Polycarbonate resin manufacturing method

By employing a melt polycondensation reaction with a dihydroxy compound and a basic compound in a solvent, the method stabilizes the polymer primary structure of polycarbonate resin, resulting in high-quality optical films with consistent mechanical and optical properties.

JP7552389B2Active Publication Date: 2024-09-18MITSUBISHI CHEM CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021013013
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-09-18
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Existing methods for producing polycarbonate resin result in unstable polymer primary structures, leading to variations in optical and mechanical properties, which affect productivity and cost due to fluctuations in the stretching process of optical films.

Method used

A method involving a melt polycondensation reaction using a dihydroxy compound with an acetal group, continuously fed into a reactor with a basic compound in a solvent containing a monohydroxy compound, to stabilize the polymer primary structure and suppress decomposition.

Benefits of technology

This approach produces polycarbonate resin with excellent optical and mechanical properties, ensuring consistent quality and enabling stable production of optical films with high stretching ratios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552389000023
    Figure 0007552389000023
  • Figure 0007552389000020
    Figure 0007552389000020
  • Figure 0007552389000022
    Figure 0007552389000022
Patent Text Reader

Abstract

To provide a method for producing a polycarbonate resin excellent in optical characteristics, mechanical characteristics and the like and good in quality uniformity.SOLUTION: The method for producing a polycarbonate resin produces a polycarbonate resin by continuously supplying a dihydroxy compound (A) having an acetal group in a part of the structure, a carbonic diester, and a polymerization catalyst to a reactor to perform a melt polycondensation reaction and includes a step of dissolving the dihydroxy compound (A) in a solvent containing a monohydroxy compound represented by the following formula (1) as a main component in a raw material dissolving tank, the solvent containing a basic compound. (In formula (1), R1 and R2 each independently represent a hydrogen atom, an optionally substituted C1-10 alkyl group, an optionally substituted C1-10 acyl group, an optionally substituted C1-10 alkoxy group, or a C1-10 alkyl ester group optionally having a substituent.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention aims to strictly control the primary polymer structure of polycarbonate resin and improve optical and mechanical properties. The present invention relates to a production method that stabilizes the quality of the physical properties. [Background technology]

[0002] With the recent development of the flat panel display field, the optical fibers used as components In addition to further improving performance and quality, there is also a demand for improved productivity and reduced costs. The material used for optical films is spiroglycol (SPG) which is a monomer. Copolymer polycarbonates using SPG have been developed, and SPG has excellent heat resistance and optical properties, especially optical properties. It has been disclosed that the low elastic modulus is an advantage (for example, Patent Documents 1 to 3). In addition, when manufacturing polycarbonate resin using SPG, the polymerization reactivity and quality are stabilized. In Patent Document 4, the amount of acidic components contained in SPG is By reducing the amount of gel in the resulting polycarbonate resin, the amount of gel in the resulting polycarbonate resin is reduced. In the continuous polymerization process, the thermal history of the raw material preparation step is reduced, and the decomposition of SPG is prevented. This suppresses the production of polycarbonate resin and stabilizes the quality of the resulting polycarbonate resin. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2006-232897 A [Patent Document 2] International Publication No. 2008 / 156186 Brochure [Patent Document 3] JP 2015-212816 A [Patent Document 4] JP 2011-26499 A [Patent Document 5] JP 2012-214774 A Summary of the Invention [Problem to be solved by the invention]

[0004] According to the investigations of the present inventors, the polyimide obtained by the methods of Patent Document 4 and Patent Document 5 is The primary polymer structure of the carbonate resin, especially the molecular weight distribution, fluctuates, which causes As a result, the physical properties of the optical film (phase difference film) became unstable. If the resin quality varies, the yield will decrease, especially in the stretching process, resulting in lower productivity and costs. Even slight decomposition of SPG is suppressed, and the resulting polycarbonate resin is It is required to completely stabilize the primary polymer structure of the lipid. The present invention relates to a polycarbonate resin having excellent optical properties, mechanical properties, etc., and good quality uniformity. The object of the present invention is to provide a method for producing fat. [Means for solving the problem]

[0005] As a result of intensive research to solve the above problems, the present inventors have found that in the raw material preparation process, As shown in G, a dihydroxy compound having an acetal group in its structure is bonded to a basic compound. They found that by exposing the polymer to water, the variation in the primary structure of the polymer can be effectively suppressed. The gist of the present invention is as follows.

[0006] [1] A dihydroxy compound (A) having an acetal group as part of its structure and a diester carbonate The melt polycondensation reaction is carried out by continuously supplying the polymerization catalyst and the polymerization mixture to the reactor to obtain polycarbonate. A method for producing a methacrylic resin, comprising the steps of: In a raw material dissolving tank, a dissolving agent containing as its main component a monohydroxy compound represented by the following formula (1) is The method includes a step of dissolving the dihydroxy compound (A) in a solvent, The method for producing a polycarbonate resin, wherein the solvent contains a basic compound.

[0007] [ka]

[0008] (R in formula (1) 1 , R 2 each independently represents a hydrogen atom, a number of carbon atoms which may be substituted an alkyl group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms which may be substituted, an alkoxy group having 1 to 10 carbon atoms which may have a substituent; It is an alkyl ester group. [2] The internal temperature of the raw material dissolving tank according to [1] above is 80° C. or higher and 150° C. or lower. A method for producing polycarbonate resin. [3] The dihydroxy compound (A) is continuously supplied to the raw material dissolving tank and dissolved. The solution containing the dihydroxy compound (A) is continuously discharged from a raw material dissolving tank, Or a method for producing a polycarbonate resin according to [2]. [4] The dihydroxy compound (A) is a compound represented by the following formula (2), The method for producing a polycarbonate resin according to any one of items 1] to 3).

[0009] [ka]

[0010] [5] Polycarbonate resin measured using deuterated chloroform solvent 1 H-NMR The content of the component detected at 5.7 to 5.8 ppm in the spectrum is expressed by the formula (2). The amount of the structural units derived from the compound represented by the preceding formula is 0.05 mol % or less. The method for producing the polycarbonate resin according to any one of [1] to [4] above. [6] The basic compound is a metal selected from the group consisting of metals in Group 2 of the long periodic table and lithium. At least one metal compound selected from the group consisting of the compounds according to any one of [1] to [5] above. A method for producing the polycarbonate resin described above. [7] The content of the basic compound in the solvent is less than or equal to the total dihydroxy group used in the melt polycondensation reaction. The amount of the compound [1] to [3] is 0.1 μmol or more and 50 μmol or less per 1 mol of the compound. [6] A method for producing a polycarbonate resin according to any one of the above. [8] The carbonic acid diester is a compound represented by the following formula (3), ] The method for producing a polycarbonate resin according to any one of the following:

[0011] [ka]

[0012] (R in Equation (3) 1 , R 2 each independently represents a hydrogen atom, a number of carbon atoms which may be substituted an alkyl group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms which may be substituted, an alkoxy group having 1 to 10 carbon atoms which may have a substituent; It is an alkyl ester group. [9] A process for recovering the monohydroxy compound produced as a by-product in the polycondensation reaction and purifying it by distillation The monohydroxy compound purified by distillation is supplied to the raw material dissolving tank. The method for producing a polycarbonate resin according to any one of the above [1] to [8], .

[10] The polycarbonate resin is derived from a dihydroxy compound represented by the following formula (4): The polycarbonate according to any one of the above [1] to [9], which contains a structural unit A method for producing resin.

[0013] [ka]

[0014]

[11] The polycarbonate resin comprises a structural unit derived from a compound represented by the following formula (5):

[0026] The method for producing the polycarbonate resin according to any one of [1] to

[10] above, method.

[0015] [ka]

[0016] (In formula (5), R 3 and R 4 each independently represents a direct bond or may have a substituent R is an alkylene group having 1 to 4 carbon atoms. 5 ~R 10 each independently represents a hydrogen atom, a substituted an alkyl group having 1 to 10 carbon atoms which may have a substituent; an aryl group having 1 to 15 carbon atoms which may have a substituent; an acyl group having 1 to 10 carbon atoms which may have a substituent; an alkoxy group having 1 to 10 carbon atoms which may be substituted, an aryloxy group having 1 to 5 carbon atoms which may have a substituent; an acyloxy group having 1 to 10 carbon atoms which may have a substituent; An amino group which may have a substituent, a vinyl group having 2 to 10 carbon atoms which may have a substituent an ethynyl group having 2 to 10 carbon atoms which may have a substituent; a sulfur atom which has a substituent; is a silicon atom having a substituent, a halogen atom, a nitro group, or a cyano group, provided that R 5 ~R 10 At least two adjacent groups among these may be bonded to each other to form a ring. X is a hydroxy group, a carboxy group, an alkyl group having 1 to 10 carbon atoms which may have a substituent. and an aryl ester group having 6 to 15 carbon atoms which may have a substituent. ) Effect of the Invention

[0017] According to the present invention, a polycarbonate having excellent optical properties, mechanical properties, etc. and good quality uniformity can be obtained. It is possible to stably produce polycarbonate resins. Transparent films made of carbonate resins are suitable for optical applications such as retardation films. There can be. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is a process diagram showing a raw material preparation process in polymerization equipment A in the production method of the present invention. [Diagram 2] FIG. 2 is a process diagram showing a raw material preparation process in polymerization equipment B in the production method of the present invention. [Diagram 3] FIG. 1 is a process diagram showing a polymerization step and a distillation step in polymerization equipment A and B in the production method of the present invention. [Figure 4] 1 is a 1H-NMR spectrum of the polycarbonate resin produced in Example 1. [Diagram 5] 1 is a 1H-NMR spectrum of the polycarbonate resin produced in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention will be described in detail below, but the present invention is not limited to the following description. The invention can be modified and implemented in any manner without departing from the spirit and scope of the invention.

[0020] In this specification, when "~" is used to express a numerical value or a physical property value, It will be used including the values ​​before and after it.

[0021] In this specification, the term "repeating structural unit" refers to a structure in which the same structure appears repeatedly in a resin. It means a structural unit that constitutes the resin by linking each other. For example, in the case of polycarbonate resin, the carbonyl group is also called the repeating structural unit. In addition, the term "structural unit" refers to a partial structure that constitutes a resin, and is a repeating structural unit. For example, a specific partial structure sandwiched between adjacent linking groups in a resin. The polymerizable reactive group present in the partial structure or the terminal portion of the polymer and the linking group adjacent to the polymerizable reactive group More specifically, in the case of polycarbonate resin, A carbonyl group is a linking group, and a partial structure sandwiched between adjacent carbonyl groups is called a structural unit. In this specification, the weight ratio of each structural unit in the polycarbonate resin is The total weight of all structural units and linking groups is calculated as 100% by weight.

[0022] The method for producing a polycarbonate resin of the present invention is a process for producing a dihydroxy group having an acetal group in a part of the structure. A hydroxy compound (hereinafter sometimes referred to as "dihydroxy compound (A)") and a carbonate A diester and a polymerization catalyst are continuously fed into a reactor to carry out a melt polycondensation reaction to produce polycarbonate. A method for producing a carbonate resin, comprising dissolving a compound represented by the following formula (1) in a raw material dissolving tank: A process for dissolving a dihydroxy compound (A) in a solvent containing a hydroxy compound as a main component. The method is characterized in that the solvent contains a basic compound.

[0023] [ka]

[0024] R in formula (1) 1 , R 2 each independently represents a hydrogen atom, an optionally substituted carbon atom an alkyl group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms which may be substituted, an alkoxy group having 1 to 10 carbon atoms which may have a substituent; It is a alkyl ester group.

[0025] The dihydroxy compound (A) used in the method of the present invention contains an acetal group in a part of its structure. Acetal groups undergo decomposition reactions such as hydrolysis when even a trace amount of acidic substances are present. In addition, the liquefaction of the dihydroxy compound (A) and the continuous polymerization method described below are easily performed. The heat of holding the amines may accelerate the decomposition reaction. If a polymerization reaction is carried out in the presence of a polyfunctional alcohol, the polymer Branched structures are generated in the molecule, and the molecular weight distribution increases. The branched structure improves the melt processing properties and functionality of the resin. In order to change the mechanical properties, etc., the decomposition of the dihydroxy compound (A) is suppressed, and the obtained This makes it possible to stabilize the quality of the polycarbonate resin.

[0026] In the method of the present invention, a monohydroxy compound represented by the above formula (1) is mainly dissolved in a raw material dissolving tank. The method includes a step of dissolving a dihydroxy compound (A) in a solvent containing the dihydroxy compound (A) as an ingredient. Since the silicon compound (A) has a relatively high melting point, a high temperature is required to melt it alone. Therefore, the melting point of the dihydroxy compound (A) is lower than that of the dihydroxy compound (A). In a solvent containing as a main component a monohydroxy compound represented by the formula (1) having solubility By dissolving the dihydroxy compound (A), the dissolution temperature is kept low and the decomposition reaction described above is prevented. In addition, the monohydroxy compound represented by the formula (1) can suppress the polymerization reaction. Since the monohydroxy compound produced in the polymerization process is also a by-product, By purifying it as necessary, it can be reused, reducing costs and the environmental impact. It is.

[0027] Furthermore, the present invention relates to a process for producing a hydroxy compound represented by the formula (1) The solvent containing the dihydroxy compound (A) contains a basic compound. By contacting the material with a basic compound before use, acidic impurities can be neutralized and decomposition can be suppressed. The basic compound used here is carried over directly into the polymerization process. Use a compound that does not adversely affect the polymerization reactivity or the quality of the resulting polycarbonate resin. Therefore, the basic compound for stabilizing the dihydroxy compound (A) is preferably It is preferable to use the polymerization catalyst used in the method of the present invention. The detailed method will be described below. .

[0028] [Raw material for polycarbonate resin] The polycarbonate resin of the present invention is a dihydroxylated polycarbonate having an acetal group in a part of its structure. The dihydroxy compound (A) contains a structural unit derived from the compound (A) having the structure There is no particular restriction as long as it has an acetal group in part, but a dialkyl group having a cyclic acetal structure is also preferred. A dihydroxy compound having a cyclic acetal structure is preferred. Examples of the esters include those represented by the following formula (2) incorporating a structure derived from pentaerythritol: Spiroglycol (also known as 3,9-bis(1,1-dimethyl-2 -hydroxyethyl-2,4,8,10-tetraoxaspiro[5,5]undecane) , dioxane glycol ( Synonyms: 2-(1,1-dimethyl-2-hydroxyethyl)-5-ethyl-5-hydroxy Methyl-1,3-dioxane), the ino Dihydroxy compounds incorporating structural units derived from sitol can be used. .

[0029] [ka]

[0030] Polycarbonate resin using such a dihydroxy compound containing an acetal group It has excellent heat resistance and optical properties, especially a low photoelastic coefficient, making it suitable for optical film applications. Among the dihydroxy compounds mentioned above, ethylenediaminetetraacetate is the most popular due to its high performance and easy availability. From the standpoint of suitability, spiro glycols are particularly useful.

[0031] In the polycarbonate resin of the present invention, the structural unit derived from the dihydroxy compound (A) is The content is preferably 1% by weight or more and 90% by weight or less. The lower limit is more preferably 5% by weight or more. The upper limit is preferably 80% by weight or less, and more preferably 70% by weight or less. By setting the content in this range, excellent optical properties of the dihydroxy compound (A) can be obtained. Obtain a resin that has excellent balance of various physical properties such as melt processability and mechanical properties while expressing its characteristics. It is possible.

[0032] The acetal group of the dihydroxy compound (A) has a structure that is vulnerable to acid and decomposes. The polyfunctional alcohol such as pentaerythritol is produced, and the resulting polycarbonate is This may increase the molecular weight distribution of the acrylate resin and change the physical properties of the resin. In the synthesis of the silyl compound (A), a strong acid is generally used as a catalyst. (A) may contain a small amount of residual acid catalyst. ) is preferably such that the content of this acid catalyst and other acidic substances is 5 ppm by weight or less. It is more preferably 3 ppm by weight or less, and particularly preferably 1 ppm by weight or less.

[0033] The polycarbonate resin of the present invention has a structural unit other than that derived from the dihydroxy compound (A). (hereinafter, may be referred to as "other structural units") Examples of compounds that form other structural units include aliphatic dihydroxy compounds, alicyclic compounds, Dihydroxy compounds, oxyalkylene glycols, aromatic-containing dihydroxy compounds, Diester compounds are also included. The polycarbonate resins embedded therein are referred to as polyester carbonate resins. In the present specification, the term "polycarbonate resin" includes polyester carbonate resin. .

[0034] Examples of the aliphatic dihydroxy compound include ethylene glycol and 1,2-propane Diol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol 1,4-butanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-Pentanediol, 1,5-Pentanediol, 1,2-Hexanediol, 1 ,3-Hexanediol, 1,4-Hexanediol, 1,5-Hexanediol, 1, 6-Hexanediol, 1,7-Heptanediol, 1,8-Octanediol, 1,9 -nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,1 Linear aliphatic dihydroxy compounds such as 2-dodecanediol, neopentyl glycol, 2 -Ethyl-1,6-hexanediol, 2,2,4-trimethyl-1,6-hexanediol Branched chain aliphatic diglycerides such as hydrogenated dilinoleyl glycol, hydrogenated dioleyl glycol, etc. Examples of hydroxy compounds include ethylene glycol, 1,3 -Propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol Xanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nona 1,10-Decanediol, 1,11-Undecanediol, 1,12-Decanediol Linear aliphatic dihydroxy compounds such as decanediol are easy to obtain and handle. This is preferable from the viewpoint of compactness.

[0035] Examples of the alicyclic dihydroxy compound include the following dihydroxy compounds: A dihydroxy compound represented by the following formula (4), 1,2-cyclohexanedimethanol, 1,3-Cyclohexanedimethanol, 1,4-Cyclohexanedimethanol, Tricyclo Rhodecane dimethanol, pentacyclopentadecanedimethanol, 2,6-decalin dimethanol Methanol, 1,5-decalin dimethanol, 2,3-decalin dimethanol, 2,3- Norbornane dimethanol, 2,5-norbornane dimethanol, 1,3-adamantanedimethanol Examples include dihydroxy compounds derived from terpene compounds such as methanol and limonene. Dihydroxy compounds that are primary alcohols of alicyclic hydrocarbons; 1,2-cyclohexyl Sandiol, 1,4-cyclohexanediol, 1,3-adamantanediol, hydrogenated Bisphenol A, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, etc. Examples of dihydroxy alicyclic hydrocarbons include secondary and tertiary alcohols. compound.

[0036] [ka]

[0037] The dihydroxy compound represented by the above formula (4) is a stereoisomeric compound. These dihydroxy compounds (1 ), which is an abundant and readily available resource and is produced from various starches. Isosorbide, which is obtained by dehydrating and condensing sorbitol, is easy to obtain and produce, and is easy to mold. Most desirable from a sexual standpoint. These dihydroxy compounds (4) may be used alone or in combination of two or more. It may also be used in combination.

[0038] Examples of oxyalkylene glycols include diethylene glycol, triethylene glycol, ethylene glycol, tetraethylene glycol, polyethylene glycol, polypropylene glycol Licor, polytetramethylene glycol, etc. can be used.

[0039] Examples of aromatic dihydroxy compounds include the following dihydroxy compounds: 2,2-bis(4-hydroxyphenyl)propane, 2,2-bis(3-methyl-4 -hydroxyphenyl)propane, 2,2-bis(4-hydroxy-3,5-dimethylphenyl)propane 2,2-bis(4-hydroxy-3,5-diethylphenyl)propane, 2,2-bis(4-hydroxy-(3-phenyl)phenyl)propane, 2,2-bis Bis(4-hydroxy-(3,5-diphenyl)phenyl)propane, 2,2-bis(4- Hydroxy-3,5-dibromophenyl)propane, Bis(4-hydroxyphenyl)methan ethane, 1,1-bis(4-hydroxyphenyl)ethane, 2,2-bis(4-hydroxy phenyl)butane, 2,2-bis(4-hydroxyphenyl)pentane, 1,1-bis( 4-hydroxyphenyl)-1-phenylethane, bis(4-hydroxyphenyl)diphenyl Phenylmethane, 1,1-bis(4-hydroxyphenyl)-2-ethylhexane, 1,1 -Bis(4-hydroxyphenyl)decane, Bis(4-hydroxy-3-nitrophenyl )methane, 3,3-bis(4-hydroxyphenyl)pentane, 1,3-bis(2-(4 -hydroxyphenyl)-2-propyl)benzene, 1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene 2,2-bis(4-hydroxyphenyl)hexaphenyl 1,1-bis(4-hydroxyphenyl)cyclohexane, bis( 4-Hydroxyphenyl)sulfone, 2,4'-dihydroxydiphenylsulfone, bis (4-hydroxyphenyl)sulfide, bis(4-hydroxy-3-methylphenyl) Sulfide, bis(4-hydroxyphenyl) disulfide, 4,4'-dihydroxydi Phenyl ether, 4,4'-dihydroxy-3,3'-dichlorodiphenyl ether, etc. Aromatic bisphenol compounds; 2,2-bis(4-(2-hydroxyethoxy)phenyl 2,2-bis(4-(2-hydroxypropoxy)phenyl)propane, 1,3-Bis(2-hydroxyethoxy)benzene, 4,4'-bis(2-hydroxyethoxy)benzene aromatic aromatic compounds such as bis(4-(2-hydroxyethoxy)phenyl)sulfone, bis(4-(2-hydroxyethoxy)phenyl)sulfone, etc. Dihydroxy compounds containing ether groups attached to aromatic groups; 9,9-bis(4-(2-hydroxyphenyl) 9,9-bis(4-hydroxyphenyl)fluorene, Fluorene, 9,9-bis(4-hydroxy-3-methylphenyl)fluorene, 9,9- Bis(4-(2-hydroxypropoxy)phenyl)fluorene, 9,9-bis(4-( 2-hydroxyethoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2 -hydroxypropoxy)-3-methylphenyl)fluorene, 9,9-bis(4-(2 -hydroxyethoxy)-3-isopropylphenyl)fluorene, 9,9-bis(4- (2-hydroxyethoxy)-3-isobutylphenyl)fluorene, 9,9-bis(4 -(2-hydroxyethoxy)-3-tert-butylphenyl)fluorene, 9,9- Bis(4-(2-hydroxyethoxy)-3-cyclohexylphenyl)fluorene, 9 ,9-Bis(4-(2-hydroxyethoxy)-3-phenylphenyl)fluorene, 9 ,9-Bis(4-(2-hydroxyethoxy)-3,5-dimethylphenyl)fluorene , 9,9-bis(4-(2-hydroxyethoxy)-3-tert-butyl-6-methyl phenyl)fluorene, 9,9-bis(4-(3-hydroxy-2,2-dimethylpropionyl) Dihydroxy compounds having a fluorene ring, such as (phenyl)oxyfluorene.

[0040] Examples of the diester compound include the following dicarboxylic acids: Taric acid, phthalic acid, isophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyl Phenyl ether dicarboxylic acid, 4,4'-benzophenone dicarboxylic acid, 4,4'-diphenyl Phenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 2,6-naphthalene Aromatic dicarboxylic acids such as phthalenedicarboxylic acid; 1,2-cyclohexanedicarboxylic acid; Alicyclic compounds such as 1,3-cyclohexanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid Dicarboxylic acids; malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid Aliphatic dicarboxylic acids such as , azelaic acid, and sebacic acid. The dicarboxylic acid itself can be used as a raw material for polyester carbonate resin. Depending on the production method, dicarboxylic acid esters such as methyl esters and phenyl esters may be used. Alternatively, dicarboxylic acid derivatives such as dicarboxylic acid halides can be used as the raw material.

[0041] When other structural units are introduced into the polycarbonate resin of the present invention, the heat resistance and melt processability are improved. It is preferable to use it for the purpose of adjusting the properties, optical properties, mechanical properties, compatibility with other resins, etc. Among the other structural units mentioned above, the ones that have the optical and mechanical properties required for optical film applications are From the viewpoint of adjusting the desired physical properties, aliphatic dihydroxy compounds and alicyclic dihydroxy compounds are Among them, it is more preferable to use an alicyclic dihydroxy compound. The dihydroxy compound represented by the above formula (4), 1,4-cyclohexane dimethanol Particularly useful are tricyclodecane dimethanol and tricyclodecane dimethanol.

[0042] When the polycarbonate resin of the present invention contains other structural units, The content of other structural units in the copolymer resin is preferably 1% by weight or more, and more preferably 5% by weight or more. More preferably, the content is 10% by weight or more, and particularly preferably 10% by weight or more. Also, the content is preferably 80% by weight or less. It is more preferably 70% by weight or less, and particularly preferably 60% by weight or less. Without significantly impairing the excellent properties of the dihydroxy compound (A), such as heat resistance and melt processability, The balance of the physical properties of the polycarbonate resin of the present invention can be adjusted. When two or more structural units are contained as structural units, the content of the other structural units shall be The total value of these two items shall be used.

[0043] Copolymerization of aromatic dihydroxy compounds and diester compounds such as bisphenol compounds When used as a synthetic component, it may be possible to improve the heat resistance of polycarbonate resin. However, on the other hand, if polycarbonate resin contains a lot of aromatic structures, the optical properties, especially the optical The elastic modulus tends to deteriorate. In addition, bisphenol compounds and diester compounds Since there is a large difference in the polymerization reactivity of the hydroxy compound (A), the bisphenol compound or diester compounds remain on the terminal groups, resulting in a high molecular weight polycarbonate resin. In order to accelerate the reaction, the reaction temperature is increased, and the mechanical properties tend to deteriorate. When the temperature is raised higher, the dihydroxy compound (A) is thermally decomposed, and the resulting polycarbonate resin is For these reasons, aromatic diolefins tend to be colored and branched. Structural units derived from hydroxy compounds or diester compounds (represented by the following formula (5) The content of the structural unit derived from the compound (excluding the structural unit derived from the compound) is preferably 10% by weight or less, and more preferably 5% by weight or less. % by weight or less is more preferable.

[0044] The polycarbonate resin of the present invention contains, as another structural unit, a polycarbonate represented by the following formula (4): It may contain a structural unit derived from a compound.

[0045] [ka]

[0046] In the resin used in the present invention, the structural unit represented by the formula (4) is 5% by mass or more, The content is preferably 80% by mass or less, and the upper limit is more preferably 70% by mass or less. The lower limit is preferably 10% by mass or more, more preferably 15% by mass or more. When the content of the structural unit represented by the formula (4) is within the above range, This results in a resin with better mechanical properties and heat resistance and a lower photoelasticity coefficient.

[0047] The polycarbonate resin of the present invention contains a compound represented by the following formula (5) as another structural unit. The copolymer may contain structural units derived from a compound.

[0048] [ka]

[0049] In formula (5), R 3 and R 4 each independently represents a direct bond, a carbon atom which may have a substituent, R is an alkylene group having a prime number of 1 to 4.5 ~R 10 each independently represents a hydrogen atom or a substituent an alkyl group having 1 to 10 carbon atoms which may have a substituent; aryl group having 1 to 15 carbon atoms which may have a substituent; an alkoxy group having 1 to 10 carbon atoms which may have a substituent, an aryloxy group having 1 to 10 carbon atoms which may have a substituent; an amino group which may have a group; a vinyl group having 2 to 10 carbon atoms which may have a substituent; An ethynyl group having 2 to 10 carbon atoms which may have a substituent, a sulfur atom which has a substituent, is a silicon atom having a group, a halogen atom, a nitro group, or a cyano group, provided that R 5 ~ R 10 At least two adjacent groups among X may be bonded to each other to form a ring. is a hydroxy group, a carboxy group, an alkyl group having 1 to 10 carbon atoms which may have a substituent An ester group or an aryl ester group having 6 to 15 carbon atoms which may have a substituent.

[0050] The structural unit derived from the compound represented by the formula (5) has physical properties such as heat resistance and photoelastic coefficient. By strictly controlling the content ratio, the retardation is smaller for shorter wavelengths. This allows the so-called reverse wavelength dispersion to be expressed with high efficiency, and is useful for optical films. In particular, when used as a quarter wave plate, it has ideal retardation characteristics over a wider wavelength range. In addition, the structural unit derived from the compound represented by the formula (5) has a negative Since it has birefringence, a structural unit derived from a dihydroxy compound (A) having positive birefringence By combining it with a polymer having an intrinsic birefringence close to zero, it is possible to obtain a polymer having an intrinsic birefringence close to zero.

[0051] The compound represented by the formula (5) is 3 is an alkylene group with 2 carbon atoms Particularly preferred. 4 R is particularly preferably an alkylene group having one carbon atom. 5 ~R 10 is a hydrogen atom is particularly preferred. X is particularly preferred to be an aryl ester group. By selecting the structure, it is possible to create structural units with excellent physical properties such as optical properties, heat resistance, and thermal stability. It is possible.

[0052] The content ratio of the structural unit derived from the compound represented by the formula (5) depends on the desired physical properties. However, the content is preferably 1% by weight or more and 70% by weight or less. % or more and 50% by weight or less is preferable, and 10% by weight or more and 30% by weight or less is more preferable.

[0053] [Manufacturing method of polycarbonate resin] The method for producing a polycarbonate resin of the present invention is a process for producing a dihydroxy group having an acetal group in a part of the structure. The hydroxy compound (A), the carbonic acid diester, and the polymerization catalyst are continuously fed to a reactor. The polycarbonate resin is produced by a melt polycondensation reaction. The process includes at least a raw material preparation step and a polymerization step, which will be described later.

[0054] Generally, polycarbonate resins can be produced by a variety of polymerization methods. Solution polymerization using sulphonic acid or carboxylic acid halide, or interfacial polymerization, or solvent-free polymerization In the method of the present invention, the melt polymerization method is The melt polymerization method does not use solvents or highly toxic compounds, so it is environmentally friendly. This reduces the load and improves productivity.

[0055] When producing a resin by melt polymerization, the dihydroxy compound (A) is used. A hydroxy compound, a carbonic acid diester, and a polymerization catalyst are mixed and subjected to a polycondensation reaction under molten conditions. The reaction rate is increased while removing the detached components from the system. At the end of the polymerization, the reaction is carried out under high temperature and high vacuum conditions. The reaction is allowed to proceed to the desired molecular weight under these conditions. When the reaction is complete, the molten resin is removed from the reactor. Thus, the polycarbonate resin of the present invention is obtained.

[0056] Carbonate diester The polycarbonate resin of the present invention is a dihydroxy compound having a dihydroxy compound (A) as an essential component. It is obtained by polycondensation of an oxy compound and a carbonic acid diester through an ester exchange reaction. The carbonic acid diester used in the method of the present invention is represented by the following formula (3): It is preferable to use a compound that is

[0057] [ka]

[0058] R in Equation (3) 1 , R 2 each independently represents a hydrogen atom, an optionally substituted carbon atom an alkyl group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms which may be substituted, an alkoxy group having 1 to 10 carbon atoms which may have a substituent; It is a alkyl ester group.

[0059] The optionally substituted alkyl group having 1 to 10 carbon atoms includes a methyl group, an ethyl group, -Linear groups such as n-propyl, n-butyl, n-pentyl, n-hexyl, and n-decyl alkyl group; isopropyl group, 2-methylpropyl group, 2,2-dimethylpropyl group, Branched alkyl groups such as 2-ethylhexyl; cyclopropyl, cyclopentyl Examples of the alkyl group include cyclic alkyl groups such as a cycloalkyl group, a cyclohexyl group, and a cyclooctyl group.

[0060] Examples of the optionally substituted acyl group having 1 to 10 carbon atoms include a formyl group, an acetyl group, Propionyl group, 2-methylpropionyl group, 2,2-dimethylpropionyl group, 2-ethylpropionyl group, aliphatic acyl groups such as 1-ethylhexanoyl group; benzoyl group, 1-naphthylcarbonyl group, 2 Examples of aromatic acyl groups include aromatic acyl groups such as 2-naphthylcarbonyl and 2-furylcarbonyl.

[0061] The optionally substituted alkoxy group having 1 to 10 carbon atoms includes a methoxy group, an ethoxy group, alkoxy groups such as isopropoxy and t-butoxy groups; acyloxy groups such as acetoxy groups Examples of such groups include silyl groups.

[0062] Examples of the alkyl ester group having 1 to 10 carbon atoms which may have a substituent include methyl ester. Examples of the aryl group include ethyl ester and ethyl ester.

[0063] R in Equation (3) 1 , R 2 each independently represents a hydrogen atom or an optionally substituted carbon atom It is more preferable that the alkyl group has a number of 1 to 10. In this case, the reactivity and availability are improved. It is superior in ease of use. Among the carbonate diesters represented by the above formula (3), from the viewpoints of reactivity and availability, , diphenyl carbonate is particularly preferred.

[0064] When carbonic acid diesters react, monohydroxy compounds are produced as by-products. When diphenyl carbonate is used, phenol is produced as a by-product. The product is preferably recovered and, if necessary, purified by a method such as distillation and reused. In this study, the recovered monohydroxy compound phenol was converted into a dihydroxy compound (A ) can be recycled and reused within the manufacturing process, making it economical. do.

[0065] Polymerization catalyst The polycondensation reaction is carried out using an ester exchange reaction catalyst (hereinafter, the ester exchange reaction catalyst is referred to as the "polymerization catalyst"). The type of polymerization catalyst determines the reaction rate of the transesterification reaction and the amount of the product. This can have a significant impact on the quality of the polycarbonate resin that is produced.

[0066] The polymerization catalyst is used to improve the transparency, color, optical properties, and heat resistance of the resulting polycarbonate resin. There are no particular limitations as long as the polymerization catalyst satisfies the requirements for mechanical properties. , Group I or Group II in the long-form periodic table (hereinafter referred to simply as "Group 1" and "Group 2" (compounds of metals such as basic boron compounds, basic phosphorus compounds, basic ammonia compounds, etc.) Among them, basic compounds such as ammonium compounds and amine compounds can be used. The polycarbonate resin obtained has a good color tone. Since the decomposition suppression effect of the oxy compound (A) is high, the oxy compound (A) is a Group 1 metal compound and / or a Group 2 metal compound. A mixture is preferred.

[0067] Examples of Group 1 metal compounds include the following compounds: sodium hydroxide, water Potassium oxide, lithium hydroxide, cesium hydroxide, sodium bicarbonate, potassium bicarbonate Lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate , cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, stearyl acetate, Sodium stearate, potassium stearate, lithium stearate, cesium stearate ammonium, sodium borohydride, potassium borohydride, lithium borohydride, Cesium boron, sodium phenylborate, potassium phenylborate, phenylborate Lithium boron, cesium phenyl boron, sodium benzoate, potassium benzoate, Lithium benzoate, Cesium benzoate, Disodium hydrogen phosphate, Dipotassium hydrogen phosphate , dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, phenyl Dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, sodium Alcoholates, phenolates, and bisphenol A of potassium, lithium, and cesium Disodium salt, dipotassium salt, dilithium salt, dicesium salt, etc. Group 1 metal compounds In terms of polymerization activity and the color tone of the resulting polycarbonate resin, lithium compounds are preferred. I wish.

[0068] Examples of Group 2 metal compounds include the following compounds: calcium hydroxide, water Barium oxide, magnesium hydroxide, strontium hydroxide, calcium bicarbonate, carbonate Barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, carbonic acid Barium, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, vinegar Magnesium acetate, Strontium acetate, Calcium stearate, Barium stearate , magnesium stearate and strontium stearate. Group 2 metal compounds The catalyst is preferably a magnesium compound, a calcium compound or a barium compound, and has a polymerization activity and From the viewpoint of the color tone of the obtained polycarbonate resin, a magnesium compound and / or a calcium compound More preferred are ammonium compounds, and most preferred are calcium compounds.

[0069] In addition, a basic boronization reaction may be carried out in conjunction with the Group 1 metal compound and / or the Group 2 metal compound. basic compounds such as basic phosphorus compounds, basic ammonium compounds, and amine compounds However, it is preferable to use only Group 1 metal compounds and / or Group 2 metal compounds. From the viewpoint of the color tone of the resulting polycarbonate resin, it is more preferable to use a Group 2 metal It is most preferred that the compound be used alone.

[0070] The amount of the polymerization catalyst used was 0.1 mole per mole of the total dihydroxy compounds used in the reaction. μmol or more is preferred, 0.5 μmol or more is more preferred, and 1 μmol or more is particularly preferred. The amount of the polymerization catalyst used is preferably 1 mole per mole of the total dihydroxy compounds used in the reaction. Preferably, the amount is 300 μmol or less, more preferably 100 μmol or less, and more preferably 50 μmol or less. By adjusting the amount of the polymerization catalyst used within the above range, the polymerization rate can be reduced. This allows the polymerization temperature to be kept low, and prevents reactions that cause quality degradation such as coloration and thermal decomposition. It becomes possible to obtain a polycarbonate resin having a desired molecular weight while suppressing the reaction.

[0071] In the method of the present invention, the polymerization catalyst is used also as a stabilizer for the dihydroxy compound (A). Generally, the position of the polymerization catalyst may be any position before the polymerization step. In the above method, it is preferable to add the dihydroxy compound (A) to a dissolving tank. In this case, the basic compound and the polymerization catalyst used in the dissolution tank of the dihydroxy compound (A) In this way, the polymerization catalyst, which is a basic compound, can remove acidic impurities. The decomposition of the dihydroxy compound (A) can be suppressed by neutralizing the dihydroxy compound (A). The law will be discussed later.

[0072] The polycondensation reaction is carried out by adjusting the molar ratio of all dihydroxy compounds and all diester compounds used in the reaction. By carefully adjusting the reaction rate, it is possible to control the molecular weight of the resulting resin. In the case of the ethylene resin, the molar ratio of all diester compounds to all dihydroxy compounds is 0.9 It is preferable to adjust it to 0 to 1.10, and more preferably to adjust it to 0.95 to 1.05. It is particularly preferable to adjust the molar ratio to 0.97 to 1.03. If the distance is too far off, a resin having the desired molecular weight cannot be produced.

[0073] The melt polymerization process is usually carried out in two or more stages. The reaction may be carried out in two or more steps by sequentially changing the conditions using two or more reactors. From the viewpoint of production efficiency, the process may be carried out in two or more steps by changing the conditions for each step. It is preferable to carry out the reaction using two or more reactors, preferably three or more reactors. The polymerization reaction may be carried out in a batch system, a continuous system, or a combination of a batch system and a continuous system. However, in the method of the present invention, a continuous system is used from the viewpoints of production efficiency and quality stability.

[0074] In order to control the reaction rate and the quality of the polycarbonate resin, the melt polycondensation reaction is carried out The molar ratio of the dihydroxy compound to the diester compound must be strictly controlled. Since it is difficult to obtain the quantitative accuracy required by the method of supplying solids, the raw material of polycarbonate resin is Dihydroxy compounds and diester compounds used as fuels are usually gassed with nitrogen or argon. Melting is carried out in an inert gas atmosphere using a batch, semi-batch, or continuous stirred tank type apparatus. Treated as a liquid.

[0075] [Raw material preparation process] In the manufacturing method of the present invention, as a part of the raw material preparation step, a raw material dissolving tank is used to dissolve the raw material represented by the above formula (1). The dihydroxy compound (A) is added to a solvent containing the monohydroxy compound as a main component. The method further comprises a step of dissolving the solvent in the solvent (dissolving step), the solvent containing a basic compound.

[0076] ·solvent In the method of the present invention, a solvent for the dihydroxy compound (A) is used which is represented by the following formula (1): A solvent containing a monohydroxy compound as the main component is used. This allows the dihydroxy compound to be The temperature required to dissolve the substance (A) can be lowered and the time required for dissolution can be shortened. The decomposition of the dihydroxy compound can be effectively suppressed. If the dihydrogen ether is used in a solvent or in an inappropriate solvent, high temperatures are required for dissolution. Decomposition reactions of the oxy compounds occur, and the physical properties of the resulting polymer cannot be controlled.

[0077] [ka]

[0078] R in formula (1) 1 , R 2 each independently represents a hydrogen atom, an optionally substituted carbon atom an alkyl group having 1 to 10 carbon atoms, an acyl group having 1 to 10 carbon atoms which may be substituted, an alkoxy group having 1 to 10 carbon atoms which may have a substituent; It is a alkyl ester group.

[0079] The optionally substituted alkyl group having 1 to 10 carbon atoms includes a methyl group, an ethyl group, -Linear chains such as n-propyl, n-butyl, n-pentyl, n-hexyl, and n-decyl alkyl group; isopropyl group, 2-methylpropyl group, 2,2-dimethylpropyl group, Branched alkyl groups such as 2-ethylhexyl; cyclopropyl, cyclopentyl Examples of the alkyl group include cyclic alkyl groups such as a cycloalkyl group, a cyclohexyl group, and a cyclooctyl group.

[0080] Examples of the optionally substituted acyl group having 1 to 10 carbon atoms include a formyl group, an acetyl group, Propionyl group, 2-methylpropionyl group, 2,2-dimethylpropionyl group, 2-ethylpropionyl group, aliphatic acyl groups such as 1-ethylhexanoyl group; benzoyl group, 1-naphthylcarbonyl group, 2 Examples of aromatic acyl groups include aromatic acyl groups such as 2-naphthylcarbonyl and 2-furylcarbonyl.

[0081] The optionally substituted alkoxy group having 1 to 10 carbon atoms includes a methoxy group, an ethoxy group, alkoxy groups such as isopropoxy and t-butoxy groups; acyloxy groups such as acetoxy groups Examples of such groups include silyl groups.

[0082] Examples of the alkyl ester group having 1 to 10 carbon atoms which may have a substituent include methyl ester. Examples of the aryl group include ethyl ester and ethyl ester. R in formula (1) 1 , R 2 each independently represents a hydrogen atom or an optionally substituted carbon atom It is more preferable that the alkyl group has a number of 1 to 10. In this case, the reactivity and availability are improved. From a similar perspective, R 1 , R 2 It is good that both are hydrogen atoms. preferable.

[0083] From the viewpoint of solubility, the solvent is, with the total weight of the solvent being 100% by weight, It is preferable that the composition contains 50% by weight or more of a monohydroxy compound represented by the formula (I), and more preferably 70% by weight or more of the monohydroxy compound represented by the formula (I). It is more preferable that the content is 85% by weight or more, and further preferably that the content is 95% by weight or more. It is particularly preferable to use the above-mentioned polycarbonate resin. From the viewpoint of excellent economic rationality, the monohydroxy group represented by the above formula (1) is It is most preferable to use a solvent consisting of the compound alone.

[0084] The monohydroxy compound represented by the following formula (1) is used in the method of the present invention. The solvent contains a compound other than the monohydroxy compound represented by the following formula (1) as a solvent component. However, if the solvent contains a large amount of carbonic acid diester, moisture may accumulate in the raw material dissolution tank. If carbon dioxide is introduced, the ester will hydrolyze and the diester / diol mixture will be produced. The carbonyl ratio in the solvent may vary, making it difficult to control the molecular weight of the resin. The weight ratio of the acid diester is less than 50% by weight, based on the total weight of the solvent being 100% by weight. It is preferable that the content is 10% by weight or less, and more preferable that the content is 5% by weight or less. is more preferable, and it is particularly preferable that it is substantially free of the above.

[0085] The monohydroxy compound used as the solvent for the dihydroxy compound (A) is It is preferable to use the same compound as the carbonic acid diester elimination component described above. When diphenyl carbonate is used as the monohydroxy compound, phenol is used as the monohydroxy compound. In this way, it is preferable to use a polycarbonate having a high polymerization reactivity and a high yield. The quality of the polymer resin is not affected, and the process of distilling and purifying the polymerization distillate described below is also performed. In the process, it is recovered together with the dihydroxy compound produced as a by-product in the polymerization reaction and reused. can be done.

[0086] Basic compounds The solvent used in the method of the present invention contains as a main component a monohydroxy compound represented by formula (1). The medium contains a basic compound. The dihydroxy compound (A) used in the present invention is decomposed by the effects of heat and traces of acidic impurities. During the raw material preparation process, the material may decompose while being handled in a molten state, resulting in the formation of branched components. However, this side effect can be suppressed by including a basic compound in the solvent.

[0087] The basic compound is not particularly limited, but examples thereof include compounds of Group I of the long periodic table, or II group (hereinafter simply referred to as "Group 1" and "Group 2") metal compounds, and bases Salts of basic boron compounds, basic phosphorus compounds, basic ammonium compounds, amine compounds, etc. Among them, the following compounds are preferred because they have good polymerization activity and the resulting polymer is The color tone of the carbonate resin is good, and the decomposition suppression effect of the dihydroxy compound (A) is excellent. Since the electrochemical activity is high, Group 1 metal compounds and / or Group 2 metal compounds are preferred.

[0088] Examples of Group 1 metal compounds include the following compounds: sodium hydroxide, water Potassium oxide, lithium hydroxide, cesium hydroxide, sodium bicarbonate, potassium bicarbonate Lithium hydrogen carbonate, cesium hydrogen carbonate, sodium carbonate, potassium carbonate, lithium carbonate , cesium carbonate, sodium acetate, potassium acetate, lithium acetate, cesium acetate, stearyl acetate, Sodium stearate, potassium stearate, lithium stearate, cesium stearate ammonium, sodium borohydride, potassium borohydride, lithium borohydride, Cesium boron, sodium phenylborate, potassium phenylborate, phenylborate Lithium boron, cesium phenyl boron, sodium benzoate, potassium benzoate, Lithium benzoate, Cesium benzoate, Disodium hydrogen phosphate, Dipotassium hydrogen phosphate , dilithium hydrogen phosphate, dicesium hydrogen phosphate, disodium phenylphosphate, phenyl Dipotassium phenylphosphate, dilithium phenylphosphate, dicesium phenylphosphate, sodium Alcoholates, phenolates, and bisphenol A of potassium, lithium, and cesium Disodium salt, dipotassium salt, dilithium salt, dicesium salt, etc. Group 1 metal compounds In terms of polymerization activity and the color tone of the resulting polycarbonate resin, lithium compounds are preferred. I wish.

[0089] Examples of Group 2 metal compounds include the following compounds: calcium hydroxide, water Barium oxide, magnesium hydroxide, strontium hydroxide, calcium bicarbonate, carbonate Barium hydrogen carbonate, magnesium hydrogen carbonate, strontium hydrogen carbonate, calcium carbonate, carbonic acid Barium, magnesium carbonate, strontium carbonate, calcium acetate, barium acetate, vinegar Magnesium acetate, Strontium acetate, Calcium stearate, Barium stearate , magnesium stearate and strontium stearate. Group 2 metal compounds The catalyst is preferably a magnesium compound, a calcium compound or a barium compound, and has a polymerization activity and From the viewpoint of the color tone of the obtained polycarbonate resin, a magnesium compound and / or a calcium compound More preferred are ammonium compounds, and most preferred are calcium compounds.

[0090] The basic compounds used in the raw material preparation process are also carried over directly to the polymerization process. It is preferable to use a compound that has no adverse effect on reactivity or on the resulting polycarbonate resin. Therefore, it is preferable to use the above-mentioned polymerization catalyst as the basic compound. The amount of the basic compound (polymerization catalyst) used in this step is determined based on the amount of the acid contained in the dihydroxy compound (A). Depending on the amount of cyclic impurities, it may be necessary to add an equimolar amount to the acidic impurities. In order to completely suppress the decomposition reaction of the silicon compound (A), the content of acidic impurities must also be sufficiently low. The amount of the basic compound (polymerization catalyst) added is reduced to the amount required for the preferred use of the polymerization catalyst described above. A range of doses is preferred.

[0091] In the raw material preparation step of the method of the present invention, a monohydroxy compound represented by the above formula (1) is The method may include a step of adding a basic compound to a solvent containing the substance as a main component. The amount of the basic compound added is 1 mol of the total dihydroxy compounds used in the melt polycondensation reaction. Preferably, the amount is 0.1 μmol or more, more preferably 0.5 μmol or more, and more preferably 1 μmol or more. The above is particularly preferred. The amount of the basic compound to be added is based on the total amount of the dihydric alcohol used in the melt polycondensation reaction. The amount of the hydroxy compound is preferably 300 μmol or less, more preferably 100 μmol or less. It is more preferable that the amount of the basic compound is 50 μmol or less, and particularly preferable that the amount of the basic compound is 50 μmol or less. By adjusting the amount, an excellent effect of inhibiting the decomposition of the dihydroxy compound (A) can be exhibited. A solvent containing the monohydroxy compound represented by the formula (1) as a main component is added with a basic compound. The timing of adding the dihydroxy compound (A) to the solvent is not particularly limited. It may be performed before, after, or simultaneously with the addition. It is preferable to add a basic compound to the solvent before adding the dihydroxy compound (A). In this case, the dihydroxy compound (A) is converted into a basic compound substantially before the application of heat. Since it comes into contact with objects, the decomposition inhibition effect is greater.

[0092] ·Dissolution process In the method of the present invention, the monohydroxy compound represented by the above formula (1) is used as a main component. The method for dissolving the dihydroxy compound (A) in a solvent containing the compound is not particularly limited. For example, a monohydroxy compound represented by the following formula (1) is melted in advance, and the melt is A method of dissolving the solid dihydroxy compound (A) in a raw material dissolving tank having a feed tank is preferred. It can be used effectively.

[0093] The procedure for dissolving the dihydroxy compound (A) is not particularly limited, but may be, for example, (a) First, a molten liquid of the monohydroxy compound represented by the formula (1) is charged into a raw material dissolving tank. Then, a basic compound is added, and then a dihydroxy compound (A) is added. ) First, a molten liquid of the monohydroxy compound represented by the formula (1) is charged into a raw material dissolving tank, Next, a procedure may be employed in which the dihydroxy compound (A) and the basic compound are added almost simultaneously. Dihydroxy compound (A) decomposes in a very short time when heat is applied. Before compound (A) is added to the raw material dissolving tank, a basic compound (polymerization catalyst) is added. Therefore, it is more preferable to adopt the procedure (A).

[0094] The internal temperature of the raw material dissolving tank is preferably 150°C or less, more preferably 140°C or less. The internal temperature of the dissolution tank is preferably 80° C. or higher, and more preferably 90° C. or higher. This makes it possible to suppress the decomposition reaction and coloring of the dihydroxy compound (A), and also to facilitate transport. It also avoids the risk of crystallization inside the pipes, etc. causing blockages.

[0095] The raw material dissolving tank may be a single tank, or two or more tanks may be connected in series. The dihydroxy compound (A) supplied to the tank is usually at room temperature. Therefore, the temperature required for dissolution is higher than the temperature required to maintain the liquid state. In this case, the part that has been completely dissolved continues to be exposed to high temperatures, making it more susceptible to thermal degradation. The liquid dissolved in the first layer is transferred to the second tank, which is kept at a lower temperature than the first tank. It is possible.

[0096] In the method of the present invention, the polymerization reaction is carried out continuously. The polymerization reaction is started by continuously supplying the above to the reaction vessel at a constant flow rate. After that, additional raw materials are periodically added so that the raw material melt does not become empty. In the dissolving process of the hydroxy compound (A), the raw material is continuously fed to the dissolving tank at a constant flow rate. At the same time, if a method is adopted in which the molten liquid is continuously discharged from the melting tank at a constant flow rate, the liquefaction and dissolution The thermal history required for maintaining the molten state can be minimized, and the residence time required for melting can be shortened. It is possible to keep the temperature constant. Decomposition of the dihydroxy compound (A) cannot be completely avoided. However, by keeping the temperature and residence time required for dissolution constant, it is possible to supply raw materials of a consistent quality to the reactor. This leads to stabilization of the quality of the resulting polycarbonate. The dihydroxy compound (A) is continuously fed to the raw material dissolving tank, and the dissolved dihydroxy compound (A) is dissolved in the raw material dissolving tank. It is particularly preferred that the solution containing compound (A) is continuously discharged from the raw material dissolver.

[0097] In a method for continuously dissolving a dihydroxy compound (A), The residence time from when the mixture is put into the dissolution tank until it is fed into the reactor is 0.5 hours or more, and 12 The upper limit is preferably 10 hours or less, and more preferably 8 hours or less. The lower limit is more preferably 1 hour or more, and particularly preferably 2 hours or more. This suppresses the decomposition reaction of the dihydroxy compound (A) and allows the raw material to be dissolved in time. In this specification, the residence time in the tank during continuous operation is defined as follows: do. Residence time [hr] = tank internal capacity [kg] / discharge amount [kg / hr]

[0098] The polymerization catalyst used is usually prepared in advance as an aqueous solution. The concentration of the aqueous catalyst solution is not particularly limited. The concentration is adjusted to an arbitrary value depending on the solubility of the catalyst in water. Other solvents such as acetone, alcohol, toluene, phenol, etc. may also be selected. The properties of the water used to dissolve the catalyst depend on the type and concentration of impurities contained. Although there is no particular limitation, distilled water, deionized water, etc. are usually preferably used.

[0099] In order to prevent the thermal deterioration of the raw materials, nitrogen or argon is used inside the equipment for the raw material preparation process and polymerization process. It is preferable to keep the atmosphere in an inert gas such as nitrogen. When solid compounds are put into the device, there is a risk that air may be entrained in the solids and become mixed in. Therefore, before adding the solid dihydroxy compound (A) to the dissolution tank, the dihydroxy compound (A) is A method of reducing or pressurizing the inside of a container that contains the compound (A) and replacing it with an inert gas, or a dissolving tank By blowing in an inert gas into the container, air can be prevented from being mixed in. By such a method, it is preferable to keep the oxygen concentration inside the dissolution tank at 0.5% by volume or less.

[0100] In order to prevent the inclusion of foreign matter from the raw materials or from the outside, the melted raw materials are filtered through a filter. In the present invention, among the multiple raw materials used, Any or all of the raw materials may be filtered, and the method is not limited thereto. No. All ingredients may be mixed together or may be filtered separately and then mixed. It is also possible to filter the reaction solution during the polycondensation reaction. Although it is possible to install a filter for each filter, it is recommended to mix all the raw materials in order to simplify the equipment. It is preferable to combine the two and then pass them through a single filter.

[0101] [Polymerization process] In a polymerization reaction, it is important to properly control the balance of temperature and pressure within the reaction system. If either the temperature or pressure is changed too quickly, unreacted monomers will enter the reaction system. As a result, the dihydroxy compound and the diester compound may be distilled out. The molar ratio may change and the desired molecular weight resin may not be obtained.

[0102] The polymerization rate varies depending on the terminal hydroxyl group, the terminal ester group, or the terminal carbonate group. Therefore, especially in continuous polymerization, the rate of unreacted monomers is controlled by the If the balance of terminal groups changes due to distillation, it becomes difficult to control the polymerization rate at a constant rate. The molecular weight of the resin depends on the melt viscosity and Because of this correlation, when the resulting resin is molded, the melt viscosity fluctuates, making it difficult to produce molded products of uniform dimensions. This may lead to problems such as not being able to obtain products.

[0103] Furthermore, if unreacted monomers are distilled off, not only the balance of the terminal groups but also the copolymerization composition of the resin will be affected. The composition of the resin of the present invention may deviate from the desired composition, and the mechanical properties and optical properties may be affected. The optical properties of polycarbonate, such as birefringence and refractive index, depend on the ratio of each structural unit in the polycarbonate resin. If the ratio is disturbed during the polycondensation reaction, the designed optical properties cannot be obtained. There is a risk that this may become

[0104] Specifically, the following reaction conditions can be adopted for the first stage reaction: That is, the internal temperature of the polymerization reactor is usually 130° C. or higher, preferably 150° C. or higher, and more preferably Preferably, the temperature is 170° C. or higher and usually 250° C. or lower, more preferably 240° C. or lower, and even more preferably The temperature is set to a range of 230°C or less. The pressure in the polymerization reactor is usually set to 70 kPa or less ( Hereinafter, pressure refers to absolute pressure.), preferably 50 kPa or less, more preferably 30 kPa or less. Pa or less, and usually 1 kPa or more, preferably 3 kPa or more, more preferably 5 kPa or more The reaction time is set within the above range. The reaction time is usually 0.1 hours or more, preferably 0.5 hours. and usually 10 hours or less, preferably 5 hours or less, more preferably 3 hours or less. Set within the range.

[0105] In the first step, the monohydroxy compound derived from the diester compound is removed from the reaction system. For example, diphenyl carbonate is used as the carbonic acid diester. In the case where the reaction is carried out in the first stage, the monohydroxy compound distilled out of the reaction system is phenyl. It's Nol.

[0106] In the first stage reaction, the lower the reaction pressure, the more the polymerization reaction can be promoted. However, on the other hand, the amount of unreacted monomer distilled off is large. In order to achieve both the promotion of the reaction by reducing the pressure, a reactor equipped with a reflux condenser should be used. It is particularly effective to use a reflux condenser in the early stages of the reaction when there is a large amount of unreacted monomer.

[0107] The second stage reaction continues as the pressure in the reaction system is gradually reduced from the pressure in the first stage. While removing monohydroxy compounds from the reaction system, the pressure in the reaction system is finally reduced to 5 kPa or less. The internal temperature is usually set to 2 kPa or less, preferably 3 kPa or less, more preferably 1 kPa or less. 10°C or higher, preferably 220°C or higher, and usually 260°C or lower, preferably 250°C or lower. The reaction temperature is preferably set to 240° C. or lower, and more preferably set to 240° C. or lower. The reaction time is usually set to 0.1 hours. or more, preferably 0.5 hours or more, more preferably 1 hour or more, and usually 10 hours or less The time is preferably set to 5 hours or less, and more preferably 3 hours or less. In order to suppress the reaction and obtain a resin with good color and thermal stability, the maximum internal temperature in all reaction stages should be The temperature is preferably 260° C. or less, more preferably 250° C. or less, and even more preferably 240° C. or less.

[0108] From the viewpoint of controlling the polymerization rate and the quality of the resulting polycarbonate resin, It is important to appropriately select the jacket temperature, internal temperature, and pressure in the reaction system. In the early stage of the polymerization reaction, a prepolymer is obtained at a relatively low temperature and low vacuum, and in the later stage of the reaction, In this case, it is preferable to increase the molecular weight to a predetermined value at a relatively high temperature and high vacuum. In the case of (a), the distillation of unreacted monomers is suppressed, and the dihydroxy compound and the diester compound are As a result, the decrease in the polymerization rate can be suppressed. It is also possible to more reliably obtain polymers with the desired molecular weight and terminal groups. do.

[0109] Once it has been confirmed that the specified melt viscosity (molecular weight) has been reached using the stirring power etc. as an indicator, Nitrogen is introduced into the reactor to return the pressure to normal pressure and stop the polymerization reaction. The resin is continuously withdrawn from the reactor and cooled to stop the polymerization reaction. The material is discharged from the cutting head in the form of strands, cooled and solidified, and cut into pellets using a rotary cutter, etc. If necessary, extrusion devolatilization, extrusion kneading, and extrusion filtration may be performed before pelletization. In this process, additives can be mixed into the resin, and low molecular weight components can be removed through a vacuum vent. Remove foreign matter by evaporating or using a polymer filter.

[0110] [Analysis of primary polymer structure of polycarbonate resin] The molecular weight distribution of the polymer can be measured by GPC analysis described later. ) decomposition occurs, and when the resulting polycarbonate resin contains a branched structure, the molecular weight The molecular weight distribution depends not only on the presence or absence of branching, but also on the type of monomer used. The results may vary depending on the type, copolymerization ratio, and molecular weight of the polymer obtained by the method of the present invention. The preferred range of the molecular weight distribution of the polycarbonate resin cannot be expressed by an absolute value. As shown in Reference Example 1 below, the dihydroxy compound (A) was not decomposed. As shown in the figure, raw materials containing a polymerization catalyst are charged all at once, and the polymerization reaction is carried out in a batch process. It is preferred that there is no increase in the molecular weight distribution of the polymer in a formulation.

[0111] In addition, if decomposition of the dihydroxy compound (A) occurs, the polymer may be decomposed by the method described below. 1 H-NMR analysis revealed that decomposition products of dihydroxy compound (A) were present at 5.7-5.8 ppm. In the method of the present invention, the peaks of different components derived from dihydroxy groups in the polymer are detected. The content of the heterogeneous component is 0.05mM relative to the total amount of structural units derived from the compound (A). It is preferably 0.03 mol % or less, more preferably 0.05 mol % or less, and more preferably 0.05 mol % or less. It is especially preferred that it be 0.01 mol % or less.

[0112] [Additives] In the range not impairing the effect of the present invention, catalyst deactivators, antioxidants, heat stabilizers, light stabilizers, purple Radiation absorbing agents, release agents, lubricants, fillers, anti-fogging agents, anti-blocking agents, Coloring agent, flame retardant, antistatic agent, conductive agent, crosslinking agent, crosslinking assistant, metal deactivator, molecular weight The polycarbonate resin of the present invention is blended with a regulator, an antibacterial agent, a fluorescent brightener, a light diffusing agent, etc. It is possible.

[0113] In addition, polycarbonate, polypropylene, etc. are used to improve the mechanical properties and solvent resistance of resins. Ester, polyamide, polystyrene, polyolefin, acrylic, amorphous polyolefin Polymers kneaded with one or more synthetic resins such as olefin, ABS, AS, and rubber. -Alloys may also be used.

[0114] The additives and modifiers may be added to the resin of the present invention by tumble mixing the components together or in any order. Rack, V-type blender, Nauta mixer, Banbury mixer, kneading roll, extruder, etc. The mixture can be produced by mixing with a mixer such as a mixer described above. Among them, the mixture can be produced by mixing with an extruder, particularly a twin screw extruder. Kneading is preferred from the viewpoint of improving dispersibility.

[0115] [Recovery of by-products] The monohydroxy compounds produced as by-products in the polymerization reaction are collected in tanks to make efficient use of resources. From this viewpoint, it is preferable to recover the recovered material by purification as necessary and then reuse the recovered material. In the case of phenol, it can be used as a raw material for diphenyl carbonate and bisphenol A. In the method of the present invention, a part of the recovered monohydroxy compound can be converted into dihydroxy compound. It can be reused as a solvent for compound (A).

[0116] In the method of the present invention, there is no particular limitation on the method for purifying the by-produced monohydroxy compound. From the viewpoint of production efficiency and productivity, it is preferable to use a distillation method. The distillation method can be a batch type or a continuous type. However, in the method of the present invention, the polymerization process is continuous and by-products are also generated continuously. In order to achieve this, it is preferable to carry out the distillation in a continuous manner. In the method of the present invention, the monohydroxylated product to be purified is The mixture is divided into components with lower boiling points (water, residual solvents in the raw materials, etc.) and components with higher boiling points (unreacted Since it contains both monomers and oligomers, two or more distillation columns are combined to It is preferred to remove the low boiling components in one and the high boiling components in the second.

[0117] [Resin Uses] The resin of the present invention and a resin composition containing the same can be molded by injection molding, extrusion molding, compression molding, etc. It can be molded into products by commonly known methods, and has excellent optical properties, heat resistance, and mechanical strength. The resin obtained by the method of the present invention has a strictly controlled primary polymer structure. By precisely controlling the temperature, it is possible to uniformize the mechanical properties, especially the melt viscosity and tensile strength. Therefore, it is particularly suitable for use in applications such as retardation films in which melt extrusion film formation and stretching are performed continuously. . EXAMPLES

[0118] The present invention will be described in more detail below using examples. The following examples are not intended to be limiting unless otherwise stated.

[0119] [Measurement method] Various physical properties were measured according to the following methods.

[0120] Reduced Viscosity The resin sample was dissolved in methylene chloride to prepare a resin solution with a concentration of 0.6 g / dL. Measurements were performed at a temperature of 20.0°C ±0.1°C using a Yurikaku Kogyo Ubbelohde viscometer. The solvent passing time t0 and the solution passing time t were measured. Using the obtained t0 and t values, The relative viscosity η is calculated by the following formula (i): rel The relative viscosity η rel Using the following According to the formula (ii), the specific viscosity η sp asked for. η rel =t / t0 (i) η sp =(η-η0) / η0=η rel -1 (ii) Then, the obtained specific viscosity η sp Divide by the concentration c [g / dL] to get the reduced viscosity η sp / c The higher this value, the larger the molecular weight.

[0121] ·Molecular weight distribution Approximately 0.1 g of the resin sample was dissolved in 2 mL of methylene chloride, and the solution was filtered through a 0.2 μm disk. The standard polystyrene was also measured by GPC. Number average molecular weight (Mn), weight average molecular weight (Mw), molecular weight distribution (Mw / Mn The equipment and conditions were as follows: Pump: LC-20AD (Shimadzu Corporation) Degasser: DGU-20A5 (Shimadzu Corporation) Column oven: CTO-20AC (Shimadzu Corporation) Detector: Differential refractive index detector RID-10A (Shimadzu Corporation) Column: PLgel 10μm Guard, PLgel 10μm MIXED-B 2 (Agilent) Oven temperature: 40℃ Eluent: Chloroform ·Flow rate: 1mL / min ·Injection volume: 10μL

[0122] · 1 H-NMR Approximately 15 mg of polycarbonate resin sample was weighed out and dissolved in approximately 0.7 mL of deuterated chloroform. This was placed in an NMR tube with an inner diameter of 5 mm. 1 H-NMR spectrum was measured. A signal based on a structural unit derived from the dihydroxy compound (A) in the recarbonate; From the signal intensity ratio of the heterogeneous structure (decomposition product of SPG) detected at 5.7-5.8 ppm, The content of the heterogeneous structure [mol%] was calculated. The apparatus and conditions used are as follows. Equipment: JNM-ECZ400S (manufactured by JEOL Ltd.) ·Measurement temperature: 30℃ Relaxation time: 6 seconds Number of times accumulated: 64

[0123] The content of heterogeneous structures was calculated using the polycarbonate resins produced in the Examples and Comparative Examples described below. The calculation method will be explained. Range for calculating integral value (a): 5.7-5.8 ppm: heterogeneous structure (proton number: 1) (b): 2.4 to 2.0 ppm: derived from BPFM repeating unit (proton number: 4) (c): 1.5-0.5 ppm: SPG repeating unit (proton count: 12) and BPF M repeating unit (proton count: 4) Calculation of the amount of heterogeneous structures relative to the total amount of SPG repeating units (a) / {(c)-(b)} / 12×100[mol%]

[0124] Resin performance evaluation The resin pellets were vacuum dried at 100°C for more than 6 hours, and then extruded in a single-screw extruder (Technovel Co., Ltd.). , screw diameter 25mm, cylinder set temperature: 240℃), T die (width 400mm, setting The machine is equipped with a constant temperature of 250°C, a chill roll (set temperature: 120-130°C), and a winder. Using a film-forming device, an unstretched film with a width of 300 mm and a thickness of 100 μm was produced. From this film, a piece of film measuring 70 mm in length and 100 mm in width was cut out and batch-type biaxial Using a stretching device (Island Industrial Co., Ltd. BIX-277-AL), perform uniaxial stretching at the free end. The stretched film was obtained. The stretching conditions were an oven temperature of 150° C. and a stretching speed of The stretching rate was 300% / min, and the stretching ratio was 2 times. If stretching was successful under these conditions, the stretching ratio was increased to 2 The stretching ratio is gradually increased to 0.1, 2.2, and so on, and the stretching is repeated until the stretching ratio reaches the point where the film breaks. And went.

[0125] Among the films stretched by the above method, the center of the film obtained at the maximum stretch ratio was cut to a width of 2 The pieces were cut into pieces of 2 cm length and measured using a phase difference measuring device (KOBRA-WPR manufactured by Oji Scientific Instruments). Measurement wavelengths: 446.3 nm, 498.0 nm, 547.9 nm, 585.9 nm The phase difference was measured at 590 nm (R590 ) and the film thickness at the measurement position, the birefringence (Δn) was calculated from the following formula. Birefringence = R590 [nm] / (film thickness [mm] x 10 6 )

[0126] [Raw materials used] The abbreviations and manufacturers of the compounds used in the following Examples and Production Examples are as follows.

[0127] [monomer] SPG: Spiroglycol (manufactured by Mitsubishi Gas Chemical Co., Ltd.) ISB: Isosorbide (manufactured by Rocket Fleuret) BPFM: Bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methyl Tan It was synthesized by the method described in JP 2015-25111 A.

[0128] [ka]

[0129] DPC: Diphenyl carbonate (Mitsubishi Chemical) PHL: Phenol (Mitsubishi Chemical) [Polymerization catalyst] Calcium acetate monohydrate (Kanto Chemical) Calcium acetate monohydrate was dissolved in demineralized water to prepare an aqueous solution of a given concentration. [Catalyst deactivator] Phosphonic acid (Tokyo Chemical Industry Co., Ltd.) [Heat stabilizer (antioxidant)] Irganox 1010: Pentaerythritol-tetrakis(3-(3,5-di-t ert-butyl-4-hydroxyphenyl)propionate (BASF)

[0130] Example 1 Polycarbonate resin was produced using the polymerization equipment A shown in Figures 1 and 3. SPG dissolution tank 1 j PHL and an aqueous catalyst solution were supplied to the first vertical reactor 21a for a residence time of 7 hours. The amount of catalyst was supplied so that 12 μmol per 1 mol of dihydroxy compound used in polymerization was used. Next, SPG was supplied for a residence time of 7 hours. ISB was charged from the flexible container 2a to the ISB dissolving tank 2b, and the overflowing molten liquid was transferred to the molten ISB tank 2d. 229.7 parts by weight of molten DPC and 100 parts by weight of PBFM were supplied from the flexible container 3a to the raw material dissolving tank 3d, and after dissolving, they were transferred to the raw material storage tank 3f. The metering pumps (1k, 2d, 3g) for each raw material were started simultaneously at the specified set flow rate, the raw material molten liquid was supplied to the first vertical reactor 21a, and polymerization was started. At the same time, the SPG metering feeder 1e, the PHL metering pump 1g, and the aqueous catalyst solution metering pump 1i also started supplying at the specified set flow rate. Additional raw materials were periodically supplied to the raw material storage tanks for PBFM, DPC, and ISB so that they did not become empty.

[0131] The flow rate of each metering pump and the operating conditions of each raw material dissolving tank were set as follows: ·SPG(1e): 30.2 parts by weight / hr ·PHL (1g): 24.7 parts by weight / hr ·SPG / PHL mixed liquid (1k): 54.8 parts by weight / hr ·ISB(2d): 40.0 parts by weight / hr ·PBFM・DPC mixed solution (3g): 99.3 parts by weight / hr -Inner temperature of raw material dissolving tank 1j: 125℃, residence time: 7 hours

[0132] The molar ratio and weight ratio of each structural unit in the resulting polycarbonate resin are as follows: . SPG / ISB / PBFM / DPC=0.266 / 0.734 / 0.126 / 0.87 4 (molar ratio), SPG / ISB / PBFM / DPC=30.0 / 39.5 / 21.4 / 9.1% by weight.

[0133] The transfer pipe at the bottom of the first vertical stirred reactor was installed so that the average residence time in the reactor was 90 minutes. The liquid level was kept constant by controlling the opening of the valve. The reaction mixture was then transferred to the second vertical stirred reactor, the third vertical stirred reactor, and the fourth horizontal stirred reactor. The first and second vertical stirred reactors were equipped with reflux condensers. This suppressed the distillation of unreacted monomers.

[0134] The reaction temperature, internal pressure, and residence time of each reactor were as follows: First vertical stirred reactor: 195°C, 2 7kPa, 90min, 2nd vertical stirring reactor: 205℃, 20kPa, 90min, 3rd vertical stirring reactor Reactor: 220°C, 10kPa, 60min, 4th horizontal stirred reactor: 235°C, 1kPa, 1 The polymerization rate was controlled by the degree of vacuum in the fourth horizontal stirring reactor, and the resulting polycarbonate was The reduced viscosity of the carbonate resin must be adjusted to 0.45 dL / g to 0.47 dL / g. I drove while driving.

[0135] The resin discharged from the fourth horizontal agitation reactor is then fed to a vented twin-screw extruder in a molten state. The polycarbonate resin that passed through the extruder continued to be in a molten state and was fed to the Foreign matter was filtered through a 10μm Ultipleat candle-type filter (Pall). The mixture was then discharged from the die in the form of strands, cooled in water, solidified, and then passed through a rotary The mixture was pelletized with a cutter to obtain a polycarbonate resin.

[0136] The extruder has three vacuum vents, which are used to devolatilize the remaining low molecular weight components in the resin. Just before the second vent, 2000 ppm of water was added to the resin, and the water was poured in to remove the volatiles. The Irganox 1010 was mixed with 100 layers of polycarbonate resin just before the third vent. 0.1 parts by weight was added per part by weight.

[0137] The phenol by-product of the polymerization reaction is collected in a distillate tank 23a and then fed to a distillation column 23c. 23f separates light-boiling impurities (mainly water) and heavy-boiling impurities (mainly monomers and oligomers) The purified phenol is returned to the melting PHL tank 1f and is then sent back to the raw material preparation process. It was used in the process.

[0138] The operation was carried out under the above operating conditions for two consecutive days, and pellets were sampled every two hours. The molecular weight distribution of the pellets was measured by GPC and found to be 2.4 to 2.5. No variation was observed in the primary polymer structure. 1 H-NMR analysis shows that the heterogeneous structure The samples with the smallest and largest molecular weight distributions were selected from the samples obtained, When the film was stretched using the method described above, it was found that the film had a stable high stretch ratio and high orientation. The evaluation results are shown in Table 1.

[0139] [Table 1]

[0140] Comparative Example 1 In Example 1, the aqueous catalyst solution was not added to the raw material dissolving tank 1j, but was added to the aqueous catalyst solution quantitative supply tank 1j. The procedure was the same as in Example 1 except that the feed was added immediately before the first reactor using pump 4d. The molecular weight distribution of the obtained polycarbonate resin was 4.0 to 5.7, which was higher than that of Example 1. As a result, the molecular weight distribution became wider and the degree of variation also became greater. 1 H-NMR analysis shows heterogeneous structure In the film stretching evaluation, the stretch ratio and orientation were higher than in Example 1. Both tropism and variability decreased significantly.

[0141] Example 2 Polycarbonate resin was produced using the polymerization equipment B shown in Figures 2 and 3. PHL, DPC, and an aqueous catalyst solution were fed to the disintegrator 11g for a retention time of 5 hours. Stir for 10 minutes. After that, PBFM and SPG were fed for a residence time of 5 hours. After all the raw materials were dissolved, The raw material mixture was transferred to the raw material storage tank 11h. The ISB was transferred from the flexible container 12a to the I The raw materials were poured into the SB melting tank 12b, and the molten liquid was transferred to the ISB melting tank 12d. The supply pumps (11i, 12e) are simultaneously started at a predetermined set flow rate to supply the first vertical reactor 21a The raw material melt was fed to the raw material storage tanks to start polymerization. Periodically, additional raw materials were supplied.

[0142] The flow rate of each metering pump and the operating conditions of each raw material dissolving tank were set as follows: ·SPG・PHL・PBFM・DPC mixed liquid (11i): 154.1 parts by weight / hr ·ISB(12e): 40.0 parts by weight / hr -Inner temperature of raw material dissolving tank for 11 hours: 125℃

[0143] The polymerization process was carried out in the same manner as in Example 1. The molecular weight distribution of the obtained polycarbonate resin was 2 The molecular weight distribution was slightly larger than that of Example 1. In the film stretching evaluation, both the stretch ratio and the orientation were slightly lower than in Example 1. The reason for the broadening of the molecular weight distribution is that the process of dissolving SPG was a batch process, and The thermal history of SPG during the decomposition process is distributed, and the decomposition products of SPG are It is thought that there was variation in the amount of waste generated.

[0144] Comparative Example 2 In Example 2, the catalyst aqueous solution was not added to the raw material dissolving tank 11g, and the catalyst aqueous solution was supplied in a fixed amount. Using pump 13d, the mixture was added just before the first reactor. The rest of the procedure was the same as in Example 1. The molecular weight distribution of the obtained polycarbonate resin was 2.9 to 3.8, which is the same as that of Example 1 and Example The molecular weight distribution was broader and the degree of variation was larger than in Example 2. In the evaluation, both the stretch ratio and the orientation were significantly lower than in Examples 1 and 2, and the variation It's gotten bigger.

[0145] Comparative Example 3 In Example 2, the raw materials were mixed in a raw material dissolving tank of 11 g without using PHL. In order to completely dissolve the mixture, the internal temperature was raised to 170°C. Otherwise, the procedure was the same as in Example 1. The molecular weight distribution of the polycarbonate resin obtained was 2.6 to 3.0, which is different from that of Example 1 and Example 2. In comparison, the molecular weight distribution was wider and the degree of variation was larger. However, both the draw ratio and the orientation were lower than those of Examples 1 and 2.

[0146] (Reference example 1) A batch-type polymerization apparatus C (not shown) equipped with an agitator and a reflux condenser was used to polymerize the polymer. Carbonate resin was produced. When the internal temperature of the reactor was 60°C or less, SP G, ISB, PBFM, DPC, and calcium acetate monohydrate were mixed in the molar ratio of SPG / I SB / PBFM / DPC=0.266 / 0.734 / 0.126 / 0.874 / 12×1 0 -6 , SPG / ISB / PBFM / DPC=30.2 / 40.0 / 30.1 / in parts by weight After thoroughly replacing the inside of the reactor with nitrogen, the reactor was heated with a heat medium. Stirring was started when the internal temperature reached 100°C. After 40 minutes from the start of the temperature increase, the internal temperature reached 220°C. The temperature is then controlled to be maintained at this temperature, and pressure reduction is started at the same time. The pressure was increased to 13.3 kPa in 90 minutes. The phenol vapor by-produced during the polymerization reaction was cooled by reflux. The small amount of monomer components contained in the phenol vapor is returned to the reactor without condensation. The phenol vapor was then collected in a condenser at 45°C. The temperature was then raised to 240°C and the internal pressure to 1 kPa. After that, the pressure was lowered to 133 Pa or less over 30 minutes. When the stirring power reaches a predetermined level, the pressure is restored and the contents are extracted in the form of strands and fed to a rotary cutter. The molecular weight distribution of the resulting polycarbonate resin was 2.5. The results were similar to those of Example 1. 1 No heterogeneous structures were detected by H-NMR analysis. In the stretching evaluation, a high stretch ratio and high orientation were obtained, similar to Example 1. By contacting the SPG with a basic compound before decomposition, the decomposition of SPG and the increase in molecular weight distribution can be suppressed. You can see that it is possible. [Explanation of symbols]

[0147] Figure 1. Raw material preparation process for polymerization facility A 1a: SPG flexible container 1b: SPG receiving hopper 1c: SPG air blower 1d: SPG raw material silo 1e: SPG weighing feeder 1F: PHL melting tank 1g: PHL constant volume supply pump 1h: Catalyst aqueous solution tank 1i: Catalyst aqueous solution constant volume supply pump 1j:SPG / PHL raw material dissolution tank 1k: SPG / PHL constant volume supply pump 2a:ISB flexible container 2b:ISB dissolution tank 2c:ISB storage tank 2d:ISB constant volume supply pump 3a:PBFM flexible container 3b: Melting DPC tank 3c: DPC fixed-volume emergency pump 3d:PBFM / DPC raw material dissolution tank 3e: Transfer pump 3f:PBFM / DPC storage tank 3g:PBFM·DPC constant volume supply pump 4a:Static mixer 4b: Filter 4c: Catalyst aqueous solution tank 4d: Catalyst aqueous solution metering pump

[0148] Figure 2. Raw material preparation process in polymerization facility B 11a: SPG flexible container 11b:PBFM flexible container 11c: PHL melting tank 11d: PHL constant volume supply pump 11e:Melting DPC Tank 11f: DPC constant volume supply pump 11g:SPG / PBFM / DPC / PHL raw material dissolution tank 11h:SPG / PBFM / DPC / PHL storage tank 11i: SPG / PBFM / DPC / PHL constant volume supply pump 12a:ISB flexible container 12b:ISB dissolution tank 12c: Transfer pump 12d:ISB storage tank 12e:ISB constant volume supply pump 13a:Static mixer 13b: Filter 13c: Catalyst aqueous solution tank 13d: Catalyst aqueous solution constant volume supply pump

[0149] Figure 3 Polymerization process and distillation process (common to both polymerization equipment A and B) 21a: First vertical stirred reactor 21b: Reflux condenser 21c: Second vertical stirred reactor 21d: Reflux condenser 21e: Third vertical stirred reactor 21f: Gear pump 21g: 4th horizontal stirred reactor 21h: Gear pump 22a: Vacuum vented twin screw extruder 22b: Gear pump 22c: Polymer filter 22d: Dice 23a: Distillate recovery tank 23b: Distillate metering pump 23c: First distillation column 23d: Metering pump 23e: Reflux condenser 23f: Second distillation tower 23g: Metering pump 23h: Reflux condenser

Claims

1. A method for producing a polycarbonate resin, comprising continuously supplying a dihydroxy compound (A) having an acetal group as a part of its structure, a carbonic acid diester, and a polymerization catalyst to a reactor to carry out a melt polycondensation reaction, comprising the steps of: The method includes a step of dissolving the dihydroxy compound (A) in a solvent containing a monohydroxy compound represented by the following formula (1) as a main component in a raw material dissolving tank, The method for producing a polycarbonate resin is characterized in that the solvent has a melting point lower than that of the dihydroxy compound (A) and contains a basic compound. 【Chemistry 1】 (R in formula (1) 1 , R 2 are each independently a hydrogen atom, an optionally substituted alkyl group having 1 to 10 carbon atoms, an optionally substituted acyl group having 1 to 10 carbon atoms, an optionally substituted alkoxy group having 1 to 10 carbon atoms, or an optionally substituted alkyl ester group having 1 to 10 carbon atoms.

2. 2. The method for producing a polycarbonate resin according to claim 1, wherein the internal temperature of the raw material dissolving tank is 80° C. or higher and 150° C. or lower.

3. 3. The method for producing a polycarbonate resin according to claim 1, wherein the dihydroxy compound (A) is continuously supplied to the raw material dissolving tank, and a solution containing the dissolved dihydroxy compound (A) is continuously discharged from the raw material dissolving tank.

4. The method for producing a polycarbonate resin according to any one of claims 1 to 3, wherein the dihydroxy compound (A) is a compound represented by the following formula (2): 【Chemistry 2】

5. Polycarbonate resin measured using deuterated chloroform solvent 1 The method for producing a polycarbonate resin according to any one of claims 1 to 4, wherein the content of a component detected at 5.7 to 5.8 ppm in a H-NMR spectrum is 0.05 mol% or less, based on the total amount of structural units derived from the compound represented by formula (2).

6. The method for producing a polycarbonate resin according to any one of claims 1 to 5, wherein the basic compound is at least one metal compound selected from the group consisting of metals in Group 2 of the long form periodic table and lithium.

7. The method for producing a polycarbonate resin according to any one of claims 1 to 6, wherein the content of the basic compound in the solvent is 0.1 µmol or more and 50 µmol or less per 1 mol of all dihydroxy compounds used in the melt polycondensation reaction.

8. The method for producing a polycarbonate resin according to any one of claims 1 to 7, wherein the carbonate diester is a compound represented by the following formula (3): 【Chemistry 3】 (R in formula (3) 1 , R 2 are each independently a hydrogen atom, an optionally substituted alkyl group having 1 to 10 carbon atoms, an optionally substituted acyl group having 1 to 10 carbon atoms, an optionally substituted alkoxy group having 1 to 10 carbon atoms, or an optionally substituted alkyl ester group having 1 to 10 carbon atoms.

9. 9. The method for producing a polycarbonate resin according to claim 8, further comprising a step of recovering a monohydroxy compound produced as a by-product in the polycondensation reaction and purifying the recovered monohydroxy compound by distillation, and the distilled and purified monohydroxy compound is supplied to the raw material dissolving tank.

10. The method for producing a polycarbonate resin according to any one of claims 1 to 9, wherein the polycarbonate resin contains a structural unit derived from a dihydroxy compound represented by the following formula (4): 【Chemistry 4】

11. The method for producing a polycarbonate resin according to any one of claims 1 to 10, wherein the polycarbonate resin contains a structural unit derived from a compound represented by the following formula (5): 【Chemistry 5】 (In formula (5), R 3 and R 4 R each independently represents a direct bond or an alkylene group having 1 to 4 carbon atoms which may have a substituent. 5 ~R 10 are each independently a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may have a substituent, an aryl group having 6 to 15 carbon atoms which may have a substituent, an acyl group having 1 to 10 carbon atoms which may have a substituent, an alkoxy group having 1 to 10 carbon atoms which may have a substituent, an aryloxy group having 6 to 15 carbon atoms which may have a substituent, an acyloxy group having 1 to 10 carbon atoms which may have a substituent, an amino group which may have a substituent, a vinyl group having 2 to 10 carbon atoms which may have a substituent, an ethynyl group having 2 to 10 carbon atoms which may have a substituent, a sulfur atom which has a substituent, a silicon atom which has a substituent, a halogen atom, a nitro group, or a cyano group, provided that R 5 ~R 10 At least two adjacent groups among these may be bonded to each other to form a ring. X is a hydroxy group, a carboxy group, an alkyl ester group having 1 to 10 carbon atoms which may have a substituent, or an aryl ester group having 6 to 15 carbon atoms which may have a substituent.

Citation Information

Patent Citations

  • Copolycarbonate polymer for binder of electrophotographic photoreceptor and its production

    JP1996311191A

  • Preparation of aromatic-aliphatic copolymerized polycarbonate

    JP1999349679A

  • Production of aromatic-aliphatic copolycarbonate

    JP2000001536A

  • Preparation of aromatic-aliphatic copolymer polycarbonate

    JP2000007777A

  • Copolycarbonate resin

    JP2006232897A