Multi-layer foam particles
Multilayer foamed particles with a polypropylene resin core and polyolefin resin fusion layer address long cooling times by utilizing ethylene-propylene random copolymers with specific properties, enabling efficient molding with improved fusion and surface quality.
Patent Information
- Application Number
- JP2021072878
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-22
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-04-22
AI Technical Summary
Existing multilayer foamed particles require long water cooling times during in-mold molding, leading to reduced productivity and potential surface unevenness or deformation due to insufficient fusion and early mold release.
Multilayer foamed particles with a polypropylene resin foam core layer and a polyolefin resin fusion layer, where the ethylene-propylene random copolymer core has specific molecular weight and crystallization/melting point ratios, allowing for faster water cooling and improved fusion properties.
The solution enables molding at lower vapor pressures with reduced water cooling times, resulting in smoother surface finishes and reduced deformation, enhancing productivity and product quality.
Smart Images

Figure 0007553403000006 
Figure 0007553403000001 
Figure 0007553403000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a multi-layered expanded bead, and more particularly to a multi-layered expanded bead which can be molded in a mold. [Background technology]
[0002] Expanded bead moldings obtained by molding expanded polypropylene resin beads in a mold are excellent in terms of ease of shaping, light weight, heat insulation, rigidity, etc., and are therefore used in a variety of applications, including automotive interior components, core materials for automotive bumpers, heat insulation materials, cushioning packaging materials, and returnable boxes.
[0003] However, it is desirable that the in-mold molding of the expanded polypropylene resin beads can be performed at a low vapor pressure, and in order to make this possible, the technique described in Patent Document 1 has been proposed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-068016 A Summary of the Invention [Problem to be solved by the invention]
[0005] Patent Document 1 discloses expanded polypropylene resin beads having a multilayer structure consisting of a core layer formed of a polypropylene resin and an outer layer formed of a polypropylene resin, in which the melting point of the polypropylene resin constituting the outer layer is 1.5 to 30.0° C. lower than the melting point of the polypropylene resin constituting the core layer. By employing such a multilayer structure, the expanded beads described in Patent Document 1 can be molded in a mold at a low molding temperature.
[0006] On the other hand, even in the case of a multi-layered expanded bead as described in Patent Document 1, the time required for the water-cooling step for cooling during in-mold molding (hereinafter, sometimes referred to as the water-cooling time) may be long, and from the viewpoint of improving productivity, it is required to further shorten the molding time. However, there are the following problems in shortening the molding time. For example, it is possible to shorten the molding time by reducing the molding pressure and shortening the time required for water-cooling. However, when molding is performed at a low steam pressure, the fusion of the expanded bead molding may be insufficient. In addition, if the molded body in the mold is released before the water-cooling step is fully completed, the surface of the obtained expanded bead molding may become uneven, impairing the surface smoothness, or the molded body released from the mold may be deformed. As described above, it is not easy to obtain a good expanded bead molding by reducing the water-cooling time.
[0007] An object of the present invention is to obtain multi-layer expanded beads which can be molded in a mold at a lower vapor pressure than conventional multi-layer expanded beads and which can shorten the water cooling time during molding in a mold. [Means for solving the problem]
[0008] According to the present invention, there is provided the following multi-layer expanded beads. [1] A multi-layer foamed particle having a polypropylene-based resin foamed core layer and a polyolefin-based resin fusion layer covering the foamed core layer, the foamed core layer is formed from a polypropylene-based resin which is an ethylene-propylene random copolymer (A) having an ethylene content of 1.5% by mass or more and 3.5% by mass or less; The ethylene-propylene random copolymer (A) has a number average molecular weight (Mn) of 30,000 or more and 50,000 or less, and a weight average molecular weight (Mw) of 200,000 or more and 500,000 or less, and the ratio (Mw / Mn) of the weight average molecular weight Mw to the number average molecular weight (Mn) is 7 or more and 15 or less. [2] The crystallization temperature Tc of the ethylene-propylene random copolymer (A). A[℃] and the melting point Tm of the ethylene-propylene random copolymer (A). A 3. The multilayer expanded beads according to 1 or 2 above, wherein [°C] satisfies the following formula (1): 40≦Tm A -Tc A ≦50 (1) [3] The multilayer foamed beads according to 1 or 2, wherein the ratio (Mz / Mn) of the Z-average molecular weight (Mz) of the ethylene-propylene random copolymer (A) to the number-average molecular weight (Mn) of the ethylene-propylene random copolymer (A) is 30 or more and 60 or less. [4] The adhesive layer is formed from a polyolefin resin (II), and the melting point Tm II [°C] and the melting point Tm of the ethylene-propylene random copolymer (A). A 4. The multilayer expanded beads according to any one of 1 to 3 above, wherein [° C.] satisfies the following formula (4): 0 <Tm A -Tm II ≦20 (4) [5] The bulk density of the multilayer foamed particles is 10 kg / m 3 More than 300kg / m 3 5. The multilayer expanded particle according to any one of 1 to 4 above, which is: Effect of the Invention
[0009] According to the present invention, it is possible to obtain multi-layered expanded beads having a polypropylene-based resin foamed core layer and a polyolefin-based resin fusion layer, which can be molded in a mold at a low vapor pressure and further require a short water cooling time during molding in a mold. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a drawing showing an example of a DSC curve of the first heating by heat flux differential scanning calorimetry. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The multi-layer expanded beads of the present invention will be described in detail below. The multilayer expanded beads of the present invention (hereinafter, simply referred to as multilayer expanded beads or expanded beads) have an expanded core layer and a fusion layer covering the expanded core layer. Furthermore, the expanded core layer is formed from a polypropylene-based resin, and the fusion layer is formed from a polyolefin-based resin (hereinafter, the polypropylene-based resin forming the expanded core layer is also referred to as polypropylene-based resin (I) and the polyolefin-based resin forming the fusion layer is also referred to as polyolefin-based resin (II)).
[0012] The foamed core layer is in a foamed state, which means that the polypropylene resin (I) forms a bubble film and bubbles are formed by the bubble film. Furthermore, the foamed core layer is covered with a fusion layer, which is formed of the polyolefin resin (II). The fusion layer is a layer that contributes to improving the fusion property of the foamed beads, and may be in a foamed state or a non-foamed state, but is preferably in a non-foamed state. The non-foamed state includes not only a state in which no bubbles are present (as will be described later, a state in which bubbles once formed during foaming of the resin particles are melted and destroyed, and the bubbles disappear), but also a state in which a small number of very small bubbles are present within a range that does not affect the mechanical strength of the obtained molded body.
[0013] The foamed core layer may be covered completely with the fusion layer or may be partially exposed. An example of a structure in which the foamed core layer is exposed is a structure in which only the peripheral surface of a cylindrical foamed core layer is covered with the fusion layer and the foamed core layer is exposed on the top and bottom surfaces of the cylinder.
[0014] The multi-layered expanded beads of the present invention have improved fusion properties of the expanded beads due to the fusion layer, and are preferably moldable in a mold at a molding temperature lower than that of the single-layered expanded beads consisting of only the expanded core layer. In order to enable such in-mold molding, for example, the polyolefin resin (II) constituting the fusion layer may be selected to have a melting point lower than that of the polypropylene resin (I) constituting the expanded core layer. When the multi-layered expanded beads thus configured are molded in a mold at a temperature range in which the expanded core layer can be secondary expanded, the fusion layer softens faster than the expanded core layer, so that a molded product having excellent heat fusion properties between the multi-layered expanded beads can be obtained. In addition, the cell structure of the expanded core layer is less likely to be damaged by heating during in-mold molding, so that a molded product of expanded beads with small shrinkage after molding can be obtained.
[0015] The phrase "moldable at a low molding temperature" means that, based on the in-mold molding temperature of expanded beads having a single-layer structure made of polypropylene-based resin (I), a molded article having similar properties (e.g., surface appearance, fusion property, recovery property) to a molded article formed from the expanded beads having a single-layer structure can be molded at a molding temperature lower than the reference in-mold molding temperature.
[0016] Next, the polypropylene resin (I) constituting the foamed core layer will be described. The polypropylene-based resin (I) constituting the foamed core layer is an ethylene-propylene random copolymer (A) having an ethylene content of 1.5% by mass or more and 3.5% by mass or less. By forming the foamed core layer using the ethylene-propylene random copolymer (A), it is possible to obtain foamed beads having excellent secondary foaming properties and excellent moldability in a mold.
[0017] The ethylene content of the ethylene-propylene random copolymer (A) forming the foamed core layer is 1.5% by mass or more and 3.5% by mass or less. By forming the foamed core layer using an ethylene-propylene random copolymer having an ethylene content within this range, the time required for the water cooling step in the in-mold molding can be shortened, thereby shortening the molding cycle. For this reason, the ethylene content is preferably 1.8% by mass or more and 3% by mass or less, more preferably 2% by mass or more and 2.5% by mass or less.
[0018] In this specification, the ethylene content of the ethylene-propylene random copolymer can be measured as follows. An ethylene-propylene copolymer with a known copolymer composition is hot pressed in a 180°C environment to produce a film with a thickness of about 100 μm. The IR spectrum of the produced film is measured to detect the 810 cm -1 absorbance at 733cm from ethylene (I810) -1 The absorbance (I733) at 1000 nm is read. Then, a calibration curve for the ethylene component content is created by plotting the absorbance ratio (I733 / I810) on the horizontal axis and the ethylene component content on the vertical axis. Next, in the same manner as in the sample preparation method used to create the calibration curve, the ethylene-propylene random copolymer resin to be measured is hot pressed to create a film with a thickness of about 100 μm, and I810 and I733 are read by IR spectrum measurement, and the ethylene component content is calculated according to the calibration curve created earlier.
[0019] The ethylene-propylene random copolymer (A) has a number average molecular weight (Mn) and a ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) within a specific range. In the ethylene-propylene random copolymer (A), the number average molecular weight (Mn) is 30,000 or more and 50,000 or less, the weight average molecular weight (Mw) is 200,000 or more and 500,000 or less, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 7 or more and 15 or less. If the ratio (Mw / Mn) is too small, deformation may not be prevented when the water cooling time is shortened. On the other hand, if the ratio (Mw / Mn) is too large, the low pressure moldability decreases, so that the water cooling time may not be shortened. From this viewpoint, the ratio (Mw / Mn) is preferably 7.5 to 13, more preferably 8 to 10, and even more preferably 8.5 to 9.5.
[0020] Regarding the factor that relates the molecular weight distribution of the ethylene-propylene random copolymer (A) constituting the foamed core layer to the water cooling time during molding, when the amounts of low molecular weight components and high molecular weight components constituting the ethylene-propylene random copolymer (A) are each within a specific range, the crystallization behavior of the ethylene-propylene random copolymer (A) changes, and the thermal conductivity and rigidity of the ethylene-propylene random copolymer (A) are improved by the crystalline portion, which is related to the cooling efficiency of the resin in the cooling process during molding and the ease of shrinkage of the molded body after demolding, and is therefore thought to contribute to shortening the cooling time. From the above viewpoints, the number average molecular weight (Mn) of the ethylene-propylene random copolymer (A) is preferably 32,000 or more and 43,000 or less, and more preferably 34,000 or more and 42,000 or less. The weight average molecular weight (Mw) of the ethylene-propylene random copolymer (A) is preferably 320,000 or more and 450,000 or less, and more preferably 330,000 or more and 430,000 or less.
[0021] The ethylene-propylene random copolymer (A) preferably has a ratio (Mz / Mn) of the Z-average molecular weight (Mz) to the number-average molecular weight (Mn) of 30 or more and 60 or less. If the ratio (Mz / Mn) is within the above range, deformation is prevented when the water cooling time is shortened, and the cooling time can be shortened without deteriorating the low pressure formability. From this viewpoint, the ratio (Mz / Mn) is preferably 35 or more and 57 or less, and more preferably 40 or more and 55 or less.
[0022] In this specification, the number average molecular weight (Mn), weight average molecular weight (Mw), and Z average molecular weight (Mz) are measured as follows. (Measurement method and conditions) Sample pretreatment: 30 mg of sample is dissolved in 20 mL of o-dichlorobenzene by shaking at 145°C, and the solution is then hot-filtered through a sintered filter with a pore size of 1.0 μm to obtain an analytical sample, which can then be measured by gel permeation chromatography.
[0023] In the ethylene-propylene random copolymer (A) used in the present invention, the crystallization temperature (Tc A ) and melting point (Tm A ) preferably satisfy the following formula (1). 40≦Tm A -Tc A ≦50 (1)
[0024] The crystallization temperature (Tc A ) and the melting point (Tm A When the foamed core layer is formed using an ethylene-propylene random copolymer (A) that satisfies the above formula (1), a good foamed bead molding can be obtained even when molding is performed using low-pressure steam. This is thought to be because the ethylene-propylene random copolymer (A) that satisfies the formula (1) tends to crystallize early in the cooling step during molding, making it possible to shorten the water cooling time during molding.
[0025] For the above reasons, the crystallization temperature (Tc A ) and melting point (Tm A ) preferably satisfies the following formula (2), and more preferably satisfies the following formula (3): 41≦Tm A -Tc A ≦48 (2) 42≦Tm A -Tc A ≦45 (3)
[0026] In this specification, the melting point means a melting peak temperature determined by heat flux differential scanning calorimetry based on JIS K7121-1987. As the condition adjustment of the test piece, "(2) A case where the melting temperature is measured after a certain heat treatment" is adopted, and a cooling rate of 10°C per minute is adopted. As the heating rate when measuring the melting temperature, a heating rate of 10°C per minute is adopted. When two or more melting peaks appear, the temperature at the apex of the melting peak with the largest area is taken as the melting point. The melting point (Tmf) of the expanded beads and multi-layer expanded beads can also be measured by the same method as above.
[0027] In this specification, the crystallization temperature means the crystallization peak temperature determined by heat flux differential scanning calorimetry based on JIS K7121-1987. As the condition adjustment of the test piece, "(2) A case where the melting temperature is measured after a certain heat treatment" is adopted, and a cooling rate of 10°C per minute is adopted. When two or more crystallization exothermic peaks appear, the temperature at the apex of the crystallization peak with the largest area is taken as the crystallization temperature. The crystallization temperature (Tcf) of the expanded beads and multi-layer expanded beads can also be measured by the same method as above.
[0028] In the heat flux differential scanning calorimetry, the heat of fusion (ΔHr) of the melting peak of the ethylene-propylene random copolymer (A) is preferably 50 J / g or more and 100 J / g or less, more preferably 60 J / g or more and 90 J / g or less. In this specification, the heat of fusion means the heat of fusion determined by heat flux differential scanning calorimetry based on JIS K7122-1987. Specifically, as the condition adjustment of the test piece, "(2) A case where the heat of fusion is measured after a certain heat treatment" is adopted, and the cooling rate at this time is 10°C per minute. The heating rate at the time of measuring the heat of fusion is 10°C per minute. In addition, when two or more melting peaks appear, the value of the heat of fusion with the largest area is adopted.
[0029] The resin constituting the foamed core layer may contain thermoplastic resins and thermoplastic elastomers other than the ethylene-propylene random copolymer (A) within the limits not impeding the intended purpose.
[0030] The polypropylene-based resin constituting the foamed core layer may contain additives such as colorants such as carbon black, lubricants, catalyst neutralizers, antioxidants, etc., as necessary, within the range that does not impair the object of the present invention. The amount of the additives added varies depending on the type, but is preferably 15 parts by weight or less, more preferably 10 parts by weight or less, even more preferably 5 parts by weight or less, and particularly preferably 1 part by weight or less, relative to 100 parts by weight of the propylene-based resin constituting the foamed core layer.
[0031] The flexural modulus of the ethylene-propylene random copolymer (A) is preferably 800 MPa or more and 1100 MPa or less, more preferably 850 MPa or more and 1000 MPa or less. If the flexural modulus is within the above range, deformation during molding in a mold is suppressed, and an expanded bead molding having good physical properties can be obtained.
[0032] In this specification, the flexural modulus is determined in accordance with JIS K7171:2008. The test piece is prepared by heat pressing a sample at 230°C to prepare a 4 mm sheet, and cutting the sheet into a length of 80 mm x width of 10 mm x thickness of 4 mm (standard test piece). The radius R1 of the indenter and the radius R2 of the support table are both 5 mm, the distance between the supports is 64 mm, and the test speed is 2 mm / min.
[0033] The melt flow rate (MFR) of the ethylene-propylene random copolymer (A) is preferably 1 g / 10 min to 20 g / 10 min, more preferably 2 g / 10 min to 15 g / 10 min, and even more preferably 3 g / 10 min to 10 g / 10 min. If the MFR is within the above range, it is easy to form expanded beads having a multilayer structure. The MFR of the ethylene-propylene random copolymer (A) is a value measured under test condition M (230° C. / 2.16 kg load) of JIS K7210:1999.
[0034] Next, the polyolefin resin (II) constituting the adhesive layer will be described. The polyolefin resin (II) is not particularly limited in composition or synthesis method as long as it is mainly composed of an olefin component, but preferably contains 50% by mass or more of an olefin component, more preferably 70% by mass or more, and even more preferably 90% by mass or more. Examples of the polyolefin resin include polypropylene resin, polyethylene resin, and the like, and further include mixtures thereof.
[0035] The polypropylene-based resin may be a propylene homopolymer or a copolymer of propylene with other olefins copolymerizable with propylene. Examples of other olefins copolymerizable with propylene include α-olefins having 4 or more carbon atoms, such as ethylene and 1-butene. Examples of the copolymer include propylene-ethylene random copolymers, propylene-ethylene block copolymers, and propylene-ethylene-butene random copolymers, and further examples include mixed resins of two or more of these.
[0036] Examples of the polyethylene resin include high density polyethylene, medium density polyethylene, low density polyethylene, linear low density polyethylene, very low density polyethylene, and ethylene-vinyl acetate copolymer, and further examples include mixed resins of two or more of these.
[0037] Among these polyolefin resins (II), from the viewpoint of excellent compatibility with the foamed core layer and improved adhesion between the foamed core layer and the adhesive layer, ethylene-propylene random copolymers or propylene-ethylene-butene random copolymers are preferred. Among the above, ethylene-propylene random copolymers are more preferred. (Hereinafter, the ethylene-propylene random copolymer used as the polyolefin resin (II) of the adhesive layer may be referred to as random copolymer (B).)
[0038] Furthermore, the ratio (EtB / EtA) of the ethylene content (EtA) of the ethylene-propylene random copolymer (A) to the ethylene content (EtB) of the random copolymer (B) is preferably greater than 1. If the ratio is within the above range, the fusion layer is less likely to peel off from the foamed core layer during molding in the mold, and an expanded bead molding having better surface smoothness is obtained. For this reason, the ratio (EtB / EtA) is more preferably 1.2 or more, and even more preferably 1.4 or more. The upper limit is approximately 3, preferably 2.5, and even more preferably 2.
[0039] The adhesive layer in the present invention may contain a thermoplastic resin or a thermoplastic elastomer other than the polyolefin resin (II) as long as the intended purpose is not impaired.
[0040] Furthermore, additives such as antistatic agents, catalyst neutralizers, lubricants, colorants such as carbon black, etc. may be added to the adhesion layer. The amount of the additives to be added varies depending on the type of additive and the purpose of use, but is preferably 15 parts by weight or less, more preferably 10 parts by weight or less, further preferably 5 parts by weight or less, and particularly preferably 3 parts by weight or less, based on 100 parts by weight of the polyolefin resin (II) forming the adhesion layer.
[0041] As described above, in the multi-layer expanded beads of the present invention, the fusion layer is formed from the polyolefin resin (II). B[°C] and the melting point Tm of the ethylene-propylene random copolymer (A). A It is preferable that the temperature [° C.] satisfies the following formula (4). 0 <Tm A -Tm II ≦20 (4) When the above range is satisfied, the adhesion layer forming the multi-layered expanded beads can function as an adhesion improving layer.
[0042] From this viewpoint, the melting point Tm of the ethylene-propylene random copolymer (A) A [° C.] preferably satisfies the following formula (5), and more preferably satisfies the following formula (6). 5 <Tm A -Tm II ≦18 (5) 8 <Tm A -Tm II ≦15 (6)
[0043] In the polyolefin resin (II), the heat of fusion (ΔHr) of the fusion peak is preferably 50 J / g or more and 90 J / g or less, more preferably 55 J / g or more and 80 J / g or less. The heat of fusion (ΔHr) of the polyolefin resin (II) is measured in the same manner as in the above-mentioned method for measuring the heat of fusion of the resin forming the foamed core layer.
[0044] The flexural modulus of the polyolefin resin (II) is preferably 500 MPa or more and 100 MPa or less, and more preferably 550 MPa or more and 800 MPa or less.
[0045] The polyolefin resin (II) preferably has a melt flow rate (MFR) of 1 g / 10 min to 20 g / 10 min, more preferably 2 g / 10 min to 15 g / 10 min, and even more preferably 3 g / 10 min to 10 g / 10 min. If the MFR is within the above range, the expanded beads have a multilayer structure and are particularly excellent in adhesiveness.
[0046] The melt flow rate (MFR) of the polyolefin resin (II) is preferably smaller than the melt flow rate of the ethylene-propylene random copolymer (A), thereby forming expanded beads having a multi-layer structure with excellent adhesiveness.
[0047] In this specification, the melt flow rate (MFR) of a polypropylene resin is measured based on JIS K7210-1:2014 (temperature: 230° C., load: 2.16 kg). For polyethylene resins, the measurements are performed at a temperature of 190°C and a load of 2.16 kgf.
[0048] The weight ratio of the foamed core layer to the adhesive layer is preferably from 99.5:0.5 to 65:35, more preferably from 99:1 to 80:20, further preferably from 97:3 to 805:20, and particularly preferably from 97:3 to 85:15. When the weight ratio is within the above range, expanded beads having good moldability can be obtained. The weight ratio of the foamed core layer to the fusion layer can be adjusted, for example, by adjusting the ratio of the extrusion rate of the raw material for forming the resin particle core layer to the raw material for forming the resin particle fusion layer in the production of the multilayer resin particles described below.
[0049] Next, the physical properties of the multi-layer expanded beads of the present invention will be described. The bulk density of the multi-layer foamed particles is 10 kg / m 3 More than 300kg / m 3 It is preferable that: When the bulk density is within the above range, the dimensional change after molding tends to be large, so that the water cooling time tends to be long, and therefore the effect of shortening the water cooling time specified by the present invention becomes more remarkable. In addition, it is possible to obtain an expanded bead molding that can be used for various applications such as automobile interior parts, core materials for automobile bumpers, heat insulation materials, cushioning packaging materials, and returnable boxes. From this viewpoint, the bulk density of the expanded beads is 20 kg / m or less. 3 More than 250kg / m 3 More preferably, it is equal to or less than 25 kg / m 3 More than 200kg / m3 The following is the result.
[0050] The method for measuring the bulk density of expanded beads is as follows. First, a measuring cylinder with a volume of 1 L is prepared. While removing static electricity from the expanded beads, the expanded beads are filled into the measuring cylinder up to the 1 L mark so that they naturally pile up. The mass of the expanded beads in this measuring cylinder, i.e., the mass of the expanded beads per 1 L of volume, is calculated as the mass per m of volume. 3 Mass per unit (kg / m 3 ) to obtain the bulk density (kg / m 3 ) can be calculated.
[0051] The average cell diameter of the foamed core layer is preferably 20 to 400 μm, more preferably 40 to 250 μm, further preferably 100 to 230 μm, and particularly preferably 150 to 200 μm. When the average cell diameter is within the above range, the foamed core layer has excellent moldability in a mold and the foamed bead molding has excellent dimensional recovery after molding.
[0052] The average cell diameter of the foamed core layer is measured as follows. Based on an enlarged photograph of a cut surface of the foamed core layer approximately in half taken with a microscope, the average bubble diameter can be determined as follows. First, in the enlarged photograph of the cut surface of the foamed core layer, four line segments are drawn from one surface of the foamed core layer to the other surface, passing through the approximate center of the bubble cut surface. However, the line segments are drawn so as to form radial straight lines extending in eight directions at equal intervals from the approximate center of the bubble cut surface to the cut particle surface. Next, the total number N (pieces) of bubbles intersecting with the four line segments is determined. The sum L (μm) of the lengths of the four line segments is determined, and the value (L / N) obtained by dividing the sum L by the sum N is regarded as the average bubble diameter of one foamed core layer. This operation is performed for 10 foamed core layers, and the arithmetic mean of the average bubble diameters of each foamed core layer is regarded as the average bubble diameter of the foamed core layer.
[0053] In the multi-layer foamed beads of the present invention, the closed cell ratio is preferably 75% or more, more preferably 80% or more, further preferably 82% or more, and particularly preferably 85% or more. If the closed cell ratio is within the above range, the multi-layer foamed beads have excellent secondary expandability, and the mechanical properties of the resulting foamed core layer molded article are good.
[0054] The closed cell ratio of the multi-layer expanded beads is measured as follows. The multi-layer foamed particles are left to stand for 10 days in a temperature-controlled room under atmospheric pressure, relative humidity of 50%, and 23°C conditions to cure. Next, in the same temperature-controlled room, the particles are cooled to a volume of about 20 cm3. 3 The multilayer foamed particles after curing are used as a measurement sample, and the apparent volume Va is accurately measured by the submersion method as described below. After the measurement sample whose apparent volume Va has been measured is thoroughly dried, the true volume Vx of the measurement sample is measured using an air comparison specific gravity meter 930 manufactured by Toshiba Beckman Co., Ltd. in accordance with procedure C described in ASTM-D2856-70. Based on these volumes Va and Vx, the closed cell ratio is calculated using the following formula (7), and the average value of N=5 is taken as the closed cell ratio of the multilayer foamed particles.
[0055] Closed cell ratio (%)=(Vx-W / ρ)×100 / (Va-W / ρ) (7) however, Vx: The true volume of the multi-layer foamed beads measured by the above method, i.e., the sum of the volume of the resin constituting the multi-layer foamed beads and the total volume of the air bubbles in the closed cell part in the multi-layer foamed beads (cm 3 ) Va: The apparent volume (cm) of the multi-layer foamed particles measured by submerging the multi-layer foamed particles in a measuring cylinder containing water and measuring the rise in the water level. 3 ) W: Weight of sample for measuring multilayer foam particles (g) ρ: Density of the resin that composes the multi-layer foamed particles (g / cm 3 )
[0056] In the present invention, it is preferred that the multi-layer expanded beads have a crystalline structure as measured by a DSC curve described below. That is, it is preferable that the DSC curve of the first heating obtained by temperature rise measurement by heat flux differential scanning calorimetry shows an endothermic peak inherent to the polypropylene-based resin (hereinafter also simply referred to as the "intrinsic peak") and a high-temperature peak resulting from secondary crystals formed by temperature treatment during foaming.
[0057] Specifically, it is preferable that a DSC curve (DSC curve of the first heating) obtained by heating 2 to 10 mg of the multilayer foamed particles from 23°C to 220°C at a heating rate of 10°C / min by heat flux differential scanning calorimetry has an endothermic peak a (hereinafter also simply referred to as the "intrinsic peak") inherent to the polypropylene-based resin and one or more endothermic peaks b (hereinafter also simply referred to as the "high-temperature peaks") originating from secondary crystals formed by temperature treatment during foaming on the high-temperature side of the inherent peak, as shown in FIG. 1.
[0058] Figure 1 shows an example of the DSC curve for the first heating. In Figure 1, a indicates the characteristic peak, b indicates the high-temperature peak, α indicates the point on the DSC curve that corresponds to 80°C, and T E is the end temperature of melting, which is the temperature when the high temperature side of endothermic peak b returns to the baseline position, β is the point on the DSC curve corresponding to the end temperature of melting TE of the high temperature peak, γ is the bottom point of the valley between intrinsic peak a and high temperature peak b, and δ is the point where a straight line parallel to the vertical axis of the graph drawn from point γ intersects with the straight line (α-β).
[0059] The apex temperature of the intrinsic peak (intrinsic peak temperature) is preferably from 135° C. to 145° C., more preferably from 138° C. to 142° C. If the intrinsic peak temperature is within the above range, highly crystalline crystals that contribute to improving rigidity are easily formed by cooling after molding. The melting end temperature (γ) of the intrinsic peak is the temperature corresponding to the bottom of the valley between the intrinsic peak a and the high-temperature peak b, and is preferably 150°C or higher and 160°C or lower, more preferably 152°C or higher and 155°C or lower.
[0060] The heat of fusion of the intrinsic peak is preferably 50 J / g or more and 70 J / g or less, more preferably 55 J / g or more and 65° C. J / g or less. When the heat of fusion of the intrinsic peak is within the above range, the dimensional stability after molding is improved.
[0061] The heat of fusion of the intrinsic peak is determined as the area surrounded by the straight line (δ-γ) connecting points δ and γ, the straight line (α-β), and the curve of the high-temperature peak a in FIG.
[0062] The apex temperature of the high-temperature peak is preferably 155°C or higher and 165°C or lower, and more preferably 157°C or higher and 162°C or lower. The high-temperature peak apex temperature and the melting end temperature (T E ) is preferably 5°C or more and 10°C or less. The melting end temperature (T E ) is preferably 165°C or higher and 170°C or lower, more preferably 166°C or higher and 169°C or lower. The melting end temperature (T E ) within the above range, the resulting expanded bead molding will have excellent mechanical strength.
[0063] The heat of fusion ΔH2 of the high-temperature peak (hereinafter also simply referred to as the high-temperature peak heat) is preferably 10 J / g or more and 15 J / g or less. When the high-temperature peak calorific value is within the above range, dimensional changes after molding are unlikely to occur, and it is possible to obtain an expanded bead molding having excellent mechanical strength. The high temperature peak of the foamed core layer can be adjusted by a known method, and a specific method for adjusting the temperature is disclosed in, for example, JP-A-2001-151928.
[0064] The high-temperature peak b is observed in the DSC curve obtained by the first heating as described above, but not in the DSC curve obtained by the second heating. In the DSC curve obtained by the second heating, only the endothermic peak specific to the propylene-based resin constituting the foamed core layer is observed.
[0065] The heat of fusion ΔH2 of the high-temperature peak is calculated as the area surrounded by the straight line (δ-γ), the straight line (α-β), and the curve of the high-temperature peak b in FIG.
[0066] Next, a multi-layer foamed bead molding (hereinafter, simply referred to as a foamed bead molding or a molding) obtained by molding the multi-layer foamed beads in a mold will be described. The density of the foamed bead molding is 10 kg / m 3 More than 300kg / m 3 It is preferably equal to or less than 20 kg / m 3 More than 200kg / m 3 More preferably, 30 kg / m or less 3 More than 100kg / m 3 In particular, when the molding density of the expanded bead molding is low, the molding time tends to be long, so that it is useful to use the expanded beads of the present invention.
[0067] The compressive stress at 50% strain of the expanded bead molding is preferably 200 kPa or more and 700 kPa or less, more preferably 250 kPa or more and 600 kPa or less, and further preferably 300 kPa or more and 500 kPa or less.
[0068] Next, the method for producing the multi-layer expanded beads of the present invention will be described. The multi-layered expanded particles can be obtained by expanding multi-layered resin particles having a resin particle core layer made of the ethylene-propylene random copolymer (A) and a resin particle fusion layer made of the polyolefin resin (II) coated thereon.
[0069] The multi-layered resin particles can be produced, for example, as follows. An apparatus in which two extruders, an extruder for a resin particle core layer and an extruder for a resin particle fusion layer, are connected to a co-extrusion die is used, and the required ethylene-propylene random copolymer (A) and additives such as a bubble regulator as required are supplied to the extruder for the resin particle core layer and melt-kneaded to form a resin melt for forming the resin particle core layer. Meanwhile, the required polyolefin resin (II) and additives as required are supplied to the extruder for the resin particle fusion layer and melt-kneaded to form a resin melt for forming the resin particle fusion layer. Next, the resin melt for forming the resin particle core layer is introduced into the co-extrusion die to form a linear flow, and at the same time, the resin melt for forming the resin particle fusion layer is introduced into the co-extrusion die, and the resin melt for forming the resin particle fusion layer is laminated so that the resin melt for forming the resin particle fusion layer surrounds the linear flow of the resin melt for forming the resin particle core layer to form a multilayered resin melt. The multilayered resin particles can be produced by extruding the resin melt having this multilayered structure from small holes in a die attached to the outlet of the extruder in the form of one or more strands, cooling the strands by passing them through water and then cutting them to an appropriate length, or by cutting and cooling them while extruding them from the die into water, etc. In this specification, the multilayered structure formed in this manner is sometimes referred to as a "sheath-core" structure.
[0070] The method for producing multilayer resin particles using the coextrusion die is described in detail in, for example, JP-B-41-16125, JP-B-43-23858, JP-B-44-29522, and JP-A-60-185816.
[0071] In order to adjust the bubble diameter of the foamed core layer, it is preferable to add a bubble regulator to the resin particle core layer. Examples of the bubble regulator include inorganic substances such as talc, calcium carbonate, borax, zinc borate, aluminum hydroxide, and alum. The amount of the bubble regulator added is preferably 0.001 to 10 parts by weight, more preferably 0.01 to 5 parts by weight, per 100 parts by weight of the resin (I) forming the resin particle core layer. When a cell regulator is added to the resin (I), the cell regulator can be blended as it is, but it is usually preferable to add it as a master batch of the cell regulator, taking into consideration dispersibility and the like.
[0072] The weight of the multilayer resin particles in the present invention is preferably from 0.02 to 20 mg, more preferably from 0.1 to 6 mg, in order to ensure uniform filling of the expanded particles in the mold.
[0073] The multi-layered expanded particles of the present invention can be produced by using the multi-layered resin particles, for example, by the so-called dispersion medium release foaming method. In the dispersion medium release foaming method, the multilayer resin particles are dispersed in a dispersion medium such as water in a sealed container such as an autoclave together with a physical foaming agent, the dispersion medium is heated to a temperature equal to or higher than the softening temperature of the resin particles to impregnate the resin particles with the foaming agent, and then, while maintaining the pressure in the sealed container at a pressure equal to or higher than the vapor pressure of the foaming agent, one end of the sealed container below the water surface is opened, and the expandable multilayer resin particles containing the foaming agent are released from the sealed container together with the dispersion medium such as water under an atmosphere of a lower pressure than the pressure in the sealed container, usually atmospheric pressure, to be foamed, thereby obtaining multilayer expanded particles. Alternatively, the expandable multilayer resin particles containing a physical foaming agent may be taken out of the sealed container and heated with a heating medium such as steam to be foamed. Furthermore, when producing multilayer resin particles using the extrusion device, a foaming agent is injected into the extruder for the resin particle core layer to form a foamable molten resin composition, and the foamable molten resin composition is laminated with the molten resin for forming the resin particle fusion layer to form a molten resin composition having a sheath-core structure, and the molten resin composition having the sheath-core structure is extruded through a die to foam, and then cut into particles, whereby expanded particles can also be obtained.
[0074] In the dispersion medium releasing and foaming method, the pressure difference between the high pressure and the low pressure when releasing from the high pressure where foaming does not occur to the low pressure where foaming occurs is preferably 400 kPa or more, more preferably 500 to 15,000 kPa.
[0075] The blowing agent used in the dispersion medium release foaming method usually includes organic physical blowing agents such as propane, isobutane, normal butane, isopentane, normal pentane, cyclopentane, normal hexane, cyclobutane, cyclohexane, chlorofluoromethane, trifluoromethane, 1,1,1,2-tetrafluoroethane, 1-chloro-1,1-difluoroethane, 1,1-difluoroethane, 1-chloro-1,2,2,2-tetrafluoroethane, and hydrofluoroolefin, and inorganic physical blowing agents such as nitrogen, carbon dioxide, argon, and air. Among these, inorganic physical blowing agents that do not destroy the ozone layer and are inexpensive are preferred, and nitrogen, air, and carbon dioxide are particularly preferred. In addition, two or more of these blowing agents can be used in combination.
[0076] The amount of the blowing agent used is appropriately selected depending on the relationship between the bulk density of the multi-layer expanded beads to be obtained and the expansion temperature. Specifically, in the case of the above blowing agents other than nitrogen and air, the amount of the blowing agent used is usually 2 to 50 parts by weight per 100 parts by weight of resin particles. In the case of nitrogen and air, the amount used is such that the pressure in the closed container is within the pressure range of 1 to 5 MPa (G).
[0077] In a sealed container, the dispersion medium for dispersing the resin particles is preferably water, but any dispersion medium that does not dissolve the resin particles can be used. Examples of such dispersion medium include ethylene glycol, glycerin, methanol, ethanol, etc.
[0078] The average cell diameter is adjusted by the type and amount of foaming agent, the foaming temperature, and the amount of foam regulator added. The bulk density (expansion ratio) is adjusted by the amount of foaming agent added, the foaming temperature, and the differential pressure during foaming. Within the appropriate range, the larger the amount of foaming agent added, the higher the foaming temperature, and the larger the differential pressure, the smaller the bulk density of the resulting expanded beads.
[0079] When the base resin particles are dispersed in a dispersion medium and heated to a foaming temperature in a closed container, a fusion inhibitor can be used to prevent the multilayer resin particles from fusing together. As the fusion inhibitor, any fusion inhibitor can be used, whether inorganic or organic, as long as it is insoluble in water or the like and does not melt when heated, but inorganic ones are generally preferred.
[0080] As inorganic anti-fusing agents, powders such as kaolin, talc, mica, aluminum oxide, titanium oxide, and aluminum hydroxide are suitable. As the anti-fusing agent, those having an average particle size of 0.001 to 100 μm, particularly 0.001 to 30 μm are preferred. The amount of anti-fusing agent added is usually preferably 0.01 to 10 parts by weight per 100 parts by weight of resin particles.
[0081] In addition, anionic surfactants such as sodium dodecylbenzenesulfonate and sodium oleate, and aluminum sulfate are preferably used as dispersion aids. The dispersion aid is preferably added in an amount of 0.001 to 5 parts by weight per 100 parts by weight of resin particles.
[0082] In the case of producing multi-layered expanded particles having a low bulk density, it is preferable to produce multi-layered expanded particles by the dispersion medium release foaming method or the like, and then further expand the obtained multi-layered expanded particles, that is, to perform so-called two-stage expansion. In the two-stage expansion, the multi-layered expanded particles are filled in a pressurizable sealed container, and pressurized with a gas such as air to increase the internal pressure of the multi-layered expanded particles to 0.01 to 0.6 MPa (G), and then the multi-layered expanded particles are taken out of the container and heated with a heating medium such as steam, whereby multi-layered expanded particles having a low bulk density can be easily obtained.
[0083] The expanded bead molding can be obtained by filling the multi-layered expanded beads into a mold and heat-molding the multi-layered expanded beads using a heating medium such as steam, according to a conventional method. Specifically, after filling the multi-layered expanded beads into a mold, steam is introduced into the mold to heat and expand the multi-layered expanded beads, which are then fused together to obtain a molding having the shape of the molding space. In addition, as a method for obtaining an expanded bead molding having a low molding density, there is a method in which, if necessary, a pressure treatment operation is carried out to increase the pressure inside the multi-layer expanded beads in the same manner as in the above-mentioned two-stage expansion, so that the internal pressure inside the multi-layer expanded beads is adjusted to 0.01 to 0.2 MPa (G), and then the multi-layer expanded beads are molded in a mold.
[0084] When the multilayer foamed beads of the present invention are used for in-mold molding, the molding steam pressure is preferably 0.05 to 0.46 MPa (G), more preferably 0.07 to 0.30 MPa (G), and further preferably 0.09 to 0.28 MPa (G).
[0085] In the present invention, the multilayer foamed particles are filled into a mold so that the compression ratio is 4 to 25% by volume, preferably 5 to 20% by volume, and then the multilayer foamed particles are molded in the mold using steam to obtain the desired molded product.
[0086] The compression ratio is adjusted by cracking the mold when the foamed particles are filled into the mold (cavity) with an amount of multi-layer foamed particles that exceeds the cavity volume. Cracking filling is a filling method in which the mold is not completely closed when the multi-layer foamed particles are filled in order to exhaust the air in the mold from the inside of the mold when filling the mold with the multi-layer foamed particles and to efficiently fill the mold with the multi-layer foamed particles. Note that cracking refers to the opening of the mold, which is finally closed when steam is introduced after the multi-layer foamed particles are filled into the mold, resulting in the filled multi-layer foamed particles being compressed. EXAMPLES
[0087] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.
[0088] Table 1 shows the type and physical properties of the ethylene-propylene random copolymer (A) used as the polypropylene resin (I) as a raw material in the examples and comparative examples, and Table 2 shows the type and physical properties of the ethylene-propylene random copolymer (B) used as the polyolefin resin (II) as a raw material.
[0089] [Table 1]
[0090] [Table 2]
[0091] In Tables 1 and 2, melting points (TmA), (Tm II ), crystallization temperature (TcA), (Tc II ), MFR, molecular weight Mn, molecular weight Mw, and molecular weight Mz were measured by the above-mentioned methods.
[0092] The heat of fusion (ΔHr) of the resin was measured by the above-mentioned method.
[0093] The flexural modulus of the resin was measured by the above-mentioned method.
[0094] Carbon black (CB) used was carbon black for coloring.
[0095] The foam regulator used was zinc borate "Fire Break ZB" manufactured by Borax.
[0096] Carbon dioxide was used as the physical foaming agent.
[0097] Examples 1 to 4, Comparative Examples 1 to 7
[0098] [Production of multi-layered resin particles] An apparatus was used in which a die for forming a multilayer strand was attached to the outlet side of an extruder for a resin particle core layer having an inner diameter of 50 mm and an extruder for a resin particle fusion layer having an inner diameter of 30 mm. The types and amounts of ethylene-propylene random copolymer (A) as polypropylene resin (I), carbon master batch, and bubble control agent master batch shown in Table 3 were fed to an extruder for resin particle core layer with an inner diameter of 50 mm, and at the same time, the types and amounts of ethylene-propylene random copolymer (B) as polyolefin resin (II) and carbon master batch shown in Table 3 were fed to an extruder for resin particle fusion layer with an inner diameter of 30 mm, and each was heated to a set temperature of 200 to 220 ° C, melted, kneaded, and then fed to the die, where they were merged in a sheath-core shape (mass ratio of core layer to fusion layer: 95:5) in the die, and co-extruded as a multilayer strand with the fusion layer coated on the side of the core layer from the hole of the nozzle attached to the tip of the extruder, and the co-extruded strand was water-cooled through water, and cut into (1.2 mg, L / D = 2.9) with a pelletizer to obtain cylindrical multilayer resin particles formed into two layers (sheath-core structure). The weight of the multilayer resin particle, L / D, is an arithmetic average value determined from 100 multilayer resin particles randomly sampled from the group of multilayer resin particles.
[0099] [Table 3]
[0100] In Table 3, the ethylene content (wt%) of the copolymer (A) and the copolymer (B) was measured by the above-mentioned method. A ), melting point (Tm II ) values are calculated from the analytical values of the raw materials shown in Tables 1 and 2.
[0101] [Manufacturing of multi-layer foamed beads] 20 kg of the above multilayered fat particles were charged into a 100 L autoclave together with 60 L of water as a dispersion medium, and 15 g of kaolin as a dispersant, 12 g of sodium alkylbenzene sulfonate as a dispersion aid, and 3 g of aluminum sulfate were added to the dispersion medium. Carbon dioxide as a foaming agent was injected into a sealed container to the container pressure shown in Table 4. The mixture was heated to the foaming temperature shown in Table 4 with stirring and maintained at the same temperature for 15 minutes to adjust the high-temperature peak heat quantity, and then the contents of the autoclave were released together with water under atmospheric pressure to obtain multilayered foamed particles.
[0102] The multilayer expanded beads thus obtained have a polypropylene-based resin expanded core layer and a polyolefin-based resin fusion layer covering the expanded core layer, and the expanded core layer is formed from an ethylene-propylene random copolymer (A) having an ethylene content of 1.5% by mass or more and 3.5% by mass or less, and the molecular weight and molecular weight distribution of the ethylene-propylene random copolymer (A) are within the specific ranges.
[0103] [Table 4]
[0104] In Table 4, the bulk density, melting point (Tmf), crystallization temperature (Tcf) and average cell diameter of the multi-layer foamed beads were measured by the above-mentioned methods.
[0105] In Table 4, the characteristic peak apex temperature, characteristic peak melting end temperature (γ), characteristic peak heat of fusion, high-temperature peak apex temperature, high-temperature peak melting end temperature (T E ), and the high temperature peak heat of fusion (ΔH2) were measured by the above-mentioned method.
[0106] [Pressure treatment of multi-layer foam particles] In Examples 1, 3, and 4 and Comparative Examples 1 to 6, the multi-layered foamed beads were placed in a pressurized tank, and the inside of the pressurized tank was pressurized with air to increase the internal pressure of the bubbles of the multi-layered foamed beads. The internal pressure of the bubbles of the multi-layered foamed beads taken out of the pressurized tank was 0.1 MPa (absolute pressure). The multi-layered foamed beads with the increased internal pressure were used to carry out the in-mold molding described below. In Example 2 and Comparative Example 7, no pressure treatment was performed, and the in-mold molding described below was carried out.
[0107] [Production of foamed bead moldings] As the molding die, a metal mold having a rectangular parallelepiped molding cavity with inner dimensions of 300 mm in the vertical direction × 250 mm in the horizontal direction × 50 mm in the thickness direction was used. The mold was filled with foamed beads in a state where the mold was opened by 5 mm from a completely closed state (the thickness direction dimension of the molded cavity at this time was 55 mm). After filling was completed, the mold was completely closed (crack amount 5 mm, 10%). Then, steam was supplied into the molded cavity to heat the foamed beads, and the foamed beads were secondary expanded and fused to form a foamed bead molded body. The heating method was as follows: with the drain valves of both sides of the mold open, steam was supplied for 5 seconds to perform preheating (exhaust process), then one-sided heating was performed at a pressure 0.08 MPa (G) lower than the molding steam pressure listed in Table 5, and one-sided heating was performed from the opposite direction at a pressure 0.04 MPa (G) lower than the molding steam pressure listed in Table 5. Then, both sides were heated (main heating) at the molding steam pressure listed in Table 5. After heating was completed, the pressure was released, and the mold was water-cooled until the surface pressure of the foamed bead molded body in the mold became 0.04 MPa (G), and the mold was opened and the foamed bead molded body was taken out of the mold. The obtained foamed bead molding was cured for 12 hours under atmospheric pressure at a temperature of 80° C. The water-cooling time was the time required for water-cooling after the end of the main heating until the surface pressure of the foamed bead molding in the mold reached 0.04 MPa (G). The physical properties of the obtained foamed bead molding are shown in Table 5.
[0108] [Table 5]
[0109] Example 2 is the same as Example 1, except that the multi-layer expanded beads were not subjected to the pressure treatment. Example 3 is an example in which the foamed core layer is the same as Example 1, but the fusion layer is different. Example 4 is the same as Example 1, except that the molecular weight distribution of the resin (I) forming the foamed core layer is different. Comparative Example 1 is the same as Example 1 except for the foamed core layer. In order to obtain a good foamed bead molding, the water cooling time was lengthened. Comparative Example 2 is an example in which only the water cooling time was shortened using the same multi-layer expanded beads as in Comparative Example 1. The obtained expanded bead molding expanded and deformed. Comparative Example 3 is the same as Example 1 except for the foamed core layer. In order to obtain a good foamed bead molding, the water cooling time was lengthened. Comparative Example 4 is the same as Example 1 except for the foamed core layer. In order to obtain a good foamed bead molding, the water cooling time was lengthened. Comparative Example 5 is the same as Example 1 except that no fusion layer was provided. The water cooling time was longer. Comparative Example 6 is an example in which single-layer expanded beads consisting of only an expanded core layer using the same resin as in Comparative Example 1 were used. Comparing Comparative Example 1 and Comparative Example 6, and Example 1 and Comparative Example 5, it is clear that the expanded beads according to the present invention have a greater effect of shortening the water cooling time when the structure is changed from a single layer to a multilayer structure. In Comparative Example 7, the resin constituting the foamed core layer and the resin constituting the fusion layer were the same as those in Comparative Example 1, and no pressure treatment was performed. Compared with Example 2, no effect of shortening the water cooling time was obtained.
[0110] In Table 5, the molding density, shrinkage rate, fusion rate, and bending strength of the expanded bead moldings were measured as follows.
[0111] [Mold density of foamed bead molded body] The weight of the expanded bead molding is divided by the volume calculated from the external dimensions of the expanded bead molding, and the value is expressed as [kg / m 3 ] was converted into units.
[0112] [Shrinkage rate] The shrinkage rate [%] of the expanded bead molding was calculated by (300 [mm] - long side length of the molding [mm]) / 300 [mm] x 100. Note that "300 [mm]" is the long side dimension (vertical dimension) of the molding die, and "long side length [mm] of the molding" is the value measured for the long side length of the expanded bead molding obtained in the examples and comparative examples after curing in an atmosphere at 80°C for 12 hours, slowly cooling, and further curing in an atmosphere at 23°C for 6 hours (n=10).
[0113] [Fusion rate] The fusion rate was measured by the following method. The expanded bead molding was folded and broken, the number of expanded beads present on the broken surface (C1) and the number of broken expanded beads (C2) were determined, and the ratio of broken expanded beads to the above-mentioned expanded beads (C2 / C1×100) was calculated as the material destruction rate. The above measurement was carried out 10 times using different test pieces to determine the material destruction rate for each, and the arithmetic average of these values was taken as the fusion rate.
[0114] [Compressive stress at 50% strain] A test piece measuring 50 mm long x 50 mm wide x 25 mm thick was cut out without removing the skin, and a compression test was carried out at a compression speed of 10 mm / min based on JIS K6767-1999 to determine the 50% compressive stress of the foamed bead molding. The test was carried out on 10 test pieces, and the average of the obtained values was taken as the compressive stress at 50% strain.
[0115] [Molecular weight measurement method and measurement conditions] Sample pretreatment: 30 mg of sample was dissolved in 20 mL of o-dichlorobenzene by shaking at 145°C, and the solution was then hot-filtered through a sintered filter with a pore size of 1.0 μm to obtain the analytical sample. Measurements were carried out under the following conditions. Measurement equipment: HLC-8321GPC / HT type high temperature gel permeation chromatograph (manufactured by Tosoh Corporation) Analysis equipment: Data processing software Empower3 (manufactured by Nihon Waters Co., Ltd.) Columns: 2 TSKgel GMH6-HT, 2 TSKgel GMH6-HTL (inner diameter 7.5 mm x length 300 mm, manufactured by Tosoh Corporation) Mobile phase: o-dichlorobenzene (containing 0.025% BHT) Column temperature: 140℃ Detector: Differential Refractometer (RI) Flow rate: 1.0mL / min Sample concentration: 0.15% (W / V)-o-dichlorobenzene Injection volume: 400μL Sampling time interval: 1 second Column calibration: Monodisperse polystyrene (Tosoh Corporation) Molecular weight conversion: Polypropylene (PP) conversion / general calibration method
[0116] [Measurement of melting point, heat of fusion, and crystallization temperature of resin (I) and resin (II) raw materials] The melting point and crystallization temperature of resin (I) or (II) were determined in accordance with JIS K7121:1987. Specifically, the melting point was determined based on the heat flux differential scanning calorimetry method described in JIS K7121:1987, in which 2 mg of pellet-shaped resin was used as a test piece, and the temperature was increased from 30°C to 200°C at a heating rate of 10°C / min, then decreased to 30°C at a cooling rate of 10°C / min, and then increased again from 30°C to 200°C at a heating rate of 10°C / min. The melting point was determined as the apex temperature of the endothermic peak determined by the DSC curve obtained when the test piece was heated from 30°C to 200°C at a heating rate of 10°C / min. The heat of the endothermic peak obtained by the DSC curve was also determined as the heat of fusion. The crystallization temperature is a value measured in accordance with JIS K7121 (1987), and the crystallization temperature (°C) was determined as the apex temperature of the crystallization heat peak on the DSC curve obtained when a sample was melted by heating it from 30°C to 200°C at a heating rate of 10°C / min and then cooling it to 30°C at a cooling rate of 10°C / min. The measurement was performed using a heat flux differential scanning calorimeter (DSC.Q1000, manufactured by TA Instruments).
[0117] [Measurement of melting point and heat of fusion of foamed beads] Approximately 3 mg of the foamed particles was sampled and measured using a differential scanning calorimeter (TA Instruments DSC.Q1000) by increasing the temperature from 23°C to 200°C at a rate of 10°C / min. A DSC curve with one or more melting peaks was obtained, and each measurement value was calculated. [Explanation of symbols]
[0118] a Specific peak b High temperature peak α Point on the DSC line corresponding to 80°C T E End of melting temperature β Melting end temperature T E The point on the DSC curve that corresponds to γ The bottom point of the valley between the intrinsic peak a and the high-temperature peak b δ The point where the line parallel to the vertical axis of the graph from point γ intersects with the line (α-β).
Claims
1. A multi-layer foamed particle having a polypropylene-based resin foamed core layer and a polyolefin-based resin fusion layer covering the foamed core layer, the foamed core layer is formed from a polypropylene-based resin which is an ethylene-propylene random copolymer (A) having an ethylene content of 1.5% by mass or more and 3.5% by mass or less; The ethylene-propylene random copolymer (A) has a number average molecular weight (Mn) of 30,000 or more and 50,000 or less, and a weight average molecular weight (Mw) of 200,000 or more and 500,000 or less, and the ratio (Mw / Mn) of the weight average molecular weight Mw to the number average molecular weight (Mn) is 7 or more and 15 or less.
2. The crystallization temperature Tc of the ethylene-propylene random copolymer (A) A [°C] and the melting point Tm of the ethylene-propylene random copolymer (A). A The multilayer foamed beads according to claim 1, wherein [°C] satisfies the following formula (1): 40≦Tm A -Tc A ≦50 ・・・(1)
3. The multi-layer foamed beads according to claim 1 or 2, wherein the ratio (Mz / Mn) of the Z-average molecular weight (Mz) of the ethylene-propylene random copolymer (A) to the number-average molecular weight (Mn) of the ethylene-propylene random copolymer (A) is 30 or more and 60 or less.
4. The adhesive layer is formed from a polyolefin resin (II), and the melting point Tm II [°C] and the melting point Tm of the ethylene-propylene random copolymer (A). A The multilayer expanded beads according to any one of claims 1 to 3, wherein [°C] satisfies the following formula (4): 0<Tm A -Tm II ≦20 ・・・(4)
5. The bulk density of the multi-layered expanded particles is 10 kg / m 3 More than 300kg / m 3 The multilayer foamed beads according to any one of claims 1 to 4, wherein:
Citation Information
Patent Citations
High-melt strength high-impact polypropylene foaming expanded beads and preparation method thereof
CN106674720A
High-melt strength high-impact polypropylene foaming expanded beads and preparation method thereof
CN106674721A
Expanded resin bead
JP1998077359A
Method for manufacturing foamed polypropylene resin particle, and formed polypropylene resin particle
JP2004068016A
Polypropylene-based resin expanded particle and in-mold formed body using the same
JP2004115785A