 or less, and more preferably 50,000 or more and 400,000 or less, because this is advantageous in terms of moldability and mechanical strength.

[0068] The melt flow rate (MFR) of the aliphatic polyester resin (A) is a value measured at 190°C under a load of 2.16 kg according to JIS K7210 (1999), and is usually 0.1 g / 10 min to 100 g / 10 min, but from the viewpoints of moldability and mechanical strength, it is preferably 50 g / 10 min or less, and particularly preferably 30 g / 10 min or less. The MFR of the aliphatic polyester resin (A) can be adjusted by the molecular weight.

[0069] The melting point of the aliphatic polyester resin (A) is preferably 70° C. or higher, more preferably 75° C. or higher, and is preferably 170° C. or lower, more preferably 150° C. or lower, and particularly preferably lower than 130° C. When there are multiple melting points, it is preferable that at least one of the melting points is within the above range. The elastic modulus of the aliphatic polyester resin (A) is preferably 180 to 1000 MPa. If the melting point is outside the above range, the moldability is poor, and if the elastic modulus is less than 180 MPa, problems are likely to occur in the molding processability, while if the elastic modulus exceeds 1000 MPa, the obtained film tends to be brittle.

[0070] The method for adjusting the melting point and elastic modulus of the aliphatic polyester resin (A) is not particularly limited. For example, the melting point and elastic modulus can be adjusted by selecting the type of copolymerization component of the aliphatic dicarboxylic acid component other than succinic acid, adjusting the copolymerization ratio of each, or combining them.

[0071] As the aliphatic polyester resin (A), commercially available products can be used, such as "BioPBS (registered trademark) FZ71PB", "BioPBS (registered trademark) FZ71PM", "BioPBS (registered trademark) FZ91PB", "BioPBS (registered trademark) FZ91PM", "BioPBS (registered trademark) FD92PB", and "BioPBS (registered trademark) FD92PM" manufactured by PTTMCC Biochem.

[0072] In the present invention, the aliphatic polyester resin (A) is not limited to one type, and a blend of two or more types of aliphatic polyester resins (A) differing in the types and ratios of constituent units, production methods, physical properties, etc. may be used.

[0073] <Polyhydroxyalkanoate (B)> The polyhydroxyalkanoate (hereinafter sometimes referred to as PHA) (B) used in the present invention is an aliphatic polyester containing a repeating unit represented by the general formula: [-CHR-CH2-CO-O-] (wherein R is an alkyl group having 1 to 15 carbon atoms), and is a copolymer containing 3-hydroxybutyrate units and 3-hydroxyhexanoate units as main constituent units.

[0074] From the viewpoint of moldability and thermal stability, the polyhydroxyalkanoate (B) used in the present invention preferably contains 80 mol% or more, more preferably 85 mol% or more, of 3-hydroxybutyrate units as a constituent component. Also, it is preferable that it is produced by a microorganism. Specific examples of the polyhydroxyalkanoate (B) include poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin, poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate) copolymer resin, etc. In particular, from the viewpoints of molding processability and physical properties of the resulting molded article, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin, ie, PHBH, is preferred.

[0075] In the polyhydroxyalkanoate (B), the composition ratio of 3-hydroxybutyrate (hereinafter sometimes referred to as 3HB) and the copolymerized comonomer such as 3-hydroxyhexanoate (hereinafter sometimes referred to as 3HH), i.e., the monomer ratio in the copolymer resin, is preferably 3-hydroxybutyrate / comonomer=97 / 3 to 80 / 20 (mol% / mol%), more preferably 95 / 5 to 85 / 15 (mol% / mol%), from the viewpoint of molding processability and molded product quality. If the comonomer ratio is less than 3 mol%, molding may be difficult because the molding temperature and the thermal decomposition temperature are close to each other. If the comonomer ratio exceeds 20 mol%, the crystallization of the polyhydroxyalkanoate (B) may be delayed, resulting in poor productivity.

[0076] The ratio of each monomer in the polyhydroxyalkanoate (B) can be measured by gas chromatography as follows. To approximately 20 mg of dried PHA, 2 ml of a sulfuric acid / methanol mixture (15 / 85 (mass ratio)) and 2 ml of chloroform are added, the container is sealed, and heated at 100°C for 140 minutes to obtain the methyl ester of the PHA decomposition product. After cooling, 1.5 g of sodium bicarbonate is gradually added to neutralize the mixture, and the mixture is left to stand until the evolution of carbon dioxide gas stops. After adding 4 ml of diisopropyl ether and mixing well, the monomer unit composition of the PHA decomposition product in the supernatant is analyzed by capillary gas chromatography to determine the ratio of each monomer in the copolymer resin.

[0077] The weight average molecular weight (hereinafter sometimes referred to as Mw) of the polyhydroxyalkanoate (B) used in the present invention can be measured by the above-mentioned gel permeation chromatography (GPC), and the weight average molecular weight (Mw) using monodisperse polystyrene as the standard substance is usually 200,000 or more and 2,500,000 or less, but is preferably 250,000 or more and 2,000,000 or less, more preferably 300,000 or more and 1,000,000 or less, because it is advantageous in terms of moldability and mechanical strength. If the weight average molecular weight is less than 200,000, the mechanical properties may be poor, and if it exceeds 2,500,000, molding processing may be difficult.

[0078] The melt flow rate (MFR) of the polyhydroxyalkanoate (B) is a value measured at 190°C under a load of 2.16 kg according to JIS K7210 (1999), and is preferably 1 g / 10 min to 100 g / 10 min, but from the viewpoints of moldability and mechanical strength, it is more preferably 80 g / 10 min or less, and particularly preferably 50 g / 10 min or less. The MFR of the polyhydroxyalkanoate (B) can be adjusted by the molecular weight.

[0079] The melting point of the polyhydroxyalkanoate (B) is preferably 100° C. or higher, more preferably 120° C. or higher, and is preferably 180° C. or lower, more preferably 170° C. or lower, and particularly preferably lower than 160° C. When there are multiple melting points, it is preferable that at least one of the melting points is within the above range.

[0080] Polyhydroxyalkanoate (B) is produced by, for example, a microorganism such as Alcaligenes eutrophus AC32 strain, which is obtained by introducing a PHA synthase gene derived from Aeromonas caviae into Alcaligenes eutrophus (international deposit under the Budapest Treaty, international depository authority: National Institute of Advanced Industrial Science and Technology Patent Organism Depositary Center (6-1-1 Central, Higashi 1-chome, Tsukuba City, Ibaraki Prefecture, Japan), original deposit date: August 12, 1996, transferred on August 7, 1997, deposit number FERM BP-6038 (transferred from original deposit FERM P-15786)) (J. Bacteriol., 179, 4821 (1997)).

[0081] As the polyhydroxyalkanoate (B), commercially available products can be used. Commercially available products of the polyhydroxyalkanoate (B) containing 3-hydroxybutyrate units and 3-hydroxyhexanoate units as main constituent units include "Aonilex (registered trademark) X131N", "Aonilex (registered trademark) X131A", "Aonilex (registered trademark) 151A", "Aonilex (registered trademark) 151C", "PHBH (registered trademark) X331N", "PHBH (registered trademark) X131A", "PHBH (registered trademark) 151A", and "PHBH (registered trademark) 151C" manufactured by Kaneka Corporation.

[0082] In the present invention, the polyhydroxyalkanoate (B) is not limited to one type, but a blend of two or more types of polyhydroxyalkanoates (B) differing in the types and ratios of constituent units, production methods, physical properties, etc. may be used.

[0083] <Inorganic filler (C)> The aliphatic polyester resin composition of the present invention further contains an inorganic filler (C) in addition to the polyester resin (A) and the polyhydroxyalkanoate (B).

[0084] Examples of the inorganic filler (C) used in the present invention include anhydrous silica, mica, talc, titanium oxide, calcium carbonate, diatomaceous earth, allophane, bentonite, potassium titanate, zeolite, sepiolite, smectite, kaolin, kaolinite, glass, limestone, carbon, wollastonite, calcined perlite, silicates such as calcium silicate, sodium silicate, and aluminum silicate, hydroxides such as aluminum oxide, magnesium carbonate, and calcium hydroxide, and salts such as ferric carbonate, zinc oxide, iron oxide, aluminum phosphate, and barium sulfate, and the like, with talc, calcium carbonate, and zeolite being preferred.

[0085] Some inorganic fillers, such as calcium carbonate and limestone, have soil conditioner properties. If a film made of an aliphatic polyester resin composition containing a biomass-derived aliphatic polyester resin (A) and a polyhydroxyalkanoate (B) that contains a particularly large amount of these inorganic fillers is dumped into the soil, the inorganic filler (C) will remain after biodegradation and will also function as a soil conditioner, thereby enhancing its significance as a biodegradable resin composition.

[0086] In addition, the inorganic filler (C) can be classified according to its shape, and includes fibrous, spherical, plate-like, and needle-like fillers, with spherical or plate-like fillers being preferred. Examples of spherical fillers include calcium carbonate, spherical silica, spherical glass beads, and graphite. Examples of plate-like fillers include talc, kaolin, mica, clay, sericite, glass flakes, synthetic hydrotalcite, various metal foils, graphite, molybdenum disulfide, tungsten disulfide, boron nitride, plate-like iron oxide, plate-like calcium carbonate, plate-like aluminum hydroxide, silicates, and zeolites. From the viewpoints of ease of blending, rigidity, moldability, decomposability, and enhancing the deodorizing effect, it is preferable to use talc, mica, or clay, calcium carbonate, silicates, and zeolites.

[0087] The particle size of the inorganic filler (C) used in the present invention is preferably 0.5 μm or more, more preferably 0.6 μm or more, even more preferably 0.7 μm or more, and particularly preferably 1.0 μm or more, for the reason of handling. On the other hand, the average particle size is preferably 30 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, and particularly preferably 10 μm or less. Here, the method for measuring the average particle size of the inorganic filler (C) is not particularly limited, but a specific example of the measurement method includes determining the specific surface area per gram of powder using a powder specific surface area measuring device SS-100 (constant pressure air permeability method) manufactured by Shimadzu Corporation, and calculating the average particle size of the filler from the measurement results of the specific surface area using the air permeability method in accordance with JIS M8511 using the following formula. Average particle size (μm) = 10,000 × {6 / (specific gravity of filler × specific surface area)}

[0088] The inorganic filler (C) may be used alone or as a mixture of two or more kinds in any combination and in any ratio.

[0089] Specific examples of talc that can be suitably used as the inorganic filler (C) include Microace manufactured by Nippon Talc Co., Ltd. and FH105 manufactured by Fuji Talc Kogyo Co., Ltd. Specific examples of calcium carbonate that can be suitably used as the inorganic filler (C) include Softon 1200 and 2200 manufactured by Bihoku Funka Kogyo Co., Ltd.

[0090] <Mixing ratio of aliphatic polyester resin (A), polyhydroxyalkanoate (B) and inorganic filler (C)> The mass ratio of the aliphatic polyester resin (A) to the polyhydroxyalkanoate (B) contained in the aliphatic polyester resin composition of the present invention is preferably aliphatic polyester resin (A) / polyhydroxyalkanoate (B)=95 / 5 to 70 / 30, more preferably 93 / 7 to 75 / 25, and even more preferably 90 / 10 to 80 / 20, from the viewpoints of improving opening properties (peel strength), rigidity, and ease of molding processability.

[0091] The content of the inorganic filler (C) in the aliphatic polyester resin composition of the present invention is 0.1 parts by mass or more, preferably 0.2 parts by mass or more, more preferably 0.3 parts by mass or more, and 15 parts by mass or less, preferably 12 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the total amount of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B). If the content of the inorganic filler (C) is less than the lower limit, the effect of improving the opening property, etc. by blending the inorganic filler (C) cannot be sufficiently obtained. On the other hand, if the content of the inorganic filler (C) is more than the upper limit, the mechanical strength, such as the tensile strength, decreases.

[0092] <Other resins> The aliphatic polyester resin composition of the present invention may contain one or more resins other than the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B), for example, synthetic resins such as aromatic polyester resins, polycarbonate, polyamide, polystyrene, polyolefin, acrylic resin, amorphous polyolefin, ABS, AS (acrylonitrile styrene), polycaprolactone, polyvinyl alcohol, and cellulose ester, and biodegradable resins such as polylactic acid and the aliphatic aromatic polyester polybutylene adipate terephthalate (PBAT), as long as the effects of the present invention are not impaired.

[0093] When the aliphatic polyester resin composition of the present invention contains these other resins, in order to effectively obtain the effects of the present invention by including the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B) as resin components, the content of the other resins is preferably 70 parts by mass or less, particularly 50 parts by mass or less, per 100 parts by mass of the total of the aliphatic polyester resin (A), the polyhydroxyalkanoate (B), and the other resins.

[0094] <Other ingredients> The aliphatic polyester resin composition of the present invention may contain, as "other components", various additives such as lubricants, plasticizers, antistatic agents, antioxidants, light stabilizers, UV absorbers, dyes, pigments, hydrolysis inhibitors, crystal nucleating agents, antiblocking agents, light resistance agents, plasticizers, heat stabilizers, flame retardants, release agents, anti-fogging agents, surface wetting improvers, incineration aids, dispersing aids, various surfactants, and slip agents, as well as fine powders of animal / plant substances such as starch, cellulose, paper, wood flour, chitin / chitosan, coconut shell powder, and walnut shell powder, or mixtures of these. Furthermore, the aliphatic polyester resin composition of the present invention may also contain functional additives such as a freshness-preserving agent and an antibacterial agent. These may be blended in any amount within the range that does not impair the effects of the present invention, and one type may be used alone, or two or more types may be mixed and used.

[0095] In order not to impair the physical properties of the aliphatic polyester resin composition of the present invention, it is usually preferable that the content of these other components is such that the total amount of the components to be mixed is 0.01 mass% or more and 40 mass% or less relative to the total amount of the aliphatic polyester resin composition of the present invention.

[0096] Among the above other components, the antifogging agent may be kneaded into the aliphatic polyester resin composition in advance, or may be applied to the surface of the film after the film is formed. Specifically, the antifogging agent used is preferably an ester surfactant of a saturated or unsaturated aliphatic carboxylic acid having 4 to 20 carbon atoms and a polyhydric alcohol.

[0097] It is preferable to add a slip agent to the aliphatic polyester resin composition of the present invention, since it can improve the moldability of the resin composition. As the slip agent, any known one can be used without any particular limitation, and specifically, there can be mentioned paraffin such as paraffin oil and solid paraffin, higher fatty acid such as stearic acid and palmitic acid, higher alcohol such as palmityl alcohol and stearyl alcohol, metal salts of fatty acid such as calcium stearate, zinc stearate, barium stearate, aluminum stearate, magnesium stearate, and sodium palmitate, fatty acid esters such as butyl stearate, glycerin monostearate, and diethylene glycol monostearate, fatty acid amides such as stearamide, methylene bis stearate, ethylene bis stearate, ethylene diamide of oxystearic acid, methylol amide, oleyl amide, stearic acid amide, and erucic acid amide, waxes such as carnauba wax and montan wax, etc. These slip agents may be used alone or in any ratio and combination of two or more. Among them, erucic acid amide is particularly preferable as the slip agent. In the aliphatic polyester resin composition of the present invention, the content of these slip agents is usually 0.01 to 2% by mass, and preferably in the range of 0.05 to 0.5% by mass, in the resin composition.

[0098] Examples of the anti-blocking agent include saturated fatty acid amides having 6 to 30 carbon atoms, saturated fatty acid bisamides, methylol amide, ethanol amide, natural silica, synthetic silica, synthetic zeolite, and talc.

[0099] Specific examples of the light stabilizer include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl)sebacate, 2-(3,5-di-t-butyl-4-hydroxyphenyl)-2-n-butyl-bis(2,2,6,6-tetramethyl-4-piperidyl)malonate, 2-(3,5-di-t -butyl-4-hydroxyphenyl)-2-n-butyl-bis(1,2,2,6,6-pentamethyl-4-piperidyl)malonate, 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butyl-bis(2,2,6,6-tetramethyl-4-piperidyl)malonate, 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butyl-bis(1,2,2,6,6-pentamethyl-4-piperidyl)malonate, tetrakis (2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, tetrakis(1,2,2,6,6-pentamethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, mixed(2,2,6,6-tetramethyl-4-piperidyl / tridecyl)-1,2,3,4-butanetetracarboxylate, mixed(1,2,2,6,6-pentamethyl-4-piperidyl / tridecyl)-1,2 ,3,4-Butanetetracarboxylate, mixed {2,2,6,6-tetramethyl-4-piperidyl / β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro[5.5]undecane]diethyl}-1,2,3,4-Butanetetracarboxylate, mixed {1,2,2,6,6-pentamethyl-4-piperidyl / β,β,β',β'-tetramethyl-3,9-[2,4,8,10-tetraoxaspiro[5.5]undecane]diethyl}-1,2,3,4-butanetetracarboxylate, 1,2-bis(3-oxo-2,2,6,6-tetramethyl-4-piperidyl)ethane, 1-(3,5-di-t-butyl-4-hydroxyphenyl)-1,1-bis(2,2,6,6-tetramethyl-4-piperidyloxycarbonyl)pentane, poly[1-oxyethylene(2,2,6,6-tetramethyl-1,4-piperidyl)oxysuccinyl], poly[2-(1,1,4-trimethylbutylimino)-4,6-triazinedicarboxylate], Examples of such compounds include N,N'-bis(3-aminopropyl)ethylenediamine-2,4-bis[N-butyl-N-(2,2,6,6-tetramethyl-4-piperidyl)amino]-6-chloro-1,3,5-triazine condensate and its N-methyl compound, and polycondensate of succinic acid and 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine.

[0100] Among these, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate and 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butyl-bis(1,2,2,6,6-pentamethyl-4-piperidyl)malonate are particularly preferred.

[0101] As the ultraviolet absorbent, among ultraviolet absorbents such as benzophenone-based, benzotriazole-based, salicylic acid-based, and cyanoacrylate-based ultraviolet absorbents, benzotriazole-based ultraviolet absorbents are preferred, and specific examples thereof include 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-hexyloxy-phenol.

[0102] Antioxidants include BHT (dibutylhydroxytoluene), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 3,3',3",5,5',5"-hexa-tert-butyl-α,α',α"-(mesitylene-2,4,6-triyl)tri-p-cresol, and octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate. propionate, 1,3,5-tris[(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, calcium diethyl bis[{3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl}methyl]phosphonate, bis(2,2'-dihybrid hindered phenol antioxidants such as N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl)-4-hydroxyphenyl]propionamide, tridecyl phosphite, diphenyldecyl phosphite, tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diyl bisphosphonate, bis[2,4-bis(1,1-dimethylethyl)- Examples of antioxidants include phosphorus-based antioxidants such as 6-methylphenyl]ethyl ester phosphorous acid and bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, lactone-based antioxidants such as the reaction product of 3-hydroxy-5,7-di-tert-butyl-furan-2-one and xylene, sulfur-based antioxidants such as dilauryl thiodipropionate and distearyl thiodipropionate, and mixtures of two or more of these antioxidants. Among these, hindered phenol-based antioxidants are preferably used.

[0103] Preferred hindered phenol-based antioxidants include Irganox 3790, Irganox 1330, Irganox 1010, Irganox 1076, Irganox 3114, Irganox 1425WL, Irganox 1098, Irganox HP2225FL, Irganox HP2341, Irgafos XP-30 (all manufactured by BASF), and Sumilizer BBM-S (manufactured by Sumitomo Chemical Co., Ltd.). The most preferred antioxidants are Irganox 1010 (pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]), Irganox 1330 (3,3',3",5,5',5"-hexa-tert-butyl-α,α',α"-(mesitylene-2,4,6-triyl)tri-p-cresol).

[0104] Any antistatic agent can be used as long as it does not significantly impair the effects of the present invention. Preferred antistatic agents are surfactant-type nonionic, cationic, and anionic antistatic agents. Examples of nonionic antistatic agents include glycerin fatty acid esters, polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, alkyldiethanolamines, hydroxyalkylmonoethanolamines, polyoxyethylene alkylamines, polyoxyethylene alkylamine fatty acid esters alkyldiethanolamides, etc. Among these, alkyldiethanolamines, etc. are preferred. Examples of the cationic antistatic agent include tetraalkylammonium salts and trialkylbenzylammonium salts. Examples of the anionic antistatic agent include alkyl sulfonates, alkyl benzene sulfonates, and alkyl phosphates. Among these, alkylbenzene sulfonates are preferred because they have good kneadability with resins and a high antistatic effect.

[0105] <Method of producing aliphatic polyester resin composition> The aliphatic polyester resin composition of the present invention is produced by mixing the aliphatic polyester resin (A), the polyalkanoate (B), and the inorganic filler (C) with other resins and other components that are used as necessary.

[0106] This mixing step is carried out by mixing the aliphatic polyester resin (A), polyhydroxyalkanoate (B), and inorganic filler (C) with other resins and other components used as necessary in a predetermined ratio simultaneously or in any order using a mixer such as a tumbler, V-type blender, Nauter mixer, Banbury mixer, kneading roll, or extruder, and preferably melt-kneading the mixture.

[0107] The kneader used in the mixing step may be a melt kneader. In addition, there is no limitation on the type of twin-screw extruder or single-screw extruder, but a twin-screw extruder is more preferable for the purpose of achieving melt kneading according to the properties of the aliphatic polyester resin (A), polyhydroxyalkanoate (B), and inorganic filler (C) used.

[0108] The temperature during melt kneading is preferably 120 to 220° C., and more preferably 130 to 160° C. Within this temperature range, it is possible to shorten the time required for the melting reaction, prevent deterioration of color tone due to deterioration of the resin, and further improve practical physical properties such as impact resistance and moist heat resistance. With regard to the melt-kneading time, from the viewpoint of more reliably avoiding the resin deterioration as described above, unnecessary lengthening should be avoided, and the time is preferably from 20 seconds to 20 minutes, more preferably from 30 seconds to 15 minutes, and it is preferable to set the melt-kneading temperature and time conditions so as to satisfy this.

[0109] [film] The film of the present invention is obtained by molding the aliphatic polyester resin composition of the present invention. Examples of the molding method include injection molding, extrusion molding, coextrusion molding (film molding by inflation method or T-die method), lamination molding, heat press molding, blow molding (various blow moldings), thermoforming (vacuum molding, pressure molding), plastic processing, powder molding (rotational molding), etc. In particular, the method of molding by extrusion molding or inflation molding (inflation method) and the T-die method are preferred because the effects of the present invention are significantly exhibited.

[0110] More specifically, for example, a method in which a film-like, sheet-like or cylindrical product extruded to a predetermined thickness from a T-die, an I-die, a round die or the like is cooled and solidified by a cooling roll, water, compressed air, etc. In this case, it is also possible to form a laminated film by laminating several types of compositions within a range that does not impair the effects of the present invention.

[0111] In the case of inflation molding, the conditions such as bubble internal pressure, heating temperature, bubble diameter, cooling rate, and take-up speed may be those generally known in the art. As for the molding conditions, for example, the blow ratio is usually set to 1.1 to 10 times, preferably 2 to 5 times, so that the tear strength of the film can be adjusted. The suitability for inflation molding is evaluated by visually checking bubble stability, frost line height, etc., and the more stable the bubble is, the more preferable it is, and the more symmetrical the bubble shape is. It is preferable that the frost line height is not too high. If the frost line is too high, it indicates that the tubular film is difficult to solidify, and film blocking may occur, leading to poor opening. If the frost line is too low, the bubble may come into contact with the air ring or die, making molding impossible. Therefore, the frost line must be at a height appropriate for the equipment, raw materials used, and processing conditions.

[0112] The lower limit of the resin temperature in the die is usually 110°C so that the melt viscosity does not become too high and the extrusion rate per power of the extruder is appropriate. On the other hand, the upper limit is usually 280°C so that resin deterioration does not adhere to the die and get mixed into the obtained film. The resin temperature in the die is preferably in the range of 120 to 250°C, more preferably 130 to 200°C.

[0113] The film of the present invention obtained by such inflation molding may have a single-layer structure or a laminate structure. The thickness of the film produced by inflation molding is usually 6 to 100 μm, and preferably 10 to 50 μm.

[0114] In the case of T-die molding, the lower limit of the resin temperature in the die is usually 120°C so that the melt viscosity does not become too high and the extrusion amount per power of the extruder is appropriate. On the other hand, the upper limit is usually 280°C so that resin deterioration does not adhere to the die and is not mixed into the obtained film. The resin temperature in the die is preferably in the range of 130 to 250°C, more preferably 140 to 220°C. In addition, the discharged molten resin is desirably cooled quickly to prevent blocking during winding, and is usually cooled by an electrostatic contact type or touch roll type casting roll. In this case, the surface temperature of the casting roll is usually controlled to 15 to 70°C, preferably 20 to 60°C. In addition, when the sheet has a thickness of 1 mm or more, it is desirably to use a multi-stage cooling roll. Other molding conditions can be adopted as usual known conditions.

[0115] The film of the present invention obtained by T-die molding may have either a single layer structure or a laminate structure. The thickness of the film formed by T-die molding is usually 3 to 200 μm, and preferably 5 to 100 μm.

[0116] The film-like molded product obtained by the inflation method or T-die method may then be uniaxially or biaxially stretched by a roll method, a tenter method, a tubular method, etc. When stretching, the stretching temperature is usually in the range of 30° C. to 110° C., and the stretching ratio is in the range of 0.6 to 10 times in the longitudinal and transverse directions, respectively. After stretching, the film may be heat-treated by a method of blowing hot air, irradiating infrared rays, irradiating microwaves, contacting with a heat roll, etc.

[0117] The film-like molded article obtained by the inflation method or the T-die method may then be laminated with another substrate. The lamination method may be a commonly known method, such as a dry lamination method, a non-solvent lamination method, or a thermal lamination method.

[0118] The film of the present invention obtained by molding the aliphatic polyester resin composition of the present invention may be subjected to various secondary processing steps in order to impart surface functions such as chemical functions, electrical functions, magnetic functions, mechanical functions, friction / wear / lubrication functions, optical functions, thermal functions, and biocompatibility. Examples of secondary processing steps include bellows processing, embossing, painting, adhesion, printing, metallizing (plating, etc.), machining, and surface treatments (antistatic treatment, corona discharge treatment, plasma treatment, photochromism treatment, physical vapor deposition, chemical vapor deposition, coating, etc.).

[0119] [Film properties] <Tensile breaking strength> The tensile breaking strength of the film of the present invention is a value measured by the method specified in JIS K7127 (1999), and from the viewpoint of practicality, is usually preferably 15 MPa or more in both the MD and TD directions, more preferably 20 MPa or more, further preferably 25 MPa or more, and particularly preferably 30 MPa or more. In particular, since inflation films are often thin, 25 MPa or more is preferable.

[0120] <Tensile modulus> The tensile modulus of the film of the present invention is a value measured by the method specified in JIS K7127 (1999), and from the viewpoint of practicality, is usually preferably 300 MPa or more in either the MD direction or the TD direction, more preferably 350 MPa or more, and even more preferably 400 MPa or more.

[0121] <haze> The film of the present invention preferably has excellent transparency, and preferably has a haze of 40 or less, particularly 35 or less, measured by the method specified in JIS K7136 (2000), regardless of the thickness.

[0122] <Opening ability> The inflation film of the present invention obtained by inflation molding needs to have a bag opening, so it is preferable that the bag opening is easy. The opening property can be evaluated as a peel strength measured by the method specified in ASTM D1893-67 (1985), and the lower the peel strength, the better. Specifically, the peel strength between the inner faces of the inflation film in the MD direction is preferably 15N or less, more preferably 12N or less, and even more preferably 10N or less.

[0123] [Application] The film of the present invention has excellent formability, transparency, surface properties and mechanical properties of the molded product while being degradable in the natural environment, and therefore can be suitably used in a wide range of applications, particularly disposable applications, such as packaging materials for liquids, powders and granules, solids, etc., for various foods, medicines, miscellaneous goods, agricultural materials, construction materials, etc. Specific applications include, for example, agricultural mulch films, tunnel films, greenhouse films, sunshades, weed control sheets, ridge sheets, germination sheets, forestry fumigation sheets, binding tapes including flat yarns, etc., diaper back sheets, packaging sheets, shopping bags, plastic bags, garbage bags, draining bags, compost bags, etc. EXAMPLES

[0124] Hereinafter, specific aspects of the present invention will be described in more detail using examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention. Note that the values ​​of various manufacturing conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiments of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0125] [Melt flow rate (MFR) measurement of resin used] Based on JIS K7210 (1999), measurements were taken using a melt indexer at 190°C and a load of 2.16 kg. The unit is g / 10 min.

[0126] [Raw materials used] Details of the resins and inorganic fillers used in the examples and comparative examples are as follows. In the following, "PBS" stands for "polybutylene succinate," "PBSA" stands for "polybutylene succinate adipate," and "PHBH" stands for "poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)."

[0127] <Aliphatic polyester resin (A)> PBSA (BioPBS (registered trademark) FD92PM manufactured by PTTMCC Biochem, succinic acid unit amount in total dicarboxylic acid unit amount: 74 mol%, adipic acid unit amount: 26 mol%, MFR: 5.0 g / 10 min, melting point: 89° C.) PBS (BioPBS FZ91PM manufactured by PTTMC BioChem, succinic acid unit amount in total dicarboxylic acid unit amount: 100 mol%, adipic acid unit amount: 0 mol%, MFR: 5.0 g / 10 min, melting point: 113° C.)

[0128] <Polyhydroxyalkanoate (B)> PHBH-1 (PHBH (registered trademark) X131A, manufactured by Kaneka Corporation, 3HB / 3HH molar ratio: 94 / 6, MFR: 6g / 10min, melting point: 140°C) PHBH-2 (Aonilex (registered trademark) X151A, manufactured by Kaneka Corporation, 3HB / 3HH molar ratio: 89 / 11, MFR: 6 g / 10 min, melting point: 131° C.)

[0129] <Inorganic filler (C)> Talc-1 (Microace SG-95, manufactured by Nippon Talc Co., Ltd., average particle size: 3 μm) Talc-2 (FH105 manufactured by Fuji Talc Industries Co., Ltd., average particle size: 5 μm) Talc-3 (Microace K-1, manufactured by Nippon Talc Co., Ltd., average particle size: 8 μm) Talc-4 (MG-115 manufactured by Fuji Talc Industries Co., Ltd., average particle size: 14 μm)

[0130] <Erucic acid amide> Mitsubishi Chemical Corporation Diamond L-200

[0131] [Evaluation method] The methods for evaluating various physical properties and characteristics in the examples and comparative examples are as follows.

[0132] <Moldability: Bubble stability> The bubble stability during inflation molding was evaluated according to the following criteria. ○: The bubbles are stable and the moldability is good. ×: The bubbles are unstable and there is a problem with moldability.

[0133] <Moldability: Mouth opening> According to ASTM D1893-67 (1985), the peel strength in the MD direction between the inner faces of the inflation film was measured and evaluated according to the following criteria. The lower the peel strength, the better the opening property, which is preferable. ○: Peel strength is 12N or less ×: Peel strength is 13N or more

[0134] <Tensile modulus> The tensile modulus in the MD and TD directions was measured based on JIS K7127 (1999) and evaluated according to the following criteria. The higher the tensile modulus, the higher the rigidity, which is preferable. ○: Tensile modulus of elasticity is 300 MPa or more ×: Tensile modulus is less than 300 MPa

[0135] <Tensile breaking strength> The tensile breaking strength in the MD and TD directions was measured based on JIS K7127 (1999) and evaluated according to the following criteria. A higher tensile breaking strength is preferable because it is less likely to break. ○: Tensile breaking strength is 25MPa or more ×: Tensile breaking strength is less than 25 MPa

[0136] <Haze measurement> Measured based on JIS K7136 (2000). The smaller the Haze value, the better the transparency, which is preferable.

[0137] <Biodegradability test at room temperature in soil> The film was stored in soil (moisture content 30%) collected from a farm in Mie Prefecture for 3 months at 28 ± 2 °C, and then weight measurement was carried out to evaluate the biodegradability at room temperature in soil according to the following criteria. The degree of degradation was calculated by the following formula. Degree of degradation (%) = 100 - (weight of sample after 3 months / weight of sample before test) × 100 〇: Degree of degradation is 90% or more ×: Degree of degradation is less than 90%

[0138] <Biodegradability test in seawater> The sheet was stored in seawater collected from Yokkaichi Port, Yokkaichi City, Mie Prefecture for 6 months at 28 ± 2 °C, and then weight measurement was carried out to evaluate the biodegradability in seawater according to the following criteria. The degree of degradation was calculated by the following formula. Degree of degradation (%) = 100 - (weight of sample after 6 months / weight of sample before test) × 100 〇: Degree of degradation is 50% or more ×: Degree of degradation is less than 50%

[0139] [Examples 1 - 8, Comparative Examples 1 - 2] The raw materials shown in Table 1 were blended at the ratios shown in Table 1, extruded into strands using a twin-screw extruder with a screw diameter of φ30 mm at a kneading temperature of 140 °C, and pelletized by a pelletizer. The obtained resin pellets were formed into an inflation film with a thickness of 30 μm at a forming temperature of 160 °C and a blow ratio of 2.5 using an extruder with a screw diameter of φ40 mm and an inflation molding machine having a round die with a diameter of 60 mm. For this film, formability evaluation (bubble stability, mouth opening property), tensile test (elastic modulus, breaking strength), Haze measurement, biodegradability evaluation at room temperature in soil, and biodegradability evaluation in seawater were carried out. The results are shown in Table 1.

[0140] [Table 1]

[0141] [Examples 9 to 12] The raw materials shown in Table 2 were blended in the ratios shown in Table 2, extruded into strands using a twin-screw extruder with a screw diameter of φ30 mm at a kneading temperature of 140°C, and pelletized using a pelletizer. The resulting resin pellets were molded using an inflation molding machine equipped with an extruder with a screw diameter of φ40 mm and a round die with a diameter of 60 mm at a molding temperature of 160°C and a blow ratio of 2.5 to obtain an inflation film with a thickness of 30 μm. This film was subjected to moldability evaluation (bubble stability, mouth opening property), tensile test (elastic modulus, breaking strength), haze measurement, evaluation of biodegradability at room temperature in soil, and evaluation of biodegradability in seawater. The results are shown in Table 2.

[0142] [Table 2]

[0143] From Table 1, it can be seen that the film of the present invention has a better balance of formability, rigidity, tensile strength, transparency, room temperature biodegradability, and marine biodegradability compared to films using conventional biodegradable resins. From Table 2, it is clear that the transparency of the film of the present invention is particularly improved by using an inorganic filler having a small particle size. The film of the present invention uses as its resin components an aliphatic polyester resin (A) and a polyhydroxyalkanoate (B) which are themselves highly biodegradable at room temperature and also have a high degree of biodegradability in the sea. In addition, the inorganic filler (C) also contributes to improving biodegradability. As a result, as shown in Tables 1 and 2, the film has excellent biodegradability at room temperature and in the sea.

[0144] In addition, in Comparative Example 1, the proportion of aliphatic polyester resin (A) is less than the range specified in the present invention, and the proportion of polyhydroxyalkanoate (B) is more than the range specified in the present invention, so the molding stability, opening property (peel strength), and tensile breaking strength are poor. Comparative Example 2 does not contain polyhydroxyalkanoate (B) and is therefore inferior in tensile modulus.< / haze>

Claims

1. An aliphatic polyester resin composition comprising: an aliphatic polyester resin (A) containing, as main structural units, a repeating unit derived from an aliphatic diol and a repeating unit derived from an aliphatic dicarboxylic acid; a polyhydroxyalkanoate (B); and an inorganic filler (C); The melting point of the aliphatic polyester resin (A) is 70° C. or more and less than 130° C., the inorganic filler (C) is one or more selected from the group consisting of anhydrous silica, calcium carbonate, talc, silicates, and zeolites; The polyhydroxyalkanoate (B) is a copolymer containing 3-hydroxybutyrate units and 3-hydroxyhexanoate units as main constituent units, a mass ratio of the aliphatic polyester resin (A) to the polyhydroxyalkanoate (B) is 95 / 5 to 70 / 30; A film using an aliphatic polyester resin composition in which the content ratio of the inorganic filler (C) per 100 parts by mass of the total amount of the aliphatic polyester resin (A) and the polyhydroxyalkanoate (B) is 0.1 to 15 parts by mass.

2. The film according to claim 1 , wherein the repeating units derived from the aliphatic dicarboxylic acid contained in the aliphatic polyester resin (A) contain succinic acid units and adipic acid units.

3. 3. The film according to claim 1, wherein the adipic acid unit content in the repeating units derived from the aliphatic dicarboxylic acid contained in the aliphatic polyester resin (A) is 18 mol % or more and 32 mol % or less.

4. The film according to any one of claims 1 to 3, wherein the inorganic filler (C) has an average particle size of 30 µm or less.

5. The film according to any one of claims 1 to 4, having a tensile breaking strength of 25 MPa or more.

6. The film according to any one of claims 1 to 5, having a haze of 40 or less.

7. The film according to any one of claims 1 to 6, which is formed by an inflation method.

8. The film according to any one of claims 1 to 6, which is formed by a T-die method.

Citation Information

Patent Citations

  • Biodegradable film

    JP2002146182A

  • Aliphatic polyester resin composition having low branching degree and high molecular weight, molded article and film

    JP2006274256A

  • Biodegradation promoting method of poly(3-hydroxybutylate)-based resin, polyester resin composition by the method, and molded body

    JP2017132967A

  • Biodegradable film

    JP2020516712A

  • Biodegradable film

    JP2020525557A