Corrosion resistance evaluation method for submerged entry nozzle
The rotary erosion test method for immersion nozzles addresses the challenge of simulating wear factors by dividing the nozzle into parts and evaluating wear resistance, ensuring accurate prediction of corrosion and erosion resistance for continuous casting processes.
Patent Information
- Application Number
- JP2020172123
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-12
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-10-12
AI Technical Summary
Existing methods for evaluating the corrosion resistance of immersion nozzles in continuous casting processes are inadequate in accurately simulating the wear and tear caused by multiple factors, particularly mold powder components and viscosity, which change over time, limiting the number of moldings and requiring a highly corrosion-resistant material.
A rotary erosion test method is employed where the immersion nozzle is divided into multiple parts, subjected to a mixture of molten steel and mold powder, and the erosion resistance is evaluated by measuring wear area and rate, accounting for changes in mold powder components and viscosity.
The method accurately evaluates the corrosion resistance of immersion nozzle materials, predicting wear and tear on actual machines with high precision, enabling efficient selection of materials that resist corrosion and erosion.
Smart Images

Figure 0007553794000004 
Figure 0007553794000009 
Figure 0007553794000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for evaluating the corrosion resistance of a submerged entry nozzle, specifically, to a method for evaluating the corrosion resistance of a powder line part material and the corrosion damage to the submerged entry nozzle by each mold powder. [Background technology]
[0002] In order to reduce steelmaking costs, it is desirable to develop technologies for improving the durability of refractories, such as submerged entry nozzles, used in the continuous casting process, and for protecting refractories by slag coating. To achieve this, it is essential to establish methods for evaluating refractories and slag that are compatible with the operating environment of actual furnaces.
[0003] Methods for evaluating the corrosion resistance of various refractories include, for example, the high-frequency induction furnace lining method and the rotary erosion method, which involve melting slag and steel at high temperatures, bringing the molten material into contact with the refractory for a certain period of time, and comparing the amount of wear on the refractory to evaluate its durability.
[0004] The high-frequency induction furnace lining method allows comparative testing of many samples at once, and also allows for atmospheric control, making it possible to reproduce melting damage close to that of an actual furnace in many cases. The rotary erosion method is a test in which refractory is lined inside an iron drum, and slag and iron are melted inside and reacted with the refractory. An appropriate amount of a mixed gas of oxygen and propane is supplied, and the heat is used to bring the temperature of the refractory surface to the specified test temperature. This test is widely conducted because the sample shape is relatively small, the furnace is easy to build and dismantle, and the equipment is simple.
[0005] Patent Document 1 discloses a method for testing the corrosion of refractory samples, in which a refractory sample is fixed to the inner surface of a rotating drum with a pedestal refractory material so that the cross-sectional outer shape is a regular polygon with at least a hexagon, a corrosive agent is added, and the drum is rotated.
[0006] Patent Document 2 discloses a method for evaluating the corrosion resistance of a refractory material by lining the inside of a drum with refractory material, repeatedly charging and discharging slag and / or molten iron into the drum for a predetermined period of time, and then measuring the remaining thickness of the refractory material inside the drum. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2000-9633 A [Patent Document 2] JP 2002-5578 A Summary of the Invention [Problem to be solved by the invention]
[0008] The submerged entry nozzle used in the continuous casting process is a refractory nozzle-shaped nozzle that pours molten steel into a mold. The durability of the powder line part of the submerged entry nozzle is an issue, and this can limit the number of consecutive castings (the number of batches in which multiple batches of molten steel are continuously cast).
[0009] The powder line of the SEN is a three-phase region where the mold powder used as a lubricant and molten steel exist, and since it is a part that is prone to wear, the refractory material for the SEN needs to be highly corrosion-resistant. Also, in order to increase the number of consecutive runs, it is necessary to select a mold powder that does not easily react with the refractory material.
[0010] Therefore, erosion tests are being conducted in which the refractory material used in the submerged entry nozzle is processed into a block, which is then lined on the inner surface of a rotating drum, and an erosion agent is poured into the drum before the drum is rotated.
[0011] However, wear in the powder line is affected by multiple factors, such as mold powder components, mold powder viscosity, molten steel components, molten steel flow rate, refractory materials, and antioxidants, and it was difficult to determine the degree of influence of each factor even after investigating the actual equipment in use.
[0012] In addition, even if the influence of each factor was evaluated by the conventional laboratory evaluation method, it was difficult to simulate the wear of the actual machine. In particular, the influence of the components and viscosity of the mold powder could not be evaluated accurately because the components and viscosity change with the passage of the test time in the conventional test method.
[0013] In view of the above circumstances, an object of the present invention is to provide a method for evaluating the corrosion resistance of an immersion nozzle, which can more accurately and efficiently evaluate the corrosion resistance of the powder line part material and the melting damage to the immersion nozzle by each mold powder. [Means for solving the problem]
[0014] In this invention, by using a rotational erosion test method that allows for the discharge and introduction of mold powder during testing, the effect of changes in the mold powder components is reduced, and further, by processing the submerged entry nozzle used in the actual machine and placing it as a test sample, it is possible to evaluate the effects of the lining used in the actual machine (the effects of antioxidants and material boundaries), etc., making it a test method that is close to the wear and tear of the actual machine. The gist of this invention is as follows.
[0015] (1) A method for evaluating the corrosion resistance of an immersion nozzle, which comprises lining a drum with samples, pouring in an erosive material, and rotating the drum, wherein the samples used are three or more samples obtained by dividing the immersion nozzle into a plurality of pieces, a mixture of molten steel and mold powder is used as the erosive material, the erosive material is repeatedly poured into the drum and discharged at predetermined intervals, the worn area of the immersion nozzle is measured, and the corrosion resistance is evaluated.
[0016] (2) A method for evaluating the corrosion resistance of an immersion nozzle, comprising: evaluating a plurality of types of mold powders having different components based on the method for evaluating the corrosion resistance of an immersion nozzle described above in (1); relatively comparing the wear rates and / or wear amounts; and evaluating the erosion resistance of each component of the mold powder.
[0017] (3) A method for evaluating the corrosion resistance of a submerged entry nozzle, comprising estimating the wear rate and / or the wear amount during actual use from the components of the mold powder using a correlation between the wear rate and / or the wear amount obtained by the method for evaluating the corrosion resistance of a submerged entry nozzle described in (2) above and a powder basicity Bi that can be calculated from the components of the mold powder. Effect of the Invention
[0018] According to the method for evaluating the corrosion resistance of an immersion nozzle of the present invention, changes in the components and viscosity of the mold powder over time can be prevented, and the corrosion resistance of the powder line material and the damage caused to the immersion nozzle by each mold powder can be evaluated more accurately and efficiently. [Brief description of the drawings]
[0019] [Figure 1] FIG. 1 is a diagram showing a drum lined with a submerged entry nozzle in the method for evaluating the corrosion resistance of a submerged entry nozzle of the present invention. [Diagram 2] FIG. 1 is a diagram showing an example of a combination of submerged entry nozzles in the method for evaluating the corrosion resistance of a submerged entry nozzle of the present invention. [Diagram 3] FIG. 2 is a diagram for explaining the circumferential length of the operating surface when the submerged entry nozzle is assembled in the method for evaluating the corrosion resistance of the submerged entry nozzle of the present invention. [Figure 4] FIG. 2 is a diagram illustrating the shape of an evaluation sample used in the examples. [Diagram 5] FIG. 1 is a diagram showing an example of the actual size and the location of damage in a method for evaluating the corrosion resistance of a submerged nozzle. [Figure 6] FIG. 1 is a graph showing an example of the relationship between powder basicity and wear rate determined using the method for evaluating the corrosion resistance of a submerged entry nozzle of the present invention, and an example of the relationship between powder basicity and wear rate determined using a conventional method for evaluating the corrosion resistance of a submerged entry nozzle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be described in detail below.
[0021] The method for evaluating the corrosion resistance of a submerged entry nozzle of the present invention is a method in which a sample, which is a submerged entry nozzle used in an actual machine divided into several pieces, is lined inside a drum (castable refractory material), an erosive material is introduced, and the drum is rotated to wear down the sample, and the worn area is measured to evaluate the corrosion resistance.
[0022] As shown in Figure 1, three or more halved submerged nozzles 1 are lined inside a drum 2. The drum 2 is held by a holding device (not shown), and a rotatable rotary furnace is formed by a rotating device configured in an appropriate manner, such as a manual type, an electric type using a motor, or a hydraulic type. If an inverter is installed in the rotary furnace to enable control of the rotation speed, it is preferable because it also makes it possible to evaluate the effect of the flow rate.
[0023] Molten steel and mold powder mixed at a specified ratio are charged into drum 2. In the present invention, by using a rotational erosion test method in which drum 2 is tilted during the test and erosive materials can be discharged and recharged at a specified time, the effects of changes in the mold powder composition are reduced and an evaluation close to the wear of the powder line part of the submerged entry nozzle used in the actual machine can be performed.
[0024] In addition, by dividing the submerged entry nozzle used in the actual machine in half and arranging it as a sample, it becomes possible to evaluate the effect of the lining used in the actual machine (the effect of the antioxidant on the nozzle surface and the effect of the material boundary). Although dividing in half is the most preferable considering the time required for processing and the arrangement in the drum, the submerged entry nozzle may be divided into three or more pieces and arranged.
[0025] For heating the sample and the erosive material, for example, a burner can be used.
[0026] An example of a combination of SENs in the corrosion resistance evaluation method of the present invention is shown in Figure 2. By arranging the SENs split in half as shown in Figure 2, the corrosion material comes into contact with the outer surface of the SENs, making it possible to conduct tests in an environment close to that of an actual machine.
[0027] 3 is a diagram illustrating the circumferential length of the working surface of the combined submerged entry nozzle in the method for evaluating the corrosion resistance of the submerged entry nozzle of the present invention. The number of combined submerged entry nozzles is N, the outer diameter of the submerged entry nozzle is R, and the angle of the working range is θ. The submerged entry nozzles can be processed and arranged so that their circumferential length L satisfies the following formula:
[0028] L≧πR×θ / 360
[0029] θ is calculated using the following formula:
[0030] θ = {(N-2) × 180} / N (N≧3)
[0031] In the present invention, the submerged nozzle that has been worn as described above is observed, the worn area is measured, and the corrosion resistance is evaluated.
[0032] Wear area (mm 2 ) and divide it by the test time to obtain the wear rate (mm 2 / min) can be obtained. Also, by dividing it by the amount of powder, the amount of wear (mm 2 / g) can be obtained. By comparing the obtained value with the results of the base powder and the material of the submerged entry nozzle, it is possible to evaluate the effect of the components regardless of the test time. The wear depth (mm) may be used instead of the wear area.
[0033] By conducting similar evaluation tests on multiple types of molding powders with different components and comparing the amount and speed of wear, it is possible to evaluate the effect of each component of the molding powder on wear.
[0034] Furthermore, by checking the correlation between the wear rate and the wear amount obtained by the evaluation method of the present invention using the powder basicity Bi calculated from the components of the mold powder, a linear correlation can be obtained with high accuracy, so that the wear of the powder line portion can be estimated by organizing using the powder basicity Bi.
[0035] The material of the submerged entry nozzle to be used in the method for evaluating the corrosion resistance of the submerged entry nozzle of the present invention is not particularly limited as long as it is a refractory material used in the submerged entry nozzle, such as silica, clay, pyrolite, zircon and zirconia, high alumina, carbon, silicon carbide, chromium, magnesia, magnesia-chromium, dolomite, magnesia-carbon, alumina-carbon, alumina-silicon carbide-carbon, and alumina-magnesia-carbon.
[0036] Furthermore, there is no particular limitation on the components of the molten steel and mold powder used as the erosive material, and any components that are used in steelmaking can be used.
[0037] There is no particular limitation on the method of adding the erosive material. The first erosive material can be added after the temperature of the sample reaches about 1550° C. For example, the erosive material can be added first by adding steel, and then adding the mold powder after the steel is melted.
[0038] The slag can be removed when the reaction between the corrosive material and the sample has subsided. For example, after the mold powder is added, the slag can be removed 15 to 30 minutes later, and then the steel and mold powder can be added again.
[0039] The present invention is applied to an oxidizing atmosphere or an Ar, N 2 , He, H 2 The method can be applied under any heating conditions, including heating in a non-oxidizing atmosphere such as under a vacuum. An oxidizing atmosphere or a mixed atmosphere of oxygen and an inert gas such as Ar is preferable because the wear can be reproduced more accurately by controlling the oxygen partial pressure.
[0040] The heating means may be burner heating, induction heating, electric resistance heating, arc heating, etc. The gas used for burner heating may be any of propane-oxygen, methane-oxygen, coke oven gas, etc. A more stable evaluation can be performed by measuring the surface temperature of the submerged nozzle with a radiation thermometer and controlling the heating conditions.
[0041] According to the method for evaluating the corrosion resistance of a submerged entry nozzle of the present invention, a high correlation can be obtained with the operation of an actual machine, and therefore the wear of the actual machine can be accurately predicted by the evaluation method of the present invention. EXAMPLES
[0042] The present invention will be described below with reference to examples, although the present invention is not limited to these examples.
[0043] [Example 1] Samples were prepared for use in the method for evaluating the corrosion resistance of the SEN of the present invention, and for use in the conventional method for evaluating the corrosion resistance of refractories. The samples are shown in Figure 4. (a) is a sample made by dividing the SEN used in the actual equipment of the present invention, and (b) and (c) are samples made by processing the refractory used in the SEN of the conventional method into blocks. The number of processing steps and preparation time are shown in Table 1.
[0044] [Table 1]
[0045] As shown in Table 1, it was confirmed that the method of the present invention makes it easy to process the samples and greatly reduces the time required.
[0046] [Example 2] Using the specimen of the present invention shown in Fig. 4(a) and the specimen of the conventional method shown in Fig. 4(b), corrosion materials (molten steel and mold powder) were placed in the drum and the drum was rotated to evaluate the corrosion of the SEN. The test conditions are shown in Table 2.
[0047] [Table 2]
[0048] The corrosion materials were charged by first charging the steel, and then charging the mold powder after the steel had melted (within about 5 minutes of charging). The first steel was charged when the temperature of the sample reached 1550°C, and the slag was removed 20 minutes after the steel was charged. The test time of 60 minutes was the time from the first steel was charged to the last slag being removed.
[0049] After the test, the sample was cut and the area that had been worn out was calculated relative to the original size, and the wear rate (mm 2 An example of the original dimensions and location of wear is shown in Figure 5. The evaluation results are shown in Table 3 and Figure 6.
[0050] [Table 3]
[0051] It has been known from wear in actual equipment and known literature that the wear rate increases as the powder basicity Bi increases. As the above results show, it was confirmed that the wear rate of the submerged entry nozzle was evaluated with good accuracy by the method of the present invention. On the other hand, the evaluation by the conventional method showed an unclear correlation between the powder basicity and the wear rate, and the evaluation accuracy was inferior to that of the present invention. [Explanation of symbols]
[0052] 1 Submerged nozzle 2 Drums
Claims
1. A method for evaluating corrosion resistance of a submerged entry nozzle, comprising lining a drum with a sample, introducing an erosive material into the drum, and rotating the drum, As the sample, three or more samples obtained by dividing the submerged nozzle into a plurality of pieces are used, A mixture of molten steel and mold powder is used as the erosive material. The process of introducing the erosive material into the drum and discharging the slag is repeated by introducing the erosive material into the drum, discharging the erosive material after 15 to 30 minutes, and introducing the erosive material again. The wear area of the above submerged nozzle is measured and the corrosion resistance is evaluated. The method for evaluating the corrosion resistance of a submerged nozzle is characterized by:
2. A method for evaluating the corrosion resistance of an immersion nozzle, comprising: evaluating a plurality of types of mold powders having different components based on the method for evaluating the corrosion resistance of an immersion nozzle according to claim 1; relatively comparing the wear rates and / or the amounts of wear; and evaluating the corrosion resistance of each component of the mold powder.
3. 3. A method for evaluating the corrosion resistance of a submerged entry nozzle, comprising: estimating the wear rate and / or the wear amount during actual use from the components of the mold powder using a correlation between the wear rate and / or the wear amount obtained by the method for evaluating the corrosion resistance of a submerged entry nozzle according to claim 2 and a powder basicity Bi that can be calculated from the components of the mold powder.
Citation Information
Patent Citations
Continuously casting steeping nozzle
JP1982051172A
Mold additive for continuously casting steel and continuously casting method
JP1993269560A
Immersion nozzle for continuous casting
JP1993329592A
Immersion nozzle for continuous casting
JP1995060418A
Zirconia-graphite refractory excellent in corrosion resistance and nozzle for continuous casting using the same