Resin composition

JP7552673B2Active Publication Date: 2024-09-18AJINOMOTO CO INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022190424
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-11-29
Publication Date
2024-09-18
Estimated Expiration
2042-11-29

Smart Images

  • Figure 0007552673000021
    Figure 0007552673000021
  • Figure 0007552673000019
    Figure 0007552673000019
  • Figure 0007552673000020
    Figure 0007552673000020
Patent Text Reader

Abstract

To provide a resin composition that contains an organic filler and can form an insulating layer capable of preventing the intrusion of conductor materials.SOLUTION: A resin composition comprises (A) an organic filler containing a group represented by formula (a-1), and (B) a curable resin. (In the formula (a-1), X represents -SO3Na, -SO3NH4, or a hydrogen atom; A represents a divalent hydrocarbon group that may have a substituent; m represents 1 when X is a hydrogen atom, and 0 or 1 when X is -SO3Na or -SO3NH4; n represents an integer of 1 or more).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, and a cured product, a sheet-like laminate material, a resin sheet, a circuit board, a semiconductor chip package, and a semiconductor device using the resin composition. [Background technology]

[0002] Circuit boards and semiconductor chip packages are generally provided with an insulating layer. For example, a printed wiring board, which is a type of circuit board, may be provided with an interlayer insulating layer as an insulating layer. Also, for example, a semiconductor chip package may be provided with a rewiring formation layer as an insulating layer. These insulating layers are usually formed from a cured product obtained by curing a resin composition (Patent Documents 1 and 2).

[0003] Moreover, the techniques of Patent Documents 3 and 4 are publicly known. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2020-23714 A [Patent Document 2] JP 2020-136542 A [Patent Document 3] International Publication No. 2021 / 039798 [Patent Document 4] Patent No. 6522135 Summary of the Invention [Problem to be solved by the invention]

[0005] In order to improve the physical properties of an insulating layer, a resin composition containing an organic filler may be used. For example, a resin composition containing an organic filler may be used to reduce stress in the insulating layer, thereby suppressing the destruction of the insulating layer due to stress. However, when a conductor layer is formed by plating on an insulating layer formed using a resin composition containing an organic filler, the conductor material may penetrate into the insulating layer.

[0006] The penetration will be specifically described below. For example, assume that a conductor layer is formed on an insulating layer containing an organic filler and a cured resin by a plating method including electroless plating. Here, unless otherwise specified, the "cured resin" refers to components other than the particles of the organic filler and the like contained in the insulating layer. In this case, when electroless plating is performed, a part of the conductor material may penetrate into the interface between the particles of the organic filler and the cured resin near the surface of the insulating layer, forming a local conductive part at the interface. The phenomenon in which the conductor material that penetrates into the insulating layer forms a conductive part at the interface between the particles of the organic filler and the cured resin is called "penetration". Hereinafter, the conductive part formed in the insulating layer by penetration in this way may be called the "penetration part".

[0007] Generally, a conductor layer is patterned to form wiring having a desired pattern shape. However, if a buried portion is formed in the insulating layer as described above, unintended electrical connection may occur between the wirings through the buried portion. Therefore, flash etching is usually performed to remove the buried portion formed in the insulating layer.

[0008] However, in recent years, the density of wiring on circuit boards and semiconductor chip packages has been increasing, which has led to a demand for narrower spaces between wiring. When the spaces between wiring are narrowed, electrical conduction is more likely to occur through the submerged portions. Therefore, even if the submerged portions are removed by flash etching, some of the submerged portions remain, increasing the possibility of unintended electrical conduction occurring.

[0009] The present invention has been devised in view of the above circumstances, and aims to provide a resin composition capable of forming an insulating layer that contains an organic filler and can suppress the infiltration of a conductive material; a cured product of the resin composition; a sheet-like laminate material and a resin sheet that contain the resin composition; and a circuit board, a semiconductor chip package, and a semiconductor device that contain the cured product of the resin composition. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that a resin composition containing a combination of an organic filler containing a specific group and a curable resin can solve the above problems, thereby completing the present invention. That is, the present invention includes the following.

[0011] [1] A resin composition comprising: (A) an organic filler containing a group represented by the following formula (a-1); and (B) a curable resin: [ka] (In formula (a-1), X represents -SO3Na, -SO3NH4 or a hydrogen atom; A represents a divalent hydrocarbon group which may have a substituent; m represents 1 when X is a hydrogen atom, and represents 0 or 1 when X is -SO3Na or -SO3NH4; n represents an integer of 1 or more. [2] The resin composition according to [1], wherein the organic filler (A) contains a group represented by formula (a-1) on the surface of the particles of the organic filler (A). [3] The resin composition according to [1] or [2], wherein the average particle size of the organic filler (A) is 5 μm or less. [4] The resin composition according to any one of [1] to [3], further comprising an inorganic filler (C). [5] The resin composition according to any one of [1] to [4], wherein the curable resin (B) contains one or more resins selected from the group consisting of epoxy resins, phenolic resins, active ester resins, cyanate ester resins, carbodiimide resins, benzoxazine resins, allyl resins, acrylic resins, styryl resins, and maleimide resins. [6] The resin composition according to any one of [1] to [5], further comprising (D) a curing accelerator. [7] The resin composition according to any one of [1] to [6], which is for forming an insulating layer. [8] A cured product of the resin composition described in any one of [1] to [7]. [9] A sheet-like laminate material comprising the resin composition according to any one of [1] to [7].

[10] A support and a resin composition layer formed on the support, A resin sheet, wherein a resin composition layer comprises the resin composition according to any one of [1] to [7].

[11] A circuit board comprising a cured product of the resin composition according to any one of [1] to [7].

[12] A semiconductor chip package comprising a cured product of the resin composition described in any one of [1] to [7].

[13] A semiconductor device comprising the circuit board according to

[11] .

[14] A semiconductor device comprising the semiconductor chip package described in

[12] . Effect of the Invention

[0012] According to the present invention, there can be provided a resin composition capable of forming an insulating layer that contains an organic filler and can suppress the infiltration of a conductive material; a cured product of the resin composition; a sheet-like laminate material and a resin sheet that contain the resin composition; and a circuit board, a semiconductor chip package, and a semiconductor device that contain the cured product of the resin composition. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a cross-sectional view that illustrates the surface vicinity of a conventional insulating layer that contains an organic filler. [Diagram 2] FIG. 2 is a cross-sectional view that shows a schematic view of the surface vicinity of a conventional insulating layer in which a resist layer is formed on an electroless plating layer. [Diagram 3] FIG. 3 is a cross-sectional view that shows a schematic view of the surface vicinity of a conventional insulating layer in which an electrolytically plated layer is formed on an electrolessly plated layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will be described below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims and their equivalents.

[0015] In the following description, the term "optionally substituted" in reference to a compound or group means both the case where none of the hydrogen atoms of the compound or group are substituted with a substituent, and the case where some or all of the hydrogen atoms of the compound or group are substituted with a substituent.

[0016] In the following description, the term "(meth)acrylic acid" includes acrylic acid, methacrylic acid, and combinations thereof, and the term "(meth)acrylate" includes acrylate, methacrylate, and combinations thereof.

[0017] In the following description, the term "dielectric constant" refers to the relative dielectric constant unless otherwise specified.

[0018] [Resin composition overview] The resin composition according to one embodiment of the present invention includes (A) an organic filler containing a group represented by the following formula (a-1) and (B) a curable resin. Hereinafter, the organic filler containing a group represented by the formula (a-1) (A) may be referred to as "(A) specific filler". By curing the resin composition according to this embodiment, an insulating layer that can suppress the penetration of a conductive material while containing an organic filler can be obtained.

[0019] [ka]

[0020] (In formula (a-1), X represents -SO3Na, -SO3NH4, or a hydrogen atom; A represents a divalent hydrocarbon group which may have a substituent; m represents 1 when X is a hydrogen atom, and represents 0 or 1 when X is -SO3Na or -SO3NH4; n represents an integer of 1 or more. * represents a bond.)

[0021] Without being bound by any particular theory, the present inventors speculate that the mechanism by which the resin composition according to the present embodiment provides the above-mentioned effects is as follows, however, the technical scope of the present invention is not limited by the speculation below.

[0022] FIG. 1 is a cross-sectional view showing the vicinity of a surface 100U of a conventional insulating layer 100 containing an organic filler. In FIG. 1, the organic filler particles 110 are drawn relatively large for ease of understanding, but the size of the organic filler particles 110 is not limited to that shown in FIG. 1. As shown in FIG. 1, the organic filler particles 110 are generally dispersed in a cured resin 120 in an insulating layer 100. Since the conventional organic filler particles 110 tend to have poor affinity with the cured resin 120, when an electroless plating layer 130 is formed on the surface 100U of the insulating layer 100 by electroless plating, a part of the conductive material may penetrate into the interface between the organic filler particles 110 and the cured resin 120. When a part of the conductive material penetrates into the interface, a penetration portion 140 may be formed as a local conductive portion at the interface.

[0023] FIG. 2 is a cross-sectional view showing the vicinity of a surface 100U of a conventional insulating layer 100 in which a resist layer 150 is formed on an electroless plating layer 130. FIG. 3 is a cross-sectional view showing the vicinity of a surface 100U of a conventional insulating layer 100 in which an electrolytic plating layer 160 is formed on an electroless plating layer 130. Usually, a resist layer 150 is formed on the electroless plating layer 130 using a photosensitive dry film, as shown in FIG. 2. Thereafter, an electrolytic plating layer 160 is formed on the electroless plating layer 130 by electrolytic plating, and the resist layer 150 is removed, and a conductor layer 170 is formed as wiring including the electroless plating layer 130 and the electrolytic plating layer 160, as shown in FIG. 3.

[0024] Usually, after removing the resist layer 150, unnecessary portions of the electroless plating layer 130 are removed by flash etching. This flash etching can remove the penetration portion 140. However, even with the flash etching, a part of the penetration portion 140 may remain in the insulating layer 100. If the remaining penetration portion 140 forms a conductive path between the conductor layers 170, unintended conduction between the conductor layers 170 may occur.

[0025] In contrast, in the insulating layer formed using the resin composition according to this embodiment, a specific filler (A) is used as an organic filler. The specific filler (A) containing a group represented by formula (a-1) improves the surface properties of the specific filler (A) and improves the affinity with the cured resin. Furthermore, the group represented by formula (a-1) may react or interact with a polar group that may be contained in the cured resin to form a loose bond. Furthermore, when the insulating layer contains an inorganic filler, the functional group on the surface of the inorganic filler particle may react or interact with the group represented by formula (a-1), which may also form a loose bond. Therefore, the crosslinked structure in the insulating layer can be made dense, so that the intrusion of the conductive material during electroless plating can be suppressed, and therefore the intrusion can be suppressed.

[0026] In addition, as described above, the affinity between the specific filler (A) and the cured resin is improved, and the crosslinked structure is dense, thereby improving the physical properties of the insulating layer. Therefore, for example, the mechanical strength of the insulating layer can be improved to increase the elongation at break and to increase the adhesion to the conductor layer. In addition, the affinity between the specific filler (A) and the cured resin is improved, and the crosslinked structure is dense, thereby improving the resistance to the roughening solution during the roughening treatment, and thus an insulating layer with small surface roughness can be obtained.

[0027] [(A) Specific filler (organic filler containing a group represented by formula (a-1)] The resin composition according to one embodiment of the present invention contains a specific filler (A) (i.e., an organic filler containing a group represented by formula (a-1)) as component (A). The specific filler (A) is present in the resin composition in particulate form, and is usually contained in the cured product while maintaining the particulate form.

[0028] The specific filler (A) contains a group represented by formula (a-1). Usually, the specific filler (A) contains a polymer, and the polymer contains a group represented by formula (a-1) in the molecule.

[0029] [ka]

[0030] In formula (a-1), X represents -SO3Na, -SO3NH4, or a hydrogen atom.

[0031] In formula (a-1), A represents a divalent hydrocarbon group which may have a substituent. The number of carbon atoms in the divalent hydrocarbon group is usually 1 or more, preferably 2 or more, and preferably 12 or less, more preferably 8 or less, and even more preferably 6 or less. The divalent hydrocarbon group in A may be an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a combination thereof. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, or an unsaturated aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear or branched chain hydrocarbon group, a cyclic hydrocarbon group (i.e., an alicyclic hydrocarbon group), or a combination of a chain hydrocarbon group and a cyclic hydrocarbon group. Among them, the divalent hydrocarbon group in A is preferably an aliphatic hydrocarbon group, more preferably a saturated aliphatic hydrocarbon group, and even more preferably an alkylene group.

[0032] Examples of the divalent hydrocarbon group in A include alkylene groups such as methylene, ethylene, propylene, and butylene groups; cycloalkylene groups such as cycloheptylene and cyclohexylene groups; and arylene groups such as phenylene and naphthylene groups. Among these, alkylene groups are preferred, with methylene and ethylene groups being more preferred, and ethylene groups being even more preferred.

[0033] Examples of the substituent that the divalent hydrocarbon group in A may have include an alkyl group, an aryl group, an alkylaryl group, an arylalkyl group, an alkyloxy group, an aryloxy group, an alkyloxyalkyl group, an aryloxyalkyl group, an alkylaryloxy group, an arylalkyloxy group, an alkylaryloxyalkyl group, an alkyloxycarbonyl group, and an alkyloxycarbonylalkyl group. The number of carbon atoms in A, including the substituent, is usually 1 or more, preferably 2 or more, and preferably 18 or less, more preferably 12 or less, and even more preferably 6 or less. Among these, A is preferably a divalent hydrocarbon group having no substituent.

[0034] In formula (a-1), m represents 1 when X is a hydrogen atom. Also, m represents 0 or 1 when X is -SO3Na or -SO3NH4. Among them, m is preferably 1 when X is any of a hydrogen atom, -SO3Na and -SO3NH4. When m is 1, the group represented by formula (a-1) has an oxyalkylene chain, and the desired effects of the present invention can be significantly obtained.

[0035] In formula (a-1), n ​​represents an integer of 1 or more. More specifically, n is usually 1 or more, and is preferably 20 or less, more preferably 15 or less, and even more preferably 10 or less.

[0036] Examples of the group represented by formula (a-1) include the groups represented by the following formulas (a-1-1) to (a-1-5). In formulas (a-1-1) to (a-1-5), R a represents an alkyl group, n1 represents an integer of 1 or more, and * represents a bond.

[0037] [ka]

[0038] The type of the group represented by formula (a-1) contained in the specific filler (A) may be one type, or two or more types.

[0039] More preferably, the specific filler (A) contains a group represented by formula (a-2).

[0040] [ka]

[0041] (In formula (a-2), R represents a divalent group; X, A, m, and n are the same as those in formula (a-1); * represents a bond.)

[0042] In formula (a-2), X, A, m and n are the same as those in formula (a-1).

[0043] In formula (a-2), R represents a divalent group, preferably a divalent organic group. The divalent organic group represents a divalent group containing at least a carbon atom as a skeletal atom, and may be linear, branched, or cyclic. The number of skeletal atoms in the divalent organic group is preferably 1 to 3000, more preferably 1 to 1000, even more preferably 1 to 100, still more preferably 1 to 50, and particularly preferably 1 to 30 or 1 to 20. Examples of the organic group include groups consisting of one or more skeletal atoms (including at least a carbon atom) selected from carbon atoms, oxygen atoms, nitrogen atoms, and sulfur atoms.

[0044] Among these, the divalent group represented by R is preferably a divalent organic group selected from the group consisting of a divalent hydrocarbon group which may have a substituent, an oxygen atom, a carbonyl group, and a combination thereof. The number of carbon atoms in this preferable divalent organic group is preferably 1 to 60, more preferably 1 to 50, and even more preferably 1 to 40.

[0045] The divalent hydrocarbon group in R may be an aliphatic hydrocarbon group, an aromatic hydrocarbon group, or a combination thereof. The aliphatic hydrocarbon group may be a saturated aliphatic hydrocarbon group, or an unsaturated aliphatic hydrocarbon group. The aliphatic hydrocarbon group may be a linear or branched chain hydrocarbon group, a cyclic hydrocarbon group (i.e., an alicyclic hydrocarbon group), or a combination of a chain hydrocarbon group and a cyclic hydrocarbon group. Among them, the divalent hydrocarbon group in R is preferably an alkylene group, an arylene group, and an arylene-alkylene-arylene group. Examples of preferred alkylene groups include a methylene group and an ethylene group. Examples of preferred arylene groups include a phenylene group. Examples of preferred arylene-alkylene-arylene groups include a phenylene-methylene-phenylene group.

[0046] Preferable examples of R include a carbonyloxy group, an alkyleneoxy group which may have a substituent, an arylene-oxy group which may have a substituent, an alkylene-oxy-carbonyl group which may have a substituent, an alkylene-oxy-alkylene-oxy group which may have a substituent, and a carbonyl-poly(oxyalkylene)-oxy-arylene-alkylene-arylene-oxy group which may have a substituent. Among these, an alkyleneoxy group which may have a substituent, an arylene-oxy group which may have a substituent, and an alkylene-oxy-alkylene-oxy group which may have a substituent are preferable.

[0047] Examples of the substituent that the divalent hydrocarbon group in R may have include the same as the substituent that the divalent hydrocarbon group in A in formula (a-1) may have. Among them, an alkyl group, an arylalkyl group, an alkyloxy group, an alkyloxyalkyl group, an alkylaryloxy group, and an alkylaryloxyalkyl group are preferred.

[0048] Particularly preferred specific examples of R include the groups of the following formulae (a-2-i) to (a-2-viii). In formulae (a-2-i) to (a-2-viii), R a each independently represents an alkyl group, n2 represents an integer of 1 or more and 4 or less, n3 represents an integer of 1 or more, n4 and n5 each independently represent 1 or 2, and * represents a bond.

[0049] [ka]

[0050] Specific examples of the group represented by formula (a-2) include the groups represented by the following formulas (a-2-1) to (a-2-17). In formulas (a-2-1) to (a-2-17), R a each independently represents an alkyl group; A 1 and A 2each independently represents an alkylene group; n6 and n7 each independently represent an integer of 1 or more; n8 represents an integer of 1 or more and 4 or less; n9 and n 10 each independently represents 1 or 2, and * represents a bond.

[0051] [ka]

[0052] [ka]

[0053] The type of the group represented by formula (a-2) contained in the (A) specific filler may be one type, or two or more types.

[0054] The (A) specific filler is generally a particle containing a polymer. Usually, the (A) specific filler contains a particulate polymer, and the polymer contains a group represented by formula (a-1), and preferably, the polymer contains a group represented by formula (a-2). The group represented by formula (a-1) or formula (a-2) is usually bonded to the molecular skeleton of the polymer by a covalent bond, so that the group does not easily come off from the polymer. Therefore, the (A) specific filler containing the polymer can stably exert the excellent effect of the group represented by formula (a-1) or formula (a-2). In the following description, the polymer containing the group represented by formula (a-1) may be referred to as "polymer (a1)".

[0055] The polymer (a1) contained in the specific filler (A) preferably contains a repeating unit represented by the following formula (a-3).

[0056] [ka]

[0057] (In formula (a-3), X, A, m, and n are the same as those in formula (a-1); R is the same as those in formula (a-2); R 1 , R2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

[0058] In formula (a-3), X, A, m, and n are the same as those in formula (a-1), and R is the same as that in formula (a-2).

[0059] In formula (a-3), R 1 , R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, and a propyl group. Among these, a hydrogen atom and a methyl group are preferred.

[0060] The amount of the repeating unit represented by formula (a-3) contained in the polymer (a1) is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 3% by mass or less, based on 100% by mass of the polymer (a1). When the amount of the repeating unit represented by formula (a-3) is within the above range, penetration of the conductive material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductive layer of the insulating layer can be generally improved.

[0061] The repeating unit represented by formula (a-3) can be obtained, for example, by polymerizing a monomer represented by the following formula (a-4).

[0062] [ka]

[0063] (In formula (a-4), X, A, m, and n are the same as those in formula (a-1); R is the same as those in formula (a-2); R 1 , R 2 and R 3 represents the same as formula (a-3).

[0064] Examples of the monomer represented by formula (a-4) include compounds represented by the following formulas (a-4-1) to (a-4-17). In formulas (a-4-1) to (a-4-17), R a represents an alkyl group, and A 1 and A 2 each independently represents an alkylene group; n6 and n7 each independently represent an integer of 1 or more; n8 represents an integer of 1 or more and 4 or less; n9 and n 10 each independently represents 1 or 2.

[0065] [ka]

[0066] [ka]

[0067] The monomer represented by formula (a-4) may be a commercially available product. Examples of commercially available products include "Latemul PD-104" and "Latemul PD-105" (compounds of formula (a-4-1)) manufactured by Kao Corporation; "Latemul PD-420", "Latemul PD-430", "Latemul PD-430S", and "Latemul PD-450" (compounds of formula (a-4-2)) manufactured by Kao Corporation; "Eleminol JS-20" (compound of formula (a-4-3)) manufactured by Sanyo Chemical Industries; "Eleminol RS-3000" (compound of formula (a-4-4)) manufactured by Sanyo Chemical Industries; "Aqualon KH-05", "Aqualon KH-10", and "Aqualon KH-1025" (compounds of formula (a-4-5)) manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; "Aqualon AR-10", "Aqualon AR-1025", "Aqualon AR-20", and "Aqualon AR-2020" (compounds of formula (a-4-6)) manufactured by Daiichi Kogyo Seiyaku Co., Ltd.; "Aqualon AN-10", "Aqualon AN-30", and "Aqualon AN-5065" (compounds of formula (a-4 -7) compound); "Anthox MS·2N-D" manufactured by Nippon Nyukazai Co., Ltd. (compound of formula (a-4-8)); "Anthox LMA-10", "Anthox LMA-20", and "Anthox LMA-27" manufactured by Nippon Nyukazai Co., Ltd. (compounds of formula (a-4-9) to formula (a-4-11)); "Anthox MS-60" manufactured by Nippon Nyukazai Co., Ltd. (compound of formula (a-4-12) or formula (a-4-13)); "ER-10" and "ER-20" manufactured by ADEKA Corporation, "ER-30" and "ER-40" (compounds of formula (a-4-14)); "SR-10", "SR-20", "SR-1025", "SR-2025", and "SR-3025" (compounds of formula (a-4-15)) manufactured by ADEKA; "NE-10", "NE-20", and "NE-30" (compounds of formula (a-4-16)) manufactured by ADEKA; and "SE-10N" and "SE-1025A" (compounds of formula (a-4-17)) manufactured by ADEKA.

[0068] The monomer represented by formula (a-4) may be used alone or in combination of two or more kinds.

[0069] The polymer (a1) may further contain an arbitrary repeating unit. A preferable arbitrary repeating unit is, for example, an aromatic vinyl compound unit. The aromatic vinyl compound unit refers to a repeating unit having a structure formed by polymerizing an aromatic vinyl compound. The aromatic vinyl compound refers to a compound containing an aromatic ring and a vinyl group bonded to the aromatic ring, and examples thereof include styrene, α-methylstyrene, 4-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methoxystyrene, pt-butylstyrene, pn-butylstyrene, p-tert-butoxystyrene, 2-chlorostyrene, 4-chlorostyrene, 2,4-dichlorostyrene, 1-vinylnaphthalene, divinylbenzene, 2-acetoxystyrene, 3-acetoxystyrene, 4-acetoxystyrene, 4-vinylphenylbenzoate, p-styrenesulfonic acid or an alkali metal salt thereof (sodium salt, potassium salt, etc.). The polymer (a1) containing an aromatic vinyl compound unit can be produced, for example, by a method including copolymerizing a monomer represented by formula (a-4) with an aromatic vinyl compound.

[0070] When aromatic vinyl compound units are used, the dielectric constant and dielectric loss tangent of the insulating layer can be improved. Conventionally, when a polymer containing aromatic vinyl compound units is used as an organic filler, there is a tendency that the conductor material is likely to infiltrate and the mechanical strength of the insulating layer is likely to be reduced. In contrast, when the polymer (a1) containing a group represented by formula (a-1) contains aromatic vinyl compound units, it is possible to suppress infiltration and improve mechanical strength while improving the dielectric constant and dielectric loss tangent.

[0071] The amount of aromatic vinyl compound units is preferably 30% by mass or more, more preferably 40% by mass or more, particularly preferably 50% by mass or more, and preferably 99.99% by mass or less, based on 100% by mass of the polymer (a1). When the amount of aromatic vinyl compound units is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0072] Further examples of the optional repeating unit include repeating units having a structure formed by polymerizing any of the following monomer compounds. Examples of the optional monomer compounds include (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, glycidyl (meth)acrylate, and benzyl (meth)acrylate; unsaturated carboxylic acids such as (meth)acrylic acid, maleic acid, and itaconic acid; N-substituted maleimides such as N-methylmaleimide and N-phenylmaleimide; and maleimides.

[0073] The type of any repeating unit contained in the polymer (a1) may be one type or two or more types. Therefore, any monomer compound such as an aromatic vinyl compound may be used alone or in combination of two or more types.

[0074] The specific filler (A) preferably contains a large amount of the above-mentioned polymer (a1), and may contain only the polymer (a1). The amount of the polymer (a1) is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 70% by mass or more, particularly preferably 90% by mass or more, and is usually 100% by mass or less, based on 100% by mass of the specific filler (A).

[0075] The (A) specific filler may contain an optional component in combination with the polymer (a1). The optional component other than the polymer (a1) that the (A) specific filler may contain may be, for example, an optional polymer. Examples of the optional polymer include acrylic polymers such as polymethyl(meth)acrylate, polyethyl(meth)acrylate, polypropyl(meth)acrylate, polybutyl(meth)acrylate, polycyclohexyl(meth)acrylate, and polyoctyl(meth)acrylate; and silicone polymers such as polydimethylsiloxane. The optional component may be used alone or in combination of two or more.

[0076] The amount of optional components in the (A) specific filler is preferably small. The amount of optional components that the (A) specific filler may contain is preferably 70% by mass or less, more preferably 50% by mass or less, even more preferably 30% by mass or less, particularly preferably 10% by mass or less, and may even be 0% by mass, based on 100% by mass of the (A) specific filler.

[0077] The specific filler (A) preferably contains a group represented by formula (a-1) on the surface of the particles of the specific filler (A). In particular, it is more preferable that the particulate polymer (a1) forms the particles of the specific filler (A), and the surface of the particles has a group represented by formula (a-1). When the particle surface of the specific filler (A) has a group represented by formula (a-1), the penetration of the conductive material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductive layer of the insulating layer can be generally improved.

[0078] The specific filler (A) containing a group represented by formula (a-1) on the surface of the particle can be produced, for example, by emulsion polymerization. As a specific example, in an oil-in-water suspension in which oil droplets containing a monomer are dispersed in an aqueous solvent such as water, the monomer represented by formula (a-4) and, if necessary, any monomer such as an aromatic vinyl compound are polymerized. In this polymerization, the group represented by formula (a-1) tends to be unevenly distributed at the interface between the aqueous solvent and the oil droplets, so that the specific filler (A) containing a particulate polymer containing a group represented by formula (a-1) on the surface can be produced. Therefore, from the viewpoint of easily obtaining a preferred specific filler (A), an emulsion polymer is preferred as the polymer (a1).

[0079] The particle shape of the (A) specific filler is preferably spherical. When the (A) specific filler having a spherical particle shape is used, the penetration of the conductor material into the insulating layer can be effectively suppressed, and moreover, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved. The value obtained by dividing the length of the major axis of the (A) specific filler particle by the length of the minor axis (aspect ratio) is preferably 2 or less, more preferably 1.5 or less, and even more preferably 1.2 or less. The (A) specific filler having a spherical particle shape can be produced, for example, by the above-mentioned emulsion polymerization.

[0080] The (A) specific filler may be used alone or in combination of two or more kinds.

[0081] The range of the average particle size of the (A) specific filler is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. The (A) specific filler having an average particle size in the above range can effectively suppress the penetration of the conductor material into the insulating layer, and moreover, can usually improve the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer. The lower limit of the average particle size of the (A) specific filler is not particularly limited, and can be, for example, 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, etc. The (A) specific filler having an average particle size in such a small range can be produced, for example, by the above-mentioned emulsion polymerization.

[0082] The average particle size of the (A) specific filler can be measured using a laser diffraction particle size distribution measuring device (e.g., "SALD-2100" manufactured by Shimadzu Corporation). With this measuring device, the volume average particle size can be measured as the average particle size of the (A) specific filler. The measurement can be performed by dispersing the (A) specific filler in an organic solvent that does not dissolve the (A) specific filler. As the organic solvent, a low polarity solvent or a medium polarity solvent is usually used, and toluene or tetrahydrofuran (THF) is preferably used, in order to suppress aggregation of the (A) specific filler.

[0083] The amount of the (A) specific filler is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the (A) specific filler is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0084] [(B) Curing resin] The resin composition according to the first embodiment of the present invention contains a (B) curable resin as the (B) component. The (B) curable resin does not include those corresponding to the above-mentioned (A) component. The (B) curable resin may be a thermosetting resin, a photocurable resin, or a combination of these. In addition, the curable resin may be used alone or in combination of two or more types.

[0085] Examples of the curable resin include epoxy resins, phenolic resins, active ester resins, cyanate ester resins, carbodiimide resins, acid anhydride resins, amine resins, benzoxazine resins, thiol resins, and radical polymerizable resins. One type of curable resin may be used alone, or two or more types may be used in combination.

[0086] From the viewpoint of obtaining the effect of the present invention remarkably, it is preferable to use a combination of an epoxy resin and a resin capable of reacting and bonding with the epoxy resin to harden the resin composition. The resin capable of reacting and bonding with the epoxy resin to harden the resin composition may be hereinafter referred to as a "hardening agent". Examples of the hardening agent include active ester resins, cyanate ester resins, phenolic resins, carbodiimide resins, acid anhydride resins, amine resins, benzoxazine resins, and thiol resins. Among the hardening agents, active ester resins, cyanate ester resins, phenolic resins, carbodiimide resins, and benzoxazine resins are preferred. In addition, the hardening agent may be used alone or in combination of two or more types.

[0087] The epoxy resin is a curable resin having an epoxy group. Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, isocyanurate type epoxy resins, and phenolphthalimidine type epoxy resins. The epoxy resin may be used alone or in combination of two or more kinds.

[0088] From the viewpoint of obtaining a cured product having excellent heat resistance, the epoxy resin preferably contains an aromatic structure. The aromatic structure is a chemical structure generally defined as aromatic, and includes polycyclic aromatic rings and aromatic heterocycles. Examples of epoxy resins containing an aromatic structure include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, bisxylenol type epoxy resins, glycidylamine type epoxy resins having an aromatic structure, glycidyl ester type epoxy resins having an aromatic structure, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins having an aromatic structure, epoxy resins having a butadiene structure having an aromatic structure, alicyclic epoxy resins having an aromatic structure, heterocyclic epoxy resins, spiro ring-containing epoxy resins having an aromatic structure, cyclohexane dimethanol type epoxy resins having an aromatic structure, naphthylene ether type epoxy resins, trimethylol type epoxy resins having an aromatic structure, and tetraphenylethane type epoxy resins having an aromatic structure.

[0089] The (B) curable resin preferably contains, as an epoxy resin, an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0090] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only liquid epoxy resins as the epoxy resin, or may contain only solid epoxy resins, or may contain a combination of liquid epoxy resins and solid epoxy resins.

[0091] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0092] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, and epoxy resin having a butadiene structure are preferred.

[0093] Specific examples of liquid epoxy resins include "HP-4032", "HP-4032-D", and "HP-4032-SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; and "EP-3950L" and "EP-3980" manufactured by ADEKA Corporation. S" (glycidylamine type epoxy resin); "EP-4088S" (dicyclopentadiene type epoxy resin) manufactured by ADEKA; "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel Chemical & Material Chemical Co., Ltd.; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase Chemtex Corporation; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" manufactured by Daicel Corporation, "JP-100" and "JP-200" (epoxy resin having a butadiene structure) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd. may be used alone or in combination of two or more types.

[0094] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0095] Preferred solid epoxy resins include bixylenol type epoxy resins, naphthalene type epoxy resins, naphthalene type tetrafunctional epoxy resins, naphthol novolac type epoxy resins, cresol novolac type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol type epoxy resins, biphenyl type epoxy resins, naphthylene ether type epoxy resins, anthracene type epoxy resins, bisphenol A type epoxy resins, bisphenol AF type epoxy resins, phenol aralkyl type epoxy resins, tetraphenylethane type epoxy resins, and phenolphthalimidine type epoxy resins.

[0096] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; and "EXA-7311" manufactured by DIC Corporation. , "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN475V", "ESN4 100V" (naphthalene type epoxy resin); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "Y Examples of epoxy resins include "X7700" (phenol aralkyl type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YX7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.

[0097] When a liquid epoxy resin and a solid epoxy resin are used in combination as the epoxy resin, the mass ratio thereof (liquid epoxy resin:solid epoxy resin) is preferably 20:1 to 1:20, more preferably 10:1 to 1:10, and particularly preferably 7:1 to 1:7.

[0098] The epoxy equivalent of the epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 3,000 g / eq., further preferably 80 g / eq. to 2,000 g / eq., and particularly preferably 110 g / eq. to 1,000 g / eq. The epoxy equivalent represents the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0099] The weight average molecular weight (Mw) of the epoxy resin is preferably 100 to 5,000, more preferably 250 to 3,000, and further preferably 400 to 1500. The weight average molecular weight of the epoxy resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0100] The amount of the epoxy resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the epoxy resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0101] The range of the amount of the epoxy resin is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on 100% by mass of the resin components in the resin composition. The resin components in the resin composition refer to the non-volatile components in the resin composition excluding particles such as (A) the specific filler and (C) inorganic filler described below. When the amount of the epoxy resin is within the above range, the penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0102] As the active ester resin, a compound having one or more active ester groups in one molecule can be used. Among them, as the active ester resin, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferred. When combined with an epoxy resin, the active ester resin can react with the epoxy resin to harden the resin composition, and is therefore sometimes called an "active ester curing agent." The active ester resin is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester resin obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester resin obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0103] Specifically, the active ester resin is preferably a dicyclopentadiene type active ester resin, a naphthalene type active ester resin containing a naphthalene structure, an active ester resin containing an acetylated product of phenol novolac, or an active ester resin containing a benzoylated product of phenol novolac, and more preferably at least one selected from a dicyclopentadiene type active ester resin and a naphthalene type active ester resin. As the dicyclopentadiene type active ester resin, an active ester resin containing a dicyclopentadiene type diphenol structure is preferable.

[0104] Commercially available active ester resins include, for example, active ester resins containing a dicyclopentadiene-type diphenol structure such as "EXB9451", "EXB9460", "EXB9460S", "EXB-8000L", "EXB-8000L-65M", "EXB-8000L-65TM", "HPC-8000L-65TM", "HPC-8000", "HPC-8000-65T", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); and active ester resins containing a naphthalene structure such as "HP-B-8151-62T", "EXB-8100L-65T", "EXB-8150-60T", and "EXB-815 Examples of such active ester resins include "EXB9401" (manufactured by DIC Corporation), which is a phosphorus-containing active ester resin; "DC808" (manufactured by Mitsubishi Chemical Corporation), which is an acetylated product of phenol novolac; "YLH1026", "YLH1030", "YLH1048" (manufactured by Mitsubishi Chemical Corporation), which is a benzoylated product of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Corporation), which is an active ester resin containing a styryl group and a naphthalene structure.

[0105] The amount of the active ester resin is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, and is preferably 60% by mass or less, more preferably 40% by mass or less, and even more preferably 20% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the active ester resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0106] The amount of the active ester resin is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the active ester resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0107] As the cyanate ester resin, a compound having one or more, preferably two or more, cyanate groups in one molecule can be used. When combined with an epoxy resin, the cyanate ester resin reacts with the epoxy resin to harden the resin composition, and is therefore sometimes called a "cyanate ester curing agent." Examples of the cyanate ester resin include bifunctional cyanate ester resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate ester resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate ester resins are partially converted to triazine. Specific examples of cyanate ester resins include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0108] The amount of the cyanate ester resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the cyanate ester resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0109] The amount of the cyanate ester resin is preferably 1% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the cyanate ester resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0110] As the phenolic resin, a compound having one or more, preferably two or more, hydroxyl groups (phenolic hydroxyl groups) bonded to an aromatic ring such as a benzene ring or a naphthalene ring in one molecule can be used. When combined with an epoxy resin, the phenolic resin can react with the epoxy resin to harden the resin composition, and is therefore sometimes called a "phenolic hardener." From the viewpoint of heat resistance and water resistance, a phenolic resin having a novolac structure is preferred. From the viewpoint of adhesion, a nitrogen-containing phenolic resin is preferred, and a triazine skeleton-containing phenolic resin is more preferred. Among these, a triazine skeleton-containing phenolic novolac resin is preferred from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion.

[0111] Specific examples of phenolic resins include "MEH-7700", "MEH-7810", "MEH-7851", and "MEH-8000H" manufactured by Meiwa Kasei Co., Ltd.; "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd.; and "SN-170", "SN-180", "SN-190", "SN-475", "SN-485", "SN-495", "SN-495V", and "SN- 375", "SN-395" manufactured by DIC Corporation; "TD-2090", "TD-2090-60M", "LA-7052", "LA-7054", "LA-1356", "LA-3018", "LA-3018-50P", "LA-1356", "TD2090", "TD-2090-60M" manufactured by Gun-ei Chemical Co., Ltd.; and the like.

[0112] The amount of the phenolic resin is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the phenolic resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0113] The amount of the phenolic resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the phenolic resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0114] As the carbodiimide resin, a compound having one or more, preferably two or more, carbodiimide structures in one molecule can be used. When combined with an epoxy resin, the carbodiimide resin reacts with the epoxy resin to harden the resin composition, and is therefore sometimes called a "carbodiimide curing agent." Specific examples of the carbodiimide resin include aliphatic biscarbodiimides such as tetramethylene-bis(t-butylcarbodiimide) and cyclohexane bis(methylene-t-butylcarbodiimide); aromatic biscarbodiimides such as phenylene-bis(xylylcarbodiimide); aliphatic polycarbodiimides such as polyhexamethylenecarbodiimide, polytrimethylhexamethylenecarbodiimide, polycyclohexylenecarbodiimide, poly(methylenebiscyclohexylenecarbodiimide), and poly(isophoronecarbodiimide); poly(phenylenecarbodiimide), poly(naphthalenecarbodiimide), and the like. Examples of polycarbodiimides include aromatic polycarbodiimides such as poly(methylenediphenylenecarbodiimide), poly(tolylenecarbodiimide), poly(methyldiisopropylphenylenecarbodiimide), poly(triethylphenylenecarbodiimide), poly(diethylphenylenecarbodiimide), poly(triisopropylphenylenecarbodiimide), poly(diisopropylphenylenecarbodiimide), poly(xylylenecarbodiimide), poly(tetramethylxylylenecarbodiimide), poly(methylenediphenylenecarbodiimide), and poly[methylenebis(methylphenylene)carbodiimide]. Commercially available carbodiimide resins include, for example, "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-05", "Carbodilite V-07" and "Carbodilite V-09" manufactured by Nisshinbo Chemical Inc.; and "Stavaxol P", "Stavaxol P400" and "Hi-Kasil 510" manufactured by Rhein Chemie.

[0115] The amount of the carbodiimide resin is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the carbodiimide resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0116] The amount of the carbodiimide resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the carbodiimide resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0117] As the acid anhydride resin, a compound having one or more, preferably two or more, acid anhydride groups in one molecule can be used. When combined with an epoxy group, the acid anhydride resin reacts with the epoxy resin to harden the resin composition, and is therefore sometimes called an "acid anhydride curing agent." Specific examples of the acid anhydride resin include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, and benzophenonetetracarboxylic dianhydride. Examples of acid anhydrides include anhydrides, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resin, which is a copolymer of styrene and maleic acid. Commercially available acid anhydride resins include, for example, "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd.; "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation; "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.; and "EF-30", "EF-40", "EF-60", and "EF-80" manufactured by Clay Valley Corporation.

[0118] As the amine-based resin, a compound having one or more, preferably two or more, amino groups in one molecule can be used. When combined with an epoxy group, the amine-based resin reacts with the epoxy resin to harden the resin composition, and is therefore sometimes called an "amine-based curing agent." Examples of the amine-based resin include aliphatic amines, polyether amines, alicyclic amines, and aromatic amines, and among these, aromatic amines are preferred. The amine-based resin is preferably a primary amine or secondary amine, and more preferably a primary amine. Specific examples of amine resins include 4,4'-methylenebis(2,6-dimethylaniline), 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, m-phenylenediamine, m-xylylenediamine, diethyltoluenediamine, 4,4'-diaminodiphenylether, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, and 2,2-bis(3-amino-4-hydroxyphenyl)propionate. Pan, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, bis(4-(4-aminophenoxy)phenyl)sulfone, bis(4-(3-aminophenoxy)phenyl)sulfone, and the like. Commercially available amine-based resins include, for example, "SEIKACURE-S" manufactured by Seika Corporation; "KAYABOND C-200S", "KAYABOND C-100", "KAYAHARD AA", "KAYAHARD AB", and "KAYAHARD AS" manufactured by Nippon Kayaku Co., Ltd.; "Epicure W" manufactured by Mitsubishi Chemical Corporation; and "DTDA" manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0119] As the benzoxazine resin, a compound having one or more, preferably two or more, benzoxazine rings in one molecule can be used. When combined with an epoxy resin, the benzoxazine resin reacts with the epoxy resin to harden the resin composition, and is therefore sometimes called a "benzoxazine curing agent." Specific examples of the benzoxazine resin include "JBZ-OP100D" and "ODA-BOZ" manufactured by JFE Chemical Corporation; "HFB2006M" manufactured by Showa Polymer Co., Ltd.; and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0120] The amount of the benzoxazine resin is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 0.5% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the benzoxazine resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0121] The amount of the benzoxazine resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 2% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the benzoxazine resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0122] Thiol-based resins, when combined with epoxy resins, can react with the epoxy resin to harden the resin composition, and are therefore sometimes called "thiol-based hardeners." Examples of thiol-based resins include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), and tris(3-mercaptopropyl)isocyanurate.

[0123] The active group equivalent of the curing agent is preferably 50 g / eq. to 3000 g / eq., more preferably 100 g / eq. to 1000 g / eq., further preferably 100 g / eq. to 500 g / eq., and particularly preferably 100 g / eq. to 300 g / eq. The active group equivalent represents the mass of the resin per equivalent of the active group.

[0124] In one example, the weight average molecular weight (Mw) range of the curing agent may be the same as the weight average molecular weight (Mw) range of the epoxy resin.

[0125] When the number of epoxy groups in the epoxy resin is 1, the number of active groups in the curing agent is preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.5 or more, and preferably 5.0 or less, more preferably 4.0 or less, and particularly preferably 3.0 or less. The "number of epoxy groups in the epoxy resin" refers to the total value obtained by dividing the mass of the non-volatile components of the epoxy resin present in the resin composition by the epoxy equivalent. The "number of active groups in the curing agent" refers to the total value obtained by dividing the mass of the non-volatile components of the curing agent present in the resin composition by the active group equivalent.

[0126] The amount of the curing agent is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the curing agent is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0127] The amount of the curing agent is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the curing agent is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0128] A compound having an ethylenically unsaturated bond can be used as the radical polymerizable resin. Thus, the radical polymerizable resin can have a radical polymerizable group containing an ethylenically unsaturated bond. Examples of the radical polymerizable group include unsaturated hydrocarbon groups such as vinyl group, allyl group, 1-propenyl group, 3-cyclohexenyl group, 3-cyclopentenyl group, 2-vinylphenyl group, 3-vinylphenyl group, and 4-vinylphenyl group; and α,β-unsaturated carbonyl groups such as acryloyl group, methacryloyl group, and maleimide group (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl group). The number of radical polymerizable groups contained in one molecule of the radical polymerizable resin may be one, but is preferably two or more. One type of radical polymerizable resin may be used alone, or two or more types may be used in combination. Preferred radical polymerizable resins include acrylic resins, styryl resins, allyl resins, and maleimide resins.

[0129] The acrylic resin may be a compound having one or more, preferably two or more (meth)acryloyl groups in one molecule. The acrylic resin may be a monomer or an oligomer. The term "(meth)acryloyl group" may include an acryloyl group, a methacryloyl group, and a combination thereof. Examples of the acrylic resin include cyclohexane-1,4-dimethanol di(meth)acrylate, cyclohexane-1,3-dimethanol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and the like. aliphatic (meth)acrylic acid ester compounds having a low molecular weight (molecular weight less than 1000) such as dioxane glycol di(meth)acrylate, 3,6-dioxa-1,8-octanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, glycerin tri(meth)acrylate, and pentaerythritol tetra(meth)acrylate; low molecular weight (molecular weight less than 1000) ether-containing (meth)acrylic acid ester compounds such as 3,6,9-trioxaundecane-1,11-diol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 9,9-bis[4-(2-acryloyloxyethoxy)phenyl]fluorene, ethoxylated bisphenol A di(meth)acrylate, and propoxylated bisphenol A di(meth)acrylate; low molecular weight (molecular weight less than 1000) isocyanurate-containing (meth)acrylic acid ester compounds such as tris(3-hydroxypropyl)isocyanurate tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, and ethoxylated isocyanuric acid tri(meth)acrylate; and high molecular weight (molecular weight 1000 or more) acrylic acid ester compounds such as (meth)acrylic-modified polyphenylene ether resin.Examples of commercially available acrylic resins include "A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.; "DCP" and "DCP-A" manufactured by Kyoeisha Chemical Co., Ltd.; "NPDGA", "FM-400", "R-604", "R-684", "R-687", "THE-330", "PET-30", and "DPHA" manufactured by Nippon Kayaku Co., Ltd.; and "SA9000" and "SA9000-111" manufactured by SABIC Innovative Plastics.

[0130] As the styryl resin, a compound having one or more, preferably two or more, styryl groups or vinylphenyl groups in one molecule can be used. The styryl resin may be a monomer or an oligomer. Examples of the styryl resin include low molecular weight (molecular weight less than 1000) styrene compounds such as divinylbenzene, 2,4-divinyltoluene, 2,6-divinylnaphthalene, 1,4-divinylnaphthalene, 4,4'-divinylbiphenyl, 1,2-bis(4-vinylphenyl)ethane, 2,2-bis(4-vinylphenyl)propane, and bis(4-vinylphenyl)ether; and high molecular weight (molecular weight 1000 or more) styrene compounds such as vinylbenzyl-modified polyphenylene ether resin and styrene-divinylbenzene copolymer. Examples of commercially available styryl resins include "OPE-2St", "OPE-2St 1200", and "OPE-2St 2200" manufactured by Mitsubishi Gas Chemical Company, Inc.

[0131] As the allyl resin, a compound having one or more, preferably two or more allyl groups in one molecule can be used.As the allyl resin, for example, aromatic carboxylic acid allyl ester compounds such as diallyl diphenate, triallyl trimellitate, diallyl phthalate, diallyl isophthalate, diallyl terephthalate, diallyl 2,6-naphthalenedicarboxylate, diallyl 2,3-naphthalenecarboxylate; isocyanuric acid allyl ester compounds such as 1,3,5-triallyl isocyanurate, 1,3-diallyl-5-glycidyl isocyanurate; epoxy-containing aromatic allyl compounds such as 2,2-bis[3-allyl-4-(glycidyloxy)phenyl]propane; benzoxazine-containing aromatic allyl compounds such as bis[3-allyl-4-(3,4-dihydro-2H-1,3-benzoxazin-3-yl)phenyl]methane; ether-containing aromatic allyl compounds such as 1,3,5-triallyl ether benzene; allyl silane compounds such as diallyl diphenyl silane. Commercially available allyl resins include, for example, "TAIC" (1,3,5-triallyl isocyanurate) manufactured by Nippon Kasei Chemical Industry Co., Ltd., "DAD" (diallyl diphenate) manufactured by Nisshoku Techno Fine Chemical Co., Ltd., "TRIAM-705" (triallyl trimellitate) manufactured by Wako Pure Chemical Industries, Ltd., trade name "DAND" (2,3-naphthalene carboxylate diallyl) manufactured by Nippon Distillation Industry Co., Ltd., "ALP-d" (bis[3-allyl-4-(3,4-dihydro-2H-1,3-benzoxazin-3-yl)phenyl]methane) manufactured by Shikoku Kasei Corporation, "RE-810NM" (2,2-bis[3-allyl-4-(glycidyloxy)phenyl]propane) manufactured by Nippon Kayaku Co., Ltd., and "DA-MGIC" (1,3-diallyl-5-glycidyl isocyanurate) manufactured by Shikoku Kasei Corporation.

[0132] As the maleimide resin, a compound having one or more, preferably two or more, maleimide groups (2,5-dihydro-2,5-dioxo-1H-pyrrol-1-yl groups) in one molecule can be used. The maleimide resin may be a monomer or an oligomer. Examples of commercially available maleimide resins include maleimide resins containing an aliphatic skeleton having 36 carbon atoms derived from dimer diamine, such as "BMI-3000J", "BMI-5000", "BMI-1400", "BMI-1500", "BMI-1700", and "BMI-689" (all manufactured by DigiCner Molecules); maleimide resins containing an indane skeleton, as described in the Japan Institute of Invention and Innovation Disclosure Technical Bulletin No. 2020-500211; and maleimide resins containing an aromatic ring skeleton directly bonded to the nitrogen atom of the maleimide group, such as "MIR-3000-70MT" (manufactured by Nippon Kayaku Co., Ltd.), "BMI-4000" (manufactured by Daiwa Kasei Co., Ltd.), and "BMI-80" (manufactured by Keiai Kasei Co., Ltd.).

[0133] The ethylenically unsaturated bond equivalent of the radical polymerizable resin is preferably 20 g / eq. to 3000 g / eq., more preferably 50 g / eq. to 2500 g / eq., further preferably 70 g / eq. to 2000 g / eq., and particularly preferably 90 g / eq. to 1500 g / eq. The ethylenically unsaturated bond equivalent represents the mass of the radical polymerizable resin per equivalent of the ethylenically unsaturated bond.

[0134] The weight average molecular weight (Mw) of the radical polymerizable resin is preferably 40000 or less, more preferably 10000 or less, further preferably 5000 or less, and particularly preferably 3000 or less. The lower limit is not particularly limited, but may be, for example, 150 or more. The weight average molecular weight of the radical polymerizable resin can be measured as a polystyrene-equivalent value by gel permeation chromatography (GPC).

[0135] The amount of the radical polymerizable resin is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and even more preferably 1% by mass or more, and is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the radical polymerizable resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0136] The amount of the radical polymerizable resin is preferably 0.1% by mass or more, more preferably 1% by mass or more, and even more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the radical polymerizable resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0137] Among the above, it is preferable that the (B) curable resin contains one or more selected from the group consisting of epoxy resin, phenolic resin, active ester resin, cyanate ester resin, carbodiimide resin, benzoxazine resin, allyl resin, acrylic resin, styryl resin and maleimide resin. At this time, the total amount of the resins selected from the above group is preferably 50% by mass or more, more preferably 70% by mass or more, particularly preferably 80% by mass or more, and usually 100% by mass or less, based on 100% by mass of the (B) curable resin. When the (B) curable resin contains such a preferable resin, it is possible to effectively suppress the penetration of the conductor material into the insulating layer, and moreover, it is usually possible to improve the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness and adhesion to the conductor layer of the insulating layer.

[0138] The amount of the (B) curable resin is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 20% by mass or more, and is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the (B) curable resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0139] The amount of the (B) curable resin is preferably 40% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more, and may be 99% by mass or less, or 98% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the (B) curable resin is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0140] [(C) Inorganic filler] The resin composition according to one embodiment of the present invention may contain an inorganic filler (C) as an optional component. The inorganic filler (C) as the component (C) does not include those corresponding to the above-mentioned components (A) and (B). The inorganic filler (C) is usually contained in the resin composition in the form of particles.

[0141] (C) An inorganic compound is used as the material of the inorganic filler. (C) Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica and alumina are preferred, and silica is particularly preferred. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferred as the silica. The (C) inorganic filler may be used alone or in combination of two or more kinds.

[0142] (C) Inorganic fillers can be classified into hollow inorganic fillers having voids inside and solid inorganic fillers having no voids inside. (C) Inorganic fillers may be used only with hollow inorganic fillers, only with solid inorganic fillers, or in combination with hollow inorganic fillers and solid inorganic fillers. When using hollow inorganic fillers, the dielectric constant of the cured product of the resin composition can usually be reduced.

[0143] Since the hollow inorganic filler has pores, it usually has a porosity of more than 0 volume%. From the viewpoint of lowering the relative dielectric constant of the insulating layer containing the cured product of the resin composition, the porosity of the hollow inorganic filler is preferably 5 volume% or more, more preferably 10 volume% or more, and particularly preferably 15 volume% or more. In addition, from the viewpoint of the mechanical strength of the cured product of the resin composition, the porosity of the hollow inorganic filler is preferably 95 volume% or less, more preferably 90 volume% or less, and particularly preferably 85 volume% or less.

[0144] The porosity P (volume %) of a particle is defined as the volume ratio of the total volume of one or more pores present inside the particle to the total volume of the particle based on the outer surface of the particle (total volume of pores / volume of particle). This porosity P is calculated by multiplying the measured value of the actual density D of the particle by the volume ratio of the particle. M (g / cm 3 ), and the theoretical density of the material that forms the particle D T (g / cm 3 ) can be calculated using the following formula (X1).

[0145]

number

[0146] Commercially available inorganic fillers (C) such as hollow inorganic fillers and solid inorganic fillers include, for example, "SP60-05" and "SP507-05" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", "YA010C", "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "UFP-30", "DAW-03", and "FB-105FD" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "Cellfiers" and "MGH-005" manufactured by Pacific Cement Corporation; and "Spherique" and "BA-1" manufactured by JGC Catalysts and Chemicals Co., Ltd.

[0147] From the viewpoint of significantly obtaining the desired effects of the present invention, the average particle size of the (C) inorganic filler is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 3 μm or less.

[0148] (C) The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample can be measured by using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, measuring the particle size distribution of the inorganic filler on a volume basis using a flow cell method, and calculating the average particle size as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0149] The specific surface area of ​​the (C) inorganic filler is preferably 0.1 m from the viewpoint of significantly obtaining the desired effects of the present invention. 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 / g or more, preferably 100m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of ​​the inorganic filler can be measured by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0150] (C) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. The surface treatment agent may be used alone or in any combination of two or more.

[0151] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0152] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a specific range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably with 0.2% to 3% by mass of the surface treatment agent, and even more preferably with 0.3% to 2% by mass of the surface treatment agent.

[0153] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition, it is more preferable that the content is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0154] (C) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0155] The amount of the (C) inorganic filler is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the (C) inorganic filler is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0156] [(D) Curing accelerator] The resin composition according to one embodiment of the present invention may contain a curing accelerator (D) as an optional component. The curing accelerator (D) as the component (D) does not include those corresponding to the above-mentioned components (A) to (C). The curing accelerator (D) acts as a catalyst for the reaction of the thermosetting resin (B) to accelerate the curing of the resin composition.

[0157] As the (D) curing accelerator, an appropriate one can be used depending on the type of the (B) curable resin. For example, when the (B) curable resin contains an epoxy resin, examples of the (D) curing accelerator that can accelerate the curing of the epoxy resin include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, and amine-based curing accelerators. The (D) curing accelerators may be used alone or in combination of two or more.

[0158] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogenhexahydrophthalate, tetrabutyl phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolylborate, tetraphenyl phosphonium bromide, and the like. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.

[0159] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].

[0160] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.

[0161] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct , 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, 2-phenylimidazoline, and other imidazole compounds and adducts of imidazole compounds and epoxy resins. Commercially available imidazole curing accelerators include, for example, "1B2PZ", "2E4MZ", "2MZA-PW", "2MZ-OK", "2MA-OK", "2MA-OK-PW", "2PHZ", "2PHZ-PW", "Cl1Z", "Cl1Z-CN", "Cl1Z-CNS", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd.; and "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0162] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0163] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, 1,8-diazabicyclo(5,4,0)-undecene, etc. Commercially available amine-based curing accelerators may be used, such as "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0164] The amount of the curing accelerator (D) is preferably 0.001% by mass or more, more preferably 0.005% by mass or more, and even more preferably 0.01% by mass or more, and is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. When the amount of the curing accelerator (D) is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0165] The amount of the curing accelerator (D) is preferably 0.001% by mass or more, more preferably 0.01% by mass or more, and even more preferably 0.02% by mass or more, and is preferably 5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.1% by mass or less, based on 100% by mass of the resin component in the resin composition. When the amount of the curing accelerator (D) is within the above range, penetration of the conductor material into the insulating layer can be effectively suppressed, and furthermore, the relative dielectric constant, dielectric loss tangent, mechanical strength, surface roughness, and adhesion to the conductor layer of the insulating layer can usually be improved.

[0166] [(E) Polymer] The resin composition according to one embodiment of the present invention may contain a (E) polymer as an optional component. The (E) polymer as the (E) component does not include those corresponding to the above-mentioned (A) to (D) components. The (E) polymer may be used alone or in combination of two or more types. The (E) polymer is usually included in the resin composition and its cured product in a compatible manner with resin components other than the (E) polymer.

[0167] The (E) polymer usually has a large molecular weight. Specifically, the weight average molecular weight Mw of the (E) polymer is preferably greater than 5000, more preferably 8000 or more, even more preferably 10000 or more, particularly preferably 20000 or more, and preferably 100000 or less, more preferably 70000 or less, even more preferably 60000 or less, particularly preferably 50000 or less. The weight average molecular weight Mw of the (E) polymer is the weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).

[0168] Examples of the (E) polymer include phenoxy resins, polyimide resins, polyvinyl acetal resins, polyolefin resins, polybutadiene resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyetheretherketone resins, polyester resins, etc. Among these, phenoxy resins and polyimide resins are preferred.

[0169] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. Specific examples of phenoxy resins include "1256" and "4250" manufactured by Mitsubishi Chemical Corporation (both of which are phenoxy resins containing a bisphenol A skeleton); "YX8100" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol S skeleton); "YX6954" manufactured by Mitsubishi Chemical Corporation (phenoxy resin containing a bisphenol acetophenone skeleton); "FX280" and "FX293" manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", "YL7482", and "YL7891BH30" manufactured by Mitsubishi Chemical Corporation.

[0170] The polyimide resin refers to a resin containing a repeating unit containing an imide bond. Usually, the polyimide resin contains a repeating unit having a structure obtained by reacting a diamine compound with an acid anhydride (imidization reaction).

[0171] Examples of the diamine compound include aliphatic diamine compounds and aromatic diamine compounds, and among these, aromatic diamine compounds are preferred. Examples of the aromatic diamine compound include phenylenediamine compounds, naphthalenediamine compounds, and dianiline compounds, and among these, dianiline compounds are preferred.

[0172] The dianiline compound refers to a compound containing two aniline structures in the molecule. Each of the benzene rings in the aniline structure may have 1 to 3 optional substituents. The two aniline structures in the dianiline compound may be directly bonded to each other, or may be bonded to each other via a linker structure having 1 to 100 skeletal atoms selected from the group consisting of carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms.

[0173] Specific examples of the "linker structure" in the dianiline compound include -NHCO-, -CONH-, -OCO-, -COO-, -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -CH=CH-, -O-, -S-, -CO-, -SO2-, -NH-, Examples of the aryl group include -Ph-, -Ph-Ph-, -C(CH3)2-Ph-C(CH3)2-, -O-Ph-O-, -O-Ph-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, -Ph-CO-O-Ph-, -C(CH3)2-Ph-C(CH3)2-, a group represented by the following formula (e-1), a group represented by (e-2), and a group consisting of a combination thereof. In this specification, "Ph" represents a 1,4-phenylene group, a 1,3-phenylene group, or a 1,2-phenylene group, unless otherwise specified. In formulas (e-1) and (e-2), "*" represents a bond.

[0174] [ka]

[0175] Examples of the dianiline compound include 4,4'-diamino-2,2'-ditrifluoromethyl-1,1'-biphenyl, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfide, 4-aminophenyl 4-aminobenzoate, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis(4-aminophenyl)propane, 4,4'-(hexafluoroisopropylidene)dianiline, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, [4-(4-aminophenoxy)phenyl]hexafluoropropane, α,α-bis[4-(4-aminophenoxy)phenyl]-1,3-diisopropylbenzene, α,α-bis[4-(4-aminophenoxy)phenyl]-1,4-diisopropylbenzene, 4,4'-(9-fluorenylidene)dianiline, 2,2-bis(3-methyl-4-aminophenyl)propane, 2,2-bis(3-methyl-4-aminophenyl)benzene, 4,4'-diamino-3,3'-dimethyl-1,1'-biphenyl, 4,4'-diamino-2,2'-dimethyl-1,1'-biphenyl, 9,9'-bis(3-methyl-4-aminophenyl)fluorene, 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane, and the like. The diamine compound may be used alone or in combination of two or more kinds.

[0176] As the acid anhydride, an acid dianhydride can usually be used, and an aromatic tetracarboxylic dianhydride is preferable. Examples of the aromatic tetracarboxylic dianhydride include benzenetetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, anthracenetetracarboxylic dianhydride, and diphthalic dianhydride, and diphthalic dianhydride is preferable.

[0177] Diphthalic dianhydride refers to a compound containing two phthalic anhydride structures in the molecule. Each of the benzene rings in the phthalic anhydride structures may have 1 to 3 optional substituents. The two phthalic anhydride structures in the diphthalic dianhydride may be directly bonded to each other, or may be bonded to each other via a linker structure having 1 to 100 skeletal atoms selected from the group consisting of carbon atoms, oxygen atoms, sulfur atoms, and nitrogen atoms.

[0178] An example of a "linker structure" in diphthalic dianhydride is -[R e -Ph] me -R e -[Ph-R e ] ne In this formula, R e each independently represents a single bond, -(substituted or unsubstituted alkylene group)-, -O-, -S-, -CO-, -SO2-, -CONH-, -NHCO-, -COO-, or -OCO-; me and ne each independently represent an integer of 0 to 2 (preferably 0 or 1). Specific examples of the linker structure include -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH2CH2CH2-, -CH2CH2CH2CH2CH2-, -CH(CH3)-, -C(CH3)2-, -O-, -CO-, -SO2-, -Ph-, -O-Ph-O-, -O-Ph-SO2-Ph-O-, -O-Ph-C(CH3)2-Ph-O-, and the like.

[0179] Examples of diphthalic dianhydrides include 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride, 3,3',4,4'-biphenyl tetracarboxylic dianhydride, 2,2',3,3'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-biphenyl tetracarboxylic dianhydride, 2,3,3',4'-benzophenone tetracarboxylic dianhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 2,3,3',4'-diphenyl sulfone tetracarboxylic dianhydride, 2,2'-bis(3,4-dicarboxyphenoxyphenyl)sulfone dianhydride, methylene-4,4'-diphthalic dianhydride, 1,1-ethynylidene-4,4'-diphthalic Dianhydride, 2,2-propylidene-4,4'-diphthalic dianhydride, 1,2-ethylene-4,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenyl)benzene dianhydride Examples of the acid anhydride include 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 4,4'-(4,4'-isopropylidenediphenoxy)bisphthalic dianhydride, etc. One type of acid anhydride may be used alone, or two or more types may be used in combination.

[0180] The polyimide resin can be produced by a conventional method. For example, the polyimide resin may be produced by a method including heating a mixture of a diamine compound, an acid anhydride, and a solvent to cause a reaction. Alternatively, a commercially available product may be used as the polyimide resin. Specific examples of commercially available polyimide resins include "SLK-6100" manufactured by Shin-Etsu Chemical Co., Ltd., "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd.

[0181] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd.; S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0182] Examples of polyolefin resins include ethylene-based copolymer resins such as low-density polyethylene, very low-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-ethyl acrylate copolymer, and ethylene-methyl acrylate copolymer; and polyolefin polymers such as polypropylene and ethylene-propylene block copolymer.

[0183] Examples of polybutadiene resins include hydrogenated polybutadiene skeleton-containing resins, hydroxy group-containing polybutadiene resins, phenolic hydroxy group-containing polybutadiene resins, carboxy group-containing polybutadiene resins, acid anhydride group-containing polybutadiene resins, epoxy group-containing polybutadiene resins, isocyanate group-containing polybutadiene resins, urethane group-containing polybutadiene resins, polyphenylene ether-polybutadiene resins, and the like.

[0184] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.

[0185] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0186] A specific example of the polyphenylene ether resin is "NORYL SA90" manufactured by SABIC.

[0187] Examples of polycarbonate resins include hydroxyl group-containing carbonate resins, phenolic hydroxyl group-containing carbonate resins, carboxyl group-containing carbonate resins, acid anhydride group-containing carbonate resins, isocyanate group-containing carbonate resins, urethane group-containing carbonate resins, etc. Specific examples of polycarbonate resins include "FPC0220" manufactured by Mitsubishi Gas Chemical Company, "T6002" and "T6001" (polycarbonate diols) manufactured by Asahi Kasei Chemicals Corporation, and "C-1090", "C-2090", and "C-3090" (polycarbonate diols) manufactured by Kuraray Co., Ltd.

[0188] A specific example of the polyether ether ketone resin is "Sumiploy K" manufactured by Sumitomo Chemical Co., Ltd.

[0189] Examples of polyester resins include polyethylene terephthalate resins, polyethylene naphthalate resins, polybutylene terephthalate resins, polybutylene naphthalate resins, polytrimethylene terephthalate resins, polytrimethylene naphthalate resins, and polycyclohexane dimethyl terephthalate resins.

[0190] The amount of the (E) polymer in the resin composition is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more, based on 100 mass% of the non-volatile components of the resin composition, and is preferably 30 mass% or less, more preferably 20 mass% or less, and even more preferably 10 mass% or less.

[0191] The amount of the (E) polymer in the resin composition is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more, based on 100 mass% of the resin components of the resin composition, and is preferably 50 mass% or less, more preferably 40 mass% or less, and even more preferably 30 mass% or less.

[0192] [(F) Optional Additives] The resin composition according to one embodiment of the present invention may contain an optional additive (F) as an optional component. The optional additive (F) as the component (F) does not include those corresponding to the above-mentioned components (A) to (E). The optional additive (F) may be, for example, a radical polymerization initiator such as a peroxide radical polymerization initiator or an azo radical polymerization initiator; an organometallic compound such as an organocopper compound, an organozinc compound, or an organocobalt compound; a colorant such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, or carbon black; a polymerization inhibitor such as hydroquinone, catechol, pyrogallol, or phenothiazine; a leveling agent such as a silicone leveling agent or an acrylic polymer leveling agent; a thickener such as bentone or montmorillonite; an antifoaming agent such as a silicone antifoaming agent, an acrylic antifoaming agent, a fluorine antifoaming agent, or a vinyl resin antifoaming agent; an ultraviolet absorbing agent such as a benzotriazole ultraviolet absorbing agent; an adhesion improver such as urea silane; a triazole adhesion imparting agent, a tetrazo Examples of the additives include adhesion promoters such as phenol-based adhesion promoters and triazine-based adhesion promoters; antioxidants such as hindered phenol-based antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; flame retardants such as phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus), nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate ester-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. (F) Optional additives may be used alone or in combination of two or more.

[0193] [(G) Solvent] The resin composition according to one embodiment of the present invention may further contain a (G) solvent as an optional volatile component in combination with the non-volatile components such as the above-mentioned components (A) to (F). As the (G) solvent, an organic solvent is usually used. Examples of the organic solvent include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, and methyl methoxypropionate. Examples of the solvent include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The (G) solvent may be used alone or in combination of two or more.

[0194] The amount of (G) solvent is not particularly limited, but when all components in the resin composition are taken as 100 mass%, it can be, for example, 60 mass% or less, 40 mass% or less, 30 mass% or less, 20 mass% or less, 15 mass% or less, 10 mass% or less, or it can be 0 mass%.

[0195] [Method of producing resin composition] The resin composition according to one embodiment of the present invention can be produced, for example, by mixing components that can be included in the resin composition. The above-mentioned components may be mixed in part or in whole at the same time, or may be mixed in order. In the process of mixing each component, the temperature may be appropriately set, and thus heating and / or cooling may be performed temporarily or throughout. In addition, stirring or shaking may be performed in the process of mixing each component.

[0196] [Characteristics of resin composition] A cured product is obtained by curing the resin composition according to one embodiment of the present invention. During the curing, heat is usually applied to the resin composition. Thus, among the components contained in the resin composition, volatile components such as (G) solvent can be volatilized by heat during curing, but non-volatile components such as components (A) to (F) do not volatilize by heat during curing. Thus, the cured product of the resin composition can contain the non-volatile components of the resin composition or their reaction products.

[0197] When a cured layer is formed by the cured product of the resin composition according to this embodiment and a conductor layer is formed on the cured layer by electroless plating, the infiltration of the conductor material into the cured layer can be suppressed. Therefore, according to the resin composition according to this embodiment, an insulating layer can be formed as a cured layer that can suppress the infiltration of the conductor material. In one example, an evaluation board B having a patterned conductor layer having a comb-tooth pattern with a predetermined line / space ratio is manufactured on an insulating layer containing a cured product of the resin composition by a method described in the examples described later. The "line" represents the wiring width of the conductor layer, and the "space" represents the distance between the wirings. In this case, even if the line / space ratio of the comb-tooth pattern is preferably 20 μm / 20 μm or less, more preferably 18 μm or less / 18 μm or less, and even more preferably 15 μm / 15 μm or less, the occurrence of conduction between the patterned conductor layers (wiring) due to the infiltration of the plating can be suppressed. The conduction can be confirmed by processing the cross section of the evaluation board B using FIB (focused ion beam) in the part where the patterned conductor layer is formed and observing the cross section.

[0198] The cured product of the resin composition according to this embodiment can usually have a low relative dielectric constant Dk. Therefore, according to the resin composition according to this embodiment, an insulating layer with a low relative dielectric constant Dk can be formed. In one example, the relative dielectric constant Dk of the cured product of the resin composition is preferably 4.0 or less, more preferably 3.8 or less, and particularly preferably 3.5 or less. There is no particular limit to the lower limit, and it can be, for example, 0.1 or more.

[0199] The cured product of the resin composition according to this embodiment can usually have a low dielectric loss tangent Df. Therefore, according to the resin composition according to this embodiment, an insulating layer with a low dielectric loss tangent Df can be formed. In one example, the dielectric loss tangent Df of the cured product of the resin composition is preferably 0.030 or less, more preferably 0.020 or less, and even more preferably 0.010 or less. There is no particular limit to the lower limit, and it can be, for example, 0.0001 or more.

[0200] The dielectric constant Dk and dielectric loss tangent Df of the cured product can be measured by a cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23° C. When the sample is a resin composition before curing, the resin composition is cured under curing conditions of 200° C. and 90 minutes to obtain a cured product, and the dielectric constant Dk and dielectric loss tangent Df of the cured product can be measured. As a specific measurement method, the method described in the Examples can be adopted.

[0201] The cured product of the resin composition according to the present embodiment can usually have high mechanical strength, for example, a large elongation at break. Therefore, according to the resin composition according to the present embodiment, an insulating layer with a large elongation at break can be formed. In one example, the elongation at break of the cured product of the resin composition is preferably 1.0% or more, more preferably 1.1% or more, and even more preferably 1.2% or more. There is no particular upper limit, and it can be, for example, 5.0% or less. The elongation at break of the cured product can be measured at 23°C in accordance with the Japanese Industrial Standard JIS K7127. When the sample is a resin composition before curing, the resin composition is cured under the curing conditions of 200°C and 90 minutes to obtain a cured product, and the elongation at break of the cured product can be measured. As a specific measurement method, the method described in the examples can be adopted.

[0202] The cured product of the resin composition according to this embodiment can usually have a small surface roughness when roughened. Therefore, according to the resin composition according to this embodiment, an insulating layer with a small surface roughness can be formed. In one example, an insulating layer containing a cured product of the resin composition is formed by a method described in the examples below, and the insulating layer is roughened to produce an evaluation substrate A. In this case, the arithmetic mean roughness Ra of the roughened surface (roughened surface) of the insulating layer can be reduced. The specific range of the arithmetic mean roughness Ra is preferably 180 nm or less, more preferably 150 nm or less, and even more preferably 130 nm or less. The lower limit can be, for example, 20 nm or more, 40 nm or more, etc. The arithmetic mean roughness Ra of the roughened surface of the insulating layer can be measured using a non-contact surface roughness meter (WYKO NT3300 manufactured by Beco Instruments). The specific measurement method can be the method described in the examples.

[0203] When a cured layer is formed by the cured product of the resin composition according to this embodiment and a conductor layer is formed on the cured layer by plating, high adhesion between the cured layer and the conductor layer can usually be obtained. Therefore, according to the resin composition according to this embodiment, an insulating layer having excellent adhesion to the conductor layer can be formed. The adhesion can be evaluated by the peel strength [kgf / cm] as the load required to peel the conductor layer from the insulating layer. Specifically, the higher the peel strength, the better the adhesion.

[0204] In one example, an evaluation substrate B having a conductor layer on an insulating layer containing a cured product of a resin composition is manufactured by the method described in the Examples below. In this case, the peel strength of the conductor layer is preferably 0.39 kgf / cm or more, more preferably 0.40 kgf / cm or more, and even more preferably 0.41 kgf / cm or more. The peel strength can be measured by forming a cut surrounding a portion of the conductor layer having a width of 10 mm and a length of 100 mm, gripping one end of this portion with a gripper, and pulling it vertically at a speed of 50 mm / min at 25°C to peel it off. The measurement can be performed in accordance with Japanese Industrial Standard JIS C6481. The specific measurement method can be the method described in the Examples.

[0205] The cured product of the resin composition according to this embodiment is usually excellent in crack resistance because the specific filler (A) can relieve stress. Therefore, according to the resin composition according to this embodiment, an insulating layer having excellent crack resistance can be formed. In one example, an insulating layer is formed on a circuit board having a conductor layer on the surface of which a wiring pattern is formed, and a roughening treatment is performed by the method described in the examples below, and the yield is obtained. In this case, the yield can be increased. The specific range of the yield is preferably 40% or more, more preferably 60% or more, and even more preferably 80% or more.

[0206] [Applications of resin composition] The resin composition according to one embodiment of the present invention can be used as a resin composition for insulating purposes, and can be particularly preferably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer). For example, the resin composition according to this embodiment can be preferably used as a resin composition for forming an insulating layer of a semiconductor chip package (resin composition for insulating layer of a semiconductor chip package) and a resin composition for forming an insulating layer of a circuit board (including a printed wiring board) (resin composition for insulating layer of a circuit board). In particular, the resin composition is suitable for forming an interlayer insulating layer provided between conductor layers.

[0207] Examples of semiconductor chip packages include FC-CSP, MIS-BGA package, ETS-BGA package, Fan-out type WLP (Wafer Level Package), Fan-in type WLP, Fan-out type PLP (Panel Level Package), and Fan-in type PLP.

[0208] The resin composition may also be used as an underfill material, for example, as a material for MUF (Molding Under Filling) that is used after a semiconductor chip is connected to a substrate.

[0209] Furthermore, the resin composition can be used in a wide range of applications in which resin compositions are used, such as sheet-like laminate materials such as resin sheets and prepregs, solder resists, die bonding materials, semiconductor encapsulating materials, hole filling resins, and component embedding resins.

[0210] [Sheet-type laminated material] The resin composition according to the present embodiment may be used by being applied in the form of a varnish, but from an industrial perspective, it is preferable to use the resin composition in the form of a sheet-like laminate material containing the resin composition.

[0211] As the sheet-like laminate material, the following resin sheets and prepregs are preferred.

[0212] In one embodiment, the resin sheet includes a support and a resin composition layer formed on the support. The resin composition layer includes a resin composition, and preferably includes only the resin composition.

[0213] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of thinning and of being able to provide a cured product having excellent insulation even if it is thin, by using the resin composition. The lower limit of the thickness of the resin composition layer is not particularly limited, but may be 5 μm or more, 10 μm or more, etc.

[0214] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0215] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0216] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0217] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0218] As the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0219] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0220] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, it is possible to suppress adhesion of dirt and scratches on the surface of the resin composition layer.

[0221] The resin sheet can be produced, for example, by preparing a liquid (varnish-like) resin composition as is or by dissolving the resin composition in a solvent to prepare a liquid (varnish-like) resin composition, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.

[0222] The solvent may be the same as the solvent explained as a component of the resin composition. The solvent may be used alone or in combination of two or more.

[0223] Drying may be performed by heating, blowing hot air, or the like. Drying conditions are not particularly limited, but drying is performed so that the content of the solvent in the resin composition layer is usually 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the solvent in the resin composition, for example, when a resin composition containing 30% by mass to 60% by mass of a solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0224] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it is usually possible to use the resin sheet by peeling off the protective film.

[0225] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with a resin composition.

[0226] The sheet-like fiber substrate used for the prepreg may be, for example, a commonly used substrate for prepreg, such as glass cloth, aramid nonwoven fabric, or liquid crystal polymer nonwoven fabric. From the viewpoint of thinning, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited, and is usually 10 μm or more.

[0227] The prepreg can be produced by a method such as a hot melt method or a solvent method.

[0228] The thickness of the prepreg can be in the same range as that of the resin composition layer in the resin sheet described above.

[0229] The sheet-like laminate material can be suitably used, for example, to form an insulating layer in the manufacture of a semiconductor chip package (insulating sheet-like laminate material for semiconductor chip package). Applicable semiconductor chip packages include, for example, fan-out type WLP, fan-in type WLP, fan-out type PLP, fan-in type PLP, etc. The sheet-like laminate material can also be used, for example, to form an insulating layer of a circuit board (insulating layer sheet-like laminate material for circuit board). Furthermore, the sheet-like laminate material may be used as a material for a MUF used after connecting a semiconductor chip to a substrate. In particular, the sheet-like laminate material is suitable for forming an interlayer insulating layer.

[0230] [Circuit board] A circuit board according to one embodiment of the present invention includes a cured product of a resin composition. Usually, the circuit board includes an insulating layer formed of the cured product of the resin composition. The insulating layer includes the cured product of the above-mentioned resin composition, and preferably includes only the cured product of the above-mentioned resin composition. This circuit board can be manufactured, for example, by a manufacturing method including the following steps (I) and (II). (I) A step of forming a resin composition layer on an inner layer substrate. (II) A step of curing the resin composition layer to form an insulating layer.

[0231] The "inner layer substrate" used in step (I) is a member that serves as the base material of a circuit board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a circuit substrate is also included in the above-mentioned "inner layer substrate". When the circuit substrate is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0232] The resin composition layer can be formed on the inner layer substrate by, for example, laminating the inner layer substrate and the resin sheet. The inner layer substrate and the resin sheet can be laminated by, for example, thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression bonding member through an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate, rather than directly pressing the resin sheet with the thermocompression bonding member.

[0233] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.

[0234] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0235] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0236] The support may be removed between step (I) and step (II) or after step (II).

[0237] In step (II), the resin composition layer is cured to form an insulating layer made of a cured product of the resin composition. The resin composition layer can be cured by a method suitable for the resin composition, such as thermal curing or photocuring. Specific curing conditions for the resin composition layer may be the conditions usually adopted when forming an insulating layer for a circuit board.

[0238] When a thermosetting resin composition is used, the curing of the resin composition may proceed as heat curing. Therefore, in this case, step (II) may include heat curing the resin composition layer. The heat curing conditions of the resin composition layer may vary depending on the type of resin composition. For example, the curing temperature is preferably 120°C to 240°C, more preferably 150°C to 220°C, and even more preferably 170°C to 210°C. The curing time may be preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0239] In addition, when the resin composition layer is thermally cured, the method for producing a circuit board preferably includes preheating the resin composition layer at a temperature lower than the curing temperature before the thermal curing. For example, prior to thermal curing of the resin composition layer, the resin composition layer may be preheated at a temperature of usually 50° C. to 150° C., preferably 60° C. to 140° C., more preferably 70° C. to 130° C. for usually 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.

[0240] On the other hand, when a photocurable resin composition is used, the curing of the resin composition may proceed as photocuring. In this case, therefore, step (II) may include photocuring the resin composition layer. The photocuring conditions of the resin composition may vary depending on the type of resin composition. For example, the resin composition layer in the irradiated area may be photocured by exposure treatment in which the resin composition layer is irradiated with actinic rays. Examples of actinic rays include ultraviolet rays, visible rays, electron beams, X-rays, etc., and ultraviolet rays are particularly preferred. The irradiation dose of ultraviolet rays is, for example, 10 mJ / cm. 2~1000mJ / cm 2 When a resin sheet having a support is used, exposure may be performed through the support, or after the support is peeled off.

[0241] In the exposure treatment, the resin composition layer may be irradiated with active light through a mask having a pattern formed thereon. Exposure methods using a mask include a contact exposure method in which exposure is performed by contacting a mask with a workpiece, and a non-contact exposure method in which exposure is performed using parallel light without contact, and either method may be used.

[0242] Step (II) may include carrying out a development treatment after the exposure treatment. According to the development treatment, the part not photocured (unexposed part) can be removed to form a pattern in the insulating layer. The development is usually carried out by wet development. In the wet development, a developer that is safe, stable, and easy to operate, such as an alkaline aqueous solution, a water-based developer, or an organic solvent, is used. Among them, a development step using an alkaline aqueous solution is preferred. As the development method, for example, a method such as spraying, swing immersion, brushing, or scraping can be adopted.

[0243] Furthermore, in the case where the resin composition layer is photocured, a post-baking treatment may be carried out as necessary after photocuring and development. Examples of the post-baking treatment include ultraviolet irradiation treatment using a high-pressure mercury lamp and heating treatment using a clean oven. The ultraviolet irradiation treatment is carried out at a dose of, for example, 0.05 J / cm. 2 ~10J / cm 2 The heat treatment can be carried out, for example, at a temperature of preferably 150° C. to 250° C. for 20 minutes to 180 minutes, and more preferably at a temperature of 160° C. to 230° C. for 30 minutes to 120 minutes.

[0244] In producing a circuit board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art that are used in producing circuit boards. When the support is removed after step (II), the removal of the support may be carried out between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). If necessary, the formation of the insulating layer and the conductor layer in steps (I) to (V) may be repeated to form a circuit board having a multilayer structure such as a multilayer printed wiring board.

[0245] In another embodiment, the circuit board can be manufactured using the above-mentioned prepreg. The manufacturing method using the prepreg can be basically the same as that using the resin sheet.

[0246] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The size and shape of the hole may be appropriately determined depending on the design of the circuit board.

[0247] Step (IV) is a step of roughening the insulating layer. Usually, in this step (IV), smears are also removed. Therefore, the roughening treatment is sometimes called "desmear treatment". The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a circuit board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.

[0248] Examples of the swelling liquid used in the roughening treatment include an alkaline solution and a surfactant solution, and an alkaline solution is preferred. As the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferred. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using a swelling liquid can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferred to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.

[0249] An example of an oxidizing agent used in the roughening treatment is an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.

[0250] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securigant P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.

[0251] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0252] The conductor layer may be a single-layer structure, or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0253] When patterning the conductor layer, it is preferable that the minimum line / space ratio of the conductor layer is small in order to utilize the advantage of being able to suppress the penetration of the conductor material. The range of the minimum line / space ratio is preferably 20 μm / 20 μm or less (i.e., pitch is 40 μm or less), more preferably 18 μm / 18 μm or less, and even more preferably 15 μm / 15 μm or less. The lower limit may be, for example, 0.5 μm / 0.5 μm or more. The pitch may be uniform or non-uniform throughout the conductor layer. The minimum pitch of the conductor layer may be, for example, 40 μm or less, 36 μm or less, or 30 μm or less.

[0254] The thickness of the conductor layer depends on the desired design of the circuit board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0255] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method. From the viewpoint of ease of production, the semi-additive method is preferred. Below, an example of forming the conductor layer by the semi-additive method is shown.

[0256] First, an electroless plating layer (plating seed layer) is formed on the surface of the insulating layer by electroless plating. Next, a mask pattern is formed on the formed electroless plating layer to expose a part of the electroless plating layer corresponding to a desired wiring pattern. After forming an electrolytic plating layer on the exposed electroless plating layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary electroless plating layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0257] [Semiconductor chip package] A semiconductor chip package according to an embodiment of the present invention includes a cured resin composition. Typically, the semiconductor chip package includes an insulating layer formed of the cured resin composition. The insulating layer includes the cured resin composition described above, and preferably includes only the cured resin composition described above. Examples of this semiconductor chip package include the following.

[0258] The semiconductor chip package according to the first example includes the above-mentioned circuit board and a semiconductor chip mounted on the circuit board. This semiconductor chip package can be manufactured by bonding the semiconductor chip to the circuit board.

[0259] The bonding conditions between the circuit board and the semiconductor chip may be any conditions that allow conductive connection between the terminal electrodes of the semiconductor chip and the circuit wiring of the circuit board. For example, the conditions used in flip-chip mounting of the semiconductor chip may be used. Also, for example, the semiconductor chip and the circuit board may be bonded via an insulating adhesive.

[0260] An example of a bonding method is a method of bonding a semiconductor chip to a circuit board. The bonding conditions are that the bonding temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and the bonding time is usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).

[0261] Another example of the bonding method is a method of bonding a semiconductor chip to a circuit board by reflow. The reflow conditions may be in the range of 120°C to 300°C.

[0262] After the semiconductor chip is bonded to the circuit board, the semiconductor chip may be filled with a molded underfill material, which may be the resin composition described above.

[0263] The semiconductor chip package according to the second example includes a semiconductor chip and an insulating layer formed of a cured product of a resin composition. Examples of the semiconductor chip package according to the second example include a fan-out type WLP and a fan-out type PLP. As a specific example, the semiconductor chip package may include a semiconductor chip; a sealing layer formed so as to cover the periphery of the semiconductor chip; a rewiring formation layer as an insulating layer provided on the surface of the semiconductor chip opposite to the sealing layer; a rewiring layer as a conductor layer; a solder resist layer; and a bump.

[0264] A method for manufacturing such a semiconductor chip package includes, for example: (A) a step of laminating a temporary fixing film on a substrate; (B) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (C) forming an encapsulation layer on the semiconductor chip; (D) peeling the substrate and the temporary fixing film from the semiconductor chip; (E) a step of forming a rewiring formation layer on the surface from which the substrate and the temporary fixing film of the semiconductor chip have been peeled off; (F) forming a rewiring layer as a conductor layer on the rewiring formation layer; and (G) forming a solder resist layer on the rewiring layer; The method for manufacturing the semiconductor chip package further comprises: (H) A process of dicing and separating multiple semiconductor chip packages into individual semiconductor chip packages. may also include

[0265] (Process (A)) Step (A) is a step of laminating a temporary fixing film on a substrate. The lamination conditions for the substrate and the temporary fixing film can be the same as the lamination conditions for the substrate and the resin sheet in the method for producing a circuit board.

[0266] Examples of the substrate include silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; and substrates made of bismaleimide triazine resins such as BT resin.

[0267] The temporary fixing film may be made of any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. Commercially available products include "Riva Alpha" manufactured by Nitto Denko Corporation.

[0268] (Process (B)) Step (B) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor chip packages to be produced, etc. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.

[0269] (Process (C)) Step (C) is a step of forming an encapsulating layer on the semiconductor chip. The encapsulating layer can be formed, for example, from a photosensitive resin composition or a thermosetting resin composition. This encapsulating layer may be formed from a cured product of the resin composition according to the above-mentioned embodiment. The encapsulating layer can usually be formed by a method including a step of forming a resin composition layer on the semiconductor chip and a step of curing this resin composition layer to form the encapsulating layer.

[0270] (Process (D)) Step (D) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable to adopt an appropriate peeling method according to the material of the temporary fixing film. For example, the peeling method may be a method of heating, foaming or expanding the temporary fixing film to peel it off. In addition, for example, the peeling method may be a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off.

[0271] When the base material and the temporary fixing film are peeled off from the semiconductor chip as described above, the surface of the encapsulating layer is exposed. The manufacturing method of the semiconductor chip package may include polishing the exposed surface of the encapsulating layer. By polishing, the smoothness of the surface of the encapsulating layer can be improved.

[0272] (Process (E)) Step (E) is a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film are peeled off. Usually, this rewiring formation layer is formed on the semiconductor chip and the sealing layer. The rewiring formation layer can be formed by a cured product of the resin composition according to the above-mentioned embodiment. Usually, the rewiring formation layer can be formed by a method including a step of forming a resin composition layer on the semiconductor chip and a step of curing the resin composition layer to form the rewiring formation layer. The formation of the resin composition layer on the semiconductor chip can be performed by the same method as the method of forming the resin composition layer on the inner layer substrate described in the above-mentioned method for producing a circuit board, except that a semiconductor chip is used instead of the inner layer substrate.

[0273] After forming a resin composition layer on a semiconductor chip, the resin composition layer is cured to obtain a rewiring formation layer as an insulating layer containing a cured product of the resin composition. The curing conditions of the resin composition layer may be the same as the curing conditions of the resin composition layer in the manufacturing method of a circuit board. When the resin composition layer is thermally cured, the resin composition layer may be subjected to a preheating treatment in which the resin composition layer is heated at a temperature lower than the curing temperature before the thermal curing. The treatment conditions of this preheating treatment may be the same as the preheating treatment in the manufacturing method of a circuit board. Usually, after forming the rewiring formation layer, holes are formed in the rewiring formation layer to connect the semiconductor chip and the rewiring layer.

[0274] (Process (F)) Step (F) is a step of forming a rewiring layer as a conductor layer on the rewiring formation layer. The method of forming the rewiring layer on the rewiring formation layer can be the same as the method of forming a conductor layer on an insulating layer in the manufacturing method of a circuit board. Steps (E) and (F) may be repeated to alternately stack (build up) the rewiring layers and the rewiring formation layers.

[0275] (Process (G)) Step (G) is a step of forming a solder resist layer on the rewiring layer. Any material having insulating properties can be used as the material of the solder resist layer. Among them, from the viewpoint of ease of manufacturing the semiconductor chip package, a photosensitive resin composition and a thermosetting resin composition are preferable. The solder resist layer may be formed by a cured product of the resin composition according to the above-mentioned embodiment.

[0276] In step (G), bumping processing may be performed to form bumps, if necessary. The bumping processing may be performed by a method such as solder balls or solder plating. In addition, the formation of via holes in the bumping processing may be performed in the same manner as in step (E).

[0277] (Process (H)) The method for manufacturing a semiconductor chip package may include a step (H) in addition to the steps (A) to (G). The step (H) is a step of dicing a plurality of semiconductor chip packages into individual semiconductor chip packages to separate them. The method for dicing the semiconductor chip packages into individual semiconductor chip packages is not particularly limited.

[0278] [Semiconductor Devices] The semiconductor device includes the above-mentioned circuit board or semiconductor chip package. Examples of the semiconductor device include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, televisions, etc.) and vehicles (e.g., motorcycles, automobiles, trains, ships, aircraft, etc.). EXAMPLES

[0279] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (25°C) and atmospheric pressure (1 atm). In addition, unless otherwise specified, "MEK" stands for methyl ethyl ketone.

[0280] <Production Example 1: Production of Fine Particles A> 97.0 parts of styrene, 1.0 part of divinylbenzene, 2.0 parts of acrylic acid, 1.0 part of a polyoxyethylene styrenated propynyl phenyl ether reactive surfactant ("Aqualon AN-5065", formula (a-4-7) manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 39.7 parts of ion-exchanged water were mixed and stirred to obtain an emulsion.

[0281] In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, 96.5 parts of ion-exchanged water and 3.0% of the above-mentioned emulsion were added. After the internal temperature of the reaction vessel was raised to 70°C and sufficiently replaced with nitrogen, 5.7 parts of a 2.5% aqueous solution of potassium persulfate was added as an initiator to start polymerization. The internal temperature was raised to 80°C and maintained at the same temperature, while the remaining emulsion and 4.0 parts of a 2.5% aqueous solution of potassium persulfate were added dropwise over 2 hours to react with each other. The fine particles A obtained by the reaction were filtered and dried to obtain fine particles A (average particle size 0.4 μm).

[0282] <Production Example 2: Production of Microparticles B> 58.0 parts of styrene, 30.0 parts of methyl methacrylate, 10.0 parts of benzyl methacrylate, 2.0 parts of acrylic acid, 0.7 parts of a polyoxyethylene alkyl ether-based reactive surfactant (ADEKA's "ADEKA Soap ER-10", formula (a-4-14)), 0.3 parts of a polyoxyethylene styrenated propynyl phenyl ether-based reactive surfactant (Dai-ichi Kogyo Seiyaku's "Aqualon AN-5065", formula (a-4-7)), and 39.7 parts of ion-exchanged water were mixed and stirred to obtain an emulsion.

[0283] Into a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, 96.5 parts of ion-exchanged water and 3.0% of the above-mentioned emulsion were added. After the internal temperature of the reaction vessel was raised to 70°C and sufficiently replaced with nitrogen, 0.5 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN) and 0.5 parts of benzoyl peroxide (BPO) were added as initiators to initiate polymerization. While raising the internal temperature to 80°C and maintaining the temperature, the remaining emulsion, 0.5 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) (ADVN) and 0.5 parts of benzoyl peroxide (BPO) were added dropwise over 2 hours to react. Fine particles B obtained by the reaction were filtered and dried to obtain fine particles B (average particle size 0.4 μm).

[0284] <Production Example 3: Production of Microparticles C> 99.0 parts of styrene, 1.0 part of divinylbenzene, 1.0 part of a polyoxyalkylene alkenyl ether reactive surfactant ("Latemul PD-104" manufactured by Kao Corporation, formula (a-4-1)), and 39.7 parts of ion-exchanged water were mixed and stirred to obtain an emulsion.

[0285] In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, 96.5 parts of ion-exchanged water and 3.0% of the above-mentioned emulsion were added. After the internal temperature of the reaction vessel was raised to 70°C and sufficiently replaced with nitrogen, 5.7 parts of a 2.5% aqueous solution of potassium persulfate were added as an initiator to start polymerization. The internal temperature was raised to 80°C and maintained at the same temperature, while the remainder of the emulsion and 4.0 parts of a 2.5% aqueous solution of potassium persulfate were added dropwise over 2 hours to cause a reaction. The fine particles C obtained by the reaction were filtered and dried to obtain fine particles C (average particle size 0.4 μm).

[0286] <Production Example 4: Production of Microparticles D> 97.0 parts of styrene, 1.0 part of divinylbenzene, 2.0 parts of acrylic acid, 1.0 part of a non-reactive surfactant (sodium dodecylbenzenesulfonate), and 39.7 parts of ion-exchanged water were mixed and stirred to obtain an emulsion.

[0287] In a reaction vessel equipped with a stirrer, a thermometer, a dropping funnel and a reflux condenser, 96.5 parts of ion-exchanged water and 3.0% of the above emulsion were added. After the internal temperature of the reaction vessel was raised to 70°C and sufficiently replaced with nitrogen, 5.7 parts of a 2.5% aqueous solution of potassium persulfate was added as an initiator to initiate polymerization. The internal temperature was raised to 80°C and maintained at the same temperature, while the remainder of the emulsion and 4.0 parts of a 2.5% aqueous solution of potassium persulfate were added dropwise over 2 hours to react. Fine particles D obtained by the reaction were filtered and dried to obtain fine particles D (average particle size 0.5 μm).

[0288] <Synthesis Example 1: Synthesis of Maleimide Compound A> Maleimide compound A was synthesized by the method described in Synthesis Example 1 of the Japan Institute of Invention and Innovation's Technical Journal Publication No. 2020-500211, to obtain a MEK solution of the maleimide compound A (70% by mass of non-volatile components).

[0289] <Synthesis Example 2: Synthesis of Polyimide Resin B> A 500 mL separable flask equipped with a water content receiver connected to a reflux condenser, a nitrogen inlet tube, and a stirrer was prepared. 20.3 g of 4,4'-oxydiphthalic anhydride (ODPA), 200 g of γ-butyrolactone, 20 g of toluene, and 29.6 g of 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane were added to this flask to prepare a reaction solution, which was stirred at 45°C for 2 hours under a nitrogen stream to carry out a reaction. Next, the reaction solution was heated and maintained at about 160°C, while condensed water was azeotropically removed together with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was flowing out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. The mixture was then cooled to obtain a polyimide solution (non-volatile content 20% by mass) containing polyimide resin B (a polyimide resin having a 1,1,3-trimethylindane skeleton) as a polymer. The obtained polyimide resin B had a repeating unit represented by the following formula (X1) and a repeating unit represented by the following formula (X2). The weight average molecular weight of the polyimide resin B was 12,000.

[0290] [ka]

[0291] <Example 1> Four parts of a biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent approximately 269 g / eq.) and two parts of a naphthalene type epoxy resin ("HP-4032-SS" manufactured by DIC Corporation, 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent approximately 145 g / eq.) were heated and dissolved in 20 parts of methyl ethyl ketone with stirring. This was cooled to room temperature to prepare a dissolved composition of the epoxy resin.

[0292] To this epoxy resin solution, 1 part of the fine particles A obtained in Production Example 1, 20 parts of an active ester compound (DIC Corporation's "HPC-8150-62T", active ester group equivalent of about 220 g / eq., toluene solution with non-volatile content of 62% by mass), and spherical silica (Admatechs Corporation's "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with a silane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM-573") were added. 2 60 parts of 1000g / g of phenol-based curing agent containing a triazine skeleton (DIC Corporation's "LA-3018-50P", active group equivalent of about 151g / eq., 2-methoxypropanol solution with a non-volatile content of 50%), 2 parts of carbodiimide-based curing agent (Nisshinbo Chemical Co., Ltd.'s "V-03", active group equivalent of about 216g / eq., toluene solution with a non-volatile content of 50%), 0.01 parts of imidazole-based curing accelerator (Shikoku Chemical Industry Co., Ltd.'s "1B2PZ", 1-benzyl-2-phenylimidazole), and 2 parts of phenoxy resin (Mitsubishi Chemical Corporation's "YX7553BH30", 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30% by mass) were mixed and uniformly dispersed using a high-speed rotating mixer to prepare a resin composition.

[0293] <Example 2> Instead of 2 parts of naphthalene type epoxy resin (DIC Corporation's "HP-4032-SS", 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent of approximately 145 g / eq.), 2 parts of bixylenol type epoxy resin (Mitsubishi Chemical Corporation's "YX4000H", epoxy equivalent of 190 g / eq.) were used. Furthermore, the amount of fine particles A was changed from 1 part to 4 parts. Apart from the above, a resin composition was prepared in the same manner as in Example 1.

[0294] <Example 3> Instead of one part of the fine particles A, one part of the fine particles B obtained in Production Example 2 was used. In addition, 5 parts of vinylbenzyl-modified polyphenylene ether ("OPE-2St 2200" manufactured by Mitsubishi Gas Chemical Co., Ltd., a toluene solution with a non-volatile content of 65%) was added to the resin composition. Furthermore, spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with a silane coupling agent ("KBM-573" manufactured by Shin-Etsu Chemical Co., Ltd.) was added. 2 The amount of cellulose acetate (C10) / g was changed from 60 parts to 70 parts. A resin composition was prepared in the same manner as in Example 1 except for the above.

[0295] <Example 4> Instead of 1 part of the fine particles A, 1 part of the fine particles B obtained in Production Example 2 was used. Also, instead of 2 parts of the naphthalene type epoxy resin ("HP-4032-SS" manufactured by DIC Corporation, 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent of about 145 g / eq.), 2 parts of the bixylenol type epoxy resin ("YX4000H" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent of 190 g / eq.) were used. Furthermore, 5 parts of the maleimide compound A obtained in Synthesis Example 1 were added to the resin composition. Also, instead of 2 parts of the phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30% by mass), 10 parts of the polyimide resin B obtained in Synthesis Example 2 (non-volatile content of 20% by mass) were used. In addition, surface-treated spherical silica (Admatechs "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) was used. 2 Instead of 60 parts of 100% glycerol, surface-treated spherical silica (UFP-30 manufactured by Denki Kagaku Kogyo Co., Ltd., average particle size 0.3 μm, specific surface area 30.7 m2 / g, carbon content per unit surface area 0.22mg / m 2 A resin composition was prepared in the same manner as in Example 1 except for the above points.

[0296] <Example 5> Instead of a part of the fine particles A, a part of the fine particles C obtained in Production Example 3 was used. In addition, surface-treated spherical silica ("SO-C2" manufactured by Admatechs Co., Ltd., average particle size 0.5 μm, specific surface area 5.8 m) was used. 2 The amount of cellulose acetate / g was changed from 60 parts to 42 parts. Furthermore, 14 parts of hollow silica particles ("BA-S" manufactured by JGC Catalysts and Chemicals, average particle size 2.6 μm, porosity 25% by volume) were added to the resin composition. Except for the above, the resin composition was prepared in the same manner as in Example 1.

[0297] <Example 6> One part of the fine particles C obtained in Production Example 3 was added to the resin composition. The amount of the phenoxy resin ("YX7553BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK with a non-volatile content of 30% by mass and cyclohexanone) was changed from 2 parts to 1 part. Furthermore, 5 parts of the polyimide resin B (non-volatile content of 20% by mass) obtained in Synthesis Example 2 was added to the resin composition. Aside from the above, the resin composition was prepared in the same manner as in Example 1.

[0298] <Example 7> 8 parts of biphenyl type epoxy resin ("NC3000L" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269 g / eq.) and 4 parts of naphthalene type epoxy resin ("HP-4032-SS" manufactured by DIC Corporation, 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent of about 145 g / eq.) were heated and dissolved in 20 parts of methyl ethyl ketone with stirring. This was cooled to room temperature to prepare a dissolved composition of the epoxy resin.

[0299] This epoxy resin solution composition was mixed with 1 part of the fine particles A obtained in Production Example 1, 6 parts of an active ester compound (DIC Corporation's "HPC-8000-65T", active ester group equivalent of about 223 g / eq., toluene solution with non-volatile content of 65%), 8 parts of a prepolymer of bisphenol A dicyanate (Lonza Japan's "BA230S75", cyanate equivalent of about 232 g / eq., MEK solution with non-volatile content of 75% by mass), and spherical silica (Admatechs' "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) surface-treated with a silane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM-573"). 2 A resin composition was prepared by mixing 60 parts of dimethylformamide (1:1 / g), 1 part of a 1 mass % MEK solution of cobalt (III) acetylacetonate (Tokyo Chemical Industry Co., Ltd.), and 2 parts of a phenoxy resin (YX7553BH30 by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a non-volatile content of 30 mass %) and dispersing the mixture uniformly in a high-speed rotating mixer.

[0300] <Example 8> A resin composition was prepared in the same manner as in Example 1, except that 2 parts of a benzoxazine-based curing agent (a MEK solution of "ODA-BOZ" manufactured by JFE Chemical Corporation with a solid content of 50 mass%; active group equivalent of approximately 218 g / eq.) was added to the resin composition.

[0301] <Comparative Example 1> Fine particles A were not used. Surface-treated spherical silica (Admatechs Co., Ltd. "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) was also used. 2 The amount of cellulose acetate (C10) / g was changed from 60 parts to 50 parts. Except for the above, the resin composition was prepared in the same manner as in Example 1.

[0302] <Comparative Example 2> Instead of 2 parts of naphthalene-type epoxy resin (DIC Corporation's "HP-4032-SS", 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent of approximately 145 g / eq.), 2 parts of bixylenol-type epoxy resin (Mitsubishi Chemical Corporation's "YX4000H", epoxy equivalent of 190 g / eq.) were used. Also, instead of 1 part of fine particles A, 1 part of rubber particles (Aica Kogyo Co., Ltd.'s "Staphyloid AC3816N", average particle size 0.3 μm) was used. Furthermore, surface-treated spherical silica (Admatechs Co., Ltd.'s "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) was used. 2 The amount of cellulose acetate (COOH / g) was changed from 60 parts to 55 parts. In addition, 0.5 parts of a reactive surfactant (ADEKA "ADEKA SOAP ER-10") was added to the resin composition. Except for the above, the resin composition was prepared in the same manner as in Example 1.

[0303] <Comparative Example 3> Instead of 2 parts of naphthalene-type epoxy resin (DIC Corporation's "HP-4032-SS", 1,6-bis(glycidyloxy)naphthalene, epoxy equivalent of approximately 145 g / eq.), 2 parts of bixylenol-type epoxy resin (Mitsubishi Chemical Corporation's "YX4000H", epoxy equivalent of 190 g / eq.) were used. Also, instead of 1 part of fine particles A, 1 part of fine particles D obtained in Production Example 4 was used. Furthermore, surface-treated spherical silica (Admatechs Corporation's "SO-C2", average particle size 0.5 μm, specific surface area 5.8 m) was used. 2 / g) was changed from 60 parts to 65 parts. Except for the above, the resin composition was prepared in the same manner as in Example 1.

[0304] <Comparative Example 4> A resin composition was prepared in the same manner as in Example 7, except that the fine particles A were not used.

[0305] <Production of resin sheets> A polyethylene terephthalate film ("AL5" manufactured by Lintec Corporation, thickness 38 μm) with a release layer was prepared as a support. The resin compositions obtained in the examples and comparative examples were uniformly applied onto the release layer of this support so that the thickness of the resin composition layer after drying was 40 μm. Thereafter, the resin composition was dried at 80°C to 100°C (average 90°C) for 4 minutes to obtain a resin sheet including a support and a resin composition layer.

[0306] <Measurement of relative permittivity (Dk) and dielectric loss tangent (Df)> The obtained resin sheet was heated at 200°C for 90 minutes to thermally cure the resin composition layer, and then the support was peeled off to obtain a cured film formed of the cured product of the resin composition. The cured film was cut into a piece having a width of 2 mm and a length of 80 mm to obtain a cured product A for evaluation.

[0307] The dielectric constant (Dk value) and dielectric loss tangent (Df value) of the obtained cured product A for evaluation were measured by the cavity resonance perturbation method at a measurement frequency of 5.8 GHz and a measurement temperature of 23° C. using an “HP8362B” manufactured by Agilent Technologies. Measurements were performed on three test pieces, and the average values ​​were calculated.

[0308] <Measurement of elongation at break> The cured product A for evaluation obtained in the same manner as above was subjected to a tensile test at 23°C in accordance with Japanese Industrial Standard JIS K7127 using a Tensilon universal testing machine (Orientec "RTC-1250A") to measure the elongation at break (%).

[0309] <Measurement of arithmetic mean roughness (Ra)> (1) Surface preparation of inner layer board: A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic "R1515A") with copper foil on the surface was prepared as an inner layer substrate. The copper foil on the surface of this inner layer substrate was etched with a microetching agent (Mec "CZ8101") with a copper etching amount of 1 μm to perform a roughening treatment. Then, it was dried at 190°C for 30 minutes.

[0310] (2) Lamination and curing of resin sheets: The resin sheet was laminated on both sides of the inner layer substrate using a batch type vacuum pressure laminator (two-stage build-up laminator "CVP700" manufactured by Nikko Materials Co., Ltd.) so that the resin composition layer was bonded to the inner layer substrate. This lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at a temperature of 100°C and a pressure of 0.74 MPa for 30 seconds.

[0311] (3) Curing of resin composition layer: The laminated resin sheet was then heat-pressed at atmospheric pressure at 100°C under a pressure of 0.5 MPa for 60 seconds to smooth it, and then placed in a 130°C oven for 30 minutes, and then transferred to a 170°C oven for 30 minutes to thermally cure the resin composition layer, thereby forming an insulating layer.

[0312] (4) Formation of via holes: A CO2 laser processing machine (Via Mechanics' "LK-2K212 / 2C") was used to form a via hole in the insulating layer under the conditions of a frequency of 2000 Hz, a pulse width of 3 μsec, an output of 0.95 W, and a shot count of 3. The formed via hole had an opening diameter (diameter) of 50 μm on the insulating layer surface and a diameter of 40 μm on the insulating layer bottom surface. The support was then peeled off to obtain a laminated substrate having a layer structure of insulating layer / inner layer substrate / insulating layer.

[0313] (5) Roughening treatment: The laminated substrate was immersed in a swelling solution, Swelling Dip Securigant P, manufactured by Atotech Japan, at 60°C for 10 minutes. Next, the laminated substrate was immersed in a roughening solution, Concentrate Compact P, manufactured by Atotech Japan (aqueous solution of KMnO4: 60g / L, NaOH: 40g / L), at 80°C for 20 minutes. After that, the laminated substrate was immersed in a neutralizing solution, Reduction Solution Securigant P, manufactured by Atotech Japan, at 40°C for 5 minutes. By immersing in the swelling solution, roughening solution, and neutralizing solution, the surface of the insulating layer of the laminated substrate was roughened, and a roughened surface was formed. The laminated substrate after this roughening treatment was designated "Evaluation Substrate A."

[0314] (6) Measurement of arithmetic mean roughness (Ra): The arithmetic mean roughness Ra of the roughened surface of the insulating layer of the obtained evaluation substrate A was measured using a non-contact surface roughness meter (WYKO NT3300 manufactured by B-CO Instruments) in VSI mode with a 50x lens and a measurement range of 121 μm × 92 μm. Measurements were performed at 10 randomly selected points, and the average value was calculated.

[0315] <Evaluation of the infiltration> (7) Heat treatment: The evaluation substrate A after the roughening treatment was heated for 30 minutes in a batch oven (manufactured by Yamato Scientific Co., Ltd., precision thermostat, DF412, air atmosphere) heated to 130°C.

[0316] (8) Formation of electroless copper plating layer: According to the semi-additive method, an electroless copper plating layer was formed on the roughened surface of the insulating layer. Specifically, an electroless plating process including the following steps 1 to 6 (copper plating process using a chemical solution manufactured by Atotech Japan) was carried out to form the electroless copper plating layer.

[0317] 1. Alkaline cleaning process (cleaning the surface of the insulating layer with via holes and adjusting the charge): The surface of the evaluation substrate A was cleaned with Cleaning Cleaner Securiganth 902 (trade name) at 60° C. for 5 minutes. 2. Soft etching process (cleaning inside the via hole): The surface of evaluation substrate A was treated with an aqueous solution of sodium peroxodisulfate acidified with sulfuric acid at 30° C. for 1 minute. 3. Pre-dip process (adjusting the charge on the surface of the insulating layer for Pd application): The surface of evaluation substrate A was treated with Pre. Dip Neoganth B (trade name) at room temperature for 1 minute. 4. Activator application process (application of Pd to the surface of the insulating layer): The surface of evaluation substrate A was treated with Activator Neoganth 834 (trade name) at 35° C. for 5 minutes. 5. Reduction step (reducing the Pd added to the insulating layer): The surface of evaluation substrate A was treated with a mixed solution of Reducer Neoganth WA (trade name) and a 10% aqueous solution of potassium formate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) at 30° C. for 5 minutes. 6. Electroless copper plating process (Cu is deposited on the surface of the insulating layer (Pd surface)) The surface of the evaluation board A was treated with a mixture of Basic Solution Printganth MSK-DK (trade name), PER-6-B-2X (manufactured by Uemura Kogyo Co., Ltd.), and Reducer Cu (trade name) at 35°C for 30 minutes to form an electroless copper plating layer on the roughened surface of the insulating layer. The thickness of the electroless copper plating layer formed was 1 μm.

[0318] (9) Formation of wiring patterns: After electroless plating, the surface of the evaluation substrate A having the electroless copper plating layer was treated with a 5% sulfuric acid aqueous solution for 30 seconds. Next, a dry film for pattern formation (Hitachi Chemical's "Photec RY-3600", thickness 19 μm) was laminated on both sides of the evaluation substrate A using a batch-type vacuum pressure laminator (Meiki Seisakusho's "MVLP-500"). The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then applying pressure at 70°C and a pressure of 0.1 MPa for 20 seconds.

[0319] Then, a glass mask (photomask) was placed on the dry film. The glass mask had a comb-shaped wiring pattern (line / space (L / S)=12 μm / 12 μm, i.e., a comb pattern with a wiring pitch of 24 μm; wiring length 15 mm, 20 lines, 10 comb patterns) for evaluating penetration and a large area pattern (a pattern wider than 150 mm×30 mm) for measuring peel strength. The dry film was irradiated with light through the glass mask using a projection exposure machine (Ushio Inc.'s "UX-2240") (exposure treatment). Next, the dry film was sprayed with a 1% aqueous sodium carbonate solution (developer) at 30° C. for 30 seconds at a spray pressure of 0.15 MPa. After that, it was washed with water and developed (pattern formation).

[0320] After development, electrolytic copper plating was performed to form a 5 μm-thick electrolytic copper plating layer on the electroless plating layer, thus forming a conductor layer including an electroless copper plating layer and an electrolytic copper plating layer (the total thickness of the electroless copper plating layer and the electrolytic copper plating layer was about 6 μm) on the roughened surface of the insulating layer.

[0321] Next, a 3% sodium hydroxide solution at 50°C was sprayed at a spray pressure of 0.2 MPa to peel off the dry films on both sides of the evaluation substrate A. The substrate was heated at 190°C for 60 minutes to perform an annealing treatment. The evaluation substrate A was then immersed in a flash etching etchant at 25°C for 4 minutes to remove the unnecessary copper layer, thereby forming a plated conductor layer. As the flash etching etchant, an aqueous solution was used in which a concentrated sulfuric acid solution of 40 g / L (a 95% aqueous solution manufactured by Fujifilm Wako Pure Chemical Industries) was dissolved in a hydrogen peroxide solution of 10 g / L (a 35% aqueous solution manufactured by Tokyo Chemical Industry Co., Ltd.). Through the above operations, an "evaluation substrate B" having a layer structure of a plated conductor layer / insulating layer / inner layer substrate / insulating layer / plated conductor layer was obtained. The plated conductor layer included a patterned conductor layer (wiring) having a comb tooth pattern for penetration evaluation, and a large-area conductor layer for peel strength measurement.

[0322] (10) Evaluation of penetration (residue removability): In the area where the comb-tooth patterned conductor layer was formed, the evaluation board B was cross-sectionally processed using an FIB (SII NanoTechnology's "SMI3050"). At 10 measurement points, it was observed whether there was conduction between the patterned conductor layers (wiring) due to plating penetration. The observation results were evaluated according to the following criteria. ○: No continuity between the wiring was confirmed at any of the 10 measurement points. ×: Conduction between the wirings was confirmed at at least one location out of 10 locations.

[0323] <Measurement of the peel strength of the conductor layer> (11) Measurement of the peel strength of the conductor layer: The evaluation board B was cut into a small piece of 150 mm x 30 mm in the part where the large-area conductor layer was formed. A cutter was used to make a cut in the conductor layer of the small piece, surrounding an area of ​​10 mm width and 100 mm length. One end of this part was peeled off and held with the grip of a tensile tester (Autocom universal testing machine "AC-50C-SL" manufactured by TSE Corporation). The load [kgf / cm] when 35 mm was peeled off by pulling vertically at a speed of 50 mm / min at room temperature (25°C) was measured as the copper foil peel strength. The measurement was performed in accordance with the Japanese Industrial Standard JIS C6481.

[0324] <Crack resistance evaluation> (1) Lamination of resin sheet: An inner layer substrate (Hitachi Chemical's "MCL-E700G", conductor layer thickness 35 μm, total thickness 0.4 mm, residual copper ratio 40%) having circuit conductors (copper) formed on both sides in a wiring pattern of line / space (L / S) = 8 μm / 8 μm was prepared. Resin sheets were laminated on both sides of this inner layer substrate so that the resin composition layer was in contact with the inner layer substrate. This lamination was performed using a vacuum pressure laminator (Meiki Seisakusho's "MVLP-500"), with vacuum suction at a temperature of 120°C for 30 seconds, followed by lamination at a temperature of 120°C and a pressure of 7.0 kg / cm. 2Then, the substrate was pressed for 30 seconds using a heat-resistant rubber under atmospheric pressure at a temperature of 120°C and a pressure of 5.5 kg / cm using a stainless steel end plate. 2 The press was performed for 60 seconds under the above conditions.

[0325] (2) Thermal curing of the resin composition layer: The resin composition layer was thermally cured by heating at 130° C. for 30 minutes and then at 170° C. for 30 minutes to obtain an insulating layer as a cured layer made of the cured resin composition. The support was then peeled off to obtain a sample substrate having a layer structure of insulating layer / inner layer substrate / insulating layer.

[0326] (3) Roughening treatment: The insulating layer of the sample substrate was subjected to a roughening treatment. Specifically, the sample substrate was immersed in a swelling solution, Swelling Dip Securigant P (manufactured by Atotech Japan), at 60°C for 10 minutes. Next, it was immersed in a roughening solution, Concentrate Compact P (aqueous solution of KMnO4: 60g / L, NaOH: 40g / L) (manufactured by Atotech Japan), at 80°C for 20 minutes. Finally, it was immersed in a neutralizing solution, Reduction Solution Securigant P (manufactured by Atotech Japan), at 40°C for 5 minutes.

[0327] (4) Crack evaluation: After the roughening treatment, the surface of the insulating layer was observed on the L / S pattern of the inner layer board. The surface of 100 inner layer boards was checked for cracks along the pattern shape, and the percentage of the number of parts on the pattern where cracks did not occur was counted. This percentage was calculated as the "yield." The calculated yield was also scored according to the following criteria. 1 point: 0% or more but less than 20%. 2 points: 20% or more but less than 40%. 3 points: 40% or more but less than 60%. 4 points: 60% or more but less than 80%. 5 points: 80% or above. Five points was evaluated as "○", three to four points as "△", and two points or less as "×".

[0328] <Result> The results of the above-mentioned Examples and Comparative Examples are shown in the following table. In the table, the abbreviations have the following meanings: Dk: relative dielectric constant Df: Dielectric tangent Elomgation: Elongation at break Ra: Arithmetic mean roughness Peel Strength: The strength with which the conductor layer is peeled off

[0329] [Table 1]

[0330] [Table 2] [Explanation of symbols]

[0331] 100 Insulating layer 100U Insulation layer surface 110 Organic filler particles 120 Cured resin 130 Electroless plating layer 140 Crawl Section 150 Resist layer 160 Electrolytic plating layer 170 Conductor Layer

Claims

1. (A) an organic filler; and (B) a curable resin, The organic filler (A) contains a group represented by the following formula (a-1) on the surface of the particle of the organic filler (A), (B) A resin composition, in which the curable resin contains an epoxy resin and an active ester resin. [Formula 1] (In formula (a-1), X is -SO 3 Na, -SO 3 N.H. 4 or a hydrogen atom; A represents a divalent hydrocarbon group which may have a substituent; m represents 1 when X is a hydrogen atom, and represents -SO 3 Na or -SO 3 N.H. 4 represents 0 or 1; n represents an integer of 1 or more.

2. The resin composition according to claim 1, wherein the organic filler (A) has an average particle size of 5 μm or less.

3. The resin composition according to claim 1 , further comprising (C) an inorganic filler.

4. The resin composition according to claim 1, wherein the curable resin (B) comprises at least one selected from the group consisting of a phenol-based resin, a cyanate ester-based resin, a carbodiimide-based resin, a benzoxazine-based resin, an allyl-based resin, an acrylic-based resin, a styryl-based resin, and a maleimide-based resin.

5. The resin composition according to claim 1 , further comprising (D) a curing accelerator.

6. The resin composition according to claim 1 , which is for forming an insulating layer.

7. A cured product of the resin composition according to any one of claims 1 to 6.

8. A sheet-like laminate material comprising the resin composition according to any one of claims 1 to 6.

9. A support and a resin composition layer formed on the support, A resin sheet, wherein the resin composition layer comprises the resin composition according to any one of claims 1 to 6.

10. A circuit board comprising a cured product of the resin composition according to any one of claims 1 to 6.

11. A semiconductor chip package comprising a cured product of the resin composition according to any one of claims 1 to 6.

12. A semiconductor device comprising the circuit board according to claim 10.

13. A semiconductor device comprising the semiconductor chip package according to claim 11.

Citation Information

Patent Citations

  • Composition for organic insulating material, organic insulating material, sealing material and circuit board

    JP2000311518A

  • Crosslinked resin particle, composition for organic insulation material, organic insulation material, sealant and circuit board

    JP2000313818A

  • Circuit board

    JP2000315845A

  • Thermosetting resin composition with low modulus, thermosetting films using the composition and cured product thereof

    JP2005036136A

  • Sealing material composition, sealing material composition for semiconductor, and fine particle for sealing material

    JP2018184550A