Compact polyurethane
The use of a boron-based fluorine-containing Lewis acid catalyst in polyurethane production addresses moisture sensitivity and enhances impact resistance and tensile strength in compact polyurethanes for fiber composites, reducing bubble formation and improving hydrophobicity.
Patent Information
- Application Number
- JP2021536085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-20
- Filing Date
- 2019-12-19
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-12-19
AI Technical Summary
Existing polyurethanes used in fiber composites are sensitive to moisture, leading to air bubbles and defects, and lack the combination of high impact resistance, tensile strength, and hydrophobicity required for compact, high-density applications.
A polyisocyanate composition and a polyol composition using a boron-based fluorine-containing Lewis acid catalyst to produce compact polyurethanes with a density of 850 g/l or more, featuring polyether polyols with a functionality of 3 to 6 and a molecular weight of 50 to 150 g/mol, ensuring high primary hydroxyl groups and hydrophobicity.
The solution results in compact polyurethanes with improved impact resistance, tensile strength, and reduced bubble formation, suitable for high-humidity environments, making them suitable for fiber composites.
Smart Images

Figure 0007553449000007 
Figure 0007553449000013 
Figure 0007553449000011
Abstract
Description
[Technical field]
[0001] The present invention relates to a compact polyurethane having a density of 850 g / l or more, which is obtainable or obtainable by reacting a polyol composition comprising at least the following components: i) a polyisocyanate composition; ii) a polyol composition, which comprises at least one polyether polyol (ii.1), which is obtainable or obtainable by reacting (ii.1.1) a polyol starter having a functionality of 3 to 6 with (ii.1.2) propylene oxide and / or butylene oxide, in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3) and optionally further auxiliaries and / or additives (ii.1.4), wherein the polyether polyol (ii.1) has an equivalent molecular weight of 50 to 150 g / mol. The present invention further relates to a process for producing such a compact polyurethane, and to a compact polyurethane obtained or obtainable by this process. The present invention further relates to the use of such a compact polyurethane having a density of 850 g / l or more for the production of a fiber composite. The present invention also relates to a corresponding fiber composite material, and to a process for producing such a fiber composite. [Background technology]
[0002] Polyurethanes (PU) are produced by numerous processing operations and are used in numerous different applications (Guenter Oertel, Polyurethane Handbook: Chemistry-Raw Materials-Processing-Application-Properties-1. January 1994). Rigid, compact and / or fiber-reinforced polyurethanes are produced from highly functional polyols with high hydroxyl numbers (US 3,464,935 A) and are highly crosslinked polymers. They should generally have long processing times ranging from 30 min to 240 min, excluding the use of very reactive starting materials. With regard to the properties of the materials, high impact resistance combined with high hardness, tensile and flexural strength is required, a combination of properties that is difficult to achieve. Furthermore, it has been found that compact polyurethanes produced in environments with high atmospheric humidity using conventional alkylene oxide-based polyether polyols or OH-terminated polyesterols (polyester polyols) have large bubbles and defects on the part surface, especially when fiber composites are produced under such conditions. The cause of this defect is the presence of moisture in the air and on the fibers, which leads to undesirable reactions with the polyurethane reaction mixture, and for this reason, in particular, it is currently preferred to use resins such as epoxies or unsaturated polyester / vinyl esters instead of polyurethanes in the corresponding processes.
[0003] With regard to the desired properties, catalysts are typically used in the preparation of the required polyether polyols and polyesterols. On an industrial scale, basic catalysts are used for the preparation of polyetherols, with KOH being the most widely used (M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, p. 119 ff.). EP 1 803 756 A1 describes polyols obtained by reaction of polyfunctional starters with propylene oxide; no catalysts for this reaction are mentioned. The reaction product of sorbitol (initiator) with propylene oxide is produced. When no cationic catalysts are used, the resulting polyols have mainly secondary hydroxyl groups, compared to polyols with a high proportion of primary hydroxyl groups as a result of using Lewis acids as catalysts, resulting in a different profile in terms of reactivity and hydrophobicity. Moreover, the polyols used in EP 1 803 756 A1 have high viscosities, for example in the range of about 10 000 MPas (25 ° C), which results in a much higher viscosity of the prepolymers again. Such high viscosity resins are disadvantageous for use as fiber composites; the flow rate during impregnation of the fibers is inversely proportional to the viscosity (Darcy's law) (see M. Neitzel, P. Mitschang, Handbuch Verbundwerkstoffe [Handbook Composite Materials], Carl Hanser Verlag, 2004, p. 164). The polyurethanes produced from the polyols of EP 1 803 756 A1 have fundamental differences in terms of their morphology compared to polyurethanes produced with polyols having more primary hydroxyl groups. For example, it is expected that the polymers produced according to EP 1 803 756 A1 consist of highly functional regions (former prepolymers) that are loosely bonded to each other with a low level of crosslinking as a result of the prepolymer mixture used.
[0004] Polyetherols are known to be prepared by Lewis acid or superacid catalyzed alkoxylation. The problem with this reaction regime is the formation of significant amounts of undesirable by-products in the form of cyclic ethers that do not carry hydroxyl groups and therefore do not participate in the formation of polyurethanes, but are responsible for the unpleasant odor of the product (M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, pp. 245-247).
[0005] Polyetherols are known that use tris(pentafluorophenyl)borane (TPB) as an alkoxylation catalyst instead of the commonly used catalysts from the group of alkali metals or amines (T. Miyajima et al., Polymer Journal (2015) 47, 771-778). When propylene oxide is used, these polyols have a high content of primary hydroxyl groups and are therefore much more reactive than commonly used polyetherols with the same composition.
[0006] WO 2016 / 064698 A1 describes the preparation of polyols with high molecular weights of more than 2500 g / mol and high contents of primary hydroxyl groups using a dual catalyst in a two-stage alkoxylation process.
[0007] US 6,531,566 B1 relates to polyoxyalkylene polyols or monools having a high content of primary hydroxyl groups and to their use in the preparation of thermosets, in which in the examples it is disclosed that glycerol-propylene oxide adducts are reacted with further propylene oxide by addition of tris(pentafluorophenyl)borane, which are then reacted with isocyanates to obtain urethane foams or polyurethane elastomers.
[0008] US 6,831,112 B2 describes polyether polyols prepared with ethylene oxide (EO) and their use in the production of rigid polyurethane foams. In the examples, propylene oxide-glycerol adducts are reacted with additional propylene oxide (PO) and ethylene oxide in the presence of tris(pentafluorophenyl)borane and used to produce polyurethane elastomers and foams.
[0009] JP 2014-167105 A discloses an example of a glycerol-initiated polyol propoxylated only with tris(pentafluorophenyl)borane (TPB) and having a hydroxyl number (OHN) of 270 mg KOH / g.
[0010] US2003 / 0100623 A1 discloses a polyol based on sorbitol (+9 PO and 1 EO) with an OHN of 450 mg KOH / g, which is alkoxylated exclusively with TPB, using almost exclusively propylene oxide, and similar polyols based on glycerol, pentaerythritol, also with the same OHN. In all examples, the TPB catalyst is subsequently removed. This document also describes the use for producing water-blown rigid foams. Thus, polyurethanes are described that both expand and crosslink in the manufacturing process. In this case, the crosslinker must be miscible with a certain amount of water and other hydrophilic polyols, resulting in a material that is entirely hydrophilic, but in addition still brittle.
[0011] Thus, according to the prior art, TPB catalysis is mainly used for the production of long-chain polyetherols, the purpose of which is to increase their reactivity. These polyols are used in combination with water as blowing agent for the production of foams. In particular, by using EO, the corresponding polyols must have sufficient hydrophilicity for water to mix with them. The known polyurethanes crosslinked using polyols catalyzed with TPB are rigid foams, which are not known for their good impact resistance.
[0012] The use of TPB-catalyzed polyols for the production of compact rigid polyurethanes does not seem promising due to their hydrophilicity. The increased reactivity is not attractive for compact polyurethanes and fiber composites, which require long processing times in addition to high hydrophobicity. Therefore, the use of TPB polyols for the production of highly crosslinked hydrophobic compact polyurethanes was not obvious. [Prior art documents] [Patent documents]
[0013] [Patent Document 1] US 3,464,935 A [Patent Document 2] EP 1 803 756 A1 [Patent Document 3] WO 2016 / 064698 A1 [Patent Document 4] US 6,531,566 B1 [Patent Document 5] US 6,831,112 B2 [Patent Document 6] JP 2014-167105 A [Patent Document 7] US2003 / 0100623 A1 [Non-patent literature]
[0014] [Non-Patent Document 1] Guenter Oertel,Polyurethane Handbook:Chemistry-Raw Materials-Processing-Application-Properties-1.January 1994 [Non-Patent Document 2] M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, p.119 ff. [Non-Patent Document 3] M. Neitzel, P. Mitschang, Handbuch Verbundwerkstoffe [Handbook Composite Materials], Carl Hanser Verlag, 2004, 164 pages [Non-Patent Document 4] M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, pp. 245-247 [Non-Patent Document 5] T. Miyajima et al., Polymer Journal (2015) 47, pp. 771-778 Summary of the Invention [Problem to be solved by the invention]
[0015] The object of the present invention was to provide a crosslinked, compact PU material, when the crosslinking agent is water-repellent and miscible with hydrophobic but not hydrophilic polyols, which should be processable to obtain a bubble-free, compact product even in the case of very high atmospheric humidity, and at the same time be impact-resistant and not brittle, like, for example, rigid foams. [Means for solving the problem]
[0016] The objective is to have at least the following components: i) Polyisocyanate composition ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) A polyol starter having a functionality of 3 to 6 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, a polyol composition obtained or obtainable by reacting This is achieved by compact polyurethanes having a density of 850 g / l or more which are obtained or can be obtained by reacting
[0017] All figures for the density of compact polyurethanes refer in each case to the pure polyurethane resin without taking into account the filler, the density being determined by the flotation method in accordance with DIN EN ISO 1183-1. If fillers or fibers are used in accordance with the instructions under (ii.1.4), the reported density of the polyurethanes according to the invention varies depending on the amount and density of the fillers used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Compact polyurethane According to the invention, the polyol starter used according to (ii.1.1) is at least one polyol having a functionality of 3 to 6, preferably 3 or 4, and according to the invention also mixtures of two or more of these polyols are encompassed. "Polyols having a functionality of 3 to 6" is understood to mean polyols having, on average, 2.8 to 3.0, or 3.8 to 4.0, or 4.8 to 5.0, or 5.8 to 6.0 hydroxyl groups per molecule. Similarly, "polyols having a functionality of 3 or 4" is understood to mean polyols having, on average, 2.8 to 3.0, or 3.8 to 4.0 hydroxyl groups per molecule. In practice, there are deviations from the nominal functionality, since various side reactions during polyol synthesis can actually result in lower functionality than the nominal functionality (M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, pp. 67-75). In the range of equivalent molecular weights of 50-150 g / mol, it is assumed that the functionality is very close to 3 or 4 or 5 or 6, preferably very close to 3 or 4.
[0019] The equivalent molecular weight (EMW) is defined as the quotient of the molecular weight of the polyether polyol (M(polyether polyol)) and the functionality of the polyether polyol (F): EMW = M (polyether polyol) / F [g].
[0020] For example, for 1 mole of glycerol alkoxylated with 1 mole of propylene oxide, EMW=(150.2 g / mol) / (3 mol -1 ), an EMW of 50 g / eq is obtained.
[0021] In one embodiment of the compact polyurethane, the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (C6F5)3B, and a mixture of BF3 and (C6F5)3B, more preferably tris(pentafluorophenyl)borane.
[0022] The use of a boron-based, fluorine-containing Lewis acid catalyst (ii.1.3) in the reaction of a polyol starter (ii.1.1) having a functionality of 3 to 6 with propylene oxide and / or butylene oxide (ii.1.2) can obtain the result that more than 50% of the hydroxyl groups present in the polyether polyol (ii.1) are primary hydroxyl groups, i.e. that a maximum of 50% of the hydroxyl groups formed are secondary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1).
[0023] In one embodiment of the compact polyurethane, the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g.
[0024] In one embodiment of the compact polyurethane, the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0025] For example, when m, n, and o are 6 in the triol of formula (I), the hydroxyl number (OHN) is 405 mg KOH / g, or an equivalent molecular weight of 134 g. When l, m, n, and o are 1 in the triol of formula (I), an OHN of 1256 mg KOH / g or an equivalent molecular weight of 45 g is obtained for the TMP.
[0026] In one embodiment of the compact polyurethanes, the polyol starter (ii.1.1) of the polyether polyol (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I): [ka] (In the formula, l, m, n and o each independently represent an integer ranging from 1 to 6).
[0027] In one embodiment of the compact polyurethane, l, m, n and o of the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, preferably l, m, n and o are all 1. In one embodiment of the compact polyurethane, the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0028] In one embodiment of the compact polyurethane, the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or only end groups based on butylene oxide. In one embodiment of the compact polyurethane, the polyether polyol (ii.1) has only end groups based on propylene oxide and / or only end groups based on butylene oxide, and does not contain any groups based on ethylene oxide. In one embodiment of the compact polyurethane, the polyether polyol (ii.1) is prepared exclusively by reaction of a polyol starter, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reaction of the triol (ii.1.1) with propylene oxide, without further alkylene oxide. Even if no ethylene oxide is used or only propylene oxide and / or butylene oxide are used, the use of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) according to the invention gives at least one polyether polyol (ii.1) having 50% or more primary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1), i.e. up to 50% of the hydroxyl groups in the polyether polyol (ii.1) are secondary hydroxyl groups.
[0029] In one embodiment of the compact polyurethane, the polyether polyol (ii.1) is based on a triol other than glycerol, preferably on the triol (ii.1.1) of formula (I) above; preferably, the polyether polyol (ii.1) has the formula (II): [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q and r are each independently zero or an integer ranging from 1 to 6, preferably zero or an integer ranging from 1 to 4, more preferably zero or an integer ranging from 1 to 3; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group. 1 , X 2 and X 3 are each a -CH2-CH(CH3)-O- group. Preferably, l, m, n and o are all 1, and p, q and r are independently a value from 0 to 2.
[0030] In one embodiment of the compact polyurethane, the reaction of (ii.1.1) with (ii.1.2) is carried out solely in the presence of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) without the use of an additional alkoxylation catalyst.
[0031] In one embodiment of the compact polyurethane, the reaction of (ii.1.1) with (ii.1.2) is carried out in a single synthetic step solely in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), which can be optionally removed after synthesis of the polyetherol but preferably remains in the product.
[0032] At least one polyether polyol (ii.1) is preferably present in the polyol composition (ii) in a range of 25% to 95% by weight, based on the total weight of the polyol composition (ii). In one embodiment of the compact polyurethane, the polyether polyol (ii.1) is used in a range of 10% to 50% by weight, based on the total weight of the polyisocyanate composition (i) and the polyol composition (ii) being 100% by weight. The polyisocyanate composition (i) and the polyol composition (ii) are preferably used in a ratio such that the molar ratio of the sum of the functionalities of the polyol composition (ii) used to the sum of the functionalities of the polyisocyanate composition (i) used is in the range of 0.7 to 2.1. Preferably, this ratio is in the range of 0.8 to 1.2. Here, a ratio of 1:1 corresponds to an isocyanate index of 100.
[0033] Surprisingly, the use of polyols produced by propoxylation from triols, particularly TMP, catalyzed by boron-based fluorine-containing Lewis acid catalysts, particularly tris(pentafluorophenyl)borane, has been shown to produce 60 kJ / m 2 Above 70kJ / m 2 It was found that compact polyurethanes with improved impact resistance of more than 80 MPa were obtained. Moreover, the Shore D hardness was comparable to that of polyurethanes produced using different polyols produced under KOH catalysis. Surprisingly, compact polyurethanes produced using polyols produced by propoxylation from triols, especially TMP, under catalysis with boron-based fluorine-containing Lewis acid catalysts, especially tris(pentafluorophenyl)borane, had significantly improved tensile strengths of more than 80 MPa.
[0034] It has been found in winding tests that the use of compact polyurethanes produced with polyols produced by propoxylation from triols, especially TMP, under catalysis with boron-based fluorine-containing Lewis acid catalysts, especially tris(pentafluorophenyl)borane, in the production of fiber composites gives significantly better results in terms of avoiding the formation of undesirable bubbles. In winding tests, it was found that when the polyols according to the invention were used, there was very little, if any, bubble formation during the production of the corresponding components, despite a high atmospheric humidity of 85%, while the use of polyols produced under catalysis with KOH caused severe foaming, i.e. the formation of undesirable bubbles to a great extent.
[0035] According to the present invention, a polyisocyanate composition is used as (i). Here, the polyisocyanate composition contains at least one polyisocyanate. Also, according to the present invention, the polyisocyanate composition may contain two or more polyisocyanates.
[0036] The at least one polyisocyanate is preferably at least one diisocyanate, more preferably selected from the group consisting of aliphatic, cycloaliphatic, araliphatic and aromatic diisocyanates, and mixtures of two or more of these diisocyanates. Specific examples include the following aromatic diisocyanates: toluene 2,4-diisocyanate, mixtures of toluene 2,4- and 2,6-diisocyanate, diphenylmethane 4,4'-, 2,4'- and / or 2,2'-diisocyanate (MDI), mixtures of diphenylmethane 2,4'- and 4,4'-diisocyanate, liquid diphenylmethane 4,4'- and / or 2,4-diisocyanates modified with urethanes, carbodiimides or uretoimines, 4,4'-diisocyanatodiphenylethane, mixtures of monomeric methane diphenyl diisocyanate and higher polycyclic homologues of methane diphenyl diisocyanate (polymeric MDI), naphthylene (1,2) and 1,5-diisocyanate, or prepolymers of these isocyanates with polyols or isocyanates with isocyanate-reactive components. The aliphatic diisocyanates used are customary aliphatic and / or cycloaliphatic diisocyanates, such as, for example, tri-, tetra-, penta-, hexa-, hepta-, and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethylbutylene 1,4-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4 and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, dicyclohexylmethane 4,4'-, 2,4'- and / or 2,2'-diisocyanate, or prepolymers of these isocyanates. Isocyanate compositions containing MDI are preferred.
[0037] The diisocyanates and polyisocyanates (i) can also be used in the form of polyisocyanate prepolymers. These polyisocyanate prepolymers can be obtained by reacting the above polyisocyanate (i) in excess with a compound having at least two isocyanate-reactive groups at a temperature of, for example, 30 to 100°C, preferably about 80°C, to obtain a prepolymer. The NCO content of the polyisocyanate prepolymer of the present invention is preferably 15% by mass to 33% by mass of NCO, particularly preferably 25% by mass to 30% by mass of NCO.
[0038] The polyisocyanate composition (i) has a viscosity at 25°C in the range of 50 mPas to 1000 mPas, preferably in the range of 50 mPas to 500 mPas, and more preferably in the range of 50 mPas to 300 mPas.
[0039] In one embodiment of the compact polyurethane, the polyol composition ii) comprises one or more further polyols, where the further polyol(s) are only polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation. The residual amount of alkali metal salts in the polyol composition ii) is n<0.5 ppm, based on the total weight of the polyol composition ii).
[0040] In one embodiment of the compact polyurethane, the further polyol(s) is / are selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and boron-containing Lewis acids, optionally polyesterols (polyester polyols) and optionally alkoxylated polyetherols (polyether polyols) in the presence of chain extenders.
[0041] Preferably, all polyols of polyol composition (ii) are prepared without the use of basic or amine catalysts. In a preferred embodiment of the compact polyurethane, polyol composition (ii) does not contain an amine or basic catalyst.
[0042] Preferably, the polyol composition (ii) comprises, in addition to at least one polyether polyol (ii.1), one or more further polyols, where the further polyol(s) are selected from the group of hydroxyl-functionalized hydrophobic compounds, which preferably have a hydrocarbon group with more than 6, particularly preferably more than 8 and less than 100, in particular more than 10 and less than 50 carbon atoms, and one or more hydroxyl groups. The compound used having at least two isocyanate-reactive groups may be, for example, a polyetherol or polyesterol. The compound used having at least two isocyanate-reactive groups is preferably a polyetherol or polyesterol containing secondary OH groups, for example polypropylene oxide. Here, the polyetherol or polyesterol preferably has a functionality of 2 to 4, particularly preferably 2 to 3, and a proportion of secondary OH groups of at least 50%, preferably at least 75%, in particular at least 85%. The compounds used, which have on average at least 1.5 isocyanate-reactive hydrogen atoms per molecule, can be all compounds with isocyanate-reactive hydrogen atoms known in polyurethane chemistry.
[0043] Examples of oleochemical polyols are described, inter alia, in M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, Chapter 17.1. As such hydroxyl-functionalized hydrophobic compounds, hydroxyl-functionalized oleochemical compounds, i.e. oleochemical polyols, are preferably used. In one embodiment of oleochemical polyols, castor oil (triglyceride mixtures) and its derivatives are used. Preferred derivatives are reaction products with alkylene oxides or ketone-formaldehyde resins. The latter compounds are sold, for example, by Covestro AG under the name Desmophen® 1150. Another group of oleochemical polyols that are preferably used can be obtained by ring-opening of epoxidized fatty acid esters, simultaneous reaction with alcohols and, optionally, subsequent further transesterification. The introduction of hydroxyl groups into fats and oils is mainly achieved by epoxidation of the olefinic double bonds present in these products and subsequent reaction of the resulting epoxide groups with mono- or polyhydric alcohols. Here, the epoxide ring is structured with a hydroxyl group or, in the case of polyfunctional alcohols, with a large amount of OH groups. Since fats and oils are mainly glycerol esters, the above reaction is accompanied by a parallel transesterification reaction. The resulting compounds preferably have a molecular weight in the range of 500 to 1500 g / mol. Products of this type are offered, for example, by BASF (under the trademark Sovermol®) or Altropol Kunststoff GmbH (under the trademark Neukapol®).
[0044] Furthermore, the polyol composition (ii) can contain polyols of the type known to those skilled in the art, for example polybutadienes based on free-radical or anionic polymerized butadiene, acrylate polyols, polysiloxane polyols, polyols obtainable by Mannich condensation, for example aromatic polyols based on bisphenol A, resorcinol, novolak or melamine. Further possibilities are polytetrahydrofuran or polycaprolactone, or copolymers of these starting materials; further possibilities are polymer polyols, for example based on triols, and particles based on polystyrene, styrene / acrylonitrile. All these types of polyols are known, for example, from M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, pp. 67-75.
[0045] In one embodiment of the compact polyurethanes, the polyol composition ii) optionally comprises polyetherols prepared from epoxides, such as, for example, propylene oxide and / or ethylene oxide and / or butylene oxide, or from tetrahydrofuran, using catalysts, such as aliphatic alcohols, phenols, amines, carboxylic acids, starter compounds with active hydrogen atoms, such as water, or compounds based on natural substances, such as sucrose, sorbitol or mannitol, including basic catalysts or double metal cyanide catalysts, as described, for example, in WO 2006 / 034800 A1, EP 0090444 B1 or WO 05 / 090440 A1.
[0046] In one embodiment of the compact polyurethane, the polyol composition ii) comprises polyesterols, polythioether polyols, polyesteramides, hydroxyl-containing polyacetals and / or hydroxyl-containing aliphatic polycarbonates, for example prepared from aliphatic or aromatic dicarboxylic acids and polyhydric alcohols, optionally preferably in the presence of an esterification catalyst. Other usable polyols are described, for example, in "Kunststoffhandbuch, Band 7, Polyurethane" [Plastics Handbook, Volume 7, Polyurethanes], Carl Hanser Verlag, 3rd Edition, 1993, Chapter 3.1. The polyester polyols can be prepared, for example, from organic dicarboxylic acids having 2 to 12 carbon atoms, preferably aliphatic dicarboxylic acids having 4 to 6 carbon atoms, and polyhydric alcohols, preferably diols, having 2 to 12 carbon atoms, preferably 2 to 6 carbon atoms. Examples of useful dicarboxylic acids include succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, maleic acid, fumaric acid, phthalic acid, isophthalic acid, and terephthalic acid. Here, the dicarboxylic acids may be used alone or in mixtures with each other. It is also possible to use the corresponding dicarboxylic acid derivatives, such as dicarboxylic acid esters of alcohols having 1 to 4 carbon atoms or dicarboxylic acid anhydrides, instead of the free dicarboxylic acids. It is preferable to use a dicarboxylic acid mixture of succinic acid, glutaric acid, and adipic acid in a ratio of, for example, 20 to 35:35 to 50:20 to 32 parts by weight, and it is particularly preferable to use adipic acid. Examples of dihydric and polyhydric alcohols, especially diols, include ethanediol, diethylene glycol, propane-1,2- and -1,3-diol, dipropylene glycol, butane-1,4-diol, butane-1,2-diol, pentane-1,5-diol, hexane-1,6-diol, decane-1,10-diol, glycerol and trimethylolpropane. It is preferred to use ethanediol, diethylene glycol, butane-1,4-diol, pentane-1,5-diol and hexane-1,6-diol.It is also possible to use polyester polyols which derive from lactones, such as ε-caprolactone, or from hydroxycarboxylic acids, such as ω-hydroxycaproic acid.
[0047] The polyester polyols can be prepared by polycondensation of organic, for example aromatic, preferably aliphatic, polycarboxylic acids and / or derivatives with polyhydric alcohols without catalyst or preferably in the presence of an esterification catalyst, suitably in an atmosphere of an inert gas, for example nitrogen, carbon monoxide, helium or argon, in the melt at temperatures of 150-250° C., preferably 180-220° C., optionally under reduced pressure, up to the desired acid number, preferably less than 10, particularly preferably less than 2. In a preferred embodiment, the esterification mixture is polycondensed at the abovementioned temperatures under standard pressure and then at a pressure of less than 500 mbar, preferably 50-150 mbar, up to an acid number of 80-30, preferably 40-30. Examples of esterification catalysts which can be used include iron, cadmium, cobalt, lead, zinc, antimony, magnesium, titanium and tin catalysts in the form of metals, metal oxides or metal salts. However, the polycondensation can also be carried out in the liquid phase in the presence of diluents and / or entraining agents, such as benzene, toluene, xylene or chlorobenzene, to remove the water of condensation by azeotropic distillation.To prepare the polyester polyols, organic polycarboxylic acids and / or derivatives and polyhydric alcohols are polycondensed, advantageously in a molar ratio of 1:1-1.8, preferably 1:1.05-1.2.
[0048] Preferably, the polyester polyols obtained have a functionality of 2 to 4, in particular 2 to 3, and a number average molecular weight of 480 to 3000 g / mol, preferably 1000 to 3000 g / mol.
[0049] In one embodiment of the compact polyurethanes, the polyol composition ii) optionally comprises a chain extender. The chain extenders used are preferably substances having a molecular weight of less than 450 g / mol, particularly preferably from 60 to 400 g / mol, the chain extenders having two isocyanate-reactive hydrogen atoms and the crosslinkers having three isocyanate-reactive hydrogen atoms. These can preferably be used individually or in the form of a mixture. It is preferable to use diols and / or triols having a molecular weight of less than 400, particularly preferably from 60 to 300, in particular from 60 to 150. Useful examples of starter molecules include aliphatic, cycloaliphatic and / or araliphatic diols having 2 to 14, preferably 2 to 10, carbon atoms, such as monoethylene glycol, propane-1,3-diol, decane-1,10-diol, 1,2-, 1,3-, 1,4-dihydroxycyclohexane, diethylene glycol, dipropylene glycol, butane-1,4-diol, butane-1,2-diol, hexane-1,6-diol and bis(2-hydroxyethyl)hydroquinone, triols such as 1,2,4-, 1,3,5-trihydroxycyclohexane, glycerol and trimethylolpropane, and low molecular weight hydroxyl-containing polyalkylene oxides based on ethylene oxide and / or 1,2-propylene oxide, and the aforementioned diols and / or triols. As chain extenders it is particularly preferable to use monoethylene glycol, butane-1,4-diol, butane-1,2-diol, diethylene glycol, glycerol or mixtures thereof.
[0050] If chain extenders and / or crosslinkers are used, the proportion of chain extenders and / or crosslinkers is typically 1-50% by weight, preferably 2-20% by weight, based on the total weight of component (ii). However, it is also possible here to omit the chain extenders or crosslinkers. However, the addition of chain extenders, crosslinkers or optionally mixtures thereof can prove advantageous for modifying the mechanical properties, for example the hardness.
[0051] Auxiliaries and / or additives (ii.1.4) can also be used optionally. Any auxiliaries and additives known for the production of polyurethanes can also be used here. Examples of the above include, for example, surface-active substances, blowing agents, foam stabilizers, cell regulators, release agents, fillers, dyes, pigments, flame retardants, hydrolysis stabilizers, fungistatic and bacteriostatic substances. These substances are known and are described, for example, in "Kunststoffhandbuch, Band 7, Polyurethane" [Plastics Handbook, Volume 7, Polyurethanes], Carl Hanser Verlag, 3rd edition, 1993, chapters 3.4.4 and 3.4.6 to 3.4.11.
[0052] As additives, conventional polyurethane catalysts can be used as catalysts (ii.1.4), which significantly accelerate the reaction of compounds (b) containing isocyanate-reactive hydrogen atoms with di- and polyisocyanates (a). Examples of conventional catalysts which can be used for the preparation of polyurethanes include: amidines such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, tertiary amines such as triethylamine, tributylamine, dimethylbenzylamine, dimethylcyclohexylamine, N-methyl-, N-ethyl- and N-cyclohexylmorpholine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutanediamine, N,N,N',N'-tetramethylhexanediamine, pentamethyldiethylenetriamine, tetramethyldiaminoethyl ether, bis(dimethylaminopropyl)urea, dimethylpiperazine, 1,2-dimethylimidazole, 1-azabicyclo[3.3.0]octane, preferably 1,4-diazabicyclo[2.2.2]octane, and alkanolamine compounds such as triethanolamine, triisopropanolamine, N-methyl- and N-ethyldiethanolamine and dimethylethanolamine. It is also possible to use organometallic compounds, preferably organotin compounds, such as tin(II) salts of organic carboxylic acids, such as tin(II) acetate, tin(II) octoate, tin(II) ethylhexoate and tin(II) laurate, and dialkyltin(IV) salts of organic carboxylic acids, such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate and dioctyltin diacetate, and also bismuth carboxylates, such as bismuth(III) neodecanoate, bismuth 2-ethylhexanoate and bismuth octanoate, or mixtures thereof. The organometallic compounds can be used alone or, preferably, in combination with strongly basic amines. When component (ii.1.4) is an ester, it is preferred to use only amine catalysts. It is also possible to use so-called latent catalysts, known to the skilled artisan, which have little catalytic activity even at room temperature and are activated, for example, only by increasing the temperature.Examples of these catalysts can be found, inter alia, in DE 102008021980 A1 or WO 2009 / 115540 A1.
[0053] The catalyst (ii.1.4) can be used as a catalyst or a combination of catalysts, for example in a concentration of 0.001% to 5% by weight, in particular 0.05% to 2% by weight, based on the weight of component (ii).
[0054] In a further preferred embodiment, the auxiliaries and additives (ii.1.4) can include basic catalysts that are not conventional polyurethane-forming catalysts. These include, for example, catalysts that catalyze the formation of polyisocyanurates. Polyisocyanurate catalysts include alkali metal carboxylates. These preferably include formates and acetates, especially acetates, such as sodium acetate and potassium acetate.
[0055] A further type of additive (ii.1.4) are deaerators, which are known to the person skilled in the art and are described, for example, in Thomas Brock, Michael Groteklaes, Peter Mischke: Lehrbuch der Lacktechnologie [Textbook of Paint Technology]. Ed.: Ulrich Zorll, 2nd edition, Vincentz Verlag, Hanover 2000, ISBN 978-3-87870-569-7, Chapter 2.4.2.1, Entschaeumer und Entluefter [Defoamers and Deaerators], p. 169 f.
[0056] In a further embodiment, it is also possible to add to the polyisocyanate composition (i) such components (ii-1.4) which do not contain isocyanate-reactive hydrogen atoms.
[0057] For the purposes of the present invention, the term "polyurethanes" includes all known polyisocyanate polyaddition products. These include addition products derived from isocyanates and alcohols, and also modified polyurethanes which may contain isocyanurate, allophanate, urea, carbodiimide, uretonimine, biuret structures, and other isocyanate addition products. These polyurethanes of the present invention include in particular solid polyisocyanate polyaddition products, such as thermosets, and foams, in particular polyurethane coatings, which have an apparent density of more than 850 g / l based on polyisocyanate polyaddition products.
[0058] In a further preferred embodiment, the polyurethane is a solid polyurethane, preferably having a density of more than 850 g / l, preferably between 850 and 1400 g / l, particularly preferably between 850 and 1100 g / l. Here, the solid polyurethane is obtained without the addition of a blowing agent. In the context of the present invention, small amounts of blowing agents, for example water present in the polyol as a result of the production process, are not to be construed as constituting the addition of a blowing agent here. The reaction mixture for producing compact polyurethanes preferably comprises less than 0.2% by weight, particularly preferably less than 0.1% by weight, in particular less than 0.05% by weight of water. The solid polyurethane preferably comprises a filler, in particular a fibrous filler. Suitable fillers are described below under (ii.1.4).
[0059] The reaction mixture is preferably prepared in a two-component process. For this purpose, a polyisocyanate composition i) and a polyol composition ii) are combined. The polyisocyanate composition comprises an isocyanate and optionally a non-isocyanate-reactive component of component (ii.1.4). Here, the composition of the polyol composition is preferably adjusted to have a viscosity at 25 ° C. of preferably less than 2000 mPas. Here, the viscosity measurement is based on DIN 53019-1 to 3. Here, the viscosity can be adjusted in particular via the selection of the compounds of component (ii.1.4) and the amount used thereof. In particular, the viscosity of the polyol component can be reduced by using substances known to the skilled person, such as acrylates or plasticizers.
[0060] The reaction mixture is cured at a temperature above 80°C, preferably between 80°C and 200°C.
[0061] Method for producing compact polyurethanes with densities of 850 g / l and above The present invention further comprises a method for producing a composition comprising at least the following components: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, a polyol composition obtained or obtainable by reacting The present invention relates to a method for producing a compact polyurethane having a density of 850 g / l or more, the method comprising the steps of:
[0062] The comments already made in the section relating to the compact polyurethanes also apply to the polyisocyanate composition (i).
[0063] In one embodiment of the method for producing a compact polyurethane having a density of 850 g / l or more, the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0064] In one embodiment of the method for producing a compact polyurethane having a density of 850 g / l or more, the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (CF5)3B and a mixture of BF3 and (CF5)3B, more preferably tris(pentafluorophenyl)borane. The use of the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) in the reaction of polyol starters (ii.1.1) having a functionality of 3 to 6 with propylene oxide and / or butylene oxide (ii.1.2) results in more than 50% of the hydroxyl groups present in the polyether polyol (ii.1) being primary hydroxyl groups, i.e. up to 50% of the hydroxyl groups formed being secondary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1).
[0065] In one embodiment of the process for the preparation of compact polyurethanes having a density of 850 g / l or more, the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range from 400 to 1200 mg KOH / g, more preferably in the range from 450 to 1200 mg KOH / g, more preferably in the range from 450 to 1000 mg KOH / g.
[0066] In one embodiment of the process for producing compact polyurethanes having a density of 850 g / l or more, the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0067] In one embodiment of the process for the preparation of compact polyurethanes having a density of 850 g / l or more, the polyether polyol (ii.1) is used in an amount of 10% to 50% by weight, based on the total weight of the polyisocyanate composition (i) and the polyol composition (ii) being 100% by weight. The polyisocyanate composition (i) and the polyol composition (ii) are preferably used in a ratio such that the molar ratio of the sum of the functionalities of the polyol composition (ii) used to the sum of the functionalities of the polyisocyanate composition (i) used is in the range of 0.7 to 2.1. Preferably, this ratio is in the range of 0.8 to 1.2. Here, a ratio of 1:1 corresponds to an isocyanate index of 100.
[0068] In one embodiment of the process for the preparation of compact polyurethanes having a density of 850 g / l or more, the polyol starter (ii.1.1) of the polyether polyol (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I): [ka] (wherein l, m, n and o are each independently an integer ranging from 1 to 6). Preferably, l, m, n and o of the at least one triol (ii.1.1) of formula (I) are each independently an integer ranging from 1 to 3, and more preferably l, m, n and o are all 1.
[0069] In one embodiment of the process for producing compact polyurethanes having a density of 850 g / l or more, the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0070] In one embodiment of the process for the preparation of compact polyurethanes having a density of 850 g / l or more, the polyether polyol (ii.1) is based on a triol other than glycerol, preferably on the triol (ii.1.1) of formula (I) above, more preferably the polyether polyol (ii.1) has the formula (II), [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q and r are each independently zero or an integer ranging from 1 to 6, preferably zero or an integer ranging from 1 to 4, more preferably zero or an integer ranging from 1 to 3; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group. 1 , X 2 and X 3 are each a -CH2-CH(CH3)-O- group. Preferably, l, m, n and o are all 1, and p, q and r are independently a value from 0 to 2.
[0071] In one embodiment of the process for producing a compact polyurethane having a density of 850 g / l or more, the residual amount of alkali metal salts in the polyol composition ii) is n<0.5 ppm, based on the total weight of the polyol composition ii).
[0072] In one embodiment of the method for producing a compact polyurethane having a density of 850 g / l or more, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3) and without the use of an additional alkoxylation catalyst. In one embodiment of the method for producing a compact polyurethane having a density of 850 g / l or more, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3) in a one-step synthesis process. The boron-based fluorine-containing Lewis acid catalyst can be optionally removed after the synthesis of the polyetherol, but preferably remains in the product.
[0073] According to a further embodiment of the process for producing compact polyurethanes with a density of 850 g / l or more, the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or only end groups based on butylene oxide. Preferably, the polyether polyol (ii.1) has only end groups based on propylene oxide and / or only end groups based on butylene oxide, and does not contain groups based on ethylene oxide. Even when no ethylene oxide is used or only propylene oxide and / or butylene oxide are used, the use of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) according to the invention results in at least one polyether polyol (ii.1) having 50% or more primary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1), i.e. up to 50% of the hydroxyl groups in the polyether polyol (ii.1) are secondary hydroxyl groups.
[0074] According to a further embodiment of the process for producing compact polyurethanes having a density of 850 g / l or more, the polyether polyol (ii.1) is prepared exclusively by reacting a polyol starter, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reacting a triol (ii.1.1) with propylene oxide, without the use of further alkylene oxides.
[0075] In one embodiment of the method for producing compact polyurethanes with a density of 850 g / l or more, the polyol composition ii) comprises one or more further polyols, where the further polyol(s) are only polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation. The further polyol(s) are preferably selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyetherols (polyetherpolyols) alkoxylated in the presence of boron-containing Lewis acids, optionally polyesterols (polyesterpolyols) and optionally chain extenders. Details in this regard have already been described at the beginning with respect to the compact polyurethanes, and these also apply to the production method described here.
[0076] In one embodiment of the process for producing a compact polyurethane having a density of 850 g / l or more, all polyols of polyol composition (ii) are prepared without the use of basic or amine catalysts. In one embodiment of the process for producing a compact polyurethane having a density of 850 g / l or more, polyol composition (ii) does not contain an amine or basic catalyst to catalyze the polyurethane reaction.
[0077] The present invention also relates to a compact polyurethane having a density of 850 g / l or more, obtained or obtainable by the process described above.
[0078] Use of compact polyurethanes having a density of more than 850 g / l in the manufacture of fibre composites The present invention also provides a method for producing a composition comprising at least the following components: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, a polyol composition obtained or obtainable by reacting and a method for the preparation of fibre composites, preferably for the impregnation of fibres, in which a compact polyurethane having a density of 850 g / l or more is obtained or is obtainable by reacting
[0079] Regarding the process for using compact polyurethanes having a density of 850 g / l or more, the explanations already given in the section relating to compact polyurethanes also apply to polyisocyanate composition (i).
[0080] In one embodiment of the method of using a compact polyurethane having a density of 850 g / l or more for the production of a fiber composite, the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0081] In one embodiment of the process for using a compact polyurethane having a density of 850 g / l or more for the production of a fiber composite, the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is a boron-based Lewis acid catalyst of formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (CF5)3B and a mixture of BF3 and (CF5)3B, more preferably tris(pentafluorophenyl)borane. The use of the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) in the reaction of a polyol starter (ii.1.1) having a functionality of 3 to 6 with propylene oxide and / or butylene oxide (ii.1.2) can obtain the result that more than 50% of the hydroxyl groups present in the polyether polyol (ii.1) are primary hydroxyl groups, i.e. up to 50% of the hydroxyl groups formed are secondary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1).
[0082] In one embodiment of the process for using compact polyurethanes having a density of 850 g / l or more for the production of fiber composites, the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g. In one embodiment of the process for using compact polyurethanes having a density of 850 g / l or more for the production of fiber composites, the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0083] In one embodiment of the process for using a compact polyurethane having a density of 850 g / l or more for the production of a fibre composite, the polyether polyol (ii.1) is used in an amount of 10% to 50% by weight, based on the total weight of the polyisocyanate composition (i) and the polyol composition (ii) being 100% by weight.
[0084] In one embodiment of the process for the use of compact polyurethanes having a density of 850 g / l or more for the production of fibre composites, the polyol starter (ii.1.1) of the polyether polyol (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I): [ka] (In the formula, l, m, n and o each independently represent an integer ranging from 1 to 6).
[0085] In one embodiment of the process for using a compact polyurethane having a density of 850 g / l or more for the preparation of a fiber composite, l, m, n and o of the at least one triol (ii.1.1) of formula (I) are each independently an integer ranging from 1 to 3, preferably l, m, n and o are all 1.
[0086] In one embodiment of the process in which a compact polyurethane having a density of 850 g / l or more is used for the preparation of a fibre composite, the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0087] In one embodiment of the process for the use of compact polyurethanes having a density of 850 g / l or more for the production of fibre composites, the polyether polyol (ii.1) is based on a triol other than glycerol, preferably on the triol (ii.1.1) of formula (I) above, more preferably having the formula (II): [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q and r are each independently zero or an integer ranging from 1 to 6, preferably zero or an integer ranging from 1 to 4, more preferably zero or an integer ranging from 1 to 3; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 are each a -CH2-CH(CH3)-O- group. Preferably, l, m, n and o are all 1, and p, q and r are independently a value from 0 to 2.
[0088] In one embodiment of the process for using compact polyurethanes having a density of 850 g / l or more for the production of fiber composites, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3) and without the use of an additional alkoxylation catalyst. In one embodiment of the process for using compact polyurethanes having a density of 850 g / l or more, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3) in a one-step synthesis process. The boron-based fluorine-containing Lewis acid catalyst can be optionally removed after the synthesis of the polyetherol, but preferably remains in the product.
[0089] In one embodiment of the process for using compact polyurethanes with a density of 850 g / l or more for the production of fiber composites, the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide. Preferably, the polyether polyol (ii.1) has only end groups based on propylene oxide and / or butylene oxide, and does not contain groups based on ethylene oxide. More preferably, the polyether polyol (ii.1) is prepared exclusively by reaction of a polyol starter, in particular a triol (ii.1.1), with propylene oxide and / or butylene oxide (ii.1.2), without further alkylene oxide. Even if no ethylene oxide is used or only propylene oxide and / or butylene oxide are used, the use of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) according to the invention gives at least one polyether polyol (ii.1) having 50% or more primary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1), i.e. up to 50% of the hydroxyl groups in the polyether polyol (ii.1) are secondary hydroxyl groups.
[0090] In one embodiment of the process for using a compact polyurethane having a density of 850 g / l or more for the manufacture of a fiber composite, the polyol composition ii) comprises one or more further polyols, whereby the further polyol(s) are exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
[0091] In one embodiment of the method for using a compact polyurethane having a density of 850 g / l or more for the production of a fiber composite, the further polyol(s) is / are selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyether polyols alkoxylated in the presence of boron-containing Lewis acids, optionally polyester polyols, and optionally chain extenders. Details regarding the hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyether polyols alkoxylated in the presence of boron-containing Lewis acids, optionally polyester polyols, and optionally chain extenders used have already been described at the beginning for the compact polyurethanes, and these details also apply to the method of use described here, the polyol composition (ii) being free of amine or basic catalysts.
[0092] In one embodiment of the method of use, the polyol composition ii) comprises one or more further polyols as hydroxyl-functionalized hydrophobic compounds, where all polyols are prepared only without alkali metal-catalyzed or amine-catalyzed alkoxylation. Traces of KOH / CsOH / amines act as catalysts for PU production and also for the reaction of water with isocyanates. The present invention therefore uses polyols and raw materials free of these components. The use of polyols prepared with KOH catalysis, which have also been purified to remove salts to a large extent, allows for foamed materials to be obtained when reacted with isocyanates at high atmospheric humidity.
[0093] In one embodiment of the method of use, the residual amount of alkali metal salt in the polyol composition ii) is n<0.5 ppm, based on the total weight of the polyol composition ii).
[0094] Preferably, the composition of the polyol component here is adjusted so as to have a viscosity at 25° C. of preferably less than 1000 mPas.
[0095] Fiber Composites The present invention also relates to a method for producing a composition comprising the following components: a) containing at least the following components: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, a polyol composition obtained or obtainable by reacting a compact polyurethane having a density of 850 g / l or more, which is obtained or obtainable by reacting b) fibers at least partially embedded in said compact polyurethane. The present invention relates to a fiber composite material comprising:
[0096] In one embodiment of the fiber composite, a compact polyurethane is obtained or obtainable by reacting components (i), (ii) and at least one degassing agent as additive ii.1.4). For the fiber composite, the explanations already given in the section on compact polyurethanes also apply to the polyisocyanate composition (i).
[0097] In one embodiment of the fibre composite the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0098] In one embodiment of the fiber composite, the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (CF5)3B and a mixture of BF3 and (CF5)3B, more preferably tris(pentafluorophenyl)borane. The use of the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) in the reaction of a polyol starter (ii.1.1) having a functionality of 3 to 6 with propylene oxide and / or butylene oxide (ii.1.2) can obtain the result that more than 50% of the hydroxyl groups present in the polyether polyol (ii.1) are primary hydroxyl groups, i.e. up to 50% of the hydroxyl groups formed are secondary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1).
[0099] In one embodiment of the fibre composite, the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g. In one embodiment of the fibre composite, the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0100] In one embodiment of the fiber composite, the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on the total weight of the polyisocyanate composition (i) and the polyol composition (ii) being 100% by weight.
[0101] In one embodiment of the fiber composite, the polyol starter (ii.1.1) of the polyether polyol of (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I): [ka] (In the formula, l, m, n and o each independently represent an integer ranging from 1 to 6).
[0102] In one embodiment of the fibre composite, l, m, n and o in at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, preferably l, m, n and o are all 1.
[0103] In one embodiment of the fibre composite, the polyether polyol (ii.1) has a hydroxyl number in the range from 200 to 2000 mg KOH / g, preferably in the range from 300 to 1500 mg KOH / g, more preferably in the range from 400 to 1300 mg KOH / g.
[0104] In one embodiment of the fibre composite, the polyether polyol (ii.1) is based on a triol other than glycerol, preferably on the triol (ii.1.1) of formula (I) above, more preferably having the formula (II): [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q and r are each independently zero or an integer ranging from 1 to 6, preferably zero or an integer ranging from 1 to 4, more preferably zero or an integer ranging from 1 to 3; X 1 , X 2 and X 3are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 are each a -CH2-CH(CH3)-O- group. Preferably, l, m, n and o are all 1, and p, q and r are independently a value from 0 to 2.
[0105] In one embodiment of the fiber composite, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) and without the use of an additional alkoxylation catalyst. In one embodiment of the fiber composite, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) in a one-step synthesis process. The boron-based fluorine-containing Lewis acid catalyst can be optionally removed after the synthesis of the polyetherol, but preferably remains in the product.
[0106] In one embodiment of the fiber composite, the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or only end groups based on butylene oxide. More preferably, the polyether polyol (ii.1) has only end groups based on propylene oxide and / or only end groups based on butylene oxide, and does not contain groups based on ethylene oxide. Even when no ethylene oxide is used or only propylene oxide and / or butylene oxide are used, the use of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) according to the invention results in at least one polyether polyol (ii.1) having 50% or more primary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1), i.e. up to 50% of the hydroxyl groups in the polyether polyol (ii.1) are secondary hydroxyl groups.
[0107] In a preferred embodiment of the fibre composite, the polyether polyol (ii.1) is prepared exclusively by reacting a polyol, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reacting a triol (ii.1.1) with propylene oxide, without further alkylene oxide.
[0108] In one embodiment of the fiber composite, the preferred fibers are glass fibers, carbon fibers, polyester fibers, natural fibers such as cellulose fibers, aramid fibers, nylon fibers, basalt fibers, boron fibers, Zylon fibers (poly(p-phenylene-2,6-benzobisoxazole)), silicon carbide fibers, asbestos fibers, metal fibers, and combinations thereof. They can take the form of, for example, short or long glass fibers, continuous fibers, laid scrims, knits, random-laid fiber mats, and plies with the same or different fiber orientations. The techniques for wetting the fibers are not particularly limited and are well known. For example, they include filament winding processes, pultrusion processes, manual lamination processes, RTM processes, and infusion processes, such as vacuum infusion processes.
[0109] In one embodiment of the fiber composite, the polyol composition ii) comprises one or more further polyols, where the further polyol(s) are only polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation. The residual amount of alkali metal salts in the polyol composition ii) is n<0.5 ppm, based on the total weight of the polyol composition ii).
[0110] In one embodiment of the fiber composite, the further polyol(s) is / are selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyetherols (polyether polyols) alkoxylated in the presence of boron-containing Lewis acids, optionally polyesterols (polyester polyols) and optionally chain extenders. Details regarding the hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, boron-containing Lewis acids, optionally polyester polyols and optionally chain extenders used polyether polyols alkoxylated in the presence of chain extenders have already been described at the beginning for the compact polyurethanes, and these details also apply to the fiber composites described here. The polyol composition (ii) is prepared without the use of amine or basic catalysts, and the polyol composition (ii) does not contain amine or basic catalysts.
[0111] Preferred fibers are glass fibers, carbon fibers, polyester fibers, natural fibers such as cellulose fibers, aramid fibers, nylon fibers, basalt fibers, boron fibers, Zylon fibers (poly(p-phenylene-2,6-benzobisoxazole)), silicon carbide fibers, asbestos fibers, metal fibers, and combinations thereof. They can take the form of, for example, short or long glass fibers, continuous fibers, laid scrims, knits, randomly laid fiber mats, and plies with the same or different fiber orientations. Techniques for wetting the fibers are not particularly limited and are well known. For example, they include filament winding processes, pultrusion processes, manual lamination processes, resin transfer molding (RTM) processes, and infusion processes, such as vacuum infusion processes.
[0112] Manufacturing method for fiber composite material The present invention also relates to a method for producing a fibre composite material, the method comprising the steps of: 1) providing a fiber; 2) At least the following ingredients: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, a polyol composition obtained or obtainable by reacting Providing 3) mixing components i) and ii) of step 2) to obtain a reactive mixture; 4) impregnating the fibers with the reactive mixture obtained in step 3); 5) curing the reactive mixture to obtain a fiber composite, the polyurethane being compact and having a density of 850 g / l or more; Includes.
[0113] The explanations already given in the section on the compact polyurethanes for the production process of the fibre composites also apply to the polyisocyanate composition (i).
[0114] In one embodiment of the method for producing a fibre composite, the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0115] In one embodiment of the process for the preparation of a fiber composite, the boron-based, fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (C6F5)3B and a mixture of BF3 and (C6F5)3B, more preferably tris(pentafluorophenyl)borane. The use of the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) in the reaction of polyol starters (ii.1.1) having a functionality of 3 to 6 with propylene oxide and / or butylene oxide (ii.1.2) results in more than 50% of the hydroxyl groups present in the polyether polyol (ii.1) being primary hydroxyl groups, i.e. up to 50% of the hydroxyl groups formed being secondary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1).
[0116] In one embodiment of the process for producing a fibre composite, the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range from 400 to 1200 mg KOH / g, more preferably in the range from 450 to 1200 mg KOH / g, more preferably in the range from 450 to 1000 mg KOH / g.
[0117] In one embodiment of the process for producing a fibre composite, the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0118] In one embodiment of the method for producing a fiber composite material, the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on the total weight of the polyisocyanate composition (i) and the polyol composition (ii) being 100% by weight.
[0119] In one embodiment of the process for producing a fibre composite, the polyol starter (ii.1.1) of the polyether polyol (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I): [ka] (In the formula, l, m, n and o each independently represent an integer ranging from 1 to 6).
[0120] In one embodiment of the process for producing a fibre composite, l, m, n and o in the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, more preferably l, m, n and o are all 1.
[0121] In one embodiment of the process for producing a fibre composite, the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0122] In one embodiment of the process for producing a fibre composite, the polyether polyol (ii.1) is based on a triol other than glycerol, preferably on the triol (ii.1.1) of formula (I) above, more preferably having the formula (II): [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q and r are each independently zero or an integer ranging from 1 to 6, preferably zero or an integer ranging from 1 to 4, more preferably zero or an integer ranging from 1 to 3; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 are each a -CH2-CH(CH3)-O- group. Preferably, l, m, n and o are all 1, and p, q and r are independently a value from 0 to 2.
[0123] In one embodiment of the process for preparing a fiber composite, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) and without the use of an additional alkoxylation catalyst. In one embodiment of the process for preparing a fiber composite, the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) in a one-step synthesis process. The boron-based fluorine-containing Lewis acid catalyst can be optionally removed after the synthesis of the polyetherol, but preferably remains in the product.
[0124] In one embodiment of the process for the preparation of a fibre composite, the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide.
[0125] In one embodiment of the process for producing a fiber composite, the polyether polyol (ii.1) has only propylene oxide-based and / or butylene oxide-based end groups and does not contain ethylene oxide-based groups. Even if no ethylene oxide is used or only propylene oxide and / or butylene oxide are used, the use of the boron-based fluorine-containing Lewis acid catalyst (ii.1.3) according to the invention results in at least one polyether polyol (ii.1) having 50% or more primary hydroxyl groups, in each case based on the totality of all hydroxyl groups in the polyether polyol (ii.1), i.e. up to 50% of the hydroxyl groups in the polyether polyol (ii.1) are secondary hydroxyl groups.
[0126] In one embodiment of the process for the preparation of fibre composites, the polyether polyol (ii.1) is prepared exclusively by reacting a polyol starter, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reacting a triol (ii.1.1) with propylene oxide, without the use of further alkylene oxide.
[0127] In one embodiment of the process for producing a fiber composite, the polyol composition ii) comprises one or more further polyols, where the further polyol(s) are exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
[0128] In one embodiment of the process for producing a fibre composite the residual amount of alkali metal salt in the polyol composition ii) is n<0.5 ppm, based on the total weight of the polyol composition ii).
[0129] In one embodiment of the method for producing a fiber composite, the further polyol(s) is / are selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyetherols (polyether polyols) alkoxylated in the presence of boron-containing Lewis acids, optionally polyesterols (polyester polyols) and optionally chain extenders. Details regarding the hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, boron-containing Lewis acids, optionally polyester polyols and optionally chain extenders used, have already been described at the beginning for the compact polyurethanes, and these details also apply to the method for producing a fiber composite described here. All polyols of the polyol composition (ii) are prepared without the use of basic or amine catalysts, and the polyol composition (ii) does not contain amine or basic catalysts.
[0130] Preferably, the composition of the polyol component is adjusted to have a viscosity (measured according to DIN 53019-1 to 3) of preferably less than 1000 mPas at 25° C. Preferably, the viscosity of polyol component (ii) (measured according to DIN 53019-1 to 3) at 23° C. is less than 500 mPas.
[0131] Preferred fibers are glass fibers, carbon fibers, polyester fibers, natural fibers such as cellulose fibers, aramid fibers, nylon fibers, basalt fibers, boron fibers, Zylon fibers (poly(p-phenylene-2,6-benzobisoxazole)), silicon carbide fibers, asbestos fibers, metal fibers, and combinations thereof. They can take the form of, for example, short or long glass fibers, continuous fibers, laid scrims, knits, randomly laid fiber mats, and plies with the same or different fiber orientations. Techniques for wetting the fibers are not particularly limited and are well known. For example, they include filament winding processes, pultrusion processes, manual lamination processes, RTM processes, and infusion processes, such as vacuum infusion processes.
[0132] The present invention is described in more detail by the following embodiments and combinations of embodiments arising from the corresponding dependent references and other references. In particular, it should be noted that in any case where a range of embodiments is mentioned, for example in the context of a phrase such as "the method according to any one of embodiments 1 to 4", each embodiment within this range is considered to be expressly disclosed to a person skilled in the art, that is, the wording of this phrase is understood by a person skilled in the art to be equivalent to "the method according to any one of embodiments 1, 2, 3, and 4".
[0133] 1. At least the following ingredients: i) Polyisocyanate composition ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, 4. A polyol composition according to claim 1, wherein the polyether polyol (ii.1) has an equivalent molecular weight of 50 to 150 g / mol. 1. A compact polyurethane having a density of 850 g / l or more, which is obtained or obtainable by reacting
[0134] 2. Compact polyurethane according to embodiment 1, having a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0135] 3. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) has the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 and (C6F5)3B are identical), more preferably said boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (C6F5)3B, and a mixture of BF3 and (C6F5)3B, more preferably tris(pentafluorophenyl)borane.
[0136] 4. The compact polyurethane according to any one of the preceding claims, wherein the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g.
[0137] 5. The compact polyurethane according to any one of the preceding claims, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0138] 6. The compact polyurethane according to any one of the preceding claims, wherein the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on 100% by weight of the total weight of the polyisocyanate composition (i) and the polyol composition (ii).
[0139] 7. The polyol starter (ii.1.1) of the polyether polyol (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I), [ka] wherein l, m, n, and o are each independently an integer ranging from 1 to 6. The compact polyurethane of any one of the preceding claims.
[0140] 8. The compact polyurethane according to embodiment 7, wherein l, m, n and o in the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, preferably l, m, n and o are all 1.
[0141] 9. The compact polyurethane according to any one of the preceding claims 7 to 8, wherein the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0142] 10. The polyether polyol (ii.1) is based on a triol other than glycerol, preferably on a triol (ii.1.1) of formula (I) according to embodiment 7 or 8, more preferably having the formula (II), [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q, and r are each independently zero or an integer ranging from 1 to 6; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 each is a -CH2-CH(CH3)-O- group),
[0143] 11. The compact polyurethane according to any one of the preceding claims, wherein the reaction of (ii.1.1) with (ii.1.2) is carried out solely in the presence of the boron-based, fluorine-containing Lewis acid catalyst (ii.1.3) and without the use of an additional alkoxylation catalyst.
[0144] 12. The compact polyurethane according to any one of the preceding claims, wherein the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide.
[0145] 13. The compact polyurethane according to any one of the preceding claims, wherein the polyether polyol (ii.1) has only propylene oxide-based and / or butylene oxide-based end groups and does not contain any ethylene oxide-based groups.
[0146] 14. A compact polyurethane according to any one of the preceding claims, wherein the polyether polyol (ii.1) is prepared exclusively by reaction of a polyol starter, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reaction of a triol (ii.1.1) with propylene oxide, without further alkylene oxide.
[0147] 15. The compact polyurethane according to any one of the preceding claims, wherein the polyol composition ii) comprises one or more further polyols, the further polyol(s) being exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
[0148] 16. The compact polyurethane according to embodiment 15, wherein the residual amount of alkali metal salt in the polyol composition ii) is n<0.5 ppm, based on the total weight of the polyol composition ii).
[0149] 17. The compact polyurethane according to any one of the preceding claims 15 to 16, wherein the further polyol(s) is selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyether polyols alkoxylated in the presence of boron-containing Lewis acids, optionally polyester polyols, and optionally chain extenders.
[0150] 18. The compact polyurethane according to any one of embodiments 15 to 17, wherein all polyols of the polyol composition (ii) are prepared without the use of a basic catalyst or an amine catalyst.
[0151] 19. The compact polyurethane according to any one of embodiments 15 to 18, wherein the polyol composition (ii) does not contain an amine catalyst or a base catalyst.
[0152] A method for producing a compact polyurethane having a density of 20.850 g / l or more, comprising the steps of: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, 4. A polyol composition according to claim 1, wherein the polyether polyol (ii.1) has an equivalent molecular weight of 50 to 150 g / mol. 1. A method for producing a compact polyurethane having a density of 850 g / l or more, comprising the reaction:
[0153] 21. A method for producing a compact polyurethane having a density of 850 g / l or more according to embodiment 20, wherein the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0154] 22. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) has the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF), tris(pentafluorophenyl)borane (CF)B, and a mixture of BF and (CF)B, more preferably tris(pentafluorophenyl)borane.
[0155] 23. Method for producing a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 20 to 21, wherein the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g.
[0156] 24. A method for producing a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 20 to 23, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0157] 25. The method for producing a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 20 to 24, wherein the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on 100% by weight of the total weight of the polyisocyanate composition (i) and the polyol composition (ii).
[0158] 26. The polyol starter (ii.1.1) of the polyether polyol of (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I), [ka] wherein l, m, n and o are each independently an integer in the range of 1 to 6.
[0159] 27. A method for producing a compact polyurethane having a density of 850 g / l or more according to embodiment 26, wherein l, m, n and o in the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, preferably l, m, n and o are all 1.
[0160] 28. A method for producing a compact polyurethane having a density of at least 850 g / l according to embodiment 26 or 27, wherein the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0161] 29. The polyether polyol (ii.1) is based on a triol other than glycerol, preferably on a triol (ii.1.1) of formula (I) according to embodiment 26 or 27, more preferably having the formula (II), [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q, and r are each independently zero or an integer ranging from 1 to 6; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 each is a -CH2-CH(CH3)-O- group),
[0162] 30. A method for producing a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 20 to 29, wherein the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), without the use of an additional alkoxylation catalyst.
[0163] 31. A method for producing a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 20 to 30, wherein the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide.
[0164] 32. A method for producing a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 20 to 31, wherein the polyether polyol (ii.1) has only end groups based on propylene oxide and / or butylene oxide, and does not contain groups based on ethylene oxide.
[0165] 33. A process for the preparation of compact polyurethanes having a density of 850 g / l or more according to any one of embodiments 20 to 32, wherein the polyether polyol (ii.1) is prepared exclusively by reaction of a polyol starter, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reaction of a triol (ii.1.1) with propylene oxide, without further alkylene oxide being used.
[0166] 34. A method for producing a compact polyurethane having a density of 850 g / l or greater according to any one of embodiments 20 to 33, wherein the polyol composition ii) comprises one or more further polyols, the further polyol(s) being exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
[0167] 35. A method for producing a compact polyurethane having a density of 850 g / l or more according to embodiment 34, wherein the residual amount of alkali metal salt in the polyol composition ii) is n<0.5 ppm, based on the total mass of the polyol composition ii).
[0168] 36. A method for producing a compact polyurethane having a density of 850 g / l or more according to embodiment 34 or 35, wherein the further polyol(s) is selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and polyether polyols alkoxylated in the presence of boron-containing Lewis acids, optionally polyester polyols and optionally chain extenders.
[0169] 37. A method for producing a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 34 to 36, wherein all polyols of the polyol composition (ii) are prepared without the use of basic or amine catalysts.
[0170] 38. A method for producing a compact polyurethane having a density of 850 g / l or greater according to any one of embodiments 34 to 37, wherein the polyol composition (ii) does not contain an amine catalyst or a base catalyst.
[0171] 39. A compact polyurethane having a density of 850 g / l or more, obtained or obtainable by the method according to any one of embodiments 20 to 38.
[0172] 40. Contains at least the following ingredients: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, 4. A polyol composition according to claim 1, wherein the polyether polyol (ii.1) has an equivalent molecular weight of 50 to 150 g / mol. 5. The method of claim 1, wherein a compact polyurethane having a density of at least 850 g / l is used for the production of fibre composites, preferably for impregnating fibres, the compact polyurethane being obtained or obtainable by reacting
[0173] 41. A method for producing a fiber composite using a compact polyurethane having a density of 850 g / l or more according to embodiment 40, wherein the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0174] 42. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 and (ii.1.3) are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (CF5)3B, and a mixture of BF3 and (CF5)3B, more preferably tris(pentafluorophenyl)borane.
[0175] 43. Use of a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 40 to 42 for the production of a fibre composite, wherein the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range from 400 to 1200 mg KOH / g, more preferably in the range from 450 to 1200 mg KOH / g, more preferably in the range from 450 to 1000 mg KOH / g.
[0176] 44. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 43 for the production of a fibre composite, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0177] 45. A method for the production of a fiber composite using a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 44, wherein the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on 100% by weight of the total weight of the polyisocyanate composition (i) and the polyol composition (ii).
[0178] 46. The polyol starter (ii.1.1) of the polyether polyol of (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I), [ka] wherein l, m, n and o are each independently an integer in the range of 1 to 6, and wherein the compact polyurethane having a density of at least 850 g / l according to any one of embodiments 40 to 45 is used for the manufacture of a fiber composite.
[0179] 47. A method for the production of a fiber composite using a compact polyurethane having a density of 850 g / l or greater according to embodiment 46, wherein l, m, n and o in the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, preferably l, m, n and o are all 1.
[0180] 48. Use of a compact polyurethane having a density of at least 850 g / l for the production of a fibre composite according to embodiment 46 or 47, wherein the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0181] 49. The polyether polyol (ii.1) is based on a triol other than glycerol, preferably on a triol (ii.1.1) of formula (I) according to embodiment 46 or 47, more preferably having the formula (II), [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q, and r are each independently zero or an integer ranging from 1 to 6; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 each is a -CH2-CH(CH3)-O- group), use of a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 40 to 48 for the manufacture of a fiber composite.
[0182] 50. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 49 for the manufacture of a fibre composite, wherein the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), without the use of an additional alkoxylation catalyst.
[0183] 51. Use of a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 40 to 50 for the production of a fibre composite, wherein the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide.
[0184] 52. Use of a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 40 to 51 for the production of a fibre composite, wherein the polyether polyol (ii.1) has only end groups based on propylene oxide and / or butylene oxide and does not contain groups based on ethylene oxide.
[0185] 53. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 52 for the production of a fibre composite, wherein the polyether polyol (ii.1) is prepared exclusively by reaction of a polyol starter, in particular a triol (ii.1.1), with propylene oxide and / or butylene oxide (ii.1.2), without further alkylene oxide being used.
[0186] 54. Use of a compact polyurethane having a density of at least 850 g / l according to any one of embodiments 40 to 53 for the manufacture of a fibre composite, wherein the polyol composition ii) comprises one or more further polyols, the further polyol(s) being exclusively polyols prepared without alkali metal-catalysed or amine-catalysed alkoxylation.
[0187] 55. A method for the production of a fiber composite using a compact polyurethane having a density of 850 g / l or more according to embodiment 54, wherein the residual amount of alkali metal salts in the polyol composition ii) is n<0.5 ppm, based on the total mass of the polyol composition ii).
[0188] 56. A method for the production of a fiber composite using a compact polyurethane having a density of 850 g / l or more according to embodiment 54 or 55, wherein the further polyol(s) is selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and boron-containing Lewis acids, optionally polyesterols (polyester polyols) and optionally alkoxylated polyetherols (polyether polyols) in the presence of chain extenders.
[0189] 57. A method for the manufacture of a fiber composite using a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 56, wherein all polyols of the polyol composition (ii) are prepared without the use of basic or amine catalysts.
[0190] 58. A method for the production of a fiber composite using a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 57, wherein the polyol composition (ii) does not contain an amine catalyst or a basic catalyst.
[0191] 59. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 58 for the manufacture of a fiber composite, wherein filament winding is used as the manufacturing method.
[0192] 60. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 58 for the production of a fibre composite, wherein vacuum infusion is used as the production method.
[0193] 61. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 58 for the production of a fibre composite, wherein resin transfer moulding is used as the production method.
[0194] 62. Use of a compact polyurethane having a density of 850 g / l or more according to any one of embodiments 40 to 58 for the production of a fiber composite, wherein pultrusion is used as the production method.
[0195] 63. The following ingredients: a) containing at least the following components: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, 4. A polyol composition according to claim 1, wherein the polyether polyol (ii.1) has an equivalent molecular weight of 50 to 150 g / mol. a compact polyurethane having a density of 850 g / l or more, which is obtained or obtainable by reacting b) fibers at least partially embedded in said compact polyurethane. A fiber composite material comprising:
[0196] 64. A fiber composite according to embodiment 63, wherein the compact polyurethane is obtained or obtainable by reacting components (i), (ii) and at least one degassing agent as additive ii.1.4).
[0197] 65. A fiber composite according to any one of embodiments 63 to 64, wherein the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0198] 66. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3 are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF), tris(pentafluorophenyl)borane (CF)B, and a mixture of BF and (CF)B, more preferably tris(pentafluorophenyl)borane.
[0199] 67. The fibre composite according to any one of embodiments 63 to 66, wherein the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g.
[0200] 68. The fibre composite according to any one of embodiments 63 to 67, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0201] 69. The fiber composite according to any one of embodiments 63 to 68, wherein the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on 100% by weight of the total weight of the polyisocyanate composition (i) and the polyol composition (ii).
[0202] 70. The polyol starter (ii.1.1) of the polyether polyol of (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I), [ka] wherein l, m, n, and o are each independently an integer in the range of 1 to 6.
[0203] 71. The fiber composite according to embodiment 70, wherein l, m, n and o in the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, preferably l, m, n and o are all 1.
[0204] 72. The fibre composite according to any one of embodiments 70 to 71, wherein the polyether polyol (ii.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1500 mg KOH / g, more preferably in the range of 400 to 1300 mg KOH / g.
[0205] 73. The polyether polyol (ii.1) is based on a triol other than glycerol, preferably on a triol (ii.1.1) of formula (I) according to embodiment 70 or 71, more preferably having the formula (II), [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q, and r are each independently zero or an integer ranging from 1 to 6; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X3 each is a -CH2-CH(CH3)-O- group.
[0206] 74. A fiber composite according to any one of embodiments 63 to 73, wherein the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based, fluorine-containing Lewis acid catalyst (ii.1.3), without the use of an additional alkoxylation catalyst.
[0207] 75. The fibre composite according to any one of embodiments 63 to 74, wherein the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide.
[0208] 76. The fiber composite according to any one of embodiments 63 to 75, wherein the polyether polyol (ii.1) has only propylene oxide-based and / or butylene oxide-based end groups and does not contain any ethylene oxide-based groups.
[0209] 77. The fibre composite according to any one of embodiments 63 to 76, wherein the polyether polyol (ii.1) is prepared exclusively by reacting a polyol, in particular a triol (ii.1.1), with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reacting a triol (ii.1.1) with propylene oxide, without further alkylene oxide being used.
[0210] 78. The fiber composite of any one of embodiments 63 to 77, wherein the fibers are selected from glass fibers, carbon fibers, polyester fibers, natural fibers such as cellulose fibers, aramid fibers, nylon fibers, basalt fibers, boron fibers, Zylon fibers (poly(p-phenylene-2,6-benzobisoxazole)), silicon carbide fibers, asbestos fibers, metal fibers, and combinations thereof.
[0211] 79. A fiber composite material according to any one of embodiments 63 to 78, wherein the fibers are in the form of short or long glass fibers, continuous fibers, laid scrims, knits, randomly laid fiber mats, and plies having the same or different fiber orientations.
[0212] 80. The fiber composite of any one of embodiments 63 to 79, wherein the polyol composition ii) comprises one or more further polyols, the further polyol(s) being exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
[0213] 81. A fiber composite according to embodiment 80, wherein the residual amount of alkali metal salt in the polyol composition ii) is n<0.5 ppm, based on the total mass of the polyol composition ii).
[0214] 82. The fiber composite according to any one of the preceding claims 80 to 81, wherein the further polyol(s) is / are selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and boron-containing Lewis acids, optionally polyesterols (polyester polyols) and optionally alkoxylated polyetherols (polyether polyols) in the presence of chain extenders.
[0215] 83. A fiber composite according to any one of embodiments 63 to 82, wherein all polyols of polyol composition (ii) are prepared using a base catalyst, an amine catalyst or no amine catalyst.
[0216] 84. The fiber composite of any one of embodiments 63 to 83, wherein the polyol composition (ii) does not contain an amine catalyst or a base catalyst.
[0217] 85. A method for producing a fiber composite material, comprising the steps of: 1) providing a fiber; 2) At least the following ingredients: i) a polyisocyanate composition, ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii.1.1) a polyol starter having a functionality of 3 to 6, preferably 3 or 4 ii.1.2) propylene oxide and / or butylene oxide; boron-based fluorine-containing Lewis acid catalysts (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives, 4. A polyol composition according to claim 1, wherein the polyether polyol (ii.1) has an equivalent molecular weight of 50 to 150 g / mol. Providing 3) mixing components i) and ii) of step 2) to obtain a reactive mixture; 4) impregnating the fibers with the reactive mixture obtained in step 3); 5) curing the reactive mixture to obtain a fiber composite, the polyurethane being compact and having a density of 850 g / l or more; A method for producing a fiber composite material, comprising:
[0218] 86. A method for producing a fiber composite according to embodiment 85, wherein the compact polyurethane has a density in the range of 850 to 1250 g / l, preferably in the range of 850 to 1100 g / l.
[0219] 87. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is represented by the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group, preferably R 1 , R 2 and R 3and (C6F5)3B are identical), more preferably the boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) is selected from boron trifluoride (BF3), tris(pentafluorophenyl)borane (C6F5)3B, and a mixture of BF3 and (C6F5)3B, more preferably tris(pentafluorophenyl)borane.
[0220] 88. The method for producing a fibre composite according to any one of embodiments 85 to 87, wherein the polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g, preferably more than 450 mg KOH / g, more preferably in the range of 400 to 1200 mg KOH / g, more preferably in the range of 450 to 1200 mg KOH / g, more preferably in the range of 450 to 1000 mg KOH / g.
[0221] 89. The method for producing a fiber composite according to any one of embodiments 85 to 88, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol, preferably in the range of 55 to 135 g / mol, more preferably in the range of 60 to 130 g / mol.
[0222] 90. The method for producing a fiber composite according to any one of embodiments 85 to 89, wherein the polyether polyol (ii.1) is used in an amount of 10% by weight to 50% by weight, based on 100% by weight of the total weight of the polyisocyanate composition (i) and the polyol composition (ii).
[0223] 91. The polyol starter (ii.1.1) of the polyether polyol of (ii.1) is a triol having a functionality of 3, preferably a triol having a functionality of 3 other than glycerol, more preferably a triol of formula (I), [ka] wherein l, m, n and o are each independently an integer in the range of 1 to 6.
[0224] 92. The method for producing a fiber composite according to embodiment 91, wherein l, m, n and o in the at least one triol (ii.1.1) of formula (I) are each independently an integer in the range of 1 to 3, more preferably l, m, n and o are all 1.
[0225] 93. The method for producing a fibre composite according to any one of embodiments 91 to 92, wherein the triol (ii.1.1) has a hydroxyl number in the range of 200 to 2000 mg KOH / g, preferably in the range of 300 to 1850 mg KOH / g, more preferably in the range of 400 to 1850 mg KOH / g.
[0226] 94. The polyether polyol (ii.1) is based on a triol other than glycerol, preferably on a triol (ii.1.1) of formula (I) according to embodiment 91 or 92, more preferably having the formula (II), [ka] (In the formula, l, m, n, and o each independently represent an integer ranging from 1 to 6, p, q, and r are each independently zero or an integer ranging from 1 to 6; X 1 , X 2 and X 3 are each independently a -CH2-CH(CH3)-O- group or a -CH2-CH(CH2-CH3)-O- group, and preferably, X 1 , X 2 and X 3 each is a -CH2-CH(CH3)-O- group.
[0227] 95. A method for producing a fiber composite according to any one of embodiments 85 to 94, wherein the reaction of (ii.1.1) with (ii.1.2) is carried out only in the presence of a boron-based, fluorine-containing Lewis acid catalyst (ii.1.3), without the use of an additional alkoxylation catalyst.
[0228] 96. A method for producing a fiber composite according to any one of embodiments 85 to 95, wherein the polyether polyol (ii.1) has no end groups based on ethylene oxide, preferably only end groups based on propylene oxide and / or butylene oxide.
[0229] 97. A method for producing a fiber composite according to any one of embodiments 85 to 96, wherein the polyether polyol (ii.1) has only propylene oxide-based and / or butylene oxide-based end groups and does not contain any ethylene oxide-based groups.
[0230] 98. Method for producing a fiber composite according to any one of embodiments 85 to 97, in which the polyether polyol (ii.1) is prepared exclusively by reacting a polyol starter, in particular a triol (ii.1.1) with propylene oxide and / or butylene oxide (ii.1.2), preferably exclusively by reacting a triol (ii.1.1) with propylene oxide, without further alkylene oxide being used.
[0231] 99. A method for producing a fiber composite according to any one of embodiments 85 to 98, wherein the polyol composition ii) comprises one or more further polyols, the further polyol(s) being exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
[0232] 100. The method for producing a fiber composite according to embodiment 99, wherein the residual amount of alkali metal salt in the polyol composition ii) is n<0.5 ppm, based on the total mass of the polyol composition ii).
[0233] 101. The method for producing a fiber composite according to any one of embodiments 99 to 100, wherein the further polyol(s) is selected from the group consisting of hydroxyl-functionalized hydrophobic compounds, oleochemical polyols, and boron-containing Lewis acids, optionally polyesterols (polyester polyols) and optionally alkoxylated polyetherols (polyether polyols) in the presence of chain extenders.
[0234] 102. The method for producing a fiber composite according to any one of embodiments 85 to 101, wherein all polyols of polyol composition (ii) are prepared without the use of a basic catalyst or an amine catalyst.
[0235] 103. The method for producing a fiber composite according to any one of embodiments 85 to 102, wherein the polyol composition (ii) does not contain an amine catalyst or a base catalyst.
[0236] 104. The method for producing a fiber composite according to any one of embodiments 85 to 103, wherein the viscosity of the polyol component (ii) at 23°C (measured according to DIN 53019-1 to 3) is less than 1000 mPas.
[0237] 105. The method for producing a fiber composite according to any one of embodiments 85 to 104, wherein the viscosity of the polyol component (ii) at 23° C. (measured according to DIN 53019-1 to 3) is less than 500 mPas.
[0238] The following examples serve to illustrate the invention but are in no way limiting with respect to the subject matter thereof. EXAMPLES
[0239] chemicals
[0240] [Table 1]
[0241] Test Method: Viscosity according to DIN 53019-1~3 Shore D hardness test according to DIN ISO 7619-1 Three-point bending test according to DIN EN ISO 178 Tensile strength according to DIN EN ISO 527 Charpy impact resistance (flatwise) according to DIN EN ISO 179-1 / 1fU Heat distortion temperature: HDT-Bf, flatwise at 0.45 MPa according to DIN EN ISO 75, Hydroxyl number (OH number, OHN): DIN 53240, Density measurement (buoyancy method): DIN EN ISO 1183-1.
[0242] Preparation of polyols 1-7 Polyol 1 Polyol 1 is 810 It was a glycerol propoxylate with an OH number of mg KOH / g and a viscosity of 1275 mPas at 25° C. The polyol was prepared under standard conditions with KOH catalysis. The residual alkalinity was 98 ppm.
[0243] Polyol 2 Initially, 198.72 g of trimethylolpropane and 1.80 g of an aqueous KOH solution (50% by weight) were charged into a 600 ml reactor at 25° C., which was then inerted three times with nitrogen. The vessel was heated to 102° C. with stirring and the starter mixture was dried under reduced pressure for 1 hour. Then, 250.38 g of propylene oxide were metered in over a period of 4 hours. After a reaction time of 2 hours, the reactor was evacuated under full vacuum for 20 minutes and then cooled to 50° C. The product obtained (430 g) had the following parameters: Hydroxyl number (OHN), 550 mg KOH / g Viscosity (25℃), 2040mPas.
[0244] Polyol 3 Initially, 1191 g of trimethylolpropane and 0.90 g of tris(pentafluorophenyl)borane were charged into a 5 liter reactor at 25° C., which was then inerted three times with nitrogen. The vessel was heated to 102° C. with stirring and the starter mixture was dried under reduced pressure for 1 hour. Then, 2508 g of propylene oxide were metered in over a period of 3.5 hours. After a reaction time of 2 hours, the reactor was evacuated under full vacuum for 20 minutes and then cooled to 50° C. The product obtained (4450 g) had the following parameters: Hydroxyl number (OHN), 550 mg KOH / g Viscosity (25℃), 1860mPas.
[0245] Polyol 4 Polyol 4 is 550 It was a glycerol propoxylate with an OH number of mg KOH / g and a viscosity of 655 mPas at 25° C. BF3 etherate (0.11% by weight based on the total mixture) was used to prepare the polyol with cationic catalysis. The reaction temperature was 105° C.
[0246] Polyol 5 Polyol 5 corresponded to the reduced alkalinity of Polyol 1. The residual alkalinity was 15 ppm.
[0247] Polyol 6 Initially, 198.9 g of trimethylolpropane and 0.50 g of BF3 etherate were charged into a 600 ml reactor at 25° C., which was then inerted three times with nitrogen. The vessel was heated to 102° C. with stirring. Then, 250.6 g of propylene oxide were metered in over a period of 3.5 hours. After a reaction time of 2 hours, the reactor was evacuated under full vacuum for 120 minutes and then cooled to 50° C. The product obtained (400 g) had the following parameters: Hydroxyl number (OHN), 550 mg KOH / g Viscosity (25℃), 1195mPas.
[0248] Polyol 7 First, 198.72 g of trimethylolpropane were charged into a 600 ml reactor at 25° C., which was then inerted three times with nitrogen. The reactor was heated to 102° C. with stirring and the starter was dried under reduced pressure for 1 hour. Then, 250.38 g of propylene oxide were metered in over a period of 4 hours. After a reaction time of 32 hours, the yield was less than 10% with respect to the addition product of TMP and three propylene oxide units.
[0249] This catalyst-free reaction regime is not economically viable in industry, so the reaction was discontinued. Under the same reaction conditions, polyols 1–6 are almost completely converted after 6 h reaction time.
[0250] Reference Example 1 - Preparation of test sheets from compact polyurethane All starting materials except the isocyanate (typical batch size: 300 g of polyol component) were mixed at room temperature under reduced pressure. The isocyanate was then added and the mixture was mixed in a Speedmixer (FA Hauschild) for 60 seconds. The reaction mixture was then poured into a 20 x 30 x 0.4 cm or 20 x 30 x 0.2 cm mould, the excess resin was removed with a doctor blade and cured at 80°C for 1 hour and then at 120°C for 2 hours. After storage at room temperature for 1 week, test specimens were crushed from the material.
[0251] Reference Example 2 - Production of a fiber composite from compact polyurethane and glass fibers using a filament winding process A conventional filament winding unit was used, which is installed in a housing equipped with an extraction system. The desired atmospheric humidity in the housing was set using a humidifier. A bobbin with continuous glass fiber mounted in the housing was used. The glass fiber was led into a not yet filled impregnation bath and then laid onto the mandrel via a laying head. Both ends of the mandrel were attached to a rotating device. The impregnation bath and the laying head were mounted on a carriage, which allows the fiber to be laid down along the length of the mandrel. The movement of the carriage, the rotation of the mandrel and the intended laying angle of the fiber on the mandrel were programmed as a function of time and then controlled by the winding software. The glass fiber used was SE3030 glass fiber from 3B (boron-free glass fiber, filament diameter 17 μm and tex 2400 (g / km)). The winding patterns selected were two circumferential plies, one ply + / - 45° and two circumferential plies. The tests were carried out at a temperature of 25° C. and an atmospheric humidity of 85%.
[0252] At the start of the test, all starting materials (typical batch size: 100 g of polyol component) except the isocyanate were mixed at room temperature. The isocyanate was then added and the mixture was mixed in a Speedmixer (FA Hauschild) for 60 seconds. The material was then loaded into the impregnation tank. The roving was then stretched manually until it could be laid and fixed on the mandrel, impregnated with resin. The winding program was then started, laying several plies of polyurethane-impregnated glass fibre on the mandrel. After the winding process was finished, the glass fibre was cut and the material was cured at room temperature for 1 hour. It was then cured at 80 °C for 1 hour and at 120 °C for 2 hours.
[0253] The quality of the part surfaces was visually assessed: 1: Smooth surface without micro-bubbles, 2: Relatively smooth surface with a small amount of microbubbles; 3: A large amount of microbubbles, 4: Rough, foamy element surface, 5: White, foamy element surface with many bubbles with diameters greater than 1mm.
[0254] Examples 1-3 - Preparation of compact polyurethanes based on TMP-initiated polyols prepared using borane fluoride catalyst for propoxylation Test samples and wound polyurethane-impregnated glass fibers were prepared according to the procedures of Reference Examples 1 and 2, but in each case using TMP-initiated polyols prepared with fluorinated borane catalysts for propoxylation. Table 1 shows the starting materials and their amounts, as well as the properties of the polyurethanes obtained individually and the fiber composites obtained.
[0255] Comparative Examples 1-3 - Preparation of compact polyurethanes based on TMP-initiated polyols prepared using KOH as catalyst for propoxylation Test samples and wound polyurethane-impregnated glass fibers were prepared according to the procedures of Reference Examples 1 and 2, but in both cases using TMP-initiated polyols prepared with KOH as catalyst for propoxylation. Table 1 shows the starting materials and their amounts, as well as the properties of the individually obtained polyurethanes and the correspondingly obtained fiber composites of Comparative Examples 1 to 3.
[0256] [Table 2]
[0257] It has been found that the use of polyols produced by propoxylation from triols, particularly TMP, under catalysis with boron-based fluorine-containing Lewis acid catalysts, particularly tris(pentafluorophenyl)borane, results in compact polyurethanes with improved impact resistance of more than 60, particularly more than 70. Furthermore, the Shore D hardness is comparable to that of polyurethanes produced using different polyols produced under catalysis with KOH. Surprisingly, the compact polyurethanes produced using polyols produced by propoxylation from triols, particularly TMP, under catalysis with boron-based fluorine-containing Lewis acid catalysts, particularly tris(pentafluorophenyl)borane, have significantly improved tensile strengths of more than 80 MPa.
[0258] In winding tests, it was found that the use of compact polyurethanes produced using polyols produced by propoxylation from triols, in particular TMP, under catalysis with boron-based fluorine-containing Lewis acid catalysts, in particular tris(pentafluorophenyl)borane, gave significantly better results in terms of avoiding the formation of unwanted bubbles: in winding tests, despite a high atmospheric humidity of 85%, the compact polyurethanes showed very little, if any, bubble formation, whereas the use of polyols produced under catalysis with KOH resulted in foaming, i.e. the formation of unwanted bubbles. Similar polyols synthesized without catalysis cannot be prepared economically.
[0259] References - Guenter Oertel,Polyurethane Handbook:Chemistry-Raw Materials-Processing-Application-Properties-1.January 1994 - US 3,464,935 A - T. Miyajima et al., Polymer Journal (2015) 47, 771-778 - WO 2016 / 064698 A1 - US 6,531,566 B1 - US 6,831,112 B2 - JP 2014-167105 A - US 2003 / 0100623 A1 - M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, Chapter 17.1 - M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, pp. 67 - 75 - Thomas Brock, Michael Groteklaes, Peter Mischke: Lehrbuch der Lacktechnologie [Textbook of Paint Technology]. Ed.: Ulrich Zorll, 2nd Edition, Vincentz Verlag, Hanover 2000, ISBN 978 - 3 - 87870 - 569 - 7, Chapter 2.4.2.1, Entschaeumer und Entluefter [Defoamers and Deaerators], p. 169 f. - Kunststoffhandbuch, Band 7, Polyurethane, Carl Hanser Verlag, 3rd Edition, 1993, Chapter 3.1 - 「Kunststoffhandbuch, Band 7, Polyurethane」, Carl Hanser Verlag, 3rd Edition, 1993, Chapters 3.4.4 and 3.4.6 - 3.4.11 - DE 102008021980 A1 - WO 2009 / 115540 A1 - WO 2006 / 034800 A1 - EP 0090444 B1 - WO 05 / 090440 A1 - EP 1 803 756 A1 - M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, p. 119 ff. - M. Neitzel, P. Mitschang, Handbook of Composite Materials, Carl Hanser Verlag, 2004, p. 164 - M. Ionescu, Chemistry and Technology of Polyols, Rapra, 2005, pp. 245 - 247
Claims
1. At least the following ingredients: i) Polyisocyanate Composition ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii. 1.1) A polyol starter having a functionality of 3 to 6 ii.1.2) propylene oxide and / or butylene oxide; a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives a polyol composition obtained or obtainable by reacting A compact polyurethane having a density of 850 g / l or more, which is obtained or obtainable by reacting The polyether polyol (ii.1) is a compact polyurethane having a hydroxyl number of more than 400 mg KOH / g.
2. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) has the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group.
3. A compact polyurethane as described in claim 1 or 2, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol.
4. 4. A compact polyurethane according to claim 1, wherein the polyol starter (ii.1.1) of the polyether polyol (ii.1) is a triol having a functionality of 3.
5. 5. A compact polyurethane according to any one of claims 1 to 4, wherein the reaction of (ii.1.1) with (ii.1.2) is carried out exclusively in the presence of a boron-based fluorine-containing Lewis acid catalyst (ii.1.3) and without the use of an additional alkoxylation catalyst.
6. 6. A compact polyurethane according to claim 1, wherein the polyether polyol (ii.1) has no end groups based on ethylene oxide.
7. 7. A compact polyurethane according to any one of claims 1 to 6, wherein the polyol composition ii) comprises one or more further polyols, said further polyol(s) being exclusively polyols prepared without alkali metal-catalyzed or amine-catalyzed alkoxylation.
8. A method for producing a compact polyurethane having a density of 850 g / l or more, comprising the steps of: i) a polyisocyanate composition; ii) a polyol composition comprising at least one polyether polyol (ii.1) wherein the at least one polyether polyol (ii.1) is ii. 1.1) A polyol starter having a functionality of 3 to 6 ii.1.2) propylene oxide and / or butylene oxide; a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives a polyol composition obtained or obtainable by reacting Including the reaction of The polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g and a density of 850 g / l or more.
9. The boron-based fluorine-containing Lewis acid catalyst of (ii.1.3) has the formula BR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 are each independently selected from the group consisting of a fluorine atom, a perfluorinated C1-C10 alkyl group, and a perfluorinated C6-C12 aryl group.
10. A method for producing a compact polyurethane having a density of 850 g / l or more as described in claim 8 or 9, wherein the polyether polyol (ii.1) has an equivalent molecular weight in the range of 50 to 140 g / mol.
11. 11. A process for the production of compact polyurethanes having a density of 850 g / l or more according to any one of claims 8 to 10, wherein the polyol starter (ii.1.1) of the polyether polyol of (ii.1) is a triol having a functionality of 3.
12. At least the following ingredients: i) a polyisocyanate composition; ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii. 1.1) A polyol starter having a functionality of 3 to 6 ii.1.2) propylene oxide and / or butylene oxide; a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives a polyol composition obtained or obtainable by reacting 1. A process for the use of a compact polyurethane having a density of at least 850 g / l for the manufacture of a fibre composite, the process comprising the steps of: The method of claim 1, wherein the polyether polyol (ii.1) has a hydroxyl number of greater than 400 mg KOH / g.
13. Ingredients below: a) at least the following ingredients: i) a polyisocyanate composition; ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii. 1.1) A polyol starter having a functionality of 3 to 6 ii.1.2) propylene oxide and / or butylene oxide; a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives a polyol composition obtained or obtainable by reacting a compact polyurethane having a density of 850 g / l or more, which is obtained or obtainable by reacting b) fibers at least partially embedded in said compact polyurethane. A fiber composite comprising: The polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g.
14. A method for producing a fiber composite material, comprising the steps of: 1) providing a fiber; 2) At least the following ingredients: i) a polyisocyanate composition; ii) a polyol composition comprising at least one polyether polyol (ii.1), said at least one polyether polyol (ii.1) being ii. 1.1) A polyol starter having a functionality of 3 to 6 ii.1.2) propylene oxide and / or butylene oxide; a boron-based fluorine-containing Lewis acid catalyst (ii.1.3), and ii.1.4) optionally in the presence of further auxiliaries and / or additives a polyol composition obtained or obtainable by reacting Providing 3) mixing components i) and ii) of step 2) to obtain a reactive mixture; 4) impregnating the fibers with the reactive mixture obtained in step 3); 5) curing the reactive mixture to obtain a fiber composite, the polyurethane being compact and having a density of 850 g / l or more; Including, The polyether polyol (ii.1) has a hydroxyl number of more than 400 mg KOH / g.
Citation Information
Patent Citations
Polyurethane resin forming composition, process for production of sealant, and process for production of hollow-fiber membrane modules
EP1803756A1
Polyol premix for polyurethane
JP2004149719A
Coating film water-proof material based on two-component urethane and polyol used for the same
JP2014122332A
Method of manufacturing alkylene oxide adduct
JP2014167105A
Flame-retardant composition, fiber-reinforced polyurethane composite article containing flame-retardant composition, and its use
JP2014520905A