Manufacturing method for steel plate with excellent fatigue crack propagation resistance

A simplified manufacturing process for steel materials with tailored chemical compositions and heat treatments forms tempered bainite or martensite structures and precipitates, significantly enhancing fatigue crack resistance in welded structures.

JP7552545B2Active Publication Date: 2024-09-18JFE STEEL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021158978
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-29
Publication Date
2024-09-18
Estimated Expiration
2041-09-29

AI Technical Summary

Technical Problem

Existing manufacturing methods for high-strength steel materials with fatigue crack propagation resistance are complex and inefficient, lacking a straightforward approach to enhance this critical property in welded structures.

Method used

A method involving specific chemical compositions and heat treatment processes, including heating to 1000-1300°C, rolling at 900°C or higher with a 50% cumulative reduction, quenching at 5°C/s or more, and tempering at 100-450°C for 10 seconds or more, to create steel materials with tempered bainite or martensite structures and precipitates, enhancing fatigue crack resistance.

Benefits of technology

The method simplifies the production of steel materials with improved fatigue crack propagation resistance, achieving a fatigue crack propagation velocity of less than 4.26×10^-8 m/cycle under a stress intensity factor range of 20 MPa√m, while maintaining mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552545000007
    Figure 0007552545000007
  • Figure 0007552545000006
    Figure 0007552545000006
  • Figure 0007552545000002
    Figure 0007552545000002
Patent Text Reader

Abstract

To provide a manufacturing method for easily manufacturing a steel material having excellent fatigue crack propagation resistance without complicated heat treatment.SOLUTION: There is provided a method for manufacturing a steel material in which a steel raw material having a chemical composition comprising, by mass%, 0.02 to 0.40% of C, 0.010 to 0.500% of Si, 0.05 to 2.00% of Mn, 0.050% or less of P, 0.050% or less of S, 0.100% or less of Al, 0.1000% or less of N and the balance Fe with inevitable impurities is heated to 1000 to 1300°C, after rolling at 900°C or more at a cumulative rolling reduction ratio of 50% or more, quenching treatment is applied and further tempering treatment is applied. A metallic structure of the steel material is any one of structures of a tempered bainite structure, a tempered martensite structure and a mixed structure of a tempered bainite structure and a tempered martensite structure or a ferrite structure having an area ratio of 50% or less is present in these metallic structures.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a steel material having excellent fatigue crack propagation resistance, more specifically, to a method for manufacturing a steel material that is used in various welded structures such as ships, marine structures, bridges, construction machinery, buildings, and tanks, and that has improved fatigue crack propagation resistance even when subjected to repeated loads. [Background technology]

[0002] In recent years, high-strength steel materials have been increasingly used in ships, marine structures, bridges, construction machinery, buildings, tanks, and other structures for the purposes of streamlining design, reducing steel weight, thinning, and reducing welding labor. In addition, these steel materials are required to have excellent fatigue resistance properties to ensure not only toughness and ductility but also weldability and structural safety.

[0003] In welded structures, fatigue failure often occurs when a fatigue crack initiates at the weld toe and propagates through the steel material, resulting in failure. This is believed to be due to the fact that the weld toe is prone to become a stress concentration area due to its shape, and also due to the occurrence of tensile residual stress after welding.

[0004] For this reason, widely known means for suppressing the generation of cracks from the weld toes include techniques for improving the shape by applying additional welding to reduce stress concentration, and techniques for introducing compressive residual stress by peening or the like.

[0005] However, it is nearly impossible to perform such treatment on an industrial scale on the numerous weld toes, and it is also difficult to say that it is realistic in terms of cost. Therefore, based on the recognition that it is important to extend the fatigue life by reducing the subsequent propagation speed of fatigue cracks in the steel material even if they are initiated, there is a strong demand from the industrial sector to improve the fatigue crack propagation properties of the steel material itself.

[0006] Here, Patent Document 1 describes a steel that has a chemical composition of C: 0.05 to 0.30%, Si: 0.03 to 0.35%, Cr: 0.05 to 2.0%, P: 0.03% or less, S: 0.003% or less, Al: 0.1% or less, with the balance being Fe and unavoidable impurities, which is hot-rolled, reheated and quenched, then reheated to a two-phase region temperature range of Ac1 transformation point + 10°C to 790°C, quenched at an average cooling rate of 5 to 60°C / s, and tempered by holding at 400 to 650°C for 10 minutes or more; the metal structure is a mixed structure of a ferrite phase with a Vickers hardness of 85 to 130 and a tempered martensite phase with a Vickers hardness of 340 to 440 with an area fraction of 15 to 85%; and the absolute value of the surface residual stress is 150 N / mm 2 The following manufacturing method for steel material having excellent fatigue crack propagation resistance has been disclosed.

[0007] Patent Document 2 describes a steel sheet containing 0.04-0.3% C, 0.01-2% Si, 0.1-3% Mn, 0.001-0.1% Al, 0.001-0.01% N, 0.02% or less P, 0.01% or less S, with the balance being iron and unavoidable impurities, and having a two-phase structure consisting of a soft phase and a hard second phase surrounding the soft phase in a mesh-like shape, and the soft phase and the hard second phase are: (1) the soft phase is ferrite, tempered bainite, tempered martensite The present invention discloses a thick steel material having excellent fatigue crack propagation resistance that satisfies all of the following conditions: (1) the hard second phase is composed of one or more of bainite, martensite, tempered bainite, and tempered martensite, and has an average Vickers hardness of 150 or less; (2) the hard second phase is composed of one or more of bainite, martensite, tempered bainite, and tempered martensite, and has an average Vickers hardness of 250 or more; and (3) the grain boundary occupancy rate of the hard second phase, as expressed by a specific formula, is 0.5 or less.

[0008] Patent Document 3 discloses a steel material having a steel composition, by mass%, of C: 0.05 to 0.30%, Si: 0.03 to 0.35%, Cr: 0.05 to 2.0%, P: 0.03% or less, S: 0.003% or less, Al: 0.1% or less, with the balance being Fe and unavoidable impurities, and having a metal structure in both the thickness direction and length direction of the plate of 80% or more of the plate thickness direction and plate length direction consisting of a mixed structure of a ferrite phase having a Vickers hardness of 130 or less and an aspect ratio of 2.5 or less, and a tempered martensite phase having an area fraction of 15 to 85% and a Vickers hardness of 340 or more and an aspect ratio of 2.5 or less, and having small material anisotropy and excellent fatigue crack propagation resistance.

[0009] Patent Document 4 discloses a steel sheet containing, by mass%, 0.03-0.30% C, 0.01-0.5% Si, 0.3-2.0% Mn, 0.001-0.1% sol. Al, with the remainder being Fe and unavoidable impurities, the structure of which is composed of a hard portion and a soft portion, and the proportions of the structure of these two portions and the average hardness in Vickers hardness satisfy a specific formula.

[0010] Furthermore, Patent Document 5 discloses a thick steel plate having excellent fatigue crack propagation properties and toughness, which is made of a steel containing, by mass%, 0.02-0.16% C, 0.05-0.5% Si, 0.005-0.060% Al, and one or more selected from 0.1-2.5% Mn, 0.1-2.0% Cu, and 0.1-6.0% Ni such that the value of 2Mn+Cu+Ni is 3.5-6.0%, with the remainder being Fe and unavoidable impurities, and which contains 5-20% by volume of retained austenite having an average diameter of 0.1-0.5 μm. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] Patent No. 4924047 [Patent Document 2] Patent No. 3785392 [Patent Document 3] Patent No. 4998708 [Patent Document 4] JP 2002-121640 A [Patent Document 5] Patent No. 4497009 Summary of the Invention [Problem to be solved by the invention]

[0012] However, the manufacturing techniques disclosed in the above Patent Documents 1 to 5 have the following problems.

[0013] The manufacturing method described in Patent Document 1 involves hot rolling, reheating and quenching, reheating to a two-phase temperature range of Ac1 transformation point +10°C to 790°C, quenching at an average cooling rate of 5 to 60°C / s, and then holding at 400 to 650°C for 10 minutes or more for tempering, but this manufacturing method is complicated.

[0014] Patent Document 2 is characterized in that a steel slab before hot rolling is subjected to a diffusion heat treatment at a heating temperature of 1200 to 1350°C for a holding time in that temperature range of 2 to 100 hours, and then hot rolling is performed at a heating temperature of Ac3 transformation point to 1250°C, and after rolling, the steel slab is acceleratedly cooled at a rate of 5 to 100°C / s from the Ar3 transformation point or higher to 400°C or lower, and further a two-phase region heat treatment is performed at a heating temperature of (Ac1 transformation point + 30°C) to (Ac3 transformation point - 10°C) and accelerated cooling at a rate of 5 to 100°C / s to 400°C or lower. However, the manufacturing methods such as the diffusion heat treatment and the two-phase region heat treatment are complicated.

[0015] Patent Document 3 is characterized in that the steel is subjected to solution heat treatment at 1200 to 1300°C for 25 to 60 hours, followed by air cooling, reheating to 1000 to 1200°C, hot rolling to a rolling end temperature of the Ar3 transformation point or higher, air cooling, reheating and holding at the Ac3 transformation point or higher, air cooling, and further reheating to a two-phase region temperature of Ac1 transformation point +10°C to Ac3 transformation point -10°C, followed by quenching at an average cooling rate of 5°C / s or more, and tempering at 400°C to 650°C. However, the manufacturing methods such as solution heat treatment and two-phase region heat treatment are complicated.

[0016] Patent Document 4 proposes the relational expression fA·HA-fB·HB≧-3500, where fA and fB are the percentages of the hard and soft parts in the structure, respectively, and HA and HB are the average Vickers hardness values ​​of the hard and soft parts, respectively. However, there is no linear relationship between fA·HA-fB·HB and the fatigue crack propagation rate, and it is unclear as an indicator.

[0017] Furthermore, Patent Document 5 is characterized in that after hot rolling, the steel is directly quenched or reheated and quenched, and then subjected to a two-phase region heat treatment in which the steel is heated to a temperature of 650°C or higher and lower than the Ac3 point and then cooled. However, the manufacturing method such as the two-phase region heat treatment is complicated.

[0018] Therefore, the present invention aims to solve the above-mentioned problems of the conventional technology and to provide a manufacturing method for easily obtaining a steel material having excellent fatigue crack propagation resistance without complicated heat treatment. Here, "steel material" includes steel plate, steel bar, steel strip, etc., but hereinafter, the explanation will be mainly on "steel plate". [Means for solving the problem]

[0019] The present inventors conducted the following experiments and carried out extensive investigations in order to solve the above problems.

[0020] [Fatigue crack propagation rate] Three types of test steels (A, B, and C) were used in the experiment. Their chemical compositions are shown in Table 1.

[0021] [Table 1]

[0022] The steel A was made by heating an ingot with the composition 0.13%C-0.26%Si-1.34%Mn-0.007%P-0.005%S-0.01%Ni-0.07%Cr-0.014%Ti-0.043%Al-0.0038%N to 1200℃, rolling it to a final thickness of 25mm at 900℃ or higher with a cumulative reduction of 80%, and then rapidly cooling it from 900℃ to 20℃ at 70℃ / s at a finishing temperature of 940℃. The steel was then tempered at 200℃ for 3600s. The relationship between the stress intensity factor range [ΔK] and the fatigue crack propagation rate [da / dN] was investigated using a CT test specimen with a thickness reduced to 12mm on both sides. Test steel B is a soft phase / hard phase dispersion steel (0.15%C-0.25%Si-1.51%Mn-0.009%P-0.005%S-0.07%Cr-0.038%Al-0.0025%N) made by heating an ingot of steel from 950°C to 1250°C, rolling it at a cumulative reduction rate of 50% or more at Ar3 or higher, starting accelerated cooling at a cooling rate of 10°C / s to 30°C / s from the temperature range of Ar3-60°C to 730°C or higher, and then cooling it to 650°C or lower and 500°C or higher. The steel used was a conventional steel (steel material made by heating a steel ingot containing 0.13%C-0.33%Si-1.45%Mn-0.009%P-0.008%S-0.05%Cr-0.012Ti-0.048%Al-0.0039%N to between 950°C and 1250°C, rolling it to a cumulative reduction rate of 50% or more at 900°C or higher, starting accelerated cooling from the temperature range from Ar3 point to Ar3 point - 100°C, and then cooling to between 700°C and 500°C).

[0023] The results are shown in Figure 1. In Figure 1, the squares (shown as "white frame with black fill" in the figure) represent data for test steel A, the triangles represent data for test steel B, and the circles represent data for test steel C. The solid line in the figure represents the level of fatigue crack propagation rate [da / dN] versus the stress intensity factor range [ΔK] for a typical conventional steel such as test steel C, where ΔK = 15 MPa m 1 / 2 3.50×10 -8 m / cycle and ΔK=25MPa m 1 / 2 When -7 The dotted line below it is half the fatigue crack propagation rate level of test steel C, ΔK = 15 MPa m1 / 2 When -8 m / cycle and ΔK=25MPa m 1 / 2 When -8 The straight line connecting the fatigue crack propagation rates of steel C and steel B is 1 / 5 of the fatigue crack propagation rate of steel C, and ΔK=15MPa m 1 / 2 When 7.00×10 -9 m / cycle and ΔK=25MPa m 1 / 2 3.40×10 -8 The results of this experiment show that sample B has a fatigue crack propagation rate level that is about half that of sample C, while sample A has a fatigue crack propagation rate level that is about one-fifth that of sample C, demonstrating that sample B has the best fatigue crack propagation resistance.

[0024] Next, a thin film sample was prepared from half the thickness of the steel plate of the above test steel A, and the metal structure was observed using a transmission electron microscope (TEM). In addition, carbides, nitrides, and carbonitrides were identified using an attached energy dispersive X-ray spectrometer (EDX) analysis. An example of the results is shown in Figure 2. Figure 2 shows a sample of one field of view (3.8 μm 2 , 10,000x), 13 precipitates consisting of carbides were observed. Similar observations were made in 10 fields of view with field intervals of 50 μm, and one or more precipitates consisting of carbides, nitrides, or carbonitrides were confirmed in 7 of the fields of view (equivalent to 70% of the 10 fields of view).

[0025] For the observation of the metal structure, a test piece taken from the center of the plate thickness (at 1 / 2 the plate thickness) of the steel material (steel plate) was polished and corroded (nital etched), and the structure was observed with a scanning electron microscope (SEM) (magnification: 500 times), and the metal structure was evaluated by taking an image and analyzing the image. As a result, the metal structure observed in the above sample steel A was a tempered bainite structure. Also, the above sample steel B had a structure in which aggregated pearlite and aggregated bainite were formed in a ferrite matrix. Furthermore, the above sample steel C had a structure in which band-shaped pearlite was formed in a ferrite matrix.

[0026] From the above experimental results, it was discovered that fatigue crack propagation characteristics can be significantly improved by using a steel material having a specific composition, whose metal structure is a tempered bainite structure, and further, in which one or more types of precipitates of carbide, nitride, and carbonitride are present.

[0027] Similarly, a decrease in the fatigue crack propagation rate was observed in steel materials having a tempered martensite structure or a mixed structure of tempered bainite and tempered martensite structures, and even if ferrite structure is present within these structures, the ferrite structure accounts for 50% or less in area ratio, and further containing one or more types of carbide, nitride, and carbonitride precipitates.

[0028] The present invention was completed based on these findings and through further investigation, and the gist of the present invention is as follows. [1] A method for producing a steel material having excellent fatigue crack propagation resistance, the method comprising heating a steel material having a chemical composition, by mass%, containing C: 0.02-0.40%, Si: 0.010-0.500%, Mn: 0.05-2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.1000% or less, with the balance being Fe and unavoidable impurities, to 1000-1300°C, rolling the steel material at 900°C or higher with a cumulative reduction rate of 50% or more, subjecting the steel material to a quenching treatment, and further subjecting the steel material to a tempering treatment. [2] A method for producing a steel material having excellent fatigue crack propagation resistance in [1], further comprising, in addition to the chemical composition of the steel material, one or more elements selected from, by mass%, Cu: 0.01-2.00%, Ni: 0.01-5.00%, Cr: 0.01-3.00%, Mo: 0.01-1.00%, Nb: 0.001-0.100%, V: 0.001-0.100%, Ti: 0.001-0.100%, B: 0.0001-0.0100%, and REM: 0.001-0.100%. [3] A method for producing a steel material having excellent fatigue crack propagation resistance according to [1] or [2], characterized in that the quenching treatment is performed by cooling from the Ar3 point or higher to 100°C or lower at a cooling rate of 5°C / s or more. [4] A method for producing a steel material having excellent fatigue crack propagation resistance according to any one of [1] to [3], characterized in that the tempering treatment is carried out at a heating temperature of 100 to 450°C for a heating time of 10 seconds or more. [5] In any one of [1] to [4], the steel material has a metal structure selected from the group consisting of a tempered bainite structure, a tempered martensite structure, and a mixed structure of a tempered bainite structure and a tempered martensite structure, and further has one or more precipitates of carbides, nitrides, and carbonitrides. A method for producing a steel material having excellent fatigue crack propagation resistance. [6] A method for producing a steel material having excellent fatigue crack propagation resistance according to [5], characterized in that each of the metal structures and a ferrite structure with an area ratio of 50% or less are present. [7] The method for producing a steel material having excellent fatigue crack propagation resistance according to any one of [1] to [6], characterized in that the steel material has a plate thickness of 5 to 100 mm. [8] In any one of [1] to [7], the number of the precipitates is 1 to 100 precipitates / 3.8 μm at the center of the plate thickness of the steel material. 2 A method for producing a steel material having excellent fatigue crack propagation resistance, characterized in that [9] In any one of [1] to [8], the stress intensity factor range [ΔK] in a fatigue crack propagation test of the steel material is 20 MPa m 1 / 2 When the fatigue crack propagation rate [da / dN] is 4.26×10 -8 The present invention relates to a method for producing a steel material having excellent fatigue crack propagation resistance, characterized in that the fatigue crack propagation resistance is less than m / cycle. Effect of the Invention

[0029] According to the present invention, a steel material having excellent fatigue crack propagation resistance can be produced by a simple production method, and this has a significant industrial effect. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a correlation diagram showing the results of fatigue crack propagation resistance tests of the steel material of the present invention and conventional steel materials. [Diagram 2] 1 is a photograph taken in observation of the metal structure of a steel material according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Hereinafter, an embodiment of the present invention will be described in detail, first with respect to a steel material obtained by the manufacturing method of the present invention.

[0032] [Basic chemical composition of steel] Next, the basic chemical composition of the steel material according to the present invention will be described. Note that hereinafter, "%" in the chemical composition means "mass %".

[0033] [C:0.02~0.40%] C must be added in an amount of 0.02% or more to ensure strength. However, adding 0.40% or more impairs weldability. Therefore, the C content is limited to the range of 0.02 to 0.40%. The C content is preferably 0.02 to 0.35%. More preferably, the C content is 0.02 to 0.33%. Further preferably, the C content is 0.02 to 0.30%.

[0034] [Si:0.010~0.500%] Silicon is effective as a deoxidizer and at least 0.010% is necessary to increase strength, but if it is added in excess of 0.500%, it deteriorates weldability and toughness. Therefore, the content is limited to the range of 0.010 to 0.500%. The content is preferably 0.050 to 0.450%. The content is more preferably 0.050 to 0.430%. The content is further preferably 0.050 to 0.400%.

[0035] [Mn: 0.05~2.00%] Mn is necessary at 0.05% or more from the viewpoint of not only increasing strength by increasing hardenability at low cost but also improving toughness, but if it exceeds 2.00%, it leads to deterioration of weldability. Therefore, the content is limited to the range of 0.05 to 2.00%. It is preferably 0.05 to 1.90%. It is more preferably 0.05 to 1.85%. It is further preferably 0.05 to 1.80%.

[0036] [P:0.050% or less] P is an impurity that deteriorates toughness, so the lower the content, the better. In view of production costs, the content is limited to a range of 0.050% or less. It is preferably 0.040% or less. It is more preferably 0.030% or less. It is further preferably 0.020% or less.

[0037] [S:0.050% or less] S is an impurity that deteriorates toughness, so the lower the content, the better. In view of production costs, the content is limited to a range of 0.050% or less. Preferably, it is 0.040% or less. More preferably, it is 0.030% or less. Even more preferably, it is 0.020% or less.

[0038] [Al:0.100% or less] Al acts as a deoxidizer and is most commonly used in the molten steel deoxidation process for high tensile steel. It also fixes N in the steel as AlN, contributing to improving the toughness of the base material. On the other hand, adding more than 0.100% of Al reduces the toughness of the base material and also mixes with the weld metal during welding, degrading the toughness. For this reason, Al is limited to 0.100% or less. It is preferably 0.080% or less. It is more preferably 0.070% or less. It is even more preferably 0.060% or less.

[0039] [N:0.1000% or less] N is undesirable because it adversely affects ductility and toughness in a solid solution state, but it is effective in improving mechanical properties if it is a small amount because it effectively works to refine austenite grains and strengthen precipitation by combining with V, Al, and Ti. However, excessive content of N increases the amount of solid solution N, which may adversely affect ductility and toughness, so N is limited to a range of 0.1000% or less. It is preferably 0.0900% or less. It is more preferably 0.0800% or less. It is even more preferably 0.0700% or less.

[0040] [Optional chemical composition of steel] The above-mentioned chemical composition is the basic chemical composition of the steel material of the present invention. In addition to this basic chemical composition, the present invention may further contain, as an optional chemical composition, one or more selected from Cu: 0.01-2.00%, Ni: 0.01-5.00%, Cr: 0.01-3.00%, Mo: 0.01-1.00%, Nb: 0.001-0.100%, V: 0.001-0.100%, Ti: 0.001-0.100%, B: 0.0001-0.0100%, and REM: 0.001-0.100%, for the purpose of adjusting strength, toughness, weldability, etc., and imparting weather resistance, etc., as necessary.

[0041] [Cu: 0.01-2.00%] Cu has the effect of increasing strength through solid solution and improving weather resistance. For this reason, the lower limit is preferably set to 0.01%. However, if the content exceeds 2.00%, it impairs weldability and makes the steel more susceptible to defects during production. Therefore, when Cu is contained, it is preferably set to 0.01 to 2.00%. More preferably, it is 0.01 to 1.50%. Even more preferably, It is 0.01 to 1.00%.

[0042] [Ni: 0.01~5.00%] Ni improves low-temperature toughness and is effective in improving weather resistance and hot brittleness that occurs when Cu is added. For this reason, the lower limit is preferably set to 0.01%. However, if the content exceeds 5.00%, it impairs weldability and leads to increased costs. Therefore, when Ni is contained, it is preferably set to 0.01 to 5.00%. More preferably, it is 0.01 to 4.00%. Even more preferably, it is 0.01 to 3.00%.

[0043] [Cr:0.01~3.00%] Cr improves weather resistance and strength. For this reason, the lower limit of its addition is preferably set at 0.01%. However, if its content exceeds 3.00%, it impairs weldability and toughness. Therefore, when Cr is contained, its content is preferably 0.01 to 3.00%. More preferably, it is 0.01 to 2.50%. Further preferably, it is 0.01 to 2.00%.

[0044] [Mo: 0.01-1.00%] Mo may be contained in an amount of 0.01% or more in order to increase strength. However, if the content exceeds 1.00%, deterioration of weldability and toughness occurs. Therefore, when Mo is contained, it is preferably 0.01 to 1.00%, more preferably 0.01 to 0.90%, and even more preferably 0.01 to 0.80%.

[0045] [Nb: 0.001~0.100%] Nb suppresses austenite recrystallization during rolling to refine the grains, and at the same time, has the effect of increasing strength through precipitation, so it may be contained in an amount of 0.001% or more. However, if it is contained in an amount exceeding 0.100%, toughness deteriorates. Therefore, if it is contained, it is preferably 0.001 to 0.100%, more preferably 0.001 to 0.090%, and even more preferably 0.001 to 0.080%.

[0046] [V:0.001~0.100%] Like Nb, V also has the function of increasing strength through precipitation, so it may be contained at 0.001% or more. However, if it is contained in excess of 0.100%, it will lead to a decrease in weldability and toughness. Therefore, if V is contained, it is preferably 0.001 to 0.100%, more preferably 0.001 to 0.090%, and even more preferably 0.001 to 0.080%.

[0047] [Ti: 0.001~0.100%] Ti may be contained in an amount of 0.001% or more in order to increase strength and improve weld toughness. However, if the content exceeds 0.100%, the cost tends to increase. Therefore, when Ti is contained, it is preferably 0.001 to 0.100%, more preferably 0.001 to 0.090%, and even more preferably 0.001 to 0.080%.

[0048] [B:0.0001~0.0100%] B may be contained in an amount of 0.0001% or more in order to improve hardenability and contribute to an increase in strength. However, if it is contained in an amount exceeding 0.0100%, it impairs weldability. Therefore, if B is contained, it is preferably 0.0001 to 0.0100%, more preferably 0.0001 to 0.0090%, and even more preferably 0.0001 to 0.0080%.

[0049] [REM:0.001~0.100%] REM refers to rare earth elements such as Sc, Y, La, and Ce. When added in small amounts, 0.001% or more may be contained because it contributes to improving HAZ toughness. However, if it is contained in excess of 0.100%, it impairs weldability. Therefore, when REM is contained, it is preferable that the content is 0.001 to 0.100%. More preferably, it is 0.001 to 0.090%. Even more preferably, it is 0.001 to 0.080%.

[0050] [Remaining chemical composition] The remaining chemical composition other than the above-mentioned chemical composition is composed of Fe and inevitable impurities. Examples of the inevitable impurity elements include O (oxygen), Sn, Sb, As, Pb, Bi, Ca, Mg, etc., and a total of 0.10% or less is acceptable. In addition, as long as the above-mentioned basic chemical composition and optional chemical composition are satisfied, the inclusion of inevitable impurity elements other than these is not prevented, and such embodiments are also included in the technical scope of the present invention.

[0051] [Metal structure of steel] In the present invention, a steel material having the above-mentioned chemical composition is produced by a manufacturing method described below to obtain a steel material having excellent fatigue crack propagation resistance. It has been found that the metal structure of the central part of the plate thickness of the obtained steel material has the following metal structure depending on the heat treatment conditions such as tempering treatment, due to the difference in chemical composition and the change in cooling rate depending on the plate thickness of the steel material. The structure is any one of tempered bainite structure, tempered martensite structure, or mixed structure of tempered bainite structure and tempered martensite structure, and there are also cases where a ferrite structure with an area ratio of 50% or less is present in the structure of these metal structures. In other words, it has the following metal structure. (a) Tempered bainite structure (b) Tempered martensite structure (c) Mixed structure of tempered bainite and tempered martensite (d) Ferrite structure with an area ratio of 50% or less and tempered bainite structure (e) Ferrite structure with an area ratio of 50% or less and tempered martensite structure (f) A mixed structure of ferrite, tempered bainite, and tempered martensite with an area ratio of 50% or less As described above, these metal structures can be determined by observing the structure using a scanning electron microscope (SEM) (magnification: 500 times).

[0052] As described above, each of the above-mentioned structures can be obtained by adjusting the chemical composition, the cooling rate, the heat treatment conditions such as the tempering treatment, and the like.

[0053] Specifically, a high cooling rate (50°C / s or higher) tends to produce a martensite structure, while a low cooling rate (10°C / s or lower) tends to produce a bainite structure. If the cooling rate is even slower (5°C / s or lower), the structure will be a bainite structure, a martensite structure, or a matrix of bainite and martensite structures with ferrite mixed in. In other words, the above-mentioned structures (a) to (f) can be obtained by the above heat treatment.

[0054] [Precipitates in metal structure] In the above-mentioned metallographic observation by TEM, it was found that it is important that one or more of the precipitates of carbide, nitride, and carbonitride exist in the metallographic structure. Specifically, in the metallographic observation, the number of precipitates is 1 to 100 / 3.8μm at the center of the plate thickness of the steel material. 2 This results in a steel material with excellent fatigue crack propagation resistance. 2 The visual field is observed in 10 fields at 50 μm intervals, and the number of the above precipitates is 1 to 100 / 3.8 μm somewhere in each of the visual fields (at least in one visual field). 2 It is preferable that:

[0055] The above-mentioned precipitates are carbides, nitrides, or carbonitrides of Fe, Si, Mn, Al, etc. in the basic chemical composition of the steel material, and further carbides, nitrides, or carbonitrides of Cr, Mo, Nb, V, Ti, etc. in the optional chemical composition. These precipitates in the metal structure are scattered in the form of small and large particles, as in the example shown in Figure 2, and their size is 10 to 500 nm.

[0056] These precipitates were obtained by cutting a 1 mm thin piece from the center of the thickness of the steel material (steel plate), polishing the cut piece from both sides to reduce the thickness to 50 μm, punching it out with a disk punch to a diameter of 3 mm, and cutting the disk into a thin piece by electrolytic polishing. The disk was washed with methanol and dried on filter paper to prepare a TEM observation sample, which was then observed by TEM (observation field: 3.8 μm 2 The presence or absence of carbides can be confirmed by analyzing the specimen with an energy dispersive X-ray spectrometer (magnification: 10,000 times). Furthermore, the carbides, nitrides, and carbonitrides were identified by analysis with an attached energy dispersive X-ray spectrometer (EDX). Here, the above-mentioned EDX analysis method can be mentioned as a method for identifying carbides, nitrides, and carbonitrides. According to this method, peaks of Fe and C appear in carbides, peaks of Fe and N appear in nitrides, and peaks of Fe, C, and N appear in carbonitrides.

[0057] [Steel manufacturing method] The method for producing a steel material according to the present invention is characterized in that a steel material adjusted to have the above-mentioned composition is heated to 1000 to 1300°C, rolled at 900°C or higher with a cumulative reduction rate of 50% or more, quenched, and then tempered. Here, the temperature is the temperature at the center of the thickness of the steel material (steel plate). As a result, the structure at the center of the thickness of the steel material is cooled at a rate adjusted according to the thickness, and the above-mentioned metal structure and precipitates within the metal structure are obtained. In the case of a steel material having such a metal structure, it has been confirmed that the fatigue crack propagation resistance is improved as described below. Such an effect has been confirmed when the thickness of the steel material (steel plate) is in the range of 5 to 100 mm. Furthermore, each step in the method for producing a steel material according to the present invention will be described in detail.

[0058] [Heating temperature: 1000~1300℃] If the heating temperature is less than 1000°C, the subsequent rolling temperature cannot be ensured. Moreover, if the temperature exceeds 1300°C, the crystal grains of the steel become coarse, making it difficult to ensure toughness. Therefore, the heating temperature is specified to be 1000 to 1300°C. It is preferably 1000 to 1250°C, and more preferably 1000 to 1200°C. Moreover, the heating time is adjusted appropriately depending on the plate thickness of the steel material, but is preferably in the range of 1 hour to 24 hours, and more preferably 1 hour to 12 hours.

[0059] [Cumulative rolling reduction rate above 900℃: 50% or more] In order to refine the austenite grains by rolling and improve toughness, rolling is performed at 900°C or higher with a cumulative reduction of 50% or more. Preferably, it is 52% or more. More preferably, it is 55% or more. As long as the temperature is 900°C or higher, it may be in either the austenite recrystallized region or the austenite non-recrystallized region. However, since excessive reduction in the austenite non-recrystallized region causes anisotropy in the mechanical properties, it is desirable to set the cumulative reduction in the austenite non-recrystallized region to 25% or less.

[0060] [Finishing temperature] The finishing temperature is the final rolling temperature. This temperature is preferably 1000 to 850°C. If it is outside this range, it is not preferable because excessive ferrite structure is generated in the next step, quenching. More preferably, it is 1000 to 900°C.

[0061] [Hardening treatment] Quenching is a manufacturing condition for making the steel material into a bainite structure, a martensite structure, or a mixed structure thereof. The specific process involves cooling from the Ar3 point or higher to 100°C or lower at a cooling rate of 5°C / s or higher. If the cooling start temperature is lower than the Ar3 point, ferrite will be excessively generated, and the desired fatigue crack propagation rate will not be obtained. Therefore, the cooling start temperature is set to the Ar3 point or higher. If the cooling rate is lower than 5°C / s, ferrite will be excessively generated, and the desired fatigue crack propagation rate will not be obtained. Therefore, the cooling rate is set to 5°C / s or higher, preferably 6°C / s or higher. If the cooling stop temperature is higher than 100°C, the desired strength will not be obtained. Therefore, the cooling stop temperature is set to 100°C or lower, preferably 80°C or lower.

[0062] The above Ar3 point can be calculated using the following formula (1) based on the composition percentage of the steel material. Ar3=910-310×C-80×Mn-20×Cu-15×Cr-55×Ni-80×Mo... (1) If not contained, the value is set to 0.

[0063] As for the quenching method, in the case of laboratory experiments, it was performed by jet water cooling from the Ar3 point or higher. In the case of actual equipment scale, the desired metal (micro)structure can be obtained by cooling using jet water cooling or laminar cooling.

[0064] [Tempering treatment] By subjecting the metal structure produced by the above-mentioned quenching treatment to a tempering treatment at 100 to 450°C for 10 seconds or more, the bainite structure becomes a tempered bainite structure, the martensite structure becomes a tempered martensite structure, and the above-mentioned carbide, nitride or carbonitride precipitates appear.

[0065] Specifically, the tempering treatment involves heating the quenched steel material at a low temperature of 100 to 450°C for 10 seconds or more. The heating time is preferably 10 seconds or more, but if it exceeds 100 minutes, the manufacturing cost becomes too high, so the heating time is preferably 10 seconds to 100 minutes. More preferably, it is 10 minutes to 60 minutes. If the heating temperature is not 100°C or more, carbides, nitrides, and carbonitrides will not precipitate, and if it exceeds 450°C, a decrease in strength will occur. Therefore, the heating temperature is preferably 100 to 450°C. More preferably, it is 150 to 450°C.

[0066] [Fatigue crack propagation resistance] The fatigue crack propagation resistance of steel materials is evaluated by determining the stress intensity factor range [ΔK] and fatigue crack propagation rate [da / dN] through fatigue crack propagation tests conforming to the ASTM E647 standard. This stress intensity factor range [ΔK] is ΔK=Kmax-Kmin, and represents the difference between the maximum and minimum values ​​of the stress intensity factor. Furthermore, the fatigue crack propagation rate [da / dN] is the amount of fatigue crack growth [m / cycle] during one cycle of the stress waveform, and is particularly pronounced in the intermediate region of ΔK (approximately ΔK=10MPa m 1 / 2 Therefore, ΔK = approximately 70 MPa m 1 / 2 ) is called the Paris law, da / dN=CΔK m A linear relationship holds: (C and m are constants).

[0067] In the present invention, a steel material with excellent fatigue crack propagation resistance is one with a stress intensity factor range [ΔK] of 20 MPa m 1 / 2 When the fatigue crack propagation rate is 4.26×10 -8 m / cycle or less.

[0068] [Mechanical properties of steel] The target values ​​of the mechanical properties of the steel material of the present invention are a yield stress (YS) of 400 MPa or more in a tensile test, a tensile strength (TS) of 500 MPa or more, and an absorbed energy ( V E0) ≥ 27J, stress intensity factor range in fatigue crack propagation test [ΔK] is 20MPa m1 / 2 Fatigue crack propagation rate at [da / dN] ≦ 4.26 × 10 -8 [m / cycle]. EXAMPLES

[0069] 26 types of steel having steel compositions A to Z shown in Table 2 were prepared, and test pieces (plates No. 1 to 34) shown in Table 3 were processed under the manufacturing conditions shown in Table 3 (heating and rolling treatment, quenching treatment, and then tempering treatment at a low temperature of 100 to 450°C for 10 seconds or more).

[0070] [Table 2]

[0071] [Table 3]

[0072] A 1 mm thin section was cut from the center of the thickness of the steel material (steel plate) that had been treated as described above, and the cut section was polished from both sides to reduce the thickness to 50 μm, and then punched out to 3 mm diameter with a disk punch. The disk was thinned by electrolytic polishing, washed with methanol, and dried on filter paper to prepare a TEM observation sample. The TEM observation (field of view: 3.8 μm 2 A 10-field microscope was used for the analysis (magnification: 10,000x) at a pitch of 50 μm for 10 fields of view. Furthermore, carbides, nitrides and carbonitrides were identified by analysis using an attached energy dispersive X-ray spectrometer (EDX). The results of observing precipitates such as carbides are shown in Table 4. All of the test pieces that are examples of the present invention had one or more types of precipitates in their metal structures, but no precipitates were observed at all in test pieces / plates No. 24, 31, 32 and 34, which are comparative examples.

[0073] [Table 4]

[0074] Next, for the tensile test, ASTM-F (6φ×24GL) round bar test pieces were taken from the center of the plate thickness, perpendicular to the rolling direction, and used for the test. For the Charpy impact test, three full-size test pieces were taken from the center of the plate thickness, in the rolling direction, and used for the test at a test temperature of 0°C. For the fatigue crack propagation rate, a fatigue crack propagation test was performed on a CT test piece with a plate thickness of 12 mm on both sides, with an R ratio of 0.1, a sine wave, and 10 Hz. The YS [MPa], TS [MPa], V E0[J], ΔK=20MPa·m 1 / 2 The fatigue crack propagation rates [da / dN] [m / cycle] at these times are shown in Table 5. Microscopic observations were performed using a SEM (magnification: 500x) after nital etching at the 1 / 2 position of the plate thickness. For TEM observations, a thin film was taken from the 1 / 2 position of the plate thickness as described above, and observed and photographed (field of view: 3.8 μm 2 , magnification: 10,000x).

[0075] [Mechanical properties of steel] Tensile test specimens (parallel portion diameter 6 mmφ) and Charpy impact test specimens (V notch) were taken from the obtained test specimens in accordance with the provisions of JIS Z 2241 and 2242, and tensile tests and impact tests were carried out.

[0076] In the tensile test, if a yield point was observed, the upper yield point was taken as the YS of the test piece. If no yield point was observed, the 0.2% proof stress was taken as the YS of the test piece. The maximum tensile stress value on the stress-strain curve was taken as TS.

[0077] In addition, Charpy impact tests were performed on three specimens each, and the absorbed energy at test temperature: 0°C V E0 was calculated and the average value was used as the value for the test piece.

[0078] The results obtained are shown in Table 5.

[0079] [Table 5]

[0080] The test pieces Nos. 1 to 22 have the steel chemical composition specified in the present invention and are produced by the steel manufacturing method specified in the present invention. The YS is 400 MPa or more, the TS is 500 MPa or more, V E0 is 27 J or more, ΔK = 20 MPa m 1 / 2 The fatigue crack propagation rate [da / dN] at this time is 4.26×10 -8 The fatigue crack propagation rate was less than [m / cycle], and a steel plate with excellent fatigue crack propagation rate resistance was obtained. Furthermore, at this time, observation of the metal structure revealed the presence of one or more types of precipitates, as shown in Table 4. Furthermore, as shown in Table 3, the metal structure was either a tempered bainite structure, a tempered martensite structure, or a mixed structure of a tempered bainite structure and a tempered martensite structure, or a structure in which a ferrite structure was present in an area ratio of 50% or less within these metal structures.

[0081] However, in the case of steel plate No. 23, the C content exceeded the value specified in the present invention, and the Charpy impact test value was below 27 J. In the case of steel plate No. 24, the C, Si, and Mn contents were below the values ​​specified in the present invention, and therefore no precipitates such as carbides were observed in any of the 10 visual fields in the metallographic observation. As a result, the YS and TS were below the target values ​​of the present invention, the Charpy impact test value was below the target values ​​of the present invention, and ΔK = 20 MPa m 1 / 2 The fatigue crack propagation rate at -8 [m / cycle], and the fatigue crack propagation resistance was poor. In the case of steel plate No. 25, the P, S, Al, and N exceeded the values ​​specified in the present invention, and therefore the Charpy impact test value was below the target value of the present invention. In the case of steel plate No. 26, the Si and Mn exceeded the values ​​specified in the present invention, and therefore the Charpy impact test value was below the target value of the present invention. In the case of steel plate No. 27, the heating temperature exceeded the value specified in the present invention, and therefore the Charpy impact test value was below the target value of the present invention. In the case of steel plate No. 28, the heating temperature was below the value specified in the present invention, and therefore the reduction at 900°C or more was not sufficient. As a result, the Charpy impact test value was below the target value of the present invention. In the case of steel plate No. 29, the cumulative reduction rate at 900°C or more was below the value specified in the present invention, and therefore the Charpy impact test value was below the target value of the present invention, and ΔK=20MPa·m 1 / 2The fatigue crack propagation rate at -8 [m / cycle], and the fatigue crack propagation resistance was poor. In the case of steel plate No. 30, the cooling start temperature was below the Ar3 point, so the metal structure became a tempered bainite structure with ferrite structures exceeding 50% by area. As a result, the YS and TS were below the target values ​​of the present invention, and ΔK = 20 MPa m 1 / 2 The fatigue crack propagation rate at -8 [m / cycle], and the fatigue crack propagation resistance was poor. In the case of steel plate No. 31, the cooling rate was below the value specified in the present invention, so the metallographic structure was a pearlite structure with ferrite structures exceeding 50% by area ratio, the YS and TS were below the target values ​​of the present invention, and no precipitates such as carbides were observed in any of the 10 visual fields in the metallographic observation. As a result, ΔK=20MPa·m 1 / 2 The fatigue crack propagation rate at -8 [m / cycle], and thus had poor fatigue crack propagation resistance. In the case of steel plate No. 32, the cooling stop temperature exceeded the value specified in the present invention, and therefore the metallographic structure became a pearlite structure with ferrite structures exceeding 50% by area ratio, the YS and TS were below the target values ​​of the present invention, and no precipitates such as carbides were observed in any of the 10 visual fields in the metallographic observation. As a result, ΔK=20MPa·m 1 / 2 The fatigue crack propagation rate at -8 [m / cycle], and the fatigue crack propagation resistance was poor. The tempering temperature of steel plate No. 33 exceeded the specified value of the present invention, so the YS and TS were below the target values ​​of the present invention. As a result, ΔK = 20 MPa m 1 / 2 The fatigue crack propagation rate at -8 [m / cycle], and the fatigue crack propagation resistance was poor. The tempering temperature of steel plate No. 34 was below the specified value of the present invention, and no precipitates such as carbides were observed in any of the 10 visual fields in the metallographic observation. As a result, the Charpy impact test value was below the target value of the present invention, and ΔK = 20 MPa m 1 / 2 The fatigue crack propagation rate at -8 [m / cycle] and the fatigue crack propagation resistance was poor.

Claims

1. A steel material having a chemical composition containing, by mass%, C: 0.02 to 0.40%, Si: 0.010 to 0.500%, Mn: 0.05 to 2.00%, P: 0.050% or less, S: 0.050% or less, Al: 0.100% or less, N: 0.1000% or less, with the balance being Fe and unavoidable impurities, is heated to a temperature of 1000 to 1300°C at the center of the plate thickness, rolled to 900°C or more with a cumulative reduction rate of 50% or more, quenched, and further tempered to obtain a steel plate, The quenching treatment is a treatment of cooling from the Ar 3 point or higher to 100° C. or lower at a cooling rate of 5° C. / s or higher, and the tempering treatment is a treatment of heating at a temperature of 100 to 450° C. for a heating time of 10 seconds or longer. The steel sheet has a metal structure selected from the group consisting of a tempered bainite structure, a tempered martensite structure, and a mixed structure of a tempered bainite structure and a tempered martensite structure, and further has at least one type of precipitate of carbide, nitride, and carbonitride, each having a size of 10 nm or more, at 1 to 100 precipitates / 3.8 μm 2 in the center of the sheet thickness. A method for producing a steel plate having excellent fatigue crack propagation resistance, comprising the steps of:

2. 2. The method for producing a steel plate having excellent fatigue crack propagation resistance according to claim 1, further comprising, in addition to the chemical composition of the steel material, one or more selected from, by mass%, Cu: 0.01 to 2.00%, Ni: 0.01 to 5.00%, Cr: 0.01 to 3.00%, Mo: 0.01 to 1.00%, Nb: 0.001 to 0.100%, V: 0.001 to 0.100%, Ti: 0.001 to 0.100%, and REM: 0.001 to 0.100%.

3. 3. The method for producing a steel plate having excellent fatigue crack propagation resistance according to claim 1, wherein the metal structures and a ferrite structure are present in an area ratio of 50% or less.

4. 4. The method for producing a steel plate having excellent fatigue crack propagation resistance according to claim 1, wherein the steel plate has a thickness of 5 to 100 mm.

5. The steel plate is subjected to a fatigue crack propagation test with a stress intensity factor range [ΔK] of 20 MPa m 1/2 In this case, the fatigue crack propagation rate [da / dN] is 4.26×10 -8 5. The method for producing a steel plate having excellent fatigue crack propagation resistance according to claim 1, wherein the steel plate has a fatigue crack propagation rate of not more than m / cycle.

Citation Information

Patent Citations

  • JP1974024047A

  • JP1974098708A

  • Steel sheet having suppressing effect on fatigue crack propagation

    JP2002121640A

  • Method for manufacturing steel material having uniform strength in sheet thickness direction and superior fatigue-crack propagation resistance

    JP2005240177A

  • High-strength steel material superior in ductile-crack initiation resistance and fatigue-crack propagation resistance, and manufacturing method therefor