Laminated core and method for manufacturing the same

JP7553879B2Active Publication Date: 2024-09-19NIPPON STEEL CORPORATION
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2024519259
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-08
Filing Date
2023-09-08
Publication Date
2024-09-19
Estimated Expiration
2043-09-08

AI Technical Summary

Technical Problem

Existing laminated core manufacturing methods face challenges in productivity due to automation difficulties and large-scale equipment requirements, particularly when laminating adhesive-coated electrical steel sheets inside or outside a mold, which result in inefficient production processes.

Method used

A method involving the lamination of electrical steel sheets with adhesive insulating coatings in a mold, where the sheets are heated to moderate temperatures and pressures, allowing for rapid bonding and cooling, thus enabling high production efficiency without the need for large cooling mechanisms.

Benefits of technology

This approach enables the production of laminated cores with sufficient tensile strength at lower temperatures and pressures, allowing for compact manufacturing equipment and streamlined processes, thereby enhancing productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553879000001
    Figure 0007553879000001
  • Figure 0007553879000003
    Figure 0007553879000003
  • Figure 0007553879000004
    Figure 0007553879000004
Patent Text Reader

Abstract

A laminated core 10 is formed by alternately laminating electromagnetic steel sheets 1 and adhesive insulating films 2. After completion of reaction of the adhesive insulating films 2, the tensile adhesive strength in a laminating direction D of the laminated core 10 is 20 MPa or higher when measured under a condition at 25°C. A method for manufacturing the laminated core 10 comprises: a punching step for punching electromagnetic steel sheets coated with the adhesive insulating films 2 and forming the electromagnetic steel sheets 1; a storage step for laminating and storing the electromagnetic steel sheets 1 in a mold after the punching step; a low-pressure adhesion step for heating the electromagnetic steel sheets 1 in the mold at a surface temperature of 60-200°C, applying pressure on the electromagnetic steel sheets at 3.0 MPa or lower, and bonding the adjacent electromagnetic steel sheets 1 to each other, to thereby form the laminated core 10; and a taking-out step for taking out the laminated core 10 from the mold after the low-pressure adhesion step.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated core and a manufacturing method for a laminated core. This application claims priority based on Japanese Patent Application No. 2022-143134 filed on September 8, 2022, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, the movement to reduce CO2 emissions has accelerated worldwide, and the application of motors (rotating electric machines, electric motors) that do not emit CO2 when in operation is spreading to various fields including automobiles. As part of this movement, motors are required to be more energy efficient and have higher output than ever before. Known lamination manufacturing technologies for laminated cores used in motors include those based on crimping and laser bonding. Laminated cores manufactured using these lamination manufacturing technologies have iron loss due to conduction from the bonded parts, and this iron loss is one of the factors that hinders power saving and high output. Recently, development of lamination manufacturing technology for laminated cores using adhesives has been progressing, with an emphasis on reducing iron loss. The lamination manufacturing technology for laminated cores using adhesives includes a method in which adhesive is applied to electromagnetic steel sheets and then punched out, and a method in which adhesive is applied to the electromagnetic steel sheets after punching out the electromagnetic steel sheets. The assembly process for stacking the adhesive-coated electromagnetic steel sheets is carried out either inside or outside the mold. The following prior art documents are related to these technologies: [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 2010-274625 [Patent Document 2] Japanese Patent Application Publication No. 2009-297758 [Patent Document 3] Japanese Patent Publication No. 2022-000888 [Patent Document 4] Japanese Patent Publication No. 2021-129453 Summary of the Invention [Problem to be solved by the invention]

[0004] The technology of laminating adhesive-coated electromagnetic steel sheets outside a mold (see Patent Document 3 or Patent Document 4) involves applying high pressure to a plurality of electromagnetic steel sheets housed inside a special jig to temporarily fix the sheets in place and removing them from the special jig, or heating the laminate fixed in the special jig at a high temperature to bond adjacent electromagnetic steel sheets together. As described above, the method of manufacturing a laminate outside a mold involves the steps of fixing in a special jig and removing the sheets, making it difficult to automate, which is a factor in reducing productivity. The technology of laminating adhesive-coated magnetic steel sheets in a mold (see Patent Document 1 or Patent Document 2) is different from the technology of laminating outside a mold in that it does not include a step of removing the laminate, and therefore is relatively easy to automate and has excellent productivity. However, after forming a laminate by adhesion through high-temperature heating, if the laminate is not rapidly cooled when transported to the next process, it takes a long time, about 3 to 4 hours, for the temperature of the laminate to drop to a temperature at which it can be transported. In addition, if the laminate is rapidly cooled when transported to the next process, a large-scale cooling mechanism for rapid cooling is required depending on the size of the laminate, and the entire manufacturing equipment including the cooling mechanism becomes large. As described above, the method of manufacturing a laminate in a mold requires a long time for manufacturing or requires a large-scale manufacturing equipment, making it difficult to scale up production, which is a factor in reducing productivity. In view of the problems with the known techniques described above, the present application provides a laminated core that can be produced with high production efficiency and a method for producing a laminated core. [Means for solving the problem]

[0005] The gist of the present invention is as follows.

[0006] (1) A laminated core according to one embodiment of the present invention has magnetic steel sheets and adhesive insulating coatings laminated alternately, and after complete reaction of the adhesive insulating coating, the tensile adhesive strength in the lamination direction is 20 MPa or more when measured at 25°C. (2) In the above item (1), the electromagnetic steel sheet in the uppermost layer may have a protrusion protruding in the stacking direction. (3) A method for manufacturing a laminated core according to one aspect of the present invention includes the steps of: laminating a plurality of electromagnetic steel sheets; , as described in (1) above The method for manufacturing a laminated core includes the steps of: punching an electromagnetic steel strip coated with an adhesive insulating coating to form the electromagnetic steel sheets; stacking the electromagnetic steel sheets and accommodating them in a mold after the punching step; heating the electromagnetic steel sheets in the mold to a surface temperature of 60°C or more and 200°C or less while applying a pressure of 3.0 MPa or less to bond adjacent electromagnetic steel sheets together to form a laminated core; and removing the laminated core from the mold after the low pressure bonding step. (4) In the above (3), the low-pressure bonding process may include an adhesion promotion process in which the temperature is increased to 100°C or more and 160°C or less at a heating rate of 0.5°C / s or more and 10.0°C / s or less, and the temperature is maintained for a period of 20 seconds or more and 120 seconds or less. (5) In the above (3) or (4), a reheating step of heating the laminated core to a temperature of 160° C. or more and 250° C. or less may be included after the removal step. (6) In any one of the above (3) to (5), in the low-pressure bonding step, the electromagnetic steel sheets in the mold may be pressed at 0.1 MPa or more. Effect of the Invention

[0007] According to the present invention, it is possible to provide a laminated core that can be manufactured with high production efficiency and a method for manufacturing a laminated core. [Brief description of the drawings]

[0008] [Figure 1] FIG. [Diagram 2] FIG. [Diagram 3] 3 is a cross-sectional view taken along the line A in FIG. 2. [Figure 4] 1 is a table showing the relationship between test specimens, test conditions, and test results in a tensile adhesion test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] To improve the productivity of laminated cores, a manufacturing technique in which adhesive-coated electromagnetic steel sheets are laminated in a mold is appropriate. However, this manufacturing technique requires high-temperature heating and cooling of the laminate (laminated core), which poses the challenge of increasing the size of the manufacturing equipment.

[0010] The laminate is heated to a high temperature in order to obtain the necessary strength using a thermosetting adhesive.

[0011] In order to promote the miniaturization or elimination of manufacturing equipment, it is effective to use an adhesive that has high strength when the laminate is completed without heating the laminate to a high temperature.

[0012] In conventional knowledge, in the manufacturing technology of laminates, there were cases where the glass transition temperature Tg (the temperature at which the adhesive hardens from a flexible state) of the adhesive used in the adhesive coating of the magnetic steel sheets was lowered (low Tg) to accelerate the adhesive hardening reaction even at low temperatures and complete hardening (attainment of the desired strength) early. However, in the case of a manufacturing technology that manufactures laminates by laminating magnetic steel sheets using an adhesive coating, there was a concern that the adhesive hardening reaction would be accelerated during transportation and storage of the manufactured laminate, resulting in unintended adhesion between materials, known as blocking. For this reason, conventional manufacturing technologies for laminates required temperature control and stacking amount control, which ultimately became an obstacle to improving production efficiency.

[0013] In order to manufacture a laminate at a low temperature without lowering the Tg, a tensile test was conducted in which a tensile force was applied to the completed laminate in the lamination direction of the steel sheets, and the tensile adhesive strength in the lamination direction of the laminate (hereinafter, the tensile adhesive strength in the lamination direction may be referred to as lamination direction tensile strength) required for a laminate used in a motor, as well as the relationship between the temperature of the adhesive and the reaction progress and strength were examined. The lamination direction tensile strength is an evaluation index uniquely determined by the present application, and is the adhesive strength of the entire laminate in the lamination direction (perpendicular to the adhesive surface of the laminate with the adhesive) of a laminate formed by fixing multiple plates with an adhesive. In detail, the lamination direction tensile strength is a value obtained by dividing the load at which the laminate breaks when a tensile load is applied to the laminate in the lamination direction by the cross-sectional area of ​​the laminate perpendicular to the lamination direction D (the adhesive area on one plate surface of the plates constituting the laminate). On the other hand, strengths measured by conventional methods include the tensile bond strength of JIS K 6849:1994 and the tensile shear bond strength of JIS K 6850:1999, but these are the bond strengths of the adhesive alone. The tensile shear bond strength is the bond strength when a shear stress parallel to the adhesive surface is applied. Here, the necessity of the lamination direction tensile strength specified in this disclosure and its differences from conventional methods will be explained. First of all, the resins used as adhesives have a bidirectional property (orientation, anisotropy). Therefore, it is necessary to evaluate them in the required direction. However, the shear tensile strength, which evaluates the tensile strength in a direction parallel to the adhesive surface, is insufficient when tension in the lamination direction is required, as in this case. Also, when tensile strength is required for test pieces containing resin, the bonding and compatibility at the interface between the resin and the steel plate are important, and the tensile bond strength of JIS K 6849:1994 is insufficient because it does not allow evaluation including the strength at the interface. In this way, the tensile strength in the lamination direction and the conventional strength represent different strengths. Using the tensile strength in the lamination direction that we have discovered, we were able to measure the adhesive strength of the entire laminate in the lamination direction, as described below. As a result of investigating the tensile strength in the lamination direction and the relationship between the temperature of the adhesive and the progress of the reaction and strength, the following findings were obtained. 1) The tensile strength in the lamination direction required for laminates used in motors varies depending on the application of the motor. For motors used in electric vehicles (EVs), drones, or vacuum cleaners, the tensile strength in the lamination direction required for laminates used in motors operated at high speed is high, at around 1 MPa, higher than the bonding strength of typical laminates bonded by crimping, which is 0.5 MPa. 2) As the temperature increases, the adhesive hardens through a process that goes from a soft state (1) to a reaction-accelerating state (2) to a reaction-completed state (3) (adhesive hardening mechanism).

[0014] In some cases, the strength exhibited at the end of the reaction (3) is emphasized, and adhesives are designed based on this strength. However, if an adhesive can ensure sufficient strength during the reaction promotion process (2) without waiting for the end of the reaction (3), then it is possible to ensure the required strength without subsequent heating.

[0015] Based on this technical concept, it was discovered that by using an adhesive that has a tensile strength in the lamination direction of 20 MPa or more at the end of the reaction, which is approximately 20 times the tensile strength in the lamination direction of approximately 1 MPa required for laminates for general motors, it is possible to ensure sufficient strength in the reaction promotion state (2) without waiting for the reaction completion state (3).

[0016] <<First embodiment>> The laminated core 10 according to the embodiment will be described. Fig. 1 is a perspective view of the laminated core 10. Fig. 2 is a plan view of the laminated core 10. Fig. 3 is a cross-sectional view taken along the line A in Fig. 2.

[0017] As shown in Fig. 1 to Fig. 3, the laminated core 10 is formed by alternately laminating magnetic steel sheets 1 and adhesive insulating coatings 2 in a lamination direction D. After the adhesive insulating coatings 2 have completely reacted, the lamination direction tensile strength in the lamination direction D is 20 MPa or more when measured under conditions of 25°C. The lamination direction tensile strength is more preferably 40 MPa or more. Here, a complete reaction refers to a cure rate of 100%, and refers to a state in which no peaks due to heat generation are generated in a DSC curve obtained by differential scanning calorimetry (DSC). As described above, the tensile strength in the lamination direction is a value obtained by dividing the load at which the laminate breaks when a tensile load is applied to the laminate in the lamination direction by the cross-sectional area of ​​the cross section perpendicular to the lamination direction D of the laminate (the adhesive area on one of the plate surfaces of the plate constituting the laminate). For example, as shown by the broken line in FIG. 1, a test specimen with a uniform cross section (for example, a cubic test specimen with a length of 45.0 mm, width of 3.6 mm, and length of 12.25 mm along the lamination direction D) cut out from the laminated core 10 is subjected to a tensile load in the lamination direction D by a tensile tester, and the maximum tensile load until the laminate breaks is divided by the cross-sectional area of ​​the cross section perpendicular to the lamination direction D of the test specimen. As shown in FIG. 1, the test specimen is a laminate in which an electromagnetic steel sheet 1 and an adhesive insulating coating 2 are laminated. The electromagnetic steel sheets constituting the test specimen are entirely bonded by an adhesive insulating coating. The breakage indicates that at least one of the adhesive insulating coatings formed between the plates constituting the laminate breaks. The tensile tester used is a tensile tester capable of subjecting the No. 5 test piece described in JIZ Z 2241:2022 to a tensile test. For example, a fully automatic tensile tester with a tester capacity of 100 kN is used. The dimensions of the test specimen are not limited to those described above, and the test specimen may be cut out from the laminated core 10 so as to include two or more layers of adhesive insulating coating 2 (three or more layers of the adherend magnetic steel sheet 1). There are also no particular limitations on the lamination direction of the test specimen and the cut-out position on the plane perpendicular to the lamination direction. However, the test specimen is cut out from the laminated core 10 so as not to include the protrusions 3. In this case, it is assumed that three or more magnetic steel sheets 1 are laminated, from the viewpoint of ease of performing the test and frequency of lamination. This allows the laminated core 10 for a motor to have the adhesive strength (for example, 1 MPa) required for the finished product to be obtained, even at a relatively low temperature (60° C. or higher and 200° C. or lower). Therefore, a high-strength laminated core 10 can be manufactured without further heating after bonding the electromagnetic steel sheets 1 together to form a laminate (laminated core). As a result, the laminated core 10 can be removed from the manufacturing equipment in a low temperature state, and the mechanism for high-temperature heating and cooling in the manufacturing equipment can be simplified, so that the manufacturing equipment for the laminated core 10 can be made compact. Thus, a laminated core 10 that can be manufactured with high production efficiency and a manufacturing method for the laminated core 10 can be provided.

[0018] The electromagnetic steel sheet 1 is, for example, an electromagnetic steel sheet 1 suitable for a high-efficiency motor. The electromagnetic steel sheet 1 may be, for example, a non-oriented electromagnetic steel sheet (for example, proprietary standard 25HX1300) having a yield strength of 394 MPa, low core loss (13.0 W / kg or less), high magnetic flux density, and a sheet thickness of 0.25 mm.

[0019] The adhesive insulating coating 2 may be an adhesive that is applied in advance to the magnetic steel sheet 1 prior to the punching step described below.

[0020] The adhesive insulating coating 2 may be coated on the surface of the magnetic steel sheet with a coating thickness of, for example, 3 μm. The adhesive insulating coating 2 may be an adhesive resin containing a thermosetting resin as shown below. The compounding ratio of the thermosetting resin, organic components other than the thermosetting resin, inorganic components, etc. shown below is adjusted so that after complete reaction, the tensile strength in the lamination direction is 20 MPa or more when measured under conditions of 25°C.

[0021] <Thermosetting resin> Specific examples of thermosetting resins include crosslinked resins such as epoxy resins, thermosetting acrylic resins, urethane resins, unsaturated polyester resins, phenolic resins, melamine resins, urea resins, and thermosetting polyimide resins. In the present invention, these resins can be used alone or in combination of two or more kinds.

[0022] (Epoxy resin) Epoxy resins are resins that contain two or more epoxy groups, and the two or more epoxy groups present in the resin are crosslinked and three-dimensionalized by an appropriate curing agent, and then cured. Examples of resins that contain epoxy groups include bisphenol-based (bisphenol A type, bisphenol F type, bisphenol AD ​​type), naphthalene-based, and cardo-skeleton epoxy resins.

[0023] (Thermosetting acrylic resin) Examples of the thermosetting acrylic resin include copolymers of acrylic acid esters or methacrylic acid esters with acrylic monomers having reactive functional groups such as hydroxyl groups, amino groups, N-methylol, N-alkoxymethylcarboxylate, allyl groups, or epoxy groups. Specific examples include copolymers of methyl acrylate or methyl methacrylate with one or more of acrylic monomers having reactive functional groups such as acrylic acid, methacrylic acid, acrylamide, N-methylolacrylamide, N-(methoxymethyl)acrylamide, allyl methacrylate, acrylic glycidyl ether, and glycidyl methacrylate. Thermosetting acrylic resins crosslink by utilizing the self-reactivity of the reactive functional groups, or crosslink by the reaction of the reactive functional groups with curing agents such as amines, and are cured.

[0024] (urethane resin) The urethane resin may be a resin consisting of a residue of a polyfunctional isocyanate compound and a hydroxyl group-containing compound. Specifically, it may be a resin consisting of an aromatic polyisocyanate such as tolylene diisocyanate, diphenylmethane isocyanate, or polymethylene polyphenylene polyisocyanate, an aliphatic polyisocyanate such as hexamethylene diisocyanate or xylene isocyanate, or a mixture thereof, and a residue of a hydroxyl group-containing compound such as polyether polyol, polyester polyol, polyacrylate polyol, or polycarbonate polyol. The urethane resin is crosslinked and cured by reaction with a curing agent such as an isocyanate-based curing agent or a polyol-based curing agent.

[0025] (Unsaturated polyester resin) Examples of unsaturated polyester resins include dehydration condensates of unsaturated dibasic acids such as maleic anhydride, fumaric acid, or itaconic acid, or compounds in which a portion of the unsaturated dibasic acids is substituted with a saturated dibasic acid such as phthalic anhydride, isophthalic acid, or terephthalic acid, and dihydric alcohols such as ethylene glycol, diethylene glycol, or propylene glycol, or compounds in which a portion of the unsaturated dibasic acids is substituted with a polyhydric alcohol such as glycerin, pentaerythritol, etc. Unsaturated polyester resins are crosslinked and cured by reaction with a curing agent such as an isocyanate-based curing agent.

[0026] (Other thermosetting resins) Examples of phenolic resins include resins having two or more phenols (phenol, cresol, etc.) in the resin. For example, resins consisting of residues of phenols and formaldehydes or aldehydes can be mentioned. Specific examples of phenolic resins include phenol novolac resins, cresol novolac resins, cresol naphthol formaldehyde polycondensates, and triphenylmethane-type polyfunctional phenyl resins. Examples of phenolic resins include phenol aralkyl resins. Examples of melamine resins include alkyl etherified melamine resins and their substitutes. Examples of urea resins include ethylene urea resins. Examples of thermosetting polyimide resins include resins consisting of residues of polyvalent carboxylic dianhydrides and diamine compounds. Specific examples of thermosetting polyimide resins include maleimide polymers, bismaleimide polymers, aminobismaleimide polymers, and bismaleimide triazine polymers. These resins also harden by crosslinking with a curing agent.

[0027] (Examples of suitable thermosetting resins) Among the above thermosetting resins, it is preferable that the thermosetting resin contains one or more selected from the group consisting of epoxy resin, acrylic resin, urethane resin, and unsaturated polyester resin, because there are many options that can make the glass transition temperature Tg 30° C. or higher, the curing reaction is fast at high temperatures, and the dispersion state of the curing agent is easy to manufacture. Among these, it is most preferable that the thermosetting resin contains an epoxy resin, because of its economical, versatile, and easy to handle properties.

[0028] <Suitable examples of adhesive resin> One suitable adhesive resin is one in which the thermosetting resin contains one or more thermosetting resins selected from the group consisting of epoxy resins, acrylic resins, urethane resins, and unsaturated polyester resins, and the total content (total mass of thermosetting resins / mass of adhesive resins×100(%)) is 20 mass% or more. If the adhesive resin contains 20 mass% or more of these thermosetting resins, the properties of these thermosetting resins can be fully utilized. Among these, an adhesive resin containing 50 mass% or more of epoxy resin is most preferable in terms of economy, versatility, and ease of handling.

[0029] The adhesive resin may contain a thermosetting resin, and may be made of a thermosetting resin or may contain organic or inorganic components other than the thermosetting resin. For example, it may contain a thermoplastic resin, an impact modifier such as core-shell rubber or natural rubber, a curing accelerator such as dimethylurea, boron trifluoride, or triphenylphosphine, a known epoxy resin modifier, a reaction control agent (such as a catalyst), a surfactant, an anti-rust agent, a lubricant, an antioxidant, an antifoaming agent, or a color pigment.

[0030] <Examples of hardeners> Specific examples of the curing agent include amine-based, amide-based, imidazole-based, acid anhydride-based, phenol-based, catalyst-based, etc. In the present invention, for example, it is possible to select a crystalline curing agent that crystallizes at room temperature from the following specific examples alone or in combination of two or more kinds.

[0031] (Amine-based hardener) Examples of the amine-based curing agent include, but are not limited to, aliphatic amines, aromatic amines, and guanidine compounds.

[0032] [Aliphatic amines] Examples of aliphatic amines include, but are not limited to, diethylenetriamine, triethylenetetraamine, tetraethylenepentamine, m-xylenediamine, trimethylhexamethylenediamine, 2-methylpentamethylenediamine, isophoronediamine, 1,3-bisaminomethylcyclohexane, bis(4-aminocyclohexyl)methane, norbornenediamine, 1,2-diaminocyclohexane, benzoylamine, methylcyclohexylamine, diazabicycloundecene, and the like.

[0033] [Aromatic amines] Examples of aromatic amines include, but are not limited to, diaminodiphenylmethane, m-phenylenediamine, diaminodiphenylsulfone (DDS), diethyltoluenediamine, trimethylenebis(4-aminobenzoate), polytetramethyleneoxide-di-p-aminobenzoate, methylaniline, and dimethylaniline.

[0034] [Guanidine compounds] Examples of guanidine compounds include, but are not limited to, dicyandiamide (DICY, cyanoguanidine) and its derivatives, methylguanidine, ethylguanidine, propylguanidine, butylguanidine, dimethylguanidine, trimethylguanidine, phenylguanidine, diphenylguanidine, and toluylguanidine.

[0035] (Amide-based hardener) Examples of amide-based curing agents include, but are not limited to, those in which an acid anhydride is added to an amine-based curing agent, and hydrazide-based compounds.

[0036] [Hydrazide compounds] Examples of hydrazide compounds include, but are not limited to, succinic acid dihydrazide, adipic acid dihydrazide, phthalic acid dihydrazide, isophthalic acid dihydrazide, terephthalic acid dihydrazide, p-oxybenzoic acid hydrazide, salicylic acid hydrazide, phenylaminopropionic acid hydrazide, and maleic acid dihydrazide.

[0037] (Imidazole-based hardener) Examples of imidazole-based curing agents include imidazole-isocyanuric acid compounds, diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (2MZ-AZINE), 1-cyanoethyl-2-ethyl-4-methylimidazole (CEMI), 2-ethyl-4-methylimidazole, and 2-undecylimidazole (C11Z).

[0038] (Acid anhydride curing agent) Examples of acid anhydride curing agents include, but are not limited to, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride.

[0039] (Phenol-based hardener) Examples of the phenol-based curing agent include, but are not limited to, phenol novolac resin, cresol novolac resin, phenol aralkyl resin, cresol aralkyl resin, naphthol aralkyl resin, biphenyl-modified phenol resin, biphenyl-modified phenol aralkyl resin, dicyclopentadiene-modified phenol resin, aminotriazine-modified phenol resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-cresol co-condensed novolac resin, and allyl acryl phenol resin.

[0040] (Catalyst type hardener) Examples of catalyst-type curing agents include, but are not limited to, cationic heat curing catalysts, BF3-amine complexes, and 1,8-diazabicyclo[5.4.0]undec-7-ene.

[0041] The curing agent preferably contains one or more crystalline curing agents selected from the group consisting of amine-based curing agents, amide-based curing agents, and imidazole-based curing agents, because the curing reaction rate of the adhesive resin composition coating during thermocompression bonding is fast and the adhesive resin composition coating can be cured relatively easily in a short time. By using such a curing agent, a difference can be set between the temperature at which the adhesive resin composition-coated electromagnetic steel sheet is stored and the heating temperature during thermocompression bonding, making it easy to control the temperature rise rate during thermocompression bonding. In terms of handling and versatility, the curing agent most preferably contains one or more selected from the group consisting of dicyandiamide (DICY), diaminodiphenylsulfone (DDS), and diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (2MZ-AZINE).

[0042] The laminated core 10 is formed by alternately laminating electromagnetic steel sheets 1 and adhesive insulating coatings 2. The laminated core 10 is made up of, for example, 600 electromagnetic steel sheets 1 and has a total thickness of about 150 mm.

[0043] Here, it is preferable that the uppermost electromagnetic steel sheet 1 has a convex portion 3 protruding in the stacking direction D. Thus, after forming the first stacked core 10 in the mold with the stacking direction D along the vertical direction, the electromagnetic steel sheet 1 at the lowermost layer of the second stacked core 10 formed on top of the first stacked core 10 in the same mold is placed in direct contact with and on top of the electromagnetic steel sheet 1 at the uppermost layer of the first stacked core 10. Then, when the second stacked core 10 is pressed in the vertical direction, the lower surface of the electromagnetic steel sheet 1 at the lowermost layer of the second stacked core 10 contacts only the upper end of the convex portion 3 formed on the upper surface of the electromagnetic steel sheet 1 at the uppermost layer of the first stacked core 10. Therefore, the adhesive force at the contact portion between the upper end of the convex portion 3 and the lower surface of the electromagnetic steel sheet 1 at the lowermost layer of the second stacked core 10 can be made smaller than the self-weight of the lowermost first stacked core 10. Therefore, when mass-producing the stacked cores 10 sequentially in the mold, due to the action of gravity, the first stacked core 10 naturally falls, so the first stacked core 10 can be separated from the second stacked core 10 and easily taken out of the mold alone. Thus, the stacked core 10 can be manufactured with high production efficiency.

[0044] The conditions for causing the above-described action of allowing the first stacked core 10 to naturally fall by the action of gravity and separating the first stacked core 10 from the second stacked core 10 are as follows. The number Q of the convex portions 3 formed on the upper surface of the uppermost electromagnetic steel sheet 1, the contact area A (m 2 ) between the upper end of the convex portion 3 and the lower surface of the lowermost electromagnetic steel sheet 1, the tensile strength σ (N / m 2 ) in the stacking direction of the stacked core 10, and the self-weight W (N) of the stacked core 10 are related by the inequality σ × A × Q < W. At this time, the adhesive area may be calculated using either the measured value from the manufactured core size or the area in the equipment design, and it is preferable to utilize the preferable one.

[0045] <<Second Embodiment>> Next, a method for manufacturing the stacked core 10 will be described. The method for manufacturing the laminated core 10 formed by laminating a plurality of electromagnetic steel sheets 1 includes a punching step of punching an electromagnetic steel strip coated with an adhesive insulating coating 2 to form the electromagnetic steel sheet 1, a housing step of laminating the electromagnetic steel sheets 1 and housing them in a mold after the punching step, a low-pressure bonding step of heating the electromagnetic steel sheets 1 in the mold to a surface temperature of 60°C to 200°C while applying a pressure of 3.0 MPa or less to bond adjacent electromagnetic steel sheets 1 to each other to form a laminated core, and a removal step of removing the laminated core 10 from the mold after the low-pressure bonding step. This allows the laminated core 10 to be integrally formed by applying pressure under conditions of relatively low temperature and relatively low pressure, and ensures the tensile strength in the lamination direction (for example, 1 MPa) required for the laminated core 10. In addition, since the applied pressure is low, no special pressurizing device for applying pressure at high pressure is required. In addition, since the applied pressure is low, the laminated core 10 can be removed from the mold early without depending on the cooling speed, without being naturally cooled over a long period of time or facilitating cooling with a special cooling device. Therefore, a method for producing the laminated core 10 with high production efficiency can be provided. Each step will be described in detail below.

[0046] (1) Preparation process An electromagnetic steel strip coated with an adhesive insulating coating 2 is prepared. Here, an adhesive resin is used as the adhesive insulating coating 2, which allows the laminated core 10 to exhibit a tensile strength in the lamination direction of 20 MPa after complete reaction. As a result, even if the laminated core 10 is formed by applying pressure at low temperature and low pressure in the low-pressure bonding process as described below, the tensile strength in the lamination direction of the laminated core 10 at the time of removal in the removal process can be made to be 1 MPa or more, which is the required level for laminated cores 10 for motors.

[0047] (2) Punching process Next, the electromagnetic steel strip coated with the adhesive insulating coating 2 is punched out to form the electromagnetic steel sheet 1 (punching process). In detail, a hollow cylindrical die is placed with its central axis aligned vertically. A punch for punching, shaped according to the outer shape of the electromagnetic steel sheet 1, is placed above the die. The electromagnetic steel strip is moved horizontally toward the die with the sheet thickness direction of the electromagnetic steel sheet 1 aligned vertically, until it is positioned between above the die and below the punch. The punch is lowered to act on the electromagnetic steel strip, punching it out.

[0048] (3) Storage process Next, after the punching step, the electromagnetic steel sheets 1 are stacked and accommodated in a die (accommodating step). In detail, the electromagnetic steel sheet 1 formed by being punched in the punching process is dropped into a die and accommodated therein. The electromagnetic steel strip is moved horizontally to punch out the next electromagnetic steel sheet 1. Then, the next electromagnetic steel sheet 1 is punched out by a punching process. The next electromagnetic steel sheet 1 falls into the die and is contained in the die stacked on top of the previous electromagnetic steel sheet 1. By repeating these procedures, the number of electromagnetic steel sheets 1 required to form the laminated core 10 is stacked in the die.

[0049] (4) Low pressure bonding process Next, the electromagnetic steel sheets 1 in the mold are heated to a surface temperature (heating temperature) of 60°C to 200°C while applying pressure of 3.0 MPa or less, and adjacent electromagnetic steel sheets 1 are bonded together to form the laminated core 10 (low pressure bonding process). If the temperature is 200°C or less, the electromagnetic steel sheets 1 in the mold can be heated without making the equipment complex or large. Here, as the adhesive insulating coating 2 of the laminated core 10, an adhesive resin is used that allows the laminated core 10 to exhibit a lamination direction tensile strength of 20 MPa after complete reaction, so that the laminated core 10 can be integrally formed by applying pressure under conditions of relatively low temperature and relatively low pressure, and the laminated direction tensile strength (for example, 1 MPa) required for the laminated core 10 can be secured. In addition, since the pressure is low, no special pressurizing device for applying pressure at high pressure is required. In addition, since the temperature is low, the laminated core 10 can be removed from the mold quickly without taking time for natural cooling or promoting cooling with a special cooling device. The heating temperature may be 150°C or less, or may be 130°C or less. The pressure may be, for example, 0.1 MPa or more, 0.5 MPa or more, or 1.0 MPa or more. The pressure may be 2.0 MPa or less, or 1.5 MPa or less. It is preferable to apply pressure to more reliably ensure tensile adhesion in the lamination direction of the laminated core, but it is not necessary to apply pressure (in this case, the pressure is 0 MPa).

[0050] (4-1) Adhesion promotion process Here, in the low pressure bonding step, the magnetic steel sheets may be heated to a temperature (heating temperature) of 100°C or more and 160°C or less at a heating rate of 0.5°C / s or more and 5.0°C / s or less, and held at this temperature for a holding time of 20 seconds or more and 120 seconds or less (adhesion promotion step). If the heating rate is too low, bonding takes a long time, and cost competitiveness decreases. Also, if the heating rate is too high, equipment is required to realize a high heating rate. Therefore, the heating rate is preferably 0.5°C / s or more and 5.0°C / s or less. This makes it possible to further promote the bonding between adjacent magnetic steel sheets 1 even when heating to 60°C or more and 200°C or less under low pressure and low temperature conditions in the low pressure bonding step. The heating temperature may be 150°C or less, or 130°C or less. The holding time may be 100 seconds or less, or 80 seconds or less. The heating rate may be 4.0°C / s or less, or 3.0°C / s or less. The temperature at which the temperature rise in the adhesion promotion step is started is not limited, but may be, for example, a temperature that is 5° C. or more lower than the temperature at which the temperature is to be raised, or may be room temperature (20° C.). The order of heating to the heating temperature of the low-pressure bonding step and the temperature increase and holding in the adhesion promotion step is not limited. For example, heating to the heating temperature of the low-pressure bonding step may be performed after the temperature increase and holding in the adhesion promotion step, or the temperature increase and holding in the adhesion promotion step may be performed during the temperature increase to the heating temperature of the low-pressure bonding step (at least a part of the time from the start of the temperature increase to the heating temperature). Furthermore, there is no limitation on the difference between the heating temperature in the low pressure bonding step and the temperature rise in the adhesion promotion step. For example, the temperature rise in the adhesion promotion step may be lower than the heating temperature in the low pressure bonding step. Cooling may be performed during the temperature rise to the heating temperature in the low-pressure bonding step or the temperature rise in the adhesion promotion step, and heating and temperature rise treatments may be performed two or more times in the low-pressure bonding step or the adhesion promotion step. However, from the viewpoint of improving production efficiency, it is preferable to perform one heating and temperature rise treatment throughout the low-pressure bonding step and the adhesion promotion step without cooling.

[0051] (5) Removal process Next, after the low pressure bonding step, the laminated core 10 is removed from the mold (removal step). At this time, the tensile strength in the lamination direction of the laminated core 10 at the time of removal is 1 MPa or more, which is required for the laminated core 10 for a motor. Therefore, the step of promoting the adhesive strength of the adhesive insulating coating 2 by further heating is no longer essential. In this manner, the laminated core 10 can be manufactured using a simple device, and the tact time and manufacturing lead time can be shortened.

[0052] (6) Reheating process After the removal step, the laminated core 10 may be heated to 160°C or higher and 250°C or lower (reheating step). This can further increase the tensile strength in the lamination direction according to the requirements for the laminated core 10. When the adhesive insulating coating is completely reacted, the tensile strength in the lamination direction measured at 25°C is 20 MPa or higher, so that the laminated core 10 can have a higher tensile strength in the lamination direction compared to conventional laminated cores.

[0053] <Other embodiments> Although one embodiment has been described in detail above with reference to the drawings, the specific configuration is not limited to the above, and various design modifications and the like are possible.

[0054] The protrusions 3 may be formed, for example, by the following method. For example, the protrusions may be formed by using a punch instead of punching out by a press process.

[0055] The laminated core 10 according to the present embodiment has magnetic steel sheets 1 and adhesive insulating coatings 2 laminated alternately, and after the adhesive insulating coatings 2 have completely reacted, the tensile strength in the lamination direction measured at 25° C. is 20 MPa or more. This allows the laminated core 10 for a motor to achieve the adhesive strength (for example, 1 MPa) required for the product, even at a relatively low temperature (60° C. or more and 200° C. or less). Therefore, the laminated core 10 having high strength can be manufactured without further heating after the magnetic steel sheets 1 are bonded together to form a laminate (laminated core). Therefore, the laminated core 10 can be removed from the manufacturing equipment at a low temperature, and the mechanism for high-temperature heating and cooling in the manufacturing equipment can be simplified, so that the manufacturing equipment for the laminated core 10 can be made compact. This allows the laminated core 10 to be manufactured with high production efficiency.

[0056] The manufacturing method of the laminated core 10 according to the present embodiment is a method for manufacturing the laminated core 10 formed by laminating a plurality of electromagnetic steel sheets 1. The manufacturing method of the laminated core 10 includes a punching step of punching an electromagnetic steel strip coated with an adhesive insulating coating 2 to form the electromagnetic steel sheet 1, a housing step of laminating the electromagnetic steel sheets 1 and housing them in a mold after the punching step, a low-pressure bonding step of heating the electromagnetic steel sheets 1 in the mold at a surface temperature of 60°C to 200°C while applying a pressure of 3.0 MPa or less to bond adjacent electromagnetic steel sheets 1 to each other to form a laminated core, and a removal step of removing the laminated core 10 from the mold after the low-pressure bonding step. This allows the laminated core 10 to be integrally formed by applying pressure under conditions of relatively low temperature and relatively low pressure, and ensures the tensile strength in the lamination direction (for example, 1 MPa) that can be required for the laminated core 10. In addition, since the applied pressure is low, no special pressurizing device for applying pressure at high pressure is required. In addition, since the applied pressure is low, the laminated core 10 can be removed from the mold quickly without being naturally cooled over a long period of time or without being accelerated by a special cooling device. Therefore, a method for producing the laminated core 10 with high production efficiency can be provided. EXAMPLES

[0057] (Layer direction tensile strength test) A test was conducted to measure the tensile strength in the lamination direction for the laminated cores manufactured under different manufacturing conditions using a fully automatic metal tensile testing machine manufactured by Shimadzu Corporation. FIG. 4 is a table showing the relationship between the test specimens, test conditions, and test results in the tensile adhesion test. In FIG. 4 , from the left, "No." indicates the number of the test specimen, "Example or Comparative Example" indicates the distinction between the example and the comparative example, "heating temperature" indicates the temperature in °C at which the stacked electromagnetic steel sheets are heated in the low-pressure bonding process in the process of forming the laminated core, "pressure" indicates the pressure in MPa at which the stacked electromagnetic steel sheets are pressed in the low-pressure bonding process in the process of forming the laminated core, "temperature rise rate" indicates the rate at which the temperature is raised from the temperature rise start temperature (room temperature (20° C.)) to the temperature rise temperature in the adhesion promotion process in °C / s, and "temperature rise amount" indicates the temperature rise amount in °C / s at which the temperature rise start temperature (room temperature (20° C.)) in the adhesion promotion process is raised from the temperature rise start temperature (room temperature (20° C.) The temperature range (= heating temperature (℃) - 20 (℃)) from the heating temperature (maximum temperature reached) is shown in ℃, "holding time" is the holding time in seconds at a temperature between 60℃ and 120℃, which is the heating temperature, and "reheating temperature" is the temperature reached by heating again after removing from the mold. "90℃ lamination direction tensile strength" is shown as "B" when the lamination direction tensile strength of the manufactured laminated core at 90℃ is 1MPa or more, "A" when the lamination direction tensile strength of the manufactured laminated core at 90℃ is 3MPa or more, and "C" when the lamination direction tensile strength is less than 1MPa. Note that under all test conditions, the heating temperature in the low pressure bonding process is the same as the heating temperature in the adhesion promotion process. The contents of the test are as follows:

[0058] The laminated core was used as a stator core for a motor. The electromagnetic steel sheets used in manufacturing the laminated core were 25HX1300 (non-oriented electromagnetic steel sheets with a thickness of 0.25 mm, low core loss, and high magnetic flux density). The laminated core is made by laminating 600 electromagnetic steel sheets. The lamination thickness (length along the lamination direction D) of the laminated core was 150 mm. The laminated core was formed by heating multiple electromagnetic steel sheets stacked in a mold to a predetermined surface temperature (heating temperature shown in FIG. 4 = heating temperature) at a predetermined heating rate shown in FIG. 4 while applying a predetermined pressure as shown in FIG. 4, starting from room temperature (20° C.) as the heating start temperature, and holding the temperature for a predetermined time as shown in FIG. 4.

[0059] The test specimen was cut into a cube shape from the laminated core as shown by the dashed line in Figure 1. The dimensions of the test specimen were 45.0 mm length along the lamination direction D × 3.6 mm width × 12.25 mm height. The 90°C lamination direction tensile strength was determined by gradually increasing the tensile load applied to the test specimen heated to 90°C in the longitudinal direction while both ends of the test specimen were held by the chucks of the tensile testing machine, and the maximum load was divided by the cross-sectional area of ​​the test specimen. Each of the magnetic steel sheets constituting the test specimen was fully bonded with an adhesive insulating coating.

[0060] The adhesive insulating coating (adhesive coat) used was an adhesive resin that had a lamination direction tensile strength of 20 MPa or more at 25°C after complete reaction, or an adhesive resin that had a lamination direction tensile strength of 14 MPa under the same conditions. The lamination direction tensile strength at 25°C after complete reaction of the adhesive resin was measured in advance using the same method as the measurement of the lamination direction tensile strength at 90°C. Specifically, in the examples of No. 1, 4, 5, 8, 9, and 11-18, the thermosetting resins used were 44 parts by mass of a phenol novolac epoxy resin (PPN201, manufactured by Nippon Kayaku Co., Ltd.), 12 parts by mass of a cresol novolac epoxy resin (YDCN-700-10, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), 10 parts by mass of a trifunctional epoxy resin (EP-3950E, manufactured by ADEKA Corporation), 10 parts by mass of a tetrafunctional epoxy resin (EP-3950E, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), and 10 parts by mass of a tetrafunctional epoxy resin (EP-3950E, manufactured by Nippon Steel Chemical & Materials Co., Ltd.). The adhesive resin used was 30 parts by mass of epoxy resin (YH-404, manufactured by Nippon Steel Materials Co., Ltd.), 4 parts by mass of bisphenol A type epoxy resin (Epicoat, manufactured by Mitsubishi Chemical Corporation), 40 parts by mass (based on thermosetting resin) of phenoxy resin (YPS-007A30, manufactured by Nippon Steel Chemical & Materials Co., Ltd.) as a thermoplastic resin, 10 parts by mass (based on thermosetting resin) of core-shell rubber, and 12 parts by mass (based on thermosetting resin) of DICY as a curing agent. The tensile strength in the lamination direction of this adhesive resin at 25°C after complete reaction was 24 MPa. In the example of No. 2, 44 parts by mass of a phenol novolac type epoxy resin (PPN201, manufactured by Nippon Kayaku Co., Ltd.), 12 parts by mass of a cresol novolac type epoxy resin (YDCN-700-10, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), 10 parts by mass of a trifunctional epoxy resin (EP-3950E, manufactured by ADEKA Corporation), 30 parts by mass of a tetrafunctional epoxy resin (YH-404, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), and 4 parts by mass of a bisphenol A type epoxy resin (Epicoat, manufactured by Mitsubishi Chemical Corporation) were used as the thermoplastic resin, 40 parts by mass (based on the thermosetting resin) of a phenoxy resin (YPS-007A30, manufactured by Nippon Steel Chemical & Materials Co., Ltd.), 10 parts by mass (based on the thermosetting resin) of core-shell rubber, and 41 parts by mass of DDS and 2 parts by mass of DCMU (based on the thermosetting resin) were used as the curing agent. After the reaction was complete, the adhesive resin had a tensile strength in the lamination direction at 25° C. of 83 MPa. In the examples of No. 3, 6, and 10, 56 parts by mass of phenol novolac type epoxy resin (PPN201, manufactured by Nippon Kayaku Co., Ltd.) and 44 parts by mass of 4-functional epoxy resin (YH-404, manufactured by Nippon Steel Chemical & Materials Co., Ltd.) were used as the thermosetting resin, 33 parts by mass (based on the thermosetting resin) of phenoxy resin (YP-50, manufactured by Nippon Steel Chemical & Materials Co., Ltd.) were used as the thermosetting resin, 5 parts by mass of core-shell rubber (based on the thermosetting resin), and 12 parts by mass of DICY and 5 parts by mass of DCMU (based on the thermosetting resin) were used as the curing agent. The tensile strength in the lamination direction of this adhesive resin at 25°C after complete reaction was 14 MPa.

[0061] The heating temperature (surface temperature) was selected from 200°C, 120°C, and 60°C and combined with other conditions.

[0062] The applied pressure was selected from 1.0 MPa, 0 MPa, and 3.0 MPa and was combined with other conditions.

[0063] The heating rate was selected from 3° C. / s, 5° C. / s, 0.15° C. / s, 10° C. / s, and 0.1° C. / s and combined with other conditions.

[0064] The temperature rise amount, which is the temperature range from room temperature (20° C.) to the heating temperature (=heating temperature), was selected from 100° C., 40° C., and 180° C. and combined with other conditions.

[0065] The holding time at the elevated temperature of 60° C. or more and 200° C. or less was selected from 20 seconds, 0 seconds, 120 seconds, and 200 seconds, and was combined with other conditions.

[0066] The reheating temperature, which is the temperature at which the molded product is heated again after being removed from the mold, was selected from among no reheating, 160°C, and 250°C, and was combined with other conditions.

[0067] A test of the tensile strength in the lamination direction was performed, and if the tensile strength in the lamination direction was 1 MPa or more, it was judged as passed, and if the tensile strength in the lamination direction was less than 1 MPa, it was judged as failed. In Fig. 4, the passed cases are indicated as "A" or "B", and the failed cases are indicated as "C".

[0068] As a result of the test, as shown in FIG. 4, the examples Nos. 1, 2, 4, 5, 8, 9, and 11-18 passed, while the comparative examples Nos. 3, 6, and 10 failed. Thus, it was confirmed that if the lamination direction tensile strength in the lamination direction D is 20 MPa or more when measured under conditions of 25°C after the adhesive insulating coating 2 has completely reacted, the lamination direction tensile strength at the time of removal from the mold (90°C) can be ensured to be 1 MPa or more even when pressurized at low temperature and low pressure in the mold. Furthermore, since the laminated core of the embodiment has a lamination direction tensile strength of 20 MPa or more under conditions of 25°C after the adhesive insulating coating has completely reacted, a laminated core having a lamination direction tensile strength higher than that of the conventional laminated core was obtained. Note that, when test specimens cut out from some of the laminated cores of the embodiment were measured, it was confirmed that the lamination direction tensile strength at 25°C was 20 MPa or more. [Explanation of symbols]

[0069] 1 Electrical steel sheet 2. Adhesive insulating coating 3 Convex 10 Laminated Core D Stacking direction

Claims

1. The magnetic steel sheets and the adhesive insulating coating are laminated alternately, After the adhesive insulating coating has completely reacted, the tensile adhesive strength in the lamination direction measured at 25° C. is 20 MPa or more. Laminated core.

2. The uppermost layer of the electromagnetic steel sheet has a protrusion protruding in the stacking direction. The laminated core according to claim 1 .

3. A method for manufacturing the laminated core according to claim 1, which is formed by laminating a plurality of electromagnetic steel sheets, comprising the steps of: a punching step of punching an electromagnetic steel strip coated with an adhesive insulating coating to form the electromagnetic steel sheet; a housing step of stacking the electromagnetic steel sheets and housing them in a mold after the punching step; a low pressure bonding process in which the electromagnetic steel sheets in the mold are heated to a surface temperature of 60° C. or more and 200° C. or less while being pressurized at 3.0 MPa or less, and adjacent electromagnetic steel sheets are bonded together to form a laminated core; and a removal step of removing the laminated core from the mold after the low pressure bonding step. A method for manufacturing a laminated core.

4. The low pressure bonding step includes an adhesion promotion step of increasing the temperature to 100° C. or more and 160° C. or less at a temperature increase rate of 0.5° C. / s or more and 5.0° C. / s or less, and maintaining the temperature for a period of 20 seconds or more and 120 seconds or less. A method for producing the laminated core according to claim 3.

5. After the removal step, a reheating step of heating the laminated core to a temperature of 160° C. or higher and 250° C. or lower is included. A method for producing the laminated core according to claim 3 or 4.

6. In the low pressure bonding step, the electromagnetic steel sheets in the mold are pressurized at 0.1 MPa or more. A method for producing the laminated core according to claim 3 or 4.