AI Technical Summary
Existing grain-oriented electrical steel sheets face challenges in achieving sufficient adhesion of insulating coatings without a forsterite coating, which is necessary to reduce iron loss, and there is a demand for coatings that do not contain chromic acid compounds due to environmental concerns.
A grain-oriented electrical steel sheet with a specific composition and structure, including a Si-based oxide film as an intermediate layer and a phosphoric acid-based coating that contains crystalline cristobalite-type aluminum phosphate, ensuring excellent adhesion without a forsterite coating and avoiding chromate.
The solution provides improved film adhesion and reduced iron loss by applying tension to the base steel plate, maintaining high crystallinity of the phosphoric acid coating, and ensuring uniform crystallization across its surface and interior regions, thereby enhancing the electrical properties of the steel sheet.
Smart Images

Figure 0007553869000010 
Figure 0007553869000008 
Figure 0007553869000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a grain-oriented electrical steel sheet. [Background technology]
[0002] Grain-oriented electrical steel sheets are mainly used in transformers. Since transformers are continuously excited and generate energy loss over a long period from installation to disposal, the energy loss when magnetized with AC, i.e., core loss, is a major index that determines the performance of a transformer.
[0003] Many methods have been proposed to reduce the iron loss of grain-oriented electrical steel sheets. For example, the Goss orientation, {110} <001> These include techniques to increase the concentration in a certain orientation, techniques to increase the content of solid solution elements such as Si that increase the electrical resistance of steel sheets, and techniques to reduce the thickness of steel sheets.
[0004] It is also known that applying tension to steel sheets is an effective method for reducing iron loss. Therefore, a coating is usually formed on the surface of grain-oriented electrical steel sheets in order to reduce iron loss. This coating applies tension to the grain-oriented electrical steel sheets, thereby reducing the iron loss of each steel sheet. This coating further ensures electrical insulation between the steel sheets when the grain-oriented electrical steel sheets are stacked for use, thereby reducing the iron loss of the steel core.
[0005] An example of a grain-oriented electrical steel sheet having a coating is one in which a forsterite coating, which is an oxide coating containing Mg, is formed on the surface of a base steel sheet, and an insulating coating is further formed on the surface of the forsterite coating. In other words, in this case, the coating on the base steel sheet includes a forsterite coating and an insulating coating. Each of the forsterite coating and the insulating coating has both an insulating function and a function of applying tension to the base steel sheet.
[0006] The forsterite coating is formed during the finish annealing, which causes secondary recrystallization in the steel sheet, by a reaction between an annealing separator mainly composed of magnesia (MgO) and silicon oxide (SiO2) formed on the base steel sheet during decarburization annealing, during heat treatment at 900 to 1200°C for 30 hours or more.
[0007] The insulating coating is formed by applying a coating solution containing, for example, phosphoric acid or a phosphate, colloidal silica, and chromic anhydride or a chromate to the steel sheet after finish annealing, and baking and drying at 300 to 950°C for 10 seconds or more.
[0008] In order for these coatings to exert their functions of insulation and tensioning the base steel sheet, high adhesion is required between the coating and the base steel sheet.
[0009] Conventionally, the adhesion has been ensured mainly by the anchor effect of the unevenness at the interface between the base steel sheet and the forsterite coating. However, in recent years, it has become clear that the unevenness at the interface hinders the magnetic domain wall movement when the grain-oriented electrical steel sheet is magnetized, and is a factor preventing low iron loss.
[0010] Therefore, in order to further reduce iron loss, a technique has been proposed in, for example, Patent Documents 1 and 2 in which an insulating coating is formed on the base steel sheet while the surface of the base steel sheet is smooth, without the presence of a forsterite coating on the base steel sheet.
[0011] In the manufacturing method of grain-oriented electrical steel sheet disclosed in Patent Document 1, the forsterite film is removed by pickling or the like, and the surface of the base steel sheet is smoothed by chemical polishing or electrolytic polishing. In the manufacturing method of grain-oriented electrical steel sheet disclosed in Patent Document 2, an annealing separator containing alumina (Al2O3) is used during finish annealing to suppress the formation of the forsterite film itself and smooth the surface of the base steel sheet.
[0012] However, the manufacturing methods of Patent Documents 1 and 2 had a problem in that when an insulating coating is formed in contact with the surface of the base steel plate (directly on the surface of the base steel plate), the insulating coating has difficulty adhering to the surface of the base steel plate (sufficient adhesion cannot be obtained).
[0013] In view of this, in order to ensure coating adhesion, techniques have been proposed in, for example, Patent Documents 3 and 4 for improving the adhesion of the insulating coating by controlling the morphology of the insulating coating or by controlling the morphology of the intermediate layer formed between the base steel sheet and the insulating coating.
[0014] In the grain-oriented electrical steel sheet disclosed in Patent Document 3, the insulating coating has a crystalline phosphide-containing layer that contains crystalline phosphide. In the grain-oriented electrical steel sheet disclosed in Patent Document 4, when the insulating coating is subjected to X-ray diffraction using a Co-Kα excitation source, the FWHM-Co, which is the half-width of the peak appearing at 2θ=24.8°, is 2.5° or less. [Prior art documents] [Patent documents]
[0015] [Patent Document 1] Japanese Patent Application Publication No. 49-096920 [Patent Document 2] International Publication No. 2002 / 088403 [Patent Document 3] International Publication No. 2019 / 013353 [Patent Document 4] International Publication No. 2019 / 013348 Summary of the Invention [Problem to be solved by the invention]
[0016] As described above, smoothing the surface of the base steel sheet of the grain-oriented electrical steel sheet is effective in reducing the iron loss of the grain-oriented electrical steel sheet. However, smoothing the surface of the base steel sheet reduces the adhesion of the insulating coating.
[0017] The techniques disclosed in Patent Documents 1 and 2 do not provide sufficient coating adhesion. In addition, the techniques disclosed in Patent Documents 3 and 4 certainly improve coating adhesion, but the inventors' investigations have revealed that there is still room for further improvement in terms of coating adhesion.
[0018] Furthermore, insulating coatings for grain-oriented electrical steel sheets generally contain chromates, and the use of chromate is also envisaged in the technology disclosed in Patent Document 4. However, in recent years, with growing awareness of environmental issues, there has been a demand for insulating coatings that do not contain chromate compounds.
[0019] The present invention has been made in view of the above problems, and has an object to provide a grain-oriented electrical steel sheet that exhibits excellent adhesion to an insulating coating even without a forsterite coating. [Means for solving the problem]
[0020] The present invention has been made to solve the above problems, and provides the following grain-oriented electrical steel sheet.
[0021] (1) The grain-oriented electrical steel sheet according to one embodiment of the present invention is A base steel plate; An intermediate layer disposed on and in contact with the base steel plate; an insulating coating disposed on and in contact with the intermediate layer; The intermediate layer is Si content: 20 atomic% or more and 70 atomic% or less, O content: 30 atomic% or more and 80 atomic% or less, Mg content: 20 atomic% or less, P content: 5 at% or less, Fe content: less than 20 atomic % and The average thickness of the oxide film is 2 nm or more and 500 nm or less, The insulating coating is P content: 5 at% or more and 30 at% or less, Si content: 5 at% or more and 30 at% or less, O content: 30 atomic% or more and 80 atomic% or less, Al content: 0.1 atomic% or more and 10 atomic% or less, Cr content: less than 1 atomic % Fe content: less than 25 atomic % Mg content: 0 atomic% or more and 10 atomic% or less, Mn content: 0 atomic% or more and 10 atomic% or less, Ni content: 0 at% to 10 at%, Zn content: 0 at% to 10 at%, V content: 0 atomic% or more and 10 atomic% or less, W content: 0 atomic% or more and 10 atomic% or less, Zr content: 0 at% to 10 at%, Co content: 0 at% to 10 at%, Mo content: 0 at% to 10 at%, It is a phosphoric acid-based coating that satisfies the above, and The average thickness of the phosphoric acid coating is 0.1 μm or more and 10 μm or less, When the phosphate-based coating is subjected to glazing incidence X-ray diffraction using a Co-Kα excitation source, the X-ray diffraction pattern has a diffraction peak at a diffraction angle 2θ=24.8° derived from cristobalite-type aluminum phosphate, and The half-width of the diffraction peak under the diffraction condition of X-ray incidence angle ω = 0.5° is defined as FWHM 0.5 The half-width of the diffraction peak under the diffraction condition of X-ray incidence angle ω = 1.0° is expressed as FWHM 1.0 When expressed as FWHM 0.5 and the FWHM 1.0 But, 0.20°≦FWHM 0.5 ≦2.00° 0.20°≦FWHM 1.0 ≦2.00° 0°≦|FWHM 0.5 -FWHM 1.0 |≦1.00° Satisfy. Effect of the Invention
[0022] According to the above-described embodiment of the present invention, it is possible to provide a grain-oriented electrical steel sheet that has excellent adhesion to an insulating coating even without a forsterite coating. [Brief description of the drawings]
[0023] [Figure 1] 1 is a cross-sectional schematic diagram showing a layer structure of a grain-oriented electrical steel sheet according to an embodiment of the present invention. FIG. [Diagram 2] 1 shows an X-ray diffraction pattern obtained by performing grazing incidence X-ray diffraction using a Co-Kα excitation source on the phosphate-based coating of the grain-oriented electrical steel sheet according to the present embodiment. [Diagram 3] 1 is a flowchart showing a method for manufacturing a grain-oriented electrical steel sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] A preferred embodiment of the present invention will be described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. Furthermore, the numerical ranges shown in this embodiment include lower and upper limits. Numerical values indicated as "more than" or "less than" are not included in the numerical range. Unless otherwise specified, "%" regarding the content of each element means "mass %" for the base steel plate, and "atomic %" for the intermediate layer and insulating coating.
[0025] Fig. 1 is a cross-sectional schematic diagram showing the layer structure of a grain-oriented electrical steel sheet according to one embodiment of the present invention. As shown in Fig. 1, the grain-oriented electrical steel sheet according to this embodiment, when viewed on a cut surface parallel to the sheet thickness direction, has no forsterite coating on the surface of base steel sheet 1, has an intermediate layer 2 mainly made of silicon oxide on the surface of base steel sheet 1, and has an insulating coating 3 derived from aluminum phosphate and colloidal silica on this intermediate layer 2.
[0026] Specifically, the grain-oriented electrical steel sheet according to this embodiment has: A base steel plate; An intermediate layer disposed on and in contact with the base steel sheet; an insulating coating disposed on and in contact with the intermediate layer; The intermediate layer is Si content: 20 atomic% or more and 70 atomic% or less, O content: 30 atomic% or more and 80 atomic% or less, Mg content: 20 atomic% or less, P content: 5 at% or less, Fe content: less than 20 atomic % and The average thickness of the oxide film is 2 nm or more and 500 nm or less, The insulating coating is P content: 5 at% or more and 30 at% or less, Si content: 5 at% or more and 30 at% or less, O content: 30 atomic% or more and 80 atomic% or less, Al content: 0.1 atomic% or more and 10 atomic% or less, Cr content: less than 1 atomic % Fe content: less than 25 atomic % Mg content: 0 atomic% or more and 10 atomic% or less, Mn content: 0 atomic% or more and 10 atomic% or less, Ni content: 0 at% to 10 at%, Zn content: 0 at% to 10 at%, V content: 0 atomic% or more and 10 atomic% or less, W content: 0 atomic% or more and 10 atomic% or less, Zr content: 0 at% to 10 at%, Co content: 0 at% to 10 at%, Mo content: 0 at% to 10 at%, It is a phosphoric acid-based coating that satisfies the above, and The average thickness of the phosphoric acid coating is 0.1 μm or more and 10 μm or less, When the phosphate-based coating is subjected to glazing incidence X-ray diffraction using a Co-Kα excitation source, the X-ray diffraction pattern has a diffraction peak at a diffraction angle 2θ=24.8° derived from cristobalite-type aluminum phosphate, and The half-width of the above diffraction peak under the diffraction condition of X-ray incidence angle ω = 0.5° is defined as FWHM.0.5 The half-width of the above diffraction peak under the diffraction condition of X-ray incidence angle ω = 1.0° is expressed as FWHM 1.0 When expressed as above, the FWHM 0.5 and the above FWHM 1.0 But, 0.20°≦FWHM 0.5 ≦2.00° 0.20°≦FWHM 1.0 ≦2.00° 0°≦|FWHM 0.5 -FWHM 1.0 |≦1.00° Satisfy.
[0027] In conventional grain-oriented electrical steel sheets, the insulating coating is amorphous, and therefore when X-ray diffraction is performed on the insulating coating, the X-ray diffraction pattern becomes a halo pattern and no clear diffraction peak is observed. On the other hand, in the grain-oriented electrical steel sheet according to this embodiment, when X-ray diffraction is performed on the phosphate coating (insulating coating), the X-ray diffraction pattern has a clear diffraction peak in addition to a halo pattern. This diffraction peak is derived from cristobalite-type aluminum phosphate. That is, in the grain-oriented electrical steel sheet according to this embodiment, a part of the phosphate coating is crystallized to become cristobalite-type aluminum phosphate.
[0028] Generally, the half-width of a diffraction peak is an index of the degree of crystallinity, with a smaller half-width value indicating a higher degree of crystallinity. In the grain-oriented electrical steel sheet according to this embodiment, the half-width of the diffraction peak derived from cristobalite-type aluminum phosphate is equal to or less than a predetermined value. That is, in the grain-oriented electrical steel sheet according to this embodiment, crystalline cristobalite-type aluminum phosphate is formed in the phosphate-based coating, and the degree of crystallinity is high.
[0029] Moreover, under the diffraction condition of an X-ray incidence angle ω=0.5°, X-rays penetrate only into the outermost surface region of the phosphate-based coating, and an X-ray diffraction pattern originating from the outermost surface region of the phosphate-based coating is obtained. On the other hand, under the diffraction condition of an X-ray incidence angle ω=1.0°, X-rays penetrate into the inner region of the phosphate-based coating, and an X-ray diffraction pattern originating from the inner region of the phosphate-based coating is obtained.
[0030] In the grain-oriented electrical steel sheet according to this embodiment, the half-width is equal to or less than a predetermined value in both the outermost surface region and the inner region of the phosphate-based coating, and the difference in the half-width between the outermost surface region and the inner region is small. That is, in the grain-oriented electrical steel sheet according to this embodiment, crystalline cristobalite-type aluminum phosphate is partially formed in the amorphous phosphate-based coating in both the outermost surface region and the inner region of the phosphate-based coating, the degree of crystallinity is high, and there is no significant difference in the degree of crystallinity between the outermost surface region and the inner region.
[0031] Each of the features will be described in detail below. First, the phosphate coating of the grain-oriented electrical steel sheet according to this embodiment will be described.
[0032] (About phosphoric acid coating) The phosphate-based coating is located on the outermost surface of the layer structure of the grain-oriented electrical steel sheet. This phosphate-based coating is formed on the base steel sheet in a high-temperature environment using a material with a smaller thermal expansion coefficient than the base steel sheet, so that a difference in shrinkage occurs between the phosphate-based coating and the base steel sheet during cooling, and as a result, the phosphate-based coating applies tension to the base steel sheet. In the grain-oriented electrical steel sheet in which tension is applied to the base steel sheet, the core loss characteristics are favorably improved.
[0033] In order for the phosphate-based coating to apply tension to the base steel sheet, it is important that the phosphate-based coating and the base steel sheet are in close contact with each other via an oxide film, which will be described later. In the grain-oriented electrical steel sheet according to this embodiment, in order to improve coating adhesion, the coating composition and thickness of the phosphate-based coating are controlled, and crystalline cristobalite-type aluminum phosphate is partially formed in the amorphous phosphate-based coating, and the crystallization state is controlled.
[0034] First, the composition of the phosphoric acid-based coating will be described.
[0035] In the grain-oriented electrical steel sheet according to the present embodiment, the phosphate-based coating contains, as a coating composition, base elements and, as necessary, optional elements, and the balance of the base elements and optional elements is preferably impurities.
[0036] Specifically, the phosphate coating contains the following basic elements: P content: 5 at% or more and 30 at% or less, Si content: 5 at% or more and 30 at% or less, O content: 30 atomic % or more and 80 atomic % or less, and Al content: 0.1 atomic% or more and 10 atomic% or less, It is sufficient to satisfy the above. In addition, the phosphoric acid coating contains the following selective elements: Mg content: 0 atomic% or more and 10 atomic% or less, Mn content: 0 atomic% or more and 10 atomic% or less, Ni content: 0 at% to 10 at%, Zn content: 0 at% to 10 at%, V content: 0 atomic% or more and 10 atomic% or less, W content: 0 atomic% or more and 10 atomic% or less, Zr content: 0 at% to 10 at%, Co content: 0 atomic % or more and 10 atomic % or less, and Mo content: 0 at% to 10 at%, It is sufficient to satisfy the above. In addition, the phosphoric acid coating contains impurities such as Cr content: less than 1 atomic %, and Fe content: less than 25 atomic % It is sufficient to satisfy the above.
[0037] The basic elements of the phosphate coating, P, Si, O, and Al, are derived from the aluminum phosphate and colloidal silica contained in the coating solution and the oxidation reaction during baking. The P content is preferably 8 atomic % or more, and preferably 23 atomic % or less or 17 atomic % or less. The Si content is preferably 10 atomic % or more, and more preferably 25 atomic % or less or 20 atomic % or less. The O content is preferably 40 atomic % or more or 50 atomic % or more, and preferably 75 atomic % or less. The Al content is preferably 1 atomic % or more, and preferably 7 atomic % or less or 4 atomic % or less.
[0038] The phosphate coating may also contain optional elements such as Mg, Mn, Ni, Zn, V, W, Zr, Co, and Mo. These optional elements may be derived from phosphates contained in the coating solution or may be incorporated into the phosphate coating by other methods.
[0039] By including one or more elements selected from Mg, Mn, Ni, Zn, V, W, Zr, Co, and Mo, the effect of improving the water resistance of the phosphate coating can be obtained. To obtain this effect, it is preferable to include one or more elements selected from the above elements in a total amount of 0.1 atomic % or more. Note that, if each element is 10 atomic % or less, the effect of the present invention is not hindered, but 5 atomic % or less is preferable, and 3 atomic % or less is more preferable.
[0040] When two or more selected from Mg, Mn, Ni, Zn, V, W, Zr, Co, and Mo are contained in combination, it is preferable that the total content of Mg+Mn+Ni+Zn is 10 atomic % or less, and it is preferable that the total content of V+W+Zr+Co+Mo is 10 atomic % or less.
[0041] The above-mentioned Cr and Fe are impurities in the phosphate-based coating, and these impurities originate from elements mixed in from the raw materials or manufacturing environment when the phosphate-based coating is formed, or from elements diffused from the base steel sheet. The lower limit of the impurity content is not particularly limited, and since the lower the better, it may be 0%.
[0042] In the grain-oriented electrical steel sheet according to this embodiment, the coating composition of the phosphate-based coating only needs to satisfy the above conditions in order to improve coating adhesion. In particular, the content of Cr contained as an impurity in the phosphate-based coating is limited to less than 1 atomic %.
[0043] Generally, phosphate coatings on grain-oriented electrical steel sheets are formed by baking a coating solution that contains phosphate, colloidal silica, and chromate, which is added to improve corrosion resistance, enhance chemical resistance, and suppress voids.
[0044] On the other hand, the phosphate coating of the grain-oriented electrical steel sheet according to the present embodiment is formed by baking a coating solution that contains aluminum phosphate and colloidal silica but does not contain chromate. Therefore, as described above, the phosphate coating of the grain-oriented electrical steel sheet according to the present embodiment has a Cr content limited to less than 1 atomic %. The Cr content is preferably 0.8 atomic % or less, and more preferably 0.5 atomic % or less.
[0045] In the grain-oriented electrical steel sheet according to the present embodiment, limiting the Cr content of the phosphate coating to less than 1 atomic % is one of the conditions for controlling the crystallization state of cristobalite-type aluminum phosphate in the phosphate coating. Details of the control conditions for cristobalite-type aluminum phosphate will be described later.
[0046] The composition of the phosphate coating can be determined by analyzing the composition of the cut surface using SEM-EDS (Scanning Electron Microscope-Energy Dispersive X-ray Spectroscopy) or TEM-EDS (Transmission Electron Microscope-Energy Dispersive X-ray Spectroscopy). The method for measuring the coating composition will be described in detail later.
[0047] Next, the thickness of the phosphoric acid-based coating will be described.
[0048] In the grain-oriented electrical steel sheet according to this embodiment, the average film thickness of the phosphate coating is 0.1 μm or more and 10 μm or less when viewed on a cut surface whose cutting direction is parallel to the sheet thickness direction.
[0049] If the average thickness of the phosphate coating is less than 0.1 μm, it becomes difficult to apply the required tension to the base steel sheet, so the average thickness is set to 0.1 μm or more, preferably 0.3 μm or more or 0.5 μm or more, and more preferably 1 μm or more.
[0050] On the other hand, if the average thickness of the phosphate coating exceeds 10 μm, the manufacturing cost increases, and if the average thickness of the phosphate coating exceeds 10 μm, the space factor decreases when the oriented electrical steel sheets are laminated to form an iron core. Therefore, the average thickness is set to 10 μm or less, and preferably 5 μm or less.
[0051] The average thickness of the phosphoric acid-based coating can be determined by line analysis of the cut surface using SEM-EDS or TEM-EDS. The method for measuring the average thickness will be described later.
[0052] Next, the crystallization state of the cristobalite-type aluminum phosphate in the phosphate-based coating will be described.
[0053] FIG. 2 shows an X-ray diffraction pattern obtained by performing grazing incidence X-ray diffraction on the phosphate-based coating of the grain-oriented electrical steel sheet according to this embodiment using a Co-Kα excitation source.
[0054] In the grain-oriented electrical steel sheet according to the present embodiment, when the phosphate-based coating is subjected to glazing incidence X-ray diffraction using a Co-Kα excitation source, the X-ray diffraction pattern has a diffraction peak at a diffraction angle 2θ=24.8° derived from cristobalite-type aluminum phosphate, and The half-width of the above diffraction peak under the diffraction condition of X-ray incidence angle ω = 0.5° is defined as FWHM. 0.5 The half-width of the above diffraction peak under the diffraction condition of X-ray incidence angle ω = 1.0° is expressed as FWHM 1.0 When expressed as above, the FWHM 0.5 and the above FWHM 1.0 But, 0.20°≦FWHM 0.5 ≦2.00° 0.20°≦FWHM 1.0 ≦2.00° 0°≦|FWHM 0.5 -FWHM 1.0 |≦1.00° Satisfy.
[0055] When an amorphous phosphate coating contains a portion of crystalline cristobalite-type aluminum phosphate, the degree of crystallinity is high, and there is no significant difference in the degree of crystallinity between the outermost surface region and the inner region of the phosphate coating, the coating adhesion is favorably improved. The details of the reason for this are unclear at present, but the following mechanism is thought to be the cause.
[0056] When aluminum phosphate crystallizes in the phosphate coating, moisture is generated, which promotes the formation of an intermediate layer and improves the adhesion of the coating. However, if aluminum phosphate crystallizes locally in the phosphate coating, for example, preferentially in the outermost surface region of the phosphate coating, then when the grain-oriented electrical steel sheet is bent to manufacture a transformer, stress is concentrated locally in the aluminum phosphate crystallized in the phosphate coating, and the coating peels off from that point.
[0057] On the other hand, in the grain-oriented electrical steel sheet according to the present embodiment, the crystallization state of aluminum phosphate is uniform between the outermost surface region and the inner region of the phosphate-based coating, so that even when bending is performed, local stress concentration is suppressed, and as a result, it is considered that the phosphate-based coating is less likely to peel off. This tendency becomes more pronounced when bending is performed under severe conditions.
[0058] In order to control the crystallization state of the cristobalite-type aluminum phosphate that partially crystallizes in the phosphate-based coating as described above, the following two conditions must be satisfied.
[0059] (I) The phosphate coating has a coating composition that satisfies the requirement of a Cr content of less than 1 atomic %. (II) When forming a phosphoric acid-based coating, the formation conditions are controlled. Only when these two conditions are both satisfied can the crystallization state of the crystalline cristobalite-type aluminum phosphate contained in the amorphous phosphate-based coating be controlled as described above.
[0060] First, as condition (I), it is important that the Cr content in the composition of the phosphate coating is less than 1 atomic %. If the Cr content in the phosphate coating is 1 atomic % or more, the crystallization of cristobalite-type aluminum phosphate in the phosphate coating is significantly inhibited. In particular, cristobalite-type aluminum phosphate is less likely to crystallize in the inner region of the phosphate coating.
[0061] At present, the details of why the crystallization of cristobalite-type aluminum phosphate is suppressed in a phosphate coating when the Cr content of the phosphate coating is 1 atomic % or more are unknown, but the following reasons are thought to be the cause: When the Cr content of a phosphate coating is 1 atomic % or more, the chemical stability is enhanced due to a reaction between the terminal structure of the phosphate molecular chain and Cr, and the crystallization of aluminum phosphate is inhibited.
[0062] On the other hand, if the Cr content of the phosphate coating is less than 1 atomic %, it is believed that the phosphate does not react with Cr, and as a result, cristobalite-type aluminum phosphate is more likely to crystallize in the phosphate coating.
[0063] Next, as condition (II), it is important to control the formation conditions when forming the phosphate coating. Even if condition (I) is satisfied, it is difficult to crystallize cristobalite-type aluminum phosphate in the above-mentioned state in the amorphous phosphate coating unless the formation conditions are suitably controlled when forming the phosphate coating. For example, if condition (I) is satisfied but condition (II) is not satisfied, the crystallization state of cristobalite-type aluminum phosphate can be controlled in the outermost surface region of the phosphate coating, but the crystallization state of cristobalite-type aluminum phosphate cannot be controlled in the inner region of the phosphate coating.
[0064] Specifically, when forming the phosphate coating, it is important to control the heating rate from room temperature to 350°C as a formation condition. In other words, it is important to set the heating rate before the crystallization of aluminum phosphate begins to be less than 30°C / sec. If the heating rate from room temperature to 350°C is less than 30°C / sec, the temperature difference between the outermost surface region and the inner region of the coating solution is small. As a result, even when the coating solution is baked to become a phosphate coating, the temperature difference between the outermost surface region and the inner region of the phosphate coating is small, and the crystallization state of the cristobalite-type aluminum phosphate is uniformly controlled.
[0065] When grazing incidence X-ray diffraction is performed on a phosphate-based coating using a Co-Kα excitation source, if the X-ray diffraction pattern has a diffraction peak at a diffraction angle 2θ = 24.8°, it can be determined that crystalline cristobalite-type aluminum phosphate is present in the amorphous phosphate-based coating.
[0066] In addition, the FWHM, which is the half-width of the diffraction peak that appears at a diffraction angle of 2θ = 24.8° under the diffraction condition of an X-ray incidence angle of ω = 0.5°, 0.5When the FWHM is 2.00° or less, it can be determined that the degree of crystallization of the cristobalite-type aluminum phosphate in the outermost surface region of the phosphate coating is high. 0.5 The upper limit of the FWHM is preferably 1.80°, and more preferably 1.60°. On the other hand, if crystallization proceeds excessively, the reaction with colloidal silica is suppressed and the film tension cannot be obtained. 0.5 The lower limit is 0.20°.
[0067] Similarly, the FWHM, which is the half-width of the diffraction peak that appears at a diffraction angle of 2θ = 24.8° under the diffraction conditions of an X-ray incidence angle of ω = 1.0°, is 1.0 When the FWHM is 2.00° or less, it can be determined that the degree of crystallization of the cristobalite-type aluminum phosphate in the inner region of the phosphate coating is high. 1.0 The upper limit of the FWHM is preferably 1.80°, and more preferably 1.60°. On the other hand, if crystallization proceeds excessively, the reaction with colloidal silica is suppressed and the film tension cannot be obtained. 1.0 The lower limit is 0.20°.
[0068] Also, FWHM 0.5 and FWHM 1.0 The absolute value of the difference between |FWHM 0.5 -FWHM 1.0 When | is 1.00° or less, it can be determined that there is no significant difference in the crystallinity of the cristobalite-type aluminum phosphate between the outermost surface region and the inner region of the phosphate coating. 0.5 -FWHM 1.0 The upper limit of | is preferably 0.80°. 0.5 -FWHM 1.0 There is no particular lower limit for |, and the smaller the better. Therefore, |FWHM 0.5 -FWHM 1.0 The lower limit of | should be 0°. However, |FWHM 0.5 -FWHM 1.0 When it is not industrially easy to set the lower limit of | to 0°, for example, |FWHM 0.5 -FWHM 1.0The lower limit of | should be set to 0.05°.
[0069] When the crystallization state of the crystalline cristobalite-type aluminum phosphate contained in the amorphous phosphate-based coating is controlled as described above, the coating adhesion is excellent even if the intermediate layer is not a forsterite coating but a Si-based oxide film, i.e., even if the surface of the base steel sheet is smooth.
[0070] The diffraction peak appearing at a diffraction angle 2θ=34.3° is derived from crystalline tridymite-type aluminum phosphate contained in the amorphous phosphate coating. Tridymite-type aluminum phosphate is considered to be a crystalline substance that corresponds to an intermediate stage in the crystallization into cristobalite-type aluminum phosphate. In other words, the presence of a large amount of tridymite-type aluminum phosphate means that the crystallization of cristobalite-type aluminum phosphate is insufficient.
[0071] In particular, even if the crystallization of cristobalite-type aluminum phosphate has progressed sufficiently in the outermost surface region of the phosphate coating, when the crystallization of cristobalite-type aluminum phosphate has not progressed sufficiently in the inner region, the peak intensity of tridymite-type aluminum phosphate tends to be relatively high in the outermost surface region. Therefore, under the diffraction condition of X-ray incidence angle ω=0.5°, it is preferable that the peak intensity of the diffraction peak appearing at a diffraction angle 2θ=34.3° is 0.50 times or less than the peak intensity of the diffraction peak appearing at a diffraction angle 2θ=24.8°.
[0072] The crystallization state of cristobalite-type aluminum phosphate in the phosphate-based coating can be confirmed by performing grazing incidence X-ray diffraction using a Co-Kα excitation source. Specifically, grazing incidence X-ray diffraction is performed on the phosphate-based coating using a Co-Kα excitation source, and the half-width of the diffraction peak that appears at a diffraction angle 2θ = 24.8° is confirmed under conditions of X-ray incidence angles ω of 0.5° and 1.0°.
[0073] Similarly, the peak intensities of cristobalite-type aluminum phosphate and tridymite-type aluminum phosphate in the phosphate-based coating can be confirmed by performing grazing incidence X-ray diffraction using a Co-Kα excitation source. Specifically, grazing incidence X-ray diffraction is performed on the phosphate-based coating using a Co-Kα excitation source, and the peak intensities of the diffraction peaks appearing at diffraction angles 2θ = 24.8° and 2θ = 34.3° are confirmed under the condition of an X-ray incidence angle ω of 0.5°. The method for measuring grazing incidence X-ray diffraction will be described in detail later.
[0074] Next, the oxide film that is the intermediate layer of the grain-oriented electrical steel sheet according to this embodiment will be described.
[0075] (About oxide film) The oxide film is located between the phosphate coating and the base steel sheet in the layered structure of the grain-oriented electrical steel sheet. This oxide film is not a forsterite film but a silicon-based oxide film, and its function is to bond the phosphate coating and the base steel sheet together.
[0076] First, the composition of the oxide film will be described.
[0077] In the grain-oriented electrical steel sheet according to the present embodiment, the oxide film contains basic elements as a coating composition. In addition to the basic elements, optional elements may be contained as necessary. The balance of the basic elements and the optional elements is preferably impurities.
[0078] Specifically, the oxide film contains the following basic elements: Si content: 20 atomic % or more and 70 atomic % or less, and O content: 30 at% or more and 80 at% or less, It is sufficient to satisfy the above. Furthermore, the oxide film may contain, as selective elements, constituent elements of the base steel sheet, and the total content thereof may satisfy the range of 0.1 atomic % to 20 atomic %. In addition, the oxide film contains impurities such as Mg content: 20 atomic% or less, P content: 5 atomic % or less, and Fe content: less than 20 atomic % It is sufficient to satisfy the above.
[0079] Generally, in grain-oriented electrical steel sheets, an annealing separator mainly composed of MgO is applied to a decarburized annealed sheet, which is then subjected to finish annealing to form a forsterite coating (a coating mainly composed of Mg2SiO4) as an intermediate layer.
[0080] When this forsterite coating is formed, the unevenness at the interface between the forsterite coating and the base steel sheet acts as an anchor to ensure adhesion of the coating, but the unevenness at the interface hinders magnetic domain wall movement when the grain-oriented electrical steel sheet is magnetized, adversely affecting iron loss characteristics.
[0081] The grain-oriented electrical steel sheet according to this embodiment aims to make the interface between the intermediate layer and the base steel sheet smooth without the presence of a forsterite coating. Then, in order to improve the coating adhesion even when this interface is made smooth, the above conditions (I) and (II) are satisfied, and the crystallization state of cristobalite-type aluminum phosphate is controlled in both the outermost surface region and the inner region of the phosphate-based coating. Note that when the intermediate layer is a forsterite coating, the problem of coating adhesion between the insulating coating and the forsterite coating does not arise in the first place. Therefore, in the grain-oriented electrical steel sheet according to this embodiment, the intermediate layer is a Si-based oxide film.
[0082] Therefore, as described above, the Mg content is limited to 20 atomic % or less in the oxide film (intermediate layer) of the grain-oriented electrical steel sheet according to this embodiment. The Mg content is preferably less than 20 atomic %, more preferably 15 atomic % or less, and even more preferably 10 atomic % or less. Details of the control conditions for forming the oxide film (intermediate layer) without forming a forsterite film will be described later.
[0083] The basic elements of the oxide film, Si and O, originate from the constituent elements of the base steel sheet and from the oxidation reaction that occurs when the oxide film is formed. The Si content is preferably 55 atomic % or less, and more preferably 45 atomic % or less. The O content is preferably 45 atomic % or more, and more preferably 75 atomic % or less, and more preferably 65 atomic % or less.
[0084] The above-mentioned Mg, P, and Fe are impurities in the oxide film, and these impurities originate from elements mixed in from the raw materials or manufacturing environment, or from elements diffused from the base steel sheet or phosphate-based coating. The P content is preferably less than 5 atomic %. The Fe content is preferably 15 atomic % or less, and more preferably 10 atomic % or less. The lower limit of the impurity content is not particularly limited, and may be 0%, since the lower the better.
[0085] The composition of the oxide film can be determined by analyzing the composition of the cut surface using SEM-EDS or TEM-EDS, in the same way as for the composition of the phosphate-based film. The method for measuring the composition of the film will be described in detail later.
[0086] Next, the thickness of the oxide film will be described.
[0087] In the grain-oriented electrical steel sheet according to this embodiment, when viewed on a cut surface whose cutting direction is parallel to the sheet thickness direction, the average thickness of the oxide film is 2 nm or more and 500 nm or less.
[0088] If the average thickness of the oxide film is less than 2 nm, the thermal stress relaxation effect is not sufficiently exhibited, so the average thickness is set to 2 nm or more, preferably 5 nm or more, and more preferably 10 nm or more.
[0089] On the other hand, if the average thickness of the oxide film exceeds 500 nm, the thickness becomes non-uniform and defects such as voids or cracks occur within the layer, so the average thickness is set to 500 nm or less, preferably 400 nm or less, and more preferably 200 nm or less, 150 nm or less, or 100 nm or less.
[0090] The average thickness of the oxide film can be determined by line analysis of the cut surface using SEM-EDS or TEM-EDS, in the same way as for the film composition of the phosphate-based film. The method for measuring the average thickness will be described in detail later.
[0091] Next, the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment will be described.
[0092] (About the base steel plate) The base steel sheet is the base material of the grain-oriented electrical steel sheet. The type of base steel sheet is not particularly limited, and a known silicon steel sheet can be used. For example, the silicon steel sheet preferably has a Si content of 0.80 mass% or more and 7.0 mass% or less and a crystal orientation of {110} <001> Preferably, it is azimuthally (Goss azimuth) controlled.
[0093] Here, <001> The orientation is such that the {110} plane of the crystal is parallel to the rolling surface and the <001> This means that the axis is arranged parallel to the rolling direction.
[0094] First, a suitable chemical composition of the silicon steel sheet will be described.
[0095] Since the chemical composition of the silicon steel sheet is not directly related to the crystallization state of cristobalite-type aluminum phosphate in the phosphate-based coating, the chemical composition of the silicon steel sheet used as the base steel sheet in the grain-oriented electrical steel sheet according to this embodiment is not particularly limited. However, the chemical composition of a silicon steel sheet preferred as the grain-oriented electrical steel sheet will be described below. Hereinafter, % relating to the chemical composition of the silicon steel sheet means % by mass.
[0096] The silicon steel sheet preferably has a chemical composition containing basic elements, optionally containing optional elements, and the balance being Fe and impurities.
[0097] Specifically, the chemical composition of the silicon steel sheet is, in mass%, Si: 0.80% or more and 7.0% or less, Mn: 0% or more and 1.0% or less, Cr: 0% or more and 0.30% or less, Cu: 0% or more and 0.40% or less, P: 0% or more and 0.50% or less, Sn: 0% or more and 0.30% or less, Sb: 0% or more and 0.30% or less, Ni: 0% or more and 1.0% or less, B: 0% or more and 0.008% or less, V: 0% or more and 0.15% or less, Nb: 0% or more and 0.20% or less, Mo: 0% or more and 0.10% or less, Ti: 0% or more and 0.015% or less, Bi: 0% or more and 0.010% or less, Al: 0% or more and 0.005% or less, C: 0% or more and 0.005% or less, N: 0% or more and 0.005% or less, S: 0% or more and 0.005% or less, Se: 0% or more and 0.005% or less The balance is preferably Fe and impurities.
[0098] In this embodiment, the silicon steel sheet may contain Si as a base element (main alloy element).
[0099] Si: 0.80% or more and 7.0% or less In the chemical composition of silicon steel sheet, Si (silicon) is an element effective in increasing electrical resistance and decreasing iron loss. If the Si content exceeds 7.0%, the material may be easily cracked during cold rolling, making rolling difficult. On the other hand, if the Si content is less than 0.80%, the electrical resistance may be small, and the iron loss in the product may increase. Therefore, Si may be contained in a range of 0.80% to 7.0%. The lower limit of the Si content is preferably 2.0%, more preferably 2.5%, and even more preferably 2.8%. The upper limit of the Si content is preferably 5.0%, and more preferably 3.5%.
[0100] In the present embodiment, the silicon steel sheet may contain impurities. Note that the term "impurities" refers to substances that are mixed in from ore or scrap as raw materials, or from the manufacturing environment, during industrial production of steel.
[0101] In addition, in this embodiment, the silicon steel sheet may contain selective elements in addition to the basic elements and impurities described above. For example, instead of a part of the Fe that is the balance described above, one or more selective elements selected from Mn, Cr, Cu, P, Sn, Sb, Ni, B, V, Nb, Mo, Ti, Bi, Al, C, N, S, and Se may be contained. These selective elements may be contained according to the purpose. Therefore, there is no need to limit the lower limit of these selective elements, and the lower limit may be 0%. Furthermore, even if these selective elements are contained as impurities, the above-mentioned effects are not impaired.
[0102] Mn: 0% or more and 1.0% or less Like Si, Mn (manganese) is an element effective in increasing electrical resistance and reducing iron loss. It also functions as an inhibitor by combining with S or Se. Therefore, Mn may be contained in a range of 1.0% or less. The lower limit of the Mn content is preferably 0.05%, more preferably 0.08%, and further preferably 0.09%. The upper limit of the Mn content is preferably 0.50%, and more preferably 0.20%.
[0103] Cr: 0% or more and 0.30% or less Cr (chromium), like Si, is an element effective in increasing electrical resistance and reducing iron loss. Therefore, Cr may be contained in a range of 0.30% or less. The lower limit of the Cr content is preferably 0.02%, more preferably 0.05%. The upper limit of the Cr content is preferably 0.20%, more preferably 0.12%.
[0104] Cu: 0% or more and 0.40% or less Cu (copper) is also an effective element for increasing electrical resistance and reducing iron loss. Therefore, Cu may be contained in a range of 0.40% or less. If the Cu content exceeds 0.40%, the iron loss reduction effect is saturated and it may cause surface defects called "copper scuffs" during hot rolling. The lower limit of the Cu content is preferably 0.05%, more preferably 0.10%. The upper limit of the Cu content is preferably 0.30%, more preferably 0.20%.
[0105] P: 0% or more and 0.50% or less P (phosphorus) is also an element effective in increasing electrical resistance and reducing iron loss. Therefore, P may be contained in a range of 0.50% or less. If the P content exceeds 0.50%, problems may occur in the rollability of the silicon steel sheet. The lower limit of the P content is preferably 0.005%, and more preferably 0.01%. The upper limit of the P content is preferably 0.30% or 0.20%, and more preferably 0.15%.
[0106] Sn: 0% or more and 0.30% or less Sb: 0% or more and 0.30% or less Sn (tin) and Sb (antimony) stabilize the secondary recrystallization and form {110} <001> These elements are effective in developing the orientation. Therefore, Sn may be contained within the range of 0.30% or less, and Sb may be contained within the range of 0.30% or less. If the Sn or Sb content exceeds 0.30%, respectively, there is a risk of adversely affecting the magnetic properties.
[0107] The lower limit of the Sn content is preferably 0.02%, and more preferably 0.05%. The upper limit of the Sn content is preferably 0.15%, and more preferably 0.10%. The lower limit of the Sb content is preferably 0.01%, and more preferably 0.03%. The upper limit of the Sb content is preferably 0.15%, and more preferably 0.10%.
[0108] Ni: 0% or more and 1.0% or less Ni (nickel) is also an element effective in increasing electrical resistance and reducing iron loss. Ni is also an element effective in controlling the metal structure of the hot-rolled sheet and improving the magnetic properties. Therefore, Ni may be contained in a range of 1.0% or less. If the Ni content exceeds 1.0%, the secondary recrystallization may become unstable. The lower limit of the Ni content is preferably 0.01%, and more preferably 0.02%. The upper limit of the Ni content is preferably 0.50% or 0.20%, and more preferably 0.10%.
[0109] B: 0% or more and 0.008% or less B (boron) is an element that is effective in exerting an inhibitor effect as BN. Therefore, B may be contained in a range of 0.008% or less. If the B content exceeds 0.008%, it may adversely affect the magnetic properties. The lower limit of the B content is preferably 0.0005%, more preferably 0.001%. The upper limit of the B content is preferably 0.005%, more preferably 0.003%.
[0110] V: 0% or more and 0.15% or less Nb: 0% or more and 0.20% or less Ti: 0% or more and 0.015% or less V (vanadium), Nb (niobium), and Ti (titanium) are elements that are effective in binding with N or C to function as inhibitors. Therefore, V may be contained in the range of 0.15% or less, Nb in the range of 0.20% or less, and Ti in the range of 0.015% or less. If these elements remain in the final product (electromagnetic steel sheet) and the V content exceeds 0.15%, the Nb content exceeds 0.20%, or the Ti content exceeds 0.015%, there is a risk of degrading the magnetic properties.
[0111] The lower limit of the V content is preferably 0.002%, more preferably 0.01%. The upper limit of the V content is preferably 0.10% or less, more preferably 0.05%. The lower limit of the Nb content is preferably 0.005%, more preferably 0.02%. The upper limit of the Nb content is preferably 0.10%, more preferably 0.08%. The lower limit of the Ti content is preferably 0.002%, more preferably 0.004%. The upper limit of the Ti content is preferably 0.010%, more preferably 0.008%.
[0112] Mo: 0% or more and 0.10% or less Mo (molybdenum) is also an element effective in increasing electrical resistance and reducing iron loss. Therefore, Mo may be contained in a range of 0.10% or less. If the Mo content exceeds 0.10%, problems may occur in the rollability of the steel sheet. The lower limit of the Mo content is preferably 0.005%, more preferably 0.01%. The upper limit of the Mo content is preferably 0.08%, more preferably 0.05%.
[0113] Bi: 0% or more and 0.010% or less Bi (bismuth) is an element that is effective in stabilizing precipitates such as sulfides and strengthening the function as an inhibitor. Therefore, Bi may be contained in a range of 0.010% or less. If the Bi content exceeds 0.010%, it may have an adverse effect on the magnetic properties. The lower limit of the Bi content is preferably 0.001%, and more preferably 0.002%. The upper limit of the Bi content is preferably 0.008%, and more preferably 0.006%.
[0114] Al: 0% or more and 0.005% or less Al (aluminum) is an element effective in exerting an inhibitor effect by bonding with N. Therefore, Al may be contained in the range of 0.01 to 0.065% before the final annealing, for example, at the slab stage. However, if Al remains as an impurity in the final product (electromagnetic steel sheet) and the Al content exceeds 0.005%, it may adversely affect the magnetic properties. Therefore, the Al content of the final product is preferably 0.005% or less. The upper limit of the Al content of the final product is preferably 0.004%, more preferably 0.003%. The Al content of the final product is an impurity, and the lower limit is not particularly limited, and the lower the better. However, since it is not industrially easy to make the Al content of the final product 0%, the lower limit of the Al content of the final product may be 0.0005%. The Al content indicates the content of acid-soluble Al.
[0115] C: 0% or more and 0.005% or less N: 0% or more and 0.005% or less C (carbon) is an element effective in adjusting the primary recrystallization texture and improving the magnetic properties. In addition, N (nitrogen) is an element effective in combining with Al or B and exerting an inhibitor effect. Therefore, C may be contained in the range of 0.020 to 0.10% before decarburization annealing, for example, at the slab stage. N may be contained in the range of 0.01 to 0.05% before finish annealing, for example, after nitriding annealing. However, if these elements remain as impurities in the final product and each of C and N exceeds 0.005%, it may adversely affect the magnetic properties.
[0116] Therefore, it is preferable that the C and N contents of the final product are each 0.005% or less. It is preferable that the C and N contents of the final product are each 0.004% or less, and more preferably 0.003% or less. It is also preferable that the total C and N content of the final product is 0.005% or less. Note that C and N in the final product are impurities, and there are no particular restrictions on their contents, with the lower the better. However, since it is not industrially easy to make the C and N contents of the final product 0%, the C and N contents of the final product may each be 0.0005% or more.
[0117] S: 0% or more and 0.005% or less Se: 0% or more and 0.005% or less S (sulfur) and Se (selenium) are elements that are effective in combining with Mn and the like to exert an inhibitor effect. Therefore, S and Se may be contained in the range of 0.005 to 0.050% each before the final annealing, for example, at the slab stage. However, if these elements remain as impurities in the final product and S and Se each exceed 0.005%, it may adversely affect the magnetic properties. Therefore, S and Se in the final product are preferably 0.005% or less. S and Se in the final product are preferably 0.004% or less, and more preferably 0.003% or less. In addition, the total content of S and Se in the final product is preferably 0.005% or less. Note that S and Se in the final product are impurities, and their contents are not particularly limited, and the lower the content, the better. However, since it is not industrially easy to make the S and Se contents of the final product 0%, the S and Se contents of the final product may be 0.0005% or more.
[0118] In this embodiment, the silicon steel sheet may contain, as an optional element, at least one selected from the group consisting of, by mass%, Mn: 0.05% or more and 1.0% or less, Cr: 0.02% or more and 0.30% or less, Cu: 0.05% or more and 0.40% or less, P: 0.005% or more and 0.50% or less, Sn: 0.02% or more and 0.30% or less, Sb: 0.01% or more and 0.30% or less, Ni: 0.01% or more and 1.0% or less, B: 0.0005% or more and 0.008% or less, V: 0.002% or more and 0.15% or less, Nb: 0.005% or more and 0.20% or less, Mo: 0.005% or more and 0.10% or less, Ti: 0.002% or more and 0.015% or less, and Bi: 0.001% or more and 0.010% or less.
[0119] The chemical composition of the silicon steel sheet may be measured by a general analytical method, the details of which will be described later.
[0120] Next, other features of the silicon steel sheet will be described.
[0121] In the grain-oriented electrical steel sheet according to the present embodiment, the silicon steel sheet has a {110} <001> It is preferable that the silicon steel sheet has a texture developed in the Goss orientation. By controlling the silicon steel sheet to have the Goss orientation, the magnetic properties are preferably improved.
[0122] The thickness of the silicon steel sheet is not particularly limited, but in order to further reduce iron loss, the average thickness is preferably 0.35 mm or less, and more preferably 0.30 mm or less. The lower limit of the thickness of the silicon steel sheet is not particularly limited, but may be 0.10 mm from the viewpoint of constraints on manufacturing facilities and costs.
[0123] The surface roughness of the silicon steel sheet (roughness of the interface between the intermediate layer and the base steel sheet) is preferably smooth. For example, the surface roughness of the silicon steel sheet is preferably 0.5 μm or less, more preferably 0.3 μm or less, in terms of arithmetic mean roughness (Ra). The lower limit of the arithmetic mean roughness (Ra) of the base steel sheet is not particularly limited, but the iron loss improvement effect saturates at 0.1 μm or less, so the lower limit may be set to 0.1 μm.
[0124] Due to the above-mentioned characteristics, the grain-oriented electrical steel sheet according to this embodiment has excellent coating adhesion even without a forsterite coating, and therefore the core loss characteristics are preferably improved.
[0125] Hereinafter, the methods for measuring the various characteristics of the grain-oriented electrical steel sheets will be described in detail.
[0126] (Measurement method) First, the layer structure of the above-mentioned grain-oriented electrical steel sheet may be specified, for example, by the following method.
[0127] A test piece is cut out from the grain-oriented electrical steel sheet, and the layer structure of the test piece is observed with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). For example, layers with a thickness of 300 nm or more can be observed with an SEM, and layers with a thickness of less than 300 nm can be observed with a TEM.
[0128] Specifically, first, a test piece is cut so that the cutting direction is parallel to the plate thickness direction (more precisely, the test piece is cut so that the cut surface is parallel to the plate thickness direction and perpendicular to the rolling direction), and the cross-sectional structure of this cut surface is observed with an SEM at a magnification that allows each layer to fit within the observation field. For example, by observing using a backscattered electron composition image (COMPO image), it is possible to infer how many layers the cross-sectional structure is made up of. For example, in a COMPO image, the base steel plate can be distinguished as a light color, the intermediate layer as a dark color, and the insulating coating as a medium color.
[0129] In order to identify each layer in the cross-sectional structure, a line analysis is performed along the plate thickness direction using SEM-EDS, and the chemical composition of each layer is quantitatively analyzed. For example, the elements to be quantitatively analyzed are five elements: Fe, P, Si, O, and Mg. The device to be used is not particularly limited, but for example, an SEM (NB5000 manufactured by Hitachi High-Technologies Corporation), an EDS (XFlash(r)6│30 manufactured by Bruker AXS), and an EDS analysis software (ESPRIT1.9 manufactured by Bruker AXS) may be used.
[0130] From the observation results of the COMPO image and the quantitative analysis results of SEM-EDS described above, if a layered region is present at the deepest position in the plate thickness direction, and the Fe content is 80 atomic % or more and the O content is less than 30 atomic %, excluding measurement noise, and if the line segment (thickness) on the scanning line of the line analysis corresponding to this region is 300 nm or more, then this region is judged to be the base steel plate, and the regions excluding this base steel plate are judged to be the intermediate layer and the insulating coating.
[0131] With respect to the region excluding the base steel plate identified above, if the results of the COMPO image observation and the SEM-EDS quantitative analysis show that the Fe content is less than 80 atomic %, the P content is 5 atomic % or more, the Si content is 5 atomic % or more, and the O content is 30 atomic % or more, excluding measurement noise, and if the line segment (thickness) on the scanning line of the line analysis corresponding to this region is 300 nm or more, this region is determined to be a phosphate-based coating. In addition to the above four elements that are used as judgment elements for identifying the phosphate-based coating, the phosphate-based coating may contain the above-mentioned selective elements derived from phosphate, such as aluminum, magnesium, nickel, and manganese.
[0132] When determining whether the region is the phosphate coating, the precipitates, inclusions, and voids contained in the coating are not included in the determination, and the region that satisfies the above quantitative analysis results as the parent phase is determined to be the phosphate coating. For example, if the presence of precipitates, inclusions, and voids on the line analysis scan line is confirmed from the COMPO image or the line analysis results, this region is not included in the determination, and the region is determined based on the quantitative analysis results as the parent phase. In addition, the precipitates, inclusions, and voids can be distinguished from the parent phase by contrast in the COMPO image, and can be distinguished from the parent phase by the abundance of the constituent elements in the quantitative analysis results. In addition, when identifying the phosphate coating, it is preferable to identify it at a position where the precipitates, inclusions, and voids are not included on the line analysis scan line.
[0133] If the region excluding the base steel plate and the phosphate-based coating specified above and the line segment (thickness) on the scanning line of the line analysis corresponding to this region is 300 nm or more, this region is determined to be an intermediate layer.
[0134] The intermediate layer may satisfy the following: Fe content is less than 80 atomic %, P content is 5 atomic % or less, Si content is 20 atomic % or more, and O content is 30 atomic % or more. If the intermediate layer is not a forsterite film but an oxide film mainly composed of silicon oxide, the intermediate layer may satisfy the following: Mg content is 20 atomic % or less. The quantitative analysis result of the intermediate layer is the quantitative analysis result of the parent phase, which does not include the analysis results of precipitates, inclusions, voids, etc. contained in the intermediate layer. When identifying the intermediate layer, it is preferable to identify it at a position where precipitates, inclusions, and voids are not included on the scanning line of the line analysis.
[0135] The above COMPO image observation and SEM-EDS quantitative analysis are used to identify and measure the thickness of each layer at five or more locations by changing the observation field. The average value is calculated from the values excluding the maximum and minimum values of the thickness of each layer measured at five or more locations, and this average value is the average film thickness of each layer.
[0136] If a layer whose line segment (thickness) on the scanning line of the line analysis is less than 300 nm is present in at least one of the five or more observation fields described above, the corresponding layer is observed in detail using a TEM, and the corresponding layer is identified and its thickness is measured using the TEM.
[0137] A test piece containing a layer to be observed in detail using a TEM is cut out by FIB (Focused Ion Beam) processing so that the cutting direction is parallel to the plate thickness direction (specifically, the test piece is cut out so that the cut surface is parallel to the plate thickness direction and perpendicular to the rolling direction), and the cross-sectional structure of this cut surface is observed (bright field image) by STEM (Scanning-TEM) at a magnification that allows the corresponding layer to fit within the observation field. If each layer does not fit within the observation field, the cross-sectional structure is observed in multiple consecutive fields of view.
[0138] In order to identify each layer in the cross-sectional structure, a line analysis is performed along the plate thickness direction using TEM-EDS, and a quantitative analysis of the chemical composition of each layer is performed. The elements to be quantitatively analyzed are five elements: Fe, P, Si, O, and Mg. The device used is not particularly limited, but for example, a TEM (JEM-2100F manufactured by JEOL Ltd.), an EDS (JED-2300T manufactured by JEOL Ltd.), and an EDS analysis software (AnalysisStation manufactured by JEOL Ltd.) may be used.
[0139] From the above-mentioned bright-field image observation results by TEM and the results of quantitative analysis by TEM-EDS, each layer is identified and the average thickness of each layer is measured. The method of identifying each layer using TEM and the method of measuring the average thickness of each layer may be performed in accordance with the above-mentioned method using SEM.
[0140] When the thickness of each layer determined by TEM is 5 nm or less, it is preferable to use a TEM with a spherical aberration correction function from the viewpoint of spatial resolution. When the thickness of each layer is 5 nm or less, point analysis may be performed at intervals of, for example, 2 nm or less along the plate thickness direction, and the line segment (film thickness) of each layer may be measured and this line segment may be used as the film thickness of each layer. For example, if a TEM with a spherical aberration correction function is used, EDS analysis can be performed with a spatial resolution of about 0.2 nm.
[0141] In the grain-oriented electrical steel sheet according to this embodiment, an oxide film is present in contact with the base steel sheet, and a phosphate-based coating is present in contact with the oxide film. Therefore, when each layer is identified using the above-mentioned criteria, no layers other than the base steel sheet, the oxide film, and the phosphate-based coating are present.
[0142] The composition of the phosphate-based coating and oxide film can be determined by performing a detailed quantitative analysis using SEM-EDS or TEM-EDS within the area of the phosphate-based coating and oxide film specified above. This quantitative analysis can be performed by line analysis or point analysis at multiple locations within the target area. In addition, when quantitatively analyzing the coating composition, the elements to be quantitatively analyzed can be all elements to be quantitatively analyzed, rather than the five elements Fe, P, Si, O, and Mg.
[0143] Next, the crystallization state of cristobalite-type aluminum phosphate in the phosphate coating and the peak intensities of cristobalite-type aluminum phosphate and tridymite-type aluminum phosphate can be confirmed by grazing incidence X-ray diffraction using a Co-Kα excitation source.
[0144] For example, grazing incidence X-ray diffraction may be performed using a Co-Kα source with an X-ray incidence angle ω of 0.5° and 1.0° and a slit width of 1.0 mm. It is then confirmed whether the obtained X-ray diffraction pattern has a diffraction peak at a diffraction angle 2θ=24.8°, and the half-width of this diffraction peak is calculated.
[0145] In addition, the peak intensities of the diffraction peak appearing at a diffraction angle of 2θ=24.8° and the diffraction peak appearing at a diffraction angle of 2θ=34.3° may be obtained from the obtained X-ray diffraction pattern. The peak intensity means the intensity obtained by subtracting the background intensity from the measured intensity. The apparatus used is not particularly limited, but for example, an X-ray diffraction apparatus SmartLab manufactured by Rigaku Corporation may be used.
[0146] Next, the chemical composition of the silicon steel sheet may be observed, for example, by the following method.
[0147] For example, the chemical composition may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Note that C and S may be measured using the combustion-infrared absorption method, N may be measured using the inert gas fusion-thermal conductivity method, and O may be measured using the inert gas fusion-non-dispersive infrared absorption method.
[0148] In addition, when the grain-oriented electrical steel sheet to be used as the measurement sample has an oxide film and a phosphate-based coating on the surface, these coatings are removed by the method described below before measuring the chemical composition.
[0149] For example, a grain-oriented electrical steel sheet having a coating may be immersed in a high-temperature alkaline solution. Specifically, the coating (oxide film and phosphate-based coating) on the silicon steel sheet may be removed by immersing the sheet in an aqueous sodium hydroxide solution of 20% by mass NaOH and 80% by mass H2O at 80°C for 20 minutes, followed by rinsing with water and drying. The time for immersion in the aqueous sodium hydroxide solution may be changed depending on the thickness of the coating on the silicon steel sheet.
[0150] The texture of silicon steel sheets can be measured by a general analytical method. For example, it can be measured by X-ray diffraction (Laue method). The Laue method is a method in which an X-ray beam is irradiated perpendicularly onto a steel sheet and the transmitted or reflected diffraction spots are analyzed. By analyzing the diffraction spots, it is possible to identify the crystal orientation at the location where the X-ray beam was irradiated. By changing the irradiation position and analyzing the diffraction spots at multiple locations, it is possible to measure the crystal orientation distribution at each irradiation position. The Laue method is a method suitable for measuring the crystal orientation of a metal structure with coarse crystal grains.
[0151] The surface roughness of the silicon steel sheet (roughness of the interface between the intermediate layer and the base steel sheet) may be measured using a contact surface roughness measuring instrument or a non-contact laser surface roughness measuring instrument. If the silicon steel sheet has an oxide film and a phosphate coating on its surface, these coatings are removed by the above-mentioned method before measuring the surface roughness.
[0152] Next, a method for manufacturing the grain-oriented electrical steel sheet according to this embodiment will be described.
[0153] (Production method) Fig. 3 is a flowchart showing a method for producing a grain-oriented electrical steel sheet according to an embodiment of the present invention, in which steps surrounded by solid lines are required steps and steps surrounded by dashed lines are optional steps.
[0154] The method for producing the grain-oriented electrical steel sheet according to the present embodiment is not limited to the method described below. The method described below is one example for producing the grain-oriented electrical steel sheet according to the present embodiment.
[0155] The method for producing a grain-oriented electrical steel sheet according to this embodiment is a method for producing a grain-oriented electrical steel sheet that does not have a forsterite coating, and includes the following steps. (i) A hot rolling process in which a steel billet having a specified chemical composition is hot rolled to obtain a hot rolled steel sheet. (ii) A cold rolling process in which the hot-rolled steel sheet is subjected to cold rolling once or two or more times with intermediate annealing to obtain a cold-rolled steel sheet. (iii) a decarburization annealing step of subjecting the cold-rolled steel sheet to decarburization annealing to obtain a decarburization annealed sheet; (iv) An annealing separator application process in which an annealing separator containing Al2O3 and MgO is applied to the decarburized annealed sheet and dried. (v) a finish annealing step in which the decarburized annealed sheet coated with the annealing separator is subjected to finish annealing to obtain a finish annealed sheet; (vi) An annealing separator removal step of removing excess annealing separator from the surface of the finish annealed sheet by a method including one or both of water washing and pickling. (vii) An insulating coating forming step of forming an insulating coating on the surface of the finish annealed sheet
[0156] The method for producing the grain-oriented electrical steel sheet according to the present embodiment may further include the following steps. (I) Hot-rolled steel sheet annealing process (II) Hot-rolled sheet pickling process for pickling hot-rolled steel sheets (III) Magnetic domain control process for performing magnetic domain control processing
[0157] Each step will be described in detail below.
[0158] <Hot rolling process> In the hot rolling process, the chemical composition is, in mass%, C: 0.020% or more and 0.10% or less, Si: 0.80% or more and 7.0% or less, Mn: 0.05% or more and 1.0% or less, S+Se total: 0% or more and 0.050% or less Acid-soluble Al: 0.010% or more and 0.065% or less, N: 0.004% or more and 0.012% or less, Cr: 0 or more and 0.30% or less, Cu: 0 or more and 0.40% or less, P: 0 or more and 0.50% or less, Sn: 0 or more and 0.30% or less, Sb: 0 or more and 0.30% or less, Ni: 0 or more and 1.0% or less, B: 0 or more and 0.008% or less, V: 0 or more and 0.15% or less, Nb: 0 or more and 0.20% or less, Mo: 0 or more and 0.10% or less, Ti: 0 or more and 0.015% or less, Bi: 0 or more and 0.010% or less, The steel slab, the balance being Fe and impurities, is hot-rolled to obtain a hot-rolled steel sheet. In this embodiment, the steel sheet after the hot rolling process is called a hot-rolled steel sheet.
[0159] There is no limitation on the method for producing the steel billet (slab) to be subjected to the hot rolling process. For example, molten steel having a predetermined chemical composition may be produced, and the molten steel may be used to produce the slab. The slab may be produced by a continuous casting method, or the molten steel may be used to produce an ingot, and the ingot may be subjected to blooming to produce the slab. Alternatively, the slab may be produced by other methods.
[0160] The thickness of the slab is not particularly limited, but is, for example, 150 to 350 mm. The thickness of the slab is preferably 220 to 280 mm. As the slab, a so-called thin slab having a thickness of 10 to 70 mm may be used.
[0161] First, the reasons for limiting the chemical composition of the steel slab will be explained. In the following, % regarding the chemical composition means % by mass.
[0162] C: 0.020% or more and 0.10% or less C (carbon) is an element effective in controlling the primary recrystallization structure, but has a negative effect on magnetic properties, so it is an element that is removed by decarburization annealing before final annealing. If the C content of a steel slab exceeds 0.10%, the decarburization annealing time becomes longer and productivity decreases. Therefore, the C content is set to 0.10% or less. It is preferably 0.085% or less, and more preferably 0.070% or less.
[0163] A lower C content is preferable, but when considering the productivity in industrial production and the magnetic properties of the product, the practical lower limit of the C content is 0.020%.
[0164] Si: 0.80% or more and 7.0% or less Silicon (Si) increases the electrical resistance of grain-oriented electrical steel sheets and reduces iron loss. If the Si content is less than 0.80%, γ transformation occurs during final annealing, damaging the crystal orientation of the grain-oriented electrical steel sheets. Therefore, the Si content is 0.80% or more. The Si content is preferably 2.0% or more, and more preferably 2.50% or more.
[0165] On the other hand, if the Si content exceeds 7.0%, the cold workability decreases and cracks are likely to occur during cold rolling. Therefore, the Si content is 7.0% or less. The Si content is preferably 5.0% or less, and more preferably 3.5% or less.
[0166] Mn: 0.05% or more and 1.0% or less Manganese (Mn) increases the electrical resistance of grain-oriented electrical steel sheets and reduces iron loss. Mn also combines with S or Se to produce MnS or MnSe, which functions as an inhibitor. When the Mn content is in the range of 0.05% to 1.0%, secondary recrystallization is stable. Therefore, the Mn content is 0.05% to 1.0%. The preferred lower limit of the Mn content is 0.08%, and more preferably 0.09%. The preferred upper limit of the Mn content is 0.50%, and more preferably 0.20%.
[0167] S and / or Se: 0% to 0.050% S (sulfur) and Se (selenium) are elements that combine with Mn to form MnS or MnSe, which function as inhibitors. If the total of either or both of S and Se (S+Se) exceeds 0.050%, the precipitation and dispersion of MnS and / or MnSe becomes non-uniform after hot rolling. In this case, the desired secondary recrystallization structure cannot be obtained, the magnetic flux density decreases, or MnS remains in the steel after purification, deteriorating the hysteresis loss. Therefore, the total content of S and Se is set to 0.050% or less.
[0168] The lower limit of the total content of S and Se is not particularly limited and may be 0%. The lower limit may be 0.003% or 0.005%. When used as an inhibitor, the lower limit is preferably 0.015% or more.
[0169] Acid-soluble Al (Sol.Al): 0.010% or more and 0.065% or less Acid-soluble Al (aluminum) (Sol.Al) is an element that combines with N to produce AlN or (Al,Si)N, which functions as an inhibitor. If the acid-soluble Al content is less than 0.010%, the effect is not fully exerted and secondary recrystallization does not proceed sufficiently. Therefore, the acid-soluble Al content is set to 0.010% or more. The acid-soluble Al content is preferably 0.015% or more, more preferably 0.020% or more.
[0170] On the other hand, if the acid-soluble Al content exceeds 0.065%, the precipitation and dispersion of AlN or (Al, Si)N becomes non-uniform, the required secondary recrystallization structure cannot be obtained, and the magnetic flux density decreases. Therefore, the acid-soluble Al (Sol.Al) is set to 0.065% or less. The acid-soluble Al is preferably 0.055% or less, more preferably 0.050% or less.
[0171] N: 0.004% or more and 0.012% or less N (nitrogen) is an element that combines with Al to form AlN or (Al, Si)N, which functions as an inhibitor. If the N content is less than 0.004%, the formation of AlN or (Al, Si)N becomes insufficient, so N is set to 0.004% or more. It is preferably 0.006% or more, and more preferably 0.007% or more.
[0172] On the other hand, if the N content exceeds 0.012%, there is a concern that blisters (voids) may be formed in the steel sheet, and therefore the N content is set to 0.012% or less.
[0173] The chemical composition of the steel slab includes the above elements, with the remainder being Fe and impurities. However, in consideration of the strengthening of the inhibitor function by compound formation and the effect on magnetic properties, one or more of the selected elements may be contained in the following ranges in place of a portion of Fe. Examples of the selected elements contained in place of a portion of Fe include Cr, Cu, P, Sn, Sb, Ni, B, V, Nb, Mo, Ti, and Bi. However, since the selected elements do not have to be contained, the lower limit is 0% for each. Furthermore, even if these selected elements are contained as impurities, the above effect is not impaired. Note that "impurities" refer to those that are mixed in from ore or scrap as raw materials, or from the manufacturing environment, etc., when steel is industrially manufactured.
[0174] Cr: 0% or more and 0.30% or less, Cu: 0% or more and 0.40% or less, P: 0% or more and 0.50% or less, Sn: 0% or more and 0.30% or less, Sb: 0% or more and 0.30% or less, Ni: 0% or more and 1.0% or less, B: 0% or more and 0.008% or less, V: 0% or more and 0.15% or less, Nb: 0% or more and 0.20% or less, Mo: 0% or more and 0.10% or less, Ti: 0% or more and 0.015% or less, Bi: 0% or more and 0.010% or less, These optional elements may be contained according to known purposes. There is no need to set a lower limit for the content of these optional elements, and the lower limit may be 0%.
[0175] Next, the conditions for hot rolling the steel slab will be described. The hot rolling conditions are not particularly limited. For example, the following conditions are used. The slab is heated prior to hot rolling. The slab is charged into a known heating furnace or a known soaking furnace and heated. As one method, the slab is heated to 1280°C or less. By setting the heating temperature of the slab to 1280°C or less, it is possible to avoid various problems (such as the need for a dedicated heating furnace and a large amount of molten scale) that occur when the slab is heated at a temperature higher than 1280°C. The lower limit of the heating temperature of the slab is not particularly limited. If the heating temperature is too low, hot rolling may become difficult and productivity may decrease. Therefore, the heating temperature may be set in the range of 1280°C or less, taking productivity into consideration. The preferable lower limit of the heating temperature of the slab is 1100°C. The preferable upper limit of the heating temperature of the slab is 1250°C.
[0176] Alternatively, the slab can be heated to a high temperature of 1320°C or higher. By heating to a high temperature of 1320°C or higher, AlN and Mn(S,Se) are dissolved and finely precipitated in the subsequent process, allowing secondary recrystallization to occur stably. It is also possible to omit the slab heating process itself and start hot rolling after casting before the slab temperature drops.
[0177] Next, the heated slab is subjected to hot rolling using a hot rolling mill to produce a hot rolled steel sheet. The hot rolling mill includes, for example, a rough rolling mill and a finishing rolling mill arranged downstream of the rough rolling mill. The rough rolling mill includes rough rolling stands arranged in a row. Each rough rolling stand includes a plurality of rolls arranged vertically. Similarly, the finishing rolling mill includes finishing rolling stands arranged in a row. Each finishing rolling stand includes a plurality of rolls arranged vertically. After rolling the heated steel material by the rough rolling mill, it is further rolled by the finishing rolling mill to produce a hot rolled steel sheet. The finishing temperature in the hot rolling process (the steel sheet temperature at the exit side of the finishing rolling stand that finally rolls down the steel sheet in the finishing rolling mill) is, for example, 700 to 1150°C. The hot rolled steel sheet is produced by the above hot rolling process.
[0178] <Hot-rolled sheet annealing process> In the hot-rolled sheet annealing process, the hot-rolled steel sheet obtained in the hot rolling process is annealed (hot-rolled sheet annealing) as necessary to obtain a hot-rolled annealed sheet. In the present embodiment, the steel sheet after the hot-rolled sheet annealing process is called a hot-rolled annealed sheet.
[0179] The hot-rolled sheet annealing is performed for the purpose of homogenizing the non-uniform structure generated during hot rolling as much as possible, controlling the precipitation of AlN as an inhibitor (fine precipitation), and controlling the second phase / solubilized carbon. The annealing conditions may be selected from known conditions according to the purpose. For example, when homogenizing the non-uniform structure generated during hot rolling, the hot-rolled steel sheet is held at an annealing temperature (furnace temperature in a hot-rolled sheet annealing furnace) of 750 to 1200°C for 30 to 600 seconds. Hot-rolled sheet annealing is not necessarily performed, and whether or not to perform the hot-rolled sheet annealing process may be determined according to the properties required for the grain-oriented electrical steel sheet to be finally manufactured and the manufacturing cost.
[0180] <Hot rolled plate pickling process> In the hot-rolled steel sheet pickling process, the hot-rolled steel sheet after the hot-rolling process, or the hot-rolled steel sheet after the hot-rolled steel sheet annealing process in the case where the hot-rolled steel sheet has been annealed, is pickled as necessary to remove scale formed on the surface. The pickling conditions are not particularly limited, and may be performed under known conditions.
[0181] <Cold rolling process> In the cold rolling process, the hot-rolled steel sheet or the hot-rolled annealed sheet after the hot rolling process, the hot-rolled sheet annealing process, or the hot-rolled sheet pickling process is subjected to cold rolling once or two or more times with intermediate annealing to obtain a cold-rolled steel sheet. In this embodiment, the steel sheet after the cold rolling process is called a cold-rolled steel sheet.
[0182] A preferred cold rolling reduction in the final cold rolling (cumulative cold rolling reduction without intermediate annealing, or cumulative cold rolling reduction after intermediate annealing) is preferably 80% or more, more preferably 90% or more. A preferred upper limit of the final cold rolling reduction is 95%.
[0183] Here, the final cold rolling reduction ratio (%) is defined as follows: Final cold rolling ratio (%) = (1 - thickness of steel plate after final cold rolling / thickness of steel plate before final cold rolling) x 100
[0184] <Decarburization annealing process> In the decarburization annealing process, the cold-rolled steel sheet produced in the cold rolling process is subjected to a magnetic domain control treatment as necessary, and then decarburization annealing is performed to cause primary recrystallization. In the decarburization annealing process, C, which adversely affects magnetic properties, is removed from the steel sheet. In this embodiment, the steel sheet after the decarburization annealing process is called a decarburization annealed sheet.
[0185] For the above purpose, in the decarburization annealing, the oxidation degree (PH2O / PH2) in the annealing atmosphere (furnace atmosphere) is set to 0.01 to 0.15, and the annealing temperature is 750 to 900°C, and the temperature is held for 10 to 600 seconds. The oxidation degree, PH2O / PH2, can be defined as the ratio of the water vapor partial pressure PH2O (atm) to the hydrogen partial pressure PH2 (atm) in the atmosphere.
[0186] If the oxidation degree (PH2O / PH2) is less than 0.01, not only will the decarburization rate slow down and productivity decrease, but decarburization will be insufficient and magnetic properties will deteriorate after final annealing. On the other hand, if it exceeds 0.15, Fe-based oxides will be formed, making it difficult to smooth the interface after final annealing.
[0187] In addition, if the annealing temperature is less than 750°C, not only will the decarburization rate slow down and productivity decrease, but decarburization failure will occur and magnetic properties will deteriorate after final annealing. On the other hand, if it is more than 900°C, the primary recrystallized grain size will exceed the desired size, and magnetic properties will deteriorate after final annealing. Furthermore, if the holding time is less than 10 seconds, decarburization cannot be performed sufficiently. On the other hand, if it is more than 600 seconds, productivity will decrease, and the primary recrystallized grain size will exceed the desired size, and magnetic properties will deteriorate after final annealing.
[0188] The heating rate in the temperature rise process up to the annealing temperature may be controlled according to the degree of oxidation (PH2O / PH2). For example, when heating including induction heating is performed, the average heating rate may be set to 5 to 1000°C / sec. When heating including electrical current heating is performed, the average heating rate may be set to 5 to 3000°C / sec.
[0189] In addition, in the decarburization annealing step, a nitriding treatment may be further performed in one or more stages before, during, or after the above-mentioned holding, in which the cold-rolled steel sheet is nitrided by annealing in an atmosphere containing ammonia. When the slab heating temperature is low, it is preferable that the decarburization annealing step includes a nitriding treatment. By further performing a nitriding treatment in the decarburization annealing step, inhibitors such as AlN or (Al,Si)N are generated before the secondary recrystallization in the finish annealing step, so that secondary recrystallization can be stably expressed.
[0190] The conditions of the nitriding treatment are not particularly limited, but it is preferable to carry out the nitriding treatment so that the nitrogen content increases by 0.003% or more, preferably by 0.005% or more, and more preferably by 0.007% or more. Since the effect is saturated when the nitrogen (N) content is 0.030% or more, the nitriding treatment may be carried out so that the nitrogen content is 0.030% or less.
[0191] The conditions of the nitriding treatment are not particularly limited, and may be performed under known conditions. For example, when the nitriding treatment is performed after decarburization annealing at an oxidation degree (PH2O / PH2) of 0.01 to 0.15 and at 750 to 900°C for 10 to 600 seconds, the cold-rolled steel sheet is not cooled to room temperature, but is held in an atmosphere containing ammonia during the temperature drop process to perform the nitriding treatment. It is preferable that the oxidation degree (PH2O / PH2) is in the range of 0.0001 to 0.01 during the temperature drop process. When the nitriding treatment is performed during decarburization annealing at an oxidation degree (PH2O / PH2) of 0.01 to 0.15 and at 750 to 900°C for 10 to 600 seconds, ammonia may be introduced into the atmospheric gas of this oxidation degree.
[0192] <Annealing separator application process> In the annealing separator application process, the decarburized annealed sheet after the decarburization annealing process (including the decarburized annealed sheet that has been subjected to nitriding treatment) is subjected to magnetic domain control treatment as necessary, and then an annealing separator containing Al2O3 and MgO is applied to the sheet, and the applied annealing separator is dried.
[0193] If the annealing separator contains MgO but does not contain Al2O3, a forsterite film is formed on the steel sheet during the final annealing process. On the other hand, if the annealing separator contains Al2O3 but does not contain MgO, mullite (3Al2O3·2SiO2) is formed on the steel sheet. This mullite impedes domain wall motion and causes deterioration of the magnetic properties of grain-oriented electrical steel sheet.
[0194] Therefore, in the manufacturing method of the grain-oriented electrical steel sheet according to the present embodiment, an annealing separator containing Al2O3 and MgO is used as the annealing separator. By using an annealing separator containing Al2O3 and MgO, it is possible to obtain a steel sheet with a smooth surface without forming a forsterite film on the surface after final annealing.
[0195] The annealing separator has a mass ratio of MgO to Al2O3, MgO / (MgO+Al2O3), of 5 to 50%, and a hydration moisture content of 1.5 mass% or less. If MgO / (MgO+Al2O3) is less than 5%, a large amount of mullite is formed, which deteriorates the iron loss. On the other hand, if it exceeds 50%, forsterite is formed, which deteriorates the iron loss.
[0196] In addition, if the hydration moisture content in the annealing separator exceeds 1.5 mass%, the secondary recrystallization may become unstable, or the steel sheet surface may be oxidized (SiO2 is formed) during finish annealing, making it difficult to smooth the steel sheet surface. The lower limit of the hydration moisture content is not particularly limited, but may be, for example, 0.1 mass%.
[0197] The annealing separator is applied to the surface of the steel sheet by water slurry application, electrostatic application, etc. In the annealing separator application step, a nitride such as manganese nitride, iron nitride, chromium nitride, etc. that decomposes before secondary recrystallization in the finish annealing step to nitride the decarburized steel sheet or decarbonitrided sheet may be further added to the annealing separator.
[0198] <Finish annealing process> The decarburized annealed sheet coated with the annealing separator is then subjected to finish annealing to obtain a finish annealed sheet. By performing finish annealing on the decarburized annealed sheet coated with the annealing separator, secondary recrystallization progresses and the crystal orientation becomes {110} <001> In this embodiment, the steel sheet after the finish annealing process is called a finish annealed sheet.
[0199] During the finish annealing, if the atmosphere (furnace atmosphere) contains hydrogen, the oxidation degree (PH2O / PH2) is set to 0.00010 to 0.2, and if the atmosphere is made of an inert gas (nitrogen, argon, etc.) that does not contain hydrogen, the dew point is set to 0° C. or lower. By setting the dew point or oxidation degree in the above range according to the atmosphere, secondary recrystallization can be stably expressed and the orientation concentration can be increased.
[0200] When the atmosphere contains hydrogen, if the oxidation degree is less than 0.00010, the dense surface silica film formed by decarburization annealing is reduced before the secondary recrystallization in the finish annealing, making the secondary recrystallization unstable. On the other hand, if the oxidation degree exceeds 0.2, the decomposition of inhibitors such as AlN or (Al,Si)N is promoted, making the secondary recrystallization unstable. Also, when the atmosphere is an inert gas that does not contain hydrogen, if the dew point is more than 0°C, the decomposition of inhibitors such as AlN or (Al,Si)N is promoted, making the secondary recrystallization unstable. The lower limit of the dew point is not particularly limited, but may be, for example, -30°C.
[0201] <Annealing separator removal process> In the annealing separator removal process, excess annealing separator, such as unreacted annealing separator that did not react with the steel sheet during final annealing, is removed from the surface of the steel sheet after final annealing (finish annealed sheet) by a method including one or both of water washing and pickling.
[0202] If the excess annealing separator on the surface of the steel sheet is not sufficiently removed, the space factor deteriorates and the performance as an iron core decreases.
[0203] In order to remove excess annealing separator, in addition to washing with water and pickling, a scrubber may be used to remove it. By using a scrubber, excess annealing separator that deteriorates wettability in the insulating coating formation process can be reliably removed.
[0204] In addition, when pickling is performed to remove excess annealing separator, pickling may be performed using an acid solution with a volumetric concentration of less than 20%. For example, it is preferable to use a solution containing one or more of sulfuric acid, nitric acid, hydrochloric acid, phosphoric acid, chloric acid, aqueous chromium oxide solution, chromium sulfuric acid, permanganic acid, peroxosulfuric acid, and peroxolinic acid in total of less than 20 volume%, more preferably less than 10 volume%. The lower limit of the volumetric concentration is not particularly limited, but may be, for example, 0.1 volume%. By using such a solution, excess annealing separator on the steel sheet surface can be efficiently removed. The volumetric percentage may be a ratio based on the volume at room temperature.
[0205] Furthermore, when pickling is performed, the solution temperature is preferably set to 20 to 80° C. By setting the solution temperature within the above range, excess annealing separator on the steel sheet surface can be efficiently removed.
[0206] <Insulating film formation process> In the insulating coating forming process, the surface of the finish annealed sheet after the annealing separator removing process is subjected to a magnetic domain control treatment as necessary, and then an insulating coating is formed. In this embodiment, the steel sheet after the insulating coating forming process is called a grain-oriented electrical steel sheet.
[0207] This insulating coating applies tension to the grain-oriented electrical steel sheet, thereby reducing the iron loss of each individual steel sheet, and when grain-oriented electrical steel sheets are stacked for use, it ensures electrical insulation between the steel sheets, thereby reducing the iron loss of the iron core.
[0208] The insulating coating is formed by applying a coating solution that is primarily composed of aluminum phosphate and colloidal silica and does not contain chromate to the surface of the finish annealed sheet, baking it at 350 to 600°C, and then heat treating it at a temperature of 800 to 1000°C.
[0209] As described above, in the grain-oriented electrical steel sheet according to this embodiment, when the insulating coating is formed in the insulating coating formation step, condensation-dehydration of the phosphate-based coating progresses, causing crystallization of aluminum phosphate. The moisture generated at this time forms an intermediate layer.
[0210] In addition, the above coating solution is a first metal phosphate which is a metal phosphate of one or more metals selected from Al, Fe, Mg, Mn, Ni, and Zn, in an amount of 100 parts by mass in terms of solid content; if necessary, 0 to 20 parts by mass, calculated on a solid content basis, of a second metal phosphate which is a metal phosphate of one or more metals selected from Co, Mo, V, W, and Zr; 35 to 125 parts by mass of colloidal silica in terms of solid content; 0.3 to 6.0 parts by mass of a polymerization aid; and preferably does not contain chromate.
[0211] The average primary particle size of the colloidal silica is preferably 7 to 30 nm.
[0212] In addition, the polymerization auxiliary is preferably at least one selected from the group consisting of nitrous acid, sodium nitrite, potassium nitrite, nitric acid, sodium nitrate, potassium nitrate, chlorous acid, sodium chlorite, phosphonic acid, sodium phosphonate, triphosphoric acid, sodium triphosphate, polyphosphoric acid, and sodium polyphosphate.
[0213] Moreover, the above coating solution preferably further contains one or more selected from the group consisting of boric acid, sodium borate, titanium oxide, molybdenum oxide, pigments, and barium titanate.
[0214] The finish annealed sheet coated with the above coating solution is heated. At this time, it is important to control the heating rate (average heating rate) from room temperature to 350°C. The heating rate from room temperature to 350°C is 10°C / sec or more and less than 30°C / sec. Controlling the heating rate from room temperature to 350°C corresponds to the above condition (II).
[0215] When the heating rate from room temperature to 350°C is less than 30°C / sec, the crystallization state of cristobalite-type aluminum phosphate is controlled in both the outermost surface region and the inner region of the phosphate coating. The reason why the heating rate affects the crystallization state is unclear at present, but the following reasons are considered. For example, if the heating rate from room temperature to 350°C is less than 30°C / sec, the temperature difference between the outermost surface region and the inner region of the coating solution before the crystallization of aluminum phosphate begins is small. As a result, even when the coating solution is baked to become a phosphate coating, the temperature difference between the outermost surface region and the inner region of the phosphate coating is small, and it is considered that the crystallization state of cristobalite-type aluminum phosphate is uniformly controlled.
[0216] The upper limit of the heating rate from room temperature to 350° C. is more preferably 25° C. / sec. On the other hand, the lower limit of the heating rate is not particularly limited, and the lower the better. However, since it is not industrially easy to bring the lower limit of the heating rate close to 0, the lower limit of the heating rate may be 10° C. / sec.
[0217] In conventional manufacturing of grain-oriented electrical steel sheets, when a finish-annealed sheet coated with a coating solution is heated, the heating rate from room temperature to 350°C is generally controlled to 40°C / sec or more. In the manufacturing method of grain-oriented electrical steel sheet according to the present embodiment, in order to control the crystallization state of cristobalite-type aluminum phosphate in the phosphate-based coating in both the outermost surface region and the inner region of the phosphate-based coating, the heating rate from room temperature to 350°C is intentionally kept low, controlled to less than 30°C / sec.
[0218] After the finish annealed sheet is heated at the above heating rate, the coating solution is baked at 350 to 600°C. If the baking temperature of the insulating coating is less than 350°C, the insulating coating will drip during passing, causing poor appearance and not being able to obtain an insulating coating with sufficient adhesion. If the baking temperature exceeds 600°C, the heating rate is too fast, so that only the outermost surface of the insulating coating hardens, and the hardening of the inside is delayed, causing poor coating formation and insufficient coating adhesion.
[0219] After the baking, the steel sheet is heat-treated at a temperature of 800 to 1000°C. If the heat treatment temperature after baking is less than 800°C, the coating will not form well (hardening will be insufficient) and sufficient coating tension will not be obtained. If the heat treatment temperature exceeds 1000°C, the phosphate will decompose, resulting in poor coating formation and insufficient coating adhesion.
[0220] When forming the coating, it is preferable to set the oxidation degree of the atmosphere (PH2O / PH2) to 0.01 to 1.5, since this makes it possible to form the insulating coating without decomposing the phosphate more than necessary.
[0221] The coating solution for forming an insulating coating can be applied to the surface of the steel sheet by a wet coating method such as a roll coater.
[0222] <Magnetic domain control process> The manufacturing method of the grain-oriented electrical steel sheet according to this embodiment may include a magnetic domain control process in which a magnetic domain control treatment is performed either between the cold rolling process and the decarburization annealing process (first), between the decarburization annealing process and the annealing separator application process (second), between the annealing separator removal process and the insulating coating formation process (third), or after the insulating coating formation process (fourth).
[0223] By carrying out the magnetic domain control treatment, it is possible to further reduce the iron loss of the grain-oriented electrical steel sheet. When the magnetic domain control treatment is carried out between the cold rolling process and the decarburization annealing process, between the decarburization annealing process and the annealing separator application process, or between the annealing separator removal process and the insulating coating formation process, linear or dot-like grooves extending in a direction intersecting the rolling direction may be formed at predetermined intervals along the rolling direction to narrow the width of the 180° magnetic domains (subdivide the 180° magnetic domains).
[0224] Furthermore, when the magnetic domain control treatment is performed after the insulating coating formation process, linear or point-like stress distortion portions or groove portions extending in a direction intersecting the rolling direction can be formed at predetermined intervals along the rolling direction to narrow the width of the 180° magnetic domains (to subdivide the 180° magnetic domains).
[0225] When forming the stress-strained portion, laser beam irradiation, electron beam irradiation, etc. can be applied. When forming the groove portion, mechanical groove formation methods using gears, etc., chemical groove formation methods in which grooves are formed by electrolytic etching, and thermal groove formation methods using laser irradiation, etc. can be applied. When the insulating coating is damaged by the formation of the stress-strained portion or groove portion, causing deterioration of properties such as insulation, the insulating coating may be formed again to repair the damage. EXAMPLES
[0226] Next, the effects of one embodiment of the present invention will be described in more detail with reference to examples, but the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.
[0227] A steel slab, the chemical composition of which was adjusted so that the silicon steel sheet had the chemical composition shown in Table 1, was heated to 1150°C and subjected to hot rolling to obtain a hot-rolled steel sheet having a thickness of 2.6 mm. This hot-rolled steel sheet was subjected to hot-rolled sheet annealing as necessary, and then subjected to one cold rolling or multiple cold rolling with intermediate annealing in between to obtain a cold-rolled steel sheet having a final thickness of 0.22 mm. This cold-rolled steel sheet was subjected to decarburization annealing, and then subjected to nitriding treatment in which the sheet was held in an atmosphere containing ammonia during cooling. Note that publicly known conditions were applied from slab heating to nitriding treatment.
[0228] [Table 1]
[0229] The decarburized and annealed sheets after the above-mentioned decarburization annealing were coated with an annealing separator having the ratio of Al2O3 to MgO (MgO / (Al2O3+MgO)) and the hydration water content shown in Tables 2 and 3, and then dried. The decarburized and annealed sheets coated with the annealing separator were subjected to finish annealing at 1200°C for 20 hours.
[0230] After that, the excess annealing separator was removed using a scrubber, and then a coating solution for forming an insulating coating with adjusted components was applied. The temperature was raised under the conditions shown in Tables 2 and 3, and the wire was baked and further heat-treated to form an insulating coating.
[0231] In addition, after the insulating film formation process, magnetic domain control was performed, in which a laser was used to form stress-strained portions or grooves.
[0232] [Table 2]
[0233] [Table 3]
[0234] For the obtained test Nos. 1 to 61, the chemical composition of the silicon steel sheet, the coating composition and average thickness of the intermediate layer, the coating composition and average thickness of the insulating coating, and the crystallization state in the insulating coating were measured according to the above-mentioned methods. These results are shown in Tables 4 to 7.
[0235] [Table 4]
[0236] [Table 5]
[0237] [Table 6]
[0238] [Table 7]
[0239] Further, the obtained test pieces No. 1 to 61 were evaluated for core loss and coating adhesion.
[0240] <Iron loss> The iron loss W17 / 50 (W / kg) of samples taken from the produced grain-oriented electrical steel sheets was measured using the Epstein test at an excitation magnetic flux density of 1.7 T and a frequency of 50 Hz in accordance with JIS C 2550-1: 2011. Iron loss W17 / 50 of less than 0.70 W / kg was judged to be acceptable.
[0241] <Coating adhesion> Test pieces taken from the manufactured grain-oriented electrical steel sheets were wrapped around cylinders of 20 mm and 15 mm diameter (bent 180°), respectively, and the remaining area rate of the coating when unbent was used to evaluate the coating adhesion of the insulating coating. The coating adhesion of the insulating coating was evaluated by visual inspection to determine whether the insulating coating had peeled off. If the coating did not peel off from the steel sheet and the remaining area rate of the coating was 90% or more, it was rated "Very Good", if it was 85% or more but less than 90%, it was rated "Good", if it was 80% or more but less than 85%, it was rated "Poor", and if it was less than 80%, it was rated "NG". In both test conditions of 20 mm diameter and 15 mm diameter, if the remaining area rate of the coating was 85% or more (the above "Very Good" or "Good"), it was judged to have passed.
[0242] The results are shown in Tables 6 and 7.
[0243] As can be seen from Tables 1 to 7, the product characteristics of the invention examples Nos. 1 to 23 and Nos. 35 to 61 were within the range of the present invention, and the coating adhesion was excellent. The iron loss characteristics were also excellent. In contrast, the comparative examples Nos. 24 to 34 had at least one of the product characteristics outside the range of the present invention, and the iron loss and / or coating adhesion were poor. [Industrial Applicability]
[0244] According to the above-described embodiment of the present invention, a grain-oriented electrical steel sheet having excellent adhesion to an insulating coating even without a forsterite coating can be provided, and thus has high industrial applicability. [Explanation of symbols]
[0245] 1. Base steel plate (silicon steel plate) 2. Intermediate layer (oxide film) 3. Insulating coating (phosphate coating)
Claims
[Claim 1] A base steel plate; An intermediate layer disposed on and in contact with the base steel plate; an insulating coating disposed on and in contact with the intermediate layer; The intermediate layer is Si content: 20 at% or more and 70 at% or less, O content: 30 at% or more and 80 at% or less, Mg content: 20 at% or less, P content: 5 atomic% or less, Fe content: less than 20 atomic %; and The average thickness of the oxide film is 2 nm or more and 500 nm or less, The insulating coating is P content: 5 at% or more and 30 at% or less, Si content: 5 at% or more and 30 at% or less, O content: 30 at% or more and 80 at% or less, Al content: 0.1 at% or more and 10 at% or less, Cr content: less than 1 atomic %; Fe content: less than 25 atomic %; Mg content: 0 at% or more and 10 at% or less, Mn content: 0 at% or more and 10 at% or less, Ni content: 0 at% or more and 10 at% or less, Zn content: 0 at% or more and 10 at% or less, V content: 0 at% or more and 10 at% or less, W content: 0 at% or more and 10 at% or less, Zr content: 0 at% or more and 10 at% or less, Co content: 0 at% or more and 10 at% or less, Mo content: 0 at% or more and 10 at% or less, It is a phosphoric acid-based coating that satisfies the above, and The average thickness of the phosphoric acid coating is 0.1 μm or more and 10 μm or less, When the phosphate-based coating is subjected to glazing incidence X-ray diffraction using a Co-Kα excitation source, the X-ray diffraction pattern has a diffraction peak at a diffraction angle 2θ=24.8° derived from cristobalite-type aluminum phosphate, and The half-width of the diffraction peak under the diffraction condition of an X-ray incidence angle ω=0.5° is defined as FWHM. 0.5 The half-width of the diffraction peak under the diffraction condition of an X-ray incident angle ω=1.0° is represented as FWHM 1.0 When expressed as above, the FWHM 0.5 and the FWHM 1.0 But, 0.20°≦FWHM 0.5 ≦2.00° 0.20°≦FWHM 1.0 ≦2.00° 0°≦|FWHM 0.5 -FWHM 1.0 |≦1.00° Satisfying Grain-oriented electrical steel sheet.