Expandable resin particles, pre-expanded particles, and foamed molded article

By employing a two-stage polymerization process with specific initiators, the expandable resin particles achieve low VOC emissions, addressing the high VOC issue in existing polystyrene particles, and produce foam molded articles with improved performance and compliance with emission standards.

JP7553430B2Active Publication Date: 2024-09-18KANEKA CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021505597
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-12
Filing Date
2020-02-06
Publication Date
2024-09-18
Estimated Expiration
2040-02-06

AI Technical Summary

Technical Problem

Existing expandable polystyrene resin particles emit high levels of volatile organic compounds (VOCs), particularly styrene and ethylbenzene, which are difficult to meet stringent emission standards in the automobile and building materials fields, necessitating prolonged drying processes that increase costs.

Method used

The development of expandable resin particles containing styrene and acrylonitrile units with a specific absorbance ratio in their infrared spectrum, produced through a two-stage polymerization process using specific polymerization initiators, resulting in a TH/TQ ratio less than 1.20, which significantly reduces VOC emissions.

Benefits of technology

The solution provides expandable resin particles with low VOC content, enabling the production of foam molded articles that meet stringent emission standards with reduced processing time and costs, ensuring minimal VOC release and maintaining excellent moldability, heat resistance, and flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553430000003
    Figure 0007553430000003
  • Figure 0007553430000002
    Figure 0007553430000002
  • Figure 0007553430000001
    Figure 0007553430000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing foamable resin particles that have a low VOC content and in which VOC off-gassing levels can be suppressed. This goal is achievable through foamable resin particles containing: a base resin comprising a styrene unit and an acrylonitrile unit as constituent units; and a foaming agent, wherein the ratio D2230 / D1600 of absorbance at wavelength 2230 cm–1 and wavelength 1600 cm–1 in the infrared absorption spectrum of the surfaces of foam particles obtained by foaming the foamable resin particles is 0.8 or higher.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to expandable resin particles, pre-expanded resin particles, and foamed molded articles which have a low content of volatile organic compounds and can suppress the amount of volatile organic compounds emitted. [Background technology]

[0002] Expandable polystyrene resin particles are well known as expandable resin particles. Expandable polystyrene resin particles are widely used because they can be easily used to obtain molded articles by in-mold foaming and are inexpensive.

[0003] Although expandable polystyrene resin particles are lightweight and have excellent heat insulation performance, the problem is that they emit a large amount of volatile organic compounds (hereinafter, sometimes referred to as "VOCs," an acronym for Volatile Organic Compounds) per unit time. In particular, with expandable polystyrene resin particles, it is difficult for the VOC components styrene and ethylbenzene to meet the strict emission standards set by the automotive and building materials industries, and measures such as drying the foamed molded body for several days are necessary, which is one of the reasons for the increase in costs.

[0004] In order to solve the above problems, Patent Documents 1 and 2 disclose that expandable polystyrene resin particles having a low residual styrene content in the resin particles can be provided by improving the production method, such as by increasing the amount of initiator added and / or adding a flame retardant later.

[0005] Furthermore, Patent Document 3 discloses heat-resistant styrene-based resin particles of a styrene / acrylonitrile / alpha-methylstyrene system produced using the initiator described in Patent Document 1 or an initiator similar to said initiator. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent Publication No. 2017-052894 [Patent Document 2] Patent Publication No. 2010-195936 [Patent Document 3] Patent Publication No. 2016-164213 Summary of the Invention [Problem to be solved by the invention]

[0007] The above-mentioned conventional technology was an improvement over typical expandable resin particles at the technical level at the time of the development of the conventional technology in terms of reducing VOC emissions. However, there is a high interest in reducing VOC emissions in the market, and the above-mentioned conventional technology had room for further improvement in terms of VOC (particularly styrene and ethylbenzene) emissions.

[0008] One embodiment of the present invention has been made in consideration of the above problems, and an object of the present invention is to provide novel expandable resin particles having a low VOC content and a low emission amount, and a novel foamed molded article having a low VOC emission amount and a low emission amount. [Means for solving the problem]

[0009] The present inventors have completed the present invention as a result of intensive research. That is, the expandable resin particles according to one embodiment of the present invention are expandable resin particles containing a base resin containing styrene units and acrylonitrile units as constituent units and a blowing agent, and the expandable resin particles are expanded to have an infrared absorption spectrum of 2230 cm at a wavelength of 2230 cm at the surface of the expanded beads. -1 and wavelength 1600cm -1 The absorbance ratio D2230 / D1600 is 0.80 or more.

[0010] Furthermore, a method for producing expandable resin particles according to one embodiment of the present invention is a method for producing expandable resin particles, comprising a copolymerization step of copolymerizing monomers including a styrene monomer and an acrylonitrile monomer, and a blowing agent impregnation step of impregnating the obtained copolymer with a blowing agent, the copolymerization step comprising a first polymerization step and a second polymerization step successively having different polymerization temperatures, the first polymerization step using a polymerization initiator including a polymerization initiator (X) having a 10-hour half-life temperature of 74°C or more and 94°C or less, the polymerization initiator (X) including benzoyl peroxide, and the TH / TQ ratio of the expandable resin particles being less than 1.20. Effect of the Invention

[0011] An embodiment of the present invention can provide expandable resin particles and pre-expanded particles (expanded particles), and a foamed molded article, which have a low content of volatile organic compounds (VOCs) and can suppress the amount of volatile organic compounds (VOCs) emitted. [Brief description of the drawings]

[0012] [Figure 1] 1 is a graph showing an example of a GPC measurement chart of expandable resin particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention.

[0014] Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" indicating a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)."

[0015] <Expandable resin particles> The expandable resin particles according to one embodiment of the present invention are expandable resin particles containing a base resin containing a styrene unit and an acrylonitrile unit as constituent units, and a blowing agent, and the expandable resin particles are expanded to have an infrared absorption spectrum at a wavelength of 2230 cm on the surface of the expanded beads. -1 and wavelength 1600cm -1 The absorbance ratio D2230 / D1600 in one embodiment of the present invention is 0.80 or more. The infrared absorption spectrum in one embodiment of the present invention can be obtained by ATR-FTIR analysis.

[0016] In this specification, the term "infrared absorption spectrum of the expanded bead surface" refers to an infrared absorption spectrum obtained by Fourier transform infrared spectroscopy using the total reflectance measurement method for the expanded bead surface. In this specification, "Fourier transform infrared spectroscopy using the total reflectance measurement method" is sometimes referred to as "ATR-FTIR analysis."

[0017] In one embodiment of the present invention, the expanded beads used for measuring the infrared absorption spectrum are obtained by treating the expandable resin beads according to one embodiment of the present invention in the following order of (1) to (3): (1) putting the expandable resin beads into a pressurized foaming machine; (2) next, by blowing steam into the foaming machine at a blowing steam pressure of 0.09 MPa to 0.10 MPa and adjusting the pressure inside the foaming machine to a range of 0.01 MPa to 0.02 MPa, the temperature inside the foaming machine is set to 100°C to 104°C, and the expanded beads are expanded to a magnification of 40 times; (3) next, the obtained expanded beads are cured at 25°C for 12 to 24 hours to obtain the expanded beads used for measuring the infrared absorption spectrum.

[0018] The expandable resin particles according to one embodiment of the present invention have the above-mentioned configuration, and thus have the advantage of being able to provide a foamed molded article with a low VOC emission amount. This allows the standards for VOC emission amount required in the fields of automobiles and building materials to be met. That is, the expandable resin particles according to one embodiment of the present invention have the advantage of being able to provide a foamed molded article with high productivity.

[0019] Here, the expandable resin particles according to one embodiment of the present invention can be used to produce expanded beads by a known method, and then the expanded beads can be used to perform expansion molding by a known method to provide a foamed molded article.

[0020] In this specification, "expandable resin particles according to one embodiment of the present invention" may be simply referred to as "the present expandable resin particles." In other words, the term "the present expandable resin particles" intends one embodiment of the expandable resin particles in the present invention.

[0021] In a broad sense, VOC means "organic compounds that are gaseous when discharged from an exhaust outlet into the atmosphere or dispersed," as defined in the Air Pollution Control Law of Japan. Compounds that should be regulated as VOCs are designated in each technical field. For example, the Ministry of Health, Labor and Welfare of Japan has established indoor concentration guideline values ​​for the following substances: formaldehyde, acetaldehyde, toluene, ethylbenzene, xylene, styrene, nonanal, tetradecane, di-n-butyl phthalate, di-2-ethylhexyl phthalate, p-dichlorobenzene, chlorpyrifos, diazinon, and fenobucarb. In addition, the Japan Automobile Manufacturers Association has set concentration restrictions for the following substances in automobile cabins: formaldehyde, acetaldehyde, toluene, ethylbenzene, xylene, styrene, tetradecane, di-n-butyl phthalate, and di-2-ethylhexyl phthalate.

[0022] In this specification, VOC refers to "compounds that may be contained in expandable resin particles or foamed molded articles, which (a) are in the form of gas when emitted into the atmosphere or dispersed, and (b) are organic compounds for which the Ministry of Health, Labor and Welfare of Japan has established indoor concentration guideline values." Specifically, VOC refers to styrene and ethylbenzene.

[0023] The base resin contained in the expandable resin particles contains, as structural units, styrene units and acrylonitrile units. In this specification, the term "styrene unit" refers to a structural unit derived from a styrene monomer, and the term "acrylonitrile unit" refers to a structural unit derived from an acrylonitrile monomer.

[0024] In the base resin contained in the expandable resin particles, it is preferable that (a) the content of styrene units is 55 parts by weight or more and 80 parts by weight or less, the content of acrylonitrile units is 20 parts by weight or more and 45 parts by weight or less, and (b) the total content of styrene units and acrylonitrile units is 100 parts by weight.

[0025] The content of the styrene unit is preferably 55 parts by weight or more and 80 parts by weight or less, more preferably 60 parts by weight or more and 80 parts by weight or less, and more preferably 65 parts by weight or more and 75 parts by weight or less. When the content of the styrene unit is (a) 55 parts by weight or more, the expandable resin particles have excellent moldability, and when it is (b) 80 parts by weight or less, the expandable resin particles can provide a foamed molded article having excellent heat resistance.

[0026] The content of the acrylonitrile unit is preferably 20 parts by weight or more and 45 parts by weight or less, more preferably 20 parts by weight or more and 40 parts by weight or less, more preferably 25 parts by weight or more and 35 parts by weight or less. When the content of the acrylonitrile unit is 20 parts by weight or more, the expandable resin particles can provide a foamed molded article that (a) has excellent gas barrier properties, so that the amount of styrene released as a VOC is small, and (b) has excellent heat resistance. When the content of the acrylonitrile unit is 45 parts by weight or less, the expandable resin particles have excellent moldability, and the polymerization stability is increased during the production of the expandable resin particles.

[0027] The expandable resin particles according to one embodiment of the present invention have an infrared absorption spectrum of 2230 cm in an ATR-FTIR analysis of the surface of the expanded particles obtained by expanding the expandable resin particles. -1 Absorbance at D2230 and 1600cm -1 The absorbance ratio D2230 / D1600 is 0.8 or more. The absorbance ratio D2230 / D1600 is preferably in the range of 1.2 to 2.5. The absorbance ratio D2230 / D1600 of 0.8 or more can significantly suppress VOC components emitted from the foamed molded article.

[0028] In this specification, "ATR-FTIR analysis" refers to "Fourier transform infrared spectroscopy using attenuated total reflection measurement method."

[0029] The base resin contained in the expandable resin particles may further contain alpha-methylstyrene units as a constituent unit. By adding alpha-methylstyrene, the glass transition temperature of the base resin increases, so that the expandable resin particles can provide a foamed molded article having sufficient heat resistance.

[0030] As used herein, an "alpha-methylstyrene unit" is a structural unit derived from an alpha-methylstyrene monomer.

[0031] The content of the alpha-methylstyrene unit is preferably 3 parts by weight or more and 15 parts by weight or less, more preferably 4 parts by weight or more and 10 parts by weight or less, and even more preferably 4 parts by weight or more and 7 parts by weight or less, when the total content of the styrene unit, the acrylonitrile unit and the alpha-methylstyrene unit in the base resin is 100 parts by weight. Alpha-methylstyrene has a methyl group at the alpha position, which is characterized by large steric hindrance and therefore poor reactivity. In addition, when alpha-methylstyrene is contained in the base resin, the alpha-methylstyrene moiety in the base resin is characterized by being easily decomposed. Therefore, when the content of the alpha-methylstyrene unit is 3 parts by weight or more, the polymerization rate does not become too fast during the production of expandable resin particles, making it easy to control the polymerization. Furthermore, when the content of alpha-methylstyrene units is 15 parts by weight or less, (a) the resulting base resin is less likely to decompose, and the expandable resin particles can provide a foamed molded article with excellent flame retardancy, (b) the reactivity during the polymerization reaction is not deteriorated, and the weight-average molecular weight of the resulting base resin does not become too low, and (c) the expandable resin particles have a low styrene content as a VOC.

[0032] In the base resin contained in the expandable resin particles, it is preferable that (a)(a-1) the content of styrene units is 55 parts by weight or more and 80 parts by weight or less, the content of acrylonitrile units is 20 parts by weight or more and 45 parts by weight or less, the content of alpha-methylstyrene units is 0 parts by weight or more and 15 parts by weight or less, and (a-2) the total content of styrene units, acrylonitrile units and alpha-methylstyrene units is 100 parts by weight, and (b)(b-1) the content of styrene units is 60 parts by weight or more and 80 parts by weight or less, the content of acrylonitrile units is 20 parts by weight or more and 40 parts by weight or less, and the content of alpha-methylstyrene units is 0 parts by weight or more and 15 parts by weight or less. It is preferred that the content of (b-2) styrene units, acrylonitrile units and alpha-methylstyrene units is 100 parts by weight, and more preferably that (c)(c-1) the content of styrene units is 60 parts by weight or more and 75 parts by weight or less, the content of acrylonitrile units is 21 parts by weight or more and 27 parts by weight or less, the content of alpha-methylstyrene units is 3 parts by weight or more and 15 parts by weight or less, and (c-2) the total content of styrene units, acrylonitrile units and alpha-methylstyrene units is 100 parts by weight.

[0033] The foaming agent contained in the expandable resin particles includes, but is not limited to, (a) aliphatic hydrocarbons such as propane, isobutane, normal butane, isopentane, normal pentane, and neopentane cyclohexane, and (b) fluorohydrocarbons with zero ozone depletion potential such as difluoroethane and tetrafluoroethane. The foaming agents described above may be used alone or in combination of two or more.

[0034] The content of the blowing agent in the present expandable resin particles is preferably 2 to 7 parts by weight, more preferably 3 to 6 parts by weight, and even more preferably 4 to 5 parts by weight, based on 100 parts by weight of the expandable resin particles. According to the above configuration, (a) it is possible to produce expanded beads having an expansion ratio of 40 times or more using the expandable resin particles, and (b) the expandable resin particles can provide a foamed molded article having excellent heat resistance and flame retardancy.

[0035] In addition to the base resin and the blowing agent, the expandable resin particles may contain other additives, such as plasticizers, cell regulators, flame retardants, flame retardant auxiliaries, heat radiation inhibitors, pigments, dyes, and antistatic agents.

[0036] Examples of the plasticizer include high-boiling plasticizers having a boiling point of 200° C. or more. Examples of such plasticizers include (a) fatty acid glycerides such as stearate triglyceride, palmitate triglyceride, laurate triglyceride, stearate diglyceride, and stearate monoglyceride, (b) vegetable oils such as coconut oil, palm oil, and palm kernel oil, (c) aliphatic esters such as dioctyl adipate and dibutyl sebacate, and (d) organic hydrocarbons such as liquid paraffin and cyclohexane. When the expandable resin particles contain a large amount of the substances listed as plasticizers, the heat resistance of the foamed molded article that the expandable resin particles can provide tends to deteriorate. Therefore, the content of the plasticizer in the expandable resin particles can be appropriately set so that the foamed molded article that the expandable resin particles can provide has the desired heat resistance.

[0037] The present expandable resin particles may contain a bubble regulator to adjust the bubble diameter in the foamed molded product that can be provided by the expandable resin particles. Examples of the bubble regulator include (a) aliphatic bisamides such as methylene bisstearic acid amide and ethylene bisstearic acid amide, and (b) polyethylene wax. The content of the bubble regulator in the present expandable resin particles is preferably less than 0.1 parts by weight per 100 parts by weight of the expandable resin particles. According to the above configuration, in the foamed molded product that can be provided by the expandable resin particles, deterioration of heat resistance and increase in VOC emission due to miniaturization of bubbles do not occur.

[0038] The present expandable resin particles may contain a flame retardant so that the foamed molded article that can be provided by the expandable resin particles has flame retardancy. The flame retardant is preferably a bromine-based flame retardant. Examples of the bromine-based flame retardant include 2,2-bis[4'-(2'',3''-dibromo-2''-methylpropyloxy)-,3',5'-dibromophenyl]-propane, hexabromocyclododecane, tetrabromocyclooctane, brominated polystyrene, and brominated butadiene-styrene block copolymer. Since the foamed molded article that can be provided by the expandable resin particles is easily flame retardant, the present expandable resin particles preferably contain 2,2-bis[4'-(2'',3''-dibromo-2''-methylpropyloxy)-,3',5'-dibromophenyl]-propane as a flame retardant. In addition, 2,2-bis[4'-(2'',3''-dibromo-2''-methylpropyloxy)-3',5'-dibromophenyl]-propane is also called tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether.

[0039] The content of the flame retardant in the expandable resin particles is preferably 1.5 parts by weight or more and 3.0 parts by weight or less, and more preferably 1.8 parts by weight or more and 2.5 parts by weight or less, relative to 100 parts by weight of the expandable resin particles. When the content of the flame retardant in the expandable resin particles is (a) 1.5 parts by weight or more, relative to 100 parts by weight of the expandable resin particles, the expandable resin particles can provide a foamed molded product with sufficient flame retardant performance, and when (b) 3.0 parts by weight or less, the expandable resin particles have a low VOC content and excellent moldability.

[0040] When the expandable resin particles contain a flame retardant, the expandable resin particles preferably further contain a flame retardant assistant. As the flame retardant assistant, a radical generator such as a peroxide can be used. Examples of such radical generators include dicumyl peroxide, t-butyl peroxybenzoate, 2,3-dimethyl-2,3-diphenylbutane, and 3,4-dialkyl-3,4-diphenylhexane. Since it has little effect on the polymerization reaction and can provide a foamed molded product with good flame retardant performance, the expandable resin particles more preferably contain a peroxide having a 10-hour half-life temperature of 130°C or more and 150°C or less as a flame retardant assistant, and particularly preferably contain dicumyl peroxide.

[0041] The content of the flame retardant auxiliary in the expandable resin particles is preferably 0.3 parts by weight or more and 1.5 parts by weight or less relative to 100 parts by weight of the expandable resin particles. When the content of the flame retardant in the expandable resin particles is (a) 0.3 parts by weight or more relative to 100 parts by weight of the expandable resin particles, the foamed molded article that can be provided by the expandable resin particles has sufficient flame retardant performance, and when it is (b) 1.5 parts by weight or less, the foamed molded article that can be provided by the expandable resin particles has sufficient heat resistance.

[0042] The content of styrene in the expandable resin particles is preferably less than 20 ppm, and the content of ethylbenzene is preferably 130 ppm or less. The content of styrene in the expandable resin particles is more preferably 10 ppm or less, and even more preferably 5 ppm or less. Particularly preferably 0 ppm or less. 0 ppm means below the detection limit in gas chromatography. The content of ethylbenzene in the expandable resin particles is more preferably 100 ppm or less, and even more preferably 70 ppm or less. According to the above configuration, the foamed molded product that can be provided by the expandable resin particles can reduce the amount of VOC released into the environment, and as a result, it is possible to suppress adverse effects on the human body. Here, the content of styrene in the expandable resin particles means the content of styrene monomer in the expandable resin particles, and the content of ethylbenzene in the expandable resin particles means the content of ethylbenzene monomer in the expandable resin particles. As a method for measuring the content of styrene and ethylbenzene in the expandable resin particles (i.e., VOC content), for example, a measurement method using gas chromatography can be mentioned. A specific method will be described in the examples below.

[0043] The expandable resin particles preferably have a base resin weight average molecular weight of 150,000 or more and 220,000 or less, more preferably 170,000 or more and 200,000 or less. When the base resin weight average molecular weight is (a) 150,000 or more, the expandable resin particles can provide a foamed molded article with sufficient strength, flame retardancy, and heat resistance, and when it is (b) 220,000 or less, the expandable resin particles have sufficient foaming power and good moldability. For example, a method for measuring the weight average molecular weight of the base resin can be a method using gel permeation chromatography.

[0044] The expandable resin particles preferably have a weight-average molecular weight of 150,000 or more and 220,000 or less, more preferably 170,000 or more and 200,000 or less. When the weight-average molecular weight of the expandable resin particles is (a) 150,000 or more, the expandable resin particles can provide a foamed molded article having sufficient strength, flame retardancy, and heat resistance, and when the weight-average molecular weight is (b) 220,000 or less, the expandable resin particles have sufficient foaming power and the moldability of the expandable resin particles is good. For example, a method for measuring the weight-average molecular weight of the expandable resin particles can be a measurement method using gel permeation chromatography.

[0045] (TH / TQ ratio of expandable resin particles) The TH / TQ ratio of the present expandable resin particles will be described. The expandable resin particles are subjected to GPC measurement using gel permeation chromatography to obtain a GPC measurement chart. The GPC measurement chart is a relationship chart between molecular weight and differential distribution value, and is obtained as a graph with the molecular weight on the horizontal axis and the differential distribution value on the vertical axis. Here, the horizontal axis is expressed in logarithm (Log). An example of a GPC measurement chart of the expandable resin particles is shown in FIG. 1.

[0046] Fig. 1 is a diagram showing an example of a GPC measurement chart of expandable resin particles. The point where the integral distribution value on the GPC curve of the GPC measurement chart is the highest is taken as the peak top, and is designated as point P as shown in Fig. 1. Next, a line L passing through point P (peak top) and perpendicular to the horizontal axis of the graph is drawn. 1 Draw a line L 1 The intersection point of the GPC curve with the line L is point P. 1 Let the intersection point of line segment PS and the horizontal axis of the graph be point S. Let the point T be the point that is 2 / 3 the length of line segment PS from point P. In other words, the length of line segment ST is twice the length of line segment PT. Next, let us consider a line L that passes through point T and is parallel to the horizontal axis of the graph. 2 Draw a line L 2 Of the two intersection points between the and GPC curves, line L 1 The intersection point on the left side (low molecular weight side) of line L is called point Q. 1The intersection point on the right side (high molecular weight side) of is defined as point H. The ratio of the length of line segment TQ to the length of line segment TH is defined as the TH / TQ ratio. The larger the TH / TQ ratio, the more the expandable resin particles contain high molecular weight components. In the production of expandable resin particles, the composition of the base resin does not change and the blowing agent does not affect the TH / TQ ratio, so the TH / TQ ratio of the expandable resin particles can also be said to be the TH / TQ ratio of the base resin. In other words, the TH / TQ ratio obtained by analyzing the base resin, which is the raw material of the expandable resin particles, can be regarded as the TH / TQ ratio of the expandable resin particles. The conditions for GPC measurement of expandable resin particles using gel permeation chromatography will be described in detail in the following examples.

[0047] The TH / TQ ratio of the expandable resin particles may be less than 1.20, may be 1.19 or less, may be 1.18 or less, may be 1.17 or less, may be 1.16 or less, may be 1.15 or less, may be 1.14 or less, may be 1.13 or less, may be 1.12 or less, may be 1.11 or less, may be 1.10 or less, or may be less than 1.10. The TH / TQ ratio of the expandable resin particles is low when a polymerization initiator (X) having a 10-hour half-life temperature of 74°C or more and 94°C or less is used in the copolymerization step (preparation step of the base resin) in the production of the expandable resin particles. In other words, the expandable resin particles produced using a polymerization initiator containing a polymerization initiator (X) having a 10-hour half-life temperature of 74°C or more and 94°C or less may have a TH / TQ ratio within the above-mentioned range. That is, the expandable resin particles produced by the production method described in the section <Production method of expandable resin particles> described later can have a TH / TQ ratio within the above-mentioned range. In addition, when benzoyl peroxide (also known as dibenzoyl peroxide), ditoluyl peroxide, toluylbenzoyl peroxide, etc. are used as the polymerization initiator (X) described later, expandable resin particles having a lower TH / TQ ratio can be obtained compared to when di-t-butylperoxyhexahydroterephthalate is used as the polymerization initiator (X). It can also be said that expandable resin particles containing a base resin containing an acrylonitrile unit as a constituent unit and having a TH / TQ ratio of less than 1.20 tend to have a low VOC content. It can also be said that expandable resin particles containing a base resin containing an acrylonitrile unit as a constituent unit and having a TH / TQ ratio of less than 1.20 tend to provide a molded product with a low VOC emission. Further, expandable resin particles having a TH / TQ ratio of less than 1.20 have the advantage that they can be easily expanded, that is, can be easily foamed.

[0048] The TH / TQ ratio of the expandable resin particles is preferably 0.90 or more, more preferably 1.00 or more. Expandable resin particles having a TH / TQ ratio of 0.90 or more have the advantage that they can provide a foamed molded article having excellent heat resistance.

[0049] In the production of expandable resin particles, the composition of the base resin does not change. In addition, in the expanded beads produced using the expandable resin particles, the structure of the expandable resin particles changes, but the composition of the expandable resin particles does not change. In addition, in the expanded beads produced using the expandable resin particles, the structure of the expanded particles changes, but the composition of the expanded particles does not change. Therefore, the type of structural unit, the content of each structural unit, and the weight average molecular weight obtained by analyzing the expandable resin particles, the expanded particles, or the expanded molded body can be regarded as the type of structural unit and the content of each structural unit contained in the base resin, which is the raw material thereof, and the weight average molecular weight of the base resin, respectively. In addition, the TH / TQ ratio obtained by analyzing the expanded particles or the expanded molded body can be regarded as the TH / TQ ratio of the expandable resin particles, which are the raw material thereof.

[0050] The weight average molecular weight of the expandable resin particles, expanded beads, or expanded molded article can be obtained by measuring the expandable resin particles, expanded beads, or expanded molded article using gel permeation chromatography. The TH / TQ ratio of the base resin, expanded beads, or expanded molded article can be calculated in the same manner as the TH / TQ ratio of the expandable resin particles, except that the base resin, expanded beads, or expanded molded article is subjected to GPC measurement using gel permeation chromatography to obtain a GPC measurement chart.

[0051] <Method of manufacturing expandable resin particles> A method for producing expandable resin particles according to one embodiment of the present invention includes a copolymerization step of copolymerizing monomers including a styrene monomer and an acrylonitrile monomer, and a blowing agent impregnation step of impregnating the obtained copolymer with a blowing agent, and the copolymerization step includes a first polymerization step and a second polymerization step successively performed at different polymerization temperatures.

[0052] In this specification, the "production method of expandable resin particles according to one embodiment of the present invention" may be simply referred to as "the present production method." In other words, the term "the present production method" intends one embodiment of the production method of expandable resin particles in the present invention. Note that the "copolymer" in the present production method corresponds to the "base resin" contained in the expandable resin particles described in the <Expandable Resin Particles> section.

[0053] Each step of the present manufacturing method will be described below, but the description in the section <Expandable resin particles> will be used as appropriate for matters other than those described in detail below. The present expandable resin particles, i.e., the expandable resin particles described in the section <Expandable resin particles>, are preferably manufactured by the present manufacturing method, but may be manufactured by a method other than the present manufacturing method. In other words, the manufacturing method of the present expandable resin particles is not limited to the embodiment of the present manufacturing method described below.

[0054] The styrene monomer may contain a small amount of ethylbenzene monomer used in the production process. The styrene monomer used in the production method of the present invention preferably has a lower content of ethylbenzene monomer in the styrene monomer, for example, preferably 130 ppm or less, more preferably 100 ppm or less, even more preferably 85 ppm or less, and particularly preferably 70 ppm or less. By using a styrene monomer with a low content of ethylbenzene monomer, the expandable resin particles obtained by the production method of the present invention have the advantage of being able to provide a foamed molded product with even less ethylbenzene emission.

[0055] In the copolymerization step of the present production method, the method for copolymerizing the monomers including the styrene monomer and the acrylonitrile monomer is not particularly limited, and a conventionally known polymerization method can be used. The copolymerization step is preferably a suspension polymerization method in which polymerization is performed in an aqueous suspension.

[0056] In this specification, the term "aqueous suspension" refers to a liquid (aqueous solution) in which resin particles, expandable resin particles, and / or monomer droplets are dispersed in water or an aqueous solution using a stirrer or the like. In the aqueous suspension, surfactants and monomers may be dissolved, or water-insoluble dispersants, polymerization initiators, crosslinking agents, plasticizers, bubble regulators, flame retardants, and flame retardant assistants may be dispersed together with the monomers. The polymerization initiators, crosslinking agents, chain transfer agents, and polymerization regulators used in the copolymerization step constitute a part of the resulting copolymer.

[0057] In the copolymerization step, the weight ratio of the resin to water in the aqueous suspension, expressed as the weight ratio of the resulting copolymer to the weight of water, is preferably 1.0 / 0.6 to 1.0 / 3.0.

[0058] Examples of dispersants that can be used in the copolymerization step include (a) poorly water-soluble inorganic salts such as tricalcium phosphate, magnesium pyrophosphate, hydroxyapatite, and kaolin, and (b) water-soluble polymers such as polyvinyl alcohol, methyl cellulose, polyacrylamide, and polyvinylpyrrolidone. When using poorly water-soluble inorganic salts as dispersants, it is preferable to use an anionic surfactant such as sodium α-olefin sulfonate or sodium dodecylbenzene sulfonate in combination with the poorly water-soluble inorganic salt, in order to increase the dispersion stability. These dispersants may be further added to the aqueous suspension at any time during the copolymerization step, as necessary.

[0059] The amount of dispersant used depends on the type of dispersant. When a poorly water-soluble inorganic salt is used as the dispersant, the amount of dispersant used is preferably 0.1 parts by weight or more and 1.5 parts by weight or less per 100 parts by weight of water. When a water-soluble polymer is used as the dispersant, the dispersant is preferably used so that the dispersant is present at 30 ppm or more and 100 ppm or less in the aqueous suspension. When an anionic surfactant is used in combination with the poorly water-soluble inorganic salt, the anionic surfactant is preferably used so that the anionic surfactant is present at 30 ppm or more and 100 ppm or less in the aqueous suspension.

[0060] In the copolymerization step in the present production method, a chain transfer agent and a polymerization regulator may be further used. Examples of the chain transfer agent include mercaptan-based compounds such as n-octyl mercaptan, n-dodecyl mercaptan, and t-dodecyl mercaptan. Examples of the polymerization regulator include α-methylstyrene dimer. Since α-methylstyrene dimer also contributes to the adjustment of the weight average molecular weight of the copolymer, it can also be called a chain transfer agent. The chain transfer agent mainly functions to adjust the weight average molecular weight of the copolymer. The polymerization regulator mainly functions to adjust the polymerization rate.

[0061] In the copolymerization step, it is preferable to use α-methylstyrene dimer as a chain transfer agent. According to the above-mentioned constitution, (a) the polymerization rate and the weight average molecular weight of the copolymer can be easily adjusted, and (b) the foamed molded article that can be provided by the expandable resin particles is less likely to emit an odor.

[0062] The amount of the chain transfer agent and polymerization regulator used is preferably 0.6 parts by weight or more, and more preferably 1.4 parts by weight or more, per 100 parts by weight of the monomer, from the viewpoint of facilitating adjustment of (a) the polymerization rate and (b) the weight-average molecular weight of the copolymer.

[0063] As the polymerization initiator, it is preferable to mainly use the polymerization initiator (X) in the first polymerization step, and mainly use the polymerization initiator (Y) in the second polymerization step.

[0064] The first polymerization step is not particularly limited in terms of the polymerization temperature and polymerization time, etc., as long as the polymerization temperature is different from that of the second polymerization step. The polymerization temperature of the first polymerization step is, for example, 85°C to 95°C, and the polymerization time of the first polymerization step is, for example, 4 hours to 7 hours.

[0065] The polymerization temperature in the first polymerization step is preferably 87°C to 93°C, more preferably 88°C to 92°C, and particularly preferably 89°C to 91°C. This configuration has the advantage that (a) expandable resin particles having D2230 / D1600 of 0.80 or more, that is, expandable resin particles having a low VOC content (emission amount), can be easily obtained. In addition, this configuration allows the decomposition amount of the polymerization initiator (e.g., polymerization initiator (X)) to be adjusted within an optimal range. As a result, (a) the polymerization rate (reaction rate) can be easily adjusted, improving polymerization stability, and (b) expandable resin particles in an appropriate molecular weight range can be easily obtained.

[0066] The polymerization time in the first polymerization step is preferably 4.5 hours to 6.5 hours, particularly preferably 5 hours to 6 hours. This configuration has the advantage of being able to achieve both productivity and polymerization stability.

[0067] In the first polymerization step, it is preferable to use a polymerization initiator (X) having a 10-hour half-life temperature of 74° C. or more and 94° C. or less.

[0068] In the first polymerization step, it is preferable to (a) use a polymerization initiator (X) having a 10-hour half-life temperature of 74° C. or more and 94° C. or less, and (b) carry out the polymerization reaction at a polymerization temperature of 85° C. or more and 95° C. or less. According to the above configuration, the polymerization reaction can be appropriately controlled.

[0069] Examples of the polymerization initiator (X) in the first polymerization step include organic peroxides such as benzoyl peroxide, lauroyl peroxide, and di-t-butylperoxyhexahydroterephthalate, and (b) azo compounds such as azobisisobutyronitrile and azobisdimethylvaleronitrile. Of these polymerization initiators, it is particularly preferable to use benzoyl peroxide as the polymerization initiator (X) because it facilitates the reaction of acrylonitrile, which can impart gas barrier properties.

[0070] The above-mentioned polymerization initiator (X) may be used alone or in combination of two or more kinds.

[0071] It is more preferable to use only polymerization initiators having a 10-hour half-life temperature of 74° C. or more and less than 90° C. as the polymerization initiator (X). That is, in the first polymerization step, it is more preferable to use only polymerization initiators having a 10-hour half-life temperature of 74° C. or more and less than 90° C. as the polymerization initiator (X) (a), and it is even more preferable to use only polymerization initiators having a 10-hour half-life temperature of 74° C. or more and less than 90° C. as the polymerization initiator (X) (b-1), and to carry out the polymerization reaction at a polymerization temperature of 85° C. or more and 95° C. or less (b-2). According to the above configuration, the polymerization initiator (X) used in the first polymerization step is mainly decomposed in the first polymerization step, so that the polymerization reaction can be more appropriately controlled.

[0072] In the first polymerization step, a polymerization initiator (X) is used, and the amount of the polymerization initiator (X) used is preferably 0.08 parts by weight or more and 0.25 parts by weight or less, more preferably 0.15 parts by weight or less and 0.20 parts by weight or less, relative to 100 parts by weight of the monomer. In the first polymerization step, when the amount of the polymerization initiator (X) used is (a) 0.08 parts by weight or more relative to 100 parts by weight of the monomer, it has the advantage that the polymerization proceeds sufficiently, and when it is (b) 0.25 parts by weight or less, the polymerization reaction does not proceed too quickly, making it easy to control the polymerization. In addition, when the amount of the polymerization initiator (X) used is 0.15 parts by weight or less and 0.20 parts by weight or less, the weight average molecular weight of the obtained expandable resin particles is 170,000 or more and less than 200,000, and good quality expandable resin particles are obtained.

[0073] In this production method, the weight average molecular weight of the copolymer can be adjusted by variously combining the polymerization initiator, the chain transfer agent, and the polymerization conditions in the first polymerization step.

[0074] The second polymerization step is carried out successively to the first polymerization at any time point after the polymerization conversion rate of the monomer reaches 85%.

[0075] Here, the polymerization conversion rate of the monomer is calculated as follows: Polymerization conversion rate of monomer (%)=(amount of monomer supplied to aqueous suspension−amount of monomer remaining in aqueous suspension) / amount of monomer supplied to aqueous suspension×100 The above "amount of monomer supplied to the aqueous suspension - amount of monomer remaining in the aqueous suspension" can be said to be the amount of monomer contained as a structural unit in the copolymer. The "amount of monomer remaining in the aqueous suspension" can be measured, for example, by filtering the aqueous suspension with filter paper or the like and subjecting the residue (which may contain monomer) obtained on the filter paper to gas chromatography.

[0076] The polymerization temperature in the second polymerization step is different from that in the first polymerization step, and the polymerization temperature in the second polymerization step is preferably 110 to 120°C. If the polymerization temperature in the second polymerization step is (a) less than 110°C, the VOC content (particularly the styrene content) in the resulting expandable resin particles cannot be reduced, and if it is (b) more than 120°C, the internal pressure of the polymerization machine used in the copolymerization step becomes high, requiring high pressure resistance, and as a result, a heavy-duty polymerization machine is required. The polymerization temperature in the second polymerization step is preferably higher than that in the first polymerization step. According to the above configuration, the VOC content in the resulting expandable resin particles can be reduced.

[0077] The polymerization time in the second polymerization step is preferably 3 to 13 hours, more preferably 4 to 11 hours, further preferably 5 to 9 hours, and particularly preferably 6 to 8 hours. If the polymerization time in the second polymerization step is (a) less than 3 hours, the VOC content (particularly the styrene content) in the obtained expandable resin particles cannot be reduced, and (b) if it exceeds 8 hours, the decomposition amount of the flame retardant auxiliary (e.g., dicumyl peroxide) increases, so that the effect of the flame retardant auxiliary is not fully exerted when the foamed molded article is burned, and as a result, the flame retardancy tends to deteriorate.

[0078] The polymerization temperature in the second polymerization step is preferably 111° C. to 119° C., more preferably 112° C. to 118° C., further preferably 113° C. to 117° C., and particularly preferably 114° C. to 116° C. This configuration has the advantage that VOCs can be efficiently reduced at or below the upper limit of the internal pressure of the polymerization machine used.

[0079] The polymerization time in the second polymerization step is preferably 4 to 11 hours, more preferably 5 to 9 hours, and particularly preferably 6 to 8 hours. This configuration has the advantage of being able to reduce VOCs while maintaining qualities such as flame retardancy.

[0080] In the second polymerization step, it is preferable to use a polymerization initiator (Y) having a 10-hour half-life temperature of 90°C or more and 100°C or less, and it is more preferable to mainly use a polymerization initiator (Y) having a 10-hour half-life temperature of 90°C or more and 100°C or less.

[0081] Examples of the polymerization initiator (Y) include t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, t-amylperoxyisopropyl monocarbonate, t-amylperoxy-2-ethylhexyl monocarbonate, and 1,1-bis(t-butylperoxy)cyclohexane. These polymerization initiators (Y) may be used alone or in combination of two or more. The polymerization initiator (Y) can be suitably used in the second polymerization step.

[0082] In addition, 1,1-bis(t-butylperoxy)cyclohexane undergoes cleavage in two stages. The 10-hour half-life temperature when 1,1-bis(t-butylperoxy)cyclohexane before cleavage undergoes the first stage cleavage is 90°C. The 10-hour half-life temperature when the intermediate product generated after the first stage cleavage undergoes the second stage cleavage is about 5°C higher than the 10-hour half-life temperature of the first stage, and is 95°C or higher. As for 1,1-bis(t-butylperoxy)cyclohexane, the final product generated after the second stage cleavage mainly acts in the second polymerization step. Therefore, in this specification, 1,1-bis(t-butylperoxy)cyclohexane is not considered to be a polymerization initiator (X) but is considered to be a polymerization initiator (Y).

[0083] As the polymerization initiator (Y), t-butylperoxy-2-ethylhexyl monocarbonate and t-amylperoxy-2-ethylhexyl monocarbonate are particularly preferred since they promote the reaction between styrene remaining in the expandable resin particles or aqueous suspension and acrylonitrile.

[0084] The amount of the polymerization initiator (Y) used in the second polymerization step is preferably 0.25 parts by weight or more and 0.90 parts by weight or less, and more preferably 0.28 parts by weight or more and 0.60 parts by weight or less, based on 100 parts by weight of the monomer. Within this range, the styrene and acrylonitrile remaining in the expandable resin particles or the aqueous suspension tend to react more easily, and the proportion of the styrene-acrylonitrile copolymer in the surface layer of the expandable resin particles tends to increase.

[0085] The second polymerization step may be carried out simultaneously as a blowing agent impregnation step, that is, in the presence of a blowing agent.

[0086] The foaming agent impregnation step is initiated by adding a foaming agent to the aqueous suspension, and the specific treatment temperature (also referred to as impregnation temperature) and treatment time (also referred to as impregnation time) are not particularly limited.

[0087] The strength of the bonding force between polymer chains in the base resin contained in the expandable resin particles and the impregnation efficiency of the blowing agent into the copolymer in the production of the expandable resin particles are inversely proportional to each other. The present production method can provide expandable resin particles containing a base resin having a strong bonding force between polymer chains. Therefore, from the viewpoint of sufficiently impregnating the copolymer with the blowing agent, the impregnation temperature in the blowing agent impregnation step in the present production method is preferably 110°C to 120°C, more preferably 111°C to 119°C, even more preferably 112°C to 118°C, and particularly preferably 114°C to 116°C. From the viewpoint of sufficiently impregnating the copolymer with the blowing agent, the impregnation time in the blowing agent impregnation step in the present production method is preferably 3 hours to 13 hours, more preferably 4 hours to 11 hours, even more preferably 5 hours to 9 hours, and particularly preferably 6 hours to 8 hours. In addition, when the second polymerization step is also performed as the blowing agent impregnation step, i.e., when the second polymerization step and the blowing agent impregnation step are performed together, the polymerization temperature of the second polymerization step can be said to be the impregnation temperature of the blowing agent impregnation step, and the polymerization time of the second polymerization step can be said to be the impregnation time of the blowing agent impregnation step.

[0088] The present production method preferably further includes a drying step of drying the expandable resin particles. The expandable resin particles are obtained in a state of being dispersed in an aqueous suspension. Therefore, when the present production method includes a drying step, the obtained expandable resin particles can be suitably used for the production of expanded beads, etc.

[0089] In the drying step, the method for drying the expandable resin particles is not particularly limited, and for example, a groove-type or cylindrical agitator dryer, a box-type or band-type through-air dryer, a fluidized bed dryer, or the like can be used.

[0090] The drying process in the drying step is preferably carried out at a temperature equal to or lower than the expansion temperature of the expandable resin particles, and from the viewpoint of productivity, is more preferably carried out at 30°C to 55°C. The water content of the resulting expandable resin particles can be adjusted by adjusting the temperature at which the drying process is carried out (also referred to as the processing temperature). When the drying process temperature in the drying step is (a) 30°C or higher, the water content does not become too high, so that the expansion particles that can be provided by the expandable resin particles can be prevented from having fine bubbles, and the amount of VOC emission can be reduced, and when the drying process temperature is (b) 55°C or lower, the water content does not become too low, so that there is no risk of the flame retardancy being deteriorated in the foamed molded article that can be provided by the expandable resin particles.

[0091] The polymerization initiator (X) preferably contains at least benzoyl peroxide. That is, a further preferred embodiment of the manufacturing method according to one embodiment of the present invention is a manufacturing method for expandable resin particles, which includes a copolymerization step of copolymerizing a monomer (monomer mixture) containing a styrene monomer and an acrylonitrile monomer, and a blowing agent impregnation step of impregnating the obtained copolymer with a blowing agent, the copolymerization step includes a first polymerization step and a second polymerization step successively having different polymerization temperatures, the first polymerization step uses a polymerization initiator containing a polymerization initiator (X) having a 10-hour half-life temperature of 74°C or more and 94°C or less, the polymerization initiator (X) contains benzoyl peroxide, and the TH / TQ ratio of the expandable resin particles is less than 1.20. According to this configuration, it is possible to provide expandable resin particles that can provide a foamed molded product with a low VOC emission amount, in other words, a foamed molded product with high productivity.

[0092] The amount of benzoyl peroxide used in the first polymerization step is preferably 0.08 parts by weight or more and 0.25 parts by weight or less, and more preferably 0.15 parts by weight or less and 0.20 parts by weight or less, based on 100 parts by weight of the monomer. According to this configuration, it is possible to provide expandable resin particles that can provide a foamed molded product with a lower VOC emission amount, in other words, a foamed molded product with higher productivity.

[0093] <Foamed product and its manufacturing method> The expandable resin particles can be made into expanded particles by a general expansion method. A specific expansion method includes a method in which the following (1) to (3) are carried out in sequence: (1) expandable resin particles are placed in a container equipped with a stirrer, (2) the expandable resin particles are heated with a heat source such as steam, and (3) the particles are expanded until a desired expansion ratio is reached, thereby obtaining expanded particles. The expanded particles may also be called pre-expanded particles, and therefore the expansion method for obtaining the pre-expanded particles may also be called a pre-expanding method.

[0094] The expanded beads obtained by expanding the expandable resin beads according to one embodiment of the present invention also constitute one embodiment of the present invention. The expanded beads according to one embodiment of the present invention can provide a foamed molded article with a low VOC emission amount, in other words, a foamed molded article with high productivity.

[0095] The expanded beads according to one embodiment of the present invention may have the following configuration. That is, the expanded beads according to another embodiment of the present invention are expanded beads obtained by expanding expandable resin beads, and the expandable resin beads contain (a) a base resin containing styrene units and acrylonitrile units as constituent units, and (b) a blowing agent, and have an infrared absorption spectrum of the surface of the expanded beads at a wavelength of 2230 cm. -1 and wavelength 1600cm -1 The absorbance ratio D2230 / D1600 is 0.80 or more.

[0096] The expanded beads according to one embodiment of the present invention may have the following structure: That is, the expanded beads according to another embodiment of the present invention (a) contain styrene units and acrylonitrile units as structural units, and (b) have an infrared absorption spectrum of the surface of the expanded beads at a wavelength of 2230 cm -1 and wavelength 1600cm -1 The absorbance ratio D2230 / D1600 is 0.80 or more.

[0097] The expanded beads can be molded into a foamed molded article by a general in-mold molding method, which includes filling a mold that can be closed but cannot be sealed with the expanded beads and heating and fusing the expanded beads with water vapor to form a foamed molded article.

[0098] The foamed molded article obtained by molding the foamed beads according to one embodiment of the present invention in a mold is also one embodiment of the present invention. The foamed molded article according to one embodiment of the present invention has an advantage that it emits a small amount of VOCs.

[0099] The foamed molded product according to one embodiment of the present invention preferably has a styrene release amount of 2 ppm or less and an ethylbenzene release amount of less than 15 ppm. Here, the styrene release amount and the ethylbenzene release amount are amounts released into a 20 ml container when 0.025 g of the foamed molded product is left in the container under a condition of 60 ° C. for 2 hours. The styrene and ethylbenzene release amounts are shown as concentrations (ppm) in the gas in a 20 ml container containing 0.025 g of the foamed molded product. The styrene release amount in the foamed molded product according to one embodiment of the present invention is preferably 1.5 ppm or less, more preferably 1.0 ppm or less, even more preferably 0.6 ppm or less, and particularly preferably 0.5 ppm or less. The ethylbenzene release amount in the foamed molded product according to one embodiment of the present invention is preferably less than 13 ppm, more preferably 10 ppm or less, even more preferably 7 ppm or less, and particularly preferably 5 ppm or less.

[0100] As used herein, the terms "emitted amount" and "diffusion amount" are synonymous and interchangeable.

[0101] When the amounts of styrene and ethylbenzene released from the foam molded product according to one embodiment of the present invention are within the above-mentioned ranges, there is an advantage in that there is no risk of adverse effects on the body, such as sick house syndrome, when the foam molded product is used as an automobile interior material or a building insulation material.

[0102] In this specification, the "foamed molded article according to one embodiment of the present invention" may be simply referred to as the "foamed molded article of the present invention." In other words, the term "foamed molded article of the present invention" is intended to mean one embodiment of the foamed molded article of the present invention.

[0103] The oxygen index of the foamed molded article is preferably 26% or more, more preferably 27% or more, even more preferably 28% or more, and particularly preferably 29% or more. According to the above configuration, when the foamed molded article is used as an automobile interior material or a building insulation material, the foamed molded article has an advantage that it can exhibit sufficient flame retardant performance.

[0104] The present foamed molded article is preferably excellent in heat resistance. For example, when the present foamed molded article is used as a heat-insulating material or as a material for parts of an automobile exposed to sunlight, the present foamed molded article is preferably small in deformation when used at 90° C. or higher. Specifically, when a foamed molded article with an expansion ratio of 40 times is left for 168 hours under conditions of 90° C., the dimensional change rate of the foamed molded article before and after leaving it is preferably 0.4% or less, more preferably 0.35% or less, even more preferably 0.3% or less, and particularly preferably 0.25% or less.

[0105] The average bubble diameter of the surface layer of the present foamed molded product is preferably 50 μm or more and less than 100 μm, more preferably 60 to 90 μm. When the average bubble diameter is 50 μm or more, (a) the cell membrane has a sufficient thickness, so that the dimensional change of the foamed molded product with respect to temperature is small, (b) the amount of VOC and total VOC released can be reduced, and (c) the cell membrane has a sufficient thickness, so that the cell membrane is not melted by pressurized steam during molding in the mold, and therefore the surface property of the foamed molded product is good. When the cell membrane is thin, the foamed molded product may expand in an environment of 90° C. or more, and the dimensional stability of the foamed molded product may be deteriorated. The expansion of the foamed molded product in a high-temperature environment is sometimes called tertiary expansion. When the average bubble diameter is less than 100 μm, the surface property of the foamed molded product is good.

[0106] In this specification, the "average cell diameter of the surface layer" refers to the average chord length of the expanded beads present on a straight line on the cut surface of the surface layer of the foamed molded article. The average chord length is a value obtained by measuring in accordance with ASTM-D-2842-97 using a photograph of the cut surface of the foamed molded article projected thereon. The average chord length is determined by arbitrarily selecting 10 expanded beads present on a straight line on the cut surface of the surface layer of the foamed molded article in the photograph of the cut surface of the foamed molded article projected thereon, measuring the chord length of each of the expanded beads, and averaging the measured values.

[0107] An embodiment of the present invention may have the following configuration.

[0108] (X1) Expandable resin particles comprising a base resin containing a styrene unit and an acrylonitrile unit as constituent units, and a blowing agent, wherein the expandable resin particles are expanded, and the surface of the expanded particles has an infrared absorption spectrum at a wavelength of 2230 cm -1 and wavelength 1600cm -1 The expandable resin particles are characterized in that the absorbance ratio D2230 / D1600 at 0.80 or more.

[0109] (X2) The expandable resin particles according to (X1), wherein the expandable resin particles have a styrene content of less than 20 ppm and an ethylbenzene content of 130 ppm or less.

[0110] (X3) Expandable resin particles according to (X1) or (X2), characterized in that the weight average molecular weight is 150,000 or more and 220,000 or less.

[0111] (X4) The expandable resin particles according to any one of (X1) to (X3), characterized in that in the base resin, (a) the content of the styrene units is 55 parts by weight or more and 80 parts by weight or less, the content of the acrylonitrile units is 20 parts by weight or more and 45 parts by weight or less, and (b) the total content of the styrene units and the acrylonitrile units is 100 parts by weight.

[0112] (X5) The expandable resin particles according to any one of (X1) to (X4), wherein a TH / TQ ratio is less than 1.20.

[0113] (X6) Expanded particles obtained by expanding the expandable resin particles according to any one of (X1) to (X5).

[0114] (X7) A foamed molded article obtained by molding the foamed beads according to (X6) in a mold.

[0115] (X8) The foam molded article according to (X7), wherein the average cell diameter of the surface layer is 50 μm or more and less than 100 μm.

[0116] (X9) The foamed molded article according to (X7) or (X8), characterized in that the amount of styrene emitted is 2 ppm or less and the amount of ethylbenzene emitted is less than 15 ppm.

[0117] (X10) A method for producing expandable resin particles, comprising: a copolymerization step of copolymerizing monomers including a styrene monomer and an acrylonitrile monomer; and a blowing agent impregnation step of impregnating the obtained copolymer with a blowing agent, wherein the copolymerization step comprises a first polymerization step and a second polymerization step which are successively performed at different polymerization temperatures, wherein the first polymerization step uses a polymerization initiator including a polymerization initiator (X) having a 10-hour half-life temperature of 74°C or more and 94°C or less, the polymerization initiator (X) includes benzoyl peroxide, and the TH / TQ ratio of the expandable resin particles is less than 1.20.

[0118] An embodiment of the present invention may have the following configuration.

[0119] (Y1) Expandable resin particles comprising a base resin containing a styrene unit and an acrylonitrile unit as constituent units, and a blowing agent, wherein the expandable resin particles are expanded, and the surface of the expanded particles has an infrared absorption spectrum at a wavelength of 2230 cm -1 and wavelength 1600cm -1 The expandable resin particles have an absorbance ratio D2230 / D1600 of 0.8 or more.

[0120] (Y2) The expandable resin particles according to (Y1), characterized in that the expandable resin particles have a styrene content of less than 20 ppm and an ethylbenzene content of 130 ppm or less.

[0121] (Y3) Expandable resin particles according to (Y1) or (Y2), characterized in that the weight average molecular weight is 150,000 or more and 220,000 or less.

[0122] (Y4) Expanded particles obtained by expanding the expandable resin particles according to any one of (Y1) to (Y3).

[0123] (Y5) A foamed molded article obtained by molding the foamed beads according to (Y4) in a mold.

[0124] (Y6) The foam molded product according to (Y5), characterized in that the average cell diameter of the surface layer is 50 μm or more and less than 100 μm.

[0125] (Y7) The foamed molded article according to (Y5) or (Y6), characterized in that the amount of styrene emitted is 2 ppm or less and the amount of ethylbenzene emitted is less than 15 ppm. EXAMPLES

[0126] Examples and comparative examples are given below, but the present invention is not limited thereto.

[0127] The polymerization initiators, flame retardants, flame retardant assistants and chain transfer agents used in the examples and comparative examples are as follows. Polymerization initiator (X): Benzoyl peroxide (Niper BW (NOF Corp.)) (10-hour half-life temperature 74°C); and Di-t-butyl peroxyhexahydroterephthalate (Kayaester HTP-65W (manufactured by Kayaku Akzo Co., Ltd.)) (10-hour half-life temperature: 83°C); Polymerization initiator (Y): t-Butylperoxy-2-ethylhexyl monocarbonate (Perbutyl E (manufactured by Nippon Oil & Fats Co., Ltd.)) (10-hour half-life temperature 99°C); and 1,1-bis(t-butylperoxy)cyclohexane (Perhexa C (manufactured by Nippon Oil & Fats Co., Ltd.)) (10-hour half-life temperature 90°C) Flame Retardant: Tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether (Pyroguard SR-130 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.)). Flame retardant synergists: Dicumyl peroxide (Percumyl D (manufactured by Nippon Oil & Fats Co., Ltd.)). Chain transfer agent: α-Methylstyrene dimer (MSD (manufactured by Nippon Oil & Fats Co., Ltd.)). In the examples and comparative examples, the molecular weight of the expandable resin particles, the contents of styrene and ethylbenzene in the expandable resin particles, and the evaluation of the expandability of the expandable resin particles were measured by the following methods. In addition, "parts" and "%" are based on weight unless otherwise specified, and respectively mean "parts by weight" and "%".

[0128] (Weight average molecular weight measurement method) 0.02 g of the expandable resin particles was dissolved in 20 cc of tetrahydrofuran, and the weight average molecular weight Mw was measured by gel permeation chromatography (GPC) (HLC-8020 manufactured by Tosoh Corporation, column: TSKgel Super HZM-H, column temperature: 40°C, flow rate: 0.35 ml / 1 min.). The weight average molecular weight was calculated as a value converted into standard polystyrene. The results are shown in Tables 1 and 2 as "Mw (weight average molecular weight)".

[0129] (Calculation method for TH / TQ ratio of expandable resin particles) 0.02 g of the obtained expandable resin particles was dissolved in 20 ml of tetrahydrofuran (THF) to obtain a sample. Thereafter, the obtained sample was subjected to GPC measurement using gel permeation chromatography under the following conditions to obtain a GPC measurement chart. Measurement equipment: Tosoh Corporation, high-speed GPC equipment HLC-8220 Columns used: 2 SuperHZM-H and 2 SuperH-RC columns manufactured by Tosoh Corporation, total of 4 columns Column temperature: 40℃ Mobile phase: THF (tetrahydrofuran) Flow rate: 0.35ml / min Injection volume: 10μl Detector: RI.

[0130] The TH / TQ ratio was determined by the above-mentioned method for the GPC curve of the obtained GPC measurement chart. The obtained results are shown in Tables 1 and 2 as "TH / TQ ratio".

[0131] (Method for measuring the content of styrene and ethylbenzene in expanded resin particles) 0.25 g of expandable resin particles was dissolved in 20 cc of methylene chloride (with cyclopentanol as internal standard), and the styrene and ethylbenzene contained in the expandable resin particles were measured using a gas chromatograph GC-2014 (capillary column: Rtx-1 manufactured by GL Science, column temperature conditions: heating from 50°C to 80°C (heating rate 3°C / min), then heating from 80°C to 180°C (heating rate 10°C / min), carrier gas: helium) manufactured by Shimadzu Corporation. The styrene and ethylbenzene contents in the expandable resin particles were quantified from the results obtained using the measured calibration curves for styrene and ethylbenzene. The results are shown in Tables 1 and 2 as "residual styrene monomer" and "ethylbenzene".

[0132] (Evaluation of expandability of expandable resin particles) The expandable resin particles were placed in a steamer at 100°C and heated for 5 minutes to obtain expanded particles. 3 and measure the volume (cm 3 The bulk ratio (cm) was measured using the following formula: 3 / g) was calculated.

[0133] Bulk magnification (cm 3 / g) = Volume of foam particles (cm 3 ) / 10g If the evaluation result is less than 40 times, the bulk ratio will not be 40 times or more even if the foam is pre-expanded using a pressurized pre-expanding machine, so this evaluation result is an index of foamability. The results are shown in Tables 1 and 2 as "foamability (40 times)". 〇(Good): 50 times or more △(Pass): 40 times or more × (bad): Less than 40 times.

[0134] The method for producing the expanded beads is as follows.

[0135] (Production of expanded beads) The expandable resin particles were sieved to separate those having a particle size of 0.5 to 1.4 mm.

[0136] The separated expandable resin particles were pre-expanded to a bulk ratio of 40 times using a pressurized pre-expanding machine (manufactured by Daikai Kogyo, BHP) under conditions of an injection steam pressure of 0.09 to 0.10 MPa, and the pre-expanded particles were then left at room temperature for one day to obtain expanded particles with a bulk ratio of 40 times.

[0137] The amount of blocking of the resulting expanded beads was measured by the following method.

[0138] (Method for measuring the amount of blocking during pre-foaming) Blocking is a mass formed when foam particles are bonded together during the pre-expansion process. If there is a large amount of blocking, poor filling occurs during the molding process, so it is better to have a small amount of blocking. The method for measuring the amount of blocking is as follows.

[0139] The entire amount of foamed particles obtained by the foaming operation was passed through a wire mesh with a mesh spacing of 1 cm. The weight of the mass remaining on the wire mesh was measured, and the amount of blocking was calculated using the following formula. Blocking amount (%) = weight of block / total weight of foam particles x 100 The blocking property was evaluated based on the obtained blocking amount according to the following criteria. The obtained results are shown in Tables 1 and 2 as "blocking amount". Good: Less than 0.05% △ (Pass): Less than 0.01% 0.05% or more × (defective): 0.1% or more.

[0140] <Absorbance ratio measurement> The absorbance ratio of the obtained expandable resin particles was determined by randomly sampling 10 pre-expanded particles (expanded particles) and performing ATR infrared spectroscopic analysis (ATR-FTIR analysis) on the surface of each pre-expanded particle (expansion ratio: 40 times) under the following conditions to obtain an infrared absorption spectrum. Equipment: FTIR [Shimadzu Corporation, FTIR-8400S] connected to a single-reflection attenuated total reflection (ATR) measurement device [PIKE, MIRacle] ATR prism (high refractive index crystal type): Zinc selenide (ZnSe) Incident angle: 45° Measurement area: 4000cm -1 ~600cm -1 Detector: DLATGS Penetration depth: 1.66 Number of reflections: 1 Resolution: 4cm -1 Number of times: 20 Other: The infrared absorption spectrum measured without contact with the sample was used as the background, and processing that is not related to the measured spectrum was performed. In the ATR method, the intensity of the infrared absorption spectrum obtained by the measurement changes depending on the degree of contact between the sample and the high refractive index crystal. -1 The degree of contact between the sample and the high refractive index crystal is adjusted so that the absorbance is 0.05 to 0.10.

[0141] Here, when the surface of the pre-expanded particles was measured, the particle surface was brought into close contact with the ATR prism as it was.

[0142] From the infrared absorption spectrum obtained as above, -1 and absorbance at 2230cm -1The absorbance ratio was calculated (D2230 / D1600). In one embodiment of the present invention, ATR-FTIR measurement is performed on the surfaces of 10 random pre-expanded particles, and the minimum and maximum absorbance ratios are excluded. The arithmetic mean of the remaining 8 absorbance ratios is then used as the absorbance ratio.

[0143] The pre-expanded particles (expanded particles) used in the measurement of absorbance ratio were obtained by treating the expandable resin particles obtained in the examples and comparative examples described later in the following order of (1) to (3): (1) the expandable resin particles were placed in a pressurized expansion machine; (2) steam was then blown into the expansion machine at an inlet steam pressure of 0.09 MPa to 0.10 MPa, and the pressure inside the expansion machine was adjusted to a range of 0.01 MPa to 0.02 MPa, thereby setting the temperature inside the expansion machine to 100°C to 104°C, thereby expanding the expanded particles to a magnification of 40 times; (3) the obtained expanded particles were then cured at 25°C for 12 to 24 hours to obtain expanded particles to be used in the measurement of infrared absorption spectrum.

[0144] The method for producing the foamed molded article is as follows.

[0145] (Production of foamed molded products) The pre-expanded particles, which had a bulk ratio of 40 times and had been left at room temperature for a day, were molded in a molding machine (Daisen, KR-57) with a blowing steam pressure of 0.05 MPa and a heating time of 22 seconds to obtain a flat foamed molded product with a thickness of 20 mm, length of 400 mm, and width of 350 mm.

[0146] The obtained foamed molded articles were evaluated for the amount of styrene and ethylbenzene emitted, the average cell diameter of the surface layer, heat resistance, and the like, by the following methods.

[0147] (Method for measuring the amount of styrene and ethylbenzene emitted from foamed molded products) A sample piece of 0.025 g was cut out from the foamed molded product. The sample piece was placed in a pressure-resistant glass container with a volume of 20 ml and placed in a Shimadzu HS-10 (connected to a GC-2014). The storage conditions of the HS-10 were set to 60°C for 2 hours, and the styrene and ethylbenzene released at that time were collected. Each substance collected was measured using a Shimadzu gas chromatography GC-2014 (capillary column: GL Science Rtx-1, column temperature conditions: heating from 50°C to 70°C (heating rate 3°C / min), then heating from 70°C to 180°C (heating rate 10°C / min), carrier gas: helium) in the same manner as the measurement method for the styrene content in the expandable resin particles. Using the measured calibration curves for styrene and ethylbenzene, the amount of styrene and ethylbenzene emitted from the foamed molded product was quantified from the obtained results. The amounts of styrene and ethylbenzene emitted were shown as concentrations (ppm) in the gas contained in a pressure-resistant glass vessel containing a sample piece.

[0148] (Measurement of the average bubble diameter of the surface layer) The average chord length of each foamed bead of the foam molded article was measured using a photograph of the cut surface of the foam molded article projected in accordance with ASTM-D-2842-97. Specifically, in the photograph of the cut surface of the foam molded article projected, the average chord length was measured from the foamed beads present on a straight line of the cut surface of the surface layer of the foam molded article. In addition, 10 foamed beads present on the surface layer of the foam molded article were arbitrarily selected, and the average of the chord lengths of each of the foamed beads was taken as the final value (average chord length). In this specification, the average chord length thus obtained was taken as the average cell diameter of the surface layer of the foam molded article.

[0149] (Heat resistance evaluation) The heat resistance of the foam molded article was evaluated by (a) calculating the dimensional change rate of the foam molded article at 90° C. and (b) observing the swelling of the surface of the foam molded article, as described below.

[0150] The foamed molded body with a molding magnification of 40 times was dried at 60°C for 24 hours. Then, a sample piece with a length of 150, width of 150, and thickness of 20 (t) mm was cut out from the foamed molded body. The dimensions of the sample piece in the length direction and width direction were measured at three points each to obtain the initial dimension (D). Then, the foamed molded body was left in a dryer at 90°C for 168 hours, and after leaving it, the same measurement was performed to obtain the dimension (E) after drying at 90°C. The dimensional change rate was calculated using the following formula, and an absolute value of the dimensional change rate of 0.4 or less, that is, a dimensional change rate of -0.4% to 0.4%, was considered to be acceptable.

[0151] When the dimensional change rate is a positive value, it indicates that the initial (before drying) dimension (D) is larger than the dimension (E) after drying, i.e., the foamed molded product has shrunk, whereas when the dimensional change rate is a negative value, it indicates that the dimension (E) after drying is larger than the initial dimension (D), i.e., the foamed molded product has expanded.

[0152] Dimensional change rate (%) = ((D) - (E)) / (D) x 100 Absolute value of dimensional change rate is 0.4 or less: 〇 (good) Absolute value of dimensional change rate is over 0.4 and 0.5 or less: △ (pass) Absolute value of dimensional change rate exceeds 0.5: × (bad) (Examples 1 to 10, Comparative Examples 1 to 5) A 6 L autoclave equipped with a stirrer was charged with 110 parts by weight of water, 0.105 parts by weight of tribasic calcium phosphate, 0.0075 parts by weight of sodium α-olein sulfonate, and the polymerization initiator, chain transfer agent, flame retardant, and flame retardant assistant in the amounts shown in Table 1, and the contents were deoxidized to a gauge pressure of -0.06 MPa using a vacuum pump.

[0153] Then, the stirring of the raw materials by the stirrer was started, and the amounts of styrene monomer, alpha methylstyrene monomer and acrylonitrile monomer listed in Table 1 were charged into the autoclave, and these raw materials were stirred for another 30 minutes. Then, the first polymerization (first polymerization step) was carried out at the temperature (first polymerization temperature) and time (first polymerization time) listed in Table 1. Then, 5 parts by weight of normal rich butane (normal butane weight parts / isobutane weight parts=70 / 30) was charged into the autoclave. Next, the second polymerization (second polymerization step) was carried out at the temperature (second polymerization temperature) and time (second polymerization temperature) listed in Table 1. Then, the temperature inside the autoclave was cooled to 40° C., dehydrated, and further dried to obtain expandable resin particles. The above-mentioned various measurements and evaluations were carried out on the obtained expandable resin particles, and the results are shown in Tables 1 and 2.

[0154] The obtained expandable resin particles were pre-expanded by the method described above to obtain expanded particles, which were then molded in a mold by the method described above to obtain an expanded molded article with a size of 40 times.

[0155] The obtained expanded beads and expanded molded articles were subjected to the above-mentioned various measurements and evaluations. The results are shown in Tables 1 and 2. [Table 1] [Table 2] [Industrial Applicability]

[0156] According to one embodiment of the present invention, it is possible to provide expandable resin particles, pre-expanded particles (expanded particles), and foamed molded articles that have a low VOC content and can suppress the amount of VOC emission. Therefore, one embodiment of the present invention can be suitably used in the fields of automobiles and building materials.

Claims

1. Expandable resin particles comprising a base resin containing a styrene unit and an acrylonitrile unit as constituent units, and a blowing agent, The expandable resin particles are expanded, and the infrared absorption spectrum of the surface of the expanded particles is 2230 cm -1 and wavelength 1600 cm -1 The expandable resin particles are characterized in that the absorbance ratio D2230 / D1600 at 0.80 or more.

2. 2. The expandable resin particles according to claim 1, wherein the expandable resin particles have a styrene content of less than 20 ppm and an ethylbenzene content of 130 ppm or less.

3. 3. The expandable resin particles according to claim 1, wherein the weight average molecular weight is from 150,000 to 220,000.

4. In the base resin, (a) the content of the styrene unit is 55 parts by weight or more and 80 parts by weight or less, and the content of the acrylonitrile unit is 20 parts by weight or more and 45 parts by weight or less, and (b) The expandable resin particles according to any one of claims 1 to 3, characterized in that the total content of the styrene units and the acrylonitrile units is 100 parts by weight.

5. 5. The expandable resin particles according to claim 1, wherein the TH / TQ ratio is less than 1.

20.

6. 6. Expanded beads obtained by expanding the expandable resin beads according to claim 1.

7. A foamed molded article obtained by molding the foamed beads according to claim 6 in a mold.

8. 8. The foamed molded article according to claim 7, wherein the average cell diameter in the surface layer is 50 μm or more and less than 100 μm.

9. 9. The foamed molded article according to claim 7, wherein the amount of styrene emitted is 2 ppm or less and the amount of ethylbenzene emitted is less than 15 ppm.

10. A method for producing expandable resin particles, comprising the steps of: a copolymerization step of copolymerizing monomers including a styrene monomer and an acrylonitrile monomer; and a blowing agent impregnation step of impregnating the obtained copolymer with a blowing agent, The copolymerization step includes a first polymerization step and a second polymerization step which are successively performed at different polymerization temperatures, In the first polymerization step, a polymerization initiator including a polymerization initiator (X) having a 10-hour half-life temperature of 74° C. or more and 94° C. or less is used, The polymerization initiator (X) contains benzoyl peroxide, The expandable resin particles have a TH / TQ ratio of less than 1.20; A method for producing expandable resin particles, characterized in that a polymerization initiator containing a polymerization initiator (Y) having a 10-hour half-life temperature of 90°C or more and 100°C or less is used in the second polymerization step.

Citation Information

Patent Citations

  • JP1971021449Y1

  • Swelling synthetic resin thermoplastic grain, manufacture thereof and utilization thereof

    JP1985219032A

  • Foamed synthetic resin thermoplastic particle and manufacture

    JP1986040335A

  • Polystyrene resin particle for foaming

    JP1992292610A

  • Foamable styrenic resin particle and method for producing the same

    JP2010195936A