Electrochemical Cell Device
Patent Information
- Application Number
- JP2022515207
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-15
- Filing Date
- 2021-01-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-01-19
Smart Images

Figure 0007552687000009 
Figure 0007552687000010 
Figure 0007552687000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrochemical cell device. This application claims priority to Japanese Patent Application No. 2020-072919, filed on April 15, 2020. The entire contents of the Japanese Patent Application are incorporated herein by reference. [Background technology]
[0002] Patent Document 1 (WO 2019 / 244480) describes a fuel cell. The fuel cell described in Patent Document 1 has a solid electrolyte layer, an anode and a cathode, an anode-side current collector, and a cathode-side current collector.
[0003] The anode and cathode sandwich a solid electrolyte layer (hereinafter, the solid electrolyte layer sandwiched between the anode and cathode is referred to as a "cell"). The anode-side current collector and cathode-side current collector sandwich the cell. The anode-side current collector and cathode-side current collector are made of a porous metal sheet made of a porous metal having a skeleton with a three-dimensional mesh structure. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2019 / 244480 Summary of the Invention
[0005] The electrochemical cell device of the present disclosure includes a cell having a first main surface and a second main surface opposite to the first main surface, a first current collector having a third main surface facing the first main surface, and a second current collector having a fourth main surface facing the second main surface. The cell is warped convexly from the second main surface toward the first main surface. The third main surface includes a recess at a position facing the center of the first main surface. The fourth main surface includes a protrusion at a position facing the center of the second main surface. Each of the first current collector and the second current collector is composed of at least one metal porous body sheet made of a metal porous body having a skeleton of a three-dimensional mesh structure. The center of the first main surface includes a portion of the first main surface that is the largest distance from the reference surface when the cell is placed on the reference surface so that the second main surface faces the flat reference surface. The center of the second main surface includes a portion of the second main surface that is the largest distance from the reference surface when the cell is placed on the reference surface so that the second main surface faces the reference surface. [Brief description of the drawings]
[0006] [Figure 1A] FIG. 1A is a cross-sectional view of an electrochemical cell device 100. [Figure 1B] FIG. 1B is an enlarged cross-sectional view of cell 10. [Diagram 2] FIG. 2 is a plan view of cell 10. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing the warped shape of the cell 10. In FIG. [Figure 4] FIG. 4 is a plan view of the current collector 20. [Diagram 5] FIG. 5 is a cross-sectional view taken along line VV of FIG. [Figure 6] FIG. 6 is a plan view of the current collector 30. [Figure 7] FIG. 7 is a cross-sectional view taken along line VII-VII of FIG. [Figure 8] FIG. 8 is a plan view of a current collector 20 of an electrochemical cell device 200. [Figure 9] FIG. 9 is a cross-sectional view taken along line IX-IX of FIG. [Figure 10]FIG. 10 is a plan view of a current collector 30 of an electrochemical cell device 200. [Figure 11] FIG. 11 is a cross-sectional view taken along line XI-XI of FIG. [Figure 12] FIG. 12 is a cross-sectional view of a current collector 20 of an electrochemical cell device 300. [Figure 13] FIG. 13 is a cross-sectional view of a current collector 30 of an electrochemical cell device 300. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] [Problem that this disclosure aims to solve] In the fuel cell described in Patent Document 1, the cells may be warped. When the cells are warped, gaps are formed between the cells and the anode-side current collector and between the cells and the cathode-side current collector (deteriorating contact between the cells and the current collectors).
[0008] The present disclosure provides an electrochemical cell device that allows for reduced gaps between the cell and the current collector. [Effects of this disclosure] The electrochemical cell device of the present disclosure allows for a reduction in the gap between the cell and the current collector.
[0009] [Description of the embodiments of the present disclosure] First, embodiments of the present disclosure will be listed and described.
[0010] (1) An electrochemical cell device according to an embodiment includes a cell having a first main surface and a second main surface opposite to the first main surface, a first current collector having a third main surface facing the first main surface, and a second current collector having a fourth main surface facing the second main surface. The cell is warped convexly from the second main surface toward the first main surface. The third main surface includes a recess at a position facing the center of the first main surface. The fourth main surface includes a protrusion at a position facing the center of the second main surface. Each of the first current collector and the second current collector is made of at least one metal porous body sheet made of a metal porous body having a skeleton with a three-dimensional mesh structure. The center of the first main surface includes a portion of the first main surface that is the largest distance from the reference surface when the cell is placed on the reference surface so that the second main surface faces the flat reference surface. The central portion of the second main surface includes a portion of the second main surface that is the largest distance from the reference surface when the cell is placed on the reference surface so that the second main surface faces the reference surface.
[0011] According to the electrochemical cell device of (1) above, it is possible to reduce the gap between the cell and the current collector.
[0012] (2) In the electrochemical cell device of (1), at least one of the porous metal sheets constituting the first current collector may be a first porous metal sheet and a second porous metal sheet. The first porous metal sheet and the second porous metal sheet may be arranged side by side in a plane perpendicular to the thickness direction of the first current collector. The second porous metal sheet may have a first through hole formed therein that penetrates the second porous metal sheet in the thickness direction at a position corresponding to the recess. The first porous metal sheet may be arranged in the first through hole. The thickness of the second porous metal sheet may be greater than the thickness of the first porous metal sheet. The recess may be defined by the inner peripheral surface of the first through hole and the main surface of the first porous metal sheet.
[0013] According to the electrochemical cell device of (2) above, it is possible to reduce the gap between the cell and the current collector.
[0014] (3) In the electrochemical cell device of (2) above, the thickness of the second porous metal sheet minus the thickness of the first porous metal sheet may be equal to the amount of warping of the cell.
[0015] According to the electrochemical cell device of (3) above, it is possible to further reduce the gap between the cell and the current collector.
[0016] (4) In the electrochemical cell device of (1) above, at least one of the porous metal sheets constituting the first current collector may be a first porous metal sheet and a second porous metal sheet. The first porous metal sheet and the second porous metal sheet may be overlapped in the thickness direction of the first current collector such that the second porous metal sheet is located on the third main surface side. The second porous metal sheet may have a first through hole formed therein that penetrates the second porous metal sheet in the thickness direction at a position corresponding to the recess.
[0017] (5) In the electrochemical cell device according to (1) to (4), at least one of the porous metal sheets constituting the second current collector may be a third porous metal sheet and a fourth porous metal sheet. The third porous metal sheet and the fourth porous metal sheet may be arranged side by side in a plane perpendicular to the thickness direction of the second current collector. The fourth porous metal sheet may have a second through hole formed therein at a position corresponding to the protrusion, the second through hole penetrating the fourth porous metal sheet in the thickness direction. The third porous metal sheet may be arranged within the second through hole. The thickness of the third porous metal sheet may be greater than the thickness of the fourth porous metal sheet.
[0018] According to the electrochemical cell device of (5) above, it is possible to reduce the gap between the cell and the current collector.
[0019] (6) In any of the electrochemical cell devices (1) to (4) above, the value obtained by subtracting the thickness of the fourth porous metal sheet from the thickness of the third porous metal sheet may be equal to the amount of warping of the cell.
[0020] According to the electrochemical cell device of (6) above, it is possible to further reduce the gap between the cell and the current collector.
[0021] (7) In the electrochemical cell device according to any one of (1) to (4), the at least one porous metal sheet constituting the second current collector may be a third porous metal sheet and a fourth porous metal sheet. The third porous metal sheet and the fourth porous metal sheet may be overlapped in the thickness direction of the second current collector such that the fourth porous metal sheet is located on the fourth main surface side. The fourth porous metal sheet may form a protrusion.
[0022] According to the electrochemical cell device of (7) above, it is possible to reduce the gap between the cell and the current collector.
[0023] (8) In the electrochemical cell device according to any one of (1) to (7) above, the first current collector may be a cathode side current collector, and the second current collector may be an anode side current collector.
[0024] According to the electrochemical cell device of (8) above, it is possible to reduce the gap between the cell and the current collector.
[0025] (9) In the electrochemical cell device of (8) above, the skeleton of each of the at least one porous metal sheet constituting the first current collector may contain nickel and cobalt. The basis weight of each of the at least one porous metal sheet constituting the first current collector is 900 g / m 2 It may be the following.
[0026] According to the electrochemical cell device of (9) above, it is possible to reduce the gap between the cell and the current collector.
[0027] (10) In the electrochemical cell device of (8) above, the skeleton of each of the at least one porous metal sheet constituting the second current collector may contain nickel. The weight of each of the at least one porous metal sheet constituting the second current collector is 1000 g / m 2It may be the following.
[0028] (11) In the electrochemical cell device according to any one of (1) to (10) above, the value obtained by dividing the amount of warping of the cell by the maximum width of the cell in a plan view may be 1 / 1000 or more.
[0029] According to the electrochemical cell device of (11) above, even if the cell is significantly warped, it is possible to reduce the gap between the cell and the current collector.
[0030] (12) The electrochemical cell device according to any one of (1) to (11) above may be a solid oxide fuel cell.
[0031] According to the electrochemical cell device of (12) above, the contact between the cell and the current collector is improved, so that the output voltage in the solid oxide fuel cell can be increased.
[0032] (13) The electrochemical cell device according to any one of (1) to (11) above may be a solid oxide electrolysis cell.
[0033] According to the electrochemical cell device of (13) above, the contact between the cell and the current collector is improved, so that the electrolysis voltage in the solid oxide electrolysis cell can be reduced.
[0034] [Details of the embodiment of the present disclosure] Next, an embodiment of the present disclosure will be described with reference to the drawings. Here, the same or corresponding parts are designated by the same reference numerals, and overlapping descriptions will not be repeated.
[0035] (First embodiment) The configuration of the electrochemical cell device according to the first embodiment (hereinafter referred to as "electrochemical cell device 100") will be described below.
[0036] The electrochemical cell device 100 is a solid oxide fuel cell (SOFC). The electrochemical cell device 100 may be a solid oxide electrolysis cell (SOEC), but in the following, an SOFC will be described as an example of the electrochemical cell device 100.
[0037] FIG. 1A is a cross-sectional view of an electrochemical cell device 100. FIG. 1A shows the structure of a unit cell included in the electrochemical cell device 100. The electrochemical cell device 100 is configured by stacking a plurality of unit cell structures. Also, in FIG. 1A, warping of the cell 10 and recesses 20c and protrusions 30c, which will be described later, are omitted. FIG. 1B is an enlarged cross-sectional view of the cell 10. As shown in FIGS. 1A and 1B, the electrochemical cell device 100 includes a cell 10, a current collector 20, a current collector 30, an interconnector 40, and an interconnector 50.
[0038] The cell 10 has a principal surface 10a and a principal surface 10b. The principal surface 10b is the surface opposite to the principal surface 10a. The cell 10 has a solid electrolyte layer 11, a cathode 12, an anode 13, and an intermediate layer 14.
[0039] The solid electrolyte layer 11 is a layer formed of a solid electrolyte. For example, the solid electrolyte layer 11 is formed of an oxide of zirconium (Zr) doped with yttrium (Y) (YSZ). The cathode 12 is formed of, for example, an oxide of lanthanum (La), strontium (Sr), and cobalt (Co) (LSC). The anode 13 is formed of, for example, a mixture of YSZ and an oxide of nickel (Ni2O). The intermediate layer 14 is formed of, for example, an oxide of cerium (Ce) doped with gadolinium (Gd) (GDC).
[0040] The cathode 12 constitutes a main surface 10a of the cell 10. The anode 13 constitutes a main surface 10b of the cell 10. The solid electrolyte layer 11 is disposed between the cathode 12 and the anode 13. An intermediate layer 14 is disposed between the solid electrolyte layer 11 and the cathode 12. The solid electrolyte layer 11 and the anode 13 are in contact with each other.
[0041] Fig. 2 is a plan view of the cell 10. As shown in Fig. 2, the cell 10 has a circular shape in a plan view. However, the planar shape of the cell 10 is not limited to this. The cell 10 may have a rectangular shape in a plan view.
[0042] Fig. 3 is a schematic cross-sectional view showing the warped shape of the cell 10. As shown in Fig. 3, the cell 10 is warped. For example, the cell 10 is warped convexly from the main surface 10b side toward the main surface 10a side. The amount of warping of the cell 10 (hereinafter referred to as "warping amount WA") is, for example, 100 µm or more. The amount of warping WA may be 1000 µm or more.
[0043] The amount of warpage WA is measured by the following method. First, the cell 10 is placed on a flat reference surface. Second, the distance (hereinafter referred to as "distance L") between the position on the main surface 10a farthest from the reference surface (hereinafter referred to as "vertex P") and the reference surface is measured using a Keyence LK-G35. The vertex P is located at the center of the cell 10 (the center of the main surface 10a) in a planar view. Third, the thickness of the cell 10 (hereinafter referred to as "thickness T") is subtracted from the distance L. This allows the amount of warpage WA to be measured.
[0044] The maximum width of the cell 10 in plan view is width W max (See Figure 2.) The amount of warping WA is the width W max The value obtained by dividing the amount of warp WA by the width W is, for example, 1 / 1000 or more. max The value divided by may be 1 / 100 or more. max When the planar shape of the cell 10 is a circle, the width W is equal to the diameter of the circle. When the planar shape of the cell is a rectangle, the width W max is equal to the length of the diagonal of the rectangle.
[0045] 1A, current collector 20 is disposed on main surface 10a, and current collector 30 is disposed on main surface 10b. From another perspective, cell 10 is sandwiched between current collector 20 and current collector 30. Current collector 20 is a cathode side current collector, and current collector 30 is an anode side current collector.
[0046] The current collector 20 has a principal surface 20a and a principal surface 20b. The principal surface 20a faces the principal surface 10a. The principal surface 20b is the opposite surface to the principal surface 20a. FIG. 4 is a plan view of the current collector 20. FIG. 5 is a cross-sectional view taken along line VV in FIG. 4. As shown in FIGS. 4 and 5, the principal surface 20a has a recess 20c. The principal surface 20a is recessed toward the principal surface 20b at the recess 20c. The recess 20c is disposed at a position facing the center of the principal surface 10a.
[0047] The current collector 20 is composed of a porous metal sheet 21 and a porous metal sheet 22. The porous metal sheet 21 and the porous metal sheet 22 are each formed of a porous metal having a skeleton with a three-dimensional mesh structure.
[0048] The porous metal skeleton constituting the porous metal sheet 21 and the porous metal sheet 22 contains, for example, nickel (Ni) and cobalt. The porous metal sheet 21 and the porous metal sheet 22 preferably have a basis weight of 900 g / m 2 The basis weight of the porous metal sheet 21 (porous metal sheet 22) is the value obtained by dividing the weight of the porous metal sheet 21 (porous metal sheet 22) by the area of the main surface of the porous metal sheet 21 (porous metal sheet 22).
[0049] The current collector 20 is circular in plan view. The porous metal sheet 21 is circular in plan view. The porous metal sheet 22 is annular in plan view. That is, the porous metal sheet 22 has a through hole 22a penetrating the porous metal sheet 22 in the thickness direction. The through hole 22a is formed at a position corresponding to the recess 20c.
[0050] The thickness of the porous metal sheet 22 (hereinafter referred to as "thickness T2") is greater than the thickness of the porous metal sheet 21 (hereinafter referred to as "thickness T1"). The porous metal sheet 21 and the porous metal sheet 22 are arranged side by side (without overlapping) in a plane perpendicular to the thickness direction of the current collector 20. The porous metal sheet 21 is arranged in the through hole 22a. Therefore, the porous metal sheet 21 and the through hole 22a form a recess 20c.
[0051] The current collector 30 has a principal surface 30a and a principal surface 30b. The principal surface 30a faces the principal surface 10b. The principal surface 30b is the opposite surface to the principal surface 30a. FIG. 6 is a plan view of the current collector 30. FIG. 7 is a cross-sectional view taken along line VII-VII in FIG. 6. As shown in FIGS. 6 and 7, the principal surface 30a has a protrusion 30c. The principal surface 30a protrudes at the protrusion 30c on the opposite side to the principal surface 30b. The protrusion 30c is disposed at a position facing the center of the principal surface 10b.
[0052] The current collector 30 is composed of a porous metal sheet 31 and a porous metal sheet 32. The porous metal sheet 31 and the porous metal sheet 32 are each formed of a porous metal having a skeleton with a three-dimensional mesh structure.
[0053] The metal porous body skeleton constituting the metal porous body sheet 31 and the metal porous body sheet 32 contains, for example, nickel. The metal porous body sheet 31 and the metal porous body sheet 32 preferably have a basis weight of 1000 g / m 2The basis weight of the porous metal sheet 31 (porous metal sheet 32) is the value obtained by dividing the weight of the porous metal sheet 31 (porous metal sheet 32) by the area of the main surface of the porous metal sheet 31 (porous metal sheet 32).
[0054] The current collector 30 is circular in plan view. The porous metal sheet 31 is circular in plan view. The porous metal sheet 32 is annular in plan view. That is, the porous metal sheet 32 has through holes 32a penetrating the porous metal sheet 32 in the thickness direction. The through holes 32a are formed at positions corresponding to the protrusions 30c.
[0055] The thickness of the porous metal sheet 31 (hereinafter referred to as "thickness T3") is greater than the thickness of the porous metal sheet 32 (hereinafter referred to as "thickness T4"). The porous metal sheet 31 and the porous metal sheet 32 are arranged side by side (not overlapping) in a plane perpendicular to the thickness direction of the current collector 30. The porous metal sheet 31 is arranged in the through hole 32a. Therefore, the porous metal sheet 31 forms the protrusion 30c.
[0056] The value obtained by subtracting thickness T1 from thickness T2 is preferably equal to the amount of warping WA. The value obtained by subtracting thickness T4 from thickness T3 is preferably equal to the amount of warping WA. If the value obtained by subtracting thickness T1 from thickness T2 is within the range of 0.95 to 1.05 times the amount of warping WA, it is included in "the value obtained by subtracting thickness T1 from thickness T2 is equal to the amount of warping WA", and if the value obtained by subtracting thickness T4 from thickness T3 is within the range of 0.95 to 1.05 times the amount of warping WA, it is included in "the value obtained by subtracting thickness T4 from thickness T3 is equal to the amount of warping WA".
[0057] The porous metal sheet 22 may be divided into a plurality of concentrically arranged porous metal sheets. In this case, the porous metal sheets arranged closer to the outside are thicker. The porous metal sheet 32 may be divided into a plurality of concentrically arranged porous metal sheets. In this case, the porous metal sheets arranged closer to the outside are thinner.
[0058] 1A, the interconnector 40 is disposed on the main surface 20b, and the interconnector 50 is disposed on the main surface 30b. From another perspective, the cell 10, the current collector 20, and the current collector 30 are sandwiched between the interconnector 40 and the interconnector 50. A groove 41 is formed in the main surface of the interconnector 40 facing the current collector 20, and a groove 51 is formed in the main surface of the interconnector 50 facing the current collector 30. The interconnector 40 and the interconnector 50 are made of a conductive material.
[0059] The effects of the electrochemical cell device 100 will be described below. In the electrochemical cell device 100, the cell 10 is convex from the main surface 10b to the main surface 10a, so that when the main surfaces 20a and 30a are flat, gaps are generated between the main surfaces 10a and 20a and between the main surfaces 10b and 30a. As a result, the contact electric resistance between the cell 10 and the current collector 20 and the contact electric resistance between the cell 10 and the current collector 30 increase, and the output voltage from the electrochemical cell device 100 decreases.
[0060] However, in the electrochemical cell device 100, since the main surface 20a has the recess 20c and the main surface 30a has the protrusion 30c, the main surface 20a easily conforms to the shape of the main surface 10a and the main surface 30a easily conforms to the shape of the main surface 10b, and as a result, the gaps between the main surface 10a and the main surface 20a and between the main surface 10b and the main surface 30a are reduced.
[0061] Therefore, according to the electrochemical cell device 100, the contact electrical resistance between the cell 10 and the current collector 20 and the contact electrical resistance between the cell 10 and the current collector 30 are reduced, and the output voltage from the electrochemical cell device 100 can be improved.
[0062] In addition, when the electrochemical cell device 100 is an SOEC, the contact electrical resistance value between the cell 10 and the current collector 20 and the contact electrical resistance value between the cell 10 and the current collector 30 are reduced, and as a result, the electrolysis voltage in the electrochemical cell device 100 can be reduced.
[0063] The skeleton of the porous metal of the porous metal sheet 21 and the porous metal sheet 22 contains nickel and cobalt, and the weight of the porous metal of the porous metal sheet 21 and the porous metal sheet 22 is 900 g / m 2 When it is equal to or less than this, the deformability of the porous metal sheets 21 and 22 can be ensured, so that the main surface 20a can more easily conform to the shape of the main surface 10a.
[0064] The skeleton of the porous metal of the porous metal sheet 31 and the porous metal sheet 32 contains nickel, and the weight of the porous metal of the porous metal sheet 31 and the porous metal sheet 32 is 900 g / m 2 When it is equal to or less than this, the deformability of the porous metal sheets 31 and 32 can be ensured, so that the main surface 30a can more easily conform to the shape of the main surface 10b.
[0065] (Power generation test) A power generation test carried out to confirm the effects of the electrochemical cell device 100 will be described below.
[0066] <Sample> For the power generation test, electrochemical cells of Samples 1 to 6 were used. In Samples 1 to 6, the shapes of the cell 10, the current collector 20, and the current collector 30 were as shown in Table 1. Although not shown in Table 1, in all of Samples 1 to 6, the thickness and diameter of the cell 10 were 0.4 mm and 100 mm, respectively.
[0067] [Table 1]
[0068] As shown in Table 1, the warpage WA was set to 100 μm in Samples 1 and 5. The warpage WA was set to 300 μm in Sample 2. The warpage WA was set to 1000 μm in Samples 3 and 6. The warpage WA was set to 2000 μm in Sample 4.
[0069] In sample 1, a porous metal sheet 21 having a thickness of 400 μm and a porous metal sheet 22 having a thickness of 500 μm were used as the current collector 20, and a porous metal sheet 31 having a thickness of 500 μm and a porous metal sheet 32 having a thickness of 400 μm were used as the current collector 30.
[0070] In sample 2, a porous metal sheet 21 having a thickness of 200 μm and a porous metal sheet 22 having a thickness of 500 μm were used as the current collector 20, and a porous metal sheet 31 having a thickness of 500 μm and a porous metal sheet 32 having a thickness of 200 μm were used as the current collector 30.
[0071] In sample 3, a porous metal sheet 21 having a thickness of 100 μm and a porous metal sheet 22 having a thickness of 1100 μm were used as the current collector 20, and a porous metal sheet 31 having a thickness of 1100 μm and a porous metal sheet 32 having a thickness of 100 μm were used as the current collector 30.
[0072] In sample 4, a porous metal sheet 21 having a thickness of 100 μm and a porous metal sheet 22 having a thickness of 2100 μm were used as the current collector 20, and a porous metal sheet 31 having a thickness of 2100 μm and a porous metal sheet 32 having a thickness of 100 μm were used as the current collector 30.
[0073] In sample 5, one porous metal sheet having a thickness of 500 μm was used as the current collector 20, and one porous metal sheet having a thickness of 500 μm was used as the current collector 30.
[0074] In sample 6, one porous metal sheet having a thickness of 1100 μm was used as the current collector 20, and one porous metal sheet having a thickness of 1100 μm was used as the current collector 30.
[0075] <Test Results> Table 2 shows that the current between the anode and cathode is 0.5 A / cm at 750°C. 2 The initial value of the anode-cathode output voltage when a current of
[0076] [Table 2]
[0077] As shown in Table 2, the output voltage of Sample 1 was greater than the output voltage of Sample 5. The output voltage of Sample 3 was greater than the output voltage of Sample 6.
[0078] From this comparison, it was experimentally demonstrated that when the main surface 20a of the current collector 20 has a concave portion 20c and the main surface 30a of the current collector 30 has a convex portion 30c, the gap between the cell 10 and the current collector 20 and the gap between the cell 10 and the current collector 30 are reduced, and the output voltage from the electrochemical cell device 100 is increased.
[0079] As the warpage WA increases, gaps become more likely to form between the cell 10 and the current collector 20 and between the cell 10 and the current collector 30, while the surface area of the cell 10 that contributes to the electrochemical reaction increases.
[0080] The output voltage of sample 6 was smaller than the output voltage of sample 5. This is believed to be because the amount of warping WA in sample 6 was larger than the amount of warping WA in sample 5, so that the gap between the cell 10 and the current collector 20 and the gap between the cell 10 and the current collector 30 increased, and the contact electrical resistance between the cell 10 and the current collector 20 and the contact electrical resistance between the cell 10 and the current collector 30 increased.
[0081] On the other hand, in Samples 1 to 4, the output voltage increased as the amount of warpage WA increased. In all of Samples 1 to 4, the value obtained by subtracting thickness T1 from thickness T2 and the value obtained by subtracting thickness T4 from thickness T3 were equal to the amount of warpage WA.
[0082] From this, it has been experimentally demonstrated that by increasing the amount of warping WA while matching the value obtained by subtracting thickness T1 from thickness T2 and the value obtained by subtracting thickness T4 from thickness T3 to the amount of warping WA, it is possible to increase the surface area of cell 10 contributing to the electrochemical reaction while reducing the gap between cell 10 and current collector 20 and the gap between cell 10 and current collector 30, in other words, to further increase the output voltage from electrochemical cell device 100.
[0083] Second embodiment The configuration of an electrochemical cell device according to a second embodiment (hereinafter referred to as "electrochemical cell device 200") will be described below. Here, differences from the configuration of the electrochemical cell device 100 will be mainly described, and overlapping descriptions will not be repeated.
[0084] The electrochemical cell device 200 includes a cell 10, a current collector 20, a current collector 30, an interconnector 40, and an interconnector 50. The cell 10 is warped convexly from the main surface 10b toward the main surface 10a. The main surface 20a has a recess 20c, and the main surface 30a has a protrusion 30c. In these respects, the configuration of the electrochemical cell device 200 is common to the configuration of the electrochemical cell device 100.
[0085] Fig. 8 is a plan view of the current collector 20 of the electrochemical cell device 200. Fig. 9 is a cross-sectional view taken along line IX-IX of Fig. 8. As shown in Fig. 8 and Fig. 9, in the electrochemical cell device 200, the current collector 20 has a porous metal sheet 23 and a porous metal sheet 24. The porous metal sheet 23 is, for example, circular in plan view. The porous metal sheet 24 is, for example, annular in plan view.
[0086] The porous metal sheet 24 has through holes 24a formed therein, which penetrate the porous metal sheet 24 in the thickness direction. The through holes 24a are arranged at positions corresponding to the recesses 20c. The porous metal sheet 23 and the porous metal sheet 24 are arranged to overlap in the thickness direction of the current collector 20. The porous metal sheet 24 is arranged on the main surface 20a side. As a result, the through holes 24a and the porous metal sheet 23 form the recesses 20c.
[0087] Fig. 10 is a plan view of the current collector 30 of the electrochemical cell device 200. Fig. 11 is a cross-sectional view taken along line XI-XI of Fig. 10. As shown in Figs. 10 and 11, the current collector 30 has a porous metal sheet 33 and a porous metal sheet 34. The porous metal sheet 33 and the porous metal sheet 34 are, for example, circular in plan view. The diameter of the porous metal sheet 33 is larger than the diameter of the porous metal sheet 34.
[0088] The porous metal sheet 33 and the porous metal sheet 34 are overlapped in the thickness direction of the current collector 30. The porous metal sheet 34 is disposed on the main surface 30a side so as to correspond to the positions of the protrusions 30c. As a result, the porous metal sheet 34 constitutes the protrusions 30c.
[0089] The effects of the electrochemical cell device 200 will be described below. In the electrochemical cell device 200, similarly to the electrochemical cell device 100, the principal surface 20a has the recessed portion 20c and the principal surface 30a has the protruding portion 30c, so that the principal surface 20a easily conforms to the shape of the principal surface 10a and the principal surface 30a easily conforms to the shape of the principal surface 10b, and the gaps between the principal surface 10a and the principal surface 20a and between the principal surface 10b and the principal surface 30a are reduced. As a result, according to the electrochemical cell device 200, the contact electric resistance value between the cell 10 and the current collector 20 and the contact electric resistance value between the cell 10 and the current collector 30 are reduced, and the output voltage from the electrochemical cell device 100 can be improved.
[0090] Third embodiment The configuration of an electrochemical cell device according to a third embodiment (hereinafter referred to as "electrochemical cell device 300") will be described below. Here, differences from the configuration of the electrochemical cell device 100 will be mainly described, and overlapping descriptions will not be repeated.
[0091] The electrochemical cell device 300 includes a cell 10, a current collector 20, a current collector 30, an interconnector 40, and an interconnector 50. The cell 10 is warped convexly from the main surface 10b toward the main surface 10a. The main surface 20a has a recess 20c, and the main surface 30a has a protrusion 30c. In these respects, the configuration of the electrochemical cell device 300 is common to the configuration of the electrochemical cell device 100.
[0092] Fig. 12 is a cross-sectional view of the current collector 20 of the electrochemical cell device 300. Fig. 13 is a cross-sectional view of the current collector 30 of the electrochemical cell device 300. As shown in Fig. 12 and Fig. 13, the current collector 20 and the current collector 30 are each composed of one porous metal sheet (porous metal sheet 25 and porous metal sheet 35).
[0093] The recesses 20c of the current collector 20 (porous metal sheet 25) and the protrusions 30c of the current collector 30 (porous metal sheet 35) can be formed, for example, by press working.
[0094] The effects of the electrochemical cell device 300 will be described below. In the electrochemical cell device 300, similarly to the electrochemical cell device 100, the principal surface 20a has the recessed portion 20c and the principal surface 30a has the protruding portion 30c, so that the principal surface 20a easily conforms to the shape of the principal surface 10a and the principal surface 30a easily conforms to the shape of the principal surface 10b, and the gaps between the principal surface 10a and the principal surface 20a and between the principal surface 10b and the principal surface 30a are reduced. As a result, according to the electrochemical cell device 300, the contact electric resistance value between the cell 10 and the current collector 20 and the contact electric resistance value between the cell 10 and the current collector 30 are reduced, and the output voltage from the electrochemical cell device 100 can be improved.
[0095] The embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. The scope of the present invention is defined by the claims, not by the embodiments described above, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]
[0096] 10 cell, 10a, 10b main surface, 11 solid electrolyte layer, 12 cathode, 13 anode, 14 intermediate layer, 20 current collector, 20a, 20b main surface, 20c recess, 21 metal porous sheet, 22 metal porous sheet, 22a through hole, 23 metal porous sheet, 24 metal porous sheet, 24a through hole, 25 metal porous sheet, 30 current collector, 30a main surface, 30b main surface, 30c protrusion, 31 metal porous sheet, 32 metal porous sheet, 32a through hole, 33, 34, 35 metal porous sheet, 40 interconnector, 41 groove, 50 interconnector, 51 groove, 100, 200, 300 electrochemical cell device, L distance, P Apex, T, T1, T2, T3, T4 Thickness, WA Warpage, W max width.
Claims
1. A cell having a first major surface and a second major surface opposite the first major surface; a first current collector having a third main surface facing the first main surface; a second current collector having a fourth main surface facing the second main surface, The cell is warped convexly from the second main surface toward the first main surface, the third main surface includes a recess at a position facing a central portion of the first main surface, the fourth main surface includes a convex portion at a position facing a central portion of the second main surface, Each of the first current collector and the second current collector is composed of at least one metal porous body sheet made of a metal porous body having a skeleton with a three-dimensional mesh structure, a central portion of the first main surface includes a portion of the first main surface that is distant from a flat reference surface when the cell is placed on the reference surface so that the second main surface faces the flat reference surface, An electrochemical cell device, wherein the central portion of the second main surface includes a portion of the second main surface that is farthest from the reference surface when the cell is placed on the reference surface so that the second main surface faces the reference surface.
2. The at least one metal porous sheet constituting the first current collector is a first metal porous sheet and a second metal porous sheet, The first metal porous sheet and the second metal porous sheet are arranged side by side in a plane perpendicular to a thickness direction of the first current collector, The second porous metal sheet has a first through hole formed therein at a position corresponding to the recess, the first through hole penetrating the second porous metal sheet in a thickness direction, the first porous metal sheet is disposed in the first through hole, The thickness of the second metal porous sheet is greater than the thickness of the first metal porous sheet, 2. The electrochemical cell device according to claim 1, wherein the recess is defined by an inner circumferential surface of the first through hole and a main surface of the first porous metal sheet.
3. 3. The electrochemical cell device according to claim 2, wherein a value obtained by subtracting a thickness of the first porous metal sheet from a thickness of the second porous metal sheet is equal to an amount of warping of the cell.
4. The at least one metal porous sheet constituting the first current collector is a first metal porous sheet and a second metal porous sheet, The first metal porous body sheet and the second metal porous body sheet are overlapped in a thickness direction of the first current collector such that the second metal porous body sheet is located on the third main surface side, 2. The electrochemical cell device according to claim 1, wherein the second porous metal sheet has a first through hole formed therein at a position corresponding to the recess, the first through hole penetrating the second porous metal sheet in a thickness direction.
5. The at least one metal porous sheet constituting the second current collector is a third metal porous sheet and a fourth metal porous sheet, The third metal porous sheet and the fourth metal porous sheet are arranged side by side in a plane perpendicular to a thickness direction of the second current collector, A second through hole is formed in the fourth porous metal sheet at a position corresponding to the protrusion, the second through hole penetrating the fourth porous metal sheet in a thickness direction, the third porous metal sheet is disposed in the second through hole, 5. The electrochemical cell device according to claim 1, wherein the third porous metal sheet has a thickness greater than a thickness of the fourth porous metal sheet.
6. 6. The electrochemical cell device according to claim 5, wherein a value obtained by subtracting a thickness of the fourth porous metal sheet from a thickness of the third porous metal sheet is equal to an amount of warping of the cell.
7. The at least one metal porous sheet constituting the second current collector is a third metal porous sheet and a fourth metal porous sheet, The third metal porous body sheet and the fourth metal porous body sheet are overlapped in a thickness direction of the second current collector such that the fourth metal porous body sheet is located on the fourth main surface side, The electrochemical cell device according to claim 1 , wherein the fourth porous metal sheet constitutes the protrusions.
8. the first current collector is a cathode-side current collector, The electrochemical cell device according to claim 1 , wherein the second current collector is an anode side current collector.
9. the skeleton of each of the at least one porous metal sheet constituting the first current collector contains nickel and cobalt; The weight per unit area of each of the at least one porous metal sheet constituting the first current collector is 900 g / m 2 9. The electrochemical cell device of claim 8, wherein:
10. the skeleton of each of the at least one porous metal sheet constituting the second current collector contains nickel; The weight per unit area of each of the at least one porous metal sheet constituting the second current collector is 1000 g / m 2 10. The electrochemical cell device according to claim 8 or claim 9, wherein:
11. 11. The electrochemical cell device according to claim 1, wherein a value obtained by dividing an amount of warping of the cell by a maximum width of the cell in a plan view is 1 / 1000 or more.
12. 12. The electrochemical cell device according to claim 1, which is a solid oxide fuel cell.
13. 12. The electrochemical cell device according to any one of claims 1 to 11, which is a solid oxide electrolysis cell.
Citation Information
Patent Citations
Solid electrolyte fuel cell
JP2003007318A
Supporting film type solid oxide fuel cell stack, and manufacturing method of the same
JP2005317241A
Fuel cell
JP2006260994A
Fuel cell and method of producing the fuel cell
JP2010015977A
Fuel cell, fuel cell stack, and manufacturing method for fuel cell or fuel cell stack
JP2013069521A