Manufacturing method of copper powder
By employing a two-step polyol solvent process with varying molecular weights, the method controls gas generation and maintains particle size, addressing the delamination issue in copper powder used for multilayer ceramic capacitors.
Patent Information
- Application Number
- JP2021086747
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-27
- Filing Date
- 2021-05-24
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-05-24
AI Technical Summary
Copper powder produced by existing methods, such as the polyol method, generates excessive gas during firing, leading to potential voids between the copper powder and dielectric layers in multilayer ceramic capacitors, compromising their integrity.
A method involving the use of two polyol solvents with different average molecular weights to control the generation of gas during the reduction process, where copper nuclei are first generated in a high molecular weight solvent and then grown in a lower molecular weight solvent, thereby controlling the particle size and reducing organic film formation.
This approach effectively reduces the amount of gas generated during firing, ensuring the copper powder maintains its particle size and oxidation resistance, preventing delamination issues in multilayer ceramic capacitors.
Smart Images

Figure 0007552501000002 
Figure 0007552501000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing copper powder by reducing a copper compound in a polyol. [Background technology]
[0002] Copper powder is also used as a material for conductive pastes to form internal and external electrodes of multilayer ceramic capacitors (MLCCs), which are electronic components, and electrodes of multilayer ceramic substrates. In recent years, as multilayer ceramic capacitors become smaller and have larger capacities, the internal electrodes are becoming thinner. For this purpose, the copper powder used in the conductive pastes (internal electrode pastes) is also required to be fine. Furthermore, it is required that the copper powder is monodispersed (monodispersed particles) with few connected particles, and has excellent oxidation resistance.
[0003] The most common method for producing copper powder is the so-called electrolytic method. However, the copper powder obtained by this method is likely to become coarse aggregates. As a method for obtaining fine copper powder, for example, Patent Document 1 discloses a method of wet reducing copper oxide in the presence of a coupling agent, and Patent Document 2 discloses a method of gas-phase reducing copper chloride, and a method using a disproportionation reaction has also been proposed. However, the copper powder obtained by these methods all have high surface activity, and may be oxidized by heating for resin hardening when used as a paste, or may be oxidized by oxygen present in small amounts in the atmosphere during firing for the purpose of volatilizing organic matter, and therefore it has not been possible to satisfy all of the requirements for fineness, monodispersity, and oxidation resistance.
[0004] In order to solve the above problems, Patent Documents 3 and 4 disclose a method of reducing copper oxide powder by heating it in a polyol solvent (polyol method). The copper powder obtained by this method (polyol copper powder) has excellent monodispersity and oxidation resistance, and is suitable for the above-mentioned conductive paste. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2-34708 [Patent Document 2] Japanese Patent Publication No. 62-63604 [Patent Document 3] Japanese Patent Application Publication No. 59-173206 [Patent Document 4] Japanese Patent Application Publication No. 5-222413 Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the copper powder (polyol copper powder) obtained by the method (polyol method) described in Patent Documents 3 and 4 above is fired, gas components derived from the organic coating formed on the copper powder surface are generated. When the copper powder is used for the internal electrodes of a multilayer ceramic capacitor, there is a risk of voids (delamination) occurring between the dielectric layer.
[0007] An object of the present invention is to provide a method for producing copper powder in a polyol process in which copper oxide powder is reduced in a polyol solvent to obtain copper powder, which can control the amount of gas generated during firing of the resulting copper powder. [Means for solving the problem]
[0008] As a result of intensive research into solving the above problems, the present inventors discovered that by changing the polyol solvent around the time when copper nuclei appear from the copper oxide powder as the reduction reaction progresses, the particle size of the resulting copper powder becomes close to that obtained when the unchanged polyol solvent is used, and the amount of gas generated during firing of the copper powder becomes close to that obtained when the changed polyol solvent is used, and thus completed the present invention.
[0009] According to an aspect of the present invention, there is provided a method for producing copper powder by reducing copper oxide powder in a polyol solvent to obtain copper powder, the method including the steps of generating copper nuclei from copper oxide powder using a first polyol solvent, and causing grain growth of the copper nuclei using a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent.
[0010] In the method for producing copper powder, the first polyol solvent and the second polyol solvent preferably have an average molecular weight difference of 10% or more. The copper oxide powder is preferably one or more selected from the group consisting of copper oxide and cuprous oxide. The moisture content of the copper oxide powder is preferably 10% by mass or less. The step of generating copper nuclei is preferably performed until the proportion of copper nuclei in the cuprous oxide powder containing copper nuclei reaches 0.1 to 0.5 in molar fraction relative to the total amount of the cuprous oxide powder containing copper nuclei. Effect of the Invention
[0011] According to the method for producing copper powder according to this embodiment, in the polyol method in which copper oxide powder is reduced in a polyol solvent to obtain copper powder, the amount of gas generated during firing of the obtained copper powder can be easily controlled. [Brief description of the drawings]
[0012] [Figure 1] 1 is a flowchart showing an example of a method for producing copper powder according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A specific embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention. In addition, in this specification, the expression "X to Y" (X and Y are arbitrary numerical values) means "X or more and Y or less."
[0014] In the polyol method, when copper oxide powder is suspended in a polyol solvent and heated, the polyol solvent acts as a reducing agent, and reduction to copper powder proceeds. When copper oxide (CuO) is used as the copper oxide powder, reduction from copper oxide (CuO) to copper (Cu) occurs via cuprous oxide (Cu2O), and when cuprous oxide (Cu2O) is used as the copper oxide, cuprous oxide (Cu2O) is reduced to copper (Cu), and in either case, copper powder (hereinafter sometimes referred to as "polyol copper powder") is finally obtained. The obtained copper powder is washed with pure water or the like and filtered, and then washed again and dried as necessary. Specifically, as an example of washing, a method is used in which the copper powder obtained by reduction (polyol copper powder) is allowed to settle and decanted, and then pure water or the like is supplied and stirred for washing. As an example of filtration, a method is used in which dehydration is performed by centrifugation.
[0015] The method for producing copper powder according to the present embodiment is a method for producing copper powder by reducing copper oxide powder in a polyol solvent to obtain copper powder, and includes a reduction step S1 in which copper nuclei are generated from the copper oxide powder using a first polyol solvent, and a reduction step S2 in which the copper nuclei are grown by using a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent (see FIG. 1). The method for producing copper powder according to the present embodiment includes, for example, a reduction step S1 in which the copper oxide powder is heated to a temperature of the first polyol solvent at a temperature of −50° C. or more and less than the boiling point of the first polyol solvent ±0° C. to generate copper nuclei from the copper oxide powder, and a reduction step S2 in which the solvent is changed to a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent, and the copper nuclei are grown by heating to a temperature of −50° C. or more and less than the boiling point of the second polyol solvent ±0° C. to grow into copper powder. The method for producing copper powder according to the present embodiment is characterized in that the polyol solvent is changed from the first polyol solvent to a second polyol solvent having a smaller average molecular weight than the first polyol solvent, and the second polyol solvent is used to grow the copper nuclei generated from the copper oxide powder. In the method for producing copper powder according to the present embodiment, for example, when copper oxide is used as the copper oxide powder, it is reduced to copper via cuprous oxide as the reduction reaction progresses, but in the stage (reduction step S1) of cuprous oxide powder containing copper nuclei (in the middle of the reduction from cuprous oxide to copper), which is the intermediate stage, the polyol solvent is changed to a polyol solvent having a smaller average molecular weight than the polyol solvent used in the reduction step S1 (reduction step S2), so that the amount of gas generated during sintering of the copper powder (polyol copper powder) obtained by the polyol method can be controlled. The first polyol solvent and the second polyol solvent may be a mixture of multiple types of polyols described below, but when multiple types of polyols are mixed, the boiling point of the polyol with the lowest boiling point is considered to be the boiling point of the mixed polyol solvent. For example, when diethylene glycol (boiling point: 245°C) and ethylene glycol (boiling point: 197°C) are mixed as the second polyol solvent, the boiling point of the second polyol solvent is considered to be 197°C.
[0016] The method for producing copper powder according to the present embodiment will now be described in detail. Fig. 1 is a flow chart showing an example of the method for producing copper powder according to the present embodiment.
[0017] (Reduction step S1) The reduction step S1 is a step of generating copper nuclei from copper oxide powder using a first polyol solvent by a polyol method. For example, in the reduction step S1, the raw copper oxide powder is suspended in a first polyol solvent to form a reaction liquid, and the liquid temperature of the first polyol solvent is heated to a temperature that is equal to or higher than the boiling point of the first polyol solvent minus 50°C and equal to or lower than the boiling point of the first polyol solvent ±0°C to obtain cuprous oxide powder containing copper nuclei. The temperature that is equal to or higher than the boiling point of the first polyol solvent minus 50°C and equal to or lower than the boiling point of the first polyol solvent ±0°C means, for example, a temperature that is equal to or higher than 250°C (boiling point minus 50°C) and equal to or lower than 300°C (boiling point ±0°C) when the boiling point of the first polyol solvent is 300°C.
[0018] The raw copper oxide powder is preferably one or more powders selected from the group consisting of copper oxide and cuprous oxide. The amount of moisture contained in the raw copper oxide powder is preferably 10% by mass or less. In the polyol method, if water is present in the system, oxidation of the polyol solvent proceeds, and the aldehyde compound produced starts to produce polyol copper powder before the total amount of copper oxide (CuO) becomes cuprous oxide (Cu2O). If the amount of moisture in the copper oxide powder exceeds 10% by mass, this effect becomes significant, and homogeneous copper powder (polyol copper powder) may not be obtained.
[0019] The ratio of copper nuclei in the cuprous oxide powder containing copper nuclei obtained in the reduction step S1 is not particularly limited as long as it contains copper nuclei generated by the polyol reaction, but when it is required to control not only the amount of gas generated when the obtained copper powder is fired but also the particle size of the copper powder, the molar fraction relative to the total amount of cuprous oxide powder containing copper nuclei is preferably 0.1 to 0.5, more preferably 0.2 to 0.4. In such a case, it is preferable that the amount of copper nuclei generated in the reduction step S1 is the above-mentioned ratio of copper nuclei. In addition, it is preferable that the reduction step S1 is a stage until the amount of copper nuclei reaches the above-mentioned ratio of copper nuclei. The conditions such as the time and temperature of the polyol reaction that are the above-mentioned preferable stage can be obtained by preliminary experiments, etc.
[0020] Considering that the organic coating formed on the copper powder surface is a product of oxidation, decomposition, and polymerization of the polyol solvent, it is considered that reducing the molecular weight of the polyol solvent used for reduction is effective in reducing the gas components derived from the organic coating, but since the reaction temperature of the reduction cannot be raised above the boiling point of the solvent, if the polyol solvent is changed to a low molecular weight one, the particle size of the copper powder obtained increases due to the decrease in reaction temperature, and the particle size is not the same as that of the copper powder obtained when the reduction is performed using the polyol solvent before the change. In the method for producing copper powder of this embodiment, when the amount of copper nuclei generated in the reduction step S1 is within the above-mentioned preferred range, even if the polyol solvent used in the reduction steps S1 and S2 is changed as in this embodiment, the particle size of the copper powder (polyol copper powder) obtained after reduction can be more reliably made almost the same as that when the copper powder is produced using only the polyol solvent before the change.
[0021] In this embodiment, in the reduction step S2 described later, the cuprous oxide powder is consumed for the grain growth of the copper nuclei obtained in the reduction step S1, and an organic coating is formed on the surface of the copper particles. If the ratio of the copper nuclei in the cuprous oxide powder containing copper nuclei is less than 0.1 in molar fraction relative to the mixture of cuprous oxide and copper nuclei, the number of copper particles serving as nuclei for grain growth is small, and the copper powder may have a coarser particle size than when the copper oxide powder is reduced by the polyol method using only the first polyol solvent. Therefore, when importance is attached to the control of the particle size of the obtained copper powder, it is preferable that the ratio of the copper nuclei in the cuprous oxide powder containing copper nuclei is 0.1 or more in molar fraction relative to the mixture of cuprous oxide and copper nuclei. On the other hand, when the ratio of copper nuclei in the cuprous oxide powder containing copper nuclei is greater than 0.5 in terms of molar fraction relative to the mixture of cuprous oxide and copper nuclei, the amount of cuprous oxide that can be consumed in the reduction step S2 is small, so the ratio of the organic coating formed by the second polyol solvent is small, and the organic coating of the obtained copper powder is mostly formed by the first polyol solvent in the reduction step S1, so that the effect of controlling the amount of gas generated may be reduced. In this embodiment, the ratio of copper nuclei in the cuprous oxide powder containing copper nuclei can be obtained by filtering the reaction solution (polyol in which the copper component is suspended) during the reduction reaction every time elapses, and the ratio of copper nuclei can be obtained from the difference in mass between the copper component and the copper component before the reduction reaction, and the ratio of the copper nuclei can also be obtained from the composition analysis of the copper component. Therefore, it is preferable to perform a preliminary evaluation of the time elapsed in the reduction step S1 and the ratio of copper nuclei in advance under the same conditions, and to determine the time of the reduction step S1 from the obtained results.
[0022] When cuprous oxide powder is used as the copper oxide powder, the reduction step S1 is a step in which a portion of the cuprous oxide is reduced to a state containing copper nuclei, and preferably, as described above, a step in which the proportion of copper nuclei becomes 0.1 to 0.5 in molar fraction relative to the total amount of the cuprous oxide powder containing copper nuclei.
[0023] The mechanism by which the amount of gas generated by the copper powder (polyol copper powder) obtained after reduction changes when the polyol solvent used in the reduction step S1 and reduction step S2 is changed as described above is unclear in detail, but is presumed to be as follows. In the reduction reaction process in the polyol solvent, copper powder is formed from copper oxide, and polyol molecules in the polyol solvent and aldehyde compounds and carboxyl compounds, which are the oxidized forms of polyol molecules, decompose or polymerize with each other, generating various organic substances, which are physically or chemically bonded to the copper particle surface to form an organic coating. Therefore, the organic substances that constitute the organic coating are derived from the polyol solvent, and if the polyol molecules used in the polyol solvent have a low molecular weight, it is considered that the various organic substances generated from it are also likely to have a low molecular weight. In other words, when the average molecular weight of the second polyol solvent used in the reduction step S2 is smaller than the average molecular weight of the first polyol solvent used in the reduction step S1, the organic coating of the obtained copper powder has a relatively low molecular weight, and as a result, the amount of gas generated during sintering is reduced. The mechanism by which the amount of gas generated by the copper powder (polyol copper powder) obtained after reduction changes is not limited to the above-mentioned mechanism.
[0024] The mechanism by which the particle size of the copper powder (polyol copper powder) obtained after reduction does not change even when the polyol solvent used in the reduction step S1 and the reduction step S2 is changed is unclear in detail, but is presumed to be as follows. If the copper nuclei generated in the reduction step S1 reach a certain level or higher, the degree of supersaturation of the copper ions in the solvent will not exceed the critical degree of supersaturation at which spontaneous nucleation occurs even locally, and the generation of new copper nuclei will be suppressed, and the copper ions eluted from the copper oxide will be used for the grain growth of the already existing copper nuclei. Therefore, even if the polyol solvent is changed in the reduction step S1 and the reduction step S2, as long as the ratio of copper nuclei in the cuprous oxide powder containing copper nuclei is within the above-mentioned ratio range, the number of particles of the copper nuclei formed in the reduction step S1 will not increase or decrease, so the particle size of the obtained copper powder will not change much. Note that the mechanism by which the particle size of the copper powder (polyol copper powder) obtained after reduction does not change even when the polyol solvent used in the reduction step S1 and the reduction step S2 is changed is not limited to the above-mentioned mechanism. The reduction step S1 will be further explained later.
[0025] (Reduction process S2) The reduction step S2 is a step of growing the copper nuclei into particles by the polyol method using a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent. In the reduction step S2, the cuprous oxide powder containing the copper nuclei obtained in the reduction step S1 is treated with a second polyol to grow the copper nuclei into particles. In the reduction step S2, for example, the copper nuclei are suspended in the second polyol solvent to form a reaction liquid, and the liquid temperature of the second polyol solvent is heated to a temperature of the boiling point of the second polyol solvent -50°C or more and the boiling point of the second polyol solvent ±0°C or less to grow the copper nuclei into copper powder (polyol copper powder). Note that the material to be subjected to the reduction step S2 may contain copper oxide powder in addition to the cuprous oxide powder containing the copper nuclei. The method of subjecting the cuprous oxide powder containing copper nuclei obtained in the reduction step S1 to the reduction step S2 is not particularly limited. For example, a method of subjecting the cuprous oxide powder containing copper nuclei to the reduction step S2 by separating the cuprous oxide powder containing copper nuclei from the first polyol solvent and suspending the separated cuprous oxide powder containing copper nuclei in a second polyol solvent, or a method of preparing the second polyol solvent by additionally mixing polyol into the reaction solution after the reduction step S1 is completed, when the second polyol solvent is mixed with the first polyol solvent, can be used. In addition, the method of separating the cuprous oxide powder containing copper nuclei obtained in the reduction step S1 is not particularly limited, and any method can be used.
[0026] In the method for producing copper powder according to this embodiment, a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent is used in the reduction step S2. The average molecular weight of the second polyol solvent is preferably 10% or more smaller than that of the first polyol solvent. In this embodiment, the average molecular weight of the second polyol solvent is 10% or more smaller than that of the first polyol solvent, meaning that, when the average molecular weight of the first polyol solvent is MW1 and the average molecular weight of the second polyol solvent is MW2, MW2≦MW1-(MW1×0.1)=0.9×MW1 is satisfied. As explained above, when the average molecular weight of the second polyol solvent is smaller than that of the first polyol solvent, the organic coating of the obtained copper powder has a low molecular weight, and the amount of gas generated during sintering is reduced. When the difference between the average molecular weight of the first polyol solvent and the average molecular weight of the second polyol solvent is 10% or more, this effect becomes significant. When the first polyol solvent and the second polyol solvent are a mixture of a plurality of polyols described below, the average molecular weight is calculated as a weighted average weighted according to the content ratio of the polyols. Furthermore, the second polyol solvent may be prepared by mixing a polyol with the first polyol solvent, so that the average molecular weight of the second polyol solvent is 10% or more smaller than the average molecular weight of the first polyol solvent.
[0027] The cuprous oxide powder containing copper nuclei to be subjected to the reduction step S2 may be one that has been subjected to a washing step after the reduction step S1. Washing may be performed using a solvent other than polyol, such as water. For example, when washing is performed using a water-based solvent, it is preferable to perform solid-liquid separation such as filtration, and then heat or dry the cuprous oxide powder containing copper nuclei after washing so that the water content in the cuprous oxide powder containing copper nuclei after washing is 10 mass% or less. Also, after the reduction step S1, the reaction liquid having the cuprous oxide powder containing the copper nuclei is cooled, and the polyol used in the reduction step S1 is mixed with a polyol to prepare a second polyol solvent, which may then be subjected to the reduction step S2. In this case, the treatment can be easily carried out.
[0028] The first polyol solvent and the second polyol solvent will be further described. In the method for producing copper powder according to this embodiment, the average molecular weight of the second polyol solvent is smaller than that of the first polyol solvent as described above. That is, the first polyol solvent and the second polyol solvent have different compositions. Here, the first polyol solvent and the second polyol solvent have different compositions, which means that the compositions of the entire solvent are different, and includes an embodiment in which at least a part of the type of polyol used is common between the first polyol solvent and the second polyol solvent, but the composition of the entire solvent is different. This embodiment may be, for example, an embodiment in which the first polyol solvent and the second polyol solvent are each a mixture of polyols containing ethylene glycol, and the average molecular weights of each of them are different.
[0029] The polyols (polyol solvents) used as the first polyol solvent and the second polyol solvent are polyhydric alcohols having a reducing effect on copper oxide powder, and preferably have 2 to 6 OH groups. The first polyol solvent and the second polyol solvent are appropriately selected, for example, according to the characteristics of the copper powder to be produced, and specifically, one or more selected from ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propylene glycol, trimethylene glycol, polyethylene glycol, and phenyl diglycol are preferred. The solvent used in the polyol method may contain other components within the scope of the present invention.
[0030] In the method for producing copper powder according to the present embodiment, the first polyol solvent used in the reduction step S1 and the second polyol solvent used in the reduction step S2 are preferably different in average molecular weight by 10% or more from the viewpoint of controlling the amount of gas generated, and more preferably different in average molecular weight by 20% or more. If the difference in average molecular weight is less than 10%, as described above, the molecular weight of the various organic substances constituting the organic coating is poorly changed, and the effect of controlling the amount of gas generated is reduced. From the above-mentioned viewpoints, the second polyol solvent is preferably small in molecular weight, for example, ethylene glycol. In addition, as shown in the examples, the first polyol solvent can be a polyol solvent having the same composition as that selected in the conventional method using one type of polyol solvent.
[0031] The temperature (heating temperature) at which the polyol solvent (first polyol solvent or second polyol solvent) is heated in the reduction step S1 or reduction step S2 is preferably set to a liquid temperature of the polyol boiling point minus 50°C or more and the polyol boiling point ±0°C or less, and more preferably set to the polyol boiling point minus 40°C or more and the polyol boiling point minus 5°C or less. If the heating temperature is set to a temperature lower than -50°C relative to the boiling point of the polyol solvent, the reduction reaction may not proceed sufficiently and cuprous oxide (CuO) may remain, resulting in a high oxygen content in the obtained copper powder (polyol copper powder), and the reaction time may be significantly extended, resulting in a deterioration in productivity. In addition, if the heating temperature is set higher than the boiling point of the polyol, the polyol may be significantly reduced (consumed) due to volatilization, and the reduction may not be sufficient. Here, when a mixture of multiple polyols is used as the polyol solvent, the boiling point of the polyol solvent is set to the boiling point of the polyol solvent with the lowest boiling point.
[0032] By the reduction step S2, a monodisperse polyol copper powder can be obtained. Note that the conditions of the polyol reaction in the reduction step S2, such as temperature and time, can be determined by carrying out a preliminary experiment.
[0033] In the method for producing copper powder of this embodiment, the carbon content of the polyol copper powder obtained can be reduced more than that of the conventional method. For example, the carbon content of the polyol copper powder obtained when copper powder is reduced from copper oxide powder without changing the first polyol solvent used in the reduction step S1 during the process can be significantly suppressed (controlled). Therefore, in the method for producing copper powder of this embodiment, the amount of gas generated during sintering of the polyol copper powder obtained when copper powder is reduced from copper oxide powder without changing the first polyol solvent used in the reduction step S1 during the process can be significantly suppressed (controlled) compared to the amount of gas generated from the polyol copper powder obtained when copper powder is reduced from copper oxide powder without changing the first polyol solvent used in the reduction step S1 during the process. In this embodiment, the amount of gas generated from the copper powder (polyol copper powder) is a value calculated by the method described in the examples described later.
[0034] The method for producing copper powder of this embodiment can be easily carried out because the polyol reaction is carried out using a polyol solvent used in the conventional polyol method as described above and a polyol solvent having a smaller average molecular weight than the polyol solvent.
[0035] As described above, the method for producing copper powder according to the present embodiment is a method for producing copper powder by reducing copper oxide powder in a polyol solvent to obtain copper powder, and includes a step of generating copper nuclei from copper oxide powder using a first polyol solvent, and a step of growing the copper nuclei by using a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent. Note that in the method for producing copper powder according to the present embodiment, the configuration other than the above is optional. According to the method for producing copper powder according to the present embodiment, in the polyol method in which copper oxide powder is reduced in a polyol solvent to obtain copper powder, the amount of gas generated during firing of the obtained copper powder can be easily controlled. EXAMPLES
[0036] The present invention will be described in more detail below by way of examples and comparative examples, but the present invention is not limited to the following examples. The methods for measuring physical properties are as follows.
[0037] (1) Average particle size The average particle size of the obtained copper powder (polyol copper powder) was determined as the particle size at which the relative particle number on a volume basis became 50% using a laser diffraction scattering type particle size measuring device (LA950V2, manufactured by Horiba, Ltd.). (2) Amount of gas generated The amount of gas generated from the obtained copper powder (polyol copper powder) was measured by using a thermogravimetric analyzer (TG-DTA: TG-DTA 2020SA, manufactured by Bruker-AXS) to measure the mass loss rate from room temperature to 700 ° C when the temperature was raised at 10 ° C / min in a He inert gas atmosphere. In addition, the gas generated by thermogravimetric measurement was measured using a mass spectrometer (Q-MS: MS9600, manufactured by Bruker-AXS) to measure the mass spectrum of m / z = 44 (corresponding to carbon dioxide), and the intensity peak area of the mass spectrum in the range from 150 ° C to 700 ° C (the area between the graph and the axis representing the Celsius temperature in a graph of Celsius temperature - mass spectrum intensity) was calculated, and the intensity peak area of this mass spectrum was used as an index of the amount of gas generated. In addition, the carbon content of the obtained copper powder (polyol copper powder) was measured using a carbon sulfur analyzer (CS844, manufactured by LECO).
[0038] Example 1 30 g of copper oxide (CuO) powder (Furukawa Chemicals, product number: FCO-M6) was placed in a 200 ml separable flask as copper oxide powder, 100 g of diethylene glycol (abbreviation: DEG, boiling point: 245°C, molecular weight: 106) was added, and the polyol solvent was heated to 230°C and kept at that temperature for 45 minutes while stirring to carry out a reduction reaction (reduction reaction S1). After cooling the reaction solution, cuprous oxide powder containing copper nuclei was obtained. The ratio of copper nuclei in the cuprous oxide powder containing copper nuclei was 0.4 in molar fraction relative to the total amount of cuprous oxide powder containing copper nuclei. The ratio of copper nuclei in the cuprous oxide powder containing copper nuclei was a value obtained by evaluating the ratio of copper nuclei at the time of 45 minutes of reduction reaction in a preliminary test carried out under the same conditions. The proportion of copper nuclei in the cuprous oxide powder containing copper nuclei was calculated by filtering the reaction solution (polyol in which copper components are suspended) subjected to a 45-minute reduction reaction, and calculating the difference between the mass and the mass when all of the copper oxide was reduced to cuprous oxide. It was also confirmed that no copper oxide remained as a copper component after the 45-minute reduction reaction.
[0039] The cuprous oxide powder containing copper nuclei was separated into solid and liquid by centrifugation, and the cuprous oxide powder containing copper nuclei was dispersed in 100 g of ethylene glycol (abbreviation: EG, boiling point: 197°C, molecular weight: 62), heated to a liquid temperature of 190°C, and held at that temperature for 60 minutes while stirring to carry out a reduction reaction (reduction reaction S2). After cooling the reaction liquid, the polyol copper powder produced was centrifuged, washed, and dried.
[0040] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.46 μm. The carbon content was 0.14 wt%, the mass loss rate in thermogravimetry was 0.38%, and the intensity peak area of the mass spectrum at m / z = 44 was 8.9 × 10 -9 The production conditions and measurement results are shown in Table 1.
[0041] Example 2 The reaction mixture was reduced to cuprous oxide powder containing a copper nucleus of 0.4 in molar fraction by the same procedure as in Example 1, and after cooling the reaction mixture, 30 g of ethylene glycol was added and heated to a liquid temperature of 190°C, and the reduction reaction was carried out by maintaining the temperature at 190°C for 60 minutes while stirring. The polyol solvent was a mixed solvent of diethylene glycol and ethylene glycol, and the average molecular weight was 96 based on the weight ratio of each. After cooling the reaction mixture, the polyol copper powder produced was centrifuged, washed, and dried.
[0042] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.45 μm. The carbon content was 0.17% by weight, the mass loss rate in thermogravimetry was 0.40%, and the intensity peak area of the mass spectrum at m / z = 44 was 9.4 × 10 -9 The production conditions and measurement results are shown in Table 1.
[0043] Example 3 A cuprous oxide powder containing copper nuclei with a molar fraction of 0.4 was obtained by the same operation as in Example 1, except that triethylene glycol was used instead of diethylene glycol, and the heating temperature in the reduction step S1 was 260°C and the stirring time was 30 minutes. The cuprous oxide powder containing copper nuclei was subjected to solid-liquid separation by centrifugation, and the cuprous oxide powder containing copper nuclei was dispersed in 100 g of ethylene glycol (abbreviation: EG, boiling point: 197°C, molecular weight: 62), heated to a liquid temperature of 190°C, and held at that temperature for 60 minutes while stirring, to carry out a reduction reaction. After cooling the reaction liquid, the polyol copper powder produced was centrifuged, washed, and dried.
[0044] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.22 μm. The carbon content was 0.25% by weight, the mass loss rate in thermogravimetry was 0.63%, and the intensity peak area of the mass spectrum at m / z = 44 was 7.6 × 10 -9 The production conditions and the measurement results are shown in Table 1.
[0045] Example 4 The reaction mixture was reduced to cuprous oxide powder containing a copper nucleus of 0.4 in molar fraction by the same procedure as in Example 3, and after cooling the reaction mixture, 30 g of ethylene glycol was added and heated to a liquid temperature of 190°C, and the reduction reaction was carried out by maintaining the temperature at 190°C for 60 minutes while stirring. The polyol solvent was a mixed solvent of triethylene glycol and ethylene glycol, and the average molecular weight was 130 based on the weight ratio of each. After cooling the reaction mixture, the polyol copper powder produced was centrifuged, washed, and dried.
[0046] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.21 μm. The carbon content was 0.25% by weight, the mass loss rate in thermogravimetry was 0.61%, and the intensity peak area of the mass spectrum at m / z = 44 was 7.9 × 10 -9 The production conditions and the measurement results are shown in Table 1.
[0047] Example 5 A cuprous oxide powder containing copper nuclei with a molar fraction of 0.4 was obtained by the same operation as in Example 1, except that tetraethylene glycol was used instead of diethylene glycol, the heating temperature in the reduction step S1 was 300°C, and the stirring time was 20 minutes. The cuprous oxide powder containing copper nuclei was subjected to solid-liquid separation by centrifugation, and the cuprous oxide powder containing copper nuclei was dispersed in 100 g of ethylene glycol (abbreviation: EG, boiling point: 197°C, molecular weight: 62), heated to a liquid temperature of 190°C, and held at that temperature for 60 minutes while stirring, to carry out a reduction reaction. After cooling the reaction liquid, the polyol copper powder produced was centrifuged, washed, and dried.
[0048] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.19 μm. The carbon content was 0.29 wt%, the mass loss rate in thermogravimetry was 0.68%, and the intensity peak area of the mass spectrum at m / z = 44 was 8.0 × 10 -9 The production conditions and measurement results are shown in Table 1.
[0049] Example 6 The reaction mixture was reduced to cuprous oxide powder containing a copper nucleus of 0.4 in molar fraction by the same procedure as in Example 5, and after cooling the reaction mixture, 30 g of ethylene glycol was added and heated to a liquid temperature of 190°C, and the reduction reaction was carried out by maintaining the temperature at 190°C for 60 minutes while stirring. The polyol solvent was a mixed solvent of triethylene glycol and ethylene glycol, and the average molecular weight was 164 based on the weight ratio of each. After cooling the reaction mixture, the polyol copper powder produced was centrifuged, washed, and dried.
[0050] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.18 μm. The carbon content was 0.34 wt%, the mass loss rate in thermogravimetry was 0.84%, and the intensity peak area of the mass spectrum at m / z = 44 was 8.9 × 10 -9 The production conditions and measurement results are shown in Table 1.
[0051] Comparative Example 1 30 g of copper oxide (CuO) powder (Furukawa Chemicals, product number: FCO-M6) was placed in a 200 ml separable flask as copper oxide powder, 100 g of diethylene glycol was added, and the polyol solvent was heated to 230°C and held at that temperature for 90 minutes while stirring to carry out a reduction reaction. After cooling the reaction solution, the resulting polyol copper powder was centrifuged, washed, and dried.
[0052] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.45 μm. The carbon content was 0.20 wt%, the mass loss rate in thermogravimetry was 0.47%, and the intensity peak area of the mass spectrum at m / z = 44 was 15.8 × 10 -9 The production conditions and measurement results are shown in Table 1.
[0053] Comparative Example 2 A polyol copper powder was obtained in the same manner as in Comparative Example 1, except that triethylene glycol was used instead of diethylene glycol, the polyol solvent was heated to 260° C., and stirred for 60 minutes.
[0054] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.22 μm. The carbon content was 0.29 wt%, the mass loss rate in thermogravimetry was 0.71%, and the intensity peak area of the mass spectrum at m / z = 44 was 8.4 × 10 -9 The production conditions and measurement results are shown in Table 1.
[0055] Comparative Example 3 A polyol copper powder was obtained in the same manner as in Comparative Example 1, except that tetraethylene glycol was used instead of diethylene glycol, the polyol solvent was heated to 300° C., and stirred for 60 minutes.
[0056] The particle size distribution of the obtained polyol copper powder was measured and it was found to be monodisperse particles with an average particle size of 0.17 μm. The carbon content was 0.43 wt%, the mass loss rate in thermogravimetry was 0.97%, and the intensity peak area of the mass spectrum at m / z = 44 was 10.5 × 10-9 The production conditions and the measurement results are shown in Table 1.
[0057] [Table 1]
[0058] (Evaluation Results) When comparing Example 1, Example 2 and Comparative Example 1, Example 3, Example 4 and Comparative Example 2, Example 5, and Example 6 and Comparative Example 3, the particle size of each of the Examples is almost the same as that of the Comparative Examples. However, by changing the polyol solvent to a low molecular weight one during the reduction, the carbon content and the mass reduction rate when heated from room temperature to 700°C in a He inert gas atmosphere are reduced, and the reduction in the intensity peak area of the mass spectrum also shows that the amount of gas generated is reduced.
[0059] From the examples and comparative examples, it is confirmed that the copper powder manufacturing method according to this embodiment can easily suppress (control) the amount of gas generated during firing of the resulting copper powder in a polyol method in which copper oxide powder is reduced in a polyol solvent to obtain copper powder.
[0060] The technical scope of the present invention is not limited to the aspects described in the above-mentioned embodiments. One or more of the requirements described in the above-mentioned embodiments may be omitted. The requirements described in the above-mentioned embodiments may be combined as appropriate. In addition, to the extent permitted by law, the disclosures of all documents cited in the above-mentioned embodiments are incorporated by reference and made part of the description in this text.
Claims
1. A method for producing copper powder by reducing copper oxide powder in a polyol solvent, comprising the steps of: generating copper nuclei from the copper oxide powder using a first polyol solvent; A step of growing the copper nuclei by using a second polyol solvent having an average molecular weight smaller than that of the first polyol solvent; A method for producing copper powder comprising the steps of:
2. The method for producing copper powder according to claim 1 , wherein the average molecular weight of the second polyol solvent is smaller than the average molecular weight of the first polyol solvent by 10% or more.
3. 3. The method for producing copper powder according to claim 1, wherein the second polyol solvent is prepared by mixing a polyol with the first polyol solvent.
4. The method for producing copper powder according to any one of claims 1 to 3, wherein the copper oxide powder is at least one selected from the group consisting of copper oxide and cuprous oxide.
5. The method for producing copper powder according to any one of claims 1 to 4, wherein the moisture content of the copper oxide powder is 10 mass% or less.
6. The method for producing copper powder according to any one of claims 1 to 5, wherein the step of generating copper nuclei is carried out up to a stage where a ratio of the copper nuclei in the cuprous oxide powder containing the copper nuclei becomes 0.1 to 0.5 in terms of molar fraction with respect to the total amount of the cuprous oxide powder containing the copper nuclei.
Citation Information
Patent Citations
Method of reducing metal compound with polyol and powdery metal manufactured thereby
JP1984173206A
Production of pulverous spherical copper powder
JP1987063604A
Manufacture of copper fine powder
JP1990034708A
Production of copper monodisperse particle
JP1993222413A
Method for manufacturing copper particulate and copper particulate dispersion liquid
JP2005097677A