Rod-shaped products
A rod-shaped molded product with optimized long and short glass fibers in a polyamide resin composition achieves high bending strength and reduced variability, addressing the strength and consistency issues of resin-based bolts.
Patent Information
- Application Number
- JP2020068038
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-06
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-04-06
AI Technical Summary
Existing resin-based bolts lack sufficient strength and exhibit significant variations in quality, making them unsuitable for applications requiring high strength and consistency.
A rod-shaped molded product is developed using a resin-attached fiber bundle of long glass fibers integrated with polyamide resin, combined with a mixture of short glass fibers, where the total fiber content ratio and length distribution are optimized to achieve a high bending strength with minimal variation.
The resulting molded product exhibits high bending strength with reduced variability, suitable for applications such as bolts and screws, by aligning long glass fibers and controlling the resin impregnation to enhance structural integrity.
Smart Images

Figure 0007553262000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rod-shaped molded product that can be used for bolts, screws, etc. [Background technology]
[0002] Resin bolts have the advantage of being lightweight, but compared to metal they are not as strong, so their strength is increased by blending fibrous fillers into the resin. Patent Document 1 describes an invention of a method for producing a rod-shaped molded article having a high degree of orientation of a fibrous filler in the longitudinal direction and high bending strength by using a specific gate for injection molding.
[0003] Patent Document 2 describes that a molded article obtained from a propylene-based resin composition containing (A) a resin-impregnated fiber bundle in which long carbon fibers having an average fiber length of 4 to 20 mm are integrated with a propylene-based resin, and (B) a mixture of short carbon fibers having an average fiber length of 0.01 to 0.5 mm and a propylene-based resin, the total content of the long carbon fibers and the short carbon fibers being 10 to 30 mass%, satisfying the relationship of long carbon fibers amount ≧ short carbon fibers amount, and having a specific gravity of 1.15 or less, can be used for automobile parts, electric / electronic parts, machine parts, sliding parts, sound absorbing materials, wood substitutes for buildings, housings for communication devices, radiation shielding materials, etc. (Claims and paragraph number 0040). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-24388 A [Patent Document 2] Patent No. 5255541 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a rod-shaped molded product which has high strength and little variation in quality and can be used for bolts, screws, etc. [Means for solving the problem]
[0006] The present invention comprises: (A) a resin-adhered fiber bundle having a length of 4 to 20 mm in which long glass fibers and polyamide-based resin are integrated; (B) A rod-shaped molded product made of a polyamide-based resin composition containing a mixture of short glass fibers having a weight-average fiber length of 0.01 to 1 mm and a polyamide-based resin, the total content of the long glass fibers and the short glass fibers in the composition is 10 to 70 mass %, and the relationship of the content of the long glass fibers ≧ the content of the short glass fibers is satisfied; The weight average fiber length of the glass fibers in the rod-shaped molded product is 0.5 mm or more, The bending strength (MPa) of ten of the rod-shaped articles is within a range of 0.90 to 1.10 times the average value of the above. Effect of the Invention
[0007] The rod-shaped product of the present invention has high strength (high bending strength) and the variation in bending strength between a plurality of rod-shaped products is small. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <Polyamide resin composition> The resin-adhered fiber bundle of component (A) is a bundle of long glass fibers that are bundled in a state of being aligned in the length direction, to which a polyamide-based resin has been brought into contact and adhered, and then cut into pieces in the range of 4 to 20 mm. Depending on the state of adhesion, the resin-attached fiber bundles of component (A) may be The resin is permeated (impregnated) to the center of the long glass fiber bundle, and the resin penetrates into the spaces between the fibers in the center of the fiber bundle (hereinafter referred to as "resin-impregnated fiber bundle"). A fiber bundle in which only the surface of the long glass fiber bundle is covered with resin (hereinafter referred to as "resin surface-coated fiber bundle"); It also includes something in between these two (wherein the surface of the fiber bundle is covered with resin, the resin is impregnated only near the surface, and the resin does not penetrate to the center) (hereinafter referred to as "partially resin-impregnated fiber bundle").
[0009] The polyamide resin can be one or more selected from polyamide 6, polyamide 66, polyamide 610, polyamide 612, polyamide 11, polyamide 12, polyamide 1010, polyamide 46, polyamide MXD, polyamide 6T, polyamide 9T, polyamide 10T, polyamide 6I, polyamide M5T, polyamide 6 / 66, polyamide 1212, polyamide 66 / 6T, polyamide 66 / 6I, and polyamide 6T / 6I / 66.
[0010] The long glass fibers may be made of known E glass, C glass, S glass or D glass.
[0011] The length of the resin-adhered fiber bundle of the component (A) is 4 to 20 mm, in a preferred embodiment of the present invention it is 5 to 15 mm, and in another preferred embodiment of the present invention it is 7 to 12 mm. The length of the resin-adhered fiber bundle is the same as the length of the long glass fibers contained in the resin-adhered fiber bundle. The diameter of the resin-coated fiber bundle is not particularly limited, but may be in the range of 0.8 to 5 mm, for example.
[0012] The long glass fibers contained in the resin-attached fiber bundle may have a fiber diameter (single fiber diameter) of 6 to 30 μm. When glass fibers having a fiber diameter of 17 μm are used, the number of long glass fibers constituting the fiber bundle is 100 to 30,000 in a preferred embodiment of the present invention, 500 to 20,000 in another preferred embodiment of the present invention, and 1,000 to 10,000 in yet another preferred embodiment of the present invention.
[0013] The resin-attached fiber bundle can be produced by a well-known manufacturing method using a die. For example, in addition to paragraph number 7 of JP-A-6-313050 and paragraph number 23 of JP-A-2007-176227, JP-B-6-2344 (Manufacturing method and molding method for resin-coated long fiber bundle), JP-A-6-114832 (Fiber-reinforced thermoplastic resin structure and its manufacturing method), JP-A-6-293023 (Manufacturing method for long fiber reinforced thermoplastic resin composition), JP-A-7-205317 (Method for taking out fiber bundle and manufacturing method for long fiber reinforced resin structure), JP-A-7-216104 (Manufacturing method for long fiber reinforced resin structure), JP-A-7-251437 (Manufacturing method and manufacturing apparatus for long fiber reinforced thermoplastic composite material), JP-A-8-118490 (Manufacturing method for crosshead die and long fiber reinforced resin structure), etc. can be applied. As the resin-coated fiber bundle, the Plastron (registered trademark) series, which contains polyamide resin and glass fiber and is sold by Daicel Polymer Co., Ltd., can also be used.
[0014] The content ratio of polyamide resin and long glass fiber in the resin-adhered fiber bundle of component (A) is 90 to 30 mass% polyamide resin and 10 to 70 mass% long glass fiber in a preferred embodiment of the present invention, 80 to 40 mass% polyamide resin and 20 to 60 mass% long glass fiber in another preferred embodiment of the present invention, and 70 to 40 mass% polyamide resin and 30 to 60 mass% long glass fiber in yet another preferred embodiment of the present invention.
[0015] The resin-attached fiber bundle of component (A) may contain known additives as necessary. Examples of known additives include release agents, antistatic agents, flame retardants, colorants, plasticizers, softeners, dispersants, stabilizers (antioxidants such as hindered phenol-based antioxidants, phosphorus-based antioxidants, and sulfur-based antioxidants, ultraviolet absorbers, heat stabilizers, etc.), antiblocking agents, crystal nucleus growth agents, fillers (particulate fillers such as silica and talc, etc.), and lubricants.
[0016] Component (B) is a mixture of short glass fibers having a weight-average fiber length of 0.01 to 1 mm and a polyamide resin. The mixture may be a mixture of short glass fibers and powdered polyamide-based resin, or may be a molded product such as pellets containing short glass fibers and polyamide-based resin. The mixture may contain the same resin additives as component (A).
[0017] The polyamide resin used may be the same as that used in component (A), but it may also be a polyamide resin different from that used in component (A). The short glass fibers that can be used are made of known E glass, C glass, S glass, or D glass.
[0018] The length of the short glass fibers contained in component (B) is from 0.01 to 1 mm in a preferred embodiment of the present invention, and from 0.02 to 0.5 mm in another preferred embodiment of the present invention.
[0019] The content ratio of polyamide resin and short glass fiber in the mixture of component (B) is 20 to 80 mass% polyamide resin and 80 to 20 mass% short glass fiber in a preferred embodiment of the present invention, 30 to 70 mass% polyamide resin and 70 to 30 mass% short glass fiber in another preferred embodiment of the present invention, and 40 to 60 mass% polyamide resin and 60 to 40 mass% short glass fiber in yet another preferred embodiment of the present invention.
[0020] The total content of the long glass fibers and short glass fibers in the polyamide resin composition is 10 to 70 mass %, in a preferred embodiment of the present invention it is 20 to 60 mass %, and in another preferred embodiment of the present invention it is 30 to 60 mass %.
[0021] The content ratio of the long glass fiber and the short glass fiber in the polyamide resin composition satisfies the relationship of the content ratio of the long glass fiber≧the content ratio of the short glass fiber. The content ratio of the long glass fiber and the short glass fiber in the polyamide resin composition is 55 to 95 mass% of the long glass fiber and 5 to 45 mass% of the short glass fiber, based on 100 mass% in total of the content of the long glass fiber and the short glass fiber, in a preferred embodiment of the present invention, 65 to 95 mass% of the long glass fiber and 5 to 35 mass% of the short glass fiber, and in a further preferred embodiment of the present invention, 75 to 95 mass% of the long glass fiber and 5 to 25 mass% of the short glass fiber.
[0022] <Rod-shaped molded product> The rod-shaped product may be any product as long as it satisfies the relationship: length of the rod-shaped product≧length in the width direction of the rod-shaped product. The rod-shaped product may have a cross-sectional shape in the width direction that is circular, elliptical, polygonal, irregular, or the like. The length of the rod-shaped product is the length from one end face to the other end face when the product is a cylinder or a prism. When the cross-sectional shape in the width direction is circular, the length in the width direction is the diameter, when the cross-sectional shape in the width direction is elliptical, the length in the width direction is the major axis length, and when the cross-sectional shape in the width direction is polygonal or irregular, the length in the width direction is the maximum length.
[0023] The weight average fiber length of the glass fibers contained in the rod-shaped molded product is 0.5 mm or more, in a preferred embodiment of the present invention, the weight average fiber length is 0.7 mm or more, and in another preferred embodiment of the present invention, the weight average fiber length is 1.0 mm or more.
[0024] The bending strength (MPa) of ten rod-shaped molded products is within the range of 0.90 to 1.10 times the average value, and in a preferred embodiment of the present invention, the bending strength (MPa) is within the range of 0.92 to 1.08 times the average value. The numerical range is the minimum value / average value to the maximum value / average value.
[0025] The rod-shaped molded product can be produced by applying a known injection molding method, or by applying the rod-shaped molded product production method described in JP-A-2017-24388 and JP-A-2017-24389. The rod-shaped product may be selected from the group consisting of pins, screws, threaded bolts, hexagonal bolts, and fully threaded hexagonal bolts.
[0026] The configurations and combinations thereof in each embodiment are merely examples, and addition, omission, substitution, and other modifications of the configurations are possible as appropriate without departing from the spirit of the present invention. The present invention is not limited to the embodiments, but is limited only by the claims. EXAMPLES
[0027] (1) Weight average fiber length of short glass fibers of component (B) The value was calculated from 500 short glass fibers of component (B). The formula used was
[0044] and
[0045] in JP 2006-274061 A.
[0028] (2) Weight average fiber length of glass fibers in rod-shaped molding The rod-shaped bodies obtained in the Examples and Comparative Examples were measured by the following method described in paragraph 0063 of JP2013-121988A. A sample of about 3 g was cut out from the rod-shaped molded product, heated to 650°C, incinerated, and the fibers were extracted. The weight-average fiber length was calculated from a portion (500 pieces) of the extracted glass fibers. The formulas used were
[0044] and
[0045] in JP 2006-274061 A.
[0029] (3) Bending strength The bending strength of the rod-shaped bodies obtained in the Examples and Comparative Examples was measured under the following conditions. Measuring equipment: Autograph AG2000 (Shimadzu Corporation) Test speed: 2mm / min Distance between supports: 40mm
[0030] Examples 1 and 2, Comparative Examples 1 to 3 The components (A) and (B) used in the examples and comparative examples are as follows. Component (A): Resin-impregnated fiber bundle consisting of 50% by mass of polyamide MXD6 and 50% by mass of long glass fiber (Plastron PAX-GF50-02; cylindrical shape with a diameter of 2.8 mm and a length of 9 mm; Daicel Polymer Co., Ltd.). The length of the resin-impregnated fiber bundle is the same as the length of the glass fiber contained therein. Component (B): Cylindrical pellets consisting of 50% by mass of polyamide MXD6 and 50% by mass of short glass fibers (Plastron PAX-SGF50; cylindrical shape with a diameter of 2.4 mm and a length of 4.0 mm; Daicel Polymer Co., Ltd.) were used. The weight average fiber length of the glass fibers contained in the resin was 0.3 mm.
[0031] Each composition of the Examples and Comparative Examples was injection molded under the following conditions to obtain round bars with a diameter of 12 mm and a length of 80 mm. The weight-average fiber length and bending strength of the obtained round bars were measured. Ten pieces were measured for each example, and the weight-average fiber length is the average value of the ten molded pieces. The results are shown in Table 1. (Injection molding conditions) Injection molding machine: Japan Steel Works J150EII Cylinder temperature: 280℃ Back pressure: 2MPa Mold temperature: 160℃ Gate: The same gate as in Example 1 (FIG. 4(a)) of JP2017-24388A was used.
[0032] [Table 1]
[0033] Comparing Examples 1 and 2 with Comparative Examples 1 to 3, it was found that by using the (A) component and the (B) component in a predetermined ratio, the bending strength of the obtained molded body could be increased to a high level and the variation in bending strength could be reduced. [Industrial Applicability]
[0034] The rod-shaped product of the present invention can be used as various pins, various screws, cut bolts, hexagonal bolts, fully threaded hexagonal bolts and other bolts.
Claims
1. (A) a resin-coated fiber bundle having a length of 4 to 20 mm in which long glass fibers and polyamide-based resin are integrated; (B) A rod-shaped molded product made of a polyamide-based resin composition containing a mixture of short glass fibers having a weight-average fiber length of 0.01 to 1 mm and a polyamide-based resin, the total content of the long glass fibers and the short glass fibers in the composition is 10 to 70 mass %, and the relationship of the content of the long glass fibers ≧ the content of the short glass fibers is satisfied; The weight average fiber length of the glass fibers in the rod-shaped molded product is 0.5 mm or more, The bending strength (MPa) of ten of the rod-shaped molded products is within a range of 0.90 to 1.10 times the average value of the above. The rod-shaped product is selected from the group consisting of pins, screws, cut bolts, hexagonal bolts, and fully threaded hexagonal bolts.
2. The length of the resin-adhered fiber bundle of the component (A) and the long glass fiber contained in the resin-adhered fiber bundle is 4 to 20 mm, and the weight average fiber length of the short glass fiber contained in the component (B) is 0.02 to 0.5 mm.
3. 3. The rod-shaped molded product according to claim 1, wherein the content of the long glass fibers and the short glass fibers is 55 to 95 mass % and 5 to 45 mass %, respectively, based on a total of 100 mass % of the long glass fibers and the short glass fibers.
4. 3. The rod-shaped molded product according to claim 1, wherein the content of the long glass fibers and the short glass fibers is 65 to 95 mass % and 5 to 35 mass %, respectively, based on a total of 100 mass % of the long glass fibers and the short glass fibers.
5. The rod-shaped molded product according to any one of claims 1 to 4, wherein the weight average fiber length of the glass fibers in the rod-shaped molded product is 0.7 mm or more.
6. The rod-shaped molded product according to any one of claims 1 to 4, wherein the weight average fiber length of the glass fibers in the rod-shaped molded product is 1.0 mm or more.
7. The rod-shaped molded product according to any one of claims 1 to 6, wherein the bending strength (MPa) of the 10 rod-shaped molded products is within a range of 0.90 to 1.10 times the average value thereof.
Citation Information
Patent Citations
Flame retardant combinations for polymer compositions and use thereof
CN109467751A
Corona discharge device for separating record sheet
JP1977055541A
Long-fiber-reinforced polyamide resin composition and its molded product
JP1993208418A
Continuous filament-reinforced polyamide resin composition and its molding
JP1994107944A
Pellet for molding fiber reinforced synthetic resin product
JP1994287317A