Manufacturing method of the joint body
Patent Information
- Application Number
- JP2022204041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2042-12-21
Smart Images

Figure 0007552680000003 
Figure 0007552680000001 
Figure 0007552680000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a bonded body suitable for use in easily and firmly bonding a base material A and a base material B. [Background technology]
[0002] In recent years, from the viewpoint of reducing the weight and improving the performance of products, the use of multi-material parts has been progressing in various fields such as automobile parts, medical equipment, and home appliances. Multi-materialization is a method of reducing the weight and increasing the strength of materials by combining materials with different functions and properties (hereinafter referred to as dissimilar materials). To realize multi-materialization, technology to firmly bond dissimilar materials is essential.
[0003] As a means for firmly joining different materials, a liquid adhesive, such as thermosetting epoxy resin adhesive (Patent Document 1, etc.), is widely used. Bonding using a liquid adhesive requires a coating step of coating a liquid resin composition and a curing step of curing the resin composition by polymerization reaction after coating. For this reason, when bonding is performed using a liquid adhesive, there is a problem that it takes a long time to apply the resin composition in the application process, and the polymerization reaction takes a long time in the curing process (i.e., the bonding process takes a long time), resulting in a lack of convenience. In this specification, the bonding process time means the time from the start point when at least one of the substrates constituting the bonded body comes into contact with the bonding agent to the end point when the fabrication of the bonded body is completed, including, for example, the time required for the step of applying a liquid adhesive to the substrates, the step of drying the adhesive, the step of placing a solid bonding agent, and the time required for bonding the substrates together (for example, curing the adhesive layer).
[0004] A technology has also been disclosed in which an epoxy resin composition is impregnated into or coated on a substrate, then semi-cured (B-staged), and used to produce a laminate with an adhesive layer in a B-stage state for producing a bonded body (Patent Document 2, etc.). However, bonding using a B-stage adhesive also requires a curing step in which the semi-cured adhesive layer is polymerized and hardened, resulting in a long bonding process time. Furthermore, B-stage adhesives have problems in that they have poor storage stability, cannot be stored for long periods at room temperature, must be stored at low temperatures, and have a short open time, making them inconvenient. In this specification, the open time refers to the time limit from when an adhesive is applied or placed on substrate A until substrate B is placed. Within the open time, the adhesive strength of the adhesive does not decrease, and substrate A and substrate B can be bonded with sufficient adhesive strength. The longer the open time, the longer the time limit from when an adhesive is applied or placed on substrate A until substrate B is placed, which is more convenient.
[0005] Thermoplastic adhesive compositions (hereinafter, hot melt adhesives) are also used as a means for joining different materials (Patent Document 3, etc.). By using a hot melt adhesive, specifically, since the hot melt adhesive uses a phase change that does not involve a polymerization reaction to perform adhesion, a coating process is not required, and the curing time is fast (i.e., the joining process time is short), making it highly convenient. In addition, it can be stored for long periods at room temperature, and is also highly convenient in that it has a long open time.
[0006] However, conventional hot melt adhesives are made of crystalline resins or resins containing crystalline resins in order to reduce the melt viscosity, so the adhesive resin has high cohesive force and cannot have sufficient interaction with the substrate. In addition, when melted and bonded, the viscosity becomes low at high temperatures, so it tends to flow out from the bonding surface, and the viscosity is difficult to control, so the film thickness is not stable. Due to these factors, there is a problem that conventional hot melt adhesives cannot stably obtain high adhesive strength. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-157018 A [Patent Document 2] Japanese Patent Application Publication No. 10-17685 [Patent Document 3] Japanese Patent Application Publication No. 10-168417 Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, among the conventional technologies, thermosetting epoxy resin adhesives with excellent adhesive properties, whether in liquid or B-stage form, have at least one of the problems of a long bonding process time and a short open time, and hot melt adhesives with a short bonding process time and a long open time have the problem that high adhesive strength cannot be stably obtained.
[0009] The present invention has been made in consideration of the above technical background, and aims to provide a technology for joining base material A and base material B, including a combination of different materials, which has a short joining process time, a long open time, and excellent adhesion. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention provides the following means. In this specification, bonding means joining two objects together, and adhesion and welding are subordinate concepts. Adhesion means joining two adherends (objects to be bonded) together using an organic material such as tape or adhesive (thermosetting resin, thermoplastic resin, etc.), while welding means melting the surface of a thermoplastic resin or the like by heat, and joining the objects together by molecular diffusion through entanglement and crystallization by contact pressure and cooling.
[0011] <Method of manufacturing the bonded body> [1] A pre-bonding process in which a substrate A, a plurality of films including a film A and a film B, and a substrate B are arranged in this order to prepare a laminate; a bonding step of heating and pressurizing the laminate to melt the film and bond the base material A and the base material B together, At least one of film A and film B contains an amorphous thermoplastic resin which is either a thermoplastic epoxy resin or a phenoxy resin, and the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group, and has a heat of fusion of 15 J / g or less. [2] The method for producing a bonded body according to [1], wherein the heating and pressurizing are carried out under conditions of 100 to 400° C. and 0.01 to 20 MPa. [3] A method for producing a bonded body obtained by bonding a substrate A, a plurality of films including a film A and a film B, and a substrate B in this order, comprising the steps of: a first bonding step of bonding the plurality of films including the film A and the film B to the substrate A by melting and then solidifying the plurality of films including the film A and the film B in a state in which the plurality of films including the film A and the film B are brought into contact with the substrate A; a second bonding step of bonding the substrate A and the substrate B by melting and then solidifying the plurality of films including the film A and the film B bonded to the substrate A in a state in which the plurality of films including the film A and the film B are brought into contact with the substrate B, a plurality of films including film A and film B each contain an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group, and has a heat of fusion of 15 J / g or less. [4] The method for producing a bonded body according to [3], wherein in the first bonding step, a plurality of films including the film A and the film B are heated to 100 to 300° C. to melt and then solidify. [5] A method for producing a bonded body obtained by bonding a substrate A, a plurality of films including a film A and a film B, and a substrate B in this order, comprising the steps of: a first bonding step of bonding the film A or the plurality of films including the film A to the substrate A by melting and then solidifying the film A or the plurality of films including the film A in a state in which the film A or the plurality of films including the film A is brought into contact with the substrate A; a first bonding step of bonding the film B or the plurality of films including film B to the substrate B by melting and then solidifying the film B or the plurality of films including film B in a state in which the film B or the plurality of films including film B is brought into contact with the substrate B; a second bonding step of bonding the substrate A and the substrate B by melting and then solidifying the film A or the multiple films including film A and the film B or the multiple films including film B in a state in which the film A or the multiple films including film A bonded to the substrate A is brought into contact with the film B or the multiple films including film B bonded to the substrate B, a plurality of films including film A and film B each contain an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group, and has a heat of fusion of 15 J / g or less. [6] The method for producing a joined body according to [5], wherein in the 1A joining step and the 1B joining step, the film A or a plurality of films including the film A and the film B or a plurality of films including the film B are heated to 100 to 300°C to melt and then solidify. [7] The method for producing a joined body according to any one of [3] to [6], wherein in the second joining step, a plurality of films including the film A and the film B are melted and then solidified by at least one selected from the group consisting of contact heating, hot air heating, heat pressing, infrared heating, hot plate welding, ultrasonic welding, vibration welding, and high-frequency induction welding. [8] The method for producing a joined body according to any one of [3] to [7], wherein in the second joining step, the films including film A and film B are heated at a temperature equal to or higher than the melting point thereof to melt and then solidify the films. [9] The method for producing a bonded body according to any one of [3] to [8], wherein in the second bonding step, a plurality of films including film A and film B are melted and then solidified at a heating temperature of 100 to 400°C under a pressure of 0.01 to 20 MPa. Effect of the Invention
[0012] According to the present invention, there can be provided a bonding technique for bonding base material A and base material B, including a combination of different materials, which has a short bonding process time, a long open time, and excellent adhesion.
[0013] Furthermore, according to the present invention, substrate A and substrate B are laminated via a laminate film layer formed by laminating a plurality of films, and the laminate film layer is melted and solidified to bond them together. This makes it possible to suppress a decrease in adhesive bonding strength due to unevenness even when the bonding surfaces of substrate A and substrate B are not smooth.
[0014] In addition, according to the present invention, bonding is performed via a laminated film layer formed by stacking multiple films, so that it is easy to adjust the thickness to an optimum level under various bonding conditions, and manufacturing management and quality control are easier than when bonding is performed via a single film having the same thickness as the laminated film layer. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is an explanatory diagram showing a configuration of a bonded body according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] [Method of Manufacturing Joint Body -Embodiment 1] The method includes a pre-bonding process in which a laminate is prepared by arranging a substrate A, a plurality of films including a film A and a film B, and a substrate B in that order, and a bonding process in which the laminate is heated and pressurized to melt the films and bond the substrate A and the substrate B together. In the pre-bonding step, the substrate A and the film are not bonded to each other, but are bonded to each other in the next bonding step. The film may have tackiness, and in that case, the film is temporarily fixed to the substrate in the pre-bonding step.
[0017] Each step will be described below.
[0018] <Pre-joining process> In the pre-bonding step, a laminate is prepared by arranging a plurality of films including film A and film B and substrate B in this order. The plurality of films including film A and film B are arranged in a laminated state. In the present disclosure, a layer consisting of a plurality of films including film A and film B is also referred to as a "laminate film layer." In the laminate, neither the substrate A nor the laminate film layer, nor the laminate film layer nor the substrate B, is bonded to each other, and each is formed by overlapping independent members. The multiple films including Film A and Film B preferably have the property of being able to retain their outer shape without deformation for 30 days or more under the condition of 23° C. without pressure, and furthermore, not being deteriorated.
[0019] (Film A, Film B) At least one of the films A and B included in the laminated film layer is an amorphous thermoplastic resin that is at least one of a thermoplastic epoxy resin and a phenoxy resin, and is an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more and a heat of fusion of 15 J / g or less. One of the films A and B does not have to be an amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more and a heat of fusion of 15 J / g or less, but is preferably a thermoplastic resin. From the viewpoint of easily obtaining the effects of the present invention, it is more preferable that both the films A and B are amorphous thermoplastic resins having an epoxy equivalent of 1,600 or more and a heat of fusion of 15 J / g or less.
[0020] The amorphous resin in the present invention is a resin that has a melting point (Tm) in a measurement using a differential scanning calorimeter (DSC), but does not have or has a very small endothermic peak (melting point) associated with a clear melting. The heat of fusion is calculated from the area of the endothermic peak of the DSC and the weight of the thermoplastic resin component. When an inorganic filler or the like is contained in the film, it is calculated from the weight of the resin component excluding the inorganic filler. Specifically, the amorphous thermoplastic resin in the present invention refers to the following. A sample is weighed out to 2-10 mg, placed in an aluminum pan, and heated from 23°C to 200°C or higher at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve. Next, when the heat of fusion is calculated from the area of the endothermic peak at the time of melting obtained from the DSC curve and the weighed value, the resin has a heat of fusion of 15 J / g or less.
[0021] In order to fully impart the properties of the amorphous thermoplastic resin to the laminated film layer, the content of the amorphous thermoplastic resin is preferably 51 mass % or more, more preferably 60 mass % or more, even more preferably 70 mass % or more, particularly preferably 80 mass % or more, and most preferably 90 mass % or more of each resin component in Film A and / or Film B. In the present disclosure, "resin components in the film" means components in the film other than the filler.
[0022] The heat of fusion is 15 J / g or less, preferably 11 J / g or less, more preferably 7 J / g or less, even more preferably 4 J / g or less, and most preferably the melting peak is below the detection limit. The epoxy equivalent is 1,600 or more, preferably 2,000 or more, more preferably 5,000 or more, and even more preferably 9,000 or more, and most preferably above the detection limit so that substantially no epoxy groups are detected.
[0023] By using Film A and / or Film B containing an amorphous thermoplastic resin with an epoxy equivalent of 1,600 or more and a heat of fusion of 15 J / g or less, the sudden viscosity drop seen in conventional hot melt adhesives does not occur when heated, and the adhesive does not reach a low viscosity state (0.001 to 100 Pa s) even in high temperature ranges exceeding 200°C. Therefore, Film A and / or Film B will not flow out of the laminate even in a molten state, the thickness of the adhesive layer can be stably secured, and high adhesive strength can be stably obtained. The epoxy equivalent weight (weight of the resin containing 1 mole of epoxy groups) referred to here is the epoxy equivalent weight of the thermoplastic epoxy resin or phenoxy resin component contained in film A and / or film B before bonding, and is a value (unit: g / eq.) measured by the method specified in JIS-K7236:2001. Specifically, a potentiometric titration device was used, cyclohexanone was used as the solvent, brominated tetraethylammonium acetate solution was added, and a 0.1 mol / L perchloric acid-acetic acid solution was used, and the solvent-diluted product (resin varnish) was calculated as a solid content equivalent value from the non-volatile content. In the case of a mixture of two or more resins, it can also be calculated from the content and epoxy equivalent weight of each resin.
[0024] The melting point of the amorphous thermoplastic resin contained in film A and / or film B is preferably 50 to 400° C., more preferably 60 to 350° C., and even more preferably 70 to 300° C. When the melting point is in the range of 50 to 400° C., film A and / or film B can be efficiently deformed and melted by heating and effectively wet and spread over the bonding surface, resulting in high adhesive strength. In this specification, the melting point of an amorphous thermoplastic resin means the temperature range in the process where the resin softens from a substantially solid state, acquires thermoplastic properties, and becomes meltable and adhesive.
[0025] Conventional thermosetting adhesives have problems in that it is difficult to disassemble the bonded body, and it is difficult to separate and recycle the base materials that make up the bonded body (i.e., poor recyclability), and it is also difficult to reattach the bonded body when there is a misalignment of the bonded part during the manufacturing process of the bonded body or when the contents or the adherend have a defect and need to be replaced (i.e., poor repairability), resulting in a lack of convenience. However, the above-mentioned film A and / or film B can be softened and melted by heat and can be easily peeled off, so it has excellent recyclability. In addition, since the above-mentioned film A and / or film B are thermoplastic, they can be reversibly softened, melted and hardened repeatedly, and therefore have excellent repairability.
[0026] <Thermoplastic epoxy resin> The thermoplastic epoxy resin is preferably a polymer of (a) a difunctional epoxy resin monomer or oligomer and (b) a difunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group. By using such a compound, the polymerization reaction for forming a linear polymer proceeds preferentially, making it possible to obtain a thermoplastic epoxy resin having the desired properties.
[0027] The (a) bifunctional epoxy resin monomer or oligomer refers to an epoxy resin monomer or oligomer having two epoxy groups in the molecule. Specific examples of the (a) include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bifunctional phenol novolac type epoxy resins, bisphenol AD type epoxy resins, biphenyl type epoxy resins, bifunctional naphthalene type epoxy resins, bifunctional alicyclic epoxy resins, bifunctional glycidyl ester type epoxy resins (e.g., diglycidyl phthalate, diglycidyl tetrahydrophthalate, dimer acid diglycidyl ester, etc.), bifunctional glycidyl amine type epoxy resins (e.g., diglycidyl aniline, diglycidyl toluidine, etc.), bifunctional heterocyclic epoxy resins, bifunctional diarylsulfone type epoxy resins, hydroquinone type epoxy resins (e.g., hydroquinone diglycidyl ether, 2,5-di-tert-butyl ether, etc.), t-Butylhydroquinone diglycidyl ether, resorcin diglycidyl ether, etc.), bifunctional alkylene glycidyl ether compounds (e.g. butanediol diglycidyl ether, butenediol diglycidyl ether, butynediol diglycidyl ether, etc.), bifunctional glycidyl group-containing hydantoin compounds (e.g. 1,3-diglycidyl-5,5-dialkylhydantoin, 1-glycidyl-3-(glycidoxyalkyl)-5,5-dialkylhydantoin, etc.), bifunctional glycidyl group-containing siloxanes (e.g. 1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane, α,β-bis(3-glycidoxypropyl)polydimethylsiloxane, etc.) and modified products thereof. Among these, bisphenol A type epoxy resins, bisphenol F type epoxy resins, and biphenyl type epoxy resins are preferred in terms of reactivity and workability. Examples of the bifunctional compound having a phenolic hydroxyl group in (b) include mononuclear aromatic dihydroxy compounds having one benzene ring, such as catechol, resorcin, and hydroquinone; bisphenols, such as bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane (bisphenol F), and bis(4-hydroxyphenyl)ethane (bisphenol AD); compounds having a condensed ring, such as dihydroxynaphthalene; Examples include bifunctional phenol compounds having an allyl group introduced therein, such as resorcinol, diallyl bisphenol A, and triallyl dihydroxybiphenyl, and dibutyl bisphenol A. Specific examples of the (b) carboxyl group-containing compound include adipic acid, succinic acid, malonic acid, cyclohexanedicarboxylic acid, phthalic acid, isophthalic acid, and terephthalic acid. Examples of the bifunctional compound having a mercapto group of (b) include ethylene glycol bisthioglycolate and ethylene glycol bisthiopropionate. Examples include: Specific examples of the (b) isocyanate group-containing bifunctional compound include diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HMDI), and tolylene diisocyanate (TDI). Specific examples of the (b) cyanate ester group-containing bifunctional compound include 2,2-bis(4-cyanatophenyl)propane, 1,1-bis(4-cyanatophenyl)ethane, and bis(4-cyanatophenyl)methane. Among the above (b), a bifunctional compound having a phenolic hydroxyl group is preferred from the viewpoint of obtaining a thermoplastic polymer, a bifunctional compound having two phenolic hydroxyl groups and a bisphenol structure or a biphenyl structure is preferred from the viewpoint of heat resistance and adhesiveness, and bisphenol A, bisphenol F or bisphenol S is preferred from the viewpoint of heat resistance and cost.
[0028] When the (a) is a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, or a biphenyl type epoxy resin, and the (b) is bisphenol A, bisphenol F, or bisphenol S, the polymer obtained by polymerization of the (a) and (b) has a main chain having a paraphenylene structure and an ether bond as a main skeleton, the main chain being linked by an alkylene group, and a structure in which a hydroxyl group generated by polyaddition is arranged in a side chain. The linear structure of the paraphenylene skeleton can increase the mechanical strength of the polymer after polymerization, and the hydroxyl groups arranged in the side chains can improve adhesion to the substrate. As a result, high adhesive strength can be achieved while maintaining the workability of thermosetting resins. Furthermore, in the case of thermoplastic resins, recycling and repair are possible by softening and melting with heat, improving the recyclability and repairability that are problems with thermosetting resins.
[0029] Phenoxy resin Phenoxy resin is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin, and has thermoplastic properties. For the production of phenoxy resin, a method of direct reaction of dihydric phenols with epichlorohydrin and a method of addition polymerization reaction of diglycidyl ether of dihydric phenols with dihydric phenols are known, but the phenoxy resin used in the present invention may be obtained by either method. In the case of direct reaction of dihydric phenols with epichlorohydrin, examples of dihydric phenols include phenols such as bisphenol A, bisphenol F, bisphenol S, biphenol, biphenylenediol, and fluorenediphenyl; and aliphatic glycols such as ethylene glycol, propylene glycol, and diethylene glycol. Among them, bisphenol A, bisphenol F, and bisphenol S are preferred from the viewpoints of cost, adhesiveness, viscosity, and heat resistance. These may be used alone or in combination of two or more. Phenoxy resin has a chemical structure similar to that of epoxy resin, with a paraphenylene structure and an ether bond as the main skeleton, a main chain connecting these, and a structure in which hydroxyl groups are arranged in the side chains.
[0030] <Physical properties of thermoplastic epoxy resin and phenoxy resin> The thermoplastic epoxy resin and the phenoxy resin preferably have a weight average molecular weight of 10,000 to 500,000, more preferably 18,000 to 300,000, and even more preferably 20,000 to 200,000, which is a value calculated in terms of polystyrene by GPC (gel permeation chromatography). The weight average molecular weight is calculated from the elution peak position detected by GPC, and each is a value of the molecular weight in terms of standard polystyrene. When the weight average molecular weight is within this range, the balance between thermoplasticity and heat resistance is good, and a bonded body can be efficiently obtained by melting, and the heat resistance is also high. When the weight average molecular weight is 10,000 or more, the heat resistance is excellent, and when it is 500,000 or less, the viscosity during melting is low and the adhesiveness is high.
[0031] <Components other than the resin component in Film A and / or Film B> If necessary, film A and / or film B may contain a filler or an additive as a component other than the resin component, to the extent that the object of the present invention is not impaired.
[0032] The filler includes inorganic fillers and organic fillers (resin powder). Examples of inorganic fillers include spherical fused silica, metal powders such as iron, silica sand, talc, calcium carbonate, mica, acid clay, diatomaceous earth, kaolin, quartz, titanium oxide, silica, phenolic resin microballoons, and glass balloons. When a filler is contained, the filler content in each of Film A and Film B, based on a total amount of 100 volume %, is preferably 50 volume % or less, more preferably 30 volume % or less, even more preferably 20 volume % or less, and most preferably 10 volume % or less. The filler content (volume %) is determined from the amount charged at 25°C. Specifically, it is calculated using the mass % of the filler, the specific gravity of the components other than the filler, and the apparent specific gravity of the filler, according to the following formula (1). (Formula 1) X=(MF / DF)÷(MF / DF+(100-MF) / DR)×100% In formula 1, X: Filler content (volume%) MF: Filler content (% by mass) DR: Specific gravity of the resin component when hardened DF: Apparent specific gravity of filler It is.
[0033] Examples of the additives include antifoaming agents, coupling agents such as silane coupling agents, pigments, etc., and these may be contained alone or in combination of two or more. The content of each of the additives in film A and / or film B is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less. The content of each resin component in Film A and / or Film B is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, still more preferably 50% by mass or more, in one embodiment 80% by mass or more, in another embodiment 90% by mass or more, and in another embodiment 99% by mass or more.
[0034] <<Production method of film A and / or film B>> The method for producing film A and / or film B is not particularly limited, but for example, it can be obtained by heating and polymerizing a monomer or oligomer of a bifunctional epoxy compound. A solvent may be added during polymerization to reduce the viscosity and facilitate stirring. When a solvent is added, it is necessary to remove the solvent, and film A and / or film B may be obtained by drying or polymerization or both on a release film or the like.
[0035] Examples of the additives include viscosity adjusters, inorganic fillers, organic fillers (resin powders), antifoaming agents, coupling agents such as silane coupling agents, pigments, etc., and these can be used alone or in combination of two or more. As the viscosity modifier, for example, a reactive diluent or the like can be used. Examples of inorganic fillers include spherical fused silica, metal powders such as iron, silica sand, talc, calcium carbonate, mica, acid clay, diatomaceous earth, kaolin, quartz, titanium oxide, silica, phenolic resin microballoons, and glass balloons. The film thus obtained has a small or substantially no content of unreacted monomers or terminal epoxy groups, and therefore has excellent storage stability and can be stored for long periods at room temperature.
[0036] <<Form of Film A and / or Film B>> From the viewpoint of obtaining a bonded body having excellent bondability in a short bonding process time, the thickness of film A and / or film B is preferably 1 mm or less, more preferably 0.5 mm or less, even more preferably 0.3 mm or less, even more preferably 0.2 mm or less, and most preferably 0.1 mm or less. When the size is within this range, the material can be sandwiched between base material A and base material B and efficiently spread across the bonding surface by applying heat or pressure, resulting in a high bonding strength.
[0037] The number of films constituting the laminated film layer can be appropriately selected depending on the state of the bonding surfaces of the substrate A and substrate B. For example, when the bonding surfaces have deep unevenness, increasing the number of films can facilitate adhesion, and an improvement in bonding strength can be expected. There is no particular restriction on the thickness of the film layer after bonding, but from the viewpoint of obtaining stable bonding strength, it is preferably 5 μm to 1 mm, more preferably 10 μm to 0.5 mm, and even more preferably 15 μm to 0.2 mm.
[0038] <Film manufacturing method> The method for producing film A and / or film B is not particularly limited. For example, a resin composition may be obtained by heating and polymerizing a monomer or oligomer of a bifunctional epoxy compound, adding a solvent to the obtained resin composition as necessary, applying the composition to a release film or the like, curing and drying, and applying pressure as necessary to obtain a film.
[0039] <Joining process> In the bonding step, the laminate is heated and pressurized to melt the laminated film layer, and then the temperature is lowered to solidify the film, thereby bonding the base material A and the base material B together.
[0040] The temperature for the heating and pressurization is preferably 100 to 400° C., more preferably 120 to 350° C., and even more preferably 150 to 300° C. By heating at 100 to 400° C., the laminated film layer is efficiently deformed and melted, and effectively wets and spreads over the bonding surface, resulting in high adhesive strength. The pressure applied during the heating and pressing is preferably 0.01 to 20 MPa, more preferably 0.1 to 10 MPa, and even more preferably 0.2 to 5 MPa. Within this pressure range, the laminated film layer is efficiently deformed and effectively wets and spreads across the bonding surface, resulting in high adhesive strength. When at least one of the substrates A and B is a thermoplastic resin, applying pressure at 0.01 to 20 MPa makes the laminated film layer and the substrate compatible, resulting in high adhesive strength.
[0041] The amorphous thermoplastic resin contained in the laminated film layer has low cohesive strength within the resin and contains hydroxyl groups, resulting in strong interaction with the substrate and enabling it to bond dissimilar materials with greater adhesive strength than conventional crystalline hot melt adhesives.
[0042] The bonding between the substrate A and the substrate B utilizes the phase change (solid-liquid-solid) of the laminated film layer and does not involve a chemical reaction, so bonding can be completed in a shorter time than with conventional thermosetting epoxy resins.
[0043] [Method of manufacturing the joint body - embodiment 2] The method for producing a bonded body according to the present embodiment is a method for producing a bonded body obtained by bonding a base material A, a plurality of films including a film A and a film B, and a base material B in this order, and includes a first bonding step of bonding the base material A and the plurality of films including a film A and a film B by melting and then solidifying the plurality of films including a film A and a film B in a state in which the plurality of films including a film A and a film B are brought into contact with the base material A, and a second bonding step of bonding the base material A and the plurality of films including a film A and a film B in a state in which the plurality of films including a film A and a film B bonded to the base material A are brought into contact with the base material B, by melting and then solidifying the plurality of films including a film A and a film B, and the plurality of films including a film A and a film B contain an amorphous thermoplastic resin which is at least any one of a thermoplastic epoxy resin and a phenoxy resin, and the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group, and has a heat of fusion of 15 J / g or less.
[0044] This manufacturing method utilizes the phase change (solid-liquid-solid) of a film containing an amorphous thermoplastic resin, which is at least one of a thermoplastic epoxy resin and a phenoxy resin, to bond substrate A and substrate B, and since no chemical reaction is involved, bonding can be completed in a shorter time than with conventional thermosetting epoxy resins, and the open time is also long. In addition, since thermoplastic epoxy resins and phenoxy resins have low cohesive strength within the resin and contain hydroxyl groups, they have strong interactions with the substrate, and can bond different materials with a stronger bonding strength than conventional crystalline hot melt adhesives. In addition, the manufacturing method is performed by dividing the process into a first bonding process and a second bonding process. By dividing the process in this way, the bonding can be performed by heating at a temperature suitable for the bonding interface, and a bonded body with excellent bonding properties can be manufactured. In addition, the heating temperature control is also easier than when the process is not divided. Furthermore, by bonding a film to the base material A in advance, the base material A and the base material B can be bonded with high precision, and the occurrence of misalignment at the bonding point can be suppressed.
[0045] <First joining process> The first bonding process is a process in which a laminated film layer consisting of multiple films including film A and film B is brought into contact with the substrate A, and the laminated film layer is melted and then solidified, thereby bonding the substrate A and the film. In the first bonding step, the base material A and the laminated film layer are bonded in advance, so that the base material A and the base material B can be bonded with high precision. In this specification, "solidified" means solid at room temperature, that is, non-fluid in an unpressurized state at 23° C. However, the film after the first bonding step may have tackiness.
[0046] The method for melting the laminated film layer includes at least one method selected from the group consisting of contact heating, hot air heating, heat pressing, hot plate welding, infrared heating, ultrasonic welding, vibration welding, and high-frequency induction welding. Among them, infrared heating is preferred from the viewpoints of ease of production and shortening the joining process.
[0047] When the laminated film layer is melted by heating, the temperature of the bonding surface of the substrate A with the laminated film layer is preferably heated to 100 to 300° C., more preferably 120 to 250° C., and even more preferably 150 to 220° C. By heating at 100 to 300° C., the film efficiently deforms and melts, and effectively wets and spreads over the bonding surface, resulting in high bonding strength. Methods for solidifying the molten film include a method of cooling at room temperature or a method of cooling using a cooling device. Here, "room temperature" means a general room temperature within the range of 5 to 30° C. Among these, the method of cooling at room temperature is preferred from the viewpoint of ease of production.
[0048] The film used and the methods of melting and solidifying it are the same as those in the first embodiment.
[0049] <Second joining process> The second bonding process is a process of bonding the substrate A and the substrate B together by melting and then solidifying the laminated film layer while the laminated film layer bonded to the substrate A is brought into contact with the substrate B.
[0050] From the viewpoint of obtaining a high bonding strength, in the second bonding step, it is preferable to heat at a temperature equal to or higher than the melting point of at least one of the films constituting the laminated film layer, and then melt and solidify the films constituting the laminated film layer. By heating at a temperature equal to or higher than the melting point of at least one of the films constituting the laminated film layer, the films constituting the laminated film layer and the substrate become compatible, and a stronger bonding strength is easily obtained.
[0051] The method for melting the films constituting the laminated film layer includes at least one method selected from the group consisting of contact heating, hot air heating, heat pressing, infrared heating, hot plate welding, ultrasonic welding, vibration welding, and high-frequency induction welding. Among these, heat pressing, ultrasonic welding, and high-frequency induction welding are preferred.
[0052] The conditions for carrying out the heat press are not particularly limited. For example, the temperature is preferably 100 to 400° C., more preferably 120 to 350° C., and even more preferably 150 to 300° C. By heating at 100 to 400° C., the films constituting the laminated film layer are efficiently deformed and melted, and effectively wet and spread over the bonding surface, resulting in high bonding strength. The pressure in the heat press is preferably 0.01 to 20 MPa, more preferably 0.1 to 10 MPa, and even more preferably 0.2 to 5 MPa. Within this pressure range, the films constituting the laminated film layer are efficiently deformed and effectively wet and spread across the bonding surface, resulting in high bonding strength. When the substrate B is a thermoplastic resin, applying a pressure of 0.01 to 20 MPa makes the film and substrate compatible, resulting in high bonding strength.
[0053] There are no particular limitations on the conditions for ultrasonic welding. For example, the transmission frequency is preferably 10 to 70 kHz, and more preferably 15 to 40 kHz. From the viewpoints of adhesion and appearance, the ultrasonic application time is preferably 0.1 to 3 seconds, and more preferably 0.2 to 2 seconds. When the substrate A and the substrate B are pressed together during the application of ultrasonic waves, the pressure is preferably 0.01 to 20 MPa, more preferably 0.1 to 10 MPa, and even more preferably 0.2 to 5 MPa. Within this pressure range, the films constituting the laminated film layer are efficiently deformed and effectively wet and spread across the bonding surface, resulting in high adhesive strength.
[0054] There are no particular limitations on the conditions for ultrasonic welding. For example, the oscillation frequency may be in the range of 1 to 1500 kHz. The oscillation frequency may be adjusted to an appropriate value depending on the size and type of the base material A and the base material B. Output power ranges from 100 to 5000W. The oscillation time may be adjusted depending on the size and type of the substrate A and substrate B, and is, for example, preferably 1.0 to 10.0 seconds, and more preferably 1.5 to 8.0 seconds.
[0055] As described above, the bonding of substrate A and substrate B utilizes the phase change of the film (solid to liquid to solid) and does not involve a chemical reaction, so bonding can be completed in a shorter time than with conventional thermosetting epoxy resins.
[0056] [Method of manufacturing the joint body - embodiment 3] The method for producing a bonded body according to the present embodiment is a method for producing a bonded body obtained by bonding a base material A, a plurality of films including film A and film B, and a base material B in this order, and includes a first bonding step of bonding the base material A and the film A or the plurality of films including film A by melting and solidifying the film A or the plurality of films including film A in a state in which the film A or the plurality of films including film A is brought into contact with the base material A, and a second bonding step of bonding the base material B and the film B or the plurality of films including film B by melting and solidifying the film B or the plurality of films including film B in a state in which the film B or the plurality of films including film B is brought into contact with the base material B. and a second bonding step of bonding the substrate A and the substrate B by melting and then solidifying the film A or the multiple films including film A and the film B or the multiple films including film B in a state in which the film A or the multiple films including film A bonded to the substrate A is brought into contact with the film B or the multiple films including film B bonded to the substrate B, wherein the multiple films including film A and film B contain an amorphous thermoplastic resin which is at least any one of a thermoplastic epoxy resin and a phenoxy resin, and the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group and has a heat of fusion of 15 J / g or less.
[0057] This manufacturing method utilizes the phase change (solid-liquid-solid) of a film containing an amorphous thermoplastic resin, which is at least one of thermoplastic epoxy resin and phenoxy resin, to bond substrate A and substrate B, and since no chemical reaction is involved, bonding can be completed in a shorter time than with conventional thermosetting epoxy resins, and the open time is also long. In addition, since thermoplastic epoxy resins and phenoxy resins have low cohesive strength within the resin and contain hydroxyl groups, they have strong interactions with the substrate, and can bond different materials with a stronger bonding strength than conventional crystalline hot melt adhesives. In addition, in this manufacturing method, the bonding is performed by dividing the process into a 1A bonding process, a 1B bonding process, and a 2nd bonding process. By dividing the process in this way, the bonding can be performed by heating at a temperature suitable for the bonding interface, and a bonded body with excellent bonding properties can be manufactured. In addition, the heating temperature control is also easier than when the process is not divided. Furthermore, by bonding film A to base material A in advance and film B to base material B, base material A and base material B can be bonded with high precision, and the occurrence of misalignment at the bonding point can be suppressed.
[0058] The film used and the methods of melting and solidifying it are the same as those in the first and second embodiments.
[0059] [zygote] FIG. 1 shows one embodiment of the bonded body of the present invention. The bonded body 1 shown in FIG. 1 is a bonded body in which a substrate A (3) and a substrate B (4) are bonded and integrated via a bonding layer 2 formed by melting and then solidifying a laminated film layer consisting of a plurality of films including a film A and a film B. The bonded body of the present invention exhibits excellent bonding strength even when it is a bonded body of different materials. The bonding strength is affected by many factors, such as the thickness of the bonding layer, the molecular weight and chemical structure of the polymer constituting the plurality of films including the film A and the film B, in addition to the strength of the interfacial interaction acting between the bonding layer and the substrate A and between the bonding layer and the substrate B, the mechanical properties, and the viscoelastic properties. Therefore, the details of the mechanism by which the bonded body of the present invention exhibits excellent bonding strength are not clear, but it is speculated that the main factors are the low cohesive force in the amorphous thermoplastic resin constituting the bonding layer 2 and the presence of hydroxyl groups in the resin, which form chemical bonds and intermolecular forces such as hydrogen bonds and van der Waals forces at the interfaces between the bonding layer and the substrate A and between the bonding layer and the substrate B. However, in the above-mentioned bonded structure, the state or characteristics of the interface of the bonded structure is an extremely thin chemical structure at the nanometer level or less, which is difficult to analyze, and it is impossible or impractical with current technology to identify and express it in a manner that distinguishes it from something that is not based on the use of multiple films including film A and film B.
[0060] The bonded body of the present invention, in which the bonding layer is made of a thermoplastic resin, is excellent in recyclability and repairability, and can be easily disassembled into base material A and base material B by heating the bonded body.
[0061] There are no particular limitations on the material or shape of the substrate A and the substrate B. The substrate A and the substrate B may be the same or different. Examples of materials constituting each substrate include glass, ceramic, magnetic material, non-magnetic material, fiber reinforced plastic (FRP), metal, wood, paper, composite glass, and resin.
[0062] Examples of glass include soda-lime glass, lead glass, borosilicate glass, and quartz glass.
[0063] Examples of ceramics include oxide-based ceramics such as alumina, zirconia, and barium titanate, hydroxide-based ceramics such as hydroxyapatite, carbide-based ceramics such as silicon carbide, and nitride-based ceramics such as silicon nitride.
[0064] Examples of the magnetic material include magnetic metals such as iron, as well as magnetic ceramics, which have a higher magnetic permeability than the non-magnetic materials described below.
[0065] Examples of non-magnetic materials include aluminum, ceramics, non-magnetic ferrite ceramics, and insulating glass ceramics whose main components are alumina and glass.
[0066] Examples of fiber reinforced plastics (FRP) include glass fiber reinforced plastics (GFRP), carbon fiber reinforced plastics (CFRP), boron fiber reinforced plastics (BFRP), aramid fiber reinforced plastics (AFRP), etc., which are made by compounding various fibers with thermosetting resins such as urethane resin, epoxy resin, vinyl ester resin, unsaturated polyester, polyamide resin, and phenolic resin to improve strength. Examples include molded bodies made from glass fiber or carbon fiber SMC (sheet molding compound).
[0067] Examples of metals include iron, aluminum, copper, magnesium, and titanium. Among these, aluminum and copper are particularly suitable from the viewpoints of light weight and ease of processing. In the present invention, the term "aluminum" is used to include aluminum and its alloys. Similarly, iron, copper, aluminum, magnesium, and titanium are also used to include their simple substances and their alloys (stainless steel, duralumin, etc.).
[0068] Examples of wood include veneer, wood single board, wood plywood, particle board, and wood fiberboard such as MDF (medium density fiberboard), and the like.
[0069] Examples of paper include kraft paper, fine paper, coated paper, and paper with barrier properties (barrier coated paper).
[0070] The resin may be either a thermoplastic resin or a thermosetting resin. Examples of the thermoplastic resin include polyolefin and its acid-modified product, polystyrene, polymethyl methacrylate, AS resin, ABS resin, thermoplastic aromatic polyester such as polyethylene terephthalate and polybutylene terephthalate, polycarbonate, polyimide, polyamide, polyamideimide, polyetherimide, polyethersulfone, polyphenylene ether and its modified product, polyphenylene sulfide, polyoxymethylene, polyarylate, polyether ketone, polyether ether ketone, polyether ketone ketone, thermoplastic epoxy, and fiber reinforcement materials thereof. Examples of the thermosetting resin include epoxy resin, vinyl ester resin, phenol resin, and urethane resin.
[0071] High adhesive strength can sometimes be achieved by pretreating substrate A and substrate B in a way that is appropriate for each substrate. Examples of pretreatment include pretreatment for cleaning the surface of the substrate or pretreatment for making the surface uneven. Specific examples include degreasing treatment, UV ozone treatment, blasting treatment, polishing treatment, plasma treatment, corona discharge treatment, laser treatment, etching treatment, and frame treatment. Only one type of pretreatment may be performed, or two or more types may be performed. Specific methods for these pretreatments can be known methods.
[0072] The degreasing treatment is a method of dissolving and removing dirt such as oil and fat on the surface of the substrate with an organic solvent such as acetone or toluene.
[0073] The UV ozone treatment is a process in which the energy of short-wavelength ultraviolet light emitted from a low-pressure mercury lamp and the ozone (O 3 ) to clean or modify surfaces. In the case of glass, it is one of the surface cleaning methods used to remove organic impurities from the surface. Generally, cleaning and surface modification equipment using low-pressure mercury lamps is called "UV ozone cleaner," "UV cleaning equipment," "ultraviolet light surface modification equipment," etc.
[0074] Examples of the blasting treatment include wet blasting, shot blasting, sand blasting, etc. Among them, wet blasting is preferred because it can provide a denser surface than dry blasting.
[0075] Examples of the polishing treatment include buff polishing using an abrasive cloth, roll polishing using abrasive paper (sandpaper), and electrolytic polishing.
[0076] The plasma treatment involves creating a plasma beam using a high-voltage power supply and a rod, which is then struck on the surface of a material to excite the molecules and put them into a functional state. Examples of such a method include atmospheric pressure plasma treatment, which can impart hydroxyl groups or polar groups to the surface of a material.
[0077] The corona discharge treatment is a method used for surface modification of a polymer film, in which electrons emitted from an electrode cleave the polymer main chain or side chain of the polymer surface layer, generating radicals that generate hydroxyl groups or polar groups on the surface.
[0078] The laser treatment is a technique for improving the surface characteristics by rapidly heating and cooling only the surface of a substrate by laser irradiation, and is an effective method for roughening the surface. Known laser treatment techniques can be used.
[0079] Examples of the etching treatment include chemical etching treatments such as an alkali method, a phosphoric acid-sulfuric acid method, a fluoride method, a chromic acid-sulfuric acid method, and an iron chloride method, and electrochemical etching treatments such as an electrolytic etching method.
[0080] The flame treatment is a method in which oxygen in the air is converted into plasma by burning a mixture of combustion gas and air, and the oxygen plasma is applied to an object to be treated, thereby making the surface hydrophilic. A known flame treatment technique can be used. EXAMPLES
[0081] Next, specific examples of the present invention will be described, but the present invention is not particularly limited to these examples. In the following examples, base material A and base material B are collectively referred to as bonding base materials.
[0082] <Joining base material> The following bonding materials were used: PA6 (6-nylon) A test piece measuring 10 mm in width, 45 mm in length, and 3 mm in thickness was obtained by injection molding using Amilan CM3001G-30 manufactured by Toray Industries, Inc. The test piece was used without surface treatment. In order to efficiently heat the material during ultrasonic welding, linear protrusions with a height of 0.5 mm and an equilateral triangular cross section were created 2.5 mm from the edge. <PBT (Polybutylene terephthalate)> SABIC 20-1001 was injection molded to obtain test pieces with a width of 18 mm, length of 45 mm, and thickness of 1.5 mm. They were used without surface treatment. <PC (Polycarbonate)> SABIC 121R was injection molded to obtain test pieces with a width of 10 mm, a length of 45 mm, and a thickness of 3 mm. They were used without surface treatment. "iron" The surface of the SPCC-SD was blasted to obtain a test piece measuring 10 mm in width, 45 mm in length, and 2.3 mm in thickness. "aluminum" The surface of A6061-T6 was blasted to obtain a test piece with a width of 10 mm, a length of 45 mm, and a thickness of 3 mm.
[0083] <Weight average molecular weight, heat of fusion and epoxy equivalent of thermoplastic epoxy resin and phenoxy resin> The weight average molecular weight, heat of fusion and epoxy equivalent of the film were determined as follows.
[0084] (Weight average molecular weight) The thermoplastic epoxy resin and the phenoxy resin were dissolved in tetrahydrofuran, and the measurement was carried out under the following conditions using Prominence 501 (manufactured by Showa Science Co., Ltd., Detector: Shodex (registered trademark) RI-501 (manufactured by Showa Denko K.K.)). Column: Showa Denko LF-804 x 2 Column temperature: 40℃ Sample: 0.4% by mass of resin in tetrahydrofuran Flow rate: 1ml / min Eluent: Tetrahydrofuran Calibration method: Conversion using standard polystyrene
[0085] (Heat of fusion) 2 to 10 mg of thermoplastic epoxy resin and phenoxy resin were weighed out and placed in an aluminum pan, and the temperature was raised from 23°C to 200°C at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve. The heat of fusion was calculated from the area of the endothermic peak at the time of melting in the DSC curve and the weighed value.
[0086] (epoxy equivalent) The values were measured according to JIS K-7236:2001 and converted into values based on the resin solid content. In the case of simple mixtures that did not involve reactions, the values were calculated from the epoxy equivalent and content of each.
[0087] < Reference example 1 > (Film P-1) In a reaction apparatus equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged, and the temperature was raised to 100°C while stirring under a nitrogen atmosphere. After visually confirming that the mixture had dissolved, the mixture was cooled to 40°C to obtain a resin composition with a solid content of about 20% by mass. The solvent was removed from the mixture to obtain a solid. A non-adhesive fluororesin film (Nitoflon (registered trademark) No. 900UL, manufactured by Nitto Denko Corporation) was placed on the upper and lower plates of a press machine, and the solid was placed on the non-adhesive fluororesin film of the lower plate. The press machine was then heated to 160°C, and the resin composition was heat-compressed for 2 hours to obtain a film (P-1) with a thickness of 100 μm and a solid content of 100% by mass. The weight-average molecular weight was about 37,000. The epoxy equivalent was above the detection limit. No heat of fusion peak was detected by DSC. (zygote) The following three types of junctions were prepared. In addition, for the open time evaluation, a bonded body for open time evaluation was also prepared in the same manner as described in the "Metal-Metal" section below, except that a film was placed on the aluminum substrate (substrate A) and left to stand for 3 days, and then the PC substrate (substrate B) was placed on top. 《Resin / Resin》 Two sheets of the film P-1 cut to a size of 10 x 15 mm were placed on top of the PBT substrate as substrate A, and then the PA6 substrate as substrate B was placed on top of the film P-1 so that the triangular protrusions were placed on top of the PBT substrate. The overlap between these substrates was 10 mm wide and 5 mm deep. The film P-1 was placed so as to cover the entire overlapping area between the substrates. In other words, the substrates A and B were not in direct contact with each other, and the film was interposed between them to prepare an unbonded laminate. In this specification, "promptly thereafter" means within about 30 minutes. The test pieces were joined together by applying heat and pressure using an ultrasonic welding machine (Seidensha Electronics Co., Ltd., oscillator JII930S, press JIIP30S). The amount of penetration was 0.6 mm, and the ultrasonic application time was within 1 second. (The process ended when the penetration was complete, even if it took less than 1 second.) The subsequent holding time was 1 second. The applied pressure was 110 N (pressure 2.2 MPa), and the oscillation frequency was 28.5 kHz. Resin and metal Two sheets of the film P-1 cut to a size of 10 x 15 mm were placed on top of the aluminum substrate as substrate A, and then the PC substrate was placed on top of the aluminum substrate as substrate B. The overlap between these substrates was 10 mm wide and 5 mm deep. The film P-1 was placed so as to cover the entire overlapping area between the substrates. In other words, the substrates A and B were not in direct contact with each other, but the film was interposed between them, and an unbonded laminate was prepared. A high-frequency induction welding machine (Seidensha Denshi Kogyo Co., Ltd., oscillator UH-2.5K, press JIIP30S) was used to heat the metal by high-frequency induction, and the test pieces were joined together by heating and pressurization. The applied pressure was 110 N (pressure 2.2 MPa), and the oscillation frequency was 900 kHz. The oscillation time was 6 seconds. 《Metal / metal》 Three sheets of the film P-1 cut to a size of 10 x 15 mm were placed on top of the aluminum substrate as substrate A, and then the iron substrate was placed on top of them as substrate B. The overlap between these substrates was 10 mm wide and 5 mm deep. The film P-1 was placed so as to cover the entire overlapping area between the substrates. In other words, the substrates A and B were not in direct contact with each other, but the film was interposed between them, and an unbonded laminate was prepared. A high-frequency induction welding machine (Seidensha Denshi Kogyo Co., Ltd., oscillator UH-2.5K, press JIIP30S) was used to heat the metal by high-frequency induction, and the test pieces were joined together by heating and pressing. The applied pressure was 110 N (pressure 2.2 MPa), and the oscillation frequency was 900 kHz. The oscillation time was 5 seconds.
[0088] <Example 2> (Film P-2) In a reaction apparatus equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer, 20 g of Enotote (registered trademark) YP-50S (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 50,000) and 80 g of cyclohexanone were charged, and the temperature was raised to 60°C while stirring, and it was confirmed that it had dissolved visually, and it was cooled to 40°C to obtain a resin composition with a solid content of 20% by mass. The solvent was removed from this to obtain a film-like film (P-2) with a thickness of 100 μm and a solid content of 100% by mass. The weight average molecular weight was 50,000, and the epoxy equivalent was above the detection limit. No heat of fusion peak was detected in DSC. (zygote) Other than using P-2 as the film Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0089] <Example 3> (Film P-3) The resin composition P-2 and a crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 98 to 2 to obtain a film (P-3). The weight average molecular weight was 36,000, the epoxy equivalent was 9600 g / eq, and the heat of fusion was 2 J / g. (zygote) Other than using P-3 as film Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0090] <Example 4> (Film P-4) The resin composition P-2 and a crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 94 to 6 to obtain a film (P-4). The weight average molecular weight was 35,000, the epoxy equivalent was 2100 g / eq, and the heat of fusion was 4 J / g. (zygote) Other than using P-4 as film Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0091] <Example 5> (Film P-5) The resin composition P-2 and a crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 89 to 11 to obtain a film (P-5). The weight average molecular weight was 33,000, the epoxy equivalent was 1745 g / eq, and the heat of fusion was 11 J / g. (zygote) Other than using P-5 as film Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0092] < Reference example 6 > (Film P-6) In a reaction apparatus equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, molecular weight approximately 4060), 0.6 equivalent (12.5 g) of bisphenol S (molecular weight 250), 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged, and the mixture was heated to 100°C while stirring under a nitrogen atmosphere. After visually confirming that the mixture had dissolved, the mixture was cooled to 40°C to obtain a resin composition with a solid content of approximately 20% by mass. The solvent was removed from the mixture to obtain a solid. A non-adhesive fluororesin film (Nitoflon (registered trademark) No. 900UL, manufactured by Nitto Denko Corporation) was placed on the upper and lower plates of a press machine, and the solid was placed on the non-adhesive fluororesin film of the lower plate. The press machine was then heated to 160°C, and the resin composition was heat-compressed for 2 hours to obtain a film (P-6) with a thickness of 100 μm and a solid content of 100% by mass. The weight-average molecular weight was about 30,000, and the epoxy equivalent was above the detection limit. No heat of fusion peak was detected by DSC. (zygote) The method for preparing the composite is as follows: except for using P-6 as the film. Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0093] < Reference example 7 > In preparing the bonded body, two sheets of the film P-1 were placed on the substrate A, and the film was melted by heating it on a hot plate at 200°C for one minute, and then cooled at room temperature for one minute to solidify the film. After bonding the substrate A and the film, the substrate B and the film were laminated so that they were in contact with each other. Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0094] < Reference example 8 > In preparing the bonded structure, one sheet of the film P-1 was placed on each of the substrate A and substrate B, and the films were melted by heating them on a hot plate at 200°C for 1 minute, and then cooled at room temperature for 1 minute to solidify the films, thereby bonding the substrate A and the film, and the substrate B and the film, respectively. Reference example 1 In the same manner as described above, three types of bonded bodies and a bonded body for open time evaluation were prepared.
[0095] <Comparative Example 1> (Film Q-1) Two liquids of thermosetting liquid epoxy adhesive E-250 (Konishi Co., Ltd., two-liquid type of bisphenol type epoxy resin and amine curing agent) were mixed, applied to a release film, cured at 100°C for 1 hour, cooled, and peeled off from the release film to obtain a film-like film (Q-1) with a thickness of 100 μm. No heat of fusion peak was detected by DSC. The epoxy equivalent and weight average molecular weight could not be measured because it was insoluble in the solvent. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that Q-1 was used as the film.
[0096] <Comparative Example 2> (Film Q-2) An amorphous polycarbonate film (Iupilon (registered trademark) FE2000, manufactured by Mitsubishi Engineering Plastics Corporation, thickness 100 μm) was used as the film (Q-2). No heat of fusion peak was detected in the DSC. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that Q-2 was used as the film.
[0097] <Comparative Example 3> (Film Q-3) Crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) was used as the film (Q-3). The epoxy equivalent was 192 g / eq. The weight average molecular weight was 340. The heat of fusion was 70 J / g. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that Q-3 was used as the film.
[0098] <Comparative Example 4> (zygote) Two liquid components of thermosetting liquid epoxy adhesive E-250 (Konishi Corporation, a two-liquid type consisting of bisphenol-type epoxy resin and amine curing agent) were mixed, applied to three types of substrates A and B similar to those in Example 1, and bonded together within one minute. After that, the substrates were fixed with clips and left to stand in an oven at 100°C for one hour to cure the adhesive components, and then cooled to room temperature to produce three types of bonded bodies. In addition, a bonded specimen for open time evaluation was also prepared in the same manner as above, except that the thermosetting liquid epoxy adhesive E-250 was applied to substrate A and substrate B, and then left to stand for 3 days before bonding.
[0099] <Comparative Example 5> In a flask, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged and stirred at room temperature to obtain a liquid resin composition with a solid content of about 20 mass%. The liquid resin composition was bar-coated on each of three types of substrate B similar to those in Example 1, dried at room temperature for 30 minutes, and then left to stand in an oven at 160 ° C. for 2 hours to form a solid thermoplastic epoxy resin polymer coating layer with a thickness of 100 μm on the surface of the substrate B. The weight average molecular weight of the coating layer was about 40,000. The epoxy equivalent was above the detection limit. No heat of fusion peak was detected in DSC. (zygote) Three types of bonded bodies were produced in the same manner as in Example 1, except that the base material A was placed directly on the base material B having the coating layer. In addition, for the open time evaluation, a joint for open time evaluation was also prepared in the same manner as above, except that a thermoplastic epoxy resin polymer coating layer was formed on the surface of substrate B, allowed to stand for 3 days, and then laminated with substrate A.
[0100] <Comparative Example 6> A reactor equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer was charged with 20 g of FENOTOTE (registered trademark) YP-50S (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 50,000) and 80 g of cyclohexanone, and the temperature was raised to 60°C while stirring. Dissolution was confirmed visually, and the mixture was cooled to 40°C to obtain a liquid resin composition with a solid content of 20% by mass. The liquid resin composition was bar-coated on each of three types of substrate B similar to those in Example 1, and the substrate was left to stand in an oven at 70°C for 30 minutes to form a phenoxy resin coating layer with a thickness of 100 μm on the surface of the substrate B. The weight average molecular weight of the coating layer was about 50,000. The epoxy equivalent was above the detection limit. No heat of fusion peak was detected in DSC. (zygote) Three types of bonded bodies were produced in the same manner as in Example 1, except that the base material A was placed directly on the base material B having the phenoxy resin coating layer. In addition, for the open time evaluation, a joint for open time evaluation was also prepared in the same manner as above, except that a phenoxy resin coating layer was formed on the surface of substrate B, which was then left to stand for 3 days, and then laminated with substrate A.
[0101] <Comparative Example 7> (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that a crystalline polyamide-based hot melt adhesive film NT-120 (manufactured by Nihon Matai Co., Ltd., thickness 100 μm) was used as the film. The heat of fusion was 60 J / g.
[0102] [Shear adhesive strength] The bonded bodies obtained in Examples 1 to 8 and Comparative Examples 1 to 7 were allowed to stand at the measurement temperature (23°C or 80°C) for 30 minutes or more, and then a tensile shear adhesive strength test was performed in an atmosphere of 23°C and 80°C in accordance with ISO19095 using a tensile testing machine (Universal testing machine autograph "AG-X plus" (manufactured by Shimadzu Corporation); load cell 10 kN, tensile speed 10 mm / min) to measure the bond strength. The measurement results are shown in Table 1.
[0103] [Joining process time] The bonding process time was measured as follows. The time from the start point when the bonding agent contacted at least one of the substrates that constitute the bonded body to the end point when the fabrication of the bonded body was completed was set as the start point, and the time from the start point to the end point was measured. The measurement results are shown in Tables 1-1 and 1-2.
[0104] [Recyclability] Each of the aluminum and iron joints was placed on a hot plate at 200°C and heated for 1 minute, after which it was judged whether it could be easily peeled off with a force of 1 N or less. If it could be peeled off, it was rated as good (A), and if it could not be peeled off, it was rated as unsatisfactory (B). The evaluation results are shown in Tables 1-1 and 1-2.
[0105] [Repairability] Of the test pieces (in which a layer of the bonded solid remains on the surface of the first substrate or the second substrate or both) whose adhesive surface broke after the tensile shear strength test at 23°C, the first substrate was placed on the second substrate, and a bonded body was prepared in the same manner as in Example 1 to obtain a repaired bonded body. The shear adhesive strength of the repaired bonded body at 23°C was measured in the same manner as in the test method, and if it was 80% or more of the first shear adhesive strength, it was judged as good (A), and if it was less than 80%, it was judged as unsatisfactory (B). The evaluation results are shown in Tables 1-1 and 1-2.
[0106] [Open Time Evaluation] The tensile shear adhesive strength test was carried out at 23°C using the bonded bodies for open time evaluation. If the shear adhesive strength was 80% or more compared to the test pieces prepared by the methods of the examples and comparative examples, it was rated as good (A), and if it was less than 80%, it was rated as unsuitable (B). A good open time rating (A) means that the open time is long and the convenience is excellent. The evaluation results are shown in Tables 1-1 and 1-2.
[0107] [Table 1-1]
[0108] [Table 1-2] [Industrial Applicability]
[0109] The joined body obtained by the manufacturing method of the present invention can be used, for example, as door side panels, bonnet roofs, tailgates, steering hangers, A-pillars, B-pillars, C-pillars, D-pillars, crash boxes, power control unit (PCU) housings, electric compressor components (inner wall portions, intake port portions, exhaust control valve (ECV) insertion portions, mount boss portions, etc.), lithium ion battery (LIB) spacers, battery cases, LED headlamps, and other automotive parts, as well as smartphones, notebook computers, tablet computers, smart watches, large liquid crystal televisions (LCD-TVs), and outdoor LED lighting structures, but is not limited to these exemplified uses. [Explanation of symbols]
[0110] 1 zygote 2 Adhesive layer 3 Base material A 4 Base material B
Claims
1. a pre-bonding process of preparing a laminate by arranging, in this order, a substrate A (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers), a plurality of films including film A and film B, and a substrate B (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers); a bonding step of heating and pressurizing the laminate to melt the film and bond the base material A and the base material B together, The plurality of films including the film A and the film B contain a phenoxy resin as an amorphous thermoplastic resin in an amount of 80 mass% or more based on the resin component, The content of each of the resin components in the film is 20% by mass or more, the resin component has an epoxy equivalent of 1,600 or more, or the resin component does not contain an epoxy group, and the resin component has a heat of fusion of 15 J / g or less; The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film, The bonding is performed by heating the molten film to wet and spread on the adhesive surfaces of the substrate A and the substrate B, and then solidifying on the adhesive surfaces. the content of the amide-based compound in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin; The content of γ-butyrolactone in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin. A method for manufacturing a joint body.
2. The method for producing a bonded body according to claim 1, wherein the heating and pressing are carried out under conditions of 100 to 400° C. and 0.01 to 20 MPa.
3. A method for producing a bonded body, which is obtained by bonding, in this order, a substrate A (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers), a plurality of films including a film A and a film B, and a substrate B (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers), the method comprising the steps of: In a state where a plurality of films including the film A and the film B are brought into contact with the substrate A, a first bonding step of bonding the base material A and the plurality of films including the film A and the film B by melting and then solidifying the plurality of films including the film A and the film B; a second bonding step of bonding the substrate A and the substrate B by melting and then solidifying the plurality of films including the film A and the film B bonded to the substrate A in a state in which the plurality of films including the film A and the film B are brought into contact with the substrate B, The plurality of films including the film A and the film B contain a phenoxy resin as an amorphous thermoplastic resin in an amount of 80% by mass or more based on the resin component, The content of each of the resin components in the film is 20% by mass or more, the resin component has an epoxy equivalent of 1,600 or more, or the resin component does not contain an epoxy group, and the resin component has a heat of fusion of 15 J / g or less; The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film, The bonding is performed by heating the molten film to wet and spread on the adhesive surfaces of the substrate A and the substrate B, and then solidifying on the adhesive surfaces. the content of the amide-based compound in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin; The content of γ-butyrolactone in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin. A method for manufacturing a joint body.
4. In the first bonding step, a plurality of films including the film A and the film B are bonded to each other. The method for producing a joint body according to claim 3, wherein the material is heated to 100 to 300° C. to melt and then solidify.
5. A method for producing a bonded body, which is obtained by bonding, in this order, a substrate A (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers), a plurality of films including a film A and a film B, and a substrate B (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers), the method comprising the steps of: a first bonding step of bonding the film A or the plurality of films including the film A to the substrate A by melting and then solidifying the film A or the plurality of films including the film A in a state in which the film A or the plurality of films including the film A is brought into contact with the substrate A; a first bonding step of bonding the film B or the plurality of films including the film B to the substrate B by melting and then solidifying the film B or the plurality of films including the film B in a state in which the film B or the plurality of films including the film B is brought into contact with the substrate B; a second bonding step of bonding the substrate A and the substrate B by melting and then solidifying the film A or the multiple films including film A and the film B or the multiple films including film B in a state in which the film A bonded to the substrate A or the multiple films including film A are brought into contact with the film B or the multiple films including film B bonded to the substrate B, The plurality of films including the film A and the film B contain a phenoxy resin as an amorphous thermoplastic resin in an amount of 80% by mass or more based on the resin component, The content of each of the resin components in the film is 20% by mass or more, the resin component has an epoxy equivalent of 1,600 or more, or the resin component does not contain an epoxy group, and the resin component has a heat of fusion of 15 J / g or less; The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film, The bonding is performed by heating the molten film to wet and spread on the adhesive surfaces of the substrate A and the substrate B, and then solidifying on the adhesive surfaces. the content of the amide-based compound in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin; The content of γ-butyrolactone in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin. A method for manufacturing a joint body.
6. 6. The method for producing a joined body according to claim 5, wherein in the 1A joining step and the 1B joining step, the film A or the multiple films including the film A and the film B or the multiple films including the film B are heated to 100 to 300° C. to melt and then solidify.
7. In the second bonding step, a plurality of films including the film A and the film B are bonded to each other.
6. The method for producing a joined body according to claim 3 or 5, wherein the material is melted and then solidified by at least one method selected from the group consisting of contact heating, hot air heating, heat pressing, infrared heating, hot plate welding, ultrasonic welding, vibration welding and high frequency induction welding.
8. 6. The method for producing a joined body according to claim 3, wherein in the second joining step, the films including the film A and the film B are heated at a temperature equal to or higher than the melting point of the films, and then solidified after melting.
9. 6. The method for producing a joined body according to claim 3 or 5, wherein in the second joining step, a plurality of films including the film A and the film B are melted and then solidified at a heating temperature of 100 to 400° C. and under a pressure of 0.01 to 20 MPa.
Citation Information
Patent Citations
Bonding of plate
JP1980012147A
Adhesion and surface working method for cloth
JP1981053072A
Prepreg and laminate
JP1998017685A
Hot-melt adhesive
JP1998168417A
Plant binding sheet
JP2009189288A