PMMA-based cast polymers with improved mechanical properties.

A composition with hydrophilic inorganic compounds and reduced styrene content enhances PMMA-based foams' mechanical strength and compatibility, addressing the limitations of existing foams by achieving high elastic modulus and compressive strength.

JP7553545B2Active Publication Date: 2024-09-18EVONIK OPERATIONS GMBH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022507616
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-08
Filing Date
2020-07-03
Publication Date
2024-09-18
Estimated Expiration
2040-07-03

AI Technical Summary

Technical Problem

Existing PMMA-based foams have insufficient mechanical strength, particularly compressive strength, and are not easily foamable with high freedom in cell size and density definition, while also containing environmentally harmful blowing agents like styrene.

Method used

A composition comprising a hydrophilic inorganic compound, urea or urea derivatives, and a monomer mixture with reduced styrene content is used to produce PMMA-based cast polymers and foams, ensuring high mechanical stability and compatibility with resin systems.

Benefits of technology

The resulting PMMA-based foams exhibit an elastic modulus of at least 4500 MPa, high compressive strength, and low density, with improved mechanical properties and reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553545000002
    Figure 0007553545000002
  • Figure 0007553545000004
    Figure 0007553545000004
  • Figure 0007553545000005
    Figure 0007553545000005
Patent Text Reader

Abstract

The present invention relates to a composition for producing PMMA-based cast polymers with a low styrene content, which uses urea (derivatives) as a compounding component and a hydrophilic inorganic filler. From the composition according to the invention, it is possible to produce PMMA-based cast polymers and molded articles with surprisingly high mechanical stability.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for producing PMMA-based cast polymers with a low styrene content, using urea (derivatives) as compounding component and hydrophilic inorganic compounds as fillers. From the composition according to the invention it is possible to produce PMMA-based cast polymers and moulded articles with surprisingly high mechanical stability.

[0002] Although poly(methyl methacrylate) (PMMA) foams have been widely described in the literature, they have so far received little industrial importance, in part due to their often-described production via a highly complex autoclave process in which PMMA is filled with a gaseous blowing agent, e.g. CO2 or N2, under high pressure in an autoclave and then allowed to expand by releasing the pressure.

[0003] PMMA plastic can be manufactured by various processes. One of these processes is chamber polymerization, also known as cast polymerization. It involves the thermal or photochemical polymerization of a pourable monomer solution between two glass plates separated from each other by a sealing rope. This monomer solution contains at least a monomer (MMA) and a polymerization initiator. After the polymerization is complete, the glass plates are removed from the resulting polymer, resulting in a polymer sheet.

[0004] These cast polymers made of PMMA have an elastic modulus of approximately 3000-3300 MPa.

[0005] In the cast polymerization, it is also possible to use comonomers and additives. In principle, all comonomers that are soluble in the respective monomer solution and copolymerizable with MMA can be used here.

[0006] The mechanical properties of the PMMA-based polymers thus obtained can be adjusted within certain narrow limits by the choice of comonomers, but it is not known, for example, that it is possible in this way to increase the modulus of elasticity beyond values ​​of, for example, 4000 MPa.

[0007] Polymethylmethacrylimide (PMMI) is a polymer based on PMMA and has an elastic modulus of about 4000 MPa (e.g. Pleximid® TT70 from Roehm GmbH). However, this polymer cannot be produced by cast polymerization.

[0008] US Patent No. 4,816,492 describes the preparation of (meth)acrylate-based foams, in which a monomer mixture is polymerized in the presence of a blowing agent. The blowing agent used is a halogenated hydrocarbon. However, halogenated hydrocarbons have problems in that they are subject to significant environmental restrictions due to their severe adverse effect on the ozone layer. Furthermore, the described foams made only from (meth)acrylates, vinyl acetate, and chlorine-containing monomers do not have sufficient compressive strength.

[0009] EP 0068439 discloses the production of PMMA-based foams by polymerization of MMA in the presence of a blowing agent and subsequent foaming. To obtain the foam, 5% to 40% by weight of a plasticizer such as an alkyl methacrylate having at least 3 carbon atoms in the alkyl group is used. The use of hydrocarbons and / or hydrofluorocarbons as blowing agents is reported.

[0010] JP 2006-045256 A discloses the use of a monomer mixture containing 50% to 70% by mass of MMA, 14% to 30% by mass of (meth)acrylic acid, and 10% to 20% by mass of styrene, and urea as a foaming agent, to produce a thermoplastic acrylic foam.

[0011] Similarly, JP 2002-003635 A describes the use of a monomer mixture containing 50% to 75% by weight of MMA, 14% to 27% by weight of (meth)acrylic acid, and 10% to 20% by weight of styrene, and urea or a urea derivative as a blowing agent, to produce a thermoplastic acrylic foam.

[0012] JP 2013-203954 A discloses a method for producing an acrylic resin foam, which includes: (a) a step of preparing a polymerizable monomer containing maleic anhydride and methacrylamide, a blowing agent containing urea, and a polymerizable solution containing a polymerization initiator; (b) a step of polymerizing the polymerizable monomer mixture; and (c) a step of foaming the foamable polymer obtained in step (b). The blowing agent further includes an alcohol having a boiling point of 70°C to 180°C. Specifically, it is proposed to use a polymerizable monomer mixture containing 35% to 60% by mass of MMA, 14% to 35% by mass of (meth)acrylic acid, 10% to 20% by mass of styrene, and 1% to 10% by mass of maleic anhydride and methacrylamide.

[0013] Patent applications JP2006-045256, JP2002-003635, and JP2013-203954 all describe a styrene content of at least 10% by weight in the polymerizable composition. Styrene is considered to be "reasonably expected to be a human carcinogen." Therefore, where possible, the amount of styrene monomer used in the polymer composition is reduced to a minimum.

[0014] It was found that the use of styrene as one of the essential components of the monomer mixture significantly reduces the solubility of urea or urea derivatives used as blowing agents. Moreover, the polymerization rate also decreases. In addition, styrene reduces the weatherability of the resulting foam.

[0015] JP 55-139433 A describes a method for producing an acrylic foam containing 50% to 96% by weight of MMA, 4% to 35% by weight of acrylic acid and / or methacrylic acid as a comonomer, a urea blowing agent, and 0.05% to 4% by weight of water. The preferred amount of styrene monomer in the monomer mixture is less than 5% by weight. This patent application does not mention or suggest any means for further increasing the mechanical strength of the acrylic foam or the cast polymer used to produce it.

[0016] For all PMMA-based foams disclosed in the prior art, their compressive strength is generally too low for use in composite materials, especially in sandwich structures. For use as a core material in sandwich composites, the mechanical properties, especially the compressive strength, are very important, since they affect the manufacturing process of the sandwich elements and the mechanical properties of the sandwich elements.

[0017] assignment The problem to be solved by the present invention was to provide a novel method for producing PMMA-based foams which does not exhibit the drawbacks described in the prior art. In particular, the foamed PMMA-based material after production must be very resistant to mechanical stresses. The foam must have in particular a very high compressive strength. Furthermore, such PMMA-based foams must have a low density, preferably below 30 kg / m 3 ~350kg / m 3 The density of the material must be 1.

[0018] A further problem to be solved by the present invention was to provide a PMMA-based cast polymer that can be easily foamed while allowing a high degree of freedom in terms of defining the cell size, cell distribution and foam density. Such an unfoamed cast polymer should exhibit very good mechanical properties. In particular, the PMMA-based cast polymer should have an elastic modulus of at least 4500 MPa measured at room temperature.

[0019] A further problem to be solved by the present invention was to provide a suitable PMMA-based polymer which, as a foam, can be easily and simply bonded to a second material, for example in the form of an outer layer, by bonding with an adhesive, melting or by resin curing at the surface. For this purpose, it is also important that the resulting PMMA foam is compatible with the resin system or adhesive used in the production of the sandwich element.

[0020] solution The above technical problems are solved by a novel composition that can be used to produce PMMA-based cast polymers and, optionally, PMMA-based foams thereof.

[0021] In particular, in the course of careful experimentation, it was surprisingly found that the presence of insoluble hydrophilic inorganic compounds in the monomer mixture allows a significant increase in the mechanical strength of PMMA-based cast polymers. To achieve good compatibility of such hydrophilic inorganic compounds with the polymer matrix and sufficient distribution of such compounds, it was necessary to reduce the amount of styrene or its derivatives to less than 4% by weight.

[0022] The subject of the present invention is a composition for producing PMMA-based cast polymers, comprising 1% to 10% by weight of urea and / or urea derivatives, 0.001% to 2.0% by weight of an initiator, 0% to 20% by weight of an additional non-polymerizable blowing agent, 0% to 5% by weight of a chain transfer agent, 0.5% to 10% by weight of a hydrophilic inorganic compound essentially insoluble in the composition, and 53% to 98.498% by weight of a monomer mixture consisting of 60% to 95% by weight of MMA, 5% to 40% by weight of acrylic acid, methacrylic acid and / or itaconic acid, less than 4% by weight of styrene, α-methylstyrene and / or chlorostyrene, and 0% to 35% by weight of additional MMA copolymerizable monomers other than urea derivatives, characterized in that the inorganic hydrophilic compound has a methanol wettability of less than 30% by volume of methanol in a methanol / water mixture.

[0023] The term "methanol wettability" means in the context of the present invention that for the determination of methanol wettability as described in EP 2 515 829, in each case 0.2 g (± 0.005 g) of hydrophobic or hydrophobized particles are weighed into a transparent centrifuge tube. 8.0 ml of a methanol / water mixture containing 10%, 20%, 30%, 40%, 50%, 60%, 70% or 80% by volume of methanol is added to each sample. The tubes are shaken for 30 seconds and then immersed in water for 2500 minutes. -1 Centrifuge at 4°C for 5 min. Methanol wettability is defined as the volume percent of methanol that is 100% of the sediment volume. The higher the number, the more hydrophobic it is.

[0024] An essential component of the composition of the present invention is a hydrophilic inorganic compound that is essentially insoluble in the composition. The hydrophilic inorganic compound is selected from the group consisting of silica, metal oxides, metal hydroxides, metal silicates, talc, and mixtures thereof. The hydrophilic inorganic compound has an average diameter d of 5 to 1000 nm. 50 has.

[0025] particle size d 50 is determined in accordance with ASTM 690-1992.

[0026] The term "inorganic compound" in the context of the present invention means that there is at most one carbon atom in each molecule of the compound. Thus, in the context of the present invention, SiC is an inorganic compound, while Na2C2O4 is not.

[0027] The term "essentially insoluble" means, in the context of the present invention, that at least 90%, preferably at least 95%, more preferably at least 99% of the total amount of such hydrophilic inorganic compounds used in the composition remains in a particulate state and is not dissolved in the composition even after being present in the composition for at least 1 hour. Inorganic compounds that react with one or more components of the composition of the present invention are not "essentially insoluble". Thus, lithium oxide is not "essentially insoluble" because it reacts with the (meth)acrylic acid or itaconic acid present. The use of urea and / or urea derivatives as components of the composition is an essential part of the present invention and, in combination with other features, leads to a significant improvement in the mechanical properties of the resulting cast polymer and foams produced therefrom.

[0028] Urea derivatives present in the composition as alternatives to urea according to the invention are preferably N-alkylureas, such as N-methylurea, or N,N'-dialkylureas, such as N,N'-dimethylurea, unsubstituted or substituted 2-imidazolidones, such as 2-imidazolidone or N,N-dimethyl 2-imidazolidone, optionally further substituted 1-methyl-2-imidazolidinone and other cyclic urea derivatives.

[0029] In a further embodiment, the urea derivative is at least partially copolymerizable with the MMA urea derivative, in particular N-(2-methacryloyloxyethyl)ethylene urea. Hereinafter, to avoid any ambiguity regarding the overall composition, such that it is copolymerizable with the MMA urea derivative is not considered to be part of the monomer mixture.

[0030] The composition for producing a PMMA-based cast polymer comprises 1% by mass to 10% by mass, preferably 2% by mass to 8% by mass, particularly preferably 3% by mass to 7% by mass of urea and / or a urea derivative, 0.001% by mass to 2.0% by mass, preferably 0.002% by mass to 1.0% by mass, particularly preferably 0.003% by mass to 0.5% by mass of at least one initiator, 0% by mass to 20% by mass of an additional non-polymerizable foaming agent, 0% by mass to 5% by mass of a chain transfer agent, 0.5% by mass to 10% by mass, preferably 1% by mass to 8% by mass, particularly preferably 2% by mass to 6% by mass of a hydrophilic inorganic compound, and 53% by mass to 98.498% by mass, preferably 57% by mass to 96.999% by mass, more preferably 64.5% by mass to 95.997% by mass of a monomer mixture.

[0031] Likewise, the monomer mixture consists of 60% by weight to 95% by weight, preferably 70% by weight to 90% by weight, particularly preferably 75% by weight to 85% by weight of MMA, 5% by weight to 40% by weight, preferably 10% by weight to 30% by weight, particularly preferably 15% by weight to 25% by weight of acrylic acid, methacrylic acid and / or itaconic acid, less than 4% by weight, preferably less than 2% by weight, particularly preferably less than 1% by weight of styrene, α-methylstyrene and / or chlorostyrene and 0% by weight to 35% by weight, preferably 0% by weight to 20% by weight, particularly preferably 0% by weight to 10% by weight, very particularly preferably at least 0.1% by weight of additional MMA copolymerizable monomers other than urea derivatives.

[0032] Particularly preferably, the composition according to the present invention comprises 2% by mass to 8% by mass of urea and / or a urea derivative, 0.002% by mass to 2.0% by mass of an initiator, 0% by mass to 20% by mass of an additional non-polymerizable blowing agent, 0% by mass to 5% by mass of a chain transfer agent, 1% by mass to 8% by mass of a hydrophilic inorganic compound, and 57% by mass to 96.998% by mass of a monomer mixture comprising 70% by mass to 90% by mass of MMA, 10% by mass to 30% by mass of acrylic acid, methacrylic acid, and / or itaconic acid, less than 4% by mass of styrene, α-methylstyrene, and / or chlorostyrene, and 0% by mass to 35% by mass of MMA copolymerizable monomers other than urea derivatives.

[0033] Particularly preferably, the monomer mixture is essentially free of styrene, α-methylstyrene and / or chlorostyrene, i.e. the amount of styrene, α-methylstyrene and / or chlorostyrene is less than 0.1% by weight, more preferably less than 0.01% by weight, of the monomer mixture.

[0034] Although PMMA-based foams containing styrene and optionally maleic acid derivatives have proven to be mechanically very stable, it has been found that the proportion of styrene leads to incompatibility of the foam with certain resins, and therefore the foams produced from the compositions according to the invention are preferably free of styrene and maleic acid derivatives.

[0035] The optional additional MMA copolymerizable monomer in the monomer mixture may be a crosslinking agent. Such a crosslinking agent may in particular be ethylene glycol dimethacrylate, triallyl cyanurate, triallyl isocyanurate, and / or allyl methacrylate. Further alternatives are di(meth)acrylates, tri(meth)acrylates, or tetra(meth)acrylates. Any crosslinking agent present may be a mixture containing at least two of these crosslinking agents. However, preferably a high degree of covalent crosslinking is not desired.

[0036] The monomer mixture present in the composition of the present invention preferably comprises at least 0.1% by weight of additional MMA copolymerizable monomers, which are crosslinkers, in particular ethylene glycol dimethacrylate, triallyl cyanurate, triallyl isocyanurate, allyl methacrylate, or mixtures thereof.

[0037] Additional optional MMA copolymerizable monomers may be alkyl acrylates. These alkyl acrylates are preferably alkyl acrylates having 1 to 8 carbon atoms in the alkyl radical, particularly preferably ethyl acrylate, n-propyl acrylate or n-butyl acrylate. Acrylates as repeat units in the polymer increase in particular the thermal stability of the polymer.

[0038] Monomers optionally present in addition to MMA may also or additionally include alkyl methacrylates other than MMA. Such alkyl methacrylates are in particular those having 2 to 8 carbon atoms in the alkyl radical. In particular, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate or 2-ethylhexyl methacrylate are preferred.

[0039] Further advantageously usable monomers from this category are in particular hydroxyl-functional alkyl (meth)acrylates. These are preferably 2-hydroxyethyl (meth)acrylate or 3-hydroxypropyl (meth)acrylate.

[0040] The monomer mixture preferably contains 5% to 10% by weight of tert-butyl methacrylate, isopropyl methacrylate, tert-butyl acrylate, and / or isopropyl acrylate.

[0041] The monomer mixture may optionally contain an N-alkyl(meth)acrylamide having 1 to 12 carbon atoms in the alkyl group, and may not contain methacrylamide or N,N-dialkylmethacrylamide as an MMA copolymerizable monomer. The N-alkyl(meth)acrylamide is particularly preferably N-methylol methacrylamide, 2-hydroxypropyl methacrylamide, or N-isopropyl methacrylamide, and particularly preferably N-isopropyl methacrylamide.

[0042] Such N-alkyl(meth)acrylamides entail great advantages, for example in terms of their subsequent bonding with outer layers to obtain sandwich components or other composites, and also overall better processability with regard to adhesive bonding, welding or surface resin curing, which is especially true when the foam of the invention does not contain styrene or maleic acid derivatives.

[0043] The chain transfer agent optionally present in the composition of the invention is preferably a compound having 1 to 5 mercaptan groups, γ-terpinene, or a mixture of at least two of these chain transfer agents.The chain transfer agent is particularly preferably pentaerythritol tetrathioglycolate, 2-mercaptoethanol, an alkyl mercaptan having 2 to 12 carbon atoms, thioglycolic acid, thioglycolate, γ-terpinene, or a mixture of at least two of these chain transfer agents.

[0044] Particularly suitable non-copolymerizable blowing agents other than urea or urea derivatives are preferably n-heptane, MTBE, methyl ethyl ketone, alcohols having 1 to 4 carbon atoms, such as tert-butanol, water, methylal and / or tert-butyl methyl ether.

[0045] The composition may also include additional ingredients, examples of which include release agents, waxes, pigments, stabilizers, especially UV stabilizers, and / or adhesion promoters.

[0046] A further object of the invention is a PMMA-based cast polymer obtained by polymerization of the composition according to the invention.

[0047] Another object of the invention is a process for producing a PMMA-based cast polymer, in which the composition according to the invention is polymerized at a temperature between 20° C. and 100° C., as described above.

[0048] Optionally, all of the composition or part of the composition may be in polymeric and / or oligomeric form to an extent of up to 80% by weight at the start of polymerization, which is known as the "syrup process" and is described in more detail below.

[0049] When oligomers or polymers are used, the polymerization is a so-called syrup polymerization, which has been shown to be particularly useful in the casting process between two plates. At the end of such a syrup polymerization, two PMMAs with different compositions can be present simultaneously as a mixture in the cast polymer or in the moulding or foam produced therefrom, without any foaming-related effects.

[0050] The polymerization process is preferably carried out in the form of bulk polymerization at a temperature between 20°C and 100°C, preferably between 30°C and 70°C.

[0051] A further object of the invention is a PMMA-based foam obtainable by foaming of the cast polymer of the invention or by foaming of an at least partially polymerized composition according to the invention.

[0052] The PMMA-based foam preferably has a compressibility of 30 kg / m2, determined according to DIN EN ISO 1183 (issue: 2013-04). 3 ~350kg / m 3 , particularly preferably 50 to 300 kg / m 3 has a density of

[0053] Another object of the invention is a process for the preparation of PMMA-based foams according to the invention, in which the composition of the invention is polymerized at a temperature between 20°C and 100°C and subsequently foamed at a temperature between 130°C and 250°C.

[0054] The foaming is preferably carried out at a temperature of 130° C. to 250° C., more preferably 150° C. to 230° C., depending on the foaming agent used.

[0055] The polymerization and / or foaming is preferably carried out in stages at different temperatures. Alternatively, or in addition, it is possible for the polymerization and foaming to be carried out at least partly simultaneously.

[0056] In such a simultaneous mode, the process can optionally be carried out in particular such that the polymerization is only incomplete, preferably to at least 80% conversion, with the final polymerization being carried out during foaming. Such a process has the advantage that the monomers remaining at the start of the foaming procedure have a plasticizing effect, and no plasticizing compounds remain in the finished foam. Thus, in such an embodiment, polymerization and foaming will be carried out partly simultaneously at one foaming temperature.

[0057] The polymerization is preferably carried out in a shape-imparting vessel, in particular in the form of a chamber polymerization between two plates, for example glass plates. In the simplest case, for example a rectangular vessel may be involved. Polymerization in such a vessel subsequently results in a sheet whose thickness is determined by the filling level in the tank / plate spacing. However, more complex vessel shapes are also conceivable. The polymerization is preferably carried out at temperatures between 30°C and 70°C. Usable initiators include well-known free radical initiators, such as for example peroxide or azo initiators, but also redox-based or UV initiators.

[0058] In particular, these redox systems and UV initiators are applied at polymerization temperatures below 40° C. UV initiators are initiated by irradiation with a suitable UV light, while redox initiators include two-component systems that are initiated by mixing the two components with a monomer.

[0059] Foaming can then take place in the same container. In that case, the increase in volume is limited to one direction, the open side of the container. However, the polymerized material can also be foamed without enclosure or in suspended form. Foaming is preferably carried out in an oven. As an alternative, foaming can also be achieved by irradiation with IR radiation, in particular radiation having a wavelength in the range 0.78-2.20 μm, preferably in the range 1.20-1.40 μm. A further alternative is foaming by microwaves. A combination of different methods, such as IR radiation, microwaves and / or heating in an oven, is also conceivable.

[0060] The foaming and polymerization can be carried out in multiple temperature stages, each as previously described. The temperature can be increased in the latter stages of the polymerization to further increase the conversion and thereby reduce the residual monomer content. The foaming temperature can be increased in stages during foaming to affect the cell distribution, cell size, and cell count.

[0061] Surprisingly, it has been found that using the composition according to the invention it is possible to obtain PMMA-based polymers having an elastic modulus of more than 4500 MPa, measured at room temperature, in comparison with pure PMMA cast polymers having an elastic modulus in the range of 2800-3300 MPa.

[0062] The PMMA-based foams produced according to the invention have a surprisingly high strength combined with a surprisingly low brittleness and can therefore be useful, for example, in lightweight construction. Furthermore, due to the excellent material properties, it is not necessary to use plasticizers, such as, for example, relatively long-chain alkyl (meth)acrylates or phthalates, which, according to current knowledge, have a positive effect on the flowability or foamability, but at the same time have a negative effect on the mechanical properties of the PMMA foam, especially its strength.

[0063] It has been found that for the same cell structure as described in the prior art, foams made from a polymer with elastic modulus X, where X>Y, exhibit better mechanical properties than foams made from a polymer with elastic modulus Y. A high elastic modulus of the polymer is therefore a prerequisite for obtaining foams with good mechanical properties.

[0064] The PMMA-based cast polymers produced according to the invention can be used in a variety of different applications. Examples of such applications include filled or transparent mouldings and glazing in advertising materials, for film production, in elements of architectural construction, as diffusers for lighting applications, in furniture construction, in shipbuilding, in vehicle construction, in the aerospace industry or in model building. It is particularly preferred if said polymers are also used to produce the PMMA foams of the invention.

[0065] The PMMA-based foams produced according to the invention can also find a very wide variety of applications: examples of such applications are as weatherproof insulation materials or core materials for sandwich composites, in wind power plant blades, in shipbuilding and subsea applications, in lightweight structures, as packaging materials, as energy absorbers in crash elements, in building construction elements, as diffusers for lighting applications, in furniture construction, in vehicle construction, in the aerospace industry or in model construction.

[0066] Working Example The PMMA polymer was produced by a casting process: for this purpose, the monomer solution was filled into a glass chamber consisting of two glass plates (400 × 300 mm) held apart and sealed with a sealing tape (13 mm thick).

[0067] To prepare the monomer solution, the ingredients were added together according to the formulation set forth below (Tables 1-4) and stirred until all ingredients were dissolved.

[0068] The glass chambers thus prepared and filled were kept in a water bath at 40° C. for polymerization. After about 27 hours, the glass chambers were subjected to a final polymerization at 115° C. After that, the glass plates and sealing ropes were removed. In all cases, a hard translucent polymer was obtained.

[0069] AEROSIL® OX50 (manufacturer: Evonik Resource Efficiency GmbH) was used as the hydrophilic inorganic compound.

[0070] Tensile tests to determine the elastic modulus of the polymers were performed using a Zwick / Roell Z030 instrument. Measurements were performed under standard conditions of 23°C and 50% humidity. Samples were stored for at least 16 hours under the same conditions (23°C - 50% humidity) before measurements. The results are shown in Table 5.

[0071] [Table 1]

[0072] [Table 2]

[0073] [Table 3]

[0074] [Table 4]

[0075] [Table 5]

[0076] Table 5 shows the results of measuring the modulus of elasticity of the polymers produced in Example 1 and Comparative Examples 1-3. The polymer produced without the use of urea as a blowing agent and silica as a filler (Comparative Example 2) shows the lowest modulus of elasticity. The use of both urea and silica but without styrene (Example 1) shows the best results. The use of urea, silica and styrene gives worse results than Example 1 (Comparative Example 1), as does the use of urea without silica (Comparative Example 3).

Claims

1. 1. A composition for producing PMMA-based cast polymers, comprising 1% to 10% by weight of urea and / or urea derivatives, 0.001% to 2.0% by weight of an initiator, 0% to 20% by weight of an additional non-polymerizable blowing agent, 0% to 5% by weight of a chain transfer agent, 0.5% to 10% by weight of a hydrophilic inorganic compound that is essentially insoluble in the composition, and 53% to 98.498% by weight of a monomer mixture, the monomer mixture consisting of 60% to 95% by weight of MMA, 5% to 40% by weight of acrylic acid, methacrylic acid, and / or itaconic acid, and 0% to 35% by weight of additional MMA copolymerizable monomers other than urea derivatives, the hydrophilic inorganic compound having a methanol wettability of less than 30% by volume of methanol in a methanol / water mixture, and the monomer mixture being essentially free of styrene, alpha-methylstyrene, and / or chlorostyrene.

2. 2. The composition according to claim 1, characterized in that the composition comprises 2% to 8% by weight of urea and / or urea derivatives, 0.002% to 1.0% by weight of an initiator, 0% to 20% by weight of an additional non-polymerizable blowing agent, 0% to 5% by weight of a chain transfer agent, 1% to 8% by weight of a hydrophilic inorganic compound, and 57% to 96.999% by weight of a monomer mixture, the monomer mixture consisting of 70% to 90% by weight of MMA, 10% to 30% by weight of acrylic acid, methacrylic acid, and / or itaconic acid, and 0% to 35% by weight of an additional MMA copolymerizable monomer other than a urea derivative.

3. 3. The composition of claim 1, wherein the hydrophilic inorganic compound is selected from the group consisting of silica, metal oxides, metal hydroxides, metal silicates, talcum, and mixtures thereof.

4. The hydrophilic inorganic compound has an average diameter d of 5 to 1000 nm as determined in accordance with ASTM 690-1992. 50 4. The composition according to claim 1, wherein the composition comprises:

5. 5. The composition according to claim 1, wherein the monomer mixture comprises at least 0.01% by weight of additional MMA copolymerizable monomers, which are crosslinkers, in particular ethylene glycol dimethacrylate, triallyl cyanurate, triallyl isocyanurate, allyl methacrylate, or mixtures thereof.

6. The composition according to any one of claims 1 to 5, characterized in that the urea derivative is selected from the group consisting of N-alkyl ureas, N,N'-dialkyl ureas, 2-imidazolidone, 1-methyl-2-imidazolidinone, and mixtures thereof.

7. 7. The composition according to claim 1, wherein the urea derivative is at least partially copolymerizable with an MMA urea derivative, in particular with N-(2-methacryloyloxyethyl)ethylene urea.

8. The composition according to any one of claims 1 to 7, characterized in that the monomer mixture comprises 5% to 10% by weight of tert-butyl methacrylate, isopropyl methacrylate, tert-butyl acrylate, and / or isopropyl acrylate.

9. A PMMA-based cast polymer obtainable by polymerization of the composition according to any one of claims 1 to 8.

10. A process for the preparation of PMMA-based cast polymers, characterized in that the composition according to any one of claims 1 to 8 is polymerized at a temperature between 20°C and 100°C.

11. 10. A PMMA-based foam obtainable by foaming of a cast polymer according to claim 9 or by foaming of an at least partially polymerized composition according to any one of claims 1 to 8.

12. The foam has a compressibility of 30 kg / m2, determined in accordance with DIN EN ISO 1183. 3 ~350kg / m 3 12. The PMMA-based foam of claim 11 having a density of

13. 13. A process for producing PMMA-based foams according to any one of claims 11 to 12, characterized in that the composition according to any one of claims 1 to 8 is polymerized at a temperature between 20°C and 100°C and subsequently foamed at a temperature between 130°C and 250°C.

14. 14. The method of claim 13, wherein the polymerizing and foaming are at least partially simultaneous.

Citation Information

Patent Citations

  • Production of acrylic foam

    JP1980139433A

  • Production of Microporous PMMA Foams by Using a Nucleating Agent

    JP2018510248A