Liquid crystal polyester resin, moldings, and electric / electronic parts

A liquid crystal polyester resin with specific structural units and properties addresses the imbalance in dielectric loss and heat resistance, improving signal quality and processing stability in high-frequency equipment.

JP7553001B2Active Publication Date: 2024-09-18ENEOS MATERIALS CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020124628
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-21
Publication Date
2024-09-18
Estimated Expiration
2040-07-21

AI Technical Summary

Technical Problem

Existing liquid crystal polyester resins do not achieve a sufficient balance between low dielectric loss tangent and high heat resistance, leading to signal deterioration and processing instability in high-frequency electronic equipment.

Method used

A liquid crystal polyester resin composition comprising structural units derived from 6-hydroxy-2-naphthoic acid, aromatic diol compounds, and isophthalic acid, with specific ratios and a controlled melting point and crystallization point difference, to achieve a low dielectric loss tangent and improved heat resistance.

Benefits of technology

The resin provides a balanced low dielectric loss tangent and high heat resistance, enhancing signal quality and processing stability in high-frequency electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553001000007
    Figure 0007553001000007
  • Figure 0007553001000013
    Figure 0007553001000013
  • Figure 0007553001000011
    Figure 0007553001000011
Patent Text Reader

Abstract

To provide a liquid crystal polyester resin that exhibits an excellent balance between heat resistance and processing stability while having a low dielectric loss tangent.SOLUTION: A liquid crystal polyester resin according to the present invention comprises a structural unit (I) derived from an aromatic hydroxycarboxylic acid, a structural unit (II) derived from an aromatic diol compound, and a structural unit (III) derived from an aromatic dicarboxylic acid; the structural unit (I) including a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid; the structural unit (III) including a structural unit (IIIA) derived from isophthalic acid, and a structural unit (IIIB) derived from 2, 6-naphthalene dicarboxylic acid; the dielectric loss tangent at a measurement frequency of 10 GHz being at most 1.50×10-3; the melting point being at least 290°C; and the temperature difference between the melting point and the crystallization point being at least 30°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal polyester resin, and more particularly to a liquid crystal polyester resin having a low dielectric tangent, a molded article containing the liquid crystal polyester resin, and an electric / electronic part including the molded article. [Background technology]

[0002] In recent years, with the increase in the volume of information and communication in the field of communications, the use of signals with high frequencies in electronic devices and communications equipment has increased. 9 Signals with frequencies in the gigahertz (GHz) band, which is 100 Hz or higher, are being used extensively. For example, high frequencies in the GHz band are used in the automotive field. Specifically, millimeter wave radar and quasi-millimeter wave radar installed in automobiles for collision prevention purposes use high frequencies of 76 to 79 GHz and 24 GHz, respectively, and are expected to become even more widespread in the future.

[0003] However, as the frequency of the signal used increases, the quality of the output signal, which may lead to erroneous recognition of information, decreases, i.e., the transmission loss increases. This transmission loss is composed of conductor loss caused by the conductor and dielectric loss caused by the insulating resin constituting the electric and electronic components such as the board in electronic devices and communication devices. Since the conductor loss is proportional to the 0.5th power of the frequency used and the dielectric loss is proportional to the 1st power of the frequency, the influence of this dielectric loss becomes very large in the high frequency band, especially in the GHz band. In addition, since the dielectric loss increases in proportion to the dielectric tangent of the resin, a resin having a low dielectric tangent is required to prevent deterioration of information. For example, Patent Document 1 proposes a liquid crystal polyester resin having a low dielectric loss, which contains a constitutional unit derived from p-hydroxybenzoic acid, a constitutional unit derived from 6-hydroxy-2-naphthoic acid, a constitutional unit derived from 4,4'-dihydroxybiphenyl, and 2,6-naphthalenedicarboxylic acid in a specific composition ratio.

[0004] In addition, resins constituting electric and electronic parts are required to have high heat resistance against heating during molding, and molded products made using the resins are also required to have high heat resistance against heating processing using solder, etc. In response to this problem, Patent Documents 2 and 3 propose liquid crystal polyester resins having excellent heat resistance and the like, which contain constitutional units derived from 6-hydroxy-2-naphthoic acid, constitutional units derived from 4,4'-dihydroxybiphenyl, and 2,6-naphthalenedicarboxylic acid in a specific composition ratio. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2006-1990 A [Patent Document 2] JP 2004-244452 A [Patent Document 3] JP 2006-225642 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the present inventors have found that even if the liquid crystal polyester resins proposed in Patent Documents 1 to 3 are used, it is not possible to obtain a liquid crystal polyester resin that has a sufficiently low dielectric tangent while also having an excellent balance between heat resistance and processing stability.

[0007] Therefore, the inventors conducted intensive research to solve the above problems, and as a result, they discovered that in a liquid crystalline polyester resin containing a structural unit derived from 6-hydroxy-2-naphthoic acid, a structural unit derived from an aromatic diol compound, a structural unit derived from isophthalic acid, and a structural unit derived from 2,6-naphthalenedicarboxylic acid, by adjusting the melting point and the temperature difference between the melting point and the crystallization point, a liquid crystalline polyester resin having a low dielectric tangent while having an excellent balance of heat resistance and processing stability can be obtained.

[0008] Therefore, an object of the present invention is to provide a liquid crystal polyester resin having a low dielectric tangent and an excellent balance between heat resistance and processing stability. Another object of the present invention is to provide a molded article containing the liquid crystal polyester resin and an electric / electronic part including the molded article. [Means for solving the problem]

[0009] The liquid crystal polyester resin according to the present invention is A structural unit (I) derived from an aromatic hydroxycarboxylic acid, A structural unit (II) derived from an aromatic diol compound, and Structural units derived from aromatic dicarboxylic acids (III) comprising The structural unit (I) includes a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid, The structural unit (III) includes a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, The dielectric tangent at a measurement frequency of 10 GHz is 1.50 x 10 -3 is as follows: The melting point is 290°C or higher, It is characterized by a temperature difference between the melting point and the crystallization point of 30°C or more.

[0010] In an embodiment of the present invention, the melting point of the liquid crystal polyester resin is preferably 340° C. or lower.

[0011] In an embodiment of the present invention, the structural unit (I) may further include a structural unit (IB) derived from p-hydroxybenzoic acid, The composition ratio (mol %) of the structural units (I) to (III) satisfies the following conditions: 36 mol%≦constituent unit (IA)≦74 mol% 0 mol%≦structural unit (IB)≦4 mol% 11 mol%≦structural unit (II)≦32 mol% 1 mol%≦structural unit (IIIA)≦7 mol% 10 mol%≦structural unit (IIIB)≦25 mol% It is preferable that the following is satisfied.

[0012] In an embodiment of the present invention, the structural unit (I) is a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid, The structural unit (III) includes a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, The composition ratio (mol %) of the structural units (I) to (III) satisfies the following conditions: 44 mol%≦constituent unit (IA)≦72 mol% 14 mol%≦structural unit (II)≦28 mol% 2 mol%≦structural unit (IIIA)≦6 mol% 12 mol% or less of structural unit (IIIB) or less than 22 mol% It is preferable that the following is satisfied.

[0013] In an embodiment of the present invention, the structural unit (I) includes a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid and a structural unit (IB) derived from p-hydroxybenzoic acid, The structural unit (III) includes a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, The composition ratio (mol %) of the structural units (I) to (III) satisfies the following conditions: 39 mol%≦constituent unit (IA)≦71 mol% 0 mol% < structural unit (IB) ≦ 3 mol% 13 mol%≦structural unit (II)≦30 mol% 2 mol%≦structural unit (IIIA)≦6 mol% 11 mol%≦structural unit (IIIB)≦24 mol% It is preferable that the following is satisfied.

[0014] In an embodiment of the present invention, the structural unit (II) derived from an aromatic diol compound is preferably a structural unit derived from 4,4'-dihydroxybiphenyl.

[0015] The molded article according to the present invention contains the liquid crystal polyester resin and is preferably in the form of fibers.

[0016] The molded article according to the present invention contains the liquid crystal polyester resin and is preferably an injection molded article.

[0017] An electric / electronic component according to the present invention is characterized by comprising the above molded article. Effect of the Invention

[0018] According to the present invention, it is possible to realize a liquid crystal polyester resin that has a low dielectric tangent and an excellent balance between heat resistance and processing stability. That is, by using the liquid crystal polyester resin of the present invention, it is possible to improve processing stability such as injection molding stability and spinning stability, and also improve the heat resistance of the produced molded product against heat processing. Therefore, when the resin is processed and molded and used as a product, it is possible to prevent a decrease in the quality of the output signal in electrical and electronic equipment and communication equipment that use high-frequency signals. Modes for carrying out the invention

[0019] (Liquid crystal polyester resin) The liquid crystal polyester resin according to the present invention comprises a structural unit (I) derived from an aromatic hydroxycarboxylic acid, a structural unit (II) derived from an aromatic diol compound, and a structural unit (III) derived from an aromatic dicarboxylic acid. In addition, the structural unit (I) of the liquid crystal polyester resin comprises a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid, and may further comprise a structural unit (IB) derived from p-hydroxybenzoic acid, and the structural unit (III) comprises a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, and has the following specific properties (dielectric loss tangent, melting point, temperature difference between the melting point and the crystallization point).

[0020] The dielectric loss tangent of the liquid crystal polyester resin according to the present invention (measurement frequency: 10 GHz) is 1.50×10-3 or less, preferably 1.00×10 -3 More preferably, it is 0.90×10 or less. -3 More preferably, it is 0.80×10 or less. -3 By setting the dielectric loss tangent of the liquid crystal polyester resin according to the present invention to the above-mentioned numerical range, a molded article having a low dielectric loss tangent can be produced, and therefore, when the resin is used as a product, deterioration in the quality of output signals in electric and electronic devices and communication devices that use high-frequency signals can be prevented. In this specification, the dielectric loss tangent at 10 GHz of the liquid crystal polyester resin can be measured by the split post dielectric resonator method (SPDR method) using a network analyzer N5247A manufactured by Keysight Technologies Inc.

[0021] The melting point of the liquid crystal polyester resin according to the present invention has a lower limit of 290° C. or more, preferably 295° C. or more, and more preferably 300° C. or more, and an upper limit of preferably 340° C. or less, more preferably 335° C. or less, and further preferably 330° C. or less. By setting the melting point of the liquid crystal polyester resin according to the present invention within the above numerical range, it is possible to improve the heat resistance of a molded article produced using the liquid crystal polyester resin against heat processing. The crystallization point of the liquid crystal polyester resin according to the present invention is preferably 240°C or higher, more preferably 245°C or higher, as a lower limit, and is preferably 295°C or lower, more preferably 290°C or lower, as an upper limit. The temperature difference between the melting point and the crystallization point of the liquid crystal polyester resin according to the present invention (= "melting point (°C)" - "crystallization point (°C)") is 30°C or more as a lower limit, preferably 35°C or more, more preferably 40°C or more, and preferably 70°C or less as an upper limit, more preferably 60°C or less. By setting the temperature difference between the melting point and the crystallization point of the liquid crystal polyester resin according to the present invention within the above numerical range, when the liquid crystal polyester is melted and molded, a sufficient time can be allowed for the liquid crystal polyester to melt and solidify, and the degree of freedom in setting temperature conditions such as the molding temperature can be increased. Therefore, processing stability such as injection molding stability and spinning stability can be improved. In this specification, the melting point and crystallization point of the liquid crystal polyester resin are values ​​measured by a differential scanning calorimeter (DSC). Specifically, the liquid crystal polyester resin is completely melted by heating from room temperature to 340 to 360 ° C. at a heating rate of 10 ° C. / min, and then cooled to 30 ° C. at a rate of 10 ° C. / min. The apex of the exothermic peak obtained when the temperature is lowered to 30 ° C. at a rate of 10 ° C. / min is the crystallization point (Tc), and the apex of the endothermic peak obtained when the temperature is further increased to 360 ° C. at a rate of 10 ° C. / min is the melting point (Tm).

[0022] The liquid crystallinity of the liquid crystal polyester resin according to the present invention can be confirmed by using a polarizing microscope (product name: BH-2) manufactured by Olympus Corporation equipped with a hot stage for a microscope (product name: FP82HT) manufactured by Mettler, for example, to heat and melt the liquid crystal polyester resin on a heating stage of the microscope, and then observing whether or not it has optical anisotropy.

[0023] From the viewpoint of moldability, the melt viscosity of the liquid crystal polyester resin according to the present invention is set to be the melting point of the liquid crystal polyester resin + 20°C and a shear rate of 100 s -1 Under the above conditions, the lower limit is preferably 20 Pa·s or more, more preferably 40 Pa·s or more, and even more preferably 50 Pa·s or more, and the upper limit is preferably 600 Pa·s or less, more preferably 350 Pa·s or less, even more preferably 320 Pa·s or less, and even more preferably 200 Pa·s or less. In this specification, the viscosity of the liquid crystal polyester resin can be measured using a capillary rheometer viscometer in accordance with JIS K7199.

[0024] The liquid crystal polyester resin according to the present invention has a composition ratio (mol %) of the structural units (I) to (III) that satisfies the following conditions: 36 mol%≦constituent unit (IA)≦74 mol% 0 mol%≦structural unit (IB)≦4 mol% 11 mol%≦structural unit (II)≦32 mol% 1 mol%≦structural unit (IIIA)≦7 mol% 10 mol%≦structural unit (IIIB)≦25 mol% It is preferable that the following is satisfied. Furthermore, in the liquid crystal polyester resin according to the present invention, when only the structural unit (IA) derived from 6-hydroxy-2-naphthoic acid is contained as the structural unit (I) derived from an aromatic hydroxycarboxylic acid and no structural unit (IB) derived from p-hydroxybenzoic acid is contained, the following conditions are satisfied: 44 mol%≦constituent unit (IA)≦72 mol% 14 mol%≦structural unit (II)≦28 mol% 2 mol%≦structural unit (IIIA)≦6 mol% 12 mol% or less of structural unit (IIIB) or less than 22 mol% It is more preferable that the following conditions are satisfied: In addition, in the liquid crystal polyester resin according to the present invention, when the structural unit (I) contains both the structural unit (IA) derived from 6-hydroxy-2-naphthoic acid and the structural unit (IB) derived from p-hydroxybenzoic acid, the following condition is satisfied: 39 mol%≦constituent unit (IA)≦71 mol% 0 mol% < structural unit (IB) ≦ 3 mol% 13 mol%≦structural unit (II)≦30 mol% 2 mol%≦structural unit (IIIA)≦6 mol% 11 mol%≦structural unit (IIIB)≦24 mol% It is more preferable that the following conditions are satisfied: The liquid crystal polyester resin according to the present invention, in which the composition ratio (mol %) of the structural units (I) to (III) satisfies the above-mentioned conditions, has a low dielectric tangent while being excellent in balance between heat resistance and processing stability.

[0025] In the liquid crystal polyester resin according to the present invention, the composition ratio of the structural unit (II) is substantially equivalent to the composition ratio of the structural unit (III) (structural unit (II) ≈ structural unit (III)). The lower limit of the total of the structural units (I) to (III) relative to the entire structural units of the liquid crystal polyester resin is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 99 mol% or more, and the upper limit is preferably 100 mol% or less.

[0026] Hereinafter, each of the structural units contained in the liquid crystal polyester resin will be described in detail.

[0027] (Structural unit (I) derived from aromatic hydroxycarboxylic acid) The liquid crystal polyester resin contains a structural unit (I) derived from an aromatic hydroxycarboxylic acid. The structural unit (I) derived from an aromatic hydroxycarboxylic acid contains a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid represented by the following formula (IA). The composition ratio (mol%) of the structural unit (IA) in the liquid crystal polyester resin is preferably 36 mol% or more and 74 mol% or less. From the viewpoint of lowering the dielectric tangent of the liquid crystal polyester resin, improving the heat resistance, and improving the processing stability, the composition ratio (mol%) of the structural unit (IA) is preferably 39 mol% or more, more preferably 44 mol% or more, and even more preferably 50 mol% or more, and the upper limit is preferably 72 mol% or less, more preferably 71 mol% or less, and even more preferably 70 mol% or less. [ka]

[0028] Examples of monomers that provide the structural unit (IA) include 6-hydroxy-2-naphthoic acid (HNA, formula (1) below), as well as its acetylated products, ester derivatives, and acid halides. [ka]

[0029] Furthermore, the structural unit (I) derived from aromatic hydroxycarboxylic acid may contain a structural unit (IB) derived from p-hydroxybenzoic acid represented by the following formula (IB). The composition ratio (mol%) of the structural unit (IB) in the liquid crystal polyester resin is preferably 0 mol% or more and 4 mol% or less. From the viewpoint of decreasing the dielectric tangent of the liquid crystal polyester resin, improving the heat resistance, and improving the processing stability, when the structural unit (IB) is contained, the composition ratio (mol%) of the structural unit (IB) is preferably more than 0 mol%, more preferably 0.5 mol% or more as a lower limit, and more preferably 3 mol% or less as an upper limit, more preferably 2 mol% or less. [ka]

[0030] Examples of monomers that provide the structural unit (IB) include p-hydroxybenzoic acid (HBA, formula (2) below), as well as its acetylated products, ester derivatives, and acid halides. [ka]

[0031] (Structural unit (II) derived from an aromatic diol compound) The liquid crystal polyester resin contains a structural unit (II) derived from an aromatic diol compound, and the composition ratio (mol%) of the structural unit (II) in the liquid crystal polyester resin is preferably 11 mol% or more and 32 mol% or less. From the viewpoint of lowering the dielectric tangent of the liquid crystal polyester resin, improving heat resistance, and improving processing stability, the composition ratio (mol%) of the structural unit (II) is preferably 13 mol% or more, more preferably 14 mol% or more, as a lower limit, and is preferably 30 mol% or less, more preferably 28 mol% or less, as an upper limit.

[0032] In one embodiment, the constitutional unit (II) is represented by the following formula (II): [ka] In the above formula, Ar 1 is selected from the group consisting of a phenyl group, a biphenyl group, a 4,4'-isopropylidenediphenyl group, a naphthyl group, an anthryl group and a phenanthryl group, which may have a substituent. Among these, a phenyl group and a biphenyl group are more preferable. Examples of the substituent include hydrogen, an alkyl group, an alkoxy group, and fluorine. The number of carbon atoms in the alkyl group is preferably 1 to 10, and more preferably 1 to 5. The alkyl group may be either a linear alkyl group or a branched alkyl group. The number of carbon atoms in the alkoxy group is preferably 1 to 10, and more preferably 1 to 5.

[0033] Examples of monomers that provide the structural unit (II) include 4,4'-dihydroxybiphenyl (BP, formula (3) below), hydroquinone (HQ, formula (4) below), methylhydroquinone (MeHQ, formula (5) below), 4,4'-isopropylidenediphenol (BisPA, formula (6) below), and acylation products, ester derivatives, and acid halides thereof. Among these, it is preferable to use 4,4'-dihydroxybiphenyl (BP) and acylation products, ester derivatives, and acid halides thereof. [ka] [ka] [ka] [ka]

[0034] (Structural unit (III) derived from aromatic dicarboxylic acid) The liquid crystal polyester resin contains a structural unit (III) derived from an aromatic dicarboxylic acid. Furthermore, the structural unit (III) derived from an aromatic dicarboxylic acid contains a structural unit (IIIA) derived from isophthalic acid represented by the following formula (IIIA). The composition ratio (mol%) of the structural unit (IIIA) in the liquid crystal polyester resin is preferably 1 mol% or more and 7 mol% or less. From the viewpoint of decreasing the dielectric tangent of the liquid crystal polyester resin, improving the heat resistance, and improving the processing stability, the composition ratio (mol%) of the structural unit (IIIA) is preferably 2 mol% or more as a lower limit, and is preferably 6 mol% or less as an upper limit, and more preferably 5 mol% or less.

[0035] [ka]

[0036] Examples of monomers that provide the structural unit (IIIB) include isophthalic acid (IPA, formula (7) below), and ester derivatives and acid halides thereof. [ka]

[0037] The structural unit (III) derived from an aromatic dicarboxylic acid includes a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid represented by the following formula (IIIB). The composition ratio (mol%) of the structural unit (IIIB) in the liquid crystal polyester resin is preferably 10 mol% or more and 25 mol% or less. From the viewpoint of decreasing the dielectric tangent of the liquid crystal polyester resin, improving the heat resistance, and improving the processing stability, the composition ratio (mol%) of the structural unit (IIIB) is preferably 11 mol% or more, more preferably 12 mol% or more, as a lower limit, and is preferably 24 mol% or less, more preferably 22 mol% or less, as an upper limit.

[0038] [ka]

[0039] Examples of monomers that provide the structural unit (IIIB) include 2,6-naphthalenedicarboxylic acid (NADA, formula (8) below), and ester derivatives and acid halides thereof. [ka]

[0040] (Method of producing liquid crystal polyester resin) The liquid crystal polyester resin according to the present invention can be produced by polymerizing the monomers that give the structural units (I) to (III) by a conventionally known method such as melt polymerization, solid-phase polymerization, solution polymerization, and slurry polymerization. In one embodiment, the liquid crystal polyester resin according to the present invention can be produced only by melt polymerization. It can also be produced by two-stage polymerization in which a prepolymer is produced by melt polymerization and then further solid-phase polymerized.

[0041] From the viewpoint of efficiently obtaining the liquid crystal polyester resin according to the present invention, the melt polymerization is preferably carried out under reflux of acetic acid in the presence of 1.05 to 1.15 molar equivalents of acetic anhydride relative to the total hydroxyl groups of the monomers, with the monomers that give the above-mentioned structural units (I) to (III) being 100 mol % in total in a predetermined blend. In addition, the melt polymerization is preferably carried out under reduced pressure. As for the reaction conditions, the reaction temperature is preferably 200 to 380°C, more preferably 240 to 370°C, and even more preferably 260 to 360°C, and the final pressure is preferably 0.1 to 760 Torr, more preferably 1 to 100 Torr, and even more preferably 1 to 50 Torr.

[0042] When the polymerization reaction is carried out in two stages, melt polymerization followed by solid-state polymerization, the polymer obtained by melt polymerization may be cooled and solidified, and then pulverized into a powder or flake form. The polymer strand obtained by melt polymerization may be pelletized into pellets. Thereafter, a known solid-state polymerization method, for example, a method of heat-treating the polymer in an inert atmosphere such as nitrogen or under vacuum at a temperature range of 200 to 350°C for 1 to 30 hours, is preferably selected. The solid-state polymerization may be carried out with stirring, or may be carried out in a stationary state without stirring.

[0043] A catalyst may or may not be used in the polymerization reaction. As the catalyst to be used, a conventionally known catalyst for polymerization of polyester resins can be used, and examples of the catalyst include metal salt catalysts such as potassium acetate, magnesium acetate, stannous acetate, lead acetate, sodium acetate, tetrabutyl titanate, and antimony trioxide, nitrogen-containing heterocyclic compounds such as N-methylimidazole, and organic compound catalysts. The amount of the catalyst to be used is not particularly limited, but is preferably 0.0001 to 0.1 parts by weight relative to 100 parts by weight of the total amount of monomers.

[0044] The polymerization reactor for melt polymerization is not particularly limited, but a reactor generally used for reactions of high-viscosity fluids is preferably used. Examples of such reactors include stirring tank-type polymerization reactors having stirring devices with stirring blades of various shapes, such as anchor type, multi-stage type, spiral belt type, spiral shaft type, etc., or modified versions of these, and mixing devices generally used for kneading resins, such as kneaders, roll mills, and Banbury mixers.

[0045] (molded product) The molded article according to the present invention contains a liquid crystal polyester resin, and its shape may be appropriately changed depending on the application, and is not particularly limited, and may be, for example, a plate, a sheet, a fiber, or the like.

[0046] In one embodiment, the molded article is preferably in the form of fibers. The fibers can be obtained by a conventional method such as melt spinning or solution spinning. The fibers may be made of only the liquid crystal polyester resin, or may be mixed with other resins.

[0047] The molded article according to the present invention may further contain a filler, such as carbon fiber, graphite, glass fiber, talc, mica, glass flake, clay, sericite, calcium carbonate, calcium sulfate, calcium silicate, silica, alumina, aluminum hydroxide, calcium hydroxide, graphite, potassium titanate, titanium oxide, fluorocarbon resin fiber, fluorocarbon resin, barium sulfate, and various whiskers.

[0048] In addition, the molded article according to the present invention may contain resins other than liquid crystal polyester resins within the scope of the present invention. For example, polyester resins such as polyethylene terephthalate, polyethylene naphthalate, polyarylate, polycyclohexylene dimethylene terephthalate, and polybutylene terephthalate, polyolefin resins such as polyethylene and polypropylene, vinyl resins such as cycloolefin polymers and polyvinyl chloride, (meth)acrylic resins such as polyacrylate, polymethacrylate, and polymethyl methacrylate, imide resins such as polyphenylene ether resins, polyacetal resins, polyamide resins, polyimides, and polyetherimides, polystyrene resins such as polystyrene, high impact polystyrene, AS resin, and ABS resin, thermosetting resins such as epoxy resins, cellulose resins, polyether ether ketone resins, fluororesins, and polycarbonate resins, and the molded article may contain one or more of these.

[0049] The molded article according to the present invention may contain other additives, such as colorants, dispersants, plasticizers, antioxidants, curing agents, flame retardants, heat stabilizers, ultraviolet absorbers, antistatic agents, and surfactants, without departing from the spirit of the present invention.

[0050] The molded article according to the present invention can be obtained by press molding, foam molding, injection molding, calendar molding, punch molding, etc. of a mixture containing the liquid crystal polyester resin and, if desired, other resins and additives, etc. The mixture can be obtained by melt-kneading the liquid crystal polyester resin, etc., using a Banbury mixer, a kneader, a single-screw or twin-screw extruder, etc.

[0051] (Electrical and electronic parts) The electric / electronic component according to the present invention comprises a molded product (e.g., an injection molded product, etc.) containing a liquid crystal polyester resin. Examples of the electric / electronic component comprising the molded product include antennas used in electronic devices and communication devices such as ETC, GPS, wireless LAN, and mobile phones, high-speed transmission connectors, CPU sockets, circuit boards, flexible printed circuit boards (FPCs), laminated circuit boards, millimeter wave and quasi-millimeter wave radars such as collision prevention radars, RFID tags, capacitors, inverter parts, cable covering materials, insulating materials for secondary batteries such as lithium ion batteries, speaker diaphragms, etc. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0053] <Production of Liquid Crystal Polyester Resin> Example 1 A polymerization vessel equipped with a stirring blade was charged with 52 mol% of 6-hydroxy-2-naphthoic acid (HNA), 24 mol% of 4,4'-dihydroxybiphenyl (BP), 5 mol% of isophthalic acid (IPA), and 19 mol% of 2,6-naphthalenedicarboxylic acid (NADA). Potassium acetate was then added as a catalyst. The polymerization vessel was depressurized and nitrogen was injected three times, after which acetic anhydride (1.05 molar equivalents relative to the hydroxyl groups) was further added. The temperature was raised to 150°C, and the acetylation reaction was carried out under reflux for 2 hours.

[0054] After the acetylation was completed, the polymerization vessel in which acetic acid had been distilled was heated at a rate of 0.5°C / min until the melting zone temperature in the vessel reached 330°C. Thereafter, the pressure in the system was reduced to 50 Torr over 30 minutes. After the stirring torque reached a predetermined value, nitrogen was introduced to return the reduced pressure to normal pressure, the polymer was extracted, and cooled and solidified. The obtained polymer was pulverized to a size that could pass through a sieve with 2.0 mm openings to obtain a polymer. The obtained polymer was subjected to a melting point +20°C and 100 s -1 The polymerization is complete when the melt viscosity at 100 s is in the range of 20 Pa s to 600 Pa s. -1If the melt viscosity at this temperature is less than 20 Pa s, the degree of polymerization is insufficient, so the temperature is raised to 300°C so that the melt viscosity is in the range of 20 Pa s to 600 Pa s, and then the temperature is held for 4 hours to carry out solid-state polymerization and complete the polymerization again.

[0055] The polyester resin was then naturally cooled at room temperature to obtain a polyester resin of the present invention. The polyester resin was heated and melted on a heating stage of the microscope using a polarizing microscope (product name: BH-2) manufactured by Olympus Corporation equipped with a hot stage for the microscope (product name: FP82HT) manufactured by Mettler, and liquid crystallinity was confirmed based on the presence or absence of optical anisotropy.

[0056] Example 2 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 58 mol%, BP 21 mol%, IPA 5 mol%, and NADA 16 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0057] Example 3 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 60 mol%, BP 20 mol%, IPA 3 mol%, and NADA 17 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0058] Example 4 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 60 mol%, BP 20 mol%, IPA 4 mol%, and NADA 16 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0059] Example 5 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 60 mol%, BP 20 mol%, IPA 6 mol%, and NADA 14 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0060] Example 6 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 70 mol%, BP 15 mol%, IPA 3 mol%, and NADA 12 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0061] Example 7 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 57 mol%, p-hydroxybenzoic acid (HBA) 1 mol%, BP 21 mol%, IPA 5 mol%, and NADA 16 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0062] Example 8 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 48 mol%, HBA 2 mol%, BP 25 mol%, IPA 3 mol%, and NADA 22 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0063] Example 9 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 48 mol%, HBA 2 mol%, BP 25 mol%, IPA 4 mol%, and NADA 21 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0064] Example 10 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 48 mol%, HBA 2 mol%, BP 25 mol%, IPA 5 mol%, and NADA 20 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0065] Example 11 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 50 mol%, HBA 2 mol%, BP 24 mol%, IPA 4 mol%, and NADA 20 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0066] Example 12 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 54 mol%, HBA 2 mol%, BP 22 mol%, IPA 3 mol%, and NADA 19 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0067] Example 13 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 58 mol%, HBA 2 mol%, BP 20 mol%, IPA 3 mol%, and NADA 17 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0068] Comparative Example 1 Except for changing the monomer charging to 50 mol % HNA, 25 mol % BP, and 25 mol % NADA, a polyester resin was obtained in the same manner as in Example 1. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0069] Comparative Example 2 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 50 mol%, BP 25 mol%, IPA 10 mol%, and NADA 15 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0070] Comparative Example 3 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 48 mol%, HBA 2 mol%, BP 25 mol%, and NADA 25 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0071] Comparative Example 4 A polyester resin was obtained in the same manner as in Example 1, except that the monomers were changed to HNA 48 mol%, HBA 2 mol%, BP 25 mol%, IPA 10 mol%, and NADA 15 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0072] Comparative Example 5 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 60 mol%, HBA 2 mol%, BP 19 mol%, and NADA 19 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0073] Comparative Example 6 A polyester resin was obtained in the same manner as in Example 1, except that the monomer charges were changed to HNA 38 mol%, HBA 12 mol%, BP 25 mol%, and NADA 25 mol%. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0074] Comparative Example 7 Except for changing the monomer charging to 27 mol % HNA and 73 mol % HBA, a polyester resin was obtained in the same manner as in Example 1. Next, the liquid crystallinity of the polyester resin was confirmed in the same manner as above.

[0075] <Preparation of flat test pieces> The liquid crystal polyester resins obtained in the examples and comparative examples were heated and melted at a temperature between the melting point and melting point + 20° C., and injection molded to prepare flat test pieces measuring 30 mm×30 mm×0.4 mm.

[0076] <Dielectric loss tangent measurement (10GHz)> The dielectric loss tangent (tan δ) in the in-plane direction of the flat test piece prepared above was measured at a frequency of 10 GHz using a network analyzer N5247A from Keysight Technologies, Inc., by the split post dielectric resonator method (SPDR method). The measurement results are shown in Table 1.

[0077] <Melt point and crystallization point measurement> The melting point and crystallization point of the liquid crystal polyester resin obtained in the examples and comparative examples were measured by a differential scanning calorimeter (DSC) manufactured by Hitachi High-Tech Science Co., Ltd. First, the liquid crystal polyester resin was completely melted by raising the temperature from room temperature to 340 to 360 ° C. at a heating rate of 10 ° C. / min, and then the apex of the exothermic peak obtained when the temperature was lowered to 30 ° C. at a rate of 10 ° C. / min was taken as the crystallization point (Tc), and the apex of the endothermic peak obtained when the temperature was further raised to 360 ° C. at a rate of 10 ° C. / min was taken as the melting point (Tm). In addition, the difference between the melting point and the crystallization point was calculated from the obtained melting point and crystallization point. The melting point, the crystallization point, and the difference between the melting point and the crystallization point are shown in Table 1.

[0078] <Evaluation of the balance between heat resistance and processing stability> The balance between heat resistance and processing stability of the liquid crystal polyester resins obtained in the examples and comparative examples was evaluated according to the following criteria. The higher the score of the evaluation criteria, the better, and a score of 3 or more was considered to be acceptable. The evaluation results are shown in Table 1. (Evaluation Criteria) 4: The melting point was 300° C. or higher and 340° C. or lower, and the difference between the melting point and the crystallization point was 30° C. or higher, and the balance between heat resistance and processing stability was particularly excellent. 3: The melting point was 290° C. or higher and lower than 300° C., and the difference between the melting point and the crystallization point was 30° C. or higher, and the material had an excellent balance between heat resistance and processing stability. 2: The melting point was less than 290°C or more than 340°C, or the difference between the melting point and the crystallization point was less than 30°C, and the balance between heat resistance and processing stability was poor. 1: The melting point was less than 290°C or more than 340°C, and the difference between the melting point and the crystallization point was less than 30°C, and the balance between heat resistance and processing stability was particularly poor.

[0079] As is clear from the results in Table 1, the liquid crystal polyester resins of Examples 1 to 13 had clearly lower dielectric tangents and better balance between heat resistance and processing stability than the general-purpose liquid crystal polyester resin of Comparative Example 7. Furthermore, the liquid crystal polyester resins of Examples 1 to 13 had better balance between heat resistance and processing stability than the liquid crystal polyester resins of Comparative Examples 1 to 6 having different compositions.

[0080] <Melt Viscosity Measurement> The liquid crystal polyester resins obtained in the examples and comparative examples were melted at a shear rate of 100 S -1 The melt viscosity (Pa s) at melting point + 20°C was measured in accordance with JIS K7199 using a capillary rheometer viscometer (Capillograph 1D, Toyo Seiki Seisakusho Co., Ltd.) and a capillary with an inner diameter of 1 mm. The measurement results are shown in Table 1.

[0081] [Table 1]

[0082] <Production and evaluation of molded products> (Molding of test pieces) The liquid crystal polyester resins obtained in Examples 1, 3, and 12 were injection molded using an injection molding machine (Rambaldi: Babyplast) to prepare dumbbell-shaped tensile test pieces in accordance with ISO527.

[0083] (Measurement of tensile strength, tensile modulus, and tensile elongation) The tensile test pieces prepared above were used to measure the tensile strength (MPa) and tensile elongation (%) in accordance with ISO 527.

[0084] [Table 2]

Claims

1. A structural unit (I) derived from an aromatic hydroxycarboxylic acid, A structural unit (II) derived from an aromatic diol compound, and Structural unit (III) derived from an aromatic dicarboxylic acid comprising The structural unit (I) includes a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid, and may further include a structural unit (IB) derived from p-hydroxybenzoic acid; The structural unit (III) includes a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, The composition ratio (mol %) of the structural units (I) to (III) satisfies the following conditions: 36 mol%≦structural unit (IA)≦74 mol% 0 mol%≦structural unit (IB)≦4 mol% 11 mol%≦structural unit (II)≦32 mol% 1 mol%≦structural unit (IIIA)≦7 mol% 10 mol%≦structural unit (IIIB)≦25 mol% Fulfilling The dielectric loss tangent at a measurement frequency of 10 GHz using the split post dielectric resonator method is 1.50 x 10 -3 is as follows: The melting point is 290° C. or higher, A liquid crystal polyester resin having a temperature difference between its melting point and crystallization point of 30° C. or more.

2. The liquid crystal polyester resin according to claim 1, having a melting point of 340° C. or lower.

3. The structural unit (I) is a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid, The structural unit (III) includes a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, The composition ratio (mol %) of the structural units (I) to (III) satisfies the following conditions: 44 mol%≦structural unit (IA)≦72 mol% 14 mol%≦structural unit (II)≦28 mol% 2 mol%≦structural unit (IIIA)≦6 mol% 12 mol%≦structural unit (IIIB)≦22 mol% The liquid crystal polyester resin according to claim 1 or 2, which satisfies the above.

4. The structural unit (I) includes a structural unit (IA) derived from 6-hydroxy-2-naphthoic acid and a structural unit (IB) derived from p-hydroxybenzoic acid, The structural unit (III) includes a structural unit (IIIA) derived from isophthalic acid and a structural unit (IIIB) derived from 2,6-naphthalenedicarboxylic acid, The composition ratio (mol %) of the structural units (I) to (III) satisfies the following conditions: 39 mol%≦structural unit (IA)≦71 mol% 0 mol%<structural unit (IB)≦3 mol% 13 mol%≦structural unit (II)≦30 mol% 2 mol%≦structural unit (IIIA)≦6 mol% 11 mol%≦structural unit (IIIB)≦24 mol% The liquid crystal polyester resin according to claim 1 or 2, which satisfies the above.

5. The liquid crystal polyester resin according to any one of claims 1 to 4, wherein the structural unit (II) derived from an aromatic diol compound is a structural unit derived from 4,4'-dihydroxybiphenyl.

6. A fibrous molded article comprising the liquid crystal polyester resin according to any one of claims 1 to 5.

7. An injection-molded article comprising the liquid crystal polyester resin according to any one of claims 1 to 5.

8. An electric / electronic component comprising the molded article according to claim 6 or 7.

Citation Information

Patent Citations

  • Aromatic liquid crystal polyester and its film

    JP2004244452A

  • Aromatic liquid crystal polyester film and laminate

    JP2006001990A

  • Aromatic liquid crystal polyester and film formed herefrom

    JP2006225642A

  • Liquid crystal polyester resin

    JP2019043996A

  • Polypropylene resin composition

    JP2019214678A