Polyhydric hydroxy resin, its production method, epoxy resin composition containing same, and cured epoxy resin product

A polyhydric hydroxy resin with an ester structure addresses the issues of high melting points and poor solubility in epoxy resin compositions, resulting in a cured product with enhanced thermal conductivity and reduced thermal expansion for semiconductor encapsulation and heat dissipation.

JP7553271B2Active Publication Date: 2024-09-18NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020110718
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-26
Publication Date
2024-09-18
Estimated Expiration
2040-06-26

AI Technical Summary

Technical Problem

Existing epoxy resin compositions face challenges with high melting points, poor solvent solubility, and difficulty in uniform mixing, leading to reduced curability, heat resistance, and thermal conductivity, making them unsuitable for high-density semiconductor packaging and heat dissipation applications.

Method used

A polyhydric hydroxy resin with an ester structure, represented by specific general formulas, is used to create an epoxy resin composition that includes this resin as a curing agent, enhancing solvent solubility and thermal conductivity while maintaining low viscosity and ease of handling.

Benefits of technology

The resulting cured epoxy resin exhibits excellent thermal conductivity, improved solvent solubility, and reduced thermal expansion, suitable for semiconductor encapsulation and heat dissipation substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553271000010
    Figure 0007553271000010
  • Figure 0007553271000012
    Figure 0007553271000012
  • Figure 0007553271000011
    Figure 0007553271000011
Patent Text Reader

Abstract

To provide a polyhydric hydroxy resin and an epoxy resin composition that are excellent in reliability and are suitable as insulation materials for electric / electronic components, such as semiconductor sealing, laminates, heat-radiation substrates.SOLUTION: The present invention discloses a polyhydric hydroxy resin represented by general formula (1), the polyhydric hydroxy resin containing at least one ester structure, and an epoxy resin composition containing the same and a cured epoxy resin [where, X is an OH group or a polyhydric hydroxyaryl group having an ester structure, n is a number of larger than 0 and 20 or less].SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyhydric hydroxy resin, a production method thereof, and an epoxy resin composition and cured epoxy resin product using the same. More specifically, the present invention relates to a polyhydric hydroxy resin which is useful as an insulating material for electric and electronic components such as semiconductor encapsulation, laminates, and heat dissipation substrates and which has excellent handleability as a solid at room temperature, low viscosity during molding, and solvent solubility, a production method thereof, an epoxy resin composition, and an epoxy resin cured product obtained by curing the same and which has excellent thermal conductivity, heat resistance, and low thermal expansion. [Background technology]

[0002] In recent years, in electronic devices, semiconductor packages have become more densely mounted, and LSIs have become more highly integrated and faster, so materials with higher dimensional stability are required. Furthermore, with the progress of single-sided mounting of packages, reducing package warpage has become an important issue, and the development of resins with lower thermal expansion is required. In response to the above trends, heat dissipation measures for heat generated from elements have become a very important issue. In particular, in the field of power devices, heat dissipation from electronic circuits has become large, so the heat dissipation of cured resins used in insulating parts has become an issue. Conventionally, this heat dissipation was achieved by the thermal conductivity of the filler, but in order to achieve even higher integration, it has become necessary to improve the thermal conductivity of the matrix resin itself.

[0003] As an epoxy resin composition having excellent high thermal conductivity, one using an epoxy resin having a mesogenic structure is known. For example, Patent Document 1 discloses an epoxy resin composition containing a biphenol-type epoxy resin and a polyhydric phenol resin curing agent as essential components, and discloses that the composition has excellent stability and strength at high temperatures and can be used in a wide range of fields such as adhesion, casting, sealing, molding, lamination, etc. Patent Document 2 discloses an epoxy compound having two mesogenic structures linked by a bent chain in the molecule. Furthermore, Patent Document 3 discloses a resin composition containing an epoxy compound having a mesogenic group.

[0004] However, such epoxy resins with mesogenic structures have high melting points, and when mixing, the high melting point components are difficult to dissolve and remain undissolved, resulting in problems with reduced curability and heat resistance. Also, high temperatures are required to mix such epoxy resins uniformly with the curing agent. At high temperatures, the curing reaction of the epoxy resin proceeds rapidly and the gelation time is shortened, severely limiting the mixing process and making it difficult to handle. If a soluble third component is added to compensate for this drawback, the melting point of the resin decreases, making it easier to mix uniformly, but the cured product has a problem of reduced thermal conductivity.

[0005] As a highly thermally conductive resin that can be melt-mixed, Patent Document 4 discloses an epoxy resin obtained by epoxidizing a mixture of hydroquinone and 4,4'-dihydroxybiphenyl, and Patent Document 5 discloses an epoxy resin obtained by epoxidizing a mixture of 4,4'-dihydroxydiphenylmethane and 4,4'-dihydroxybiphenyl. However, these resins have poor solubility in solvents, and their applications are limited.

[0006] Patent Document 6 discloses an epoxy resin composition using a phenolic compound having a diphenyl ester structure, but because of its high melting point, it is difficult to melt and knead uniformly, and fine pulverization by jet mill grinding or the like is necessary, and because of its poor solvent solubility, it is difficult to apply it to substrates or sheets that require varnish formation. Patent Document 7 discloses a bifunctional ester group-containing phenol of hydroquinone and p-hydroxybenzoic acid, but because of its high crystallinity, there are problems with solvent solubility and melt kneadability. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 7-90052 [Patent Document 2] Japanese Patent Application Publication No. 9-118673 [Patent Document 3] Japanese Patent Application Publication No. 11-323162 [Patent Document 4] WO2009 / 110424 [Patent Document 5] JP 2010-43245 A [Patent Document 6] JP 2010-184993 A [Patent Document 7] US4762901 publication Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, an object of the present invention is to provide a polyhydric hydroxy resin which overcomes the above-mentioned problems, is useful as an insulating material for electric and electronic components such as semiconductor encapsulation, laminates, and heat dissipation substrates, has excellent handleability as a solid at room temperature, has low viscosity during molding, and has excellent solvent solubility, and is also useful as an insulating material for electric and electronic components such as semiconductor encapsulation, laminates, and heat dissipation substrates, and provides a method for producing the same, an epoxy resin composition containing the same, and a cured epoxy resin product. [Means for solving the problem]

[0009] Through extensive research, the present inventors have discovered that a polyhydric phenol resin having a specific ester group is expected to solve the above problems, and that the cured product thereof exhibits an effect on thermal conductivity.

[0010] That is, the present invention relates to a polyhydric hydroxy resin represented by the following general formula (1), which contains at least one ester structure. [ka] [wherein X represents an OH group or a monovalent substituent represented by formula (a), and n represents a number greater than 0 and less than or equal to 20.] [ka] (Here, Y represents an aromatic hydrocarbon group having 6 to 12 carbon atoms, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, and p represents a number from 1 to 3.)

[0011] The polyhydric hydroxy resin preferably has a number average molecular weight of 3,000 or less.

[0012] The present invention also relates to a method for producing the above-mentioned polyhydric hydroxy resin, which comprises reacting 0.1 to 0.7 moles of an OH group-containing ester represented by general formula (3) with 1 mole of OH groups of the polyhydric hydroxy resin represented by general formula (2). [ka] (Here, n is a number greater than 0 and less than or equal to 20.) [ka] (wherein Y represents an aromatic hydrocarbon group having 6 to 12 carbon atoms, and R and R 1 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, and p represents a number from 1 to 3.

[0013] The present invention also relates to an epoxy resin composition comprising an epoxy resin and a curing agent, characterized in that any of the polyhydric hydroxy resins described above is used as an essential component as a part or the whole of the curing agent.

[0014] The epoxy resin in the epoxy resin composition of the present invention is preferably a difunctional crystalline epoxy resin.

[0015] Furthermore, the present invention relates to an epoxy resin cured product obtained by curing the above-mentioned epoxy resin composition. Effect of the Invention

[0016] The polyhydric hydroxyl resin of the present invention and the epoxy resin composition using the same are excellent in solvent solubility, moldability, and reliability, and exhibit excellent high thermal conductivity of the cured product. In addition, by suppressing crystallinity, the yield is improved, which is advantageous in terms of production. Furthermore, it has been found that the hydroquinone-based polyhydric hydroxyl resin, which is the basic skeleton, has the effect of suppressing the increase in molecular weight due to self-polymerization during esterification. This makes it possible to control the molecular weight and esterification ratio, which is usually difficult. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a GPC chart of the ester group-containing polyhydric hydroxy resin (Example 1). [Diagram 2] FIG. 2 is an IR chart of the ester group-containing polyhydric hydroxy resin (Example 1). [Diagram 3] FIG. 3 is an FD-MS spectrum of the ester group-containing polyhydric hydroxy resin (Example 1). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below.

[0019] The polyhydric hydroxy resin of the present invention is represented by the above general formula (1) and contains at least one ester structure represented by formula (a). n is the number of repetitions (number average) and is a number greater than 0 and not greater than 20. Since the component with n=0 has the strongest crystallinity and excellent orientation while having low solvent solubility, it is preferably a mixture of components with different n values. Furthermore, a component with a large n has high viscosity, reduces fluidity, and requires a long time to dissolve in a solvent due to self-aggregation, so it is more preferably a mixture of components with n greater than 0 and not greater than 10. As for the molecular weight, the number average molecular weight is preferably 3000 or less.

[0020] The ester structure, which is a monovalent substituent, is represented by the above formula (a), where Y represents an aromatic hydrocarbon having 6 to 12 carbon atoms, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, and p represents a number from 1 to 3. Preferred structures of Y are a benzene ring, a naphthalene ring, and a biphenyl structure. Furthermore, the more rigid the polycyclic aromatic, the more it contributes to orientation and thermal stability, but the more the solvent solubility decreases and it becomes difficult to balance with reactivity, so a more preferred structure is a benzene ring. In a structure in which the number of OH groups in the monovalent substituent is 2 or more, the reaction control becomes complicated and abrupt, and it is also difficult to universally supply raw materials, so p is more preferably 1.

[0021] The polyhydric hydroxy resin containing an ester structure represented by the above general formula (1) can be obtained by reacting the polyhydric hydroxy resin represented by the above general formula (2) with the OH group-containing ester represented by the above general formula (3) under an acid catalyst. For this reaction, normal esterification conditions can be appropriately adopted. Here, the polyhydric hydroxy resin represented by the general formula (2) can be obtained by a condensation reaction between hydroquinone and formaldehyde. The production method is a general phenol resin production method, and paraform or formalin may be used as formaldehyde, and the reaction may be carried out under an acid catalyst. The ratio of formaldehyde used as a condensation agent to 1 mole of OH group of hydroquinone is preferably in the range of 0.1 to 0.5 moles, more preferably in the range of 0.2 to 0.4 moles. If it is more than 0.5 moles, the viscosity increases and the solvent solubility decreases, making it difficult to handle. If the amount is less than 0.1 mol, the amount of the polymerizable component is small, and a large amount of unreacted monomer remains, which may result in a decrease in the heat resistance, thermal conductivity, mechanical strength, etc. of the cured product. In addition, when removing a large amount of unreacted hydroquinone, a high-temperature and high-pressure process is required, which is also a problem in terms of production, so the above range is preferable. In addition, the OH group-containing ester represented by the general formula (3) includes p-hydroxybenzoic acid, 4-hydroxy-2 methylbenzoic acid, 4-hydroxy-3 methylbenzoic acid, 2,4-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 6-hydroxy-2 naphthoic acid, 3,5-dihydroxy-2-naphthalene carboxylic acid, and 4-(4-hydroxyphenyl)benzoic acid, and the carboxylic acid ester includes methyl p-hydroxybenzoate, ethyl p-hydroxybenzoate, methyl 6-hydroxy-2 naphthoate, ethyl 6-hydroxy-2 naphthoate, and methyl 4'-hydroxy[1,1'-biphenyl]-4-carboxylate, etc., and in terms of reactivity and solvent solubility, p-hydroxybenzoic acid and methyl p-hydroxybenzoate are preferred. As the modification rate of the esterification in these reactions, it is preferable to react 0.1 to 0.7 moles of the OH group-containing ester represented by the general formula (3) with 1 mole of the OH group of the polyhydric hydroxy resin represented by the general formula (2). If the amount is less than 0.1 mol, the effect of promoting orientation is small, and no improvement in thermal conductivity during curing can be expected.On the other hand, if it is more than 0.7 mol, it is not preferable because steric hindrance becomes large and it becomes a factor of irregular orientation. In addition, since self-polymerization of OH-containing carboxylic acid is likely to occur as a side reaction, partial esterification is preferable. More preferably, the range of 0.4 to 0.6 mol is preferable from the viewpoint of improving the thermal conductivity of the cured product.

[0022] The epoxy resin composition of the present invention is an epoxy resin composition containing an epoxy resin and a curing agent, and contains, as an essential component, a polyhydric hydroxyl resin represented by the above general formula (1) as a part or all of the curing agent.

[0023] The amount of epoxy resin is determined by considering the equivalent balance with the OH group of the curing agent. For 1 equivalent of epoxy group, the OH group of the curing agent is generally in the range of 0.5 to 2.0 equivalents, preferably 0.7 to 1.5 equivalents. Outside this range, unreacted monomers remain, which may reduce the heat resistance, thermal conductivity, mechanical strength, etc. of the cured product.

[0024] In addition to the polyhydric hydroxy resin of the present invention represented by the general formula (1), other types of curing agents may be blended in the epoxy resin composition as a curing agent component, and all types of curing agents generally known as curing agents can be used. Examples of such other types of curing agents include dicyandiamide, polyhydric phenols, acid anhydrides, aromatic and aliphatic amines, etc. Specific examples of polyhydric phenols include dihydric phenols such as bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, 4,4'-biphenol, 2,2'-biphenol, hydroquinone, resorcin, and naphthalenediol, and trihydric or higher phenols such as tris-(4-hydroxyphenyl)methane, 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, phenol novolac, o-cresol novolac, naphthol novolac, and polyvinylphenol. Further examples include polyhydric phenolic compounds synthesized by using dihydric phenols such as phenols, naphthols, bisphenol A, bisphenol F, bisphenol S, fluorene bisphenol, 4,4'-biphenol, 2,2'-biphenol, hydroquinone, resorcin, and naphthalenediol with a condensing agent such as formaldehyde, acetaldehyde, benzaldehyde, p-hydroxybenzaldehyde, or p-xylylene glycol.

[0025] Examples of the acid anhydride include phthalic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylhimic anhydride, nadic anhydride, and trimellitic anhydride.

[0026] Furthermore, the amines include aromatic amines such as 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylsulfone, m-phenylenediamine, and p-xylylenediamine, and aliphatic amines such as ethylenediamine, hexamethylenediamine, diethylenetriamine, and triethylenetetramine. In the resin composition of the present invention, one or more of these curing agents can be used in combination. In the case of the epoxy resin composition of the present invention, the amount of the polyhydric hydroxyl resin represented by the general formula (1) is preferably in the range of 5 to 100 wt %, and more preferably 60 to 100 wt %, of the total amount of the curing agent. From the viewpoint of reliability and thermal conductivity of the cured product, the other curing agent is preferably a dihydric phenol, and more preferably 4,4'-biphenol, 2,2'-biphenol, hydroquinone, resorcin, naphthalenediol, or 4,4'-dihydroxydiphenyl ether.

[0027] As the epoxy resin component in the epoxy resin composition of the present invention, any ordinary epoxy resin having two or more epoxy groups in the molecule can be used. Examples include bisphenol A, bisphenol F, 3,3',5,5'-tetramethyl-4,4'-dihydroxydiphenylmethane, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxydiphenyl ketone, fluorene bisphenol, 4,4'-biphenol, 3,3',5,5'-tetramethyl-4,4'-dihydroxybiphenyl, 2,2'-biphenol, resorcinol, catechol, t-butyl catechol, etc. t-Butylhydroquinone, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,4-dihydroxynaphthalene, 2,5-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 2,8-dihydroxy Examples of the glycidyl ethers include divalent phenols such as naphthalene, allyl or polyallyl products of the above dihydroxynaphthalene, allyl bisphenol A, allyl bisphenol F, and allyl phenol novolac, and trivalent or higher phenols such as phenol novolac, bisphenol A novolac, o-cresol novolac, m-cresol novolac, p-cresol novolac, xylenol novolac, poly-p-hydroxystyrene, tris-(4-hydroxyphenyl)methane, 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, fluoroglycinol, pyrogallol, t-butylpyrogallol, allyl pyrogallol, polyallyl pyrogallol, 1,2,4-benzenetriol, 2,3,4-trihydroxybenzophenone, phenol aralkyl resins, naphthol aralkyl resins, and dicyclopentadiene-based resins, and glycidyl ethers derived from halogenated bisphenols such as tetrabromobisphenol A. These epoxy resins can be used alone or in combination of two or more.

[0028] In order to obtain a cured product with excellent thermal conductivity, a bifunctional epoxy resin with strong crystallinity is preferred. For example, glycidyl ethers derived from dihydric phenols such as 4,4'-biphenol, 2,2'-biphenol, hydroquinone, resorcin, and 4,4'-dihydroxyphenyl ether are preferred. In particular, those containing an epoxidized product of 4,4'-biphenol are preferred.

[0029] In the epoxy resin composition of the present invention, oligomers or polymeric compounds such as polyester, polyamide, polyimide, polyether, polyurethane, petroleum resin, indene resin, indene-coumarone resin, and phenoxy resin may be appropriately blended as other modifiers, etc. The amount of addition is usually within the range of 1 to 30 parts by weight per 100 parts by weight of the total of the resin components.

[0030] The epoxy resin composition of the present invention may further contain additives such as inorganic fillers, pigments, flame retardants, thixotropy-imparting agents, coupling agents, flowability improvers, etc. Examples of inorganic fillers include silica powders such as spherical or crushed fused silica and crystalline silica, alumina powders, glass powders, mica, talc, calcium carbonate, alumina, hydrated alumina, etc., and the preferred amount of the fillers used in semiconductor encapsulation is 70% by weight or more, and more preferably 80% by weight or more.

[0031] The pigments include organic or inorganic extender pigments, scaly pigments, etc. The thixotropy-imparting agents include silicone-based, castor oil-based, aliphatic amide wax, oxidized polyethylene wax, organic bentonite-based, etc.

[0032] Furthermore, in the epoxy resin composition of the present invention, a curing accelerator can be used as necessary. Examples include amines, imidazoles, organic phosphines, Lewis acids, etc., specifically, tertiary amines such as 1,8-diazabicyclo(5,4,0)undecene-7, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol, imidazoles such as 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, and 2-heptadecylimidazole, organic phosphines such as tributylphosphine, methyldiphenylphosphine, triphenylphosphine, diphenylphosphine, and phenylphosphine, tetra-substituted phosphonium and tetra-substituted borates such as tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate, and tetraphenylboron salts such as 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate. The amount added is usually within the range of 0.01 to 5 parts by weight per 100 parts by weight of the total resin components.

[0033] Furthermore, if necessary, the epoxy resin composition of the present invention may contain a release agent such as carnauba wax or OP wax, a coupling agent such as γ-glycidoxypropyltrimethoxysilane, a colorant such as carbon black, a flame retardant such as antimony trioxide, a stress reducing agent such as silicone oil, a lubricant such as calcium stearate, and the like.

[0034] The epoxy resin composition of the present invention can be made into a varnish state by dissolving an organic solvent therein, and then impregnating a fibrous material such as glass cloth, aramid nonwoven fabric, or polyester nonwoven fabric made of liquid crystal polymer or the like, followed by removing the solvent to form a prepreg. In some cases, the composition can be coated on a sheet-like material such as copper foil, stainless steel foil, polyimide film, or polyester film to form a laminate.

[0035] The epoxy resin composition of the present invention can be heat-cured to obtain the resin cured product of the present invention. The cured product can be obtained by molding the epoxy resin composition by a known method such as casting, compression molding, transfer molding, etc. The temperature at this time is usually in the range of 100 to 220°C. EXAMPLES

[0036] The present invention will be specifically described below with reference to synthesis examples, examples, and comparative examples. However, the present invention is not limited to these. Unless otherwise specified, "parts" refers to parts by weight, and "%" refers to % by weight. In addition, the following methods were used for the measurement.

[0037] 1) Measurement of OH equivalent Approximately 6 mg / eq of sample was weighed out into a 100 mL stoppered flask, 3 mL of a mixture of acetic anhydride and pyridine (volume ratio: 3:1) was added, a cooling tube was attached, the mixture was heated to reflux on a hot plate for 5 minutes, and after cooling for 5 minutes, 1 mL of water was added. The solution was titrated potentiometrically with a 0.5 mol / L KOH / MeOH solution to calculate the concentration.

[0038] 2) Measurement of epoxy equivalent A potentiometric titrator was used, and methyl ethyl ketone was used as the solvent. Tetraethylammonium bromide acetate solution was added, and the measurement was performed using a 0.1 mol / L perchloric acid-acetic acid solution in the potentiometric titrator.

[0039] 3) Melting point The DSC peak temperature was determined using a differential scanning calorimeter (EXSTAR6000 DSC / 6200 manufactured by SII NanoTechnology Inc.) at a temperature rise rate of 5°C / min. In other words, this DSC peak temperature was taken as the melting point of the resin.

[0040] 4) Melt Viscosity The viscosity was measured at 150° C. using a Brookfield CAP2000H rotational viscometer.

[0041] 5) Softening point Measured by the ring and ball method according to JIS-K-2207.

[0042] 6) GPC measurement The main body (HLC-8220GPC, Tosoh Corporation) was equipped with columns (TSKgelG4000HXL, TSKgelG3000HXL, TSKgelG2000HXL, Tosoh Corporation) in series, and the column temperature was set to 40°C. Tetrahydrofuran (THF) was used as the eluent, with a flow rate of 1 mL / min, and a differential refractive index detector was used as the detector. 0.1 g of sample was dissolved in 10 mL of THF and filtered through a microfilter, and 50 μL of the sample was used. Data processing was performed using GPC-8020 model II version 6.00, Tosoh Corporation. The number average molecular weight (Mn) was determined from a calibration curve using standard polystyrene.

[0043] 7) Glass transition temperature (Tg) The Tg was measured at a heating rate of 10°C / min using a thermomechanical measurement device (EXSTAR6000TMA / 6100 manufactured by SII NanoTechnology Inc.).

[0044] 8) 10% weight loss temperature (Td10), residual coal rate Using a thermogravimetric / differential thermal analyzer (SII NanoTechnology EXSTAR6000TG / DTA6200), the 10% weight loss temperature (Td10) was measured under a nitrogen atmosphere at a heating rate of 10°C / min. The weight loss at 700°C was also measured and calculated as the residual carbon ratio.

[0045] 9) Thermal conductivity The thermal conductivity was measured by the unsteady hot wire method using a NETZSCH LFA447 thermal conductivity meter.

[0046] 10) Infrared absorption (IR) measurement Using a Fourier transform infrared spectrophotometer (Perkinelmer Inc., Frontier Gold FT-IR Spectrometer), the total reflection method (ATR method) was used to measure the wavelengths of 400 to 4000 cm -1The absorbance was measured.

[0047] 11) Field desorption ionization mass spectrometry (FD-MS) The measurement was performed using a mass spectrometer JMS-T100GCV (manufactured by JEOL Ltd.) The sample was dissolved in acetone and subjected to the measurement.

[0048] Reference example 1 In a flask equipped with a Dean-Stark tube, 300.0 g of hydroquinone, 28.9 g of paraformaldehyde, and 263.1 g of diethylene glycol dimethyl ether were charged, and the mixture was heated to about 100°C while stirring under a nitrogen stream to dissolve. Next, 0.33 g of p-toluenesulfonic acid was added, and the mixture was heated to 160°C and reacted for 6 hours while dehydrating to produce a polyhydric hydroxy resin. Diethylene glycol dimethyl ether was distilled off, methyl isobutyl ketone was added, and the mixture was neutralized, washed with water, and filtered, and then methyl isobutyl ketone was distilled off under reduced pressure to obtain 295.1 g of polyhydric hydroxy resin a according to general formula (2). The OH equivalent of this polyhydric hydroxy resin a was 59 g / eq. The number average molecular weight was 430, and it was a mixture with n (number average) of 0 to 5.

[0049] Example 1 50.0 g (about 0.85 mol) of the polyhydric hydroxy resin a obtained in Reference Example 1, 58.5 g (about 0.42 mol) of p-hydroxybenzoic acid, 200.0 g of chlorobenzene, and 1.9 g of p-toluenesulfonic acid were charged, and the temperature was raised to 120° C. while stirring under a nitrogen stream, and the water in the system was refluxed and dehydrated for 5 hours. After cooling to room temperature, filtration, repeated washing with water, and drying under reduced pressure were performed to obtain 44.9 g of ester group-containing polyhydric hydroxy resin A in the form of a yellowish brown powder. The number average molecular weight was 484, and it was a mixture in which n (number average) was 0 to 5. The content (GPC area %) of n=0 was 11 area %. The GPC chart is shown in FIG. 1, the IR chart is shown in FIG. 2, and the FD-MS spectrum is shown in FIG. 3. The melting point by DSC was confirmed to have three peak temperatures of 177° C., 193° C., and 247° C. The OH equivalent was calculated from the feed ratio, GPC, and FD-MS analysis of each component, and was found to be 119 g / eq.

[0050] Example 2 The reaction was carried out in the same manner as in Example 1, except that 79.7 g (approximately 0.42 mol) of 6-hydroxy-2-naphthoic acid was used instead of p-hydroxybenzoic acid, to obtain 87.9 g of a brown powdery ester group-containing polyhydric hydroxy resin (polyhydric hydroxy resin B). The calculated OH equivalent of this resin was 156 g / eq.

[0051] Reference example 2 In a flask equipped with a Dean-Stark tube, 50.0g of hydroquinone, 39.9g of p-hydroxybenzoic acid, 0.75g of boric acid, 3.1g of sulfuric acid, and 400g of xylene were charged, and the mixture was heated to 130°C under stirring under a nitrogen stream, and reacted for 5 hours while refluxing to remove water in the system. After cooling to room temperature, the mixture was filtered and neutralized, and then repeatedly washed with water, and then washed with methanol. After drying under reduced pressure, 54.1g of white crystals were obtained. The calculated OH equivalent was 115g / eq., and the melting point by DSC was 240°C.

[0052] Reference example 3 50.0g of hydroquinone and 100.0g of 4,4'-dihydroxybiphenyl were dissolved in 1000g of epichlorohydrin and 150g of diethylene glycol dimethyl ether, and 16.5g of 48% sodium hydroxide was added at 60°C and stirred for 1 hour. Then, 148.8g of 48% aqueous sodium hydroxide solution was added dropwise over 3 hours under reduced pressure (about 130 Torr). During this time, the water generated was removed from the system by azeotropy with epichlorohydrin, and the distilled epichlorohydrin was returned to the system. After the dropwise addition was completed, the reaction was continued for another 1 hour to dehydrate, and then epichlorohydrin was distilled off, 600g of methyl isobutyl ketone was added, and the salt was removed by washing with water. Then, 13.5g of 48% sodium hydroxide was added at 85°C, stirred for 1 hour, and washed with 200mL of warm water. After that, water was removed by separation, and methyl isobutyl ketone was distilled off under reduced pressure to obtain 224 g of a white crystalline modified epoxy resin (epoxy resin A). The epoxy equivalent was 138, the hydrolyzable chlorine was 320 ppm, and the melting point by the capillary method was 10 The temperature ranged from 4°C to 141°C, and the viscosity at 150°C was 3.4 mPa·s.

[0053] Examples 3 to 7, Comparative Examples 1 to 5 As the epoxy resin component, the epoxy resin of Reference Example 3 (epoxy resin A), an epoxidized product of 4,4'-dihydroxydiphenyl ether (epoxy resin B: manufactured by Nippon Steel Chemical & Material Co., Ltd., YSLV-80DE 163 g / eq.), a biphenyl-based epoxy resin (epoxy resin C: manufactured by Japan Epoxy Resins, YX-4000H, epoxy equivalent 188 g / eq.), or a phenol novolac-type epoxy resin (epoxy resin D: manufactured by Nippon Steel Chemical & Material Co., Ltd. Terial Co., Ltd., YDPN-638, epoxy equivalent 177 g / eq.) was used, and as the curing agent, polyhydric hydroxy resin A (curing agent A) of Example 1, polyhydric hydroxy resin B (curing agent B) of Example 2, polyhydric hydroxy resin a (curing agent C) of Reference Example 1, hydroquinone (curing agent D), phenol novolac resin (curing agent E: hydroxyl equivalent 105, softening point 67°C), or the reaction product of hydroquinone and p-hydroxybenzoic acid (curing agent F) of Reference Example 2 was used. In addition, triphenylphosphine was used as a curing accelerator, and an epoxy resin composition was obtained with the formulation shown in Table 1. The numerical values ​​in the table indicate the parts by weight in the formulation. This epoxy resin composition was used to mold at 175°C, and post-cured at 175°C for 5 hours to obtain a cured product test piece, which was then subjected to various physical property measurements.

[0054] [Table 1]

[0055] As is clear from these results, the epoxy resin compositions obtained in the examples have excellent moldability, and the cured products thereof have good thermal conductivity, heat resistance and low thermal expansion, and are therefore suitable for use in power devices and automotive applications.

Claims

1. A polyhydric hydroxy resin represented by the following general formula (1), which contains at least one ester structure: 【Chemistry 1】 [wherein X represents an OH group or a monovalent substituent represented by formula (a), at least one of which is represented by formula (a); n represents the repeat number (number average) and indicates a mixture of components greater than 0 and not greater than 20; and the proportion of n=0 components in GPC measurement is 11 area % or less.] 【Chemistry 2】 (Here, Y represents an aromatic hydrocarbon group having 6 to 12 carbon atoms, R represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, and p represents a number from 1 to 3.)

2. 2. The polyhydric hydroxy resin according to claim 1, which has a number average molecular weight of 3,000 or less.

3. A method for producing the polyhydric hydroxy resin according to claim 1 or 2, comprising the steps of: A method for producing a polyhydric hydroxy resin, comprising reacting 0.1 to 0.7 moles of an OH-containing ester represented by general formula (3) with 1 mole of OH groups of a polyhydric hydroxy resin represented by general formula (2). 【Chemistry 3】 (Here, n is the repeat number (number average) and indicates a mixture of components greater than 0 and not greater than 20, and n=0 components account for 11 area % or less in GPC measurement.) 【Chemistry 4】 (wherein Y represents an aromatic hydrocarbon group having 6 to 12 carbon atoms, and R and R 1 each independently represents a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms, and p represents a number from 1 to 3.

4. 3. An epoxy resin composition comprising an epoxy resin and a curing agent, the epoxy resin composition comprising the polyhydric hydroxyl resin according to claim 1 or 2 as a part or the whole of the curing agent.

5. 5. The epoxy resin composition according to claim 4, wherein the epoxy resin is a difunctional crystalline epoxy resin.

6. 6. An epoxy resin cured product obtained by curing the epoxy resin composition according to claim 4 or 5.

Citation Information

Patent Citations

  • Novel curing agent for epoxy resin

    JP1988152616A

  • Epoxy resin composition

    JP1995090052A

  • Liquid crystal epoxy monomer and liquid crystal epoxy resin

    JP1997118673A

  • Insulation composition

    JP1999323162A

  • Epoxy resin composition

    JP2000264954A