Room temperature curable organopolysiloxane composition, cured product thereof, and article

A room-temperature-curable organopolysiloxane composition with a hydrolyzable silyl group and catechol structure addresses adhesion and chemical resistance issues, providing durable adhesion to metals and resins in automobile engines and electrical components.

JP7552485B2Active Publication Date: 2024-09-18SHIN ETSU CHEMICAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021067212
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-12
Publication Date
2024-09-18
Estimated Expiration
2041-04-12

AI Technical Summary

Technical Problem

Existing room-temperature-curable organopolysiloxane compositions struggle with adhesion to metals and resins, particularly polybutylene terephthalate and polyphenylene sulfide, and lack sufficient chemical resistance to engine oil and long-life coolant, making them unsuitable for applications in automobile engines and electrical components.

Method used

A room-temperature-curable organopolysiloxane composition incorporating a hydrolyzable silyl group and a catechol structure protected by a silyl group in one molecule, along with specific components like diorganopolysiloxane, hydrolyzable organosilane compounds, and a curing catalyst, enhances adhesion and chemical resistance.

Benefits of technology

The composition achieves excellent adhesiveness to resins and metals, maintaining chemical resistance to engine oil and long-life coolant, suitable for durable applications in automobile engines and electrical components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552485000005
    Figure 0007552485000005
  • Figure 0007552485000022
    Figure 0007552485000022
  • Figure 0007552485000021
    Figure 0007552485000021
Patent Text Reader

Abstract

To provide a room temperature-curable organopolysiloxane composition which gives a cured product having adhesion to metal and a resin, chemical resistance against engine oil and a long-life coolant and good rubber physical properties, a cured product of the same, and an article having the cured product.SOLUTION: In a room temperature-curable organopolysiloxane composition, a hydrolyzable organosilane compound having a catechol structure protected with a hydrolyzable silyl group and a silyl group in one molecule and / or its partial hydrolysis condensate is used.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a room-temperature-curable organopolysiloxane composition, and in particular to a room-temperature-curable organopolysiloxane composition that has adhesion to metals and resins, and has chemical resistance to engine oils and long-life coolants, and that gives a cured product having good rubber physical properties, as well as a cured product thereof and an article comprising the cured product. [Background technology]

[0002] Conventionally, chemical-resistant gaskets and packing materials made of cork, organic rubber, asbestos, etc. have been used to seal the periphery of electrical components in automobile engines and engine control units, but these have the disadvantages of complicated inventory management and work processes, and furthermore, their sealing performance is unreliable. For this reason, the FIPG (Formed In Place Gasket) method, which uses a room temperature curable organopolysiloxane composition as a liquid gasket, is adopted for this type of application.

[0003] In recent years, attempts have been made to use resins for some of the metals used in automobile engines and various electrical components in order to improve fuel efficiency and reduce the weight of automobiles. The resins used for these components are generally resins that show little change in mechanical properties and durability tests against engine oil and long-life coolant, that is, resins that are very stable mechanically and chemically. Resins with high chemical stability have no or very few active groups, so it is considered difficult to obtain good adhesion and furthermore to stably maintain that adhesion. As a method for improving adhesion to resins, a method of adding an oligomer of an aminosilane coupling agent to a room temperature curable organopolysiloxane composition (Patent Publication No. 3714861: Patent Document 1) is known, but when an oligomer of an aminosilane coupling agent is blended into a composition for applications requiring resistance to engine oil and long-life coolant, it cannot be used because of poor chemical resistance. In addition, a method of selecting a filler for a room temperature curable organopolysiloxane composition (JP Patent Publication No. 2004-292724: Patent Document 2) and a method of selecting the structure of a titanium catalyst used as a curing catalyst (JP Patent No. 4438937, JP Patent No. 4530136, JP Patent No. 4658654, JP Patent No. 4530177: Patent Documents 3-6) are known, but these compositions have problems in that it takes time to obtain a cured product and that their chemical resistance is inferior to that of FIPG, which has been used conventionally. In addition, as a method for improving adhesion to various adherends, there are reports of introducing alkoxysilyl groups into aromatic compounds to improve adhesion to polybutylene terephthalate and high impact polystyrene, but there are no reports on adhesion or chemical resistance to polyphenylene sulfide, which is more difficult to adhere to (JP Patent No. 3518399: Patent Document 7).

[0004] In order to satisfy the above-mentioned requirements for chemical resistance and adhesiveness, we have recently focused on the special chemical structure of the adhesive protein of the mussel, which is an outstanding underwater adhesive, and on research into the adhesive mechanism that skillfully utilizes this structure. Although much remains unknown about the adhesion mechanism, it is known that a compound with a catechol structure contained in the adhesive plays an important role.

[0005] In Patent Document 8 (JP Patent Publication 2010-144148 A), a polydopamine thin film is formed to improve the adhesion between a plated lead frame and an epoxy resin or silicone resin. In Non-Patent Document 1 (J. Am. Chem. Soc. 2012, 134, 20139-20145), a silyl-protected catechol-containing silicone is synthesized by an enethiol reaction between a silyl-protected vinyl-containing catechol compound and a mercapto-containing silicone, and the silicone is used as a component for an adhesive composition.

[0006] As described above, there are examples in which a compound having a catechol structure is used as a component of an adhesive composition. However, there have been no reports to date of an organosilicon compound having a hydrolyzable silyl group and a catechol structure protected by a silyl group in the molecule, or of a moisture-curable, room-temperature-curable organopolysiloxane composition containing this compound. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 3714861 [Patent Document 2] JP 2004-292724 A [Patent Document 3] Patent No. 4438937 [Patent Document 4] Patent No. 4530136 [Patent Document 5] Patent No. 4658654 [Patent Document 6] Patent No. 4530177 [Patent Document 7] Patent No. 3518399 [Patent Document 8] JP 2010-144148 A [Non-patent literature]

[0008] [Non-Patent Document 1] J.Am.Chem.Soc.2012,134,20139-20145 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a room-temperature-curable organopolysiloxane composition which has adhesion to metals and resins, and which has chemical resistance to engine oils and long-life coolants, and which gives a cured product having good rubber physical properties, as well as a cured product thereof, and an article comprising the cured product. [Means for solving the problem]

[0010] As a result of extensive investigations aimed at achieving the above object, the present inventors have discovered that by using a hydrolyzable organosilane compound having a hydrolyzable silyl group and a catechol structure protected by a silyl group in one molecule, and / or a partial hydrolysis condensate thereof, in a room-temperature-curable organopolysiloxane composition, it is possible to improve adhesion to engineering plastics (such as nylon 66, polybutylene terephthalate, polyphenylene sulfide, etc.) and further improve chemical resistance to chemicals such as engine oil and long-life coolant, thereby completing the present invention.

[0011] That is, the present invention provides the following room temperature curable organopolysiloxane composition, cured product, and article. [1] (A) 100 parts by mass of a diorganopolysiloxane having silicon-bonded hydroxyl groups and / or hydrolyzable silyl groups at both molecular chain terminals and having a viscosity at 23°C of 20 to 1,000,000 mPa s, which is represented by the following general formula (1): [ka] [In the formula, R 1 R is independently a group selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms. 2 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms. a is independently 0, 1, or 2 for each silicon atom to which it is bonded, but R 1 is an alkyl or alkoxyalkyl group, a is independently 0 or 1 for each silicon atom to which it is bonded; 1 When is a hydrogen atom, a is 2. n is a number that provides a viscosity of 20 to 1,000,000 mPa s at 23°C of the diorganopolysiloxane. Y is independently an oxygen atom, an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms, or a group represented by the following formula (2): [ka] (In the formula, R 2 is as defined above, and Z is independently an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms. The wavy line indicates the bonding position to the silicon atom. (B) a hydrolyzable organosilane compound having three or more silicon-bonded hydrolyzable groups in the molecule other than the components (A), (C), and (D) and / or a partial hydrolysis condensate thereof: 0.1 to 40 parts by mass, (C) A hydrolyzable organosilane compound represented by the following general formula (3) having a catechol structure blocked with a triorganosilyl group and a hydrolyzable silyl group in the molecule, and / or a partial hydrolysis condensate thereof: (However, the partial hydrolysis condensate is a partial hydrolysis condensate having a triorganosilyl-group-blocked catechol structure obtained by hydrolysis and condensation of a hydrolyzable silyl group of a hydrolyzable silyl-group-containing monovalent hydrocarbon group represented by the following formula (4) in a hydrolyzable organosilane compound represented by the following general formula (3).) : 0.1 to 10 parts by mass, and [ka] [In the formula, R 3 ~R6 are each independently a group or atom selected from a hydrogen atom, an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4), 3 ~R 6 At least one of R is a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4): 7 are independently an unsubstituted or substituted monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. [ka] (In the formula, R 8 , R 9 are each independently an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms, b is 0, 1 or 2, and m is an integer of 1 to 10. The wavy line indicates the bonding position to the benzene ring.) (D) Curing catalyst: 0.01~3 parts by mass A room temperature curable organopolysiloxane composition comprising: [2] In the general formula (3), R 7 is a methyl group or an ethyl group. [3] R in general formula (3) 3 ~R 6 In R 4 and / or R 5 is a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by formula (4), and the other R 3 ~R 6 wherein each independently represents a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms. [4] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [3], further comprising, as component (E), 0.01 to 5 parts by mass of a silane coupling agent represented by the following general formula (5) and / or a partial hydrolysis condensate thereof, per 100 parts by mass of component (A): [ka] (In the formula, R 10 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one nitrogen atom. 11 , R 12 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and c is 0, 1, or 2. [5] The room-temperature-curable organopolysiloxane composition according to any one of [1] to [4], further comprising at least one inorganic filler as component (F). [6] A cured product obtained by curing the room-temperature-curable organopolysiloxane composition according to any one of [1] to [5]. [7] An article having the cured product according to [6]. Effect of the Invention

[0012] According to the present invention, it is possible to obtain a room-temperature-curable organopolysiloxane composition which gives a cured product having excellent adhesion to resins, excellent rubber physical properties, and good chemical resistance, a cured product thereof, and an article comprising the cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below. Unless otherwise specified, "room temperature" refers to a state where the temperature is 23°C ± 5°C and the humidity is 50% RH ± 5% RH.

[0014] [Component (A)] The component (A) is a diorganopolysiloxane having hydroxyl groups and / or hydrolyzable silyl groups bonded to silicon atoms at both ends of the molecular chain, and is the main component of the room temperature curable organopolysiloxane composition of the present invention. The molecular structure of the diorganopolysiloxane is linear. The diorganopolysiloxane may have a silalkylene structure (-Si-R-Si-) in the molecular chain. In the above formula, R is an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms, and some or all of the hydrogen atoms bonded to the carbon atoms may be substituted with halogen atoms or cyano groups.

[0015] Here, examples of the divalent hydrocarbon group of R include alkylene groups such as methylene, ethylene, propylene, tetramethylene, hexamethylene, octamethylene, decamethylene, and 2-methylpropylene; arylene groups such as phenylene; groups in which these alkylene groups and arylene groups are bonded; and groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms or cyano groups. The divalent hydrocarbon group may be linear or branched, but is preferably a linear alkylene group such as a methylene group, ethylene group, propylene group, butylene group, or hexylene group, and particularly preferably an ethylene group.

[0016] The diorganopolysiloxane of the (A) component has a viscosity at 23°C of 20 to 1,000,000 mPa·s, preferably 100 to 300,000 mPa·s, more preferably 1,000 to 200,000 mPa·s, and particularly preferably 5,000 to 100,000 mPa·s. If the viscosity of the diorganopolysiloxane is less than the lower limit (20 mPa·s), a large amount of the (B) component described below is required, which is economically disadvantageous. If the viscosity of the diorganopolysiloxane exceeds the upper limit (1,000,000 mPa·s), workability decreases, which is not preferable. In the present invention, the viscosity can be measured using a rotational viscometer (for example, BL type, BH type, BS type, cone plate type, rheometer, etc.).

[0017] The hydrolyzable silyl group in the diorganopolysiloxane of component (A) is an alkoxy group or an alkoxyalkoxy group. With regard to the number of hydroxyl groups and hydrolyzable silyl groups bonded to silicon atoms present at each end of the diorganopolysiloxane, when the diorganopolysiloxane has a hydroxyl group bonded to a silicon atom at the end, it has one hydroxyl group (i.e., a silanol group or a hydroxysilyl group) bonded to a silicon atom at each end of the molecular chain. When the diorganopolysiloxane has an alkoxy group or an alkoxyalkoxy group at the end, it has two alkoxy groups bonded to a silicon atom (i.e., a dialkoxysilyl group or a dialkoxyalkoxysilyl group) or three alkoxy groups bonded to a silicon atom (i.e., a trialkoxysilyl group or a trialkoxyalkoxysilyl group) at each end of the molecular chain.

[0018] The alkoxy group is preferably an alkoxy group having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, and an octyloxy group. The alkoxyalkoxy group is preferably an alkoxyalkoxy group having a total of 2 to 10 carbon atoms, such as a methoxymethoxy group, a methoxyethoxy group, and an ethoxymethoxy group. As the diorganopolysiloxane of the component (A), in particular, one having a hydroxyl group, a methoxy group, or an ethoxy group at both ends of the diorganopolysiloxane is preferred.

[0019] Examples of organic groups bonded to silicon atoms other than hydroxyl groups and hydrolyzable silyl groups bonded to silicon atoms include unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, and octadecyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine, bromine, and chlorine or cyano groups, such as halogenated monovalent hydrocarbon groups such as 3-chloropropyl and 3,3,3-trifluoropropyl; and cyanoalkyl groups such as β-cyanoethyl and γ-cyanopropyl. Among these, the methyl group is preferable.

[0020] The above-mentioned (A) diorganopolysiloxane is a compound represented by the following general formula (1). [ka] [In the formula, R 1 R is independently a group selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms. 2 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms. a is independently 0, 1, or 2 for each silicon atom to which it is bonded, but R 1 is an alkyl or alkoxyalkyl group, a is independently 0 or 1 for each silicon atom to which it is bonded; 1 When is a hydrogen atom, a is 2. n is a number that provides a viscosity of 20 to 1,000,000 mPa s at 23°C of the diorganopolysiloxane. Y is independently an oxygen atom, an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms, or a group represented by the following formula (2): [ka] (In the formula, R 2 is as defined above, and Z is independently an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms. The wavy line indicates the bonding position to the silicon atom.

[0021] In the above formula (1), R 1 are independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, and an octyl group, and an alkoxyalkyl group having 2 to 10 carbon atoms, such as a methoxymethyl group, a methoxyethyl group, and an ethoxymethyl group. A hydrogen atom, a methyl group, or an ethyl group is preferable. R 2 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms. Examples of the monovalent hydrocarbon group include organic groups bonded to silicon atoms other than the above-mentioned hydroxyl groups and hydrolyzable silyl groups bonded to silicon atoms, and among these, a methyl group is preferred. a is independently 0, 1, or 2 for each silicon atom to which it is bonded, 1 is an alkyl or alkoxyalkyl group, a is independently 0 or 1 for each silicon atom to which it is bonded; 1 When is a hydrogen atom, a is 2. n is a number that provides a viscosity of the diorganopolysiloxane at 23° C. of 20 to 1,000,000 mPa·s, preferably 100 to 300,000 mPa·s, more preferably 1,000 to 200,000 mPa·s, and particularly preferably 5,000 to 100,000 mPa·s, and may be, for example, an integer of 30 to 3,000, preferably an integer of 50 to 2,500, more preferably an integer of 100 to 2,000, and particularly preferably an integer of about 250 to 1,500. The repeat number (n) of diorganosiloxane units in a molecule can be determined, for example, as the polystyrene-equivalent number average degree of polymerization (or number average molecular weight) in gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent.

[0022] In the above formula (1), Y is independently an oxygen atom, an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms, or a group represented by the following formula (2). [ka] (In the formula, R 2 is as defined above, and Z is independently an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms. The wavy line indicates the bonding position to the silicon atom.

[0023] Here, examples of the divalent hydrocarbon groups of Y and Z include alkylene groups such as methylene, ethylene, propylene, tetramethylene, hexamethylene, octamethylene, decamethylene, and 2-methylpropylene; arylene groups such as phenylene; groups in which these alkylene groups and arylene groups are bonded; and groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms or cyano groups. The divalent hydrocarbon group may be linear or branched, but is preferably a linear alkylene group such as a methylene group, ethylene group, propylene group, butylene group, or hexylene group, and particularly preferably an ethylene group. It is particularly preferred that Y is an oxygen atom or an ethylene group.

[0024] The diorganopolysiloxane can be produced by a conventional method. The diorganopolysiloxane may be used alone or in combination of two or more kinds.

[0025] [(B) Component] Component (B) is a hydrolyzable organosilane compound having three or more hydrolyzable groups bonded to silicon atoms in the molecule and / or a partial hydrolysis condensate thereof (an organosiloxane oligomer having at least two, preferably three or more, residual hydrolyzable groups in the molecule, which is produced by partially hydrolyzing the organosilane compound). Component (B) undergoes a condensation reaction with component (A) to form a crosslinked structure. However, in the present invention, component (B) is a compound different from component (A) and components (C), (D), and (E) described below.

[0026] Examples of the hydrolyzable group contained in the hydrolyzable organosilane compound or its partial hydrolyzed condensate (organosiloxane oligomer) of component (B) include an alkoxy group, an alkoxyalkoxy group, an acyloxy group, an alkenoxy group, a ketoxime group, an aminoxy group, and an amide group, all of which have 1 to 10 carbon atoms. Examples of such groups include alkoxy groups such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, a hexyloxy group, and an octyloxy group; alkoxyalkoxy groups such as a methoxyethoxy group, an ethoxyethoxy group, and a methoxypropoxy group; acyloxy groups such as an acetoxy group and an octanoyloxy group; alkenoxy groups such as a vinyloxy group, an isopropenoxy group, and a 1-ethyl-2-methylvinyloxy group; ketoxime groups such as a dimethylketoxime group, a methylethylketoxime group, and a methylisobutylketoxime group; aminoxy groups such as a dimethylaminooxy group and a diethylaminooxy group; and amide groups such as an N-methylacetamide group and an N-ethylacetamide group.

[0027] Organic groups bonded to silicon atoms other than the above hydrolyzable groups include unsubstituted or substituted monovalent hydrocarbon groups having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms. Examples of the monovalent hydrocarbon groups include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, and octadecyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; and groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or with cyano groups, for example, halogenated alkyl groups such as 3-chloropropyl and 3,3,3-trifluoropropyl. Among these, preferred organic groups are methyl, ethyl, propyl, vinyl and phenyl.The hydrolyzable silane compound and / or its partial hydrolysis condensate, which is the component (B), does not contain, in the molecule, a monovalent hydrocarbon group having a functional group containing a nitrogen atom as a monovalent hydrocarbon group bonded to a silicon atom, other than the hydrolyzable groups.

[0028] Examples of the hydrolyzable organosilane compound of component (B) include alkoxysilanes such as methyltrimethoxysilane, ethyltrimethoxysilane, decyltrimethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, phenyltriethoxysilane, tetramethoxysilane, and tetraethoxysilane; ketoxime silanes such as methyltris(dimethylketoxime)silane, methyltris(methylethylketoxime)silane, ethyltris(methylethylketoxime)silane, methyltris(methylisobutylketoxime)silane, and vinyltris(methylethylketoxime)silane (or vinyltributanoximesilane); methyltri(methoxymethoxy)silane, ethyltri(methoxymethoxy)silane, and vinyltri(methoxy alkoxyalkoxysilanes such as methyltris(N,N-diethylaminooxy)silane; amidosilanes such as methyltris(N-methylacetamido)silane, methyltris(N-butylacetamido)silane, and methyltris(N-cyclohexylacetamido)silane; alkenoxysilanes such as methyltriisopropenoxysilane, vinyltriisopropenoxysilane, and phenyltriisopropenoxysilane; and acetoxysilanes such as methyltriacetoxysilane and vinyltriacetoxysilane.

[0029] The weight average molecular weight of the organosiloxane oligomer which is the partial hydrolysis condensate of the hydrolyzable organosilane compound of component (B) is not particularly limited, but it is preferable that the organosiloxane oligomer is an oligomer in which the silane compound is polymerized by 2 to 100 units, preferably 2 to 20 units. The organosiloxane oligomer may be a mixture of oligomers having a plurality of degrees of polymerization.

[0030] The component (B) may be used alone or in combination of two or more. In the present invention, a hydrolyzable organosilane compound having two hydrolyzable groups in one molecule and / or a partial hydrolysis condensate thereof may be used in combination as another component within a range that does not impair the effects of the present invention.

[0031] The amount of the (B) component is 0.1 to 40 parts by mass, preferably 1 to 20 parts by mass, per 100 parts by mass of the (A) component. If the amount of the (B) component is less than the lower limit (0.1 parts by mass), the curability and storage stability may be reduced. If the amount of the (B) component is more than the upper limit (40 parts by mass), not only is it uneconomical, but the elongation of the cured product may be reduced and the durability may be deteriorated.

[0032] [(C) component] Component (C) is a hydrolyzable organosilane compound and / or a partial hydrolysis condensate thereof, which has a catechol structure blocked with a triorganosilyl group in one molecule (i.e., a structure in which both of the two hydroxy groups present in the catechol are blocked and protected with triorganosilyl groups) and a hydrolyzable silyl group, as represented by the following general formula (3), and imparts the high adhesiveness derived from the triorganosilyl group-blocked catechol structure to the room-temperature-curable organopolysiloxane composition of the present invention. [ka] [In the formula, R 3 ~R 6 are each independently a group or atom selected from a hydrogen atom, an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4), 3 ~R 6 At least one of R is a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4): 7 are independently an unsubstituted or substituted monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. [ka] (In the formula, R 8 , R 9 are each independently an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms, b is 0, 1 or 2, and m is an integer of 1 to 10. The wavy line indicates the bonding position to the benzene ring.)

[0033] In the hydrolyzable organosilane compound of component (C) represented by the above general formula (3), R 3 ~R 6 are each independently a group or atom selected from a hydrogen atom, an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4). Examples of the unsubstituted or substituted monovalent hydrocarbon group include a group having 1 to 10 carbon atoms, preferably a group having 1 to 10 carbon atoms, such as a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, a heptyl group, an octyl group, a 2-ethylhexyl group, a nonyl group, a decyl group, etc. monovalent aliphatic hydrocarbon groups such as alkenyl groups having 2 to 6 carbon atoms, such as vinyl group, allyl group, propenyl group, isopropenyl group, etc.; aryl groups having 6 to 10 carbon atoms, such as phenyl group, tolyl group, xylyl group, naphthyl group, etc.; aralkyl groups having 7 to 10 carbon atoms, such as benzyl group, etc.; and unsubstituted or substituted monovalent hydrocarbon groups having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, such as chloromethyl group, trifluoropropyl group, etc. In the hydrolyzable organosilane compound represented by the above formula (3), R 3 ~R 6 Among these, at least one (i.e., 1 to 4), preferably 1 to 3, and more preferably 1 or 2, is a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the above formula (4). 3 ~R 6 Among them, R 4 and / or R 5 is preferably a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by formula (4). 3 ~R6 Among these, the remaining R other than the hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the above formula (4) 3 ~R 6 is preferably a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, more preferably a hydrogen atom, a methyl group, or an ethyl group.

[0034] In the hydrolyzable organosilane compound of component (C) represented by the above general formula (3), R 7 are independently an unsubstituted or substituted monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. Examples include alkyl groups having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and more preferably 1 to 3 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, 2-ethylhexyl, nonyl, and decyl groups; monovalent aliphatic hydrocarbon groups such as alkenyl groups having 2 to 6 carbon atoms, such as vinyl, allyl, propenyl, and isopropenyl groups; aryl groups having 6 to 10 carbon atoms, such as phenyl, tolyl, xylyl, and naphthyl groups; and halogen-substituted monovalent aliphatic hydrocarbon groups such as halogen-substituted alkyl groups having 1 to 6 carbon atoms, such as chloromethyl and trifluoropropyl groups. Preferably, they are alkyl groups having 1 to 6 carbon atoms, and more preferably methyl or ethyl groups.

[0035] In the hydrolyzable silyl group-containing monovalent hydrocarbon group (hydrolyzable silyl group-substituted alkyl group) represented by the above formula (4), R 8 , R 9each independently represents an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms. Examples of such alkyl groups include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, and an octyl group; a cycloalkyl group such as a cyclohexyl group; an alkenyl group such as a vinyl group, an allyl group, and a propenyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, and a naphthyl group; and an aralkyl group such as a benzyl group, a phenylethyl group, and a phenylpropyl group, and preferably a methyl group, an ethyl group, or a propyl group. m is an integer of 1 to 10, preferably an integer of 1 to 6, and more preferably an integer of 2 to 4. b is 0, 1 or 2, and preferably 0 or 1.

[0036] The organosilicon compound (hydrolyzable organosilane compound) of component (C) can be produced by known methods. Specifically, the compound can be produced by reacting a compound having a catechol structure and a terminal alkenyl group protected by an alkyl group with a triorganohydrogensilane in the presence of a catalyst (dehydrogenation condensation reaction and dealkane condensation reaction), or by protecting a compound having a terminal alkenyl group and a catechol structure with hexaorganodisilazane (triorganosilylation) to produce a compound having a catechol structure and a terminal alkenyl group blocked with a triorganosilyl group, and then hydrosilylating the compound having a catechol structure and a terminal alkenyl group blocked with a triorganosilyl group and a hydrogenorganosilane compound having a hydrolyzable silyl group in the presence of a catalyst.

[0037] Specific structural examples of component (C) include the following, where Me represents a methyl group, Et represents an ethyl group, Pr represents a propyl group, and Ph represents a phenyl group. [ka]

[0038] The amount of the (C) component is 0.1 to 10 parts by mass, preferably 0.2 to 8 parts by mass, more preferably 0.3 to 5 parts by mass, and most preferably 0.5 to 2 parts by mass, based on 100 parts by mass of the (A) component. If the amount of the (C) component is less than the lower limit (0.1 parts by mass), the desired adhesiveness cannot be obtained. On the other hand, if the amount of the (C) component is more than the upper limit (10 parts by mass), the rubber properties are deteriorated.

[0039] [(D) component] The component (D) is a curing catalyst. Examples of the curing catalyst include condensation catalysts that have been generally used as curing accelerators for compositions, such as organic tin compounds such as dibutyltin methoxide, dibutyltin diacetate, dibutyltin dioctate, dibutyltin dilaurate, dioctyltin dilaurate, dioctyltin dioctate, dioctyltin diversatate, dimethyltin dimethoxide, and dimethyltin diacetate; organic titanium compounds such as tetrapropyl titanate, tetrabutyl titanate, tetra-2-ethylhexyl titanate, and dimethoxytitanium diacetylacetonate; hexylamine, tetramethylguanidine, and salts thereof, and these may be used alone or in combination of two or more.

[0040] The amount of component (D) is 0.01 to 3 parts by mass, preferably 0.02 to 2.5 parts by mass, and more preferably 0.03 to 2 parts by mass, per 100 parts by mass of component (A). If the amount of component (D) is less than the lower limit, the catalytic effect is not obtained. If the amount of component (D) is more than the upper limit, the storage stability and appearance of the composition may deteriorate.

[0041] [(E) component] The room-temperature-curable organopolysiloxane composition of the present invention can contain, as component (E), a silane coupling agent represented by the following general formula (5) (i.e., a hydrolyzable organosilane compound having a nitrogen-functional group-containing monovalent hydrocarbon group) and / or a partial hydrolysis condensate thereof (an organosiloxane oligomer produced by partially hydrolyzing the organosilane compound and containing at least two, and preferably three or more, residual hydrolyzable groups in the molecule). [ka] (In the formula, R 10 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one nitrogen atom. 11 , R 12 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and c is 0, 1 or 2, preferably 0 or 1.

[0042] In the above formula (5), R 10 is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one group having a nitrogen atom (for example, an unsubstituted or substituted amino group, an unsubstituted or substituted imino group, an amido group, a ureido group, a guanidyl group, an isocyanate group, etc.), and specific examples thereof include monovalent hydrocarbon groups having 1 to 20 carbon atoms, particularly 3 to 14 carbon atoms, and having at least one nitrogen atom, such as an N-β(aminoethyl)-γ-aminopropyl group, a γ-aminopropyl group, an N-phenyl-γ-aminopropyl group, a γ-ureidopropyl group, a γ-isocyanatopropyl group, a γ-(2-butanimino)propyl group, a γ-formaminopropyl group, and a γ-tetramethylguanidylpropyl group. Among these, a γ-aminopropyl group and an N-β(aminoethyl)-γ-aminopropyl group are preferred. Also, R 11 , R 12are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, particularly 1 to 6 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, and octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine, bromine, and chlorine or cyano groups, for example, halogenated monovalent hydrocarbon groups such as 3-chloropropyl and 3,3,3-trifluoropropyl; and cyanoalkyl groups such as β-cyanoethyl and γ-cyanopropyl. Among these, methyl, ethyl, propyl, and isopropyl groups are preferred.

[0043] Specific examples of the silane coupling agent represented by formula (5) include γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropyltripropoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β(aminoethyl)-γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, γ-(2-butaneimino)propyltrimethoxysilane, γ-(2-butaneimino)propyltriethoxysilane, γ-formaminopropyltrimethoxysilane, γ-formaminopropyltriethoxysilane, γ-tetramethylguanidylpropyltrimethoxysilane, and the like. Among these, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, and N-β(aminoethyl)-γ-aminopropyltriethoxysilane are preferred.

[0044] The amount of the (E) component, when blended, is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, even more preferably 0.3 to 3 parts by mass, and most preferably 0.5 to 2 parts by mass, based on 100 parts by mass of the (A) component. If the amount of the (E) component is less than the lower limit (0.01 parts by mass), the desired adhesiveness may not be obtained. If the amount of the (E) component is more than the upper limit (5 parts by mass), not only is it disadvantageous in terms of cost, but it may also lead to reduced elongation, reduced chemical resistance, or deteriorated durability.

[0045] [Component (F)] The room temperature curable organopolysiloxane composition of the present invention may contain an inorganic filler as component (F). The inorganic filler is a reinforcing or non-reinforcing filler for imparting rubber properties to the composition. Examples of the filler include silica-based fillers such as dry silica such as calcined silica and fumed silica (also known as fumed silica and fumed silica), wet silica such as precipitated silica and sol-gel silica, which may be surface-treated or untreated, carbon black, talc, bentonite, calcium carbonate, zinc carbonate, magnesium carbonate, calcium oxide, zinc oxide, magnesium oxide, aluminum oxide, and aluminum hydroxide, among which calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide are preferred, and calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide, whose surfaces have been hydrophobized, are more preferred. In this case, it is preferred that these inorganic fillers have a low water content. There are no particular limitations on the type, amount, or treatment method of the surface treatment agent, but representative examples include organosilicon compounds such as chlorosilanes, alkoxysilanes, and organosilazanes, fatty acids, paraffins, silane coupling agents, and titanium coupling agents.

[0046] The inorganic filler of component (F) may be used alone or in combination of two or more kinds. When component (F) is used, the blending amount is preferably in the range of 1 to 500 parts by mass, more preferably 20 to 300 parts by mass, per 100 parts by mass of component (A). If it is less than 1 part by mass, sufficient rubber strength cannot be obtained, and the problem of being unsuitable for the intended use may arise, while if it exceeds 500 parts by mass, the ejection property from the cartridge deteriorates, storage stability decreases, and the mechanical properties of the obtained rubber properties may also deteriorate.

[0047] In addition, the room temperature curable organopolysiloxane composition of the present invention may contain other commonly known additives in addition to the above-mentioned components, as long as they do not impair the purpose of the present invention.Additives include polyethers as thixotropy improvers, silicone oils as plasticizers, isoparaffins, etc., and if necessary, colorants such as pigments, dyes, and fluorescent whitening agents, bioactive additives such as antifungal agents, antibacterial agents, and marine organism repellents, surface modifiers such as phenyl silicone oils, fluorosilicone oils, and organic liquids that are incompatible with silicone as bleeding oils, and solvents such as toluene, xylene, solvent volatile oils, cyclohexane, methylcyclohexane, and low boiling point isoparaffins.

[0048] The room-temperature-curable organopolysiloxane composition of the present invention can be prepared by mixing the above-mentioned components (A) to (D) and, if necessary, components (E) and (F) and other additives, etc., by known methods. The room-temperature curable organopolysiloxane composition of the present invention is a room-temperature curable composition, and the curing conditions are not particularly limited. For example, the composition (room-temperature curable organopolysiloxane composition) can be poured into a 2 mm mold and cured (left to stand) for 7 days at 23°C and 50% RH to obtain a cured product (silicone rubber sheet) having a thickness of 2 mm.

[0049] Furthermore, the room temperature curable organopolysiloxane composition of the present invention has adhesion to metals and resins, is chemically resistant to engine oils and long-life coolants, and gives a cured product having good rubber physical properties.

[0050] Examples of articles having a cured product obtained by curing the room-temperature-curable organopolysiloxane composition of the present invention include oil seals for automobile engines, oil seals for transmissions, oil seals for cooling coolants, and airtight seals for electrical components such as power control units, engine control units, and battery packs. EXAMPLES

[0051] The present invention will be specifically described below with reference to Synthesis Examples, Examples, and Comparative Examples, but the present invention is not limited to the following Examples. In all of the Examples and Comparative Examples, a planetary mixer (manufactured by Inoue Seisakusho Co., Ltd.) was used as an appropriate mixer. In the following Examples, physical properties such as viscosity (measured by a rotational viscometer) not otherwise specified are values ​​at 23°C.

[0052] A synthesis example of a silane compound having a hydrolyzable silyl group and a catechol structure protected by a silyl group in one molecule, which is used in the present invention, is shown below. The synthesized compound is 1 The synthesis was confirmed by H-NMR. In the following structural formulas, Me represents a methyl group and Et represents an ethyl group.

[0053] [Synthesis Example 1] 164g (1 mole) of eugenol, 400g of toluene, and 0.4g of pentafluorophenylboron were placed in a 2L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, and 244g (2.1 moles) of triethylsilane was added dropwise at an internal temperature of 90°C over 2 hours. After cooling to room temperature, 2g of Kyoward 500 (manufactured by Kyowa Chemical Industry Co., Ltd.) was added and stirred for 2 hours. After that, filtration and stripping were performed, and 374g of an organosilicon compound represented by the following formula (6) was obtained. 1 The H-NMR spectrum confirmed that the reaction product had the structure shown in the following chemical formula (6). [ka]

[0054] Into a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 189 g (0.5 mol) of the organosilicon compound (6) obtained above and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.5 × 10 platinum atoms) were added. -4 61 g (0.5 mol) of trimethoxysilane was added dropwise over 2 hours at an internal temperature of 75 to 85° C. After that, the mixture was stirred at 80° C. for 1 hour and stripped to obtain 247 g of a solution containing an organosilicon compound represented by the following formula (7). 1 The reaction product was confirmed to have the structure shown in the following chemical formula (7) by H-NMR spectrum. The obtained organosilicon compound is designated as Silane A. [ka]

[0055] [Synthesis Example 2] In a 2L separable flask equipped with a stirrer, reflux condenser, dropping funnel and thermometer, 150g (1 mol) of allylcatechol and 400g of toluene were placed, and 323g (2.0 mol) of hexamethyldisilazane was added dropwise over 4 hours at an internal temperature of 60°C. After that, stripping was performed to obtain 289g of an organosilicon compound represented by the following formula (8). 1 The H-NMR spectrum confirmed that the reaction product had the structure shown in the following chemical formula (8). [ka]

[0056] Into a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 147 g (0.5 mol) of the organosilicon compound (8) obtained above and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.5 × 10 platinum atoms) were added. -461 g (0.5 mol) of trimethoxysilane was added dropwise over 2 hours at an internal temperature of 75 to 85° C. After that, the mixture was stirred at 80° C. for 1 hour and stripped to obtain 197 g of a solution containing an organosilicon compound represented by the following formula (9). 1 The reaction product was confirmed to have the structure shown in the following chemical formula (9) by H-NMR spectrum. The obtained organosilicon compound is designated as Silane B. [ka]

[0057] [Comparative Synthesis Example 1] 164g (1 mole) of eugenol and 400g of toluene were placed in a 1L separable flask equipped with a stirrer, reflux condenser, dropping funnel and thermometer, and 162g (1 mole) of hexamethyldisilazane was added dropwise over 4 hours at an internal temperature of 60°C. After that, stripping was performed to obtain 229g of an organosilicon compound represented by the following formula (10). 1 The H-NMR spectrum confirmed that the reaction product had the structure shown in the following chemical formula (10). [ka]

[0058] Into a 1 L separable flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 118 g (0.5 mol) of the organosilicon compound (10) obtained above and a toluene solution of platinum-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex (0.5 × 10 platinum atoms) were added. -4 61 g (0.5 mol) of trimethoxysilane was added dropwise over 2 hours at an internal temperature of 75 to 85° C. After that, the mixture was stirred at 80° C. for 1 hour and stripped to obtain 171 g of a solution containing an organosilicon compound represented by the following formula (11). 1 The reaction product was confirmed to have the structure shown in the following chemical structural formula (11) by H-NMR spectroscopy. The obtained organosilicon compound is designated as Silane C. [ka]

[0059] [Example 1] (A) 100 parts by mass of dimethylpolysiloxane (where Y=oxygen atom, n=about 600, the same applies below) with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (in formula (1) Y=oxygen atom, n=about 600, the same applies below) was mixed with (F) 100 parts by mass of heavy calcium carbonate (trade name: MC Coat P-20, Maruo Calcium Co., Ltd.) whose surface was treated with paraffin, and (F) 10 parts by mass of fumed silica whose surface was treated with dimethyldichlorosilane, and then (B) 10 parts by mass of vinyltris(methylethylketoxime)silane was added and mixed under reduced pressure. Next, (C) 1 part by mass of silane A obtained in the above Synthesis Example 1 and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 1.

[0060] [Example 2] (A) 100 parts by mass of dimethylpolysiloxane with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (F) 100 parts by mass of heavy calcium carbonate with a surface treated with paraffin (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltris(methylethylketoxime)silane was added and mixed under reduced pressure. Next, (C) 1 part by mass of silane B obtained in the above Synthesis Example 2 and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 2.

[0061] [Example 3] (A) 100 parts by mass of dimethylpolysiloxane with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (F) 100 parts by mass of heavy calcium carbonate with a surface treated with paraffin (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltris(methylethylketoxime)silane was added and mixed under reduced pressure. Next, (C) 1 part by mass of silane B obtained in the above Synthesis Example 2, (E) 1 part by mass of γ-aminopropyltrimethoxysilane, and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 3.

[0062] [Example 4] (A) 100 parts by mass of dimethylpolysiloxane with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (F) 100 parts by mass of heavy calcium carbonate with a surface treated with paraffin (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltrimethoxysilane was added and mixed under reduced pressure. Next, (C) 1 part by mass of silane B obtained in the above Synthesis Example 2, (E) 1 part by mass of γ-aminopropyltrimethoxysilane, and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 4.

[0063] [Example 5] (A) 100 parts by mass of dimethylpolysiloxane (where Y=oxygen atom, n=approximately 600) with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with trimethoxysilyl groups (in formula (1)), (F) 100 parts by mass of heavy calcium carbonate (trade name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) with a surface treated with paraffin, and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltrimethoxysilane was added and mixed under reduced pressure. Next, (C) 1 part by mass of silane B obtained in the above Synthesis Example 2, (E) 1 part by mass of γ-aminopropyltrimethoxysilane, and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 5.

[0064] [Comparative Example 1] (A) 100 parts by mass of dimethylpolysiloxane with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (F) 100 parts by mass of heavy calcium carbonate with a surface treated with paraffin (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltris(methylethylketoxime)silane was added and mixed under reduced pressure. Next, (E) 1 part by mass of γ-aminopropyltrimethoxysilane and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 6.

[0065] [Comparative Example 2] (A) 100 parts by mass of dimethylpolysiloxane with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (F) 100 parts by mass of heavy calcium carbonate with a surface treated with paraffin (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltris(methylethylketoxime)silane was added and mixed under reduced pressure. Next, (C') 1 part by mass of silane C obtained in the above Comparative Synthesis Example 1 and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain Composition 7.

[0066] [Comparative Example 3] (A) 100 parts by mass of dimethylpolysiloxane with a viscosity of 20,000 mPa·s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxydimethylsilyl groups), (F) 100 parts by mass of heavy calcium carbonate with a surface treated with paraffin (product name: MC Coat P-20, manufactured by Maruo Calcium Co., Ltd.) and (F) 10 parts by mass of fumed silica with a surface treated with dimethyldichlorosilane were added and mixed, and then (B) 10 parts by mass of vinyltris(methylethylketoxime)silane was added and mixed under reduced pressure. Next, (C') 1 part by mass of silane C obtained in the above Comparative Synthesis Example 1, (E) 1 part by mass of γ-aminopropyltrimethoxysilane, and (D) 0.1 part by mass of dioctyltin diversatate were added and mixed thoroughly under reduced pressure to obtain composition 8.

[0067] The formulation of the obtained composition is shown in Tables 1 and 2.

[0068] [Table 1]

[0069] [Table 2]

[0070] [Test Method] The compositions (room temperature curable organopolysiloxane compositions) prepared in the above Examples and Comparative Examples were poured into a 2 mm mold and cured at 23°C and 50% RH for 7 days to obtain a 2 mm thick rubber sheet. The rubber properties (hardness, elongation at break, tensile strength) of the 2 mm thick sheet were measured in accordance with JIS K 6249.

[0071] This composition was also used to bond aluminum 25 mm wide and 100 mm long to a bond area of ​​2.5 mm using nylon 66 (PA66) (trade name: Zydel 80G33HS1L, manufactured by DuPont), polybutylene terephthalate (PBT) (trade name: Duranex 3300, manufactured by Polyplastics), and polyphenylene sulfide (PPS) (trade name: Thirsteel GS-40, manufactured by Tosoh Corporation), which are considered promising resins for automobile engines. 2 Shear adhesion test specimens (test specimens between the same materials) with a bond thickness of 1 mm were prepared and aged for 7 days at 23°C and 50% RH. Using these test specimens, the shear adhesive strength and cohesive failure rate for aluminum and each resin were measured according to the method specified in JIS K 6249, and the cohesive failure rates were compared.

[0072] In addition, to confirm chemical resistance (engine oil resistance), the obtained cured silicone rubber sheet and shear adhesion test specimen were immersed in engine oil [product name: Toyota Castle Oil SN 0W-20] and left at 120°C for 10 days, and then the same test as that performed at the initial stage of production was performed to confirm chemical resistance.

[0073] Furthermore, to confirm chemical resistance (LLC resistance), the cured silicone rubber sheet and shear adhesion test specimens obtained were immersed in a 50 mass% solution of LLC and tap water [product name: Toyota Super Long Life Coolant] and left at 100°C for 10 days, and then a test to confirm chemical resistance was performed in the same way as for the initial production. The test results for rubber properties (hardness, elongation at break, tensile strength), shear adhesive strength, and cohesive failure rate are shown as the average of three test results (N=3).

[0074] The results are shown in Table 3.

[0075] [Table 3]

[0076] In Examples 1 to 5, which used the room temperature curable organopolysiloxane composition of the present invention, good adhesion was shown from the beginning to aluminum, PA66, PBT, and PPS. Furthermore, good adhesion was maintained even after engine oil resistance and LLC resistance tests. For PBT after the LLC resistance test, the adherend deteriorated significantly, resulting in destruction of the adherend. On the other hand, Comparative Examples 1 and 3 did not contain the component (C) according to the present invention, but contained the component (E), and therefore showed a large decrease in physical properties after durability tests (for example, confirmation tests for chemical resistance 4 (LLC resistance)). In addition, Comparative Examples 2 and 3 contained the component (C') that did not have a catechol structure blocked with a triorganosilyl group (i.e., a structure in which one of the two hydroxyl groups present in the catechol is blocked and protected with a trimethylsilyl group, while the other is blocked and protected with a methyl group), but did not show any effect of improving adhesion to resins (initial adhesion). The above results demonstrate the effectiveness of the room temperature curable organopolysiloxane composition of the present invention.

Claims

1. (A) 100 parts by mass of a diorganopolysiloxane having hydroxyl groups and / or hydrolyzable silyl groups bonded to silicon atoms at both molecular chain terminals and having a viscosity at 23° C. of 20 to 1,000,000 mPa s, which is represented by the following general formula (1): [Formula 1] [In the formula, R 1 are independently a group selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and an alkoxyalkyl group having 2 to 10 carbon atoms. 2 is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms. a is independently 0, 1, or 2 for each silicon atom to which it is bonded, but R 1 is an alkyl group or an alkoxyalkyl group, a is independently 0 or 1 for each silicon atom to which it is bonded; 1 is a hydrogen atom, a is 2. n is a number that provides a viscosity of the diorganopolysiloxane at 23° C. of 20 to 1,000,000 mPa·s. Y is independently an oxygen atom, an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms, or a group represented by the following formula (2): [chemical 2] (In the formula, R 2 is as defined above, and Z is independently an unsubstituted or substituted divalent hydrocarbon group having 1 to 20 carbon atoms. The wavy line indicates the bonding position to the silicon atom. (B) a hydrolyzable organosilane compound having three or more hydrolyzable groups bonded to silicon atoms in the molecule other than the components (A), (C), and (D) and / or a partial hydrolysis condensate thereof: 0.1 to 40 parts by mass, (C) 0.1 to 10 parts by mass of a hydrolyzable organosilane compound represented by the following general formula (3) having a catechol structure blocked with a triorganosilyl group and a hydrolyzable silyl group in the molecule, and / or a partial hydrolyzed condensate thereof (wherein the partial hydrolyzed condensate is a partial hydrolyzed condensate having a triorganosilyl-group-blocked catechol structure obtained by hydrolysis and condensation of the hydrolyzable silyl group of the hydrolyzable silyl-group-containing monovalent hydrocarbon group represented by the following formula (4) in the hydrolyzable organosilane compound represented by the following general formula (3)): [C3] [In the formula, R 3 ~R 6 are each independently a group or atom selected from a hydrogen atom, an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4), 3 ~R 6 At least one of R is a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by the following formula (4): 7 are independently an unsubstituted or substituted monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms or an aryl group having 6 to 10 carbon atoms. [C4] (In the formula, R 8 , R 9 are each independently an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 10 carbon atoms, or an aryl group having 6 to 10 carbon atoms, b is 0, 1 or 2, and m is an integer from 1 to 10. The wavy line indicates the bonding position to the benzene ring. (D) Curing catalyst: 0.01 to 3 parts by mass A room temperature curable organopolysiloxane composition comprising:

2. In the general formula (3), R 7 2. The room temperature curable organopolysiloxane composition according to claim 1, wherein is a methyl group or an ethyl group.

3. R in the general formula (3) 3 ~R 6 In the above, R 4 and / or R 5 is a hydrolyzable silyl group-containing monovalent hydrocarbon group represented by formula (4), and the other R 3 ~R 6 3. The room-temperature-curable organopolysiloxane composition according to claim 1, wherein each independently represents a hydrogen atom or an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms.

4. The room-temperature-curable organopolysiloxane composition according to any one of claims 1 to 3, further comprising, as component (E), 0.01 to 5 parts by mass of a silane coupling agent represented by the following general formula (5) and / or a partial hydrolysis condensate thereof, per 100 parts by mass of component (A): [C5] (In the formula, R 10 R is a monovalent hydrocarbon group having 1 to 20 carbon atoms and at least one nitrogen atom. 11 , R 12 are each independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and c is 0, 1, or 2.

5. 5. The room-temperature-curable organopolysiloxane composition according to claim 1, further comprising at least one inorganic filler as component (F).

6. A cured product obtained by curing the room temperature curable organopolysiloxane composition according to any one of claims 1 to 5.

7. An article comprising the cured product according to claim 6.

Citation Information

Patent Citations

  • Room temperature curable organopolysiloxane composition

    JP2004292724A

  • Method to adhere plated substrate, surface-modified plated substrate, and composite molded article

    JP2010144148A

  • Organic silicon compound, adhesive composition, and article

    JP2015182978A

  • Room temperature curable organopolysiloxane composition

    JP3518399B2

  • Room temperature curable organopolysiloxane composition

    JP3714861B2