Method for producing fluoropolymer, aqueous dispersion and fluoropolymer composition

The method produces fluoropolymers in an aqueous medium without emulsifiers, addressing environmental concerns and achieving stable dispersion by using a specific polymer and water-soluble initiators to polymerize fluoromonomers.

JP7552585B2Active Publication Date: 2024-09-18AGC INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021509607
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-27
Filing Date
2020-03-26
Publication Date
2024-09-18
Estimated Expiration
2040-03-26

AI Technical Summary

Technical Problem

Existing methods for producing fluoropolymers using an aqueous medium require the use of emulsifiers, which can lead to environmental impact and necessitate their removal depending on the application.

Method used

A method for producing fluoropolymers without emulsifiers by polymerizing a specific polymer containing a compound represented by formula (1) in an aqueous medium, followed by polymerizing fluoromonomers such as tetrafluoroethylene, chlorotrifluoroethylene, or vinylidene fluoride, using a water-soluble polymerization initiator.

Benefits of technology

This approach allows for the production of fluoropolymers in an aqueous medium with low environmental impact, eliminating the need for emulsifiers and ensuring stable dispersion without the use of additional stabilizing agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552585000001
    Figure 0007552585000001
  • Figure 0007552585000002
    Figure 0007552585000002
Patent Text Reader

Abstract

Provided is a method for producing a fluorine-containing polymer in which an aqueous medium having a low environmental impact is used and in which no emulsifier is required. In the method for producing a fluorine-containing polymer, at least one fluorine-containing monomer selected from among tetrafluoroethylene, chlorotrifluoroethylene, and fluorinated vinylidene is polymerized within an aqueous medium in the presence of a first polymer including a unit based on a compound represented by formula (1) below. Formula (1): CXY=CR1-L-R2 (wherein each of X and Y independently represents a hydrogen atom, a halogen atom, or a methyl group). R1 represents a hydrogen atom, a halogen atom, or an alkyl group having 1-3 carbon atoms. L represents -CO-O-*, -O-CO-*, or -O-. * represents a position of bonding with R2. R2 represents a cyclic alkyl group, a monovalent aromatic hydrocarbon group, or a chain alkyl group having 1-6 carbon atoms. An ethereal oxygen atom may be present between the carbon-carbon bonds of the chain alkyl group having 1-6 carbon atoms that is represented by R2, and the hydrogen atoms included in the cyclic alkyl group, the monovalent aromatic hydrocarbon group, and the chain alkyl group having 1-6 carbon atoms represented by R2 may be substituted with halogen atoms.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a fluoropolymer, an aqueous dispersion and a fluoropolymer composition. [Background technology]

[0002] Fluorine-containing polymers such as ethylene / tetrafluoroethylene copolymers and tetrafluoroethylene / perfluoroalkyl vinyl ether copolymers have been used in various industrial fields due to their excellent heat resistance, chemical resistance, flame retardancy, weather resistance, etc. As a method for producing a fluorine-containing polymer, there is mentioned a method in which a fluorine-containing emulsifier is used to emulsion-polymerize a fluorine-containing monomer in an aqueous medium (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2007 / 046377 Summary of the Invention [Problem to be solved by the invention]

[0004] The method of Patent Document 1 has a small environmental impact because an aqueous medium is used. However, when a large amount of an emulsifier, which is an essential component, remains in the aqueous dispersion obtained by polymerization, it becomes necessary to remove the emulsifier depending on the application.

[0005] The present invention provides a method for producing a fluoropolymer which uses an aqueous medium which has a small environmental load and does not require an emulsifier. [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found that the above problems can be solved by the following configuration.

[0007] [1] A method for producing a fluorine-containing polymer, comprising polymerizing, in an aqueous medium, at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride in the presence of a first polymer containing a unit based on a compound represented by the following formula (1): CXY=CR 1 -LR 2 (1) Here, X and Y each independently represent a hydrogen atom, a halogen atom, or a methyl group. 1 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 3 carbon atoms. L represents -CO-O-*, -O-CO-*, or -O-. However, * is R 2 R represents the bond position. 2 represents a cyclic alkyl group, a monovalent aromatic hydrocarbon group, or a chain alkyl group having 1 to 6 carbon atoms. 2 may have an ether oxygen atom between the carbon-carbon bonds of the chain alkyl group having 1 to 6 carbon atoms; 2 The hydrogen atoms contained in the cyclic alkyl group, the monovalent aromatic hydrocarbon group and the chain alkyl group having 1 to 6 carbon atoms may be substituted with halogen atoms. [2] The method according to [1], wherein the first polymer is present in an amount of 0.0001 to 1.0 part by mass per 100 parts by mass of the aqueous medium. [3] The method according to [1] or [2], wherein the first polymer present in the aqueous medium is composed of particles having a volume-based cumulative 50% diameter of 10 to 1000 nm. [4] The method according to any one of [1] to [3], wherein the first polymer is a polymer obtained by polymerizing the compound represented by formula (1) using 0.1 to 5.0 mol of a water-soluble polymerization initiator per 1 mol of the compound represented by formula (1).

[0008] [5] A method for producing a fluorine-containing polymer, comprising polymerizing a compound represented by the following formula (1) in an aqueous medium to obtain an aqueous medium in which a first polymer is present, and then polymerizing at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride in the aqueous medium in which the first polymer is present to produce a fluorine-containing polymer: CXY=CR 1 -LR 2 (1) Here, X and Y each independently represent a hydrogen atom, a halogen atom, or a methyl group. 1 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 3 carbon atoms. L represents -CO-O-*, -O-CO-*, or -O-. However, * is R 2 R represents the bond position. 2 represents a cyclic alkyl group, a monovalent aromatic hydrocarbon group, or a chain alkyl group having 1 to 6 carbon atoms. 2 may have an ether oxygen atom between the carbon-carbon bonds of the chain alkyl group having 1 to 6 carbon atoms; 2 The hydrogen atoms contained in the cyclic alkyl group, the monovalent aromatic hydrocarbon group and the chain alkyl group having 1 to 6 carbon atoms may be substituted with halogen atoms. [6] The production method described in [5], wherein the aqueous medium in which the first polymer is present is an aqueous medium that has been used in the production of the first polymer and has resulted in the first polymer being present in the aqueous medium. [7] The method according to [5] or [6], wherein the compound represented by formula (1) is polymerized using 0.1 to 5.0 mol of a water-soluble polymerization initiator per 1 mol of the compound represented by formula (1). [8] The method according to any one of [5] to [7], wherein the amount of the first polymer present in the polymerization of the fluorine-containing monomer is 0.0001 to 1.0 parts by mass per 100 parts by mass of the aqueous medium.

[0009] [9] An aqueous fluoropolymer dispersion comprising an aqueous medium, particles having a volume-based cumulative 50% diameter of 20 to 3,000 nm comprising a fluoropolymer having units based on at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride, and a first polymer comprising units based on a compound represented by the following formula (1), the first polymer being contained as particles in the aqueous medium or contained in particles comprising the fluoropolymer: CXY=CR 1 -LR 2 (1) Here, X and Y each independently represent a hydrogen atom, a halogen atom, or a methyl group. 1 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 3 carbon atoms. L represents -CO-O-*, -O-CO-*, or -O-. However, * is R 2 R represents the bond position. 2 represents a cyclic alkyl group, a monovalent aromatic hydrocarbon group, or a chain alkyl group having 1 to 6 carbon atoms. 2 may have an ether oxygen atom between the carbon-carbon bonds of the chain alkyl group having 1 to 6 carbon atoms; 2 The hydrogen atoms contained in the cyclic alkyl group, the monovalent aromatic hydrocarbon group and the chain alkyl group having 1 to 6 carbon atoms may be substituted with halogen atoms.

[10] The fluoropolymer aqueous dispersion according to [9], wherein the particles containing the fluoropolymer are contained in an amount of 1.0 to 50.0 parts by mass per 100 parts by mass of the aqueous medium.

[11] The fluoropolymer aqueous dispersion according to [9] or

[10] , wherein the first polymer particles are contained in an amount of 0.0001 to 1.0 part by mass per 100 parts by mass of the aqueous medium.

[12] The fluoropolymer aqueous dispersion according to any one of [9] to

[11] , wherein the content of particles of the first polymer is 0.001 to 5.00 parts by mass per 100 parts by mass of the particles containing the fluoropolymer.

[13] The aqueous fluoropolymer dispersion according to any one of [9] to

[12] , wherein the particles of the first polymer have a volume-based cumulative 50% diameter of 10 to 1,000 nm.

[0010]

[14] A fluorine-containing polymer comprising a first polymer containing a unit based on a compound represented by the following formula (1) and a unit based on at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride, and having an infrared absorption spectrum of 1500 to 1800 cm -1 A polymer composition having a peak derived from a unit based on a compound represented by the following formula (1): CXY=CR 1 -LR 2 (1) Here, X and Y each independently represent a hydrogen atom, a halogen atom, or a methyl group. 1 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 3 carbon atoms. L represents -CO-O-*, -O-CO-*, or -O-. However, * is R 2 R represents the bond position. 2 represents a cyclic alkyl group, a monovalent aromatic hydrocarbon group, or a chain alkyl group having 1 to 6 carbon atoms. 2 may have an ether oxygen atom between the carbon-carbon bonds of the chain alkyl group having 1 to 6 carbon atoms; 2 The hydrogen atoms contained in the cyclic alkyl group, the monovalent aromatic hydrocarbon group and the chain alkyl group having 1 to 6 carbon atoms may be substituted with halogen atoms.

[15] The polymer composition according to

[14] , wherein the content of the first polymer is 0.001 to 5.00 parts by mass based on 100 parts by mass of the fluoropolymer. Effect of the Invention

[0011] According to the present invention, there can be provided a method for producing a fluoropolymer which uses an aqueous medium which has a small environmental load and does not require an emulsifier. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The terms used in the present invention have the following meanings. A "unit" is a general term for an atomic group derived from one monomer molecule that is formed directly by polymerization of the monomer. The content (mass%) of each unit relative to the total units contained in the polymer is determined by analyzing the polymer using solid-state nuclear magnetic resonance spectroscopy (NMR), but can be estimated from the amount of each monomer charged. Usually, the content of each unit calculated from the amount of each monomer charged is approximately equal to the actual content of each unit. The "volume-based cumulative 50% diameter" is the particle diameter at the point on the cumulative curve where the cumulative volume is 50% when the particle size distribution is measured by a laser diffraction / scattering method and the total volume of the particle group is set to 100%. Hereinafter, this is also referred to as "D50". The "peak of infrared absorption spectrum" was measured using an infrared spectrophotometer (manufactured by ThemoFisher SCIENTIFIC) for a 100 μm thick film obtained by press-molding a composition containing a fluoropolymer.

[0013] The process for producing a fluorine-containing polymer of the present invention is a process for polymerizing at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride (hereinafter also referred to as "specific fluorine-containing monomer") in an aqueous medium in the presence of a first polymer (hereinafter also referred to as "specific polymer") containing units based on a compound represented by the following formula (1) (hereinafter also referred to as "compound (1)"). The method for producing the fluorine-containing polymer of the present invention may use a specific polymer obtained by separate polymerization, or may involve polymerizing a specific polymer in an aqueous medium and subsequently polymerizing a specific fluorine-containing monomer in the same polymerization system. Subsequent polymerization in the same polymerization system means that an aqueous medium in which a specific polymer is present after being used for the production of the specific polymer is used, and a specific fluorine-containing monomer is polymerized in the aqueous medium in which the specific polymer is present. A commercially available product may be used as the specific polymer obtained by separate polymerization. The preferred method for producing the fluoropolymer of the present invention is to polymerize compound (1) in an aqueous medium to obtain an aqueous medium in which a specific polymer is present, and then to polymerize a specific fluorine-containing monomer in the aqueous medium in which the specific polymer is present to produce a fluoropolymer. In this two-step production method, the first step of obtaining an aqueous medium in which the specific polymer is present is hereinafter referred to as "Step 1", and the second step of producing a fluoropolymer is hereinafter referred to as "Step 2". The polymerization of the compound (1) in step 1 and the polymerization of the specific fluorine-containing monomer in step 2 are each preferably carried out in the presence of a polymerization initiator. As the polymerization initiator, a water-soluble polymerization initiator is preferable.

[0014] <Process 1> In step 1, two or more types of compound (1) may be used in combination. CXY=CR 1 -LR 2 (1) Here, X and Y each independently represent a hydrogen atom, a halogen atom, or a methyl group. 1 represents a hydrogen atom, a halogen atom, or an alkyl group having 1 to 3 carbon atoms. L represents -CO-O-*, -O-CO-*, or -O-. However, * is R 2 R represents the bond position. 2 represents a cyclic alkyl group, a monovalent aromatic hydrocarbon group, or a chain alkyl group having 1 to 6 carbon atoms. 2 may have an ether oxygen atom between the carbon-carbon bonds of the chain alkyl group having 1 to 6 carbon atoms; 2 The hydrogen atoms contained in the cyclic alkyl group, the monovalent aromatic hydrocarbon group and the chain alkyl group having 1 to 6 carbon atoms may be substituted with halogen atoms. R 2 Examples of the cyclic alkyl group include a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. Examples of the monovalent aromatic hydrocarbon group include a phenyl group and a naphthyl group. Examples of the linear alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, and an i-butyl group.

[0015] In order to easily obtain the specific polymer, each group in the formula (1) is preferably one shown below. X and Y are preferably each independently a hydrogen atom, a fluorine atom or a chlorine atom, and more preferably both are a hydrogen atom. R 1 As the alkyl group, an alkyl group having 1 to 3 carbon atoms is preferable, and a methyl group is particularly preferable. As L, -CO-O-* and -O-CO-* are preferred, and -CO-O-* is particularly preferred. R 2 As the alkyl group, a cyclohexyl group, a phenyl group, a chain alkyl group having 1 to 4 carbon atoms, a chain fluoroalkyl group having 1 to 4 carbon atoms, and a chain alkyl group having 2 to 5 carbon atoms and having an etheric oxygen atom between the carbon-carbon bond are preferred, and a chain alkyl group having 1 to 4 carbon atoms and a chain fluoroalkyl group having 1 to 4 carbon atoms are particularly preferred.

[0016] The compound represented by formula (1) is preferably a compound represented by formula (1-1). CH2=C(CH3)-CO-OR 21 (1-1) However, R 21 is a cyclohexyl group, a phenyl group, a chain alkyl group having 1 to 4 carbon atoms, a chain fluoroalkyl group having 1 to 4 carbon atoms, or a chain alkyl group having 2 to 3 carbon atoms and an etheric oxygen atom between the carbon-carbon bonds. R 21 As the alkyl group, a chain alkyl group having 1 to 4 carbon atoms and a chain fluoroalkyl group having 1 to 4 carbon atoms are preferable.

[0017] (aqueous medium) Examples of the aqueous medium include water and a mixture of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include tert-butanol, propylene glycol, and dipropylene glycol. In the case of a mixture of water and a water-soluble organic solvent, the concentration of the water-soluble organic solvent is preferably 10% by mass or less. The aqueous medium is preferably water alone.

[0018] (Water-soluble polymerization initiator) As the water-soluble polymerization initiator, a water-soluble radical initiator and a water-soluble oxidation-reduction catalyst are preferred. As the water-soluble radical initiator, preferred are persulfates such as ammonium persulfate and potassium persulfate, water-soluble organic peroxides such as disuccinic acid peroxide, bisglutaric acid peroxide, and tert-butyl hydroperoxide. As the water-soluble redox catalyst, a combination of an oxidizing agent such as bromic acid or a salt thereof, chloric acid or a salt thereof, persulfuric acid or a salt thereof, permanganic acid or a salt thereof, or hydrogen peroxide, and a reducing agent such as sulfurous acid or a salt thereof, hydrogen sulfite or a salt thereof, thiosulfuric acid or a salt thereof, organic acid, or inorganic salt, is preferred. As the persulfate, potassium persulfate or ammonium persulfate is preferred. As the sulfite, sodium sulfite is preferred. As the inorganic salt, a combination of sulfate anion, sulfite anion, and chloride anion with a metal ion is preferred. As the metal ion, a transition metal is preferred, and examples thereof include manganese, iron, cobalt, nickel, copper, zinc, cerium, and silver ions, and among these, iron ion is preferred. As the inorganic salt, iron (II) sulfate is preferred. As the water-soluble polymerization initiator, a water-soluble oxidation-reduction catalyst is preferred, and among them, a combination of potassium persulfate and sodium sulfite, a combination of potassium persulfate, sodium sulfite, and an inorganic salt is preferred, and a combination of potassium persulfate and sodium sulfite, and a combination of potassium persulfate, sodium sulfite, and iron (II) sulfate are more preferred. Since the polymerization of compound (1) easily proceeds, the pH of the reaction system is preferably 3 to 10, and more preferably 6 to 8. To adjust the pH, a sulfite such as sodium sulfite, ammonia, sodium hydroxide, hydrochloric acid, etc. may be added as necessary. The water-soluble polymerization initiator may be used in combination of two or more kinds. As a method for adding the water-soluble polymerization initiator, the entire amount may be added to the reaction system before starting the polymerization reaction, or the water-soluble polymerization initiator may be added to the reaction system continuously or intermittently.

[0019] The amount of compound (1) used is preferably 0.0001 to 1.0 part by mass, more preferably 0.001 to 0.5 part by mass, based on 100 parts by mass of the aqueous medium. Within this range, a decrease in the polymerization rate can be prevented, and the amount of the specific polymer mixed in the fluoropolymer produced in step 2 can be reduced. As a method for charging compound (1), it is preferable to perform initial lump addition, in which the entire amount is charged into the reaction system before starting the polymerization reaction.

[0020] The amount of the water-soluble polymerization initiator used is preferably 0.1 to 5.0 mol, more preferably 0.1 to 2.0 mol, further preferably 0.1 to 1.5 mol, particularly preferably 0.2 to 1.0 mol, relative to 1 mol of compound (1).

[0021] The polymerization temperature of the compound (1) is preferably 10 to 95° C., more preferably 50 to 90° C. The polymerization time is preferably 5 to 400 minutes, more preferably 5 to 300 minutes, in the case of batch processing. The pressure conditions during polymerization are preferably reduced pressure conditions or normal pressure conditions.

[0022] By the above polymerization, an aqueous dispersion containing the specific polymer is obtained. The specific polymer is in the form of particles and is uniformly dispersed in the aqueous medium. The aqueous dispersion is in a colloidal state. It is presumed that the particles of the specific polymer (hereinafter also referred to as "specific particles") solubilize the specific fluorine-containing monomer by adsorbing and incorporating the specific fluorine-containing monomer at the hydrophobic portion during polymerization of the specific fluorine-containing monomer described below, and that the specific fluorine-containing monomer is polymerized within the particles of the specific particles by adding an initiator thereto. It is also presumed that the specific particles contribute to dispersion stabilization in aqueous media and organic solvents. The D50 of the specific particles is preferably from 10 to 1000 nm, more preferably from 10 to 300 nm, further preferably from 10 to 200 nm, and particularly preferably from 10 to 150 nm.

[0023] The specific particles are composed of a polymer containing units based on compound (1). The content of the units based on the compound (1) in the polymer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on the total units of the polymer. The upper limit is 100% by mass.

[0024] The polymerization makes it easy to obtain a fluoropolymer aqueous dispersion containing specific particles having a D50 of 10 to 1000 nm in an amount of 0.0001 to 1.0 part by mass relative to 100 parts by mass of the aqueous medium. The specific particles are preferably contained in an amount of 0.005 to 0.5 part by mass, more preferably 0.002 to 0.1 part by mass, relative to 100 parts by mass of the aqueous medium.

[0025] <Process 2> Step 2 is a method for producing a fluorine-containing polymer, comprising polymerizing at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride (i.e., the specific fluorine-containing monomer) in an aqueous medium containing the specific polymer obtained in step 1. The polymerization of the specific fluorine-containing monomer is preferably carried out using a water-soluble polymerization initiator, and examples of the water-soluble polymerization initiator include the water-soluble polymerization initiators described in step 1. The polymerization of the specific fluorine-containing monomer is also preferably carried out using a chain transfer agent. Examples of the fluorine-containing polymer include a tetrafluoroethylene-based polymer having a unit based on tetrafluoroethylene (TFE) (hereinafter also referred to as "TFE unit"), polyvinylidene fluoride (hereinafter also referred to as "PVdF"), polychlorotrifluoroethylene, and a copolymer of ethylene and chlorotrifluoroethylene. Among these, a tetrafluoroethylene-based polymer is preferable.

[0026] The fluorine-containing polymer may be prepared by copolymerizing a monomer other than the specific fluorine-containing monomer. Other monomers include fluorine-containing monomers such as hexafluoropropylene (hereinafter also referred to as "HFP"), perfluoro(alkyl vinyl ether) (hereinafter also referred to as "PAVE"), and fluoroalkylethylene (hereinafter also referred to as "FAE"). Examples of PAVE include CF2=CFOCF3 (hereinafter also referred to as "PMVE"), CF2=CFOCF2CF3, CF2=CFOCF2CF2CF3 (hereinafter also referred to as "PPVE"), CF2=CFOCF2CF2CF2CF3, and CF2=CFO(CF2)8F, with PMVE and PPVE being preferred. Examples of FAE include CH2=CH(CF2)2F (hereinafter also referred to as "PFEE"), CH2=CH(CF2)3F, CH2=CH(CF2)4F (hereinafter also referred to as "PFBE"), CH2=CF(CF2)3H, and CH2=CF(CF2)4H, with PFEE and PFBE being preferred. Other monomers include ethylene, propylene, vinyl chloride, vinylidene chloride, and vinyl fluoride. Other monomers include monomers having an oxygen-containing polar group. The oxygen-containing polar group is preferably a hydroxyl group, a carbonyl group-containing group, an acetal group, or an oxycycloalkane group, and more preferably an acid anhydride residue. The monomer having an acid anhydride residue is preferably a monomer having a cyclic acid anhydride residue, and more preferably itaconic anhydride (hereinafter also referred to as "IAH"), citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride (also called hymic anhydride, hereinafter also referred to as "NAH"), or maleic anhydride.

[0027] Examples of tetrafluoroethylene polymers include copolymers of TFE and PAVE, copolymers of TFE and HFP (hereinafter also referred to as "FEP"), copolymers of TFE and ethylene (hereinafter also referred to as "ETFE"), copolymers of TFE and propylene, and copolymers of TFE and vinylidene fluoride. However, the tetrafluoroethylene polymer of the present invention does not include the specific highly heat-resistant polymer described below. Specific high heat resistant polymer: A polymer which, when heated at 10°C / min in a differential scanning calorimeter, exhibits an initial endothermic peak of at least 340°C or higher, and which exhibits an endothermic peak of at least 340°C or higher after the initial endothermic peak. The tetrafluoroethylene polymer of the present invention has melt moldability or elasticity.

[0028] In the present invention, the tetrafluoroethylene polymer is preferably ETFE, PFA or FEP, and among these, ETFE described below and PFA described below are particularly preferred. The FEP is preferably an FEP in which the proportion of HFP units relative to the total of TFE units and HFP units is 1 to 15 mol %, and more preferably an FEP in which the proportion is 5 to 13 mol %.

[0029] ETFE has TFE units and units based on ethylene (hereinafter also referred to as "E units"). In a copolymer having TFE units and E units, the proportion of E units to the total of E units and TFE units is preferably 20 to 70 mol%, more preferably 25 to 60 mol%, and particularly preferably 35 to 55 mol%. The total proportion of E units and TFE units relative to all units constituting ETFE is preferably 80 mol % or more, more preferably 85 mol % or more, and even more preferably 90 mol % or more. It is also preferred that the copolymer contains FAE units in addition to the E units and TFE units. The proportion of the FAE units in the total of the E units and TFE units is preferably 0.1 to 10 mol %, more preferably 0.1 to 5 mol %, and particularly preferably 0.2 to 4 mol %. It is also preferable to have a monomer unit having an oxygen-containing polar group in addition to the E unit and the TFE unit. The ratio of the monomer unit having an oxygen-containing polar group to the total of the E unit and the TFE unit is preferably 0.01 to 5 mol%, more preferably 0.05 to 3 mol%. The method for producing the fluorine-containing polymer of the present invention is emulsion polymerization using an aqueous medium, and even if a monomer having an oxygen-containing polar group, such as a monomer having a highly hydrophilic cyclic acid anhydride residue, is used, it is not too soluble, copolymerization with tetrafluoroethylene, etc. is easy, and the oxygen-containing polar group can be easily introduced into the fluorine-containing polymer.

[0030] The copolymer of TFE and PAVE has TFE units and PAVE units. As the copolymer of TFE and PAVE, a copolymer in which the ratio of PAVE units to the total of TFE units and PAVE units is 0.1 mol% or more and less than 20 mol% (hereinafter also referred to as "PF1") and a copolymer in which the ratio of PAVE units is 20 to 70 mol% (hereinafter also referred to as "PF2") are preferred.

[0031] In PF1, the proportion of PAVE units to the total of TFE units and PAVE units is preferably from 0.5 to 10 mol %, more preferably from 0.5 to 5.0 mol %. PF1 may be a copolymer consisting of only TFE units and PAVE units, or may contain one or more units based on other monomers other than these. As the other monomers, other fluorine monomers and monomers having an oxygen-containing polar group are preferred. As the other fluorine monomer, hexafluoropropylene is preferred. As the monomer having an oxygen-containing polar group, NAH is preferred. When units based on other monomers are included, the content ratio of the other fluorine monomer is preferably 0.1 to 10 mol %, more preferably 0.1 to 6 mol %, based on the total of the TFE units and the PAVE units. As the monomer having an oxygen-containing polar group, 0.01 to 5 mol %, more preferably 0.05 to 3 mol % is preferred. The total proportion of TFE units and PAVE units relative to all units constituting PF1 is preferably 80 mol % or more, more preferably 85 mol % or more, and even more preferably 90 mol % or more. PF1 will also be referred to as "PFA" below.

[0032] In PF2, the proportion of PAVE units to the total of TFE units and PAVE units is preferably from 20 to 50 mol %, more preferably from 25 to 45 mol %. In addition to the TFE units and PAVE units, it is also preferable to have units based on a monomer having a fluorine atom and a nitrile group (hereinafter also referred to as "CN units"), or units based on a monomer having a fluorine atom and multiple vinyl groups (hereinafter also referred to as "DV units"). Examples of the monomer having a fluorine atom and a nitrile group include CF2=CFO(CF2)5CN and CF2=CFOCF2CF(CF3)CF2CF2CN. Examples of the monomer having a fluorine atom and a plurality of vinyl groups include CF2=CFO(CF2)3OCF=CF2, CF2=CFO(CF2)4OCF=CF2, and CH2=CH(CF2)6CH=CH2. The proportion of CN units to the total of TFE units and PAVE units is preferably from 0.1 to 10.0 mol %, more preferably from 0.5 to 5.0 mol %. The proportion of DV units to the total of TFE units and PAVE units is preferably from 0.01 to 1.0 mol %, more preferably from 0.01 to 0.5 mol %. The total proportion of TFE units and PAVE units relative to all units constituting PF2 is preferably 80 mol % or more, more preferably 85 mol % or more, and even more preferably 90 mol % or more.

[0033] The specific fluorine-containing monomer and other monomers are charged into a reaction system (i.e., a polymerization reaction vessel) by a conventional method. For example, TFE is charged into the reaction system continuously or intermittently so that the polymerization pressure becomes a predetermined pressure. Also, for example, other monomers are dissolved in an aqueous medium, and the obtained solution is charged into the reaction system continuously or intermittently. When a water-soluble polymerization initiator is used, the water-soluble polymerization initiator may be added to the reaction system all at once or in portions. When using a chain transfer agent, the chain transfer agent is preferably an alcohol, a hydrocarbon, or a hydrofluorocarbon, since it has an effect of stabilizing the end structure of the resin, and more preferably an alcohol or a hydrocarbon. As the alcohol, methanol or ethanol is preferable, since it is easily dissolved in water and easily separated from the copolymer after production. As the hydrocarbon, n-pentane, cyclohexane, methane, and propane, which have good thermal stability and high chain transferability when introduced into the end structure of the resin, are preferable.

[0034] The polymerization temperature is preferably 10 to 95° C., more preferably 15 to 90° C. The polymerization pressure is preferably 0.5 to 4.0 MPa, more preferably 0.6 to 3.5 MPa In the case of batch processing, the polymerization time is preferably 90 to 1000 minutes, more preferably 90 to 700 minutes.

[0035] The production of the specific polymer and the production of the fluorine-containing polymer may be carried out continuously in the same polymerization reaction vessel. In the production method of the present invention, it is sufficient that specific particles are formed in the production of the specific polymer, and the production of a fluorine-containing polymer may be carried out before the compound (1) is completely consumed in the production of the specific polymer. In this case, it is considered that a fluorine-containing polymer containing a unit based on the compound (1) may be produced.

[0036] When the production of the specific polymer and the production of the fluoropolymer are carried out continuously, the specific polymer obtained in step 1 and present in step 2 is preferably 0.0001 to 1.0 part by mass, more preferably 0.001 to 0.5 part by mass, per 100 parts by mass of the aqueous medium.

[0037] When the production of the specific polymer and the production of the fluoropolymer are not carried out continuously, it is possible to omit step 1. Instead of step 1, a commercially available specific polymer is prepared, and the specific polymer present in step 2 is preferably 0.0001 to 1.0 part by mass, more preferably 0.001 to 0.5 part by mass, based on 100 parts by mass of the aqueous medium. Incidentally, an example of a commercially available specific polymer is Poly(2,2,3,3,4,4,4-heptrafluorobutyl methacrylate) manufactured by Aldrich. For the commercially available specific polymer, D50 is also preferably from 10 to 1000 nm, more preferably from 10 to 300 nm, further preferably from 10 to 200 nm, and particularly preferably from 10 to 150 nm. The content of units based on compound (1) in a commercially available polymer is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more, based on the total units of the polymer. The upper limit is 100% by mass.

[0038] By the above procedure, an aqueous fluoropolymer dispersion containing particles having a D50 of 20 to 3000 nm, which contains a fluoropolymer having units based on the specific fluorine-containing monomer, and the specific particles can be easily obtained. In addition, as described above, it is assumed that the monomer polymerizes within the specific particle during polymerization of the specific fluorine-containing monomer, and therefore the generated fluorine-containing polymer particle may incorporate the specific particle, resulting in the generation of particles containing the fluorine-containing polymer and the specific polymer. In particular, when the specific particle has high affinity with the specific fluorine-containing monomer (for example, when the specific particle is a particle of a specific polymer having a fluorine atom), it is considered that particles containing the fluorine-containing polymer and the specific polymer and having a D50 of 20 to 3000 nm are likely to be generated. The fluoropolymer aqueous dispersion of the present invention is an aqueous dispersion comprising an aqueous medium, fluoropolymer-containing particles having a D50 of 20 to 3000 nm, and a specific polymer contained as particles in the aqueous medium or contained in the particles containing the fluoropolymer as described above. Hereinafter, unless otherwise specified, particles containing a fluoropolymer refer to particles which may contain a specific polymer. The fluoropolymer aqueous dispersion preferably contains 1.0 to 50.0 parts by mass, and more preferably 3 to 40 parts by mass, of particles containing the fluoropolymer per 100 parts by mass of the aqueous medium. The fluoropolymer aqueous dispersion preferably contains the specific polymer in an amount of 0.0001 to 1.0 part by mass per 100 parts by mass of the aqueous medium. In the fluoropolymer aqueous dispersion, the content of the specific polymer per 100 parts by mass of the particles containing a fluoropolymer is preferably from 0.001 to 5.00 parts by mass, more preferably from 0.005 to 3.00 parts by mass. The particle size of the particles containing a fluoropolymer is preferably from 20 to 1000 nm.

[0039] The aqueous dispersion having particles containing the fluoropolymer of the present invention does not require an emulsifier, and therefore can easily be made into a dispersion in an organic solvent such as N-methylpyrrolidone or acetone by solvent substitution. An aqueous dispersion having particles containing a fluoropolymer is mixed with an organic solvent, and the mixture is evaporated or dehydrated using anhydrous sodium sulfate or the like to give a dispersion in an organic solvent.

[0040] In the aqueous dispersion containing the fluoropolymer of the present invention, the fluoropolymer is stably dispersed even without containing an emulsifier, and therefore the aqueous dispersion can be suitably used for coating applications, as a binder, etc.

[0041] The polymer composition of the present invention contains the specific polymer and a fluorine-containing polymer containing units based on the specific fluorine-containing monomer, and has an infrared absorption spectrum of 1500 to 1800 cm -1 The compound (1) has a peak at 1700 to 1800 cm -1 It is preferable that the composition has a peak at . The above-mentioned peak in the infrared spectrum is a peak derived from units based on compound (1) present in the specific polymer, and in some cases is also a peak derived from units based on compound (1) which may be contained in the fluoropolymer as described above. The polymer composition of the present invention can be easily obtained from the aqueous dispersion of the present invention obtained in the above step 2. That is, a powder of the polymer composition can be obtained by agglomerating the polymer from the aqueous dispersion of the present invention. Furthermore, the powdered polymer composition obtained by agglomeration can be homogenized by melt kneading or the like to form a molding material in the form of pellets, granules, or the like, containing the fluorine-containing polymer and the specific polymer, and the powdered polymer composition obtained by agglomeration can also be made into a molded product by melt molding or the like.

[0042] Flocculation methods include, but are not limited to, freeze flocculation, acid flocculation, base flocculation, and flocculation using a coagulant. In the case of freeze aggregation, the aggregation temperature is preferably 0 to 5° C. The aggregation time is preferably 1 hour or more, more preferably 2 hours or more. In the case of acid coagulation, a method of adding an acid-containing solution to the aqueous dispersion of the present invention is preferred. Examples of the acid to be added include hydrochloric acid, nitric acid, sulfuric acid, oxalic acid, hydrofluoric acid, etc., and among these, hydrochloric acid is preferred. The concentration of the acid in the acid-containing solution is preferably 0.1 to 50 mass%, more preferably 1 to 30 mass%, and even more preferably 1 to 10 mass%. The base coagulation is preferably carried out by adding a solution containing a base to the aqueous dispersion of the present invention. Examples of the base to be added include sodium hydroxide, potassium hydroxide, and ammonium carbonate, and among these, sodium hydroxide is preferred. The concentration of the base in the solution containing the base is preferably 0.1 to 50% by mass, more preferably 1 to 30% by mass, and even more preferably 1 to 10% by mass. For the flocculation using a coagulant, a known coagulant can be used. Known coagulants include aluminum salts, calcium salts, and magnesium salts. Specifically, aluminum sulfate, represented by the general formula M'Al(SO4)2· 12 HO (wherein M' is a monovalent cation other than lithium), calcium nitrate, and magnesium sulfate are included, among which alum is preferred, and potassium alum, where M is potassium, is particularly preferred. As the coagulation method, base coagulation is preferred since coagulation is particularly likely to proceed. Although the reason for this is unclear, it is believed that by applying basic conditions, the specific polymer can be hydrolyzed, and the fluorine-containing polymer can be efficiently hydrolyzed.

[0043] The melting point of the fluoropolymer in the polymer composition of the present invention is preferably 150° C. or higher, more preferably 150 to 330° C., more preferably 180 to 320° C., further preferably 220 to 310° C., and still more preferably 260 to 300° C. A melting point in this range is preferable because the heat resistance of the fluoropolymer is high. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following examples, the infrared absorption spectrum of 1700 to 1800 cm-1 The fluoropolymer having a peak in the range means a fluoropolymer containing the specific polymer used in the production of the fluoropolymer, i.e., the polymer composition containing the specific polymer and a fluoropolymer (however, this does not deny the existence of a fluoropolymer having a unit based on compound (1). Even in the case where the infrared absorption spectrum was not measured, the fluoropolymers obtained in the examples are recognized to be the above-mentioned polymer compositions containing a specific polymer and a fluoropolymer.

[0045] The various measurement and evaluation methods are as follows. D50 (nm) of polymer particles in aqueous dispersion: An aqueous dispersion of polymer particles was used as a sample, and the particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer (Otsuka Electronics Co., Ltd., ELSZ). Identification of specific polymer: The fact that a specific polymer has been obtained 1 This was confirmed by H-NMR analysis.

[0046] Q (mm 3 / s) measurement: The Q value (also called volumetric flow rate) was measured using a flow tester (Shimadzu Corporation) at 380°C for PFA and 297°C for ETFE and FEP, with loads of 7 kg, 30 kg, or 50 kg.

[0047] Proportion of each unit in the polymer: The ratio of each unit in the polymer is 19 The values ​​were determined by F-NMR analysis, fluorine content analysis, and infrared absorption spectroscopy.

[0048] Storage modulus of polymer G': The polymer was measured using a rubber processing analyzer (RPA2000, manufactured by Alpha Technologies) according to ASTM D5289 and ASTM D6204 under conditions of temperature: 100°C, amplitude: 0.5 degrees, and frequency: 50 times / min, and the measured value was taken as the storage modulus G'. The storage modulus G' of the polymer is an indicator of the rubber properties of a crosslinked rubber article.

[0049] Melting point(℃): The melting point is the temperature at the endothermic peak due to melting measured under a nitrogen atmosphere using a differential scanning calorimeter (DSC 3500Sirius manufactured by NETZSCH). The temperature change program during the measurement was -20°C → 310°C → -70°C → 310°C, with a heating rate of 10°C / min and a cooling rate of 5°C / min. The temperature at the endothermic peak due to the heat of fusion during the second heating after cooling to -70°C was taken as the "melting point".

[0050] Thermogravimetric loss temperature (5% weight loss point, 1% weight loss point): This is the temperature at which the weight decreases by 5% or 1% when the temperature is increased at 10°C / min in an air atmosphere using a differential thermogravimetry (TG-DTA) apparatus (STA2500Regulus, manufactured by NETZSCH).

[0051] [Preparation of aqueous dispersion of specific polymer] (Reference example 1) After replacing the air in a 1L glass polymerization tank with nitrogen, the tank was depressurized to -0.1 MPaG, and ultrapure water (740 g), sodium sulfite (88 mg), and n-butyl methacrylate (hereinafter also referred to as "nBMA") (330 mg) were charged. Next, the solution in the polymerization tank was heated to 60°C while stirring, and 3.8 ml of a solution (5 mass%) of potassium persulfate (hereinafter also referred to as "KPS") dissolved in deionized water was poured into the polymerization tank to polymerize nBMA. After 30 minutes, the mixture was removed from the polymerization tank to obtain an aqueous dispersion of poly-nBMA. The D50 of the poly-nBMA particles in the aqueous dispersion was 60 nm. After that, water was removed under reduced pressure, and the mixture was dried in vacuum at room temperature. The obtained poly(nBMA) was dissolved in acetone-d6 and subjected to NMR analysis. 1H-NMR (acetone-d6): 1.0ppm (br, 3H), 1.1ppm (br, 2H), 1.3ppm (br, 1H), 1.9-2.4ppm (br, 6H), 4.2ppm (br, 2H)

[0052] (Reference example 2) Except for using 2,2,3,3,4,4,4-heptafluorobutyl methacrylate (hereinafter also referred to as "MHFBE") (624 mg) instead of nBMA (330 mg), an experiment was carried out in the same manner as in Reference Example 1. The D50 of the polyMHFBE particles in the aqueous dispersion was 131 nm. 1 H-NMR (acetone-d6): 1.1ppm (br, 2H), 1.3ppm (br, 1H), 1.9-2.4ppm (br, 2H), 4.8ppm (br, 2H)

[0053] (Reference example 3) After replacing the air in a 1L glass polymerization vessel with nitrogen, the pressure was reduced to -0.1MPaG, and ultrapure water (740g), sodium sulfite (88mg), nBMA (330mg), iron(II) sulfate heptahydrate (11mg), and Chelate HC (17mg) were charged. Next, the solution in the polymerization vessel was heated to 60°C while stirring, and 3.8ml of a solution (5% by mass) of KPS dissolved in deionized water was poured into the polymerization vessel to polymerize nBMA. After 30 minutes, the reaction solution was removed from the polymerization vessel, and an aqueous dispersion of poly-nBMA was obtained. The D50 of the poly-nBMA particles in the aqueous dispersion was 86nm.

[0054] (Reference example 4) Except for using i-butyl methacrylate (330 mg) instead of nBMA (330 mg), an experiment was carried out in the same manner as in Reference Example 3. The D50 of the poly(i-butyl methacrylate) particles in the aqueous dispersion was 58.3 nm.

[0055] (Reference example 5) Except for using cyclohexyl methacrylate (390 mg) instead of nBMA (330 mg), an experiment was carried out in the same manner as in Reference Example 3. The D50 of the poly(cyclohexyl methacrylate) particles in the aqueous dispersion was 94.3 nm.

[0056] (Reference example 6) Except for using phenyl methacrylate (377 mg) instead of nBMA (330 mg), an experiment was carried out in the same manner as in Reference Example 3. The poly(phenyl methacrylate) particles in the aqueous dispersion had a D50 of 41.6 nm.

[0057] (Reference example 7) Except for using 2-methoxyethyl methacrylate (335 mg) instead of nBMA (330 mg), an experiment was carried out in the same manner as in Reference Example 3. The D50 of the poly(2-methoxyethyl methacrylate) particles in the aqueous dispersion was 103.7 nm.

[0058] (Reference example 8) Except for using MHFBE (624 mg) instead of nBMA (330 mg), an experiment was carried out in the same manner as in Reference Example 3. The D50 of the polyMHFBE particles in the aqueous dispersion was 90.6 nm.

[0059] Comparative Example 1 After replacing the air in a 1.2L stainless steel polymerization tank with nitrogen, the tank was depressurized to -0.1MPaG, and ultrapure water (630g), t-butanol (72g), CF3CF2OCF2CF2OCF2COONH4 aqueous solution (30% by mass, 12g), and NaOH aqueous solution (2% by mass, 3.5g) were charged. Next, the solution in the polymerization tank was heated to 60°C while stirring, and pressurized to 1.9MPaG with a mixed monomer of TFE / E = 86 / 14 molar ratio. A solution (5% by mass) of KPS dissolved in deionized water was injected into the polymerization tank. When the pressure in the polymerization tank began to drop, a mixed monomer of TFE / E = 54 / 46 molar ratio was added to maintain the internal pressure of the polymerization tank at 1.9MPaG, and polymerization was allowed to proceed. When the continuous charging of the mixed monomer reached 50g, the polymerization tank was cooled to room temperature, and the gas in the polymerization tank was released to the atmosphere. The polymerization time was 210 minutes. The solids concentration of the obtained aqueous dispersion of the copolymer was about 7%. The D50 of the copolymer particles in the aqueous dispersion was 297 nm. The aqueous dispersion was cooled to aggregate the copolymer particles and obtain a powder. The copolymer powder was then dried at 150° C. The Q value of the obtained copolymer powder under a load of 50 kg was 115 mm 3 The molar ratio of TFE units to E units in the copolymer was 54.7 / 45.3.

[0060] [Production of fluorine-containing polymer] Example 1 [Process 1] After replacing the air in a 2.1L stainless steel polymerization vessel with nitrogen, the pressure was reduced to -0.1MPaG, and ultrapure water (1274g), sodium sulfite (152mg), nBMA (568mg), iron(II) sulfate heptahydrate (19mg), and Chelate HC (29mg) were charged. Next, the solution in the polymerization vessel was heated to 60°C while stirring, and 6.5ml of a solution (5% by mass) of KPS dissolved in deionized water was poured into the polymerization vessel to polymerize nBMA. From the amount of nBMA charged, the amount of poly-nBMA in 100 parts by mass of aqueous medium was 0.044 parts by mass. [Process 2] Next, the polymerization tank was pressurized to 2.6 MPaG with a mixed monomer with a TFE / E=86 / 14 molar ratio, and 19.5 ml of a solution (5 mass%) of KPS dissolved in deionized water was injected into the polymerization tank. When the pressure in the polymerization tank began to drop, a mixed monomer with a TFE / E=54 / 46 molar ratio was added so as to maintain the internal pressure in the polymerization tank at 2.6 MPaG, and polymerization was allowed to proceed. Every time 5 g of the mixed monomer was injected, an aqueous sodium sulfite solution (1.8 mass%, 2 mL) was added to the polymerization tank. When the continuous feeding of the mixed monomer reached 140 g, the polymerization tank was cooled to room temperature. The polymerization time was 377 minutes. The solid concentration of the obtained aqueous dispersion of the fluoropolymer was about 9%. In addition, the D50 of the fluoropolymer particles in the aqueous dispersion of the fluoropolymer was 240 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. The fluoropolymer powder was then dried at 150° C. The Q value of the obtained fluoropolymer powder under a load of 50 kg was 56 mm 3The molar ratio of TFE units / E units in the fluoropolymer was 54.7 / 45.3. The melting point of the obtained fluoropolymer was 270° C. The melting point of the obtained fluoropolymer was 1740 cm -1 A peak in the infrared absorption spectrum due to a specific polymer was detected.

[0061] N-methylpyrrolidone (hereinafter also referred to as "NMP") (20 g) was added to the obtained aqueous dispersion of the fluoropolymer (20 g) to prepare a mixed liquid. Thereafter, water was removed under reduced pressure, and anhydrous magnesium sulfate was added. The anhydrous magnesium sulfate was removed by filtration, and an NMP dispersion of ETFE was obtained. The solid content was about 9%.

[0062] Example 2 [Process 1] After replacing the air in a 1.2 L stainless steel polymerization tank with nitrogen, the tank was depressurized to -0.1 MPaG and ultrapure water (740 g), sodium sulfite (88 mg), and MHFBE (624 mg) were charged. Next, the solution in the polymerization tank was heated to 60°C while stirring, and 3.8 ml of a solution (5 mass%) of KPS dissolved in deionized water was poured into the polymerization tank to polymerize MHFBE. Based on the amount of MHFBE charged, the amount of polyMHFBE per 100 parts by mass of the aqueous medium was 0.084 parts by mass. [Process 2] Next, the polymerization tank was pressurized to 1.9 MPaG with a mixed monomer of TFE / E=86 / 14 molar ratio, and 11.3 ml of a solution (5 mass%) of KPS dissolved in deionized water and PFBE (0.85 g) were injected into the polymerization tank. When the pressure in the polymerization tank started to drop, a mixed monomer of TFE / E=54 / 46 molar ratio was added to maintain the internal pressure of the polymerization tank at 1.9 MPaG, and polymerization was allowed to proceed. When the amount of the mixed monomer added reached 40 g, PFBE (0.85 g) was added. When the continuous feeding of the mixed monomer reached 60 g, the polymerization tank was cooled to room temperature. The polymerization time was 690 minutes. The solid concentration of the obtained aqueous dispersion of fluoropolymer was about 8%. In addition, the D50 of the fluoropolymer particles in the aqueous dispersion was 221 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. The fluoropolymer powder was then dried at 150° C. The Q value of the obtained fluoropolymer powder under a load of 50 kg was 0.35 mm. 3 / s, and the molar ratio of TFE units / E units / PFBE units in the fluoropolymer was 54.2 / 45.1 / 0.67. The melting point of the obtained fluoropolymer was 265°C. The obtained fluoropolymer had a melting point of 1760cm -1 A peak in the infrared absorption spectrum due to a specific polymer was detected.

[0063] Example 3 [Process 1] After replacing the air in a 2.1L stainless steel polymerization vessel with nitrogen, the pressure was reduced to -0.1MPaG, and ultrapure water (1274g), sodium sulfite (152mg), nBMA (568mg), iron(II) sulfate heptahydrate (19mg), and Chelate HC (29mg) were charged. Next, the solution in the polymerization vessel was heated to 60°C while stirring, and 10ml of a solution (3.3% by mass) of KPS dissolved in deionized water was poured into the polymerization vessel to polymerize nBMA. Based on the amount of nBMA charged, the amount of poly-nBMA per 100 parts by mass of the aqueous medium was 0.044 parts by mass. [Process 2] After 30 minutes, the tank was pressurized to 2.6 MPaG with a mixed monomer with a TFE / E=86 / 14 molar ratio, and 40 ml of a solution of KPS dissolved in deionized water (3.3 mass%), PFBE (1.5 g), and an aqueous solution of IAH (5 mass%, 2 mL) were injected into the polymerization tank. When the pressure in the polymerization tank began to drop, a mixed monomer with a TFE / E=54 / 46 molar ratio was added to maintain the internal pressure of the polymerization tank at 2.6 MPaG, and an aqueous solution of IAH (5 mass%, 2 mL) was added every time 10 g of the mixed monomer was charged, and polymerization was allowed to proceed. When the continuous charge of the mixed monomer reached 50 g, the polymerization tank was cooled to room temperature. The polymerization time was 450 minutes. The solid concentration of the obtained aqueous dispersion of fluoropolymer was about 4%. The D50 of the fluoropolymer particles in the aqueous dispersion was 135 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. The fluoropolymer powder was then dried at 150° C. The Q value of the obtained fluoropolymer powder under a load of 50 kg was 13 mm 3 / s, and the molar ratio of TFE units / E units / PFBE units / IAH units in the copolymer was 54.1 / 45.6 / 0.3 / 0.2.

[0064] Example 4 [Process 1] After replacing the air in a 1.2 L stainless steel polymerization tank with nitrogen, the tank was depressurized to -0.1 MPaG and ultrapure water (740 g), sodium sulfite (88 mg), and MHFBE (624 mg) were charged. Next, the solution in the polymerization tank was heated to 60°C while stirring, and 3.8 ml of a solution (5 mass%) of KPS dissolved in deionized water was poured into the polymerization tank to polymerize MHFBE. Based on the amount of MHFBE charged, the amount of polyMHFBE per 100 parts by mass of the aqueous medium was 0.084 parts by mass. [Process 2] After 30 minutes, the tank was pressurized to 1.9 MPaG with a mixed monomer with a TFE / E=86 / 14 molar ratio, and 15.1 ml of a solution (5 mass%) of KPS dissolved in deionized water, PFBE (1.1 g), and methanol (1.5 g) were injected into the polymerization tank. When the pressure in the polymerization tank began to drop, a mixed monomer with a TFE / E=54 / 46 molar ratio was added to maintain the internal pressure of the polymerization tank at 1.9 MPaG, and polymerization was allowed to proceed. When the continuous feeding of the mixed monomer reached 30 g, the polymerization tank was cooled to room temperature. The polymerization time was 407 minutes. The solid concentration of the obtained aqueous dispersion of fluoropolymer was about 4%. In addition, the D50 of the fluoropolymer particles in the aqueous dispersion was 141 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. The fluoropolymer powder was then dried at 150° C. The Q value of the obtained fluoropolymer powder under a load of 50 kg was 130 mm 3 / s, and the molar ratio of TFE units / E units / PFBE units in the fluorine-containing polymer was 54.0 / 45.0 / 1.0.

[0065] Example 5 [Process 1] After replacing the air in a 1.2 L stainless steel polymerization vessel with nitrogen, the pressure was reduced and ultrapure water (740 g), sodium sulfite (88 mg), nBMA (330 mg), iron(II) sulfate heptahydrate (11 mg), and Chelate HC (17 mg) were charged. Next, the solution in the polymerization vessel was heated to 60°C while stirring, and 3.8 ml of a solution (5 mass%) of KPS dissolved in deionized water was poured into the polymerization vessel to polymerize nBMA. Based on the amount of nBMA charged, the amount of poly-nBMA per 100 parts by mass of the aqueous medium was 0.044 parts by mass. [Process 2] After 30 minutes, the reactor was pressurized to 1.4 MPaG with TFE, and 25 ml of a solution (5 mass%) of KPS dissolved in deionized water and PPVE (23.5 g) were injected into the polymerization tank. When the pressure in the polymerization tank began to drop, TFE was added to maintain the internal pressure of the polymerization tank at 1.4 MPaG, and polymerization was allowed to proceed. Every time 3 g of the mixed monomer was injected, an aqueous sodium sulfite solution (1.2 mass%, 1.9 mL) was added to the polymerization tank. When the continuous feeding of TFE reached 30 g, the polymerization tank was cooled to room temperature. The polymerization time was 197 minutes. The solids concentration of the obtained aqueous dispersion of fluoropolymer was about 4%. In addition, the D50 of the fluoropolymer particles in the aqueous dispersion was 131 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. The fluoropolymer powder was then dried at 150° C. The Q value of the obtained fluoropolymer powder under a load of 50 kg was 680 mm 3 / s, and the molar ratio of TFE units / PPVE units in the fluoropolymer was 98.6 / 1.4.

[0066] Example 6 [Process 1] After degassing a 2100mL stainless steel pressure reactor equipped with an anchor impeller, 1000g of ultrapure water, sodium sulfite (119mg), nBMA (297mg), and iron(II) sulfate heptahydrate (15mg) were charged. Next, the solution in the polymerization vessel was heated to 70°C while stirring, and 5ml of a solution (5% by mass) of KPS dissolved in ultrapure water was poured into the polymerization vessel to polymerize nBMA. Based on the amount of nBMA charged, the amount of poly-nBMA per 100 parts by mass of the aqueous medium was 0.030 parts by mass. [Process 2] After 30 minutes, 82g of PMVE and 17g of TFE were charged (TFE:PMVE=25:75 molar ratio). The temperature was raised, and when the internal temperature reached 80°C, the pressure inside the reactor was 1.14MPaG. 40mL of a solution (5% by mass) of ammonium persulfate dissolved in ultrapure water was added to start polymerization. Immediately after that, 0.7g of 1,4-diiodoperfluorobutane was charged together with 10g of ultrapure water. As the polymerization progressed, TFE was injected when the pressure inside the reactor dropped to 1.13MPaG, and the pressure inside the reactor was increased to 1.14MPaG. This was repeated, and 7g of PMVE was also injected every time 8g of TFE was injected. When the total added mass of TFE reached 80 g, the addition of the monomer (hereinafter referred to as "post-added monomer") to be injected after the start of polymerization was stopped, the temperature inside the reactor was cooled to 10°C, the polymerization reaction was stopped, and a latex containing a fluorine-containing polymer (hereinafter also referred to as "fluorine-containing elastic copolymer" was obtained. The polymerization time was 300 minutes. The total added masses of the post-added monomers were 80 g of TFE and 63 g of PMVE, which was converted to a molar ratio of TFE:PMVE=65:35. The solid content concentration of the aqueous dispersion of the obtained copolymer was about 13%. The latex was added to a 5% by mass aqueous solution of potassium aluminum sulfate to coagulate and separate the fluorine-containing elastic copolymer. The fluorine-containing elastic copolymer was filtered, washed with desalted water, and vacuum-dried at 50°C to obtain a white fluorine-containing elastic copolymer. The molar ratio of each monomer in the fluorinated elastic copolymer was TFE:PMVE=63.3:36.7, the content of iodine atoms was 0.15% by mass, and the storage modulus G' of the fluorinated elastic copolymer was 112 kPa.

[0067] Example 7 The experiment was carried out in the same manner as in Example 6, except that i-butyl methacrylate (568 mg) was used instead of nBMA (568 mg). The polymerization time was 375 minutes. The solid content of the obtained aqueous dispersion of the copolymer was about 13%. The latex was added to a 5% by mass aqueous solution of potassium aluminum sulfate to coagulate and separate the fluorinated elastic copolymer. The fluorinated elastic copolymer was filtered, washed with desalted water, and vacuum dried at 50°C to obtain a white fluorinated elastic copolymer. The molar ratio of each monomer in the fluorinated elastic copolymer was TFE:PMVE=64.7:35.3, and the iodine atom content was 0.15% by mass. The storage modulus G' of the fluorinated elastic copolymer was 152 kPa.

[0068] Example 8 [Process 1] After degassing a 2100mL stainless steel pressure reactor equipped with an anchor impeller, 1000g of ultrapure water, sodium sulfite (119mg), nBMA (297mg), and iron(II) sulfate heptahydrate (15mg) were charged into the reactor. The solution in the reactor was then heated to 70°C with stirring, and 5mL of a 5% by mass ultrapure aqueous solution of KPS was poured into the reactor to polymerize nBMA. Based on the amount of nBMA charged, the amount of poly-nBMA per 100 parts by mass of the aqueous medium was 0.030 parts by mass. [Process 2] After 30 minutes, 0.4g of 8CNVE (CF2=CFOCF2CF(CF3)OCF2CF2CN) was charged together with 10g of ultrapure water. Then, 63g of PMVE and 13g of TFE were charged (TFE:PMVE=24:74 molar ratio). The temperature was raised, and when the internal temperature reached 80°C, the pressure inside the reactor was 0.93MPaG. 40mL of a 5% by mass ultrapure aqueous solution of ammonium persulfate was added to start polymerization. As the polymerization progressed, TFE was injected when the pressure inside the reactor dropped to 0.92MPaG, and the pressure inside the reactor was increased to 0.93MPaG. This was repeated, and every time 6g of TFE was injected, 7g of PMVE and 0.4g of 8CNVE were also injected. When the total added mass of TFE reached 80g, the addition of the post-added monomer was stopped, the temperature inside the reactor was cooled to 10°C, the polymerization reaction was stopped, and a latex containing a fluorinated elastic copolymer was obtained. The polymerization time was 300 minutes. The total added masses of the post-added monomers were 80g of TFE, 50g of PMVE, and 4.3g of 8CNVE, which was converted to a molar ratio of TFE:PMVE:8CNVE=72:27:1. The solids concentration of the aqueous dispersion of the obtained copolymer was about 14%. The latex was added to a 5% by mass aqueous solution of potassium aluminum sulfate to coagulate and separate the fluoroelastic copolymer. The fluoroelastic copolymer was filtered, washed with desalted water, and vacuum dried at 50°C to obtain a white fluoroelastic copolymer. The molar ratio of each monomer in the fluoroelastic copolymer was TFE:PMVE:8CNVE=69.1:30.3:0.6. The storage modulus G' of the fluoroelastic copolymer was 359 kPa.

[0069] Example 9 A 1.3 L stainless steel polymerization tank was purged with nitrogen, then the pressure was reduced to -0.1 MPaG, and ultrapure water (640 g), t-butanol (11 g), and poly(MHFBE) (50 mg) (manufactured by Aldrich, product name: Poly(2,2,3,3,4,4,4-heptrafluorobutyl methacrylate)) were charged, and the solution in the polymerization tank was heated to 60°C with stirring. Next, HFP (16 g) was charged, the polymerization tank was pressurized to 1.6 MPaG with TFE monomer, and 20 ml of a solution (5 mass%) of APS dissolved in deionized water was injected into the polymerization tank. When the pressure in the polymerization tank started to drop, TFE monomer was added so as to maintain the internal pressure in the polymerization tank at 1.6 MPaG, and polymerization was allowed to proceed. When the continuous charging of TFE monomer reached 83 g, the polymerization tank was cooled to room temperature. The solid content concentration of the obtained aqueous dispersion of fluoropolymer was about 7%. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. Next, this fluoropolymer powder was dried at 150°C. The Q value of the obtained fluoropolymer powder under a load of 7 kg was 23 mm 3 The molar ratio of TFE units to HFP units in the fluoropolymer was 98.6 / 1.4.

[0070] Example 10 After replacing the air in a 1.2L stainless steel polymerization tank with nitrogen, the tank was depressurized to -0.1MPaG, and ultrapure water (740g), sodium sulfite (88mg), poly(MHFBE) (30mg), and t-butanol (11g) were charged. Next, the solution in the polymerization tank was heated to 60°C while stirring, the polymerization tank was pressurized to 2.6MPaG with a mixed monomer with a TFE / E=86 / 14 molar ratio, and 19.5ml of a solution (5 mass%) in which KPS was dissolved in deionized water was injected into the polymerization tank. When the pressure in the polymerization tank began to drop, a mixed monomer with a TFE / E=54 / 46 molar ratio was added so as to maintain the internal pressure in the polymerization tank at 2.6MPaG, and polymerization was allowed to proceed. When the continuous charging of the mixed monomer reached 30g, the polymerization tank was cooled to room temperature. The polymerization time was 110 minutes. The solids concentration of the resulting aqueous dispersion of fluoropolymer was about 4%. The D50 of the fluoropolymer particles in the fluoropolymer aqueous dispersion was 250 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. Next, this fluoropolymer powder was dried at 150°C. The Q value of the obtained fluoropolymer powder under a load of 30 kg was 5.5 mm3 / s, and the molar ratio of TFE units / E units in the fluoropolymer was 54.7 / 45.3. The melting point of the obtained fluoropolymer was 272°C. The obtained fluoropolymer had a melting point of 1760 cm -1A peak in the infrared absorption spectrum due to a specific polymer was detected.

[0071] Example 11 After replacing the air in a 1.2 L stainless steel polymerization tank with nitrogen, the tank was depressurized to -0.1 MPaG and ultrapure water (740 g), sodium sulfite (88 mg), and MHFBE (624 mg) were charged. Next, the solution in the polymerization tank was heated to 60°C while stirring, and 4 ml of a solution (5 mass%) of KPS dissolved in deionized water was poured into the polymerization tank to polymerize MHFBE. Based on the amount of MHFBE charged, the amount of polyMHFBE per 100 parts by mass of the aqueous medium was 0.084 parts by mass. Next, the polymerization tank was pressurized to 2.6 MPaG with a mixed monomer with a TFE / E=86 / 14 molar ratio, and 12 ml of a solution (5 mass%) of KPS dissolved in deionized water, t-butanol (11 g), and MeOH (2.2 g) were injected into the polymerization tank. When the pressure in the polymerization tank began to drop, a mixed monomer with a TFE / E=54 / 46 molar ratio was added to maintain the internal pressure of the polymerization tank at 2.6 MPaG, and polymerization was allowed to proceed. When the amount of the mixed monomer added reached 10 g, PFBE (0.7 g) was added. After that, PFBE (0.7 g) was added every time 14 g of the mixed monomer was added. When the continuous feeding of the mixed monomer reached 80 g, the polymerization tank was cooled to room temperature. The polymerization time was 458 minutes. The solid concentration of the obtained aqueous dispersion of fluoropolymer was about 9%. In addition, the D50 of the fluoropolymer particles in the aqueous dispersion was 262 nm. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. Then, this fluoropolymer powder was dried at 150°C. The Q value of the obtained fluoropolymer powder under a load of 7 kg was 5 mm3 / s, and the molar ratio of TFE units / E units / PFBE units in the fluoropolymer was 53.8 / 45.3 / 0.96. The melting point of the obtained fluoropolymer was 262°C. The obtained fluoropolymer had a melting point of 1760 cm -1 A peak in the infrared absorption spectrum due to a specific polymer was detected at 429°C. The 1% weight loss temperature and the 5% weight loss temperature were 429°C and 455°C, respectively, as determined by TG-DTA.

[0072] Example 12 [Process 1] After replacing the air in a 2.1L stainless steel polymerization vessel with nitrogen, the pressure was reduced to -0.1MPaG, and ultrapure water (1274g), sodium sulfite (152mg), nBMA (568mg), iron(II) sulfate heptahydrate (19mg), and Chelate HC (29mg) were charged. Next, the solution in the polymerization vessel was heated to 60°C while stirring, and 6.5ml of a solution (5% by mass) of KPS dissolved in deionized water was poured into the polymerization vessel to polymerize nBMA. From the amount of nBMA charged, the amount of poly-nBMA in 100 parts by mass of aqueous medium was 0.044 parts by mass. [Process 2] Next, the polymerization tank was pressurized to 2.5 MPaG with vinylidene fluoride (hereinafter also referred to as "VDF"), and 19.5 ml of a solution (5 mass%) of KPS dissolved in deionized water was injected into the polymerization tank. When the pressure inside the polymerization tank started to drop, VDF was added so as to maintain the internal pressure inside the polymerization tank at 2.5 MPaG, and polymerization was allowed to proceed. When the continuous feeding of VDF reached 30 g, the polymerization tank was cooled to room temperature, and the gas inside the polymerization tank was released to the atmosphere. The polymerization time was 120 minutes. The solids concentration of the obtained aqueous dispersion of the fluoropolymer was about 4%. The aqueous dispersion was cooled to aggregate the fluoropolymer particles to obtain a powder. The fluoropolymer powder was then dried at 150° C. The Q value of the obtained fluoropolymer powder under a load of 30 kg was 1 mm 3 The melting point of the obtained fluoropolymer was 172°C. -1 A peak in the infrared absorption spectrum due to a specific polymer was detected.

[0073] The production methods of the respective Examples are summarized in Table 1, and the fluoropolymer aqueous dispersions are summarized in Table 2, respectively. In Table 1, the term "amount of polymerization initiator" refers to the amount (molar amount) of the water-soluble polymerization initiator used relative to 1 mole of compound (1) in step 1, and the term "amount of specific polymer" refers to the content (parts by mass) of the specific polymer in 100 parts by mass of the aqueous medium used in step 2. In addition, in Table 2, "amount of fluoropolymer" refers to the content (parts by mass) of the fluoropolymer per 100 parts by mass of water in the obtained aqueous dispersion, "amount of specific polymer A" refers to the content (parts by mass) of the specific polymer per 100 parts by mass of water in the obtained aqueous dispersion, and "amount of specific polymer B" refers to the content (parts by mass) of the specific polymer per 100 parts by mass of the fluoropolymer in the obtained aqueous dispersion.

[0074] [Table 1]

[0075] [Table 2] The entire contents of the specification, claims and abstract of Japanese Patent Application No. 2019-060003, filed on March 27, 2019, are hereby incorporated by reference as the disclosure of the specification of the present invention.

Claims

1. In an aqueous medium, at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride is polymerized in the presence of a first polymer containing a unit based on a compound represented by the following formula (1-1): The method for producing a fluorine-containing polymer, wherein the first polymer is a polymer obtained by polymerizing a compound represented by formula (1-1) using 0.1 to 5.0 mol of a water-soluble polymerization initiator relative to 1 mol of the compound represented by formula (1-1). CH 2 =C(CH 3 )-CO-O-R 21 ... (1-1) However, R 21 represents a cyclohexyl group, a phenyl group, a chain alkyl group having 1 to 4 carbon atoms, a chain fluoroalkyl group having 1 to 4 carbon atoms, or a chain alkyl group having 2 to 3 carbon atoms and an etheric oxygen atom between the carbon-carbon bonds.

2. The method according to claim 1, wherein the amount of the first polymer present is 0.0001 to 1.0 part by mass per 100 parts by mass of the aqueous medium.

3. 3. The method according to claim 1, wherein the first polymer present in the aqueous medium is composed of particles having a volume-based cumulative 50% diameter of 10 to 1000 nm.

4. A method for producing a fluorine-containing polymer, comprising polymerizing a compound represented by the following formula (1-1) in an aqueous medium to obtain an aqueous medium in which a first polymer is present, and then polymerizing at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride in the aqueous medium in which the first polymer is present to produce a fluorine-containing polymer. CH 2 =C(CH 3 )-CO-O-R 21 ... (1-1) However, R 21represents a cyclohexyl group, a phenyl group, a chain alkyl group having 1 to 4 carbon atoms, a chain fluoroalkyl group having 1 to 4 carbon atoms, or a chain alkyl group having 2 to 3 carbon atoms and an etheric oxygen atom between the carbon-carbon bonds.

5. The method according to claim 4 , wherein the aqueous medium in which the first polymer is present is an aqueous medium which has been used in the production of the first polymer and in which the first polymer is present.

6. The method according to claim 4 or 5, wherein the compound represented by formula (1-1) is polymerized using 0.1 to 5.0 moles of a water-soluble polymerization initiator per mole of the compound represented by formula (1-1).

7. The method according to any one of claims 4 to 6, wherein the amount of the first polymer present in the polymerization of the fluorine-containing monomer is 0.0001 to 1.0 parts by mass per 100 parts by mass of the aqueous medium.

8. A fluoropolymer aqueous dispersion comprising: an aqueous medium; particles having a volume-based cumulative 50% diameter of 20 to 3,000 nm, the particles comprising a fluoropolymer having units based on at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride; and a first polymer comprising units based on a compound represented by the following formula (1-1), the first polymer being contained as particles in the aqueous medium or contained in particles comprising the fluoropolymer; and no emulsifier. CH 2 =C(CH 3 )-CO-O-R 21 ... (1-1) However, R 21 represents a cyclohexyl group, a phenyl group, a chain alkyl group having 1 to 4 carbon atoms, a chain fluoroalkyl group having 1 to 4 carbon atoms, or a chain alkyl group having 2 to 3 carbon atoms and an etheric oxygen atom between the carbon-carbon bonds.

9. The fluoropolymer aqueous dispersion according to claim 8, comprising 1.0 to 50.0 parts by mass of the particles containing the fluoropolymer per 100 parts by mass of the aqueous medium.

10. The fluoropolymer aqueous dispersion according to claim 8 or 9, wherein the particles of the first polymer are contained in an amount of 0.0001 to 1.0 part by mass per 100 parts by mass of the aqueous medium.

11. The fluoropolymer aqueous dispersion according to any one of claims 8 to 10, comprising 0.001 to 5.00 parts by mass of particles of the first polymer per 100 parts by mass of particles containing the fluoropolymer.

12. The fluoropolymer aqueous dispersion according to any one of claims 8 to 11, wherein the particles of the first polymer are particles having a volume-based cumulative 50% diameter of 10 to 1000 nm.

13. The present invention relates to a fluorine-containing polymer comprising a first polymer containing a unit based on a compound represented by the following formula (1-1) and a unit based on at least one fluorine-containing monomer selected from tetrafluoroethylene, chlorotrifluoroethylene and vinylidene fluoride, and does not contain an emulsifier. The fluorine-containing polymer has an infrared absorption spectrum of 1500 to 1800 cm. -1 has a peak derived from a unit based on a compound represented by the following formula (1-1), The polymer composition, wherein the content of the first polymer is 0.001 to 2.108 parts by mass based on 100 parts by mass of the fluoropolymer. CH 2 =C(CH 3 )-CO-O-R 21 ... (1-1) However, R 21 represents a cyclohexyl group, a phenyl group, a chain alkyl group having 1 to 4 carbon atoms, a chain fluoroalkyl group having 1 to 4 carbon atoms, or a chain alkyl group having 2 to 3 carbon atoms and an etheric oxygen atom between the carbon-carbon bonds.

Citation Information

Patent Citations

  • Polymerization of Fluoropolymers Using Non-Fluorinated Surfactants

    JP2009504841A

  • Aqueous fluorocopolymer dispersion

    WO1995008582A1

  • Method for producing melt-moldable fluororesin

    WO2007046377A1

  • Production method for aqueous dispersion

    WO2018181740A1

  • Modified polytetrafluoroethylene, molded article, and method for producing stretched porous material

    WO2019065640A1