Ultrafine ferrite-cementite structure steel, ultrafine ferrite-austenite structure steel, ultrafine martensite structure steel, and method for producing ultrafine martensite-austenite structure steel

By employing ultrafine ferrite-cementite structure steel with controlled annealing and warm rolling, the method addresses the inefficiency of long annealing times in producing high-strength, high-ductility ferritic-austenitic steels, achieving superior mechanical properties in a shorter timeframe.

JP7553065B2Active Publication Date: 2024-09-18UNIV OF HYOGO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2019159068
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-08-30
Publication Date
2024-09-18
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

Existing methods for producing ferritic-austenitic steel with high strength and ductility require long annealing times, making them impractical for widespread use.

Method used

The production method involves using ultrafine ferrite-cementite structure steel as a pre-structure, with specific compositions of C, Si, and Mn, and employing warm rolling and controlled annealing at low temperatures to achieve ultrafine ferritic-austenitic and martensitic-austenitic steels in a significantly shorter time.

Benefits of technology

This approach results in high-strength, high-ductility steels that can be produced efficiently, with tensile strengths up to 1500 MPa and total elongations over 30%, suitable for applications in buildings, bridges, and automobile components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553065000017
    Figure 0007553065000017
  • Figure 0007553065000007
    Figure 0007553065000007
  • Figure 0007553065000019
    Figure 0007553065000019
Patent Text Reader

Abstract

To provide a method for producing a superfine ferrite-cementite structure steel, a superfine ferrite-austenite structure steel, a superfine martensite structure steel and a superfine martensite-austenite structure steel having sufficient mechanical strength and ductility even if being used to constructions, bridges or the like, automobile undercarriage steels and mechanical parts such as gears, and further capable of producing these structure steels at a relatively low temperature in an extra-short time.SOLUTION: A high strength and high ductility superfine ferrite-cementite structure steel has a composition in which the contents of C, Si and Mn satisfy 0.05 wt.%<C<0.3 wt.%, 0.5 wt.%<Si<2 wt.% and 3 wt.%<Mn<10 wt.%, respectively, and the balance Fe with inevitable impurities, and has a ferrite grain size of 2.0 μm or lower. In the cementite, Mn enters into a solid solution, and the value of x in the chemical equation (Fe1-x, Mnx)3C of the cementite is 0.3 to below 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing ultrafine-grained ferrite-cementite steel, ultrafine-grained ferrite-austenite steel, ultrafine-grained martensite steel, and ultrafine-grained martensite-austenite steel, which have high strength and high ductility and are suitable for use in structures such as buildings and bridges, automotive suspension steel, and machine gears and other parts. [Background technology]

[0002] In recent years, from the perspective of protecting the global environment, improving fuel efficiency by reducing the weight of automobile bodies and collision safety from the perspective of protecting passengers have become more important than ever. It is possible to strengthen the body of a vehicle by increasing the thickness of the steel plate or adding reinforcing members, but this will increase the weight of the vehicle. One technology that can meet these conflicting demands is the development of high-strength steel plate, or so-called hi-tensile steel. However, increasing the strength of steel plate comes with the issue of deterioration of formability, so it is necessary to develop high-strength, highly formable steel plate with high formability according to the parts to which it is applied. Therefore, hi-tensile steel that utilizes a retained austenite type composite structure has attracted attention as a way to achieve both high strength and high ductility.

[0003] When this high-tensile steel containing metastable austenite is deformed, the austenite undergoes a processing-induced transformation to martensite during deformation, hardening the steel, suppressing localization of deformation and transferring deformation to untransformed austenite, resulting in high elongation. Since plastic deformation is promoted by processing-induced martensite transformation, this phenomenon is called the TRIP (Transformation Induced Plasticity) phenomenon, and this retained austenite steel is called TRIP steel. Currently, the target for high-tensile steel for next-generation automobiles is said to be tensile strength TS × total elongation T.EI ≧ 30,000 MPa%, and material development to achieve this goal is underway.

[0004] Against this background, it has been reported that low-C, medium-Mn steel with a ferritic-austenite structure and a composition of 0.1%C-2%Si-5%Mn can be manufactured by an extremely simple two-phase annealing process compared to conventional TRIP steels, and that it exhibits high strength (1200 MPa) and high ductility (T.EI = 25%) (see, for example, non-patent documents 1 and 2). [Prior art documents] [Patent documents]

[0005] [Non-Patent Document 1] S. Torizuka and T. Hanamura: Bull. Iron Steel Inst. Jpn., 17(2012), 852. [Non-Patent Document 2] T. Hanamura, S. Torizuka, A. Sunahara, M. Imagumbai and H. Takechi: ISIJ Int., 51(2011), 685. Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the case of ferrite-austenite steel with the above composition, it takes a long annealing time of about 1 hour to obtain the optimum austenite fraction (20 to 30%), and it is difficult to manufacture it by continuous annealing. This makes it difficult to put it to practical use. Therefore, it is necessary to develop a method for efficiently obtaining the desired ferrite-austenite steel in a short time of about 10 minutes.

[0007] Therefore, the inventors have conducted extensive research and found that by using an ultrafine ferrite-cementite steel as the precursor to a ferrite-austenite steel, it is possible to obtain an ultrafine ferrite-austenite steel in an annealing time of only 10 minutes, one-sixth the time required by conventional methods. Furthermore, they have found that by adjusting the content of Mn among the metallic elements that are the main raw materials, it is possible to produce ultrafine equiaxed martensite with high strength and high ductility by quenching at a relatively low temperature of 750°C.

[0008] The present inventors have investigated the mechanism in detail and found that in the steel with an ultrafine ferrite-cementite structure as the pre-structure, Fe 3 Cementite in the form of (Fe 5 ,Mn 5 ) 3 It was found that, like C, part of the Fe (50 wt%) is replaced by Mn. In this way, it was discovered that the presence of a high concentration of Mn in cementite increases the rate of reverse transformation from ferrite to austenite and allows the annealing temperature to be lowered.

[0009] The present invention has been made based on the above findings, and has an objective of providing high-strength, high-ductility ultrafine ferrite-cementite structure steel, ferrite-austenite structure steel, ultrafine martensite structure steel, and ultrafine martensite-austenite structure steel that have sufficient mechanical strength and ductility even when used in parts such as buildings and bridges, automobile suspension steel, and machine gears, and further providing a manufacturing method by which these can be produced at a relatively low temperature in an extremely short time. [Means for solving the problem]

[0010] According to the present invention, in order to solve the above problems, the following technical means or techniques are provided. [1] A steel having an ultrafine ferrite-cementite structure, the contents of C, Si and Mn being 0.05wt%≦C≦0.3wt%, 0.5≦Si≦2wt%, 3wt%≦Mn≦10wt%, respectively, with the balance being Fe and unavoidable impurities, and the ferrite grain size being 2.0μm or less, wherein Mn is dissolved in the cementite, and the value of x in the chemical formula of the cementite (Fe1-x,Mnx)3C is 0.3 or more and less than 1. [2] An ultrafine-grained ferrite-austenite structure steel having a structure obtained by annealing the ultrafine-grained ferrite-cementite structure steel of the first invention described above between two phase regions, the ultrafine-grained ferrite-austenite structure steel having a tensile strength of 1400 MPa or more and a total elongation of 25% or more. [3] A high-strength, high-ductility ultrafine-grained ferrite-austenite steel according to the second aspect of the present invention, characterized in that it has a tensile strength of 1500 MPa or more and a total elongation of 30% or more. [4] The ultrafine ferrite-austenite structure steel of the third invention, wherein the austenite volume fraction is 40% or more and V γ xCin γ ≧0.07. [5] An ultrafine martensite steel having a structure obtained by annealing the ultrafine ferrite-cementite steel of the first invention in the austenite region before the annealing, characterized in that the ultrafine martensite steel has a tensile strength of 1500 MPa or more and a total elongation of 15% or more. [6] A martensite-austenite structure steel in which the ultrafine-grained ferrite-cementite structure steel of the first invention is used as a structure before annealing in the austenite region and two-phase region, the ultrafine-grained martensite-austenite structure steel being characterized in that it has a tensile strength of 1500 MPa or more and a total elongation of 20% or more. [7] A method for producing a steel with an ultrafine ferrite-cementite structure according to the first invention, comprising the steps of: subjecting a raw material having the above-mentioned chemical components to warm rolling at a rolling reduction rate of 50% or more in a temperature range of 300 to 600°C to form a fine ferrite-cementite structure; and concentrating Mn in the cementite. [8] A method for producing an ultrafine-grained ferrite-cementite steel produced by the seventh invention described above, comprising holding the steel at a temperature in the range of 625 to 750°C for 180 to 1200 seconds, and then cooling the steel in water or air. [9] A method for producing ultrafine martensite steel or martensite-austenite steel, comprising holding the ultrafine ferrite-cementite steel of the seventh invention at a temperature in the range of 625 to 800°C for 1 to 600 seconds, followed by water cooling or air cooling to produce a structure which is equiaxed martensite having a single block structure, or ultrafine equiaxed martensite-austenite steel having a single block structure. Effect of the Invention

[0011] According to the present invention, since the above-mentioned configuration is adopted, it is possible to obtain the excellent effect of having sufficient mechanical strength and ductility even when used for parts such as buildings and bridges, automobile suspension steel, machine gears, etc. In addition, it is possible to obtain the excellent effect of being able to produce ultrafine ferrite-cementite structure steel, etc. at a relatively low temperature in an extremely short time. [Brief description of the drawings]

[0012] [Figure 1] (a) is an SEM image of the fine ferrite-cementite (α+θ) structure before annealing in the dual-phase region, and (b) is an SEM image of the martensite (μ) structure. [Diagram 2] FIG. 2 is a diagram showing the relationship between the two-phase annealing time and the structure. [Diagram 3] FIG. 1 is a graph showing the change in austenite volume fraction with changes in intercritical annealing temperature and time. [Figure 4](a)(b)(c) are schematic diagrams of the process of austenite (γ) formation by reverse transformation. [Diagram 5] (a) SEM images of the fine ferrite-cementite (α+θ) structure before annealing, and (b) SEM images of the ferrite-cementite (α+θ) structure before annealing and the martensite (M) structure obtained by heating to 675°C and immediately water-cooling without holding at that temperature. [Figure 6] (a) TEM images of the fine ferrite-cementite (α+θ) structure before annealing, and (b) TEM images of the ferrite-cementite (α+θ) structure before annealing and the martensite (M) structure after heating to 675°C and immediately water-cooling without holding at that temperature. [Figure 7] FIG. 1 shows the results of a TEM-EDS analysis. [Figure 8] FIG. 1 shows the results of Mn concentration mapping by a field emission electron probe microanalyzer (FE-EPMA) for a ferrite-austenite (α+γ) structure after intercritical annealing. [Figure 9] FIG. 3 is a diagram showing nominal stress-nominal strain curves obtained in a round bar tensile test of the four ferrite-austenite (α+γ) structures shown in FIG. 2. [Figure 10] This figure shows the nominal stress-nominal strain curves of plate-shaped tensile test pieces of ferrite-cementite (α+θ) and martensite (M) structure steels annealed at 675°C for 3600 s, and the change in austenite (γ) volume fraction during tensile deformation. [Figure 11] This figure plots the relationship between the strength and ductility balance of ferrite-austenite (α+γ) structure steel and conventional TRIP steel, based on the plate tensile test results shown in Fig. 10. [Figure 12] FIG. 1 shows nominal stress-nominal strain curves of ferritic-austenitic steel with a 2%Si-5%Mn composition, annealed at 675° C. for 1 hour with varying C contents of 0.075, 0.1, 0.15, 0.2, and 0.3 wt. [Figure 13]FIG. 1 shows nominal stress-nominal strain curves of ferritic-austenitic steel with a 2%Si-5%Mn composition, annealed at 700° C. for 1 hour with varying C contents of 0.075, 0.1, 0.15, 0.2, and 0.3 wt. [Figure 14] FIG. 1 shows the relationship between uniform elongation and VγxCinγ in low carbon, 2%Si-5%Mn, ultrafine grained ferrite-austenite steel. [Figure 15] FIG. 1 is a graph showing the relationship between tensile strength and austenite volume fraction Vγ of a low-carbon, 2%Si-5%Mn, ultrafine-grained ferrite-austenite steel. [Figure 16] FIG. 1 is a diagram showing a nominal stress-nominal strain curve of a ferrite-austenite structure steel having an ultrafine ferrite-cementite structure steel with a composition of 0.15C-2%Si-5%Mn as a pre-annealing structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the present invention will be described in detail with reference to the embodiments. In this specification, the steel structures described as ultrafine-grained ferrite-cementite steel, ultrafine-grained ferrite-austenite steel, and ultrafine-grained martensite-austenite steel refer to dual-phase steels having the structures described before and after the hyphen.

[0014] The high-strength, high-ductility steel with an ultrafine-grained ferrite-cementite structure of the present invention has the following contents: C, Si and Mn are 0.05wt%≦C≦0.3wt%, 0.5≦Si≦2wt%, 3wt%≦Mn≦10wt%, respectively, with the balance being Fe and unavoidable impurities; the ferrite grain size is 2.0μm or less; Mn is dissolved in the cementite; and the value of x in the chemical formula of the cementite, (Fe1-x, Mnx)3C, is 0.3 or more and less than 1.

[0015] In the ferrite-cementite structure steel of the present invention, the C content is 0.05wt%≦C≦0.3wt%. C is necessary to ensure hardenability and tensile strength, but if it is less than 0.05wt%, the tensile strength of the steel may not be sufficiently satisfied, and if it exceeds 0.3wt%, the ductility and toughness of the steel may decrease, and the weldability may decrease.

[0016] In the ferrite-cementite structure steel of the present invention, the Si content is 0.5wt%≦Si≦2wt%. Si is a substitutional element that greatly hardens the material, and is an effective element for improving the strength of steel. However, if the Si content is excessively high, a large amount of Si scale is generated during heating in hot working, which results in extra costs for scale removal and makes surface defects more likely to occur due to the scale. Therefore, it is preferable that the upper limit of Si is 2wt%.

[0017] In the ferrite-cementite structure steel of the present invention, the Mn content is 3wt%≦Mn≦10wt%. Mn is an austenite forming element, improves hardenability, and forms martensite from fine γ grains. In addition, if the Mn content is within the above range, even if annealing is performed at a relatively low temperature and for a short time, Mn is dispersed and dissolved in the cementite formed during warm rolling at a high concentration where the value of x (weight ratio) in (Fe1-x, Mnx)3C is 0.3 or more and less than 1, for example, about 0.3 to 0.55, and it is considered that the high concentration of Mn effectively acts as a preferential nucleation site for reverse transformation austenite. As a result, it is possible to form highly stable austenite in a short time.

[0018] On the other hand, if the Mn concentration becomes too high, the segregation of Mn in the steel during solidification becomes excessive, impairing the uniformity inside the material. Also, surface cracks are more likely to occur during the hot working process in the material preparation process. Therefore, it is desirable to set the upper limit of Mn at 10 wt%.

[0019] The fine structure of the ultrafine ferrite-cementite steel of the present invention has a ferrite grain size of 2.0 μm or less, more preferably 1.0 μm. If the ferrite grain size exceeds 2.0 μm, the yield point decreases, which is undesirable.

[0020] The ultrafine ferrite-austenite structure steel of the present invention is an ultrafine ferrite-austenite structure steel having a structure obtained by annealing the ultrafine ferrite-cementite structure steel in a dual-phase intercritical region before annealing, and has a tensile strength of 1400 MPa or more and a total elongation of 25% or more. When the ultrafine ferrite-cementite structure steel is annealed in a dual-phase intercritical region before annealing, a higher austenite volume fraction can be obtained than in conventional TRIP steels, and although the amount of solute C in the austenite is low, the high concentration of solute Mn stabilizes the austenite and provides high ductility.

[0021] When the ultrafine-grained ferrite-cementite structure steel of the present invention is subjected to intercritical annealing before being annealed, it is possible to obtain a high-strength, high-ductility ultrafine-grained ferrite-austenite structure steel characterized by a tensile strength of 1500 MPa or more and a total elongation of 30% or more. For example, by annealing for an extremely short period of time, such as about 10 minutes, it is possible to obtain an ultrafine-grained ferrite-austenite structure steel having higher yield stress, tensile strength and total elongation than conventional TRIP steels and an extremely good balance of strength and ductility.

[0022] Furthermore, in the ultrafine ferrite-austenite structure steel of the present invention, the austenite volume fraction is 40% or more and V γ xCin γ It is considered preferable that V is ≧0.07. γ xCin γ ≧0.14 is an example.

[0023] The ultrafine martensite steel of the present invention is a martensite steel having a structure obtained by annealing the ultrafine ferrite-cementite steel in the austenite region before the annealing, and is preferably considered to have a tensile strength of 1500 MPa or more and a total elongation of 15% or more.

[0024] Moreover, it is considered preferable that the ultrafine martensite-austenite structure steel has a tensile strength of 1500 MPa or more and a total elongation of 20% or more.

[0025] Furthermore, the martensite-austenite steel of the present invention is a martensite-austenite steel having a structure before annealing in a dual-phase region that is the high-strength, high-ductility ultrafine-grained ferrite-cementite steel, and is preferably considered to have a tensile strength of 1400 MPa or more and a total elongation of 25% or more, and more preferably a tensile strength of 1500 MPa or more and a total elongation of 30% or more.

[0026] Martensite has a complex hierarchical structure made up of four components. Prior austenite (γ) grains, which are 30 μm in size, are packed with packets that are several μm in size, and these pockets are made up of long, thin blocks that are about 1 μm wide. These blocks are further made up of laths. In other words, the four components of prior austenite grains, packets, blocks, and laths are stacked on top of each other. Carbide particles several to tens of nm in size are dispersed at the grain boundaries and within the grains of these four components, forming a complex hierarchical structure.

[0027] Usually, one prior austenite (γ) grain in martensite has multiple packets, and within each packet, blocks with various orientations (variants) are transformed and generated. The block boundaries are high-angle grain boundaries. However, when the γ grain size is refined, single-packet multi-block martensite may be generated, and when refined further, single-block (single-variant) martensite may be generated. In other words, when prior austenite is refined, the number of blocks that can be generated within it decreases. Eventually, only one block can be generated. It is as if one prior austenite has transformed into one ferrite grain. However, generally, when the γ grain size is refined, the hardenability decreases and martensite does not form.

[0028] However, in the present invention, by adding an appropriate amount of Mn and forming the structure before the two-phase annealing into ultrafine ferrite-cementite, it is possible to make the prior γ grain size 2.0 μm or less, and by further adding an appropriate amount of Mn, it is possible to make the structure into equiaxed martensite with a single block structure. Here, ultrafine means that the prior austenite grain size is 2.0 μm or less. The single block structure means a structure in which only one block exists from the austenite grain. The adjacent blocks have different austenite parent phases. This can be confirmed by variant analysis of the EBSD (electron backscatter diffraction) observation results of the structure.

[0029] Next, a method for producing the steel with an ultrafine ferrite-cementite structure and the steel with an ultrafine ferrite-austenite structure of the present invention will be described.

[0030] In the method for producing steel with an ultrafine ferrite-cementite structure of the present invention, first, Fe powder, C powder, Si powder and Mn powder are adjusted to 0.05wt%≦C≦0.3wt%, 0.5≦Si≦2wt%, 3wt%≦Mn≦10wt%, with the remainder being Fe, to obtain a raw material. Then, the raw material with the above chemical components is subjected to warm rolling at a rolling reduction rate of 50% or more in the temperature range of 300 to 600°C to obtain a fine ferrite-cementite structure, and Mn is concentrated in the cementite.

[0031] The method for producing an ultrafine-grained ferrite-austenite structure steel of the present invention is characterized in that the ultrafine-grained ferrite-cementite structure steel produced by the above-mentioned method is held at a temperature in the range of 625 to 750°C for 180 to 1200 seconds, and then water-cooled or air-cooled.

[0032] Warm rolling may be any of the following industrially performed methods: flat roll rolling in a thick steel plate production line, forging in an extra-thick steel plate production line, grooved roll rolling in a bar or steel wire production line, and shaped roll rolling in a bar or shaped steel line. Plastic strain is applied to the material by any of these processing methods. This warm rolling is performed at a temperature range of 300 to 600°C with a rolling reduction of 50 to 90%, resulting in an ultrafine ferrite-cementite structure. If the warm rolling temperature is less than 300°C, cementite is not formed, while if it exceeds 600°C, austenite is reverse transformed and formed. If the rolling reduction rate is less than 50%, the initial structure is in a work hardened state, and fine ferrite and fine cementite are not sufficiently developed. During this warm rolling, the martensite structure, which is the structure before rolling, changes to a ferrite-cementite structure. The ferrite is ultrafine, and Mn is concentrated in the cementite.

[0033] The ultrafine ferrite-austenite structure steel obtained by warm rolling in this way is used as a structure before dual phase annealing, then held at a temperature range of 625-800°C for 1 second to 1 hour, and then cooled by water or air to produce a high strength, high ductility steel material with a structure of equiaxed martensite with a single variant or an ultrafine martensite-austenite structure. If the reheating temperature is less than 625°C, the ferrite-cementite structure does not completely reverse transform, and austenite fraction is not sufficiently obtained. If it exceeds 800°C, the reverse transformed austenite structure becomes coarse, and fine martensite cannot be obtained.

[0034] The method for producing ultrafine martensite steel and martensite-austenite steel of the present invention is characterized in that the ultrafine ferrite-cementite steel is held at a temperature in the range of 625 to 800°C for 1 to 600 seconds, and then water-cooled or air-cooled to produce a structure which is equiaxed martensite having a single block structure or an ultrafine equiaxed martensite-austenite steel having a single block structure. EXAMPLES

[0035] The present invention will now be described more specifically with reference to examples. <Example> (1) Test materials and structural observation As the main raw materials for melting, Fe powder, C powder, Si powder, and Mn powder (0.1wt%C-2wt%Si-5wt%Mn), with the remainder being Fe powder, were prepared. These main raw materials for melting were melted using a high-frequency vacuum induction heating furnace, and steel ingots measuring 100mm long x 100mm wide x 300mm high were cast to form the material for the high-strength, high-ductility steel material of the present invention. These materials were hot forged at 1200°C and formed into square bars measuring 38mm x 38mm.

[0036] Next, this material was heated at 550℃ for 1 hour, and then reheated every 3 passes. It was then warm grooved rolled at a reduction rate of 90% until the cross section was 14mm x 14mm, and the structure was preliminarily made into ultrafine ferrite-cementite. Figure 1(a) shows a photograph of the obtained ultrafine ferrite-cementite structure taken with a field emission scanning electron microscope (FE-SEM). The ferrite grain size of the obtained structure was approximately 0.5μm.

[0037] In order to make the structure of this rolled material martensite (comparative example), it was heated and held at 1200℃ for 1 hour to austenitize it, and then air-cooled. The FE-SEM image of the austenite structure after air-cooling is shown in Figure 1(b). In the following, ferrite is abbreviated as α, austenite as γ, cementite as θ, and martensite as M. The fine α+θ structure material and the comparative M structure material were heat-treated for 10 minutes, 30 minutes, and 1 hour, respectively, at 625℃ and 675℃, which are in the α+γ two-phase region.

[0038] The solute C concentration in the γ grains was determined from the results of X-ray diffraction using a SmartLab made by Rigaku Corp. The lattice constant can be calculated from the Bragg equation and the interplanar spacing d using formula (1).

[0039]

number

[0040] Since Cu-Kα radiation was used, λ = 1.542 (A) was substituted, and θ was the angle obtained by measurement. h, k, and l are plane indices (hkl). From this formula, the lattice constants of gamma in the gamma phase (111), (200), and (220) were calculated. These were then converted into (cos 2 θ / sinθ)+(cos 2 θ / θ) to 90, the lattice constant a of γ is calculated. γ (A) was calculated using the Dyson and Holmes formula shown in Equation (2).

[0041] Mn γ was calculated by substituting the Mn concentration in γ measured by a field emission electron probe microanalyzer (FE-EPMA).

[0042]

number

[0043] (2) Tensile test The tensile test was performed using a round bar tensile test piece with a diameter of 3.5 mm and a parallel section length of 24.5 mm taken from the heat-treated square bar at a crosshead speed of 0.5 mm / min (strain rate of 4.9 × 10 -4 s -1 The test was carried out at 17.0 mm. The displacement was measured using an extensometer with a gauge length of 17.0 mm.

[0044] (3) Tensile test In-situ transmission X-ray diffraction experiment In order to directly analyze the effect of γ in the α+γ structure obtained by dual-phase annealing on strength and ductility, the change in γ volume fraction during tensile testing was measured. Tensile test specimens were taken from heat-treated square bars so that the RD direction was the tensile direction. Plate-shaped tensile test specimens with a parallel section length of 12 mm and width of 2.5 mm were prepared. The plate thickness was thinned to 0.5 mm to allow the transmission of synchrotron radiation. In-situ measurement of the change in γ volume fraction while proceeding with tensile deformation requires a diffraction profile change over a wide range of diffraction angles in a short time. Therefore, in this example, the beamlines BL19B2 and BL15XU of the SPring-8 synchrotron radiation facility, which can use high-brightness X-rays, were used. The X-ray energy was 30 keV, and the beam size was 2.5 mm in the test specimen width direction and 200 μm in the tensile direction. A small tensile tester was installed on a goniometer, and X-rays were incident from the normal direction of the tensile test specimen. A one-dimensional detector, MYTHEN, or an imaging plate (IP) or a two-dimensional detector, PILATUS, was installed behind the test piece, and an in-situ transmission X-ray diffraction experiment was performed at 30 keV. The crosshead speed of the tensile test was 0.245 mm / min, and the time resolution was 2 s.

[0045] The initial γ volume fraction was calculated from the theoretical hkl diffraction intensity and the peak area intensity ratio of the α phase (110), (200), (211) and the γ phase (111), (200), (220) at the obtained scattering angle using Equation (3). The subscript j indicates the jth diffraction peak used in the calculation, and n indicates the number of diffraction peaks of γ and α used in the calculation (n = 3).

[0046]

number

[0047] The γ volume fraction during the tensile test was calculated from the product of the reduction rate from the initial peak area intensity sum of the γ phase (200), (211), and (311) and the initial γ volume fraction. <Comparative Example> Conventional TRIP steel was prepared as a comparative material. That is, a cold-rolled steel sheet with a composition of 0.13%C-2%Si-1.6%Mn was held at 830°C for 60 seconds, slowly cooled to 700°C at 10K / s, and then rapidly cooled to 400°C at 60K / s, and then austempered by holding at 400°C for 10s, 60s, and 480s. In all other respects, various tests were performed in the same manner as in the examples. <Result> Figure 1 (a) shows SEM images of the fine α+θ structure, which was the structure before dual-phase annealing, and (b) the M structure (comparative example). The fine α+θ structure is a structure consisting of fine elongated α grains and granular θ, with white particles of θ dispersed in large quantities at the α grain boundaries and within the grains. In contrast, the M structure is composed of packets and blocks, with the blocks being plate-like grains, with a large number of block boundaries and no θ. Dual-phase annealing was performed on these fine α+θ and M structures.

[0048] Figure 2 shows the relationship between the two-phase annealing time and the structure. The annealing times are limited to 600 s and 3600 s, and the EBSD-IPF (inverse pole figure) map, grain boundary map, and phase map are shown. The ND direction of the observation surface is mapped, and the relationship between color and orientation is shown in the stereo triangle. The red lines on the grain boundary map are high-angle grain boundaries with a misorientation angle of 15° or more, blue are medium-angle grain boundaries with a misorientation angle of 5 to 15°, and light blue are low-angle grain boundaries with a misorientation angle of less than 5°. It is composed almost entirely of high-angle grain boundaries. The red and green colors on the phase map represent the ferrite phase (α) and the austenite phase (γ), respectively.

[0049] When the fine α+θ structure before annealing was annealed in the two-phase region at 675°C, it became a structure consisting of α and γ, both of which were equiaxed, and the α and γ grain sizes were less than 2μm, resulting in an ultrafine equiaxed grain structure. This is because γ was generated using the θ grains dispersed in the structure before annealing as nuclei, and the shape of the γ was spherical near the grain boundary triple junction and plate-like on the grain boundaries.

[0050] On the other hand, when the comparative example, pre-annealed structure M, was annealed in the two-phase region at 675°C, both α and γ had plate-like and acicular structures, just like the pre-annealed structure. Martensite has a packet-block-lath structure, with the blocks consisting of a group of laths with almost the same crystal orientation, and blocks in the same packet share the (111) plane of the prior γ. The phase map and IPF map obtained by EBSD analysis confirmed that acicular γ had formed at the block boundaries. In addition, acicular γ had formed within the blocks. This is thought to be the result of γ also forming at the lath boundaries of M. From this, it is thought that the nucleation sites of γ are the lath and block boundaries of M.

[0051] When the annealing time was increased from 600 to 3600 s, the α grains became slightly coarser when the annealing time was increased from 600 to 3600 s. On the other hand, the γ grains increased in both size and volume fraction. When the annealing time was increased from 600 to 3600 s, the α grains and γ grains both became coarser.

[0052] Figure 3 shows the change in the austenite volume fraction with the change in temperature and time in the two-phase annealing. At all annealing temperatures, the austenite volume fraction increased with increasing annealing time. In addition, when comparing the same holding time, the austenite volume fraction increased at 675°C. This is thought to be because the phase ratio of austenite in the α-γ equilibrium fraction increases at higher annealing temperatures and also because diffusion becomes faster. When the prior structure was fine α+θ, a large amount of austenite was obtained with annealing at 675°C for 3600 s, with a volume fraction of 36.4%. In contrast, when the prior structure was M, the volume fraction was 24.3%. Furthermore, when the prior structure was fine α+θ, the austenite volume fraction was high at 20% even after a short annealing time of 600 s, which is twice the 10% obtained when the prior structure was M.

[0053] FIG. 4 is a schematic diagram of the process of γ generation by reverse transformation. As shown in FIG. 4(b), in the case of reverse transformation from the pre-annealing structure M, a large number of θ precipitate from M, which is a supersaturated C solid solution, at lath and block boundaries, which then combine and connect to grow into fine needle-like θ, and γ nucleates from the needle-like θ. As a result, acicular γ is thought to be generated from the needle-like θ. On the other hand, as shown in FIG. 4(a), in the case of reverse transformation from the pre-annealing structure of fine α+θ, γ nucleates from θ, which is originally dispersed in large amounts at the α grain boundaries and within the grains, and equiaxed γ is thought to be generated. In this way, it is believed that the finely dispersed θ acts effectively as a preferential nucleation site for reverse transformation γ, making it possible to form a large amount of γ (21%) in an extremely short time (600 s). For this reason, it is considered that it is extremely important in the present invention that the structure before two-phase annealing is ferrite-cementite.

[0054] According to Thermo-Calc calculations, the composition of θ at 550°C, which is the rolling temperature for producing the fine α+θ structure before annealing, is (Fe 0.49 , Mn 0.51 ) 3 C, and it is believed that Mn is highly concentrated in θ. On the other hand, when the structure before annealing is M, it is produced by quenching from 1200℃, so it is believed that Mn and C are uniformly present in the martensite.

[0055] Figures 5 and 6 show SEM and TEM images of the fine α+θ structure before annealing, and the α+θ and M structures before annealing, which were heated to 675°C and immediately water-cooled without holding. Samples for TEM observation were prepared using the extraction replica method. Figure 5(a) shows that in the fine α+θ structure, the elongated α has recrystallized and become equiaxed. θ can also be confirmed. Figure 5(b) shows the precipitation of many small spherical θ, and also the precipitation of an acicular structure.

[0056] As is clear from Fig. 6(a), the fine α+θ structure before annealing contains a large amount of θ grains. As shown in Fig. 6(b), the number of θ grains decreases and their size also becomes smaller immediately after heating to 675℃. This is because the formation of γ grains has started due to reverse transformation. When the structure before annealing is M, the acicular structure observed in Fig. 5(b) is thought to be θ grains from Fig. 6(c). Some of them are also thought to be γ grains. From the results of TEM-EDS analysis in Fig. 7, θ grains in the fine α+θ structure before annealing contained 50.8 (wt%) Mn, which is almost the stoichiometric composition. However, the Mn concentration in θ grains decreased immediately after heating to the two-phase region, which is thought to be because Mn migration to reverse transformation γ grains has already occurred. When the structure before annealing is Mn, the acicular θ grains were formed during the heating process, and the Mn concentration in θ grains was 36.6 (wt%), which was lower than that of the fine α+θ grains.

[0057] Therefore, when the pre-annealing structure is fine α+θ, Mn is already present in high concentration in the finely dispersed θ, and it is believed that this high concentration of Mn enables the rapid formation of highly stable γ. Furthermore, the concentration of Mn in the cementite is an essential phenomenon for rapid austenite formation.

[0058] Figure 8 shows the results of Mn concentration mapping by FE-EPMA for the α+γ structure after annealing in the dual-phase region. Figure 8(a) shows the results for a sample with a fine α+θ structure before annealing and annealed at 675℃ for 3600s, confirming that the Mn concentration in γ is extremely high. Quantitative analysis showed that the Mn concentration was 9.6wt% on average at five points that showed high concentrations.

[0059] On the other hand, FIG. 8(b) shows the results when the structure before annealing was M and annealing was performed at 675°C for 600 s. Mn concentration mapping confirmed that the Mn concentration was relatively uniform.

[0060] Figure 9 shows the nominal stress-nominal strain curves obtained in the round bar tensile tests of the four α+γ structures shown in Figure 2. When the prior structure was FAW α+θ, discontinuous yielding occurred, whereas when the prior structure was M, continuous yielding occurred, and the shapes of the nominal stress-nominal strain curves were different.

[0061] On the other hand, in both pre-annealing structures, as the annealing time in the two-phase region was increased, the yield stress decreased and the tensile strength increased. This is because, as is clear from Figure 2, when the pre-annealing structure is α+θ, the α grains become coarse as the annealing time is increased, and it is thought that the α grain size determines the yield point. When the pre-annealing structure is M, the blocks also clearly become coarse, and it is thought that this effect caused the yield point to decrease with long-term annealing. On the other hand, the tensile strength is higher with longer annealing times because the γ volume fraction increases, as is clear from Figure 3.

[0062] When the pre-annealing structure was α+θ, a very short annealing time (600 s) showed high yield stress (870 MPa), tensile strength (960 MPa) and total elongation (33.5%), with a strength-ductility balance of 32,200 MPa%, demonstrating excellent mechanical properties exceeding 30,000 MPa%, which is an indicator of excellent strength-ductility balance. Furthermore, even with an annealing time of 3,600 s, although the yield stress (770 MPa) decreased slightly, the material showed high tensile strength (1,090 MPa) and total elongation (32.4%), as well as a strength-ductility balance of 35,300 MPa%, demonstrating excellent mechanical properties. On the other hand, in the case of the comparative example where the pre-annealing structure was M, after an annealing time of 600 s, the specimen exhibited a yield stress (600 MPa), tensile strength (897 MPa) and total elongation (25.4%), resulting in a strength-ductility balance of 22,780 MPa%, and after an annealing time of 3,600 s, the specimen exhibited a yield stress (550 MPa), tensile strength (970 MPa) and total elongation (32.3%), resulting in a strength-ductility balance of 31,330 MPa%.

[0063] The α+θ structure before annealing provides a better balance of strength and ductility than M. As is clear from the results in Figure 3, the main reason for this is thought to be that the γ volume fraction is higher in the α+θ structure before annealing than in M.

[0064] Figure 10 shows the nominal stress-nominal strain curves and the change in γ volume fraction during tensile deformation for plate-shaped tensile test pieces of α+γ steel with α+θ and M prior structures and annealed at 675℃ for 3600s. For comparison, the nominal stress-nominal strain curves and the change in γ volume fraction during tensile testing for conventional TRIP steel (austempered for 480s) are also shown. As with the round bar tensile tests, the fine α+θ prior structure had superior strength and ductility compared to the M prior structure. Although the deformation-induced transformation progresses rapidly from the start of plastic deformation, the α+θ prior structure retains γ up to a higher strain range, which is thought to be the mechanism behind the high strength and high ductility. Although the γ volume fraction of conventional TRIP steel is low at 10%, γ remains up to a higher strain range, demonstrating the TRIP effect.

[0065] Table 1 shows the change in austenite stability caused by the intercritical annealing conditions.

[0066] [Table 1]

[0067] As shown in Table 1, the concentration of solute carbon in γ (C γ ) decreases as the annealing time increases. This means that the γ volume fraction (γ R ) increases. The product of solute carbon concentration and γ volume fraction, R ×C γ is an index that indicates how much of the 0.1% added C is dissolved in γ, and the maximum is 0.1. When the structure before annealing is M, γ R ×C γ is 0.033 to 0.057, which is considered to be a state in which a large amount of solute C remains in M. On the other hand, when the pre-annealing structure is fine α+θ, γ R ×C γThe α+θ ratio is 0.073-0.091, which means that after annealing for 3600 seconds, θ has almost completely changed to γ. Even after annealing for 600 seconds, θ has almost completely changed to γ. When the prior structure is α+θ, the added C precipitates as θ beforehand, which is thought to be the mechanism by which C can be efficiently dissolved in a large amount of γ. Conventional TRIP steel contains 0.13% C, while γ R ×C γ The carbon concentration ratio in gamma was 74%, which was almost the same as the 73% obtained when the pre-annealing structure was α+θ and annealed for 600 s. This means that the pre-annealing structure of α+θ gives an efficiency comparable to that of austempering.

[0068] The stability of gamma is considered using the Md30 formula shown in equation (4). Md30 is the temperature at which 50% of the entire structure transforms into the M phase when a tensile true strain of 0.30 is applied to a sample with a gamma single-phase structure. The higher this value, the more unstable gamma is.

[0069]

number

[0070] When the prior annealing structure was α+θ and annealed at 675°C for 3600 s, and when the prior annealing structure was M and annealed at 675°C for 3600 s, the Md30 was 200°C and 227°C, respectively. In the case of the prior annealing structure α+θ, despite the high gamma volume fraction, the stability was also high, so it is believed that gamma remained into the high strain range compared to when the prior annealing structure was M. This is believed to have resulted in high ductility. The Md30 of conventional TRIP steel was -76°C. Although the gamma volume fraction was low and the tensile strength was low, it is believed that the extremely high stability meant that high ductility was exhibited.

[0071] Figure 11 plots the relationship between the strength and ductility balance of the α+γ steel and conventional TRIP steel based on the results of the plate tensile tests shown in Figure 10. The strength and ductility balance of the α+γ steel with a 0.1%C-2%Si-5%Mn composition is superior to that of conventional TRIP steel. Conventional TRIP steel exhibits high ductility by concentrating extremely high C in a small amount of γ through austempering, but its strength is low due to its low γ volume fraction. In contrast, the α+γ steel with a 0.1%C-2%Si-5%Mn composition has a fine α+θ structure before annealing, which gives it a higher γ volume fraction than conventional TRIP steel. Although the amount of solute C in γ is low, the effect of solute Mn stabilizes γ, resulting in high ductility. Note that the total elongation depends on the size of the test piece, so this comparison was made using the same plate tensile test pieces. Even with an extremely short annealing time of 600 s, the steel showed excellent mechanical properties. <Strength test of ultrafine ferrite-austenite structure steels depending on carbon content> 2%Si-5%Mn steels with varying C contents of 0.075, 0.1, 0.15, 0.2, and 0.3wt% were prepared by vacuum melting and hot forging, and ultrafine ferrite (α) + austenite (γ) structures were prepared by warm groove rolling. These specimens were annealed in the two-phase region at 675°C and 700°C for 1 h each to prepare test materials. Strength and ductility were examined by round bar tensile tests, and the structures were observed by SEM-EBSD. Furthermore, thin plate specimens (GL = 12 mm, T = 0.4 mm) were prepared and in-situ XRD was performed during tensile deformation using high-brilliance X-rays from SPring-8. The γ volume fraction during the tensile test (CHS = 0.245 mm / min) was calculated from the integrated intensity ratio of each peak.

[0072] Figures 12 and 13 show the nominal stress-nominal strain curves (solid lines) and the γ volume fraction during tensile testing (dashed lines) of the test materials annealed at 675°C and 700°C, respectively. Comparing the physical properties of the 0.15C test materials from Figures 12 and 13, the 675°C annealed material showed a tensile strength of 1000MPa and a total elongation of 40%, with 5% γ remaining at the time of fracture, whereas the 700°C annealed material showed a tensile strength of 1480MPa and a total elongation of 30%.

[0073] Figure 14 shows the relationship between the γ volume fraction and tensile strength. It was confirmed from Figure 14 that the tensile strength increases as the γ volume fraction increases. Figure 15 shows the relationship between the γ volume fraction of the 675°C annealed material and the concentration of solute carbon in γ, Cin γ The product, V γ xCin γ The relationship between the uniform elongation and the strain is shown in Fig. γ xCin γ When we look at the circled area in Fig. 14, we can see that even though the solute carbon concentration in γ is the same, there is a difference of about 10% in the uniform elongation. γ xCin γ For example, V γ xCin γ From these, it is preferable that the tensile strength is determined by the γ volume fraction and the uniform elongation is determined by V γ xCin γ In addition, as shown in Fig. 16, the 700°C annealed material with 0.15% C had a large γ volume fraction of 45% and V γ xCin γ By achieving a content of 0.15%, outstanding ultra-high strength and high ductility were achieved.

Claims

1. An ultrafine equiaxed grain ferrite-austenite structure steel having a C, Si and Mn content of 0.05 wt%≦C≦0.3 wt%, 0.5 wt%≦Si≦2 wt%, 3 wt%≦Mn≦10 wt%, with the balance being Fe and unavoidable impurities, a ferrite grain size of 2.0 μm or less, and an austenite grain size of 2.0 μm or less, An ultrafine ferrite-austenite structure steel, characterized in that an austenite volume fraction is 40% or more, VγxCinγ≧0.07, where Vγ represents the austenite volume fraction, Cinγ represents a concentration of solute carbon in austenite, and the steel has a tensile strength of 1400 MPa or more and a total elongation of 25% or more.

2. A material having a martensite structure in which the contents of C, Si and Mn are 0.05 wt%≦C≦0.3 wt%, 0.5 wt%≦Si≦2 wt%, 3 wt%≦Mn≦10 wt%, respectively, with the balance being Fe and unavoidable impurities, is heated to a temperature range of 300 to 600° C. and subjected to warm rolling at a rolling reduction rate of 50% or more to obtain a fine ferrite-cementite structure having a ferrite grain size of 2 μm or less, Mn is concentrated in the cementite, and an ultrafine ferrite-cementite structure steel in which the value of x in the chemical formula of the cementite (Fe1-x, Mnx)3C is 0.3 or more and less than 1 is obtained; The ultrafine ferrite-cementite structure steel is held at a temperature range of 625 to 750° C. for 180 to 1200 seconds, and then water-cooled or air-cooled; A method for producing an ultrafine ferrite-austenite structure steel, comprising:

3. A material having C, Si and Mn contents of 0.05 wt%≦C≦0.3 wt%, 0.5 wt%≦Si≦2 wt%, 3 wt%≦Mn≦10 wt%, respectively, with the balance being Fe and unavoidable impurities, is heated to a temperature range of 300 to 600° C. and subjected to warm rolling processing at a rolling reduction rate of 50% or more to form a fine ferrite-cementite structure, and Mn is concentrated in the cementite to obtain an ultrafine ferrite-cementite structure steel; The ultrafine ferrite-cementite structure steel is held in a two-phase temperature range of 625 to 800°C for 1 to 600 seconds, and then water-cooled or air-cooled to produce a structure that is an ultrafine equiaxed martensite-austenite structure steel having a single block structure; A method for producing martensite-austenite steel, comprising:

Citation Information

Patent Citations

  • High strength steel material having excellent strength, ductility and energy absorption power, and method for producing the same

    JP2012224884A

  • Steel sheet for hot press and manufacturing method therefor, hot press member and manufacturing method therefor

    JP2017179589A

  • High strength high ductility fine martensite structure steel material and manufacturing method therefor

    JP2019143244A