Dispersion
A dispersion of fine fibrous cellulose with anionic groups and organic onium ions in organic solvents achieves high thixotropy, addressing the lack of stability in existing dispersions and enhancing application performance.
Patent Information
- Application Number
- JP2020171468
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-09
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-10-09
AI Technical Summary
Existing dispersions of fine fibrous cellulose in organic solvents lack high thixotropy, which is essential for applications requiring stable viscosity under varying shear conditions.
A dispersion containing fibrous cellulose with a fiber width of 1000 nm or less, anionic groups at 0.50 mmol/g or more, and organic onium ions as counterions, achieving a B-type viscosity of 50 Pa·s or more, along with specific light transmittance and solvent properties, enhances thixotropic properties.
The dispersion exhibits high thixotropy, allowing for stable viscosity changes under shear, improving handling and application performance in various products.
Smart Images

Figure 0007552226000005 
Figure 0007552226000006 
Figure 0007552226000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion. Specifically, the present invention relates to a dispersion comprising fine fibrous cellulose and an organic solvent. [Background technology]
[0002] Conventionally, cellulose fibers have been widely used in clothing, absorbent articles, paper products, etc. As cellulose fibers, in addition to fibrous cellulose with a fiber diameter of 10 μm to 50 μm, fine fibrous cellulose with a fiber diameter of 1 μm or less is also known. Fine fibrous cellulose has attracted attention as a new material and has a wide range of applications. For example, the development of sheets, resin composites, and thickeners containing fine fibrous cellulose is underway.
[0003] Generally, fine fibrous cellulose is stably dispersed in aqueous solvents, and is therefore often provided in the form of an aqueous dispersion and used for various purposes. On the other hand, when fine fibrous cellulose is mixed with a resin component to produce a composite or the like, there is a demand for mixing the fine fibrous cellulose with an organic solvent. As a technology to meet such a demand, a technology for producing a fine fibrous cellulose-containing dispersion in which fine fibrous cellulose is dispersed in a dispersion medium containing an organic solvent has been studied (Patent Documents 1 to 4).
[0004] For example, Patent Documents 1 to 3 disclose a fine fibrous cellulose composite in which a surfactant is adsorbed to fine fibrous cellulose having a carboxyl group. These disclose a method of finely dispersing cellulose fibers in an aqueous solvent, aggregating the fine fibrous cellulose, and dispersing it in an organic solvent, and a method of obtaining fine fibrous cellulose by finely dispersing cellulose fibers in an organic solvent. Patent Document 4 discloses a spray composition containing hydrophobically modified cellulose fibers in which at least one modifying group selected from anionic groups and hydroxyl groups of cellulose fibers is bonded, and an organic medium. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-140738 A [Patent Document 2] JP 2016-188375 A [Patent Document 3] JP 2019-49091 A [Patent Document 4] JP 2020-76054 A Summary of the Invention [Problem to be solved by the invention]
[0006] Dispersions obtained by dispersing fine fibrous cellulose in an organic solvent have a wide range of applications. For example, in applications such as paints, the dispersions are sometimes required to have high thixotropy.
[0007] Therefore, in order to solve such problems of the conventional technology, the present inventors have carried out research with the aim of providing a dispersion liquid obtained by dispersing fine fibrous cellulose in an organic solvent, which dispersion liquid has high thixotropy. [Means for solving the problem]
[0008] As a result of intensive investigations aimed at solving the above problems, the present inventors have found that in a dispersion containing fine fibrous cellulose having a predetermined amount or more of anionic groups and an organic solvent, a highly thixotropic dispersion can be obtained by introducing an organic onium ion as a counter ion for the anionic groups of the fine fibrous cellulose and further adjusting the B-type viscosity measured under predetermined conditions to 50 Pa s or more. Specifically, the present invention has the following configuration.
[0009] [1] A dispersion containing fibrous cellulose having a fiber width of 1000 nm or less and an organic solvent, The fibrous cellulose has an anionic group, and the content of the anionic group is 0.50 mmol / g or more; The fibrous cellulose has an organic onium ion as a counter ion of the anionic group, A dispersion having a B-type viscosity of 50 Pa s or more, as measured by the following measurement method (A); Measurement method (A): The B-type viscosity is measured in accordance with JIS Z 8803 (2011) when the fibrous cellulose concentration of the dispersion is 3 mass % (w / w), the rotation speed is 0.6 rpm, and the temperature is 23°C. [2] The dispersion according to [1], having a light transmittance of 80% or more as measured by the following measurement method (B); Measurement method (B): The fibrous cellulose concentration of the dispersion was set to 3 mass % (w / w), and the dispersion was sealed in a quartz cell with an optical path length of 10 mm, and the light transmittance at a wavelength of 660 nm was measured using an ultraviolet-visible spectrophotometer. [3] The dispersion according to [1] or [2], wherein the fiber width of the fibrous cellulose is 10 nm or less. [4] The dispersion liquid according to any one of [1] to [3], wherein the anionic group is at least one selected from the group consisting of a phosphorus oxoacid group, a substituent derived from a phosphorus oxoacid group, a sulfur oxoacid group, and a substituent derived from a sulfur oxoacid group. Effect of the Invention
[0010] According to the present invention, it is possible to obtain a dispersion liquid having high thixotropy, which is prepared by dispersing fine fibrous cellulose in an organic solvent. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the relationship between the amount of NaOH dropped onto a slurry containing fibrous cellulose having phosphorus oxoacid groups and pH. [Diagram 2] FIG. 2 is a graph showing the relationship between the amount of NaOH dropped onto a slurry containing fibrous cellulose having a carboxy group and pH. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below. The following description of the components may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments.
[0013] (dispersion) The present invention relates to a dispersion containing fibrous cellulose having a fiber width of 1000 nm or less and an organic solvent. Here, the fibrous cellulose has an anionic group, and the content of the anionic group is 0.50 mmol / g or more. The fibrous cellulose also has an organic onium ion as a counter ion of the anionic group. The B-type viscosity of the dispersion measured by the following measurement method (A) is 50 Pa s or more. Measurement method (A): The B-type viscosity is measured in accordance with JIS Z 8803 (2011) when the fibrous cellulose concentration in the dispersion is 3 mass % (w / w), the rotation speed is 0.6 rpm, and the temperature is 23° C. The B-type viscosity of the dispersion is preferably the viscosity of a dispersion consisting of an organic solvent and fibrous cellulose.
[0014] The B-type viscosity of the dispersion of this embodiment measured by the above measurement method (A) may be 50 Pa·s or more, preferably 55 Pa·s or more, more preferably 60 Pa·s or more, even more preferably 70 Pa·s or more, even more preferably 80 Pa·s or more, even more preferably 90 Pa·s or more, and particularly preferably 100 Pa·s or more. The upper limit of the B-type viscosity of the dispersion measured by the above measurement method (A) is not particularly limited, but is preferably, for example, 500 Pa·s or less.
[0015] The dispersion of the present invention has the above-mentioned constitution, and therefore has high thixotropy. That is, the dispersion of the present invention has a property that the viscosity decreases when shear is applied. The thixotropy of the dispersion can be evaluated, for example, by the TI value calculated by the following formula. TI value = (viscosity value at 0.6 rpm / viscosity value at 60 rpm) Here, the viscosity value at 0.6 rpm is the Brookfield viscosity value when an organic solvent dispersion having a fibrous cellulose concentration of 3% by mass is left at rest for 24 hours at 23° C., and then rotated at 0.6 rpm for 3 minutes. The viscosity value at 60 rpm is the Brookfield viscosity value when an organic solvent dispersion having a fibrous cellulose concentration of 3% by mass is left at rest for 24 hours at 23° C., and then rotated at 60 rpm for 3 minutes. The Brookfield viscosity is measured using a Brookfield viscometer, and the Brookfield analog viscometer can be, for example, a Brookfield T-LVT viscometer.
[0016] The TI value of the dispersion calculated by the above method is preferably 20.0 or more, more preferably 30.0 or more, even more preferably 40.0 or more, and even more preferably 50.0 or more. The upper limit of the TI value of the dispersion is not particularly limited, but is preferably, for example, 500 or less.
[0017] In this embodiment, the light transmittance of the dispersion liquid measured by the following measurement method (B) is preferably 80% or more, more preferably 84% or more, even more preferably 88% or more, and particularly preferably 90% or more. Measurement method (B): The fibrous cellulose concentration of the dispersion is set to 3% by mass (w / w), and the dispersion is sealed in a quartz cell with an optical path length of 10 mm, and the light transmittance at a wavelength of 660 nm is measured using an ultraviolet-visible spectrometer. As the ultraviolet-visible spectrometer, for example, V-770 manufactured by JASCO Corporation can be used. The zero point measurement is performed using ion-exchanged water placed in the same glass cell.
[0018] (Organic solvent) The dispersion of the present invention contains an organic solvent. The dispersion of the present invention is a fine fibrous cellulose-containing dispersion in which fine fibrous cellulose, which will be described later, is dispersed in a dispersion medium containing an organic solvent. The dispersion of the present invention may further contain water in addition to the organic solvent as a dispersion medium, but the content of water relative to the total mass of the dispersion is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less. In this embodiment, it is preferable that the dispersion medium does not substantially contain water, and it is particularly preferable that the content of water relative to the total mass of the dispersion is 0% by mass.
[0019] The dielectric constant of the organic solvent of the dispersion at 25° C. is preferably not more than 60, and more preferably not more than 50. Since the fibrous cellulose contained in the dispersion can exhibit excellent dispersibility even in an organic solvent with a low dielectric constant, the dielectric constant of the organic solvent at 25° C. may be not more than 45, may be not more than 40, or may be not more than 35.
[0020] The Hansen solubility parameter (HSP) δd of the organic solvent is 5MPa. 1 / 2 More than 20MPa 1 / 2 It is preferable that the pressure is less than 10MPa. 1 / 2 More than 19MPa 1 / 2 It is preferable that Δh is 1 MPa or less. 1 / 2 More than 40MPa 1 / 2 It is preferable that the pressure is less than 2MPa. 1 / 2 More than 30MPa 1 / 2 It is more preferable that Δp is 0 MPa or less. 1 / 2 More than 4MPa 1 / 2 The range is as follows: δh is 0 MPa 1 / 2 More than 6MPa 1 / 2 It is also preferable that the following ranges are simultaneously satisfied.
[0021] Examples of organic solvents include methanol (dielectric constant 32.6), ethanol (dielectric constant 24.3), n-propyl alcohol (dielectric constant 20.1), isopropyl alcohol (IPA) (dielectric constant 18.62), 1-butanol (dielectric constant 18), m-cresol (dielectric constant 11.8), glycerin (dielectric constant 42.5), acetic acid (dielectric constant 6.15), pyridine (dielectric constant 12.3), tetrahydrofuran (THF) (dielectric constant 7.5), acetone (dielectric constant 20.7), methyl ethyl ketone (MEK) (dielectric constant 15.45), ethyl acetate ( Dielectric constant 6.4), aniline (dielectric constant 6.89), N-methyl-2-pyrrolidone (NMP) (dielectric constant 32.2), dimethyl sulfoxide (DMSO) (dielectric constant 45), N,N-dimethylformamide (DMF) (dielectric constant 38), hexane (dielectric constant 1.8), cyclohexane (dielectric constant 2.0), benzene (dielectric constant 2.3), toluene (dielectric constant 2.4), p-xylene (dielectric constant 2.3), styrene (dielectric constant 2.3 to 3.4), diethyl ether (dielectric constant 4.3), chloroform (dielectric constant 4.8), etc. can be mentioned. Among them, the organic solvent is preferably at least one selected from the group consisting of toluene, xylene, and styrene.
[0022] The content of the organic solvent is preferably 10% by mass or more, more preferably 50% by mass or more, based on the total mass of the solids contained in the dispersion, and is preferably 99.9% by mass or less, more preferably 99.0% by mass or less, and even more preferably 95.0% by mass or less, based on the total mass of the solids contained in the dispersion.
[0023] (Fine fibrous cellulose) The dispersion of the present invention contains fibrous cellulose having a fiber width of 1000 nm or less. The fiber width of the fibrous cellulose is preferably 100 nm or less, more preferably 50 nm or less, even more preferably 20 nm or less, even more preferably 10 nm or less, and particularly preferably 8 nm or less. In this specification, fibrous cellulose having a fiber width of 1000 nm or less is also referred to as fine fibrous cellulose.
[0024] The average fiber width of the fibrous cellulose is, for example, 1000 nm or less. The average fiber width of the fibrous cellulose is, for example, preferably 2 nm or more and 1000 nm or less, more preferably 2 nm or more and 100 nm or less, even more preferably 2 nm or more and 50 nm or less, and particularly preferably 2 nm or more and 10 nm or less. The fibrous cellulose is, for example, a single fiber cellulose.
[0025] The fiber width of fibrous cellulose is measured, for example, using an electron microscope as follows. First, an aqueous suspension of fibrous cellulose with a concentration of 0.05% by mass or more and 0.1% by mass or less is prepared, and this suspension is cast on a hydrophilically treated carbon film-coated grid to prepare a sample for TEM observation. When wide fibers are included, an SEM image of the surface cast on glass may be observed. Next, observation is performed using an electron microscope image at a magnification of 1000x, 5000x, 10000x, or 50000x depending on the width of the fiber to be observed. However, the sample, observation conditions, and magnification are adjusted to satisfy the following conditions.
[0026] (1) A straight line X is drawn at any point within the observed image, and 20 or more fibers intersect with the straight line X. (2) Within the same image, draw a line Y that intersects the line perpendicularly, and 20 or more fibers intersect the line Y.
[0027] For observation images that satisfy the above conditions, the width of the fibers that intersect with lines X and Y is visually read. In this manner, three or more sets of observation images of at least the surface portions that do not overlap each other are obtained. Next, for each image, the width of the fibers that intersect with lines X and Y is read. In this manner, the width of at least 20 fibers x 2 x 3 = 120 fibers is read. The average value of the read fiber widths is then determined as the average fiber width of the fibrous cellulose.
[0028] The fiber length of the fibrous cellulose is not particularly limited, but is preferably 0.1 μm or more and 1000 μm or less, more preferably 0.1 μm or more and 800 μm or less, and even more preferably 0.1 μm or more and 600 μm or less. By setting the fiber length within the above range, destruction of the crystalline region of the fibrous cellulose can be suppressed. In addition, it is also possible to set the slurry viscosity of the fibrous cellulose to an appropriate range. The fiber length of the fibrous cellulose can be determined by image analysis using, for example, TEM, SEM, or AFM.
[0029] The fibrous cellulose preferably has an I-type crystal structure. Here, the fact that the fibrous cellulose has an I-type crystal structure can be identified from a diffraction profile obtained from a wide-angle X-ray diffraction photograph using CuKα (λ=1.5418 Å) monochromatized with graphite. Specifically, it can be identified from the presence of typical peaks at two positions, around 2θ=14° to 17° and around 2θ=22° to 23°. The proportion of I-type crystal structure in the fine fibrous cellulose is, for example, preferably 30% or more, more preferably 40% or more, and even more preferably 50% or more. This can be expected to provide even more excellent performance in terms of heat resistance and low linear thermal expansion coefficient. The degree of crystallinity can be determined by measuring an X-ray diffraction profile and using the pattern in a conventional manner (Seagal et al., Textile Research Journal, Vol. 29, p. 786, 1959).
[0030] The axial ratio (fiber length / fiber width) of the fibrous cellulose is not particularly limited, but is preferably, for example, 20 to 10,000, and more preferably 50 to 1,000. By setting the axial ratio to the above lower limit or more, a sheet containing fine fibrous cellulose can be easily formed. In addition, by setting the axial ratio to the above upper limit or less, it is preferable in that, for example, when the fibrous cellulose is treated as a dispersion liquid, handling such as dilution is facilitated.
[0031] Fibrous cellulose has, for example, both crystalline and non-crystalline regions. Fine fibrous cellulose having both crystalline and non-crystalline regions and having an axial ratio within the above range can be realized by the method for producing fine fibrous cellulose described below.
[0032] The fibrous cellulose has an anionic group. Examples of the anionic group include a phosphorus oxoacid group or a substituent derived from a phosphorus oxoacid group (sometimes simply referred to as a phosphorus oxoacid group), a carboxy group or a substituent derived from a carboxy group (sometimes simply referred to as a carboxy group), and a sulfur oxoacid group or a substituent derived from a sulfur oxoacid group (sometimes simply referred to as a sulfur oxoacid group). Among them, the anionic group is preferably at least one selected from the group consisting of a phosphorus oxoacid group, a substituent derived from a phosphorus oxoacid group, a sulfur oxoacid group, and a substituent derived from a sulfur oxoacid group. When the anionic group is at least one selected from the group consisting of a phosphorus oxoacid group, a substituent derived from a phosphorus oxoacid group, a sulfur oxoacid group, and a substituent derived from a sulfur oxoacid group, a dispersion liquid having higher transparency and higher viscosity is more easily obtained.
[0033] The phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group is, for example, a substituent represented by the following formula (1). A plurality of types of the substituent represented by the following formula (1) may be introduced into each fibrous cellulose. In this case, the plurality of introduced substituents represented by the following formula (1) may be the same or different.
[0034] [ka]
[0035] In formula (1), a, b, and n are natural numbers, and m is an arbitrary number (where a=b×m). At least one of the n α and α' is O. - and the rest are R or OR. Note that all of α and α' are O - The n α's may all be the same or may be different. b+ is a cation of one or more valences consisting of organic or inorganic substances.
[0036] Each R is a hydrogen atom, a saturated linear hydrocarbon group, a saturated branched hydrocarbon group, a saturated cyclic hydrocarbon group, an unsaturated linear hydrocarbon group, an unsaturated branched hydrocarbon group, an unsaturated cyclic hydrocarbon group, an aromatic group, or a group derived therefrom. In formula (1), n is preferably 1.
[0037] Examples of saturated linear hydrocarbon groups include, but are not limited to, methyl, ethyl, n-propyl, or n-butyl groups. Examples of saturated branched hydrocarbon groups include, but are not limited to, i-propyl or t-butyl groups. Examples of saturated cyclic hydrocarbon groups include, but are not limited to, cyclopentyl or cyclohexyl groups. Examples of unsaturated linear hydrocarbon groups include, but are not limited to, vinyl or allyl groups. Examples of unsaturated branched hydrocarbon groups include, but are not limited to, i-propenyl or 3-butenyl groups. Examples of unsaturated cyclic hydrocarbon groups include, but are not limited to, cyclopentenyl or cyclohexenyl groups. Examples of aromatic groups include, but are not limited to, phenyl or naphthyl groups.
[0038] In addition, the derivative group in R is a carboxy group, a carboxylate group (-COO -), a functional group in which at least one selected from functional groups such as a hydroxyl group, an amino group, and an ammonium group is added or substituted, but is not particularly limited. The number of carbon atoms constituting the main chain of R is not particularly limited, but is preferably 20 or less, and more preferably 10 or less. By setting the number of carbon atoms constituting the main chain of R within the above range, the molecular weight of the phosphorus oxoacid group can be set to an appropriate range, which facilitates penetration into the fiber raw material and increases the yield of fine cellulose fibers. Note that when there are multiple Rs in formula (1) or when multiple types of substituents represented by the above formula (1) are introduced into the fibrous cellulose, the multiple Rs may be the same or different.
[0039] β b+ is a monovalent or higher cation made of an organic or inorganic substance. An example of the monovalent or higher cation made of an organic substance is an organic onium ion. An example of the organic onium ion is an organic ammonium ion or an organic onium ion. An example of the organic ammonium ion is an aliphatic ammonium ion or an aromatic ammonium ion, and an example of the organic onium ion is an aliphatic phosphonium ion or an aromatic phosphonium ion. An example of the monovalent or higher cation made of an inorganic substance is an ion of an alkali metal such as sodium, potassium, or lithium, an ion of a divalent metal such as calcium or magnesium, a hydrogen ion, an ammonium ion, or the like. In addition, in formula (1), β b+ When a plurality of substituents represented by the above formula (1) are present or when a plurality of substituents represented by the above formula (1) are introduced into the fibrous cellulose, the plurality of β b+ may be the same or different. The organic or inorganic cations of monovalent or higher are β b+ Sodium or potassium ions are preferred because they are less likely to yellow when the fiber raw material containing the cation is heated and are easy to use industrially, but there is no particular limitation.
[0040] More specifically, examples of the phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group include a phosphoric acid group (-PO3H2), a salt of a phosphoric acid group, a phosphorous acid group (phosphonic acid group) (-PO2H2), and a salt of a phosphorous acid group (phosphonic acid group). In addition, the phosphorus oxoacid group or the substituent derived from the phosphorus oxoacid group may be a group in which a phosphoric acid group is condensed (e.g., a pyrophosphate group), a group in which a phosphonic acid is condensed (e.g., a polyphosphonic acid group), a phosphoric ester group (e.g., a monomethyl phosphate group, a polyoxyethylene alkyl phosphate group), an alkyl phosphonic acid group (e.g., a methyl phosphonic acid group), and the like.
[0041] The sulfur oxoacid group (sulfur oxoacid group or a substituent derived from a sulfur oxoacid group) is, for example, a substituent represented by the following formula (2). A plurality of substituents represented by the following formula (2) may be introduced into each fibrous cellulose. In this case, the plurality of introduced substituents represented by the following formula (2) may be the same or different.
[0042] [ka]
[0043] In the above structural formula, b and n are natural numbers, p is 0 or 1, and m is an arbitrary number (where 1=b×m). When n is 2 or more, the multiple p's may be the same or different. In the above structural formula, β b+is a monovalent or higher cation made of an organic or inorganic substance. An example of the monovalent or higher cation made of an organic substance is an organic onium ion. An example of the organic onium ion is an organic ammonium ion or an organic onium ion. An example of the organic ammonium ion is an aliphatic ammonium ion or an aromatic ammonium ion, and an example of the organic onium ion is an aliphatic phosphonium ion or an aromatic phosphonium ion. An example of the monovalent or higher cation made of an inorganic substance is an ion of an alkali metal such as sodium, potassium, or lithium, an ion of a divalent metal such as calcium or magnesium, a hydrogen ion, an ammonium ion, or the like. When multiple types of substituents represented by the above formula (2) are introduced into the fibrous cellulose, the multiple β b+ may be the same or different. The organic or inorganic cations of monovalent or higher are β b+ Sodium or potassium ions are preferred because they are less likely to yellow when the fiber raw material containing the cation is heated and are easy to use industrially, but there is no particular limitation.
[0044] The content (amount introduced) of the anionic group may be, for example, 0.50 mmol / g or more per 1 g (mass) of fibrous cellulose, more preferably 0.60 mmol / g or more, even more preferably 0.80 mmol / g or more, and particularly preferably 1.00 mmol / g or more. The content (amount introduced) of the anionic group is, for example, preferably 5.20 mmol / g or less per 1 g (mass) of fibrous cellulose, more preferably 3.65 mmol / g or less, even more preferably 3.00 mmol / g or less, even more preferably 2.50 mmol / g or less, and particularly preferably 2.00 mmol / g or less. Here, the denominator in the unit mmol / g is calculated based on the fact that the counter ion of the anionic group is a hydrogen ion (H +By setting the amount of anionic groups introduced within the above range, the content of organic onium ions that the fibrous cellulose can contain can be set within an appropriate range, thereby more effectively increasing the dispersibility of the fibrous cellulose in organic solvents.
[0045] The amount of anionic groups introduced into the fibrous cellulose can be measured, for example, by neutralization titration. In the measurement by neutralization titration, an alkali such as an aqueous sodium hydroxide solution is added to the obtained slurry containing the fibrous cellulose, and the amount introduced is measured by determining the change in pH.
[0046] 1 is a graph showing the relationship between the amount of NaOH dropped onto a slurry containing fibrous cellulose having phosphorus oxo acid groups and pH. The amount of phosphorus oxo acid groups introduced into the fibrous cellulose is measured, for example, as follows. First, a slurry containing fibrous cellulose is treated with a strongly acidic ion exchange resin. If necessary, the measurement target may be subjected to a defibration treatment similar to the defibration treatment step described below prior to the treatment with the strongly acidic ion exchange resin. Next, the change in pH is observed while adding the aqueous sodium hydroxide solution, and a titration curve such as that shown in the upper part of Figure 1 is obtained. In the titration curve shown in the upper part of Figure 1, the measured pH is plotted against the amount of alkali added, and in the titration curve shown in the lower part of Figure 1, the increment (derivative value) of pH (1 / mmol) against the amount of alkali added is plotted. In this neutralization titration, two points are confirmed in the curve plotting the measured pH against the amount of alkali added, where the increment (derivative value of pH against the amount of alkali added) is maximum. Of these, the first maximum point of the increment obtained after starting to add the alkali is called the first endpoint, and the next maximum point of the increment is called the second endpoint. The amount of alkali required from the start of titration to the first end point is equal to the amount of the first dissociated acid of the fibrous cellulose contained in the slurry used for titration, the amount of alkali required from the first end point to the second end point is equal to the amount of the second dissociated acid of the fibrous cellulose contained in the slurry used for titration, and the amount of alkali required from the start of titration to the second end point is equal to the total amount of dissociated acid of the fibrous cellulose contained in the slurry used for titration. The value obtained by dividing the amount of alkali required from the start of titration to the first end point by the solid content (g) in the slurry to be titrated is the amount of phosphorus oxo acid group introduced (mmol / g). Note that when simply referring to the amount of phosphorus oxo acid group introduced (or the amount of phosphorus oxo acid group), it refers to the amount of the first dissociated acid. In FIG. 1, the region from the start of titration to the first end point is called the first region, and the region from the first end point to the second end point is called the second region. For example, when the phosphorus oxoacid group is a phosphate group and this phosphate group undergoes condensation, the amount of weak acid groups in the phosphorus oxoacid group (also referred to as the second dissociated acid amount in this specification) appears to decrease, and the amount of alkali required in the second region becomes smaller than the amount of alkali required in the first region. On the other hand, the amount of strong acid groups in the phosphorus oxoacid group (also referred to as the first dissociated acid amount in this specification) is equal to the amount of phosphorus atoms regardless of the presence or absence of condensation. In addition, when the phosphorus oxoacid group is a phosphorous acid group, the phosphorus oxoacid group no longer has weak acid groups, so the amount of alkali required in the second region becomes smaller or may become zero. In this case, there is only one point on the titration curve where the pH increment is maximum.
[0047] The above-mentioned amount of phosphorus oxoacid groups introduced (mmol / g) indicates the amount of phosphorus oxoacid groups possessed by the acid-type fibrous cellulose (hereinafter referred to as the amount of phosphorus oxoacid groups (acid type)), since the denominator indicates the mass of the acid-type fibrous cellulose. On the other hand, when the counter ion of the phosphorus oxoacid group is replaced with an arbitrary cation C so as to be the charge equivalent, the amount of phosphorus oxoacid groups possessed by the fibrous cellulose in which the cation C is the counter ion (hereinafter referred to as the amount of phosphorus oxoacid groups (C type)) can be obtained by converting the denominator to the mass of the fibrous cellulose when the cation C is the counter ion. That is, it is calculated according to the following formula. Amount of phosphorus oxoacid group (C type) = Amount of phosphorus oxoacid group (acid type) / {1+(W-1)×A / 1000} A [mmol / g]: total amount of anions derived from phosphorus oxoacid groups in fibrous cellulose (total amount of dissociated acid from phosphorus oxoacid groups) W: Formula weight per valence of cation C (e.g., Na is 23, Al is 9)
[0048] 2 is a graph showing the relationship between the amount of NaOH dropped onto a dispersion containing fibrous cellulose having a carboxy group as an anionic group and pH. The amount of carboxy groups introduced into the fibrous cellulose is measured, for example, as follows. First, a dispersion liquid containing fibrous cellulose is treated with a strongly acidic ion exchange resin. If necessary, a defibration treatment similar to the defibration treatment step described below may be performed on the measurement target prior to the treatment with the strongly acidic ion exchange resin. Next, the change in pH is observed while adding the aqueous sodium hydroxide solution, and a titration curve as shown in the upper part of FIG. 2 is obtained. In the titration curve shown in the upper part of FIG. 2, the measured pH is plotted against the amount of added alkali, and in the titration curve shown in the lower part of FIG. 2, the increment (differential value) (1 / mmol) of pH against the amount of added alkali is plotted. In this neutralization titration, one point where the increment (differential value of pH against the amount of added alkali) is maximum is confirmed in the curve plotting the measured pH against the amount of added alkali, and this maximum point is called the first end point. Here, the region from the start of titration to the first end point in FIG. 2 is called the first region. The amount of alkali required in the first region is equal to the amount of carboxyl groups in the dispersion used for titration. The amount of alkali required in the first region of the titration curve (mmol) is divided by the solid content (g) in the dispersion containing the fibrous cellulose to be titrated to calculate the amount of carboxyl groups introduced (mmol / g).
[0049] The above-mentioned amount of carboxyl groups introduced (mmol / g) indicates the amount of carboxyl groups in the acid-type fibrous cellulose (hereinafter referred to as the amount of carboxyl groups (acid type)) since the denominator is the mass of the acid-type fibrous cellulose. On the other hand, when the counter ion of the carboxyl group is replaced with any cation C so as to be the charge equivalent, the amount of carboxyl groups in the fibrous cellulose in which the cation C is the counter ion (hereinafter referred to as the amount of carboxyl groups (C type)) can be obtained by converting the denominator to the mass of the fibrous cellulose when the cation C is the counter ion. That is, it is calculated by the following formula. Carboxylic acid amount (C type) = Carboxylic acid amount (acid type) / {1 + (W-1) x (Carboxylic acid amount (acid type)) / 1000} W: Formula weight per valence of cation C (e.g., Na is 23, Al is 9)
[0050] In the measurement of the amount of anionic groups by titration, if the amount of sodium hydroxide solution dropped is too large or the titration interval is too short, the amount of anionic groups may be lower than the actual amount, and an accurate value may not be obtained. As an appropriate amount of drop and titration interval, for example, it is preferable to titrate 10 to 50 μL of 0.1N sodium hydroxide solution every 5 to 30 seconds. In addition, in order to eliminate the influence of carbon dioxide dissolved in the fibrous cellulose-containing slurry, it is preferable to measure while blowing an inert gas such as nitrogen gas into the slurry from 15 minutes before the start of titration until the end of titration.
[0051] The amount of sulfur oxoacid groups introduced into fibrous cellulose can be calculated by freeze-drying a slurry containing fibrous cellulose, pulverizing the slurry, and measuring the amount of sulfur in the resulting pulverized sample. Specifically, a slurry containing fibrous cellulose is freeze-dried, and the resulting pulverized sample is subjected to pressurized heating decomposition using nitric acid in a closed container, and then appropriately diluted and the amount of sulfur is measured by ICP-OES. The amount of sulfur oxoacid groups (unit: mmol / g) of fine fibrous cellulose is calculated by dividing the value by the bone dry mass of the fibrous cellulose used.
[0052] (Method of producing fine fibrous cellulose) <Textile raw materials> Fine fibrous cellulose is produced from a fiber raw material containing cellulose. The fiber raw material containing cellulose is not particularly limited, but it is preferable to use pulp because it is easily available and inexpensive. Examples of pulp include wood pulp, non-wood pulp, and deinked pulp. Examples of wood pulp include, but are not particularly limited to, chemical pulp such as hardwood kraft pulp (LBKP), softwood kraft pulp (NBKP), sulfite pulp (SP), dissolving pulp (DP), soda pulp (AP), unbleached kraft pulp (UKP), and oxygen bleached kraft pulp (OKP), semi-chemical pulp such as semi-chemical pulp (SCP) and chemi-ground wood pulp (CGP), and mechanical pulp such as groundwood pulp (GP) and thermomechanical pulp (TMP, BCTMP). Examples of non-wood pulp include, but are not particularly limited to, cotton-based pulp such as cotton linters and cotton lint, and non-wood-based pulp such as hemp, wheat straw, and bagasse. The deinked pulp is not particularly limited, and may be deinked pulp made from waste paper. The pulp of this embodiment may be one of the above, or a mixture of two or more. Among the above pulps, wood pulp and deinked pulp are preferable from the viewpoint of availability. Among wood pulps, chemical pulp is more preferable, and kraft pulp and sulfite pulp are even more preferable, from the viewpoint of a high cellulose ratio and a high yield of fine fibrous cellulose during defibration treatment, and of small decomposition of cellulose in the pulp and of obtaining long-fiber fine fibrous cellulose with a large axial ratio. The viscosity tends to be high when long-fiber fine fibrous cellulose with a large axial ratio is used.
[0053] As the fiber raw material containing cellulose, for example, cellulose contained in sea squirts and bacterial cellulose produced by acetic acid bacteria can be used. Also, instead of the fiber raw material containing cellulose, fibers formed from linear nitrogen-containing polysaccharide polymers such as chitin and chitosan can be used.
[0054] <Phosphorus oxo acid group introduction step> The manufacturing process of fine fibrous cellulose includes an anionic group introduction step. An example of the anionic group introduction step is a phosphorus oxoacid group introduction step. The phosphorus oxoacid group introduction step is a step of reacting at least one compound (hereinafter also referred to as "compound A") selected from compounds capable of introducing phosphorus oxoacid groups by reacting with hydroxyl groups possessed by a fiber raw material containing cellulose with the fiber raw material containing cellulose. This step results in the production of fibers into which phosphorus oxoacid groups have been introduced.
[0055] In the phosphorus oxoacid group introduction step according to this embodiment, the reaction of the cellulose-containing fiber raw material with compound A may be carried out in the presence of at least one selected from urea and its derivatives (hereinafter also referred to as "compound B"). Alternatively, the reaction of the cellulose-containing fiber raw material with compound A may be carried out in the absence of compound B.
[0056] An example of a method for acting compound A on a fiber raw material in the presence of compound B includes a method of mixing compound A and compound B with a fiber raw material in a dry state, a wet state, or a slurry state. Of these, it is preferable to use a fiber raw material in a dry state or a wet state, and it is particularly preferable to use a fiber raw material in a dry state, since the reaction is highly uniform. The form of the fiber raw material is not particularly limited, but it is preferable to use, for example, a cotton-like or thin sheet-like form. Compound A and compound B can be added to the fiber raw material in a powder form, a solution form dissolved in a solvent, or a melted state by heating to a melting point or higher. Of these, it is preferable to add them in a solution form dissolved in a solvent, especially in an aqueous solution form, since the reaction is highly uniform. In addition, compound A and compound B may be added to the fiber raw material simultaneously, separately, or as a mixture. The method of adding compound A and compound B is not particularly limited, but when compound A and compound B are in a solution state, the fiber raw material may be immersed in the solution to absorb the liquid and then removed, or the solution may be dropped onto the fiber raw material. In addition, the required amounts of compound A and compound B may be added to the fiber raw material, or excess amounts of compound A and compound B may be added to the fiber raw material, respectively, and then the excess compound A and compound B may be removed by squeezing or filtration.
[0057] The compound A used in this embodiment may be any compound having a phosphorus atom and capable of forming an ester bond with cellulose, and may include, but is not limited to, phosphoric acid or a salt thereof, phosphorous acid or a salt thereof, dehydrated condensed phosphoric acid or a salt thereof, and anhydrous phosphoric acid (diphosphorus pentoxide). Phosphoric acid may be used with various purities, for example, 100% phosphoric acid (orthophosphoric acid) or 85% phosphoric acid. Phosphorous acid may be 99% phosphorous acid (phosphonic acid). Dehydrated condensed phosphoric acid is a phosphoric acid in which two or more molecules are condensed by a dehydration reaction, and examples of the phosphoric acid include pyrophosphoric acid and polyphosphoric acid. Phosphates, phosphites, and dehydrated condensed phosphates include lithium salts, sodium salts, potassium salts, and ammonium salts of phosphoric acid, phosphorous acid, or dehydrated condensed phosphoric acid, and these may be neutralized to various degrees. Among these, from the viewpoints of high efficiency of introduction of phosphorus oxoacid groups, easier improvement of defibration efficiency in the defibration step described below, low cost, and ease of industrial application, phosphoric acid, sodium salt of phosphoric acid, potassium salt of phosphoric acid, ammonium salt of phosphoric acid, or phosphorous acid, sodium salt of phosphorous acid, potassium salt of phosphorous acid, or ammonium salt of phosphorous acid are preferred, and phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, ammonium dihydrogen phosphate, or phosphorous acid, sodium phosphite are more preferred.
[0058] The amount of compound A added to the fiber raw material is not particularly limited, but for example, when the amount of compound A added is converted into the amount of phosphorus atoms, the amount of phosphorus atoms added to the fiber raw material (bone dry mass) is preferably 0.5% by mass or more and 100% by mass or less, more preferably 1% by mass or more and 50% by mass or less, and even more preferably 2% by mass or more and 30% by mass or less. By setting the amount of phosphorus atoms added to the fiber raw material within the above range, the yield of fine fibrous cellulose can be further improved. On the other hand, by setting the amount of phosphorus atoms added to the fiber raw material to the above upper limit or less, a balance between the effect of improving the yield and the cost can be achieved.
[0059] As described above, the compound B used in this embodiment is at least one selected from urea and its derivatives. Examples of the compound B include urea, biuret, 1-phenylurea, 1-benzylurea, 1-methylurea, and 1-ethylurea. From the viewpoint of improving the uniformity of the reaction, it is preferable to use an aqueous solution of compound B. Also, from the viewpoint of further improving the uniformity of the reaction, it is preferable to use an aqueous solution in which both compound A and compound B are dissolved.
[0060] The amount of compound B added relative to the fiber raw material (bone dry mass) is not particularly limited, but is preferably, for example, 1 mass% or more and 500 mass% or less, more preferably 10 mass% or more and 400 mass% or less, and even more preferably 100 mass% or more and 350 mass% or less.
[0061] In the reaction of a fiber raw material containing cellulose with compound A, in addition to compound B, for example, amides or amines may be included in the reaction system. Examples of amides include formamide, dimethylformamide, acetamide, and dimethylacetamide. Examples of amines include methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, triethylamine in particular is known to act as a good reaction catalyst.
[0062] In the phosphorus oxo acid group introduction step, it is preferable to add or mix the compound A or the like to the fiber raw material, and then heat-treat the fiber raw material. It is preferable to select a temperature for the heat treatment that can efficiently introduce the phosphorus oxo acid group while suppressing thermal decomposition and hydrolysis of the fiber. The heat treatment temperature is, for example, preferably 50°C to 300°C, more preferably 100°C to 250°C, and even more preferably 130°C to 200°C. In addition, for the heat treatment, various devices having a heat medium can be used, such as a hot air dryer, a stirring dryer, a rotary dryer, a disk dryer, a roll-type heater, a plate-type heater, a fluidized bed dryer, a band-type dryer, a filtration dryer, a vibration fluidized dryer, an airflow dryer, a reduced pressure dryer, an infrared heater, a far-infrared heater, a microwave heater, or a high-frequency dryer.
[0063] In the heat treatment according to the present embodiment, for example, a method of adding compound A to a thin sheet-like fiber raw material by a method such as impregnation, followed by heating, or a method of heating while kneading or stirring the fiber raw material and compound A in a kneader or the like, can be adopted. This makes it possible to suppress unevenness in the concentration of compound A in the fiber raw material and introduce phosphorus oxoacid groups more uniformly onto the surface of the cellulose fibers contained in the fiber raw material. This is believed to be due to the fact that when water molecules move to the surface of the fiber raw material as it dries, the dissolved compound A is attracted to the water molecules by surface tension and similarly moves to the surface of the fiber raw material (i.e., unevenness in the concentration of compound A is caused).
[0064] In addition, the heating device used in the heat treatment is preferably a device that can constantly discharge, for example, the moisture held by the slurry and the moisture generated by the dehydration condensation (phosphorylation) reaction between compound A and hydroxyl groups contained in cellulose or the like in the fiber raw material, outside the device system. Examples of such heating devices include ovens that use a blowing system. By constantly discharging the moisture within the device system, it is possible to suppress the hydrolysis reaction of phosphate ester bonds, which is the reverse reaction of phosphate esterification, and also to suppress acid hydrolysis of the sugar chains in the fibers. This makes it possible to obtain fine fibrous cellulose with a high axial ratio.
[0065] The time for the heat treatment is, for example, preferably from 1 second to 300 minutes after the moisture is substantially removed from the fiber raw material, more preferably from 1 second to 1000 seconds, and even more preferably from 10 seconds to 800 seconds. In this embodiment, the introduction amount of phosphorus oxo acid groups can be kept within a preferred range by setting the heating temperature and heating time within appropriate ranges.
[0066] The phosphorus oxo acid group introduction step may be carried out at least once, but may also be carried out twice or more. By carrying out the phosphorus oxo acid group introduction step twice or more, a large number of phosphorus oxo acid groups can be introduced into the fiber raw material.
[0067] The amount of phosphorus oxo acid groups introduced into the fiber raw material may be, for example, 0.50 mmol / g or more per 1 g (mass) of the fiber raw material, more preferably 0.60 mmol / g or more, even more preferably 0.80 mmol / g or more, and particularly preferably 1.00 mmol / g or more. The content (amount introduced) of phosphorus oxo acid groups is, for example, preferably 5.20 mmol / g or less per 1 g (mass) of fibrous cellulose, more preferably 3.65 mmol / g or less, even more preferably 3.00 mmol / g or less, even more preferably 2.50 mmol / g or less, and particularly preferably 2.00 mmol / g or less. By setting the amount of phosphorus oxo acid groups introduced within the above range, the content of organic onium ions that may be contained in the fibrous cellulose can be set to an appropriate range, and thus the dispersibility of the fibrous cellulose in organic solvents can be more effectively improved.
[0068] <Carboxy group introduction step> The process for producing fine fibrous cellulose may include, for example, a carboxyl group introduction step as an anionic group introduction step. The carboxyl group introduction step is carried out by subjecting a fiber raw material containing cellulose to an oxidation treatment such as ozone oxidation, oxidation by the Fenton method, or TEMPO oxidation treatment, or treating the raw material with a compound having a carboxylic acid-derived group or a derivative thereof, or an acid anhydride of a compound having a carboxylic acid-derived group or a derivative thereof.
[0069] Examples of compounds having a group derived from a carboxylic acid include, but are not limited to, dicarboxylic acid compounds such as maleic acid, succinic acid, phthalic acid, fumaric acid, glutaric acid, adipic acid, and itaconic acid, and tricarboxylic acid compounds such as citric acid and aconitic acid. Examples of derivatives of compounds having a group derived from a carboxylic acid include, but are not limited to, imidized products of acid anhydrides of compounds having a carboxy group, and derivatives of acid anhydrides of compounds having a carboxy group. Examples of imidized products of acid anhydrides of compounds having a carboxy group include, but are not limited to, imidized products of dicarboxylic acid compounds such as maleimide, succinimide, and phthalimide.
[0070] The acid anhydride of a compound having a group derived from a carboxylic acid is not particularly limited, but examples thereof include acid anhydrides of dicarboxylic acid compounds such as maleic anhydride, succinic anhydride, phthalic anhydride, glutaric anhydride, adipic anhydride, itaconic anhydride, etc. Furthermore, the derivative of an acid anhydride of a compound having a group derived from a carboxylic acid is not particularly limited, but examples thereof include acid anhydrides of compounds having a carboxy group such as dimethylmaleic anhydride, diethylmaleic anhydride, diphenylmaleic anhydride, etc., in which at least a part of the hydrogen atoms is substituted with a substituent such as an alkyl group or a phenyl group.
[0071] When the TEMPO oxidation treatment is performed in the carboxyl group introduction step, it is preferable to perform the treatment under conditions of pH 6 or more and 8 or less. Such a treatment is also called neutral TEMPO oxidation treatment. The neutral TEMPO oxidation treatment can be performed, for example, by adding pulp as a fiber raw material, a nitroxy radical such as TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl) as a catalyst, and sodium hypochlorite as a sacrificial reagent to a sodium phosphate buffer solution (pH = 6.8). By further adding sodium chlorite, the aldehyde generated in the oxidation process can be efficiently oxidized to a carboxyl group. The TEMPO oxidation treatment may also be performed under conditions of pH 10 or more and 11 or less. Such a treatment is also called alkaline TEMPO oxidation treatment. The alkaline TEMPO oxidation treatment can be performed, for example, by adding a nitroxy radical such as TEMPO as a catalyst, sodium bromide as a co-catalyst, and sodium hypochlorite as an oxidizing agent to pulp as a fiber raw material.
[0072] The amount of carboxyl groups introduced into the fiber raw material varies depending on the type of the substituent. For example, when the carboxyl groups are introduced by TEMPO oxidation, the amount is 0.50 mmol / g or more per 1 g (mass) of the fiber raw material, more preferably 0.60 mmol / g or more, even more preferably 0.80 mmol / g or more, and particularly preferably 1.00 mmol / g or more. The amount of carboxyl groups introduced into the fibrous cellulose is preferably 3.65 mmol / g or less, more preferably 3.00 mmol / g or less, even more preferably 2.50 mmol / g or less, and even more preferably 2.00 mmol / g or less. In addition, when the substituent is a carboxymethyl group, the amount of carboxyl groups introduced may be 5.8 mmol / g or less per 1 g (mass) of the fine fibrous cellulose. By setting the amount of carboxyl groups introduced within the above range, the content of organic onium ions that the fine fibrous cellulose may contain can be set to an appropriate range, and the dispersibility of the fibrous cellulose in an organic solvent can be more effectively improved.
[0073] <Sulfur oxoacid group introduction step> The process for producing fine fibrous cellulose may include, for example, a sulfur oxoacid group introduction step as an anionic group introduction step, in which hydroxyl groups in a fiber raw material containing cellulose react with sulfur oxoacid to obtain cellulose fibers having sulfur oxoacid groups (sulfur oxoacid group-introduced fibers).
[0074] In the sulfur oxo acid group introduction step, instead of compound A in the above-mentioned <phosphorus oxo acid group introduction step>, at least one compound (hereinafter also referred to as "compound C") selected from compounds capable of introducing sulfur oxo acid groups by reacting with hydroxyl groups of fiber raw materials containing cellulose is used. Compound C may be any compound having a sulfur atom and capable of forming an ester bond with cellulose, and may include, but is not limited to, sulfuric acid or a salt thereof, sulfurous acid or a salt thereof, and sulfuric acid amide. As sulfuric acid, sulfuric acid of various purities may be used, for example, 96% sulfuric acid (concentrated sulfuric acid). As sulfurous acid, 5% sulfurous acid water may be used. As sulfates or sulfites, lithium salts, sodium salts, potassium salts, ammonium salts of sulfates or sulfites may be used, and these may have various degrees of neutralization. As sulfuric acid amides, sulfamic acid or the like may be used. In the sulfur oxo acid group introduction step, it is preferable to use compound B in the above-mentioned <phosphorus oxo acid group introduction step> in the same manner.
[0075] In the sulfur oxoacid group introduction step, it is preferable to mix the cellulose raw material with an aqueous solution containing sulfur oxoacid and urea and / or a urea derivative, and then heat-treat the cellulose raw material. It is preferable to select a heat-treatment temperature that allows efficient introduction of sulfur oxoacid groups while suppressing thermal decomposition and hydrolysis of the fibers. The heat-treatment temperature is preferably 100°C or higher, more preferably 120°C or higher, and even more preferably 150°C or higher. The heat-treatment temperature is preferably 300°C or lower, more preferably 250°C or lower, and even more preferably 200°C or lower.
[0076] In the heat treatment step, it is preferable to heat until substantially no moisture is present. For this reason, the heat treatment time varies depending on the amount of moisture contained in the cellulose raw material and the amount of the aqueous solution containing sulfur oxoacid and urea and / or a urea derivative added, but is preferably, for example, 10 seconds or more and 10,000 seconds or less. For the heat treatment, various devices having a heat medium can be used, such as a hot air dryer, a stirring dryer, a rotary dryer, a disk dryer, a roll type heater, a plate type heater, a fluidized bed dryer, a band type dryer, a filtration dryer, a vibration fluidized dryer, an airflow dryer, a reduced pressure dryer, an infrared heater, a far infrared heater, a microwave heater, and a high frequency dryer.
[0077] The amount of sulfur oxoacid groups introduced into the cellulose raw material may be 0.50 mmol / g or more per 1 g (mass) of fibrous cellulose, more preferably 0.60 mmol / g or more, even more preferably 0.80 mmol / g or more, and particularly preferably 1.00 mmol / g or more. The amount of sulfur oxoacid groups introduced is preferably 5.00 mmol / g or less per 1 g (mass) of fibrous cellulose, more preferably 3.00 mmol / g or less. By setting the amount of sulfur oxoacid groups introduced within the above range, the content of organic onium ions that can be contained in the fine fibrous cellulose can be set to an appropriate range, and thus the dispersibility of the fibrous cellulose in organic solvents can be more effectively improved.
[0078] <Cleaning process> In the method for producing fine fibrous cellulose in this embodiment, a washing step can be carried out on the anionic group-introduced fiber as necessary. The washing step is carried out, for example, by washing the anionic group-introduced fiber with water or an organic solvent. The washing step may be carried out after each step described below, and the number of washing steps carried out in each washing step is not particularly limited.
[0079] <Alkaline treatment process> When producing fine fibrous cellulose, an alkali treatment may be performed on the fiber raw material between the anionic group introduction step and the defibration step described below. The alkali treatment method is not particularly limited, but may be, for example, a method of immersing the anionic group-introduced fiber in an alkali solution.
[0080] The alkaline compound contained in the alkaline solution is not particularly limited, and may be an inorganic alkaline compound or an organic alkaline compound. In this embodiment, it is preferable to use, for example, sodium hydroxide or potassium hydroxide as the alkaline compound because of its high versatility. The solvent contained in the alkaline solution may be either water or an organic solvent. Among them, the solvent contained in the alkaline solution is preferably a polar solvent including water or a polar organic solvent exemplified by alcohol, and more preferably an aqueous solvent including at least water. As the alkaline solution, for example, an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution is preferable because of its high versatility.
[0081] The temperature of the alkaline solution in the alkaline treatment step is not particularly limited, but is preferably, for example, from 5° C. to 80° C., and more preferably from 10° C. to 60° C. The time for immersing the anionic group-introduced fiber in the alkaline solution in the alkaline treatment step is not particularly limited, but is, for example, preferably from 5 minutes to 30 minutes, and more preferably from 10 minutes to 20 minutes. The amount of the alkaline solution used in the alkaline treatment is not particularly limited, but is, for example, preferably from 100 mass% to 100,000 mass%, and more preferably from 1,000 mass% to 10,000 mass%, based on the absolute dry mass of the anionic group-introduced fiber.
[0082] In order to reduce the amount of alkaline solution used in the alkaline treatment step, the anionic group-introduced fiber may be washed with water or an organic solvent after the anionic group-introducing step and before the alkaline treatment step. From the viewpoint of improving handleability, it is preferable to wash the alkaline-treated anionic group-introduced fiber with water or an organic solvent after the alkaline treatment step and before the defibration treatment step.
[0083] <Acid treatment process> When producing fine fibrous cellulose, the fiber raw material may be subjected to an acid treatment between the step of introducing anionic groups and the defibration treatment step described below. For example, the anionic group introduction step, acid treatment, alkali treatment, and defibration treatment may be performed in this order.
[0084] The method of acid treatment is not particularly limited, but may be, for example, a method of immersing the fiber raw material in an acidic solution containing an acid. The concentration of the acidic solution used is not particularly limited, but is preferably, for example, 10% by mass or less, and more preferably, 5% by mass or less. The pH of the acidic solution used is not particularly limited, but is preferably, for example, 0 to 4, and more preferably, 1 to 3. The acid contained in the acidic solution may be, for example, an inorganic acid, a sulfonic acid, a carboxylic acid, or the like. Examples of inorganic acids include sulfuric acid, nitric acid, hydrobromic acid, hydroiodic acid, hypochlorous acid, chlorous acid, chloric acid, perchloric acid, phosphoric acid, and boric acid. Examples of sulfonic acids include, for example, methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid. Examples of carboxylic acids include, for example, formic acid, acetic acid, citric acid, gluconic acid, lactic acid, oxalic acid, and tartaric acid. Among these, it is particularly preferable to use hydrochloric acid or sulfuric acid.
[0085] The temperature of the acid solution in the acid treatment is not particularly limited, but is preferably, for example, 5° C. to 100° C., and more preferably, 20° C. to 90° C. The immersion time in the acid solution in the acid treatment is not particularly limited, but is preferably, for example, 5 minutes to 120 minutes, and more preferably, 10 minutes to 60 minutes. The amount of the acid solution used in the acid treatment is not particularly limited, but is preferably, for example, 100 mass% to 100,000 mass%, and more preferably, 1000 mass% to 10,000 mass%, based on the absolute dry mass of the fiber raw material.
[0086] <Defibrillation process> The anionic group-introduced fibers are defibrated in a defibration process to obtain fine fibrous cellulose. In the defibration process, for example, a defibration treatment device can be used. The defibration treatment device is not particularly limited, but for example, a high-speed defibrator, a grinder (stone mill type grinder), a high-pressure homogenizer or an ultra-high-pressure homogenizer, a high-pressure collision type grinder, a ball mill, a bead mill, a disk type refiner, a conical refiner, a biaxial kneader, a vibration mill, a homomixer under high-speed rotation, an ultrasonic disperser, or a beater can be used. Among the above defibration treatment devices, it is more preferable to use a high-speed defibrator, a high-pressure homogenizer, or an ultra-high-pressure homogenizer, which are less affected by the grinding media and have less risk of contamination.
[0087] In the defibration process, for example, the anionic group-introduced fiber is preferably diluted with a dispersion medium to form a slurry. As the dispersion medium, one or more selected from water and organic solvents such as polar organic solvents can be used. The polar organic solvent is not particularly limited, but for example, alcohols, polyhydric alcohols, ketones, ethers, esters, aprotic polar solvents, etc. are preferable. Examples of alcohols include methanol, ethanol, isopropanol, n-butanol, isobutyl alcohol, etc. Examples of polyhydric alcohols include ethylene glycol, propylene glycol, glycerin, etc. Examples of ketones include acetone, methyl ethyl ketone (MEK), etc. Examples of ethers include diethyl ether, tetrahydrofuran, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono n-butyl ether, propylene glycol monomethyl ether, etc. Examples of esters include ethyl acetate, butyl acetate, etc. Aprotic polar solvents include dimethylsulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), and N-methyl-2-pyrrolidinone (NMP).
[0088] The solid content concentration of the fine fibrous cellulose during the defibration treatment can be appropriately set. In addition, the slurry obtained by dispersing the anionic group-introduced fibers in a dispersion medium may contain solid contents other than the anionic group-introduced fibers, such as urea having hydrogen bonding properties.
[0089] (Organic onium ion) The fine fibrous cellulose contains organic onium ions as counter ions of the anionic groups. In this embodiment, at least a part of the organic onium ions exists as counter ions of the fibrous cellulose, but the dispersion may contain free organic onium ions. The organic onium ions do not form covalent bonds with the fibrous cellulose.
[0090] The organic onium ion preferably satisfies at least one of the following conditions (a) and (b): (a) Contains a hydrocarbon group having 5 or more carbon atoms. (b) The total number of carbon atoms is 17 or more. That is, the fibrous cellulose preferably contains, as a counter ion of an anionic group, at least one selected from an organic onium ion containing a hydrocarbon group having 5 or more carbon atoms and an organic onium ion having a total carbon number of 17 or more. By using an organic onium ion that satisfies at least one of the above conditions (a) and (b), the dispersibility of the fine fibrous cellulose in organic solvents can be more effectively improved.
[0091] The hydrocarbon group having 5 or more carbon atoms is preferably an alkyl group having 5 or more carbon atoms or an alkylene group having 5 or more carbon atoms, more preferably an alkyl group having 6 or more carbon atoms or an alkylene group having 6 or more carbon atoms, even more preferably an alkyl group having 7 or more carbon atoms or an alkylene group having 7 or more carbon atoms, and particularly preferably an alkyl group having 10 or more carbon atoms or an alkylene group having 10 or more carbon atoms. Of these, the organic onium ion preferably has an alkyl group having 5 or more carbon atoms, and more preferably an organic onium ion containing an alkyl group having 5 or more carbon atoms and having a total of 17 or more carbon atoms.
[0092] The organic onium ion is preferably an organic onium ion represented by the following general formula (A).
[0093] [ka]
[0094] In the above general formula (A), M is referred to as the central element of the organic onium ion. M is preferably a nitrogen atom or a phosphorus atom. R1 to R4 each independently represent a hydrogen atom or an organic group. However, it is preferable that at least one of R1 to R4 is an organic group having 5 or more carbon atoms, or the total number of carbon atoms of R1 to R4 is 17 or more. Among them, M is preferably a nitrogen atom. That is, the organic onium ion is preferably an organic ammonium ion. Furthermore, it is preferable that at least one of R1 to R4 is an alkyl group having 5 or more carbon atoms, and the total number of carbon atoms of R1 to R4 is 17 or more.
[0095] Examples of organic onium ions include lauryl trimethyl ammonium, cetyl trimethyl ammonium, stearyl trimethyl ammonium, octyl dimethyl ethyl ammonium, lauryl dimethyl ethyl ammonium, didecyl dimethyl ammonium, lauryl dimethyl benzyl ammonium, tributyl benzyl ammonium, methyl tri-n-octyl ammonium, hexyl ammonium, n-octyl ammonium, dodecyl ammonium, tetradecyl ammonium, hexadecyl ammonium, stearyl ammonium, N,N-dimethyl dodecyl ammonium, N,N-dimethyl tetradecyl ammonium, N,N-dimethyl hexadecyl ammonium, N,N-dimethyl-n-octadecyl ammonium, dihexyl ammonium, di(2 -ethylhexyl)ammonium, di-n-octylammonium, didecylammonium, didodecylammonium, didecylmethylammonium, N,N-didodecylmethylammonium, polyoxyethylenedodecylammonium, alkyldimethylbenzylammonium, di-n-alkyldimethylammonium, behenyltrimethylammonium, tetraphenylphosphonium, tetraoctylphosphonium, acetonyltriphenylphosphonium, allyltriphenylphosphonium, amyltriphenylphosphonium, benzyltriphenylphosphonium, ethyltriphenylphosphonium, diphenylpropylphosphonium, triphenylphosphonium, tricyclohexylphosphonium, tri-n-octylphosphonium, etc. The alkyl group in alkyldimethylbenzylammonium and di-n-alkyldimethylammonium may be a straight-chain alkyl group having 8 to 18 carbon atoms.
[0096] As shown in general formula (A), the central element of an organic onium ion is bonded to a total of four groups or hydrogen. In the above-mentioned organic onium ion names, if there are less than four groups bonded, the remaining are bonded to hydrogen atoms to form the organic onium ion. For example, in the case of N,N-didodecylmethylammonium, it can be determined from the name that two dodecyl groups and one methyl group are bonded. In this case, hydrogen is bonded to the remaining group to form the organic onium ion.
[0097] When the organic onium contains O atoms, the larger the mass ratio of C atoms to O atoms (C / O ratio), the more preferable, and for example, C / O>5. By making the C / O ratio greater than 5, it becomes easier to obtain a fibrous cellulose concentrate when an organic onium ion or a compound that forms an organic onium ion by neutralization is added to a slurry containing fine fibrous cellulose.
[0098] The molecular weight of the organic onium ion is preferably 2000 or less, more preferably 1800 or less. By setting the molecular weight of the organic onium ion within the above range, the handleability of the fibrous cellulose can be improved. In addition, by setting the molecular weight of the organic onium ion within the above range, the decrease in the content of the fibrous cellulose in the dispersion can be suppressed.
[0099] The content of organic onium ions is preferably 0.5 to 2 times the molar amount of the anionic group contained in the fine fibrous cellulose, but is not particularly limited. The content of organic onium ions can be measured by tracking the atoms typically contained in the organic onium ions. Specifically, when the organic onium ions are ammonium ions, the amount of nitrogen atoms is measured, and when the organic onium ions are phosphonium ions, the amount of phosphorus atoms is measured. In addition, when the fine fibrous cellulose contains nitrogen atoms or phosphorus atoms in addition to the organic onium ions, a method for extracting only the organic onium ions, for example, an extraction operation using an acid, is performed, and then the amount of the target atom is measured.
[0100] The organic onium ion is preferably an ion that exhibits hydrophobicity. That is, the fine fibrous cellulose in the present embodiment exhibits hydrophobicity by having an organic onium ion. As a result, the dispersibility in an organic solvent is improved, and a dispersion liquid exhibiting a desired viscosity and light transmittance can be obtained. And, such a dispersion liquid can exhibit high thixotropy.
[0101] (optional ingredient) The dispersion of the present embodiment may be a dispersion consisting of the above-mentioned fine fibrous cellulose and organic solvent, but may contain optional components in addition to the above-mentioned fine fibrous cellulose and organic solvent. The optional components may include, for example, resins. The type of resin is not particularly limited, but may include, for example, thermoplastic resins and thermosetting resins.
[0102] Examples of the resin include acrylic resins, polycarbonate resins, polyester resins, polyamide resins, silicone resins, fluorine resins, chlorine resins, epoxy resins, melamine resins, phenol resins, polyurethane resins, diallyl phthalate resins, alcohol resins, cellulose derivatives, and precursors of these resins. Examples of the cellulose derivatives include carboxymethyl cellulose, methyl cellulose, and hydroxyethyl cellulose.
[0103] The dispersion may contain a resin precursor as the resin. The type of the resin precursor is not particularly limited, but examples thereof include precursors of thermoplastic resins and thermosetting resins. The precursor of the thermoplastic resin means a monomer or an oligomer having a relatively low molecular weight used to produce a thermoplastic resin. The precursor of the thermosetting resin means a monomer or an oligomer having a relatively low molecular weight that can form a thermosetting resin by polymerization or crosslinking reaction due to the action of light, heat, or a curing agent.
[0104] The dispersion may further contain a water-soluble polymer as a resin in addition to the above-mentioned resin types. Examples of the water-soluble polymer include synthetic water-soluble polymers (e.g., carboxyvinyl polymer, polyvinyl alcohol, alkyl methacrylate-acrylic acid copolymer, polyvinylpyrrolidone, sodium polyacrylate, polyethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, isoprene glycol, hexylene glycol, 1,3-butylene glycol, polyacrylamide, etc.), thickening polysaccharides (e.g., xanthan gum, guar gum, tamarind gum, carrageenan, locust bean gum, quince seed, alginic acid, pullulan, carrageenan, pectin, etc.), starches such as cationic starch, raw starch, oxidized starch, etherified starch, esterified starch, and amylose, glycerins such as glycerin, diglycerin, and polyglycerin, hyaluronic acid, and metal salts of hyaluronic acid.
[0105] Examples of optional components include surfactants, organic ions, coupling agents, inorganic layered compounds, inorganic compounds, leveling agents, preservatives, antifoaming agents, organic particles, lubricants, antistatic agents, ultraviolet protection agents, dyes, pigments, stabilizers, magnetic powders, orientation promoters, plasticizers, dispersants, and crosslinking agents.
[0106] (Method of producing dispersion liquid) The method for producing the dispersion includes a step of adding an organic onium ion or a compound that forms an organic onium ion upon neutralization to a slurry containing fine fibrous cellulose obtained through the above-mentioned defibration process to obtain a fibrous cellulose agglomerate (concentrate), and a step of dispersing the fibrous cellulose agglomerate (concentrate) in an organic solvent.
[0107] In the step of obtaining a fibrous cellulose aggregate (concentrate), the above-mentioned organic onium ion or a compound that forms an organic onium ion by neutralization is added to the fine fibrous cellulose-containing slurry obtained in the above-mentioned defibration treatment step. In this case, the organic onium ion is preferably added as a solution containing the organic onium ion, and more preferably as an aqueous solution containing the organic onium ion.
[0108] An aqueous solution containing an organic onium ion usually contains an organic onium ion and a counter ion (anion). When preparing an aqueous solution of an organic onium ion, if the organic onium ion and the corresponding counter ion have already formed a salt, the organic onium ion may be dissolved in water as is. When preparing an aqueous solution of an organic onium ion, if the organic onium ion and the corresponding counter ion have already formed a salt, the organic onium ion may be dissolved in water or hot water.
[0109] In addition, organic onium ion may be generated only after neutralization with acid, such as dodecylamine. In this case, organic onium ion is obtained by reaction between a compound that forms organic onium ion by neutralization and an acid. In this case, the acid used for neutralization may be inorganic acid such as hydrochloric acid, sulfuric acid, nitric acid, etc., or organic acid such as lactic acid, acetic acid, formic acid, oxalic acid, etc. In the flocculation process, a compound that forms organic onium ion by neutralization may be directly added to the fibrous cellulose-containing slurry, and the anionic group contained in the fibrous cellulose may be used as a counterion to convert to organic onium ion.
[0110] The amount of organic onium ion added is preferably 2% by mass or more, more preferably 10% by mass or more, even more preferably 50% by mass or more, and particularly preferably 100% by mass or more, based on the total mass of the fibrous cellulose. The amount of organic onium ion added is preferably 1000% by mass or less, based on the total mass of the fibrous cellulose. The molar number of the organic onium ion to be added is preferably 0.2 times or more, more preferably 0.5 times or more, and even more preferably 1.0 times or more, the value obtained by multiplying the amount (molar number) of inorganic oxo acid groups contained in the fibrous cellulose by the valence. The molar number of the organic onium ion to be added is preferably 10 times or less the value obtained by multiplying the amount (molar number) of inorganic oxo acid groups contained in the fibrous cellulose by the valence.
[0111] When the organic onium ion is added and stirred, an aggregate is generated in the fibrous cellulose-containing slurry. The aggregate is an aggregate of fibrous cellulose having an organic onium ion as a counter ion. In this specification, such an aggregate is also called a fibrous cellulose concentrate. The fibrous cellulose-containing slurry in which the aggregate is generated is filtered under reduced pressure to recover the fibrous cellulose aggregate (concentrate).
[0112] The obtained fibrous cellulose aggregate may be washed with ion-exchanged water. By repeatedly washing the fibrous cellulose aggregate with ion-exchanged water, excess organic onium ions and the like contained in the fibrous cellulose aggregate can be removed.
[0113] The solid content concentration of the obtained fibrous cellulose aggregate is preferably 5% by mass or more, more preferably 15% by mass or more, and even more preferably 25% by mass or more. The solid content concentration of the fibrous cellulose aggregate may be 100% by mass.
[0114] The moisture content of the fibrous cellulose aggregate may be 0% by mass, 0.5% by mass or more, 1% by mass or more, 3% by mass or more, or 5% by mass or more, based on the total mass of the fibrous cellulose aggregate. The moisture content of the fibrous cellulose aggregate is preferably 20% by mass or less, more preferably 15% by mass or less, based on the total mass of the fibrous cellulose aggregate. The moisture content in the fibrous cellulose aggregate can be measured by placing 200 mg of the fibrous cellulose aggregate on a moisture meter (MS-70, manufactured by A&D Co., Ltd.) and heating at 140°C. The moisture content in the fibrous cellulose aggregate can be calculated from the measured moisture content.
[0115] The fibrous cellulose agglomerate may be one that has been subjected to a drying step, an aging step, a spray drying step, a granulation step, a sheeting step, a heating step, a wetting step, a grinding step, a spraying step, a soaking step, a filtration step, a freezing step, a sublimation step, a water squeezing step, a pressurized dehydration step, a centrifugal dehydration step, a surface treatment step, etc. Among these, the fibrous cellulose agglomerate is preferably one that has been subjected to a drying step, which allows the production of a fibrous cellulose agglomerate with a low water content.
[0116] In the step of dispersing the fibrous cellulose aggregate (concentrate) in an organic solvent, the fibrous cellulose aggregate (concentrate) obtained in the step of obtaining the fibrous cellulose aggregate (concentrate) described above is dispersed in an organic solvent. Note that this dispersion step is also called a redispersion step because it is a step of dispersing the fibrous cellulose aggregate (concentrate) again in a solvent.
[0117] The dispersing device used when dispersing the fibrous cellulose aggregates (concentrate) in an organic solvent may be, for example, the same as the defibration processing device described in the above defibration processing. Among them, when dispersing the fibrous cellulose aggregates (concentrate) in an organic solvent, it is preferable to disperse the fibrous cellulose aggregates (concentrate) using a high-pressure homogenizer or an ultra-high-pressure homogenizer. By using a high-pressure homogenizer in the redispersion step, the redispersibility of the fibrous cellulose aggregates (concentrate) is improved, making it easier to obtain a highly viscous and highly transparent dispersion liquid.
[0118] In addition, in the redispersion step or before the redispersion step, a step of heating the suspension obtained by dispersing the fibrous cellulose aggregates (concentrate) in an organic solvent is preferably provided. That is, the method for producing a dispersion preferably includes a step of adding an organic onium ion or a compound that forms an organic onium ion by neutralization to a slurry containing fine fibrous cellulose to obtain a fibrous cellulose aggregate (concentrate), a step of suspending the fibrous cellulose aggregate (concentrate) in an organic solvent to obtain a suspension, and a step of heating the suspension and treating it with a high-pressure homogenizer or an ultra-high-pressure homogenizer to obtain a dispersion. In this case, it is preferable that the suspension is heated to 40°C or higher. In the heating step, the temperature of the suspension is preferably 100°C or lower. Conventionally, in the redispersion step, cooling was usually performed for the purpose of suppressing thermal denaturation of the fibrous cellulose aggregates (concentrate). However, in this embodiment, a heating step is deliberately provided in the redispersion step or before the redispersion step. And, by providing such a heating step, it has been possible to successfully obtain a dispersion having a higher viscosity and high transparency.
[0119] When the suspension is heated in the redispersion step or before the redispersion step, the liquid temperature after passing through the dispersion device is preferably 40° C. or higher. When a high-pressure homogenizer or ultra-high-pressure homogenizer is used as the dispersion device, the liquid temperature after passing through the grinding mechanism is preferably 40° C. or higher. In order to make the liquid temperature after passing through the dispersion device 40° C. or higher, for example, the pressure during passage through the dispersion device can be increased, the inner diameter of the internal flow path of the grinding processor can be reduced, the pump speed can be increased, the grinding processor can be heated before and / or after passing through the pump, and / or the suspension to be tested can be heated in advance.
[0120] In the present specification, the step of preheating the suspension to be tested is sometimes referred to as a preheating step. In the preheating step, it is preferable to heat the suspension so that the liquid temperature is 40° C. or more and 100° C. or less. In the present embodiment, it is preferable to provide such a preheating step, and by preheating the suspension before the high-pressure homogenizer treatment to 40° C. or more, the dispersibility of the fine fibrous cellulose in the organic solvent is further improved, and a dispersion liquid having a higher viscosity and higher transparency is easily obtained.
[0121] The process for producing the dispersion may further include a step of dispersing an optional component in the obtained dispersion. The optional components used in this step include the optional components described above.
[0122] (Application) The dispersion of the present invention may be used as a thickener for various applications. For example, the dispersion of the present invention can be used as an additive to food, cosmetics, cement, paint (for painting vehicles such as automobiles, ships, and aircraft, for building materials, for daily necessities, etc.), ink, medicine, packaging materials, coating materials, etc. In addition, the dispersion of the present invention can be applied to daily necessities by adding it to a resin-based material. Among them, the dispersion of the present invention is preferably used for paint.
[0123] The dispersion of the present invention is preferably used for forming a molded body. The shape of the molded body is not particularly limited, and it can be, for example, a sheet-like, granular, or thread-like molded body. Among them, the dispersion of the present invention is preferably used for the application of a sheet-like molded body. For example, the dispersion of the present invention can be formed into a film and used as various films.
[0124] Molded articles obtained by coating the dispersion on a substrate are also suitable for applications such as reinforcing materials, interior materials, exterior materials, packaging materials, electronic materials, optical materials, acoustic materials, process materials, components for transport equipment, components for electronic devices, and components for electrochemical elements. EXAMPLES
[0125] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below. In the following, Example 4 shall be read as Reference Example 4.
[0126] <Manufacturing example A> The raw pulp used was softwood kraft pulp (solid content 93% by mass, basis weight 208 g / m) manufactured by Oji Paper. 2 A sheet-like pulp (with a Canadian Standard Freeness (CSF) of 700 ml when disintegrated and measured according to JIS P 8121) was used. This raw pulp was subjected to phosphorus oxo-oxidation treatment as follows. First, a mixed aqueous solution of ammonium dihydrogen phosphate and urea was added to 100 parts by mass (bone dry mass) of the raw pulp to adjust the total weight to 45 parts by mass of ammonium dihydrogen phosphate, 120 parts by mass of urea, and 150 parts by mass of water, to obtain a chemical-impregnated pulp. Next, the obtained chemical-impregnated pulp was heated in a hot air dryer at 165°C for 200 seconds to introduce phosphoric acid groups into the cellulose in the pulp, to obtain a phosphorylated pulp.
[0127] The phosphorylated pulp was then washed. The washing was carried out by pouring 10 L of ion-exchanged water into 100 g (bone dry weight) of phosphorylated pulp to obtain a pulp dispersion, stirring the pulp to uniformly disperse it, and then repeatedly filtering and dehydrating the pulp. The washing was completed when the electrical conductivity of the filtrate reached 100 μS / cm or less.
[0128] Next, the phosphorylated pulp after washing was subjected to a neutralization treatment as follows. First, the phosphorylated pulp after washing was diluted with 10 L of ion-exchanged water, and then a 1N aqueous solution of sodium hydroxide was added little by little while stirring to obtain a phosphorylated pulp slurry having a pH of 12 to 13. Next, the phosphorylated pulp slurry was dehydrated to obtain a phosphorylated pulp that had been subjected to a neutralization treatment. Next, the above-mentioned washing treatment was performed on the phosphorylated pulp after the neutralization treatment.
[0129] The infrared absorption spectrum of the phosphorylated pulp obtained was measured using FT-IR. -1 Absorption due to the P=O of the phosphate group was observed near the nucleus, confirming that the phosphate group had been added to the pulp. In addition, when the obtained phosphorylated pulp was analyzed using an X-ray diffractometer, typical peaks were confirmed at two positions, near 2θ=14° to 17° and near 2θ=22° to 23°, confirming that it had cellulose type I crystals.
[0130] Ion-exchanged water was added to the obtained phosphorylated pulp to prepare a slurry with a solid content (fibrous cellulose concentration) of 2% by mass. This slurry was treated six times with a wet pulverizer (Starburst, manufactured by Sugino Machine Co., Ltd.) at a pressure of 200 MPa to obtain a fine fibrous cellulose dispersion A containing fine fibrous cellulose.
[0131] X-ray diffraction confirmed that this fine fibrous cellulose maintained cellulose type I crystals. The fiber width of the fine fibrous cellulose was measured using a transmission electron microscope and found to be 2 to 5 nm. Image analysis using AFM revealed that 100 pieces of fine fibrous cellulose were extracted and the number average aspect ratio was calculated to be 300. The amount of phosphoric acid groups (amount of first dissociated acid) measured by the method for measuring the amount of phosphorus oxo acid groups described below was 1.45 mmol / g. The total amount of dissociated acid was 2.45 mol / g.
[0132] <Manufacturing example B> A phosphite pulp was obtained by the same procedure as in Production Example A, except that 33 parts by mass of phosphorous acid (phosphonic acid) was used instead of ammonium dihydrogen phosphate to introduce a phosphite group into the cellulose in the pulp.
[0133] The infrared absorption spectrum of the obtained phosphorous pulp was measured using FT-IR. -1 Absorption due to the P=O of the phosphonic acid group, which is a tautomer of the phosphorous acid group, was observed near the nucleus, confirming that the phosphorous acid group (phosphonic acid group) was added to the pulp. In addition, when the obtained phosphorous-containing pulp was analyzed using an X-ray diffraction device, typical peaks were confirmed at two positions, around 2θ=14° to 17° and around 2θ=22° to 23°, confirming that it has cellulose type I crystals.
[0134] The resulting phosphorous-subtilized pulp was treated in a wet pulverizer in the same manner as in Production Example A to obtain a fine fibrous cellulose dispersion B containing fine fibrous cellulose.
[0135] X-ray diffraction confirmed that this fine fibrous cellulose maintained cellulose type I crystals. The fiber width of the fine fibrous cellulose was measured using a transmission electron microscope and found to be 3 to 5 nm. Image analysis using AFM revealed that 100 pieces of fine fibrous cellulose were extracted and the number average aspect ratio was calculated to be 280. The amount of phosphorous acid groups (amount of first dissociated acid) measured by the method for measuring the amount of phosphorus oxo acid groups described below was 1.51 mmol / g. The total amount of dissociated acid was 1.54 mmol / g.
[0136] <Manufacturing example C> A sulfated pulp was obtained by the same procedure as in Production Example A, except that 38 parts by mass of amidosulfuric acid was used instead of ammonium dihydrogen phosphate.
[0137] The infrared absorption spectrum of the sulfated pulp obtained was measured using FT-IR. -1 Absorption due to sulfate groups (sulfonic acid groups) was observed near the 2θ=14° to 17° angle, confirming that sulfate groups (sulfonic acid groups) had been added to the pulp. In addition, when the obtained sulfated pulp was analyzed using an X-ray diffractometer, typical peaks were confirmed at two positions, near 2θ=14° to 17° and near 2θ=22° to 23°, confirming that it had cellulose type I crystals.
[0138] Ion-exchanged water was added to the obtained sulfated pulp, and the mixture was stirred to prepare a slurry with a solid content concentration (fibrous cellulose concentration) of 2% by mass. This slurry was treated six times with a wet pulverizer (Starburst, manufactured by Sugino Machine Co., Ltd.) at a pressure of 200 MPa to obtain a fine fibrous cellulose dispersion C containing fine fibrous cellulose. In addition, 100 pieces of fine fibrous cellulose were extracted from the image analysis by AFM, and the number average value of the aspect ratio was calculated, and the number average value of the aspect ratio was 280. The amount of sulfate group (sulfonic acid group) measured by the method for measuring the amount of sulfur oxo acid group described later was 1.30 mmol / g.
[0139] <Manufacturing example D> As the raw material pulp, softwood kraft pulp (undried) manufactured by Oji Paper Co., Ltd. was used. This raw material pulp was subjected to an alkaline TEMPO oxidation treatment as follows. First, the raw material pulp equivalent to 100 parts by mass of dry mass, 1.6 parts by mass of TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl), and 10 parts by mass of sodium bromide were dispersed in 10,000 parts by mass of water. Next, a 13% by mass aqueous solution of sodium hypochlorite was added to 10 mmol per 1.0 g of pulp to start the reaction. During the reaction, a 0.5 M aqueous solution of sodium hydroxide was added dropwise to keep the pH at 10 to 10.5, and the reaction was deemed to be complete when no change in pH was observed.
[0140] The TEMPO oxidized pulp was then washed. The washing was performed by dehydrating the pulp slurry after TEMPO oxidation to obtain a dehydrated sheet, pouring 5,000 parts by mass of ion-exchanged water into the sheet, stirring to disperse the sheet uniformly, and then filtering and dehydrating the sheet. The washing was completed when the electrical conductivity of the filtrate reached 100 μS / cm or less.
[0141] In addition, the obtained TEMPO oxidized pulp was analyzed using an X-ray diffraction device, and typical peaks were confirmed at two positions, around 2θ = 14° to 17° and around 2θ = 22° to 23°, confirming the presence of cellulose type I crystals.
[0142] Ion-exchanged water was added to the obtained TEMPO oxidized pulp to prepare a slurry with a solid concentration (fibrous cellulose concentration) of 2 mass %. This slurry was treated six times with a wet pulverizer (Starburst, manufactured by Sugino Machine Co., Ltd.) at a pressure of 200 MPa to obtain a fine fibrous cellulose dispersion D containing fine fibrous cellulose.
[0143] X-ray diffraction confirmed that the fine fibrous cellulose maintained cellulose type I crystals. The fiber width of the fine fibrous cellulose was measured using a transmission electron microscope and found to be 2 to 5 nm. Image analysis using AFM was also performed to extract 100 pieces of fine fibrous cellulose and calculate the number average aspect ratio, which was found to be 250. The amount of carboxyl groups measured by the method for measuring the amount of carboxyl groups described below was 1.80 mmol / g.
[0144] [Measurement of phosphorus oxoacid group content] In measuring the amount of phosphorus oxoacid groups (amount of phosphoric acid groups or amount of phosphorous acid groups) of fine fibrous cellulose, ion-exchanged water was first added to the target fine fibrous cellulose to prepare a slurry with a solid content of 0.2% by mass. The obtained fine fibrous cellulose dispersion was treated with an ion-exchange resin, and then titrated with an alkali to measure the amount of phosphorus oxoacid groups. Treatment with ion exchange resin was carried out by adding 1 / 10 by volume of a strongly acidic ion exchange resin (Amberjet 1024; Organo Corporation, conditioned) to the above-mentioned fine fibrous cellulose dispersion, shaking for 1 hour, and then pouring onto a mesh with 90 μm openings to separate the resin and the slurry. The titration using alkali was performed by adding 10 μL of 0.1N sodium hydroxide solution every 5 seconds to the fine fibrous cellulose dispersion after the ion exchange resin treatment, while measuring the change in the pH value of the slurry. Nitrogen gas was blown into the slurry 15 minutes before the start of the titration. In this neutralization titration, two points of maximum increment (differential value of pH with respect to the amount of alkali added) were observed on the curve plotting the measured pH against the amount of alkali added. Of these, the first maximum increment point obtained after the start of the alkali addition is called the first end point, and the second maximum increment point obtained next is called the second end point (Figure 1). The amount of alkali required from the start of the titration to the first end point is equal to the amount of first dissociated acid in the slurry used for the titration. The amount of alkali required from the start of the titration to the second end point is equal to the total amount of dissociated acid in the slurry used for the titration. The amount of alkali (mmol) required from the start of titration to the first end point was divided by the solid content (g) in the slurry to be titrated, and this value was taken as the amount of phosphorus oxoacid groups (mmol / g).
[0145] [Measurement of Carboxy Group Amount] In measuring the amount of carboxy groups in fine fibrous cellulose, ion-exchanged water was first added to the target fine fibrous cellulose to prepare a slurry with a solid content of 0.2% by mass. The resulting fine fibrous cellulose dispersion was treated with an ion-exchange resin, and then titrated with an alkali to measure the amount of carboxy groups. Treatment with ion exchange resin was carried out by adding 1 / 10 by volume of a strongly acidic ion exchange resin (Amberjet 1024; Organo Corporation, conditioned) to the above-mentioned fine fibrous cellulose dispersion, shaking for 1 hour, and then pouring onto a mesh with 90 μm openings to separate the resin and the slurry. The titration using alkali was carried out by adding 50 μL of 0.1 N sodium hydroxide solution once every 30 seconds to the fine fibrous cellulose dispersion after the ion exchange resin treatment, while measuring the change in pH value of the dispersion. The amount of carboxyl groups (mmol / g) was calculated by dividing the amount of alkali (mmol) required in the region corresponding to the first region shown in Figure 2 by the solid content (g) in the slurry to be titrated.
[0146] [Measurement of the amount of sulfur oxoacid groups] The amount of sulfur oxoacid groups in the fine fibrous cellulose was measured as follows. The fine fibrous cellulose obtained in Production Example C was frozen in a freezer and then dried for 3 days in a freeze dryer (FreeZone, manufactured by Labconco). The freeze-dried product was pulverized into a powder form using a hand mixer (Labo Millser PLUS, manufactured by Osaka Chemical) at a rotation speed of 20,000 rpm for 60 seconds. The freeze-dried and pulverized samples were subjected to pressure heating decomposition using nitric acid in a closed vessel. The samples were then appropriately diluted and the amount of sulfur was measured using ICP-OES. The value calculated by dividing the amount by the bone dry mass of the fine fibrous cellulose used was taken as the amount of sulfur oxoacid groups (unit: mmol / g) of the fine fibrous cellulose.
[0147] <Example 1> When 100 g of a 3.86 mass% aqueous solution of di-n-stearyldimethylammonium chloride (hereinafter also referred to as DSDMA) was added to 100 g of fine fibrous cellulose dispersion A and stirred for 5 minutes, aggregates were generated in the fine fibrous cellulose dispersion. The fine fibrous cellulose dispersion in which the aggregates were generated was filtered under reduced pressure to obtain fine fibrous cellulose aggregates. The obtained fine fibrous cellulose aggregates were repeatedly washed with ion-exchanged water to remove excess di-n-stearyldimethylammonium chloride and eluted ions contained in the fine fibrous cellulose aggregates, thereby obtaining a fine fibrous cellulose concentrate. The obtained fine fibrous cellulose concentrate was air-dried to obtain fine fibrous cellulose concentrate A with a solid content concentration of 90 mass%.
[0148] Toluene was added to the fine fibrous cellulose concentrate A so that the solid content concentration (fibrous cellulose concentration) was 3 mass % to prepare a suspension. The suspension was preheated in a hot water bath to a temperature of 40°C. The suspension preheated to 40°C was treated five times at a pressure of 100 MPa with a high-pressure homogenizer (Beryu-Mini, manufactured by Biryu Co., Ltd.). The liquid temperature after passing through the pulverization treatment section was also measured. In this way, a toluene dispersion of the fine fibrous cellulose concentrate A was obtained.
[0149] The toluene dispersion obtained above was left to stand at 23°C for 24 hours, and then the viscosity was measured using a Brookfield type viscometer (analog viscometer T-LVT, manufactured by BLOOKFIELD). The measurement conditions were 23°C, and the viscosity was measured when rotated at 0.6 rpm or 60 rpm for 3 minutes. The TI value, which is an index of thixotropy, was calculated according to the following formula. TI value = (viscosity value at 0.6 rpm / viscosity value at 60 rpm)
[0150] The toluene dispersion obtained above was sealed in a quartz glass cell for liquids with an optical path length of 10 mm, and the light transmittance at a wavelength of 660 nm was measured using an ultraviolet-visible spectrophotometer (V-770, manufactured by JASCO Corporation). The zero point measurement was performed using ion-exchanged water placed in the same glass cell. In each of the Examples and Comparative Examples, the light transmittance was measured immediately after redispersion in an organic solvent.
[0151] <Example 2> An organic solvent dispersion was obtained in the same manner as in Example 1, except that fine fibrous cellulose dispersion B was used.
[0152] <Example 3> An organic solvent dispersion was obtained in the same manner as in Example 1, except that fine fibrous cellulose dispersion C was used.
[0153] <Example 4> An organic solvent dispersion was obtained in the same manner as in Example 1, except that pre-heating was not carried out before the treatment with the high-pressure homogenizer.
[0154] <Example 5> An organic solvent dispersion was obtained in the same manner as in Example 1, except that fine fibrous cellulose dispersion D was used.
[0155] <Example 6> An organic solvent dispersion was obtained in the same manner as in Example 1, except that xylene was used instead of toluene.
[0156] <Example 7> An organic solvent dispersion was obtained in the same manner as in Example 1, except that didecyldimethylammonium chloride (hereinafter, also referred to as DDDMA) was used instead of di-n-stearyldimethylammonium chloride.
[0157] <Comparative Example 1> An organic solvent dispersion was obtained in the same manner as in Example 1, except that pre-heating was not performed and the toluene suspension was treated for 10 minutes using an ultrasonic homogenizer (Hielscher, UP400S) instead of the high-pressure homogenizer.
[0158] [Table 1]
[0159] The dispersions obtained in the examples were highly viscous and highly transparent, and had improved thixotropy. In Examples 1 to 3, 5, and 6, the viscosity and transparency were further improved by setting the liquid temperature immediately after the pulverization treatment with the high-pressure homogenizer to 40°C or higher.
Claims
1. A dispersion containing fibrous cellulose having a fiber width of 1000 nm or less and an organic solvent, The fibrous cellulose has an anionic group, and the content of the anionic group is 0.50 mmol / g or more, The fibrous cellulose has an organic onium ion as a counter ion of the anionic group, A dispersion having a B-type viscosity of 80 Pa s or more as measured by the following measurement method (A); Measurement method (A): The B-type viscosity of the dispersion liquid is measured in accordance with JIS Z 8803 (2011) when the fibrous cellulose concentration of the dispersion liquid is 3 mass % (w / w), the rotation speed is 0.6 rpm, and the temperature is 23°C.
2. The dispersion according to claim 1, which has a light transmittance of 80% or more as measured by the following measurement method (B); Measurement method (B): The dispersion liquid is adjusted to a fibrous cellulose concentration of 3 mass % (w / w) and sealed in a quartz cell with an optical path length of 10 mm, and the light transmittance at a wavelength of 660 nm is measured using an ultraviolet-visible spectrophotometer.
3. 3. The dispersion according to claim 1 or 2, wherein the fiber width of the fibrous cellulose is 10 nm or less.
4. The dispersion according to any one of claims 1 to 3, wherein the anionic group is at least one selected from the group consisting of a phosphorus oxoacid group, a substituent derived from a phosphorus oxoacid group, a sulfur oxoacid group, and a substituent derived from a sulfur oxoacid group.
Citation Information
Patent Citations
Composite body of micro cellulose fiber, liquid dispersion of micro cellulose fiber and composite material
JP2011140738A
Fine cellulose fiber composite, fine cellulose fiber dispersion, and composite material
JP2016188375A
Fibrous cellulose, fibrous cellulose-containing composition, fibrous cellulose dispersion and manufacturing method of fibrous cellulose
JP2018145398A
Reactant fiber and method for producing fine cellulose fiber dispersion
JP2019049091A
Fine cellulose fiber composite dispersion
JP2019119868A