Resin composition for carbon fiber composite material, towpreg
The resin composition for tow prepregs, comprising epoxy resin and organophilic phyllosilicate clay minerals, addresses unwinding and width accuracy issues, ensuring high-speed unwinding without defects and providing heat resistance for aerospace applications.
Patent Information
- Application Number
- JP2021529752
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-02-08
- Filing Date
- 2019-12-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-12-19
AI Technical Summary
Existing tow prepregs face issues with unwinding properties, width accuracy, and heat resistance, particularly during high-speed unwinding and lamination processes, leading to defects such as fuzz and fiber bridges, which are critical for aerospace applications.
A resin composition for tow prepregs containing epoxy resin, liquid multifunctional amine type epoxy resin, and organophilic phyllosilicate clay minerals, which provides high storage modulus, thixotropy, and excellent heat resistance, ensuring good unwinding properties and width accuracy.
The resin composition maintains the shape and width accuracy of tow prepregs during high-speed unwinding, preventing fuzz and fiber bridges, and achieves high heat resistance suitable for aerospace applications.
Smart Images

Figure 0007552595000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a towpreg that exhibits good unwinding properties from a bobbin and good width precision after unwinding, and that provides a composite material with excellent heat resistance, and a resin composition that provides such a towpreg. [Background technology]
[0002] In the manufacture of fiber-reinforced composite materials, prepregs are often used, which are intermediate substrates in which reinforcing fibers are aligned in one direction, or in which sheet-like materials such as woven fabrics and nonwoven fabrics are impregnated with thermosetting resin. On the other hand, in addition to sheet-like prepregs, there are also narrow intermediate substrates called tow prepregs, yarn prepregs, or strand prepregs, which are made by impregnating reinforcing fiber bundles in which several thousand to several tens of thousands of filaments are aligned in one direction with thermosetting resin.
[0003] Examples of lamination methods for these intermediate substrates include the hand lay-up method, the ATL (Automated Tape Laying) method, and the AFP (Automated Fiber Placement) method. However, when manufacturing large composite materials such as aircraft, automated lamination methods such as the ATL method and the AFP method are used because they enable a dramatic improvement in productivity (see, for example, Patent Document 1). Among them, the AFP method employs a technique of laminating slit tape prepregs obtained by cutting prepregs into tape-like shapes in the fiber direction. This method is suitable for manufacturing parts with relatively many curved surfaces, such as aircraft fuselages, and can minimize defects during molding, so it has become a method that has been widely used in recent years.
[0004] In the automatic lamination method, the intermediate substrate is once wound on a bobbin after the reinforcing fiber bundle is impregnated with a thermosetting resin during the manufacturing process. Then, in the manufacturing process of the fiber-reinforced composite material, the tow prepreg wound on the bobbin is unwound and used. If the intermediate substrates are adhered to each other during unwinding, fluff and fiber bridges will occur due to the resistance at the time of separation of the adhered intermediate substrates, and the quality of the intermediate substrate will be significantly reduced, so it is necessary to prevent the adhesion of the intermediate substrates wound on the bobbin. In addition, if the intermediate substrate positions overlap during lamination by the machine, the mechanical properties after curing of the laminate will be significantly reduced, so it is also important that the intermediate substrate has high width accuracy. In addition to these characteristics, the intermediate substrate must also have high heat resistance in order to be used in aviation applications.
[0005] Patent Document 2 discloses a towpreg that is excellent in unwinding properties by using a low-viscosity resin. On the other hand, when a low-viscosity resin is used, it becomes difficult to maintain the shape of the towpreg, and it is impossible to achieve the width precision that is essential for automatic lamination. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2008-517810 [Patent Document 2] JP 2011-157491 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention overcomes the drawbacks of the conventional technology and relates to a towpreg that provides a composite material with excellent heat resistance, with good unwinding properties from a bobbin and good width precision after unwinding, and to a resin composition that provides such a towpreg. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention employs the following means: That is, the towpreg of the present invention is a towpreg impregnated with an epoxy resin composition containing the following components [A] to [C]:
[0009] [A] an epoxy resin that is solid at 23°C in an amount of 30 parts by mass or more out of 100 parts by mass of the total epoxy resin components; [B] a multifunctional amine-type epoxy resin that is liquid at 23°C in an amount of 20 parts by mass or more out of 100 parts by mass of the total epoxy resin components; and [C] Clay Minerals As Organophilic phyllosilicates .
[0010] The present invention also relates to a fiber-reinforced composite material obtained by heat curing the towpreg of the present invention.
[0011] The present invention also relates to an article of manufacture comprising or consisting of one or more fiber-reinforced composite materials according to the invention, for example a composite material for aerospace applications or the aviation industry, such as an aircraft, typically an aircraft fuselage. Effect of the Invention
[0012] According to the present invention, the resin composition impregnated in the towpreg has a high storage modulus at room temperature of 23° C., and the resin exhibits thixotropy, so that the fluidity of the resin during storage is extremely low. Even if the towpreg is stored for a long time after being wound around a bobbin, the towpreg does not adhere to each other and exhibits good unwinding properties. In addition, even if pressure is applied to the outer surface of the towpreg by the winding tension during production, and the towpreg is pressed against the bobbin, the shape of the towpreg is unlikely to deform. Therefore, even if the towpreg wound around the bobbin is unwound at high speed, fluff and fiber bridges are unlikely to occur, the towpreg is easy to unwind, and the state after unwinding is good. Such a high speed is, for example, more than 10 m / min. Furthermore, the width of the towpreg does not fluctuate during storage on the bobbin, and the width precision is not disturbed when the towpreg is unwound, so the width precision after unwinding of the towpreg is also good. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (Towpreg) The towpreg of the present invention refers to a narrow intermediate substrate obtained by impregnating a reinforcing fiber bundle (tow) in which several thousand to several tens of thousands of filaments are arranged in one direction with a thermosetting resin. The narrow width of the towpreg means a dimension of 2.0 inches or less, preferably 1.0 inches or less, and more preferably 0.5 inches or less. When the above width range is satisfied, the towpreg has a high fiber basis weight, and the molding cycle time can be effectively shortened. It is preferable that the towpreg of the present invention satisfies all of the following conditions [T1] to [T3]. [T1] to [T3] will be explained in order below.
[0014] The towpreg of the present invention preferably satisfies the following requirement: [T1] A sample obtained by winding a 1.2 m towpreg around a bobbin having an outer diameter of 8.25 cm for 30 seconds under a load of 9.8 N is stored in an environment of 23°C / 50 RH% for 5 days, and then unwound at 1.0 m / min. The tension is more preferably 3.0 N or less. If the tension is greater than 5.0 N, a large resistance occurs when unwound at high speed, making unwinding difficult, leading to the generation of a large amount of fluff and fiber bridges on the towpreg surface, and the condition of the surface after unwinding is also deteriorated. Furthermore, the tension during unwinding causes deformation of the towpreg, and the width accuracy of the towpreg after unwinding is also deteriorated.
[0015] The tension required for unwinding referred to here means the load when the bobbin is unwound at 1.0 m / min using a universal testing machine (eg, Instron universal testing machine, manufactured by Instron Corporation).
[0016] In addition, in the towpreg of the present invention, a sample in which a towpreg cut to a length of 7.6 cm was sandwiched between two 2.6 cm × 7.6 cm glass plates was placed at a thickness of 2.48 × 10 3When stored for two days in an environment of 23°C / 50RH% with a pressure of 100 Pa applied, the width expansion of the towpreg is 3.0% or less. If the width expansion is more than 3.0%, the shape of the towpreg is easily changed due to the winding tension when winding the towpreg onto a bobbin and the resistance during unwinding, and the width accuracy of the towpreg after being released at high speed is deteriorated. Furthermore, a large width variation causes the end of the towpreg to be rubbed during unwinding, which generates fuzz. As a result, the surface condition after unwinding is also deteriorated.
[0017] The width expansion of the towpreg referred to here refers to a value calculated using the following formula (1) from the values obtained by measuring the width of the towpreg before and after storage using an optical microscope (e.g., VHX-500F: manufactured by KEYENCE Corporation). (Towpreg width after storage / Towpreg width before storage-1) x 100...Formula (1) Furthermore, in the towpreg of the present invention, the glass transition temperature when the towpreg is cured for 2 hours at a temperature [T3] of 180° C. or higher is 180° C. or higher. The glass transition temperature is more preferably 200° C. or higher. When the towpreg exhibits a glass transition temperature of 180° C. or higher, it can be preferably used in aerospace applications that require high heat resistance.
[0018] The glass transition temperature referred to here means the onset temperature of the storage modulus of a carbon fiber reinforced polymer (CFRP) having a thickness of 2 mm obtained by laminating towpregs and curing the towpregs at 180°C for two hours, measured using a dynamic viscoelasticity measuring device (e.g., DISCOVERY HR-2: manufactured by TA Instruments) at a heating rate of 5°C / min in a cantilever bending mode with a frequency of 1 Hz. (Epoxy resin composition) In addition, in the epoxy resin composition contained in the towpreg of the present invention, [R1] is the thixotropy coefficient at 60°C (η * 0.1Hz / η * 10Hz) is 3.0 or more. If the thixotropy coefficient is less than 3.0, the resin will flow when the towpreg is stored for a long period of time while wound on a bobbin, causing the towpreg to adhere to each other, which will deteriorate the unwinding property when the towpreg is unwound at high speed. The thixotropy coefficient is more preferably 4.0 or more.
[0019] The thixotropy coefficient at 60°C is defined as a value calculated using the following formula (2) from the viscosity measured at 60°C in a torsional mode at frequencies of 0.1 Hz and 10 Hz using a dynamic viscoelasticity measuring device (e.g., DISCOVERY HR-2: manufactured by TA Instruments). Viscosity at 0.1Hz (η * 0.1Hz ) / Viscosity at 10Hz (η * 10Hz )...Equation (2) In addition, in the epoxy resin composition contained in the towpreg of the present invention, the storage modulus at 1 Hz at 23°C, [R2], is 2.0 × 10 5 More preferably, the pressure is 2.0×10 Pa or more. 5 Pa ~ 6.0 × 10 6 Pa. The storage modulus is 2.0×10 5 If the storage modulus is lower than 3.0×10 Pa, it becomes difficult for the towpreg to retain its shape, and the width precision after high-speed unwinding deteriorates. 5 Pa or more.
[0020] The storage modulus of the resin composition referred to here is a value measured using a dynamic viscoelasticity measuring device (eg, DISCOVERY HR-2: manufactured by TA·Instruments) at a temperature of 23° C. in a torsion mode at a frequency of 1 Hz.
[0021] Furthermore, in the epoxy resin composition contained in the towpreg of the present invention, the glass transition temperature of the epoxy resin composition [R3] when cured at a temperature of 180°C or higher for 2 hours is 180°C or higher. When the towpreg exhibits a glass transition temperature of 180°C or higher, it can be preferably applied to aerospace applications requiring heat resistance. The glass transition temperature is more preferably 200°C or higher.
[0022] The glass transition temperature referred to here means the onset temperature of the storage modulus when the temperature of a sample cured at 180°C for 2 hours is measured using a dynamic viscoelasticity measuring device (e.g., ATD-3000: manufactured by Alpha Technologies) at a heating rate of 5°C / min and a frequency of 1.64 Hz in torsion mode.
[0023] The structure of the epoxy resin contained in the towpreg of the present invention is not particularly limited, but examples of usable epoxy resins include bisphenol type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, bisnaphthalene type epoxy resins, dicyclopentadiene type epoxy resins, tetraphenylethane type epoxy resins, triphenylmethane type epoxy resins, glycidylamine type epoxy resins, and aminophenol type epoxy resins.
[0024] The epoxy resin composition contained in the towpreg of the present invention contains, as an essential component, 30 parts by mass or more of an epoxy resin that is solid at room temperature 23° C. per 100 parts by mass of epoxy resin. The amount is more preferably 40 parts or more. When the above range is satisfied, a resin composition having a good storage modulus at 1 Hz at room temperature 23° C. can be obtained, and a towpreg with good impregnation can also be obtained.
[0025] Furthermore, the epoxy resin composition [A] contained in the towpreg of the present invention contains, as an essential component, 30 parts by mass or more of an epoxy resin that is solid at room temperature of 23° C. per 100 parts by mass of epoxy resin. More preferably, it is 40 parts or more. When the above range is satisfied, both the storage modulus at 23° C. and the impregnation performance can be maintained at preferred levels.
[0026] Furthermore, the epoxy resin composition contained in the towpreg of the present invention preferably contains an epoxy resin having an epoxy equivalent of 300 g / eq or less in an amount of 20 parts or more based on the solid epoxy. When the above range is satisfied, a towpreg having good impregnation performance and surface quality can be obtained.
[0027] [B] The epoxy resin composition contained in the towpreg of the present invention contains, as an essential component, 20 parts by mass or more of a polyfunctional amine-type epoxy resin that is liquid at 23°C per 100 parts by mass of epoxy resin. When the above range is satisfied, a resin composition that exhibits good heat resistance after curing can be obtained. Furthermore, since the epoxy resin contains a polyfunctional amine-type epoxy resin, the dispersion of particles such as the curing agent and inorganic particles is good, and the epoxy resin suppresses waviness of the towpreg during impregnation, a towpreg with good width precision can be obtained.
[0028] By using in combination an epoxy resin that is solid at room temperature (23°C) and has an epoxy equivalent of 300 g / eq or less, and a polyfunctional amine-type epoxy resin that is liquid at 23°C, an epoxy resin composition with even better heat resistance after curing can be obtained.
[0029] Commercially available bisphenol-type epoxy resins that are solid at room temperature include jER (registered trademark) 1001, 1004, 1007, 4004P, and 4007P (manufactured by Mitsubishi Chemical Corporation), and Araldite (registered trademark) GT7071 and GT6084-2 (manufactured by Huntsman).
[0030] Examples of commercially available epoxy resins that are solid at room temperature and have an epoxy equivalent of 300 g / eq or less include cresol novolac epoxy resins such as "Epicron (registered trademark)" N-660, N-665, and N-695 (manufactured by DIC Corporation), phenol aralkyl epoxy resins such as NC-3000 and NC-3000L (manufactured by Nippon Kayaku Co., Ltd.), bisnaphthalene epoxy resins such as "Epicron (registered trademark)" HP-4700, HP-4710, and HP-4770 (manufactured by DIC Corporation), and dicyclopentadiene epoxy resins such as "Epicron (registered trademark)" HP-7200 and HP-7200H (manufactured by DIC Corporation) and Tactix556 (manufactured by Huntsman).
[0031] These epoxy resins which are solid at room temperature may be added not only alone but also in combination of two or more kinds.
[0032] Commercially available polyfunctional amine-type epoxy resins that are liquid at 23°C include glycidyl amine-type epoxy resins such as "Sumiepoxy (registered trademark)" ELM434 (manufactured by Sumitomo Chemical Co., Ltd.) and "Araldite (registered trademark)" MY720 and MY721 (manufactured by Huntsman Corporation); and aminophenol-type epoxy resins such as "Sumiepoxy (registered trademark)" ELM100 and ELM120 (manufactured by Sumitomo Chemical Co., Ltd.), "Araldite (registered trademark)" MY0500, MY0510 and MY0600 (manufactured by Huntsman Corporation), and "jER (registered trademark)" 630 (manufactured by Mitsubishi Chemical Corporation).
[0033] Examples of the curing agent for the epoxy resin composition contained in the towpreg of the present invention include aromatic amines, dicyandiamide, and adipic dihydrazide, either singly or in mixtures. Examples of aromatic amines include meta-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, and meta-xylylenediamine.
[0034] These curing agents may be used alone or in appropriate combination. Aromatic amines are particularly preferred because they can impart heat resistance to the resin cured product. From the viewpoint of imparting heat resistance, it is preferred to add aromatic amines so that the epoxy equivalent ratio, which is the molar ratio of the epoxy group of the epoxy resin to the active hydrogen of the aromatic amines, is 0.7 to 1.2.
[0035] The epoxy resin composition may contain inorganic particles to impart thixotropy to the resin composition and provide releasability when formed into a towpreg. , i.e., organophilic phyllosilicates as clay minerals. It is necessary to contain the inorganic particles. The inorganic particles preferably have a rod-like, tubular, or plate-like shape. Record As the earth mineral, an organophilic phyllosilicate such as "Garamite (registered trademark)"-1958, -7305 (manufactured by BYK Additives & Instruments) can be used. The epoxy resin composition , sticky Earth Minerals Organophilic phyllosilicates as As a result, the resin composition acquires thixotropy and exhibits excellent unwinding properties when formed into a towpreg, along with maintaining good impregnation properties and good width precision of the towpreg.
[0036] In addition, the epoxy resin composition contained in the towpreg of the present invention can be blended with a thermoplastic resin component within a range that does not impair the effects of the present invention. Specific examples include polyacetal resin, polyvinyl formal, polymethyl methacrylate, polyamide, polyimide, polyvinylpyrrolidone, polysulfone, etc. Among them, polysulfone and polyimide are preferred because the resin itself has excellent heat resistance, and polyethersulfone is particularly preferred. If the polyethersulfone has a weight average molecular weight of 30,000 g / mol or less, it is preferred because the impregnation of the resin into the towpreg is improved.
[0037] An example of a commercially available polyethersulfone product is "Sumikaexcel (registered trademark)" PES (manufactured by Sumitomo Chemical Co., Ltd.), and an example of a commercially available polyimide product is "Matrimid 5218 (manufactured by Huntsman Corporation)". (Method of producing epoxy resin composition) In producing the epoxy resin composition of the present invention, the raw materials may be kneaded using a machine such as a kneader, a planetary mixer, a three-roll mill, or a twin-screw extruder, or the raw materials may be mixed by hand using a beaker, a spatula, or the like, provided that uniform kneading is possible. (Fiber-reinforced composite materials) Next, the fiber reinforced composite material will be described. A fiber reinforced composite material can be obtained by heat curing the towpreg of the present invention. The reinforcing fibers used in the present invention are not particularly limited, and glass fibers, carbon fibers, aramid fibers, boron fibers, alumina fibers, silicon carbide fibers, etc. can be used. Only one type of these fibers can be used, or two or more types of them can be mixed and used. Among them, it is preferable to use carbon fibers from the viewpoint of obtaining a lightweight and highly elastic fiber reinforced composite material. EXAMPLES
[0038] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the description of these examples. Measurements of various physical properties were carried out in an environment of a temperature of 23° C. and a relative humidity of 50%, unless otherwise specified.
[0039] The materials used to manufacture each towpreg are as follows: <Materials used> (Epoxy resin that is liquid at room temperature of 23°C) "Araldite (registered trademark)" LY1556 (bisphenol type epoxy resin, epoxy equivalent: 187g / eq, manufactured by Huntsman) "Araldite (registered trademark)" GY282 (bisphenol type epoxy resin, epoxy equivalent: 167g / eq, manufactured by Huntsman) (Liquid polyfunctional amine epoxy resin at 23℃) "Araldite (registered trademark)" MY0510 (aminophenol type epoxy resin, epoxy equivalent: 96g / eq, manufactured by Huntsman) "Araldite (registered trademark)" MY721 (glycidylamine type epoxy resin, epoxy equivalent: 115g / eq, manufactured by Huntsman) (Epoxy resin that is solid at room temperature of 23℃) "Araldite (registered trademark)" MY9665T (glycidylamine type epoxy resin, epoxy equivalent: 120g / eq, manufactured by Huntsman) "Araldite (registered trademark)" GT7071 (bisphenol type epoxy resin, epoxy equivalent: 490g / eq, manufactured by Huntsman) "Araldite (registered trademark)" GT6084-2 (bisphenol type epoxy resin, epoxy equivalent: 862g / eq, manufactured by Huntsman) "Epiclon (registered trademark)" HP4710 (bisnaphthalene type epoxy resin, epoxy equivalent: 172g / eq, manufactured by DIC Corporation) "Epiclon (registered trademark)" HP7200L (dicyclopentadiene type epoxy resin, epoxy equivalent: 247g / eq, manufactured by DIC Corporation) (hardening agent) "Aradur®" 9664-1 (4,4'-diaminodiphenyl sulfone, Huntsman) "Aradur®" 9771-1 (3,3'-diaminodiphenyl sulfone, Huntsman) (Inorganic particles) (1) Clay minerals Garamite®-7305 (organophilic phyllosilicate, BYK Additives & Instruments) Garamite®-1958 (organophilic phyllosilicate, BYK Additives & Instruments) (2) Fumed silica "AEROSIL®" R 202 (fumed silica, manufactured by Evonik) Typically, the towpreg composition contains 1 to 10% inorganic particles based on 100 parts of the epoxy resin composition. (thermoplastic resin) "Sumikaexcel (registered trademark)" PES 2603MP (polyethersulfone, weight average molecular weight: 16000 g / mol, manufactured by Sumitomo Chemical Co., Ltd.) Typically, the towpreg composition contains 1 to 20% thermoplastic resin per 100 parts of the epoxy resin composition. (Reinforced Fiber) "TORAYCA (registered trademark)" T700G-12K (carbon fiber, manufactured by Toray Carbon Fibers Europe) <Method of producing epoxy resin composition> A predetermined amount of the epoxy resin composition, excluding the curing agent and inorganic particles, was placed in a kneader, and the mixture was heated and kneaded to obtain a transparent viscous liquid. After the viscous liquid was cooled while being kneaded, the curing agent and inorganic particles were added, and the mixture was kneaded to obtain an epoxy resin composition.
[0040] Table 1 shows the compositions of the epoxy resin compositions of the examples and comparative examples. <Method of measuring the characteristics of epoxy resin composition> (1) Method for measuring storage modulus of epoxy resin composition at room temperature (23°C) Using a dynamic viscoelasticity measuring device (DISCOVERY HR-2: manufactured by TA Instruments) and a parallel plate with a diameter of 8 mm, the uncured resin composition was set so that the distance between the upper and lower jigs was 500 μm, and the storage modulus was measured in torsion mode at a temperature of 23°C and a frequency of 1 Hz. (2) Method for measuring the thixotropy coefficient of an epoxy resin composition at 60°C Using a dynamic viscoelasticity measuring device (DISCOVERY HR-2: manufactured by TA Instruments) and a parallel plate with a diameter of 25 mm, the uncured resin composition was set so that the distance between the upper and lower jigs was 500 μm, and the viscosity was measured in a torsional mode at a temperature of 60° C. and frequencies of 0.1 Hz and 10 Hz. The thixotropy coefficient can be calculated from the obtained viscosity using the following formula (3). Viscosity at 0.1Hz (η * 0.1Hz ) / Viscosity at 10Hz (η * 10Hz )...Equation (3) <Method for measuring the glass transition temperature of cured epoxy resin> The uncured epoxy resin composition degassed in vacuum was heated at a rate of 2.0°C / min using a dynamic viscoelasticity measuring device (ATD-3000: manufactured by Alpha Technologies), cured at a temperature of 180°C for 2 hours, and then heated at a rate of 5°C / min to measure the storage modulus in a torsion mode at a frequency of 1.64 Hz. The onset temperature of the storage modulus at this time was defined as the glass transition temperature. <Towpreg manufacturing method> Each of the various epoxy resin compositions produced using the compositions in Table 1 was impregnated into a reinforcing fiber bundle by the pultrusion molding method described below to produce a towpreg.
[0041] Specifically, a reinforcing fiber bundle is passed through a tow prepreg manufacturing device equipped with a creel for sending out reinforcing fibers, a resin bath for impregnating with epoxy resin, a slit die at the outlet of the resin bath for shaping, a drive station equipped with a chiller, and a winder to create a yarn path. The epoxy resin composition was adjusted to a temperature of 80°C in a separate hot air oven and supplied to a resin bath also adjusted to a temperature of 80°C. The reinforcing fibers are supplied with the epoxy resin composition by passing through the resin bath, and then the resin content is adjusted by passing through a die. Finally, the fibers pass through a drive station cooled to 20°C or less, and are then wound up by a winder to form a towpreg bobbin. When winding up with the winder, a back film was supplied together with the towpreg as necessary in order to prevent adhesion between the towpregs. Winding was performed on towpregs both with and without the back film.
[0042] The line speed during production of the towpreg was 1 m / min, the winding line tension was 12 N or less, and the resin content was adjusted to 34 wt %. <Method of evaluating towpreg characteristics> (1) Evaluation of the state of the towpreg after high-speed unwinding The bobbins of the towpregs wound around bobbins without a backing film obtained in each of the Examples and Comparative Examples were left for 30 minutes or more in an environment of a temperature of 23°C ± 5°C and a relative humidity of 60% ± 20%, then set on a creel and the towpregs were unwound at 20 m / min using a winder, and the state of the towpregs was evaluated. A was determined if the unwinding property was good and no fluff or fiber bridges occurred after unwinding, B was determined if fluff occurred after unwinding, and C was determined if a large amount of fluff or fiber bridges occurred after unwinding, making unwinding difficult. (2) Evaluation of width accuracy after high-speed unwinding of towpreg The bobbins of towpregs wound around bobbins without a backing film obtained in each of the examples and comparative examples were left for 30 minutes or more in an environment of a temperature of 23°C ± 5°C and a relative humidity of 60% ± 20%, then set on a creel, and 18 m of the towpreg was unwound at 2 m / min using a winder. The width of the unwound towpreg was then measured at 481 points spaced 3.75 cm apart using a microscope (VHX-500F: manufactured by KEYENCE Corporation), and the standard deviation was defined as the width precision. (3) Towpreg winding test A 1.2 m length was taken from the towpreg with a backing film wound around a bobbin obtained in each Example and Comparative Example, one end of the towpreg was fixed with tape to a bobbin with an outer diameter of 8.25 cm, and a 1.0 kg weight was attached to the other end. The bobbin was then attached to a creel so that the weight floated, and the towpreg without a backing film was wound up around the bobbin over 30 seconds with a tension of 9.8 N applied to the towpreg, to produce a sample.
[0043] The sample was stored for 5 days in an environment at a temperature of 23°C ± 5°C and a relative humidity of 50% ± 10%, and then set on a creel. The tension was measured using an Instron universal testing machine (manufactured by Instron) when unwound at a crosshead speed of 1.0 m / min. (4) Pressure deformation test of towpreg A 7.6 cm length was taken from the towpreg with the back film wound on a bobbin obtained in each Example and Comparative Example, and the towpreg was sandwiched between 2.6 cm × 7.6 cm glass plates to prepare a sample. The width of the towpreg in the sample was measured at 7 points at 1.0 cm intervals using a microscope (VHX-500F: manufactured by KEYENCE Corporation) (the average width value was W b (Assuming that.)
[0044] Next, a 500 g weight was placed on the sample, and the sample was weighed down to 2.48 × 10 3 After storing the sample for two days in an environment with a temperature of 23°C ± 5°C and a relative humidity of 50% ± 10% under a pressure of 100 Pa, the width of the towpreg in the sample was measured again at seven points using a microscope (the average width was taken as Wa The width expandability of the towpreg before and after pressure was calculated using the following formula (4). (The width of the towpreg after storage W a / Towpreg width before storage W b -1)×100...Equation (4) (5) Method for measuring the glass transition temperature of towpreg From the bobbins of the towpregs wound around the bobbins with the backing film obtained in each of the Examples and Comparative Examples, 25 cm was taken out, and the towpregs were laminated in 8 plies on an aluminum plate and cured at a temperature of 180°C for 2 hours to obtain a plate-shaped fiber-reinforced composite material with a thickness of 2 mm. A test piece with a width of 10 mm and a length of 35 mm was cut out from this fiber-reinforced composite material, and the storage modulus was measured in a cantilever bending mode with a frequency of 1 Hz by heating at a heating rate of 5°C / min using a dynamic viscoelasticity measuring device (e.g., DISCOVERY HR-2: manufactured by TA Instruments). The onset temperature of the storage modulus at this time was defined as the glass transition temperature. (6) Observation of towpreg surface quality The towpreg bobbins immediately after production were used to observe the surface quality of the towpreg. When the surface quality was good and no fuzz or towpreg waviness was observed, it was judged as A, when small fuzz or small towpreg waviness was observed, it was judged as B, when a large amount of fuzz or large towpreg waviness was observed, it was judged as C, and when a large amount of fuzz or carbon fiber breakage was observed, it was judged as D. Therefore, in the case of D, it was not possible to produce a towpreg. Example 1 An epoxy resin composition was produced according to the above <Production method of epoxy resin composition> using 50 parts by mass of Araldite (registered trademark) MY0510 and 50 parts by mass of Epicron (registered trademark) HP4710 as the epoxy resin, 45.9 parts of Aradur (registered trademark) 9664-1 as the curing agent, 10 parts by mass of Sumikaexcel (registered trademark) PES 2603MP as the thermoplastic resin, and 3 parts by mass of Garamite (registered trademark) -7305 as the inorganic particles, and then a towpreg with a resin content of 34 wt% was produced according to the above <Production method of towpreg>.
[0045] The appearance and width precision of the towpreg after high speed unwinding, the winding test, the pressure deformation test, the glass transition temperature after curing at 180°C for 2 hours, the thixotropy coefficient of the epoxy resin composition at 60°C, the storage modulus at 23°C and 1 Hz, and the glass transition temperature after curing at 180°C for 2 hours are shown in Table 1. (Examples 2 to 4) An epoxy resin composition and a towpreg having a resin content of 34 wt % were produced in the same manner as in Example 1, except that the components and amounts of the epoxy resin composition were changed as shown in Table 1.
[0046] With regard to the towpreg and epoxy resin composition of each example, the state and width precision of the towpreg after high speed unwinding, the winding test, the pressure deformation test, the glass transition temperature after curing at 180°C for 2 hours, the thixotropy coefficient of the epoxy resin composition at 60°C, the storage modulus at 23°C and 1 Hz, and the glass transition temperature after curing at 180°C for 2 hours are shown in Table 1. Comparative Example 1 An epoxy resin composition and a towpreg with a resin content of 34% by weight were produced in the same manner as in Example 1 using the components shown in Comparative Example 1 in Table 1. In Comparative Example 1, the epoxy resin composition impregnated in the towpreg did not contain inorganic particles, and the thixotropy coefficient at 60°C was 1.3 and less than 3.0, so the results of the towpreg winding test were 5.8 N and more than 5.0 N, and resistance occurred when the towpreg was unwound at high speed, resulting in the generation of a large amount of fuzz and fiber bridges. Therefore, the condition after unwinding was poor, and the width precision after unwinding was also poor at 0.23. Comparative Example 2 An epoxy resin composition and a towpreg with a resin content of 34% by weight were produced in the same manner as in Example 1 using the components shown in Comparative Example 2 in Table 1. In Comparative Example 2, no epoxy resin that is solid at room temperature was included, and the storage modulus at 23°C of the epoxy resin composition impregnated into the towpreg was 1.0 × 10 5 Pa and 2.0 x 10 5Pa or less, and the results of the pressure deformation test of the towpreg were 5.9% and 3.0% or more. Therefore, the width accuracy after the towpreg was unwound at high speed was poor. Comparative Example 3 An epoxy resin composition and a towpreg with a resin content of 34% by weight were produced in the same manner as in Example 1 using the components shown in Example 3 in Table 1. In Comparative Example 3, since no epoxy that was solid at room temperature was included, the epoxy resin was unable to achieve desirable levels in both storage modulus at 23°C and impregnation performance. Due to high viscosity at the impregnation temperature, breakage of the carbon fibers occurred during towpreg production, and a towpreg could not be obtained. Comparative Example 4 An epoxy resin composition and a towpreg with a resin content of 34% by weight were produced in the same manner as in Example 1 using the components shown in Comparative Example 4 in Table 1. In Comparative Example 4, the epoxy resin did not contain a multifunctional amine-type epoxy resin. Therefore, the towpreg waving occurred during production, and the width accuracy after the towpreg was unwound at high speed was poor. Comparative Example 5 An epoxy resin composition and a towpreg with a resin content of 34% by weight were produced in the same manner as in Example 1 using the components shown in Comparative Example 5 in Table 1. In Comparative Example 5, fused silica was added as the inorganic particles instead of clay minerals, so the towpreg was in a poor state when unwound at high speed, with a large amount of fuzz and fiber bridges occurring. Furthermore, the width precision of the towpreg after unwound at high speed was 0.24, which was also poor.
[0047] [Table 1]
Claims
1. A towpreg comprising reinforcing fiber bundles aligned in one direction impregnated with an epoxy resin composition, the epoxy resin composition comprising the following components [A] to [C]: [A] an epoxy resin that is solid at 23°C in an amount of 30 parts by mass or more out of 100 parts by mass of the total epoxy resin components; [B] a polyfunctional amine-type epoxy that is liquid at 23°C in an amount of 20 parts by mass or more out of 100 parts by mass of the total epoxy resin components, and [C] Organophilic phyllosilicates as clay minerals; A towpreg comprising:
2. 2. The towpreg of claim 1, wherein the epoxy resin composition has an epoxy equivalent of 300 g / eq or less in an amount of 20 parts or more in the solid epoxy resin.
3. The towpreg according to any one of claims 1 to 2, wherein the epoxy resin composition has a multifunctional amine-type epoxy in an amount of 20 parts by mass or more per 100 parts by mass of a total epoxy resin component.
4. The towpreg meets the following conditions [T1] to [T3]: [T1] A sample obtained by winding 1.2 m of the towpreg around a bobbin having an outer diameter of 8.25 cm under a load of 9.8 N for 30 seconds is stored in an environment of 23° C. / 50% RH for 5 days and then unwound at 1.0 m / min. The tension required is 5.0 N or less; [T2] The towpreg cut to a length of 7.6 cm was sandwiched between two 2.6 cm x 7.6 cm glass plates to form a sample, and the sample was then sandwiched between two 2.6 cm x 7.6 cm glass plates to form a sample having a thickness of 2.48 x 10 mm. 3 The towpreg has a width expansion of 3.0% or less when stored for two days in an environment of 23° C. / 50% RH under a pressure of 1.0 Pa; and [T3] The glass transition temperature of the cured product obtained by curing the towpreg at 180 ° C. for 2 hours is 180 ° C. or higher. The towpreg according to any one of claims 1 to 3, wherein
5. The epoxy resin composition satisfies the following conditions [R1] to [R3]: [R1] Thixotropy coefficient at 60 ° C. (η * 0.1Hz / * 10Hz ) is 3.0 or more; [R2] Storage modulus at 1 Hz at 23 °C is 2.0 × 10 5 Pa or more; and [R3] The glass transition temperature of the cured product obtained by curing the epoxy resin at 180°C for 2 hours is 180°C or higher. The towpreg according to any one of claims 1 to 4, wherein
6. 5. The towpreg according to claim 4, wherein the cured product obtained by curing the towpreg at 180°C for two hours has a glass transition temperature of 200°C or higher.
7. 6. The towpreg according to claim 5, wherein the cured product obtained by curing the epoxy resin at 180°C for two hours has a glass transition temperature of 200°C or higher.
8. The towpreg according to any one of claims 1 to 7, wherein the epoxy resin composition contains an aromatic amine as a curing agent.
9. The towpreg according to any one of claims 1 to 8, wherein the epoxy resin composition contains an epoxy resin having at least one structure selected from the group consisting of a naphthalene skeleton, a dicyclopentadiene skeleton, a phenol aralkyl skeleton, and a cresol novolac skeleton, in an amount of 20 parts or more based on the solid epoxy resin.
10. The towpreg according to any one of claims 1 to 9, wherein the epoxy resin composition contains an epoxy resin having an epoxy equivalent of 200 g / eq or less in an amount of 20 parts or more based on the solid epoxy resin.
11. The towpreg according to any one of claims 1 to 10, wherein the solid epoxy has a naphthalene skeleton.
12. The towpreg according to any one of claims 1 to 5 and 8 to 9, wherein the solid epoxy has a dicyclopentadiene skeleton.
13. The towpreg according to any one of claims 1 to 12, wherein the epoxy resin composition contains a thermoplastic resin.
14. The towpreg of claim 13, wherein the thermoplastic resin is polyethersulfone.
15. 15. The towpreg of claim 14, wherein the polyethersulfone has a weight average molecular weight of 30,000 g / mol or less.
16. The towpreg according to any one of claims 1 to 15, wherein the polyfunctional amine-type epoxy resin is an aminophenol type.
17. A fiber-reinforced composite material produced by heat curing the towpreg according to any one of claims 1 to 16.
18. 18. An article of manufacture comprising or consisting of one or more fibre reinforced composite materials according to claim 17.
19. 19. Product according to claim 18, characterized in that the product is a composite material for aerospace applications or the aeronautical industry, such as aircraft, typically aircraft fuselages.
Citation Information
Patent Citations
Epoxy resin composition for yarn prepreg and yarn prepreg
JP1994345884A
System and method for automatic fiber layup
JP2008517810A
Epoxy resin composition for tow prepreg and tow prepreg
JP2011157491A
Epoxy resin composition for tow prepreg and tow prepreg
JP2012056980A
Epoxy resin composition, molding material and fiber-reinforced composite material
JP2013032510A